Dry electrode for secondary battery, secondary battery comprising same, and manufacturing method therefor

The introduction of a binder and plasticizer with a low melting point in the dry electrode manufacturing process for secondary batteries addresses issues of ductility and binding force, resulting in improved electrolyte impregnation and battery performance.

WO2024248192A1PCT designated stage expired Publication Date: 2024-12-05ENPLUS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/007667
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2023-06-05
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional dry processes for manufacturing secondary battery electrodes result in decreased ductility, low electrolyte impregnation, reduced binding force between active and conductive materials, and increased agglomeration, leading to poor performance and resistance issues.

Method used

A dry electrode manufacturing method involving a binding medium with a binder and plasticizer, where the plasticizer has a melting point of 200°C or lower, is used to create pores and maximize binder fiberization, improving dispersibility and binding power, and incorporating a dry process without solvents to enhance electrode performance.

Benefits of technology

The method increases electrolyte impregnability, improves activation speed, and enhances charging and discharging capacity, lifespan, and resistance reduction effects in secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023007667_05122024_PF_FP_ABST
    Figure KR2023007667_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a dry electrode for a secondary battery, a secondary battery comprising same, and a manufacturing method therefor, by which an electrode for a secondary battery having excellent performance can be manufactured even if a dry process in which a solvent is not used is applied in manufacturing the electrode for a secondary battery. The dry electrode for a secondary battery according to the present invention comprises: an electrode current collector; and an electrode layer positioned on the electrode current collector. In addition, the electrode layer comprises an electrode material comprising an active material, a conductive material, and a binding medium. In addition, the binding medium comprises a binder and a plasticizer, and the plasticizer may have a melting point of 200 ℃ or less. In addition, the electrode material is formed in a form in which a plurality of pores caused by the plasticizer are present in a region corresponding to the binding medium.
Need to check novelty before this filing date? Find Prior Art

Description

Dry electrode for secondary battery, secondary battery including same, and method for manufacturing same

[0001] The present invention relates to an electrode for a secondary battery, and more particularly, to a dry electrode for a secondary battery capable of manufacturing an electrode for a secondary battery with excellent performance even when a dry process that does not use a solvent is applied in manufacturing the electrode for a secondary battery, a secondary battery including the same, and a manufacturing method thereof.

[0002] Interest in energy storage technology is growing, and as the application of energy storage devices expands to areas such as mobile phones, laptops, and automobiles, research and development efforts in electrochemistry are increasing.

[0003] There is growing interest in energy storage, and among these, interest in the development of rechargeable secondary batteries is increasing.

[0004] In developing secondary batteries, active research and development is being conducted on new electrode and battery designs to improve capacity density and specific energy.

[0005] Secondary battery electrodes are manufactured by laminating an electrode layer formed by binding active materials and conductive agents with a binder onto a current collector. Specifically, a method commonly used is to apply a slurry containing electrode active materials, binders, and conductive agents onto a current collector, and then remove the solvent using heat or other means (i.e., a wet process).

[0006] However, this method of manufacturing electrodes using a wet process has the disadvantage of requiring the removal of solvents from the electrode slurry, which reduces economic feasibility and productivity and may cause environmental pollution problems.

[0007] To improve these shortcomings, a method for manufacturing electrodes without using electrode slurry (i.e., dry process) has been proposed.

[0008] The dry process is a technology for manufacturing an electrode film by mixing an active material, binder, and conductive material without a liquid medium such as a solvent or dispersion medium, and then passing the powder mixture through a rolling roll.

[0009] However, when electrodes for secondary batteries were manufactured using the conventional dry process, the following problems occurred. That is, according to the dry manufacturing process, as the density increased, the ductility decreased, the electrolyte impregnation property was low, which slowed down the activation speed of the battery, the fiberization of the binder was not sufficient, which lowered the bonding strength of the active material and the conductive material, and the decrease in the dispersibility of the binder caused a clumping phenomenon, which ultimately led to a decrease in the resistance reduction effect of the electrode and a decrease in the performance of the secondary battery.

[0010] For this reason, electrodes for secondary batteries produced using a dry process are attracting attention as next-generation electrodes because they do not use solvents. However, for their commercialization, electrode manufacturing technology that can improve or eliminate the aforementioned problems is needed.

[0011] The present invention is intended to solve the above problems, and an object of the present invention is to provide a dry electrode for a secondary battery, which can solve the problems of electrodes according to a conventional dry process even when the electrode is manufactured by a dry process that does not use a solvent, a secondary battery including the same, and a manufacturing method thereof.

[0012] Here, the problems of the electrode according to the conventional dry process are that as the density increases, the ductility decreases, the electrolyte impregnation property is low, which reduces the activation speed of the battery, the fiberization of the binder is not sufficient, which reduces the bonding force between the active material and the conductive material, and the clumping phenomenon occurs due to the decrease in the dispersibility of the binder, which reduces the resistance reduction effect of the electrode and the performance of the secondary battery.

[0013] A dry electrode for a secondary battery according to the present invention for achieving the above purpose comprises: an electrode current collector; and an electrode layer positioned on the electrode current collector.

[0014] And, the electrode layer includes an electrode material including an active material, a conductive material, and a binding medium.

[0015] And, the binding medium includes a binder and a plasticizer, and the plasticizer may have a melting point of 200°C or lower.

[0016] And, the electrode material is formed in a form in which a plurality of pores induced by the plasticizer exist in a region corresponding to the binding medium.

[0017] A method for manufacturing a dry electrode for a secondary battery according to the present invention is a method for manufacturing an electrode for a secondary battery using a dry process, comprising: a first step of manufacturing an electrode composition by stirring a mixture including an active material, a conductive material, and a binding medium; a second step of forming an electrode material by applying pressure to the electrode composition; and a third step of manufacturing an electrode for a secondary battery by attaching the electrode material to an electrode current collector.

[0018] And, the binding medium includes a binder and a plasticizer, and the plasticizer having a melting point of 200°C or lower can be used.

[0019] And, the electrode material of the second step is formed in a form in which a plurality of pores induced by the plasticizer exist in a region corresponding to the binding medium.

[0020] According to the dry electrode for a secondary battery and the method for manufacturing the same according to the present invention, the contact angle of the electrode can be lowered, and the impregnation property of the electrolyte can be increased, thereby improving the activation speed of the battery.

[0021] In addition, since the fiberization of the binder can be maximized compared to the conventional dry process, the bonding power of conductive materials can be further improved, the dispersibility of the binder can be improved, so that the clumping phenomenon of the binder itself can be suppressed, and the ductility of the electrode can be increased.

[0022] Accordingly, a secondary battery having a dry electrode for a secondary battery according to the present invention can have improved charge and discharge capacity, life characteristics, and resistance reduction effect.

[0023] Figure 1 is a flowchart of a method for manufacturing a dry electrode for a secondary battery according to the present invention.

[0024] Figure 2 is a scanning electron microscope (SEM) analysis photograph of a region including a binding medium region and pores in a dry electrode for a secondary battery according to the present invention.

[0025] Figure 3 is a scanning electron microscope (SEM) analysis photograph of a dry electrode manufactured according to Comparative Example 1.

[0026] Figure 4 is a scanning electron microscope (SEM) analysis photograph of a dry electrode manufactured according to Example 1 of the present invention.

[0027] Figure 5 shows the contact angle test results of a dry electrode manufactured according to Comparative Example 1.

[0028] Figure 6 shows the contact angle test results of a dry electrode manufactured according to Example 1 of the present invention.

[0029] Figure 7 is a graph showing the results of initial charge and discharge capacity tests of dry electrodes manufactured according to Example 1 and Comparative Examples 2, 3, and 4.

[0030] Figure 8 is a graph showing the results of a life characteristic test of dry electrodes manufactured according to Example 1 and Comparative Examples 2, 3, and 4.

[0031] Figure 9 is a graph showing the results of resistance characteristic tests of dry electrodes manufactured according to Example 1 and Comparative Examples 2, 3, and 4.

[0032] [Explanation of symbols]

[0033] AM: Active material F1: Fibrosis

[0034] P1: Pore C1: Clumping of binder

[0035] K1: Area corresponding to the binding medium

[0036] The terminology used herein is merely used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this specification, it should be understood that the terms "comprises" or "has" indicate the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but do not exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0037] In addition, in this specification, "on or above" means located above or below the target part, but does not necessarily mean located above the direction of gravity. That is, "on or above" as referred to in this specification includes not only cases where it is located above or below the target part, but also cases where it is located in front of or behind the target part.

[0038] Additionally, when a part, such as a region, plate, etc., is said to be "on or above" another part, this includes not only cases where it is in contact with or spaced apart from the other part "directly on or above" the other part, but also cases where there is another part in between.

[0039] Additionally, in this specification, when a component is referred to as being “connected” or “connected” to another component, it should be understood that the component may be directly connected or connected to the other component, but may also be connected or connected via another component in between, unless there is a specific description to the contrary.

[0040] Additionally, in this specification, terms such as first, second, etc. may be used to describe various components, but the components should not be limited by the terms. The terms are used only for the purpose of distinguishing one component from another.

[0041] Hereinafter, various embodiments, advantages and features of the present invention will be described in detail with reference to the attached drawings.

[0042] FIG. 1 is a flow chart of a method for manufacturing a dry electrode for a secondary battery according to the present invention, and FIG. 2 is a scanning electron microscope (SEM) analysis photograph of a region including a binding medium region and pores in a dry electrode for a secondary battery according to the present invention.

[0043] A dry electrode for a secondary battery according to the present invention includes an electrode current collector and an electrode layer positioned on the electrode current collector, and the electrode layer includes an electrode material formed by dry mixing an active material, a conductive material, and a binding medium.

[0044] The electrode current collector is a substrate that facilitates electron flow and evenly distributes electrons, and can be formed in the form of a foil or thin plate.

[0045] According to one example of the present invention, the collector can be formed to have a tensile strength of 5 kgf / cm2 or more and 45 kgf / cm2 or less.

[0046] And, the surface friction coefficient of the entire body can be formed to have a static friction coefficient of 0.1 or more and 0.85 or less, and a kinetic friction coefficient of 0.2 or more and 0.85 or less.

[0047] According to one example of the present invention, the current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and may be formed of, for example, copper, aluminum, stainless steel, nickel, titanium, calcined carbon, etc., or may be formed of copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., or an aluminum-cadmium alloy, etc.

[0048] According to one embodiment, the negative current collector may be formed of copper foil, and the positive current collector may be formed of aluminum foil, and in the above case, the negative current collector may be formed to have a thickness of 15 to 25 μm.

[0049] The electrode layer is formed by including an electrode material, and the electrode material can be formed by applying external force and pressure to an electrode composition in which an active material, a conductive material, and a binding medium are mixed.

[0050] In one embodiment, the electrode material may be formed in the form of a sheet or film. For example, the electrode material may be formed in the form of a free-standing film. In this case, an electrode layer may be formed by attaching the electrode material in the form of a sheet or film onto a current collector.

[0051] That is, the electrode layer can be formed by a lamination process after an electrode material in the form of a sheet or film is attached to an electrode current collector. For example, the electrode layer can be formed by first manufacturing the electrode material in the form of a free-standing film, and then attaching such a free-standing film to an electrode current collector and then using a lamination process.

[0052] Active materials are substances that react chemically to produce electrical energy when the battery discharges.

[0053] In one embodiment, the active material may be a cathode active material. In this case, the cathode active material may include at least one selected from lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMnO4, LiMnO2), lithium nickel oxide (LiNiO2), lithium iron phosphate (LiFePO4), lithium-excess oxide (Li2NiCoMnO2), lithium copper oxide (Li2CuO2), Ni-site type lithium nickel oxide, lithium manganese composite oxide, lithium manganese composite oxide having a spinel structure, and LiMn2O4 in which a part of the chemical formula Li is substituted with an alkaline earth metal ion.

[0054] In another embodiment, the active material may be a negative electrode active material. In this case, a known negative electrode active material for secondary batteries may be used as the negative electrode active material. For example, the negative electrode active material may be lithium metal, a lithium alloy, petroleum coke, activated carbon, graphite, silicon, tin, a metal oxide, or other carbon materials.

[0055] The content of the active material may be 85 to 98.9 wt% based on the total weight of the electrode composition of the present invention, but is not necessarily limited thereto. For example, the content of the active material may be 86 to 97.9 wt%, or 87 to 96.9 wt%.

[0056] Here, the 'electrode composition' refers to a composition that forms an electrode material attached to a current collector, in which an active material, a conductive material, and a binding medium are mixed in a dry manner.

[0057] According to one example of the present invention, the active material may have a span value of 0.2 to 1.5, as defined by the following mathematical expression 1.

[0058] Mathematical formula 1

[0059] Span Value = (D90 - D10) / D50

[0060] (In mathematical formula 1, D90, D10, and D50 represent particle sizes corresponding to 90%, 10%, and 50% of the maximum value in the cumulative distribution of solid particle sizes, respectively.)

[0061] A conductive material is used to provide conductivity to an electrode, and in the battery to be constructed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, carbon graphene, and carbon fiber; graphite such as natural graphite or artificial graphite; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskey such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used.

[0062] In the above case, the content of the conductive material may be 0.3 to 11 wt% based on the total weight of the electrode composition of the present invention, but is not necessarily limited thereto. For example, the content of the conductive material may be 0.4 to 10.5 wt%, 0.5 to 10 wt%, or 0.6 to 9.5 wt%.

[0063] Here, the 'electrode composition' refers to a composition that forms an electrode material attached to a current collector, in which an active material, a conductive material, and a binding medium are mixed in a dry manner.

[0064] Meanwhile, the secondary battery electrode according to the present invention corresponds to a dry electrode manufactured through a dry process that does not use a liquid solvent. However, the following problems have occurred when manufacturing secondary battery electrodes through conventional dry processes.

[0065] That is, according to the dry manufacturing process, as the density increases, the ductility decreases, the electrolyte impregnation property is low, which reduces the activation speed of the battery, the fiberization of the binder is not sufficient, which reduces the bonding force between the active material and the conductive material, and the clumping phenomenon occurs due to the decrease in the dispersibility of the binder, which ultimately leads to a decrease in the resistance reduction effect of the electrode and a decrease in the performance of the secondary battery.

[0066] The inventor of the present invention has confirmed that, when manufacturing an electrode for a secondary battery through such a dry process, the aforementioned problems can be improved or eliminated, especially when manufacturing an electrode material using a composition (hereinafter referred to as a "binding medium") further including a plasticizer that satisfies certain requirements.

[0067] The binding medium of the present invention includes a binder and a plasticizer.

[0068] The binder plays a role of improving the binding force of the conductive material and the adhesion force between the active material and the current collector. According to an example of the present invention, the binder may be polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof may be used.

[0069] In one embodiment, the binder may include polytetrafluoroethylene (PTFE). Polytetrafluoroethylene (PTFE) has the characteristic of fibers being pulled out of particles when an external force, including a shear force, is applied.

[0070] In the above case, when a strong external force including a shear force is applied to an electrode composition including polytetrafluoroethylene (PTFE) as a binder, fiberization (F1) of the polytetrafluoroethylene (PTFE) progresses, and the conductive material and active material particles can be physically bound by this fiberization (F1).

[0071] According to one embodiment, the "strong external force including a shear force" applied to the electrode composition may be applied by the rotational force of the blades or screw of the stirrer or mixer during the process of stirring the electrode composition. Here, the rotational speed of the stirrer or mixer may be at least 7,000 RPM, preferably at least 8,000 RPM; at least 9,000 RPM; or at least 10,000 RPM.

[0072] When forming an electrode material using the electrode composition described above, the plasticizer causes pores (P1) to be created in at least a region (K1) corresponding to the binding medium in the electrode material, thereby improving or eliminating the above-mentioned problems associated with the dry process.

[0073] Here, the above-mentioned “region corresponding to the binding medium (K1)” refers to a region where binder particles and plasticizer particles are formed into a plurality of granules and arranged adjacent to each other through steps S20 to S40 described below (see ‘K1’ in Fig. 2).

[0074] According to one example of the present invention, the content of the binding medium may be 0.3 to 11 wt%, preferably 0.6 to 8 wt%, and more preferably 0.9 to 5 wt%, based on the total weight of the electrode composition.

[0075] Here, the 'content of the binding medium' refers to the sum of the weight % of the binder and the plasticizer. And the 'electrode composition' refers to a composition that forms an electrode material attached to a current collector, in which an active material, a conductive material, and a binding medium are mixed in a dry manner.

[0076] When the content of the binding medium is less than 0.3 wt%, the bridging effect between particles within the electrode material may be insufficient, which may significantly reduce the tensile strength, and the physical properties of the binder may be significantly reduced, which may drastically reduce the bonding strength between the active material and the conductive material. Furthermore, when the content of the binding medium exceeds 11 wt%, the binder may act as resistance in the electrode, making it difficult to expect high output.

[0077] And, in the binding medium, the content of the plasticizer may be 5 to 20 parts by weight, preferably 6 to 17 parts by weight, and more preferably 7 to 14 parts by weight, per 100 parts by weight of the binder.

[0078] If the plasticizer content exceeds 20 parts by weight, the binder properties of the binding medium may deteriorate significantly, leading to a sharp decline in the bonding strength between the active material and the conductive material. Furthermore, if the plasticizer content is less than 5 parts by weight, the performance improvement effect due to the plasticizer is minimal.

[0079] Here, the above ‘performance improvement effect by plasticizer’ is as follows.

[0080] That is, by applying a dry process that does not use a liquid solvent, but adding a plasticizer to the composition for electrode manufacturing and manufacturing an electrode material through steps S20 to S40 described below, the problems of the conventional dry electrode can be improved, and accordingly, the resistance reduction effect of the electrode and the secondary battery performance (e.g., charge / discharge capacity, lifespan, etc.) can be improved.

[0081] Specifically, electrode materials produced through conventional dry processes exhibit hydrophobic properties. Conversely, the present invention enhances hydrophilic properties, thereby reducing the electrode contact angle and enhancing electrolyte impregnation, thereby improving battery activation speed. Furthermore, compared to conventional dry processes, binder fiberization can be maximized, thereby further enhancing the binding strength of conductive materials. Furthermore, the improved binder dispersibility can suppress the binder's own agglomeration.

[0082] According to one example of the present invention, the plasticizer may have a melting point of 200°C or less, preferably 185°C or less, more preferably 175°C or less, or 165°C or less.

[0083] In one embodiment, the plasticizer may include polycarboxylate ether (PCE). Using polycarboxylate ether as a plasticizer can increase the hydrophilicity of the electrode material, thereby lowering the contact angle of the electrode, and obtain high surface energy, thereby enabling strong interaction with the electrolyte and stably dispersing the binder.

[0084] For reference, the melting point of polycarboxylate ether (PCE) is 160 to 170°C.

[0085] According to one example of the present invention, the plasticizer may be mixed in a powder form, and the particle size of the plasticizer may be 1 to 30 ㎛ based on granulometry, preferably 5 to 25 ㎛, and more preferably 10 to 20 ㎛.

[0086] Meanwhile, upon completion of steps S20 to S40, which will be described later, the electrode material is prepared in a form in which a plurality of pores (P1) induced by a plasticizer exist in the aforementioned "region (K1) corresponding to the binding medium." In other words, the electrode material has a porous structure in which pores (P1) in the form of holes, grooves, or pores are formed in the region (K1) corresponding to the binding medium.

[0087] According to one example of the present invention, the pores (P1) generated in the region (K1) corresponding to the binding medium may have a size of 1 to 100 nm, but are not necessarily limited thereto. For example, the pores (P1) may have a size of 1 to 90 nm; 1 to 80 nm; 1 to 70 nm; 1 to 60 nm; 3 to 100 nm; 5 to 100 nm; 7 to 100 nm; 9 to 100 nm; 3 to 90 nm; 5 to 80 nm; or 5 to 60 nm.

[0088] According to one embodiment of the present invention, the density of the plasticizer may be lower than the density of the binder. For example, the density of the plasticizer may be 0.8 to 1.3 g / cc, and the density of the binder may be 2.00 to 2.3 g / cc.

[0089] Hereinafter, a method for manufacturing a dry electrode for a secondary battery described above will be described with reference to FIGS. 1 and 2.

[0090] (1) Mixture preparation step (S10)

[0091] The mixture preparation step (S10) is a step for preparing a material for manufacturing an electrode composition, and prepares a composition including an active material, a conductive material, and a binding medium. Here, the binding medium includes at least a binder and a plasticizer.

[0092] (2) Mixture stirring step (S20)

[0093] The mixture stirring step (S20) is a step for preparing an electrode composition by stirring a mixture containing an active material, a conductive material, and a binding medium. Here, details regarding the active material, the conductive material, and the binding medium are the same as those described above in the dry electrode section for secondary batteries.

[0094] According to one embodiment, the mixture stirring step (S20) can be performed using mixing equipment such as a powder mixer or a stirrer at, for example, 5,000 to 15,000 rpm for 10 to 30 minutes.

[0095] Meanwhile, the fiberization (F1) of the binder can proceed in this mixture stirring step (S20).

[0096] In addition, the "pores (P1) generated in at least the region (K1) corresponding to the binding medium" described in the dry electrode section for secondary batteries above can be induced by a plasticizer in the mixture stirring step (S20).

[0097] In the above case, an external force according to the stirring action of step S20 is applied to the binder and the plasticizer, and the action according to this external force may cause the fiberization (F1) of the binder to progress and the creation of pores (P1) by the plasticizer to occur.

[0098] According to one embodiment, the stirring action of step S20 may be an external force applied to the binder and plasticizer by rotation of the blades or screw of the mixing equipment.

[0099] According to one embodiment, the external force applied to the binder and plasticizer in the stirring operation of step S20 may include a shear force.

[0100] According to one embodiment, when a strong external force including a shear force is applied to a binding medium including a plasticizer, frictional heat is generated, causing the plasticizer to melt, and during the process of melting and then hardening again, pores (P1) may be formed by gas components or bubbles remaining inside.

[0101] Therefore, considering the temperature of this frictional heat, a plasticizer having a melting point of 200°C or lower, preferably 185°C or lower, more preferably 175°C or lower, or 165°C or lower can be used.

[0102] According to another embodiment, the pores (P1) and fiberization (F1) of the binder generated at least in the region (K1) corresponding to the binding medium may be induced in the extrusion step (S30) described below.

[0103] That is, in the extrusion step (S30), an external force (e.g., shear force) may be applied to the binding medium to induce the formation of pores (P1) and binder fiberization (F1).

[0104] According to one embodiment, the mixture stirring step (S20) may be configured to stir at 10,000 rpm for 20 minutes using a mixing device (Powder Mixer).

[0105] (3) Electrode composition extrusion step (S30)

[0106] The electrode composition extrusion step (S30) is a step in which the electrode composition of step S20 is extruded and fed into a rolling mill.

[0107] According to one embodiment, the extruder used in the extrusion step (S30) may be configured to perform milling by rotation, or mixing by blending, applying a shear force to the mixture (i.e., electrode composition) of step S20.

[0108] For example, the electrode composition extrusion step (S30) may be configured to extrude the electrode composition from a Twin Screw Type extruder having a maximum torque of 200 Nㆍm and an L / D ratio of 30 or more.

[0109] (4) Electrode composition rolling step (S40)

[0110] The electrode composition rolling step (S40) is a step of manufacturing an electrode material by applying pressure to the electrode composition that has gone through steps S20 and S30. Here, the 'pressure' may include a rolling force resulting from rolling.

[0111] According to one embodiment, the electrode material of step S40 may be formed in the form of a sheet or film. For example, the electrode material may be manufactured in the form of a free-standing film.

[0112] According to one embodiment, the electrode composition rolling step (S40) may be configured such that a mixture (i.e., electrode composition) is fed into an extruder having two pairs of 2-rolls each having a diameter of 100 mm formed at the bottom at a speed of 500 rpm and 2.5 g / sec in an 85°C atmosphere, and the mixture is extruded such that the shear force increases while rolling is performed by a preforming roll (roll diameter: 100 mm, roll temperature: 95°C, speed: 80 rpm, roll spacing: 300 μm).

[0113] (5) Dry electrode manufacturing step (S50)

[0114] The dry electrode manufacturing step (S50) is a step of manufacturing an electrode for a secondary battery by forming an electrode layer using the electrode material of step S40. The electrode material may be attached to a current collector or a pretreated current collector.

[0115] In one embodiment, the electrode material may be formed in the form of a sheet or film. For example, the electrode material may be formed in the form of a free-standing film. In this case, an electrode layer may be formed by attaching the electrode material in the form of a sheet or film onto a current collector.

[0116] That is, the electrode layer can be formed by a lamination process after an electrode material in the form of a sheet or film is attached to an electrode current collector. For example, the electrode layer can be formed by first manufacturing the electrode material in the form of a free-standing film, and then attaching such a free-standing film to an electrode current collector and then using a lamination process.

[0117] According to one embodiment, the dry electrode manufacturing step (S50) can manufacture a dry electrode having a thickness of about 200 μm including the current collector by repeatedly feeding the electrode material in the form of a sheet or film rolled in step S40 into a calendar roll (calendar temperature: 130°C) several times, while adjusting the gap between the rolls.

[0118] Meanwhile, the electrode for a secondary battery manufactured according to the manufacturing method described above may have a deviation in the contact angle of the electrode of 0.01° or more and 5.0° or less.

[0119] In addition, the dry electrode for a secondary battery manufactured according to the manufacturing method described above can be included in a secondary battery. In the above case, the dry electrode for a secondary battery of the present invention can be included in the positive electrode or negative electrode of the secondary battery.

[0120] According to one embodiment, the secondary battery of the present invention may include an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, and an electrolyte.

[0121] The separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator used in a known lithium secondary battery can be used without any special restrictions. In particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture retention capacity is preferable.

[0122] The electrolyte may be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, or a molten inorganic electrolyte that can be used in the manufacture of a lithium secondary battery, but is not necessarily limited thereto.

[0123] In one embodiment, the electrolyte may include an organic solvent and a lithium salt. Any organic solvent capable of acting as a medium through which ions involved in the electrochemical reaction of the battery can move may be used without particular limitation. The lithium salt may be used without particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery.

[0124] Hereinafter, the characteristics and performance improvement effects of secondary batteries according to the dry electrode for secondary batteries of the present invention will be described through the following examples and comparative examples. However, the following examples are only illustrative of the contents of the present invention, and the scope of the present invention is not limited by the examples.

[0125] [Comparative Example 1]

[0126] Comparative Example 1 produced a dry electrode using a binding medium that did not contain a plasticizer but only a binder.

[0127] Specifically, 97.0 g of LiNixCoyMnzO2 positive electrode active material, 1.5 g of carbon nanotube conductive material, and 1.5 g of polytetrafluoroethylene (PTFE) binder were added, stirred at 10,000 rpm for 20 minutes using a powder mixer, and then extruded using a twin screw type extruder with a maximum torque of 200 Nㆍm and an L / D ratio of 30 or more.

[0128] Then, the mixture (i.e., electrode composition) was fed into an extruder having two pairs of 2-rolls with a diameter of 100 mm formed at the bottom at a speed of 500 rpm and 2.5 g / sec in an 85°C atmosphere.

[0129] Then, as the mixture was extruded, the shear force increased and rolling was performed using a preforming roll (roll diameter: 100 mm, roll temperature: 95°C, speed: 80 rpm, roll gap: 300 μm).

[0130] Then, the rolled sheet was repeatedly fed into a calendar roll (calendar temperature: 130℃) 5 times as if it were a collector, and the gap between the rolls was adjusted, and finally, a dry electrode having a thickness of 200㎛ including the collector was manufactured.

[0131]

[0132] [Example 1]

[0133] Example 1 manufactures a dry electrode under the same process conditions as Comparative Example 1, but the difference is that the dry electrode is manufactured using a binding medium that includes a plasticizer in addition to a binder.

[0134] And, in Example 1, a dry electrode was manufactured with a plasticizer addition amount satisfying the content of the plasticizer suggested in the present invention.

[0135] Specifically, Example 1 produced a dry electrode having a thickness of 200 μm under the same process conditions as Comparative Example 1, except that 97.0 g of LiNixCoyMnzO2 positive electrode active material, 1.5 g of carbon nanotube conductive material, 1.35 g of polytetrafluoroethylene (PTFE) binder, and 0.15 g of polycarboxylate ether (PCE) plasticizer were added.

[0136]

[0137] [Comparative Example 2]

[0138] Comparative Example 2 manufactures a dry electrode under the same process conditions as Comparative Example 1, but the difference is that the dry electrode is manufactured using a binding medium that contains a plasticizer in addition to a binder.

[0139] However, in Comparative Example 2, a dry electrode was manufactured with a plasticizer content exceeding the amount of plasticizer presented in the present invention.

[0140] Specifically, Comparative Example 2 produced a dry electrode having a thickness of 200 μm under the same process conditions as Comparative Example 1, except that 97.0 g of LiNixCoyMnzO2 positive electrode active material, 1.5 g of carbon nanotube conductive material, 1.1 g of polytetrafluoroethylene (PTFE) binder, and 0.4 g of polycarboxylate ether (PCE) plasticizer were added.

[0141]

[0142] [Comparative Example 3]

[0143] Comparative Example 3 manufactures a dry electrode under the same process conditions as Comparative Example 1, but the difference is that the dry electrode is manufactured using a binding medium that contains a plasticizer in addition to a binder.

[0144] However, in Comparative Example 3, a dry electrode was manufactured with a plasticizer content exceeding the amount of plasticizer presented in the present invention.

[0145] Specifically, Comparative Example 3 produced a dry electrode having a thickness of 200 μm under the same process conditions as Comparative Example 1, except that 97.0 g of LiNixCoyMnzO2 positive electrode active material, 1.5 g of carbon nanotube conductive material, 0.75 g of polytetrafluoroethylene (PTFE) binder, and 0.75 g of polycarboxylate ether (PCE) plasticizer were added.

[0146] [Experimental Example 1]: Analysis of Fibrosis and Clumping

[0147] In order to observe the particle shape and surface of the dry electrodes manufactured in Comparative Example 1 and Example 2, a scanning electron microscope (SEM) was used, and the results are shown in FIGS. 3 and 4, respectively.

[0148] FIG. 3 is a scanning electron microscope (SEM) analysis photograph of a dry electrode manufactured according to Comparative Example 1, and FIG. 4 is a scanning electron microscope (SEM) analysis photograph of a dry electrode manufactured according to Example 1 of the present invention.

[0149] Referring to Fig. 3, it can be confirmed that the dry electrode manufactured according to Comparative Example 1 did not undergo sufficient fiberization and that a lot of binder clumping (C1) occurred.

[0150] On the other hand, referring to FIG. 4, it can be confirmed that the dry electrode manufactured according to Example 1 of the present invention exhibits excellent fiberization (F1) compared to Comparative Example 1, while no clumping of the binder occurs.

[0151]

[0152] [Experimental Example 2]: Contact Angle Analysis of Electrodes

[0153] The dry electrodes manufactured according to Comparative Example 1 and Example 2 were adjusted to a porosity of 20%, and each was sampled to a size of 5 cm x 5 cm, and 200 μl of distilled water was dropped at each corner and the center to check the contact angle. The test results are shown in Figs. 5 and 6, respectively.

[0154] Figure 5 shows the results of a contact angle test of a dry electrode manufactured according to Comparative Example 1, and Figure 6 shows the results of a contact angle test of a dry electrode manufactured according to Example 1 of the present invention.

[0155] Referring to FIGS. 5 and 6, it can be confirmed that the dry electrode manufactured according to Example 1 of the present invention has increased hydrophilicity and thus has a lower contact angle than that of Comparative Example 1.

[0156] Accordingly, the dry electrode according to Example 1 of the present invention can obtain high surface energy, so that it can strongly interact with the electrolyte and stably disperse the binder.

[0157]

[0158] [Experimental Example 3]: Battery charge / discharge performance test (Coin half cell test)

[0159] In order to measure the electrical characteristics of the dry electrodes manufactured according to Example 1 and Comparative Examples 1 to 3, CR2032 type coin cells were assembled and charge / discharge tests were performed at 2.8 V to 4.3 V at a current density of 0.1 C, and the test results are shown in Fig. 7 and Table 1 below.

[0160] [Table 1]

[0161]

[0162] Figure 7 is a graph showing the results of initial charge and discharge capacity tests of dry electrodes manufactured according to Example 1 and Comparative Examples 2, 3, and 4.

[0163] Referring to Table 1 and FIG. 7, it can be confirmed that the dry electrodes manufactured using a plasticizer (i.e., Example 1, Comparative Example 2, and Comparative Example 3) have superior charge and discharge capacities than the dry electrodes manufactured without using a plasticizer (i.e., Comparative Example 1).

[0164] Furthermore, when comparing a dry electrode manufactured using a plasticizer with a value satisfying the plasticizer content suggested in the present invention (i.e., Example 1) and a dry electrode manufactured with a value outside the plasticizer content suggested in the present invention (i.e., Comparative Examples 2 and 3), it can be confirmed that the dry electrode manufactured according to Example 1 of the present invention has the best charge and discharge capacity.

[0165] [Experimental Example 4]: Battery Life Characteristics Test

[0166] In order to measure the life characteristics of the dry electrodes manufactured according to Example 1 and Comparative Examples 1 to 3, the current density of 50 mA / g and the efficiency of 50 cycles were measured, and the test results are shown in Fig. 8.

[0167] Figure 8 is a graph showing the results of a life characteristic test of dry electrodes manufactured according to Example 1 and Comparative Examples 2, 3, and 4.

[0168] Referring to FIG. 8, it can be confirmed that the dry electrode manufactured according to Example 1 of the present invention has the best life characteristics.

[0169] Meanwhile, when examining the life characteristics of dry electrodes manufactured using a plasticizer, such as in Comparative Example 2 and Comparative Example 3, it can be confirmed that the life characteristics are lower than those of dry electrodes manufactured without using a plasticizer (i.e., Comparative Example 1).

[0170] That is, it can be seen that when a dry electrode (i.e., Comparative Examples 2 and 3) is manufactured with a value that deviates from the plasticizer content suggested in the present invention, the life characteristics may be worse than that of a dry electrode manufactured without using a plasticizer.

[0171]

[0172] [Experimental Example 5]: Test of electrode resistance characteristics

[0173] In order to confirm the resistance value of the dry electrodes manufactured according to Example 1 and Comparative Examples 1 to 3, AC impedance measurement was performed, and the test results are shown in Fig. 9.

[0174] Figure 9 is a graph showing the results of resistance characteristic tests of dry electrodes manufactured according to Example 1 and Comparative Examples 2, 3, and 4.

[0175] Referring to FIG. 9, it can be confirmed that the dry electrode manufactured according to Example 1 of the present invention has the best resistance characteristics.

[0176] Meanwhile, when examining the resistance characteristics of dry electrodes manufactured using a plasticizer, such as in Comparative Example 2 and Comparative Example 3, it can be confirmed that the resistance characteristics are worse than those of dry electrodes manufactured without using a plasticizer (i.e., Comparative Example 1).

[0177] That is, it can be seen that when a dry electrode (i.e., Comparative Examples 2 and 3) is manufactured with a value that deviates from the plasticizer content suggested in the present invention, the resistance characteristics may be worse than those of a dry electrode manufactured without using a plasticizer.

[0178]

[0179] While the preferred embodiments of the present invention have been described and illustrated using specific terminology, such terminology is solely for the purpose of clearly describing the present invention. It is to be understood that the embodiments of the present invention and the terminology described herein may be modified and altered in various ways without departing from the spirit and scope of the appended claims. Such modified embodiments should not be understood individually from the spirit and scope of the present invention, but should be considered to fall within the scope of the claims.

Claims

1. A method for manufacturing an electrode for a secondary battery using a dry process, A first step of preparing an electrode composition by stirring a mixture including an active material, a conductive material, and a binding medium; A second step of forming an electrode material by applying pressure to the electrode composition; and A third step of manufacturing an electrode for a secondary battery by attaching the electrode material to an electrode current collector is included. The above-mentioned bonding medium is, Containing binders and plasticizers, The above plasticizer is, The melting point is below 200℃, The electrode material of the second step is, A method for manufacturing a dry electrode for a secondary battery, characterized in that a plurality of pores caused by the plasticizer are formed in a region corresponding to the above-mentioned binding medium.

2. In paragraph 1, The above pores are, A method for manufacturing a dry electrode for a secondary battery, characterized in that an external force is applied to the binding medium by stirring or extruding the mixture.

3. In paragraph 1, The above binder, A method for manufacturing a dry electrode for a secondary battery, characterized in that an external force is applied to the binding medium by stirring or extruding the mixture, thereby causing fiberization.

4. In paragraph 2 or paragraph 3, A method for manufacturing a dry electrode for a secondary battery, characterized in that the external force includes a shear force.

5. In paragraph 1, The content of the above bonding medium is: 0.3 to 11 wt% based on the total weight of the above electrode composition, The content of the above plasticizer is, A method for manufacturing a dry electrode for a secondary battery, characterized in that the amount is 5 to 20 parts by weight based on 100 parts by weight of the binder.

6. In paragraph 1, A method for manufacturing a dry electrode for a secondary battery, characterized in that the pores have a size of 1 to 100 nm.

7. In paragraph 1, A method for manufacturing a dry electrode for a secondary battery, characterized in that the melting point of the plasticizer is 185°C or lower.

8. In paragraph 1, A method for manufacturing a dry electrode for a secondary battery, characterized in that the density of the plasticizer is smaller than the density of the binder.

9. In paragraph 1, A method for manufacturing a dry electrode for a secondary battery, characterized in that the plasticizer comprises polycarboxylate ether (PCE).

10. In paragraph 1, A method for manufacturing a dry electrode for a secondary battery, characterized in that the binder comprises polytetrafluoroethylene (PTFE).

11. In paragraph 1, Between the first step and the second step, A method for manufacturing a dry electrode for a secondary battery, characterized in that it further comprises a step of extruding the electrode composition.

12. In paragraph 1, The second step includes a step of forming the electrode material by rolling the electrode composition, A method for manufacturing a dry electrode for a secondary battery, characterized in that the pressure of the second step includes a rolling force.

13. In paragraph 1, A method for manufacturing a dry electrode for a secondary battery, characterized in that the electrode material is formed in the form of a sheet or film.

14. As a dry electrode for secondary batteries, An electrode current collector; and an electrode layer positioned on the electrode current collector, The above electrode layer is, An electrode material comprising an active material, a conductive material, and a binding medium, The above-mentioned bonding medium is, Containing binders and plasticizers, The above plasticizer is, The melting point is below 200℃, The above electrode material is, A dry electrode for a secondary battery, characterized in that it is formed in a form in which a plurality of pores caused by the plasticizer exist in an area corresponding to the above-mentioned bonding medium.

15. In paragraph 14, The content of the above bonding medium is: 0.3 to 11 wt% based on the total weight of the above electrode material, The content of the above plasticizer is, A dry electrode for a secondary battery, characterized in that the amount is 5 to 20 parts by weight based on 100 parts by weight of the binder.

16. In paragraph 14, A dry electrode for a secondary battery, characterized in that the pores have a size of 1 to 100 nm.

17. In paragraph 14, A dry electrode for a secondary battery, characterized in that the melting point of the plasticizer is 185°C or lower.

18. In paragraph 14, A dry electrode for a secondary battery, characterized in that the density of the plasticizer is smaller than the density of the binder.

19. In paragraph 14, A dry electrode for a secondary battery, characterized in that the plasticizer comprises polycarboxylate ether (PCE).

20. In paragraph 14, A dry electrode for a secondary battery, characterized in that the binder comprises polytetrafluoroethylene (PTFE).

21. In paragraph 14, A dry electrode for a secondary battery, characterized in that the active material comprises a lithium oxide system.

22. In paragraph 14, A dry electrode for a secondary battery, characterized in that the electrode material is in the form of a sheet or film.

23. In paragraph 14, A dry electrode for a secondary battery, characterized in that the deviation of the contact angle of the electrode is 0.01° or more and 5.0° or less.

24. In paragraph 14, A dry electrode for a secondary battery, characterized in that the above active material has a span value of 0.2 to 1.5, as defined by the following mathematical formula 1. Mathematical formula 1 Span Value = (D90 - D10) / D50 (In mathematical formula 1, D90, D10, and D50 represent particle sizes corresponding to 90%, 10%, and 50% of the maximum value in the cumulative distribution of solid particle sizes, respectively.) 25. As a secondary battery, A dry electrode for a secondary battery according to any one of claims 14 to 24; and A secondary battery characterized by including a separator interposed between the positive and negative electrodes of the secondary battery.

26. In paragraph 25, A secondary battery characterized in that the above dry electrode for a secondary battery is included in the positive or negative electrode of the secondary battery.

Citation Information

Patent Citations

  • Block Stacking Arrangement

    KR1020230130546A

  • Method, system and non-transitory computer-readable recording medium for discriminating main disease from sub disease based on machine learning

    KR1020240124769A

  • KR20220126129A

  • KR20230064383A

  • KR20230069002A