Monomer for electrolyte, electrolyte for secondary battery comprising same, manufacturing method thereof, and lithium secondary battery comprising same
The development of a monomer for electrolytes, forming a cross-linked polymer, addresses the safety concerns of lithium secondary batteries by enhancing flame retardancy and ionic conductivity, resulting in improved stability and electrochemical performance in lithium secondary batteries.
Patent Information
- Application Number
- PCT/KR2024/007150
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-24
- Filing Date
- 2024-05-27
- Publication Date
- 2024-12-05
AI Technical Summary
Commercially available lithium secondary batteries using liquid electrolytes face safety issues such as leakage and explosion due to environmental changes and external shocks, and solid electrolytes like gel polymer or composite polymer electrolytes have a high risk of ignition, necessitating improved flame retardancy and ionic conductivity.
A monomer for electrolytes is developed, represented by specific chemical formulas, which, when polymerized, forms a cross-linked or network polymer with enhanced flame retardancy and ionic conductivity, incorporated into a composite electrolyte with an organic and inorganic component, and used in lithium secondary batteries to improve stability and electrochemical properties.
The electrolyte monomer significantly enhances the ignition stability and ionic conductivity of lithium secondary batteries, leading to improved lifespan and electrical characteristics, with self-extinguishing properties and high-temperature stability.
Smart Images

Figure KR2024007150_05122024_PF_FP_ABST
Abstract
Description
Monomer for electrolyte, electrolyte for secondary battery containing same, method for producing same, and lithium secondary battery containing same
[0001] The present disclosure relates to a monomer for an electrolyte, an electrolyte for a secondary battery comprising the same, a method for producing the same, and a lithium secondary battery comprising the same.
[0002]
[0003] Secondary batteries, which can be repeatedly charged and discharged, are widely used as power sources for portable electronic communication devices such as camcorders, mobile phones, and laptops, thanks to the advancements in the information and communication and display industries. Furthermore, battery packs containing secondary batteries are being developed and applied as power sources for eco-friendly vehicles such as hybrid vehicles.
[0004] Examples of secondary batteries include lithium secondary batteries, nickel-cadmium batteries, and nickel-hydrogen batteries. Among these, lithium secondary batteries are actively being researched and developed due to their high operating voltage and energy density per unit weight, as well as their advantages in charging speed and weight reduction.
[0005] Currently commercialized lithium secondary batteries primarily use liquid electrolytes, posing safety concerns such as leakage, ignition, and explosion when exposed to rapid environmental changes, such as temperature fluctuations or external shocks. To address these issues, efforts are underway to solidify the electrolyte to ensure stability and improve energy density.
[0006] All-solid-state batteries can contain solid electrolytes, such as gel polymers, oxides or sulfides, or composite polymers. This can enhance safety against ignition and explosion due to external impacts or environmental changes.
[0007] However, among solid-state electrolytes, gel polymer electrolytes or composite polymer electrolytes may have a relatively high risk of ignition. Therefore, there is a need to improve the ignition safety of gel polymer electrolytes or composite polymer electrolytes.
[0008]
[0009] An object of the present disclosure is to provide an electrolyte monomer having improved flame retardancy.
[0010] An object of the present disclosure is to provide an electrolyte for a secondary battery having improved flame retardancy and ionic conductivity.
[0011] The present disclosure provides a method for producing an electrolyte for a secondary battery having improved flame retardancy and ionic conductivity.
[0012] An object of the present disclosure is to provide a lithium secondary battery with improved stability and electrochemical properties.
[0013]
[0014] The electrolyte monomer according to exemplary embodiments may include a first monomer represented by chemical formula 1 and a second monomer represented by chemical formula 2.
[0015] [Chemical Formula 1]
[0016]
[0017] In the above chemical formula 1, R1 may be a substituted or unsubstituted alkylene group having C2 to C12, or a substituted or unsubstituted oxyalkylene group having C2 to C10, and j is an integer of 1 to 5.
[0018] [Chemical Formula 2]
[0019]
[0020] In the above chemical formula 2, R2, R3 and R4 can each independently be a substituted or unsubstituted alkylene group having a carbon number of 2 to 10, or a substituted or unsubstituted alkoxy group having a carbon number of 2 to 10, and l, m and n are each independently integers of 0 to 5.
[0021] In some embodiments, the ratio of the content of the second monomer to the content of the first monomer may be 0.5 to 2 by weight.
[0022] In some embodiments, R1 in formula 1 may be a C2 to C10 fluorine-substituted alkylene group, or a C2 to C10 fluorine-substituted oxyalkylene group, and l, m, and n in formula 2 may each independently be 0 to 3.
[0023] In some embodiments, R2, R3 and R4 in formula 2 may be the same as each other, and l, m and n may be the same integers as each other.
[0024] In some embodiments, the first monomer may include at least one of a monomer represented by Chemical Formula 1-1 and a monomer represented by Chemical Formula 1-2.
[0025] [Chemical Formula 1-1]
[0026]
[0027] [Chemical Formula 1-2]
[0028]
[0029] In some embodiments, the second monomer may include at least one of a monomer represented by Chemical Formula 2-1 to a monomer represented by Chemical Formula 2-3.
[0030] [Chemical Formula 2-1]
[0031]
[0032] [Chemical Formula 2-2]
[0033]
[0034] [Chemical Formula 2-3]
[0035] .
[0036] An electrolyte for a secondary battery according to exemplary embodiments may include a flame retardant compound and a lithium salt, which includes a polymer derived from the above-described electrolyte monomer.
[0037] In some embodiments, the electrolyte for the secondary battery may further include a composite electrolyte including an organic polymer and an inorganic electrolyte, and the composite electrolyte may have a film form.
[0038] In some embodiments, the inorganic electrolyte may comprise an oxide-based solid electrolyte.
[0039] In some embodiments, the content of the flame retardant compound may be 3 wt% to 30 wt% of the total weight of the electrolyte for the secondary battery.
[0040] A lithium secondary battery according to exemplary embodiments may include a positive electrode, a negative electrode opposite to the positive electrode, and an electrolyte layer disposed between the positive electrode and the negative electrode, the electrolyte layer including the aforementioned secondary battery electrolyte.
[0041] In a method for manufacturing an electrolyte for a secondary battery according to exemplary embodiments, a mixture including the above-described electrolyte monomer and electrolyte solution can be manufactured. The mixture can be cured to manufacture an electrolyte for a secondary battery.
[0042] In some embodiments, the mixture may further comprise an organic polymer and an inorganic electrolyte.
[0043] In some embodiments, the content of the monomer for the electrolyte may be from 3 wt% to 30 wt% of the total weight of the mixture.
[0044] In some embodiments, the electrolyte may include an ether electrolyte containing fluorine (F).
[0045] In some embodiments, the content of the ether electrolyte containing fluorine (F) may be 10 wt% to 60 wt% of the total weight of the electrolyte.
[0046] In some embodiments, the mixture may further comprise a thermal initiator, and curing the mixture may comprise heat treating the mixture.
[0047] In some embodiments, the mixture may further comprise a photoinitiator, and curing the mixture may comprise irradiating the mixture with light.
[0048]
[0049] The electrolyte monomer according to exemplary embodiments of the present disclosure may use a plurality of self-extinguishing electrolyte monomers together. The ignition stability of the electrolyte including the electrolyte monomers may be improved.
[0050] The electrolyte monomer according to exemplary embodiments of the present disclosure may be included in an electrolyte for a secondary battery in a predetermined content range. This may improve both the stability and electrical properties of the electrolyte.
[0051] Lithium secondary batteries according to exemplary embodiments of the present disclosure may include the electrolyte for secondary batteries. The battery may exhibit improved room-temperature and high-temperature safety and ionic conductivity, thereby improving lifespan characteristics and electrical properties.
[0052]
[0053] FIG. 1 is a schematic process flow diagram for explaining a method for manufacturing an electrolyte for a secondary battery according to exemplary embodiments.
[0054] Figure 2 is a schematic cross-sectional view showing an electrode cell according to exemplary embodiments.
[0055] Figure 3 is a schematic diagram showing the structure of an electrolyte layer for a secondary battery according to exemplary embodiments.
[0056] FIG. 4 is a graph showing DSC evaluation of lithium secondary batteries manufactured according to exemplary embodiments and comparative examples.
[0057]
[0058] According to exemplary embodiments, a monomer for an electrolyte, a method for producing an electrolyte for a secondary battery comprising the same, and an electrolyte for a secondary battery produced thereby are provided. In addition, a lithium secondary battery comprising an electrolyte layer comprising the electrolyte for a secondary battery is provided.
[0059] Hereinafter, the present disclosure will be described in detail with reference to the attached drawings. However, these are merely exemplary and the present disclosure is not limited to the specific embodiments described as examples.
[0060] Hereinafter, unless otherwise specifically defined in this specification, when a part such as a layer, film, thin film, region, or plate is said to be “on” another part, this may include not only the case where it is “directly above” the other part, but also the case where there is another part in between.
[0061] If there are isomers of a compound represented by a chemical formula used in the present disclosure, the compound represented by the chemical formula means a representative chemical formula that includes the isomers.
[0062] The term “substituted” as used in the present disclosure may mean that at least one of the hydrogen atoms of the compound is substituted with a substituent such as a halogen group, a hydroxyl group, a heteroalkyl group, a heterocycloalkyl group, a heteroaryl group, an amine group, a nitrile group, a nitro group, or a silyl group.
[0063] The term “unsubstituted” as used herein may mean that all hydrogen atoms of a compound are unsubstituted.
[0064] The term “substituted or unsubstituted Y group of Ca to Cb” used in the present disclosure means that the Y group in an unsubstituted state has a to b carbon atoms, and does not include the carbon atoms of the substituent substituted on the Y group.
[0065] The term "oxyalkylene group" as used herein is used to encompass compounds in which any one of the methylene groups (-CH2-) of a straight-chain or branched-chain saturated hydrocarbon is replaced with an oxygen atom. For example, the oxyalkylene group may be represented as "-Ra-O-" or "-Ra-O-Rb-" (Ra and Rb are alkylene groups).
[0066] The term "flame retardancy" used in this disclosure refers to the ability of a sample to burn when in contact with a flame (ignition source), but to prevent or suppress combustion by emitting flames on its own when the flame is removed. The flame retardancy can be evaluated by the time it takes for a sample to be extinguished when the torch is removed after igniting it by supplying a flame of a certain heat amount to the sample for more than 1 second. The shorter the time taken for extinguishment, the better the flame retardancy can be evaluated.
[0067] Specifically, the term flame retardant compound used in the present disclosure may be a compound that, when glass fiber cut to 16 pi is impregnated with the flame retardant compound and cured as needed, and then ignited by supplying a flame of a constant heat amount for 1 second or more using a torch and the torch is removed, has an extinguishing time (s / g) relative to the mass of the sample of 60 s / g or less, specifically 55 s / g or less, and more specifically 53 s / g or less.
[0068] The electrolyte monomer according to exemplary embodiments may include a first monomer represented by chemical formula 1 and a second monomer represented by chemical formula 2.
[0069] [Chemical Formula 1]
[0070]
[0071] In chemical formula 1, R1 is a substituted or unsubstituted alkylene group having C2 to C12, C2 to C10 or C2 to C8, or a substituted or unsubstituted oxyalkylene group having C2 to C10, C2 to C8 or C2 to C6,
[0072] In chemical formula 1, j can be an integer from 1 to 5, from 1 to 4, or from 1 to 3.
[0073] The compound represented by the formula (1) may include equivalents, for example, at least one hydrogen bonded to the carbon of the formula (1) may be further substituted with an equivalent range of substituents, for example, at least one hydrogen bonded to the carbon of the formula (1) may be further substituted with deuterium or an alkyl group having 1 to 5 carbon atoms.
[0074] [Chemical Formula 2]
[0075]
[0076] In chemical formula 2, R2, R3 and R4 are each independently a substituted or unsubstituted alkylene group having C2 to C10, C2 to C8 or C2 to C6, or a substituted or unsubstituted oxyalkylene group having C2 to C10, C2 to C8 or C2 to C6,
[0077] In chemical formula 2, l, m, and n can each independently be an integer from 0 to 5, 0 to 4, or 0 to 3.
[0078] The compound represented by the formula 2 may include equivalents, for example, at least one hydrogen bonded to the carbon in the formula 2 may be further substituted with an equivalent range of substituents, for example, at least one hydrogen bonded to the carbon in the formula 2 may be further substituted with deuterium or an alkyl group having 1 to 5 carbon atoms.
[0079] For example, an oxymethylene group may have a structure in which one of the carbon atoms of an ethylene group is replaced by an oxygen atom. Examples of an oxyalkylene group include an oxymethylene group, an oxyethylene group, an oxypropylene group, an oxybutylene group, an oxypentylene group, a dimethyloxypropylene group, and an ethyloxypropylene group.
[0080] The second monomer is a phosphorus compound containing a phosphate group. The phosphorus compound can be thermally decomposed upon combustion to produce polymetaphosphate. In addition, as the polymetaphosphate is produced, a carbon compound (e.g., charcoal) can be produced through dehydration and esterification and dehydrogenation of the polymetaphosphate. The polymetaphosphate can form a protective layer, and the carbon compound can form a carbon film. The phosphorus compound can block oxygen and heat by the protective layer and carbon film formed upon combustion. Therefore, the monomer represented by the chemical formula 2 can have high self-extinguishing properties. Accordingly, the flame retardancy of an electrolyte including the monomer represented by the chemical formula 2 can be improved.
[0081] The first monomer may include two acrylate groups, and the second monomer may include three acrylate groups. For example, the molecular terminals of the first monomer and the second monomer may both include acrylate groups. Accordingly, the first monomer and the second monomer may be polymerized or copolymerized with each other. The first monomer and the second monomer may be copolymerized into a crosslinked polymer or a network polymer. The crosslinked polymer or the network polymer may have thermosetting properties. Therefore, the polymerization of the electrolyte monomer may improve flame retardancy.
[0082] In some embodiments, the content of the second monomer relative to the first monomer may be 0.5 to 2, 0.5 to 1.5, 0.8 to 1.5, or 0.8 to 1.2 by weight. In this range, the first monomer and the second monomer may be copolymerized so that the copolymer may be copolymerized as a whole into a crosslinked polymer or a network polymer. Accordingly, the thermosetting properties of the copolymer (e.g., the copolymer of the first monomer and the second monomer) may be improved, and the flame retardancy of an electrolyte including the copolymer may be improved.
[0083] In some embodiments, R1 in the above chemical formula 1 may be a fluorine-substituted alkylene group having a group number of C2 to C12, C2 to C10, or C2 to C8. Accordingly, the first monomer may include fluorine. The fluorine atom can suppress a combustion reaction by receiving electrons from a radical that causes a chain combustion reaction upon ignition. Therefore, the flame retardancy of the first monomer may be improved. In addition, the fluorine may react with lithium to form a protective film on the surface of the lithium electrode, thereby improving the stability and capacity efficiency of the secondary battery.
[0084] In some embodiments, R1 in the above formula 1 may be a fluorine-substituted oxyalkylene group of C2 to C10, C2 to C8, or C2 to C6. Accordingly, the dehydration reaction of polymetaphosphoric acid may be promoted due to the oxygen of the oxyalkylene group included in the first monomer, thereby forming a carbon compound, and the flame retardancy of the electrolyte monomer including the first monomer may be further improved.
[0085] The term "fluorine substituted" as used in this application may mean that at least one of the hydrogen atoms of the compound is replaced with fluorine (F).
[0086] In some embodiments, l, m, and n in the above chemical formula 2 may each independently be 0 to 3, 0 to 2, or 1. Accordingly, the phosphorus content may be high within the same capacity (or molecule). Accordingly, a protective layer by phosphorus may be easily formed, and flame retardancy may be improved.
[0087] In some embodiments, R2, R3, and R4 in the above chemical formula 2 may each independently be an unsubstituted alkylene group having C2 to C10, C2 to C8, or C2 to C4. Accordingly, the production of carbon compounds produced by the esterification reaction and dehydrogenation reaction of the polymetaphosphoric acid may be promoted, thereby improving self-extinguishing properties upon ignition.
[0088] In some embodiments, at least two of R2, R3, and R4 in the above chemical formula 2 may be the same. In one embodiment, R2, R3, and R4 in the above chemical formula 2 may be the same. Accordingly, when the monomer represented by the above chemical formula 1 and / or the monomer represented by the above chemical formula 2 is polymerized, the polymerization may be stably extended. Accordingly, the mechanical stability of the electrolyte for a secondary battery including the polymer derived from the monomer for the electrolyte may be improved.
[0089] In some embodiments, at least two of l, m, and n in the chemical formula 2 may be the same integer. In one embodiment, l, m, and n in the chemical formula 2 may be the same integer. Accordingly, the lengths of the functional groups of the chemical formula 2 (e.g., functional groups including a (meth)acrylate group) may be the same or similar. Accordingly, the monomer represented by the chemical formula 2 may be stably polymerized and extended. Accordingly, the mechanical stability of the electrolyte for a secondary battery may be improved.
[0090] In some embodiments, the first monomer may comprise a monomer represented by the following chemical formula 1-a.
[0091] [Chemical Formula 1-a]
[0092]
[0093] In the above chemical formula 1-a, o may be an integer of 1 to 5, 1 to 4, or 1 to 3. Accordingly, the first monomer may include an alkoxy group and fluorine, so that the flame retardancy of the electrolyte including the monomer represented by the above chemical formula 1-a may be further improved. In addition, since two acrylate groups may be included at the terminal, it may be copolymerized with the second monomer to form a crosslinked polymer or a network polymer, so that high-temperature stability may be improved.
[0094] In some embodiments, the compound represented by Formula 1-a may include equivalents, wherein at least one hydrogen bonded to the carbon of Formula 1-a may be further substituted with an equivalent range of substituents. For example, at least one hydrogen bonded to the carbon of Formula 1-a may be further substituted with a deuterium or an alkyl group having 1 to 5 carbon atoms.
[0095] In some embodiments, the first monomer may comprise a monomer represented by the following chemical formula 1-b.
[0096] [Chemical Formula 1-b]
[0097]
[0098] In the above chemical formula 1-b, r may be an integer of 1 to 8, 1 to 6, or 2 to 6. Accordingly, the first monomer may include fluorine and may include two acrylate groups at the terminal. Accordingly, the flame retardancy of the electrolyte including the monomer represented by chemical formula 1-b may be further improved, and the electrolyte may be copolymerized with the second monomer to form a crosslinked polymer or a network polymer, thereby improving high-temperature stability.
[0099] In some embodiments, the compound represented by Formula 1-b may include equivalents, wherein at least one hydrogen bonded to the carbon of Formula 1-b may be further substituted with an equivalent range of substituents. For example, at least one hydrogen bonded to the carbon of Formula 1-b may be further substituted with deuterium or an alkyl group having 1 to 5 carbon atoms.
[0100] In one embodiment, the first monomer may include at least one of a monomer represented by the following chemical formula 1-1 and a monomer represented by the following chemical formula 1-2.
[0101] [Chemical Formula 1-1]
[0102]
[0103] [Chemical Formula 1-2]
[0104]
[0105] The monomer represented by the above chemical formula 1-1 and the monomer represented by the above chemical formula 1-2 contain a fluorine atom and both terminals are acrylate groups (two acrylate groups). Accordingly, the flame retardancy of the first monomer including at least one of the monomer represented by the above chemical formula 1-1 and the monomer represented by the above chemical formula 1-2 can be improved. In addition, the flame retardancy can be improved by copolymerizing with the second monomer to form a crosslinked polymer or a network polymer.
[0106] In some embodiments, the compounds represented by Formulae 1-1 and 1-2 may include equivalents, and at least one hydrogen bonded to a carbon atom of Formulae 1-1 and 1-2 may be further substituted with an equivalent range of substituents. For example, at least one hydrogen bonded to a carbon atom of Formulae 1-1 and 1-2 may be further substituted with a deuterium atom or an alkyl group having 1 to 5 carbon atoms.
[0107] In some embodiments, the second monomer may comprise a monomer represented by the following chemical formula 2-a.
[0108] [Chemical Formula 2-a]
[0109]
[0110] In the above chemical formula 2-a, s1, s2, and s3 can each independently be an integer of 0 to 5, 0 to 4, or 0 to 3. Accordingly, the phosphorus content per molecule of the second monomer can increase, and fluorine can be included. Therefore, the flame retardancy of an electrolyte including a monomer represented by the above chemical formula 2-a can be improved. In addition, the compound represented by the above chemical formula 2-a can include three acrylate groups at the terminal. Therefore, it can be stably polymerized with the first monomer to form a network-like polymer, and high-temperature stability can be further improved.
[0111] In some embodiments, the compound represented by Formula 2-a may include equivalents, wherein at least one hydrogen bonded to the carbon of Formula 2-a may be further substituted with an equivalent range of substituents. For example, at least one hydrogen bonded to the carbon of Formula 2-a may be further substituted with deuterium or an alkyl group having 1 to 5 carbon atoms.
[0112] In some embodiments, the second monomer may comprise a monomer represented by the following chemical formula 2-b.
[0113] [Chemical Formula 2-b]
[0114]
[0115] In the above chemical formula 2-b, t1, t2, and t3 can each independently be 1 to 5, 1 to 4, or 1 to 3. The monomer represented by the above chemical formula 2-b can contain both an alkoxy group and fluorine. Accordingly, the flame retardancy of an electrolyte including the monomer represented by the above chemical formula 2-b can be improved. In addition, the monomer represented by the above chemical formula 2-b can contain three acrylate groups at the terminal. Therefore, it can be polymerized with the first monomer to form a network polymer, and high-temperature stability can be further improved.
[0116] In some embodiments, the compound represented by Formula 2-b may include equivalents, and at least one hydrogen bonded to the carbon of Formula 2-b may be further substituted with an equivalent range of substituents. For example, at least one hydrogen bonded to the carbon of Formula 2-b may be further substituted with deuterium or an alkyl group having 1 to 5 carbon atoms.
[0117] In one embodiment, the second monomer may include at least one of a monomer represented by the following chemical formula 2-1 to a monomer represented by the following chemical formula 2-3.
[0118] [Chemical Formula 2-1]
[0119]
[0120] [Chemical Formula 2-2]
[0121]
[0122] [Chemical Formula 2-3]
[0123]
[0124] The monomer represented by the above chemical formula 2-1 to the above chemical formula 2-3 is a phosphorus compound containing a phosphate group and all terminals are acrylate groups (three acrylate groups). Accordingly, the flame retardancy of the second monomer including at least one of the monomer represented by the above chemical formula 2-1 to the above chemical formula 2-2 can be improved. In addition, the flame retardancy can be improved by copolymerizing with the first monomer to form a crosslinked polymer or a network polymer.
[0125] In some embodiments, the compounds represented by Formulae 2-1 to 2-3 may include equivalents, and at least one hydrogen bonded to a carbon atom of Formulae 2-1 to 2-3 may be further substituted with an equivalent range of substituents. For example, at least one hydrogen bonded to a carbon atom of Formulae 2-1 to 2-3 may be further substituted with a deuterium or an alkyl group having 1 to 5 carbon atoms.
[0126] In some embodiments, the electrolyte monomer may include at least one of the monomer represented by the above chemical formula 1-a and the monomer represented by the above chemical formula 1-b, and at least one of the monomer represented by the above chemical formula 2-a and the monomer represented by the above chemical formula 2-b. Accordingly, the electrolyte monomer may be stably copolymerized into a crosslinked polymer or a network polymer, and flame retardancy may be improved.
[0127] In some embodiments, the electrolyte monomer may include at least one of the monomer represented by Chemical Formula 1-1 and the monomer represented by Chemical Formula 1-2, and at least one of the monomer represented by Chemical Formula 2-1 to the monomer represented by Chemical Formula 2-3. Accordingly, the electrolyte monomer may be more stably copolymerized into a crosslinked polymer or a network polymer, and flame retardancy may be further improved.
[0128] In one embodiment, the electrolyte monomer may include both the monomer represented by the above chemical formula 1-1 and the monomer represented by the above chemical formula 2-1. Accordingly, the electrolyte monomer may be copolymerized into a copolymer containing fluorine and having a high weight-based phosphorus content. Accordingly, the flame retardancy of the copolymer may be further improved.
[0129] An electrolyte for a secondary battery according to exemplary embodiments (hereinafter, abbreviated as “electrolyte”) may include a flame-retardant compound (110) and a lithium salt, which include a polymer derived from the above-described electrolyte monomer. In some embodiments, the electrolyte may include a flame-retardant compound (110), a lithium salt, and an electrolyte. For example, the flame-retardant compound may include a polymer of the above-described electrolyte monomer.
[0130] The above lithium salt is, for example, Li + X - can be expressed as . The anion of the lithium salt (X - ) as F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C -, CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - Examples include:
[0131] According to exemplary embodiments, the flame retardant compound (110) may include a polymer of the above-described electrolyte monomer. For example, the flame retardant compound (110) may be a polymer and / or copolymer of the above-described electrolyte monomer. Accordingly, side reactions of the flame retardant compound (110) with compounds such as lithium salts, or electrolytes, etc. may be suppressed. In addition, the flame retardant compound (110) may include a phosphorus-containing functional group, thereby blocking oxygen during combustion and preventing thermal runaway.
[0132] In some embodiments, the flame retardant compound (110) may be a compound polymerized or copolymerized with an electrolyte monomer having a thermally reactive functional group and / or a photoreactive functional group. For example, the electrolyte monomer described above contains an acrylate group. Accordingly, the acrylate group may function as a thermally reactive functional group or a photoreactive functional group.
[0133] In some embodiments, the flame retardant compound (110) may have a structure in which an acrylate group of a monomer represented by the above chemical formula 1 and an acrylate group of a monomer represented by the above chemical formula 2 are copolymerized.
[0134] For example, the flame retardant compound (110) may have a structure in which at least one acrylate group among the monomer represented by the chemical formula 1-a and the monomer represented by the chemical formula 1-b, and at least one acrylate group among the monomer represented by the chemical formula 2-a and the monomer represented by the chemical formula 2-b, are copolymerized.
[0135] For example, the flame retardant compound (110) may have a structure in which at least one acrylate group among the monomers represented by the chemical formula 1-1 and the monomers represented by the chemical formula 1-2, and at least one acrylate group among the monomers represented by the chemical formula 2-1 to the monomers represented by the chemical formula 2-3, are copolymerized. Accordingly, the flame retardant compound (110) may be formed in a network or cross-linked polymer form. Accordingly, the flame retardancy of the electrolyte including the flame retardant compound (110) may be further improved.
[0136] In some embodiments, the electrolyte (100) may further include a composite electrolyte comprising an organic polymer and an inorganic electrolyte.
[0137] In some embodiments, the composite electrolyte may have a film form. In one embodiment, the organic polymer and the inorganic electrolyte may form a composite film. For example, the organic polymer and the inorganic electrolyte may be physically bound within the composite film.
[0138] The organic polymer may be an ion-conducting polymer. For example, the organic polymer may include repeating units of ether, styrene, and fluorinated hydrocarbon groups.
[0139] In some embodiments, the organic polymer is polyvinylidene fluoride (PVDF), polystyrene (PS), polyether sulfone (PES), polyurethane (PU), polyethylene oxide (PEO), polyvinylidene fluoride-co-hexafluoropropylene (PVDF-co-HFP), polyimide (PI), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyvinyl alcohol (PVA), polyacrylonitrile (PAN), polyethyl methacrylate (PEMA), polycaprolactone (PCL), and Polyvinyl pyrrolidone (PVP) and the like may be included. In one embodiment, the organic polymer may include at least one of polyvinylidene fluoride, polystyrene, polyethersulfone, and polyurethane. Accordingly, the mobility of lithium ion conduction within the composite electrolyte may be improved, thereby improving ion conductivity.
[0140] In some embodiments, the inorganic electrolyte may be an oxide-based solid electrolyte. For example, the oxide-based solid electrolyte may include an ion-conducting compound containing a metal or oxygen. For example, the oxide-based solid electrolyte may include an LLTO-based compound, an LLZO-based compound, a Li 6.4 La3Zr 1.4 Ta 0.6 O 12 , Li6La2CaTa2O12, Li6La2ANb2O 12(A is Ca or Sr), Li2Nd3TeSbO 12 , Li3BO 2.5 N 0.5 , Li9SiAlO8, LAGP compounds, LATP compounds, Li 1+x Ti 2-x Al x Si y (PO4)3(0≤x≤1, 0≤y≤1), LiAl x Zr 2-x (PO4)3(0≤x≤1, 0≤y≤1), LiTi x Zr 2-x (PO4)3(0≤x≤1, 0≤y≤1), LISICON compounds, LIPON compounds, perovskite compounds, NASICON compounds, metal oxides such as Al2O3, ZnO2, Ce2O2, TiO2, ZrO2, HfO2, MnO2, MgO, WO2, V2O5, etc. may be included.
[0141] In one embodiment, the inorganic electrolyte may be a lithium-containing oxide-based solid electrolyte. For example, the lithium-containing oxide-based solid electrolyte may include an LLTO-based compound, an LLZO-based compound (e.g., a garnet-type LLZO-based compound), a NASICON-based compound, a LATP-based compound, a perovskite-based compound, etc. Accordingly, the ionic conductivity and mechanical strength of the electrolyte (100) may be improved, lithium dendrite may be suppressed, and high-temperature stability and life characteristics may be improved.
[0142] In some embodiments, the content of the flame retardant compound (110) may be 3 wt% to 20 wt%, 3 wt% to 15 wt%, or 3 wt% to 10 wt% of the total weight of the electrolyte for a secondary battery. In the above range, the ionic conductivity of the electrolyte (100) may be improved while the flame retardancy may be improved. In one embodiment, the content of the flame retardant compound (110) may be 4 wt% to 10 wt%, 4 wt% to 8 wt%, or 4.5 wt% to 8 wt% of the total weight of the electrolyte for a secondary battery. In the above range, the ionic conductivity of the electrolyte (100) may be improved while the flame retardancy is improved.
[0143] In some embodiments, pores may be formed in the composite membrane. Accordingly, a flame-retardant compound (110) may be positioned in the pores of the composite membrane. Accordingly, the ionic conductivity and flame retardancy of the electrolyte (100) may be improved, and resistance may be reduced.
[0144] FIG. 1 is a process flow diagram illustrating a method for manufacturing an electrolyte for a secondary battery according to exemplary embodiments. Hereinafter, the method for manufacturing the electrolyte for a secondary battery described above will be described with reference to FIG. 1.
[0145] Referring to FIG. 1, a mixture including the above-described electrolyte monomer and electrolyte solution can be prepared (e.g., step S10).
[0146] For example, a mixture can be prepared by mixing the above-described electrolyte monomer and electrolyte solution.
[0147] In some embodiments, the mixture may further comprise an organic polymer and an inorganic electrolyte. For example, the mixture may comprise an electrolyte monomer, an electrolyte solution, an organic polymer, and an inorganic electrolyte.
[0148] In some embodiments, the organic polymer and the inorganic electrolyte may be mixed with the electrolyte monomer and the electrolyte solution in the form of a composite electrolyte membrane.
[0149] The above composite electrolyte membrane can be manufactured by drying a preliminary composite membrane including the organic polymer, the inorganic electrolyte, the first solvent, and the second solvent.
[0150] In some embodiments, the solubility of the organic polymer in the first solvent may be greater than the solubility of the organic polymer in the second solvent. For example, the solubility of the organic polymer in the first solvent may be at least 1 g / 100 g, at least 33 g / 100 g, at least 10 g / 100 g, at least 100 g / 100 g, or from 100 g / 100 g to 1,000 g / 100 g. For example, the solubility of the organic polymer in the second solvent may be less than 1 g / 100 g, less than 0.1 g / 100 g, or less than 0.01 g / 100 g.
[0151] In one embodiment, the organic polymer within the preparatory composite membrane may be soluble in the first solvent and insoluble in the second solvent.
[0152] For example, the organic polymer may be soluble in the first solvent. Accordingly, the organic polymer may be dissolved in the first solvent.
[0153] For example, the organic polymer may be insoluble in the second solvent. Accordingly, the organic polymer may not substantially dissolve in the second solvent.
[0154] The above 'solubility' refers to the mass (g) of an organic polymer dissolved in 100 g of a first solvent or a second solvent. For example, a solubility of 1 g / 100 g may mean that 1 g of an organic polymer dissolves in 100 g of a first solvent or a second solvent.
[0155] In some embodiments, the first solvent may be miscible with the second solvent. For example, the first solvent and the second solvent may be mixed or blended.
[0156] The above organic polymer and the above inorganic electrolyte may be the above-described organic polymer and inorganic electrolyte.
[0157] The first solvent may be a solvent that dissolves the organic polymer and is mixed with the second solvent. The first solvent may include, for example, tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-Me-THF), N-methyl-2-pyrrolidone (NMP), 1,3-dioxolane, vinylene carbonate (VC), etc. These may be used alone or in combination of two or more. In one embodiment, the first solvent may be tetrahydrofuran.
[0158] The second solvent may be a solvent that does not dissolve the organic polymer and is mixed with the first solvent. The second solvent may include, for example, heptane, octane, nonane, decane, dodecane, 2,2,4-trimethylpentane, etc. These may be used alone or in combination of two or more. In one embodiment, the second solvent may be octane.
[0159] The above drying can be performed by casting the preliminary composite film on a substrate (e.g., a glass substrate, a plastic substrate, etc.).
[0160] In exemplary embodiments, drying the preliminary composite membrane to produce the composite membrane may include removing the first solvent from the preliminary composite membrane and removing the second solvent.
[0161] In some embodiments, drying the preliminary composite membrane to produce a composite membrane may include removing the first solvent at a first temperature and removing the second solvent at a second temperature. For example, the composite membrane may be produced by drying the first solvent in the preliminary composite membrane and then drying the second solvent. The first drying and the second drying may be performed sequentially, or the second drying may be performed after a certain period of time has elapsed after the first drying. Accordingly, the first solvent may be dried first, and then the second solvent may be dried.
[0162] In some embodiments, the content of the monomer for the electrolyte may be 3 wt% to 20 wt%, 3 wt% to 15 wt%, or 3 wt% to 10 wt% of the total weight of the mixture. In this range, the ionic conductivity of the electrolyte may be improved while the flame retardancy may be improved. In one embodiment, the content of the monomer for the electrolyte may be 4 wt% to 10 wt%, 4 wt% to 8 wt%, or 4.5 wt% to 8 wt% of the total weight of the mixture. In this range, the ionic conductivity of the electrolyte may be further improved while the flame retardancy of the electrolyte is improved.
[0163] In some embodiments, the above-described electrolyte monomer may include a phosphorus-containing functional group and at least one of a thermally reactive functional group and a photoreactive functional group.
[0164] In some embodiments, the electrolyte may include a thermal initiator and / or a photoinitiator for inducing thermal curing and / or photocuring of the flame-retardant monomer. In one embodiment, the content of the thermal initiator and / or photoinitiator may be 0.5 to 2 parts by weight per 100 parts by weight of the mixture included in each electrolyte composition.
[0165] For example, the thermal initiator may include an azo compound such as 2,2-azobis(2-cyanobutane), 2,2-azobis(methylbutyronitrile), 2,2'-azoisobutyronitrile (AIBN), azobisdimethyl-valeronitrile (AMVN), or a peroxide compound such as benzoyl peroxide, acetyl peroxide, dilauryl peroxide, di-tert-butyl peroxide, cumyl peroxide, or hydrogen peroxide.
[0166] For example, the photoinitiator may include acyl phosphines such as 2-hydroxy-2-methyl-1-phenylpropan-1-one (HMPP), benzoin ether, dialkyl acetophenone, hydroxyl alkylketone, phenyl glyoxylate, Benzyl Dimethyl Ketal, 2,4,6-trimethyl-benzoyl-trimethyl phosphine oxide, and α-aminoketones.
[0167] In some embodiments, the electrolyte may include a lithium salt. The lithium salt may include the lithium salt described above. Accordingly, the ionic conductivity of the electrolyte for a secondary battery may be improved.
[0168] According to exemplary embodiments, the mixture may include an electrolyte.
[0169] In some embodiments, the electrolyte may include an ether electrolyte containing fluorine (F). For example, the ether electrolyte containing the fluorine is 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,2-trofluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 2,2,3,3-tetrafluoro-1,4-dimethoxybutane (FDMB), 1,1,2,2,3,3,4,4-octafluoro-5-methoxy pentane, and At least one of bis(2,2,2-trifluoroethyl)ether may be included. Due to the electronegativity of fluorine in the ether-based electrolyte containing fluorine, the dissociation of the lithium salt may be affected. The fluorine separated from the fluorine-based electrolyte may react with lithium to form a protective film on the surface of the lithium electrode, thereby improving the stability and capacity efficiency of the secondary battery. In addition, the separated fluorine may suppress a chain reaction when ignited, thereby improving flame retardancy.
[0170] In some embodiments, the electrolyte may include an organic solvent. For example, the organic solvent may be a carbonate organic solvent such as propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), dipropyl carbonate (DPC), and vinylene carbonate (VC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, sulfolane, gamma-butyrolactone, propylene sulfite, and tetrahydrofuran. These may be used alone or in combination of two or more.
[0171] In some embodiments, the content of the fluorine-containing ether electrolyte in the total volume of the electrolyte may be 10% to 60% by volume, 20% to 60% by volume, or 20% to 55% by volume. In this range, the flame retardancy of the electrolyte including the fluorine-containing solvent may be improved, and the capacity efficiency of a secondary battery including the electrolyte may be improved.
[0172] In one embodiment, the electrolyte may further include an additive. The additive may include, for example, a cyclic carbonate compound, a fluorine-substituted cyclic carbonate compound, a sultone compound, a cyclic sulfate compound, a cyclic sulfite compound, a phosphate compound, and a borate compound.
[0173] The above cyclic carbonate compound may include vinylene carbonate, vinyl ethylene carbonate (VEC), etc.
[0174] The above fluorine-substituted cyclic carbonate compound may include fluoroethylene carbonate (FEC), etc.
[0175] The above sultone compounds may include 1,3-propane sultone, 1,3-propene sultone, 1,4-butane sultone, etc.
[0176] The above cyclic sulfate compound may include 1,2-ethylene sulfate, 1,2-propylene sulfate, etc.
[0177] The above cyclic sulfite compound may include ethylene sulfite, butylene sulfite, etc.
[0178] The above phosphate compound may include lithium difluoro bis-oxalato phosphate, lithium difluoro phosphate, etc.
[0179] The above borate compound may include lithium bis(oxalate) borate, etc.
[0180] In one embodiment, the organic solvent may be a carbonate-based organic solvent. Accordingly, the electrical and chemical stability of the electrolyte for a secondary battery may be improved.
[0181] According to exemplary embodiments, the mixture can be cured (e.g., step S20). Accordingly, an electrolyte for a secondary battery can be manufactured.
[0182] In some embodiments, the electrolyte monomer may be polymerized or copolymerized while the mixture is cured. Accordingly, the secondary battery electrolyte may include a flame retardant compound comprising a polymer of the electrolyte monomer.
[0183] In some embodiments, the content of the electrolyte monomer in the total weight of the mixture may be substantially the same as the content of the flame retardant compound in the total weight of the electrolyte. For example, the weight that decreases or increases as the mixture is cured may be 0.0001 wt% or 0.00001 wt% or less with respect to the total weight of the electrolyte monomer. Accordingly, the content of the electrolyte monomer in the total weight of the mixture may be substantially the same as the content of the flame retardant compound in the total weight of the electrolyte.
[0184] In some embodiments, curing the mixture may be heat treating the mixture. For example, by heat curing the mixture, the electrolyte monomer within the mixture may be polymerized or copolymerized into a flame retardant compound.
[0185] In some embodiments, the heat treatment may be from 40° C. to 160° C., 60° C. to 160° C., 80° C. to 160° C., 80° C. to 140° C., or 80° C. to 120° C. In one embodiment, the heat treatment may be performed by increasing the temperature from room temperature (e.g., 25° C.) at 1° C. / min to 10° C. / min, 2° C. / min to 10° C. / min, or 3° C. / min to 10° C. / min.
[0186] In some embodiments, the heat treatment may be performed for 30 minutes to 2 hours, 30 minutes to 1.5 hours, or 45 minutes to 1.25 hours.
[0187] In the above temperature and time range, the electrolyte monomer within the mixture can be sufficiently polymerized or copolymerized.
[0188] In some embodiments, curing the mixture may involve irradiating the mixture with light. For example, by curing the mixture with light, the electrolyte monomer within the mixture may polymerize or copolymerize into a flame-retardant compound. Accordingly, the polymerization or copolymerization reaction of the electrolyte monomer can be performed at a relatively low temperature. Consequently, side reactions of the electrolyte solution and the like caused by high-temperature heat treatment can be prevented.
[0189] In some embodiments, the UV photocuring process for the photopolymerization is performed at a wavelength of 250 nm to 400 nm and at 800 mW / cm 2 1100mW / cm 2 The process can be performed using light of a certain wavelength. In one embodiment, the UV photocuring process can be performed for 5 to 20 seconds. Within the above wavelength and intensity range, the flame-retardant monomer can be sufficiently polymerized or copolymerized.
[0190] Figure 2 is a schematic cross-sectional view showing an electrode cell according to exemplary embodiments.
[0191] A secondary battery according to exemplary embodiments may include an electrode cell. Referring to FIG. 2, the electrode cell may include a positive electrode (240), a negative electrode (260) facing the positive electrode (240), and an electrolyte layer (210) disposed between the positive electrode (240) and the negative electrode (260).
[0192] The positive electrode (240) may include a positive electrode current collector (235) and a positive electrode active material layer (210) disposed on at least one surface of the positive electrode current collector (235).
[0193] The positive electrode current collector (235) may include stainless steel, nickel, aluminum, titanium, or an alloy thereof. The positive electrode current collector (235) may also include aluminum or stainless steel surface-treated with carbon, nickel, titanium, or silver. The positive electrode current collector (235) may have a thickness of, but is not limited to, 10 μm to 50 μm, for example.
[0194] The above positive electrode active material may include a compound capable of reversibly intercalating and deintercalating lithium ions.
[0195] According to exemplary embodiments, the positive electrode active material may include a lithium-nickel metal oxide. The lithium-nickel metal oxide may further include at least one of cobalt (Co), manganese (Mn), and aluminum (Al).
[0196] In some embodiments, the positive electrode active material or the lithium-nickel metal oxide may include a layered structure or crystal structure represented by the following chemical formula 3.
[0197] [Chemical Formula 3]
[0198] Li x Ni a M b O 2+2
[0199] In chemical formula 3, 0.9≤x≤1.2, 0.6≤a≤0.99, 0.01≤b≤0.4, -0.5≤z≤0.1 may be satisfied. As described above, M may include Co, Mn, and / or Al.
[0200] The chemical structure represented by Chemical Formula 3 represents the bonding relationship included in the layered structure or crystal structure of the positive electrode active material and does not exclude additional elements. For example, M includes Co and / or Mn, and Co and / or Mn can serve as the main active element of the positive electrode active material together with Ni. Chemical Formula 3 is provided to express the bonding relationship of the main active elements and should be understood as a formula encompassing the introduction and substitution of additional elements.
[0201] In one embodiment, auxiliary elements may be further included in addition to the main active element to enhance the chemical stability of the positive electrode active material or the layered structure / crystal structure. The auxiliary elements may be incorporated into the layered structure / crystal to form bonds, and in this case, it should be understood that they are also included within the chemical structure range represented by Chemical Formula 3.
[0202] The auxiliary element may include, for example, at least one of Na, Mg, Ca, Y, Ti, Hf, V, Nb, Ta, Cr, Mo, W, Fe, Cu, Ag, Zn, B, Al, Ga, C, Si, Sn, Sr, Ba, Ra, P, or Zr. The auxiliary element may also act as an auxiliary active element that contributes to the capacity / output activity of the positive electrode active material together with Co or Mn, for example, Al.
[0203] For example, the positive electrode active material or the lithium-nickel metal oxide may include a layered structure or crystal structure represented by the following chemical formula 3-1.
[0204] [Chemical Formula 3-1]
[0205] Li x Ni a M1 b1 M2 b2 O 2+z
[0206] In Chemical Formula 3-1, M1 may include Co, Mn, and / or Al. M2 may include the auxiliary elements described above. In Chemical Formula 3-1, 0.9≤x≤1.2, 0.6≤a≤0.99, 0.01≤b1+b2≤0.4, -0.5≤z≤0.1 may be satisfied.
[0207] The above-described positive electrode active material may further include a coating element or doping element. For example, elements substantially identical to or similar to the above-described auxiliary elements may be used as the coating element or doping element. For example, the above-described elements may be used singly or in combination of two or more.
[0208] The above coating element or doping element may be present on the surface of the lithium-nickel metal oxide particle, or may penetrate through the surface of the lithium-nickel metal composite oxide particle and be included in the bonding structure represented by the above chemical formula 3 or the above chemical formula 3-1.
[0209] The above positive electrode active material may include a nickel-cobalt-manganese (NCM) lithium oxide. In this case, an NCM lithium oxide with an increased nickel content may be used.
[0210] Ni can be provided as a transition metal associated with the output and capacity of a lithium secondary battery. Therefore, by employing a high-content (High-Ni) composition as described above in the positive electrode active material, a high-capacity positive electrode and a high-capacity lithium secondary battery can be provided.
[0211] However, as the Ni content increases, the long-term storage stability and lifespan stability of the cathode or secondary battery may relatively deteriorate, and side reactions with the electrolyte may also increase. However, according to exemplary embodiments, the inclusion of Co can maintain electrical conductivity, while the inclusion of Mn can improve lifespan stability and capacity retention characteristics.
[0212] The content of Ni (e.g., the mole fraction of nickel among the total moles of nickel, cobalt, and manganese) in the NCM-based lithium oxide may be 0.6 or more, 0.7 or more, or 0.8 or more. In some embodiments, the content of Ni may be 0.8 to 0.95, 0.82 to 0.95, 0.83 to 0.95, 0.84 to 0.95, 0.85 to 0.95, or 0.88 to 0.95.
[0213] In some embodiments, the positive electrode active material may include a lithium cobalt oxide-based active material, a lithium manganese oxide-based active material, a lithium nickel oxide-based active material, or a lithium iron phosphate (LFP)-based active material (e.g., LiFePO4).
[0214] In some embodiments, the positive electrode active material may include, for example, a Mn-rich active material, an LLO (Li rich layered oxide) / OLO (Over Lithiated Oxode) active material, or a Co-less active material having a chemical structure or crystal structure represented by the following chemical formula 4.
[0215] [Chemical Formula 4]
[0216] p[Li2MnO3]·(1-p)[Li q JO2]
[0217] In chemical formula 4, 0 <p<1이고, 0.9≤q≤1.2이며, J는 Mn, Ni, Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg 및 B 중 적어도 하나의 원소를 포함할 수 있다.
[0218] In some embodiments, the positive electrode active material may be a sodium-based active material or a potassium-based active material. The sodium-based active material may include a layered structure or crystal structure in which Li of the above-described chemical formulas 3, 3-1, and / or 4 is substituted with Na and / or K.
[0219] In some embodiments, the positive electrode active material may be a calcium-based active material. The calcium-based active material may include, for example, a calcium-cobalt active material and a calcium-phosphate active material.
[0220] For example, a positive electrode slurry can be prepared by mixing the positive electrode active material in a solvent. After coating the positive electrode slurry on a positive electrode current collector, drying and rolling can be performed to prepare a positive electrode active material layer. The coating process can be performed by methods such as gravure coating, slot die coating, multilayer simultaneous die coating, imprinting, doctor blade coating, dip coating, bar coating, casting, etc., but is not limited thereto. The positive electrode active material layer (230) can further include a binder and optionally can further include an electrolyte, a conductive agent, a thickener, etc.
[0221] Solvents used in the manufacture of the positive electrode active material layer (230) include, for example, N-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMA), N,N-dimethylaminopropylamine (DMAPA), ethylene oxide (EO), tetrahydrofuran (THF), etc.
[0222] In one embodiment, the electrolyte included in the positive electrode active material layer (230) may be the electrolyte for a secondary battery described above. In one embodiment, the electrolyte included in the positive electrode active material may be the inorganic electrolyte described above. For example, the secondary battery may be provided as an all-solid-state battery including the electrolyte described above or an inorganic electrolyte.
[0223] The above binder may include polyvinylidenefluoride (PVDF), poly(vinylidene fluoride-co-hexafluoropropylene) copolymer, polyacrylonitrile, polymethylmethacrylate, acrylonitrile butadiene rubber (NBR), polybutadiene rubber (BR), styrene-butadiene rubber (SBR), etc. In one embodiment, a PVDF series binder may be used as the positive electrode binder.
[0224] The conductive material may be added to enhance the conductivity and / or mobility of lithium ions or electrons of the positive electrode active material layer (230). For example, the conductive material may include, but is not limited to, a carbon-based conductive material such as graphite, carbon black, acetylene black, Ketjen black, graphene, carbon nanotubes, vapor-grown carbon fiber (VGCF), carbon fiber, etc., and / or a metal-based conductive material including a perovskite material such as tin, tin oxide, titanium oxide, LaSrCoO3, LaSrMnO3, etc.
[0225] The positive electrode active material layer (230) may further include a thickener and / or a dispersant. In one embodiment, the positive electrode active material layer (230) may include a thickener such as carboxymethyl cellulose (CMC).
[0226] The negative electrode (260) may include a negative electrode current collector (255) and a negative electrode active material layer (250) disposed on at least one surface of the negative electrode current collector (255).
[0227] The negative electrode current collector (255) may include, for example, copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, etc. The negative electrode current collector (255) is not limited thereto, but may have a thickness of, for example, 10 μm to 50 μm.
[0228] The negative electrode active material layer (250) may include a negative electrode active material. A material capable of adsorbing and desorbing lithium ions may be used as the negative electrode active material. For example, the negative electrode active material may be a carbon-based material such as crystalline carbon, amorphous carbon, a carbon composite, or carbon fiber; lithium metal; a lithium alloy; a silicon (Si)-containing material, or a tin (Sn)-containing material.
[0229] Examples of the above amorphous carbon include hard carbon, soft carbon, coke, mesocarbon, mesocarbon microbead (MCMB), and mesophase pitch-based carbon fiber (MPCF).
[0230] Examples of the above crystalline carbon include graphite-based carbons such as natural graphite, artificial graphite, graphitized coke, graphitized MCMB, and graphitized MPCF.
[0231] The lithium metal may be pure lithium metal or lithium metal having a protective layer formed thereon for suppressing dendrite growth, etc. In one embodiment, a lithium metal-containing layer deposited or coated on a negative electrode current collector may be used as the negative electrode active material layer (250). In one embodiment, a lithium thin film layer may also be used as the negative electrode active material layer (250).
[0232] Elements included in the above lithium alloy include aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium, or indium.
[0233] The above silicon-containing material can provide increased capacity characteristics. The above silicon-containing material is Si, SiO x (0 <x<2), 금속 도핑된 SiO x (0 <x<2), 실리콘-탄소 복합체 등을 포함할 수 있다. 상기 금속은 리튬 및 / 또는 마그네슘을 포함할 수 있으며, 금속 도핑된 SiO x (0 <x<2)는 금속 실리케이트를 포함할 수 있다.
[0234] For example, the negative electrode slurry can be prepared by mixing the negative electrode active material in a solvent. After coating / depositing the negative electrode slurry on a negative electrode current collector (255), drying and rolling can be performed to prepare a negative electrode active material layer (250). The coating process can be performed using substantially the same method as the method for preparing the positive electrode active material layer (230). The negative electrode active material layer (250) can further include a binder and optionally can further include an electrolyte, a conductive material, a thickener, etc.
[0235] In some embodiments, the negative electrode may include a negative electrode active material layer (250) in the form of lithium metal formed through a deposition / coating process.
[0236] Examples of solvents for the negative electrode active material layer include water, pure water, deionized water, distilled water, ethanol, isopropanol, methanol, acetone, n-propanol, t-butanol, etc.
[0237] In one embodiment, the electrolyte included in the negative electrode active material layer (250) may be the electrolyte for a secondary battery described above. In one embodiment, the electrolyte included in the negative electrode active material layer (250) may be the inorganic electrolyte described above. For example, the secondary battery may be provided as an all-solid-state battery including the electrolyte described above or an inorganic electrolyte.
[0238] The above-described materials that can be used in manufacturing the anode as the binder, conductive agent and thickener can be used.
[0239] In some embodiments, a styrene-butadiene rubber-based binder, carboxymethyl cellulose, a polyacrylic acid-based binder, a poly(3,4-ethylenedioxythiophene, PEDOT)-based binder, or the like may be used as the negative electrode binder.
[0240] Figure 3 is a schematic diagram showing the structure of an electrolyte layer for a secondary battery according to exemplary embodiments.
[0241] Referring to FIG. 3, the electrolyte layer (210) may include the electrolyte (100) described above. For example, the electrolyte layer (210) may include a flame retardant compound (110) included in the electrolyte (100). For example, the electrolyte layer (210) may include a film formed by impregnating and curing the mixture described above into a separator. The electrolyte layer (210) may be a separator including an electrolyte.
[0242] According to exemplary embodiments, an electrolyte layer (210) may be interposed between the positive electrode (240) and the negative electrode (260). The electrolyte layer (210) may be a solid electrolyte layer (210). For example, the solid electrolyte layer (210) may be a gel-polymer electrolyte layer (210) including the electrolyte described above.
[0243] According to exemplary embodiments, an electrode cell (200) is defined by an anode (240), a cathode (260), and a solid electrolyte layer (210), and a plurality of electrode cells (200) may be stacked to form an electrode assembly. For example, the electrode assembly may be formed through winding, lamination, folding, or the like.
[0244] For example, electrode tabs (positive electrode tab and negative electrode tab) may protrude from the positive electrode collector (235) and the negative electrode collector (255), respectively, and extend to one side of the case. The electrode tabs may be fused together with the one side of the case and connected to electrode leads (positive electrode lead and negative electrode lead) that extend or are exposed to the outside of the case.
[0245] For example, pouch-shaped cases, square cases, cylindrical cases, coin-shaped cases, etc. can be used.
[0246] Hereinafter, embodiments of the present disclosure will be further described with reference to specific experimental examples. The embodiments and comparative examples included in the experimental examples are merely illustrative of the present disclosure and do not limit the scope of the appended claims. It will be apparent to those skilled in the art that various changes and modifications to the embodiments are possible within the scope and technical idea of the present disclosure, and it is natural that such changes and modifications fall within the scope of the appended claims.
[0247] Manufacturing Example 1: Manufacturing of a monomer represented by Chemical Formula 1-1
[0248] [Reaction Formula 1]
[0249]
[0250] A 1 L round-bottom flask was charged with 100 mL of tetrahydrofuran (THF), perfluoro-3,6-dioxaoctan-1,8-diol (10 g, 34.0 mmol), and triethylamine (7.91 g, 78.2 mmol), and the mixture was cooled to 0 °C through a reactor. After cooling, acryloyl chloride (6.31 g, 69.7 mmol) was added over 1 hour, and the mixture was stirred at room temperature (25 °C) for 18 hours. After completion of the reaction, the triethylamine hydrochloride (TEA-HCl) salt was removed through a filtration device. Tetrahydrofuran (THF) was removed through reduced pressure distillation to replace the solvent. 100 mL of dichloromethane was added. After changing the solvent, the mixture was washed once each with 0.1 N HCl aqueous solution, NaHCO3 aqueous solution, and ultra-pure water (UPW), and then dried under reduced pressure to remove dichloromethane. After removal, 9.6 g of the monomer represented by Chemical Formula 1-1 was obtained (yield: 70.2%) through chromatography using hexane / ethyl acetate as the mobile phase.
[0251] The results of analyzing the monomer obtained in the above manufacturing example 1 using NMR (Nuclear Magnetic Resonance) are as follows.
[0252] 1 H-NMR (500 MHz, CDCl3): 6.52–6.56 (d, 2H), 6.18–6.23 (m, 2H), 5.98–6.00 (d, 2H), 4.55–4.59 (t, 4H)
[0253] Manufacturing Example 2: Manufacturing of a monomer represented by Chemical Formula 2-3
[0254] [Reaction Formula 2]
[0255]
[0256] In the above Preparation Example 1, tetrafluoro-1,4-butanediol (10 g, 61.70 mmol) and triethylamine (7.49 g, 74.04 mmol) were added instead of perfluoro-3,6-dioxaoctan-1,8-diol (10 g, 34.0 mmol) and triethylamine (7.91 g, 78.2 mmol), and after cooling, acryloyl chloride (5.08 g, 56.15 mmol) was added instead of acryloyl chloride (6.31 g, 69.7 mmol), to obtain 4.47 g of an intermediate (intermediate yield: 36.9%).
[0257] In a 1 L round-bottom flask, 50 mL of dichloromethane, triethylamine (2.16 g, 21.34 mmol), POCl3 (0.99 g, 6.47 mmol), and the above intermediate were added, cooled to 0 °C through a reactor, and stirred for 24 hours. After stirring, dichloromethane was removed by washing once each with 0.1 N HCl aqueous solution, NaHCO3 aqueous solution, and ultra-pure water (UPW), and then drying under reduced pressure. After removal, 3.12 g of a monomer represented by the chemical formula 2-3 was obtained through chromatography using hexane / ethyl acetate as a mobile phase (final yield: 25.8%).
[0258] The results of analyzing the monomer obtained in the above manufacturing example 2 using NMR (Nuclear Magnetic Resonance) are as follows.
[0259] 1 H-NMR (500 MHz, CDCl3): 6.51 to 6.55 (m, 3H), 6.17 to 6.23 (m, 3H), 5.97 to 6.00 (m, 3H), 4.63 to 4.68 (q, 6H), 4.52 to 4.59 (m, 6H)
[0260]
[0261] Example 1
[0262] (1) Preparation of mixture
[0263] A mixture was prepared by mixing a monomer for electrolyte, which is a mixture of a monomer represented by the following chemical formula 1-1 and a monomer represented by the following chemical formula 2-3, in a weight ratio of 1:1, with a 1.0 M LiPF6 solution (a mixed solvent of EC / EMC / FLE03 (an ether electrolyte containing fluorine) in a volume ratio of 25:25:50).
[0264] The content of the monomer for the electrolyte relative to the total weight of the electrolyte for the secondary battery was 7.5 wt%.
[0265] [Chemical Formula 1-1]
[0266]
[0267] [Chemical Formula 2-3]
[0268]
[0269] (2) Manufacturing of lithium secondary batteries
[0270] LiNi as a cathode active material 0.6 Co 0.2 Mn 0.2O2, polyvinylidene fluoride (PVDF) as a binder, and carbon black as a conductive material were mixed in a weight ratio of 90:5:5 to prepare a cathode slurry. The cathode slurry was uniformly applied to an aluminum foil, dried and rolled, and then notched into a circular shape with a diameter of φ14 to prepare a cathode.
[0271] A negative electrode slurry was prepared by mixing natural graphite as a negative active material, SBR / CMC as a binder, and carbon black as a conductive material in a weight ratio of 96:3:1. The negative electrode slurry was uniformly applied onto a Cu foil, dried and rolled, and then notched into a circular shape with a diameter of φ16 to prepare a negative electrode.
[0272] Polyethylene (PE) was prepared as a separator. The positive and negative electrodes were positioned facing each other with the separator in between, and then compressed to form an electrode assembly. The electrode assembly was placed within a coin cell outer case measuring 20 mm in diameter and 1.6 mm in height, and the mixture was injected and impregnated for 12 hours. Thereafter, the electrode assembly was heat-cured at 70°C for 1 hour to manufacture a coin cell secondary battery.
[0273] Examples 2 to 10
[0274] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the type and content of the electrolyte monomer, the type and content of the ether solvent containing fluorine, and the content of the electrolyte monomer relative to the total weight of the electrolyte were changed as shown in Table 1 below when manufacturing the electrolyte for a secondary battery.
[0275] Comparative Example 1
[0276] LiNi as a cathode active material 0.6 Co 0.2 Mn 0.2O2, polyvinylidene fluoride (PVDF) as a binder, carbon black as a conductive material, and LLZTO as a solid electrolyte were mixed in a weight ratio of 80:1.5:1.5:17 to prepare a cathode slurry. The cathode slurry was uniformly applied to a 12 ㎛ thick aluminum foil, dried and rolled, and then notched into a circular shape with a diameter of φ14 to prepare a cathode.
[0277] A negative electrode slurry was prepared by mixing natural graphite as a negative electrode active material, SBR / CMC as a binder, and carbon black as a conductive material in a weight ratio of 96:3:1. The negative electrode slurry was uniformly applied onto a 10 ㎛ thick Cu foil, dried and rolled, and then notched into a circular shape with a diameter of φ16 to prepare a negative electrode.
[0278] A separator was prepared by cutting polyethylene (PE) into 20 ㎛ thick pieces and then notching them into a circular shape with a diameter of φ19. The anode and cathode were positioned facing each other with the separator in between, and the tab portions of the anode and cathode were welded, respectively.
[0279] A combination of welded anode / separator / cathode was placed in a coin cell outer case having a diameter of 20 mm and a height of 1.6 mm, an electrolyte was injected, and the resulting material was impregnated for 12 hours to manufacture a coin cell secondary battery.
[0280] The electrolyte was prepared by dissolving 1.0 M LiPF6 in a mixed solvent of EC / EMC / DEC (25 / 45 / 30; volume ratio), to which 5 wt% of FEC (Florinated Ethylene Carbonate), 0.5 wt% of Propane Sulfone, and 0.5 wt% of ESA (ethylene sulfate) were added.
[0281] Comparative Examples 2 to 9
[0282] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the type of electrolyte monomer, the content of electrolyte monomer, and the content of electrolyte monomer relative to the total weight of the electrolyte were changed as shown in Table 1 below when manufacturing an electrolyte for a secondary battery.
[0283] Type and content of monomer for electrolyte (weight % of total monomer weight) Type and content of ether electrolyte containing fluorine (volume % of total volume of mixed solvent) Content of monomer for electrolyte (weight % of total monomer weight) A1A2A3FLE01FLE02FLE03FLE04Example 15050---50-7.5Example 23070---50-7.5Example 37030---50-7.5Example 45050-39---7.5Example 55050---50--7.5Example 65050----317.5Example 75050---20-7.5Example 85050---60-7.5Example 95050---50-3Example 105050---50-15Comparative Example 1--------Comparative Example 2--100--50-5Comparative Example 3--100--50-7.5Comparative Example 4-5050--50-5Comparative Example 5-5050--50-7.5Comparative Example 6-100---50-5Comparative Example 7-100---50-7.5Comparative Example 850-50--50-5Comparative Example 950-50--50-7.5
[0284] The specific ingredients listed in Table 1 are as follows.
[0285] A1: Monomer represented by the above chemical formula 1-1
[0286] A2: Monomer represented by the above chemical formula 2-3
[0287] A3: A compound represented by the following chemical formula 5
[0288] [Chemical Formula 5]
[0289]
[0290] FLE01: 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether
[0291] FLE02: 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether
[0292] FLE03: 2,2,3,3-tetrafluoro-1,4-dimethoxybutane (FDMB)
[0293] FLE04: 1,1,2,2,3,3,4,4-octafluoro-5-methoxy pentane
[0294]
[0295] Experimental Example 1: Electrolyte Evaluation
[0296] (1) Self-digestion assessment
[0297] 1) Examples 1 to 10 and Comparative Examples 2 to 9
[0298] Glass fiber was cut into 16 pi and dried at 120°C to produce dry glass fiber, and the mass (g) of the dry glass fiber was measured.
[0299] After sequentially placing the gasket and the above-mentioned dry glass fiber in the bottom of the coin cell, 0.5 ml of the mixture prepared according to the above-described examples and comparative examples (Comparative Examples 2 to 9) was injected, and then the spacer and cap were sequentially covered to prepare a coin cell.
[0300] Afterwards, the dry glass fiber was injected to impregnate the mixture, and then cured at 70°C for 1 hour. The coin cell was disassembled to prepare a sample (a sample in which the dry glass fiber impregnated with the mixture was cured), and the mass (g) of the sample was measured.
[0301] After igniting the above sample, the time until the fire went out (extinguishing time) was measured.
[0302] The self-extinguishing time was calculated according to Equation 1 below.
[0303] [Formula 1]
[0304]
[0305] 2) Comparative Example 1
[0306] Glass fiber was cut into 16 pi and dried at 120°C to produce dry glass fiber.
[0307] After 3 ml of the electrolyte according to Comparative Example 1 described above was poured into a sealed container, the mass (g) of the electrolyte was measured.
[0308] Afterwards, the dry glass fiber was placed inside a sealed container and impregnated with the electrolyte to prepare a sample, and then the sample was taken out and the mass (g) of the remaining electrolyte that was not impregnated was measured.
[0309] After igniting the above sample, the time until the fire went out (extinguishing time) was measured.
[0310] The self-extinguishing time was calculated according to Equation 2 below.
[0311] [Formula 2]
[0312]
[0313] The results of calculating self-digestion time are shown in Table 2 below.
[0314] Separator Self-extinguishing time (s / g) Example 148.27 Example 250.23 Example 351.40 Example 450.30 Example 549.35 Example 650.66 Example 750.81 Example 849.11 Example 952.51 Example 1040.45 Comparative Example 1112.02 Comparative Example 265.03 Comparative Example 365.39 Comparative Example 456.33 Comparative Example 558.97 Comparative Example 682.34 Comparative Example 776.25 Comparative Example 858.14 Comparative Example 951.04
[0315] Referring to Table 2, in examples in which the monomers represented by Chemical Formula 1-1 and Chemical Formula 2-1 were used together as electrolyte monomers, the self-extinguishing time was 51 s / g or less.
[0316] In Comparative Example 1, which used only a separator without using an electrolyte monomer, the self-extinguishing time exceeded 100 s / g.
[0317] In Comparative Examples 2 to 9, in which the monomers represented by Chemical Formula 1-1 and Chemical Formula 2-1 were not used together as electrolyte monomers or in which other compounds were used as electrolyte monomers, the self-extinguishing time was 51 s / g or more.
[0318] Experimental Example 2: Lithium Secondary Battery Evaluation
[0319] (1) Life characteristics evaluation
[0320] The discharge capacity of the lithium secondary batteries according to the above-described examples and comparative examples was measured after 50 cycles of 0.5 C-rate CC discharge (2.7 V cut-off) at 25°C. The discharge capacity was calculated as a ratio (%) to the initial discharge capacity to evaluate the life characteristics.
[0321] The evaluation results are shown in Table 3 below.
[0322] (2) DSC evaluation
[0323] The heating start temperature and heating amount of lithium secondary batteries manufactured according to the above-described examples and comparative examples were measured using differential scanning calorimetry (DSC).
[0324] The measured fever onset temperature and calorific value are shown in Table 3 below.
[0325] Classification Life Characteristics (%) Heating Start Temperature (℃) Calorific Value (J / g) Example 193.9203.4155.26 Example 291.5202.3776.48 Example 391.3202.8377.79 Example 496.5201.7671.69 Example 595.2202.7024.21 Example 695.9202.6566.17 Example 797.0202.8857.32 Example 896.8203.0156.08 Example 998.0201.0958.35 Example 1094.0204.4224.79 Comparative Example 198.1195.12108.28Comparative Example 292.3195.74107.84Comparative Example 391.1198.2992.64Comparative Example 492.1196.03105.99Comparative Example 591.0198.5787.51Comparative Example 691.4196.9292.64Comparative Example 790.2200.9679.39Comparative Example 891.6196.7392.91Comparative Example 990.7199.8184.29
[0326] FIG. 4 is a graph showing DSC evaluation of lithium secondary batteries manufactured according to exemplary embodiments and comparative examples.
[0327] Referring to Table 3 and FIG. 4, in examples using a lithium secondary battery including an electrolyte layer using a monomer represented by Chemical Formula 1-1 and a monomer represented by Chemical Formula 2-1 together as monomers, the life characteristics were 91% or more, the heat generation start temperature exceeded 201°C, and the heat generation amount was less than 78 J / g.
[0328] In Comparative Example 1, which used a separator without using an electrolyte layer, the temperature at which heat generation started decreased and the amount of heat generation increased.
[0329] In Comparative Examples 2 to 9, where the monomer represented by Chemical Formula 1-1 and the monomer represented by Chemical Formula 2-1 were not used together as monomers, the life characteristics were deteriorated, the temperature at which heat generation started increased, and the amount of heat generation increased.
Claims
1. A monomer for an electrolyte, comprising a first monomer represented by chemical formula 1 and a second monomer represented by chemical formula 2: [Chemical Formula 1] (In Chemical Formula 1, R1 is a substituted or unsubstituted alkylene group having C2 to C12, or a substituted or unsubstituted oxyalkylene group having C2 to C10, and j is an integer from 1 to 5) [Chemical Formula 2] (In Chemical Formula 2, R2, R3 and R4 are each independently a substituted or unsubstituted alkylene group having a group of C2 to C10, or a substituted or unsubstituted oxyalkylene group having a group of C2 to C10, and l, m and n are each independently an integer of 0 to 5.) 2. A monomer for electrolyte according to claim 1, wherein the ratio of the content of the second monomer to the content of the first monomer is 0.5 to 2 by weight.
3. In claim 1, R1 in chemical formula 1 is a C2 to C10 fluorine-substituted alkylene group, or a C2 to C10 fluorine-substituted oxyalkylene group, A monomer for electrolyte, wherein in chemical formula 2, l, m and n are each independently 0 to 3.
4. In claim 3, in chemical formula 2, R2, R3 and R4 are the same as each other, Monomer for electrolyte, where l, m and n are equal integers.
5. In claim 1, the first monomer is an electrolyte monomer comprising at least one of a monomer represented by chemical formula 1-1 and a monomer represented by chemical formula 1-2: [Chemical Formula 1-1] [Chemical Formula 1-2] .
6. In claim 1, the second monomer is an electrolyte monomer comprising at least one of a monomer represented by Chemical Formula 2-1 to a monomer represented by Chemical Formula 2-3: [Chemical Formula 2-1] [Chemical Formula 2-2] [Chemical Formula 2-3] .
7. A flame retardant compound comprising a polymer derived from an electrolyte monomer according to claim 1; and An electrolyte for a secondary battery, comprising a lithium salt.
8. In claim 7, further comprising a composite electrolyte comprising an organic polymer and an inorganic electrolyte, The above composite electrolyte is an electrolyte for a secondary battery having a film form.
9. An electrolyte for a secondary battery according to claim 8, wherein the inorganic electrolyte comprises an oxide-based solid electrolyte.
10. In claim 7, the content of the flame retardant compound is 3 wt% to 20 wt% of the total weight of the electrolyte for a secondary battery.
11. Bipolar; a cathode opposite to the anode; and A lithium secondary battery comprising an electrolyte layer disposed between the positive electrode and the negative electrode and including an electrolyte for a secondary battery according to claim 7.
12. A step of preparing a mixture comprising an electrolyte monomer and an electrolyte solution according to claim 1; and A method for manufacturing an electrolyte for a secondary battery, comprising a step of curing the above mixture.
13. A method for manufacturing an electrolyte for a secondary battery according to claim 12, wherein the mixture further comprises an organic polymer and an inorganic electrolyte.
14. A method for producing an electrolyte for a secondary battery, wherein the content of the monomer for the electrolyte is 3 wt% to 20 wt% of the total weight of the mixture according to claim 12.
15. A method for manufacturing an electrolyte for a secondary battery, wherein the electrolyte comprises an ether solvent containing fluorine (F) in claim 12.
16. A method for manufacturing an electrolyte for a secondary battery, wherein the content of the ether-based electrolyte containing fluorine (F) in claim 15 is 10% by volume to 60% by volume of the total volume of the electrolyte.
17. In claim 12, the mixture further comprises a thermal initiator, A method for manufacturing an electrolyte for a secondary battery, wherein the step of curing the mixture includes heat treating the mixture.
18. In claim 12, the mixture further comprises a photoinitiator, A method for manufacturing an electrolyte for a secondary battery, wherein the step of curing the mixture includes irradiating the mixture with light.
Citation Information
Patent Citations
Phosphate cross-linking agent and preparation method thereof, phosphate-based cross-linked gel polymer electrolyte and preparation method and application thereof
CN111499663A
Perfluorinated phosphate crosslinker for gel polymer electrolyte, gel polymer electrolyte prepared from the same and electrochemical device comprising the electolyte
KR1020110010516A
Gel polymer electrolyte and electrochemical device comprising the same
KR1020150050508A
Organic / inorganic composite electrolyte, electrode-electrolyte assembly and lithium secondary battery containing the same, and manufacturing method of the electrode-electrolyte assembly
KR1020160068464A