Positive electrode active material, and positive electrode and lithium secondary battery comprising same

The use of a lithium complex transition metal oxide with a single particle structure and amorphous lithium coatings addresses the issues of particle collapse and lithium by-product reactions in high-nickel batteries, enhancing energy density and lifespan while preventing slurry gelation, resulting in improved battery performance.

WO2024248573A1PCT designated stage expired Publication Date: 2024-12-05LG CHEM LTD

Patent Information

Application Number
PCT/KR2024/007595
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-06-03
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

High-nickel positive electrode active materials in secondary batteries face issues such as particle collapse due to microcracks during charging and discharging, leading to decreased energy density and lifespan, and the presence of lithium by-products on the surface causes side reactions and slurry gelation, affecting battery performance.

Method used

A lithium complex transition metal oxide with a single particle structure and a coating portion containing amorphous lithium compounds, specifically boron and cobalt, is used to reduce lithium elution and side reactions, and improve dispersibility, thereby enhancing the stability and performance of the positive electrode active material.

Benefits of technology

The solution effectively reduces particle breakage, side reactions, and slurry gelation, leading to improved energy density, lifespan, and charge/discharge efficiency of lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024007595_05122024_PF_FP_ABST
    Figure KR2024007595_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a positive electrode active material capable of improving the performance of a lithium secondary battery. The present invention relates to a positive electrode active material, and a positive electrode and a lithium secondary battery comprising same, the positive electrode active material including: a lithium composite transition metal oxide in the form of a single particle; and a coating part formed on the lithium composite transition metal oxide and including an amorphous lithium compound, wherein the coating part includes: a first coating part; and a second coating part, the first coating part has a discontinuously formed island shape and the second coating part has a continuously formed coating layer shape, and the first coating part and the second coating part each independently include boron (B) and cobalt (Co), and selectively include one or more coating elements selected from the group consisting of Co, Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La, and Hf.
Need to check novelty before this filing date? Find Prior Art

Description

Cathode active material, and cathode and lithium secondary battery containing the same

[0001] Cross-citation with related applications

[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2023-0071875, filed June 2, 2023, the entire contents of which are incorporated herein by reference.

[0003] Technology field

[0004] The present invention relates to a positive electrode active material, and a positive electrode and a lithium secondary battery including the same.

[0005]

[0006] Recently, with the advancement of technology such as electric vehicles, the demand for high-capacity secondary batteries is increasing, and accordingly, research on cathodes using high-nickel (High Ni) cathode active materials with excellent capacity characteristics is being actively conducted.

[0007] Since the high-nickel cathode active material uses a co-precipitation method to manufacture it, the manufactured high-nickel cathode active material has the form of secondary particles in which primary particles are aggregated. However, the active material in the form of secondary particles has the disadvantage that microcracks occur in the secondary particles during long-term charge / discharge processes, causing side reactions. In addition, when the electrode density is increased to improve energy density, the secondary particles cause structural collapse, which reduces the active material and electrolyte, resulting in a decrease in energy density and a decrease in life characteristics.

[0008] To solve the problems of such secondary particle-type high-nickel positive electrode active materials, single-particle nickel-based positive electrode active materials have recently been developed. Single-particle nickel-based positive electrode active materials have the advantage of not causing particle collapse even when the electrode density is increased for high energy density. However, since a relatively high sintering temperature is required to manufacture single-particle nickel-based positive electrode active materials, the layered structure of R-3m is not properly maintained, and lithium escapes from the crystal structure, causing a phase change to the Fm-3m rock-salt structure, such as NiO, and the crystallinity of the positive electrode active material decreases, so the proportion of NiO on the surface of the manufactured single-particle particles increases. As NiO increases, resistance increases and energy density and output decrease.

[0009] In addition, in order to manufacture a positive electrode using a positive electrode active material, a process of mixing a conductive agent, a binder, an additive, and a solvent with the positive electrode active material to make a slurry must be performed. However, at this time, the Li byproduct located on the surface alkalizes the solvent, and the alkalized solvent mixes with the binder to gel the slurry. Therefore, it is difficult to uniformly coat the slurry for manufacturing a positive electrode using the gelled slurry.

[0010] Therefore, there is a need to develop a method that can prevent performance degradation of the positive electrode active material and gelation of the slurry by introducing an additional process during the manufacture of the positive electrode active material to suppress the reaction of Li byproducts present on the surface of the positive electrode active material with external substances.

[0011]

[0012] [Prior Art Literature]

[0013] [Patent Document]

[0014] (Patent Document 1) KR 2019-0094529 A1

[0015]

[0016] The problem to be solved by the present invention is to provide a cathode active material in which lithium ion dissolution and side reactions between lithium ions and electrolytes are reduced by forming an amorphous lithium compound on the surface of the cathode active material to reduce lithium by-products, and in which gelation of the cathode slurry is suppressed during the manufacture of the cathode slurry.

[0017] Another problem to be solved by the present invention is to provide a positive electrode and a lithium secondary battery including the positive electrode active material.

[0018]

[0019] To solve the above problem, the present invention provides a cathode active material, a cathode including the same, and a lithium secondary battery.

[0020] (1) The present invention provides a cathode active material comprising a lithium composite transition metal oxide in the form of a single particle; and a coating portion formed on the lithium composite transition metal oxide and including an amorphous lithium compound; wherein the coating portion includes a first coating portion; and a second coating portion; wherein the first coating portion has an island shape formed discontinuously, and the second coating portion has a coating layer shape formed continuously, and wherein the first coating portion and the second coating portion each independently include boron (B) and cobalt (Co), and optionally include one or more coating elements selected from the group consisting of Co, Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La, and Hf.

[0021] (2) The present invention provides a positive electrode active material having a sequential phase gradient from an amorphous structure to a spinel structure and a layered structure in the center direction from the surface in the above (1).

[0022] (3) The present invention provides a positive electrode active material in (1) or (2) above, wherein the first coating portion is dispersed and distributed on at least one of the surface of the lithium composite transition metal oxide and the surface of the second coating portion.

[0023] (4) The present invention provides a positive electrode active material according to any one of (1) to (3), wherein the amorphous lithium compound includes lithium boron oxide.

[0024] (5) The present invention provides a positive electrode active material in any one of the above (1) to (4), wherein the coating part includes at least one compound selected from the group consisting of lithium cobalt oxide, lithium boron oxide, and lithium cobalt-boron oxide.

[0025] (6) The present invention provides a positive electrode active material in any one of the above (1) to (5), wherein the lithium composite transition metal oxide has a composition represented by the following chemical formula 1.

[0026] [Chemical Formula 1]

[0027] Li a Ni b Co c Mn d M 1 e O2

[0028] In the above chemical formula 1,

[0029] M 1 is at least one selected from the group consisting of Al, B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,

[0030] 0.9≤a≤1.1, 0.6≤b<1, 0 <c<0.4, 0<d<0.4, 0≤e<0.1이다.

[0031] (7) The present invention provides a positive electrode active material in any one of the above (1) to (6), wherein the first coating part includes a compound having a composition represented by the following chemical formula 2.

[0032] [Chemical Formula 2]

[0033] Li f Co g B h M 2 i M 3 j O2

[0034] In the above chemical formula 2,

[0035] M 2 is at least one selected from the group consisting of Ni and Mn,

[0036] M 3 is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,

[0037] 0.9≤f≤1.1, 0.6≤g<1, 0 <h<0.3, 0<i<0.4, 0≤j<0.1이다.

[0038] (8) The present invention provides a positive electrode active material in any one of the above (1) to (7), wherein the second coating part includes a compound having a composition represented by the following chemical formula 3.

[0039] [Chemical Formula 3]

[0040] Li k Co l B m M 4 n M 5 o O2

[0041] In the above chemical formula 3,

[0042] M 4 is at least one selected from the group consisting of Ni and Mn,

[0043] M 5 is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,

[0044] 0.9≤k≤1.1, 0.6≤l<1, 0 <m<0.3, 0≤n<0.4, 0≤o<0.3이다.

[0045] (9) The present invention provides a positive electrode active material in any one of the above (1) to (8), wherein the first coating part includes a compound having a composition represented by the following chemical formula 2, and the second coating part includes a compound having a composition represented by the following chemical formula 3.

[0046] [Chemical Formula 2]

[0047] Li f Co g B h M 2 i M 3 j O2

[0048] In the above chemical formula 2,

[0049] M 2 is at least one selected from the group consisting of Ni and Mn,

[0050] M 3 is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,

[0051] 0.9≤f≤1.1, 0.6≤g<1, 0 <h<0.3, 0<i<0.4, 0≤j<0.1이고,

[0052] [Chemical Formula 3]

[0053] Li k Co l B mM 4 n M 5 o O2

[0054] In the above chemical formula 3,

[0055] M 4 is at least one selected from the group consisting of Ni and Mn,

[0056] M 5 is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,

[0057] 0.9≤k≤1.1, 0.6≤l<1, 0 <m<0.3, 0≤n<0.4, 0≤o<0.3이다.

[0058] (10) The present invention provides a positive electrode active material in any one of the above (1) to (9), wherein the total area of ​​the coating portion is 10% or more and 100% or less of the total surface area of ​​the lithium composite transition metal oxide.

[0059] (11) The present invention provides a positive electrode comprising a positive electrode active material according to any one of (1) to (10).

[0060] (12) The present invention provides a lithium secondary battery comprising a positive electrode according to (11); a negative electrode; a separator interposed between the positive electrode and the negative electrode; and an electrolyte.

[0061]

[0062] The cathode active material of the present invention comprises a lithium composite transition metal oxide in the form of a single particle; and a coating portion formed on the lithium composite transition metal oxide and including an amorphous lithium compound; wherein the coating portion comprises a first coating portion; And a second coating portion; wherein the first coating portion is in the form of an island formed discontinuously, and the second coating portion is in the form of a coating layer formed continuously, and the first coating portion and the second coating portion each independently include boron (B) and cobalt (Co), and optionally include one or more coating elements selected from the group consisting of Co, Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, thereby reducing the elution of lithium ions from the positive electrode active material by forming the amorphous lithium compound, suppressing side reactions with the electrolyte, and preventing an increase in pH of the slurry due to lithium byproducts, thereby suppressing gelation.

[0063]

[0064] Figure 1 is a SEM image of the positive electrode active material manufactured in Example 1.

[0065] Figure 2 is a SEM image of the positive electrode active material manufactured in Example 2.

[0066] Figure 3 is a SEM image of the positive electrode active material manufactured in Example 3.

[0067] Figure 4 is an SEM image of the positive electrode active material manufactured in Comparative Example 1.

[0068] Figure 5 is an SEM image of the positive electrode active material manufactured in Comparative Example 2.

[0069] Fig. 6(A) is an EPMA analysis image of the positive electrode active material manufactured in Example 1, Fig. 6(B) is an EPMA analysis image of the positive electrode active material manufactured in Example 2, and Fig. 6(C) is an EPMA analysis image of the positive electrode active material manufactured in Example 3.

[0070] Fig. 7(A) is a TEM image of a cross-section of a positive electrode active material manufactured in Example 1, and Fig. 7(B) is a TEM image of a cross-section of a positive electrode active material manufactured in Example 2.

[0071]

[0072] Hereinafter, the present invention will be described in more detail to help understand the present invention.

[0073] The terms or words used in the description and claims of the present invention should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.

[0074] In the present invention, the term 'primary particle' means the smallest particle unit that can be distinguished as a single lump when observing the cross-section of a positive electrode active material through a scanning electron microscope (SEM), and may be composed of multiple crystal grains.

[0075] In the present invention, the term "secondary particle" refers to a secondary structure formed by the aggregation of multiple primary particles. The average particle diameter of the secondary particles can be measured using a particle size analyzer.

[0076] In this specification, the term 'single particle form' is a concept that is contrasted with the spherical secondary particle form formed by agglomeration of tens to hundreds of primary particles manufactured by a conventional method, and means a form formed of 50 or fewer primary particles. Specifically, in the present invention, the single particle form may be a single particle formed of one primary particle, or may be a secondary particle form formed by agglomeration of 2 or more, 3 or more, 4 or more, 5 or more, 10 or more, and 30 or less, 35 or less, 40 or less, 45 or less, or 50 or less primary particles.

[0077] In the present invention, the term 'average particle diameter (D50 )' means the particle size at the 50% point of the volume cumulative distribution according to particle size. The above average particle size is calculated by dispersing the powder to be measured in a dispersion medium, introducing it into a commercially available laser diffraction particle size measuring device (e.g., S3500 from Microtrac), and measuring the difference in diffraction pattern according to particle size when the particles pass through the laser beam to calculate the particle size distribution, and calculating the particle diameter at the point where it becomes 50% of the volume cumulative distribution according to particle size in the measuring device, thereby obtaining D 50 can be measured.

[0078]

[0079] positive electrode active material

[0080]

[0081] Hereinafter, the positive electrode active material of the present invention will be described.

[0082]

[0083] The cathode active material of the present invention comprises a lithium composite transition metal oxide in the form of a single particle; and a coating portion formed on the lithium composite transition metal oxide and including an amorphous lithium compound; wherein the coating portion comprises a first coating portion; and a second coating portion; wherein the first coating portion has an island shape formed discontinuously, and the second coating portion has a coating layer shape formed continuously, and the first coating portion and the second coating portion each independently include boron (B) and cobalt (Co), and optionally include one or more coating elements selected from the group consisting of Co, Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La, and Hf.

[0084]

[0085] The lithium composite transition metal oxide is in the form of a single particle composed of 50 or fewer primary particles. That is, the lithium composite transition metal oxide is in the form of a single particle or a single particle composed of 2 or more and 50 or fewer particles. Specifically, it may be in the form of 2 or more and 40 or fewer, 2 or more and 30 or fewer, 2 or more and 20 or fewer, or 2 or more and 10 or fewer primary particles, and preferably 2 or more and 10 or fewer. The single particle form is distinguished from secondary particles composed of more than 50 primary particles aggregated.

[0086] When the lithium composite transition metal oxide is in the form of a single particle, the stability is excellent, so that when the positive electrode active material containing it is rolled, the positive electrode active material is less likely to break or crack, thereby reducing side reactions between the positive electrode active material and the electrolyte. This improves the durability against volume changes during charge and discharge of the battery, thereby improving the life characteristics. On the other hand, the secondary particle lithium composite transition metal oxide is prone to particle breakage during the electrode rolling process, which increases the surface area of ​​the positive electrode active material, thereby worsening the storage and life performance at high temperatures. In particular, in the case of a lithium composite transition metal oxide containing a high nickel content, the problem of particle breakage occurring during rolling for the manufacture of the positive electrode is further increased, and in this case, side reactions between the lithium composite transition metal oxide and the electrolyte may increase, and the physical properties of the battery may deteriorate.

[0087]

[0088] The lithium composite transition metal oxide may have a layered (R-3m) structure, and may have a high NiO content before the coating is formed on the lithium composite transition metal oxide. Since the formation of NiO is induced by the high sintering temperature required during the production of the lithium composite transition metal oxide, the lithium composite transition metal oxide may have a high NiO content on the surface, and the NiO has the problem of lowering the energy density of the battery and deteriorating the resistance characteristics and output characteristics.

[0089] The present invention has the effect of reducing side reactions between a positive electrode active material and an electrolyte by including a coating portion, and reducing the NiO content in the positive electrode active material. In addition, by including boron (B) and cobalt (Co) in the first coating portion and the second coating portion, the density of the positive electrode active material is reduced, thereby improving the dispersibility of the positive electrode active material when preparing a positive electrode slurry. In addition, when the prepared positive electrode slurry is stored, the precipitation of positive electrode active material particles within the positive electrode slurry over time is reduced, thereby reducing gelation, i.e., the phenomenon of aggregation between particles as the positive electrode active material particles precipitate downward within the positive electrode slurry. On the other hand, when the lithium composite transition metal oxide does not include a coating portion, there is a problem of poor life characteristics due to a side reaction between the positive electrode active material and the electrolyte, and when the first coating portion and the second coating portion do not include boron and cobalt, there is an excessive presence of lithium byproducts, and the dispersibility of the positive electrode active material is poor, so there is a problem of excessive gelation occurring when manufacturing the positive electrode slurry.

[0090]

[0091] According to one embodiment of the present invention, the positive electrode active material may have a sequential phase gradient from an amorphous structure to a spinel structure and a layered structure in a center-to-surface direction. Specifically, the amorphous structure may include lithium boron oxide, the spinel structure may include lithium cobalt oxide, and the like, and the layered structure may include lithium cobalt oxide, nickel cobalt manganese aluminum oxide, and the like.

[0092]

[0093] According to one embodiment of the present invention, the first coating portion may be dispersed and distributed on at least one of the surface of the lithium composite transition metal oxide and the surface of the second coating portion. The term "dispersed and distributed" refers to a form in which the first coating portion is formed by dot-wise dispersion rather than being formed in a continuous, connected manner. In this case, the first coating portion has the effect of improving capacity characteristics and lifespan characteristics, etc., without acting as a resistor.

[0094]

[0095] According to one embodiment of the present invention, the amorphous lithium compound may include lithium boron oxide. In this case, the density of the positive electrode active material is reduced, thereby improving the dispersibility of the positive electrode active material when preparing the positive electrode slurry. In addition, when the prepared positive electrode slurry is stored, the precipitation of positive electrode active material particles within the positive electrode slurry over time is reduced, thereby reducing gelation, i.e., the phenomenon of aggregation between particles as the positive electrode active material particles precipitate downward within the positive electrode slurry.

[0096]

[0097] According to one embodiment of the present invention, the coating portion may include one or more compounds selected from the group consisting of lithium cobalt oxide, lithium boron oxide, and lithium cobalt-boron oxide. In this case, lithium byproducts on the surface of the positive electrode active material are reduced, the dispersibility of the positive electrode active material is improved, and gelation is suppressed during the preparation of the positive electrode slurry.

[0098]

[0099] According to one embodiment of the present invention, the lithium composite transition metal oxide may have a composition represented by the following chemical formula 1.

[0100] [Chemical Formula 1]

[0101] Li a Ni b Co c Mn d M 1 e O2

[0102] In the above chemical formula 1,

[0103] M 1 is at least one selected from the group consisting of Al, B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,

[0104] 0.9≤a≤1.1, 0.6≤b<1, 0 <c<0.4, 0<d<0.4, 0≤e<0.1이다.

[0105] In the above chemical formula 1,

[0106] Above M 1 is a doping element, specifically, the above M 1 is at least one selected from the group consisting of Al, B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf. The above M 1Although not essential, it can improve capacity characteristics and life characteristics.

[0107] The above a may be 0.9 or greater, or 1.0 or greater, and 1.1 or less. When l satisfies the above range, high safety and high energy density per unit volume can be achieved.

[0108] The above b is the molar ratio of nickel (Ni) among all metals excluding lithium in the lithium complex transition metal compound, and may be 0.6 or more, 0.7 or more, 0.8 or more, or 0.9 or more, and may be 0.96 or less, 0.97 or less, 0.98 or less, 0.99 or less, or less than 1. When b satisfies the above range, high-energy characteristics can be implemented.

[0109] The above c is the molar ratio of cobalt (Co) among all metals excluding lithium in the lithium complex transition metal compound, and may be greater than 0, 0.01 or more, or 0.02 or more, and may be 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, 0.1 or less, 0.11 or less, 0.12 or less, 0.13 or less, 0.14 or less, 0.15 or less, 0.16 or less, 0.17 or less, 0.18 or less, 0.19 or less, 0.2 or less, 0.21 or less, 0.22 or less, 0.23 or less, 0.24 or less, 0.25 or less, 0.26 or less, 0.27 or less, 0.28 or less, 0.29 or less, 0.3 or less, It may be 0.31 or less, 0.32 or less, 0.33 or less, 0.34 or less, 0.35 or less, 0.36 or less, 0.37 or less, 0.38 or less, 0.39 or less, or less than 0.4. When c satisfies the above range, stability can be improved during the charge and discharge process, and rate characteristics can be enhanced.

[0110] The above d is the molar ratio of manganese (Mn) among all metals excluding lithium in the lithium complex transition metal compound, and may be greater than 0, 0.01 or more, or 0.02 or more, and may be 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, 0.1 or less, 0.11 or less, 0.12 or less, 0.13 or less, 0.14 or less, 0.15 or less, 0.16 or less, 0.17 or less, 0.18 or less, 0.19 or less, 0.2 or less, 0.21 or less, 0.22 or less, 0.23 or less, 0.24 or less, 0.25 or less, 0.26 or less, 0.27 or less, 0.28 or less, 0.29 or less, 0.3 or less, 0.31 or less, 0.32 or less, 0.33 or less, 0.34 or less, 0.35 or less, 0.36 or less, 0.37 or less, 0.38 or less, 0.39 or less, or less than 0.4. When d satisfies the above range, high temperature stability can be increased, and side reactions with the electrolyte can be relatively reduced.

[0111] The above e is M among all metals except lithium in the lithium complex transition metal compound. 5 In a molar ratio of , e may be 0 or more, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, or 0.05 or more, and may be 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, or less than 1. When e satisfies the above range, the stability of the crystal structure of the positive electrode active material may be improved and the particle shape may be improved.

[0112]

[0113] According to one embodiment of the present invention, the first coating portion may include a compound having a composition represented by the following chemical formula 2.

[0114] [Chemical Formula 2]

[0115] Li f Co g B h M 2i M 3 j O2

[0116] In the above chemical formula 2,

[0117] M 2 is at least one selected from the group consisting of Ni and Mn,

[0118] M 3 is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,

[0119] 0.9≤f≤1.1, 0.6≤g<1, 0 <h<0.3, 0<i<0.4, 0≤j<0.1이다.

[0120] In the above chemical formula 2, M 2 is at least one selected from the group consisting of Ni and Mn, and M 3 is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta and Hf. The above M 3 Although not essential, it can improve capacity characteristics and life characteristics.

[0121] The above f may be 0.9 or greater, or 1 or greater, and 1.1 or less.

[0122] The above g may be 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more, or less than 1.

[0123] The above h may be greater than 0, greater than or equal to 0.1, or greater than or equal to 0.2, and less than or equal to 0.3.

[0124] The above i may be greater than 0, greater than or equal to 0.1, or greater than or equal to 0.2, and may be less than or equal to 0.3, or less than 0.4.

[0125] The above j may be greater than or equal to 0, less than or equal to 0.05, or less than or equal to 0.1.

[0126] When the above f, g, h, i, and j are within the above ranges, the capacity characteristics, efficiency characteristics, and resistance characteristics of the manufactured battery can be improved.

[0127]

[0128] According to one embodiment of the present invention, the first coating portion may include a lithium cobalt oxide coating portion; a lithium boron oxide coating portion; and a lithium cobalt-boron oxide coating portion positioned between the lithium cobalt oxide coating portion and the lithium boron oxide coating portion. The lithium boron oxide coating portion may include Li2BO3Li2B4O7, and Li x B y O z It may include at least one selected from the group consisting of (1≤x≤2, 1≤y≤4, 2≤z≤4), and the lithium cobalt-boron oxide coating part is LiCoBO3, and LiMg 0.1 Co 0.9 It may include one or more species selected from the group consisting of BO3.

[0129]

[0130] According to one embodiment of the present invention, the first coating portion may have a boron (B) content of 0.1 mol% or more and 1.25 mol% or less among the total metal excluding lithium in the positive electrode active material. Specifically, the boron (B) content may be 0.1 mol% or more, or 0.15 mol% or more, and 1.1 mol% or less, 1.2 mol% or less, or 1.25 mol% or less. When the boron (B) content is within the above range, there is an effect of reducing gelation of the positive electrode slurry due to a decrease in the density of the positive electrode active material, an improvement in the dispersibility of the positive electrode active material, and an increase in sphericity.

[0131]

[0132] According to one embodiment of the present invention, the second coating portion may include a compound having a composition represented by the following chemical formula 3.

[0133] [Chemical Formula 3]

[0134] Li k Co l B m M 4 n M 5 o O2

[0135] In the above chemical formula 3,

[0136] M 4 is at least one selected from the group consisting of Ni and Mn,

[0137] M 5 is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,

[0138] 0.9≤k≤1.1, 0.6≤l<1, 0 <m<0.3, 0≤n<0.4, 0≤o<0.3이다.

[0139] In the above chemical formula 3, M 4 is at least one selected from the group consisting of Ni and Mn, and M 5 is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta and Hf. The above M 5 Although not necessarily included, it can improve capacity characteristics and life characteristics.

[0140] The above k may be 0.9 or greater, or 1 or greater, and 1.1 or less.

[0141] The above l may be 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more, or less than 1.

[0142] The above m may be greater than 0, greater than or equal to 0.1, or greater than or equal to 0.2, and less than or equal to 0.3.

[0143] The above n may be greater than 0, greater than or equal to 0.1, or greater than or equal to 0.2, and may be less than or equal to 0.3, or less than 0.4.

[0144] The above o may be 0 or greater, and 0.1 or less, 0.2 or less, or 0.3 or less.

[0145] When the above k, l, m, n, and o are within the above ranges, the capacity characteristics, efficiency characteristics, and resistance characteristics of the manufactured battery can be improved.

[0146]

[0147] According to one embodiment of the present invention, the first coating portion may include a compound having a composition represented by the chemical formula 2, and the second coating portion may include a compound having a composition represented by the chemical formula 3.

[0148]

[0149] In this specification, the surface refers to the outermost layer of the lithium composite transition metal oxide. In addition, a region having a constant thickness from the outermost layer of the lithium composite transition metal oxide toward the center may be referred to as a surface portion. The surface portion may be a region having a depth of 1 nm to 50 nm, specifically 5 nm to 30 nm, from the outermost layer of the lithium composite transition metal oxide toward the center. In contrast to the surface portion, the interior of the lithium composite transition metal oxide excluding the surface portion may be referred to as a core.

[0150]

[0151] The surface of the above lithium composite transition metal oxide may be doped with cobalt, boron, or cobalt and boron diffused from the coating portion.

[0152]

[0153] The coating portion may be formed on the outermost surface of the lithium composite transition metal oxide, and the coating portion may be formed on part or all of the outer surface.

[0154] According to one embodiment of the present invention, the coating portion may have a total area of ​​10% or more and 100% or less of the total surface area of ​​the lithium composite transition metal oxide. Specifically, the coating portion may have a total area of ​​10% or more, 15% or more, 20% or more, 25% or more, 30% or more, 35% or more, 40% or more, 45% or more, or 50% or more of the total surface area of ​​the lithium composite transition metal oxide, and may have a total area of ​​55% or less, 60% or less, 65% or less, 70% or less, 75% or less, 80% or less, 90% or less, 95% or less, or 100% or less. When the total area of ​​the coating portion is within the above range, it is possible to prevent a side reaction between the positive electrode active material and the electrolyte without acting as a resistor, and there is an effect of improving the life characteristics and capacity characteristics of the battery.

[0155]

[0156] According to one embodiment of the present invention, the first coating portion and the second coating portion may have the same or different compositions. The content may be a comparison of the contents of the first coating portion and the second coating portion belonging to an area twice the diameter of the first coating portion centered on the first coating portion. If the compositions are different, the contents of coating elements excluding B and Co may be different, and the content of coating elements excluding B and Co in the first coating portion may be higher than the content of coating elements excluding B and Co in the second coating portion.

[0157]

[0158] Method for manufacturing positive electrode active material

[0159] Next, a method for manufacturing the positive electrode active material of the present invention will be described. The method for manufacturing the positive electrode active material of the present invention is a method for manufacturing the positive electrode active material according to the present invention.

[0160]

[0161] The cathode active material according to the present invention comprises: (1) a step of mixing a lithium composite transition metal oxide in the form of a single particle and a cobalt-containing raw material, and optionally mixing a coating element-containing raw material to prepare a mixture; (2) a step of firing the mixture to prepare a sintered product; and (3) a step of mixing the sintered product and a boron-containing raw material, and heat-treating the mixture to form a coating portion including cobalt (Co) and boron (B) on the lithium composite transition metal oxide; wherein the coating element is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La, and Hf, and the firing may be performed at a temperature of 600°C or more and 800°C or less.

[0162]

[0163] The cathode active material according to the present invention described above can be manufactured by appropriately controlling the type of raw material, the mixing ratio of raw materials, the heat treatment step, the heat treatment temperature, the heat treatment heating rate, the heat treatment atmosphere, etc.

[0164]

[0165] Hereinafter, each step of the present invention will be described in detail.

[0166]

[0167] (1) Step

[0168] The present invention includes a step (1) of preparing a mixture by mixing a lithium composite transition metal oxide in the form of single particles and a cobalt-containing raw material, and optionally mixing a coating element-containing raw material.

[0169]

[0170] The mixture of the present invention is a lithium composite transition metal oxide mixture of the present invention, which is mixed by a dry mixing method using a solid raw material mixture. The dry mixing method has the advantage of being able to be mass-produced through a relatively simple synthesis process.

[0171]

[0172] According to one embodiment of the present invention, the cobalt-containing raw material may be mixed in an amount of 0.1 mol% to 10 mol%, specifically 0.5 mol% to 5 mol%, and more specifically 1 mol% to 3 mol%, with respect to the lithium composite transition metal oxide. When the cobalt raw material is mixed within the above range, a coating portion including cobalt can be sufficiently formed on the lithium composite transition metal oxide without unreacted cobalt compounds remaining on the particle surface.

[0173]

[0174] The above cobalt-containing raw material may be an oxide, hydroxide, oxyhydroxide, carbonate, sulfate, halide, sulfide, acetate, nitrate, carboxylate, or a combination thereof containing cobalt, and examples thereof include Co(OH)2, CoOOH, Co(OCOCH3)2ㆍ4H2O, Co(NO3)2ㆍ6H2O, or Co(SO4)2ㆍ7H2O, and any one of these or a mixture of two or more thereof may be used, and specifically, Co(OH)2 may be used.

[0175]

[0176] The coating element is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf. The coating element-containing raw material may be, for example, an oxide, a hydroxide, an oxyhydroxide, a carbonate, a sulfate, a halide, a sulfide, an acetate, a nitrate, a carboxylate or a combination thereof containing the coating element, and specifically, Co(OH)2, ZrO2, Zr(OH)4, ZnO, TiO2, WO3, Al2O3, Al(OH)3, Al2(SO4)3,·xH2O, AlCl3, C2H5O4Al, Al-isopropoxide, Al(NO3)3, AlF, Li3WO4, (NH4) 10 W 12 O 41 ㆍ5H2O, or NH4H2PO4, etc., but are not limited thereto.

[0177]

[0178] According to one embodiment of the present invention, the coating element-containing raw material may be used in an amount such that the coating element is 0.001 mol% to 10 mol%, specifically 0.005 mol% to 5 mol%, based on the total metal moles of the lithium composite transition metal oxide. When the mixing amount of the coating element-containing raw material is within the above range, the effect of effectively suppressing side reactions with the electrolyte can be expected, and the electrochemical characteristics can be further improved.

[0179]

[0180] According to one embodiment of the present invention, the lithium composite transition metal oxide in the form of a single particle may be manufactured by a method including: (A) mixing a composite transition metal hydroxide containing nickel, cobalt, and manganese and a first lithium-containing raw material, and first firing the mixture at a temperature of 800°C or more and 950°C or less to produce a first fired product; and (B) second firing the first fired product at a temperature of 680°C or more and 850°C or less to produce a second fired product.

[0181] Specifically, the first calcination may be performed at a temperature of 800°C or higher, or 820°C or higher, and 850°C or lower, 900°C or lower, or 950°C or lower, and the second calcination may be performed at a temperature of 680°C or higher, 700°C or higher, or 720°C or higher, and 750°C or lower, 760°C or lower, 770°C or lower, 780°C or lower, 790°C or lower, 800°C or lower, 810°C or lower, 820°C or lower, 830°C or lower, 840°C or lower, or 850°C or lower. When the first calcination is performed within the above temperature range, sufficient energy required for single particle formation can be supplied, and when the second calcination is performed within the above range, the crystallinity of the lithium composite transition metal oxide can be increased.

[0182]

[0183] The above first calcination may be performed under an oxygen atmosphere in order to prevent the lithium composite transition metal oxide from degenerating into a rock salt structure.

[0184] The above primary firing may be performed for 3 hours or more, 4 hours or more, 5 hours or more, or 6 hours or more, and 9 hours or less, 10 hours or less, 11 hours or less, or 12 hours or less, in order to agglomerate primary particles and improve the crystallinity of the primary fired product.

[0185]

[0186] The above secondary calcination may be performed under an oxygen atmosphere in order to prevent the lithium composite transition metal oxide from degenerating into a rock salt structure.

[0187] The above secondary firing may be performed for 3 hours or more, and 9 hours or less, 10 hours or less, 11 hours or less, or 12 hours or less, in order to increase the crystallinity of the internal crystal structure of the positive electrode active material.

[0188]

[0189] According to one embodiment of the present invention, immediately after step (A), a step (A1) of crushing the primary sintered product may be further included. In this case, by controlling the particle size, the process efficiency and the quality of the positive electrode active material can be improved. In order to prevent the initial resistance from increasing, the primary sintered product may be crushed to an average particle size (D 50 ) may be ground to a size of 3 ㎛ to 20 ㎛.

[0190]

[0191] The grinding in the above step (A1) can be performed using a pin mill, an ACM, a jet mill, etc. Meanwhile, the pin mill can be performed under conditions of 18,000 rpm, the ACM can be performed under conditions of 6,000 rpm for classification and 12,000 rpm for main processing using a device from Hosokawa, and the jet mill can be performed under conditions of 6 bar for grinding pressure and 3,500 rpm for classification using a device from ZM solution. In this case, the desired average particle size (D 50 ) can be easily obtained.

[0192]

[0193] (2) Step

[0194] Thereafter, a step (2) of firing the mixture to produce a fired product is included.

[0195] The above firing is performed at a temperature of 500°C or higher and 800°C or lower. Specifically, the above firing is performed at a temperature of 500°C or higher, 550°C or higher, 600°C or higher, 650°C or higher, or 700°C or higher, and 750°C or lower, or 800°C or lower. When the above-mentioned firing temperature satisfies the above-mentioned range, during the heating process for firing, a coating portion including cobalt on a lithium composite transition metal oxide, specifically, a discontinuous island shape is formed on the surface of the lithium composite transition metal oxide, so that cobalt existing in the LiCoO2 phase can penetrate into the lithium composite transition metal oxide to an appropriate depth to appropriately change the NiO layer, which is a degenerate layer, into a nickel cobalt manganese (NCM) oxide layer structure, and accordingly, the surface portion of the lithium composite transition metal oxide has a layered (R-3m) structure, and an oxidation number gradient layer in which the oxidation number of nickel increases in the outermost direction is included in the surface portion, so that excellent effects can be exhibited in cell performance such as charge / discharge capacity, initial efficiency, and initial resistance. On the other hand, when the firing temperature is less than 500°C, the thickness of the coating portion becomes thick and the coating portion is formed too much, making it difficult to achieve the advantage of forming the coating portion as described above, and when the firing temperature exceeds 800°C, cobalt may be deeply doped into the lithium composite transition metal oxide, preventing the coating portion from being properly formed on the surface.

[0196]

[0197] The above firing can be performed for 2 hours or more, and 6 hours or less, 9 hours or less, or 12 hours or less. If the above firing is performed within the above time range, excellent productivity can be achieved, and uniform firing can be achieved.

[0198]

[0199] According to one embodiment of the present invention, when step (2) is performed, a coating portion including Co can be formed on a lithium composite transition metal oxide, and specifically, a second coating portion represented by chemical formula 1 or 2 described herein can be formed.

[0200]

[0201] (3) Step

[0202] (3) step of mixing the above-mentioned sintered product and a boron-containing raw material and performing heat treatment to form a coating portion including cobalt (Co) and boron (B) on the lithium composite transition metal oxide;

[0203]

[0204] The above boron-containing raw material may be an oxide, hydroxide, oxyhydroxide, carbonate, sulfate, halide, sulfide, acetate, nitrate, carboxylate, or a combination thereof containing boron, and examples thereof include, but are not limited to, B(OH)3, H2BO3, HBO2, H3BO3, H2B4O7, B2O3, C6H5B(OH)2, (C6H5O)3B, [(CH3(CH2)3O)3B, C3H9B3O6, (C3H7O3)B, etc.

[0205]

[0206] According to one embodiment of the present invention, the boron-containing raw material may be mixed so that the boron-containing raw material is present in an amount of 0.15 mol% to 1.25 mol%, specifically 0.20 mol% to 1.10 mol%, and more specifically 0.25 to 1.05 mol% with respect to the sintered product. When the mixing amount of the boron-containing raw material is within the above range, the boron content of the formed coating portion can satisfy the appropriate range.

[0207]

[0208] According to one embodiment of the present invention, the heat treatment may be performed at a temperature of 200°C or higher, 250°C or higher, or 300°C or higher, and 350°C or lower, 400°C or lower, 420°C or lower, 440°C or lower, 460°C or lower, 480°C or lower, or 500°C or lower. When the heat treatment temperature satisfies the above range, the boron-containing raw material can appropriately form an amorphous boron coating portion rather than boron oxide. When the heat treatment temperature is excessively high, boron oxide may be formed on the surface of the lithium composite transition metal oxide, thereby deteriorating the properties as a positive electrode active material, and when the heat treatment temperature is excessively low, the coating portion may not be appropriately formed.

[0209]

[0210] The above heat treatment may be performed for 2 hours or more, or 3 hours or more, and 6 hours or less, 7 hours or less, 8 hours or less, 9 hours or less, 10 hours or less, 11 hours or less, or 12 hours or less. If the above heat treatment is performed within the above time range, excellent productivity can be exhibited, and uniform sintering can be achieved.

[0211]

[0212] According to one embodiment of the present invention, when step (3) is performed, a coating portion including B can be formed on a lithium composite transition metal oxide, and specifically, a first coating portion represented by chemical formula 2 described herein or a second coating portion represented by chemical formula 3 can be formed.

[0213]

[0214] According to one embodiment of the present invention, in steps (1) to (3), cobalt, boron, or cobalt and boron may diffuse toward the center from the surface of the lithium composite transition metal oxide, thereby forming a coating portion.

[0215]

[0216] According to another embodiment of the present invention, a positive electrode comprising the above-described positive electrode active material is provided.

[0217] Specifically, the positive electrode includes a positive electrode current collector, and a positive electrode active material layer formed on the positive electrode current collector and including the positive electrode active material described above.

[0218] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesive strength of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.

[0219] The above positive electrode active material layer may include a conductive material and a binder together with the positive electrode active material described above.

[0220] At this time, the conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskey such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like, and one type alone or a mixture of two or more types thereof may be used. The conductive material may typically be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.

[0221] The above binder serves to improve the adhesion between positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.

[0222] The above-mentioned positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the above-mentioned positive electrode active material is used. Specifically, the positive electrode active material layer forming composition, which is manufactured by mixing or dispersing the above-mentioned positive electrode active material and optionally a binder and a conductive agent in a solvent, is applied onto a positive electrode current collector, followed by drying and rolling. At this time, the types and contents of the positive electrode active material, binder, and conductive agent are as described above.

[0223] The solvent may be a solvent generally used in the relevant technical field, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.

[0224] Additionally, in another method, the positive electrode may be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the resulting film on a positive electrode current collector by peeling it off from the support.

[0225] According to another example of the present invention, an electrochemical device including the positive electrode is provided. The electrochemical device may be, specifically, a battery, a capacitor, or the like, and more specifically, a lithium secondary battery.

[0226] The lithium secondary battery specifically includes a positive electrode, a negative electrode positioned opposite the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode is as described above. In addition, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0227] In the above lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.

[0228] The above negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0229] The above negative electrode active material layer optionally includes a binder and a conductive material together with the negative electrode active material.

[0230] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; SiO x(0 < x < 2), SnO2, vanadium oxide, lithium vanadium oxide, and other metal oxides capable of doping and dedoping lithium; or composites containing the above metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.

[0231] Additionally, the binder and conductive material may be the same as those described above for the positive electrode.

[0232] The above-described negative electrode active material layer may be manufactured by, for example, applying a negative electrode forming composition prepared by dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, onto a negative electrode current collector and drying the coating, or by casting the negative electrode forming composition onto a separate support and then laminating the resulting film onto a negative electrode current collector by peeling it off from the support.

[0233] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used as a separator in lithium secondary batteries can be used without special restrictions, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture retention capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. can also be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength can be used, and can optionally be used in a single-layer or multi-layer structure.

[0234] In addition, examples of the electrolyte used in the present invention include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.

[0235] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0236] As the organic solvent, any solvent that can serve as a medium through which ions involved in the electrochemical reaction of the battery can move may be used without particular limitation. Specifically, the organic solvent includes ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); Alcohol solvents such as ethyl alcohol, isopropyl alcohol, etc.; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched, or cyclic hydrocarbon group, which may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, carbonate solvents are preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.

[0237] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2. LiCl, LiI, or LiB(C2O4)2. It is preferable that the concentration of the lithium salt be used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.

[0238] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 wt% based on the total weight of the electrolyte.

[0239] As described above, a lithium secondary battery including a cathode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0240] Accordingly, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.

[0241] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0242] There is no particular limitation on the external shape of the lithium secondary battery of the present invention, but it may be a cylindrical shape using a can, a square shape, a pouch shape, or a coin shape.

[0243] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but can also be preferably used as a unit battery in a medium- to large-sized battery module including a plurality of battery cells.

[0244]

[0245] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0246]

[0247] Manufacturing example

[0248] Manufacturing Example 1

[0249] Complex transition metal hydroxide [Composition: Ni 0.95 Co 0.03 Mn 0.02 (OH)2, average particle size (D) 50 ) 3.5 ㎛] and LiOH were mixed so that the molar ratio of (Ni+Co+Mn):Li was 1:1.05, and the first fired product was manufactured by first firing at 820°C for 6 hours under an oxygen atmosphere, and then the first fired product was crushed and second fired at 750°C for 9 hours under an oxygen atmosphere to obtain single particle form, LiNi 0.95 Co 0.03 Mn 0.02 A lithium composite transition metal oxide having a composition represented by O2 was prepared.

[0250]

[0251] Examples and Comparative Examples

[0252] Example 1

[0253] The lithium composite transition metal oxide manufactured in Manufacturing Example 1 and powder-type Co(OH)2 (Hwayou Cobalt Co.) were charged into a reactor so that the molar ratio of lithium composite transition metal oxide and Co(OH)2 was 97.82:2.18, and a mixture was prepared by dry mixing using an acoustic mixer. The mixture was calcined at 700°C for 5 hours to obtain a calcined product in a cake state, which was then pulverized to prepare a calcined product in a powder form.

[0254] The above powder-type sintered product and B(OH)3 were added so that the molar ratio of the sintered product and B(OH)3 was 99.55:0.45, and dry-mixed using an acoustic mixer, followed by heat treatment at 300°C for 5 hours to obtain a cake-like positive electrode active material, which was then pulverized to produce a powder-type positive electrode active material. The above positive electrode active material is a coating portion including cobalt and boron formed on a lithium composite transition metal oxide in the form of a single particle, and has an average particle diameter (D50 ) is 3.8 ㎛.

[0255]

[0256] Example 2

[0257] In a reactor, lithium composite transition metal oxides, powder-form Co(OH)2 (Hwayou Cobalt Co., Ltd.) and Al(OH)3 manufactured in Manufacturing Example 1 were charged so that the molar ratio of lithium composite transition metal oxides, Co(OH)2 and Al(OH)3 was 97.72:2.18:0.1, and a mixture was prepared by dry mixing using an acoustic mixer. The mixture was calcined at 700°C for 5 hours to obtain a calcined product in a cake state, which was then pulverized to prepare a calcined product in a powder state.

[0258] The above powder-type sintered product and B(OH)3 were added so that the molar ratio of the sintered product and B(OH)3 was 99.37:0.63, and dry-mixed using an acoustic mixer, followed by heat treatment at 300°C for 5 hours to obtain a cake-like positive electrode active material, which was then pulverized to manufacture a powder-type positive electrode active material. The above positive electrode active material is a coating portion including cobalt and boron formed on a lithium composite transition metal oxide in the form of a single particle, and has an average particle diameter (D 50 ) is 3.9 ㎛.

[0259]

[0260] Example 3

[0261] In a reactor, lithium composite transition metal oxides, powder-form Co(OH)2 (Hwayou Cobalt Co., Ltd.) and Al(OH)3 manufactured in Manufacturing Example 1 were charged so that the molar ratio of lithium composite transition metal oxides, Co(OH)2 and Al(OH)3 was 97.4:2.5:0.1, and a mixture was prepared by dry mixing using an acoustic mixer. The mixture was calcined at 720°C for 5 hours to obtain a calcined product in a cake state, which was then pulverized to prepare a calcined product in a powder form.

[0262] The above powder-type sintered product and B(OH)3 were added so that the molar ratio of the sintered product and B(OH)3 was 99.55:0.45, and dry-mixed using an acoustic mixer, followed by heat treatment at 330°C for 5 hours to obtain a cake-like positive electrode active material, which was then pulverized to manufacture a powder-type positive electrode active material. The above positive electrode active material is a coating portion including cobalt and boron formed on a lithium composite transition metal oxide in the form of a single particle, and has an average particle diameter (D 50 ) is 3.9 ㎛.

[0263]

[0264] Comparative Example 1

[0265] The lithium composite transition metal oxide manufactured in Manufacturing Example 1 and Co(OH)2 in powder form (Hwayou Cobalt Co.) were charged into a reactor so that the molar ratio of the lithium composite transition metal oxide and Co(OH)2 was 97.82:2.18, and a mixture was prepared by dry mixing using an acoustic mixer. The mixture was calcined at 820°C for 5 hours to obtain a calcined product in a cake state, which was then pulverized to prepare a calcined product in a powder form.

[0266] The above powder-type sintered product and B(OH)3 were added so that the molar ratio of the sintered product and B(OH)3 was 99.1:0.9, and dry-mixed using an acoustic mixer, followed by heat treatment at 300°C for 5 hours to obtain a cake-like positive electrode active material, which was then pulverized to manufacture a powder-type positive electrode active material. The above positive electrode active material is a coating portion including cobalt and boron formed on a lithium composite transition metal oxide in the form of a single particle, and has an average particle diameter (D 50 ) is 3.8 ㎛.

[0267]

[0268] Comparative Example 2

[0269] The lithium composite transition metal oxide and Al(OH)3 prepared in Manufacturing Example 1 were charged into a reactor so that the molar ratio of the lithium composite transition metal oxide and Al(OH)3 was 98.1:1.9, and a mixture was prepared by dry mixing using an acoustic mixer. The mixture was calcined at 500°C for 5 hours to obtain a sintered product in a cake state, which was then pulverized to prepare a sintered product in a powder form.

[0270] The above powder-type sintered product and B(OH)3 were added so that the molar ratio of the sintered product and B(OH)3 was 99.37:0.63, and dry-mixed using an acoustic mixer, followed by heat treatment at 300°C for 5 hours to obtain a cake-like positive electrode active material, which was then pulverized to manufacture a powder-type positive electrode active material. The above positive electrode active material is a coating portion including aluminum and boron formed on a lithium composite transition metal oxide in the form of a single particle, and has an average particle diameter (D 50 ) is 3.9 ㎛.

[0271]

[0272] Experimental example

[0273] Experimental Example 1: SEM Image Analysis

[0274] Using a scanning electron microscope (JEOL, JSM-7610F), SEM images of each positive electrode active material manufactured in the examples and comparative examples were taken, and these images are shown in Figures 1 to 5.

[0275] Figure 1 is a SEM image of the positive electrode active material manufactured in Example 1.

[0276] Figure 2 is a SEM image of the positive electrode active material manufactured in Example 2.

[0277] Figure 3 is a SEM image of the positive electrode active material manufactured in Example 3.

[0278] Figure 4 is an SEM image of the positive electrode active material manufactured in Comparative Example 1.

[0279] Figure 5 is an SEM image of the positive electrode active material manufactured in Comparative Example 2.

[0280]

[0281] Through Figures 1 to 3, it was confirmed that the positive electrode active material manufactured in the example was in the form of a single particle.

[0282] In FIGS. 1 to 3 and 5, the uneven and uneven portions, i.e., the uneven portions, are portions where the coating portion exists. Through FIGS. 1 to 3, it was confirmed that the positive electrode active material manufactured in the examples includes a first coating portion in the form of a discontinuously formed island. On the other hand, FIG. 4 confirmed that there are no uneven portions, i.e., it does not include the first coating portion.

[0283]

[0284] Experimental Example 2: EPMA Image Analysis

[0285] EPMA cross-sectional analysis was performed to confirm the surface coating characteristics of the positive electrode active materials manufactured in the examples. First, the positive electrode slurry was prepared by mixing the positive electrode active materials manufactured in Examples 1 to 3, carbon black conductive agent, and PVDF binder in a weight ratio of 95:2:3 in N-methylpyrrolidone (NMP) solvent. The prepared positive electrode slurry was applied to one surface of an aluminum current collector, dried at 130°C, and rolled to an electrode porosity of 20% to prepare a positive electrode. In order to create a flat surface for EPMA cross-sectional analysis, the positive electrode was subjected to Ar-ion milling using a HITACHI IM-5000 equipment at an acceleration voltage of 6 kV to obtain a cross-section of the positive electrode sample. Then, the cross-sectional image of the positive electrode sample was observed using a JEOL JXA-iHP200F equipment at an acceleration voltage of 15 kV and a probe current of 50 nA, and the results are shown in Fig. 6.

[0286]

[0287] Fig. 6(A) is an EPMA analysis image of the positive electrode active material manufactured in Example 1, Fig. 6(B) is an EPMA analysis image of the positive electrode active material manufactured in Example 2, and Fig. 6(C) is an EPMA analysis image of the positive electrode active material manufactured in Example 3.

[0288]

[0289] In the above Fig. 6, the green portion is the portion where the coating layer including Co exists. Through Fig. 6, it was confirmed that the green portion exists continuously, and it was confirmed that it includes a second coating portion in the form of a coating layer continuously formed on a lithium composite transition metal oxide.

[0290]

[0291] Experimental Example 3: TEM-EDS Image Analysis

[0292] Using a transmission electron microscope (TEM) (FEI, Titan cubed G2 60-300), TEM images of the cross-sections of the positive electrode active materials manufactured in the examples and comparative examples were obtained, and the TEM images of the cross-sections of the positive electrode active materials manufactured in examples 1 and 2 are shown in Fig. 7.

[0293]

[0294] Fig. 7(A) is a TEM image of a cross-section of a positive electrode active material manufactured in Example 1, and Fig. 7(B) is a TEM image of a cross-section of a positive electrode active material manufactured in Example 2.

[0295]

[0296] Through FIG. 7, it was confirmed that the positive electrode active materials manufactured in Examples 1 and 2 included a coating portion including an amorphous lithium compound.

[0297]

[0298] Experimental Example 4: XPS Etching Analysis

[0299] The distribution of B and Co on the surface of the coating portion of each of the positive electrode active materials manufactured in the above examples and comparative examples was analyzed using ESCA (K-Alpha, Thermo Fisher Scientific Inc.). The depth profiling conditions were to perform etching at a rate of 0.3 nm / 10 s using an Ar ion source, and the content of boron (B) (atomic%) and cobalt (Co) (atomic%) included in the coating layer with a thickness of 0 to 100 nm were measured, and are shown in Tables 1 and 2 below, respectively.

[0300]

[0301] Etching time (s) Boron (B) content (atomic%) Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2010.111.210.211.110.91010.210.910.111.110.2309.29.88.89.79.25077.37.97.38.11006.56.566.56.22004.44.444.343003.53.83.13.83.85002.83.02.53.13.010001.81.91.21.91.920001.31.611.71.8300011.10.81.01.0

[0302] Etching time (s) Cobalt (Co) content (atomic%) Example 1 Example 2 Example 3 Comparative Example 3 Comparative Example 4 01.20.9 1.31.00 102.5 2.32.7 2.30.13 04.14 5.13 0.15 05.14.9 5.94.10.3 1007.55.37.94.80.2 2008.88 96.20.4 30010.28.9 10.97 1.15 008.88.19.56.81.3 10006.56.17 6.81.5 20004.13.6 5.52.52.13 0003.12.8 32.13.1

[0303] Through Tables 1 and 2, it was confirmed that the coating portion of the positive electrode active material manufactured in Examples 1 to 3 contained boron (B) and cobalt (Co).

[0304]

[0305] Experimental Example 5: Viscosity Analysis of Anode Slurry

[0306] Preparation of cathode slurry

[0307] Each of the positive electrode active materials manufactured in the above examples and comparative examples, carbon black (DENKA, FX35), PVdF (Kureha, KF9709) and BM740H (zeon) as binders were added to a solvent (N-methylpyrrolidone (NMP)) at a weight ratio of 95:2:2.8:0.2, and then stirred at 1,500 rpm for 95 minutes using a homogenizer (homogenizing disper model 2.5, primix) to manufacture a positive electrode slurry.

[0308]

[0309] Measurement of anode slurry viscosity

[0310] After collecting each of the above-mentioned manufactured positive electrode slurries, the viscosity was measured by shearing at 16 rpm for 1 minute using a viscometer (DV2T viscometer, Brookfield Ametek). The viscosity change over time was measured for up to 7 days after the manufacture of the positive electrode slurry, and the results are shown in Table 3 below.

[0311] Slurry viscosity (cP) = shear stress (g / cm·s) / shear rate (1 / s)

[0312]

[0313] Viscosity (cP) Initial After 3 days After 7 days Example 14,800 7,350 9,270 Example 25,100 7,150 9,630 Example 34,920 7,710 9,450 Comparative Example 15,540 - (gelled) - (gelled) Comparative Example 26,500 - (gelled) - (gelled)

[0314] Through Table 3, it was confirmed that the positive electrode slurry containing the positive electrode active materials manufactured in Examples 1 to 3 had lower viscosity at the beginning, after 3 days, and after 7 days compared to the positive electrode slurry containing the positive electrode active materials manufactured in Comparative Examples 1 and 2.

[0315]

[0316] Experimental Example 6: Evaluation of Lithium Byproducts

[0317] For each positive electrode active material manufactured in the above examples and comparative examples, the content of lithium byproduct (lithium byproduct (mol%)) was measured using the Warder titration method, which titrates the amount of OH ions and CO3 ions using an 888 titrando device from Mettler Toledo, and the results are shown in Table 4 below.

[0318]

[0319] Lithium byproduct (mol%) Li2CO3LiOHTotal Example 10.1400.2010.349 Example 20.2590.1700.429 Example 30.1900.1820.372 Comparative Example 10.3500.1310.481 Comparative Example 20.450.5230.973

[0320] Through Table 4, it was confirmed that the positive electrode active materials manufactured in Examples 1 to 3 had a lower content of lithium byproducts compared to the positive electrode active materials including the positive electrode active materials manufactured in Comparative Examples 1 and 2.

[0321]

[0322] Experimental Example 7: Evaluation of Electrochemical Properties

[0323] Each of the positive electrode active materials manufactured in the above examples and comparative examples, carbon black (DENKA, FX35), and PVdF (Kureha, KF9709) and BM740H (zeon) as binders were added to a solvent (N-methylpyrrolidone (NMP)) at a weight ratio of 95:2:2.8:0.2, and then stirred at 1,500 rpm for 95 minutes using a homogenizer (homogenizing disper model 2.5, primix) to manufacture a positive electrode slurry.

[0324] The positive electrode slurry manufactured above was coated on one side of an aluminum foil current collector, dried at 130°C for 3 hours, and then rolled using a roll pressing method to manufacture a positive electrode having a porosity of 20% in the positive electrode layer after rolling.

[0325] An electrode assembly was manufactured by interposing a separator between the positive electrode and the lithium metal disk negative electrode manufactured above, and then positioning it inside a battery case, and then injecting an electrolyte solution in which 1 M LiPF6 was dissolved in an organic solvent of EC / EME / DMC (3:3:4, volume ratio) to manufacture a lithium secondary battery.

[0326] The lithium secondary battery manufactured in this way was charged in CC / CV mode at a constant current (CC) of 0.1 C at 25°C until the voltage reached 4.25 V (end current 0.005 C), then left for 20 minutes and discharged in CC mode at a constant current (CC) of 0.1 C until the voltage reached 2.5 V, and the charge capacity (mAh) and discharge capacity (mAh) were measured, and the percentage of discharge capacity to charge capacity (efficiency (%)) was calculated, and is shown in Table 5 below.

[0327] In addition, the DC internal resistance (DCIR) (Ω) was calculated and shown in Table 5 below. The DCIR is a value calculated by dividing the difference between the voltage at 10 seconds and the initial voltage while discharging with a constant current of 0.2 C during the initial charge and discharge by the applied current.

[0328]

[0329] Charge capacity (mAh / g)Discharge capacity (mAh / g)Efficiency (%)DCIR(Ω)Example 1247.2217.287.922.1Example 2248.3217.987.823.2Example 3247.5217.387.821.2Comparative example 1242.1211.487.327.3Comparative example 2240.3202.584.326.0

[0330] Through Table 5, it was confirmed that the batteries including the positive electrode active materials manufactured in Examples 1 to 3 had superior battery characteristics related to charge / discharge capacity, efficiency, and DCIR compared to the batteries including the positive electrode active materials manufactured in Comparative Examples 1 and 2.

Claims

1. Lithium composite transition metal oxide in single particle form; and A coating portion formed on the above lithium composite transition metal oxide and including an amorphous lithium compound; The above coating portion includes a first coating portion; and a second coating portion; The first coating portion is in the form of an island formed discontinuously, and the second coating portion is in the form of a coating layer formed continuously. A cathode active material, wherein the first coating portion and the second coating portion each independently include boron (B) and cobalt (Co), and optionally include at least one coating element selected from the group consisting of Co, Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La, and Hf.

2. In paragraph 1, A cathode active material having a sequential phase gradient from an amorphous structure to a spinel structure and a layered structure from the surface to the center.

3. In paragraph 1, A positive electrode active material in which the first coating portion is dispersed and distributed on at least one of the surface of the lithium composite transition metal oxide and the surface of the second coating portion.

4. In paragraph 1, The amorphous lithium compound is a cathode active material containing lithium boron oxide.

5. In paragraph 1, A cathode active material, wherein the coating portion comprises at least one compound selected from the group consisting of lithium cobalt oxide, lithium boron oxide, and lithium cobalt-boron oxide.

6. In paragraph 1, The above lithium composite transition metal oxide is a positive electrode active material having a composition represented by the following chemical formula 1: [Chemical Formula 1] Li a Ni b Co c Mr d M 1 e O2 In the above chemical formula 1, M 1 is at least one selected from the group consisting of Al, B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, 0.9≤a≤1.1, 0.6≤b<1, 0 <c<0.4, 0<d<0.4, 0≤e<0.1이다.

7. In paragraph 1, The first coating portion is a positive electrode active material comprising a compound having a composition represented by the following chemical formula 2: [Chemical Formula 2] Li f Co g B h M 2 i M 3 j O2 In the above chemical formula 2, M 2 is at least one selected from the group consisting of Ni and Mn, M 3 is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, 0.9≤f≤1.1, 0.6≤g<1, 0 <h<0.3, 0<i<0.4, 0≤j<0.1이다.

8. In paragraph 1, The second coating portion is a positive electrode active material comprising a compound having a composition represented by the following chemical formula 3: [Chemical Formula 3] Li k Co l B m M 4 n M 5 o O2 In the above chemical formula 3, M 4 is at least one selected from the group consisting of Ni and Mn, M 5 is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, 0.9≤k≤1.1, 0.6≤l<1, 0 <m<0.3, 0≤n<0.4, 0≤o<0.3이다.

9. In paragraph 1, The positive electrode active material wherein the first coating portion includes a compound having a composition represented by the following chemical formula 2, and the second coating portion includes a compound having a composition represented by the following chemical formula 3: [Chemical Formula 2] Li f Co g B h M 2 i M 3 j O2 In the above chemical formula 2, M 2 is at least one selected from the group consisting of Ni and Mn, M 3 is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, 0.9≤f≤1.1, 0.6≤g<1, 0 <h<0.3, 0<i<0.4, 0≤j<0.1이고, [Chemical Formula 3] Li k Co l B m M 4 n M 5 o O2 In the above chemical formula 3, M 4 is at least one selected from the group consisting of Ni and Mn, M 5 is at least one selected from the group consisting of Al, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, 0.9≤k≤1.1, 0.6≤l<1, 0 <m<0.3, 0≤n<0.4, 0≤o<0.3이다.

10. In paragraph 1, A positive electrode active material having a total area of ​​the coating portion of 10% or more and 100% or less of the total surface area of ​​the lithium composite transition metal oxide.

11. A positive electrode comprising a positive electrode active material according to any one of claims 1 to 10.

12. The anode according to Article 11; cathode; a separator interposed between the anode and the cathode; and A lithium secondary battery comprising an electrolyte.

Citation Information

Patent Citations

  • Cathode active material for lithium ion secondary batteries, method for manufacturing the same, and lithium ion secondary batteries including the same

    KR102084689B1

  • How to build a homepage with improved loading speed

    KR1020210156368A

  • Exhaust diffuser system and gas turbine including the same

    KR1020230030446A

  • System and method for testing speech fluency

    KR1020240153055A

  • Method for manufacturing cathode active material for lithium secondary battery, and cathode active material manufactured thereby

    WO2023054959A1

Cited By

  • High-nickel ternary positive electrode material, preparation method thereof, positive electrode sheet, secondary battery and electric device

    CN122868506A