Method for recovering lithium

The lithium recovery method employs a chelate resin to efficiently bind and separate lithium ions from low-concentration solutions, addressing inefficiencies and pollution in existing methods by optimizing pH and solution ratios, achieving rapid and environmentally friendly lithium recovery.

WO2024248256A1PCT designated stage expired Publication Date: 2024-12-05KOREA ZINC CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/020325
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-27
Filing Date
2023-12-11
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current methods for lithium recovery from ore and brine are inefficient, requiring multiple processes, generating significant environmental pollution, and taking a long time, especially when lithium concentration is low.

Method used

A lithium recovery method using a chelate resin to bind lithium ions, adjusting pH, and passing acidic and water solutions through the resin to separate lithium ions, followed by phosphorus addition to form lithium phosphate, optimizing ratios and concentrations to enhance efficiency and minimize sludge generation.

Benefits of technology

This method efficiently recovers lithium from low-concentration solutions in a short time, reducing environmental pollution and operational costs by effectively binding and separating lithium ions from the chelate resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023020325_05122024_PF_FP_ABST
    Figure KR2023020325_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for recovering lithium. Provided according to an embodiment of the present invention may be a method for recovering lithium, the method comprising the steps of: preparing a lithium-containing solution containing lithium ions; exchanging the lithium ions with the ions included in the chelate resin so that the lithium ions are bonded to the chelate resin while the lithium-containing solution passes through the chelate resin; and passing an acidic solution through the chelate resin to which the lithium ions are bonded so that the lithium ions are separated from the chelate resin.
Need to check novelty before this filing date? Find Prior Art

Description

Lithium recovery method

[0001] The present invention relates to a method for recovering lithium.

[0002] Lithium (Li) is an essential industrial raw material used in a wide range of industries. While lithium was traditionally used in ceramics and chemical additives, the recent shift toward wireless and electrified power generation has led to its widespread use in electronic devices such as mobile phones and laptops. In particular, the increasing demand for lithium batteries used in electric vehicles (Battery Electric Vehicles, BEVs) necessitates the development of technologies for effectively and economically extracting lithium from lithium-containing resources.

[0003] Lithium, which typically exists in nature, is distributed in trace amounts in soil, rocks, and natural waters. Therefore, lithium must be recovered from these concentrated sources, and the recovered lithium must be processed into a compound for use. For example, commercially viable lithium is concentrated in minerals or brine.

[0004] The process of recovering lithium from ore involves multiple processes for lithium-containing raw materials, such as spodumene, lepidolite, amblygonite, or petalite. Furthermore, the process of recovering lithium from ore involves mining, crushing, separation, and beneficiation, followed by further processing steps such as heating, concentration, filtration, and additive addition. Because the process of recovering lithium from ore requires multiple processes, it increases facility investment and operating costs, and generates a large amount of acidic sludge, which can cause serious environmental pollution.

[0005] Meanwhile, to address the challenges inherent in lithium recovery from ore, a method for recovering lithium from brine contained in salt lakes is being developed. Conventional methods for recovering lithium from brine involve naturally evaporating the brine to increase its lithium concentration, which is then precipitated as lithium carbonate. However, the natural evaporation process takes a long time, exceeding a year, and the lithium often precipitates along with other substances during the concentration process.

[0006] Accordingly, there is a need for a lithium recovery method that can effectively recover lithium from a low-concentration lithium-containing solution in a short period of time.

[0007] The present invention was invented with the above background in mind, and aims to efficiently recover lithium even when the lithium concentration of a lithium-containing solution is low.

[0008] In addition, the purpose is to recover lithium from a lithium-containing solution in a short period of time without allowing the lithium-containing solution to evaporate naturally for a long time.

[0009] Additionally, the purpose is to minimize the amount of sludge generated and prevent environmental pollution.

[0010] According to one embodiment of the present invention, a method for recovering lithium may be provided, comprising the steps of: preparing a lithium-containing solution containing lithium ions; exchanging lithium ions with ions contained in a chelating resin so that the lithium ions are bound to the chelating resin while the lithium-containing solution passes through the chelating resin; and passing an acidic solution through the chelating resin to which the lithium ions are bound so that the lithium ions are separated from the chelating resin.

[0011] According to one embodiment of the present invention, a method for recovering lithium may be provided, further comprising a step of mixing an alkaline solution into the lithium-containing solution to adjust the pH of the lithium-containing solution, wherein the lithium-containing solution passes through the chelating resin while the pH is adjusted to 10 to 13 by the alkaline solution.

[0012] According to one embodiment of the present invention, a lithium recovery method may be provided in which the lithium-containing solution is provided such that the ratio of the amount of lithium-containing solution passing through the chelating resin to the amount of the chelating resin is 4.17 to 8.33.

[0013] According to one embodiment of the present invention, a lithium recovery method can be provided in which the ratio of the amount of lithium ions bound to the chelate resin to the amount of the chelate resin is 1 to 1.3.

[0014] According to one embodiment of the present invention, a lithium recovery method may be provided in which the acidic solution is provided such that the ratio of the amount of acidic solution passing through the chelating resin to the amount of the chelating resin is 1.5 to 2.5.

[0015] According to one embodiment of the present invention, a lithium recovery method may be provided, further comprising a step of passing water through a chelate resin to which lithium ions are bound so as to separate the lithium ions from the chelate resin, wherein the step of passing water through the chelate resin is performed after the step of passing an acidic solution through the chelate resin.

[0016] According to one embodiment of the present invention, a lithium recovery method may be provided, further comprising a step of providing a phosphorus supplying material including at least one of phosphorus, phosphoric acid, and phosphate to a lithium purification solution containing lithium ions separated from the chelating resin, wherein the lithium ion concentration in the lithium-containing solution is 0.39 g / L or less.

[0017] According to one embodiment of the present invention, a method for recovering lithium may be provided, wherein the lithium-containing solution includes seawater or brine having a sodium (Na) concentration of 30 g / L to 50 g / L.

[0018] According to one embodiment of the present invention, a lithium recovery method can be provided in which the ion included in the chelating resin exchanged with the lithium ion is a hydrogen ion.

[0019] According to one embodiment of the present invention, a method for recovering lithium can be provided, wherein the acid concentration of the acid solution is 1.472 eq / L to 2.208 eq / L.

[0020] According to the present invention, there is an effect of efficiently recovering lithium even if the lithium concentration of the lithium-containing solution is low.

[0021] In addition, there is an effect that lithium can be recovered from a lithium-containing solution in a short period of time without naturally evaporating the lithium-containing solution for a long time.

[0022] Additionally, it has the effect of minimizing the amount of sludge generated and preventing environmental pollution.

[0023] Figure 1 is a flowchart sequentially showing a lithium recovery method according to one embodiment of the present invention.

[0024] Figure 2 is a graph showing lithium binding capacity according to pH.

[0025] Figure 3 is a graph showing lithium binding capacity according to the ratio of sample amount to chelate resin amount.

[0026] Figure 4 is a graph showing the hydrogen ion exchange rate according to the ratio of acid solution to chelate resin amount.

[0027] The embodiments of the present invention are provided for the purpose of illustrating the technical concept of the present invention. The scope of the rights according to the present invention is not limited to the embodiments presented below or the specific descriptions of these embodiments.

[0028] Hereinafter, the present invention will be described with reference to the drawings.

[0029] Figure 1 is a flowchart sequentially showing a lithium recovery method according to one embodiment of the present invention.

[0030] Referring to Fig. 1, in the lithium recovery method (S1), lithium is recovered from a lithium-containing solution. For example, in the lithium recovery method (S1), lithium can be recovered from seawater or brine in the form of lithium phosphate (Li3PO4).

[0031] The lithium recovery method (S1) may include a step (S100) of preparing a lithium-containing solution containing lithium ions. In the present specification, the lithium-containing solution contains lithium ions, and for example, the concentration of lithium ions in the lithium-containing solution may be 0.39 g / L or less. In addition, the lithium-containing solution may be seawater or brine having a sodium (Na) concentration of 30 g / L to 50 g / L. In the step (S100) of preparing the lithium-containing solution, the lithium-containing solution may be provided such that the ratio of the amount of the lithium-containing solution passing through the chelate resin to the amount of the chelate resin is 4.17 to 8.33. That is, the amount of the lithium-containing solution provided in the step (S100) of preparing the lithium-containing solution may have a volume ratio of 4.17 to 8.33 times the amount of the chelate resin.

[0032] The lithium recovery method (S1) may include a step (S200) of mixing an alkaline solution into the lithium-containing solution to adjust the pH of the lithium-containing solution. In the step (S200) of mixing the alkaline solution into the lithium-containing solution, the alkaline solution is mixed into the lithium-containing solution so that the pH of the lithium-containing solution is adjusted to 10 to 13. For example, the alkaline solution may be sodium hydroxide (NaOH). In addition, the step (S200) of mixing the alkaline solution into the lithium-containing solution may be performed before the alkaline solution passes through the chelating resin. In this case, the lithium-containing solution passes through the chelating resin while the pH is adjusted to 10 to 13 by the alkaline solution. In the present specification, the chelating resin may be, for example, an ion exchange resin polymerized by adding DVB (Divinylbenzene) to polystyrene.

[0033] The lithium recovery method (S1) may include a step (S300) of exchanging lithium ions with ions contained in the chelate resin so that the lithium ions are bound to the chelate resin while the lithium-containing solution passes through the chelate resin. In the step (S300) of exchanging the ions contained in the chelate resin with lithium ions, the lithium-containing solution, whose pH was adjusted in the step (S200) of mixing the basic solution with the lithium-containing solution, passes through the chelate resin. While the lithium-containing solution passes through the chelate resin, the lithium ions contained in the lithium-containing solution are exchanged with the ions contained in the chelate resin. In other words, the lithium ions contained in the lithium-containing solution are bound to the chelate resin, and the ions bound to the chelate resin are separated from the chelate resin. In this case, the lithium ions contained in the lithium-containing solution are separated from the lithium-containing solution while remaining bound to the chelate resin. For example, according to one embodiment of the present invention, the chelate resin may contain hydrogen ions, and the hydrogen ions may be exchanged with the lithium ions of the lithium-containing solution.

[0034] The lithium recovery method (S1) may include a step (S400) of passing an acidic solution through a chelate resin to which lithium ions are bound so that lithium ions are separated from the chelate resin. In the step (S400) of passing the acidic solution through the chelate resin, the acidic solution is passed through the chelate resin to which lithium ions are bound, and while the acidic solution passes through the chelate resin, lithium ions are separated from the chelate resin. The acid concentration of the acidic solution is 1.472 eq / L to 2.208 eq / L. For example, the acidic solution may be sulfuric acid (H2SO4) having a concentration of 72 g / L or more and 108 g / L or more. In addition, in the step (S400) of passing the acidic solution through the chelate resin, the acidic solution may be provided such that the ratio of the amount of the acidic solution passing through the chelate resin to the amount of the chelate resin is 1.5 to 2.5. That is, the amount of acid solution provided in the step (S400) of passing the acid solution through the chelate resin may be 1.5 to 2.5 times the volume ratio of the amount of the chelate resin.

[0035] The lithium recovery method (S1) may include a step (S500) of passing water through a chelate resin to which lithium ions are bound so that lithium ions are separated from the chelate resin. In the step (S500) of passing water through the chelate resin, water is passed through the chelate resin to which lithium ions are bound, and while the water passes through the chelate resin, lithium ions are separated from the chelate resin. This step (S500) of passing water through the chelate resin may be performed after the step (S400) of passing an acidic solution through the chelate resin. In this case, as the acidic solution passes through the chelate resin, lithium ions are primarily separated from the chelate resin (S400), and as water passes through the chelate resin, lithium ions are secondarily separated from the chelate resin (S500). In this step (S500) of passing water through the chelate resin, the ratio of water passing through the chelate resin to the amount of water may be provided to be 1.5 to 2.5. That is, the amount of water provided in the step of passing water through the chelate resin (S500) may be 1.5 to 2.5 times the volume ratio of the amount of chelate resin.

[0036] The lithium recovery method (S1) may include a step (S600) of providing a phosphorus supply material including at least one of phosphorus, phosphoric acid, and phosphate to a lithium purification solution. Here, the lithium purification solution is a solution including lithium ions separated from a chelating resin. In the step (S600) of providing the phosphorus supply material, the phosphorus supply material may react with lithium ions to produce lithium phosphate (Li3PO4). Here, the phosphorus supply material includes at least one of phosphorus, phosphoric acid, and phosphate, and the phosphate may be at least one of potassium phosphate, sodium phosphate, and ammonium phosphate.

[0037] In this way, the lithium recovery method (S1) can recover lithium ions in the form of lithium phosphate from seawater or brine containing low concentrations of lithium ions of 0.39 g / L or less.

[0038] Hereinafter, the lithium recovery method of the present invention will be described by way of an example.

[0039] Analysis results according to pH

[0040] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 pHpH 2pH 6pH 9pH 10pH 11.5pH 13pH 14 Sample volume (mL) 1,000 1,000 1,000 1,000 1,000 1,000 1,000 1,000 Chelate resin volume (mL) 180 180 180 180 180 180 180 Total reaction Limg / L 250 250 250 250 250 250 250 Nag / L 40.34 0.34 0.34 0.34 0.34 0.34 0.34 Reaction Limg / L11397.082.746.416.858.778.3Nag / L22.430.532.134.833.634.238.2Lithium recovery rate (%)54.861.266.981.493.376.568.7Lithium binding capacity0.760.850.931.131.301.060.95

[0041] In the above Table 1, Examples 1 to 7 were tested under the same experimental conditions while only changing the pH of the lithium-containing solution. Here, the pH is adjusted in the step (S200) of mixing an alkaline solution into the lithium-containing solution. In the present specification, the lithium recovery rate (%) represents the percentage of the amount of lithium bound to the chelate resin with respect to the amount of lithium contained in the lithium-containing solution before the reaction. In addition, the lithium binding capacity represents the amount of lithium bound to the chelate resin with respect to the amount of chelate resin, and means the degree to which lithium is recovered in the chelate resin. In other words, when the absolute amount (mg) of lithium in the sample to be treated is the same, the higher the lithium binding capacity means that a greater amount of lithium is recovered in the same chelate resin. As can be seen in the above Table 1 and Fig. 2, it can be seen that the lithium recovery rate and lithium binding capacity change as the pH changes. It can be seen that the lithium-containing solution (Examples 4 to 6) with the pH adjusted to 10 to 13 is more preferable in terms of the lithium recovery rate and lithium binding capacity.

[0042] Analysis results according to the ratio of sample volume to chelate resin volume

[0043] Example 8 Example 9 Example 10 Example 11 Example 12 Sample amount (mL) 500 7 50 1,000 1,500 2,000 Chelate resin amount (mL) 180 180 180 180 180 180 pH before reaction 11.5 11.5 11.5 11.5 Limg / L 250 250 250 250 250 Limg / L after reaction 0.1 1 8.5 0 16.8 0 9 7.2 0 13 8.7 0 Ratio of sample amount to chelate resin amount 2.7 8 4.1 7 5.5 6 8.3 3 11.1 1 Lithium binding capacity 0.6 9 1.0 11.3 0 1.2 7 1.2 4

[0044] In the above Table 2, Examples 8 to 12 were tested while changing the sample amount under the same experimental conditions. In this specification, the sample amount refers to the amount of the lithium-containing solution passing through the chelate resin. That is, the above Table 2 was tested while changing the ratio of the amount of the lithium-containing solution passing through the chelate resin to the amount of the chelate resin. As can be seen in the above Table 2 and Fig. 3, it can be seen that the lithium binding capacity changes when the sample amount to the chelate resin amount changes. Furthermore, it can be seen that when the ratio of the sample amount to the chelate resin amount is 4.17 to 8.33 (Examples 9 to 11), the lithium binding capacity is more preferable. When the ratio of the sample amount to the chelate resin amount is 4.17 or more, as in Example 9, the lithium binding capacity has a remarkable effect of 1 or more. When the ratio of the sample amount to the chelate resin amount is 8.33 or less, as in Example 11, it is possible to maintain the lithium binding capacity at a predetermined level while preventing the amount of sample introduced from becoming excessively large.

[0045] Analysis results according to the ratio of acid solution to chelate resin amount

[0046] Example 13 Example 14 Example 15 Example 16 Example 17 Amount of chelating resin (mL) 180 Total amount of bound Li (mg) 233 Acid concentration of acid solution used (eq / L as acid) 1.84 Amount of liquid mL 90 180 270 360 450 Limg / L 3.86.36 1357 2465 Ratio of liquid to resin amount 0.5 11.52 2.5 Amount of acid consumed (eq as acid) 0.166 0.33 10.49 7 0.66 20.82 8 Total amount of Li extracted after hydrogen ion exchange (mg) 0.34 1.13 165.5 120 5.92 20 9.25 Hydrogen ion exchange rate (%) 0.15 0.49 7 1.0 38 8.38 8 9.81

[0047] In the above Table 3, Examples 13 to 17 were tested under the same experimental conditions while changing the amount of liquid. In this specification, the amount of liquid means the amount of acid solution passing through the chelate resin. That is, the above Table 3 was tested while changing the ratio of the amount of acid solution passing through the chelate resin to the amount of chelate resin. As can be seen in the above Table 3 and Fig. 4, it can be seen that the hydrogen ion exchange rate changes when the amount of acid solution consumed changes. It can be seen that the hydrogen ion exchange rate is more preferable when the ratio of the amount of liquid to the amount of chelate resin is 1.5 to 2.5 by volume ratio (Examples 15 to 17). When the ratio of the amount of liquid to the amount of chelate resin is 1.5 or more by volume ratio as in Example 15, the hydrogen ion exchange rate is significantly increased, and there is an effect of improving the amount of lithium recovered. In addition, when the ratio of the amount of liquid to the amount of chelate resin is 2.5 or less in volume ratio as in Example 17, it is possible to prevent the amount of acid solution introduced from becoming excessively large. Although the embodiments of the present invention have been described above with reference to the attached drawings, those skilled in the art will understand that the present invention can be implemented in other specific forms without changing the technical idea or essential features thereof.

[0048] Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. The scope of the present invention is defined by the claims rather than the detailed description above, and all modifications or variations derived from the meaning and scope of the claims and their equivalents should be construed as being included within the scope of the present invention.

Claims

1. A step of preparing a lithium-containing solution containing lithium ions; A step of exchanging the lithium ions with ions contained in the chelating resin so that the lithium ions are bound to the chelating resin while the lithium-containing solution passes through the chelating resin; and A step of passing an acidic solution through a chelate resin to which the lithium ions are bound so that the lithium ions are separated from the chelate resin, Lithium recovery method.

2. In paragraph 1, Further comprising a step of mixing a basic solution into the lithium-containing solution to adjust the pH of the lithium-containing solution, The lithium-containing solution is passed through the chelating resin while the pH is adjusted to 10 to 13 by the alkaline solution. Lithium recovery method.

3. In paragraph 1, The lithium-containing solution is provided such that the ratio of the amount of lithium-containing solution passing through the chelating resin to the amount of the chelating resin is 4.17 to 8.

33. Lithium recovery method.

4. In paragraph 2 or paragraph 3, The ratio of the amount of lithium ions bound to the chelate resin to the amount of the chelate resin is 1 to 1.3, Lithium recovery method.

5. In paragraph 3, The above acidic solution is provided so that the ratio of the amount of acidic solution passing through the chelating resin to the amount of the chelating resin is 1.5 to 2.

5. Lithium recovery method.

6. In paragraph 1, Further comprising a step of passing water through the chelate resin to which the lithium ions are bound so that the lithium ions are separated from the chelate resin, The step of passing water through the chelating resin is performed after the step of passing an acidic solution through the chelating resin. Lithium recovery method.

7. In paragraph 1, Further comprising the step of providing a phosphorus supplying material comprising at least one of phosphorus, phosphoric acid and phosphate to a lithium purification solution containing lithium ions separated from the chelating resin, The lithium ion concentration in the lithium-containing solution is 0.39 g / L or less, Lithium recovery method.

8. In paragraph 7, The lithium-containing solution includes seawater or brine having a sodium (Na) concentration of 30 g / L to 50 g / L. Lithium recovery method.

9. In paragraph 1, The ions contained in the chelating resin exchanged with the lithium ions are hydrogen ions. Lithium recovery method.

10. In paragraph 1, The acid concentration of the above acid solution is 1.472 eq / L to 2.208 eq / L, Lithium recovery method.

Citation Information

Patent Citations

  • Treatment and recovery method of lithium battery electrolyte production wastewater

    CN115650532A

  • Lithium hexafluorophosphate wastewater treatment method

    CN115784539A

  • Method for recovering with high purity lithium, lithium carbonate, lithium hydroxide and synthetic method of cathod material for lithium secondary battery from sea water

    KR1020120015658A

  • Method recovering useful metal in concentrated water according to seawater-desalination

    KR102415550B1

  • KR20200090741A