Polyester resin composition and polyester film

The polyester resin composition addresses the challenges of electrostatic chargeability, foreign matter, and heat resistance by using specific additives, resulting in high-quality films with enhanced electrostatic properties and reduced defects.

WO2024252686A1PCT designated stage expired Publication Date: 2024-12-12TORAY INDUSTRIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/027111
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-08
Filing Date
2023-07-25
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Conventional polyester resin compositions fail to simultaneously improve electrostatic chargeability during film forming, reduce metal foreign matter, and suppress gel-like substances caused by thermal decomposition, while maintaining excellent heat resistance and transparency.

Method used

A polyester resin composition with specific formulations, including p-toluenesulfonic acid and quaternary phosphonium components, within defined ranges, along with controlled metal and phosphorus content, to enhance electrostatic properties and reduce foreign substances, achieving improved heat resistance and transparency.

Benefits of technology

The composition achieves good electrostatic application properties, reduced foreign matter, and excellent heat and hydrolysis resistance, resulting in high-quality films with fewer defects and improved transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-M000001
    Figure JPOXMLDOC01-APPB-M000001
  • Figure JPOXMLDOC01-APPB-M000002
    Figure JPOXMLDOC01-APPB-M000002
  • Figure JPOXMLDOC01-APPB-M000003
    Figure JPOXMLDOC01-APPB-M000003
Patent Text Reader

Abstract

[Problem] To provide a polyester resin composition which has little foreign material, good color tone, excellent transparency, excellent heat resistance and hydrolysis resistance, and good static electricity application properties during film formation, and which, when used as a film for a dry film resist support, has few defects due to light exposure faults. [Solution] A polyester resin composition having an inherent viscosity of not less than 0.55 dL / g, said polyester resin composition being characterized in that: with respect to the total amount of the polyester resin composition, the content of a p-toluenesulfonic acid component is 0.07-0.65 mol / t and the content of a quaternary phosphonium component is 0.07-0.65 mol / t; a heat resistance parameter X represented by expression 1 is 1.0≤X≤1.3; the number of pieces of foreign material having an equivalent circle diameter of 0.2 μm or greater is not more than 650 pieces / 0.1 mm2; molten specific resistance is not more than 4.0×106Ω・cm; and a color tone b value in a color-difference meter is not more than 10.0.
Need to check novelty before this filing date? Find Prior Art

Description

Polyester resin composition and polyester film

[0001] The present invention relates to a polyester resin composition.

[0002] Polyesters have excellent mechanical properties, thermal properties, chemical resistance, electrical properties, and moldability, and are used in a variety of applications. Among polyesters, polyethylene terephthalate (hereinafter referred to as PET) in particular has excellent transparency and processability, and is therefore used in a variety of applications, such as various optical films, for example, prism sheets for liquid crystal display components, light diffusion sheets, reflectors, base films for touch panels, anti-reflection base films, explosion-proof base films for displays, PDP filter films, and films for dry film resist supports. However, as the range of applications expands, the required quality also improves. For example, in the case of films for dry film resist supports, ultraviolet irradiation during the exposure process causes scattering and reflection of ultraviolet light, which can lead to reduced resolution and defects of fine wiring. Therefore, a resin composition that suppresses film defects such as metal foreign matter and gel-like foreign matter generated by thermal decomposition of polyester is desired.

[0003] Furthermore, when forming a film from PET resin, an electrostatic casting method is often used, in which a high voltage is applied to the upper surface of an unsolidified sheet material to make the sheet material adhere to a rotating cooling drum. In the electrostatic casting method, if the speed of the rotating cooling drum is increased to increase the film production speed, the adhesion between the sheet material and the rotating cooling drum decreases, resulting in a decrease in the uniformity of film thickness and transparency, and defects on the film surface due to uneven voltage application.

[0004] To address these issues, studies have been conducted as shown in the following documents.

[0005] For example, Patent Document 1 proposes a method of adding a large amount of an alkali metal compound, an alkaline earth metal compound, or a phosphorus compound to a polyester as a method for improving electrostatic applicability. However, although this method can improve electrostatic applicability to some extent, it uses a large amount of a metal compound, typified by magnesium acetate, which generates metal foreign matter, resulting in a problem of not meeting the required quality of the polyester film.

[0006] Patent Document 2 proposes a method of adding a quaternary phosphonium sulfonate as a method of improving electrostatic applicability. However, because a large amount of alkali metal or alkaline earth metal is contained in this method, it is insufficient to suppress metallic foreign matter, and also insufficient to suppress gel-like foreign matter due to thermal decomposition.

[0007] Patent Document 3 proposes a method for producing a polyester resin composition in which a sulfonic acid compound is added and no metal elements other than a polymerization catalyst are added. However, the amount of phosphoric acid added is large, and is insufficient to obtain electrostatic applicability for film formation.

[0008] JP 2006-249213 A International Publication No. 1990 / 8171 JP 10-36495 A

[0009] However, simply adding a sulfonic acid compound or a phosphonium sulfonate compound to a polyester resin composition is insufficient to obtain electrostatic applicability for film formation. Furthermore, the addition of a sulfonic acid compound and an alkali metal leads to the generation of foreign matter, and the heat resistance of the polyester resin composition deteriorates, causing gelation. In other words, the above-mentioned conventional techniques are insufficient to simultaneously improve electrostatic applicability during film formation, reduce foreign matter derived from metal compounds, and suppress the generation of gel-like foreign matter by improving heat resistance. The object of the present invention is to provide a polyester resin composition that has low foreign matter content, good color tone, excellent transparency, excellent heat resistance and hydrolysis resistance, and good electrostatic applicability during film formation.

[0010] As a result of extensive research to solve the above problems, the present invention has the following features: (1) A polyester resin composition having an intrinsic viscosity of 0.55 dL / g or more, wherein the content of a p-toluenesulfonic acid component is 0.07 to 0.65 mol / t and the content of a quaternary phosphonium component is 0.07 to 0.65 mol / t relative to the total weight of the polyester resin composition, the heat resistance parameter X represented by formula 1 is 1.0≦X≦1.3, and the number of foreign particles having a circle equivalent diameter of 0.2 μm or more is 650 / 0.1 mm 2 The melting resistivity is 4.0 × 10 6A polyester resin composition having a viscosity of Ω·cm or less and a color b value measured by a color difference meter of 10.0 or less.

[0011]

[0012] (2) The polyester resin composition according to (1), wherein the content of alkali metal elements is 3 ppm by weight or less, relative to the total weight of the polyester resin composition. (3) The polyester resin composition according to (2), wherein the content of antimony element is 15 ppm by weight or less, and the content of titanium element is 0.1 ppm by weight to 20 ppm by weight, relative to the total weight of the polyester resin composition. (4) The polyester resin composition according to (3), wherein the content of manganese element is 5 to 40 ppm by weight, and the content of phosphorus element is 3 to 50 ppm by weight, relative to the total weight of the polyester resin composition. (5) The polyester resin composition according to (2), wherein the content of antimony element is 15 ppm by weight or less, and the content of germanium element is 5 ppm by weight to 150 ppm by weight, relative to the total weight of the polyester resin composition. (6) The polyester resin composition according to (5), having a manganese content of 5 to 40 ppm by weight and a phosphorus content of 3 to 50 ppm by weight, relative to the total weight of the polyester resin composition. (7) The polyester resin composition according to (2), having an antimony content of 15 ppm by weight or less and an aluminum content of 0.1 ppm by weight to 100 ppm by weight, relative to the total weight of the polyester resin composition. (8) The polyester resin composition according to (7), having a manganese content of 5 to 40 ppm by weight and a phosphorus content of 3 to 50 ppm by weight, relative to the total weight of the polyester resin composition. (9) The polyester resin composition according to (2), having an antimony content of 50 ppm by weight to 150 ppm by weight, relative to the total weight of the polyester resin composition. (10) The polyester resin composition according to (9), wherein the manganese element content is 5 to 40 ppm by weight and the phosphorus element content is 3 to 50 ppm by weight, based on the total weight of the polyester resin composition.(11) A polyester resin composition having an intrinsic viscosity of 0.55 dL / g or more, wherein the content of a p-toluenesulfonic acid component is 0.07 to 0.65 mol / t, the content of a quaternary phosphonium component is 0.07 to 0.65 mol / t, and the content of an alkali metal element is 3 ppm by weight or less, relative to the total weight of the polyester resin composition; the heat resistance parameter X represented by Equation 1 is 1.0≦X≦1.3; and the number of foreign particles having a circle equivalent diameter of 0.2 μm or more is 630 / 0.1 mm. 2 Hereinafter, a polyester resin composition having a color tone b value of 10.0 or less as measured by a color difference meter.

[0013]

[0014] (12) The polyester resin composition according to (11), wherein the antimony content is 15 ppm by weight or less and the titanium content is 0.1 ppm by weight to 20 ppm by weight, relative to the total weight of the polyester resin composition. (13) The polyester resin composition according to (12), wherein the manganese content is 5 to 40 ppm by weight and the phosphorus content is 3 to 50 ppm by weight, relative to the total weight of the polyester resin composition. (14) The polyester resin composition according to (11), wherein the antimony content is 15 ppm by weight or less and the germanium content is 5 ppm by weight to 150 ppm by weight, relative to the total weight of the polyester resin composition. (15) The polyester resin composition according to (14), wherein the manganese content is 5 to 40 ppm by weight and the phosphorus content is 3 to 50 ppm by weight, relative to the total weight of the polyester resin composition. (16) The polyester resin composition according to (11), wherein the antimony content is 15 ppm by weight or less and the aluminum content is 0.1 ppm by weight to 100 ppm by weight, relative to the total weight of the polyester resin composition. (17) The polyester resin composition according to (16), wherein the manganese content is 5 to 40 ppm by weight and the phosphorus content is 3 to 50 ppm by weight, relative to the total weight of the polyester resin composition. (18) The polyester resin composition according to (11), wherein the antimony content is 50 ppm by weight to 150 ppm by weight, relative to the total weight of the polyester resin composition. (19) The polyester resin composition according to (18), wherein the manganese content is 5 to 40 ppm by weight and the phosphorus content is 3 to 50 ppm by weight, relative to the total weight of the polyester resin composition. (20) A polyester film obtained using the polyester resin composition according to any one of (1) to (19).

[0015] The present invention provides a polyester resin composition which has little foreign matter, good color tone, excellent transparency, excellent heat resistance and hydrolysis resistance, and good electrostatic applicability during film formation, and which has few defects due to exposure damage when used as a film for a dry film resist support.

[0016] The present invention will be described in detail below. In this specification, "weight," "wt %," and "parts by weight" are synonymous with "mass," "mass %," and "parts by mass," respectively. "Element" may also be used synonymously with "atom."

[0017] The polyester resin composition used in the present invention refers to a polyester resin composition obtained by polycondensation of a dicarboxylic acid component and a diol component.

[0018] Examples of the dicarboxylic acid component of the present invention include terephthalic acid, 2,6-naphthalenedicarboxylic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 5-sodium sulfoisophthalic acid, oxalic acid, succinic acid, adipic acid, sebacic acid, malonic acid, and dimer acid. More preferred embodiments of the dicarboxylic acid of the present invention are terephthalic acid, 2,6-naphthalenedicarboxylic acid, isophthalic acid, or alkyl esters thereof, because they have a high melting point and can provide a polyester composition that is easily processable into films, fibers, and the like. Terephthalic acid or its alkyl esters are more preferred, because they have a high melting point and provide better processability.

[0019] The diol component of the present invention may be selected from aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,2-hexanediol, 1,6-hexanediol, and neopentyl glycol; saturated alicyclic primary diols such as cyclohexanedimethanol, cyclohexanediethanol, norbornanedimethanol, norbornanediethanol, tricyclodecanedimethanol, tricyclodecanediethanol, decalindimethanol, and decalindiethanol; saturated heterocyclic primary diols containing cyclic ethers such as isosorbide; and other cycloaliphatic diols. Examples of suitable diols include various alicyclic diols such as cyclohexanediol, bicyclohexyl-4,4'-diol, 2,2-bis(4-hydroxycyclohexylpropane), 2,2-bis(4-(2-hydroxyethoxy)cyclohexyl)propane, cyclopentanediol, 3-methyl-1,2-cyclopentadiol, 4-cyclopentene-1,3-diol, and adamantanediol, and aromatic diols such as paraxylene glycol, bisphenol A, bisphenol S, styrene glycol, 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, and 9,9'-bis(4-hydroxyphenyl)fluorene. In addition to diols, polyfunctional alcohols such as trimethylolpropane and pentaerythritol can also be used, provided that the effects of the present invention are not impaired. Among these, diols with a boiling point of 230°C or less are preferred because they can be easily distilled out of the reaction system, and aliphatic diols are more preferred because they are low cost and highly reactive. Furthermore, ethylene glycol is particularly preferred from the viewpoint of the mechanical properties of the resulting polyester resin composition and molded articles thereof.

[0020] The polyester in the present invention is not particularly limited, but preferably contains, as a main constituent, at least one structural unit selected from ethylene terephthalate, ethylene-2,6-naphthalate, propylene terephthalate, butylene terephthalate, hexamethylene terephthalate, cyclohexanedimethylene terephthalate, propylene-2,6-naphthalate, butylene-2,6-naphthalate, hexamethylene-2,6-naphthalate, and cyclohexanedimethylene-2,6-naphthalate units. Among these, polyesters containing ethylene terephthalate as a main constituent unit are particularly preferred due to their excellent moldability. Two or more polyesters may be mixed, or copolymerized polyesters may be used, as long as the effects of the present invention are not impaired. However, from the viewpoint of not impairing the thermal properties of the polyester resin composition, such as the melting point and glass transition temperature, it is preferred that 99 mol % or more of the polyester's structural units be ethylene terephthalate, and it is particularly preferred that the polyester be polyethylene terephthalate, which is substantially free of copolymerized components.

[0021] The polyester resin composition of the present invention must contain a p-toluenesulfonic acid component and a quaternary phosphonium component. By including a p-toluenesulfonic acid component and a quaternary phosphonium component in the polyester resin composition, good electrostatic applicability can be obtained during film formation.

[0022] The content of the p-toluenesulfonic acid component in the polyester resin composition of the present invention must be 0.07 to 0.65 mol / t relative to the total weight of the polyester resin composition. It is preferably 0.20 to 0.60 mol / t, and more preferably 0.25 to 0.50 mol / t. If the content of the p-toluenesulfonic acid component is less than 0.07 mol / t, the melt resistivity of the polyester resin composition when melted may increase, resulting in poor electrostatic applicability during film formation. If the content of p-toluenesulfonic acid exceeds 0.65 mol / t, foreign matter derived from the p-toluenesulfonic acid component may worsen the solution haze of the polyester resin composition, and the sulfonic acid groups may also worsen the hydrolysis resistance of the polyester resin composition.

[0023] In the present invention, the term "p-toluenesulfonic acid component" refers to a compound having a p-toluenesulfonate anion, such as p-toluenesulfonic acid and its alkali metal salts. Specific examples include p-toluenesulfonic acid, sodium p-toluenesulfonate, potassium p-toluenesulfonate, and methyl p-toluenesulfonate. However, from the perspective of suppressing the formation of foreign matter in the polyester resin composition, it is preferable that the p-toluenesulfonic acid component does not contain an alkali metal, and p-toluenesulfonic acid is preferred. Since the p-toluenesulfonic acid component does not have an ester-forming functional group, it is dispersed in the polyester resin without being copolymerized with it. This allows for good electrostatic applicability during film formation without impairing the thermal properties of the polyester resin composition, such as the melting point and glass transition point. In addition, because it does not have an ester-forming functional group, it can suppress the formation of foreign matter derived from the sulfonic acid compound, even if it forms. The use of a linear alkyl group having 6 or more carbon atoms or an aryl group having 8 or more carbon atoms other than the p-toluenesulfonic acid component is undesirable because, if foreign matter derived from the sulfonic acid compound is formed, the foreign matter tends to become coarse and, in addition, in the process of discharging the polyester resin composition in strand form from a polycondensation reaction tank into cold water and pelletizing it, the cold water tends to foam more, impairing productivity.On the other hand, the use of benzenesulfonic acid or an alkylsulfonic acid having 5 or less carbon atoms is undesirable because it is less likely to remain in the polyester resin composition, resulting in poor electrostatic applicability during film formation.

[0024] The polyester resin composition of the present invention must have a quaternary phosphonium component content of 0.07 to 0.65 mol / t relative to the total weight of the polyester resin composition. This is preferably 0.10 to 0.49 mol / t, and more preferably 0.15 to 0.33 mol / t. If the quaternary phosphonium component content is less than 0.07 mol / t, the melt resistivity of the polyester resin composition when melted may increase, resulting in poor electrostatic applicability during film formation. If the quaternary phosphonium component content exceeds 0.65 mol / t, foreign matter may be generated, and the solution haze of the polyester resin composition may worsen.

[0025] In the present invention, the quaternary phosphonium component refers to a compound having a quaternary phosphonium cation. Specific examples of the quaternary phosphonium include tetraethylphosphonium, tetrabutylphosphonium, tetrahexylphosphonium, methyltributylphosphonium, ethyltributylphosphonium, octyltributylphosphonium, hexadecyltributylphosphonium, benzyltrimethylphosphonium, benzyltriethylphosphonium, and 3-(trifluoromethyl)phenyltrimethylphosphonium. Examples of the quaternary phosphonium component include hydroxides and halides such as chlorides and bromides of these compounds. Among these, tetrabutylphosphonium hydroxide is preferred.

[0026] In the present invention, the method for incorporating the p-toluenesulfonic acid component and the quaternary phosphonium component into the polyester resin composition is not particularly limited. This can be achieved by known methods, such as adding them during the polycondensation reaction of the polyester resin composition or kneading them with the polyester resin composition after the polycondensation reaction using a twin-screw kneading extruder or the like. In particular, in order to suppress foreign matter in the polyester resin composition derived from p-toluenesulfonic acid or the quaternary phosphonium component, a method for incorporating them is preferred in which the p-toluenesulfonic acid component and the quaternary phosphonium component are added separately to the reaction system before the start of the polycondensation reaction of the polyester resin composition. Another suitable method is to neutralize the p-toluenesulfonic acid component and the quaternary phosphonium component to prepare a diol solution of quaternary phosphonium p-toluenesulfonate, pass the solution through a filter, and then add the solution to the reaction system before the start of the polycondensation reaction.

[0027] The intrinsic viscosity of the polyester resin composition of the present invention is 0.55 dL / g or more. There is no upper limit, but it is preferably 0.75 dL / g or less. If it is less than 0.55 dL / g, the mechanical properties during film molding may be inadequate. From the viewpoints of reducing the temperature rise due to shear heat during melt extrusion in film molding, suppressing the regeneration of cyclic trimers when the resin is melted, and preventing deterioration of mechanical properties during film molding due to thermal degradation of the resin, the intrinsic viscosity of the polyester resin composition is preferably 0.60 dL / g or more.

[0028] The polyester resin composition of the present invention must have a heat resistance parameter X, represented by Formula 1, that satisfies 1.0≦X≦1.3. Preferably, 1.0≦X≦1.2, and more preferably, 1.0≦X≦1.1. The heat resistance parameter X in the present invention is a parameter that indicates the heat resistance stability of the polyester resin composition. When the polyester is not modified at all, X=1, and the more modified it is, the larger the value becomes. When X exceeds 1.3, the heat resistance of the polyester resin composition decreases, and when formed into a film, a large amount of gel-like foreign matter is generated. Details of the method for measuring the heat resistance parameter X in a polyester resin composition will be explained in the examples.

[0029]

[0030] 1610 cm -1 is an IR absorption peak characteristic of thermally denatured polyesters (gelled products formed by repeated hydrolysis, thermal decomposition and crosslinking reactions of polyesters), and 1580 cm -1 is the IR absorption peak of the polyester main chain. -1 The reason for this is to take into consideration measurement errors, but the peaks with the highest absorption intensities within this range are defined as the absorptions of the thermally modified polyester and the polyester main chain, respectively. -1 Absorption near 1610 cm -1 The ratio of the absorptions in the vicinity indicates the ratio of the heat-modified polyester to the polyester main chain.

[0031] The polyester resin composition of the present invention has a particle count of 650 particles / 0.1 mm2 with a circular equivalent diameter of 0.2 μm or more. 2 It is necessary that the number of particles is less than 630 / 0.1 mm. 2 More preferably, 600 pieces / 0.1 mm or less. 2 More preferably, 500 pieces / 0.1 mm or less 2 The polyester resin composition contains 650 foreign matters per 0.1 mm2 of equivalent circle diameter of 0.2 μm or more. 2 If more foreign matter is present, the transparency of the polyester resin composition may be impaired. Details of the method for measuring the number of foreign matter particles in the polyester resin composition will be described in the Examples.

[0032] The first polyester resin composition of the present invention has a melt resistivity of 4.0×10 6 The second polyester resin composition must have a melt resistivity of 4.0×10 6 It is preferably 3.5×10 Ω cm or less. 6 Ω cm or less, and more preferably 3.0 × 10 6 The melt resistivity of the polyester resin composition is 4.0×10 6 If the resistivity is greater than Ω·cm, the electrostatic applicability may be poor when the polyester resin composition is used to form a film. Details of the method for measuring the melt resistivity of the polyester resin composition will be described in the examples.

[0033] The polyester resin composition of the present invention must have a color tone b value of 10.0 or less as measured by a color difference meter. The higher the color tone b value, the more yellowish the polyester resin composition. A value above 10.0 results in a strong yellowish appearance, making this unsuitable. Furthermore, the color tone b value is preferably 9.0 or less. In the polyester resin composition of the present invention, known compounds can be used as the polycondensation reaction catalyst. Examples include oxides, carboxylates, acetates, hydroxides, chelate complexes, and alkoxides of antimony, titanium, aluminum, tin, germanium, zinc, cobalt, lead, manganese, and magnesium, as well as hydrates of these metal compounds. These polycondensation reaction catalysts may be added in the form of powder, slurry, or solution. From the viewpoint of dispersibility, they are preferably added as a solution or slurry. The solvent used in this case is preferably the same as that of the diol component of the polyester resin composition. When an antimony compound is used as a polycondensation reaction catalyst in the polyester resin composition of the present invention, the antimony element content is preferably in the range of 50 ppm by weight to 150 ppm by weight relative to the total weight of the polyester resin composition, from the viewpoints of polymerization reactivity and activity in decomposition reactions. An antimony element content exceeding 150 ppm by weight is undesirable because the amount of metallic antimony in the polyester resin composition increases, resulting in the formation of foreign matter during film processing. An antimony element content below 50 ppm by weight may result in insufficient polymerization activity, preventing the polyester resin composition from achieving the target intrinsic viscosity. From the viewpoints of suppressing deterioration of solution haze and suppressing metallic antimony in the polyester resin composition, the antimony element content is preferably in the range of 50 ppm by weight to 120 ppm by weight, and even more preferably in the range of 50 ppm by weight to 100 ppm by weight.

[0034] When a titanium compound is used as a polycondensation reaction catalyst in the polyester resin composition of the present invention, the antimony element content is preferably 15 ppm by weight or less, more preferably 10 ppm by weight or less, based on the total weight of the polyester resin composition. Furthermore, the titanium element content is preferably 0.1 to 20 ppm by weight, more preferably 2 to 15 ppm by weight. An antimony element content of 15 ppm by weight or less can reduce the amount of metallic antimony-derived foreign matter in the polyester resin composition. Metallic antimony is generated by the reduction of antimony compounds such as antimony trioxide, and is known to become foreign matter in the polyester resin composition, causing reduced transparency and defects during film molding. A titanium element content of more than 20 ppm by weight is undesirable because it deteriorates the color tone b value and heat resistance of the polyester resin composition. A titanium element content of less than 0.1 ppm by weight can result in insufficient polymerization activity, preventing the polyester resin composition from achieving the target intrinsic viscosity.

[0035] When a germanium compound is used as a polycondensation reaction catalyst in the polyester resin composition of the present invention, the antimony content is preferably 15 ppm by weight or less, more preferably 10 ppm by weight or less, relative to the total weight of the polyester resin composition. Furthermore, the germanium content is preferably 5 ppm by weight to 150 ppm by weight. When the antimony content is 15 ppm by weight or less, foreign matter derived from metallic antimony in the polyester resin composition can be reduced, thereby suppressing defects during film molding. When the germanium content exceeds 150 ppm by weight, foreign matter is more likely to be generated, and the solution haze of the polyester resin composition may worsen. When the germanium content is less than 5 ppm by weight, the polymerization activity may be insufficient, and the polyester resin composition may not reach the target intrinsic viscosity.

[0036] When an aluminum compound is used as a polycondensation reaction catalyst in the polyester resin composition of the present invention, the antimony content is preferably 15 ppm by weight or less, more preferably 10 ppm by weight or less, based on the total weight of the polyester resin composition. Furthermore, the aluminum content is preferably 0.1 ppm by weight to 100 ppm by weight, with the upper limit of the aluminum content being more preferably 50 ppm by weight, even more preferably 30 ppm by weight. Furthermore, the lower limit of the aluminum content is more preferably 3 ppm by weight. An antimony content of 15 ppm by weight or less can reduce the amount of metallic antimony-derived foreign matter in the polyester resin composition, thereby suppressing defects during film molding. An aluminum content exceeding 100 ppm by weight is undesirable because it increases the likelihood of foreign matter generation, worsening the solution haze of the polyester resin composition and deteriorating the color tone b value and heat resistance. An aluminum content of less than 0.1 ppm by weight can result in insufficient polymerization activity, preventing the polyester resin composition from achieving the target intrinsic viscosity.

[0037] The polyester resin composition of the present invention can contain elemental manganese. The content of elemental manganese relative to the total weight of the polyester resin composition is preferably 5 to 40 ppm by weight, more preferably 5 to 30 ppm by weight. By incorporating elemental manganese, gel-like foreign matter can be reduced. However, if the content of elemental manganese exceeds 40 ppm by weight, the amount of foreign matter increases, which undesirably worsens the solution haze of the polyester resin composition. Furthermore, if the content of elemental manganese is less than 5 ppm by weight, the amount of gel-like foreign matter produced increases, which is undesirable.

[0038] The polyester resin composition of the present invention may contain a phosphorus compound other than the quaternary phosphonium component. The phosphorus compound other than the quaternary phosphonium component may be one or more selected from the group consisting of phosphoric acid, phosphorous acid, phosphonic acid, phosphonoacetic acid, or their methyl esters, ethyl esters, phenyl esters, and half esters. Two or more of these may be mixed and used, and phosphoric acid is more preferred.

[0039] The polyester resin composition of the present invention preferably has a phosphorus content of 3 to 50 ppm by weight, and more preferably 5 to 40 ppm by weight, relative to the total weight of the polyester resin composition. The phosphorus content represents the total amount of the quaternary phosphonium component and other phosphorus compounds. A phosphorus content of more than 50 ppm by weight is undesirable because it increases the amount of foreign matter and worsens the solution haze of the polyester resin composition. A phosphorus content of less than 3 ppm by weight is undesirable because it increases the melt resistivity of the polyester resin composition when melted, resulting in poor electrostatic applicability during film formation.

[0040] The polyester resin composition of the present invention may contain an alkali metal element within a range that does not impair the effects of the present invention. However, from the viewpoint of suppressing foreign matter having a circular equivalent diameter of 0.2 μm or more and suppressing an increase in solution haze of the polyester resin composition, the content of alkali metals is preferably 3 ppm by weight or less relative to the total weight of the polyester resin composition, and more preferably is substantially free of alkali metals. To incorporate an alkali metal element into the polyester resin composition of the present invention, an alkali metal compound is used. Examples of the alkali metal compound include lithium acetate, alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide, alkali metal phosphate salts such as sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, and tripotassium phosphate, and alkali metal salts of sulfonic acid compounds such as sodium methanesulfonate, potassium methanesulfonate, sodium butylsulfonate, potassium butylsulfonate, sodium trifluoromethanesulfonate, potassium trifluoromethanesulfonate, sodium tetrafluoroethanesulfonate, and tetrafluoroethanesulfonic acid. Examples of alkali metal compounds include potassium, sodium nonafluorobutanesulfonate, potassium nonafluorobutanesulfonate, sodium benzenesulfonate, potassium benzenesulfonate, sodium p-toluenesulfonate, potassium p-toluenesulfonate, sodium 2,4,6-trimethylbenzenesulfonate, potassium 2,4,6-trimethylbenzenesulfonate, sodium styrenesulfonate, potassium styrenesulfonate, sodium perfluorooctane sulfonate, potassium perfluorooctane sulfonate, sodium heptadecafluorooctane sulfonate, potassium heptadecafluorooctane sulfonate, etc. These alkali metal compounds can be incorporated into the polyester resin composition by known methods, such as by adding them during the polycondensation reaction of the polyester resin composition or by kneading them with the polyester resin composition after the polycondensation reaction using a twin-screw kneading extruder or the like.

[0041] The polyester resin composition of the present invention can contain particles. Examples of inorganic particles that can be contained in the polyester resin composition of the present invention include silica, alumina, barium sulfate, barium carbonate, magnesium oxide, magnesium sulfate, magnesium carbonate, zinc oxide, zinc sulfide, zinc carbonate, titanium dioxide, cerium oxide, zirconium oxide, iron oxide, kaolin, talc, mica, carbon black, and silicon. Examples of organic particles include crosslinked polystyrene, crosslinked silicon, crosslinked acrylic, crosslinked styrene-acrylic, crosslinked polyester, polyimide, and melamine resin particles. However, the type of particle is not particularly limited. From the viewpoints of economy, thermal stability, and particle dispersibility, silica particles, alumina particles, and crosslinked polystyrene particles are preferably used.

[0042] The method for incorporating particles into the polyester resin composition of the present invention is not particularly limited, but from the viewpoint of improving particle dispersibility, it is preferable to incorporate particles into the polyester resin composition by a method of adding them during the polycondensation reaction of the polyester resin composition or a method of kneading them with the polyester resin composition after the polycondensation reaction using a twin-screw kneading extruder, etc. Furthermore, the number of particle types to be incorporated into the polyester resin composition of the present invention is not particularly limited as long as the effects of the present invention are not impaired, and one or more types of particles can be incorporated.

[0043] The form of the particles to be added to the polyester resin composition of the present invention may be either a powder or a slurry, and from the viewpoint of dispersibility, it is preferable to add the particles as a slurry. The slurry may be either a water slurry or a slurry of the diol component of the polyester composition, but from the viewpoint of particle dispersibility in the polyester resin composition, it is preferable that the slurry is the same as the diol component of the polyester.

[0044] The method for producing the polyester resin composition of the present invention will be specifically described below.

[0045] For example, when the polyester in the present invention is polyethylene terephthalate (hereinafter referred to as PET), it is usually produced by a process in which terephthalic acid or dimethyl terephthalate and ethylene glycol are used as raw materials, and a low polymer such as bishydroxyethyl terephthalate (hereinafter referred to as BHET) is obtained by a reaction such as an esterification reaction or a transesterification reaction, and then a high molecular weight PET is obtained by a polycondensation reaction.

[0046] The reaction for obtaining low-polymer BHET is not particularly limited and can be carried out by a known reaction. For example, BHET can be obtained by a transesterification reaction using dimethyl terephthalate and ethylene glycol as raw materials, which proceeds by adding a transesterification catalyst, or by an esterification reaction using terephthalic acid and ethylene glycol as raw materials, which proceeds without a catalyst due to the autocatalytic action of carboxylic acid. Alternatively, BHET can be obtained by depolymerizing recycled PET products. The esterification reaction is preferred because the reaction proceeds sufficiently without a catalyst due to the autocatalytic action of carboxylic acid, eliminating the need for adding a reaction catalyst such as a calcium compound, magnesium compound, or manganese compound. By carrying out the esterification reaction without a catalyst, thermal decomposition and the generation of foreign matter during the polycondensation reaction can be suppressed.

[0047] The resulting BHET is then transferred to a polymerization vessel, where additives such as a p-toluenesulfonic acid component and a quaternary phosphonium component, as well as a polycondensation reaction catalyst, are added. The temperature inside the vessel is then slowly heated to 279°C, and the pressure is reduced from normal pressure to 133 Pa or less. As the polymerization reaction progresses, the viscosity of the reactants increases. The reaction is terminated when a predetermined stirring torque is reached, yielding molten PET. The resulting molten PET is then extruded in the form of strands from a die, cooled, and pelletized using a cutter to produce a polyester resin composition.

[0048] The obtained polyester resin composition is preferably pre-crystallized before the drying step. Pre-crystallization can be performed by applying a mechanical impact to the polyester resin composition to perform a shearing treatment, or by performing a heat treatment under a hot air stream.

[0049] The polyester composition of the present invention may be subjected to solid-state polymerization to obtain a high-molecular-weight polyester resin composition. The solid-state polymerization can be carried out by heating the polyester composition under an inert gas atmosphere or under reduced pressure at a temperature below the melting point of the polyester resin composition, without any particular limitations on the apparatus or method. The inert gas may be any gas inert to the polyester resin composition, such as nitrogen, helium, or carbon dioxide, but nitrogen is preferred for economic reasons. Under reduced pressure conditions, achieving a higher vacuum is advantageous because it shortens the time required for the solid-state polymerization reaction; specifically, maintaining a pressure of 110 Pa or less is preferred.

[0050] The polyester resin composition of the present invention can be suitably used for various applications such as films, fibers, and molded articles, and is particularly suitable for use in films due to its excellent electrostatic applicability and transparency. When molding the polyester resin composition of the present invention into a film, the film can be molded using a known molding method. When processing the polyester resin composition of the present invention into a film, one or more additives, such as colorants including pigments and dyes, lubricants, antistatic agents, flame retardants, ultraviolet absorbers, antibacterial agents, nucleating agents, plasticizers, and mold release agents, can be added within a range that does not impair the effects of the present invention.

[0051] Films made from the polyester resin composition of the present invention may be unstretched films obtained by melt extrusion, or may be stretched films obtained by uniaxial or biaxial stretching. Furthermore, when biaxial stretching is performed, sequential biaxial stretching or simultaneous biaxial stretching may be used. For example, pellets of the obtained polyester resin composition are vacuum-dried at 180°C for at least 3 hours, then fed into an extruder heated to 280-320°C under a nitrogen stream or vacuum to prevent a decrease in intrinsic viscosity. The pellets are then passed through a fiber-sintered stainless steel metal filter, extruded through a slit die, and cooled while applying a static charge to the casting drum to obtain an unstretched film. This unstretched film is then introduced into an infrared heater and stretched between rolls in the longitudinal direction, i.e., the running direction of the film, to obtain a uniaxially stretched film. The uniaxially stretched film is then stretched in the width direction perpendicular to the longitudinal direction while gripped with clips and heated, and then cooled to complete the crystal orientation, obtaining a sequentially biaxially stretched film. Alternatively, an unstretched film is stretched simultaneously in the longitudinal and transverse directions to obtain a simultaneously biaxially stretched film.

[0052] The film made of the polyester resin composition of the present invention may be a single-layer film made entirely of the same resin, or may be a single-layer film made by blending the polyester resin composition of the present invention with another polyester resin composition. It may also be a laminate film containing at least one film layer containing the polyester resin composition of the present invention. When a film layer containing the polyester resin composition of the present invention is laminated, the blending amount of the polyester resin composition of the present invention is not particularly limited. Furthermore, from the viewpoint of imparting easy slippage to the resulting polyester film, a polyester resin composition containing particles may be blended.

[0053] The polyester resin composition of the present invention has few foreign matters, good color tone, excellent transparency (haze), heat resistance, and good electrostatic applicability, and therefore can be suitably used for films for release applications such as substrates for molding green sheets for multilayer ceramic capacitors, separators for liquid crystal polarizers, and substrates for dry film resists, as well as high-quality films for optical applications. Polyester films made from the polyester resin composition of the present invention are characterized by good electrostatic applicability during molding, little unevenness in film thickness, little metal foreign matter, and excellent transparency.

[0054] The present invention will be described in more detail below with reference to examples. The methods for measuring physical properties and evaluating effects were as follows.

[0055] (1) Intrinsic Viscosity [η] of Polyester Resin Composition (Unit: dL / g) 0.1 g of polyester resin composition was weighed out to within 0.001 g accuracy and dissolved in 10 mL of o-chlorophenol (hereinafter referred to as OCP) by heating at 100°C for 30 minutes. The solution was cooled to room temperature, and 8 mL of the solution was placed in an Ostwald viscometer placed in a water bath at 25°C, and the number of seconds it took for the viscometer to pass the marked line was measured (A seconds). Similarly, using 8 mL of OCP alone, the number of seconds it took for the viscometer to pass the marked line was measured (B seconds). The intrinsic viscosity [η] was calculated using the formula: [η] = -1 + [1 + 4 × K × {(A / B) - 1}]^0.5 / (2 × K × C). Here, K is 0.343, and C is the concentration of the sample solution (g / 100 mL).

[0056] (2) Polymerization time of polyester resin composition In the polycondensation reaction of the polyester resin composition, the time when the temperature inside the apparatus started to rise and the pressure started to be reduced from normal pressure was defined as 0 minutes, and the time when a predetermined stirring torque was reached was defined as the end of the reaction, and this was defined as the polymerization time. A polymerization time exceeding 5 hours was deemed inappropriate because it impaired the production efficiency of the polyester resin composition.

[0057] (3) Element Contents in Polyester Resin Composition (Unit: ppm by weight) The contents of phosphorus (atom), magnesium (atom), manganese (atom), antimony (atom), titanium (atom), germanium (atom), and aluminum (atom) were determined by molding sample pellets of the polyester resin composition into a cylindrical shape using a melt press, measuring the fluorescent X-ray intensity using an X-ray fluorescence analyzer (model number: 3270) manufactured by Rigaku Corporation, and calculating from a calibration curve prepared in advance. The contents of alkali metal elements (lithium (atom), sodium (atom), and potassium (atom)) were quantified by atomic absorption spectrometry (polarized Zeeman atomic absorption spectrophotometer Model 180-80 manufactured by Hitachi, Ltd., flame: acetylene air).

[0058] (4) Color Tone of Polyester Resin Composition Resin pellets of the polyester resin composition were filled into a cylindrical powder measurement cell, and the b value was measured using a reflection method with a color difference meter (SM Color Meter SM-T) manufactured by Suga Test Instruments Co., Ltd., with n = 3. The arithmetic mean of the measured values ​​was taken as the color tone b value, which was used as an evaluation index for color tone. If this value was 9.0 or less, it was rated as good; if it was greater than 9.0 and less than 10.0, it was rated as pass; and if it exceeded 10.0, it was rated as fail.

[0059] (5) Content of p-toluenesulfonic acid component and quaternary phosphonium component (unit: mol / t) 0.5 g of a polyethylene terephthalate resin composition was dissolved in 8 mL of hexafluoroisopropanol, diluted with 10 mL of dichloromethane, and then reprecipitated by gradually adding 30 mL of methanol. Centrifugation was performed, and the supernatant was collected in a Daruma flask. The residue was washed with 10 mL of dichloromethane and 20 mL of methanol, and the supernatant was collected in the same Daruma flask. Nitrogen gas was gently blown into the Daruma flask while heating it to 80°C, and after concentration, the solution was made up to 100% with dimethyl sulfoxide to prepare a sample for liquid chromatography (hereinafter referred to as HPLC). The content (mol / t) of the p-toluenesulfonic acid component in the sample was determined using a pre-prepared calibration curve for p-toluenesulfonic acid, and the content (mol / t) of the quaternary phosphonium component was determined using a pre-prepared calibration curve for each substance (the same applies when tetrabutylphosphonium hydroxide, tetraethylphosphonium hydroxide, or other quaternary phosphonium compounds were added) using an HPLC system. Each component separated by HPLC was identified by liquid chromatography mass spectrometry (LC-MS).

[0060] The HPLC measurement conditions were as follows: Manufacturer: HITACHI Model name: Chromaster (detector: 5420, column oven: 6310) Column: ODS-2 6.0 x 250 mm, 5 μm (GL Sciences) Mobile phase: A:B = 40:60 (A: 0.1% phosphoric acid aqueous solution, B: acetonitrile) Flow rate: 1.2 mL / min Injection volume: 30 μL Column temperature: 45°C UV wavelength: 235 nm.

[0061] (6) Melt Resistivity of Polyester Resin Composition (Unit: Ω cm) After melting a polyethylene terephthalate resin composition at 290°C, a sample with an area of ​​0.5 cm 2 Two stainless steel electrodes were inserted in parallel with an 8 mm gap between them, and after the temperature stabilized, the resistance value (R) was measured using a resistance meter (HIOKI EE Corporation: Resistance Meter RM3545). Subsequently, the melting resistivity (ρ) was calculated using the formula ρ (Ω cm) = R × 0.5 / 0.8.

[0062] (7) Heat Resistance of Polyester Resin Composition (Main Chain Scission Rate (%BB)) (Unit: %) Five grams of a polyester resin composition was placed in a test tube, vacuum dried at 160°C for 5 hours, and then melted in a 290°C oil bath under a nitrogen gas flow of 300 mL / min for 6 hours. Using the intrinsic viscosity [η]6hr of the melt and the intrinsic viscosity [η]0hr before melting, the main chain scission rate was calculated according to the formula: Main Chain Scission Rate (%) = 0.27 × {[η]6hr^(-1.33) - [η]0hr^(-1.33)}. A value of 0.43% or less was considered good; a value greater than 0.43% but less than 0.48% was considered pass; and a value greater than 0.48% was considered fail.

[0063] (8) Amount of COOH End Groups in the Polyester Resin Composition (Unit: eq / t) Measured by the Maurice method (M.J. Maurice, F. Huizinga, Anal. Chem. Acta, 22, 363 (1960)). That is, 0.5 g of polyester resin composition was weighed to an accuracy of within 0.001 g. 50 ml of a solvent containing a 7 / 3 mass ratio of o-cresol and chloroform was added to the sample, and the mixture was heated until the internal temperature reached 90°C, after which the mixture was dissolved by heating and stirring for 20 minutes. A blank solution containing only the mixed solvent was also prepared by heating the mixture separately. The solution was cooled to room temperature, and titrated with a 1 / 50 N solution of potassium hydroxide in methanol using a potentiometric titrator. Titration was also performed on the blank solution containing only the mixed solvent. The amount of COOH end groups in the polyester resin composition was calculated using the following formula: Amount of COOH terminal group (eq / t)={(V1-V0)×N×f}×1000 / S, where V1 is the titration solution volume (mL) of the sample solution, V0 is the titration solution volume (mL) of the blank solution, N is the normality (N) of the titration solution, f is the titration solution factor, and S is the mass (g) of the polyester resin composition.

[0064] (9) Hydrolysis Resistance of Polyester Resin Composition (Increase in COOH End Groups (ΔCOOH)) (Unit: eq / t) The polyester resin composition was subjected to wet heat treatment in saturated steam at 155°C for 4 hours, and the amount of COOH end groups before and after treatment was measured to calculate the increase in COOH end groups (ΔCOOH = COOH after treatment - COOH before treatment) to evaluate hydrolysis resistance. The treatment device used was a PRESSERCOOKER 306SIII (manufactured by HIRAYAMA SEISAKUSHO CO., LTD.). The lower the ΔCOOH value, the better the hydrolysis resistance. A ΔCOOH value of 80.0 or less of the polyester resin composition of the present invention was rated as good, a value greater than 80.0 and less than 90.0 was rated as pass, and a value greater than 90.0 was rated as fail.

[0065] (10) Solution Haze of Polyester Resin Composition (Unit: %) 2.0 g of the polyester resin composition was dissolved in 20 mL of a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (60:40 wt%) by stirring at 100°C for 60 minutes, and after cooling to room temperature, the solution was placed in a 20 mm glass cell and measured with a haze computer (HGM-2DP) manufactured by Suga Test Instruments. If the solution haze measurement value was 1.0% or less, the transparency of the polyester resin composition was good; if it was more than 1.0% and 1.2% or less, the transparency was rated as pass; and if it exceeded 1.2%, it was rated as fail.

[0066] (11) Number of foreign particles in the polyester resin composition (unit: particles / 0.1 mm 2 ) The polyester resin composition is removed using a plasma low-temperature ashing method to expose large foreign matter. Processing conditions are selected to minimize damage to the foreign matter. The foreign matter is observed using a scanning electron microscope (SEM), and the foreign matter images are processed using an image analyzer. The SEM magnification is selected to be 1000x. Measurements are made at different observation locations over an area of ​​0.1 square mm, and of the white matter observed, those with a circular equivalent diameter of 0.2 μm or more are considered foreign matter, and the number of foreign matter particles is counted.

[0067] (12) Heat resistance parameter X (measurement of FT-IR absorption peaks before and after heat treatment) Sampling was performed from the inside of each sample, and the FT-IR of the polymer was measured before heat treatment and after heat treatment at 285°C for 5 hours under a nitrogen atmosphere using a micro-infrared spectrometer (FT-IR MICROSCOPE: Nicolet Continuum II (micro-FT-IR manufactured by ThermoFisher Scientific)). -1 and 1580 cm -1 ±10cm -1 The absorption intensity was determined. In order to minimize measurement variations, the same sample was measured five times and the arithmetic mean was used. The obtained absorption intensity was used to calculate the heat resistance parameter X according to Equation 1.

[0068]

[0069] (13) Number of metallic antimony particles in the filtered matter of the polyester resin composition (unit: particles / 0.1 mm 2 2.0 g of resin pellets of the polyester resin composition were dissolved in 20 mL of a dichloromethane-OCP mixed solvent and filtered through a membrane filter with a pore size of 0.1 μm. The foreign matter remaining on the filter after filtration was observed using a backscattered electron image of a scanning electron microscope (SEM), and the foreign matter image was processed using an image analyzer. The SEM magnification was set to 1000x. Measurements were conducted over an area of ​​0.1 square mm or more at different observation points, and the number of white matter observed, with those with a circular equivalent diameter of 0.2 μm or more, was counted as metallic antimony in the filtered matter, and this was used as an index of the number of metallic antimony in the polyester resin composition. The white matter observed in the backscattered electron image was confirmed to be antimony by observation using SEM-EDX (energy dispersive X-ray spectroscopy). The fewer the number of metallic antimony in the filtered matter, the better; 100 particles / 0.1 mm 2 If it is less than 101 pieces / 0.1 mm, it is good. 2 More than 500 pieces / 0.1mm 2 If it is less than 501 pieces / 0.1 mm, it passes. 2 If it was more than that, it was deemed a failure.

[0070] (14) Film-forming properties of polyester film (static application properties) When unstretched films were formed in the examples and comparative examples, the film-forming properties were judged according to the following criteria. ∘ (Good): A film could be formed without any problems. Δ (Pass): A decrease in adhesion to the casting drum was observed, but film formation was not a problem. × (Fail): Adhesion to the casting drum was poor, making it difficult to form a film.

[0071] (15) Conductive Circuit Yield Evaluation When stretched films were produced in the Examples and Comparative Examples, the conductor circuit yield was evaluated using the following procedure. (i) A negative resist "PMER N-HC600" manufactured by Tokyo Ohka Kogyo Co., Ltd. was applied to a one-side mirror-polished 6-inch Si wafer, and a 7 μm-thick resist layer was produced by spinning it with a large spinner. Next, a pre-heat treatment was performed for approximately 20 minutes at a temperature of 70°C using a nitrogen-circulating ventilated oven. (ii) The surface of the polyester film was placed in contact with the resist layer, and a polyester film was laminated onto the resist layer using a rubber roller. A photomask patterned with chromium metal was placed on top of the polyester film, and exposure was performed through the photomask using an I-line stepper. (iii) After peeling the polyester film from the resist layer, the resist layer was placed in a container containing developer N-A5 and developed for approximately 1 minute. The wafer was then removed from the developer and washed with water for approximately 1 minute. (iv) From the results of the open / short test of the conductor circuit created after development, those with an occurrence rate of open defects or short defects of less than 5% were evaluated as ○ (good), those with an occurrence rate of 5% or more but less than 10% were evaluated as △ (pass), and those with an occurrence rate of 10% or more were evaluated as × (fail). Note that an evaluation of △ or higher is considered to be at a practical level.

[0072] Example 1 A slurry consisting of 86 parts by weight of terephthalic acid and 37 parts by weight of ethylene glycol (1.15 times the molar ratio of terephthalic acid to terephthalic acid) was gradually added to an esterification reactor charged with 105 parts by weight of BHET dissolved at 250°C, and the esterification reaction was allowed to proceed while distilling off water. The temperature in the reaction system was controlled to 245 to 250°C, and the esterification reaction was terminated when the reaction rate reached 95%, and 105 parts by weight of the resulting esterification reaction product (equivalent to 100 parts by weight of PET) was charged in a molten state into a polymerization reactor equipped with a distillation device.

[0073] 0.0112 parts by weight of tetrabutylphosphonium hydroxide was added as an ethylene glycol solution, followed by 0.0077 parts by weight of p-toluenesulfonic acid as an ethylene glycol solution. Subsequently, 0.0090 parts by weight of manganese acetate tetrahydrate was added as an ethylene glycol solution, followed by 0.0084 parts by weight of diantimony trioxide as an ethylene glycol slurry. The pressure in the polymerization reactor was gradually reduced to 0.13 kPa or less over 35 minutes, and simultaneously the temperature was gradually increased to 279°C, and the polymerization reaction was carried out until the intrinsic viscosity of the polyester resin composition reached 0.62 dL / g. The polycondensation reactor was then returned to atmospheric pressure with nitrogen gas, and the polyester resin composition was extruded into cold water in the form of a strand, extruded into cylindrical pellets using an extrusion cutter, and the number of foreign matter particles of 0.2 μm or more in equivalent circle diameter was 490 / 0.1 mm. 2 , the melting resistivity is 2.2 × 10 6 A polyester resin composition having a viscosity of Ω·cm and a heat resistance parameter X of 1.1 was obtained.

[0074] The obtained polyester resin composition contained the p-toluenesulfonic acid component, the quaternary phosphonium component, elemental antimony, elemental phosphorus, and elemental manganese in the amounts shown in Table 1. The color tone b value was 6.8, the main chain scission rate (% BB) as a heat resistance index was 0.38%, the increase in COOH terminal groups (ΔCOOH) as a hydrolysis resistance index was 72.9 eq / t, and the solution haze was 0.9%, all of which were good values. In addition, the number of metallic antimony particles in the filtered matter was 270 / 0.1 mm 2 , which was within the acceptable range.

[0075] Subsequently, the resulting resin pellets of the polyester resin composition were dried under reduced pressure at 160°C for 8 hours, then fed into an extruder and melt-extruded at 285°C. The resulting unstretched sheet was cast onto an electrostatically charged casting drum at 20°C to obtain an unstretched sheet. This unstretched sheet was stretched 3.5 times in the longitudinal direction using a stretching roll heated to 90°C, then stretched 4.0 times in the transverse direction at 120°C using a tenter-type stretching machine, and then heat-set at 230°C for 10 seconds. After uniformly cooling in a cooling zone, the sheet was wound around a roll to obtain a polyester film with a thickness of 16 μm. The film-forming properties of this polyester film were evaluated to demonstrate good electrostatic applicability. Furthermore, the yield of conductor circuits using the resulting polyester film was evaluated to be good.

[0076] Examples 2 to 7, Comparative Examples 1 to 3 Polyester resin compositions and polyester films were obtained in the same manner as in Example 1, except that the amount of p-toluenesulfonic acid added was changed to the contents shown in Tables 1 and 2. The results are shown in Table 2. In Examples 2 to 4 and Comparative Example 1, as the p-toluenesulfonic acid content increased, the solution haze of the polyester resin composition increased due to an increase in foreign matter with a circular equivalent diameter of 0.2 μm or more, and ΔCOOH also increased. These indicators were within the acceptable range in Examples 2 to 4, but failed in Comparative Example 1. In Examples 5 to 7 and Comparative Example 2, as the p-toluenesulfonic acid content decreased, the melt resistivity increased, and the electrostatic applicability tended to deteriorate in the film-forming property evaluation of the polyester film. In addition, the number of metallic antimony atoms in the filtered residue of the polyester resin composition also increased. In addition, the yield evaluation of conductor circuits using the obtained polyester films tended to deteriorate. These indices were within the acceptable range for Examples 5 to 7, but were unsuccessful for Comparative Example 2, and the yield of the conductor circuit in Comparative Example 2 could not be evaluated because a film could not be obtained. Furthermore, in Comparative Example 3, the melt resistivity increased significantly because the p-toluenesulfonic acid component was not added, and the film-forming properties of the polyester film were unacceptable. The number of metallic antimony particles in the filtered matter of the polyester resin composition was also unacceptable, and the yield of the conductor circuit in Comparative Example 3 could not be evaluated because a film could not be obtained.

[0077] Examples 8 to 14, Comparative Examples 4 to 6 Polyester resin compositions and polyester films were obtained in the same manner as in Example 1, except that the amount of tetrabutylphosphonium hydroxide added was changed to the contents shown in Tables 1 and 2. The results are shown in Table 2. In Examples 8 to 11 and Comparative Example 4, as the quaternary phosphonium component content increased, the solution haze of the polyester resin composition increased due to an increase in foreign matter with a circular equivalent diameter of 0.2 μm or more. The number of metallic antimony particles in the filtered matter of the polyester resin composition also increased. Furthermore, the yield evaluation of the conductor circuit using the obtained polyester film tended to deteriorate. These indicators were within the acceptable range in Examples 8 to 11, but failed in Comparative Example 4. In Examples 12 to 14 and Comparative Example 5, as the quaternary phosphonium component content decreased, the melt resistivity increased, and the electrostatic applicability in the film-forming evaluation of the polyester film tended to deteriorate. Furthermore, ΔCOOH also tended to increase. These indices were within the acceptable range in Examples 12 to 14, but were unsuccessful in Comparative Example 5, and the yield of the conductor circuit could not be evaluated because a film could not be obtained. Furthermore, in Comparative Example 6, the melt resistivity increased significantly because a quaternary phosphonium component was not added, and the film-forming properties of the polyester film were unacceptable. The ΔCOOH value was also significantly unacceptable, and the yield of the conductor circuit could not be evaluated because a film could not be obtained.

[0078]

[0079]

[0080] Example 15 A slurry consisting of 86 parts by weight of terephthalic acid and 37 parts by weight of ethylene glycol (1.15 times the molar ratio of terephthalic acid to terephthalic acid) was gradually added to an esterification reactor charged with 105 parts by weight of BHET dissolved at 250°C, and the esterification reaction was allowed to proceed while distilling off water. The temperature in the reaction system was controlled to 245 to 250°C, and the esterification reaction was terminated when the reaction rate reached 95%, and 105 parts by weight of the resulting esterification reaction product (equivalent to 100 parts by weight of PET) was charged in a molten state into a polymerization reactor equipped with a distillation device.

[0081] 0.0175 parts by weight of tetrabutylphosphonium p-toluenesulfonate, which had been previously prepared by neutralizing equimolar amounts of p-toluenesulfonic acid and tetrabutylphosphonium hydroxide, was added as an ethylene glycol solution. Subsequently, 0.0090 parts by weight of manganese acetate tetrahydrate was added as an ethylene glycol solution. Then, 0.0050 parts by weight of tetra-n-butyl titanate was added as an ethylene glycol solution. The pressure in the polymerization reactor was gradually reduced to 0.13 kPa or less over 35 minutes. At the same time, the temperature was gradually increased to 279°C, and the polymerization reaction was carried out until the intrinsic viscosity of the polyester resin composition reached 0.62 dL / g. The polycondensation reactor was then returned to atmospheric pressure with nitrogen gas, and the polyester resin composition was extruded into cold water in the form of a strand. The extrusion cutter cut the resulting pellets into cylindrical pellets. The number of foreign matter particles with a circle equivalent diameter of 0.2 μm or more was 380 particles / 0.1 mm. 2 , the melting resistivity is 2.2 × 10 6 A polyester resin composition having a Ω-cm resistance and a heat resistance parameter X of 1.1 was obtained. A polyester film was also obtained in the same manner as in Example 1. The results are shown in Table 4. The color tone b value of the obtained polyester resin composition was a little high at 8.2, but was still within the good range. Furthermore, compared to the polyester resin composition of Example 1, there was less foreign matter with a circle equivalent diameter of 0.2 μm or more. Furthermore, since no antimony catalyst was used, metallic antimony was not observed in the filtered matter of the polyester resin composition. In an evaluation of the film-forming properties of this polyester film, the electrostatic applicability was good. Furthermore, the yield of conductor circuits using the obtained polyester film was evaluated as good.

[0082] Examples 16-19, Comparative Examples 7 and 8: A polyester resin composition and a polyester film were obtained in the same manner as in Example 15, except that the amount of tetra-n-butyl titanate added was changed to the titanium element content shown in Table 3. The results are shown in Table 4. In Examples 16 and 17 and Comparative Example 7, the color tone b value, % BB, and ΔCOOH tended to increase as the titanium element content increased, but these indicators were within the acceptable range for Examples 16 and 17. On the other hand, in Comparative Example 7, the color tone b value and % BB failed. In Examples 18 and 19 and Comparative Example 8, the polymerization time tended to increase as the titanium element content decreased, but Examples 18 and 19 were within the acceptable range. On the other hand, in Comparative Example 8, the titanium element content was low, resulting in insufficient activity in the polycondensation reaction, and the target intrinsic viscosity was not reached even after the polymerization time exceeded 5 hours. Therefore, evaluation of the properties of the polyester resin composition and polyester film was not performed.

[0083] Example 20 A polyester resin composition and polyester film were obtained in the same manner as in Example 15, except that 0.0072 parts by weight of germanium dioxide was added as an ethylene glycol solution instead of tetra-n-butyl titanate as a polycondensation reaction catalyst. The color tone b value was 6.8, %BB was 0.34%, ΔCOOH was 68.5 eq / t, and solution haze was 0.5%, all of which were good values. Because no antimony catalyst was used, metallic antimony was not observed in the filtered residue of the polyester resin composition. In an evaluation of the film-forming properties of the polyester film, electrostatic applicability was good, and the yield of conductor circuits using the obtained polyester film was evaluated as good.

[0084] (Examples 21 and 22, Comparative Examples 9 and 10) A polyester resin composition and a polyester film were obtained in the same manner as in Example 20, except that the amount of germanium dioxide added was changed to the germanium element content shown in Table 3. In Example 21, the number of foreign particles with a circle equivalent diameter of 0.2 μm or more was 610 / 0.1 mm. 2The solution haze of the polyester resin composition was 1.1%, which was within the acceptable range. In addition, in the evaluation of the film formability of the polyester film, the electrostatic applicability was good, and the yield of the conductor circuit using the obtained polyester film tended to deteriorate, but was within the acceptable range. In Comparative Example 9, the number of foreign particles with a circle equivalent diameter of 0.2 μm or more was 680 / 0.1 mm. 2 The viscosity increased even more, and the solution haze of the polyester resin composition was 1.4%, failing the test. In Example 22, the germanium element amount was lower and the polymerization time was longer than in Example 20, but all of the polyester resin composition property evaluations were within the acceptable range. In addition, the yield evaluation of the conductor circuit using the obtained polyester film tended to deteriorate, but was still within the acceptable range. In Comparative Example 10, the germanium element amount was even lower than in Example 22, and the activity of the polycondensation reaction was insufficient, so the target intrinsic viscosity was not reached even after the polymerization time exceeded 5 hours. Therefore, the property evaluation of the polyester resin composition and polyester film was not performed.

[0085] Example 23 A polyester resin composition and polyester film were obtained in the same manner as in Example 15, except that instead of adding tetra-n-butyl titanate as the polycondensation reaction catalyst, an ethylene glycol solution of aluminum acetate was added, and the aluminum element content was set as shown in Table 3. The color tone b value was 6.9, %BB was 0.38%, ΔCOOH was 70.6 eq / t, and solution haze was 0.9%, all of which were good values. Since no antimony catalyst was used, metallic antimony was not observed in the filtered residue of the polyester resin composition. In an evaluation of the film-forming properties of the polyester film, electrostatic applicability was good, and the yield of conductor circuits using the obtained polyester film was evaluated as good.

[0086] (Examples 24-28, Comparative Examples 11 and 12) Polyester resin compositions and polyester films were obtained in the same manner as in Example 23, except that the amount of aluminum acetate added was changed to the aluminum content shown in Table 3. In Examples 24-26 and Comparative Example 11, as the aluminum content increased, the solution haze of the polyester resin composition increased due to an increase in foreign matter with a circular equivalent diameter of 0.2 μm or more, and the color tone b value, % BB, and ΔCOOH tended to increase; however, these indicators were within the acceptable range in Examples 24-26. Furthermore, the yield evaluation of the conductor circuit using the polyester film obtained in Example 26 tended to deteriorate, but was still within the acceptable range. On the other hand, in Comparative Example 11, the % BB and solution haze were unacceptable, and the yield evaluation of the conductor circuit using the obtained polyester film was also unacceptable. In Examples 27 and 28 and Comparative Example 12, the polymerization time tended to increase as the aluminum content decreased, but Examples 27 and 28 were within the acceptable range. On the other hand, in Comparative Example 12, the content of aluminum element was low and the activity of the polycondensation reaction was insufficient, so the target intrinsic viscosity was not reached even after the polymerization time exceeded 5 hours. Therefore, the characteristics of the polyester resin composition and the polyester film were not evaluated.

[0087]

[0088]

[0089] Examples 29-35, Comparative Examples 13 and 14: Polyester resin compositions and polyester films were obtained in the same manner as in Example 1, except that the polycondensation reaction catalyst was changed from diantimony trioxide to tetra-n-butyl titanate, and the titanium element and p-toluenesulfonic acid component were changed to the contents shown in Table 5. The results are shown in Table 6. Example 29 had the same contents of p-toluenesulfonic acid component, quaternary phosphonium component, titanium element, and phosphorus element as Example 15, but the method of adding the p-toluenesulfonic acid component and quaternary phosphonium component was changed. As a result, the number of foreign matter particles with a circle-equivalent diameter of 0.2 μm or more decreased. In evaluations of the obtained polyester resin compositions and polyester films, all indicators were within the acceptable range. In Examples 30-32 and Comparative Example 13, as the p-toluenesulfonic acid component content increased, the amount of foreign matter with a circle-equivalent diameter of 0.2 μm or more increased, resulting in an increase in the solution haze of the polyester resin composition and an increase in ΔCOOH. These indices were within the acceptable range in Examples 30 to 32, but were unacceptable in Comparative Example 13. In Examples 33 to 35 and Comparative Example 14, the melt resistivity increased as the content of the p-toluenesulfonic acid component decreased, and the electrostatic applicability tended to deteriorate in the film-forming property evaluation of the polyester film, and while the indices were within the acceptable range in Examples 33 to 35, they were unacceptable in Comparative Example 14. Furthermore, in Comparative Example 14, the yield of the conductor circuit could not be evaluated because a film could not be obtained.

[0090] Examples 36-42, Comparative Examples 15 and 16: Polyester resin compositions and polyester films were obtained in the same manner as in Example 1, except that the polycondensation reaction catalyst was changed from diantimony trioxide to tetra-n-butyl titanate, and the contents of titanium, phosphorus, and the quaternary phosphonium component were changed to those shown in Table 5. The results are shown in Table 6. In Examples 36-39 and Comparative Example 15, as the quaternary phosphonium component content increased, the solution haze of the polyester resin composition increased due to an increase in foreign matter with a circle equivalent diameter of 0.2 μm or more. Examples 36-39 were within the acceptable range, but Comparative Example 15 failed. Furthermore, the yield evaluation of conductor circuits using the obtained polyester film tended to deteriorate in Example 39 but was within the acceptable range, while Comparative Example 15 failed. In Examples 40-42 and Comparative Example 16, as the quaternary phosphonium component content decreased, the melt resistivity increased, and the electrostatic applicability in the film-forming evaluation of the polyester film tended to deteriorate. ΔCOOH also tended to increase. These indices were within the acceptable range in Examples 40 to 42, but were unacceptable in Comparative Example 16. Furthermore, in Comparative Example 16, the yield of the conductor circuit could not be evaluated because a film could not be obtained.

[0091]

[0092]

[0093] Examples 43, 44, Comparative Examples 17, 18 In Examples 43, 44, and Comparative Example 17, polyester resin compositions and polyester films were obtained in the same manner as in Example 29, except that after the addition of tetra-n-butyl titanate, an ethylene glycol solution of manganese acetate was then added, resulting in the manganese content shown in Table 7. The results are shown in Table 8. In Example 43, the manganese content was reduced from the polyester resin composition of Example 29, resulting in a slight increase in the heat resistance parameter X. As a result, the yield of conductor circuits using the resulting polyester film tended to deteriorate, but was still within the acceptable range. Furthermore, in the film-forming property evaluation of the polyester film, the electrostatic applicability was good. In Example 44, the manganese content was increased compared to Example 29, resulting in a further increase in the number of foreign matter particles with a circle equivalent diameter of 0.2 μm or more and an increase in solution haze, but still within the acceptable range. Furthermore, in the film-forming property evaluation of the polyester film, the electrostatic applicability was good, and the yield of conductor circuits using the resulting polyester film was also good. In Comparative Example 17, the manganese element content was further increased from Example 44. The number of foreign matter particles with a circular equivalent diameter of 0.2 μm or more further increased, the solution haze increased, and the polyester film obtained was rejected, and the yield of the conductor circuit using the polyester film obtained was also rejected. In Comparative Example 18, the same procedure as in Example 29 was performed except that manganese acetate was not added. The heat resistance parameter X exceeded the specified range, and the yield of the conductor circuit using the polyester film obtained was also rejected.

[0094] Comparative Example 19 A polyester resin composition and a polyester film were obtained in the same manner as in Example 29, except that an ethylene glycol solution of magnesium acetate was added instead of manganese acetate to achieve the magnesium element content shown in Table 7. The results are shown in Table 8. The use of magnesium acetate caused the heat resistance parameter X to exceed the specified range, and therefore the yield evaluation of the conductor circuit using the obtained polyester film failed.

[0095] Examples 45 to 47 Polyester resin compositions and polyester films were obtained in the same manner as in Example 29, except that phosphoric acid was added as an ethylene glycol solution between the addition of tetrabutylphosphonium hydroxide and p-toluenesulfonic acid and the addition of tetra-n-butyl titanate, and the phosphorus content was adjusted to the value shown in Table 7. The results are shown in Table 8. In Example 45, all of the polyester resin composition properties were within the acceptable range, compared to the polyester resin composition of Example 29, which had a reduced manganese content and no phosphoric acid added. In Examples 46 and 47, the amount of phosphoric acid added was further increased from that of Example 45, thereby increasing the phosphorus content. As a result, all of the polyester resin compositions were within the acceptable range in the property evaluation.

[0096] Example 48 A polyester resin composition and a polyester film were obtained in the same manner as in Example 29, except that the quaternary phosphonium component was changed from tetrabutylphosphonium hydroxide to an ethylene glycol solution of tetraethylphosphonium hydroxide. The results are shown in Table 8. The obtained polyester resin composition had properties equivalent to those of the polyester resin composition of Example 29, and all of the indices were within the acceptable range. Furthermore, in an evaluation of the film-forming properties of the polyester film, the electrostatic applicability was good, and the yield of conductor circuits using the obtained polyester film was evaluated as good.

[0097] Comparative Examples 20-22: A polyester resin composition and a polyester film were obtained in the same manner as in Example 45, except that a sulfonic acid compound listed in Table 7 was used instead of p-toluenesulfonic acid. The results are shown in Table 8. In Comparative Example 20, dodecylbenzenesulfonic acid, which has a larger carbon number than p-toluenesulfonic acid, was used. As a result, the number of foreign particles with a circle-equivalent diameter of 0.2 μm or more was higher than that of the polyester resin composition of Example 45, and the solution haze was high, resulting in a failure. Furthermore, the melt resistivity was high, and the electrostatic applicability in the film-forming evaluation of the polyester film was unsatisfactory. The yield of the conductor circuit was not evaluated because a film could not be obtained. In Comparative Example 21, 3,5-dicarboxybenzenesulfonic acid, which has two ester-forming functional groups, was used. As a result, the number of foreign particles with a circle-equivalent diameter of 0.2 μm or more was higher than that of the polyester resin composition of Example 45, and the solution haze was high, resulting in a failure. As a result, the yield of the conductor circuit using the resulting polyester film was unsatisfactory. Furthermore, although the melt resistivity was high, the electrostatic applicability was within the acceptable range in the evaluation of polyester film formability. In Comparative Example 22, methanesulfonic acid, which has a smaller carbon number than p-toluenesulfonic acid, was used, resulting in a higher melt resistivity compared to the polyester resin composition of Example 45, and the electrostatic applicability was unacceptable in the evaluation of polyester film formability. Furthermore, the yield of the conductor circuit could not be evaluated because a film could not be obtained. (Example 49) 87 parts by weight of ethylene glycol was charged to a reactor per 250 parts by weight of the recovered PET product, and the temperature was simultaneously increased to initiate depolymerization at 240°C under normal pressure. The temperature was then gradually increased, and the depolymerization reaction was completed after 2 hours and 50 minutes. The reaction product, BHET, was filtered through a pleated filter with 10 μm openings, and 105 parts by weight (equivalent to 100 parts by weight of PET) was charged in a molten state into a polymerization reactor equipped with a distillation device. 0.0112 parts by weight of tetrabutylphosphonium hydroxide, then 0.0077 parts by weight of p-toluenesulfonic acid were added as an ethylene glycol solution, followed by 0.0090 parts by weight of manganese acetate tetrahydrate as an ethylene glycol solution, and then 0.0050 parts by weight of tetra-n-butyl titanate as an ethylene glycol solution.Subsequently, the pressure inside the polymerization reaction tank was gradually reduced to 0.13 kPa or less over 35 minutes, and at the same time, the temperature was gradually increased to 279°C, and the polymerization reaction was carried out until the intrinsic viscosity of the polyester resin composition reached 0.62 dL / g. Thereafter, the polycondensation reaction tank was returned to normal pressure with nitrogen gas, and the polyester resin composition was discharged into cold water in the form of a strand from a die and pelletized into cylindrical pellets using an extrusion cutter, and the number of foreign matter particles having an equivalent circle diameter of 0.2 µm or more was 400 / 0.1 mm. 2 , the melting resistivity is 2.2 × 10 6 A polyester resin composition having a resistivity of Ω·cm and a heat resistance parameter X of 1.1 was obtained. The obtained polyester resin composition contained the p-toluenesulfonic acid component, quaternary phosphonium component, titanium element, and phosphorus element in the amounts shown in Table 7. The color tone b value was 8.2, %BB was 0.41%, ΔCOOH was 77.2 eq / t, and solution haze was 0.7%, all of which were good values. Furthermore, since no antimony catalyst was used, metallic antimony was not observed in the filtered residue of the polyester resin composition. Subsequently, a polyester film was obtained in the same manner as in Example 1. In an evaluation of the film-forming properties of this polyester film, electrostatic applicability was good, and the yield of conductor circuits using the obtained polyester film was evaluated as good.

[0098]

[0099]

[0100] (Examples 50 to 53) Polyester resin compositions and polyester films were obtained in the same manner as in Example 1, except that the amount of diantimony trioxide added was changed to the contents shown in Table 9. The results are shown in Table 10. As the antimony element content of the obtained polyester resin compositions increased, the %BB and the number of metallic antimony particles in the filtered residue of the polyester resin compositions tended to increase, but all indicators were within the acceptable range. Furthermore, in an evaluation of the film-forming properties of the polyester films, the electrostatic applicability was good, and the yield of conductor circuits using the obtained polyester films was also good.

[0101] Examples 54 and 55: A polyester resin composition and a polyester film were obtained in the same manner as in Example 1, except that the p-toluenesulfonic acid component was replaced with a mixture of p-toluenesulfonic acid and sodium p-toluenesulfonate, and the alkali metal content was set as shown in Table 9. The results are shown in Table 10. As the alkali metal element content increased, the solution haze of the polyester resin composition increased due to an increase in foreign matter with a circle equivalent diameter of 0.2 μm or more, but was within the acceptable range. Meanwhile, in an evaluation of the film-forming properties of the obtained polyester film, the electrostatic applicability was good. Furthermore, the yield of conductor circuits using the obtained polyester film was evaluated as good in Example 54, and tended to deteriorate in Example 55, but was still within the acceptable range.

[0102] Comparative Example 23 A polyester resin composition and a polyester film were obtained in the same manner as in Example 1, except that the p-toluenesulfonic acid component was changed to sodium p-toluenesulfonate and the alkali metal content was set as shown in Table 9. The results are shown in Table 10. The obtained polyester resin composition had a higher alkali metal element content than the polyester resin composition of Example 55, and the number of foreign particles with a circle equivalent diameter of 0.2 μm or more was 760 / 0.1 mm 2 Since these were unsuitable, the solution haze of the polyester resin composition was 1.4%, which was unacceptable, and the yield of the conductor circuit using the obtained polyester film was also unacceptable.

[0103] Examples 56 and 57 A polyester resin composition and a polyester film were obtained in the same manner as in Example 1, except that phosphoric acid was added as an ethylene glycol solution between the addition of tetrabutylphosphonium hydroxide and p-toluenesulfonic acid and the addition of diantimony trioxide, and that an ethylene glycol solution of manganese acetate was added after the addition of diantimony trioxide, resulting in the contents shown in Table 9. The results are shown in Table 10. The color tone b value of the polyester resin composition obtained in Example 58 was 7.0, % BB was 0.29%, and ΔCOOH was 78.7 eq / t, all of which were good values. The solution haze was 1.1%, and the number of metallic antimony particles in the filtered product was 270 / 0.1 mm2 The color tone b value of the polyester resin composition obtained in Example 57 was 7.3, the % BB was 0.30%, and the ΔCOOH was 66.9 eq / t, all of which were good values. The solution haze was 1.1%, and the number of metallic antimony particles in the filtered product was 270 / 0.1 mm 2 In the film-forming property evaluation of the polyester films obtained in Examples 56 and 57, the electrostatic applicability was good. In addition, the yield evaluation of the conductor circuit using the obtained polyester film was good in Example 56, and tended to deteriorate in Example 57, but was still within the acceptable range.

[0104] Examples 58 and 59: Polyester resin compositions and polyester films were obtained in the same manner as in Examples 56 and 57, except that the polycondensation reaction catalyst was changed from diantimony trioxide to an ethylene glycol solution of germanium dioxide, and the germanium content was set as shown in Table 9. The results are shown in Table 10. The polyester resin compositions obtained in Examples 58 and 59 all had acceptable properties, and furthermore, no metallic antimony was observed in the filtered residue of the polyester resin composition, resulting in good results. Furthermore, in the film-forming evaluation of the obtained polyester films, the electrostatic applicability was good in all cases. Furthermore, the yield of conductor circuits using the obtained polyester films was good in Example 58, and tended to deteriorate in Example 59, but remained within the acceptable range.

[0105]

[0106]

Claims

1. A polyester resin composition having an intrinsic viscosity of 0.55 dL / g or more, the content of a p-toluenesulfonic acid component is 0.07 to 0.65 mol / t and the content of a quaternary phosphonium component is 0.07 to 0.65 mol / t relative to the total weight of the polyester resin composition, the heat resistance parameter X represented by formula 1 is 1.0≦X≦1.3, and the number of foreign particles having a circle equivalent diameter of 0.2 μm or more is 650 pieces / 0.1 mm 2 The melting resistivity is 4.0×10 6 A polyester resin composition having a viscosity of Ω·cm or less and a color tone b value of 10.0 or less as measured by a color difference meter.

2. The polyester resin composition according to claim 1, wherein the content of alkali metal elements is 3 ppm by weight or less based on the total weight of the polyester resin composition.

3. The polyester resin composition according to claim 2, wherein the antimony element content is 15 ppm by weight or less and the titanium element content is 0.1 ppm by weight to 20 ppm by weight, based on the total weight of the polyester resin composition.

4. The polyester resin composition according to claim 3, wherein the manganese element content is 5 to 40 ppm by weight and the phosphorus element content is 3 to 50 ppm by weight, based on the total weight of the polyester resin composition.

5. The polyester resin composition according to claim 2, wherein the antimony element content is 15 ppm by weight or less and the germanium element content is 5 ppm by weight to 150 ppm by weight, based on the total weight of the polyester resin composition.

6. The polyester resin composition according to claim 5, wherein the manganese element content is 5 to 40 ppm by weight and the phosphorus element content is 3 to 50 ppm by weight, based on the total weight of the polyester resin composition.

7. The polyester resin composition according to claim 2, wherein the antimony element content is 15 ppm by weight or less and the aluminum element content is 0.1 ppm by weight to 100 ppm by weight, based on the total weight of the polyester resin composition.

8. The polyester resin composition according to claim 7, wherein the manganese element content is 5 to 40 ppm by weight and the phosphorus element content is 3 to 50 ppm by weight, based on the total weight of the polyester resin composition.

9. The polyester resin composition according to claim 2, wherein the content of antimony element is 50 ppm by weight to 150 ppm by weight based on the total weight of the polyester resin composition.

10. The polyester resin composition according to claim 9, wherein the manganese element content is 5 to 40 ppm by weight and the phosphorus element content is 3 to 50 ppm by weight, based on the total weight of the polyester resin composition.

11. A polyester resin composition having an intrinsic viscosity of 0.55 dL / g or more, the content of a p-toluenesulfonic acid component being 0.07 to 0.65 mol / t, the content of a quaternary phosphonium component being 0.07 to 0.65 mol / t, and the content of an alkali metal element being 3 ppm by weight or less, based on the total weight of the polyester resin composition, the heat resistance parameter X represented by formula 1 being 1.0≦X≦1.3, and the number of foreign matters having a circle equivalent diameter of 0.2 μm or more is 630 pieces / 0.1 mm 2 The polyester resin composition has a color tone b value of 10.0 or less as measured by a color difference meter.

12. The polyester resin composition according to claim 11, wherein the antimony element content is 15 ppm by weight or less and the titanium element content is 0.1 ppm by weight to 20 ppm by weight, based on the total weight of the polyester resin composition.

13. The polyester resin composition according to claim 12, wherein the manganese element content is 5 to 40 ppm by weight and the phosphorus element content is 3 to 50 ppm by weight, based on the total weight of the polyester resin composition.

14. The polyester resin composition according to claim 11, wherein the antimony element content is 15 ppm by weight or less and the germanium element content is 5 ppm by weight to 150 ppm by weight, based on the total weight of the polyester resin composition.

15. The polyester resin composition according to claim 14, wherein the manganese element content is 5 to 40 ppm by weight and the phosphorus element content is 3 to 50 ppm by weight, based on the total weight of the polyester resin composition.

16. The polyester resin composition according to claim 11, wherein the antimony element content is 15 ppm by weight or less and the aluminum element content is 0.1 ppm by weight to 100 ppm by weight, based on the total weight of the polyester resin composition.

17. The polyester resin composition according to claim 16, wherein the manganese element content is 5 to 40 ppm by weight and the phosphorus element content is 3 to 50 ppm by weight, based on the total weight of the polyester resin composition.

18. The polyester resin composition according to claim 11, wherein the content of antimony element is 50 ppm by weight to 150 ppm by weight based on the total weight of the polyester resin composition.

19. The polyester resin composition according to claim 18, wherein the manganese element content is 5 to 40 ppm by weight and the phosphorus element content is 3 to 50 ppm by weight, based on the total weight of the polyester resin composition.

20. A polyester film obtained by using the polyester resin composition according to any one of claims 1 to 19.

Citation Information

Patent Citations

  • Preparation of multi-layer film

    JP2000211009A

  • Polyethylene terephthalate resin composition and film made from the same

    JP2018062574A

  • Polyester resin composition and manufacturing method therefor

    JP2020007542A

  • Polyester resin composition and polyester film including the same

    JP2022089784A

  • Biaxially oriented polyester film and laminate

    JP2023015002A