Method for preparing cathode active material for lithium secondary battery, cathode active material prepared using same, and lithium secondary battery comprising same
Patent Information
- Application Number
- PCT/KR2023/015842
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2023-10-13
- Publication Date
- 2024-12-05
Smart Images

Figure KR2023015842_05122024_PF_FP_ABST
Abstract
Description
Method for producing a cathode active material for a lithium secondary battery, cathode active material produced thereby, and lithium secondary battery comprising the same
[0001] The present invention relates to a method for producing a positive electrode active material for a lithium secondary battery, a positive electrode active material produced therefrom, and a lithium secondary battery including the same.
[0002]
[0003] Lithium secondary batteries produce electrical energy through oxidation and reduction reactions when lithium ions are inserted / deintercalated from the positive and negative electrodes, while an organic electrolyte or polymer electrolyte is charged between the positive and negative electrodes, which are made of active materials capable of intercalating and deintercalating lithium ions.
[0004] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMn2O4, etc.), and lithium iron phosphate compound (LiFePO4) have been used as cathode active materials for lithium secondary batteries. Among these, lithium cobalt oxide (LiCoO2) is widely used due to its high operating voltage and excellent capacity characteristics, and is applied as a cathode active material for high voltage. However, due to the rising price of cobalt (Co) and unstable supply, it is difficult to use it in large quantities as a power source in fields such as electric vehicles, and the need for the development of a cathode active material that can replace it has arisen.
[0005] Accordingly, nickel-cobalt-manganese lithium composite transition metal oxides (hereinafter simply referred to as 'NCM-based lithium composite transition metal oxides') in which some of the cobalt (Co) is replaced with nickel (Ni) and manganese (Mn) have been developed. However, the NCM-based lithium composite transition metal oxides developed previously are generally in the form of secondary particles in which primary particles are aggregated, and have a large specific surface area, low particle strength, and a high content of lithium byproducts, which causes problems such as large gas generation during cell operation and low stability.
[0006]
[0007] Accordingly, one object of the present invention is to provide a method for manufacturing a positive electrode active material for a lithium secondary battery having excellent particle strength, a positive electrode active material manufactured thereby, and a lithium secondary battery including the same.
[0008]
[0009] A method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment of the present invention may include the steps of: preparing a nickel-containing transition metal precursor; forming a mixture including the transition metal precursor and a lithium raw material and then firing the mixture to obtain a fired product; washing the obtained fired product and then separating the mixture to obtain a precipitate; and drying the precipitate to obtain a positive electrode active material. The step of drying the precipitate to obtain the positive electrode active material may be performed within a drying time of 2 hours.
[0010] The step of drying the above sediment to obtain a positive electrode active material can be performed at a temperature of 110°C to 130°C.
[0011] The step of drying the above sediment to obtain a positive electrode active material can be performed while stirring at a stirring speed of 1 rpm to 10 rpm.
[0012] The content of nickel in the above transition metal precursor may be 80 mol% or more based on the total mole number of transition metals.
[0013] The above lithium raw material is LiOH.
[0014] The step of forming a mixture containing the above transition metal precursor and lithium raw material and then calcining it to obtain a calcined product can be performed in an oxygen atmosphere.
[0015] In the step of forming a mixture containing the above transition metal precursor and lithium raw material and then firing it to obtain a sintered product, the above doping raw material can be further mixed.
[0016] The above doping raw material may include at least one selected from Al, Zr, B, Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, and Sr.
[0017] The positive electrode active material manufactured above may have a residual lithium content of less than 0.4 wt%.
[0018] The above-mentioned manufactured positive electrode active material may have an average particle diameter (D50) of 8 μm or more.
[0019] The above lithium transition metal oxide can be represented by the following chemical formula 1.
[0020] [Chemical Formula 1]
[0021] Li a Ni x Co y Mn z M1 k O2
[0022] (In the above chemical formula 1, 0.8 ≤ a ≤ 1.1, 0.6 ≤ x < 1.0, 0 ≤ y ≤ 0.1, 0 ≤ z ≤ 0.1, 0 ≤ k ≤ 0.1, x + y + z + k = 1,
[0023] M1 is one or more elements selected from Al, Zr, B, Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, and Sr.)
[0024] A positive electrode active material for a lithium secondary battery according to another embodiment of the present invention can be manufactured according to the manufacturing method of the positive electrode active material for a lithium secondary battery.
[0025] A positive electrode for a lithium secondary battery according to another embodiment of the present invention includes the positive electrode active material for a lithium secondary battery.
[0026] A lithium secondary battery according to another embodiment of the present invention includes the positive electrode for the lithium secondary battery.
[0027]
[0028] A method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment of the present invention can produce a positive electrode active material with excellent particle strength by controlling drying process conditions. Accordingly, the life characteristics and safety of the battery can be improved.
[0029]
[0030] Figure 1 is an SEM image according to Experimental Example 1.
[0031]
[0032] The terms first, second, and third, etc., are used to describe, but are not limited to, various parts, components, regions, layers, and / or sections. These terms are used only to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, a first part, component, region, layer, or section described below may be referred to as a second part, component, region, layer, or section without departing from the scope of the present invention.
[0033] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the present invention. As used herein, the singular forms "singular" and "comprising" include plural forms as well, unless the context clearly dictates otherwise. The word "comprising" as used herein specifies a particular feature, region, integer, step, operation, element, and / or component, but does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.
[0034] When a part is referred to as being "on" or "over" another part, it can be directly on or over the other part, or there may be other parts intervening. Conversely, when a part is referred to as being "directly on" another part, there are no other parts intervening.
[0035] Although not defined otherwise, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with the relevant technical literature and the present disclosure, and are not to be construed as ideal or overly formal unless otherwise defined.
[0036] Also, unless otherwise stated, % means weight%, and 1 ppm is 0.0001 weight%.
[0037] In this specification, the term "combination(s) thereof" described in the expression in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expression in the Makushi format, and means including any one or more selected from the group consisting of said components.
[0038] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.
[0039]
[0040] One embodiment of the present invention provides a method for producing a cathode active material for a lithium secondary battery, comprising the steps of: preparing a nickel-containing transition metal precursor; forming a mixture comprising the transition metal precursor and a lithium raw material and then firing the mixture to obtain a sintered product; washing the obtained sintered product and then separating the mixture to obtain a precipitate; and drying the precipitate to obtain a cathode active material, wherein the step of drying the precipitate to obtain the cathode active material is performed within a drying time of 2 hours.
[0041] A method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment of the present invention relates to a method for forming a lithium transition metal oxide in the form of secondary particles formed by agglomeration of a plurality of primary particles.
[0042] Active materials in the form of secondary particles have low particle strength. When manufacturing electrodes using positive electrode active materials containing secondary particles and then rolling them, particle breakage is severe, resulting in increased gas generation and reduced stability during battery operation. Therefore, enhancing particle strength to minimize particle breakage in positive electrode active materials in the form of secondary particles is necessary.
[0043] Accordingly, through repeated research, the inventors of the present invention have discovered a method for manufacturing a positive electrode active material capable of improving secondary particle strength, thereby completing the present invention. Hereinafter, a method for manufacturing a positive electrode active material according to one embodiment of the present invention will be described in detail, step by step.
[0044]
[0045] First, a nickel-containing transition metal precursor is prepared.
[0046] The above nickel-containing transition metal precursor may be a transition metal hydroxide.
[0047] The above transition metal hydroxide may be manufactured by, for example, adding a complexing agent-containing solution and a pH adjusting agent-containing solution to a transition metal-containing solution including a nickel raw material and optionally a cobalt raw material or a manganese raw material, and performing a co-precipitation reaction.
[0048] The above nickel raw material is not particularly limited as long as it is used in the art for manufacturing a positive electrode active material precursor. For example, the nickel raw material may be a nickel-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, may be NiSO4, NiSO4·6H2O, Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, fatty acid nickel salt, nickel halide, or a combination thereof, but is not limited thereto.
[0049] The above cobalt raw material is not particularly limited as long as it is used in the art for manufacturing a positive electrode active material precursor. For example, the cobalt raw material may be a cobalt-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, CoSO 4, It may be, but is not limited to, CoSO4ㆍ7H2O, Co(OH)2, CoOOH, Co(OCOCH3)2ㆍ4H2O, Co(NO3)2ㆍ6H2O or a combination thereof.
[0050] The manganese raw material is not particularly limited as long as it is used in the art for manufacturing a precursor of a cathode active material. For example, the manganese raw material may be a manganese-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof, and specifically, may be a manganese salt such as MnSO4, MnCO3, Mn(NO3)2, manganese acetate, manganese dicarboxylic acid salt, manganese citrate, and manganese fatty acid salt, manganese oxide such as Mn2O3, MnO2, and Mn3O4, oxyhydroxide, manganese chloride, or a combination thereof, but is not limited thereto.
[0051] The above transition metal-containing solution may be prepared by adding a nickel raw material and optionally a cobalt raw material or a manganese raw material to a solvent, specifically, water, or a mixture of water and an organic solvent (e.g., alcohol, etc.) that can be uniformly mixed with water.
[0052] The above complexing agent-containing solution performs the function of forming a complex, and may include, but is not limited to, NH3, NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, NH4CO3 or a combination thereof as the complexing agent. Meanwhile, the complexing agent-containing solution may be used in the form of an aqueous solution, and at this time, water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that can be uniformly mixed with water may be used as the solvent.
[0053] At this time, the content of nickel in the transition metal precursor may be 60 mol% or more based on the total mole number of transition metals, and specifically, may be 80 mol% or more. This is advantageous for increasing the capacity of the battery, so it is preferable to include a molar content of nickel of 80 mol% or more.
[0054] Additionally, the cobalt content in the transition metal precursor may be 11 mol% or less based on the total moles of the transition metal. Since the cobalt content is sufficiently low as described above, there is an advantage in that the manufacturing cost can be significantly reduced.
[0055]
[0056] Next, a mixture containing the above transition metal precursor and lithium raw material is formed and then calcined in an oxygen atmosphere to form a lithium transition metal oxide in the form of secondary particles.
[0057] The above lithium raw material is not particularly limited as long as it is commonly used in the art, but may be, for example, LiOH.
[0058] At this time, the mixture can be prepared so that the molar ratio (Li / Me) of lithium (Li) to the total metal (Me) excluding lithium is in the range of 1.0 to 1.1, or in the range of 1.01 to 1.08.
[0059]
[0060] In addition, at this time, the sintering is performed at a temperature of 650°C to 950°C, more specifically, 700 to 850°C, and even more specifically, 700 to 800°C. If the sintering temperature is too low, the primary inner crystal grain size may not grow sufficiently, which may deteriorate the particle strength, and the primary particle diameter may not grow sufficiently, which may lower the rolling density and deteriorate the electrode energy density. If the sintering temperature is too high, over-sintering may occur, which may deteriorate the electrochemical characteristics such as capacity and output. As long as the sintering temperature is within the above range, there is no particular limitation on the sintering temperature profile. That is, within the sintering temperature range within the above range, there may be a temperature-rising section, a temperature-falling section, or a constant temperature section. In addition, within the sintering temperature range within the above range, there may be a high-temperature sintering region and a low-temperature sintering region.
[0061] In addition, at this time, the firing time in the above temperature range is performed for 12 hours or more, and more specifically, it can be 12 to 24 hours. If the firing time is too short, the crystal grain size within the primary particles may not grow sufficiently, which may deteriorate the particle strength, and the particle diameter of the primary particles may not grow sufficiently, which may lower the rolling density and deteriorate the electrode energy density. However, if the firing temperature is too high, over-firing may occur, which may lower the electrochemical characteristics such as capacity and output.
[0062] The mixture including the above transition metal precursor and lithium raw material further includes a doping raw material, and the doping raw material M1 may include at least one selected from Al, Zr, B, Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La and Sr.
[0063] The content of the doping element in the above doping raw material may be in the range of 0.0005 mol to 0.04 mol or 0.001 mol to 0.03 mol, based on 1 mol of the total of the transition metal and doping element of the transition metal precursor.
[0064] Next, a step of washing and separating the obtained calcined material to obtain a precipitate can be performed.
[0065] As an example, the washing solution used in the washing process may be distilled water or an alkaline aqueous solution, but is not particularly limited thereto. In addition, as long as the sediment can be effectively separated after washing is completed, the method is not particularly limited.
[0066] The method for producing a positive electrode active material for a lithium secondary battery according to the present invention includes a step of drying the separated precipitate to obtain a positive electrode active material.
[0067] After loading the above-mentioned separated sediment into a dryer and stirring it with a stirrer at a predetermined speed, it can be dried for a period of less than 2 hours, and specifically, it can be dried for 30 minutes to 2 hours.
[0068] The above drying temperature may be in the range of 110°C to 130°C, and specifically in the range of 115°C to 125°C.
[0069] Additionally, the stirring speed of the stirrer may be 20 rpm or less, specifically 10 rpm or less, and more specifically in the range of 1 rpm to 10 rpm.
[0070] By stirring the above-mentioned sediment at the above-mentioned temperature and stirring speed range for the above-mentioned time, a positive electrode active material with improved particle strength can be manufactured.
[0071] If the drying time and drying temperature exceed the above range, the drying conditions are harsh, which can cause secondary particle breakage due to rapid evaporation of internal moisture. In addition, if the stirring speed exceeds the above stirring speed range, excessive external force may be applied to the positive electrode active material, which can cause particle breakage. On the other hand, if the drying temperature and stirring speed are below the above range, it takes an excessive amount of time to achieve the desired moisture content, which can lower the overall productivity.
[0072]
[0073] The above-mentioned manufactured positive electrode active material may have a surface residual lithium content of less than 0.4 wt% based on the total weight of the positive electrode active material. Accordingly, side reactions during the charge / discharge process of the battery can be reduced, and life characteristics and safety can be improved.
[0074] The above-mentioned manufactured positive electrode active material may have an average particle diameter (D50) of 8 μm or more. Since the average particle diameter of the positive electrode active material is sufficiently large, the rolling density can be improved, thereby improving the electrode energy density. In the present specification, the average particle diameter (D50) can be defined as a particle diameter corresponding to 50% of the volume accumulation amount in the particle diameter distribution curve. The above-mentioned average particle diameter (D50) can be measured using, for example, a laser diffraction method.
[0075]
[0076] The above lithium transition metal oxide can be more specifically represented by the following chemical formula 1.
[0077] [Chemical Formula 1]
[0078] Li a Ni x Co y Mn z M1k O2
[0079] In the above chemical formula 1, 0.8 ≤ a ≤ 1.2, 0.6 ≤ x < 1.0, 0 ≤ y ≤ 0.1, 0 ≤ z ≤ 0.1, 0 ≤ k ≤ 0.1, x + y + z + k = 1,
[0080] M1 is one or more elements selected from Al, Zr, B, Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, and Sr.
[0081] In the lithium transition metal oxide of the above chemical formula 1, lithium may be included in a content corresponding to a, that is, 0.8≤a≤1.2. If a is too small, the capacity may be reduced, and if a is too large, the strength of the sintered positive electrode active material may be increased, making pulverization difficult, and the amount of gas generated may increase due to an increase in lithium byproducts. Considering the effect of improving the capacity characteristics of the positive electrode active material according to the control of the lithium content and the sinterability balance during the production of the active material, the lithium may be included in a content of 0.9≤a≤1.1 more preferably.
[0082] In the lithium transition metal oxide of the above chemical formula 1, nickel may be included in an amount corresponding to x, that is, 0.6≤x<0.1, and specifically, 0.8≤a≤0.95. If the nickel content is too low, it may be difficult to achieve high capacity of the battery, and if the nickel content is too high, the battery life and thermal safety may be reduced due to a decrease in the structural stability of the active material, and the manufacturing cost may increase.
[0083] In the lithium transition metal oxide of the above chemical formula 1, cobalt may be included in an amount corresponding to y, i.e., 0≤y≤0.1 or 0.03≤y≤0.1. If the cobalt content is too low, it may be difficult to simultaneously achieve sufficient rate characteristics and high powder density of the active material. If the cobalt content is too high, the overall cost of the raw material may increase and the reversible capacity may decrease.
[0084] In the lithium transition metal oxide of the above chemical formula 1, manganese may be included in a content corresponding to z, that is, 0≤z≤0.1, and specifically, if the manganese content is too low, the production cost may increase and the stability of the active material may decrease. If the manganese content is too high, the capacity and output characteristics of the battery may decrease.
[0085] In the lithium transition metal oxide of the above chemical formula 1, M1 is a doping element and may include at least one selected from among Al, Zr, B, Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, and Sr.
[0086]
[0087] Another embodiment of the present invention provides a positive electrode active material for a lithium secondary battery manufactured according to the above-described manufacturing method.
[0088] The above-mentioned positive electrode active material is manufactured according to the manufacturing method described above, so that it can have excellent particle strength and a high degree of single particle formation.
[0089] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery comprising the positive electrode active material for a lithium secondary battery.
[0090] Specifically, the positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, and including the positive electrode active material described above.
[0091] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesion of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.
[0092] The above-described positive electrode active material layer may include a binder and / or a conductive material together with the above-described positive electrode active material.
[0093] At this time, the binder plays a role of improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one kind alone or a mixture of two or more kinds thereof may be used, but is not limited thereto. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.
[0094] And, the conductive material is used to provide conductivity to the electrode, and in the battery to be constructed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One type alone or a mixture of two or more types among these may be used, but the present invention is not limited thereto. The conductive material may typically be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.
[0095] The above positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the above positive electrode active material is used.
[0096] Specifically, the positive electrode can be manufactured by applying a composition for forming a positive electrode active material layer, including the positive electrode active material described above and optionally a binder, a conductive agent, or a solvent, on a positive electrode current collector, followed by drying and rolling. At this time, the types and contents of the positive electrode active material, binder, and conductive agent are as described above.
[0097] The solvent may be a solvent generally used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.
[0098] Alternatively, the positive electrode may be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the resulting film on a positive electrode current collector by peeling it off from the support.
[0099]
[0100] Another embodiment of the present invention provides a lithium secondary battery including a positive electrode for a lithium secondary battery.
[0101] The above lithium secondary battery may more specifically include a positive electrode; a negative electrode; a separator; and an electrolyte.
[0102] The above lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.
[0103] The above negative electrode may include a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.
[0104] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.
[0105] The negative electrode active material layer may optionally include a binder and a conductive material together with the negative electrode active material. As an example, the negative electrode active material layer may be manufactured by applying a composition for forming a negative electrode active material layer comprising the negative electrode active material and optionally a binder and a conductive material onto a negative electrode current collector and drying the composition, or by casting the negative electrode forming composition onto a separate support and then laminating the resulting film onto a negative electrode current collector by peeling the film off from the support.
[0106] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples thereof include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, and Al alloy; metallic oxides capable of doping and dedoping lithium, such as SiOβ (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.
[0107] The above binder and conductive material may be the same as those described above for the positive electrode.
[0108] The above separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used as a separator in lithium secondary batteries can be used without any particular restrictions. In particular, a separator having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.
[0109]
[0110] The above electrolyte may include, but is not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0111] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.
[0112] The organic solvent may be used without any particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched, or cyclic hydrocarbon group, and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a linear carbonate compound having low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.
[0113] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2. LiCl, LiI, or LiB(C2O4)2. It is preferable that the concentration of the lithium salt be used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.
[0114] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexamethylphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 wt% based on the total weight of the electrolyte.
[0115] As described above, a lithium secondary battery including a cathode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0116] Accordingly, another embodiment of the present invention provides a battery module including the lithium secondary battery as a unit cell and a battery pack including the same.
[0117] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0118] Hereinafter, embodiments of the present invention will be described in more detail through examples. However, the following examples are only preferred embodiments of the present invention, and the present invention is not limited to the following examples.
[0119]
[0120] (Example)
[0121] (1) Manufacturing of positive electrode active material
[0122] (Mixed) (Ni 0.89 Co 0.04 Mn 0.07 )(OH)2 was mixed with LiOH·H2O and Al(OH)3 as a precursor. At this time, the molar ratio of lithium (Li) to the total metal (Me) excluding lithium (Li / Me) was designed to be 1.06, and 0.02 mol of Al was added to be doped.
[0123] (After calcination), the mixture was placed in a calciner, heated to 770°C in an oxygen atmosphere, calcined for 14 hours while maintaining the temperature at 770°C, and then naturally cooled to produce a lithium transition metal oxide.
[0124] (Washing) The lithium transition metal oxide manufactured above was washed with distilled water and then the precipitate was separated.
[0125] (Drying) After placing the separated precipitate in a dryer, the temperature was raised to maintain a constant temperature, and the precipitate was dried while stirring with a stirrer to manufacture a positive electrode active material for a lithium secondary battery.
[0126] Drying temperature, time and stirring speed are shown in Table 1 below.
[0127] Drying temperature (℃) Drying time (min) Stirring speed (rpm) Residual lithium content (wt%) Daily positive electrode active material production (ton / day) Example 1 20 1 20 10 0.38 or less 28.8 Example 2 1 20 1 20 9 0.38 or less 28.8 Example 3 1 20 1 20 8 0.38 28.8 Comparative example 1 1 8 0 2 40 1 (120 min), 10 (120 min) 0.37 14.4 Comparative example 2 1 8 0 2 40 1 (120 min), 5 (120 min) 0.40 14.4 Comparative example 3 1 5 0 2 40 1 (120 min), 5 (120 min) 0.40 14.4 Comparative example 4 1 20 2 40 1 (120 min), 5 (120 min) 0.38 14.4
[0128] Experimental Example 1 - Measurement of Residual Lithium
[0129] For the positive electrode active materials manufactured according to the Examples and Comparative Examples, the residual lithium was measured using the T50 model of METTLER TOLEDO. The measurement results confirmed that the residual lithium content on the surface of the manufactured positive electrode active materials was less than 0.4 wt%.
[0130] Referring to Table 1 above, it can be confirmed that the production amount of positive electrode active materials according to the manufacturing method according to Examples 1 to 3 is 28.8 tons / day, which is a significant increase compared to Comparative Examples 1 to 4. In addition, it can be seen that Comparative Examples 1 to 4 have a higher drying temperature and a longer drying time compared to Examples 1 to 3, resulting in higher overall production energy consumption.
[0131]
[0132] Experimental Example 2 - Evaluation of average particle size (D50)
[0133] For the positive electrode active materials manufactured according to the examples and comparative examples, the particle size corresponding to 50% of the volume accumulation amount was measured using the laser diffraction method.
[0134]
[0135] (2) Manufacturing of coin-type half-cells
[0136] A positive electrode active material having a coating layer was manufactured by mixing about 1.927 g of Co(OH)2 per 100 g of the positive electrode active material manufactured according to the Examples and Comparative Examples and heat-treating the mixture at 600°C for 6 hours in an oxygen atmosphere. A CR2032 coin cell was manufactured using the positive electrode active material having the coating layer formed thereon, using the following method.
[0137] Specifically, a positive electrode active material, a conductive agent (acetylene black FX35, Denka), and a polyvinylidene fluoride binder (trade name: KF9709) were mixed in a weight ratio of 96.5:1.5:2 95:2.2:2.8, and the mixture was added to an N-methyl-2-pyrrolidone solvent so that the solid content was about 65 to 69 wt% to prepare a positive electrode active material slurry.
[0138] The above slurry was coated on an aluminum foil (Al foil, thickness: 20 ㎛), which is a positive electrode collector, using a doctor blade, dried, and rolled to manufacture a positive electrode. The loading amount of the positive electrode was about 15-16 mg / cm2, and the rolling density was about 3.5 g / cm 3 It was.
[0139] A 2032 coin-type half-cell was manufactured using the above positive electrode, lithium metal negative electrode (400 μm thick, NEBA), electrolyte, and polypropylene polyethylene separator by a conventional method. The electrolyte was manufactured by dissolving 1 M LiPF6 in a mixed solvent of ethylene carbonate, dimethyl carbonate, and diethyl carbonate (mixing ratio EC:DMC:DEC=1:2:1 volume %) to prepare a mixed solution, to which 3 wt% of vinylene carbonate (VC) was added and used.
[0140]
[0141] Experimental Example 3: Capacity Evaluation
[0142] Coin-type half-cells manufactured according to the examples and comparative examples were aged at room temperature (25°C) for 10 hours, and then a charge-discharge test was performed.
[0143] Capacity evaluation was conducted using 200 mAh / g as the reference capacity, and the charge / discharge conditions were CC / CV 2.5–4.25 V, 1 / 20 C cut-off. The initial capacity was measured by charging at 0.2 C and discharging at 0.2 C. The results are shown in Table 2 below.
[0144]
[0145] Experimental Example 4: Measurement of Life Characteristics
[0146] The life characteristics of lithium secondary batteries manufactured according to the examples and comparative examples were evaluated, and the results are shown in Table 2 below.
[0147] Specifically, the life characteristics were measured by performing 50 charge / discharge cycles at 45°C under the conditions of 0.5C charge and 1.0C discharge, and the capacity retention rate of the 50th cycle compared to the first cycle was measured.
[0148] Charge capacity (mAh / g)Discharge capacity (mAh / g)Life characteristics (45℃ 50cycle, %)Example 123321096.5Example 223321096.5Example 323321096.5Comparative example 1233 Less than 210 Less than 96.5Comparative example 2233 Less than 210 Less than 96.5Comparative example 3233 Less than 210 Less than 96.5Comparative example 4233 Less than 210 Less than 96.5
[0149] Referring to Table 2, it was confirmed that when the positive electrode active material according to Examples 1 to 3 was applied, the charge / discharge capacity and life characteristics were improved compared to Comparative Examples 1 to 4.
[0150]
[0151] Although the preferred embodiments of the present invention have been described above, the present invention is not limited thereto, and various modifications can be made within the scope of the patent claims, the detailed description of the invention, and the attached drawings, and it is obvious that this also falls within the scope of the present invention.
[0152] Accordingly, the actual scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. Step of preparing a nickel-containing transition metal precursor; A step of forming a mixture containing the above transition metal precursor and lithium raw material and then calcining it to obtain a calcined product; A step of washing and separating the obtained sintered material to obtain a sediment; and A step of drying the above sediment to obtain a positive electrode active material; The step of drying the above sediment to obtain a positive electrode active material is performed within a drying time of 2 hours. A method for manufacturing a cathode active material for a lithium secondary battery.
2. In paragraph 1, The step of drying the above sediment to obtain a positive electrode active material is as follows: Performed at a temperature of 110℃ to 130℃, A method for manufacturing a cathode active material for a lithium secondary battery.
3. In paragraph 1, The step of drying the above sediment to obtain a positive electrode active material is as follows: Stirring is performed at a stirring speed of 1 rpm to 10 rpm. A method for manufacturing a cathode active material for a lithium secondary battery.
4. In paragraph 1, The content of nickel in the above transition metal precursor is 80 mol% or more based on the total mole number of transition metals. A method for manufacturing a cathode active material for a lithium secondary battery.
5. In paragraph 1, The above lithium raw material is LiOH. A method for manufacturing a cathode active material for a lithium secondary battery.
6. In paragraph 1, The step of forming a mixture containing the above transition metal precursor and lithium raw material and then calcining it to obtain a calcined product is as follows: carried out in an oxygen atmosphere, A method for manufacturing a cathode active material for a lithium secondary battery.
7. In paragraph 1, In the step of forming a mixture containing the above transition metal precursor and lithium raw material and then calcining it to obtain a calcined product, Further mixing of the above doping raw materials, The above doping raw material includes at least one selected from Al, Zr, B, Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La and Sr. A method for manufacturing a cathode active material for a lithium secondary battery.
8. In paragraph 1, The above-mentioned manufactured positive electrode active material has a residual lithium content of less than 0.4 wt%. A method for manufacturing a cathode active material for a lithium secondary battery.
9. In paragraph 1, The above-mentioned manufactured positive electrode active material has an average particle diameter (D50) of 8 μm or more. A method for manufacturing a cathode active material for a lithium secondary battery.
10. In paragraph 1, The above lithium transition metal oxide is a method for producing a positive electrode active material for a lithium secondary battery represented by the following chemical formula 1: [Chemical Formula 1] Li a Ni x Co y Mr z M1 k O2 (In the above chemical formula 1, 0.8 ≤ a ≤ 1.1, 0.6 ≤ x < 1.0, 0 ≤ y ≤ 0.1, 0 ≤ z ≤ 0.1, 0 ≤ k ≤ 0.1, x + y + z + k = 1, M1 is one or more elements selected from Al, Zr, B, Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, and Sr.) 11. A positive electrode active material for a lithium secondary battery, manufactured according to any one of the manufacturing methods of clauses 1 to 10.
12. A positive electrode for a lithium secondary battery comprising the positive electrode active material for a lithium secondary battery of Article 11.
13. A lithium secondary battery comprising the positive electrode for a lithium secondary battery of Article 12.
Citation Information
Patent Citations
Cathode active material for lithium ion secondary battery and manufacturing method therefor, and lithium ion secondary battery
JP2021005548A
Positive electrode active material for rechargable lithium battery, method for manufacturing the same, and rechargable lithium battery including the same
KR1020150141254A
Preparation method of cathode active material, and cathode active material made by the same
KR1020170080483A
Fabric with improved heat insulation and elasticity and clothing including thereof
KR1020230111577A
Positive electrode active material for non-aqueous electrolyte secondary battery and method for manufacturing the same, positive electrode mixed material paste for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
US20190165360A1