Thermoplastic elastomer foamed fiber, and preparation method therefor and use thereof
Through supercritical fluid microextrusion technology, the problems of uneven diameter and high density of polymer foamed fibers are solved, and the diameter of thermoplastic elastomer foamed fibers are uniform, low density and uniform cell size, which is suitable for large-scale continuous Manufactured and suitable for functional clothing and consumer electronics.
Patent Information
- Application Number
- PCT/CN2024/096672
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-06
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-12
AI Technical Summary
The existing polymer foamed fiber preparation methods have problems such as high extrusion system pressure, uneven diameter of foamed fibers, high density, and uneven cell size, which limits its application in functional clothing, consumer electronics and other fields.
The supercritical fluid microextrusion foaming technology is adopted to control the residence time of polymer/foaming agent during the microextrusion process to control the nucleation and growth of the cell, reduce the pressure of the extrusion system, and achieve uniform diameter and low density. Preparation of thermoplastic elastomer foamed fibers with uniform cell size.
It realizes uniform diameter control, low density and uniform cell size of thermoplastic elastomer foam fibers, improves production stability and processing efficiency, is suitable for large-scale continuous production, and has a gentle and environmentally friendly process.
Smart Images

Figure CN2024096672_12122024_PF_FP_ABST
Abstract
Description
Thermoplastic elastomer foam fiber and its preparation method and application Technical Field
[0001] The invention belongs to the technical field of polymer foaming fibers and processing thereof, and particularly relates to a thermoplastic elastomer foaming fiber and a preparation method and application thereof. Background Art
[0002] Polymer foam fibers combine the advantages of both fiber and cellular structures, offering unparalleled advantages over fiber materials, such as low density, high elasticity, large specific surface area, and rapid mass transfer. They hold significant potential for application in a wide range of emerging fields, including functional clothing, wearables, consumer electronics, filtration separation, and catalysis. Existing methods for preparing polymer foam fibers, including coagulation bath phase separation and highly inward emulsion templates, involve the use of large amounts of organic solvents and complex processing. These processes are environmentally unfriendly, have limited applicable polymer systems, and exhibit low processing efficiency, limiting their application.
[0003] Supercritical fluids, including supercritical CO2 and supercritical N2, are widely available, residue-free, and environmentally friendly, making them one of the most important and promising physical foaming agents for polymers. The academic paper Polymer Engineering Sciences, 2013, 53:2360, reports on the continuous extrusion foaming of thermoplastic polyurethane (TPU) fibers. This study used supercritical CO2 as the physical foaming agent. By injecting the supercritical fluid into an extruder system, the high-pressure TPU / CO2 melt rapidly released pressure at the extruder die to foam, producing TPU foamed fibers with a diameter of 0.3 to 1.2 mm and a wide size distribution. However, during the supercritical fluid extrusion foaming process, the pressure in the extruder system can reach as high as 30-50 MPa. When the molten polymer / fluid melt is ejected and foamed through the extremely fine die, extreme shear stress is generated within the foamed fibers, and the supercritical fluid rapidly escapes from the TPU melt. This results in uneven diameters and densities exceeding 0.9 g / cm2 in the resulting TPU foamed fibers. 3 , and the problem of uneven bubble size makes it difficult to meet actual application needs.
[0004] Summary of the Invention
[0005] The present invention provides a thermoplastic elastomer foam fiber, its preparation method, and application. The thermoplastic elastomer foam fiber produced by the present invention has a uniformly controllable diameter between 0.3 and 1.0 mm, low density, and uniform cell size. Furthermore, the preparation method of the present invention eliminates high extrusion system pressure; polymer foaming occurs during a micro-extrusion foaming process. Controlling the residence time of the polymer / foaming agent during the micro-extrusion foaming process controls the nucleation and growth of the cells. This results in a gentle process, enabling large-scale continuous production.
[0006] In order to achieve the above object, the present invention adopts the following technical solution: a thermoplastic elastomer foam fiber, comprising the following components in parts by weight: 80 to 100 parts of thermoplastic elastomer, 0 to 10 parts of nucleating agent, 0 to 1 part of chain extender, and 0 to 0.5 part of antioxidant;
[0007] The thermoplastic elastomer has a melting point of 180-230°C and a hardness of 45-82D;
[0008] The thermoplastic elastomer foam fiber has an open-pore structure on the surface and a closed-pore structure inside. The thermoplastic elastomer foam fiber has a diameter of 0.3 to 1.0 mm, an average deviation of ±0.05 mm, and a density of 0.60 to 0.90 g / cm 3 The average cell size of the internal closed-cell structure is 1 to 100 μm.
[0009] Preferably, the thermoplastic elastomer foamed fiber comprises the following components in parts by weight: 90-95 parts of thermoplastic elastomer, 1-3 parts of nucleating agent, 0.2-0.5 parts of chain extender, and 0.2-0.3 parts of antioxidant.
[0010] Preferably, the thermoplastic elastomer includes one or more of TPU, polyester elastomer (TPEE), nylon elastomer (PEBA), ethylene vinyl acetate (EVA), and polyolefin elastomer.
[0011] Preferably, the nucleating agent includes at least one of calcium carbonate, talc, mica, montmorillonite, nano-silica, carbon black, and carbon nanotubes.
[0012] Preferably, the chain extender comprises at least one of a difunctional acid derivative, an isocyanate, an anhydride and an epoxide.
[0013] Preferably, the antioxidant includes at least one of an amine antioxidant and a phosphorus antioxidant.
[0014] Preferably, the particle size of the nucleating agent is 0.05 to 5 μm.
[0015] The present invention also seeks to protect a processing device for the thermoplastic elastomer foam fiber, which comprises a wire feeding unit, a heat insulation unit, a micro-extrusion heating unit, a micro-extrusion die, a heating tunnel and a drawing unit in sequence.
[0016] The wire feed unit described in the present invention is responsible for stably feeding the supercritical fluid-treated polymer filament into the micro-extrusion foaming system. The wire feed unit is powered by rotating gears. These gears must exert a strong extrusion force on the polymer. They must also be resistant to wear during long-term use. Preferably, the gears are made of hard aluminum, stainless steel, alloy steel, or the like.
[0017] The insulation unit prevents heat from the heating unit from being transferred to the wire feeder, which could significantly soften the wire and affect wire feeding stability. The temperature after cooling through the insulation unit is no greater than the softening temperature of the polymer filament or impregnated polymer filament. Preferably, the wire feeder includes a grooved aluminum member and an active cooling device with a fan.
[0018] The micro-extrusion heating unit can quickly heat the polymer filaments, causing the polymer system to transition from a glassy state to a highly elastic state and a viscous flow state, resulting in cell nucleation and rapid cell growth.
[0019] The present invention also claims a method for preparing the thermoplastic elastomer foamed fiber, comprising the following steps:
[0020] S1, premixing all components, melt-extruding, drying, and winding to obtain a thermoplastic elastomer filament;
[0021] S2, impregnating the thermoplastic elastomer filament with a supercritical fluid, and after the impregnation is complete, removing the polymer filament and subjecting it to a low-temperature air-locking treatment to obtain an impregnated thermoplastic elastomer filament;
[0022] S3. Micro-extrusion foaming: The impregnated thermoplastic elastomer filament is heated and foamed, shaped in a channel, and stretched at a constant speed to obtain thermoplastic elastomer foamed fibers.
[0023] Preferably, in step S1, the melt extrusion is performed using a twin-screw extruder, and the temperature of the melt extrusion is 100-250° C. The temperature from the feed port to the extrusion head of the extruder is set to 100 / 190 / 200 / 215 / 220 / 190-200° C.
[0024] Preferably, in step S1, all the components are premixed and then dried with hot air, and the moisture content of the materials after drying is less than 0.05%.
[0025] Preferably, in step S1, the diameter of the thermoplastic elastomer filament is 1.65-1.80 mm.
[0026] Preferably, in step S2, the supercritical fluid is supercritical CO2 fluid, supercritical N2 fluid or a mixed fluid of supercritical CO2 fluid and supercritical N2 fluid.
[0027] Preferably, in step S2, the solubility of the supercritical fluid in the thermoplastic elastomer filament is 0.5-7.0 wt.%. More preferably, the solubility of the supercritical fluid in the thermoplastic elastomer filament is 1.0-6.0 wt.%.
[0028] Preferably, in step S2, the temperature of the low-temperature gas lock is -18 to 0°C, and during the low-temperature gas lock treatment, the weight loss rate of the supercritical fluid is not higher than 20%.
[0029] Preferably, in step S3, the hardness of the impregnated thermoplastic elastomer filament is not less than Shore 40D.
[0030] Preferably, in step S3, the wire feeding speed for heating and foaming the impregnated thermoplastic elastomer wire is 50 to 100 mm / s, more preferably 70 to 100 mm / s.
[0031] Preferably, in step S3, the temperature of the heating and foaming is 170-260°C, and the residence time is 0.3-3.0s. More preferably, the temperature of the heating and foaming is 180-250°C, and the residence time is 0.5-2.0s.
[0032] The tunnel shaping in the present invention is used to keep the melt-foamed fibers warm to a certain extent, so that the foamed fibers are in a high elastic range, and to make the foamed fibers plastically deformable by stretching, thereby increasing the elasticity of the foamed fibers.
[0033] Preferably, in step S3, the temperature of the tunnel shaping is 80-140° C., and the residence time in the tunnel is 0.5-5 s.
[0034] More preferably, the temperature of the tunnel shaping is 90-130° C., and the residence time in the tunnel is 1-4 seconds.
[0035] Preferably, in step S3, the speed of the constant speed stretching is 3-5 m / min.
[0036] The present invention also seeks to protect an application of the thermoplastic elastomer foam fiber in the fields of catalysis, functional clothing, electronic wearable devices, and filtration separation.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] (1) The thermoplastic elastomer supercritical fluid micro-extruded foam fiber of the present invention can be prepared continuously for a long time, with open pores on the surface and closed pores inside. It has the advantages of uniform thickness, excellent elastic tensile performance, low density, wear resistance, weavability, dense pore distribution, simple and easy preparation process, low cost, and green environmental protection.
[0039] (2) There is no high extrusion system pressure in the thermoplastic elastomer micro-extrusion foaming system of the present invention. Polymer foaming occurs in the micro-extrusion foaming process, and the nucleation and growth of the foam cells are controlled by controlling the residence time of the polymer in the micro-extrusion foaming process, so that the foam cell structure of the foamed fiber is uniform, the thickness of the foamed fiber is uniform, and the diameter of the foamed fiber is uniform and controllable, thereby improving the production stability of the micro-extruded foamed fiber. The processing process of the present invention is gentle and can achieve large-scale continuous production. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] FIG1 is a schematic diagram of a processing device for thermoplastic elastomer foamed fibers according to the present invention.
[0041] FIG2 is a schematic diagram of a product of thermoplastic elastomer foamed fiber of the present invention.
[0042] FIG3 is a SEM photograph of the thermoplastic elastomer foamed fiber prepared in Example 3 of the present invention.
[0043] FIG4 is a SEM photograph of the thermoplastic elastomer foamed fiber prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0044] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0045] In the Examples and Comparative Examples, the experimental methods used are conventional methods unless otherwise specified, and the materials and reagents used are commercially available unless otherwise specified.
[0046] The materials used in the examples and comparative examples are as follows (the parts involving hardness refer to Shore hardness):
[0047] Thermoplastic Elastomer A (TPU):
[0048] A1: 45D, melting point 210°C, brand 58134, Lubrizol, USA.
[0049] A2: 60D, melting point 210°C, brand 58863, Lubrizol, USA.
[0050] A3: 80D, melting point 210°C, brand 59600, Lubrizol, USA.
[0051] A4: 60D, melting point 230°C, brand 260, Bayer, Germany.
[0052] A5: 40D, melting point 190°C, brand B90A11U, BASF, Germany.
[0053] A6:60D, melting point is 240℃, brand S60D, BASF, Germany.
[0054] Thermoplastic Elastomer B (TPEE):
[0055] 60D, melting point 210℃, brand 7246, DuPont, USA.
[0056] Thermoplastic Elastomer C (PEBA):
[0057] 60D, melting point 200℃, brand 7033, Arkema, France.
[0058] Thermoplastic elastomer D (EVA):
[0059] 45D, melting point 190℃, model 750, Tosoh, Japan.
[0060] Nucleating agent:
[0061] Calcium carbonate, with an average particle size of 1 μm, is commercially available.
[0062] Talc powder, with an average particle size of 1 μm, is commercially available.
[0063] Nano-silica, with an average particle size of 200 nm, is commercially available.
[0064] Carbon black, with an average particle size of 3 μm, is commercially available.
[0065] Chain Extender:
[0066] Epoxy chain extender, commercially available.
[0067] Antioxidants:
[0068] Hindered phenolic antioxidant, commercially available.
[0069] Examples 1 to 14 and Comparative Examples 1 to 4
[0070] The components and weight proportions of the thermoplastic elastomer foamed fibers of Examples 1 to 14 and Comparative Examples 1 to 2 are shown in Table 1.
[0071] The preparation method of the thermoplastic elastomer foamed fiber of Examples 1 to 14 and Comparative Examples 1 to 2 comprises the following steps:
[0072] S1. All components are premixed, added to a twin-screw extruder, melt-extruded, dried, and wound to obtain a thermoplastic elastomer filament; wherein all components are dried with hot air after premixing, and the moisture content after drying is less than 0.05%. The temperature from the feed port to the extruder head is set to 100 / 190 / 200 / 215 / 220 / 195°C, and the diameter of the wound filament is 1.65-1.80 mm;
[0073] S2. Place the thermoplastic elastomer filament in a high-pressure device and immerse it in a supercritical fluid (supercritical CO2 fluid). After the immersion is completed, take out the polymer filament and perform a low-temperature gas-locking treatment to obtain an impregnated thermoplastic elastomer filament; wherein the solubility of the supercritical fluid in the thermoplastic elastomer filament is 0.5 to 7.0 wt.%, the low-temperature gas-locking temperature is -18 to 0°C, and during the low-temperature gas-locking treatment, the weight loss rate of the supercritical fluid is not higher than 20%.
[0074] S3. The impregnated thermoplastic elastomer filament is mounted on the unwinding wheel of a micro-extrusion foaming device, and is rapidly heated and foamed by the micro-extrusion device, shaped in a tunnel, and stretched at a constant speed to obtain a thermoplastic elastomer foamed fiber; wherein the hardness of the impregnated thermoplastic elastomer filament is not less than Shore 40D, the temperature for heating and foaming is 170-260°C, the temperature for tunnel shaping is 80-140°C, the residence time in the tunnel is 0.5-5s, and the speed of constant stretching is 5m / min.
[0075] Table 1 Component dosage (parts by weight)
[0076] Comparative Example 3
[0077] Compared with Example 3, the only difference of this comparative example is that the temperature of the tunnel heating is 150°C.
[0078] The formulation components, other condition parameters and preparation method are the same as those in Example 3.
[0079] The thermoplastic elastomer foamed fiber finally obtained in this comparative example has a diameter of 0.4 mm and a density of 1.15 g / cm 3 The bubbles disappear, and the fiber has poor elasticity and is easy to break when rolled up.
[0080] Comparative Example 4
[0081] Compared with Example 3, the difference of this comparative example is that the thermoplastic elastomer filament obtained in step S1 does not undergo step S2, but is directly extruded to obtain unfoamed thermoplastic elastomer fibers, and then the fibers are immersed in a supercritical fluid under the same conditions, and then the fibers are heated and foamed using an oil bath commonly used in the industry.
[0082] The formula components are the same as in Example 3.
[0083] The diameter of the thermoplastic elastomer foamed fiber prepared in this comparative example is 0.4 mm and the density is 1.20 g / cm 3 ,Since the fibers are very thin, the supercritical fluid escapes from the fibers quickly and there are no bubbles.
[0084] From the data in Table 1, it can be seen that the diameter of the thermoplastic elastomer foamed fiber prepared in the embodiment of the present invention is between 0.3 and 1.0 mm and can be uniformly controlled, and the density is low and can be maintained at 0.60 to 0.90 g / cm 3 The pore size is uniform, the pore distribution is dense, and long-term continuous preparation can be achieved.
[0085] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the present invention. Anyone skilled in the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by one of ordinary skill in the art without departing from the spirit and technical principles disclosed herein are intended to be covered by the claims of the present invention.
Claims
1. A thermoplastic elastomer foam fiber, characterized in that: The invention comprises the following components in parts by weight: 80 to 100 parts of thermoplastic elastomer, 0 to 10 parts of nucleating agent, 0 to 1 part of chain extender, and 0 to 0.5 part of antioxidant; The thermoplastic elastomer has a melting point of 180-230°C and a hardness of 45-82D; The thermoplastic elastomer foam fiber has an open-cell structure on the surface and a closed-cell structure inside. The thermoplastic elastomer foam fiber has a diameter of 0.3-1.0 mm, an average deviation of ±0.05 mm, and a density of 0.60-0.90 g / cm 3 The average cell size of the internal closed-cell structure is 1 to 100 μm.
2. The thermoplastic elastomer foamed fiber according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 90-95 parts of thermoplastic elastomer, 1-3 parts of nucleating agent, 0.2-0.5 parts of chain extender and 0.2-0.3 parts of antioxidant.
3. The thermoplastic elastomer foamed fiber according to claim 1, characterized in that: At least one of the following (1) to (5): (1) The thermoplastic elastomer includes one or more of TPU, polyester elastomer, nylon elastomer, ethylene vinyl acetate, and polyolefin elastomer; (2) The nucleating agent includes at least one of calcium carbonate, talc, mica, montmorillonite, nano-silica, carbon black, and carbon nanotubes; (3) the chain extender comprises at least one of a difunctional acid derivative, an isocyanate, an anhydride and an epoxide; (4) The antioxidant includes at least one of an amine antioxidant and a phosphorus antioxidant; (5) The particle size of the nucleating agent is 0.05 to 5 μm.
4. A processing device for thermoplastic elastomer foamed fibers as claimed in any one of claims 1 to 3, characterized in that: The micro extrusion machine comprises a wire feeding unit, a heat insulation unit, a micro extrusion heating unit, a micro extrusion die, a heating tunnel and a drawing unit in sequence.
5. A method for preparing the thermoplastic elastomer foamed fiber according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1, premixing all components, melt-extruding, drying, and winding to obtain a thermoplastic elastomer filament; S2, impregnating the thermoplastic elastomer wire with a supercritical fluid, and after the impregnation is completed, taking out the polymer wire and subjecting it to low-temperature air-locking treatment to obtain an impregnated thermoplastic elastomer wire; S3, heating and foaming the impregnated thermoplastic elastomer filaments, shaping them in a channel, and stretching them at a constant speed to obtain thermoplastic elastomer foamed fibers.
6. The method for preparing thermoplastic elastomer foamed fiber according to claim 5, characterized in that: At least one of the following (1) to (3): (1) In step S1, the melt extrusion is performed using a twin-screw extruder, and the temperature of the melt extrusion is 100 to 250° C.; (2) In step S1, all the components are dried by hot air after premixing, and the moisture content after drying is less than 0.05%; (3) In step S1, the diameter of the thermoplastic elastomer filament is 1.65 to 1.80 mm.
7. The method for preparing thermoplastic elastomer foamed fiber according to claim 5, characterized in that: At least one of the following (1) to (3): (1) In step S2, the supercritical fluid is a supercritical CO2 fluid, a supercritical N2 fluid, or a mixed fluid of a supercritical CO2 fluid and a supercritical N2 fluid; (2) In step S2, the solubility of the supercritical fluid in the thermoplastic elastomer filament is 0.5 to 7.0 wt.%; (3) In step S2, the temperature of the low-temperature gas lock is -18 to 0°C, and during the low-temperature gas lock treatment, the weight loss rate of the supercritical fluid is not higher than 20%.
8. The method for preparing thermoplastic elastomer foamed fiber according to claim 5, characterized in that: At least one of the following (1) to (5): (1) In step S3, the hardness of the impregnated thermoplastic elastomer wire is not less than Shore 40D; (2) In step S3, the wire feeding speed of heating the impregnated thermoplastic elastomer wire for foaming is 50 to 100 mm / s; (3) In step S3, the temperature of the heating and foaming is 170 to 260° C., and the residence time of the heating and foaming is 0.3 to 3.0 s; (4) In step S3, the temperature of the tunnel shaping is 80 to 140° C., and the residence time in the tunnel is 0.5 to 5 seconds; (5) In step S3, the speed of the constant speed stretching is 3 to 5 m / min.
9. An application of the thermoplastic elastomer foam fiber according to any one of claims 1 to 3 in the fields of catalysis, functional clothing, electronic wearable devices, and filtration separation.
Citation Information
Patent Citations
Process for molding thermoplastic polyurethane elastomer foamed monofilaments
CN107916467A
Thermoplastic elastomer physical foaming coiled material and semi-continuous preparation method thereof
CN113248770A
High-hardness thermoplastic polyurethane foaming coiled material and semi-continuous preparation method thereof
CN114456433A
Cross-linked thermoplastic elastomer micro-foaming coiled material as well as preparation method and application thereof
CN114989570A
Foaming cross-linked thermoplastic elastomer material and application thereof
CN115895097A
Cited By
Supercritical lightweight fabric and production method thereof
CN120797290A
A supercritical lightweight fabric and its production method
CN120797290B