Method for producing fluororesin composition
The method of combining thermally treated and untreated fluororesins, followed by controlled heating and washing, addresses the reuse challenges of PTFE waste by enhancing chemical resistance in recycled molded products, improving both recycling efficiency and product performance.
Patent Information
- Application Number
- PCT/JP2024/019936
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-05-30
- Publication Date
- 2024-12-05
AI Technical Summary
The reuse of fired polytetrafluoroethylene (PTFE) waste is challenging due to its hard and non-moldable nature after crushing, resulting in inferior chemical resistance when recycled into molded products.
A method involving a combination of a first fluororesin with a thermal history above its melting point and a second fluororesin without such history, where the mixture is washed and heated at a controlled rate to minimize thermogravimetric reduction, enhancing chemical resistance while allowing for non-melt moldability.
This approach enables the production of molded articles with improved chemical resistance, even when using recycled fluororesin materials that have been heated above their melting point, thereby increasing recycling efficiency and product performance.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Method for producing fluororesin composition
[0001] The present invention relates to a method for producing a fluororesin composition. This application claims priority to Japanese Patent Application No. 2023-091858, filed on June 2, 2023, the contents of which are incorporated herein by reference.
[0002] Polytetrafluoroethylene resin (molding powder) obtained by suspension polymerization of tetrafluoroethylene (TFE) is compression molded and then sintered to form a molded body. The molded body obtained by sintering is processed into a molded product of the desired shape by cutting or other processes. However, once-sintered polytetrafluoroethylene resin (sintered PTFE) such as cutting chips generated during processing is hard, and even if it is crushed and compressed, it does not come together and cannot be molded. For this reason, it has been difficult to reuse it.
[0003] Patent Document 1 describes that when a powder of sintered PTFE is mixed with a PTFE dispersion (a dispersion of unsintered PTFE) obtained by emulsion polymerization of TFE, and the mixture is compression-molded and sintered to produce a molded body, the porosity after sintering decreases and the tensile strength after sintering increases as the mixing ratio of unsintered PTFE increases. For example, the document describes an example in which the porosity after sintering becomes 0% when the mixing ratio of unsintered PTFE is 100%.
[0004] Patent No. 6612001
[0005] The inventors of the present application produced sintered PTFE molded articles by the method described in Patent Document 1 using powder obtained by pulverizing cutting chips of sintered PTFE, and found that the chemical resistance of the sintered PTFE molded articles was inferior to that of molded articles produced using unsintered PTFE.
[0006] An object of the present invention is to provide a method for producing a fluororesin composition that can produce a molded article having high chemical resistance even when using a fluororesin that has a thermal history of being heated to above its melting point.
[0007] The present invention has the following aspects: [1] A method for producing a fluororesin composition comprising a first fluororesin that has a thermal history of being heated to or above its melting point, and a second fluororesin that has no thermal history of being heated to or above its melting point, wherein the first fluororesin and the second fluororesin are non-melt-formable fluororesins, the method comprising washing crushed material containing the first fluororesin, and mixing the washed crushed material with the second fluororesin, wherein the thermal weight loss rate calculated by the following formula I when the temperature of the washed crushed material is raised from 30 to 280°C at a rate of 10°C / min is 3% or less. Thermal weight loss rate = (W B1 -W A1 ) / W B1 ×100 Formula I In the above formula I, W B1 is the mass of the crushed material at 30 ° C., and W A1 is the mass of the crushed material at 280°C. [2] The method for producing a fluororesin composition according to [1], wherein the first fluororesin has tetrafluoroethylene units, and the content of the tetrafluoroethylene units relative to the total mass of the first fluororesin is 99 mass% or more. [3] The method for producing a fluororesin composition according to [1] or [2], wherein the second fluororesin has tetrafluoroethylene units, and the content of the tetrafluoroethylene units relative to the total mass of the second fluororesin is 99 mass% or more. [4] The method for producing a fluororesin composition according to any of [1] to [3], wherein the content of the first fluororesin relative to the total mass of the first fluororesin and the second fluororesin is 10 mass% or more.
[0008] According to the present invention, there can be provided a method for producing a fluororesin composition that can yield a molded article having high chemical resistance even when using a fluororesin that has a thermal history of being heated to a temperature above its melting point.
[0009] The following definitions of terms apply throughout the present specification and claims. "Monomer-based unit" is a collective term for an atomic group formed directly by polymerization of one monomer molecule and an atomic group obtained by chemically converting a portion of the atomic group. In this specification, a monomer-based unit is also simply referred to as a monomer unit. "Monomer" means a compound having a polymerizable carbon-carbon double bond. "Melting point" means the temperature corresponding to the maximum value of the melting peak measured by differential scanning calorimetry (DSC). The "to" symbol indicating a range of values means that the values before and after it are included as the lower and upper limits. "Average particle size" means the 50% cumulative value (median diameter, D50) in the number-based particle size distribution determined using a laser diffraction / scattering particle size distribution analyzer (e.g., HORIBA, Ltd., LA-920 measuring instrument). "Melt-moldable" means exhibiting melt fluidity. "Exhibiting melt fluidity" means that there is a temperature at which the melt flow rate is 0.1 to 1000 g / 10 min at a temperature 20°C or more higher than the melting point of the resin under a load of 49 N. "Melt flow rate" means the melt mass flow rate (MFR) defined in JIS K 7210:1999 (ISO 1133:1997). "Non-melt moldable" means that the material does not exhibit the melt fluidity. "Standard specific gravity (hereinafter also referred to as "SSG")" is a value that serves as an index of average molecular weight; the larger this value, the smaller the molecular weight. It can be measured in accordance with ASTM D1457-91a and D4895-91a.
[0010] <<Method for Producing Fluororesin Composition>> The method for producing a fluororesin composition of this embodiment is a method for producing a fluororesin composition comprising a first fluororesin (hereinafter also referred to as "fluororesin 1") that has a thermal history of being heated to or above its melting point, and a second fluororesin (hereinafter also referred to as "fluororesin 2") that does not have a thermal history of being heated to or above its melting point. Fluororesin 1 and fluororesin 2 are non-melt-formable fluororesins. The method for producing a fluororesin composition of this embodiment includes washing a crushed material containing fluororesin 1, and mixing the washed crushed material with fluororesin 2. The thermal weight loss rate calculated by the following formula I when the washed crushed material is heated to 30 to 280°C at a rate of 10°C / min is 3% or less,
[0011] Thermogravimetric reduction rate = (W B1 -W A1 ) / W B1 ×100 Formula I In the above formula I, W B1 is the mass of the crushed material at 30 ° C., and W A1 is the mass of the crushed material at 280°C.
[0012] <Non-melt-formable fluororesin> Both fluororesin 1 and fluororesin 2 are non-melt-formable fluororesins. Fluororesin 1 and fluororesin 2 may be the same or different. Fluororesin 1 and fluororesin 2 may each independently be one type of fluororesin, or two or more types of fluororesins may be used in combination. When two or more types of fluororesins are used in combination, it is sufficient that the mixture of the two or more types of fluororesins is non-melt-formable.
[0013] As the fluororesin 1 and the fluororesin 2, a polymer having a tetrafluoroethylene unit (hereinafter also referred to as a "TFE unit") is preferable, and examples thereof include polytetrafluoroethylene (PTFE), a tetrafluoroethylene-ethylene copolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, a tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer, a tetrafluoroethylene-chlorotrifluoroethylene copolymer, a tetrafluoroethylene-ethylene-hexafluoropropylene copolymer, and a tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer.
[0014] Preferably, fluororesin 1 and fluororesin 2 are each independently PTFE. The content of TFE units in PTFE relative to the total mass of the fluororesin is preferably 99% by mass or more. The content of TFE units relative to the total mass of PTFE is more preferably 99.5% by mass or more, and may be 100% by mass.
[0015] Examples of the monomer units other than the TFE units include the above-mentioned ethylene units, hexafluoropropylene units, perfluoro(alkyl vinyl ether) units, chlorotrifluoroethylene units, vinylidene fluoride units, as well as monomer units based on perfluoro(2,2-dimethyl-1,3-dioxole), perfluoro(4-methoxy-1,3-dioxole), perfluoroalkylethylene, etc. The monomer units other than the TFE units may be one type or two or more types. By including monomer units other than the TFE units, the crystallization of PTFE is suppressed to some extent, and the tensile strength, tensile elongation, dielectric breakdown resistance, creep resistance, etc. are improved.
[0016] (Fluororesin 1) Fluororesin 1 has a thermal history of being heated to or above its melting point at least once. Fluororesin 1 can be obtained by pulverizing cuttings generated when a primary molded body produced by heating to or above its melting point is processed into a secondary molded body such as an industrial part of a desired shape, or by pulverizing an unnecessary secondary molded body. The pulverization can be performed using a pulverizer or the like. After coarse pulverization, the material may be further pulverized. An example of the heating is heating by firing required for producing a molded body. By heating to or above its melting point, the melting point of fluororesin 1 is lowered below the melting point of fluororesin 1 before being heated to or above its melting point. The fact that "has a thermal history of being heated to or above its melting point at least once" can be confirmed by differential scanning calorimetry (DSC).
[0017] The melting point of fluororesin 1 before being heated to or above its melting point is preferably 360°C or lower, more preferably 355°C or lower, and even more preferably 350°C or lower. There are no particular restrictions on the lower limit of the melting point, but it is preferably 100°C or higher, and more preferably 150°C or higher. The melting point is preferably 100 to 360°C, more preferably 100 to 355°C, and even more preferably 150 to 350°C. When the melting point is within the above range, the mechanical strength of the resulting molded article is likely to be improved.
[0018] The melting point of fluororesin 1 is preferably 335°C or lower, more preferably 330°C or lower. There is no particular limitation on the lower limit of the melting point, but it is preferably 100°C or higher, more preferably 150°C or higher. The melting point is preferably 100 to 335°C, more preferably 150 to 330°C. When the melting point is within the above range, the mechanical strength of the obtained molded article is likely to be improved.
[0019] The bulk density of fluororesin 1 is preferably 100 g / L or more, more preferably 105 g / L or more, and even more preferably 110 g / L or more. When the bulk density is equal to or greater than the lower limit, less air is carried over during the production of a molded body, resulting in excellent deaeration properties and good fusion between powder particles. Furthermore, voids are less likely to remain in the resulting molded body, and the uniformity of the molded body is also likely to be improved.
[0020] The average particle size of the fluororesin 1 is preferably 1 to 500 μm, more preferably 5 to 300 μm, and even more preferably 5 to 100 μm. When the average particle size of the fluororesin 1 is within the above range, the uniformity of the obtained molded article is improved.
[0021] The fluororesin 1 may be, for example, crushed pieces of a molded product obtained by a method including a step of heating a molding material containing PTFE obtained by suspension polymerization to above its melting point. PTFE obtained by suspension polymerization has an extremely high melt viscosity and exhibits non-melt moldability, which means that it cannot be molded by general thermoplastic resin molding methods such as extrusion molding and injection molding. Therefore, when molding PTFE produced by suspension polymerization (hereinafter also referred to as "molding powder"), a method is used in which the molding powder is filled into a mold, compression molded, and then sintered.
[0022] Specifically, the molding powder is molded by first filling a mold with the molding powder at room temperature and compression-molding it to form a preform, which is then heated to or above the melting point of PTFE for sintering to form a primary molded body. The molding powder may be granulated as needed and used as a granulated product. During granulation, inorganic fillers and other optional components may be added. The primary molded body is then machined, such as by cutting, to form a secondary molded body of the desired shape. Examples of secondary molded bodies include industrial components such as gaskets, linings, and insulating films, and square tanks that are subjected to strong acids and strong alkalis in the semiconductor industry. Powders such as shavings, scraps, etc. (hereinafter also referred to as "shavings, etc.") generated when cutting a primary molded body to form a secondary molded body, as well as powders obtained by crushing the shavings, etc., and powders obtained by crushing unwanted secondary molded bodies can be used as the fluororesin 1. In this specification, the shavings, etc. and powders are collectively referred to as "crushed material." The secondary molded body or shavings, etc. can be crushed using a crusher or the like. After the coarse crushing, it may be further pulverized. The volume of each crushed material is, for example, 50 cm 3 The following is the result.
[0023] The method for producing a fluororesin composition of this embodiment includes washing crushed material containing fluororesin 1. The crushed material consists essentially of only fluororesin 1. However, during machining of the primary molded body, trace amounts of impurities such as oil stains and dirt may adhere to the fluororesin 1. In other words, the crushed material consists of fluororesin 1 and the trace amounts of impurities.
[0024] The thermal weight loss rate of the crushed material before washing, calculated by the above formula I (hereinafter sometimes referred to as the "thermal weight loss rate before washing"), is preferably 3 to 20%, more preferably 3 to 15%, and even more preferably 3 to 10%. When the thermal weight loss rate before washing is equal to or greater than the lower limit of the above range, the effects of the present invention are easily achieved. When the thermal weight loss rate before washing is equal to or less than the upper limit of the above range, the chemical resistance of the resulting molded product is easily improved. The thermal weight loss rate of the crushed material after washing, calculated by the above formula I (hereinafter sometimes referred to as the "thermal weight loss rate after washing"), is 3% or less, preferably 2% or less, and more preferably 1.5% or less. The lower limit of the thermal weight loss rate after washing is not particularly limited, but may be 0%. That is, the thermal weight loss rate after washing is preferably 0 to 3%, more preferably 0 to 2%, and more preferably 0 to 1.5%. When the thermal weight loss rate after washing is equal to or less than the above upper limit, the chemical resistance of the resulting molded product is easily improved. In order to more reliably obtain the effects of the present invention, it is most preferable that the rate of thermal weight loss after washing is 0%.
[0025] Examples of washing liquids for washing the crushed material include water, organic solvents, surfactants, etc. Furthermore, washing liquids such as aqueous solutions containing two or more of these may also be used. The amount of washing liquid used is preferably 10 to 5,000 parts by mass, more preferably 50 to 4,000 parts by mass, and even more preferably 100 to 3,000 parts by mass, per 100 parts by mass of the crushed material. Washing may be performed by Method 1, in which the crushed material is immersed in the washing liquid and allowed to stand, Method 2, in which the crushed material is stirred, or Method 3, in which the washing liquid is poured over the crushed material. The immersion time is preferably more than 0 hours and not more than 100 hours, more preferably more than 0 hours and not more than 80 hours, and even more preferably more than 0 hours and not more than 60 hours. The temperature of the washing liquid is preferably 0 to 200°C, more preferably 10 to 150°C. In Methods 1 and 2, the crushed material and the washing liquid are then preferably subjected to solid-liquid separation by filtration or the like, followed by drying. In Method 1 and Method 2, when the process from adding a washing solution to the mixture to solid-liquid separation is counted as one washing, washing is preferably carried out 1 to 30 times, more preferably 1 to 25 times, and even more preferably 2 to 20 times. Similarly, washing in Method 3 is preferably carried out multiple times.
[0026] The crushed material to be washed may be crushed material such as shavings directly generated during the production of a secondary molded body, or may be crushed powder obtained by pulverizing a secondary molded body or shavings, etc. From the viewpoint of operability, crushed material such as shavings directly generated during the production of a secondary molded body is preferred.
[0027] (Fluororesin 2) Fluororesin 2 does not have a thermal history of being heated to or above its melting point. The melting point of fluororesin 2 is preferably 360°C or lower, more preferably 355°C or lower, and even more preferably 350°C or lower. The lower limit of the melting point is not particularly limited, but is preferably 100°C or higher, and more preferably 150°C or higher. The melting point is preferably 100 to 360°C, more preferably 100 to 350°C, and even more preferably 150 to 350°C. When the melting point is within the above range, the mechanical strength of the obtained molded product is likely to be improved.
[0028] The fluororesin 2 may be, for example, a fluororesin produced by emulsion polymerization. Emulsion polymerization is a polymerization method in which a monomer is polymerized in an aqueous medium containing water to obtain a dispersion containing particles of the fluororesin 2. In general, emulsion polymerization is performed by a method in which a reaction liquid containing water, a polymerization initiator, and a surfactant is polymerized in the reaction liquid while the reaction liquid is stirred.
[0029] From the viewpoint of suppressing coloration of the resulting molded article, the content of the nonionic surfactant is preferably 2 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.1 parts by mass or less, per 100 parts by mass of the fluororesin in the dispersion. Examples of nonionic surfactants will be described later.
[0030] The content of the fluororesin 2 in the dispersion is preferably from 5 to 40% by mass, more preferably from 7 to 35% by mass, and even more preferably from 10 to 30% by mass.
[0031] The average particle size of the fluororesin 2 contained in the dispersion is preferably 0.05 to 0.5 μm, more preferably 0.08 to 0.45 μm, and even more preferably 0.10 to 0.35 μm. When the average particle size is within this range, the emulsion stability is excellent.
[0032] The fluororesin 2 preferably contains PTFE obtained by emulsion polymerization. In the method of producing PTFE by emulsion polymerization, TFE monomer is homopolymerized in the reaction solution, or TFE monomer is copolymerized with a monomer other than TFE monomer in the reaction solution to obtain a dispersion in which PTFE particles are dispersed in a dispersion medium. For example, in the presence of an aqueous medium, a polymerization initiator, an anionic fluorine-containing emulsifier, and a stabilizing aid, the TFE monomer is emulsion-polymerized, preferably over 1 to 20 hours, at a pressure of preferably 0.5 to 3.0 MPa, to obtain a dispersion. The nonionic surfactant may also be blended. Alternatively, a dispersion may be obtained without using a fluorine-based surfactant by the methods described in WO 2021 / 085470, WO 2022 / 181662, etc.
[0033] Examples of the anionic fluorine-containing emulsifier will be described later. The amount of the anionic fluorine-containing emulsifier used in the emulsion polymerization step of TFE monomer is preferably 0.15 to 2.0 parts by mass, more preferably 0.2 to 1.0 part by mass, and even more preferably 0.2 to 0.5 part by mass, per 100 parts by mass of the PTFE to be produced.
[0034] As the stabilizing aid, paraffin wax, fluorine-based oil, fluorine-based solvent, silicone oil, etc. are preferred, with paraffin wax being more preferred. One stabilizing aid may be used alone, or two or more may be used in combination. Paraffin wax may be liquid, semi-solid, or solid at room temperature, with saturated hydrocarbons having 12 or more carbon atoms being preferred. The melting point of paraffin wax is preferably 40 to 65°C, more preferably 50 to 65°C. The amount of stabilizing aid used is preferably 0.1 to 12 parts by mass, more preferably 0.1 to 8 parts by mass, per 100 parts by mass of the aqueous medium used.
[0035] As the polymerization initiator, a water-soluble radical initiator or a water-soluble oxidation-reduction catalyst is preferably used. As the water-soluble radical initiator, persulfates such as ammonium persulfate and potassium persulfate; and water-soluble organic peroxides such as disuccinic acid peroxide, bisglutaric acid peroxide, and tert-butyl hydroperoxide are preferred. The polymerization initiator may be used alone or in combination of two or more. Oil-soluble initiators can also be used. As the polymerization initiator, disuccinic acid peroxide is more preferred. The amount of the polymerization initiator used is preferably 0.01 to 0.20 parts by mass, more preferably 0.01 to 0.15 parts by mass, per 100 parts by mass of the PTFE to be produced.
[0036] The standard specific gravity (SSG) of the PTFE resin contained in the dispersion is an index of the average molecular weight of PTFE, and it can be conceptually classified as high molecular weight PTFE when the SSG is 2.14 or more but less than 2.22, and low molecular weight PTFE when the SSG is 2.22 to 2.4. Since the physical properties of PTFE decrease when the molecular weight is low, the SSG is preferably 2.14 or more but less than 2.22, and more preferably 2.14 to 2.21.
[0037] (Anionic Fluorine-Containing Emulsifier) Examples of the anionic fluorine-containing emulsifier used in emulsion polymerization include fluorine-containing emulsifiers represented by general formula (1) (hereinafter also referred to as "fluorine-containing emulsifier (1)"). General formula (1): XCF 2 CF 2 (O) m CF 2 CF 2 OCF 2 COOA (wherein X is a hydrogen atom or a fluorine atom, and A is a hydrogen atom, an alkali metal, or NH 4 and m is 0 or 1. The fluorine-containing emulsifier (1) is preferred in that it has a good effect of stabilizing the polymerization of PTFE particles.
[0038] The X is preferably a fluorine atom in terms of polymerization stability. The m is preferably 1 in terms of polymerization stability and mechanical stability of the dispersion. Specific examples of A include H, Li, Na, K, and NH. 4 The fluorine-containing emulsifier (1) has good solubility in water and metal ion components are unlikely to remain as impurities, and therefore, NH 4 Particularly preferred examples of the fluorine-containing emulsifier (1) are CF 3 CF 2 CF 2 CF 2 OCF 2 COONH 4 , C 2 F 5 OCF 2 CF 2 OCF 2 COONH 4 (hereinafter referred to as EEA), with EEA being more preferred.
[0039] The fluorine-containing emulsifier (1) can be produced by fluorinating an ester of a corresponding non-fluorine-containing carboxylic acid or partially fluorinated carboxylic acid by a known fluorination method such as a liquid-phase fluorination method in which the ester is reacted with fluorine in a liquid phase, a fluorination method using cobalt fluoride, or an electrochemical fluorination method, hydrolyzing the ester bond of the obtained fluorinated ester, purifying it, and then neutralizing it with ammonia.
[0040] (Nonionic Fluorine-Containing Emulsifier) Examples of the nonionic surfactant to be blended in the aqueous emulsion obtained by emulsion polymerization include a nonionic surfactant represented by general formula (2) (hereinafter also referred to as "nonionic surfactant (2)") and a nonionic surfactant represented by general formula (3) (hereinafter also referred to as "nonionic surfactant (3)"). General formula (2): R 1 -O-D-H (wherein, R 1 is an alkyl group having 8 to 18 carbon atoms, O is an oxygen atom, and D is a polyoxyalkylene chain consisting of 5 to 20 oxyethylene groups and 1 to 2 oxypropylene groups.) General formula (3): R 2 -OE-G (wherein, R 2 is an alkyl group having 6 to 18 carbon atoms, O is an oxygen atom, E is a polyoxyalkylene chain consisting of 1 to 3 oxybutylene groups and 5 to 20 oxyethylene groups, and G is a hydrogen atom or a methyl group.) One type of nonionic surfactant may be used alone, or two or more types may be used in combination.
[0041] The nonionic surfactant contained in the dispersion is preferably one or more selected from the group consisting of nonionic surfactants (2) and (3), and two or more may be used in combination. Nonionic surfactants (2) and (3) may also be combined.
[0042] Note that nonionic surfactants are mixtures of multiple molecules with a certain chain length distribution and a mixture of isomers, and the chain length of the polyoxyalkylene chain represents the average chain length of the multiple molecules. The number of oxyethylene groups and oxypropylene groups in the polyoxyalkylene chain is an average value. Also, when multiple types of nonionic surfactants are mixed and used, it is sufficient that the average number of oxyalkylene groups in each nonionic surfactant is within the above-mentioned range. Furthermore, each numerical value is not limited to an integer.
[0043] In the nonionic surfactant (2), R 1 The number of carbon atoms in the alkyl group represented by R is preferably in the range of 8 to 18, and more preferably 10 to 16. 1When the number of carbon atoms is equal to or greater than the lower limit of the above range, the surface tension of the dispersion is likely to be low and the wettability is likely to be improved. When the number of carbon atoms is equal to or less than the upper limit, the storage stability of the dispersion is excellent. When the alkyl group, which is the hydrophobic group, has a branched structure in which it branches off midway, this is preferred in that it is easier to improve the wettability of the dispersion. The alkyl group having a branched structure is preferably an alkyl group branched in the range from the carbon atom at the base of the alkyl group to the fifth carbon atom, and more preferably an alkyl group branched in the range from the carbon atom at the base of the alkyl group to the third carbon atom. In addition, the branched carbon atom may be a secondary carbon atom or a tertiary carbon atom, and a secondary carbon atom is preferred. The alkyl group having a branched structure includes, for example, C 10 H 21 CH (CH 3 ) CH 2 -, C 9 H 19 CH(C 3 H 7 ) -, C 6 H 13 CH(C 6 H 13 )- and the like can be exemplified.
[0044] In the nonionic surfactant (2), the hydrophilic group D is a polyoxyalkylene chain consisting of 5 to 20 oxyethylene groups and 1 to 2 oxypropylene groups. In particular, a polyoxyalkylene chain consisting of 7 to 12 oxyethylene groups and 1 to 2 oxypropylene groups results in favorable dispersion properties. When D contains an oxypropylene group, defoaming properties are likely to be improved. Having 2 or fewer oxypropylene groups is preferred in that it reduces surface tension, facilitates wettability, and reduces repelling during recoating. Furthermore, in D, the oxypropylene group may be present between the polyoxyethylene groups or may be bonded to the end of the polyoxyethylene chain. Bonding an oxypropylene group to the end of the polyoxyethylene chain facilitates enhanced defoaming properties. In particular, bonding an oxypropylene group to the molecular terminal of the polyoxyethylene chain facilitates enhanced defoaming properties.
[0045] In the nonionic surfactant (2), the average number of oxyethylene groups per molecule is preferably 5 to 20, more preferably 7 to 12. When the average number of oxyethylene groups per molecule is equal to or greater than the lower limit of the above range, good storage stability is likely to be obtained. When the average number of oxyethylene groups per molecule is equal to or less than the upper limit of the above range, good wettability is likely to be obtained. As the nonionic surfactant (2), C 13 H 27 O (C 2 H 4 O) 8 C 3 H 6 OH, C 13 H 27 O (C 2 H 4 O) 9 C 3 H 6 OH, C 13 H 27 O (C 2 H 4 O) 10 (C 3 H 6 O) 2 H, C 16 H 27 O (C 2 H 4 O) 12 (C 3 H 6 O) 2 Commercially available nonionic surfactants having an average molecular structure such as H can be used.
[0046] The content of the nonionic surfactant (2) is preferably 2 to 12 parts by mass, more preferably 4 to 12 parts by mass, per 100 parts by mass of the fluororesin in the dispersion. When the content is equal to or greater than the lower limit of the above range, good storage stability is likely to be obtained. A high content of the nonionic surfactant (2) is suitable for applications requiring thick coating, but no improvement in performance is observed even when the content exceeds the upper limit of the above range, and therefore, for economic reasons, it is preferably equal to or less than the upper limit of the above range.
[0047] In the nonionic surfactant (3), R 2The number of carbon atoms in the alkyl group represented by the formula (I) is preferably in the range of 6 to 18, more preferably 8 to 16, and even more preferably 10 to 14. When the number of carbon atoms in the alkyl group is equal to or greater than the lower limit of the above range, the surface tension of the dispersion tends to be low and wettability tends to be increased. When the number of carbon atoms in the alkyl group is equal to or less than the upper limit of the above range, the dispersion tends to have excellent storage stability. When the number of carbon atoms in the alkyl group is within the above range, the wettability and storage stability are good.
[0048] R 2 The alkyl group represented by the formula (I) preferably has a branched structure, since it is easier to increase the wettability of the dispersion. The branched carbon atom may be a secondary carbon atom or a tertiary carbon atom, and a secondary carbon atom is preferred. The alkyl group having a branched structure is preferably a C 10 H 21 CH (CH 3 ) CH 2 -, C 9 H 19 CH(C 3 H 7 ) -, C 6 H 13 CH(C 6 H 13 ) -, CH(CH 3 ) 2 CH 2 CH (CH 3 ) 2 CH 2 CH (CH (CH 3 ) 2 CH 2 - etc. can be exemplified. 2 In the alkyl group represented by the formula (I), 10% or less of the hydrogen atoms in the alkyl group may be substituted with a halogen atom such as a fluorine atom, a chlorine atom, a bromine atom, etc. The alkyl group may also contain one or two unsaturated bonds.
[0049] E in general formula (3) is a polyoxyalkylene chain consisting of 1 to 3 oxybutylene groups and 5 to 20 oxyethylene groups. The number of oxybutylene groups is preferably 1 to 2.5, more preferably 1 to 2. When it is equal to or greater than the lower limit of the above range, the defoaming properties, wettability, and viscosity properties tend to be good. When it is equal to or less than the upper limit, the viscosity increase of the dispersion is suppressed, and good stability is likely to be obtained. When it is within the above range, properties such as viscosity, stability, defoaming properties, and wettability are good, which is preferable. The oxybutylene group may be branched or linear, with branched being preferred.
[0050] The oxybutylene group is —CH 2 -CH(C 2 H 5 )-O-,-CH(C 2 H 5 ) CH 2 -O-, -CH(CH 3 )-CH(CH 3 ) —O—, —CH 2 CH 2 -CH(CH 3 ) —O—, —CH 2 CH 2 CH 2 CH 2 Among them, —CH 2 -CH(C 2 H 5 )-O-,-CH(C 2 H 5 ) CH 2 —O—, —CH 2 CH 2 -CH(CH 3 )-O- is preferred. Examples of raw materials for the oxybutylene group include various butylene oxides, and specific examples include 1,2-butylene oxide, 2,3-butylene oxide, tetrahydrofuran, and methyloxetane.
[0051] In the nonionic surfactant (3), the number of oxyethylene groups in the polyoxyalkylene chain is 5 to 20, preferably 6 to 15, and more preferably 7 to 13. When the number is equal to or greater than the lower limit of the above range, the storage stability of the dispersion tends to be good. When the number is equal to or less than the upper limit, the wettability tends to be good. When the number is within the above range, properties such as viscosity, stability, defoaming property, and wettability are good, which is preferable. The oxybutylene groups in the polyoxyalkylene chain may have a block structure or a random structure.
[0052] The oxybutylene group may be present at any position in the polyoxyalkylene chain, but R 2 It is preferable that the —O— group is present in the range up to 70% of the total length of the polyoxyalkylene chain, and R 2 It is more preferable that the R of the polyoxyalkylene chain is present in the range from the —O— group side to 50% of the total length of the polyoxyalkylene chain. 2 The portion bonded to the -O- group is preferably an oxybutylene group, more preferably a polyoxybutylene chain consisting of 1 to 2 oxybutylene groups. Furthermore, the portion of the polyoxyalkylene chain bonded to the G group is preferably an oxyethylene group, more preferably a polyoxyethylene chain consisting of 5 to 20 oxyethylene groups. Polyoxyalkylene chains having these preferred structures are preferred because they have better properties such as viscosity, stability, defoaming properties, and wettability. G in general formula (3) is a hydrogen atom or a methyl group, preferably a hydrogen atom.
[0053] The nonionic surfactant (3) can be obtained by addition reaction of butylene oxide and ethylene oxide with a higher alcohol by a known method. Butylene oxide and ethylene oxide may be mixed and reacted simultaneously, or butylene oxide may be reacted first and then ethylene oxide, or ethylene oxide may be reacted first and then butylene oxide. The method of reacting butylene oxide first and then ethylene oxide is preferred.
[0054] As the nonionic surfactant (3), C 13 H27 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 8 H、C 10 H 21 HH(H) 3 )CH 2 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 8 H、C 10 H 21 HH(H) 3 )CH 2 OCH(C 2 H 5 )CH 2 O(C 2 H 4 O) 8 H、C 12 H 25 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 8 H、C 8 H 17 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 10 H、C 12 H 25 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 10 H、C 13 H 27 OCH 2 CH(C 2 H 5 )O(C 2 H 4 O) 11 H、C 13 H 27 OCH 2 CH 2 OCH 2 CH(C2 H 5 )O(C 2 H 4 O) 8 H、C 12 H 25 O(CH 2 CH(C 2 H 5 )O) 2 (C 2 H 4 O) 8 H、C 10 H 21 CH(CH 3 )CH 2 O(C 2 H 4 O) 9 CH 2 CH(C 2 H 5 )OH、C 16 H 33 OC 2 H 4 P.S. 2 H 5 )CH 2 O(C 2 H 4 O) 9 H、C 12 H 25 SO 2 CH(C 2 H 5 )O(C 2 H 4 O) 8 CH 2 CH(C 2 H 5 )OH、C 13 H 27 P.S. 3 )CH(CH 3 )O(C 2 H 4 O) 8 H、C 10 H 21 CH(CH 3 )CH 2 P.S. 3 )CH(CH 3 )O(C 2 H 4 O) 8 H、C 10 H 21 CH(CH 3)CH 2 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 8 H、C 12 H 25 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 8 H、C 8 H 17 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 10 H、C 12 H 25 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 10 H、C 13 H 27 OCH(CH) 3 )CH(CH 3 )O(C 2 H 4 O) 11 H、C 13 H 27 O(CH) 2 ) 4 O(C 2 H 4 O) 8 H、C 12 H 25 O(CH) 2 ) 4 O(C 2 H 4 O) 8 H、C 8 H 17 O(CH) 2 ) 4 O(C 2 H 4 O) 10 H、C 12 H 25 O(CH) 2 ) 4 O(C 2 H 4 O) 10 H、C 13 H27 O(CH 2 ) 4 O(C 2 H 4 O) 11 H, C 13 H 27 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 8 H, C 12 H 25 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 8 H, C 8 H 17 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 10 H, C 12 H 25 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 10 H, C 13 H 27 O(CH 2 ) 2 CH(CH 3 )O(C 2 H 4 O) 11 Examples include H, etc.
[0055] When the dispersion contains nonionic surfactant (3), the content of nonionic surfactant (3) is preferably 0.1 to 12 parts by mass, more preferably 0.5 to 11 parts by mass, and even more preferably 1 to 10 parts by mass, per 100 parts by mass of the fluororesin in the dispersion. When the content is equal to or greater than the lower limit of the above range, good storage stability is likely to be obtained. In addition, cracks are less likely to occur in the fluororesin coating film, and repellency is less likely to occur. A high content of nonionic surfactant (3) is suitable for applications requiring thick coating, but no improvement in performance is observed even when the content exceeds the upper limit of the above range, and therefore, for economic reasons, it is preferable that the content be equal to or less than the upper limit of the above range.
[0056] When nonionic surfactant (2) and nonionic surfactant (3) are used in combination as a nonionic surfactant, the average number of oxybutylene groups per molecule of the nonionic surfactant as a whole is preferably 0.5 to 2, more preferably 0.7 to 1.7, and even more preferably 0.9 to 1.5. Nonionic surfactant (2) and nonionic surfactant (3) may be added separately. A mixture containing nonionic surfactant (3) and nonionic surfactant (2) by-produced during the preparation of nonionic surfactant (3) may also be used.
[0057] The dispersion contains water as a dispersion medium for the fluororesin particles. This water may be water contained in the aqueous emulsion obtained by emulsion polymerization, or water prepared separately from the water in the aqueous emulsion. The dispersion may optionally contain one or more of a pH adjuster (e.g., ammonia), an anionic surfactant, a polyethylene oxide thickener, a polyurethane thickener, a thixotropic agent, a silicone wettability improver, a fluorine wettability improver, or a preservative. Furthermore, the dispersion may contain one or more of a water-soluble organic solvent, an organic solvent (e.g., toluene, xylene), a pigment (e.g., titanium oxide, iron oxide, carbon black, cobalt blue), glass powder, hollow glass beads, or a colorant (e.g., graphite particles, silica particles, mica, or titanium oxide-coated mica powder).
[0058] <Mixing of first fluororesin and second fluororesin> Fluororesin 1 and fluororesin 2 can be mixed by mixing the crushed material containing fluororesin 1 after the washing with fluororesin 2. The crushed material consists essentially of fluororesin 1. The crushed material is preferably in powder form. That is, when crushed material such as shavings that are directly generated during the production of a secondary molded body is washed, it is preferable to crush and finely pulverize the washed shavings using a crusher or the like to form powder.
[0059] The mixing method may be exemplified by the following modes (1) to (4), with mode (4) being preferred. (1) Dry mixing of powdered fluororesin 1 (crushed material) and powdered fluororesin 2. (2) Mixing of powdered fluororesin 1 (crushed material) and a dispersion in which fluororesin 2 is dispersed. (3) Mixing of a dispersion in which fluororesin 1 (crushed material) is dispersed with powdered fluororesin 2. (4) Mixing of a dispersion in which fluororesin 1 (crushed material) is dispersed with a dispersion in which fluororesin 2 is dispersed.
[0060] The dispersion in which the fluororesin 1 is dispersed is preferably a dispersion obtained by mixing the powdered fluororesin 1 produced by the above-described production method with a water-soluble organic solvent. From the viewpoint of miscibility with the fluororesin 1 and water, the water-soluble organic solvent is preferably one or more water-soluble organic solvents selected from the group consisting of aprotic water-soluble organic solvents and alcohols. The alcohols may have an amino group or an alkoxy group as a substituent. The aprotic water-soluble organic solvent is preferably acetone, tetrahydrofuran, or acetonitrile. The alcohol is preferably methanol, ethanol, propanol, isopropyl alcohol, or 1-methoxy-2-propanol. Of these, isopropyl alcohol is more preferable as the water-soluble organic solvent. One type of water-soluble organic solvent may be used alone, or two or more types may be used in combination.
[0061] The content of Fluororesin 1 relative to the total mass of the dispersion in which Fluororesin 1 is dispersed is preferably from 3 to 70 mass %, more preferably from 5 to 65 mass %, and even more preferably from 10 to 60 mass %.
[0062] The dispersion in which the fluororesin 2 is dispersed is preferably a dispersion in which the fluororesin 2 is dispersed by the above-mentioned emulsion polymerization. A dispersion in which a nonionic surfactant has been blended into the dispersion to improve storage stability may also be used. When using powdered fluororesin 2, the powdered fluororesin 2 may be obtained by separating the fluororesin 2 from the solvent by filtration, drying, or the like from the dispersion in which the fluororesin 2 is dispersed.
[0063] The content of the fluororesin 2 relative to the total mass of the dispersion in which the fluororesin 2 is dispersed is preferably from 5 to 40 mass %, more preferably from 7 to 35 mass %, and even more preferably from 10 to 30 mass %.
[0064] In the cases of the above embodiments (2) to (4), the combined content of fluororesin 1 and fluororesin 2 relative to the total mass of the mixture is preferably 10 to 50 mass%, more preferably 12 to 45 mass%, and even more preferably 15 to 35 mass%. When the combined content of fluororesin 1 and fluororesin 2 is equal to or greater than the lower limit of the above range, fluororesin 1 and fluororesin 2 tend to aggregate, facilitating solid-liquid separation. When the combined content of fluororesin 1 and fluororesin 2 is equal to or less than the upper limit of the above range, mixing of fluororesin 1 and fluororesin 2 is likely to be promoted.
[0065] In the case of the above embodiment (4), the content of the water-soluble organic solvent relative to 100 parts by mass of water in the mixture is preferably 1 to 150 parts by mass, more preferably 3 to 140 parts by mass, and even more preferably 5 to 130 parts by mass.
[0066] In this embodiment, the mixture may be washed. The mixture can be washed by adding a washing liquid to a mixture containing powdered fluororesin 1 and fluororesin 2. In the above embodiments (2) to (4), the mixture is stirred and agglomerated to obtain an agglomerate. The agglomerate is filtered to separate the agglomerate and the solvent, and the agglomerate is washed with a large amount of water. Thereafter, the mixture is dried to obtain a mixture containing powdered fluororesin 1 and fluororesin 2.
[0067] Examples of cleaning liquids used to wash the mixture include water and organic solvents. Alternatively, cleaning liquids such as aqueous solutions containing two or more of these may be used. The amount of cleaning liquid used is preferably 10 to 5,000 parts by mass, more preferably 50 to 4,000 parts by mass, and even more preferably 100 to 3,000 parts by mass, relative to 100 parts by mass of the solid content of the mixture. Washing may be performed by Method 1, in which the mixture is immersed in the cleaning liquid and allowed to stand, Method 2, in which the mixture is stirred, or Method 3, in which the cleaning liquid is poured over the mixture. The immersion time is preferably more than 0 hours and not more than 100 hours, more preferably more than 0 hours and not more than 80 hours, and even more preferably more than 0 hours and not more than 60 hours. The temperature of the cleaning liquid is preferably 0 to 200°C, more preferably 10 to 150°C. In Methods 1 and 2, the mixture and the cleaning liquid are then preferably subjected to solid-liquid separation by filtration or the like, followed by drying. In Method 1 and Method 2, when the process from adding a washing solution to the mixture to solid-liquid separation is counted as one washing, washing is preferably carried out 1 to 30 times, more preferably 1 to 25 times, and even more preferably 2 to 20 times. Similarly, washing in Method 3 is preferably carried out multiple times.
[0068] <Fluororesin Composition> The fluororesin composition produced by the production method of this embodiment contains fluororesin 1 and fluororesin 2. The fluororesin composition may contain one or more solid components other than fluororesin 1 and fluororesin 2. Examples of other solid components include solid components used in the production process of fluororesin 1, solid components used in the production process of fluororesin 2, and solid components added after the production of fluororesin 1 and fluororesin 2. Specific examples include inorganic fillers, pigments (e.g., titanium oxide, iron oxide, carbon black, cobalt blue, etc.), colorants (e.g., graphite particles, silica particles, mica or titanium oxide-coated mica powder, etc.), the additives, etc. Examples of inorganic fillers include reinforcing fibers (e.g., glass fiber, carbon fiber, etc.), glass powder, bronze powder, graphite powder, hollow glass beads, etc. The content of other solid components is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less, based on the total mass of the solid contents of the fluororesin composition. It may be zero.
[0069] The total content of fluororesin 1 and fluororesin 2 relative to the total mass of the solid content of the fluororesin composition is preferably 30 to 100 mass%, more preferably 40 to 100 mass%, and even more preferably 50 to 100 mass%. The fluororesin composition is preferably solid, more preferably powdered. The content of fluororesin 1 relative to the total mass of fluororesin 1 and fluororesin 2 is preferably 10 mass% or more, more preferably 10 to 90 mass%, even more preferably 15 to 85 mass%, and particularly preferably 20 to 80 mass%. When the content of fluororesin 1 is equal to or greater than the lower limit of the above range, recycling efficiency is improved when fluororesin 1 is derived from cuttings or the like during the production of the secondary molded body described above (in the case of recycled fluororesin). When the content of fluororesin 1 is equal to or less than the upper limit of the above range, the surface smoothness and compressive strength of the resulting molded body are likely to be improved.
[0070] <Molded body> The molded body of this embodiment can be obtained by compression molding the powdered fluororesin composition described above and firing it. Specifically, the powdered fluororesin composition is placed in a mold and compression molded under pressure to obtain a preform, and the preform obtained is fired to obtain a primary molded body. The shape of the primary molded body is not particularly limited. For example, it may be a block shape such as a cylindrical or polygonal pillar shape.
[0071] When the fluororesin composition is compression molded, the pressure is 100 to 350 kg / cm 2 The baking temperature after the preforming is preferably 360 to 380°C.
[0072] The obtained molded article (primary molded article) may be processed by cutting or the like to produce a molded article (secondary molded article) having a desired shape. Examples of uses of the secondary molded article include seals, packings, rollers, sockets, and joints.
[0073] The molded article of this embodiment may be the primary molded article or the secondary molded article.
[0074] (Chemical Resistance of Molded Article) The chemical resistance of the molded article can be evaluated by Immersion Tests 1 to 3 in the Examples described later. The mass change rate 1 in Immersion Test 1 is preferably 5% or less, more preferably 2% or less, and even more preferably 1% or less. The mass change rate 2 in Immersion Test 2 is preferably 5% or less, more preferably 2% or less, and even more preferably 1% or less. The mass change rate 3 in Immersion Test 3 is preferably 8% or less, more preferably 5% or less, and even more preferably 1% or less.
[0075] <Mechanism of Action> The fluororesin composition of the present invention contains fluororesin 1 that has a thermal history of being heated to or above its melting point. When fluororesin 1 originates from chips or the like during the production of the above-mentioned secondary molded article, trace amounts of impurities such as oil stains and dust from the cutting process or the like may be mixed in. The present inventors have found for the first time that the mixing of such impurities impairs the chemical resistance of molded articles obtained from the fluororesin composition. They have also found that washing the crushed material such as chips can suppress the decrease in chemical resistance and increase the recycling efficiency of the fluororesin.
[0076] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. In the following examples, Example 1 is an example, and Example 2 is a reference example.
[0077] <Evaluation Method> (Melting Point) Using a differential scanning calorimeter (DSC 8500, manufactured by Perkin Elmer), the fluororesin was heated to 380° C. at a rate of 10° C. / min in an air atmosphere, and the melting point was determined from the endothermic peak. When there were multiple endothermic peaks, the peak temperature of the largest endothermic peak was used.
[0078] (Average Particle Diameter) Using a laser diffraction / scattering particle size distribution analyzer (LA-920, manufactured by Horiba, Ltd.), powdered fluororesin was dispersed in water, and the particle size distribution was measured on a number basis to calculate the average particle diameter.
[0079] (Standard Specific Gravity) Measured in accordance with ASTM D1457-91a and D4895-91a.
[0080] (Thermal Weight Loss Rate) Using a NEXTA STA200 manufactured by Hitachi High-Tech Science Corporation, the crushed material before and after washing, which will be described later, was heated from 30 to 280°C at a rate of 10°C / min, and the thermal weight loss rate was measured according to the above formula I.
[0081] (Immersion Test 1) 0.5 g of the molded article obtained in Example 1 or Example 2 was placed in a container, and 35 mL of hydrofluoric acid with a concentration of 46.0 to 48.0 mass % was added. The container was sealed and left to stand at 85°C for 7 days while changing the liquid every day. Thereafter, the molded article was washed with water and dried, and the mass of the molded article after the immersion test was measured. The mass change rate 1 was calculated using the following formula II. Mass change rate 1=(W B2 -W A2 ) / W B2 × 100 Formula II In the above Formula II, W B2 is the mass of the molded body before the immersion test, and W A2 is the mass of the molded body after the immersion test.
[0082] (Immersion Test 2) 0.5 g of the molded article obtained in Example 1 or Example 2 was placed in a container, and a mixed solution of sulfuric acid and hydrogen peroxide (volume ratio of 98% sulfuric acid:30% hydrogen peroxide solution 2:1) was added until the molded article was completely immersed. The container was sealed and left to stand at 80°C for 7 days while changing the solution every day. Thereafter, the molded article was washed with water and dried, and the mass of the molded article after the immersion test was measured. Mass change rate 2 was calculated using the following formula III. Mass change rate 2=(W B3 -W A3 ) / W B3 × 100 Formula III In the above formula III, W B3 is the mass of the molded body before the immersion test, and W A3 is the mass of the molded body after the immersion test.
[0083] (Immersion Test 3) A test was carried out in the same manner as in Immersion Test 2, except that the standing period was changed to 28 days. The mass change rate 3 was calculated using the following formula IV. Mass change rate 3 = (W B4 -W A4 ) / W B4 ×100 Formula IV In the formula IV, W B4 is the mass of the molded body before the immersion test, and W A4 is the mass of the molded body after the immersion test.
[0084] (Production Example 1) A powdery fluororesin A (molding powder) consisting of only TFE units was produced by suspension polymerization. The fluororesin A was a fluororesin that had no thermal history of being heated above its melting point.
[0085] (Production Example 2) Fluororesin A was preformed and then baked at or above its melting point to produce a primary molded body. A secondary molded body was cut out from the resulting primary molded body to obtain crushed pieces (crushed material before washing). 1000 parts by mass of water was added to 100 parts by mass of the crushed material, and the mixture was stirred and then filtered for washing. After repeating this washing three times, the washed crushed material was dried at 200°C for 10 hours. The dried crushed material (crushed material after washing) was pulverized to obtain powdered fluororesin B with an average particle size of 50 μm or less. Fluororesin B was a fluororesin with a thermal history of being heated above its melting point. The melting point of the resulting fluororesin B was 329°C. The resulting fluororesin B was non-melt-moldable, as there was no temperature at which the melt flow rate was 0.1 to 1000 g / 10 min at temperatures 20°C or more higher than the melting point of the resin under a load of 49 N. 200 g of fluororesin B and 200 g of isopropanol were mixed to obtain dispersion B. The content of fluororesin B relative to the total mass of dispersion B was 50 mass%. The thermal weight loss rate of the crushed material before washing, calculated from the above formula I, was 4.4%, and the melting point was 326°C. The thermal weight loss rate of the crushed material after washing, calculated from the above formula I, was 0%.
[0086] (Production Example 3) 36 g of EEA, 555 g of paraffin wax (melting point 55 ° C), and 61.3 L of deionized water were charged into a 100 L stainless steel autoclave equipped with a baffle and a stirrer. After the interior of the autoclave was purged with nitrogen and reduced pressure, TFE was introduced and the temperature was raised to 62 ° C with stirring. TFE was further injected until the internal pressure reached 1.765 MPa, and 26.3 g of disuccinic acid peroxide (concentration 80 mass%, remainder water) was dissolved in 1 L of warm water at about 70 ° C and injected. After about 3 minutes, the internal pressure of the autoclave dropped to 1.716 MPa, so TFE was injected to maintain the internal pressure at 1.765 MPa, and polymerization was allowed to proceed. During the polymerization, EEA was dissolved in warm water and a total of 53 g of EEA was injected in two batches. The autoclave temperature was gradually raised to 72°C, and the reaction was terminated when the amount of TFE injected reached 22 kg, and the TFE in the autoclave was released into the atmosphere. The polymerization time was 105 minutes. After cooling, the solidified paraffin wax on top was removed, yielding Dispersion C, in which fluororesin C composed solely of TFE units produced by emulsion polymerization was dispersed. The content of fluororesin C relative to the total mass of Dispersion C was approximately 25.0 mass%, and the EEA concentration was 0.40 mass parts per 100 mass parts of fluororesin C. The average particle size of fluororesin C in Dispersion C was 0.26 μm. The standard specific gravity (SSG) of fluororesin C was 2.21. The melting point of fluororesin C was 337°C. The resulting fluororesin C was non-melt-moldable, as there was no temperature at which the melt flow rate was 0.1 to 1,000 g / 10 min at temperatures 20°C or more higher than the melting point of the resin under a load of 49 N.
[0087] Example 1 798 g of dispersion C and 802 g of water were placed in an 8 L stainless steel tank equipped with a baffle and a stirrer and stirred. 400 g of dispersion B was added to the stirred dispersion C to obtain dispersion D containing a mixture of fluororesin B and fluororesin C. The mass ratio of fluororesin B to fluororesin C in dispersion D (fluororesin B:fluororesin C) was 1:1. The mass ratio of IPA to water (IPA:water) in dispersion D was 12:88. The total content of fluororesin B and fluororesin C relative to the total mass of dispersion D was 20.0 mass%. The mixture was stirred at 680 rpm using a stirrer for 10 minutes to aggregate the solids in dispersion D, and the aggregates and solvent were separated by filtration. The filtered aggregates were washed with a large amount of water, and then placed in a tray and vacuum dried at 25°C for 2 hours or more, and then dried at 200°C for 10 hours or more, thereby obtaining fluororesin composition 1, which was a mixture of powdered fluororesin B and powdered fluororesin C. 345 g of the obtained fluororesin composition 1 was placed in a mold with a diameter of 7.3 mm and subjected to a pressure of 320 kg / cm. 2 A preform was obtained by pressing at 380°C for 2 hours. This preform was then fired at 380°C for 2 hours to obtain a molded body. The obtained molded body was skived to produce a sheet with a thickness of 0.5 mm, and a test specimen in the shape of a microdumbbell measuring 16 mm x 45 mm was punched out to obtain molded body 1. Immersion tests 1 to 3 were carried out using molded body 1. The results are shown in Table 1.
[0088] (Example 2) A molded body was prepared in the same manner as in Example 1, except that fluororesin A was used instead of fluororesin composition 1, to obtain molded body 2, which was a microdumbbell-shaped test piece. Immersion tests 1 to 3 were carried out using molded body 2. The results are shown in Table 1.
[0089]
[0090] Molded body 1 of Example 1 showed a small mass change rate in immersion tests 1 to 3, and was found to have excellent chemical resistance.
Claims
1. A method for producing a fluororesin composition comprising a first fluororesin having a thermal history of being heated to or above its melting point, and a second fluororesin having no thermal history of being heated to or above its melting point, wherein the first fluororesin and the second fluororesin are non-melt moldable fluororesins, the method includes washing a crushed material containing the first fluororesin, and mixing the washed crushed material with the second fluororesin, wherein the thermal weight loss rate calculated by the following formula I when the washed crushed material is heated to 30 to 280°C at a rate of 10°C / min is 3% or less. Thermal weight loss rate = (W B1 -W A1 ) / W B1 × 100 Formula I In the above formula I, W B1 is the mass of the crushed material at 30° C., and W A1 is the mass of the crushed material at 280°C.
2. A method for producing a fluororesin composition as described in claim 1, wherein the first fluororesin has tetrafluoroethylene units and the content of the tetrafluoroethylene units relative to the total mass of the first fluororesin is 99 mass% or more.
3. A method for producing a fluororesin composition as described in claim 2, wherein the second fluororesin has tetrafluoroethylene units and the content of the tetrafluoroethylene units relative to the total mass of the second fluororesin is 99 mass% or more.
4. A method for producing a fluororesin composition according to any one of claims 1 to 3, wherein the content of the first fluororesin relative to the total mass of the first fluororesin and the second fluororesin is 10 mass% or more.
Citation Information
Patent Citations
Game machine
JP2023091858A
Method for producing sintered fluororesin body, sintered fluororesin body, method for producing fluororesin dispersion, method for producing sintered body, fluororesin dispersion, and sintered body
JP6612001B1
Method for producing polytetrafluoroethylene aqueous dispersion
WO2021085470A1
Method for producing polytetrafluoroethylene aqueous dispersion
WO2022181662A1
Graft modification method for regeneration of polytetrafluoroethylene powder
CN114437403A