Organic coating for sulfide-containing solid electrolyte material, solid electrolyte, and solid battery comprising same

The application of a long-chain thiol organic coating on sulfide-containing solid electrolytes addresses their moisture and air sensitivity, enhancing stability and maintaining ionic conductivity, facilitating the use of these electrolytes in practical battery applications.

WO2024248525A1PCT designated stage expired Publication Date: 2024-12-05LG ENERGY SOLUTION LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/007448
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-05-30
Filing Date
2024-05-31
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Sulfide-containing solid electrolytes are hypersensitive to moisture and air, leading to chemical instability and loss of ionic conductivity, which hinders their practical use in all-solid-state batteries, requiring expensive and cumbersome handling conditions.

Method used

A reversible organic coating made from long-chain thiols, such as 1-undecanethiol, is applied to sulfide-containing solid electrolytes, providing protection against moisture and air without significantly altering ionic conductivity, allowing the electrolytes to maintain stability and functionality under ambient conditions.

Benefits of technology

The organic coating extends the exposure time of sulfide solid electrolytes to ambient air, maintaining ionic conductivity for up to 2 days at 33% relative humidity, significantly improving their chemical and interfacial stability, and enabling the use of sulfide electrolytes in cost-competitive and energy-efficient solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024007448_05122024_PF_FP_ABST
    Figure KR2024007448_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a coated sulfide-containing solid electrolyte material, a solid electrolyte thereof, and a solid battery comprising the solid electrolyte. According to an aspect of the present disclosure, a coating is formed on a surface of a sulfide-containing solid electrolyte material and includes, for example, a compound having a thiol with a long hydrophobic tail, such as 1-undecanethiol. The coating may, for example, provide protection from air and moisture at ambient conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Organic coating for sulfide-containing solid electrolyte material, solid electrolyte and solid battery comprising the same

[0001] Cross-reference to related applications

[0002] This application claims priority to U.S. Provisional Application No. 63 / 505,240, filed May 31, 2023, U.S. Non-Provisional Application No. 18 / 661,381, filed May 10, 2024, and Korean Patent Application No. 10-2024-0070959, filed May 30, 2024, the entire contents of which are expressly incorporated herein by reference in their entirety.

[0003] Technology field

[0004] The present disclosure relates to an organic coating for a sulfide-containing solid electrolyte material, a solid electrolyte thereof, and a solid battery thereof. According to an aspect of the present disclosure, the organic coating is made of a thiol having a hydrophobic chain, which protects the sulfide-containing solid electrolyte material from air and moisture under ambient conditions.

[0005] Electric transportation systems and stationary energy storage systems continue to grow. Consequently, the importance of high-energy-density battery technology with enhanced safety is growing.

[0006] Much effort has been focused on using lithium metal in the cathode. Lithium (Li) metal has a high energy density of 3860 mAh g compared to a standard hydrogen electrode. -1 Because of its high specific capacity and low electrochemical potential of -3.040 V, it is expected to meet high energy density requirements. However, the commercialization of lithium metal anodes with conventional flammable liquid organic electrolytes (OLEs) faces many obstacles, including undesirable reactions between lithium metal and OLEs. Furthermore, flammable OLEs also pose safety concerns.

[0007] To avoid the safety issues of conventional lithium-ion batteries using flammable organic electrolytes, all-solid-state batteries (ASSBs) using non-flammable solid electrolytes are being widely promoted. Solid electrolytes also ensure better interfacial stability, opening the way to using lithium metal as an anode, resulting in batteries with higher energy density. Solid electrolytes (SEs) are stable at high temperatures, have improved safety (e.g., can reduce the risk of fire and explosion), and have good ionic conductivity and excellent ductility. In particular, sulfide-containing SEs have high ionic conductivity at room temperature (e.g., Li 10 GeP2S 12 12mS cm -1 and Li 5.5 PS 4.5 Cl 1.5 9.4mS cm -1 ) has been studied, which even surpasses OLE. In addition, the flexible nature of sulfide-containing SE may enable high ductility, which may be beneficial for the solid-solid interface. Therefore, it is expected that using SE can provide longer battery life.

[0008] However, despite extensive research, certain limitations still need to be overcome. For example, sulfide-containing solid electrolytes are sensitive to moisture, hindering their practical manufacturing. Sulfide-containing solid electrolytes also have extremely low air stability, a significant limitation. Hydrolysis produces toxic H2S gas, along with a significant loss of ionic conductivity.

[0009] Due to their low chemical stability, sulfide-containing solid electrolytes are typically handled in an inert glove box with a very low moisture content (dew point -80°C). However, maintaining this moisture content in practical applications is costly and difficult to commercialize.

[0010] The low chemical stability of most sulfide electrolyte materials is due to the structure, chemical bonding, and non-bridging sulfur units in the glass network. Glasses with a lower concentration of Li modifier units are chemically more stable because they have fewer non-bridging sulfur bonds, which are vulnerable to chemical degradation. Lithium ions form ionic bonds with sulfur, which are generally weaker than other covalent bonds in the glass network, making lithium ions susceptible to leaching by water. To realize sulfide solid electrolytes for all-solid-state batteries, chemical stability must be addressed.

[0011] Researchers have closely investigated this problem by various approaches, such as (1) adding metal oxides (e.g., ZnO, Fe2O3, Bi2O3) to sulfide SEs to suppress H2S production by absorbing H2S, (2) partially substituting S with O to form acid sulfur compounds with improved air stability and a wide electrochemical window, (3) chemical doping or substitution according to the hard / soft acid-base theory, or (4) designing and tuning the nanostructure of the materials to protect them from moisture and air, e.g., through core-shell coatings.

[0012] The aforementioned approaches have improved the chemical stability of sulfide solid electrolytes. However, challenges remain. For example, metals exhibit the following reaction M x O y + H2S → M x S y + Because it has a large negative Gibbs free energy change (ΔG) for H2O, it absorbs H2S by undergoing an acid-base reaction with H2S. While effective for moisture protection, its ionic conductivity decreases when a "foreign" non-ionic conducting material is introduced. For example, ZnO can effectively absorb H2S, but it also reduces its conductivity.

[0013] Hard acid (small, non-polar) P 5+Soft acid (large, polarizable) Cu +15 , As 5+16 , Sn 4+17 and Sb 5+18 When replaced with , the ion is a soft base S 2- Binds tightly to hard base O 2- Since it resists the attack of lithium, it can mitigate fast-acting hydrolysis. Although the chemical stability of the electrolyte itself can be improved, the interfacial stability with lithium metal is often sacrificed, which often reduces the overall efficiency of the all-solid-state battery.

[0014] Building novel nanostructures and fine-tuning the morphology of sulfide electrolytes can be accomplished effectively at the laboratory scale. However, scaling up to manufacturing levels is impractical and often results in reduced conductivity.

[0015] Therefore, despite efforts to improve the chemical stability of sulfide-containing electrolytes, many shortcomings remain, such as poor conductivity and interfacial stability. Therefore, the need for improved all-solid-state batteries remains.

[0016] The present disclosure relates to a sulfide-containing solid electrolyte material, the solid electrolyte, and a solid battery thereof that provide enhanced stability. The solid electrolyte (SSE) also provides higher interfacial stability and better mechanical properties, thereby suppressing Li dendrite penetration, thereby paving the way for the implementation of lithium metal anodes that enable high cell energy densities.

[0017] The present disclosure relates to an organic coating for a sulfide-containing solid electrolyte suitable for use in a solid-state battery, and to the use of the coated sulfide-containing solid electrolyte and sulfide-containing solid electrolyte composition. According to the present disclosure, the stability of the sulfide-containing solid electrolyte composition, for example, against moisture and / or air, is improved, and processing under ambient conditions is facilitated. In addition, the present disclosure relates to providing a solid-state battery having excellent electrical and chemical properties, including safety, thermal stability, energy density, cycle life characteristics, and Coulombic efficiency. It will be readily understood that these and other objects and advantages of the present disclosure can be realized by the means or methods set forth in the appended claims, and combinations thereof.

[0018] Sulfide solid electrolytes are promising candidates for realizing all-solid-state batteries (ASSBs) due to their excellent ionic conductivity and excellent ductility. However, they are highly sensitive to moisture and require processing environments that are not compatible with today's lithium-ion battery manufacturing infrastructure. For example, in lithium argyrodite, bridging sulfur units (PSPs) within the network can react with water to produce OH and SH species, which further react to produce both OH and toxic H2S gas. During hydrolysis, these species can attach PS bonds, thereby forming PO bonds and PS4, which are important for high Li ion conductivity. 3- By collapsing the unit, H2S is released.

[0019] Moisture sensitivity can lead to catastrophic losses in ionic conductivity, requiring academic research to handle sulfide SSEs in an inert glovebox atmosphere with exceptionally low moisture levels (dew point of -80°C). In industrial settings, dry rooms with dew points below -60°C are required, which is significantly more cumbersome and expensive than the current lithium-ion battery manufacturing infrastructure, which has a dew point of ~-40°C.

[0020] One aspect described herein relates to a reversible surface modification strategy that enables the processing of sulfide SSEs (e.g., Li6PS5Cl) under humid ambient air. This protection mechanism can be effective for extended periods of time (e.g., hours to days, or longer) without significantly altering the ionic conductivity and redox stability of the material. Long-chain alkyl thiols, such as 1-undecanethiol, have been shown to be chemically compatible with the electrolyte and have minimal effect on its ionic conductivity. Importantly, the thiol modification extends the amount of time that the sulfide SSEs can be exposed to air at 33% relative humidity (33% RH) while limiting the degradation of their structure, while maintaining a 1 mS cm for up to 2 days. -1 The protection time is improved by more than 100 times compared to competing approaches while maintaining the conductivity above. Experimental and calculation results show that the thiol group is fixed on the SSE surface, while the hydrophobic hydrocarbon tail provides protection by repelling water. The modified Li6PS5Cl SSE has Li 0.5 In / LiNi 0.8 Co 0.1 Mn 0.1 When implemented in O2ASSB, it retains its functionality even after exposure to ambient humidity. This proposed protection strategy, based on surface molecular interactions, represents a significant step forward toward cost-competitive and energy-efficient sulfide SSE fabrication for ASSB applications.

[0021] One aspect of the present disclosure relates to a sulfide-containing solid electrolyte having an organic coating, and a solid-state battery comprising the electrolyte. In certain aspects, the organic coating serves as a protective agent for the sulfide-containing solid electrolyte under ambient conditions. For example, the organic coating may provide protection from moisture and / or air.

[0022] In one aspect of the present disclosure, an organic coating is formed from long-chain thiols and applied to a sulfide-containing solid electrolyte material, such as Li6PS5Cl (LPSCl). The coating has a minimal effect on the ionic conductivity of the electrolyte. Some mechanistic studies have shown that the thiol groups interact with sulfur on the surface (sulfur in sulfide-containing solid electrolytes), while the hydrocarbon tails provide a protective function. For example, the hydrocarbon tails can be oriented outward, forming a "lipid barrier" that repels water and other polar substances. As illustrated in Figure 1, the thiol-coated electrolyte (e.g., where the thiol groups interact with the LPSCl surface) provides hydrophobic tail ends, which block water and protect the electrolyte.

[0023] In one aspect, the coating extends the exposure time to ambient air with humidity up to 20% for up to three days without significant structural or conductivity degradation. This durability represents a two-fold improvement over competing approaches. The coated LPSCl was also shown to maintain its functionality when implemented in a solid-state battery with an oxide anode. Therefore, this protective mechanism based on surface molecular interactions represents a significant advance in the practical application and commercialization of sulfide electrolytes in all-solid-state batteries.

[0024] One aspect relates to a solid electrolyte composition comprising a sulfide-containing solid electrolyte material having a surface, and an organic coating formed on the surface of the sulfide-containing solid electrolyte material. The organic coating is formed on the surface of the sulfide-containing solid electrolyte material. In some aspects, the coating is formed of at least one of the compounds represented by the following formulae 1 and 2:

[0025] [Chemical Formula 1]

[0026] RA

[0027] [Chemical Formula 2]

[0028] R-A'-R

[0029] In the above formula, A is an SH group, an isocyanate, an amine, or a leaving group (including, but not limited to, an organosilicon compound such as triethoxysilyl or trimethoxysilyl); A' is an -S- moiety or a -SS- moiety; and each R is independently a substituted or unsubstituted C3-C20 alkyl group. And, using the above solid electrolyte composition, a solid electrolyte for a solid battery can be manufactured.

[0030] In one aspect, the organic coating is formed by adsorption onto the surface of the sulfide-containing solid electrolyte material. Thus, in some aspects, the compound of Formula 1 or Formula 2 is attached to the surface of the sulfide-containing solid electrolyte material by non-covalent attachment (including but not limited to chemisorption, van der Waals interactions, or ionic interactions).

[0031] Alternatively, the coating may be formed by reacting a compound of Formula 1 and / or Formula 2 with a sulfide-containing solid electrolyte material, for example, the reaction product or residue of the compound of Formula 1 and / or Formula 2 forms the coating. Thus, in some aspects of the present disclosure, the compound of Formula 1 or Formula 2 reacts with the sulfide-containing solid electrolyte material to form a covalent bond. In some aspects, the covalent bond formed is a sulfide bond or a disulfide bond.

[0032] In some aspects, in the compound of formula 1, A is a thiol (-SH group), an isocyanate, an amine, or a suitable leaving group. In some aspects of the present disclosure, the leaving group may be triethoxysilyl or trimethoxysilyl.

[0033] In one aspect, at least one of R in the compound of formula 1 or formula 2 is a C6-C16 alkyl group. In one aspect, at least one of R in the compound of formula 1 or formula 2 is a C8-C12 alkyl group.

[0034] In one aspect, the compound of formula 1 or formula 2 has a total number of carbon atoms of 6 to 16. In one aspect, the compound of formula 1 or formula 2 has a total number of carbon atoms of 8 to 12.

[0035] In one aspect, at least one of R in the compound of formula 1 or formula 2 is a substituted C3-C20 alkyl group, wherein the substituted C3-C20 alkyl group has one or more substituents selected from fluorine, chlorine, bromine, ester, and ketone moieties.

[0036] In one aspect, each R group is selected to provide a compound of formula 1 or formula 2 that is an amphiphilic molecule (e.g., the R group can repel water and polar organic solvents) and chemically adsorb to the surface of the sulfide solid electrolyte. See, e.g., FIGS. 1A and 1B. The head group can enable both stabilization of the sulfide SSE surface and attachment to the sulfide SSE surface. For example, in the case of the A-thiol head group, it is not expected to replace the S atom of the existing PS bond in the SSE, but rather is expected to attach to the surface S atom via SS bond formation. A sufficiently long chain alkyl tail (e.g., C 11 H 23 -) can ensure high hydrophobicity.

[0037] In one aspect, the compound of formula 1 is 1-undecanethiol. As described below, 1-undecanethiol is chemically compatible with electrolytes and has a minimal effect on ionic conductivity. For example, thiol modification extends the time that sulfide SSEs can be exposed to air at 33% relative humidity (33% RH) while limiting the degradation of their structure, while maintaining a 1 mS cm for up to 2 days. -1 The protection time was improved by more than 100 times compared to competing approaches while maintaining the conductivity above. Experimental and calculation results showed that the thiol group is fixed on the SSE surface, while the hydrophobic hydrocarbon tail provides protection by repelling water. The modified Li6PS5Cl SSE has Li 0.5 In / LiNi 0.8 Co 0.1 Mn 0.1 When implemented in O2ASSB, it retains its functionality even after exposure to ambient humidity. This proposed protection strategy, based on surface molecular interactions, represents a significant step forward toward cost-competitive and energy-efficient sulfide SSE fabrication for ASSB applications.

[0038] In one aspect, the sulfide-containing solid electrolyte material is selected from the group consisting of inorganic electrolyte materials and organic electrolyte materials. According to an aspect of the present disclosure, the sulfide-containing solid electrolyte material is an inorganic electrolyte.

[0039] In some aspects of the present invention, the sulfide-containing solid electrolyte is Li3P7S 11 , Li3P7S 11 , Li 10 GeP2S 12 , at least one selected from the group consisting of Na3PS4 and Li6PS5Cl. Among the SSE materials, Li 9.6 P3S 12 , Li 10 GeP2S 12 , and Li 9.54 Si 1.74 P1.44 S 11.7 Cl 0.3 Sulfides such as these have a superionic conductivity (~10 -2 S cm -1 Sulfide SSEs are particularly attractive due to their high modulus and deformability. In addition, sulfide SSEs exhibit lower Young's modulus values ​​than oxide glasses and ceramics, which is beneficial for creating favorable interfacial contact with electrode materials through mechanical compression.

[0040] In some aspects of the present disclosure, the sulfide-containing solid electrolyte comprises at least one selected from the group consisting of LPS-based glasses and glass ceramics of the formula xLi2S·yP2S5 (where x+y=1).

[0041] In some aspects of the present invention, the sulfide-containing solid electrolyte comprises an argyrodite-based solid electrolyte of the formula Li6PS5X (wherein X is Cl, Br, or I).

[0042] In some aspects of the present invention, the sulfide-containing solid electrolyte comprises an argyrodite-based solid electrolyte of the formula Li6?yPS5?yCl1+y (wherein y<1).

[0043] In another aspect, the present disclosure relates to a method for preparing a solid electrolyte composition, the method comprising providing a sulfide-containing solid electrolyte material and combining at least one of the compounds of formula 1 or formula 2 described herein to form a coated sulfide-containing solid electrolyte material.

[0044] In another aspect, the present disclosure relates to a method for preparing a solid electrolyte, the method comprising providing a sulfide-containing solid electrolyte and combining the solid electrolyte with at least one of the compounds of formula 1 and formula 2 described herein to form a coated sulfide-containing solid electrolyte material.

[0045] Another aspect relates to a solid electrolyte comprising the above solid electrolyte composition.

[0046] Another aspect relates to an all-solid-state battery comprising a cathode; an anode; and a solid electrolyte interposed between the cathode and the anode, as described herein.

[0047] The present specification discloses a sulfide-containing solid electrolyte composition that protects the sulfide-containing electrolyte from air and / or moisture using an organic coating, and a solid electrolyte and a solid battery thereof.

[0048] For example, an organic coating of a long-chain alkyl thiol (e.g., 1-undecanethiol) chemically adsorbed onto the surface of a sulfide electrolyte protects the material from moisture and air. In Figure 1, 1-undecanethiol is adsorbed onto the surface of Li6PS5Cl, and may be attached via, for example, weak van der Waals forces. The hydrophilic functional thiol groups interact with Li6PS5Cl to form weak bonds, while the hydrophobic carbon tails act as a water-repelling shield. The non-invasive 1-undecanethiol coating was demonstrated to protect Li6PS5Cl from moisture and air without compromising its conductivity. The integrity of the crystal and bonding structures was confirmed by X-ray powder diffraction (XRD), Raman spectroscopy, and X-ray photoelectron spectroscopy (XPS), as described in more detail herein.

[0049] The coated solid electrolyte material was found to maintain its performance in both symmetric and full lithium cells after exposure to air or moisture. The inventors discovered that a coating formed, for example, with a long-chain alkyl thiol, protects the sulfide solid electrolyte from air or moisture, opening the way to large-scale production even under ambient conditions.

[0050] According to the present disclosure, sulfide-containing solid electrolyte materials (e.g., LPSCs, etc.) can now be used openly for long periods of time under ambient conditions, thereby greatly simplifying the manufacturing process and facilitating commercialization.

[0051] For example, in one sun, LPSCs coated with 1-undecanethiol were evaluated after exposure to ambient air for up to 7 days. The evolution of the material after air exposure was observed via XRD, Raman spectroscopy, and XPS. It was found that 1-undecanethiol could protect the LPSCs from ambient air for up to 3 days with minimal conductivity loss. The XRD results (Figs. 2a and 3a) showed that there was no sign of new phase formation and the integrity of the original structure of the LPSCs remained unchanged after up to 3 days of air exposure, indicating that 1-undecanethiol successfully functioned as a protectant. At the 5th day of air exposure, a small secondary phase peak appeared. The main LPSC peak remained until the 7th day, but the impurity peaks were more distinct.

[0052] The accompanying drawings illustrate aspects of the present disclosure and, together with the detailed description, serve to further understand the technical concepts of the present disclosure, and the present disclosure should not be construed as being limited to the drawings. In the drawings, the shape, size, scale, or proportion of elements may be exaggerated for clarity of explanation.

[0053] Figure 1a is a schematic diagram of an organic compound (1-undecanethiol) coated on an LPSC to form a thiol-coated LPSC for moisture protection. Figure 1b is a schematic diagram showing a strategy for protecting the LPSC in humid ambient air. The LPSC is hydrolyzed to increase the ionic conductivity by 10 4 While the conductivity loss is reduced by a factor of 10, 1-undecanethiol (SH) adsorbed on the LPSC surface protects the material, resulting in less than a 10-fold loss in conductivity at 33% relative humidity (RH). SH forms a hydrophobic shield around the LPSC particles.

[0054] Figure 2a shows the PXRD purification of 1-undecanethiol (or “11Thiol”) mixed with LPSC after vacuum drying.

[0055] Figure 2b shows the electrochemical impedance spectroscopy results for LPSC and LPSC / 11Thiol mixtures.

[0056] Figure 3a shows the PXRD results of 1-undecanethiol coated LPSC according to the mentioned air exposure time, and studies the structural evolution of 1-undecanethiol mixed with LPSC from day 1 to day 7.

[0057] Figure 3b shows Raman spectra of pristine LPSC and LPSC / 1-undecanethiool mixture after 1 to 7 days of air exposure.

[0058] Figure 3c shows the electrochemical impedance spectroscopy results of LPSC and LPSC / 1-undecanthiol mixture on days 1 to 7 of air exposure.

[0059] Figures 3d and 3e show XPS results of LPSC and LPSC / 1-undecanthiol mixtures on days 1 to 7 of air exposure.

[0060] Figure 3f shows the ionic conductivity results of untreated LPSC and LPSC / 1-undecanthiol mixture on the 1st to 7th day of air exposure.

[0061] Figure 3g shows the electrochemical impedance spectroscopy results comparing untreated LPSCs and 1-undecanthiol coated LPSCs after 1 day of air exposure.

[0062] Figure 4a shows the ion exchange membranes collected from untreated LPSC samples, and pure LPSC samples and 1-undecanethiool (thiol) coated LPSC samples exposed to ambient air for various amounts of time. 31P spin echo ss-NMR spectra are shown. 'Wet' and 'dry' samples represent (wet) LPSC samples exposed to 1-undecanethiol solution, and (dry) LPSC samples subsequently dried.

[0063] Figure 4b shows the results collected from pure 1-undecanethiol solution, wet coated LPSC, and then dried LPSC samples. 1 H spin echo NMR spectrum is shown. 1 1-undecanethiol spectrum 1 H resonances and their corresponding intramolecular positions are labeled (af) in the upper left corner. The resonances of pure 1-undecanethiol shifted in the coated sample are indicated by the original positions with red dashed lines, and the final positions with black dashed lines and asterisks. In both panels, the spectra are scaled to have the same maximum intensity. All spectra were acquired at 18.8 T under 60 kHz magic angle spinning (MAS).

[0064] Figure 5 shows the bulk and grain boundary conductivity results of LPSC and LPSC / 1-undecanthiol mixtures on the first to seventh days of air exposure.

[0065] Figure 6a shows the 0.1 mA / cm for the untreated LPSC cycle. 2 It represents a symmetrical cycle test for 15 hours.

[0066] Figure 6b shows the 0.1 mA / cm for the LPSC / 1-undecanethiol mixture. 2 It represents a symmetrical cycle test for 15 hours.

[0067] Figures 6c to 6f show LiNi assembled using LPSC (Figures 6c and 6e) or 1-undecathiol coated LPSC (Figures 6d and 6f). 0.8 Co 0.1 Mn 0.1O2(NCM811)|LPSCl|LiIn all-solid-state full cells are presented. Due to the organic coating protection, both cells exhibit similar second cycle charge capacity and second cycle coulombic efficiency (CE) (Figures 6c and 6d). The LPSCl fuel cell maintains similar capacity and cycle retention even after 15 cycles, with discharge capacities of 132.9 mAh / g for the LPSC (Figure 6e) and 133.9 mAh / g for the LPSC coated with 1-undecanethiol (Figure 6f). These observations demonstrate the remarkable and powerful protective effect of 1-undecanethiol on LPSCs when exposed to air.

[0068] Figure 7 shows a comparison of critical current density and lifetime performance between untreated LPSC and LPSC / 1-undecanthiol mixture.

[0069] Figure 8 shows the results collected from pure 1-undecanethiol solution, wet coated LPSC and then dried LPSC samples. 1 H NMR spectrum is shown.

[0070] Figure 9a is a Raman spectra of the untreated pure SH solution and the pure SH solution after 1 day, 2 days, and 3 days of exposure to air at 33% RH (labeled SH 1D air, SH 2D air, and SH 3D air, respectively). Figure 9b is a Raman spectra of the untreated pure SH solution and the pure SH solution after 1 day, 2 days, and 3 days of exposure to air at 33% RH (labeled SH 1D air, SH 2D air, and SH 3D air, respectively). 1 H liquid NMR spectrum.

[0071] Figures 10a-g show the chemical compatibility between SH surface modifier and LPSC. Figure 10a shows the calculated adsorption energies of undecane (CH) and SH on the LPSC surface. Figure 10b shows the calculated adsorption energies of undecane (CH) and SH on the LPSC surface at 18.8 T in pure SH solution and SH@LPSC sample. 1H spin echo NMR spectrum is shown. SH@LPSC spectrum was acquired at magic angle spinning (MAS) speed of 60 kHz. SH@LPSC spectrum 1 H resonances and their intramolecular corresponding positions are labeled (af) in the upper left corner. They are associated with SH molecules in pure SH solution and SH@LPSC samples. 1 The positions of the H resonances are marked by red dashed lines and black dashed lines / asterisks, respectively. Figures 10c and 10d are the S 2p (Figure 10c) and P 2p (Figure 10d) XPS spectra collected from LPSC and SH@LPSC. Figures 10e and 10f are cryo-TEM images of LPSC (Figure 10e) and SH@LPSC (Figure 10f), the latter visualizing the modified layer on the LPSC surface in SH@LPSC. Figure 10g is a Nyquist plot of LPSC and SH@LPSC pellets sandwiched between two titanium rods.

[0072] Figure 11 shows the synthesis process of the surface-modified electrolyte including the following sequence: planetary centrifugal mixing of LPSC and SH using Thinky, vacuum drying at 80°C for 2 hours with or without exposure to air to remove residual absorbent, and structural characterization.

[0073] Figure 12 is a Rietveld refinement of the XRD pattern obtained from SH@LPSC without air exposure.

[0074] Figure 13 shows the collected samples from pure LPSC after vacuum drying at 80°C for 2 hours, SH@LPSC after vacuum drying at 80°C for 2 hours, and SH@LPSC after vacuum drying at 80°C for 2 hours and additional heat treatment at 300°C for 3 hours. 1H spin echo NMR spectra. All spectra were acquired at 18.8 T with a MAS rate of 20 kHz. The spectra were scaled to have the same number of scans and total sample mass. All other measurement conditions were identical and a recycle delay of 5*T1 was used. In the inserted table, in the spectra 1 The weight percentage of SH in the dried SH@LPSC sample, determined from the fit and integration of the H NMR signals, is reported. The signal from the SH surface modifier is collected in the SH@LPSC. 1 H dominates the spectrum, but is very small from the LPSC phase. 1 Since only the H signal is generated, the SH residues represent only a small mass fraction of the sample. This is unique to LPSC. 1 Some of the H signals (see spectra obtained from untreated LPSC) are lost during heat treatment at 300°C. In thiol quantification, from untreated material 1 The contribution from SH is separated by subtracting the H signal from the total signal intensity. When this is done for the sample heated at 300°C, a negative signal intensity is obtained, indicating that some of the protons in the untreated LPSC are released from the sample during heating at 300°C.

[0075] Figure 14 shows the SH residue in the SH@LPSC sample. 1 Representative fittings obtained from H quantification are shown. All spectra were acquired at 18.8 T with a MAS rate of 20 kHz. T2* measurements were performed to fit the attenuation of each component and compensate for signal loss during the 50 μs echo delay.

[0076] Figures 15a-g illustrate the evaluation of LPSC and SH@LPSC exposed to humid ambient air. (Figure 15a) Schematic diagram of a homemade setup for controlled humid air exposure, including a thermogravimetric sensor that tracks the change in relative humidity within a sealed container. (Figure 15b) XRD patterns collected from LPSC and SH@LPSC exposed to humid air for up to 3 days. (Figure 15c) Raman spectra of LPSC and SH@LPSC after 1 and 3 days of exposure to humid air. (Figures 15d-e) Ionic conductivities of LPSC and SH@LPSC as a function of air exposure time and relative humidity. (Figure 15f) Comparison of ionic conductivities as a function of humid air exposure time, highlighting the significantly superior stability of the present SH@LPSC SSE for exposure times up to two orders of magnitude longer. (Figure 15g) Comparison of ionic conductivity loss rates. When normalized by exposure duration, the dramatic improvement provided by SH is also evident.

[0077] Figure 16 shows the moisture uptake of LPSC and SH@LPSC samples exposed to air at 33% RH. Figure 16a quantifies the moisture uptake of LPSC and SH@LPSC samples as a function of time through the decrease in relative humidity inside the container. The moisture uptake in Figure 16b, i.e., the first derivative of the curve in Figure 16a, shows that the lower moisture uptake of SH@LPSC indicates that its moisture stability is better than that of pure LPSC.

[0078] Figure 17 shows the complete XRD patterns collected from LPSC and SH@LPSC samples exposed to air at 33%RH for 5 hours to 3 days.

[0079] Figure 18 shows the ionic conductivity of 200 mg of LPSC and SH@LPSC (200 mg of LPSC and 40 mg of SH) as a function of air exposure time and relative humidity.

[0080] Figures 19a-c show the material degradation analysis upon moisture exposure. Figures 19a-b show XPS, and Figure 19c shows the XPS collected from LPSC and SH@LPSC after 1 or 3 days of air exposure. 31 P spin echo solid-state NMR spectrum is shown. The solid-state NMR spectrum was obtained at 18.8 T at a MAS rate of 60 kHz.

[0081] Figure 20 is collected from LPSC and SH@LPSC samples exposed to air at 33%RH for 0 to 3 days. 6 Li spin echo ssNMR spectrum is shown. The spectrum was obtained at 18.8 T under magic angle spinning at 20 kHz.

[0082] Figure 21 is collected from SH@LPSC and SH@LPSC samples exposed to air at 33%RH for 1 day. 1 H spin echo ssNMR spectrum is shown. The spectrum was obtained at 18.8 T under magic angle spinning at 10 kHz.

[0083] Figure 22 shows the LPSC and CH@LPSC on the 0th to 3rd day of exposure to air at a humidity of 33%RH. 6 Li spin echo ssNMR spectra are shown. All spectra were obtained at 18.8 T under a MAS rate of 20 kHz.

[0084] Figure 23 shows the LPSC and CH@LPSC on the 0th to 3rd day of exposure to air at a humidity of 33%RH. 31 P spin echo ss-NMR spectra are shown. All spectra were obtained at 18.8 T under a MAS rate of 60 kHz.

[0085] Figure 24 shows the Li / Li symmetric cell critical current densities of (a) LPSC, (b) SH@LPSC 1D air, and (c) LPSC 1D air at room temperature.

[0086] Figure 25 shows the electrochemical performance of LPSC and SH@LPSC samples after 1 day of exposure to 33%RH air. (a) NCM811 composite|LPSC|LPSC 1D air|Li 0.5 In cell, (c) NCM811 composite|LPSC|SH@LPSC 1D air|Li 0.5 Voltage profiles of the cell at 60°C and 0.1°C rate. (b) and (d) are the 50-cycle capacity retention rates of the cells shown in (a) and (c), respectively.

[0087] Figure 26 (a) shows the NCM811 complex|LPSC|Li during the first 5 cycles. 0.5 In (a) shows the voltage profile of the cell, and (b) shows the NCM811 composite|LPSC|Li 0.5 Indicates the long-term cycle performance of In.

[0088] Figure 27 shows that all SH residues are completely removed through the 300°C heating process. (a) XRD pattern, (b) Nyquist plot of pellets sandwiched between two titanium rods of LPSC, SH@LPSC vacuum-dried at 80°C for 2 hours, and SH@LPSC vacuum-dried at 80°C for 2 hours and then heated at 300°C for 3 hours, respectively.

[0089] Hereinafter, the present disclosure will be described in detail. It should be understood that the terms and words used in this specification and the appended claims should not be construed as limited to their ordinary or dictionary meanings, but rather should be interpreted based on meanings and concepts consistent with the technical spirit of the present disclosure, based on the principle that the inventor can appropriately define terms for the best explanation. Therefore, it should be understood that the aspects of the present disclosure described in this specification and the elements depicted in the drawings are only aspects of the present disclosure and do not completely represent the technical spirit of the present disclosure, and that other equivalents and modifications may exist at the time of filing this application. Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly known to those skilled in the art. If there are multiple definitions for a term in this specification, the definitions provided herein shall take precedence.

[0090] Unless otherwise stated, all percentages, parts and ratios in this disclosure are by weight.

[0091] Unless otherwise indicated, the numerical parameters set forth in the specification and attached claims below are approximations that may vary depending upon the desired properties sought to be obtained in accordance with aspects of the present disclosure. Whenever a numerical range having a lower and an upper limit is disclosed, any number falling within that range and any subsumed range are specifically disclosed. In particular, any range of values ​​disclosed herein (in the form "from about A to about B," or equivalently "from about a to b," or equivalently "about ab") should be understood to describe all numbers and ranges subsumed within the broader range of values.

[0092] Although compositions and methods are described herein as "comprising" various components or steps, it is also possible for the compositions and methods to "consist essentially of" or "consist of" the various components and steps. The term "comprises" as used herein specifies the presence of the stated elements, but does not exclude the presence or addition of one or more other elements, unless the context clearly dictates otherwise.

[0093] The terms "about" and "substantially" are used herein to mean at or near the numerical value when manufacturing and material tolerances inherent in the circumstances are given, and are used to prevent unscrupulous infringers from unfairly taking advantage of the disclosure when precise or absolute values ​​are mentioned to aid understanding of the disclosure. The terms "about" and "approximately" used with a numerical variable generally mean the value of that variable, and any value of that variable within experimental error (e.g., a 95% confidence interval for the mean) or within ±10% of the specified value or within a wider range. Unless otherwise indicated, all numbers expressing quantities of ingredients, properties such as molecular weights, reaction conditions, and the like used in this specification and any related claims are to be understood as being modified by the term "about."

[0094] As used herein, “A and / or B” specifies “A or B or both.”

[0095] One aspect of the present disclosure relates to a solid-state battery comprising a solid electrolyte material as an electrolyte. Specific examples of the solid-state battery include any type of primary battery, secondary battery, fuel cell, solar cell, or capacitor, such as a supercapacitor. In particular, the secondary battery is specifically a lithium-ion secondary battery.

[0096] In one aspect of the present disclosure, a solid-state battery according to the present disclosure includes a cathode, an anode, and a solid electrolyte interposed between the cathode and the anode. The composition and effects of the present disclosure are described in detail below.

[0097] In the present disclosure, a solid electrolyte composition comprises a sulfide-containing solid electrolyte material having an organic coating. In one aspect, a long-chain thiol may be used as the organic coating. According to an aspect of the present disclosure, the coating contains hydrophobic chains, which form a hydrophobic barrier to protect the sulfide-containing solid electrolyte material from air, water, and / or ambient conditions.

[0098] As described above, sulfide-containing solid electrolytes are highly susceptible to nucleophilic attack from polar organic solvents. Many common solvents used in conventional liquid lithium-ion batteries are unsuitable for use with SSEs. In one aspect, surface molecular engineering enables the processing of sulfide solid electrolytes in humid ambient air.

[0099] For the purposes of the present disclosure, any suitable sulfide-containing electrolyte material may be used. As used herein, the term "sulfide-based electrolyte" means an electrolyte containing ions (e.g., Li + ) and electrically insulate the positive and negative electrodes of the electrochemical cell. Exemplary sulfide-containing electrolytes are described in the literature [Shaojie Chenet al., "Sulfide solid electrolytes for all-solid-state lithium batteries: Structure, conductivity, stability and application," Energy Storage Materials, Volume 14, Pages 58-74 (September 2018), which is expressly incorporated herein by reference in its entirety.

[0100] For example, many sulfide-containing electrolyte materials have (~10 -2 S cm -1 It is particularly attractive due to its high superionic conductivity and deformability. In particular, Li3P7S 11 , Li 10 GeP2S 12 , and Na3PS4 and Li6PS5Cl have been reported to exhibit high ionic conductivities; some even exhibit conductivities close to liquid electrolytes. According to aspects of the present disclosure, sulfide solid electrolyte materials also provide low Young's moduli, which is beneficial for creating favorable interfacial contact with electrode materials by simple cold pressing at room temperature.

[0101] According to an aspect of the present disclosure, a sulfide-containing solid electrolyte contains sulfur (S) and a metal belonging to group I or II of the periodic table, for example, Li. + may have an ionic conductivity of 1x10. Additionally, in one aspect of the present disclosure, the selected solid electrolyte may have an ionic conductivity of 1x10 -5 S / cm, or according to some aspects of the present disclosure 1x10 -3 It has an ionic conductivity of more than S / cm.

[0102] Non-limiting examples of sulfide-containing solid electrolytes include Li-PS-based glasses, Li-PS-based glass ceramics, and argyrodite-based sulfide-containing solid electrolytes.

[0103] Non-limiting examples of sulfide-containing solid electrolytes include at least one of xLi2S-yP2S5, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2, or Li2S-GeS2-ZnS, Li6PS5X (X = at least one of Cl, Br, and I).

[0104] In an aspect of the present disclosure, the sulfide-containing solid electrolyte may include at least one selected from an LPS-based glass or glass ceramic such as xLi2S-yP2S5, and an argyrodite-based sulfide-containing solid electrolyte (Li6PS5X; X = Cl, Br, I).

[0105] The sulfide-containing solid electrolyte material is processed to form a coating on its surface. The sulfur or leaving group appears to react with sulfur in the electrolyte material to interact noncovalently or form covalent bonds, such as sulfide bonds or disulfide bonds.

[0106] The sulfur of the organic compound can attach to the surface of the solid electrolyte material (e.g., perhaps by forming a disulfide bond or sulfide bond at one end), and the hydrophobic tail is arranged to surround the electrolyte material. This hydrophobic layer forms a barrier to water and protects the electrolyte material.

[0107] To form an organic coating, a sulfide-containing solid electrolyte material may be combined with at least one compound selected from the compounds of the following formulae 1 and 2:

[0108] [Chemical Formula 1]

[0109] RA

[0110] [Chemical Formula 2]

[0111] R-A'-R

[0112] In the above formula, A is a -SH group, isocyanate, amine, or a suitable leaving group (e.g., triethoxysilyl or trimethoxysilyl); A' is a -S- moiety or a -SS- moiety; and each R is independently a substituted or unsubstituted C3-C20 alkyl group.

[0113] In certain aspects, each R group is independently selected such that the compound of Formula 1 or Formula 2 is a liquid. According to some aspects of the present disclosure, the total number of carbon atoms (including chains and substituents) will be from 6 to 16 carbons, or according to some aspects of the present disclosure, from 6 to 12 carbons, from 8 to 12 carbons, or from 10 to 12 carbons. The compound of Formula 1 can have a total of 6 carbons, 7 carbons, 8 carbons, 9 carbons, 10 carbons, 11 carbons, 12 carbons, 13 carbons, 14 carbons, 15 carbons, 16 carbons, 17 carbons, 18 carbons, 19 carbons, or 20 carbons. If the total number of carbon atoms is too low, the volatility of the compound may be too high to be usable. If the total number of carbon atoms is too high, the compound may not be a liquid. Thus, according to some aspects of the present disclosure, the total number of carbon atoms and the substituents and backbone can be adjusted as needed to render the compound liquid.

[0114] Each R group is independently a substituted or unsubstituted C3-C20 alkyl group, which is substituted or unsubstituted n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, tert-pentyl, isopentyl, n-hexyl, isohexyl, sec-hexyl, tert-hexyl, n-heptyl, isoheptyl, sec-heptyl, tert-heptyl, n-octyl, isooctyl, sec-octyl, tert-octyl, n-nonyl, isononyl, sec-nonyl, tert-nonyl, n-decyl, isodecyl, sec-decyl, tert-decyl, n-undecyl, isodecyl, sec-undecyl, tert-undecyl, n-dodecyl, isododecyl, sec-dodecyl, tert-dodecyl, etc. Including but not limited to:

[0115] The R group may be substituted with one or more groups including, but not limited to, an ester, a ketone, a halogen (e.g., fluorine, chlorine, bromine), and / or one or more C3-C20 alkyl groups (e.g., a C3-C8 alkyl group). In some aspects, the R group may be substituted with an aryl group (e.g., phenyl) or a heteroaryl group (e.g., a 5- or 6-membered ring including, but not limited to, pyridine, pyrrole, furan, or thiophene).

[0116] The term "leaving group" may be understood as defined by the IUPAC and may refer to an atom or group of atoms that is removed from the main or residual portion of a substrate during a reaction or an elementary step of a reaction, for example. For example, a leaving group may be a fragment that leaves together with a pair of electrons in heterolytic bond cleavage. In certain aspects, a leaving group may be an anionic or neutral species that leaves a neutral or cationic substrate. Any suitable leaving group compatible with the solid electrolyte material may be used.

[0117] In some aspects, the A group may be a “triethoxysilyl” moiety (e.g., derived from HSi(OC2H5)3) or a “trimethoxysilyl” moiety (e.g., derived from HSi(OCH3)3).

[0118] The term "thiol" may be understood as an organosulfur compound of the form R-SH, where R represents alkyl or other organic substituents.

[0119] The term "isocyanate" may be understood as a functional group having the formula RN=C=O, where R may be an alkyl or aryl group.

[0120] The term "amine" may be understood as a compound or functional group containing a basic nitrogen atom with a lone pair. Amines are formally derivatives of ammonia (NH3) in which one or more hydrogen atoms are replaced by a substituent such as an alkyl or aryl group (e.g., alkylamines and arylamines). The substituent -NH2 is called an amino group. In certain aspects, amines may include primary amines, secondary amines, and / or tertiary amines. In certain aspects, the amino group may be further converted into a useful leaving group, for example, by conversion to an ammonium salt, an aryl(sulfonyl)amino group, etc.

[0121] In some aspects, the sulfide-containing solid electrolyte material and the compound of formula 1 can be combined in a weight ratio of about 1:1 to 25:1, or in some aspects, in a weight ratio of about 1:1 to 10:1, a weight ratio of about 1:1 to 5:1, or a weight ratio of about 1:1.

[0122] Since sulfide-containing materials are sensitive to air and moisture and can decompose to produce toxic gases such as H2S, according to some aspects of the present disclosure, all synthesis and testing steps are performed in an argon-filled glovebox (e.g., MBraun MB 200B, H2O <0.5 ppm, O2 <5.0 ppm). Optionally, the reaction mixture of the sulfide-containing solid electrolyte material and the compound of formula 1 may further include a suitable solvent to aid dispersion.

[0123] Suitable reaction conditions may be used. In one aspect, the reaction temperature may be from room temperature to about 50°C. In some aspects, the reaction temperature may be from about 15°C to about 40°C, from about 20°C to about 40°C, or from about 25°C to about 40°C.

[0124] In one aspect, the reaction time may be about 30 minutes. In some aspects, the reaction time may be about 1 hour to about 8 hours, and in some aspects, about 2 hours to about 7 hours, or about 3 hours to about 5 hours.

[0125] The progress of the reaction may be monitored using any suitable technique, including but not limited to, X-ray photoelectron spectroscopy or nuclear magnetic resonance (NMR).

[0126] After the reaction is complete, the coated solid electrolyte material can be dried under any suitable conditions. In one aspect, the drying temperature may be from about 30°C to about 100°C, from about 40°C to about 100°C, or from about 50°C to about 100°C. According to some aspects of the present disclosure, the drying is performed under vacuum conditions. In one aspect, the drying time may be at least 30 minutes. In another aspect, the drying time may be at least 1 hour, and in some aspects, at least 2 hours, at least 8 hours, or at least 12 hours.

[0127] In the present disclosure, the average particle size of the sulfide-containing solid electrolyte material can be adjusted to a range suitable for a solid-state battery. In some aspects of the present disclosure, the solid electrolyte can have an average particle size of 0.1 μm to 50 μm.

[0128] In some aspects of the present disclosure, the solid electrolyte membrane can be prepared by any suitable method.

[0129] For example, after coating a solid electrolyte material, it can be optionally combined with other components and mixed to obtain a homogeneous mixture, as needed. This mixture can then be added to a predetermined organic solvent and dispersed to produce a slurry, which can then be applied to a molding plate and subsequently dried to form a sheet. If necessary, the resulting sheet can be pressed to obtain a solid electrolyte membrane.

[0130] The thickness of the solid electrolyte layer formed by the lithium-tin-metal-sulfide compound varies greatly depending on the structure of the all-solid-state battery. For example, in some aspects, it may be 0.1 μm or more and 1 mm or less, and in further aspects, it may be 1 μm or more and 100 μm or less. The solid electrolyte has high lithium ion conductivity in some aspects, and the lithium ion conductivity at room temperature is, in some aspects, for example, 1×10 -4 It is more than S / cm.

[0131] In one aspect, the solid electrolyte may further include a solid electrolyte generally used in all-solid-state batteries. As an example, an inorganic solid electrolyte or an organic solid electrolyte may be used.

[0132] For inorganic solid electrolytes, ceramic materials, crystalline materials or amorphous materials can be used, and thio-LISICON (Li 3.25 Ge 0.25 P 0.75S4), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5, Li3PS4, Li7P3S 11 , Li2O-B2O3, Li2O-B2O3-P2O5, Li2O-V2O5-SiO2, Li2O-B2O3, Li3PO4, Li2O-Li2WO4-B2O3, LiPON, LiBON, Li2O-SiO2, LiI, Li3N, Li5La3Ta2O 12 , Li7La3Zr2O 12 , Li6BaLa2Ta2O 12 , Li3PO (4-3 / 2w) Nw (where w is w<1), and Li 3.6 Si 0.6 P 0.4 Inorganic solid electrolytes such as O4 can be used.

[0133] In addition, examples of organic solid electrolytes include organic solid electrolytes prepared by mixing lithium salts with polymer materials such as polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate ester polymers, agitated lysine, polyester sulfide, polyvinyl alcohol, and polyvinylidene fluoride. In this case, these may be used alone or in combination of at least two.

[0134] The above-described coated sulfide-containing electrolyte material can be used as a solid electrolyte for an all-solid-state battery. The all-solid-state battery includes a positive electrode and a negative electrode, with a solid electrolyte interposed between them.

[0135] Meanwhile, the positive and negative electrodes of the all-solid-state battery according to the aspect of the present disclosure are not particularly limited, and any suitable ones known in the art may be used.

[0136] The all-solid-state battery proposed according to the aspect of the present disclosure defines the composition of the solid electrolyte as described above, and other elements constituting the battery, i.e., the positive electrode and the negative electrode, are not specifically limited in the present disclosure and follow the description below.

[0137] In one aspect, the negative electrode of the all-solid-state battery may be lithium metal alone, or the negative electrode active material may be laminated on the negative electrode current collector.

[0138] The negative electrode current collector is not particularly limited as long as it is conductive and does not cause any chemical change in the all-solid-state battery, and examples thereof include copper, stainless steel, aluminum, nickel, titanium, sintered carbon, copper or stainless steel whose surface is treated with carbon, nickel, titanium, silver, etc., or an aluminum-cadmium alloy. In addition, the negative electrode current collector, like the positive electrode current collector, may include various forms such as a film, a sheet, a foil, a net, a porous body, a foam, and a non-woven fabric having fine irregularities formed on the surface.

[0139] The negative active material may be any one selected from the group consisting of lithium metal, lithium alloy, lithium metal composite oxide, lithium-containing titanium composite oxide (LTO), and combinations thereof. In this case, the lithium alloy may be an alloy of lithium and at least one metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba, Ra, Al, and Sn. In addition, the lithium metal composite oxide may be an oxide (MeO) of lithium and any one metal (Me) selected from the group consisting of Si, Sn, Zn, Mg, Cd, Ce, Ni, and Fe. x ) may be, for example, LixFe2O3(0≤x≤1) or LixWO2(0≤x≤1).

[0140] In addition, the negative active material is Sn x Me 1-x Me' y O z(Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of groups 1, 2 and 3 of the periodic table, halogens; 0 <x=1; 1=y=3; 1=z=8)와 같은 금속 복합 산화물; SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O 4  and oxides such as Bi2O5; and carbon-based negative electrode active materials such as crystalline carbon, amorphous carbon or carbon composites, which may be used alone or in combination of two or more.

[0141] In some aspects of the present disclosure, the positive electrode may include a positive electrode active material layer comprising a positive electrode active material, a positive electrode conductive material, and a solid electrolyte. The positive electrode active material layer may further include a positive electrode binder resin, if necessary. Additionally, the positive electrode may optionally include a current collector, and the positive electrode active material layer may be positioned on at least one surface of the current collector.

[0142] In some aspects of the present disclosure, the cathode active material is lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or the like. 1+x Mn 2-x O4 (x is 0 to 0.33, e.g., LiMn2O4), LiMnO3, LiMn2O3, LiMnO2, lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV2O4, V2O5, Cu2V2O7, formula LiNi 1-x M x O2(M = Co, Mn, Al, Cu, Fe, Mg, B or Ga, 0 <x<1)으로 표시되는 Ni-사이트 리튬 니켈 산화물, 예를 들어, LiNi 1-z (Co,Mn,Al) z O2(0 <z<1); 식 LiMn 2-x M xLithium manganese complex oxides represented by O4 (M = Co, Ni, Fe, Cr, Zn or Ta, x = 0.01 to 1), e.g., LiMn 1.5 Ni 0.5 O4 or Li2Mn3MO8 (M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which Li in the formula is partially replaced by an alkaline earth metal ion; disulfide compound; Fe2(MoO4)3, and It may include at least one of lithium iron phosphate (LiFePO4). In some aspects of the present disclosure, the lithium iron phosphate may have all or at least a portion of the surface of the active material particles coated with a carbon material to improve conductivity.

[0143] According to an aspect of the present disclosure, the positive electrode active material is lithium nickel cobalt manganese oxide (e.g., Li(Ni,Co,Mn)O2, LiNi 1-z (Co,Mn,Al) z O2(0 <z<1)), 리튬 철 인산염(예를 들어, LiFePO4 / C), 리튬 니켈 망간 스피넬(예를 들어, LiNi 0.5 Mn 1.5 O4), lithium nickel cobalt aluminum oxide (e.g., Li(Ni,Co,Al)O2), lithium manganese oxide (e.g., LiMn2O4), and lithium cobalt oxide (e.g., LiCoO2).

[0144] According to some aspects of the present disclosure, the positive electrode active material may include a lithium transition metal composite oxide, and the transition metal may include at least one of Co, Mn Ni, and Al.

[0145] In some aspects of the present disclosure, the lithium transition metal composite oxide may comprise at least one of the compounds represented by Formula 1 below.

[0146] [Formula 1]

[0147] Li xNi a Co b Mn c M z O

[0148] In the above equation 1, 0.5≤x≤1.5, 0 <a≤1, 0≤b<1, 0≤c<1, 0≤z<1, 1.5<y<5, a+b+c+z는 1 이하이고, M은 Al, Cu, Fe, Mg 및 B로부터 선택되는 적어도 하나를 포함할 수 있다.

[0149] In some aspects of the present disclosure, the positive electrode active material comprises a positive electrode active material having a high Ni content of 0.5 or more, a specific example of which is LiNi 0.8 Co 0.1 Mn 0.1 May contain O2.

[0150] In some aspects of the present disclosure, the anode conductive material may be at least one conductive material selected from the group consisting of, for example, graphite, carbon black, carbon fibers or metal fibers, metal powders, conductive whiskers, conductive metal oxides, activated carbon, and polyphenylene derivatives. More specifically, the anode conductive material may be at least one conductive material selected from the group consisting of natural graphite, artificial graphite, Super-p, acetylene black, Kejen black, channel black, furnace black, lamp black, thermal black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide.

[0151] The current collector is not limited to a specific type and may include any material that does not cause a chemical change in the battery and has high conductivity (e.g., stainless steel, copper, aluminum, nickel, titanium, sintered carbon, or aluminum or stainless steel with a surface treated with carbon, nickel, titanium, or silver).

[0152] The cathode binder resin may include an electrode polymer commonly used in the art. Non-limiting examples of the binder resin include, but are not limited to, polyvinylidene difluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, and carboxyl methyl cellulose.

[0153] In some aspects of the present disclosure, the solid electrolyte included in the positive electrode may include at least one selected from a polymer-based solid electrolyte, an oxide-based solid electrolyte, and a sulfide-containing solid electrolyte. In some aspects of the present disclosure, the positive electrode active material may include the sulfide-containing solid electrolyte described in the solid electrolyte membrane.

[0154] In some aspects of the present disclosure, the positive electrode active material is included in the positive electrode in an amount of 50 wt% or more based on 100 wt% of the positive electrode active material layer. In addition, according to aspects of the present disclosure, the solid electrolyte is included in the positive electrode in an amount of 10 wt% to 40 wt% based on 100 wt% of the positive electrode active material layer.

[0155] Meanwhile, in some aspects of the present disclosure, the positive electrode has a capacity of 5 mAh / cm 2 Above, 6mAh / cm 2 or 10 mAh / cm 2 The battery according to the present disclosure can have a load (per electrode area) above. When a high-load positive electrode is applied, the battery can be operated at an electrochemically stable level.

[0156] Meanwhile, in some aspects of the present disclosure, the positive electrode active material layer can be obtained by preparing a slurry by adding a positive electrode active material, a conductive agent, a binder resin, and a solid electrolyte to an appropriate solvent, and casting the slurry, or by a manufacturing method using a dry mixing process without a solvent. Meanwhile, in some aspects of the present disclosure, it is possible to obtain a high-load positive electrode by achieving uniform mixing of the positive electrode active material in the positive electrode. In this embodiment, the positive electrode is obtained by a dry mixing process without using a solvent.

[0157] A method for manufacturing a positive electrode active material layer using a dry mixing method can be described, for example, as follows. First, a positive electrode material including a positive electrode active material, a conductive material, and a binder resin is placed in a mixing device and mechanically mixed to obtain a mixture. The mixing device may include any type of device capable of forming a relatively homogeneous mixture phase, such as a well-known mixer stirrer, and is not limited to a specific type of device. Meanwhile, in some aspects of the present disclosure, a temperature raising process may be included to improve the dispersion of solids in the mixing process and induce a fibrous form of the binder resin. In the temperature raising process, the temperature may be appropriately controlled in the range of about 30°C to 100°C. Next, the mixture is extruded into the shape of an electrode (a wide film shape) using an extruder, and the thickness can be controlled through a pressing process to form a positive electrode active material layer. The positive electrode active material layer may be applied to an electrode without a current collector, or, if necessary, a current collector may be attached to the obtained positive electrode active material layer to manufacture a positive electrode including a current collector.

[0158] Example

[0159] (1) Preparation of 1-undecanethiol coated Li6PS5Cl

[0160] Li6PS5Cl (purchased from NEI) was used as received. All samples were handled in a glove box with oxygen and moisture levels less than 0.5 ppm. 560 mg of Li6PS5Cl and 112 mg of 1-undecanethiol (Sigma-Aldrich) (5:1 weight ratio) were weighed into a 30 mL plastic vial containing a zirconium ball and spin-mixed at 2000 rpm for 20 minutes using a planetary mixer (THINKY™).

[0161] (2) Air exposure and drying of the sample

[0162] A 30 mL plastic vial containing a mixture of 560 mg of Li6PS5Cl and 112 mg of 1-undecanethiool from the previous step was placed in a 16 oz airtight bottle to minimize air exposure. Humidity and temperature were recorded. The samples were exposed for the following exposure times: 1 day (24 hours), 3 days (72 hours), 5 days (120 hours), and 7 days (168 hours). After air exposure, the samples were placed in a vacuum oven to dry the excess solvent and moisture on the material surface. The samples were vacuum-dried at 80 °C for 2 hours with a heating gradient of 1 °C / min. The samples were then transferred to a glovebox for further use.

[0163] (3) NMR characteristic analysis

[0164] Samples containing 1-undecanethiol coating material 1 H and 31 The effectiveness of the coating in preventing chemical degradation of LPSCs when exposed to ambient conditions was evaluated by P solid-state NMR (ss-NMR) and the interaction mechanism between the organic molecules of the coating and the LPSC surface was understood. Since ss-NMR is element-specific and sensitive to both crystalline and amorphous phases, it is possible to determine the interaction mechanism within the 1-undecanethiol molecule. 1 H nucleus and LPSC electrolyte 31 P nuclei can be selectively probed.

[0165] Figure 4a shows the morphology of pristine LPSCs, and pristine LPSCs and 1-undecanthiol (thiol) coated LPSC samples after exposure to ambient air for the various amounts of time mentioned. 31 P ss-NMR spectra are shown. Obtained from untreated LPSC sample and wet and dry samples coated with thiol. 31 No clear differences were observed between the P spectra, indicating that the LPSC bulk structure remained unchanged upon exposure to the coating solution and subsequent exposure to air.

[0166] To establish a baseline for the effects of air exposure on LPS, pure LPSC samples exposed to air for 1 day 31 The P ss-NMR spectra were collected and are presented in the upper part of Fig. 4a. As shown, the LPSC bulk structure is significantly degraded when exposed to air without coating, which is due to the formation of POS3 in a γ-Li3PS4-like environment, respectively. 3- Tetrahedral units and isolated PS4 3- The broad resonances of the untreated LPSC at 82.9 and 88.7 ppm, which are assigned to the tetrahedron, are lost and sharp resonances appear. In contrast, the resonances collected from the thiol-coated sample exposed to ambient air for 1 day are 31 The P ss-NMR spectrum was almost identical to that obtained from the untreated sample, indicating that the coating protected the LPSC structure from degradation. Even after 3 days in air, no changes were observed in the untreated sample. 31 Most of the P spectral features were retained. Nevertheless, the resonances at 82.9 and 88.7 ppm and the PS4 isolated in a β-Li3PS4-like environment were 3-The onset of degradation is indicated by the third resonance at 86.8 ppm assigned to the tetrahedron. As the exposure time increases, the broad LPSC resonances mostly disappear, with the peaks at 82.9 ppm, 86.8 ppm, and 88.7 ppm becoming larger, indicating the loss of the LPSC bulk structure. Interestingly, the coated LPSC sample exhibits a higher intensity of resonances at 86.8 ppm and 88.7 ppm, indicating that the isolated PS4, similar to Li3PS4, is formed when the coated sample is exposed to air. 3- It appears that more tetrahedra are formed compared to the pure sample.

[0167] Collected from a set of samples coated with undecane instead of 1-undecanethiool and exposed to air following the same procedure as above. 31 The P spectrum highlights the role of thiol chain ends in the protection mechanism of LPSCs. Coating with undecane, which has methyl end groups rather than thiol groups, resulted in a decrease in the LPSC sample's oxidation rate after only one day of air exposure. 31 Significant changes in the P resonance occur. The above results clearly demonstrate that the thiol coating delays the onset of degradation and largely preserves the LPSC structure even after exposure to ambient air for up to 72 hours.

[0168] To investigate the interaction properties between the organic molecules of the coating and the LPSC surface and to evaluate the efficiency of the drying step, a series of experiments were performed on pure 1-undecanethiol solution and on wet and dry thiol-coated LPSC samples. 1 H ss-NMR spectrum (shown in Fig. 4b) was collected. The spectrum obtained from pure undecanthiol solution showed six 1 H resonances can be resolved and these are compared with predicted shifts and integrated signal intensities from the ACD / HNMR Predictor software package. 1 Based on the agreement between the H environmental multiplicities, six compounds exist in the undecanthiol molecule. 1H was assigned to the local environment (labeled (af)). As shown in Figure 4b, when the 1-undecanethiol solution was mixed with LPSC ('LPSC coated, wet' sample), all of these resonances remained, but the (a) and (b) resonances were shifted downfield (to more positive ppm frequencies). The (a) and (b) resonances were associated with carbons 1 and 2 bonds away from the thiol terminal group, respectively. 1 corresponds to the H nucleus. In NMR, the isotropic shift of a nucleus depends on the degree of shielding from the static magnetic field provided by the local electron cloud and therefore varies greatly depending on its binding environment. Therefore, the change in the isotropic shift of the (a) and (b) resonances suggests that the undecanethiol molecule interacts or binds to the LPSC surface at the thiol terminus. The downfield shift of the (a) resonance (0.2 ppm) is larger than that of the (b) resonance (0.08 ppm), which is closer to the thiol terminus. 1 This is consistent with a greater change in the electron cloud around the H nucleus.

[0169] Thiol group 1 The disappearance of the (d) resonance assigned to H would provide further evidence that the thiol termini are attached to the LPSC surface, but it is difficult to reliably evaluate the change in the (d) signal intensity because the signal overlaps with the (c) and (e) resonances and the amount of undecanethiols in the 'LPSC coated, wet' and 'LPSC coated, dry' samples is unknown. An upfield shift (0.08 ppm) corresponding to the undecanethiols methyl chain termini is observed in the (f) resonance. This slight upfield shift is tentatively attributed to the weak van der Waals bonding interaction between the methyl termini of the undecanethiols molecules and the LPSC surface. This assignment is based on the nearly identical upfield shift observed when the LPSC is coated with undecane, as shown in Figure 8. 1 This is supported by the observation of H shift.

[0170] As confirmed by the spectrum shown in Fig. 8, a broad band was observed between 0.5 and 1 ppm. 1 The H resonance corresponds to the protonated impurity in the untreated material. Even after exposing the LPSC sample to a 1-undecanethiol solution and drying it at 80°C, the coating was not completely removed, which is a strong result collected from the 'LPSC coated, dry' sample. 1 This is evidenced by the H NMR signals. This spectrum contains similar (af) resonances to those obtained from the 'LPSC coated wet' sample, but an additional broad signal is observed in the range of 3-3.5 ppm. This additional signal may be due to the presence of undecanthiol molecules with various orientations and restricted movements on the surface of the dry LPSC particles, resulting in various chemical shifts and signal broadening.

[0171] (4) PXRD characterization

[0172] Samples were also characterized using powder XRD ("PXRD") measurements. After coating the adsorbent onto the LPSC, the compatibility of the coating was assessed by examining the crystal structure and changes in conductivity (if any) via EIS.

[0173] As shown in Figures 2a and 3a, the XRD results show that there is no change in the bulk crystal structure after 1-undecanethiol is coated on the LPSC. That is, the LPSC has an argyrodite structure. After exposure to 1-undecanethiol, Rietveld refinement shows that the argyrodite structure remains the same. There is no change in the bulk crystal structure.

[0174] (5) Raman characteristic analysis

[0175] Raman diffraction was measured using a Bruker instrument at a scan rate of 2° / min over a range of 10°–80°. Samples were prepared by grinding powders in a glove box covered with Kapton tape to prevent exposure to air. Raman spectroscopy was performed using a 532 nm source.

[0176] 424.5 cm using Raman spectroscopy -1 The structural evaluation upon air exposure was performed by monitoring the change in the peak at (Fig. 3b). This peak shifted to lower wavenumbers as the material deteriorated. Samples exposed for up to 3 days showed no shift in the main peak. These results are consistent with the XRD results showing no change in the bulk structure up to that point. 424.5 cm -1 The peak of PS4 is the key structural component responsible for the excellent ion conduction of these sulfide solid electrolyte materials. 3- This corresponds to a bond. The shift in this bond is attributed to the formation of oxythiophosphate species, but further research is needed for precise speciation.

[0177] (6) XPS characteristics

[0178] X-ray photoelectron spectroscopy (XPS) was also used to observe the evolution of oxidation states or bonding after exposure of the samples to air. The main peaks of interest are S 2p and P 2p, as they contain the main characteristic bonding of LPSC (Figures 3d and 3e). Untreated LPSC exhibits an S 2p signal at 161.5 eV and a P 2p signal at 132.0 eV. The peak at 160.3 eV, which begins to appear after 5 days of air exposure, is where the Li2S peak should be located, indicating that LPSC has begun to decompose via hydrolysis. On the other hand, the P 2p peak appearing around 133 eV is consistent with the formation of POxSy oxysulfide. However, it is impossible to identify which species exactly because various oxysulfide species generally all appear in that region. However, the signal at 133.6 eV may also signal that a Li3PO4 species has been formed.

[0179] (7) Electrochemical properties analysis

[0180] The samples were characterized using electrochemical impedance spectroscopy (EIS). For ionic conductivity measurements, all materials were cold-pressed into dense pellets at less than 6 tons. The pellets had a diameter of 13 mm and a thickness of 470 μm for 100 mg pellets and 1200 μm for 260 mg pellets. The pellets were prepared by pressing the powder with a titanium rod in a PEEK Swagelok die. The titanium rod served as a blocking electrode. Impedance measurements were performed using a frequency response analyzer (CH Instruments workstation) over a frequency range of 1 to 100 MHz with an amplitude of 5 mV.

[0181] For reference, a control conductivity test was conducted using untreated LPSCs (Fig. 3). For untreated LPSCs, the material no longer retained ionic conductivity after one day of air exposure.

[0182] (8) Cell fabrication and cyclability measurement

[0183] To evaluate the electrochemical performance of the aforementioned sulfide SSE samples, all-solid-state batteries (ASSBs) with a diameter of 13 mm were assembled using a polyaryl ether ketone (PEEK) mold and a Ti rod. Symmetric cells were fabricated using 100 μm of Li metal as both electrodes. LPSC, 1-undecanethiol / LPSC (1200 μm) exposed to air for 1 day, was used as the electrolyte. The full cell consisted of NCM811 (LG Energy Solution)-LPSC-VGCF cathode composites with a weight ratio of 66:31:3, respectively, at a concentration of 3 mg / cm. 2 The electrodes were fabricated by loading LiIn alloy. A LiIn alloy was used as the cathode. An electrolyte layer of untreated LPSC (450 μm) was placed between the cathode and the LPSC coated with 1-undecanethion and exposed to air. Cell measurements were performed on a LAND multichannel battery test system. The galvanostatic charge / discharge tests of the symmetrical cells were performed at room temperature (20-25°C) with a constant current of 0.1 mA / cm 2 , and each stage lasted for 1 hour. The constant current charge / discharge tests of the full cell were performed at a rate of 0.05C for the first cycle and 0.1C for the subsequent cycles within the voltage range of 1.9 to 3.65 V at temperatures below 60°C.

[0184] A study was conducted to investigate whether air-exposed LPSCs could maintain their functionality in all-solid-state batteries. As a result of the symmetrical cycling test, the untreated LPSC (Fig. 6a) exhibited a current density of 0.1 mA / cm 2 It can be seen that the cycle was maintained for 15 hours. The 1-undecanethiool-coated LPSCl (Fig. 6b) after 1-day air exposure remained stable even after longer cycles than the untreated one. Note that the polarization was slightly higher when using the 1-undecanethiool / LPSC exposed to air for 1 day.

[0185] To study the cycling stability, LiNi 0.8 Co 0.1 Mn 0.1O2(NCM811)|LPSCl|LiIn all-solid-state full cells were prepared. These were assembled using either untreated LPSCs or 1-undecanethiol / LPSCs exposed to air for 1 day (1D) (Figures 6c-6f). With the protection of the 1-undecanethiol coating, both cells exhibited similar second-cycle charge capacities and second-cycle coulombic efficiencies (CEs) (Figures 6c and 6d). The LPSCl full cells maintained similar capacities and cycle retention rates after 15 cycles, with discharge capacities of 132.9 mAh / g for the LPSCs (Figure 6e) and 133.9 mAh / g for the 1D 1-undecanethiol / LPSCs (Figure 6f). These observations demonstrate the surprisingly potent protective effect of 1-undecanethiol on LPSCs when exposed to air.

[0186] The conductivity of 1-undecanethioll coated LPSC is 2.2 mScm -1 1.73mScm at -1 , which was found to slightly decrease. This small decrease may be due to the introduction of non-conductive foreign matter, and the minimal effect on ionic conductivity is very unusual among polar organic solvents.

[0187] In summary, XRD, Raman, and XPS results all indicate that 1-undecanethiol-coated LPSCs remain protected without damage to their structure and conductivity even when exposed to air for up to 3 days.

[0188] (9) Chemical compatibility of SH and LPSC

[0189] To gain insight into the water-repellent ability of SH upon long-term air exposure, the interaction of 1-undecanethiol (SH) with water was studied without LPSC. Figure 9a shows the Raman spectra recorded for the SH solution upon exposure to air at 33% RH for 1, 2, and 3 days to monitor the change in CS stretching frequency in the range of 300-1900 cm. -1 Shows the area. SH is 639cm -1Maintains CS bond peak at 450-495cm -1 There is no evidence for SS bond formation, suggesting that SH molecules maintain their structural integrity in ambient air. In the same series of SH samples, 1 H nuclear magnetic resonance (NMR) spectra (shown in Figure 9b) were also collected, which revealed six 1 6 assigned to the H local environment 1 It exhibits H resonance. With long-term exposure, 1 The H signal shows a constant isotropic shift, the H2O peak does not appear, and the change in signal intensity is minimal. This suggests that the structure of the SH molecule remains unchanged and the diffusion of H2O within the SH is very slow.

[0190] By introducing small molecules into the system, the ionic conductivity of SSE can be maintained well, unlike previously reported polymer surface modifiers. This protection mechanism is highly effective. SH@LPSC maintains an ionic conductivity of 1 mS cm even after exposure (33% RH) for up to 2 days. -1 After 3 days of exposure to 33% RH, the SH@LPSC powder retained its original color and crystallinity, whereas the control material exhibited a sharp drop in conductivity with obvious discoloration (Fig. 1b).

[0191] (10) Chemical interaction between LPSC and SH

[0192] To explore the chemical interaction between LPSC and 1-undecanethiol (SH), density functional theory (DFT) calculations were performed on the adsorption energies of undecane (CH), which does not contain a thiol head group, and SH, which contains a thiol functional group, on the LPSC surface. Figure 10a shows that both organic compounds can adsorb onto the LPSC surface, but SH exhibits a much higher surface adsorption tendency (-3.82 eV) than CH (-1.172 eV). Furthermore, SH can form SS bonds with LPSC.

[0193] Density functional theory (DFT) calculations were performed with VASP code49. The Perdew-Burke-Ernzerhof (PBE) functional within the generalized gradient approximation (GGA)50 was used to account for the exchange correlation, while the projector augmented-wave pseudopotential (PAW)51 with a kinetic energy cutoff of 500 eV was used to describe the expansion of the electronic eigenfunctions. The vacuum thickness was set to 15 Å to minimize interlayer interactions. The Brillouin-zone integration was sampled by a Γ-centered 3 × 3 × 1 Monkhorst-Pack k-point. All atomic positions were energized and force-dependent, respectively, by 1 × 10 -5 eV and 0.03 eV / Å were sufficiently relaxed to reach a tolerance. Dispersion-corrected DFT-D method was used to consider long-range interactions.

[0194] SH-modified LPSCs (SH@LPSCs) were prepared by mixing the desired amounts of materials using a planetary centrifugal mixer (Fig. 11). Subsequently, the mixture was vacuum-dried at 80°C for 2 h to remove the unbound SH remaining on the LPSC surface. The compatibility of SH and LPSCs was evaluated by monitoring potential changes in the crystal structure and ionic conductivity of SH@LPSCs. Rietveld refinement of the XRD pattern obtained from the SH@LPSC sample (Fig. 12) shows that the argyrodite structure remains intact. 1H spin-echo NMR spectra (shown in Fig. 10b) were collected from the pure SH solution and the SH@LPSC sample to investigate the nature of the interaction between SH and the LPSC surface. In the spectrum obtained from the SH solution, six 1H resonances can be resolved, which are assigned to six 1H localized environments (labeled (af)) in the SH molecule. This assignment is based on the predicted 1H shifts from the ACD / HNMR Predictor software package, as well as the observed integrated signal intensities and expected 1H site multiplicities. In SH@LPSC, all SH resonances remain visible, but the (a) and (b) resonances shift downfield (to more positive ppm frequencies). The (a) and (b) resonances correspond to 1H nuclei bound to carbons located one and two bonds away from the thiol terminal, respectively. In NMR, the isotropic shift of a nucleus is a sensitive probe of local structural changes because it depends on the degree of shielding from the static magnetic field provided by the local electron cloud. Here, the changes in the isotropic shifts of the (a) and (b) resonances suggest that SH molecules bind to the LPSC surface at the thiol terminal. a) The downfield shift of resonance (0.2 ppm) is larger than that of (b) resonance (0.08 ppm), which is consistent with a larger shift in the electron cloud around the 1H nucleus closest to the thiol terminus.The apparent disappearance of the (d) resonance assigned to the thiol 1H group in the SH@LPSC spectrum may provide further evidence for the attachment of thiol-terminated groups to the LPSC surface; however, this signal overlaps with the (c) and (e) resonances, and the presence of residual free SH molecules in the SH@LPSC sample makes it difficult to correlate the change in (d) signal intensity with the attachment chemistry. For the (f) resonance, an upfield shift corresponding to the SH methyl chain termini is observed (0.08 ppm). This slight upfield shift was tentatively attributed to the weak van der Waals interaction between the methyl termini of the SH molecules and the LPSC surface. The broad 1H resonance observed between 0.5 and 1 ppm in the SH@LPSC spectrum in Figure 10b corresponds to that obtained from pure LPSC, as shown in Figure 13. 1 As confirmed by the H spectrum, it corresponds to a protonated impurity in the LPSC SSE. When the SH@LPSC sample was subjected to a vacuum drying procedure at 80°C for 2 h, the corresponding 1 As evidenced by the remaining SH signals in the H NMR spectrum (Fig. 13), the SH residue was not completely removed, and signal integration suggests that approximately 4-5 wt% SH was present in the sample. However, if desired, almost all of the SH modifier can be volatilized after further heat treatment at 300°C (Fig. 13). Further details on the quantification procedure are provided in Fig. 13, and representative fittings of the corresponding spectra are provided in Fig. 14.

[0195] The bonding interactions between SH and LPSC were further investigated using surface-sensitive XPS analysis, and the results are presented in Figures 10c-d. LPSC and SH@LPSC exhibit PS bonds derived from PS43- at 161.5 eV in the S 2p spectrum and 131.9 eV in the P 2p spectrum. The Li-S (Figure 10c) and PO (Figure 10d) signals at 160 eV and 133.5 eV for LPSC originate from surface decomposition products such as Li2S and POxSy during LPSC transport. In SH@LPSC, the increase in the intensity of the SH peak at 160 eV, which overlaps with the Li-S, and the simultaneous decrease in the PO peak at 133.5 eV suggest the formation of a thin SH film on the LPSC surface. The increase in the intensity of the SS peak at 164.5 eV in the SH@LPSC sample (Figure 10c) can be attributed to the cross-linking of sulfur atoms. This provides strong evidence that SS bonds are established between SH molecules and S atoms on the surface of LPSC. The completeness of the PS bond at 131.9 eV in Figure 10d indicates good compatibility between SH and LPSC. These findings confirm the existence of SS interactions between SH and LPSC, and are in good agreement with DFT calculations and NMR results.

[0196] As shown in Fig. 10e-f, cryo-TEM images of the untreated LPSC and SH@LPSC samples reveal the nanoscale distribution of crystalline and amorphous regions. The presence of SH modification on the surface of LPSC does not alter the bulk crystal structure, as evidenced by the similarity in the lattice spacing measured in SH@LPSC (0.182 nm, Fig. 10f) to that measured in the untreated LPSC (0.185 nm, Fig. 10e). This observation demonstrates the compatibility of SH with LPSC. An amorphous layer with a thickness of approximately 3 nm exists on the surface of the LPSC particles in the SH@LPSC sample, which was attributed to SH adsorption.

[0197] The sum of the bulk resistance and grain boundary resistance of SH@LPSC shows a slight increase from 20 to 22 ohm compared to that of the untreated LPSC (Fig. 10g). This slight increase may be due to the presence of 4-5 wt% nonconductive SH residue remaining after the drying procedure at 80°C. The Li ion conductivity was 1.8±0.16 mS cm, respectively, based on the average of three independent measurements. -1 and 1.6±0.03mS cm -1 (The error is equivalent to 1 standard deviation). It is quite unusual that the SH surface modifier has a minimal effect on the conductivity of LPSCs. For example, when sulfide SSEs are exposed to other polar solvents such as diethylene glycol dimethyl ether or propylene carbonate, a two-fold decrease in ionic conductivity is typically observed due to nucleophilic attack of SSE species from electron donors from the solvent molecules. In the case of propylene carbonate, the resulting mixture becomes sticky and the ionic conductivity is too low to be measured.

[0198] (11) Effectiveness of protection against moisture

[0199] To investigate the chemical stability of LPSC against hydrolysis, LPSC and SH@LPSC were evaluated after exposure to humid ambient air for 5 hours and up to 3 days. Samples are labeled "LPSC 5H air," e.g., LPSC 5H air, indicating a sample exposed for 5 hours.

[0200] A 12 mL plastic vial containing a mixture of 600 mg of LPSC and 120 mg of SH was placed in a 16 oz bottle and exposed to air with an initial humidity of 33% RH at room temperature. The exposure times were 5 h, 1 day, 2 days, and 3 days. A mixture of 600 mg of LPSC and 600 mg of SH (1:1 by weight) in the same 12 mL plastic vial was exposed to a fume hood for open-environment testing with a humidity of 40% RH for 10 min. After air exposure, the sample was placed in a vacuum oven and dried with a heating gradient of 1 °C / min at 80 °C for 2 h to dry the excess solvent and moisture on the material surface. The dried sample was then transferred to a glove box for further testing. It is noted that the heating process at 300 °C completely removes all SH residues, with crystal structure and conductivity matching those of untreated LPSC (Figure 27). However, the drying step at 80°C was sufficient to remove most of the SH without detrimentally affecting the conductivity and stability of Li.

[0201] To quantitatively assess the air stability of various LPSC samples under specific humidity conditions, a home-built system was used, as illustrated in Figure 15a. A humidifier was used to ensure a consistent initial humidity of 33% RH. Unless otherwise noted, 600 mg of LPSC, or a mixture of 600 mg of LPSC and 120 mg of SH, was placed in a 16-oz airtight container. A thermo-hygrometer was placed near the sample to monitor changes in the ambient humidity level over time. Figure 16a shows the evolution of relative humidity (RH) within the container as a function of exposure time (t). Because this is a closed environment, water consumption through reaction with LPSC leads to a decrease in the relative humidity. After 72 hours (3 days) of exposure, the relative humidity inside the LPSC container decreased from 33% to 7%. In contrast, the relative humidity inside the SH@LPSC container decreased from 33% to 13%. The moisture absorption of LPSC was estimated by first-order differentiation of relative humidity with respect to time. The results shown in Figure 16b reveal a significant reduction in moisture absorption of SH@LPSC, further confirming the effectiveness of the SH surface modifier in mitigating moisture reactivity. The air-exposed samples were vacuum-dried at 80°C for 2 hours prior to subsequent characterization.

[0202] From the XRD pattern in Fig. 15b, it can be seen that in the SH@LPSC sample, no new phases were formed after 1 day of exposure to 33% RH air, whereas new peaks began to appear at 25° and 35° with very low intensities after 3 days of exposure. The basic structure of LPSC remained unchanged, suggesting that SH effectively acts as a protective agent. In contrast, the XRD pattern of LPSC after 3 days of exposure to 33% RH air shows the main Li2S and LiCl decomposition phases, indicated by peaks at 25° and 35°. The full XRD dataset is provided in Fig. 17.

[0203] The evolution of the bulk LPSC structure upon exposure to moist air was monitored using Raman spectroscopy. At this time, PS4 3- 424.5cm equivalent to the unit -1 The peak shift was monitored (Fig. 15c), which is a key structural component responsible for the excellent ion conductivity of sulfide SSE. As the material deteriorates, the peak shifts to lower wavenumbers, which is likely due to the decomposition of PS bonds into PO bonds to form oxy-thiophosphate species, but further investigation is needed for accurate speciation. The spectrum obtained from the SH@LPSC 1D air sample was characterized by a peak at 424.5 cm -1 While there is no change in peak, the SH@LPSC 3D air sample is PS4 3- The shift of the same peak is very small when 16.2% of the unit is degraded. In contrast, the LPSC 1D air sample shows a significant peak shift, which is comparable to the PS4 3- This represents a 41.8% degradation of the unit. These results are consistent with the XRD results that show that for SH@LPSC SSE, the bulk structure begins to degrade only after about 3 days of exposure to humid air.

[0204] Figures 15d-e plot the ionic conductivities of the electrolyte pellets manufactured by cold pressing. With the application of the SH absorbent, the ionic conductivity of SH@LPSC is 1.8±0.16 mS cm based on the average of three independent measurements, as shown in Figures 15d-e. -1 1.6±0.03mS cm -1 The ionic conductivity decreases slightly. This slight decrease may be due to the introduction of low ionic conductivity components into the system. SH@LPSC exhibits excellent stability after 5 h, 1 day, and 2 days of air exposure, which shows a change in ionic conductivity of 1.1 mScm over that time. -1 at 1.0mS cm -1, which is very small (Fig. 15e). In contrast, the LPSC without SH coating has an ionic conductivity of 0.15 mS cm after 5 h of air exposure. -1 The ionic conductivity of LPSC during exposure is significantly reduced (Fig. 3e). The change in ionic conductivity of LPSC during exposure is a function of both humidity and time. When the amount of LPSC in the closed vessel is reduced from 600 mg (Fig. 15e) to 200 mg (Fig. 18), increasing the H2O to LPSC ratio, the relative effectiveness of SH protection becomes much more pronounced. SH@LPSC exhibits an ionic conductivity of 0.4 mS cm after 1 day of air exposure. -1 LPSC(0.003mS cm -1 ) is two orders of magnitude higher than that of LPSC and SH@LPSC (weight ratio LPSC:SH = 1:1). The experiments were performed by exposing LPSC and SH@LPSC (weight ratio LPSC:SH = 1:1) to air in a chemical fume hood at 40% RH. Due to the combined effects of the complex airflow pattern in the fume hood and the possible loss of SH, the experimental conditions cannot be controlled to the same extent as the closed system used in the rest of this study, which would allow for easier quantification of the sample trends. Nevertheless, the values ​​of SH@LPSC and LPSC were 0.5 mS cm, respectively. -1 and 0.003mS cm -1 When the conductivity of , a two-order of magnitude improvement in ionic conductivity retention is again observed (Fig. 15d). To contextualize the results, Figs. 15f-g summarize previously reported stability data collected on modified LPSC electrolytes after air / moisture exposure. SH protection extends the LPSC protection time from minutes to days (Fig. 15f). The conductivity loss rate is typically ~100-fold lower (Fig. 15g). This approach enables sulfide SSE processing under standard ambient conditions without additional humidity control, resulting in a significant reduction in manufacturing costs. Furthermore, stability in a standard dry room with a dew point of -40°C is also fully expected.

[0205] (12) Surface protection mechanism

[0206] The trend of material changes after exposure to air (33%RH) was monitored using XPS and solid-state NMR (ssNMR), and the results are shown in Fig. 19. Examination of LPSC 1D air and LPSC 3D air samples revealed SO at 167 eV. x 2- The SO peak from the origin appears (Fig. 19a), and the PO peak intensity from the oxysulfide (POxSy) at 132.5 eV increases (Fig. 19b), indicating that hydrolysis occurs to produce S 2- It can be seen that oxidation has occurred. In contrast, no SO peak appears in SH@LPSC 1D air and SH@LPSC 3D air samples (Fig. 19a), and the intensity of the PO peak remains unchanged (Fig. 19b) compared to SH@LPSC (Fig. 10d). The SS bond strengths of SH@LPSC 1D and SH@LPSC 3D are almost the same as those of SH@LPSC. The bonding between SH and LPSC protects the surface from oxidation, while the hydrolysis reaction is significantly reduced, effectively preserving the important PS 3 units.

[0207] LPSC and SH@ LPSC samples were also exposed to humid ambient air before and after 31 P and 6Li ssNMR were investigated, and the results are shown in Fig. 19c and Fig. 20, respectively. Since ssNMR is element-specific and sensitive to both crystalline and amorphous phases, it is possible to determine the presence of crystalline phases in the LPSC electrolyte. 31 P and 6 Li nuclei can be selectively probed. Obtained from LPSC and SH@ LPSC samples. 31 No obvious difference is observed between the P spectra, indicating that the bulk structure of LPSC does not change when mixed with SH. Collected from SH@LPSC 1D air sample. 31The P ssNMR spectra are almost identical to those obtained from LPSC, indicating that the coating protects the LPSC structure from degradation. Even after 3 days in air, the SH@LPSC sample shows no significant changes compared to the untreated LPSC. 31 Most of the P spectral features are retained. Nevertheless, new resonances appear at 82.9 and 88.7 ppm, as well as β-Li3PS. 4 PS4 isolated from similar environment 3- The onset of degradation is indicated by the appearance of the third resonance at 86.8 ppm, which is assigned to the tetrahedron. Unprotected exposure to air leads to a significant degradation of the LPSC bulk structure, with the broad resonance of the untreated LPSC disappearing and sharp resonances at 82.9 and 88.7 ppm, respectively, being assigned to the POS3. 3- PS4 isolated from tetrahedral units and Li3PS4-like environments 3- It is reflected that the tetrahedrons are assigned to the isolated PS4. Interestingly, the air exposure of the SH@LPSC sample 3- More Li3PS like tetrahedrons 4- , which is evidenced by the higher resonance intensities of 86.8 ppm and 88.7 ppm in the spectra collected from the SH@LPSC 3D air sample compared to those obtained from the LPSC 3D air sample. In summary, 31 P and 6 From the Li ssNMR results, it is clearly demonstrated that SH modification delays the onset of degradation and largely preserves the LPSC structure even after exposure to ambient air for up to 3 days. Finally, the collected data from SH@LPSC and SH@LPSC 1D air samples 1The H spectra (Fig. 21) suggest that the amount of SH adsorbed on the LPSC surface decreases with air exposure time (probably due to evaporation), as evidenced by the decrease in the broad peak (~3.5 ppm) near (a), which may partially explain the decreasing efficiency of the SH coating with increasing exposure time.

[0208] In a series of samples modified with CH instead of SH, before and after exposure to 33%RH air for 1 or 2 days 6 Li and 31 P spectra were collected. These samples are labeled CH@LPSC, CH@LPSC 1D air and CH@LPSC 3D air. The results shown in Figures 22-23 emphasize that the thiol chain terminal of SH plays an important role in the protection mechanism of LPSC. Coating with CH (methyl rather than thiol terminal) does not protect LPSC SSE from hydrolysis, and the CH@LPSC 1D air sample 6 Li and 31 Significant changes are observed in the P resonance.

[0209] SH's air stability and ability to form SS bonds with the LPSC surface have been confirmed, making it a powerful hydrophobic protective agent. Specifically, SH forms a strong impermeable layer that prevents water from reaching the LPSC surface. This protective layer prevents LPSC from reacting with ambient moisture for up to several days. The slow degradation of SH@LPSC upon prolonged air exposure may be related to water infiltration through defects bypassing the SH protective layer or through SH evaporation, exposing the unbound LPSC surface.

[0210] (13) Improved electrochemical performance

[0211] The electrochemical stability of LPSC and SH@LPSC SSEs in Li symmetric cells and full cells was studied by exposing them to air for 1 day. Li / Li symmetric cells are commonly used to evaluate the interfacial stability of SSEs and lithium metal. The critical current density (CCD) is an indicator of how well SSEs can withstand short circuits caused by lithium dendrite growth. Figure 24 shows that the CCD value of SH@LPSC 1D air at room temperature was 0.6 mA cm -2 While it is unchanged compared to the untreated LPSC, the CCD value of LPSC 1D air is 0.63 mA cm -2 at 0.3mA cm -2 shows a decrease. Therefore, in SH@LPSC 1D air, the surface modification due to air exposure does not appear to change the interaction between LPSC and Li. Also, Fig. 25 shows the 1.5 mAh cm -2 Li at capacity load 0.5 In / LiNi 0.8 Co 0.1 Mn 0.1 The constant current cycling performance of O2 is shown. Compared with the baseline cell using the untreated LPSC electrolyte (Fig. 26), the cell fabricated with LPSC after 1 day of air exposure (Fig. 25(a)) showed an increase in electrolyte resistance after the formation cycle, resulting in a decrease in cell voltage of ~80 mV and a discharge capacity of 135 mAh g. -1 In contrast, after 1 day of air exposure, the cell fabricated with SH@LPSC (Fig. 25(c-d)) had a similar capacity of 155 mAh g as the untreated LPSC full cell (Fig. 26). -1 , and exhibits a capacity retention of 80% even after 50 cycles. This observation provides strong evidence for the remarkable protective effect of SH on LPSCs, especially in mitigating the adverse effects of moisture exposure.

[0212] These experiments demonstrate that the long-chain thiol, 1-undecanethiol, can effectively protect Li6PS5Cl solid electrolyte from exposure to humid air. 1-Undecanethiol is chemically compatible with Li6PS5Cl, has a minimal effect on the conductivity, and can be largely removed by a vacuum drying process. Structural analysis revealed that the -SH terminal groups form SS bonds with S atoms on the surface of the solid electrolyte without destroying the PS network, which is essential for ionic conductivity. The hydrocarbon tail of the thiol forms a hydrophobic layer that effectively repels water. The novel SH surface modification was found to be effective in maintaining the bulk structure and ionic conductivity of Li6PS5Cl even after prolonged exposure to humid air. The SH-modified solid electrolyte exhibited a ionic conductivity of > 1 mS cm for 2 days when exposed to air at a relative humidity of 33%. -1 Maintains ionic conductivity. These outstanding results represent a significant advance in moisture protection time, surpassing previous studies in this field by two orders of magnitude. With 1-undecanethiol protection, the electrolyte exhibits similar performance in all-solid-state batteries even after one day of air exposure. These results demonstrate the potential of 1-undecanethiol surface modification to preserve extremely air-sensitive sulfide solid electrolytes outside of a glovebox or dry room, paving the way for more practical, efficient, and scalable methods for manufacturing sulfide solid-state batteries.

[0213] Material properties specifications

[0214] Raman spectroscopy (Renishaw™ inVia™) measurements were performed over a range of 300–2500 cm at an excitation wavelength of 785 nm. -1 The measurements were performed in the range. All powders were prepared by hand-grinding in a glove box covered with Kapton tape to prevent air exposure during measurements. Liquid SH samples before and after air exposure were 1H NMR spectroscopy was used for analysis. To prepare the sample, 100 μl of SH or air-exposed SH specimen was mixed with 1000 μl of chloroform D (99%, Sigma-Aldrich) and then transferred to an NMR sample tube. 1 H NMR was performed on a 500 MHz spectrometer (ECA500, JEOL). Powder XRD (D8 DISCOVERY, Bruker) was measured at a scan rate of 2° / min from 10° to 80°. Samples were sealed using Kapton tape. For cryo-TEM imaging, specimens were placed on copper grids and fixed in a dual-tilt cryo-TEM transfer holder in a liquid nitrogen environment. Cryo-TEM images were captured using a JEM-2100F electron microscope operating at an accelerating voltage of 200 kV. XPS analysis was performed using an AXIS Supra XPS instrument from Kratos Analytical. XPS data were 10 -8 Spectra were acquired using a monochromatized Al Kα source emitting at 1,486.7 eV in an ultra-high vacuum environment of 10 Torr with the sample. The sample was transferred from a nitrogen-filled glovebox to avoid further air exposure. A 10 keV Ar (1000 atoms) cluster source was applied for 60 s for surface cleaning prior to analysis. All XPS spectra were corrected for the extrinsic C 1s peak at 284.6 eV and then analyzed using CasaXPS software. For solid-state NMR, all spectra were acquired at 18.8 T (800 MHz for 1H) on a Bruker Ultrashield Plus standard bore magnet equipped with an Avance III console. 1 H and 31P solid-state NMR spectra were obtained at a spinning speed of 60 kHz using a 1.3 mm HX MAS probe equipped with a zirconia rotor sealed with a Vespel cap under Ar. An N2 gas flow (2000 l / hr) was used to control the rotor temperature and protect the sample from moisture contamination. Data were acquired using a rotor-synchronized spin-echo pulse sequence (90°-TR-180°-TR-477 ACQ). 1 For H, 90° and 180° flip angles at 75 W were used at 1.6 μs and 3.2 μs, respectively. 31 For P, 90° and 180° flip angles at 75 W were used with 1.5 μs and 3.0 μs, respectively. For liquid undecane and 1-undecanethiols 1 The H solution spectrum was obtained using a BBO 800MHz S4 5mm probe. The data were obtained using a direct excitation, single pulse sequence with a 30° flip angle and 4.8µs at 21W. The 1H chemical shift was determined using adamantane at 0.247ppm of tetrakis(trimethylsilyl)silane. 1 Indirectly referenced the H signal. 31 P chemical shift at 0 ppm of 85% H3PO4 31 Refer to the P signal. 6 Li solid-state NMR spectra were obtained at a spinning speed of 20 kHz using a 3.2-mm HXY MAS probe equipped with a zirconia rotor sealed under Ar with a Vespel cap. Rotor-synchronized spin-echo pulse sequences were used with 90° and 180° flip angles of 8.0 μs and 16.0 μs, respectively, at 200 W. 6 Li chemical shifts were referenced to 0 ppm of 1 M LiCl. In the SH@LPSC sample 1 Spectra for H quantification were obtained at a rotation speed of 20 kHz using a 2.5 mm HX MAS probe with a zirconia rotor sealed with a Vespel cap under Ar. Sample content for quantification and1 To maximize the H signal, a larger rotor size was used. The rotor-synchronized spin-echo pulse sequence used 90° and 180° flip angles of 2.66 μs and 5.32 μs at 100 W, respectively. T2* measurements of each sample were performed to compensate for the uneven signal attenuation during the 50 μs echo delay. For each sample, a series of rotor-synchronized spin-echoes (90°-TR-180°-TR-ACQ) with variable echo delays were acquired and the spectra were fitted using an in-house package to obtain the T2* values. The exact 1 To ensure H quantification, spectral and T2* measurements were also obtained with an empty rotor. The same measurements were then repeated for adamantane of known mass, and the signal contribution from the empty rotor was subtracted. 1 The H content was corrected by the integrated spectral intensity. The same measurements were performed on the untreated LPSC sample and two SH@LPSC samples dried at 80°C and 300°C, respectively. For each sample, the proton content was calculated by considering the T2* signal attenuation of each fitted component and the contribution of the empty rotor. For the dried SH@LPSC sample, the 1-undecanethiol content of the sample was calculated by subtracting the proton content of the untreated LPSC.

[0215] Battery assembly

[0216] To evaluate the electrochemical performance, ASSB Swagelok cells consisting of polyaryl ether ether ketone (PEEK) molds and Ti rods were assembled. In the symmetric cell, 200 mg of solid electrolyte powder was compressed into pellets with a diameter of 13 mm by applying a pressure of 375 MPa. Lithium metal foils with a diameter of 1.11 cm and a thickness of 100 μm were attached to both sides of the electrolyte pellets. The resulting Li / SSE / Li symmetric cell was then sandwiched between two Ti rods. In the full cell, NCM811 (LiNi 0.8 Co 0.1 Mn 0.1The cathode composite was fabricated by mixing O2, LG Energy Solution)-LPSC (Ampcera Inc., used as received)-vapor-grown carbon fiber (Sigma Aldrich) in a weight ratio of 60:37:3. 100 mg of untreated LPSC and 100 mg of air-exposed SSE (sample in Figure 15f) were compressed at 30 MPa to form a double-layer electrolyte pellet. Then, the cathode composite weighing 16.2 mg was introduced onto the untreated LPSC side and pressed at 375 MPa. Li with a diameter of 1.11 cm 0.5 The alloy was attached to the air-exposed SSE side and pressed at 125 MPa. After that, the obtained Li 0.5 The in-air exposed SSE / LPSC / anode cell was sandwiched between two Ti rods. During testing, the symmetric and full cells were maintained at 30 MPa and 55 MPa, respectively. All cells were assembled in an argon-atmosphere glovebox.

[0217] electrochemical testing

[0218] Cell measurements were performed on a LAND multichannel battery test system. Galvanostatic charge-discharge tests of symmetric cells were performed at room temperature with stepwise increasing current densities for 0.5 h per half cycle. Galvanostatic charge-discharge tests of full cells were performed at 60°C at a rate of 0.1C over a voltage range of 1.9–3.65 V. Impedance measurements were performed at room temperature using a frequency response analyzer (CH Instruments workstation) over a frequency range of 7–100 MHz with an amplitude of 5 mV. The impedance measurement setup used 100 mg of electrolyte with a diameter of 13 mm and pressed and maintained at 375 MPa at room temperature, while a Ti rod served as a blocking electrode.

[0219] It will be appreciated by those skilled in the art that aspects of the present disclosure can be practiced within a wide range of equivalent parameters without affecting the scope of the disclosure set forth herein. All publications, patent applications, and patents disclosed herein are incorporated by reference in their entirety.

Claims

1. A sulfide-containing solid electrolyte material having a surface; and Organic coating formed on the surface of the above sulfide-containing solid electrolyte material A solid electrolyte composition comprising: A solid electrolyte composition wherein the coating is formed of at least one of the compounds of the following chemical formulas 1 and 2: [Chemical Formula 1] RA [Chemical Formula 2] R-A'-R In the above formula, A is an SH group, isocyanate, amine, or leaving group; A' is the -S- moiety or the -SS- moiety; Each R is independently a substituted or unsubstituted C3-C20 alkyl group.

2. In paragraph 1, A solid electrolyte composition in which the compound of the above chemical formula 1 or 2 is attached to the surface of the sulfide-containing solid electrolyte material by chemical adsorption, van der Waals interaction, or ionic interaction.

3. In paragraph 1, A solid electrolyte composition in which the compound of the above chemical formula 1 or chemical formula 2 reacts with the above sulfide-containing solid electrolyte material to form a covalent bond.

4. In paragraph 1, A solid electrolyte composition, wherein A in the compound of the above chemical formula 1 is an SH group.

5. In paragraph 1, A solid electrolyte composition, wherein in the compound of the above chemical formula 1, A is at least one leaving group selected from triethoxysilyl and trimethoxysilyl.

6. In paragraph 1, A solid electrolyte composition, wherein at least one of R in the compound of the above chemical formula 1 or chemical formula 2 is a C6-C16 alkyl group.

7. In paragraph 1, A solid electrolyte composition, wherein at least one of R in the compound of the above chemical formula 1 or chemical formula 2 is a C8-C12 alkyl group.

8. In paragraph 1, A solid electrolyte composition, wherein the total number of carbon atoms in the compound of the above chemical formula 1 or chemical formula 2 is 6 to 16.

9. In paragraph 1, A solid electrolyte composition, wherein the total number of carbon atoms in the compound of the above chemical formula 1 or chemical formula 2 is 8 to 12.

10. In paragraph 1, A solid electrolyte composition, wherein at least one of R in the compound of the above chemical formula 1 or 2 is a C3-C20 alkyl group, and the C3-C20 alkyl group has one or more substituents selected from the group consisting of fluorine, chlorine, bromine, ester, and ketone moieties.

11. In paragraph 1, A solid electrolyte composition wherein the compound of the above chemical formula 1 is 1-undecanethiol.

12. In paragraph 1, A solid electrolyte composition, wherein the above sulfide-containing solid electrolyte material is selected from the group consisting of inorganic electrolyte materials and organic electrolyte materials.

13. In paragraph 1, A solid electrolyte composition wherein the above sulfide-containing solid electrolyte material is an inorganic electrolyte.

14. In paragraph 1, The above sulfide-containing solid electrolyte is Li3P7S 11 , Li 10 GeP2S 12 A solid electrolyte composition comprising at least one selected from Na3PS4 and Li6PS5Cl.

15. In paragraph 1, A solid electrolyte composition comprising at least one selected from the group consisting of LPS-based glasses and glass ceramics of the formula xLi2S·yP2S5 (wherein x+y=1).

16. In paragraph 1, The above sulfide-containing solid electrolyte is a solid electrolyte composition comprising an argyrodite-based solid electrolyte of the formula Li6PS5X (wherein X is Cl, Br, or I).

17. In paragraph 1, The above sulfide-containing solid electrolyte is formula Li 6-y PS 5-y Cl 1+y A solid electrolyte composition comprising an argyrodite-based solid electrolyte (wherein y is <1).

18. Providing a sulfide-containing solid electrolyte material, By combining the above solid electrolyte material with at least one of the compounds of the following chemical formulas 1 and 2, a coated sulfide-containing solid electrolyte material is formed, Forming a solid electrolyte using the above-mentioned coated sulfide-containing solid electrolyte material A method for producing a solid electrolyte composition according to claim 1, comprising: [Chemical Formula 1] RA [Chemical Formula 2] R-A'-R In the above formula, A is an SH group, isocyanate, amine, or leaving group; A' is the -S- moiety or the -SS- moiety; Each R is independently a substituted or unsubstituted C3-C20 alkyl group.

19. Providing a sulfide-containing solid electrolyte, Combining the above solid electrolyte with at least one of the compounds of the following chemical formulas 1 and 2 to form a coated sulfide-containing solid electrolyte material. A method for producing a solid electrolyte, comprising: [Chemical Formula 1] RA [Chemical Formula 2] R-A'-R In the above formula, A is an SH group, isocyanate, amine, or leaving group; A' is -S-; Each R is independently a substituted or unsubstituted C3-C20 alkyl group.

20. A solid electrolyte comprising a solid electrolyte composition according to paragraph 1.

21. Cathode; Bipolar; and A solid electrolyte according to claim 20, interposed between the cathode and the anode An all-solid-state battery comprising:

Citation Information

Patent Citations

  • Polymer electrolyte composition containing a thiol-ene compound as a main component

    KR1019990008210A

  • Negative electrode, nonaqueous electrolyte secondary battery and method for manufacturing the same

    KR1020110021662A

  • Loading and packing device for rope

    KR1020210099351A

  • Wheel type diamond tools

    KR102197214B1