Skyrmion transistor

The skyrmion transistor addresses the challenge of non-uniform skyrmion manipulation by using a hydrogen-ion controlled skyrmion gate with a MgO/CoFeB/AlOx structure, achieving stable and efficient skyrmion generation and storage with spatially uniform magnetic anisotropy.

WO2024248241A1PCT designated stage expired Publication Date: 2024-12-05KOREA RES INST OF STANDARDS & SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/017624
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2023-11-06
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing voltage-controlled skyrmion technologies face challenges with slow and non-uniform operations due to defects and oxygen ion migration, lacking a mechanism for spatially uniform magnetic anisotropy control necessary for efficient skyrmion manipulation and storage in electronic devices.

Method used

A skyrmion transistor design featuring a substrate with a magnesium oxide (MgO) and cobalt iron boron (CoFeB) thin film stack, incorporating an aluminum oxide (AlOx) layer formed by atomic layer deposition, and a gate voltage-controlled skyrmion gate that adjusts perpendicular magnetic anisotropy, enabling uniform skyrmion generation and storage by manipulating hydrogen ions for stable operation.

Benefits of technology

The solution provides a fast, stable, and non-volatile skyrmion transistor with spatially uniform magnetic anisotropy, allowing for efficient skyrmion generation, storage, and manipulation, overcoming previous limitations of defect-induced non-uniformity and oxygen ion migration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023017624_05122024_PF_FP_ABST
    Figure KR2023017624_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A skyrmion transistor of the present invention comprises: a substrate; a skyrmion channel formed on the substrate, and composed of a first thin film stack which includes a magnesium oxide (MgO) layer, a cobalt iron boron (CoFeB) layer and a heavy metal layer and of which one side is grounded; and a skyrmion generator and a skyrmion gate, which are composed of the first thin film stack and a second thin film stack formed in a predetermined upper area thereof and composed of an aluminum oxide (AlOx) layer and an electrode layer. The skyrmion gate of the present invention can pass or block skyrmion by controlling a gate voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Skyrmion transistor

[0001] The present invention relates to a skyrmion transistor, and more particularly, to a skyrmion transistor using a gate voltage.

[0002]

[0003] While traditional microelectronic devices perform charge transfer operations based on electrons, spin electronics perform information storage, transmission, and processing based on the spin properties of electrons.

[0004] Spintronics is the field that develops next-generation electronic devices, such as memory, using spin. Existing semiconductor-based electronic device technologies control only charge with electric fields, without considering the quantum mechanical spin of the two properties of electrons: charge and spin. Spintronics technology, which simultaneously controls both charge and spin, is expected to overcome the technological limitations of existing electronic devices. Spintronic devices have high potential for use as next-generation electronic devices due to their unique spin-like properties, such as non-volatility, as well as ultra-high speed, ultra-low power, and ultra-high frequency.

[0005] Recently, research is being actively conducted to develop next-generation electronic devices such as memory, logic devices, and communication devices using magnetic skyrmions (spin structures formed by arranging spins in a vortex shape) as shown in Fig. 1.

[0006] In order to utilize skyrmions in electronic devices, each skyrmion, which is the basic unit of information storage (bit), must be able to be created and destroyed at a desired location, and the created skyrmions must be able to be moved with very high efficiency.

[0007] Although several studies have suggested the possibility of realizing skyrmion devices using voltage-controlled skyrmion manipulation (S. Luo, M. Song, X. Li, Y. Zhang, J. Hong, X. Yang, X. Zou, N. Xu, L. You, Nano Lett. 2018, 18), it has not yet been experimentally demonstrated. This is because most voltage-controlled skyrmion manipulations are dominated by defects or oxygen ion transport, resulting in slow or spatially non-uniform operation.

[0008] In particular, for skyrmion logic devices, skyrmions must often move across controlled and uncontrolled regions while maintaining phase information, so a continuously well-connected interface between regions of different magnetic anisotropy is essential. However, such technology has not yet been available. Existing voltage-controlled magnetic anisotropy (VCMA) technology controls magnetic properties by applying a voltage to a magnetic thin film and an insulator containing oxygen by bonding them. This is a mechanism whereby an electric field controls magnetic anisotropy by changing the oxidation state of the interface between the oxide layer and the magnetic layer through the movement of oxygen ions.

[0009] However, these conventional voltage-controlled magnetic anisotropy techniques exhibit slow and non-uniform operation due to spatial non-uniformity of magnetic anisotropy caused by oxygen migration or defects.

[0010] Recent studies (AJ Tan, M Huang, CO Avci, F Buttner, Mann, W Hu, C Mazzoli, S. Wilkins, HL Tuller, GSD Beach, Nat. Mater. 2019, 18, 35) report voltage-controlled magnetic anisotropy using protons instead of oxygen, demonstrating relatively fast and stable operation. However, these studies do not demonstrate spatial uniformity of the magnetic anisotropy.

[0011]

[0012] The present invention aims to provide a fast and stable non-volatile skyrmion transistor using a voltage-controlled magnetic anisotropy technique exhibiting spatially uniform magnetic anisotropy.

[0013]

[0014] The skyrmion transistor of the present invention comprises: a substrate; a skyrmion channel formed on the substrate, the first thin film stack including a magnesium oxide (MgO) layer, a cobalt iron boron (CoFeB) layer, and a heavy metal layer, one side of which is grounded; and a skyrmion channel formed on the first thin film stack and aluminum oxide (AlO) formed in a predetermined region above the first thin film stack. x ) and an electrode layer, and a skyrmion generator and a skyrmion gate.

[0015] Additionally, in the present invention, the skyrmion gate can allow skyrmions to pass through or block them by controlling the gate voltage.

[0016] In addition, in the present invention, the gate voltage is applied to control the perpendicular magnetic anisotropy of the gate region, thereby adjusting the energy barrier through which skyrmions can pass, and there is a threshold value of the perpendicular magnetic anisotropy of the gate region at which the transistor can operate, and the transistor can operate above the threshold value.

[0017] Additionally, in the present invention, the skyrmion gate can allow or block skyrmions by controlling the in-plane current.

[0018] In addition, in the present invention, the skyrmion generator is characterized in that it controls the vertical magnetic anisotropy of the skyrmion generator region by applying a voltage to the skyrmion generator region through the electrode layer and adjusts the vertical magnetic field of the skyrmion generator region and the skyrmion channel region to form a skyrmion generation state in the skyrmion generator region and a skyrmion stable state in the skyrmion channel region, and applies an in-plane current to discharge skyrmions from the skyrmion generator region to the skyrmion channel region.

[0019] In addition, in the present invention, when a voltage is applied to the gate region, vertical magnetic anisotropy appears spatially uniformly within the gate region.

[0020] In addition, in the present invention, the aluminum oxide layer is formed by atomic layer deposition (ALD) using an aluminum precursor and water, and is formed at a relatively low temperature within a temperature range in which deposition is possible, and the aluminum oxide layer is characterized in that it contains hydrogen.

[0021] In addition, in the present invention, it is preferable that the heavy metal layer is made of at least one of W, Ta, Nb, and Hf, and an ultra-thin metal layer may be interposed between the cobalt iron boron layer and the magnesium oxide layer, and a natural oxide layer or a metal oxide layer may be formed on the upper portion of the heavy metal layer.

[0022] In addition, in the present invention, the magnetic image within the gate region using a MOKE (Magneto-optical Kerr effect) microscope is characterized by showing a uniform stripe domain width.

[0023] In addition, in the present invention, it is characterized in that the magnetization domains are spatially continuously connected at the interface between the gate region and the non-gate region having different perpendicular magnetic anisotropies, and the domain wall chirality is well preserved.

[0024] In addition, in the present invention, the in-plane current is a pulse current, and the number of skyrmions generated can be controlled by controlling the amplitude and time thereof.

[0025]

[0026] The present invention proposes a voltage-controlled skyrmion stability technology by manipulating the PMA and stripe domain width. Because the shape and phase of the skyrmion are well preserved as it passes through the interface between the controlled and non-controlled regions, the spatial uniformity of the voltage-controlled region can be appropriately applied to the skyrmion transistor of the present invention.

[0027] In addition, a new skyrmion generator having a skyrmion storage concept can be provided using the voltage-controlled skyrmion stability technology presented in the present invention, and a new non-volatile skyrmion transistor can be provided by combining this skyrmion generator concept with a precise voltage-controlled PMA.

[0028]

[0029] Figure 1 is a diagram showing a conventional voltage-controlled magnetic anisotropy (VCMA) experimental setup.

[0030] Figure 2 is a conceptual diagram representing a skyrmion.

[0031] Figure 3 illustrates the structure of a thin film stack according to one embodiment of the present invention.

[0032] Figure 4 is a diagram of the MOKE microscope experiment setup.

[0033] Figure 5 illustrates the planar structure and pattern of a thin film stack according to one embodiment of the present invention.

[0034] Figure 6 shows that the stripe domain width changes when a positive voltage pulse is applied to the gate region.

[0035] Figure 7 is a fast Fourier transform image of the gate area and the non-gate area.

[0036] Figure 8 (a) shows the relationship between the gate voltage pulse and the vertical magnetic anisotropy field, and (b) shows X-ray photoelectron spectroscopy analysis of the non-gate (solid line) and gate (dashed line) regions using in situ etching.

[0037] Figure 9 shows the movement of the gate region due to strong transverse current injection.

[0038] Figure 10 shows the results of investigating the spatial uniformity of voltage-controlled vertical magnetic anisotropy.

[0039] Figure 11 shows the results of investigating the magnetic domain connection between the gate region and the non-gate region.

[0040] Figure 12 shows various μ0H Z It shows a MOKE image of the stripe domain.

[0041] Figure 13 is a phase diagram between the stripe domain-skyrmion-uniform state under voltage-controlled stripe domain width and z-axis magnetic field.

[0042] Figure 14 (a) shows the mapping of the effective perpendicular magnetic anisotropy field, and (b) and (c) show the MOKE images in the initial state and after in-plane current injection, respectively.

[0043] FIG. 15 (a) illustrates a skyrmion transistor according to an embodiment of the present invention, and (b) to (p) illustrate the operation of the skyrmion transistor according to an embodiment of the present invention.

[0044] Figure 16 shows the number of skyrmions generated from the skyrmion generator depending on the amplitude and time of the injected current pulse.

[0045] Figure 17 shows a micromagnetic simulation for a skyrmion transistor.

[0046] Figure 18 illustrates various operations of a skyrmion transistor.

[0047] Figure 19 shows the H between the channel region and the gate region. k It shows the threshold current of the skyrmion to overcome the energy barrier of the gate as a function of the difference.

[0048] Figure 20 shows that a skyrmion transistor does not operate when the PMA of the gate region is less than the threshold value.

[0049] Figure 21 is a graph showing VCMA efficiency with respect to electric field.

[0050] Figure 22 is a graph showing energy consumption for VCMA operation.

[0051] Figure 23 is a graph showing total energy dissipation with respect to gate length.

[0052]

[0053] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings. However, the present invention is not limited to the embodiments described herein and may be embodied in other forms. Rather, the embodiments introduced herein are provided to ensure that the disclosure is thorough and complete and to sufficiently convey the spirit of the present invention to those skilled in the art.

[0054]

[0055] The skyrmion transistor of the present invention comprises a skyrmion channel, a skyrmion generator formed in a predetermined region thereon, and a skyrmion gate, and can pass or block skyrmions by controlling the gate voltage.

[0056] The skyrmion channel is formed on a substrate and comprises a first thin film stack including a magnesium oxide (MgO) layer, a cobalt iron boron (CoFeB) layer, and a heavy metal layer, one side of which is grounded.

[0057] The skyrmion generator and skyrmion gate are formed by the first thin film stack and aluminum oxide (AlO) formed in a predetermined region on the upper portion thereof. x ) is composed of a second thin film stack consisting of a layer and an electrode layer.

[0058] The above skyrmion generator controls the vertical magnetic anisotropy of the region by applying a voltage to the skyrmion generator region through the electrode layer and adjusts the vertical magnetic field of the skyrmion generator region and the skyrmion channel region to form a skyrmion generation state in the skyrmion generator region and a skyrmion stable state in the skyrmion channel region, and can discharge skyrmions from the skyrmion generator region to the skyrmion channel region by applying an in-plane current.

[0059] In addition, in the present invention, it is preferable that the heavy metal layer is made of at least one of W, Ta, Nb, and Hf, and an ultra-thin metal layer may be interposed between the cobalt iron boron layer and the magnesium oxide layer, and a natural oxide layer or a metal oxide layer may be formed on the upper portion of the heavy metal layer.

[0060]

[0061] Hereinafter, a skyrmion transistor according to an embodiment of the present invention will be described with reference to the drawings.

[0062] FIG. 3 illustrates the structure of a thin film stack applied to a skyrmion transistor according to one embodiment of the present invention, and FIG. 4 is a MOKE microscope experiment setup diagram.

[0063] Figure 5 shows the planar structure and pattern of a thin film stack according to one embodiment of the present invention. MgO / Ta / CoFeB / W / TaOX The thin film stack is patterned in the shape of wires indicated by black dashed lines, and AlO X (2 nm) / Pt(2 nm) thin film stacks are grown in the white dashed area. Dark and light gray patterns correspond to -z and +z magnetization, respectively. (Scale bar: 30 μm)

[0064] Figure 6 shows that the stripe domain width changes when a positive voltage pulse is applied to the gate region (Scale bar: 10 μm), and Figure 7 is a fast Fourier transform (FFT) image of the gate region and non-gate region (Scale bar: 0.1 μm -1 )

[0065]

[0066] The basic structure of a skyrmion transistor according to an embodiment of the present invention is as illustrated in Fig. 3. The thin film stack of the skyrmion generating device of the present invention comprises a substrate and MgO (1.0 nm) / Ta (0.07 nm) / Co 20 Fe 60 B 20 (1.0 nm) / W(3.0 nm) / TaO X A first thin film stack consisting of (2 nm) and AlO X It consists of a second thin film stack consisting of (2 nm) / Pt(2 nm).

[0067] In the present invention, the first thin film stack may be composed only of a magnesium oxide (MgO) layer, a cobalt iron boron (CoFeB) layer, and a heavy metal layer, and the heavy metal layer may use at least one of W, Ta, Nb, and Hf. A metal oxide layer as in Fig. 3 may be formed on the heavy metal layer, or may be formed as a natural oxide layer.

[0068] An ultra-thin metal layer can be interposed between the CoFeB layer and the MgO layer to control the perpendicular magnetic anisotropy (PMA) appearing at the interface and to more precisely control the PMA.

[0069]

[0070] In one embodiment of the present invention, MgO (1 nm) / Ta (0.07 nm) / Co is deposited on a thermally oxidized Si substrate using a magnetron sputtering system. 20 Fe 60 B 20 (1.0 nm) / W(3 nm) / TaOx(2 nm) stacks were deposited on a thermally oxidized silicon substrate using a magnetron sputtering system at a base pressure of 4.0 torr at room temperature, and then a post-annealing process was performed at 350°C for 1 hour under vacuum conditions of 5.0 or less to promote PMA.

[0071] To precisely control the PMA occurring at the CoFeB / MgO interface, an ultra-thin (0.07 nm) Ta layer was inserted. Since the PMA occurring at the CoFeB / MgO interface must be small for skyrmion formation, inserting an ultra-thin Ta layer, approximately one atomic layer, reduces the PMA occurring at the CoFeB / MgO interface, enabling more precise PMA control.

[0072] MgO / Ta / CoFeB / W / TaO X The first thin film stack was patterned into a wire shape using photolithography and ion milling (black dashed line area in Fig. 5). Then, AlO X (2 nm) / Pt(2 nm) layer was deposited on the gate area (white dashed line area in Fig. 5) on top of the first thin film stack.

[0073]

[0074] Here AlO x The layers were deposited using a thermal atomic layer deposition (ALD) system at 120°C. Trimethyl-aluminum (TMA) and water (H2O) were used as precursors, and nitrogen gas (N2) was used as a carrier and purging gas.

[0075] In the present invention, AlO xThe layer is formed at a relatively low temperature of 120°C within the temperature range where deposition is possible, so that hydrogen is not lost during the deposition process and AlO x It exists within the layer. That is, in the present invention, AlO x The layer contains hydrogen, and when an electric field is applied through the Pt layer, which is the electrode layer, hydrogen ions play a role and control PMA.

[0076]

[0077] To realize voltage-controlled skyrmion operation, spatially uniform control and an interface where two different regions are continuously well-connected are essential. When a voltage is applied to the gate region of a skyrmion transistor according to an embodiment of the present invention having a structure as shown in FIG. 3, perpendicular magnetic anisotropy appears spatially uniform and the gate region and non-gate region are continuously well-connected. This can be proven using MOKE (Magneto-optical Kerr effect) microscopy images.

[0078] As illustrated in Fig. 4, using a MOKE microscope, a magnetic image of a CoFeB layer, as shown in Fig. 5, can be obtained through sufficiently thin Pt and W layers while simultaneously applying an electric voltage and a perpendicular magnetic field. Dark gray and light gray in Fig. 5 represent the -z and +z magnetization domains for the MOKE image.

[0079] As shown in Fig. 3, a gate voltage is applied to the Pt top electrode, and the bottom electrode of the Ta / CoFeB / W layer is grounded. Therefore, most of the voltage drop occurs in the TaO layer, which has high resistance. X / AlO X It occurs between layers.

[0080] In the absence of applied voltage, the magnetic channel exhibits a stripe domain pattern with a constant stripe domain width (λ) as shown in (a) of Fig. 6.

[0081] The stripe domain width is exponentially proportional to the domain wall energy.

[0082] Neel-type domain wall energy , where A is the exchange stiffness and Keff( ) is the PMA energy density per volume, D is the Dzyaloshinski Moriya Interaction (DMI) energy density per area, and the last term is the volume demagnetization energy density.

[0083] Therefore, if A and D have the same values, changing the PMA will result in a change in the stripe domain width.

[0084] Figure 6(a) shows that the entire region has the same PMA value. Then, after applying a gate voltage pulse of 4 V for 2 seconds in the left dashed line region (gate region), the stripe domain width is reduced only within the gate region, as shown in Figure 6(b). Adding a gate voltage pulse injection further reduces the stripe domain width, as shown in Figure 6(c). The voltage-controlled stripe domain width remains even after the gate voltage is turned off, indicating non-volatile operation.

[0085] When a fast Fourier transform (FFT) is performed on the gate region and non-gate region shown in Fig. 6, the images appear as in (a) to (f) of Fig. 7. These FFT images clearly show that there is a change in the stripe domain width when the gate voltage is applied.

[0086]

[0087] To clarify that applying the gate voltage manipulates the PMA and not the DMI or other parameters, the H field in the gate region was measured after applying each gate voltage pulse using the MOKE microscope system. kThe values ​​were measured directly. Note that the change in DMI due to gate voltage can be ignored.

[0088]

[0089] In the above formula, m z is the normalized perpendicular magnetization corresponding to the normalized MOKE signal, and H z is the vertical magnetic field. H k is a valid PMA field, and using this equation, H k You can get it.

[0090] Figure 8 (a) shows the relationship between the gate voltage pulse and the vertical magnetic anisotropy field, and (b) shows the X-ray photoelectron spectroscopy analysis of the non-gated (solid line) and gated (dashed line) regions using in situ etching. In Figure 8 (a), the squares are μ0H after applying a positive gate voltage pulse. k , and the circle represents μ0H after applying a negative gate voltage pulse. k It represents.

[0091] Initial H of 2,221 Oe k Starting from , a gate voltage pulse of 3.6 V is applied for 3 seconds, H k is decreased (see Fig. 8 (a)). Then, using repetitive gate pulses, H is increased at about 1,025 Oe as shown in the curve connected by the square in Fig. 8 (a). k The value It's saturated.

[0092] Saturated H k A negative gate voltage pulse of -4.0 V was sequentially applied for 3 seconds from H k , and eventually saturates at 2,037 Oe.

[0093] That is, depending on the polarity or number of the applied gate voltage pulses, H kYou can see that you can freely control the stripe domain width by manipulating .

[0094]

[0095] Research on voltage-controlled magnetic phenomena has utilized oxygen ion transport as a fundamental mechanism. However, the experimental results obtained through one embodiment of the present invention cannot be explained by the oxygen ion transport mechanism.

[0096] In the thin film stack structure of the present invention as shown in Fig. 3, the voltage drop is mainly due to TaO X / AlO X occurs between the layers, indicating that the electric field exists only between the oxide layers.

[0097] A typical VCMA experiment using the oxygen ion transport concept applies a gate voltage directly to the oxide layer in the substrate / magnetic film / insulator (oxide layer) as shown in Fig. 1. However, in the thin film stack structure of the present invention (Fig. 3), the voltage is not directly applied to the oxide layer (MgO layer) in contact with the magnetic film (CoFeB), but the Ta / CoFeB / W layer is grounded and the TaO layer is grounded. X / AlO X A voltage is applied to the upper Pt electrode of the layer.

[0098] Therefore, the positive gate voltage that reduces the PMA in the initial state is W / TaO x Oxygen ions (O) at the interface 2- ) attracts oxygen ions. Therefore, oxygen ion transport cannot be the mechanism explaining the present invention unless the W layer initially has high resistance and abundant oxygen ions.

[0099] To determine the oxygen state inside the W layer for the gate / non-gate region, as shown in Fig. 8 (b), XPS (X-ray photoelectron spectroscopy) analysis using in situ etching was performed.

[0100] H in the gated / non-gated area before placing the sample inside the chamber kwere measured as 1,025 Oe and 2,221 Oe, respectively. In Fig. 8 (b), the dashed curve represents the spectrum of the gate region, and the solid curve represents the spectrum of the non-gate region.

[0101] Each curve is applied with the etching time shown on the right side of Fig. 8 (b).

[0102] Spin-orbit splitting of the W4f core level for the W metal state is well observed in both regions at the binding energy position of W4f (28 eV to 38 eV). The W metal peak starts to appear from an etching time of 300 s.

[0103] Also, Fe2p 3 / 2 At the binding energy position (704 eV~711 eV), Fe2p3 for Fe metal state after 480 s of etching time / 2 The peak of Fe2p is observed at an etching time of 660 s. 3 / 2 The sufficient peak intensity indicates that the spectra at an etching time of 660 s reflect the analysis near the CoFeB layer.

[0104] However, the oxide states of W and Fe were not observed in both the gate region and the non-gate region at all etching times. Therefore, oxygen ion transport can be excluded as the fundamental mechanism for VCMA in the present invention.

[0105] One remaining possibility is protons. Recently, various papers have reported controlling magnetic properties through hydrogen adsorption. Furthermore, a proton pump operated by a gate voltage has recently been demonstrated to control magnetic anisotropy or ferrimagnetic ordering. Experimentally, it has been demonstrated that a gate voltage can generate protons by dissociating H2O from the surface atmosphere, and that these protons can alter magnetic properties. The most likely candidate for the present invention would be protons.

[0106] The non-volatile and reversible operation of VCMA can be said to be due to ion migration by applying a gate voltage.

[0107] First, we can consider the most common oxygen ion, which, as explained above, can rule out oxygen transport as a fundamental mechanism.

[0108] The first reason is that there is no driving force to move the oxygen ions pre-existing in the two insulating layers (AlOx, TaOx) toward the ferromagnetic layer (CoFeB). As mentioned above, the electric field existing only in the insulating layer cannot push the oxygen ions out of the insulating layer. The XPS analysis in Figure 8 (b) also did not reveal any oxygen spectra before and after VCMA.

[0109] Next, the boron ions inside the CoFeB layer can be considered. When the post-annealing process was performed to promote PMA in the present invention, the large negative mixing enthalpy (ΔH) of W and B W-B =-31kJ / mol), boron atoms in the CoFeB layer diffuse into the adjacent W layer. Therefore, the electric field is TaO X It can affect the boron ions near the interface between the W layer and the SiO layer.

[0110] Figure 9 illustrates the movement of the gate region due to strong transverse current injection. This provides indirect experimental evidence that boron is not involved in the underlying mechanism. As shown in Figure 9, a gate voltage sufficient to reduce the PMA in the gate region was injected. Therefore, the gray region in the gate region in Figure 9(a) represents a stripe domain with a width smaller than the optical resolution or the in-plane magnetization state. After the gate voltage was turned off, a strong current (4.0 V) was applied along the -x-axis for 5 minutes (Figure 9(b)). As shown in Figure 9(b), the strong and long in-plane current injection pushes the existing gray region to the left, restoring the gate region. Subsequently, a 4.0-V current was injected along the +x-axis for 5 minutes. In this case, the current pushes the existing gray region to the right, slightly restoring the left region. However, when gate control is disabled, transverse current injection does not change the magnetic anisotropy even at higher (10 V) amplitudes and for longer (10 minutes) times. Changes in magnetic anisotropy due to lateral current injection have not been reported in CoFeB-based structures, except for the Joule heating effect. The direction of operation in Figure 9 indicates that Joule heating is not the dominant mechanism. Therefore, boron ions already present before gate actuation cannot explain the experimental results above. Therefore, the fundamental mechanism for VCMA in the present invention can be attributed to hydrogen ion migration.

[0111]

[0112] Realizing voltage-controlled skyrmion motion requires spatially uniform control and a consistently well-connected interface between two distinct regions. However, oxygen ion transport-based VCMA exhibits spatially non-uniform behavior or defect generation due to the heavy and large nature of oxygen ions. For example, if a defect is created during VCMA operation, the transported skyrmion may become trapped, restricting its further movement or even causing it to disappear.

[0113] Figure 10 shows the results of investigating the spatial uniformity of voltage-controlled perpendicular magnetic anisotropy. In Figure 10, (a) shows the initial state, and (b) and (c) show the mapping of the effective perpendicular magnetic anisotropy field after applying a positive gate voltage pulse.

[0114] Figure 11 illustrates the results of investigating the magnetic domain connection between the gated and non-gate regions. Figure 11 shows the continuous deformation of the stripe domain through two different perpendicular magnetic anisotropy regions, and the bold arrows in Figure 11(b) indicate the magnetization direction at the domain wall, indicating that chirality is well preserved.

[0115] As shown in Fig. 10, after each gate voltage pulse, H k The spatial uniformity of the voltage-controlled stripe domain width was investigated by spatially mapping the gate edge noise data. This is because the 2x2 pixels of the original MOKE image are analyzed as one mapping data point in the xy plane. For the initial state (Fig. 10(a)), the gating region (dashed box in Fig. 10(a)) has almost the same mapping (H) as the non-gating region. k , has an average value of 2803 Oe).

[0116] After applying the first gate voltage pulse of 4 V for 3 seconds, H in the gating region k is well controlled as shown in (b) of Fig. 10 (average value, 2234 Oe). The standard deviation of the inner gate area is 91 Oe. The second gate voltage pulse of 4 V for 3 seconds is H k (H k The average value of , 1749 Oe) is further lowered. Here, H k The standard deviation of H is 67 Oe. k Considering the error range of the method of measuring this voltage-controlled stripe domain width operation, it is very uniform within the gate area.

[0117] In addition, the present invention investigated the magnetic domain connection between two different stripe domain width regions, as shown in FIG. 11. The dashed box region is the voltage-controlled stripe domain width region, and the other region is the non-gated region. FIG. 11(b) is an enlarged image of the solid box in FIG. 11(a). The stripe domain width inside the non-gated region is almost twice that inside the gated region. However, at the interface of the two regions (the dashed line in FIG. 11(a)), the two types of stripe domains with different stripe domain widths are well connected by a spatially continuous stripe domain deformation, as shown in FIG. 11(b).

[0118] Due to the interfacial DMI from the W layer, the domain walls of the stripe domains in both regions have a Neel-type domain wall configuration with left-handed chirality, as indicated by the bold arrows in Fig. 11(b). It can be seen that the domain wall chirality, which determines the topological features, is well preserved across the different stripe domain width regions.

[0119]

[0120] A skyrmion generator of a skyrmion transistor according to an embodiment of the present invention having a structure as shown in FIG. 3 has a spatially uniform magnetic anisotropy and an interface in which the gate region and the non-gate region are continuously well connected, so that skyrmions can be generated and stored quickly and stably.

[0121] Figure 12 shows various μ0H Z The MOKE images of the stripe domain are shown in (Scale bar 5 μm). In Fig. 12, (a) to (d) are MOKE images in the initial state, (e) to (h) are MOKE images after the 6th gate voltage pulse, and (i) to (l) are MOKE images after the 7th gate voltage pulse.

[0122] Figure 13 is a phase diagram between the stripe domain-skyrmion-uniform state under voltage-controlled stripe domain width and a z-axis magnetic field. The white, dark gray, and light gray regions represent the uniform state, skyrmion+stripe state, and skyrmion state, respectively.

[0123] Figure 14 (a) shows the mapping of the effective perpendicular magnetic anisotropy field, while (b) and (c) show MOKE images in the initial state and after in-plane current injection, respectively. In Figure 14 (a), the left region is the non-gated region and the right region is the gated region. Figure 14 (b) is the initial state MOKE image, and (c) is the MOKE image after in-plane current pulse injection. (Scale bar 3 μm)

[0124] Skyrmion properties, including skyrmion radius or skyrmion stability, are determined by the stripe domain width at zero magnetic field. In particular, the z-axis magnetic field (H Z ) the energy landscape for the stripe domain-skimmy-homogeneous state is primarily a function of the stripe domain width, independent of other material parameters.

[0125] For example, the initial state has a stripe domain width of 4.58 μm at zero magnetic field, as shown in Fig. 12 (a). Then, +H Z When applied, the -z-axis stripe area gradually shrinks, eventually reaching +H of 10.6 Oe. Z A uniform magnetic state is formed in (Fig. 12 (a) to (d)).

[0126] Then, when six positive gate voltage pulses of 3.6 V are injected for 3 seconds, the stripe domain width is reduced to 2.19 μm as shown in (e) of Fig. 12. Here, +H Z Applying +H will result in the same behavior as the initial state, but to reach a uniform state Z The amplitude increases slightly from 10.6 Oe to 12.8 Oe (Fig. 12 (d) and (h)).

[0127] Then, adding a positive gate voltage pulse of 3.6 V for 3 s reduces the stripe domain width to 1.80 μm as shown in (i) of Fig. 12. As shown in (k) of Fig. 12, +H of 10.0 Oe Z When applied, it becomes a skyrmion state, and +H of 14.0 Oe Z A uniform state appears in .

[0128] The phase transition from the stripe domain state to the skyrmion state can occur when the thermal fluctuations at the two adjacent domain walls of the stripe domain are sufficient. Therefore, the skyrmion state is not observed beyond a certain stripe domain width, even though the skyrmion state is generally a minimum state (see Fig. 13).

[0129] In Fig. 13, the initial state (Fig. 12(a)) corresponds to the black circle on the far right in Fig. 13. When a positive gate voltage pulse is applied, the stripe domain width decreases (arrows along the curve in Fig. 13), and +H is required to reach a uniform state. Z increases. Finally, below the stripe domain width of 1.80 μm, H Z Only by applying H can the skyrmion state be observed. In Fig. 13, the skyrmion is in a global minimum state near the curve, which is H Z It cannot be observed by itself.

[0130] According to this phase diagram, it can be seen that the skyrmions within the gated control region with a stripe domain width of 1.80 μm can be transferred to the non-gated region using spin-orbit torque (SOT) (long arrows indicated to the right in the center of Fig. 13).

[0131] To verify this, the stripe domain width of about 1.80 μm was voltage-controlled in each right region of (a) to (c) in Fig. 14, and each left region of (a) to (c) was not gated. (a) in Fig. 14 clearly shows that the two regions have different H k H showing k Shows mapping data.

[0132] +H of 8.7 Oe Z In the non-gate region, the skyrmion or skyrmion+stripe domain state is present. In this state, the thermal energy is insufficient to spontaneously generate skyrmions, but once generated, skyrmions are stable.

[0133] The gate region is +H of 8.7 Oe Z Below, the skyrmion state is present, and skyrmions are spontaneously generated due to the sufficiently small stripe domain width, as shown in (b) of Fig. 14. Here, when an in-plane current pulse of 0.5 V is injected for 10 ms, skyrmions in the gate region are pushed to the non-gate region by the SOT, as shown in (c) of Fig. 14, and skyrmions are spontaneously generated to fill the empty space in the gate region. Skyrmions moved in the gate region have a +H of 8.7 Oe. Z It is stable even within the non-gate area.

[0134] Skyrmion transport from the gated region to the non-gate region is only possible when the shape and phase of the skyrmion are well preserved as it passes through the gated / non-gate interface. This operation suggests that the present invention can be used as a novel skyrmion generator, and since skyrmions are generated spontaneously, the gated region can be considered a skyrmion reservoir.

[0135]

[0136] FIG. 15 (a) illustrates a skyrmion transistor according to an embodiment of the present invention, and (a) to (P) illustrate the operation of the skyrmion transistor according to an embodiment of the present invention.

[0137] In (a) of Fig. 15, the horizontally long dashed box (1) is a skyrmion channel, the left dashed box (2) acts as a skyrmion generator, and the right dashed box (3) is a skyrmion gate. (Scale bar, 10 μm) In Fig. 15, (b) shows the initial state, (c) shows the state where a skyrmion is generated, and (d) to (f) show the skyrmion moving and passing through the skyrmion gate region.

[0138] In Fig. 15, (g) to (k) show the operation after lowering the PMA of the skyrmion gate region by applying a positive gate voltage pulse, and (k) shows that the generated skyrmion is blocked at the right interface of the skyrmion gate region.

[0139] In Fig. 15, (l) to (p) show the operation after the PMA is recovered in the skyrmion gate region by applying a negative gate voltage pulse, and (p) indicates that the skyrmion can pass through the skyrmion gate region again.

[0140] As illustrated in FIG. 15, the present invention provides a novel nonvolatile skyrmion transistor by combining a novel skyrmion generator and a precise voltage-controlled PMA operation. Below, we experimentally demonstrate the voltage-controlled skyrmion stability technology for application in skyrmion logic devices.

[0141] A transistor is a semiconductor device used to switch electrical signals. In this sense, the skyrmion transistor of the present invention can function as a switch for skyrmion operation. When the gate voltage is turned off (or on), skyrmions can pass through, and when the gate voltage is turned on (or off), skyrmions can be blocked.

[0142] In (a) of Fig. 15, the dashed box (1) is H k The skyrmion channel is 946 Oe (non-gate region), and the dashed box (2) used as a skyrmion generator controls the voltage to generate an H of 524 Oe.k The dashed box (3) (skyrmion gate) is initially identical to the skyrmion channel because it is not gate controlled.

[0143] In the initial state V SD When a pulse of 0.2 V is applied for 10 ms, the skyrmions inside the skyrmion generator can be pushed into the skyrmion channel, thereby generating skyrmions in the skyrmion channel, as shown in (c) of Fig. 15. After that, V SD When the pulse is 100 ms, the skyrmion is pushed to the right by the SOT, which does not generate additional skyrmions, as shown in (d) and (e) of Fig. 15. In addition, as shown in (f) of Fig. 15, the skyrmion passes through the skyrmion gate because the skyrmion gate is identical to the skyrmion channel.

[0144] Next, a positive gate voltage (V ) of 3.0 V is applied for 3 seconds. G ) by applying the H of the skyrmion gate k was reduced to 830 Oe. Similarly, V SD When the pulse is 10 ms, a skyrmion is generated in the skyrmion channel (Fig. 15 (h)), and V is 0.05 V. SD When the pulse is 100 ms, the skyrmion moves ((i) and (j) in Fig. 15). However, as shown in (k) in Fig. 15, the skyrmion cannot pass through the right interface of the skyrmion gate while passing through the left interface of the skyrmion gate.

[0145] And a negative gate voltage of -3.5 V for 3 seconds (V G ) to H of the skyrmion gate with 923 Oe k If the gate is reversed, the skyrmion can pass through the skyrmion gate region again, as shown in (p) of Fig. 15. The operations of (b) to (p) of Fig. 15 represent the operation of the skyrmion transistor of the present invention.

[0146]

[0147] Figure 16 illustrates the number of skyrmions generated from the skyrmion generator as a function of the amplitude and duration of the injected current pulse. The number of magnetic skyrmions emitted from the skyrmion generator can be controlled by selecting the width (duration of the pulse) and amplitude (intensity of the pulse) of the injected current pulse, as shown in Figure 16. Furthermore, existing skyrmions can move within the red zero skyrmion generation range.

[0148]

[0149] Figure 17 shows a micromagnetic simulation of a skyrmion transistor. Spin dynamics simulations were performed using MuMax3 software to elucidate the microscopic mechanism of skyrmion transistor operation. In Figure 17, (a) shows the spatial distribution of PMA energy density per volume, (b) shows its line profile (the central low PMA region is the gate region), (c) shows the initial skyrmion position, and (d) shows skyrmion trajectories by SOTs with different PMA energy densities in the gate region.

[0150] The material parameters were selected to stabilize the skyrmion for the micromagnetic simulation of Fig. 17. Here, the saturation magnetization was 1,130 kA / m 3 , exchange stiffness is 16 pJ / m, DMI energy density is -3 mJ / m 2 , the damping constant is 0.3. The PMA energy density in the ungated region is 1.25 MJ / m 3 , and the PMA energy density in the gate region is 1.20 MJ / m 3 1.24 MJ / m 3 It varies from 9 A / m to 9 A / m to move the skyrmion. 2 A spin polarization current was injected in the y-axis direction.

[0151] In order to schematically explain the skyrmion transistor of the present invention, the spatial distribution of the PMA energy density is set as in (a) of Fig. 17, and K UThe line profile of the distribution is presented in Fig. 17(b). The lower K in the center U Some areas are gated areas, while others are non-gate areas.

[0152] Non-gate area (K i ) of K U was set to 1.25 MJ / m3, and the gate area (K g ) of K U is a variable. Initially, a skyrmion is placed at the left end (Fig. 17(c)), and a spin-polarized current in the y-direction is injected to obtain three different K g Moves the skyrmion by value.

[0153] K g As in (d) of Figure 17, 1.24 MJ / m 3 When less than , the skyrmion cannot pass through the gate area, and the blocked point is the same as the starting point of the gradient area indicated by the vertical black dashed line in Fig. 17.

[0154] Considering the energy of the skyrmion, the energy of the skyrmion is K U Because it is proportional to K U The potential energy of the skyrmion can act as a force on the skyrmion. Therefore, a force will be exerted on the skyrmion, just as a negative gradient potential energy exerts a force on a classical particle. Therefore, a high driving current can allow the skyrmion to pass through the gate.

[0155]

[0156] Below, various device performances of the skyrmion transistor of the present invention are described.

[0157] Figure 18 illustrates various operations of a skyrmion transistor. In Figure 18, (a) to (d) show the skyrmion conversion motion through a gate region with an initial PMA (1,062 Oe) by a 17.8 μA current pulse, (e) to (g) show that a skyrmion driven by a 17.8 μA current pulse is blocked at the right interface (977 Oe) of the gate region, and (h) shows that the higher the current pulse (21.3 μA), the more skyrmions pass through the gate region.

[0158] Figure 19 shows the H between the channel region and the gate region. k The threshold current of the skyrmion to overcome the energy barrier of the gate as a function of the difference is shown in Fig. 20, and it shows that the skyrmion transistor does not operate when the PMA of the gate region is less than the threshold.

[0159] To verify the various performances of the skyrmion transistor of the present invention, skyrmion transistor operations were performed at various current densities.

[0160] As shown in (a) to (d) of Fig. 18, since the gate region is identical to the channel region, skyrmions pass through the gate region with a current pulse of 17.8 μA for 30 ms. This means that skyrmions can be passed or blocked by controlling the in-plane current. Therefore, the skyrmion transistor of the present invention can be operated by controlling not only the gate voltage but also the in-plane current.

[0161] And by injecting the gate voltage, H in the gate region k The value was lowered to 977 Oe. H between the gate region and the channel region k The difference in values ​​creates an energy barrier for the skyrmion, which blocks the translational motion of the skyrmion by a current pulse of 17.8 μA for 30 ms (Fig. 18(g)).

[0162] However, as illustrated in (h) of Fig. 18, a high current pulse (21.3 μA 30 ms) induces a higher spin-orbit torque (SOT) that allows the skyrmion to pass through the gate. Since the PMA can act as the potential energy of the skyrmion, the height of the energy barrier is H k It depends on the difference in value.

[0163] In the present invention, H k The critical amplitude of a 30 ms current pulse was tested to overcome the energy barrier as a function of the difference in values. H k Difference in values ​​(ΔH k ) is defined by the formula below.

[0164]

[0165] The threshold current is ΔH k As increases, increases.

[0166] Since the potential energy is the local energy of the skyrmion as a function of the PMA, H k determines the potential energy of the skyrmion. Skyrmions have low H k High H in the area k To get to the area ΔH k (i.e., the effective force due to the potential energy gradient) must be overcome.

[0167] Also, H in the gate area k When the value is controlled to be too small (627 Oe in (a) to (c) of Fig. 20), the skyrmion entering the gate becomes longer as in (c) of Fig. 20. H to reach the skyrmion state z The size of H k increases with the decrease of .

[0168] Threshold H for skyrmion state zIn the stripe domain, the skyrmion is more stable than the skyrmion, and the skyrmion elongates into the stripe domain in the gate region. Then, when a sufficient current pulse is injected to push the elongated domain, the domain becomes longer and no new skyrmion is created.

[0169] This is the specific range of H over which the skyrmion transistor can operate. k This means that there is a need to consider this when designing skyrmion transistor-based devices.

[0170]

[0171] Figure 21 is a graph showing the VCMA efficiency with respect to an electric field. As shown in Figure 21, the VCMA efficiency was confirmed experimentally. The VCMA efficiency is obtained from the slope of the linear fitting line for the graph in Figure 21. The value of -0.72 fJ / Vm is lower than the reported value. However, considering that the fundamental mechanism of VCMA is a proton-mediated process, the efficiency calculated by the electric field should be considered with caution.

[0172]

[0173] Figure 22 is a graph showing energy consumption for VCMA operation, and Figure 23 is a graph showing total energy dissipation with respect to gate length.

[0174] In the present invention, the total energy dissipation for one gate operation was calculated by considering the maximum stored energy of the capacitor. TaO x and AlO x Using dielectric constants of 22 and 9 respectively, 2.81×10 -12 10×10㎛ as F 2 Total TaO of x (2nm) / AlO x (2 nm) layer can be calculated. Then, the energy stored during the 3-V gate operating in the insulating layer is 4.21×10 -12 It's J.

[0175] Here, what is adjusted through the gate operation is the effective PMA energy density (J / m 3 ) rather than the interfacial PMA energy density (J / m 2 ) . This means that the charge required to induce the VCMA effect is proportional to the gating area. Therefore, the total energy dissipation decreases as the square of the gate length, as shown in Fig. 23.

[0176] In addition, the experimental electrical energy for the gating operation to manipulate the PMA was also measured using E=VIt, where V is the voltage, I is the leakage current, and t is the duration of the gating voltage pulse. Figure 22 shows H k It is shown that the minimum electrical energy required to operate a gate decreases as the square of the gate length. Therefore, for a gate area of ​​~100 nm, the energy required for operation is expected to be reduced to the nJ scale.

[0177] Finally, the device of the present invention exhibits leakage current in the μA range, which is a factor in increasing energy consumption. In the present invention, experiments were conducted on thin AlO x Using layers of AlO x Clear MOKE images were obtained through the Pt layer. Therefore, minimizing leakage current can further reduce energy consumption by optimizing the thickness or quality of the dielectric layer. It is noteworthy that since proton-based VCMA is driven by an electrochemical reaction, not an electric field, the operating voltage is independent of the dielectric layer thickness.

[0178]

[0179] As described above, the present invention proposes a voltage-controlled skyrmion stability technique by manipulating the PMA and stripe domain width. Because the shape and phase of the skyrmion are well preserved as it passes through the interface between the controlled and non-controlled regions, the spatial uniformity of the voltage-controlled region can be optimally applied to the skyrmion transistor of the present invention.

[0180] In addition, a new skyrmion generator having a skyrmion storage concept can be provided using the voltage-controlled skyrmion stability technology presented in the present invention, and a new non-volatile skyrmion transistor can be provided by combining this skyrmion generator concept with a precise voltage-controlled PMA.

[0181] The present invention will open new avenues for designing and realizing skyrmion devices, including skyrmion transistor-based logic devices.

[0182]

[0183] As described above, the best practice embodiments have been disclosed in the drawings and specifications. While specific terminology has been used herein, it is solely for the purpose of describing the present invention and is not intended to limit the scope of the invention as defined in the claims. Therefore, those skilled in the art will understand that various modifications and equivalent embodiments are possible. Therefore, the true scope of technical protection of the present invention should be determined by the technical spirit of the appended claims.

Claims

1. Substrate; A skyrmion channel formed on the substrate, comprising a first thin film stack including a magnesium oxide (MgO) layer, a cobalt iron boron (CoFeB) layer, and a heavy metal layer, one side of which is grounded; and The first thin film stack and aluminum oxide (AlO) formed in a predetermined area above the first thin film stack x A skyrmion transistor comprising a skyrmion generator and a skyrmion gate, the skyrmion transistor comprising a second thin film stack comprising a ) layer and an electrode layer.

2. In paragraph 1, The above skyrmion gate is, A skyrmion transistor characterized in that a gate voltage can be adjusted to allow passage or block skyrmions.

3. In paragraph 2, A skyrmion transistor characterized in that the energy barrier through which skyrmions can pass is adjusted by controlling the vertical magnetic anisotropy of the gate region by applying the gate voltage.

4. In paragraph 3, A skyrmion transistor characterized in that there exists a threshold of perpendicular magnetic anisotropy in the gate region at which the transistor can operate.

5. In paragraph 1, The above skyrmion gate is, A skyrmion transistor characterized in that it can pass or block skyrmions by controlling the in-plane current.

6. In paragraph 1, The above skyrmion generator is, A skyrmion transistor characterized in that a voltage is applied to the skyrmion generator region through the electrode layer to control the vertical magnetic anisotropy of the skyrmion generator region, and a vertical magnetic field of the skyrmion generator region and the skyrmion channel region is adjusted to form a skyrmion generation state in the skyrmion generator region and a skyrmion stable state in the skyrmion channel region, and skyrmions are ejected from the skyrmion generator region to the skyrmion channel region by applying an in-plane current.

7. In paragraph 1, A skyrmion transistor characterized in that when a voltage is applied to the gate region, vertical magnetic anisotropy appears spatially uniformly within the gate region.

8. In paragraph 1, The above aluminum oxide layer is, A skyrmion transistor formed by atomic layer deposition (ALD) using an aluminum precursor and water, characterized in that the deposition is performed at a relatively low temperature within a temperature range where deposition is possible.

9. In paragraph 8, A skyrmion transistor, characterized in that the above aluminum oxide layer contains hydrogen.

10. In paragraph 1, A skyrmion transistor, characterized in that the heavy metal layer is made of at least one of W, Ta, Nb, and Hf.

11. In paragraph 1, A skyrmion transistor characterized in that an ultra-thin metal layer is interposed between the cobalt iron boron layer and the magnesium oxide layer.

12. In paragraph 1, A skyrmion transistor characterized in that a natural oxide layer or a metal oxide layer is formed on the upper portion of the heavy metal layer.

13. In paragraph 1, A skyrmion transistor characterized in that the magnetic image within the gate region using a MOKE (Magneto-optical Kerr effect) microscope shows a uniform stripe domain width.

14. In paragraph 1, A skyrmion transistor characterized in that magnetization domains are spatially continuously connected at the interface between the gate region and the non-gate region having different perpendicular magnetic anisotropies.

15. In paragraph 1, A skyrmion transistor characterized in that domain wall chirality is well preserved at the interface between the gate region and the non-gate region having different perpendicular magnetic anisotropy.

16. In paragraph 1, A skyrmion transistor characterized in that the above-mentioned in-plane current is a pulse current, and the number of skyrmions generated can be controlled by controlling the amplitude and time thereof.

Citation Information

Patent Citations

  • Skyrmion Memory Device

    KR101902261B1

  • Tuna franchise business management system and method

    KR1020220038981A

  • Compound and organic light emitting device comprising same

    KR1020240114886A

  • Switching skyrmions with VCMA / electric field for memory, computing, and information processing