Treatment method of waste battery

The method addresses the inefficiencies in recycling medium to large-sized batteries by automating the disassembly and processing of pack-type batteries to recover valuable metals, achieving high recovery rates and purity through a sequential discharging, shredding, firing, and wet processing approach.

WO2024248255A1PCT designated stage expired Publication Date: 2024-12-05KOREA ZINC CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/020320
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-16
Filing Date
2023-12-11
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current waste battery processing technologies are inadequate for efficiently recycling medium to large-sized batteries used in electric vehicles, as they lack integrated recycling methods to recover valuable metals from pack-type batteries, leading to inefficiencies and increased impurity contamination.

Method used

A method involving a discharging, disassembly, shredding, firing, grinding, and wet processing sequence to recover metals from pack-type batteries, which includes automated processes to minimize impurities and reduce the time required for metal recovery, focusing on the direct extraction of metal compounds like lithium hydroxide, lithium carbonate, and nickel cobalt manganese compounds.

Benefits of technology

This method significantly reduces the time and loss of metal components by dismantling batteries to the cell level, minimizing impurities, and achieving high recovery rates of lithium and manganese, while producing high-purity metal compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023020320_05122024_PF_FP_ABST
    Figure KR2023020320_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A treatment method of a waste battery according to the present invention comprises: a discharge process for discharging waste batteries; a disassembly process for disassembling the discharged waste batteries into individual cells; a crushing process for crushing the disassembled waste batteries; a firing process for firing the waste batteries crushed into the individual cells; a grinding process for grinding the fired waste batteries; and a wet process for extracting and collecting metal from the ground waste batteries.
Need to check novelty before this filing date? Find Prior Art

Description

How to dispose of waste batteries

[0001] The present invention relates to a method for processing waste batteries, and more particularly, to a method for recovering metal in the form of a compound from a pack-type battery whose lifespan has ended.

[0002] The recent expansion of the battery electric vehicle (BEV) market has led to an increase in demand for secondary batteries. Secondary batteries do not last forever and have a limited shelf life. After their lifespan has ended, secondary batteries can be disposed of, reused, or recycled. Research is ongoing to recover valuable rare metals within secondary batteries through recycling.

[0003] Previously, processing technology development focused primarily on small-sized waste batteries, leading to the development of component technologies rather than integrated process technologies. However, the recent increase in battery demand is driven by the growing demand for mid- to large-sized batteries, which power electric vehicles. Therefore, waste battery processing technologies targeting these batteries are needed. Furthermore, rather than focusing solely on individual component technologies, the development of integrated recycling technologies encompassing the entire battery, from the final product to the metal compound, is crucial.

[0004] The purpose of the present invention is to provide a method for processing waste batteries, which can efficiently recover metals in batteries in the form of compounds through a discharge process, a disassembly process, a crushing process, a sintering process, a grinding process, and a wet process from batteries in the form of packs whose lifespan has ended.

[0005] A method for processing waste batteries according to one embodiment of the present invention comprises a discharging process for discharging waste batteries; a dismantling process for dismantling the discharged waste batteries into cell units; a crushing process for crushing the dismantled waste batteries into cell units; a firing process for firing the crushed waste batteries; a crushing process for crushing the fired waste batteries; and a wet process for extracting and recovering metals from the crushed waste batteries.

[0006] The above-mentioned waste batteries may be batteries in packs whose lifespan has ended.

[0007] The method for processing waste batteries according to the present invention can discharge the waste batteries so that the voltage of the waste batteries becomes 30 V or less through the discharging process.

[0008] The method for processing waste batteries according to the present invention can crush batteries in cell units into sizes of 20 cm or less through the crushing process.

[0009] In the method for processing waste batteries according to the present invention, the process of separating black mass from the crushed waste batteries can be omitted.

[0010] In the waste battery processing method of the present invention, the discharging process, the disassembly process, the crushing process, the firing process, and the pulverization process can be performed continuously by automated equipment.

[0011] In the waste battery processing method of the present invention, the discharging process, the dismantling process, and the crushing process can be performed by automated equipment using a robot.

[0012] In the waste battery treatment method of the present invention, metal compounds can be recovered through the wet process.

[0013] The above metal compound may include at least one selected from the group consisting of lithium hydroxide, lithium carbonate, and lithium phosphate.

[0014] The above metal compound may include one sulfate selected from the group consisting of nickel, cobalt and manganese.

[0015] The above metal compound may include a nickel-cobalt-manganese compound in a solution state.

[0016] According to the present invention, by disassembling discharged waste batteries into cell units and then performing a wet process, the time required to recover metals in the form of compounds from the batteries can be shortened, and byproducts generated during the process operation can be reduced, thereby increasing the metal recovery rate.

[0017] In particular, the present invention can minimize the loss rate of metal components present in a pack-type battery by recovering metals directly through a wet process without a separate process of separating black mass after crushing / pulverizing the battery in cell units.

[0018] In addition, the present invention can drastically reduce the time required to recover metal in the form of a compound from a pack-type battery by automating the discharge, dismantling, crushing, firing and pulverizing processes excluding the wet process.

[0019] Figure 1 is a diagram showing the overall process of a waste battery processing method according to the present invention.

[0020] Figure 2 is an overall process diagram showing detailed processes of a waste battery processing method according to the present invention.

[0021] A method for processing waste batteries according to the present invention includes a discharging process for discharging waste batteries, a dismantling process for dismantling the discharged waste batteries into cell units, a crushing process for crushing the dismantled waste batteries into cell units, a firing process for firing the crushed waste batteries, a crushing process for crushing the fired waste batteries, and a wet process for extracting and recovering metals from the crushed waste batteries.

[0022] Hereinafter, the present invention will be described with reference to the drawings. Figure 1 is a diagram illustrating the overall process of a waste battery processing method according to the present invention. As illustrated in Figure 1, the waste battery processing method according to one embodiment of the present invention may include a discharging process (S100), a dismantling process (S200), a crushing process (S300), a firing process (S400), a grinding process (S500), and a wet process (S600).

[0023] Discharge process (S100)

[0024] The discharging process (S100) is a process for discharging the power accumulated in a waste battery to prevent an explosion of the waste battery that may occur during a subsequent process. For example, in the discharging process (S100), the waste battery may be connected to a discharger and discharged so that the voltage of the waste battery becomes 30 V or less, preferably 0.2 V or less. By discharging the waste battery to a voltage within the above-mentioned numerical range through the discharging process (S100), an explosion of the waste battery in the subsequent dismantling process (S200) can be prevented and its stability can be ensured.

[0025] The waste battery processing method according to the present invention can be performed on medium- to large-sized batteries used in electric vehicles. In this case, the waste batteries discharged through the discharge process (S100) may be batteries in packs whose lifespan has ended.

[0026] The discharge process (S100) can be performed through mechanical discharge using a discharger, or brine discharge using brine. Preferably, the discharge process (S100) is performed through mechanical discharge. Using mechanical discharge can ensure safety against fire and explosion, enable confirmation of the discharge status, and reduce discharge time and incidental costs.

[0027] Dismantling process (S200)

[0028] The dismantling process (S200) is a process for dismantling waste batteries in pack form into smaller units. The dismantling process (S200) according to the present invention dismantles waste batteries in pack form into cell units. For example, the dismantling process (S200) can dismantle waste batteries in pack form into modules and then into cells.

[0029] Although there is convenience in directly using waste batteries in packs for recycling, there is a problem that the inflow of impurities increases because the BMS (Battery Management System) and various control devices are also introduced. Therefore, in order to recycle batteries, they must be disassembled at least to the module level, and the present invention is characterized by disassembling waste batteries in pack form to the cell level rather than the module level. According to the present invention, compared to the case where waste batteries in pack form are disassembled to the module level, the present invention can significantly reduce the amount of impurities (e.g., Al and Fe) introduced into the recovered metal materials by disassembling waste batteries in pack form to the cell level. In addition, since the amount of aluminum introduced into the recovered metal materials is significantly less, there is an advantage in that a separate process for removing aluminum can be minimized in the recovery of metal materials.

[0030] Meanwhile, when dismantling a pack-type waste battery only down to the module unit, since the dry process (sintering process) is performed at a high temperature of at least 1200℃, manganese (Mn) is discharged as slag in the form of manganese oxide (MnO), making manganese recovery impossible, and lithium volatilizes in a gaseous state, which may reduce the lithium recovery rate. On the other hand, when dismantling a pack-type waste battery down to the cell unit as in the present invention, the temperature in the dry process can be relatively lowered, so manganese recovery is possible, unlike when dismantling a pack-type waste battery down to the module unit, and the lithium (Li) recovery rate can be significantly increased compared to when dismantling down to the module unit.

[0031] According to one embodiment, the disassembly process (S200) may be performed after the discharge process (S100), as illustrated in FIG. 1. However, the present invention is not limited thereto, and according to another embodiment, unlike as illustrated in FIG. 1, the disassembly process (S200) may be performed first, followed by the discharge process (S100).

[0032] Shredding process (S300)

[0033] The shredding process (S300) is a process for crushing waste batteries disassembled into individual cells. The shredding process (S300) can crush individual cells into sizes of 20 cm or less, specifically 15 cm or less, and more specifically 10 cm or less. By crushing batteries into sizes within the above numerical range through the shredding process (S300), the crushed batteries can be reduced and fired more uniformly in the firing process (S400).

[0034] The shredding process (S300) can be performed under a nitrogen (N2) atmosphere while spraying water to prevent sparks and explosions. After shredding, the sprayed water and electrolyte flowing from the spent battery can be removed. For example, the water and electrolyte can be removed by centrifugation using a rotary barrel.

[0035] The shredding process (S300) may include a drying process (not shown) for drying the shredded batteries.

[0036] According to the present invention, the above-described discharge process (S100), dismantling process (S200), and crushing process (S300) can be performed by automated equipment using a robot, thereby significantly reducing the time required to recover metal from waste batteries.

[0037] Firing process (S400)

[0038] The firing process (S400) is a process for dry processing the shredded batteries. Specifically, the firing process (S400) may be a process (IAR: Inert Atmospheric Roaster) for reducing and firing the shredded batteries in an inert gas atmosphere. For example, in the firing process (S400), the shredded batteries, which are 5 cm to 10 cm in size, may be reduced and fired in a nitrogen (N2) atmosphere at a temperature of 800°C to 900°C for 1 to 3 hours. By firing the shredded batteries in an inert gas atmosphere, lithium (Li) can be converted into a Li2CO3 form that can be dissolved in water. In the process of reducing and calcining the crushed batteries for lithium separation, some high-oxide compounds (Me2O3, Me=Ni, Co, Mn) are reduced to low-oxide compounds (MeO, Me=Ni, Co, Mn), which may reduce the amount of auxiliary materials (H2O2, hydrogen peroxide) used during sulfuric acid leaching.

[0039] Crushing process (S500)

[0040] The crushing process (S500) is a process for crushing batteries that have been dry-processed through the firing process (S400). For example, in the crushing process (S500), batteries that have been reduced and fired through a ball mill can be classified into 80% or more at 200 mesh or less.

[0041] The crushing process (S500) can be performed under a nitrogen (N2) atmosphere while spraying water to prevent sparks and explosions. After crushing, the sprayed water and electrolyte flowing from the spent battery can be removed. For example, the water and electrolyte can be removed by centrifugation using a rotary barrel.

[0042] In the waste battery processing method according to the present invention, a separate process for separating black mass after crushing / pulverizing individual cells is omitted. Since the present invention recovers metals directly through a wet process without a separate process for separating black mass, the loss rate of metal components present within pack-type batteries can be minimized.

[0043] The discharge process (S100), dismantling process (S200), crushing process (S300), firing process (S400), and crushing process (S500) according to the present invention can be performed continuously by automated equipment. Therefore, an integrated recycling process technology is possible, from waste batteries in pack form to the final target metal compound, and the time required to recover metals from waste batteries can be significantly reduced.

[0044] Wet process (S600)

[0045] The wet process (S600) is a process for recovering metal materials using crushed batteries. The metal recovered through the wet process (S600) may be in the form of a compound. For example, the wet process (S600) can recover metal materials in the form of a compound from crushed batteries following the crushing process (S500).

[0046] The metal compound recovered through the wet process (S600) may include at least one selected from the group consisting of lithium hydroxide, lithium carbonate, and lithium phosphate. Through the wet process (S600) of the present invention, it is possible to produce high-purity lithium carbonate (Li2CO3) and high-purity lithium hydroxide (LiOH·H2O) with excellent lithium recovery rate. Lithium hydroxide can be produced through a pre-separation process (S610), a weak acid leaching process (S612), a post-separation process (S614), a lithium phosphate production process (S616), a lithium sulfate solution production process (S618), a lithium carbonate production process (S620), a lithium hydroxide solution production process (S622), and an ion exchange resin process (S624), as described below.

[0047] Additionally, the metal compound recovered through the wet process (S600) may include copper (II) sulfide (CuS).

[0048] In one embodiment of the present invention, the metal compound recovered through the wet process (S600) may include one type of sulfate selected from the group consisting of nickel, cobalt, and manganese. In another embodiment of the present invention, the metal compound recovered through the wet process (S600) may include a nickel-cobalt-manganese compound in a solution state, for example, an NCM (Ni, Co, Mn) solution.

[0049] Nickel sulfate can be manufactured through a pre-separation process (S610), a weak acid leaching process (S612), a post-separation process (S614), a two-stage leaching process (S626), a first solvent extraction process (S628), and a first impurity removal process (S630), as described below.

[0050] Cobalt sulfate can be manufactured through a pre-separation process (S610), a weak acid leaching process (S612), a post-separation process (S614), a two-stage leaching process (S626), a first solvent extraction process (S628), a second solvent extraction process (S632), and a second impurity removal process (S634), as described below.

[0051] Manganese sulfate can be manufactured through a pre-separation process (S610), a weak acid leaching process (S612), a post-separation process (S614), a two-stage leaching process (S626), a first solvent extraction process (S628), a second solvent extraction process (S632), and a third impurity removal process (S636), as described below.

[0052] Hereinafter, each step of the wet process (S600) will be described in more detail with reference to FIG. 2. FIG. 2 is a process diagram of the wet process (S600) among the waste battery processing methods according to the present invention.

[0053] Line separation process (S610)

[0054] The pre-separation process (S610) is a process for leaching and separating lithium (Li) by adding water to the crushed battery after calcination. For example, in the pre-separation process (S610), the crushed battery after the crushing process (S500) is dissolved in water, and a lithium (Li) solution is leached at 10°C to 30°C for 1 to 3 hours to produce a lithium carbonate (Li2CO3) solution, and the cake can be separated. Through the pre-separation process (S610), the operating cost and raw material cost of the lithium phosphate manufacturing process (S616) described later can be reduced, the mixing of impurities can be minimized when manufacturing high-purity lithium hydroxide can be reduced, and the processing cost can be reduced when manufacturing lithium hydroxide.

[0055] After the pre-separation process (S610), a first evaporation and concentration process (not shown) may be performed. The first evaporation and concentration process is a process of manufacturing lithium carbonate (Li2CO3) crystals by evaporating and concentrating the lithium (Li) solution (filtrate) produced in the pre-separation process (S610). By manufacturing lithium carbonate crystals through the pre-separation process (S610) and the first evaporation and concentration process, the amount of phosphoric acid (H3PO4) and sodium hydroxide (NaOH) used in the lithium phosphate manufacturing process (S616) described later can be reduced by more than 50%, and the loss of lithium (Li) distributed as a filtrate in the lithium phosphate manufacturing process (S616) can be significantly reduced.

[0056] Mild acid leaching process (S612)

[0057] The weak acid leaching process (S612) is a process of leaching the cake separated in the pre-separation process (S610) using sulfuric acid (H2SO4). Specifically, the weak acid leaching process (S612) is a process of reducing and leaching the cake generated after lithium is separated in the pre-separation process (S610) with sulfuric acid and hydrogen peroxide (H2O2) at 80°C to 85°C for 1 to 4 hours. When nickel (Ni), cobalt (Co), and manganese (Mn) are dissolved from the cake from which lithium (Li) has been separated through the pre-separation process (S610), the amount of auxiliary materials used can be minimized and stable process management in a continuous process is possible.

[0058] Post-separation process (S614)

[0059] The post-separation process (S614) is a process of neutralizing the leaching filtrate generated in the weak acid leaching process (S612) and separating it into a lithium (Li) solution and a nickel cobalt manganese cake (hereinafter, NCM cake). Specifically, in the post-separation process (S614), the leaching filtrate from the weak acid leaching process (S612) is neutralized (pH 10 to pH 12) with sodium hydroxide (NaOH) and reacted at 70°C to 85°C for 4 to 8 hours, thereby precipitating and recovering nickel (Ni), cobalt (Co), and manganese (Mn), and distributing lithium (Li) into the filtrate for separation. In the post-separation process (S614), the precipitation rate of nickel (Ni), cobalt (Co), and manganese (Mn) can be 99.9% or more.

[0060] Additionally, in the post-separation process (S614), the filtered NCM cake can be repulped twice or more to remove residual sodium salt (Na Salt). For example, the sodium (Na) content in the NCM cake can be removed from 3.43% to 0.4%. In the present specification, the repulping process means a process of repulping a solid cake with water to wash away the filtrate component (e.g., residual sodium salt) present in the cake.

[0061] Lithium phosphate manufacturing process (S616)

[0062] The lithium phosphate manufacturing process (S616) is a process of producing a lithium phosphate (Li3PO4) cake by adding phosphoric acid (H3PO4) and sodium hydroxide (NaOH) to the lithium (Li) solution separated by the post-separation process (S614). Specifically, phosphoric acid (H3PO4) is added to the lithium (Li) solution separated by the post-separation process (S614) and reacted at 70°C to 85°C for 1 to 4 hours to precipitate and recover lithium (Li) in the form of lithium phosphate (Li3PO4). In addition, sodium hydroxide (NaOH) may be added to neutralize the solution to a pH of 10.0 to 12.0.

[0063] Lithium sulfate solution manufacturing process (S618)

[0064] The lithium sulfate solution manufacturing process (S618) is a process for manufacturing a lithium sulfate (Li2SO4) solution by dissolving the lithium carbonate (Li2CO3) crystals recovered by evaporation and concentration of the solution (lithium carbonate (Li2CO3) solution) manufactured from the separation process (S610) and the lithium phosphate (Li3PO4) cake produced in the lithium phosphate manufacturing process (S616) with sulfuric acid, respectively. For example, the temperature in the lithium sulfate solution manufacturing process (S618) is 60°C to 80°C, the reaction time is 0.5 to 3 hours, and the pH is 2.0 or less.

[0065] After the lithium sulfate solution manufacturing process (S618), a second evaporation and concentration process (not shown) may be performed. The second evaporation and concentration process is a process of evaporating and concentrating the lithium sulfate solution produced in the lithium sulfate solution manufacturing process (S618) to separate lithium sulfate (Li2SO4) crystals and phosphoric acid (H3PO4) filtrate. The phosphoric acid (H3PO4) filtrate can be recycled to the lithium phosphate manufacturing process (S616) and used as a lithium precipitation by-product. The evaporation condensate generated in the second evaporation and concentration process can be recycled as a process solution for the lithium (Li) separation process (S610). This can reduce the amount of waste liquid generated outside the system and the amount of fresh water introduced into the system.

[0066] The first phosphorus removal process (not shown) is a process in which lithium sulfate (Li2SO4) crystals manufactured in the second evaporation and concentration process are dissolved in pure water, and then phosphorus (P) is removed using aluminum sulfate (Al2(SO4)3) and caustic soda (NaOH). For example, by adding aluminum sulfate (Al2(SO4)3) to the solution manufactured in the lithium sulfate solution manufacturing process (S618) to adjust the pH to 5.0 to 6.0 and reacting at 50°C to 70°C for 4 to 8 hours, most of the phosphorus (P) can be removed by precipitation, and iron (Fe) and other impurities can also be removed by coprecipitation.

[0067] Lithium carbonate manufacturing process (S620)

[0068] The lithium carbonate manufacturing process (S620) is a process of adding sodium carbonate (Na2CO3) to lithium sulfate (Li2SO4) manufactured in the lithium sulfate solution manufacturing process (S618) to precipitate lithium carbonate (Li2CO3). For example, in the lithium carbonate manufacturing process (S620), sodium carbonate (Na2CO3) is added to the filtrate generated in the first phosphorus removal process and reacted at 80°C to 85°C for 1 to 6 hours to precipitate lithium carbonate.

[0069] Preferably, a repulping process may be performed to remove residual sodium (Na) salts from the cake in the lithium carbonate manufacturing process (S620). In this case, repulping may be performed at 80°C to minimize lithium (Li) loss. The filtrate from the lithium carbonate manufacturing process (S620) may be recycled to the lithium phosphate manufacturing process (S616).

[0070] Lithium hydroxide solution manufacturing process (S622)

[0071] The lithium hydroxide solution manufacturing process (S622) is a process of dissolving the lithium carbonate cake produced from the lithium carbonate in pure water, and then adding calcium oxide (CaO) to manufacture a lithium hydroxide (LiOH) solution. For example, calcium oxide (CaO) and water may be added to the lithium carbonate cake produced in the lithium carbonate manufacturing process (S620), and reacted at 80°C to 100°C for 3 hours or less, and then reacted at 80°C to 100°C for 2 hours or less to manufacture a lithium hydroxide (LiOH) solution. Preferably, a repulping process may be performed to recover lithium contained in the calcium carbonate (CaCO3) residue produced in the lithium hydroxide solution manufacturing process (S622).

[0072] Ion exchange resin process (S624)

[0073] The ion exchange resin process (S624) is a process for removing calcium (Ca) and magnesium (Mg), which are impurities in the lithium hydroxide (LiOH) solution manufactured above.

[0074] The third evaporation and concentration process (not shown) is a process for producing lithium hydroxide (LiOH) crystals by evaporating and concentrating the lithium hydroxide (LiOH) solution produced in the lithium hydroxide solution production process (S622) and / or the ion exchange resin treatment solution from which impurities have been removed through the ion exchange resin process (S624). Specifically, in the third evaporation and concentration process, a LiOH·H2O product can be produced by evaporating and concentrating the lithium hydroxide (LiOH) solution and / or the ion exchange resin treatment solution.

[0075] Two-stage leaching process (S626)

[0076] The two-stage leaching process (S626) is a process of leaching the weak acid leaching process cake generated in the weak acid leaching process (S612) and the NCM cake generated in the post-separation process (S614) using sulfuric acid and hydrogen peroxide (H2O2). For example, in the two-stage leaching process (S626), the weak acid leaching process cake and the NCM cake from which lithium is separated can be dissolved (pH 1.5 to 2.5) with sulfuric acid (H2SO4) at 60°C to 80°C for 2 to 4 hours. A small amount of reducing agent can be added to improve the dissolution rate of the NCM cake, and at this time, hydrogen peroxide (H2O2) can be used as the reducing agent.

[0077] Preferably, an impurity removal process may be performed to remove impurities from the filtrate generated in the two-stage leaching process (S626). In this case, the impurity removal process may include a first copper removal process and a first aluminum & phosphorus removal process. The first copper removal process (not shown) is a process of injecting NaSH to remove copper (Cu), which is an impurity, from the filtrate generated in the two-stage leaching process (S626). The first aluminum & phosphorus removal process (not shown) is a process of injecting caustic soda (NaOH) and oxygen gas (O2) to remove aluminum (Al) and phosphorus (P), which are additional impurities, from the filtrate generated in the first copper removal process.

[0078] First solvent extraction process (S628)

[0079] The first solvent extraction process (S628) is a process for extracting cobalt using an extractant from the filtrate generated in the two-stage leaching process (S626) and / or the filtrate generated in the impurity removal process described above.

[0080] Preferably, a nickel hydroxide manufacturing process and a nickel weak acid leaching process can be performed on the filtrate generated from the first solvent extraction process (S628). For example, the nickel hydroxide manufacturing process (not shown) is a process of manufacturing nickel hydroxide (Ni(OH)2) using caustic soda (NaOH) on the filtrate generated from the first solvent extraction process (S628). The nickel weak acid leaching process (not shown) is a process of dissolving the cake generated from the nickel hydroxide manufacturing process by adding water, sulfuric acid (H2SO4), and hydrogen peroxide (H2O2).

[0081] First impurity removal process (S630)

[0082] The first impurity removal process (S630) is a process for removing impurities from the filtrate generated from the first solvent extraction process (S628) and / or the filtrate generated from the nickel hydroxide manufacturing process and the nickel weak acid leaching process. Specifically, the first impurity removal process (S630) may include a second copper removal process and a first aluminum removal process. For example, the second copper removal process is a process of injecting sodium hydrogen sulfide (NaSH) to remove copper (Cu), an impurity, from the filtrate generated from the nickel weak acid leaching process. The first aluminum removal process is a process of injecting caustic soda (NaOH) and injecting oxygen gas (O2) to remove aluminum (Al), an additional impurity, from the filtrate generated from the second copper removal process.

[0083] The fourth evaporation and concentration process (not shown) is a process for manufacturing nickel sulfate (NiSO4) crystals by evaporating and concentrating the solution produced in the first impurity removal process (S630).

[0084] Second solvent extraction process (S632)

[0085] The second solvent extraction process (S632) is a process for extracting manganese using an extractant from the stripped liquid generated in the first solvent extraction process (S628).

[0086] Preferably, a first cobalt extraction process (not shown) may be performed on the filtrate generated from the second solvent extraction process (S632). The first cobalt extraction process is a process of extracting cobalt from the filtrate generated from the second solvent extraction process (S632) using an extractant.

[0087] Second impurity removal process (S634)

[0088] The second impurity removal process (S634) is a process for removing impurities from the filtrate generated from the second solvent extraction process (S632) and / or the filtrate generated from the first cobalt extraction process. Specifically, the second impurity removal process (S634) may include a third copper removal process (not shown) and a second aluminum removal process (not shown). For example, the third copper removal process is a process of injecting sodium hydrogen sulfide (NaSH) to remove copper (Cu), an impurity, from the stripped liquid generated from the first cobalt extraction process. The second aluminum removal process is a process of injecting caustic soda (NaOH) and injecting oxygen gas (O2) to remove aluminum (Al), an additional impurity, from the filtrate generated from the third copper removal process.

[0089] The fifth evaporation and concentration process (not shown) is a process for producing cobalt sulfate (CoSO4) crystals by evaporating and concentrating the filtrate generated in the second impurity removal process (S634).

[0090] Third impurity removal process (S636)

[0091] The third impurity removal process (S636) is a process for removing impurities from the stripped liquid generated in the second solvent extraction process (S632). Specifically, the third impurity removal process (S636) may include a fourth copper removal process (not shown) and a third aluminum removal process (not shown). The fourth copper removal process is a process of injecting sodium hydrogen sulfide (NaSH) to remove copper (Cu) from the stripped liquid generated in the second solvent extraction process (S632). The third aluminum removal process is a process of injecting caustic soda (NaOH) and oxygen gas (O2) to remove aluminum (Al), which is an additional impurity, from the filtrate generated in the fourth copper removal process.

[0092] The sixth evaporation and concentration process (not shown) is a process for producing manganese sulfate (MnSO4) crystals by evaporating and concentrating the filtrate generated in the third impurity removal process (S636).

[0093] Hereinafter, the present invention will be described in detail through examples and comparative examples. In the examples, valuable metals were recovered from waste batteries through the aforementioned processes. Meanwhile, in the comparative examples, valuable metals were recovered using the same method as in the examples, except that the waste batteries in packs were disassembled into modules in the disassembly process (S200).

[0094] The amount of impurities in the materials recovered in the examples and comparative examples is shown in Table 1 below. At this time, the method for calculating the amount of impurities is as follows. Specifically, the amount of NCM622 waste batteries processed per day was 285.7 tons based on packs, 205.5 tons based on modules excluding other parts after dismantling the packs, and 168.2 tons based on cells excluding other parts after dismantling the modules. At this time, the amount of impurities in the materials recovered from module-type waste batteries was calculated by deriving the ratio of aluminum (Al) and iron (Fe).

[0095] Comparative Example Example Dismantling to module unit Dismantling to cell unit Al component ratio (%) 12.202.63 Inflow (ton / day) 25.104.42 Fe component ratio (%) 3.000.00 Inflow (ton / day) 6.170.00

[0096] According to Table 1, in the example of dismantling waste batteries from pack to cell, it can be confirmed that the inflow of aluminum (Al) and iron (Fe) is significantly reduced compared to the comparative example. Specifically, the inflow of aluminum (Al) in the example was reduced by 82.4% compared to the comparative example, and the inflow of iron (Fe) was reduced by 100%.

[0097] Meanwhile, the recovery rates of each valuable metal among the materials recovered in the examples and comparative examples are shown in Table 2 below. The recovery rate of each valuable metal refers to a value calculated by excluding the loss in the process of recovering the target metal (e.g., Li) in a commercial form (e.g., LiOH). At this time, the weight of the raw material (and slag) containing the target metal was measured using a balance, and the concentration of the metal in the form of a leached compound was measured using ICP-AES spectroscopic analysis, and the recovery rate of each metal was calculated from this.

[0098] Comparative Example Example Dismantling to module unit Dismantling to cell unit Dismantling recovery rate (%) Li88.4Li98.3Ni96.5Ni95.1Co96.5Co94.7Mn-Mn95.1Cu97.9Cu99.9

[0099] According to Table 2, it can be confirmed that the lithium (Li) recovery rate in the example significantly increased compared to the comparative example. In addition, it can be confirmed that manganese (Mn) recovery was possible in the example, unlike the comparative example.

[0100] While the present invention has been described in connection with certain embodiments herein, it should be understood that various modifications and variations can be made without departing from the spirit and scope of the invention, as understood by those skilled in the art. Furthermore, such modifications and variations are intended to fall within the scope of the claims appended to this specification.

Claims

1. Discharging process for discharging waste batteries; A dismantling process for dismantling the discharged waste battery into cell units; A shredding process for shredding waste batteries disassembled into the above cell units; A firing process for firing the above-mentioned shredded waste batteries; A crushing process for crushing the above-mentioned calcined waste batteries; and A method for processing waste batteries, comprising a wet process for extracting and recovering metals from the crushed waste batteries.

2. In paragraph 1, A method for processing waste batteries, wherein the waste batteries are batteries in packs whose lifespan has ended.

3. In paragraph 1, A method for processing a waste battery, wherein the waste battery is discharged through the above-mentioned discharge process so that the voltage of the waste battery becomes 30 V or less.

4. In paragraph 1, A method for processing waste batteries, wherein the batteries are crushed into cell units of 20 cm or less in size through the above crushing process.

5. In paragraph 1, A method for processing waste batteries, wherein the process of separating black mass from the crushed waste batteries is omitted.

6. In paragraph 1, A method for processing waste batteries, wherein the above-mentioned discharge process, the above-mentioned dismantling process, the above-mentioned crushing process, the above-mentioned calcination process and the above-mentioned crushing process are performed continuously by automated equipment.

7. In paragraph 1, A method for processing waste batteries, wherein the above-mentioned discharge process, the above-mentioned dismantling process, and the above-mentioned crushing process are performed by automated equipment using a robot.

8. In paragraph 1, A method for processing waste batteries, wherein metal compounds are recovered through the above wet process.

9. In paragraph 8, A method for treating waste batteries, wherein the metal compound comprises at least one selected from the group consisting of lithium hydroxide, lithium carbonate, and lithium phosphate.

10. In paragraph 8, A method for treating waste batteries, wherein the metal compound comprises one sulfate selected from the group consisting of nickel, cobalt and manganese.

11. In paragraph 8, A method for processing waste batteries, wherein the metal compound comprises a nickel-cobalt-manganese compound in a solution state.

Citation Information

Patent Citations

  • Apparatus for cutting waste battery module and Pre-processing method for recycling waste battery module using the same

    KR102407105B1

  • Eco-friendly recycling method for wasted battery

    KR102447931B1

  • Dismantling system of spent lithium ion battery pack

    KR102512096B1

  • KR20220038441A