Glass for coating semiconductor element and sintered body for coating semiconductor element
A glass composition with specific SiO2, ZnO, B2O3, Al2O3, and MgO + CaO ratios addresses environmental concerns and devitrification issues in semiconductor glass coatings, providing thermal stability and preventing cracks in semiconductor elements.
Patent Information
- Application Number
- PCT/JP2024/020388
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-08
- Filing Date
- 2024-06-04
- Publication Date
- 2024-12-12
AI Technical Summary
Existing glasses used for covering semiconductor elements, such as lead-based glasses, have environmental concerns due to lead content and are prone to devitrification during the melting process, while zinc-based glasses also devitrify easily and contain harmful components.
A glass composition with SiO2 + ZnO 40-75%, B2O3 0-20%, Al2O3 5-15%, MgO + CaO 8-22%, and a molar ratio of Al2O3 / (SiO2 + ZnO) ≤ 0.2, substantially free of lead, is developed to minimize environmental impact and devitrification risk, with a thermal expansion coefficient of 20-55 × 10^-7 /°C, suitable for semiconductor devices.
The proposed glass composition effectively reduces environmental impact and devitrification during melting, maintaining thermal stability and preventing cracks in semiconductor elements, while being free from lead and alkaline impurities, ensuring long-term semiconductor performance.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Glass for covering semiconductor elements and sintered body for covering semiconductor elements
[0001] The present invention relates to a glass for covering a semiconductor element and a sintered body for covering a semiconductor element.
[0002] In general, the surfaces of semiconductor elements such as silicon diodes and transistors, including the PN junctions, are covered with glass, which stabilizes the surface of the semiconductor element and prevents its characteristics from deteriorating over time.
[0003] The properties required for a glass for covering semiconductor elements include: (1) a thermal expansion coefficient that matches that of the semiconductor element so as to prevent cracks and the like due to differences in the thermal expansion coefficient between the semiconductor element and the glass; (2) the glass must be capable of covering the semiconductor element at low temperatures (for example, 900°C or lower) so as to prevent deterioration of the characteristics of the semiconductor element; and (3) the glass must be free of impurities such as alkaline components that have adverse effects on the surface of the semiconductor element.
[0004] Conventionally, ZnO-B has been used as a glass for covering semiconductor elements. 2 O 3 -SiO 2 zinc-based glass such as PbO—SiO 2 -Al 2 O 3 PbO-SiO 2 -Al 2 O 3 -B 2 O 3 Although lead-based glasses such as PbO-SiO are known, currently, from the viewpoint of workability, 2 -Al 2 O 3 PbO-SiO 2 -Al 2 O 3 -B 2 O 3 Lead-based glasses such as lead-based glasses have become mainstream (see, for example, Patent Documents 1 to 4).
[0005] Japanese Patent Laid-Open No. 48-43275 Japanese Patent Laid-Open No. 50-129181 Japanese Patent Publication No. 1-49653 Japanese Patent Laid-Open No. 2008-162881
[0006] However, the lead component of lead-based glass is harmful to the environment, and the zinc-based glass described above contains small amounts of lead and bismuth components, so it cannot be said to be completely harmless to the environment.
[0007] Furthermore, zinc-based glass has the problem of being more susceptible to devitrification during the melting process than lead-based glass.
[0008] The present invention has been made in view of the above circumstances, and its technical object is to provide a glass for covering semiconductor elements that has a small environmental impact and is resistant to devitrification during the melting process.
[0009] As a result of extensive research, the inventors have found that the devitrified material generated in the glass melting process is gahnite (ZnAl 2 O 4 ) and SiO 2 -ZnO-Al 2 O 3 In Al-based glasses, 2 O 3 and SiO 2 The inventors have found that by controlling the ratio of the total content of SiO and ZnO, it becomes difficult for gahnite to be generated in the glass melting process, and have proposed this invention. 2 +ZnO 40-75%, B 2 O 3 0-20%, Al 2 O 3 5 to 15%, MgO + CaO 8 to 22%, and in molar ratio, Al 2 O 3 / (SiO 2 +ZnO) is 0.2 or less and is substantially free of lead. 2 +ZnO" means SiO 2 "MgO+CaO" is the total content of MgO and CaO. 2 O 3 / (SiO 2 +ZnO) means Al 2 O 3 The content of SiO 2The value is obtained by dividing by the total content of ZnO and ZnO. Furthermore, "substantially free of ..." means that the component in question is not intentionally added as a glass component, but does not mean that even unavoidable impurities are completely excluded. Specifically, it means that the content of the component in question, including impurities, is less than 0.1 mass %.
[0010] The glass for covering semiconductor elements of the present invention has a thermal expansion coefficient of 20 to 55×10 in the temperature range of 30 to 300°C. -7 / ° C. Here, the "coefficient of thermal expansion in the temperature range of 30 to 300° C." refers to a value measured using a push rod type thermal expansion coefficient measuring device.
[0011] According to the present invention, it is possible to provide a glass for covering semiconductor elements that has a small environmental impact and is resistant to devitrification during the melting process.
[0012] The glass for covering semiconductor elements of the present invention has a glass composition containing, in mol %, SiO 2 +ZnO 40-75%, B 2 O 3 0-20%, Al 2 O 3 5 to 15%, MgO + CaO 8 to 22%, and in molar ratio, Al 2 O 3 / (SiO 2 +ZnO) is 0.2 or less, and is substantially free of lead. The reasons for limiting the content of each component are explained below. In the following explanation of the content of each component, % means mol% unless otherwise specified. In this specification, a numerical range indicated using "to" means a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively.
[0013] SiO 2 and ZnO are components that stabilize the glass. 2 +ZnO is 40 to 75%, preferably 45 to 70%, 50 to 68%, 53 to 65%, and particularly preferably 55 to 64%. 2 If the amount of +ZnO is too small, gahnite is likely to precipitate during the melting process. 2If the amount of +ZnO is too large, the softening point of the glass tends to increase significantly.
[0014] SiO 2 The content is preferably 25 to 40%, 22 to 38%, 24 to 36%, particularly preferably 26 to 34%.
[0015] The ZnO content is preferably 15 to 40%, 22 to 38%, 24 to 36%, and particularly preferably 26 to 34%.
[0016] B 2 O 3 is a component that forms a glass network and enhances the softening and fluidity of the glass. 2 O 3 The content of is 0 to 20%, preferably 0 to 18%, and particularly preferably 0 to 16%. 2 O 3 If the content is too high, the thermal expansion coefficient tends to be unduly high and the acid resistance tends to decrease.
[0017] Al 2 O 3 is a component that stabilizes the glass. 2 O 3 The content of Al is 5 to 15%, preferably 6 to 14%, 7 to 13%, 8 to 12%, or 8 to 11%, and particularly preferably 9 to 10%. 2 O 3 If the content of Al is too low, vitrification becomes difficult. 2 O 3 If the content is too high, gahnite is likely to precipitate during the melting process, and the softening point of the glass is likely to increase significantly.
[0018] In molar ratio, Al 2 O 3 / (SiO 2 +ZnO) is 0.2 or less, preferably 0.19 or less, and particularly preferably 0.18 or less. 2 O 3 / (SiO 2 If the ratio of Al to ZnO is too large, gahnite tends to precipitate during the melting process. 2 O 3 / (SiO 2 The lower limit of the ratio (ZnO + ZnO) is not particularly limited, but is practically 0.07 or more.
[0019] MgO and CaO are components that reduce the viscosity of the glass. The total content of MgO and CaO is 8 to 22%, and preferably 10 to 20%. If the total content of MgO and CaO is too low, the softening temperature of the glass tends to increase. On the other hand, if the total content of MgO and CaO is too high, the thermal expansion coefficient may become too high, the acid resistance may decrease, or the insulating properties may decrease.
[0020] The content of MgO is preferably 2 to 20%, more preferably 3 to 15%, and even more preferably 4 to 13%.
[0021] The CaO content is preferably 2 to 20%, 3 to 15%, and particularly preferably 4 to 13%.
[0022] In addition to the above components, other components (e.g., SrO, BaO, MnO 2 , Ta 2 O 5 , Nb 2 O 5 , CeO 2 , Sb 2 O 3 etc.) may be contained in an amount of up to 7% (preferably up to 3%).
[0023] From an environmental point of view, it contains substantially no lead components (e.g., PbO, etc.) and substantially no Bi. 2 O 3 It is also preferable that the solution does not contain alkaline components (Li, 2 O, Na 2 O and K 2 It is also preferable that the compound is substantially free of fluorine-containing compounds.
[0024] The glass for covering semiconductor elements of the present invention has a thermal expansion coefficient of 20 to 55×10 in the temperature range of 30 to 300°C. -7 / °C, particularly 30 to 50 × 10 -7 If the thermal expansion coefficient is outside the above range, cracks, warping, etc. are likely to occur due to the difference in thermal expansion coefficient with the semiconductor element.
[0025] The glass for covering a semiconductor element of the present invention is preferably in a powder form, which makes it easy to cover the surface of a semiconductor element using, for example, a paste method or an electrophoretic coating method.
[0026] Average particle diameter D of glass powder 50 The average particle diameter D of the glass powder is preferably 25 μm or less, particularly preferably 15 μm or less. 50 If the average particle diameter D of the glass powder is too large, it becomes difficult to form a paste. In addition, it becomes difficult to apply the paste by electrophoresis. 50 The lower limit of the average particle diameter D is not particularly limited, but in reality it is 0.1 μm or more. 50 " is a value measured on a volume basis and refers to a value measured by a laser diffraction method.
[0027] The glass for covering semiconductor elements of the present invention may be mixed with ceramic powder to form a composite powder, if necessary. Addition of ceramic powder makes it easier to adjust the thermal expansion coefficient.
[0028] The amount of ceramic powder is preferably less than 25 parts by mass, particularly less than 20 parts by mass, per 100 parts by mass of glass powder. If the content of ceramic powder is too high, the softening and fluidity of the glass is impaired, making it difficult to coat the surface of the semiconductor element.
[0029] Average particle diameter D of ceramic powder 50 The average particle diameter D of the ceramic powder is preferably 30 μm or less, and particularly preferably 20 μm or less. 50 If the average particle diameter D of the ceramic powder is too large, the surface smoothness of the coating layer is likely to decrease. 50 The lower limit is not particularly limited, but in reality it is 0.1 μm or more.
[0030] Next, an example of the method for producing the glass for covering a semiconductor element and the sintered body for covering a semiconductor element according to the present invention will be described.
[0031] First, raw material powders prepared to obtain a desired glass composition are melted at 1300 to 1550°C for 1 to 2 hours until a homogeneous glass is obtained. The resulting molten glass is then formed into a film or the like, which is then crushed and classified to produce a powdered glass for coating semiconductor devices.
[0032] Next, the surface of the semiconductor element is coated with a powdered glass for covering a semiconductor element, for example, by using a paste method, an electrophoretic coating method, or the like. Then, by performing a heat treatment, the glass for covering a semiconductor element that has covered the surface of the semiconductor element becomes a sintered body for covering a semiconductor element in which no crystals are precipitated. It is preferable that the sintered body for covering a semiconductor element has the same composition range as the glass composition of the glass for covering a semiconductor element.
[0033] The present invention will be described in detail below based on examples. Note that the following examples are merely illustrative and the present invention is not limited to the following examples in any way.
[0034] Table 1 shows examples of the present invention (samples Nos. 1 to 4, 9, and 10) and comparative examples (samples Nos. 5 to 8).
[0035]
[0036] Each sample was prepared as follows: First, raw material powders were mixed to form a batch having the glass composition shown in the table, and the batch was melted at 1500°C for 1 hour to form a glass. The molten glass was then formed into a film, pulverized in a ball mill, and classified using a 350-mesh sieve to determine the average particle diameter D 50 A glass powder having a particle size of 12 μm was obtained.
[0037] The thermal expansion coefficient and devitrification resistance of each sample were evaluated, and the results are shown in Table 1.
[0038] The thermal expansion coefficient is a value measured in the temperature range of 30 to 300°C using a push rod type thermal expansion coefficient measuring device.
[0039] The devitrification resistance was evaluated as follows. 100 g of the glass film of each sample was placed in a platinum crucible, and after holding at 1150 ° C for 24 hours, it was confirmed by visual observation that devitrification (gahnite) had occurred. Thereafter, the sample was held at 1400 ° C for 10 minutes, and if no devitrification (gahnite) was observed by visual observation, it was marked as "◯", and if devitrification (gahnite) was observed, it was marked as "X". The devitrification was measured using an X-ray diffractometer and confirmed to be gahnite.
[0040] As is clear from Table 1, Samples Nos. 1 to 4, 9, and 10 were rated as good in terms of devitrification resistance and had thermal expansion coefficients of 20 to 55×10 -7 / °C. When Samples No. 1 to 4 were fired for 10 minutes at the temperatures shown in the table, no crystals were precipitated.
[0041] On the other hand, samples No. 5 to 8 are Al 2 O 3 / (SiO 2 Since the ratio of ZnO to the total ZnO is too large, the resistance to devitrification is poor, and it is considered that this glass may cause problems in the melting process.
Claims
1. The glass composition is, in mole percent, SiO 2 +ZnO 40-75%, B 2 O 3 0-20%, Al 2 O 3 5 to 15%, MgO + CaO 8 to 22%, and in molar ratio, Al 2 O 3 / (SiO 2 +ZnO) is 0.2 or less, and is substantially free of lead components.
2. The thermal expansion coefficient in the temperature range of 30 to 300°C is 20 to 55 x 10 -7 2. The glass for covering a semiconductor element according to claim 1, wherein the temperature is 100° C. or more.
3. Composition: SiO 2 +ZnO 40-75%, B 2 O 3 0-20%, Al 2 O 3 5 to 15%, MgO + CaO 8 to 22%, and in molar ratio, Al 2 O 3 / (SiO 2 +ZnO) is 0.2 or less, and is substantially free of lead components.
Citation Information
Patent Citations
Glass composition for coating
JP1991126639A
Semiconductor element coating glass and semiconductor coating material using same
JP2020055725A
Resin-sealed semiconductor device and production method for resin-sealed semiconductor device
WO2013168236A1
Encapsulating glass composition
WO2018221426A1
Glass for semiconductor element coating and material for semiconductor coating using same
WO2020158187A1
Cited By
Glass for coating semiconductor element, and sintered body for coating semiconductor element
WO2026205040A1