Method for polishing object to be polished, and polishing pad

The polishing method and pad utilize a hydrolyzable resin and abrasive grains to adjust the abrasive grain protrusion height based on pH and concentration, allowing a single pad to perform various polishing stages, thus improving efficiency by eliminating the need for multiple pads and equipment.

WO2024248130A1PCT designated stage expired Publication Date: 2024-12-05KUREHA CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/020033
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-31
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing polishing methods for semiconductor wafers require multiple polishing pads with different abrasive grain sizes, leading to inefficient processing due to the need for additional equipment and time-consuming processes, as the degree of polishing cannot be effectively changed with a single pad.

Method used

A polishing method and pad using a hydrolyzable resin and abrasive grains, where the abrasive grain protrusion height is adjusted by varying the pH and concentration of the polishing liquid, allowing for a single pad to perform from rough to precision polishing by promoting hydrolysis of the resin to expose or bury abrasive grains.

Benefits of technology

Enables efficient change in polishing rate and surface roughness using a single polishing pad, enhancing processing efficiency by adjusting the abrasive grain protrusion height through pH and concentration changes in the polishing liquid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024020033_05122024_PF_FP_ABST
    Figure JP2024020033_05122024_PF_FP_ABST
Patent Text Reader

Abstract

This method for polishing an object to be polished includes a step for polishing the object to be polished by sliding a polishing pad having a polishing layer containing a composition including a hydrolyzable resin and abrasive grains relative to the object to be polished. The step for polishing the object to be polished includes: a first step for polishing the object to be polished while supplying a first polishing liquid containing a hydrolysis promoter for promoting hydrolysis onto the surface of the polishing layer; and a second step, after the first step, for polishing the object to be polished while supplying a second polishing liquid having a lower concentration of the hydrolysis promoter than the first polishing liquid onto the surface of the polishing layer.
Need to check novelty before this filing date? Find Prior Art

Description

Polishing method for object to be polished and polishing pad

[0001] The present invention relates to a polishing method for an object to be polished and a polishing pad.

[0002] In the manufacturing process of substrates used in semiconductor devices, a cylindrical single crystal (ingot) is sliced ​​into discs to form wafers, which are then roughly polished (lapping, primary polishing) to ensure that both sides of the wafer are parallel and to the specified thickness. The roughly polished wafers then undergo chemical etching and precision mechanical polishing (secondary polishing, mechanical polishing) to achieve a highly flat mirror surface. Finally, a chemical process is added to achieve atomic-level flatness by finishing polishing (chemical mechanical polishing, CMP).

[0003] In such polishing processes, a polishing method using a polishing pad is adopted. As a polishing pad, a polishing pad having a polishing layer containing a binder resin and abrasive grains fixed by the binder resin is known (see, for example, Patent Document 1). As the binder resin, a curable resin such as a phenol resin, an epoxy resin, or an acrylic phenol resin is usually used.

[0004] In polishing, in order to smooth the surface of the workpiece, it is common to use multiple polishing pads with different abrasive grain sizes depending on the degree of polishing, from rough polishing to precision mechanical polishing. For example, rough polishing is performed using a polishing pad with a large abrasive grain size, and then precision mechanical polishing is performed using a polishing pad with a small abrasive grain size.

[0005] JP 2018-51733 A

[0006] However, when using multiple polishing pads with different abrasive grain sizes, it is necessary to use multiple devices for each polishing pad or to replace the polishing pads. This requires additional capital investment and requires time and effort for processing, resulting in poor work efficiency. Therefore, it is desirable to be able to change the polishing level with a single polishing pad.

[0007] The present invention has been made in consideration of the above circumstances, and aims to provide a polishing method and a polishing pad for an object to be polished that can change the polishing speed and surface roughness of the object to be polished with a single polishing pad, thereby improving work efficiency.

[0008] [1] A method for polishing an object to be polished, comprising the steps of polishing the object by sliding the object against a polishing pad having a polishing layer containing a composition including a hydrolyzable resin and abrasive grains, the step of polishing the object comprising: a first step of polishing the object while supplying a first polishing liquid containing a hydrolysis accelerator to the surface of the polishing layer, and a second step of polishing the object while supplying a second polishing liquid having a lower concentration of hydrolysis accelerator than the first polishing liquid to the surface of the polishing layer after the first step. [2] The method for polishing an object to be polished according to [1], wherein the first step polishes the object while adjusting the height of protruding abrasive grains from the surface of the polishing layer to H1 by supplying the first polishing liquid, and the second step polishes the object while adjusting the height of protruding abrasive grains from the surface of the polishing layer to H2, which is lower than H1, by supplying the second polishing liquid. [3] The method for polishing an object to be polished according to [1] or [2], wherein the hydrolysis accelerator is an alkaline substance. [4] The method for polishing a workpiece according to any one of [1] to [3], wherein the hydrolyzable resin is primarily composed of a glycolic acid polymer. [5] The method for polishing a workpiece according to any one of [1] to [4], wherein the pH of the first polishing liquid is higher than 12 and the pH of the second polishing liquid is 12 or less. [6] A polishing pad, comprising a polishing layer containing a composition containing a hydrolyzable resin and abrasive grains, wherein, when H1' is the height of abrasive grains protruding from the surface of the polishing layer when polished with a polishing liquid having a pH of 13, and H2' is the height of abrasive grains protruding from the surface of the polishing layer when polished with a polishing liquid having a pH of 12, H2' / H1' is 0.79 or less. [7] The polishing pad according to [6], wherein the median diameter of the abrasive grains is 2 μm or more and 50 μm or less. [8] The polishing pad according to [6] or [7], wherein a molded product of the composition excluding the abrasive grains exhibits a thickness reduction rate of 12 μm / h or more when immersed in water at 60°C. [9] The polishing pad according to any one of [6] to [8], wherein the tensile strength of a molded body made of the composition excluding the abrasive grains is 55 MPa or more.

[0009] According to the present invention, it is possible to provide a method for polishing an object to be polished that can change the polishing rate and the surface roughness of the object to be polished using a single polishing pad, thereby improving processing efficiency.

[0010] Fig. 1A is a schematic cross-sectional view showing the state of abrasive grains near the surface of the polishing layer, and Fig. 1B is a graph showing an example of the relationship between the pH of the polishing liquid and the protruding height of the abrasive grains in the polishing layer. Fig. 2A is a schematic plan view of a polishing pad according to one embodiment of the present invention, and Fig. 2B is a schematic cross-sectional view of the polishing pad of Fig. 2A taken along line 2B-2B. Fig. 3 is a schematic cross-sectional view showing a polishing method for a polished object according to one embodiment of the present invention. Figs. 4A to 4C are schematic cross-sectional views showing the molding process in an example. Figs. 5A and 5B are graphs showing the pH dependence of the protruding height of the abrasive grains in the polishing pads of the example and comparative example.

[0011] The present inventors have investigated various binder resins for fixing abrasive grains in polishing pads and found that hydrolyzable resins such as glycolic acid polymers and lactic acid polymers exhibit appropriate disintegration properties upon hydrolysis. They have also found that using such hydrolyzable resins as the binder resin makes it possible to easily expose the abrasive grains buried in the binder resin to the surface of the polishing layer.

[0012] Furthermore, after further investigation, the inventors discovered that by adjusting the pH of the polishing liquid that is brought into contact with an abrasive layer containing a hydrolyzable resin and abrasive grains, the height at which the abrasive grains protrude from the surface of the abrasive layer can be changed, thereby changing the polishing speed and the surface roughness (abrasiveness) of the object to be polished.

[0013] 1A is a schematic cross-sectional view showing the state of abrasive grains 112 near the surface of the polishing layer, and FIG. 1B is a graph showing an example of the relationship between the pH of the polishing liquid and the protruding height of the abrasive grains in the polishing layer. In FIG. 1A, (a) shows the polishing layer immediately after preparation, (b) shows the polishing layer after contact with a relatively weakly alkaline polishing liquid, and (c) shows the polishing layer after contact with a relatively strongly alkaline polishing liquid.

[0014] In the polishing layer immediately after fabrication, the abrasive grains 112 are embedded in the hydrolyzable resin 111 and are not exposed on the surface of the polishing layer (see (a) in FIG. 1A). On the other hand, when the polishing layer is brought into contact with an alkaline polishing liquid, the hydrolysis of the hydrolyzable resin 111 is promoted, causing it to disintegrate, and parts of the tips of the abrasive grains 112 are exposed on the surface of the polishing layer (see (b) in FIG. 1A). When the polishing layer is brought into contact with an even stronger alkaline polishing liquid, the hydrolysis of the hydrolyzable resin 111 progresses further, causing the tips of the abrasive grains 112 to protrude even higher (see (c) in FIG. 1A).

[0015] Thus, as the pH of the polishing liquid increases, the proportion of abrasive grains 112 that protrude higher from the surface of the polishing layer increases (see FIG. 1A). As a result, as the pH of the polishing liquid increases, the protruding height of the abrasive grains on the polishing layer increases, and the polishing rate also increases (see FIG. 1B). In other words, simply by changing the pH of the polishing liquid and, therefore, the concentration of the alkaline substance as a hydrolysis promoter, it is possible to adjust the polishing rate and the surface roughness of the workpiece, so that a single polishing pad can be used for everything from rough polishing to precision mechanical polishing.

[0016] That is, a method for polishing a workpiece according to one embodiment of the present invention includes a step of polishing the workpiece by supplying a polishing liquid containing water to the surface of a polishing pad having a polishing layer containing a hydrolyzable resin and abrasive grains, while sliding the polishing pad and the workpiece relative to each other, and polishing the workpiece. In this step, the polishing process is performed while gradually reducing the protruding height of the abrasive grains by decreasing the concentration of the hydrolysis accelerator in the polishing liquid.

[0017] Hereinafter, the polishing pad used in the method for polishing an object to be polished will be described, and then the method for polishing an object to be polished will be described.

[0018] 1. Polishing Pad Figure 2A is a schematic plan view of a polishing pad 100 according to one embodiment of the present invention, and Figure 2B is a schematic cross-sectional view of the polishing pad 100 of Figure 2A taken along line 2B-2B.

[0019] The polishing pad 100 according to this embodiment includes a polishing layer 110 containing a hydrolyzable resin and abrasive grains (see FIG. 2B). The polishing layer 110 includes a hydrolyzable resin 111 and abrasive grains 112 fixed by the hydrolyzable resin 111. In this embodiment, grooves 110A are arranged on the surface of the polishing layer 110, forming an uneven pattern. While FIG. 2 shows an example in which the polishing pad 100 is made up of the polishing layer 110, the present invention is not limited to this, and the polishing pad 100 may further include other layers.

[0020] 1-1. Abrasive Layer The abrasive layer contains a composition containing a hydrolyzable resin and abrasive grains.

[0021] 1-1-1. Hydrolyzable Resin The hydrolyzable resin is not particularly limited as long as it is a resin that exhibits hydrolysis. Hydrolyzable resins include resins that are decomposed by microorganisms as well as resins that are decomposed by hydrolysis not involving microorganisms.

[0022] The hydrolyzable resin includes polyester having ester bond in the main chain, polycarbonate having carbonate bond in the main chain, etc. Examples of the hydrolyzable resin include lactic acid polymer, glycolic acid polymer, hydroxybutyric acid polymer, hydroxyvaleric acid polymer, caprolactone polymer, ethylene succinate polymer, butylene succinate polymer (such as polybutylene succinate, polybutylene succinate adipate, polybutylene succinate terephthalate, polyethylene succinate, polybutylene succinate carbonate, etc.), dioxanone polymer, trimethylene carbonate polymer, etc. Among these, lactic acid polymer and glycolic acid polymer are preferred, and glycolic acid polymer is preferred from the viewpoint of having higher strength and hydrolysis rate and being easier to adjust the protruding height of the abrasive grains of the polishing layer. That is, the hydrolyzable resin preferably contains glycolic acid polymer as the main component. "Containing a glycolic acid polymer as a main component" means that the content of glycolic acid polymer relative to the total amount of hydrolyzable resin is 50% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0023] Glycolic acid polymers are made up of structural units derived from glycolic acid (-(-O-CH 2 The glycolic acid polymer is a polymer containing a structural unit derived from glycolic acid, and is a polymer containing a structural unit derived from glycolic acid as a main component. The glycolic acid polymer may be a homopolymer of glycolic acid or a copolymer of glycolic acid and a monomer copolymerizable therewith.

[0024] Examples of copolymerizable monomers include: glycols such as ethylene glycol, propylene glycol, butanediol, heptanediol, hexanediol, octanediol, nonanediol, decanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, bisphenol A, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; dicarboxylic acids such as oxalic acid, adipic acid, sebacic acid, azelaic acid, dodecanedioic acid, malonic acid, glutaric acid, cyclohexanedicarboxylic acid, terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, bis(p-carboxyphenyl)methane, anthracenedicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, 5-sodium sulfoisophthalic acid, and 5-tetrabutylphosphonium isophthalic acid; hydroxycarboxylic acids such as lactic acid, hydroxypropionic acid, hydroxybutyric acid, hydroxyvaleric acid, hydroxycaproic acid, and hydroxybenzoic acid; lactides; Lactones such as caprolactone, valerolactone, propiolactone, undecalactone, and 1,5-oxepan-2-one; and carbonates such as trimethylene carbonate.

[0025] The term "mainly composed of glycolic acid-derived structural units" means that the content of glycolic acid-derived structural units is 50% by mass or more relative to the total amount of structural units constituting the glycolic acid polymer.The content of glycolic acid-derived structural units is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more.When the content of the structural units constituting the glycolic acid polymer is 50% by mass or more, the strength of the glycolic acid polymer can be increased, so that sufficient strength can be obtained when used in a polishing pad.In addition, when the content of the structural units constituting the glycolic acid polymer is 70% by mass or more, hydrolysis is more likely to proceed, making it easier to adjust the protruding height of the abrasive grains in the polishing layer.

[0026] Among these, from the viewpoint of having higher strength and hydrolysis rate, the glycolic acid polymer is preferably a homopolymer of glycolic acid.

[0027] The weight-average molecular weight of the hydrolyzable resin is not particularly limited, but is preferably 70,000 or more and 500,000 or less. When the weight-average molecular weight of the hydrolyzable resin is 70,000 or more, the strength of the hydrolyzable resin is higher, thereby further improving the retention and durability of abrasive grains. In addition, sufficient strength is obtained for handling, such as when removing the polishing pad from the mold during molding or when attaching the polishing pad to the platen of a polishing device. When the weight-average molecular weight of the hydrolyzable resin is 500,000 or less, not only can moldability be further maintained, but the time until disintegration due to hydrolysis can also be shortened. From the same viewpoint, the weight-average molecular weight of the hydrolyzable resin is more preferably 90,000 or more and 400,000 or less, even more preferably 100,000 or more and 350,000 or less, and particularly preferably 110,000 or more and 300,000 or less.

[0028] The weight-average molecular weight of the hydrolyzable resin can be measured by gel permeation chromatography (GPC). The measurement conditions can be as follows: (Measurement conditions) Apparatus: "Shodex-104" manufactured by Showa Denko Column: Two HFIP-606M columns connected in series with one HFIP-G column as a pre-column Column temperature: 40°C Eluent: HFIP solution containing 5 mM sodium trifluoroacetate Flow rate: 0.6 mL / min Detector: RI (differential refractive index) detector Molecular weight calibration: Five types of standard polymethyl methacrylate with different molecular weights

[0029] The content of the hydrolyzable resin is preferably 20% by mass or more and 90% by mass or less, more preferably 30% by mass or more and 80% by mass or less, even more preferably 40% by mass or more and 70% by mass or less, and particularly preferably 43% by mass or more and 52% by mass or less, relative to the total amount of the polishing layer (or the total amount of the above composition).If the content of the hydrolyzable resin is less than 20% by mass, the strength of the polishing layer containing abrasive grains will be weakened, which is not preferred.If the content of the hydrolyzable resin is more than 90% by mass, the proportion of abrasive grains will be reduced, which is not preferred, and the polishing speed will be slow.When the content of the hydrolyzable resin is above the above content, the proportion of hydrolyzable resin that collapses due to hydrolysis will be greater than a predetermined amount, so that it is easier to adjust the protruding height of the abrasive grains in the polishing layer while suppressing excessive collapse of the polishing layer.

[0030] 1-1-2. Abrasive Grains The material of the abrasive grains is not particularly limited, and examples thereof include diamond, silicon carbide, boron carbide, boron nitride, silicon nitride, cerium oxide, aluminum oxide, zirconium oxide, silicon oxide, iron oxide, manganese oxide, magnesium oxide, calcium oxide, barium oxide, zinc oxide, titanium oxide, chromium oxide, barium carbonate, and calcium carbonate. Among these, diamond, boron carbide, and boron nitride are preferred from the viewpoint of further increasing the polishing rate, and diamond is more preferred from the viewpoint of facilitating processing of high-hardness substrates such as SiC substrates.

[0031] The median diameter of the abrasive grains varies depending on the desired degree of polishing, but is preferably 2 μm or more and 50 μm or less, more preferably 3 μm or more and 40 μm or less, even more preferably 5 μm or more and 20 μm or less, and particularly preferably 6 μm or more and 15 μm or less.

[0032] The median diameter of the abrasive grains can be determined from the particle size distribution measured in accordance with particle size analysis - laser diffraction and scattering method (ISO 13320:2020). Specifically, it can be measured using a laser diffraction particle size analyzer (e.g., Malvern Mastersizer 3000) at a measurement temperature of 21°C, using ion-exchanged water as the dispersion medium, with a refractive index of 1.330, and using the Mie theory as the light scattering model.

[0033] The average particle size of the abrasive grains may be, for example, 1 nm or more and 1 mm or less. The average particle size of the abrasive grains can be measured in the same manner as above.

[0034] The content of the abrasive grains is not particularly limited, but is preferably 10% by mass or more and 80% by mass or less relative to the polishing layer (or the total amount of the composition). When the content of the abrasive grains is 10% by mass or more, the polishing rate can be further increased. When the content of the abrasive grains is 80% by mass or less, the formability or processability into a polishing pad can be further improved. From the same viewpoint, the content of the abrasive grains is more preferably 20% by mass or more and 70% by mass or less relative to the polishing layer (or the total amount of the composition), even more preferably 30% by mass or more and 60% by mass or less, and particularly preferably 48% by mass or more and 57% by mass or less.

[0035] The content of abrasive grains can be measured by thermogravimetric analysis (TGA).Specifically, on the surface of the polishing layer of unused polishing pad, when any straight line passing through the center O of the polishing layer is designated as line L, and the straight line passing through the center O of the polishing layer perpendicular to line L is designated as line M, the center O of the polishing layer, the midpoint between the center O of the polishing layer and the end of the polishing layer on line L are designated as a1 and a2, and the midpoint between the center O of the polishing layer and the end of the polishing layer on line M are designated as b1 and b2, then, from the range including the measurement points of O, a1, a2, b1 and b2, 100 mg or more of measurement samples are taken from the polishing layer, and suitably pulverized, and used as the measurement samples from each measurement point.20±2 mg of measurement sample is placed in a platinum pan, and in an air atmosphere, it is heated from room temperature to 800 ° C at a rate of 10 ° C / min, and kept at 800 ° C for 30 minutes, and components other than abrasive grains are burned off, and the weight of remaining sample is divided by the mass of measurement sample to determine the content of abrasive grains in the polishing layer at each measurement point. In the present application, the arithmetic mean value of the abrasive grain content at each of the five points was taken as the representative value of the abrasive grain content of the polishing layer.

[0036] 1-1-3. Other Components The composition may further contain other components in addition to the hydrolyzable resin and abrasive grains. Examples of other components include resins other than the hydrolyzable resin and hydrolysis accelerators. In particular, from the viewpoint of further increasing the polishing rate, it is preferable that the composition further contains a hydrolysis accelerator. One type of hydrolysis accelerator may be used alone, or two or more types may be used in combination.

[0037] The hydrolysis accelerator is a compound that accelerates the hydrolysis reaction of the hydrolyzable resin, and is preferably a compound that dissolves in the polishing solution to accelerate the penetration of the solution into the glycolic acid polymer, and more preferably a compound that generates an acid or alkali in the presence of water. Examples of such decomposition accelerators include carboxylic acid anhydrides, phosphorus compounds, cyclic esters, and basic metal oxides.

[0038] Examples of carboxylic acid anhydrides include hexanoic anhydride, octanoic anhydride, decanoic anhydride, lauric anhydride, myristic anhydride, palmitic anhydride, stearic anhydride, benzoic anhydride, succinic anhydride, maleic anhydride, phthalic anhydride, trimellitic anhydride, tetrahydrophthalic anhydride, butanetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, diphenylsulfonetetracarboxylic dianhydride, biphenyltetracarboxylic dianhydride, ethylene glycol bisanhydrotrimellitate, and glycerin bisanhydrotrimellitate monoacetate. Among these, phthalic anhydride, trimellitic anhydride, benzoic anhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, and benzene-1,2,4,5-tetracarboxylic anhydride (pyromellitic anhydride) are preferred.

[0039] The phosphorus compound is preferably an organic phosphorus compound such as a phosphate ester or a phosphite ester, and more preferably an organic phosphorus compound having at least one selected from the group consisting of a long-chain alkyl group having 8 to 24 carbon atoms, an aromatic ring, and a pentaerythritol skeleton.

[0040] Examples of phosphate esters having a long-chain alkyl group having 8 to 24 carbon atoms include mono- or di-stearyl acid phosphate or a mixture thereof, and di-2-ethylhexyl acid phosphate. Examples of phosphites having an aromatic ring include tris(nonylphenyl)phosphite. Examples of phosphites having a pentaerythritol skeleton include cyclic neopentanetetraylbis(2,6-di-tert-butyl-4-methylphenyl)phosphite, cyclic neopentanetetraylbis(2,4-di-tert-butylphenyl)phosphite, and cyclic neopentanetetraylbis(octadecyl)phosphite.

[0041] Examples of cyclic esters include glycolide, lactide, ε-caprolactone, γ-valerolactone, δ-valerolactone, diglycolic anhydride, and glutaric anhydride.

[0042] Examples of basic metal oxides include magnesium oxide, zinc oxide, calcium oxide, sodium oxide, and copper oxide.

[0043] Among these, cyclic esters are preferred, and glycolide is more preferred, from the viewpoint of being relatively stable during molding and further promoting the hydrolysis of the hydrolyzable resin in the polishing layer permeated with water.

[0044] The content of the hydrolysis accelerator is preferably 0.5% by mass or more and 50% by mass or less relative to the total amount of the hydrolyzable resin. When the content of the hydrolysis accelerator is 0.5% by mass or more, the hydrolysis of the hydrolyzable resin can be further accelerated, and the decrease in the polishing rate can be further reduced. When the content of the hydrolysis accelerator is 50% by mass or less, not only can the bleed-out of the hydrolysis accelerator be more unlikely to occur, but excessive collapse due to excessive hydrolysis can also be further suppressed. From the same viewpoint, the content of the hydrolysis accelerator is more preferably 1% by mass or more and 30% by mass or less, and even more preferably 10% by mass or more and 25% by mass or less.

[0045] The thickness of the polishing layer is not particularly limited, but when used for processing a substrate of a semiconductor device, for example, it is preferably 0.1 mm or more and 50 mm or less, more preferably 0.3 mm or more and 30 mm or less, even more preferably 0.4 mm or more and 10 mm or less, and particularly preferably 0.5 mm or more and 5 mm or less. A thickness of 0.1 mm or more is preferable from the viewpoint that the polishing layer can sufficiently hold abrasive grains.

[0046] 1-1-4. Physical Properties (Protruding Height of Abrasive Grains) The polishing degree of the polishing layer can be adjusted by the protruding height of the abrasive grains on the surface of the polishing layer. As described above, the protruding height of the abrasive grains can be adjusted by the concentration of the hydrolysis accelerator in the polishing liquid, preferably the pH. From the viewpoint of adjusting the polishing degree over a wider range, it is preferable that the change in the protruding height of the abrasive grains on the polishing layer relative to the change in the pH of the polishing liquid is large.

[0047] For example, when the height of the abrasive grains protruding from the surface of the polishing layer when polished with a polishing liquid having a pH of 13 is H1', ​​and the height of the abrasive grains protruding from the surface of the polishing layer when polished with a polishing liquid having a pH of 12 is H2', the ratio H2' / H1' is preferably 0.79 or less, and more preferably 0.44 or less. The polishing conditions can be the same as those in the examples described below.

[0048] The protruding height of the abrasive grains on the surface of the polishing layer can be determined using a laser microscope (for example, Keyence VK-X260). The center of the polishing pad is O, and the distance from the center O to the edge of the polishing pad (polishing layer) is 1. A circle with a radius of 0.6 is drawn from the center O, and the circumference of the circle is divided into 6 equal parts, with each of the 6 points on the circumference being used as measurement points. The arithmetic mean of the measurement points was used as a representative value of the protruding height of the abrasive grains on the surface of the polishing layer. The protruding height of the abrasive grains at each measurement point was determined by observing a field of view including each measurement point with a laser microscope having an observation magnification of 50 times and an objective lens N.A. = 0.95, and the protruding height of the abrasive grains observed within the same field of view was defined as Ha, and the protruding height of the nth abrasive grain in order of increasing height was defined as Ha(n). Next, when the height indication is set based on the apex of the protruding portion of the abrasive grain, and the height of the flat area (height of the binder resin) observed due to the difference in contrast nearest to Ha(n) is taken as Hb(n), the protruding height H(n) of the abrasive grain can be obtained by subtracting Hb(n) from Ha(n). The height H of the abrasive grain in this application is the arithmetic mean value of the heights of the abrasive grains for n = 1 to 5, and can be obtained by Equation 1.

[0049] The ratio H2' / H1' can be adjusted by the composition of the polishing layer, specifically, the type and amount of hydrolyzable resin and the type and amount of hydrolysis promoter contained in the polishing layer. For example, if the content of hydrolyzable resin, preferably glycolic acid polymer, is increased, the change in the height of protruding abrasive grains from the polishing layer surface when the pH is reduced from 13 to 12 is large, and therefore the ratio H2' / H1' tends to decrease.

[0050] (Thickness reduction rate) When a molded body of the composition (base material) excluding the abrasive grains is immersed in water at 60 ° C, the thickness reduction rate is preferably 12 μm / h or more. A polishing layer containing a composition having such a thickness reduction rate can more easily adjust the protruding height of the abrasive grains by changing the concentration of the hydrolysis accelerator in the polishing liquid. There is no particular limit to the upper limit of the thickness reduction rate, but from the viewpoint of extending the life of the polishing pad, it is preferably 2 mm / h or less, more preferably 1 mm / h or less, even more preferably 500 μm / h or less, and particularly preferably 100 μm / h or less.

[0051] The rate of thickness reduction can be measured by the following procedure. 1) The above composition containing no abrasive grains is injection molded to obtain a 10 mm x 10 mm x 120 mm prism, and a cubic test piece (molded body) with a side length of 10 mm is obtained from the prism. Molded bodies of the above composition containing no abrasive grains can also be obtained by heating and melting a molded body of a composition containing abrasive grains, i.e., the abrasive layer. The abrasive layer is heated and melted, and the resulting molten material is passed through a filter to separate the abrasive grains and the composition containing the other hydrolyzable resin, i.e., the composition not containing abrasive grains, and the abrasive-free composition is molded to produce a molded body, which can be used as a test piece. 2) Next, the test piece is placed in a 1 L autoclave, the autoclave is filled with water (deionized water) at 60°C, and the test piece is completely immersed at normal pressure. The above procedure is repeated to prepare immersion test pieces with different immersion times. Each immersion test piece is cut to expose the cross section. After drying, the thickness of the core (hard part) of the test piece is measured. The thickness reduction is measured from the difference with the thickness (10 mm) before immersion. 3) The time change in the thickness reduction of the test piece is determined based on the measured values ​​of the thickness reduction of the test piece measured after different immersion times. Then, the thickness reduction rate of the 10 mm test piece is calculated (unit: mm / h) from the time change in the thickness reduction of the test piece within the range where the time change in the thickness reduction of the test piece is linear.

[0052] The rate of thickness reduction can be adjusted by, for example, the type of binder resin and the type and content of the hydrolysis accelerator. For example, when the binder resin is a glycolic acid polymer, the rate of thickness reduction tends to be high. Furthermore, when the content of the hydrolysis accelerator is high, the rate of thickness reduction tends to be high.

[0053] (Tensile strength) The tensile strength of the composition excluding the abrasive grains at 25°C is preferably 55 MPa or more. A tensile strength of 55 MPa or more can further increase the retention of the abrasive grains. From the same viewpoint, the tensile strength is more preferably 60 MPa or more. There is no particular upper limit to the tensile strength, but it can be, for example, 1000 MPa or less. The tensile strength can be measured in accordance with ISO 527.

[0054] (Tensile modulus) The tensile modulus of the composition excluding the abrasive grains at 25°C is preferably 1 GPa or more. If the tensile modulus is 1 GPa or more, when the polishing pad is brought into contact with the workpiece and a load is applied, the abrasive grains protruding from the surface are less likely to be pushed back into the base material. This can further reduce the decrease in polishing rate. In addition, it can reduce the edge sagging of the workpiece after polishing (a phenomenon in which the edge is intensively scraped and the dimensional accuracy is reduced). From the same viewpoint, the tensile modulus is more preferably 3 GPa or more, and even more preferably 5 GPa or more. The upper limit of the tensile modulus is not particularly limited, but can be, for example, 50 GPa or less. The tensile modulus can be measured in accordance with ISO 527.

[0055] The tensile strength and tensile modulus of the composition excluding the abrasive grains can be adjusted by the type and molecular weight of the binder resin contained in the composition and the type and content of the hydrolysis accelerator. For example, if a glycolic acid polymer is used as the binder resin, the tensile strength tends to be high. Furthermore, if the content of the hydrolysis accelerator is low, the tensile strength tends to be high.

[0056] 1-1-5. Shape In this embodiment, as described above, grooves 110A may be formed as needed on the surface of polishing layer 110 (see FIGS. 1A and 1B). This allows the polishing liquid containing water to easily spread over the entire surface of polishing layer 110 via grooves 110A, and also allows shavings generated by hydrolysis of the hydrolyzable resin to be easily discharged to the outside through grooves 110A.

[0057] 1-2. Other Layers As described above, the polishing pad 100 may further include other layers as necessary. Examples of the other layers include a substrate layer and an adhesive layer. The substrate layer may be, for example, a resin film. The adhesive layer may be an adhesive layer for attaching the polishing pad 100 to a polishing platen (platen 210 described below).

[0058] 1-3. Manufacturing Method The polishing pad according to this embodiment can be manufactured by any method. For example, the polishing pad can be manufactured through the steps of 1) obtaining a composition containing a hydrolyzable resin and abrasive grains, and 2) molding the obtained composition.

[0059] In step 1), the composition can be obtained by kneading, for example, a hydrolyzable resin and abrasive grains. Examples of kneading machines that can be used include rolls, kneaders, Banbury mixers, and extruders (single-screw or multi-screw). Kneading is preferably performed under heating to improve processability.

[0060] In step 2), the obtained composition is molded into a predetermined shape. The molding method is not particularly limited, and may be, for example, any of injection molding, melt extrusion molding, solidification extrusion molding, and compression molding.

[0061] In this embodiment, grooves may be formed on the surface of the polishing layer obtained by molding. The grooves may be formed by cutting the surface of the molded product of the composition, or by molding the composition using a metal mold or die on which a pattern corresponding to the grooves is formed.

[0062] 2. Method for Polishing an Object to be Polished A method for polishing an object to be polished according to one embodiment of the present invention will now be described with reference to the drawings.

[0063] 3 is a schematic diagram showing a polishing apparatus 200 using the polishing pad 100 according to the present embodiment. Note that detailed illustration of the polishing pad 100 is omitted in FIG.

[0064] 3, polishing apparatus 200 includes polishing pad 100, a disc-shaped surface plate 210 that supports polishing pad 100, a disc-shaped polishing head 230 that holds workpiece 220, a weight 240, and a supply nozzle 250 that supplies polishing liquid W. Surface plate 210 is rotatable by a rotation shaft (not shown), and polishing head 230 is rotatable by a rotation shaft 230A.

[0065] In this embodiment, the polishing pad 100 and the object to be polished 220 are slid relative to each other while the polishing liquid W is supplied to the surface of the polishing layer of the polishing pad 100, thereby polishing the object to be polished 220.

[0066] Specifically, first, the polishing pad 100 is attached to the surface plate 210. Next, the workpiece 220 held by the polishing head 230 is pressed against the polishing surface of the polishing pad 100, and the surface plate 210 and / or the polishing head 230 are rotated while supplying the polishing liquid W from the supply nozzle 250. This causes the polishing pad 100 and the workpiece 220 to slide relative to each other, polishing the processed surface (surface to be polished) of the workpiece 220.

[0067] The type of the object to be polished 220 is not particularly limited, and examples thereof include materials for semiconductor devices and electronic components, particularly Si substrates, SiC substrates, GaAs substrates, glass, substrates for hard disks and LCDs (liquid crystal displays), etc. Among these, semiconductor wafers are preferred, and SiC substrates, sapphire substrates, or GaN substrates used in power devices are more preferred.

[0068] In this embodiment, the polishing solution W contains at least water and a hydrolysis accelerator. The same hydrolysis accelerators as those described above can be used. From the viewpoint of further increasing the hydrolysis rate of the hydrolyzable resin, the polishing solution W preferably contains an alkaline or acidic substance as the hydrolysis accelerator, with an alkaline substance being more preferred. In an aqueous solution containing an alkaline substance, carboxylic acid terminals generated by hydrolysis remain as carboxylate ions, and oligomers of the polymer generated by hydrolysis are likely to be eluted into the solution. Therefore, compared with acidic substances, alkaline substances can more effectively accelerate hydrolysis with a smaller amount of addition. Examples of alkaline substances include alkali metal hydroxides such as sodium hydroxide (NaOH) and potassium hydroxide (KOH), and organic alkalis such as tetramethylammonium hydroxide.

[0069] In this embodiment, from the viewpoint of performing rough polishing to precision mechanical polishing, the concentration of the hydrolysis promoter in the polishing liquid is gradually decreased, thereby gradually decreasing the protruding height of the abrasive grains in the polishing layer while polishing the workpiece 220 (see FIG. 1A).

[0070] That is, the process of polishing the workpiece 220 involves the following steps in order: a first step in which the workpiece 220 is polished while supplying a first polishing liquid (polishing liquid W) containing a hydrolysis promoter to the surface of the polishing layer; and a second step in which the workpiece 220 is polished while supplying a second polishing liquid (polishing liquid W) having a lower concentration of hydrolysis promoter than the first polishing liquid. The difference in concentration of the hydrolysis promoter between the first polishing liquid and the second polishing liquid depends on the type of hydrolysis promoter, but can be, for example, 1.5 to 1,000,000 times the concentration of the substance in the solution of the first polishing liquid relative to the second polishing liquid. As described above, since the hydrolysis promoter is preferably an alkaline substance, for example, the first step is preferably performed by polishing the workpiece 220 while supplying a first polishing liquid with a relatively high pH, ​​and the second step is preferably performed by polishing the workpiece 220 while supplying a second polishing liquid with a lower pH than the first polishing liquid.

[0071] In the first step, a first polishing liquid is supplied to adjust the height of protruding abrasive grains on the polishing layer surface to H1, and then the workpiece 220 is polished. In the second step, a second polishing liquid having a lower pH than the first polishing liquid is supplied to adjust the height of protruding abrasive grains on the polishing layer surface to H2, which is lower than H1, and then the workpiece 220 is polished. The heights H1 and H2 of protruding abrasive grains on the polishing layer surface can be measured by the method described above.

[0072] The pH of the first polishing liquid and the second polishing liquid may be set so as to achieve the desired height of abrasive grain protrusion on the surface of the polishing layer, and although this depends on the type of hydrolyzable resin, it is usually in the range of 1 to 14, preferably 7 to 14.

[0073] For example, glycolic acid polymers exhibit a high hydrolysis rate when the pH of the polishing liquid W is in the range of 9 or higher, preferably 12 or higher, and more preferably 13 or higher. Therefore, it is preferable that in the first step, the workpiece 220 is polished while supplying a first polishing liquid having a pH higher than 12, and then in the second step, the workpiece 220 is polished while supplying a second polishing liquid having a pH of 12 or lower.

[0074] The pH of the polishing liquid W is a value measured with a pH meter at 20° C. The pH of the polishing liquid W can be adjusted by the concentration (content) of the alkaline substance.

[0075] The temperature of the polishing liquid W is not particularly limited, but can be set to 1°C or higher and 60°C or lower.

[0076] (Function) In the above embodiment, as described above, a first polishing step is performed in which the workpiece 220 is polished in a state in which the protruding height of the polishing layer is relatively increased by supplying a first polishing liquid having a relatively high concentration of hydrolysis accelerator, and then a second polishing step is performed in which the workpiece 220 is polished in a state in which the protruding height of the polishing layer is relatively decreased by supplying a second polishing liquid having a relatively low concentration of hydrolysis accelerator. As a result, by simply changing the pH of the polishing liquid, it is possible to perform processes from rough polishing to precision mechanical polishing with a single polishing pad.

[0077] 3. Modifications In the above embodiment, a polishing pad having grooves arranged on the surface of the polishing layer is used, but this is not limiting, and a polishing pad having no grooves arranged on the surface of the polishing layer may also be used.

[0078] In the above embodiment, a polishing pad made of a polishing layer is used, but the present invention is not limited to this, and a polishing pad having a base layer and a polishing layer may be used. In this case, the polishing layer may be disposed uniformly over the entire base layer or may be disposed in a pattern.

[0079] Furthermore, in the above embodiment, an example was shown in which the process of polishing the object to be polished 220 includes at least the first and second processes, but if necessary, a further process of polishing the object to be polished 220 may be performed while supplying a polishing liquid having an even lower pH than the second polishing liquid.

[0080] The present disclosure will be described below with reference to examples, which should not be construed as limiting the scope of the present disclosure.

[0081] 1. Materials 1-1. Binder resins ・PGA-1 (homopolymer of glycolic acid, weight average molecular weight 298,000) ・PGA-2 (homopolymer of glycolic acid, weight average molecular weight 115,000) ・PPS (polyphenylene sulfide, weight average molecular weight 60,400)

[0082] The weight average molecular weight of each resin was measured by gel permeation chromatography (GPC).

[0083] (Weight average molecular weight of PGA) Apparatus: "Shodex-104" manufactured by Showa Denko K.K. Column: Two HFIP-606M columns connected in series with one HFIP-G column as a pre-column Column temperature: 40°C Eluent: HFIP solution containing 5 mM sodium trifluoroacetate Flow rate: 0.6 mL / min Detector: RI (differential refractive index) detector Molecular weight calibration: Five types of standard polymethyl methacrylate with different molecular weights

[0084] (Weight average molecular weight of PPS) Apparatus: Senshu Scientific High Temperature GPC SSC-7000 Column temperature: 210°C Eluent: 1-chloronaphthalene Flow rate: 0.7 mL / min Detector: UV detector (360 nm) Molecular weight calibration: 5 types of standard polystyrene with different molecular weights

[0085] 1-2. Abrasive grain: #800 GC fine grain abrasive (silicon carbide abrasive, manufactured by Naniwa Kenma Kogyo Co., Ltd.)

[0086] 1-3. Hydrolysis accelerator: glycolide: pyromellitic anhydride = 14:5 (weight ratio)

[0087] 2. Preparation and Evaluation of Polishing Pads 2-1. Preparation of Polishing Pads (Examples 1 to 3, Comparative Example 1) (1) Kneading Step The binder resin shown in Table 1 was weighed to 67% by volume (Examples 1 to 3: 50% by mass, Comparative Example 1: 46% by mass), and #800 GC fine abrasive (manufactured by Naniwa Abrasive Industries Co., Ltd.) was weighed to 33% by volume (Examples 1 to 3: 50% by mass, Comparative Example 1: 54% by mass), and kneaded using a Labo Plastomill (manufactured by Toyo Seiki Seisakusho Co., Ltd.) to obtain a composition. Kneading was performed at a predetermined heater temperature, with a preheating time of 1 minute, a kneading time of 5 minutes, and a rotation speed of 50 rpm. The heater temperature was set to 250 ° C. for PGA and 320 ° C. for PPS.

[0088] 4A to 4C are schematic cross-sectional views showing the molding process in the example. In the figures, reference numeral 301 denotes a ferroelectric plate, and 302 denotes an aluminum foil.

[0089] As shown in Figure 4, a 0.3 mm thick aluminum punched sheet 303 with 3 mm diameter through-holes spaced 5 mm apart was prepared. A 0.5 mm thick SUS mold 304 with 150 mm diameter holes was placed on the aluminum punched sheet 303 as shown in Figure 4, and the kneaded composition 305 was placed in the SUS mold 304 and press-molded to obtain a polishing pad 100 consisting of a 0.8 mm thick polishing layer with grooves on the surface, as shown in Figures 1A and 1B. The temperature of the press was set to the same temperature as the heater temperature of the Labo Plastomill.

[0090] 2-2. Evaluation Immediately after molding, the polishing pad had abrasive grains embedded in the resin, so it was sharpened with an #800 grindstone before a polishing test was carried out.

[0091] 3, the polishing test was performed by mounting a polishing pad on a polishing apparatus 200. Specifically, the polishing pad was attached to a surface plate 210 (polishing plate) using a double-sided adhesive film (e.g., AS ONE OCA50-A4). The double-sided adhesive sheet was attached using a rubber roller or the like to prevent air bubbles from being trapped when attached to the polishing pad and polishing plate.

[0092] Next, a 15 x 15 mm square Si substrate, which was the workpiece 220, was pressed against the rotating polishing pad to perform polishing. The polishing conditions were as follows. At this time, the load of the jig (polishing head 230) and weight 240 was applied to the substrate. (Polishing conditions) Polishing device: Dialap ML-150P (manufactured by Marutoh Co., Ltd.) Polishing disc rotation speed: 100 rpm Polishing disc diameter: 150 mm diameter Forced drive or oscillation of workpiece: None Surface pressure: 440 gf / cm 2 Polishing liquid flow rate: 100 mL / min. Polishing liquid: NaOH aqueous solution (20°C)

[0093] Polishing solutions were prepared by varying the concentration of NaOH to have pH values ​​of 13, 12, and 9. The pH was then changed in the order of 13, 12, and 9, and the polishing rate, protrusion height, and surface roughness of the workpiece at each pH were measured by the following methods.

[0094] (1) Polishing Rate The workpiece was attached to a jig with wax and polished. The thickness of the workpiece was measured with an electric micrometer, Millimar 1240 (manufactured by Mahr). The thickness of the workpiece was measured at five locations and the average value was used. The polishing rate was calculated from the polishing time (min) and the thickness reduction (removal amount, μm).

[0095] (2) Surface Roughness of the Polished Workpiece Using a laser microscope VK-X260 (manufactured by Keyence Corporation), the arithmetic mean height Sa (μm) of the surface of the Si substrate, which was the polished workpiece, after polishing for 1 hour was measured and used as the surface roughness. The measurement was performed using an objective lens with a magnification of 20 and an N.A. of 0.46.

[0096] (3) Protruding Height of Abrasive Grains For Example 1, Comparative Example 1, and Comparative Example 2, the polishing pads used for 60 minutes of polishing were removed from the polishing apparatus, and ion-exchanged water was poured over them three times to remove the polishing liquid and shavings from the surface. A paper towel was placed on the polishing pad to remove moisture, and then the pad was air-dried.

[0097] After drying, 3D data of the outermost surface of the polishing pad was obtained at the position of the convex portion of the polishing layer using a laser microscope VK-X260 (manufactured by Keyence Corporation). At this time, an objective lens with a magnification of 50x and an N.A. of 0.95 was used. Specifically, the center of the polishing pad was defined as O, and the distance from the center O to the edge of the polishing pad (polishing layer) was defined as 1. A circle with a radius of 0.6 was drawn from the center O, and the circumference of the circle was divided into 6 equal parts, with each of the 6 points on the circumference being used as measurement points. The arithmetic mean of the measurement points was used as a representative value of the protruding height of the abrasive grains on the surface of the polishing layer. The protruding height of the abrasive grains at each measurement point was determined by observing the field of view including each measurement point with a laser microscope with an objective lens N.A. of 0.95 at a magnification of 50x, and the protruding height of the abrasive grains observed within the same field of view was defined as Ha, and the protruding height of the nth abrasive grain in order of increasing height was defined as Ha(n). Next, when the height indication was set based on the apex of the protruding portion of the abrasive grain, and the height of the flat area (height of the binder resin) observed due to the difference in contrast nearest to Ha(n) was designated as Hb(n), the protruding height H(n) of the abrasive grain was calculated by subtracting Hb(n) from Ha(n). The height H of the abrasive grain was calculated as the arithmetic mean value of the heights of the abrasive grains for n = 1 to 5, and was calculated using the above-mentioned formula 1.

[0098] (4) Thickness Reduction Rate (Preparation of Test Pieces) A ​​composition was prepared in the same manner as in the kneading step, except that no abrasive grains were added to the composition obtained in the kneading step. A 10 mm x 10 mm x 120 mm square pillar was obtained from this resin composition, and a cubic test piece (molded body) with a side length of 10 mm was obtained from the square pillar.

[0099] (Immersion Test) The obtained test specimens were placed in a 1 L autoclave. The autoclave was then filled with water (deionized water) at 60°C or 80°C, and the test specimens were completely immersed at normal pressure to perform an immersion test. Test specimens with different immersion times were prepared by removing the test specimens after immersion at predetermined time intervals, and each test specimen was cut to expose its cross section. After leaving the specimens to dry overnight in a dry room, the thickness of the core (hard part) of each test specimen was measured. The thickness loss was measured from the difference with the thickness before immersion (initial thickness, specifically, 10 mm). The time-dependent change in the thickness loss of the test specimen was calculated based on the measured values ​​of the thickness loss of the test specimens measured for different immersion times. The thickness loss rate of a 10 mm thick test specimen was calculated (unit: mm / h) from the time-dependent change in the thickness loss of the test specimen within the range in which the time-dependent change in the thickness loss of the test specimen was linear.

[0100] (5) Tensile Strength The tensile strength of the composition prepared in (4) above was measured in accordance with ISO 527.

[0101] The evaluation results for Examples 1 to 3 and Comparative Example 1 are shown in Table 1. Note that Fig. 5A shows a graph of the pH dependence of the protrusion height of the abrasive grains for Example 1, and Fig. 5B shows a graph of the pH dependence of the protrusion height of the abrasive grains for Comparative Example 1. In Fig. 5A and Fig. 5B, each plot indicates the protrusion height of each abrasive grain at each pH.

[0102]

[0103] As shown in Table 1, in the polishing pad of Comparative Example 1, which uses non-hydrolyzable PPS as the binder resin, even when the pH of the polishing liquid is changed to 13, 12, or 9, the protruding height of the abrasive grains does not change significantly for any of the abrasive grains, indicating low pH dependency (see Figure 5B).

[0104] In contrast, in the polishing pads of Examples 1 to 3, which use hydrolyzable PGA as the binder resin, the proportion of abrasive grains with large protruding heights increases as the pH of the polishing liquid increases, indicating high pH dependency (see Figure 5A).

[0105] From these findings, it can be seen that in a polishing pad using a hydrolyzable resin as the binder resin, the surface roughness of the polishing layer can be changed by changing the pH of the polishing liquid.

[0106] This application claims priority based on Japanese Patent Application No. 2023-091782, filed June 2, 2023. The contents of the specification and drawings of that application are incorporated herein by reference in their entirety.

[0107] According to the present invention, it is possible to provide a method for polishing an object to be polished, which makes it possible to change the degree of polishing with one polishing pad and to improve processing efficiency.

[0108] REFERENCE SIGNS LIST 100 Polishing pad 110 Polishing layer 110A Groove 111 Hydrolyzable resin 112 Abrasive grains 200 Polishing device 210 Surface plate 220 Object to be polished 230 Polishing head 230A Rotating shaft 240 Weight 250 Supply nozzle 301 Ferro plate 302 Aluminum foil 303 Aluminum punching sheet 304 SUS mold 305 Composition

Claims

1. A method for polishing an object to be polished, comprising the steps of polishing the object to be polished by sliding the object to be polished against a polishing pad having a polishing layer containing a composition including a hydrolyzable resin and abrasive grains relative to one another, the step of polishing the object to be polished comprising: a first step of polishing the object to be polished while supplying a first polishing liquid containing a hydrolysis promoter that promotes hydrolysis to a surface of the polishing layer; and a second step of polishing the object to be polished while supplying, after the first step, a second polishing liquid having a lower concentration of hydrolysis promoter than the first polishing liquid to the surface of the polishing layer.

2. A method for polishing an object to be polished as described in claim 1, wherein in the first step, the object to be polished is polished in a state in which the height of protruding abrasive grains on the surface of the polishing layer is adjusted to H1 by supplying the first polishing liquid, and in the second step, the object to be polished is polished in a state in which the height of protruding abrasive grains on the surface of the polishing layer is adjusted to H2 lower than H1 by supplying the second polishing liquid.

3. The method for polishing an object to be polished according to claim 1 or 2, wherein the hydrolysis promoter is an alkaline substance.

4. The method for polishing an object to be polished according to any one of claims 1 to 3, wherein the hydrolyzable resin is mainly composed of a glycolic acid polymer.

5. A method for polishing an object to be polished according to any one of claims 1 to 4, wherein the pH of the first polishing liquid is higher than 12, and the pH of the second polishing liquid is 12 or less.

6. A polishing pad comprising an abrasive layer containing a composition including a hydrolyzable resin and an abrasive grain, wherein when the height of protruding abrasive grains from the surface of the polishing layer when polished with an abrasive liquid having a pH of 13 is H1', ​​and when the height of protruding abrasive grains from the surface of the polishing layer when polished with an abrasive liquid having a pH of 12 is H2', H2' / H1' is 0.79 or less.

7. The polishing pad according to claim 6, wherein the median diameter of the abrasive grains is 2 μm or more and 50 μm or less.

8. The polishing pad according to claim 6 or 7, wherein when a molded product of said composition excluding said abrasive grains is immersed in water at 60° C., the rate of thickness reduction is 12 μm / h or more.

9. The polishing pad according to any one of claims 6 to 8, wherein a molded body made of said composition excluding said abrasive grains has a tensile strength of 55 MPa or more.

Citation Information

Patent Citations

  • Polishing cloth, polishing apparatus and method for manufacturing semiconductor device

    JP2002190460A

  • Wafer surface treatment device