Compositions and methods for solid-state electrochemical cells

A multi-phase polymer electrolyte with a robust inert scaffold and lithium salt-containing plasticized phase addresses the instability issues in lithium-ion batteries, achieving superior ionic conductivity and mechanical stability for room-temperature operation and high energy density in lithium batteries.

WO2024249183A1PCT designated stage expired Publication Date: 2024-12-05ENERGY EXPLORATION TECHNOLOGIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/US2024/030426
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-21
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current lithium-ion batteries face limitations due to the chemical and electrochemical instability of liquid electrolytes with lithium metal, leading to dendrite formation and thermal runaway, and existing polymer electrolytes lack sufficient lithium-ion conductivity and mechanical stability for room-temperature commercial applications.

Method used

A multi-phase polymer electrolyte with a robust inert polymer scaffold and a lithium salt-containing plasticized phase, which is easily scalable and adaptable for large-scale production, providing high ionic conductivity and mechanical stability, and is synthesized using a method that allows for room-temperature operation of all-solid-state lithium batteries.

Benefits of technology

The polymer electrolyte achieves superior performance at room temperature with enhanced ionic conductivity and electrochemical stability, enabling long-cycle life and high energy density in lithium batteries, surpassing traditional Poly(ethylene oxide) based electrolytes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2024030426_05122024_PF_FP_ABST
    Figure US2024030426_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed herein is a composition for an electrochemically stable and mechanically flexible polymer electrolyte for lithium-metal and Lithium-ion batteries and methods of making and integrating this polymer electrolyte into an all-solid-state battery. This polymer is designed to improve ionic conductivity by creating a multi-dimensional membrane with a uniform lithium salt distribution. This solid electrolyte is electrochemically stable during galvanostatic cycling with commercially relevant cathode materials and a lithium metal anode, allowing for higher energy densities to be achieved relative to current lithium-ion batteries. This electrolyte is produced with an easy and scalable manufacturing method that is amenable to roll-to-roll processing.
Need to check novelty before this filing date? Find Prior Art

Description

COMPOSITIONS AND METHODS FOR SOLID-STATE ELECTROCHEMICAL CELLS

[0001] This application claims the benefit of priority to United States Provisional Application No.63 / 469,350, filed on May 26, 2023, the entire contents of which are hereby incorporated by reference. BACKGROUND 1. Technical Field

[0002] The present disclosure generally relates to compositions for use in a solid-state electrochemical cell and methods for producing components of the cell. More specifically, the present disclosure relates to compositions for use in a solid-state electrochemical cell consisting of a polymeric lithium-ion conducting electrolyte and methods for fabricating this electrolyte. 2.Description of Related Art

[0003] Although the lithium-ion battery has enabled a slew of electronic devices to become portable, it still has intrinsic limitations that prevent it from powering larger electronic devices for desired durations, such as passenger electric vehicles. One such limitation is owing to the chemical and electrochemical instability of the liquid electrolyte with lithium metal. Lithium metal does not plate / strip densely and uniformly; instead, lithium metal deposits on point charge concentrations that then develop into nucleation sites for further non-uniform lithium metal deposition forming what is referred to in the field as a lithium metal dendrite. After this process has occurred for a prolonged period, the lithium metal dendrite(s) can become long enough and numerous enough to grow through the porous polymeric separator and short- circuit the cell and consequently cause thermal runaway, igniting the often-flammable solvent of the liquid electrolyte and causing catastrophic failure. A similar process can occur for lithium-ion batteries with a graphite or silicon anode if the charging conditions of the battery are such that it is more favorable for lithium to plate on the surface of the graphite or silicon particle rather than intercalate or alloy with the particle, respectively. Therefore, lithium-ion batteries must be carefully charged to prevent such conditions, and secondary lithium metal batteries are dangerous with extremely limited cycle life.

[0004] An alternative to a traditional secondary lithium battery is an all-solid-state lithium battery. An all-solid-state lithium battery replaces the separator and liquid electrolyte with a solid lithium-ion conductor, often termed a solid electrolyte. There are additional engineering challenges in developing all- solid-state batteries behind the base challenge of finding materials with sufficient lithium-ion conductivity, among other properties, that can serve as a solid electrolyte. As an example, since a liquid electrolyte is not present in the battery to penetrate the pores of the composite cathode electrode matrix and promote lithium-ion conduction from the bulk of the cathode composite, some solid electrolyte material must be added to the cathode composite during fabrication to enable full electrochemical activity of all the available operational lithium in the cathode active material. One approach is to use a lithium-ion conducting polymer in place of the inert solid polymer separator and liquid electrolyte. This strategy -1- 4856-8944-3776, v.1provides unique advantages over other categories of solid electrolyte materials, such as ease of large-scale manufacture. However, most known polymer electrolyte materials do not have the requisite lithium-ion conductivity to be effective in a commercial lithium battery and maintain poor interfacial contact with the two electrodes of the battery; these two factors cause a need for high temperature operation of all-solid- state batteries with a polymer electrolyte. Additionally, many polymer electrolytes conduct the accompanying anion as well as the lithium ion in the solvated salt within the polymer matrix, leading to poor energy efficiency of the overall battery, or a large overpotential between the charge voltage and the discharge voltage. A prime example of a well-studied polymer electrolyte system that displays many of the shortcoming associated with this class of materials is the Polyethylene oxide (PEO) system, which has been studied with a variety of lithium salts.

[0005] Plasticizing, gelation, and the addition of inorganic ceramic fillers to form composite polymer electrolytes are different avenues that have been attempted to develop a polymer-based electrolyte for lithium batteries. However, each of these approaches have their shortcomings, and none have yielded an effective polymer electrolyte suitable for room-temperature commercial application. Composite polymer electrolytes consisting of a ceramic filler can form ion pairs within the polymer matrix to enhance ionic conductivity. The inorganic filler by itself is brittle but incorporating it into the polymer system improves the overall mechanical stability of the electrolyte. Additionally, the interaction between the polymer matrix and the surface of the inorganic filler reduces crystallinity of the overall polymer and creates a “space charge” region around each filler particle where ionic conduction is improved beyond that of the base polymer electrolyte. Plasticizers lower the glass-transition temperature, thereby lowering the overall crystallinity of the polymer electrolyte and increasing the degree of dissociation of the lithium salt into the polymer matrix, which is ultimately favorable for ionic conduction of the polymer-salt complex. The lowering of the glass-transition temperature also reduces the rigidity of the polymer matrix and negatively effects the mechanical strength of the polymer when used in battery operation. Therefore, plasticized electrolytes need a support material to handle volume changes during cell cycling. Gel polymer electrolytes are designed to lower the interfacial resistances by adding a small amount of solvent. The solvent affects the crystallinity of the polymer and forms a better interface between the electrolyte and electrodes. The ionic conductivity of the amorphous region of the polymer is promoted even further with more absorption of solvent in the amorphous regions. The complexity of these systems allows for a high degree of compositional tuning to affect the performance characteristics of the product polymer electrolyte.

[0006] Therefore, there remains a need to develop new lithium battery compositions, in particular new polymer compositions that may be used in the preparation of the electrolyte component of solid-state lithium batteries. SUMMARY

[0007] The polymer electrolyte presented in this work incorporated the benefits of all four types as well as designing the polymer that has a wider electrochemical window. It consists of an inert porous -2- 4856-8944-3776, v.1polymer support structure that can be impregnated with a solution consisting of a monomer and lithium salt. Once saturated into the inert porous polymer support structure, the entire membrane can be cured to solidify through a thermal or ultra-violet treatment. The resulting polymer electrolyte is mechanically robust owing to the robust inert solid polymer support structure and has a high ionic conductivity owing to the gel like nature of the gel-like nature of the polymer phase within the impregnated pore structure of the inert solid-polymer backbone. Additionally, this strategy is easily adaptable to large-scale production. This combination of materials demonstrates an unexpected stability at high voltage and ionic conductivity compared to similar materials in the art. All-solid-state lithium metal batteries cycled with the disclosed electrolyte strategy demonstrated far superior performance at room-temperature than cells fabricated with a standard solid-polymer electrolyte formulation of Poly(ethylene oxide) with lithium bis(trifluoromethanesulfonyl)imide salt.

[0008] Other objects, features and advantages of the present disclosure will become apparent from the following detailed description. It should be understood, however, that the detailed description and the specific examples, while indicating specific embodiments of the invention, are given by way of illustration only, since various changes and modifications within the spirit and scope of the invention will become apparent to those skilled in the art from this detailed description. Note that simply because a particular compound is ascribed to one particular generic formula doesn’t mean that it cannot also belong to another generic formula. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] The following drawings form part of the present specification and are included to further demonstrate certain aspects of the present invention. The invention may be better understood by reference to one or more of these drawings in combination with the detailed description of specific embodiments presented herein.

[0010] Figure 1. Schematic of a secondary lithium battery consisting of a lithium metal anode. Note: The components and the distances between them are not drawn to scale.

[0011] Figures 2A & 2B. molecular structures for (a) acrylate and (b) methacrylate precursors.

[0012] Figure 3. Chemical structure of one embodiment of the disclosed invention; cross-linked methacrylate polymer with uniformly distributed Succinonitrile (SN) plasticizer and Lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) salt. This structure infiltrates the pores of a porous inert polymer membrane to form a two-phase polymer electrolyte.

[0013] Figure 4. (a) Linear sweep voltammetry conducted with a BioLogic SP200 at a scan rate of 0.1 mV / s from 3.0 V to 7.5 V versus Li+ / Li0on a full cell with an LiFePO4 composite cathode and a lithium metal anode.

[0014] Figure 5. Easy and scalable manufacturing process of enclosed polymer electrolyte. The precursor solution can be added to the cell and cured to form sufficient interface. Demonstration of how -3- 4856-8944-3776, v.1the disclosed polymer electrolyte strategy can be implemented for large-scale cell manufacturing. The precursor solution can be added to a dry cell assembled with pre-existing lithium battery manufacturing equipment and cured in-situ to form the polymer electrolyte disclosed herein. And an example of a free- standing polymer electrolyte membrane made via the disclosed polymer electrolyte strategy.

[0015] Figure 6. Galvanostatic cycling data of a full cell consisting of an LiFePO4composite cathode, a 100µm lithium metal anode, and a PEO electrolyte with LiTFSI salt (EO:Li ratio of 2:3) at 50oC. The cathode composition was 50-90wt% active material, 3.3-17wt% conductive carbon, 3.3-17wt% binder, 3- 15wt% plasticizer, and 0.4-1wt% lithium salt. This plot shows 25 cycles at a C / 10 rate. The C-rate was calculated relative to the theoretical capacity of the cathode active material within the composite cathode.

[0016] Figure 7. Galvanostatic cycling data at 50oC of a full cell consisting of an LiFePO4 composite cathode, a 100µm lithium metal anode, and an embodiment of the polymer electrolyte concept disclosed herein – 42wt% poly(ethylene glycol) methyl ether methacrylate, 31wt% succinonitrile, 23wt% lithium bis(trifluoromethanesulfonyl)imide, 1wt% polyethylene glycol diacrylate, 0.2wt% azobisisobutyronitrile, and 2.8wt% fluoroethylene carbonate. The cathode composition was 70wt% LiFePO4, 10wt% carbon black, 10wt% polyvinylidene fluoride, 9wt% succinonitrile, and 1wt% lithium difluorooxalato borate. This figure shows 25 cycles at a C / 10 rate. The C-rate was calculated relative to the theoretical capacity of the cathode active material within the composite cathode.

[0017] Figure 8. Room-temperature galvanostatic cycling data for a full cell consisting of an LiFePO4composite cathode, a 100µm lithium metal anode, and an embodiment of the polymer electrolyte concept disclosed herein 42wt% methyl methacrylate, 31wt% succinonitrile, 23wt% lithium bis(trifluoromethanesulfonyl)imide, 1wt% polyethylene glycol diacrylate, 0.2wt% azobisisobutyronitrile, and 2.8wt% fluoroethylene carbonate. The cathode composition was 70wt% LiFePO4, 10wt% carbon black, 10wt% polyvinylidene fluoride, 9wt% succinonitrile, and 1wt% lithium difluorooxalato borate. This cell was cycled at a C / 10 rate. The C-rate was calculated relative to the theoretical capacity of the cathode active material within the composite cathode. DETAILED DESCRIPTION

[0018] The present disclosure provides a formulation for a polymer electrolyte for use in an all-solid- state battery. Furthermore, the present disclosure also provides an all-solid-state battery consisting of this polymer electrolyte formulation. The disclosed formulation of polymer electrolyte is a multi-phase polymer that synergistically takes advantage of the positive aspects of several different classes of polymer electrolyte materials while mitigating their downsides. This polymer is designed to improve ionic conductivity by creating a three-dimensional lithium conducting network with a uniform lithium salt distribution within a mechanically robust inert polymer scaffold matrix. This solid electrolyte is electrochemically stable during galvanostatic cycling with commercially relevant cathode materials and a lithium metal anode, allowing for higher energy densities to be achieved relative to current lithium-ion -4- 4856-8944-3776, v.1batteries. This electrolyte is produced with an easy and scalable manufacturing method that is amenable to roll-to-roll processing.

[0019] An electrochemically and mechanically stable polymer electrolyte with a high ionicconductivity and methodology for implementing it into an all-solid-state battery are described. An example of the solid-state battery was synthesized, and its basic material properties were tested to evaluate its suitability towards secondary battery applications. The polymer electrolyte demonstrated sufficient ionic conductivity (2.2 × 10-5Scm-1) at room temperature to allow for operation of an all-solid-state battery and a high oxidation stability (stable above 5V versus Li+ / Li0) that allows for the developments of all-solid- state batteries with high voltage cathodes for superior energy density. Additionally, the synthetic method for the polymer electrolyte used in this battery is easily scalable with currently employed manufacturing methods used to commercially produce lithium-ion batteries. I. Lithium Batteries

[0020] Lithium-ion batteries are an electrochemical cell that converts electrical energy into storedchemical energy and typically consist of four primary components: 1) a cathode, 2) an anode, 3) a separator, and 4) an electrolyte. Each of these components is critical to proper operation of a rechargeable (secondary) lithium-ion battery. The electrolyte is typically comprising a solvent with a solvated salt of the species responsible for chemical energy storage in the electrochemical cell – i.e., for a secondary lithium battery, the electrolyte is a solvent with a solvated lithium conducting salt. The separator in current lithium-ion batteries is typically an inert stretched polyolefin (PO) such as polypropylene (PP) or polyethylene (PE) membrane (or a combination thereof) that contains nanopores that allow for the liquid electrolyte to infiltrate the pores and ions to conduct through the separator. The primary function of the separator is to allow for close contact between the anode and the cathode without allowing them to physically touch while also allowing for ions to diffuse back and forth between the two electrodes via the liquid electrolyte. A brief schematic of a secondary lithium battery is provided in Figure 1 – in this instance, the anode is a lithium metal anode. i. Lithium Battery Electrolyte Compositions

[0021] The three-dimensional polymer backbone of the two-phase polymer electrolyte is formed by amonomer and surrounds a lithium salt containing plasticized phase. Among different monomer options, methacrylate was chosen for its superior stability compared to acrylate (e.g., butyl acrylate), but other suitable options include styrenes (e.g., sodium styrenesulfonate). Figure 2 shows the molecular structure for acrylate and methacrylate monomers with methacrylate replacing the ketone α-hydrogen (α-H) which is labile or active towards redox reactions, providing a large electrochemical stability window for this demonstration of the invention.

[0022] The chemical structure of the polymer electrolyte may further comprise a monomer of theformula: -5- 4856-8944-3776, v.1(I) wherein: R1is a group of the formula: −(CH2CH2O)nOR1′, wherein: n is an integer from 1 to 50; and R1′ is hydrogen, alkyl(C≤12), or substituted alkyl(C≤12); and R2 is alkyl(C≤12) or substituted alkyl(C≤12).

[0023] In particular, the monomer has an R1′ that is alkyl(C≤12)such as alkyl(C≤8), alkyl(C≤6), or alkyl(C≤4). In one embodiment, R1′ is methyl. The monomer may also comprise an n that is from 2 to 40, from 3 to 30, or from 5 to 25.

[0024] The resultant polymer may contain one or more cross-linking monomers. These cross-linking monomers may comprise a polyethylene glycol (PEG) or polypropylene glycol (PPG) polymers. The PEG or PPG polymers may have from about 1 to about 100 repeating units, from about 2 to about 75 repeating units, or from about 5 to about 50 repeating units.

[0025] The electrolyte compositions described herein may comprise an amount of the methacrylate polymer that is from about 20 wt.% and 65 wt.%. The amount of the methacrylate polymer is from about 20, 25, 30, 35, 40, 45, 50, 55, 60, to about 65 wt.%, or any range derivable therein. The polymer may further comprise one or more crosslinking monomers that are linked through a PEG or PPG linker. The amount of the crosslinking monomer in the composition may be from about 0.5 wt.% to about 2 wt.%. In some embodiments, the crosslinking monomers comprises from about 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2 wt.%, or any range derivable therein. Furthermore, the polymerization may need an initiator. In some aspects, the polymerization may occur through the use of a radical initiator such as an azo type radical initiator. Some non-limiting types of radical initiators include azobisisobutyronitrile and azobisdimethylvaleronitrile. The amount of the radical initiator in the composition may be from about 0.1 wt.% to about 0.5 wt.%. The amount of the radical initiator may be from about 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, to about 0.5 wt.%, or any range derivable therein.

[0026] Figure 3 shows the final chemical structure of the polymer electrolyte of the present disclosure. The main advantage of this electrolyte is its scalability; as an example, a 5 µm porous polyethylene (PE) membrane can be used, which is easy to manufacture in a roll-to-toll fashion. This porous PE membrane can be saturated by a monomer electrolyte solution cured with a thermal or UV treatment. The precursor solution consists of the monomer, cross-linking agent, polymerization initiator, lithium salt, plasticizer, and possibly other additives. -6- 4856-8944-3776, v.1

[0027] In particular, the electrolyte composition may further comprise a lithium salt. The lithium salt is a lithium salt with an anion that is an organic anion. The organic anion is a hydrophobic anion such as alkylsulfonyl imide anion such as a bis(alkylsulfonyl) imide. The lithium salt may be bis(trifluoromethanesulfonyl)imide. The composition may comprise 15 wt.% to about 30 wt.%. The composition may comprise an amount of the lithium salt from about 15, 17.5, 20, 22.5, 25, 27.5, to about 30 wt.%, or any range derivable therein.

[0028] Furthermore, the electrolyte composition may further comprise a plasticizer. In some aspects, the plasticizer is a compound containing two or more functional groups on an alkyl chain. The functional group may be nitrile, a carboxylic acid, a hydroxy, nitro, or amine group. In particular, the plasticizer may comprise an alkyl chain with from 1-6 carbon atoms. In particular, the plasticizer may have two carbon atoms such as succinonitrile. The electrolyte composition may comprise from about 20 wt.% to about 65 wt.%. The amount of the plasticizer may be from about 20, 25, 30, 35, 40, 45, 50, 55, 60 to about 65 wt.%, or any range derivable therein. Furthermore, it is contemplated that the electrolyte composition may further comprise from about 1 wt.% to about 3.5 wt.% of other additives. In some aspects, the present additives may further comprise from about 1, 1.2, 1.4, 1.5, 1.6, 1.8, 2, 2.2, 2.4, 2.5, 2.6, 2.8, 3, 3.2, 3.4, to about 3.5 wt.%, or any range derivable therein of the other additives.

[0029] Extensive electrochemical characterization was performed to demonstrate the superior performance of this invention compared to other polymer electrolytes that have been reported. Full small- scale electrochemical cells were also constructed with a commercially relevant lithium iron phosphate (LiFePO4; LFP) cathode, and a lithium metal anode. The cells show long-cycle life without penetration of dendritic lithium which often leads to an internal short circuit and consequently thermal runaway of the cell. For comparison, similar cells were assembled with a poly(ethylene oxide)-LiTFSI polymer electrolyte.

[0030] These electrolyte compositions may be used in a battery. The battery then comprises an anode and a cathode. When the electrolyte composition is present in the battery, then the battery may comprise from about 5% to about 95%, from about 10% to about 50%, or from about 12% to about 25% by weight. The amount of the electrolyte composition may be present from about 5%, 7.5%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 25%, 27.5%, 30%, 32.5%, 35%, 37.5%, 40%, 45%, 50%, 55%, 60%, 70%, 80%, to about 90%, or any range derivable therein. In particular, the battery may contain a cathode active material. The cathode active material may contain a phosphate group. The cathode active material may also comprise lithium. Some non-limiting examples of cathode active materials include lithium iron phosphate (LiFePO4), lithium nickel cobalt manganese oxide (LiNixMnyCozO2;x+y+z = 1), lithium manganese oxide (LiMn2O4), lithium cobalt oxide (LiCoO2), lithium nickel cobalt aluminium oxide (LiNixCoyAlzO2; x+y+z = 1), or lithium nickel manganese oxide (LiNi0.5Mn1.5O4). Several non-limiting examples of these active materials containing lithium include LiNi0.6Mn0.2Co0.2O2, LiNi0.8Mn0.1Co0.1O2, and LiNi0.83Mn0.11Co0.06O2. Furthermore, the cathode may further comprise a conductive carbon material. The conductive carbon -7- 4856-8944-3776, v.1material may be Carbon Black, carbon nanotubes, Super C65, Super P, Acetylene Black, Ketjen Black, Denka Black, or multi-layer graphene. In some aspects, the cathode may from about 1% to about 25% or from about 5% to about 15% of the conductive carbon material. The amount of conductive carbon material may be from 1%, 2.5%, 5%, 6%, 8%, 10%, 12% 14%, 16%, 18%, 20%, 22%, 24%, to about 25%, or any range derivable therein. The cathode may further comprise a binder. The binder may be a fluoropolymer such as polyvinylidene fluoride (PVDF), polyvinyl butyral (PVB), or polytetrafluoroethylene (PTFE). Other options for binder are styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC). In some aspects, the cathode may from about 1% to about 25% or from about 5% to about 15% of the binder. The amount of binder may be from 1%, 2.5%, 5%, 6%, 8%, 10%, 12% 14%, 16%, 18%, 20%, 22%, 24%, to about 25%, or any range derivable therein. The cathode may further comprise one more additives like a dinitrile or a borate (e.g., lithium difluoro(oxalato)borate, lithium bisoxalatodifluorophosphate, or Lithium bis(oxalato)borate). The amount of these additives in the cathode may be from about 0.1% to about 10% or from about 0.5% to about 5%. The amounts of additives may be from about 0.1%, 0.25%, 0.5%, 0.75%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, to about 10%, or any range derivable therein. Additionally, the cathode of the battery could be a nickel containing cathode.

[0031] In some aspects, the battery further comprises an anode. The anode may be a lithium anode. In other aspects, the battery is anode free. If lithium is used in the anode, then the anode comprises a thickness of lithium from about 0 µm to about 100 µm, from about 10 µm to about 75 µm, or from about 20 µm to about 40 µm. The thickness of the lithium may be from about 0 µm, 10 µm, 15 µm, 20 µm, 25 µm, 30 µm, 35 µm, 40 µm, 45 µm, 50 µm, 55 µm, 60 µm, 65 µm, 70 µm, 75 µm, 80 µm, 90 µm, to about 100 µm, or any range derivable therein.

[0032] The battery prepared using these electrolyte compositions may comprise an energy density of greater than 300 Wh / kg, greater than 350 Wh / kg, or greater than 400 Wh / kg. The energy density may be from about 300 Wh / kg to about 700 Wh / kg, from about 350 Wh / kg to about 600 Wh / kg, or from about 400 Wh / kg to about 550 Wh / kg. Furthermore, the fabrication process may be modified within the scope described in this application to achieve the appropriate scale and characteristics. In particular, the methods may be modified and optimized in such a way to ensure that the battery obtains maximum electrolyte soakage and that the battery contains a smooth interface between the electrolyte solution and the electrodes. These modifications may include changes to the curing time, temperatures, or pressure to enhance uniform polymerization. For example, the pressure applied during the cell fabrication and testing could be greater than 1 atm. The pressure could be greater than 1 atm, greater than 2 atm, or greater than 3 atm, or form about 2 atm to about 8 atm. EXAMPLES

[0033] The following examples are included to demonstrate preferred embodiments of the invention. It should be appreciated by those of skill in the art that the techniques disclosed in the examples which -8- 4856-8944-3776, v.1follow represent techniques discovered by the inventor to function well in the practice of the invention, and thus can be considered to constitute preferred modes for its practice. However, those of skill in the art should, in light of the present disclosure, appreciate that many changes can be made in the specific embodiments which are disclosed and still obtain a like or similar result without departing from the spirit and scope of the invention. Example 1: Ionic Conductivity of Solid State Electrolyte Solution

[0034] Basic material performance testing was conducted as well as practical device testing to demonstrate the superiority of the disclosed invention relative to pre-existing commercial technology and previously reported materials in the academic literature. A primary shortcoming of materials with good performance that are reported in the academic literature is their inability to be scaled in such a way that is amenable for practical and economical commercialization.

[0035] The basic material properties that are important for electrolyte materials are its ionic conductivity and electrochemical stability. The ionic conductivity of the material dictates how fast the material can transport ionic charge through the battery from one electrode to the other to compensate for the external electronic charge that is simultaneously being transferred from one electrode to another. This material property is typically measured with Electrochemical Impedance Spectroscopy (EIS). The cell configuration for testing this property was a symmetric lithium metal cell – a cell with lithium metal serving as both electrodes. Once an impedance spectrum is obtained, the overall resistance of the cell can be determined from looking at the “real impedance” in the obtained plot. This resistance value can then be plugged into the equation, ^ ^ = (1) ^ ∗ ^ Where σ is the ionic conductivity of thein Scm-1, l is the thickness of the sample in cm, R is the resistance in ohms measured with EIS, and A is the cross-sectional area of the electrode being used to test the sample in cm. The prepared example of the disclosed electrolyte technology was determined to have a room-temperature ionic conductivity of 2.2 × 10-5Scm-1. This ionic conductivity is a magnitude greater than that of the industry standard PEO-LiTFSI based polymer electrolyte materials that have an ionic conductivity in the range of 1×10-7- 1×10-6Scm-1.

[0036] The electrochemical stability of the material can be segmented into two different categories: 1) Oxidation stability or the ability of the material to withstand high potentials, and 2) Reduction Stability or the ability of the material to withstand extremely low potentials. For the purposes of a lithium metal battery, the measured battery voltage is the potential difference between a cathode active material and lithium metal. Thus, the electrolyte material must have an electrochemical stability window that can withstand the operational voltage of the battery with these two components. -9- 4856-8944-3776, v.1

[0037] Few known electrolyte materials are known to be stable at a low enough potential to encompass the Li+ / Li0redox couple that is responsible for the plating / stripping process of lithium metal during battery operation. It is usually the case that materials chemically breakdown on contact with lithium metal and get reduced, or electrochemically breakdown during battery operation. The nature of the polymer electrolyte concept disclosed herein can be tailored depending on the monomer used to infiltrate the inert polymer backbone such that the overall polymer electrolyte structure is stable with lithium metal or induces a chemical reaction that produces a product that is favorable for overall lithium metal battery operation. The porous inert polymer backbone material should be selected such that it is fully (chemically and electrochemically) inert when in contact with lithium metal. The example polymer electrolyte material synthesized to demonstrate the concepts disclosed was 22-62wt% methacrylate, 20-62wt% plasticizer, 15- 30wt% lithium salt, 0.5-2wt% cross-linking agent, 0.1-0.5wt% cross-linking initiator, and 1.9-3.5wt% other additives.

[0038] Many polymer electrolyte materials have oxidation stability up to 4.2-4.5 V versus Li+ / Li0. This level of stability is sufficient to encompass some commercially relevant Li-ion battery cathodes, such as olivine structured LiFePO4with a flat Fe2+ / 3+redox couple of 3.45 V versus Li+ / Li0. However, it is not high enough to fully encompass the transition-metal redox couples of next generation Li-ion battery cathodes that have a higher voltage for their redox couples, such as high-nickel layer-structured LixNi1-x-yMnxCoyO2that requires voltages up to 4.4V or greater versus Li+ / Li0to realize the high capacity this cathode can afford owing to its sloping voltage curve. For the model system synthesized to demonstrate the concept disclosed in this report, linear sweep voltammetry (LSV) was performed on a full cell with an LiFePO4composite cathode and a pure lithium metal anode. Figure 4 demonstrates the results of the LSV experiment and shows a breakdown current for the methacrylate infused PE electrolyte of over 5.0V versus Li+ / Li0. This oxidation stability is high enough to encompass most next-generation lithium battery cathodes of interest for high energy-density cells - such as LiCoPO4and its related doped compounds, high nickel Li[NixMnyCoz]O2(x+y+z=1), Li[NixCoyAlz]O2(x + y + z = 1), Li[NixMny]O2(x + y = 1), or Li[LixNiyMnz]O2(x + y + z = 1), and LiNi0.5Mn1.5O4. Example 2: Manufacturability of the Electrolyte Solution

[0039] The disclosed strategy for producing a polymer electrolyte of high electrochemical stability and ionic conductivity is also amenable to large scale manufacturing for the material itself as well as for all-solid-state cells consisting of the polymer electrolyte materials. Figure 5 highlights this point as a dry lithium cell can be assembled as normal with the desired cathode and anode, then the precursor solution can be injected as a normal liquid electrolyte would and the precursor solution within the cell can be cured in-situ to finally form an all-solid-state battery with the polymer electrolyte disclosed herein. Alternatively, Figure 5 also shows how a free-standing solid electrolyte membrane can be prepared if desired via casting the precursor solution over a porous inert polymer backbone before curing the entire membrane with the -10- 4856-8944-3776, v.1precursor solution embedded within the pore structure to finally form the free-standing two-phase polymer electrolyte membrane. Example 3: Battery Operations

[0040] After assessing the material properties of the new polymer electrolyte material, full cell operation was performed to assess its device performance relative to other well-known polymer electrolyte materials. Figure 6 shows galvanostatic charge / discharge data for a full lithium metal battery assembled with an LiFePO4 composite cathode and a well-known PEO-LiTFSI (EO:Li ratio of 2:3) electrolyte composition assembled for comparison purposes to provide a baseline for comparison of the disclosed technology to a well-known and well-studied system. Figure 7 shows galvanostatic charge / discharge data for a lithium metal battery assembled with a polymer electrolyte composed of poly(ethylene glycol) methyl ether methacrylate, succinonitrile, lithium bis(trifluoromethanesulfonyl)imide, polyethylene glycol diacrylate, azobisisobutyronitrile, and fluoroethylene carbonate, an example composition of the polymer electrolyte concept disclosed herein. The composite cathode composition was 70 wt% active material, 10wt% conductive carbon, 10wt% binder, 9wt% plasticizer, and 1wt% lithium salt. This compositional for the cathode composite could be extended to 50-90wt% active material, 3.3-17wt% conductive carbon, 3.3- 17wt% binder, 3-15wt% plasticizer, and 0.4-1wt% lithium salt. The anode composition was 100 µm pure lithium – it should be noted that this invention could be extended to alternative anode compositions and materials, such as silicon, graphite, anode-less, and / or combinations / composites thereof but for the purposes of demonstration only lithium metal was used as an anode material. The assembled full cell with the methacrylate infused PE electrolyte shows greater energy efficiency via a lower overpotential between the charge and discharge voltages. Additionally, the all-solid-state cell with the methacrylate infused PE electrolyte shows greater cycling stability and coulombic efficiency indicative of its superior ionic conductivity and electrochemical stability with the lithium metal anode. Although the data presented is at 50oC, this temperature is still lower than that required for operation of the only all-solid-state battery in commercial use, which uses a PEO-based electrolyte like that which data is shown for in Figure 6, which requires 80oC for to demonstrate sufficient ionic conductivity for industrial use.

[0041] The PEO-based electrolyte could not operate for extended cycling at room-temperature (25oC), but the methacrylate infused PE electrolyte disclosed herein show sufficient ionic conductivity and electrochemical stability to allow for room-temperature operation. Figure 8 shows room-temperature cycling data for a full cell of a similar make up to that described in Figure 7. The room-temperature cycled cell showed extremely stable cycling for the first 65 cycles and a high coulombic efficiency between the charge and discharge cycles. This cell had a cycle life (cycles until 80% state-of-health is reached) of 105 cycles at room-temperature. Therefore, this polymer electrolyte strategy, with further optimization can provide a stepwise improvement in lithium battery technology in general, but especially for polymer-based all-solid-state batteries with a lithium metal anode. -11- 4856-8944-3776, v.1

[0042] The disclosed polymer electrolyte strategy can be extended to alternative lithium salts, monomers, and inert polymer backbone materials. Example monomers or polymers that can be used additively, in combination, or solely incorporated into this polymer electrolyte strategy include, but are not limited to, methyl methacrylate (MM), 2-methoxy methacrylate (2MM), n-butyl methacrylate (NBM), and poly(ethylene glycol) methyl ether methacrylate (PEGMEM). Alternative lithium salts that can be additively, in combination, or solely incorporated into this strategy include, but are not limited to, lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiDFP), lithium difluorooxalato borate (LiDFOB), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and lithium bis(fluorosulfonyl)imide (LiFSI). Alternative inert polymer backbone materials that can be additively, in combination, or solely incorporated into this strategy include, but are not limited to, polypropylene, polyolefin. * * * * * * * * * * * * * * * *

[0043] All of the compositions and methods disclosed and claimed herein can be made and executed without undue experimentation in light of the present disclosure. While the disclosure may have focused on several embodiments or may have been described in terms of preferred embodiments, it will be apparent to those of skill in the art that variations and modifications may be applied to the compositions and methods without departing from the spirit, scope, and concept of the invention. All variations and modifications apparent to those skilled in the art are deemed to be within the spirit, scope, and concept of the invention as defined by the appended claims. -12- 4856-8944-3776, v.1

Claims

CLAIMS What is claimed is:

1. An electrolyte composition comprising: (A) a methacrylate polymer, wherein the polymer further comprises at least one cross-linking monomer; (B) a lithium salt, and (C) a plasticizer.

2. The electrolyte composition of claim 1, wherein the methacrylate polymer further comprises one or more polyethylene glycol repeating units.

3. The electrolyte composition of either claim 1 or claim 2, wherein the methacrylate polymer further comprises one or more polyethylene glycol repeating units on the monomer of the methacrylate.

4. The electrolyte composition according to any one of claims 1-3, wherein the methacrylate monomer further comprises a formula: wherein:R1 is a group of the formula: −(CH2CH2O)nOR1′, wherein: n is an integer from 1 to 50; and R1′ is hydrogen, alkyl(C≤12), or substituted alkyl(C≤12); and R2is alkyl(C≤12)or substituted alkyl(C≤12).

5. The electrolyte composition of claim 4, wherein R1′ is alkyl(C≤12)or substituted alkyl(C≤12).

6. The electrolyte composition of claim 5, wherein R1′ is alkyl(C≤12).

7. The electrolyte composition of claim 6, wherein R1′ is8. The electrolyte composition according to any one of claims 4-7, wherein n is an integer from 1 to about 25.

9. The electrolyte composition of claim 8, wherein n is an integer from 3 to 10.

10. The electrolyte composition according to any one of claims 4-9, wherein R2is alkyl(C≤12).

11. The electrolyte composition of claim 10, wherein R2is methyl.

12. The electrolyte composition according to any one of claims 4-11, wherein the methacrylate monomer is further defined as: -13- 4856-8944-3776, v.

1.

13. The electrolyte composition according to any one of claims 1-12, wherein the electrolyte composition comprises an amount of methacrylate polymer from about 20% to about 65% by weight.

14. The electrolyte composition of claim 13, wherein the amount of the methacrylate polymer is from about 22% to about 62%.

15. The electrolyte composition of claim 14, wherein the amount of the methacrylate polymer is from about 25% to about 50%.

16. The electrolyte composition according to any one of claims 1-15, wherein the lithium salt is a lithium salt comprises a hydrophilic anion.

17. The electrolyte composition of claim 16, wherein the lithium salt comprises an imide anion.

18. The electrolyte composition of claim 17, wherein the lithium salt comprises an alkylsulfonyl imide anion.

19. The electrolyte composition of claim 18, wherein the lithium salt is lithium bis(trifluoromethanesulfonyl)imide.

20. The electrolyte composition according to any one of claims 1-19, wherein the electrolyte composition comprises an amount of the lithium salt from about 15% to about 30% by weight.

21. The electrolyte composition of claim 20, wherein the amount of the lithium salt is from about 20% to about 30% by weight.

22. The electrolyte composition of claim 21, wherein the amount of the lithium salt is from about 15% to about 25% by weight.

23. The electrolyte composition according to any one of claims 1-22, wherein the plasticizer is a substituted alkane.

24. The electrolyte composition of claim 23, wherein the alkane is substituted with one or more nitrile groups.

25. The electrolyte composition of either claim 23 or claim 24, wherein the alkane comprises 2 carbon atoms to 8 carbon atoms.

26. The electrolyte composition according to any one of claim 23-25, wherein the plasticizer is succinonitrile.

27. The electrolyte composition according to any one of claims 1-26, wherein the electrolyte composition comprises an amount of the plasticizer from about 20% to about 65% by weight.

28. The electrolyte composition of claim 27, wherein the amount of the plasticizer is from about 20% to about 62% by weight. -14- 4856-8944-3776, v.

129. The electrolyte composition of either claim 27 or claim 28, wherein the amount of the plasticizer is from about 3% to about 40% by weight.

30. The electrolyte composition according to any one of claims 1-29, wherein the electrolyte composition further comprises a radical initiator.

31. The electrolyte composition of claim 30, wherein the radical initiator is an azo compound.

32. The electrolyte composition of claim 31, wherein the radical initiator is azobisisobutyronitrile.

33. The electrolyte composition according to any one of claims 1-32, wherein the methacrylate polymer further comprises a cross-linking.

34. The electrolyte composition of claim 33, wherein the methacrylate polymer comprises a cross- linking monomer with two methacrylate moieties.

35. The electrolyte composition of claim 34, wherein the cross-linking monomer comprises a polyethylene glycol or a polypropylene glycol moiety.

36. The electrolyte composition according to any one of claims 1-35, wherein the electrolyte composition comprises an amount of a cross-linking monomer from about 0.1% to about 5% by weight.

37. The electrolyte composition of claim 36, wherein the amount of the cross-linking monomer comprises from about 0.5% to about 2% by weight of the composition.

38. The electrolyte composition according to any one of claims 1-37, wherein the electrolyte composition comprises an additive.

39. The electrolyte composition of claim 38, wherein the additive is an organic additive.

40. The electrolyte composition of either claim 38 or claim 39, wherein the additive is a carbonate.

41. The electrolyte composition according to any one of claims 38-40, wherein the additive is a halogen substituted carbonates.

42. The electrolyte composition according to any one of claims 38-41, wherein the additive is fluoroethylene carbonate.

43. The electrolyte composition according to any one of claims 1-42, wherein the electrolyte composition comprises an amount of the additive from about 1% to about 10% by weight.

44. The electrolyte composition of claim 43, wherein the amount of the additive is from about 1.5% to about 5% by weight.

45. The electrolyte composition of either claim 43 or claim 44, wherein the amount of the additive is from about 1.9% to about 3.5% by weight.

46. A battery comprising the electrolyte composition according to any one of claims 1-45.

47. The battery of claim 46, wherein the amount of the electrolyte composition in the battery is from about 5% to about 95% by weight. -15- 4856-8944-3776, v.

148. The battery of either claim 46 or claim 47, wherein the amount of the electrolyte composition is from about 10% to about 50% by weight.

49. The battery according to any one of claims 46-48, wherein the amount of the electrolyte composition is from about 12% to about 25% by weight.

50. The battery according to any one of claims 46-49, wherein the battery comprises a cathode and an anode.

51. The battery of claim 50, wherein the cathode comprises the electrolyte composition.

52. The battery of either claim 50 or claim 51, wherein the cathode comprises a cathode active material.

53. The battery of claim 52, wherein the cathode active material is a phosphate compound.

54. The battery of either claim 52 or claim 53, wherein the cathode active material is LiFePO4.

55. The battery of claim 52, wherein the cathode active material is an oxide.

56. The battery of either claim 52 or claim 55, wherein the cathode active material is lithium nickel- manganese-cobalt oxide.

57. The battery of either claim 52 or claim 55, wherein the cathode active material is lithium nickel- cobalt-aluminum oxide.

58. The battery according to any one of claims 46-57, wherein the cathode further comprises a conductive carbon material.

59. The battery of claim 58, wherein the conductive carbon material is sub-micron carbon material.

60. The battery of claim 59, wherein the conductive carbon material is a sub-micron carbon material with a roughly spherical shape 61. The battery according to any one of claims 46-60, wherein the battery comprises an amount of a conductive carbon material from about 1% to about 25% by weight.

62. The battery of claim 61, wherein the amount of the conducive carbon material from about 5% to about 15% by weight.

63. The battery according to any one of claims 46-62, wherein the cathode further comprises a binder.

64. The battery of claim 63, wherein the binder is a fluoropolymer.

65. The battery of either claim 63 or claim 64, wherein the binder is polyvinylidene fluoride.

66. The battery according to any one of claims 46-65, wherein the battery comprises an amount of a binder from about 1% to about 25% by weight.

67. The battery of claim 66, wherein the amount of the binder from about 5% to about 15% by weight.

68. The battery according to any one of claims 46-67, wherein the cathode further comprises dinitrile. -16- 4856-8944-3776, v.

169. The battery of claim 68, wherein the dinitrile is a C2-C8 dinitrile.

70. The battery of either claim 68 or claim 69, wherein the dinitrile is succinonitrile.

71. The battery according to any one of claims 46-70, wherein the battery comprises an amount of a dinitrile from about 1% to about 25% by weight.

72. The battery of claim 71, wherein the amount of the dinitrile from about 5% to about 15% by weight.

73. The battery according to any one of claim 46-72, wherein the cathode comprises a lithium borate.

74. The battery of claim 73, wherein the lithium borate is lithium difluorooxalato borate.

75. The battery according to any one of claims 46-74, wherein the battery comprises an amount of a lithium borate from about 0.1% to about 10% by weight.

76. The battery of claim 75, wherein the amount of the lithium borate from about 0.5% to about 5% by weight.

77. The battery according to any one of claims 46-76, wherein the anode comprises a lithium metal anode.

78. The battery of claim 77, wherein the anode comprises an amount of lithium from about 0 µm to about 100 µm of lithium.

79. The battery of claim 78, wherein the anode comprises an amount of lithium from about 10 nm to about 75 µm of lithium.

80. The battery of claim 79, wherein the anode comprises an amount of lithium from about 20 nm to about 40 µm of lithium.

81. The battery according to any one of claims 46-76, wherein the anode comprises no lithium metal in the anode and only a current collector.

82. The battery of claim 46-80, wherein the anode comprises lithium that is plated in situ after cell assembly during the first cycle.

83. The battery of claim 82, wherein the anode comprises lithium that is plated during each cycle.

84. A method of making a battery comprising admixing an electrolyte composition according to any one of claims 1-45 to a battery comprising an anode and a cathode. -17- 4856-8944-3776, v.1

Citation Information

Patent Citations

  • Polymer composition with electrophilic groups for stabilization of lithium sulfur batteries

    US10141604B2

  • Coated lithium metal negative electrode

    US20180151887A1

  • Polymer for lithium ion secondary battery and lithium ion secondary battery using same

    US8354188B2

  • Electrolyte for electrochemical device, method for preparing the same and electrochemical device including the same

    US8852815B2

  • Block copolymer including a polyanion based on a TFSILi anion monomer as a battery electrolyte

    US9431677B2