Battery and method for manufacturing battery
The battery design with a concave-convex pattern and recessed portions addresses the issue of irregular electrode layer gaps in flexible batteries, ensuring reliable performance and safety through consistent spacing and reinforcing structures, even under repeated bending.
Patent Information
- Application Number
- PCT/KR2023/018164
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2023-11-13
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional battery designs face issues with irregular electrode layer gaps and deformation when bent, leading to reliability and safety concerns in flexible devices, as the curvature causes the outermost electrode to slide and become deformed, resulting in irregular gaps and potential short circuits.
A battery design featuring an electrode assembly with a concave-convex pattern and recessed portions on the convex parts, where the convex portions have depressions to maintain even spacing and prevent electrode layer gaps, combined with a reinforcing structure to support the exterior material's shape during bending.
The design effectively suppresses irregular electrode layer gaps and maintains the integrity of the battery's performance even after repeated bending, enhancing durability and safety by preventing electrode lifting and deformation, while maintaining consistent electrode spacing.
Smart Images

Figure KR2023018164_05122024_PF_FP_ABST
Abstract
Description
Batteries and methods of manufacturing batteries
[0001] The present invention relates to a battery that can be charged and discharged and can be provided as a power source for mobile or flexible devices, etc.
[0002] A battery, or electrochemical cell, is an assembly that can provide electrical energy and is composed of at least two electrodes and an electrolyte. In particular, secondary batteries that can be charged and discharged are widely used in various advanced electronic devices, including smartphones.
[0003] Recently, various attempts have been made to break away from conventional forms in the design of mobile devices, including smartphones, and various wearable devices. Furthermore, attention is growing toward flexible devices that can bend while maintaining functionality. Consequently, the implementation of technologies that ensure the reliability and safety of flexible batteries embedded in these devices and used as power sources is emerging as a key issue.
[0004] In this regard, prior art patent document 1 (KR10-2022-0015290 A) discloses a technology for forming a pattern on an outer casing. However, patent document 1 discloses a configuration for forming at least one pattern portion on an outer casing in the TD (Transverse Direction) of the outer casing, but this pattern causes a change in the gap between the layers of electrodes laminated within the outer casing when the battery is repeatedly bent at a large curvature, and when a large gap is formed, the reliability and safety of the battery are lowered, which causes a problem.
[0005] Let us briefly explain the problem of increasing gaps between electrode layers in batteries manufactured using conventional technology.
[0006] Within the outer shell of a conventional battery, positive and negative electrodes are arranged in a straight line. The electrodes are stacked in close contact and maintain a constant distance apart, ensuring a regular layer gap between the electrodes. Insulating material is included between each electrode to prevent short circuits that could occur if the positive and negative electrodes meet directly, and to allow lithium ions to move.
[0007] However, in the case of a conventional battery that has been repeatedly bent, when the battery is bent, the outermost electrode slides inward due to the curvature, and when the battery is straightened again, the outermost electrode does not return to its original position and becomes deformed, causing some sections of the electrode layer gap to be lifted, resulting in an irregular gap.
[0008] Specifically, when a battery is deformed from a flat first state to a bent second state, and then deformed to return to a flat third state, an electrode (e.g., the outermost electrode) that is severely deformed into a bend or irregular waveform shape is difficult to return to a flat state. In particular, in a structure where one side of the electrode is fixed and the other side is not fixed, the electrode arranged at the outermost side is relatively more prone to deformation than the other electrodes, and thus has a problem in that the electrode is likely to lift or bend toward the pouch during the restoration process of the battery, easily generating an irregular gap.
[0009] One object of the present invention is to provide a battery including an electrode assembly including a plurality of electrodes and an outer case for accommodating the electrode assembly and having a protruding pattern formed thereon including at least one concave portion and at least one convex portion.
[0010] Another object of the present invention is to provide a flexible battery in which a portion of a convex portion is formed as a sunken portion, thereby suppressing an irregular electrode layer gap that may occur due to bending of the battery.
[0011] However, the technical tasks that this embodiment seeks to accomplish are not limited to the technical tasks described above, and other technical tasks may exist.
[0012] As a means for achieving the above-described technical task, one embodiment of the present invention can provide a battery including an electrode assembly including a plurality of electrodes and an outer material accommodating the electrode assembly and having a concave-convex pattern formed thereon including at least one concave portion and at least one convex portion, wherein a recessed portion is formed in which a portion of the convex portion is recessed.
[0013] According to one embodiment, each of the at least one convex portions may have at least two recessed portions formed in one direction corresponding to the width of the battery.
[0014] According to one embodiment, the spacing between at least two recessed portions formed on a first convex portion among the at least one convex portion and the spacing between at least two recessed portions formed on a second convex portion located next to the first convex portion may be designed to be the same.
[0015] According to one embodiment, the recessed portion may be formed to have a first gap with an edge area of the outer material.
[0016] According to one embodiment, the spacing between at least two recessed portions formed on a first convex portion among the at least one convex portion and the spacing between at least two recessed portions formed on a second convex portion located next to the first convex portion may be designed to be different.
[0017] According to one embodiment, the recessed portion formed in the first convex portion may be formed to have a second gap with the edge area of the outer material.
[0018] According to one embodiment, the recessed portion formed in the second convex portion may be formed to have a third gap with the edge area of the outer material.
[0019] According to one embodiment, the outer material may have a receiving portion for receiving the electrode assembly and a sealing portion for sealing the electrode assembly by bonding a sealing surface along an edge of the receiving portion.
[0020] According to one embodiment, the at least one concave portion and the at least one convex portion may have an edge area forming a boundary line that contacts the sealing portion at an end in one direction corresponding to the width of the battery.
[0021] According to one embodiment, the sealing portion may be characterized by having a pattern having a lower height than the uneven pattern in the thickness direction of the outer material.
[0022] According to one embodiment, a reinforcing structure can be formed in the recessed portion to maintain the recessed portion shape of the outer material.
[0023] Another embodiment of the present invention may provide a battery manufacturing method including the steps of forming at least one convex portion in one direction on an outer material, forming at least one concave portion at a position adjacent to the convex portion, forming a depressed portion in the at least one convex portion, inserting an electrode assembly into the outer material in which the depressed portion is formed, and sealing the outer material in which the electrode assembly is inserted.
[0024] According to another embodiment, the method further includes a step of pressing the outer material having the convex portion formed thereon, and the step of forming the recessed portion may form the recessed portion in the convex portion of the pressed outer material.
[0025] According to another embodiment, the step of forming the concave portion may be performed before or after the step of pressing the outer material on which the convex portion is formed.
[0026] According to another embodiment, when the concave portion is formed after pressing the outer material on which the convex portion is formed, the step of additional pressing on the outer material may be further included.
[0027] According to the present invention, a battery includes an electrode assembly including a plurality of electrodes, an outer material for accommodating the electrode assembly, and having a concave-convex pattern formed thereon including at least one concave portion and at least one convex portion, and a depressed portion formed in which a portion of the convex portion is sunken, thereby suppressing the occurrence of an irregular electrode layer gap and a large gap when the battery is bent.
[0028] In addition, by forming a reinforcing structure in a sunken area where some areas of the convex portion are sunken to maintain the shape of the sunken area, when the battery is bent or deformed, the effect of reducing cracks in the exterior material can be achieved by resistance according to the strength and support capacity of the reinforcing structure.
[0029] FIG. 1 is an exemplary drawing showing a battery according to a first embodiment of the present invention.
[0030] Figure 2 is an exemplary drawing showing an enlarged area A of the battery of Figure 1.
[0031] FIG. 3 is an exemplary drawing showing a battery according to a second embodiment of the present invention.
[0032] Figure 4 is an exemplary drawing showing an enlarged area B of the battery of Figure 3.
[0033] FIG. 5 is an exemplary drawing comparing and evaluating a flexible battery having only a protruding pattern formed according to one embodiment of the present invention and a flexible battery having a protruding pattern and a depression formed therein.
[0034] Figure 6 is an exemplary drawing showing a reinforcing structure for an exterior material formed in a recessed portion in the present invention.
[0035] Figure 7 is a flowchart of a method for manufacturing a battery in the present invention.
[0036] Figure 8 is an exemplary drawing showing the pattern depth formed in each manufacturing step of the outer material in the present invention.
[0037] Below, with reference to the attached drawings, embodiments of the present invention are described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein. In the drawings, irrelevant parts have been omitted for clarity of description, and similar reference numerals have been used throughout the specification to indicate similar elements.
[0038] Throughout the specification, when it is said that a part "includes" a component, unless otherwise specifically stated, this does not mean that other components are excluded, but rather that other components may be included. Furthermore, throughout the specification, when it is said that a part is "connected" to another part, this includes not only cases where they are directly connected, but also cases where they are connected via another component, and cases where other elements are electrically connected between them. Furthermore, throughout the specification, when it is said that a part is located "on" another part, this includes not only cases where a part is in contact with another part, but also cases where another component exists between the two parts.
[0039] The battery, or electrochemical cell, according to the present invention may be a lithium ion battery. Specifically, the electrochemical cell according to the present invention may be configured such that the electrode assembly is contained and sealed within an outer case together with an electrolyte, and is charged and discharged by the movement of lithium ions. The electrochemical cell according to the present invention may be configured to be flexible and bendable while maintaining its function. Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.
[0040] FIG. 1 is an exemplary drawing showing a battery according to a first embodiment of the present invention, and FIG. 2 is an exemplary drawing showing an enlarged area A of the battery of FIG. 1. According to the first embodiment, the battery (10) is designed such that the distance between at least two recessed portions formed on a first convex portion among at least one convex portion and the distance between at least two recessed portions formed on a second convex portion are equal.
[0041] Referring to FIG. 1, a battery (10) according to a first embodiment of the present invention may include an outer case (100), an electrode assembly, and an electrode lead (102). The electrode assembly may include a plurality of electrodes, may further include an active material and a separator, and may be formed in a structure in which these are laminated in the thickness direction.
[0042] The electrode may include first and second electrode plates of different polarities, and an active material may be applied to both surfaces or single surfaces of each of the first and second electrode plates. A separator may be interposed between the first and second electrode plates. For example, the first electrode plate may be a current collector used as a negative electrode, such as copper, aluminum, or stainless steel, and the negative electrode active material may be carbon, lithium, silicon, or SiO. xIt can be composed of one or more combinations of silicon derivatives, silicon-graphite composites, tin, and silicon-tin composites. In addition, the second electrode plate may be composed of a current collector used as a positive electrode made of aluminum, stainless steel, etc., and the positive electrode active material may be composed of one or more combinations of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium cobalt-manganese oxide, lithium cobalt-nickel oxide, lithium manganese-nickel oxide, lithium cobalt-nickel-manganese oxide, lithium cobalt-nickel-aluminum oxide, and lithium iron phosphate. The electrode assembly may have a shape in which the first and second electrode plates extend in the longitudinal direction among the two directions in which they form a plane, longer than the width direction, and thin in the thickness direction in which the active material and the separator are laminated, which intersects (for example, is perpendicular to) the direction in which the plane is formed.
[0043] Additionally, the electrode assembly may include electrode connection tabs and lead connection tabs. The electrode connection tabs may be formed to protrude from one longitudinal end of the first and second electrode plates, and electrode connection tabs protruding from electrodes having the same polarity may be coupled to each other. By the electrode connection tabs, the electrodes may be electrically connected in parallel. The lead connection tabs are connected to the electrode leads (102), and may protrude from the positive and negative electrode plates and be coupled to the electrode leads (102).
[0044] The outer covering (100) according to the first embodiment of the present invention is formed to accommodate an electrode assembly. The outer covering (100) may be formed of a laminated film including, for example, polypropylene (PP), metal, and nylon layers. In addition to nylon, a combination of other materials such as polyethylene terephthalate (PET), polyvinyl chloride (PVC), polycarbonate (PC), polyethylene (PE), and polyimide (PI) is also possible.
[0045] More specifically, the outer material (100) of the first embodiment is formed with a concave-convex pattern (120) including at least one concave portion (122) and at least one convex portion (121). At least one concave portion (122) and at least one convex portion (121) have an edge area (130) that forms a boundary line that contacts a sealing portion (140) at an end in one direction corresponding to the width of the battery.
[0046] The edge area (130) may include a boundary line between the uneven pattern (120) and the sealing portion (140). That is, as illustrated in FIG. 1, the edge area (130) may include two points of each uneven pattern (120) that touch the sealing portion (140) and a boundary line extending along the gap between the two points. The boundary line of the edge area (130) may extend approximately in a straight line along the flat sealing portion (140), and may be connected to the boundary line of the edge area (130) of the adjacent uneven pattern (120) to extend as a single line.
[0047] For example, the uneven pattern (120) is a pattern that extends in one direction and is repeatedly arranged in a direction intersecting the one direction, and specifically, may alternately protrude or recess (i.e., alternately protrude in opposite directions) in the thickness direction, so as to have an uneven shape along the one direction. Here, the one direction may be the width direction described above, and the direction in which the uneven pattern (120) is repeated may be the length direction. By the uneven pattern (120) that protrudes and recesses, the outer material (100) forming the receiving portion (110) may form a wave or wrinkle pattern in the length direction.
[0048] Below, the uneven pattern (120) will be described in more detail with reference to FIG. 2.
[0049] A recessed portion (123) is formed in a portion of the convex portion (121) where a portion of the convex portion (121) is recessed. For example, a recessed portion (123) in a dot shape may be formed in the central region of the convex portion (121). Here, at least two recessed portions (123) are formed in one direction corresponding to the width of the battery in each of at least one convex portion (121).
[0050] At this time, the central area of the convex portion (121) may be an area set based on the central point based on the long axis (length direction axis) and short axis (width direction axis) of the convex portion (121).
[0051] For example, when setting a central region based on a central point based on a major axis of a convex portion (121) having a length L in the longitudinal direction and a minor axis of a convex portion (121) having a width W in the width direction, the central region may mean a region including a position spaced apart by 0.01L to 0.45L, 0.05L to 0.4L, 0.1L to 0.3L in the longitudinal direction and a position spaced apart by 0.01W to 0.45W, 0.05W to 0.4W, 0.1W to 0.3W in the width direction from the central point, but the present invention is not limited thereto.
[0052] In addition, it goes without saying that the recessed portion (123) may include not only the aforementioned dot shape but also one or more shapes selected from among a prism, a cylinder, and modified shapes thereof.
[0053] For example, the shape of the recessed portion (123) may include a tapered structure in which the area of the lower portion of the recessed portion (123) becomes narrower than the area of the upper portion in the thickness direction of the convex portion (121). In other words, it may include a shape in which the cross-sectional area becomes narrower in the thickness direction on the surface of the convex portion (121).
[0054] Since the shape of the recessed portion (123) includes a tapered structure, it may be advantageous in suppressing the occurrence of irregular electrode layer gaps and large gaps when the battery is bent.
[0055] For example, the outer diameter size of the recessed portion (123) can be freely adjusted within the range of the width length based on the width length of the convex portion (121).
[0056] For example, when the width length of the convex portion (121) is W, the outer diameter size of the recessed portion (123) may be 0.1W to 0.9W, 0.2W to 0.9W, 0.3W to 0.9W, 0.3W to 0.85W, or 0.3W to 0.8W, but is not limited thereto. Here, the outer diameter means the largest diameter of the recessed portion (123) formed at the uppermost end of the convex portion (121).
[0057] In addition, the depth of the recessed portion (123) can be freely adjusted within the range of the height based on the height of the convex portion (121).
[0058] For example, when the height of the convex portion (121) is H, the depth of the recessed portion (123) may be, but is not limited to, 0.05H to 0.9H, 0.1H to 0.9H, 0.1H to 0.8H, 0.2H to 0.8H, 0.3H to 0.8H, 0.4H to 0.8H, or 0.5H to 0.8H.
[0059] However, as described above, in order to effectively suppress the occurrence of irregular electrode layer gaps and large gaps when bending the battery, it may be advantageous for the size of the shape of the recessed portion (123) based on the outer diameter size of the recessed portion (123) and the depth of the recessed portion (123) to be within the range described above.
[0060] For example, the widths of the convex portion (121) and the concave portion (122) may be the same or different, but regardless of the widths of the convex portion (121) and the concave portion (122), the same effect can be achieved by forming a sunken portion (123) in which a portion of the convex portion (121) is sunken as described above.
[0061] Referring to FIG. 2, for example, the spacing (150) between at least two recessed portions (123a) formed on a first convex portion (121a) among at least one convex portion (121) and the spacing (150) between at least two recessed portions (123b) formed on a second convex portion (121b) located next to the first convex portion (121a) are designed to be the same.
[0062] Here, the recessed portion (123) formed in the first convex portion (121a) is formed to have an edge area (130) and a first gap (135a, 135b). To this end, at least two recessed portions (123a, 123b) may be formed at a point spaced apart from the edge areas (130) located at both ends of the outer material (100) by 0.1K to 0.4K, preferably 0.15K to 0.35K, more preferably 0.2K to 0.35K, and even more preferably 0.25K (1 / 4K), based on the distance K between the edge areas (130) at both ends.
[0063] For example, one of the at least two recessed portions (123a) formed in the first convex portion (121a) may be formed to have a first gap (135a) from an edge area (130a) located at one end of the outer covering (100), and the other of the at least two recessed portions (123a) formed in the first convex portion (121a) may be formed to have a first gap (135b) from an edge area (130b) located at the other end of the outer covering (100). This design is to support the at least two recessed portions so that, when the battery (10) is deformed, the internal electrodes are not lifted and deformed into the empty space between the uneven pattern of the outer covering (100) and the electrode assembly, or, in severe cases, the electrodes are not bent. For example, the first gap (135a, 135b) is when the distance between the convex portion and the depressions located on the adjacent convex portion is the same, and specifically, it can mean a point that is 1 / 4 of the length between the edge regions of both ends from one edge region.
[0064] Specifically, since the recessed portion (123) formed in the first convex portion (121a) is formed to have an edge region (130) and a first gap (135a, 135b), according to the bending evaluation result of the battery (10), when the distance between the positive and negative electrode layers inside the outer covering (100) is 0.02 mm before bending the battery (10), when the battery (10) is bent 100 times and when it is bent 3,000 times, the distance between the electrode layers of 0.02 mm is maintained in all cases, thereby suppressing the deterioration of battery performance and the deterioration of the durability of the outer covering (100) due to the occurrence of an irregular electrode layer gap and a large gap, and at the same time suppressing lithium plating that may occur due to the enlarged electrode layer gap, thereby eliminating the risk of safety.
[0065] FIG. 3 is an exemplary drawing showing a battery according to a second embodiment of the present invention, and FIG. 4 is an exemplary drawing showing an enlarged area B of the battery of FIG. 3.
[0066] According to the second embodiment, the battery (20) is designed such that the spacing between at least two recessed portions formed on the first convex portion among at least one convex portion and the spacing between at least two recessed portions formed on the second convex portion are different.
[0067] Referring to FIG. 3, a battery (20) according to a second embodiment of the present invention may include an outer case (200), an electrode assembly, and an electrode lead (202). The electrode assembly may include a plurality of electrodes, may further include an active material and a separator, and may be formed in a structure in which these are laminated in the thickness direction.
[0068] Additionally, the electrode assembly may include electrode connection tabs and lead connection tabs. The electrode connection tabs may be formed to protrude from one longitudinal end of the first and second electrode plates, and electrode connection tabs protruding from electrodes having the same polarity may be coupled to each other. By the electrode connection tabs, the electrodes may be electrically connected in parallel. The lead connection tabs are connected to the electrode leads (202), and may protrude from the positive and negative electrode plates and be coupled to the electrode leads (202).
[0069] The outer material (200) according to the second embodiment of the present invention is formed to accommodate an electrode assembly.
[0070] Specifically, the outer material (200) includes a receiving portion (210) and a sealing portion (240). The receiving portion (210) forms a space for receiving an electrode assembly, and the sealing portion (240) can be joined to seal the received electrode assembly from the outside. For example, the receiving portion (210) can correspond to an area of two outer materials (200) that face each other while being spaced apart from each other. In order to form the receiving portion (210), the outer material (200) can be processed to be pressed and protruded in the thickness direction so that a preset area of the outer material (200) has the shape of a roughly rectangular bowl (or cup).
[0071] More specifically, the outer material (200) of the second embodiment is formed with a concave-convex pattern (220) including at least one concave portion (222) and at least one convex portion (221). At least one concave portion (222) and at least one convex portion (221) have an edge area (230) that forms a boundary line that contacts a sealing portion (240) at an end in one direction corresponding to the width of the battery.
[0072] For example, the uneven pattern (220) is a pattern that extends in one direction and is repeatedly arranged in a direction intersecting the one direction, and specifically, may alternately protrude or recess (i.e., alternately protrude in opposite directions) in the thickness direction, so as to have an uneven shape along the one direction. Here, the one direction may be the width direction described above, and the direction in which the uneven pattern (120) is repeated may be the length direction. By the uneven pattern (120) that protrudes and recesses, the outer material (100) forming the receiving portion (110) may form a wave or wrinkle pattern in the length direction.
[0073] Below, the uneven pattern (220) will be described with reference to FIG. 4.
[0074] A recessed portion (223) is formed in the convex portion (221) by sinking a portion of the convex portion (221). At this time, the shape and size of the recessed portion (223) are the same as those described above, and a detailed description thereof is omitted.
[0075] For example, if a dot-shaped recessed portion (223) is formed in the center region of the convex portion (221), a dot-shaped recessed portion (223) may be formed in the outer region of the next convex portion (221). Here, at least two recessed portions (223) are formed in one direction corresponding to the width of the battery in each of at least one convex portion (221). For example, the widths of the convex portion (221) and the concave portion (222) may be the same or different, but the same effect may be achieved regardless of the widths.
[0076] Referring to FIG. 4, for example, the spacing (250) between at least two recessed portions (223a) formed in the first convex portion (221a) among at least one convex portion (221) and the spacing (251) between at least two recessed portions (223b) formed in the second convex portion (221b) located next to the first convex portion (221a) are designed to be different.
[0077] Here, the recessed portion (223a) formed in the first convex portion (221a) is formed to have an edge area (230a) and a second gap (250a), and the recessed portion (223b) formed in the second convex portion (221b) is formed to have an edge area (230b) and a third gap (250b).
[0078] To this end, at least two recessed portions (223a) formed in the first convex portion (221a) may be formed at a point spaced apart from each of the edge areas (230a) located at both ends of the outer material (100) by 0.1K to 0.25K, preferably 0.15K to 0.25K, and more preferably 0.2K (1 / 5K) based on the distance K between the edge areas (230a) at both ends.
[0079] In addition, at least two recessed portions (223b) formed in the second convex portion (221b) may be formed at a point that is 0.25K' to 0.4K', preferably 0.25K' to 0.35K', and more preferably 0.33K' (1 / 3K') apart from each of the edge areas (230b) located at both ends of the outer material (100) based on the distance K' between the edge areas (230b) at both ends.
[0080] Specifically, at least two recessed portions (223a) formed in the first convex portion (221a) are formed at a point that is 1 / 5 of the length (K) between the edge regions (230a) located at both ends of the outer material (100), so that at least two recessed portions (223a) have a second gap (250a), and at least two recessed portions (223b) formed in the second convex portion (221b) are formed at a point that is 1 / 3 of the length (K') between the edge regions (230b) located at both ends of the outer material (100), so that at least two recessed portions (223b) have a third gap (250b). In this case, if the depression is formed so as to deviate from the edge region by 1 / 5 of the length between the edge regions at both ends, the depression may not be able to suppress the internal electrode from being lifted in the cell width direction (large gap).
[0081] In addition, if the two depressions are crowded in the center of the outer material by forming the depressions so that they deviate from the edge area by 1 / 3 of the length between the edge areas of both ends (i.e., the distance between the depressions is equal to or smaller than the outer diameter of the depressions), interference occurs between the depressions, which deforms the shape of the outer material and cannot have the effect of suppressing the gap between the electrodes from growing (large gap).
[0082] For example, one of the at least two recessed portions (223a) formed in the first convex portion (221a) is formed to have an edge area (230a) located at one end of the outer material (100) and a second gap (250a), and at least two recessed portions (223b) formed in the second convex portion (221b) are formed to have an edge area (230b) located at one end of the outer material (100) and a third gap (250b).
[0083] In the same manner, one of the at least two recessed portions (223b) formed on the first convex portion (221a) may be formed to have a second gap with an edge area (not shown) located at the other end of the outer material (100), and one of the at least two recessed portions (223b) formed on the second convex portion (221b) may be formed to have a third gap with an edge area (not shown) located at the other end of the outer material (100).
[0084] This design is to prevent the inner electrodes from being lifted and deformed into the empty space between the uneven pattern of the outer material (100) and the electrode assembly, or in severe cases, from being bent, when the battery (10) is deformed.
[0085] Specifically, at least two depressed portions (223a) formed in the first convex portion (221a) are formed to have an edge area (230) and a second gap (250a), and at least two depressed portions (223b) formed in the second convex portion (221b) are formed to have an edge area (230) and a third gap (250b), so that according to the bending evaluation result of the battery (20), when the distance between the positive and negative electrode layers inside the outer material (200) is 0.02 mm before bending the battery (20), when the battery (20) is bent 100 times and when it is bent 3,000 times, the distance between the electrode layers of 0.02 mm is maintained, thereby preventing deterioration of battery performance and deterioration of the durability of the outer material (100) due to occurrence of an irregular electrode layer gap and a large gap. By suppressing lithium plating that may occur due to the gap between electrode layers increasing while simultaneously suppressing it, safety risks can be eliminated.
[0086] The exterior material (100) in the first embodiment and the exterior material (200) in the second embodiment include a receiving portion (110, 210) and a sealing portion (140, 240).
[0087] The receiving portion (110, 210) forms a space for receiving the electrode assembly, and the sealing portion (140, 240) can be joined to seal the received electrode assembly from the outside. To form the receiving portion (110, 210) in the outer material, the outer material (100, 200) can be processed by pressing the sealing portion (140, 240) in the thickness direction so that a predetermined area of the outer material (100, 200) has the shape of a roughly square bowl (or cup).
[0088] The sealing portion (140, 240) seals the electrode assembly by bonding the sealing surfaces along the edges of the receiving portion (110, 210). For example, the sealing surface refers to the surface of the outer material (100, 200), and by bonding two sealing surfaces overlapping along the edges of the receiving portion (110, 210), the internal space (receiving portion (110, 210)) can be isolated from the outside. Here, the electrode assembly and electrolyte described above can be accommodated in the internal space, and the electrode assembly and electrolyte can be maintained in a sealed state.
[0089] In addition, the sealing portion (140, 240) may have a flat plate shape extending in the width direction or the length direction. For example, the flat plate shape of the sealing portion (140, 240) may be a shape that is not curved so that the surfaces face each other. Alternatively, the sealing portion (140, 240) may have a pattern different from the uneven pattern (120, 220), for example, the sealing portion (140, 240) may have a pattern with a lower height than the uneven pattern (120, 220) in the thickness direction of the exterior material (100, 200).
[0090] According to one embodiment of the present invention, the outer shell (100, 200) is formed so that the uneven pattern (120, 220) of the receiving portion (110, 210) and the sealing portion (140, 240) are in close contact. Accordingly, a space between the uneven pattern (120, 220) and the sealing portion (140, 240), where stress may be concentrated, is not formed in the present embodiment. By eliminating the structurally vulnerable portion, there is an effect that the possibility of damage to the end portion of the uneven pattern or the sealing portion (140, 240) in one direction in a usage environment where repetitive bending is applied can be significantly reduced. Therefore, the battery (10, 20) and the outer shell (100, 200), which correspond to the electrochemical cell according to the present invention, can have improved durability without further reinforcing or adding materials, and the possibility of breakage and leakage can be reduced, thereby improving safety.
[0091] Meanwhile, the electrode leads (102, 202) are connected to the electrode assembly inside the outer material (100, 200) and extend to be exposed to the outside of the outer material (100, 200). The electrode leads (102, 202) function as terminals for electrical connection with the electrode assembly accommodated inside the outer material (100, 200), and can be joined to penetrate the sealing portion (140, 240) while being interposed between the sealing surfaces when the sealing portion (140, 240) is formed. A pair of electrode leads (102, 202) of the positive and negative electrodes can be connected to each other with the same poles as the lead connection tabs provided in the electrode assembly.
[0092] FIG. 5 is a diagram showing the results of torsion and twist evaluations of a flexible battery manufactured by applying an outer material having only a rough pattern according to a comparative example and a flexible battery manufactured by applying an outer material having a rough pattern and a depressed portion according to an embodiment of the present invention. Referring to FIG. 5, the present invention forms a depressed portion (123, 223) of a dot pattern on a convex portion (121, 221) of an outer material (100, 200) (without a reinforcing structure), thereby suppressing the occurrence of irregular electrode layer gaps and large gaps that occur when deformation such as bending, twisting, or torsion is applied to the battery.
[0093] Hereinafter, a first flexible battery using an outer material having only a protruding-concave pattern including convex portions (121, 221) and concave portions (122, 222) according to a conventional comparative example and a second flexible battery using an outer material having a protruding-concave pattern including convex portions (121, 221) and concave portions (122, 222) according to the first and second embodiments of the present invention and a depressed portion (123, 223) formed on the convex portions (121, 221) will be described by comparison. For example, an experiment can be performed by applying a torsion of ±15° to the first flexible battery based on a predetermined cycle, and applying a twist of ±22.5° and a torsion of ±40° to the second flexible battery.
[0094] For example, after recording the OCV (Open Circuit Voltage) and AC impedance (1,000 Hz) values of the initial battery with each flexible battery 100% charged, insulation treatment is performed by attaching PI (Polyimide) tape to the terminals of each flexible battery, and then each flexible battery is fixed to the clamp of the test equipment.
[0095] The clamps that hold both ends of the flexible battery can be evaluated for torsion, in which one clamp is repeatedly twisted at a constant angle, and twist, in which two clamps are rotated and twisted at + and - angles in opposite phases.
[0096] Afterwards, the OCV and AC impedance (1,000 Hz) values of the flexible battery are measured according to the evaluation method, and the deformation of the exterior material of the flexible battery, cracks, leakage, ignition, explosion, etc. are checked before and after the evaluation.
[0097] Specifically, in the case of the comparative example (first flexible battery), it was observed that the outer shape of the pouch of the battery was deformed, and also, after the twist evaluation, 14 irregular electrode layer gaps were found inside the first flexible battery.
[0098] However, according to the first and second embodiments of the present invention, when the OCV and AC impedance values of the second flexible battery were measured after evaluation of torsion or twist (maximum twisting angle + / - 45 degrees, 3,000 times), it was confirmed that the OCV and AC impedance values (1000) did not significantly decrease or increase from the initial values, and the external shape of the pouch of the battery also did not significantly change. In addition, in order to impart flexibility, when a dot-shaped recessed portion was formed on the convex portion in order to suppress the gap of irregular electrode layers (increased distance between positive and negative electrodes) inside the outer packaging material due to repeated deformation on the convex portion formed in the width direction of the battery, in the second flexible battery to which the first embodiment (straight-shaped dot pattern) and the second embodiment (dispersed dot pattern) were applied, no irregular electrode layer gaps or large gaps were found inside, and no deformation, cracks, or leakage of the external pouch of the battery occurred.
[0099] Through these experimental results, it can be confirmed that a flexible battery in which a rough pattern is formed and a dot-patterned depression is formed on a convex portion can perform stable electrochemical operation even when evaluated under harsh torsion or twisting, and that the pouch crack and mechanical durability are also significantly improved.
[0100] FIG. 6 is an exemplary drawing illustrating a reinforcing structure further included in an exterior material having a recessed portion formed therein according to the present invention. Referring to FIGS. 1 to 6, a battery (10, 20) is formed with a reinforcing structure (500, 510a, 510b) for an exterior material (100, 200).
[0101] The (a) plan view, (b) side view, and (c) internal view of the outer casing (100) according to the first embodiment are illustrated, and in the battery (10), a reinforcing structure (500) for the outer casing (100) is formed in at least two recessed portions (123) formed in the convex portion (121) of the outer casing (100). For example, in the case of the battery (10) designed so that the interval between at least two recessed portions (123a) formed in the first convex portion (121a) of at least one convex portion (121) and the interval between at least two recessed portions (123b) formed in the second convex portion (121b) located next to the first convex portion (121a) are the same, the reinforcing structure (500) for the outer casing (100) is formed in the recessed portion (123).
[0102] In addition, although not shown in the drawing, a reinforcing structure (500) for the exterior material (100) may be formed in the recessed portion (123), and a reinforcing structure (510b) for the exterior material (100) may be formed in other external areas of the exterior material.
[0103] The (d) plan view, (e) side view, and (f) internal view of the outer casing (200) according to the second embodiment are illustrated, wherein the battery (20) has at least two recessed portions (223) formed in the convex portion (221) of the outer casing (200) and / or reinforcing structures (510a, 510b) formed in other external areas of the outer casing (200). For example, in the case of a battery (20) designed such that the interval between at least two depressed portions (223a) formed in a first depressed portion (221a) of at least one of the convex portions (221) and the interval between at least two depressed portions (223b) formed in a second depressed portion (221b) located next to the first convex portion (221a) are different, a reinforcing structure (510a) for the outer material (200) is formed in the depressed portion (223), and a reinforcing structure (510b) for the outer material (200) is formed in an external area of the outer material other than the recessed portion (223).
[0104] These reinforcing structures (500, 510a, 510b) may be polymers. In particular, the reinforcing structures (500, 510a, 510b) may be composed of an elastomer having a shore hardness of at least 60 among polymers. The elastomer includes, for example, butyl rubber, ethylene-vinyl acetate copolymer (EVA), isoprene (IR), natural rubber (NR), neoprene (CR), polyurethane elastomers, silicone elastomers, etc.
[0105] Let us assume that silicone elastomer is used as the reinforcing structure (500, 510a, 510b). Here, the reinforcing structure (500, 510a, 510b) can be molded at a molding temperature of 90°C, a molding time of 120 seconds, and a molding pressure of 4 MPa.
[0106] For example, when using a silicone elastomer with a low hardness of about 30 to 50 Shore hardness, the reinforcing structure (500, 510a, 510b) does not perform the function of preventing deformation of the sunken part, and thus is not suitable as a reinforcing structure (500, 510a, 510b).
[0107] However, in the case of using a silicone elastomer having a Shore hardness of at least 60, as in the present invention, the reinforcing structure (500, 510a, 510b) has the advantage of being easy to mold, being able to prevent deformation of the sunken portion, and being able to properly perform the function of preventing the battery from bending.
[0108] In addition, when bending 3000 times at a radius of curvature of 15 mm was performed on the flexible battery, there was no destruction or damage to the reinforcing structure (500, 510a, 510b), and since the reinforcing structure (500, 510a, 510b) is attached to the surface of the battery, the adhesive strength with heterogeneous materials (PET, NY, and silicone) is also superior to that using a general adhesive, and the process of attaching the adhesive can be omitted during molding, which can provide the advantage of simplifying the process.
[0109] Additionally, the occurrence of cracks can be suppressed compared to cracks in a flexible battery to which the reinforcing structure (500, 510a, 510b) is not attached.
[0110] In addition, as a result of comparing the shape and number of cracks in flexible batteries to which reinforcing structures (500, 510a, 510b) with low Shore hardness (e.g., 30 to 50) were applied, the size of the cracks was smaller and the number of cracks was also significantly lower in batteries to which silicone elastomer with Shore hardness of 60 or higher was applied, so when using silicone elastomer, it is preferable to use a Shore hardness of 60 (elastic modulus of 0.16 kgf / mm2) or higher. At this time, the upper limit of the Shore hardness of the reinforcing structures (500, 510a, 510b) is not limited as long as it does not cause damage to the flexible battery due to curing during the forming process of the reinforcing structures (500, 510a, 510b), but may have a value of 100 or less.
[0111] The pouch damage of the outer material (100, 200) formed at the center of the battery in which the electrode assembly (101, 201) is accommodated by repeated deformation (bending) can be minimized.
[0112] The reinforcing structures (500, 510a, 510b) arranged in the uneven pattern (120, 220) prevent the battery from being deformed beyond a standard range or a limit, thereby preventing the risk of change in the electrode interface caused by deformation of the pouch shape when the battery is repeatedly bent or excessively bent. Through this, the distance between the negative electrode and the positive electrode, which should be in close contact, is prevented from increasing as the gap between the electrode layers (Electrode Layer Gap) laminated within the pouch (outer material) increases, and a rapid increase in resistance or Li plating issues can be prevented.
[0113] The method for manufacturing an outer material (100, 200) according to the present invention may be a method for processing an outer material (100, 200), accommodating and sealing an electrode assembly (101, 201), and assembling an electrochemical cell (10). The method for manufacturing an outer material (100, 200) according to the present invention includes a step of forming a concave-convex pattern (120, 220) and a step of forming a sealing portion (140, 240). The step of forming the concave-convex pattern (120, 220) may be a step of deforming the outer material (100, 200) by applying pressure, etc., and the step of forming the sealing portion (140, 240) may be a step of bonding the outer material (100, 200) to accommodate the electrode assembly (101, 201).
[0114] In addition, in the step of forming the sealing portion (140, 240) of the present invention, an overlapping area, which is a part of the uneven pattern (120, 220), may be combined to overlap with the sealing portion (140, 240). The overlapping area may be an end portion in one direction (width direction) of the uneven pattern (120, 220), and the overlapping area may overlap with the sealing portion (140, 240) so that the two sealing surfaces may be joined. Consequently, the overlapping area may be processed to form a part of the uneven pattern (120, 220) when the uneven pattern (120, 220) is formed, and may ultimately be included in one area of the sealing portion (140, 240). Accordingly, an edge area (130, 230) may be formed between the overlapping area and the uneven pattern (120, 220).
[0115] FIG. 7 is a diagram showing a flow chart of a method for manufacturing a battery (10) described through the first embodiment and a battery (20) described through the second embodiment, wherein each battery can be manufactured through the same process.
[0116] In step S610, at least one convex portion (121, 221) may be formed in one direction on the outer material (100, 200). For example, at least one convex portion (121, 221) may be positioned between two concave portions (122, 222) and may be formed to protrude in the opposite direction to the concave portions (122, 222).
[0117] Based on the width of the convex portion, the outer diameter of the recessed portion can be designed to be 30 to 85% of the width of the convex portion. If the outer diameter of the recessed portion is less than 30% of the width of the convex portion, it cannot prevent the occurrence of irregular electrode interlayer gaps and large gaps. If the outer diameter of the recessed portion is greater than 85%, there is a problem of interfering with neighboring recessed portions, thereby deforming the shape of the recessed portion.
[0118] In step S620, a recessed portion (123, 223) may be formed in at least one convex portion (121, 221). For example, when the width of the convex portion (121, 221) is W, the outer diameter size of the recessed portion (123) may be, but is not limited to, 0.3W to 0.85W, or 0.35W to 0.8W.
[0119] For example, a recessed portion (123, 223) can be formed by a precision pneumatic press that presses a punch processed in a dot shape. Here, the precision pneumatic press is configured as a four-axis set in which a punch and a die are equipped with a ball bushing, and the gap between the punch and the die is physically controlled by a limit block, thereby adjusting the depth of the recessed portion (123, 223) and preventing damage to the outer material (100, 200) by controlling the press dropping speed.
[0120] In step S630, at least one concave portion (122, 222) may be formed adjacent to the convex portion (121, 221). The concave portion (122, 222) may be formed to protrude toward the internal space of the receiving portion (110), i.e., toward the electrode assembly (101, 201) to be received. In addition, the convex portion (121, 221) may be positioned between two concave portions (122, 222) and may be formed to protrude in the opposite direction to the concave portions (122, 222).
[0121] Here, the step of forming the concave portion (122, 222) can be performed before or after the step of pressing the outer material (100, 200) in which the convex portion (121, 221) is formed, which will be described later, and when the concave portion (122, 222) is formed after pressing the outer material (100, 200) in which the convex portion (121, 221) is formed, additional pressing can be performed on the outer material (100, 200).
[0122] In step S640, an electrode assembly (101, 201) can be inserted into an outer material (100, 200) in which a recessed portion (123, 223) is formed.
[0123] In step S650, the outer material (100, 200) into which the electrode assembly (101, 201) is inserted can be sealed.
[0124] Although not shown in FIG. 7, the step of pressing the outer material (100, 200) in which the convex portions (121, 221) are formed may further be included. At this time, the step of forming the recessed portions (123, 223) may include the step of forming the recessed portions (123, 223) in the convex portions (121, 221) of the pressed outer material (100, 200).
[0125] In the above description, steps S610 to S650 may be further divided into additional steps or combined into fewer steps, depending on the implementation of the present invention. Furthermore, some steps may be omitted as needed, and the order of the steps may be switched.
[0126] For example, the process may be performed by first forming a concave portion (122, 222) in the outer material (100, 200), then sequentially pressing the formed concave portion (122, 222), forming a convex portion (121, 221), and forming a depressed portion (123, 223) in the formed convex portion (121, 221). That is, the process may proceed in the following order: forming a concave portion in the outer material -> pressing -> forming a convex portion -> forming a depressed portion.
[0127] Additionally, it is obvious that the process can proceed in the following order: forming a concave part in the outer material -> pressing -> forming a convex part -> additional pressing -> forming a sunken part.
[0128] At this time, the depth of the depression formed in the convex portion can be freely adjusted within the range of the height based on the height of the convex portion. For example, when the height of the convex portion is H, the depth of the depression can be 0.05H to 0.9H, 0.1H to 0.9H, 0.1H to 0.8H, 0.2H to 0.8H, 0.3H to 0.8H, 0.4H to 0.8H, or 0.5H to 0.8H, but is not limited thereto.
[0129] Hereinafter, with reference to Fig. 8, the pattern depth for each process, including the depth of the sunken part, will be described as an example.
[0130] Fig. 8 is an exemplary drawing illustrating the pattern depth formed on the outer material according to each process in the present invention. With respect to Fig. 8, the process of performing additional pressing on the outer material (100, 200) in which convex portions (121, 221) are formed, and then the process of forming a concave portion (122, 222) on the outer material (100, 200) after pressing, and the pattern depth for each process are described below.
[0131] Referring to drawing (a) of FIG. 8, at least one convex portion (801) may be formed in one direction of the outer material (800). For example, at least one convex portion (801) having a pattern depth of 0.45 to 0.50 mm may be formed in the outer material (800).
[0132] Referring to drawing (b) of FIG. 8, pressing (802) can be performed on an outer material (800) having a convex portion (801) formed thereon. For example, pressing (802) can be performed on an outer material (800) having a convex portion (801) formed thereon so that the pattern depth becomes 0.30 to 0.35 mm through pressing (802) of the convex portion (801).
[0133] Referring to drawing (c) of FIG. 8, a recessed portion (803) may be formed in a convex portion (801) of a pressed outer material. For example, in an outer material (800) in which a convex portion (801) is formed, at least two recessed portions (803) having a pattern depth of 0.40 to 0.45 mm based on the maximum height of the pressed convex portion (801) may be formed.
[0134] Referring to drawing (d) of FIG. 8, at least one concave portion (804) may be formed at a position adjacent to a convex portion (801). For example, at least one concave portion (804) having a pattern depth of 0.65 to 0.70 mm may be formed on the outer material (800). At this time, the depth of the concave portion (804) pattern may be based on the maximum height of the pressed convex portion (801).
[0135] Referring to drawing (e) of FIG. 8, when the concave portion (804) is formed after pressing the formed outer covering (800) of the convex portion (801), additional pressing (805) may be performed on the outer covering (100, 200). For example, pressing (805) may be performed on the outer covering (800) on which the concave portion (804) is formed so as to have a pattern depth of 0.50 to 0.55 mm. At this time, the pattern depths of the finally formed convex portion (801) and concave portion (804) may be the same, and the pattern depth of the recessed portion (803) may satisfy the depth range of the recessed portion described above.
[0136] As described above, when the process proceeds in the order of forming a convex portion on the outer material -> pressing -> forming a dent portion -> forming a concave portion -> additional pressing, since pressing is performed after the convex portion is formed, the upper part of the convex portion is pressurized evenly, so that it is advantageous in that it is easy to form the dent portion at the correct position and with a uniform depth when forming the dent portion. Thereafter, since additional pressing is performed after the concave portion is formed, the pattern depth of the outer material is uniformly formed as a target value overall, thereby providing the advantage of increasing the accuracy of the pattern process and reducing the defect rate.
[0137] At this time, pressing is performed by adjusting the pressing pressure, time, gap, etc., so that the depression does not become severely deformed or there is no risk of being crushed.
[0138] In addition, even if pressing is performed twice, it has the advantage of not causing cracks due to destruction of the metal layer within the outer material when the depth of the pressed pattern is not pressed by more than 90% of the depth of the convex portion.
[0139] In this way, by simplifying the pattern process, it is possible to provide the advantage of reducing the defect rate and reducing the process time by shortening the process steps.
[0140] Meanwhile, separately from Fig. 8, the process of forming a concave portion before the step of pressing the outer material in which the convex portion is formed and the pattern depth for each process are described below.
[0141] At least one convex portion may be formed in one direction of the outer covering material. For example, the outer covering material may be formed with at least one convex portion having a pattern depth of 0.45 to 0.55 mm.
[0142] At least one concave portion may be formed adjacent to the convex portion. For example, at least one concave portion having a pattern depth of 0.70 to 0.75 mm may be formed on the exterior material. In this case, the concave portion pattern depth may be based on the maximum height of the convex portion, and when the concave portion is formed following the convex portion, the pattern depth of the convex portion may be formed to be equal to the pattern depth of the concave portion based on the lowest end of the concave portion.
[0143] When at least one concave portion is formed in the outer covering material, pressing may be performed on the outer covering material having at least one convex portion formed thereon. For example, pressing may be performed on the outer covering material having at least one convex portion formed thereon so that the convex portion has a pattern depth of 0.50 to 0.55 mm.
[0144] A depression may be formed in the convex portion of the pressed outer covering material. For example, in the pressed outer covering material having the convex portion formed, at least two depressions may be formed that satisfy the depth range of the depressions described above based on the maximum height of the convex portion.
[0145] As described above, when the process proceeds in the order of forming a convex part on the outer material -> forming a concave part -> pressing -> forming a depressed part, the pattern process is simplified, thereby providing the advantage of reducing the defect rate and reducing the process time by shortening the process steps.
[0146] Here, when forming convex and concave portions on the outer material before the pressing process, the pressure is not constant, so the concave portions can easily be pressed by the same load, resulting in an irregular pattern depth reduction. However, by performing the pressing process as a final step, optimization can be achieved through upper and lower mold designs to prevent severe, asymmetrical, or uneven deformation.
[0147] Additionally, it goes without saying that an additional pressing process may be included as needed after the formation of the depression.
[0148] The effects exerted by the recessed portion formed in the convex portion of the present invention are as follows. These effects may be obtained by performing the same evaluation on a conventional exterior material (where only the convex portion and the recessed portion are formed in the exterior material) and the exterior material of the present invention (where not only the convex portion and the recessed portion are formed in the exterior material, but also the recessed portion is formed in the convex portion).
[0149] Specifically, the evaluation methods included 1) conducting a bending evaluation (bending radius 15 mm, repeated 100 times) and then evaluating the cracks and damage of the exterior material, and 2) using CT imaging to check the internal electrode arrangement and degree of adhesion.
[0150] As a result of evaluating the conventional exterior material and the exterior material of the present invention, it was found that since the conventional exterior material does not form a dent, when repeatedly bent at a large curvature, or when the battery is misused or abused to bend or deform beyond the standard range or limit, cracks may occur in the exterior material due to the bending or folding of the battery, which may damage the battery, and this may cause a problem in that the electrolyte may leak.
[0151] On the other hand, the outer material of the present invention can minimize the occurrence of irregular electrode layer gaps and large gaps by forming a recessed portion in a convex portion.
[0152] In addition, it can be confirmed that when the flexible battery including the outer material with the depression and the reinforcing structure formed in the depression proposed in the present invention is repeatedly bent, no cracks occur in the outer material due to the resistance according to the strength and support capacity of the reinforcing structure. Specifically, when examining the interior of the outer material proposed in the present invention, it can be confirmed that the outer material of the present invention maintains a uniform gap between each electrode layer in all sections when bent.
[0153] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will readily appreciate that the present invention can be readily modified into other specific forms without altering the technical spirit or essential characteristics of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single entity may be implemented in a distributed manner, and similarly, components described as distributed may be implemented in a combined manner.
[0154] The scope of the present invention is indicated by the claims that follow rather than the detailed description, and all changes or modifications derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.
[0155] 10, 20: Battery, electrochemical cell
[0156] 100, 200: Exterior material
[0157] 101, 201: Electrode assembly
[0158] 102, 202: Electrode leads
[0159] 110, 210: Reception area
[0160] 120, 220: Uneven pattern
[0161] 121, 221: Convex part
[0162] 122, 222: Concave
[0163] 123, 223: Depression
[0164] 130, 230: Edge area
[0165] 140, 240: Sealing part
Claims
1. In the battery, An electrode assembly comprising a plurality of electrodes; and An outer material having a concave-convex pattern formed thereon, which accommodates the electrode assembly and includes at least one concave portion and at least one convex portion. Including, A battery in which a recessed portion is formed in the convex portion, where a portion of the convex portion is recessed.
2. In paragraph 1, A battery, wherein each of the at least one convex portion has at least two depressed portions formed in one direction corresponding to the width of the battery.
3. In paragraph 2, A battery, wherein the spacing between at least two recessed portions formed on a first convex portion among the at least one convex portion and the spacing between at least two recessed portions formed on a second convex portion located next to the first convex portion are designed to be the same.
4. In paragraph 2, A battery wherein the above-mentioned recessed portion is formed to have a first gap with the edge area of the outer material.
5. In paragraph 2, A battery, wherein the spacing between at least two recessed portions formed on a first convex portion among the at least one convex portion and the spacing between at least two recessed portions formed on a second convex portion located next to the first convex portion are designed to be different.
6. In paragraph 5, A battery, wherein the recessed portion formed in the first convex portion is formed to have a second gap with the edge area of the outer material.
7. In paragraph 5, A battery, wherein the recessed portion formed in the second convex portion is formed to have a third gap with the edge area of the outer material.
8. In paragraph 1, The above exterior material is, A receiving portion for receiving the electrode assembly; and A battery having a sealing portion that seals the electrode assembly by bonding sealing surfaces along the edges of the receiving portion.
9. In paragraph 8, A battery, wherein at least one concave portion and at least one convex portion have an edge area forming a boundary line that contacts the sealing portion at an end in one direction corresponding to the width of the battery.
10. In paragraph 8, A battery characterized in that the sealing portion has a pattern having a lower height than the uneven pattern in the thickness direction of the outer material.
11. In paragraph 1, A battery in which a reinforcing structure for the outer material is formed in the above-mentioned recessed portion.
12. In a method for manufacturing a battery, A step of forming at least one convex portion in one direction on the outer material; A step of forming at least one concave portion at a position adjacent to the convex portion; A step of forming a recessed portion in at least one of the above convex portions; A step of inserting an electrode assembly into the outer material in which the above-mentioned depression is formed; and A step of sealing the outer material into which the electrode assembly is inserted. A method for manufacturing a battery, comprising:
13. In paragraph 12, A step of pressing the outer material on which the above convex portion is formed Including more, A battery manufacturing method, wherein the step of forming the above-mentioned depression is to form the depression in the convex portion of the pressed outer material.
14. In paragraph 12, A battery manufacturing method, wherein the step of forming the concave portion is performed before or after the step of pressing the outer material on which the convex portion is formed.
15. In paragraph 14, In the case where the concave portion is formed after pressing the outer material on which the convex portion is formed, a step of additional pressing on the outer material A method for manufacturing a battery, comprising:
Citation Information
Patent Citations
Antioxidant, hair root improvement, and hair loss prevention and improvement composition comprising the viola papilionacea extract as an active ingredient, and food and external preparations containing the same
KR1020230119310A
Exterior package for flexible electrochemical device and electrochemical device including the exterior package
CN106450066A
Flexible battery and wearable device containing the same
KR1020160090108A
Brown asphalt
KR1020220058318A
Environmentally friendly power generation device
KR1020240020806A