Porous membrane, filter member, and member supply assembly

The porous membrane with a thermoplastic resin and tortoiseshell-like structure addresses the challenge of secure attachment to device casings by maintaining compressibility and mechanical strength, ensuring secure bonding and appropriate pressure.

WO2024253193A1PCT designated stage expired Publication Date: 2024-12-12NITTO DENKO CORP

Patent Information

Application Number
PCT/JP2024/020916
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-09
Filing Date
2024-06-07
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Existing porous membranes with high mechanical strength may not ensure appropriate attachment pressure when attached to device casings due to potential thickness reduction during attachment, leading to insecure bonding.

Method used

A porous membrane with a thermoplastic resin having a melting point of 180°C or more and 300°C or less, featuring a tortoiseshell-like structure formed by nodes and fibrils, which maintains compressibility of 20% or less in the thickness direction, and an optional adhesive layer for secure attachment.

Benefits of technology

The porous membrane effectively suppresses thickness reduction during attachment, ensuring appropriate attachment pressure and secure bonding to device casings while maintaining mechanical strength and air permeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024020916_12122024_PF_FP_ABST
    Figure JP2024020916_12122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a porous membrane which contains, as a main component, a thermoplastic resin having a melting point of 180-300°C and has a tortoiseshell structure configured of a plurality of nodes and a plurality of fibrils. Alternatively, provided is a porous membrane which contains, as a main component, a thermoplastic resin having a melting point of 180-300°C and which, when a pressure of 2.5 N / mm2 is applied thereto, has a compressibility along the thickness direction of the porous film of 20% or less. The thermoplastic resin includes, for example, a polymethylpentene resin. When a section of the porous membrane is examined, there are, for example, a plurality of nodes arranged along the thickness direction.
Need to check novelty before this filing date? Find Prior Art

Description

Porous membrane, filter element and element supply assembly

[0001] The present invention relates to a porous membrane, a filter element, and an element supply assembly.

[0002] Fluororesin porous membranes are used in a variety of applications, such as filters, sound-permeable membranes, air-permeable membranes, diaphragms, liquid absorbents, etc. Fluorine-free porous membranes have also been proposed for use in these applications.

[0003] For example, Patent Document 1 discloses a biaxially stretched olefin-based resin microporous film having micropores and containing an olefin-based resin, characterized in that the biaxially stretched olefin-based resin microporous film has a puncture strength of 0.7 N or more and an air permeability of 75 to 400 s / 100 mL.

[0004] Japanese Patent Application Laid-Open No. 2017-095576

[0005] Even if a porous membrane has excellent mechanical strength such as puncture resistance, it may not be possible to ensure an appropriate attachment pressure when attaching it to, for example, a device housing.

[0006] Therefore, an object of the present invention is to provide a porous membrane that is suitable for attachment to a housing or the like of a device.

[0007] The present invention provides a porous membrane containing, as a main component, a thermoplastic resin having a melting point of 180°C or more and 300°C or less, the porous membrane having a hexagonal structure formed by a plurality of nodes and a plurality of fibrils.

[0008] From another aspect, the present invention provides a porous membrane containing, as a main component, a thermoplastic resin having a melting point of 180°C or more and 300°C or less, the membrane having a strength of 2.5 N / mm 2 The porous membrane has a compressibility of 20% or less in the thickness direction when a pressure of 1000 kJ / cm is applied thereto.

[0009] From another aspect, the present invention provides a filter member comprising: the porous membrane of the present invention; and a pressure-sensitive adhesive layer bonded to the porous membrane.

[0010] From yet another aspect, the present invention provides a member supply assembly comprising a filter member to be placed on a surface of an object having an opening, and a base sheet on which the filter member is placed, wherein the filter member comprises: a porous membrane having a shape that covers the opening when placed on the surface; and an adhesive layer bonded to the porous membrane, and the porous membrane is the porous membrane of the present invention.

[0011] According to the present invention, a porous film suitable for attachment to a housing or the like of a device can be provided.

[0012] FIG. 1A is a cross-sectional view schematically showing an example of a porous membrane of the present invention. FIG. 1B is a cross-sectional view schematically showing an example of the surface of a porous membrane of the present invention. FIG. 2 is a cross-sectional view schematically showing an example of a ventilation member of the present invention. FIG. 3 is a cross-sectional view schematically showing a first variation of the ventilation member of FIG. 2. FIG. 4 is a cross-sectional view schematically showing a second variation (wound body) of the ventilation member of FIG. 2. FIG. 5 is a cross-sectional view schematically showing an example of a filter member of the present invention. FIG. 6 is a cross-sectional view schematically showing a first variation of the filter member 4 of FIG. 5. FIG. 7 is a cross-sectional view schematically showing a second variation of the filter member 4 of FIG. 5. FIG. 8 is a cross-sectional view schematically showing a third variation of the filter member 4 of FIG. 5. FIG. 9 is a cross-sectional view schematically showing an example of a member supply assembly of the present invention. FIG. 10 is a diagram (2500x magnification) showing the results of observation of the surface of the porous membrane of Example 1 with a scanning electron microscope (SEM). FIG. 11 is a diagram (2500x magnification) showing the results of SEM observation of the surface of the porous membrane of Example 2. FIG. 12A is a diagram (2500x magnification) showing the results of SEM observation of the surface of the porous membrane of Example 3. FIG. 12B is a partial enlarged view (10000x magnification) of FIG. 12A. FIG. 12C is a diagram (1500x magnification) showing the results of SEM observation of the cross section of the porous membrane of Example 3. FIG. 13 is a diagram (2500x magnification) showing the results of SEM observation of the surface of the porous membrane of Example 4. FIG. 14A is a diagram (2500x magnification) showing the results of SEM observation of the surface of the porous membrane of Example 5. FIG. 14B is a partial enlarged view (10000x magnification) of FIG. 14A. FIG. 15A is a diagram (2500x magnification) showing the results of SEM observation of the surface of the membrane of Comparative Example 1. FIG. 15B is a partial enlarged view (10000x magnification) of FIG. 15A. 15C is a diagram (2000x magnification) showing the results of SEM observation of the cross section of the film of Comparative Example 1. FIG. 16 is a diagram (2500x magnification) showing the results of SEM observation of the surface of the film of Comparative Example 2. FIG. 17 is a diagram (2500x magnification) showing the results of SEM observation of the surface of the film of Comparative Example 3. FIG. 18A is a diagram (2500x magnification) showing the results of SEM observation of the surface of the film of Reference Example 2. FIG. 18B is a partial enlarged view (20000x magnification) of FIG. 18A. FIG. 19 is a graph showing the results of measuring the actual temperature of the film from after heat pressing to cooling using a thermocouple at 100 ms intervals for Example 1, Examples 6-7, and Comparative Example 4.Fig. 20 is a schematic diagram for explaining how to determine the distance between island regions of the porous film in Fig. 1. Fig. 21 is a schematic cross-sectional view for explaining a compression test.

[0013] A porous membrane according to a first aspect of the present invention is a porous membrane containing, as a main component, a thermoplastic resin having a melting point of 180°C or more and 300°C or less, and the porous membrane has a hexagonal structure formed by a plurality of nodes and a plurality of fibrils.

[0014] In the second aspect of the present invention, for example, in the porous membrane according to the first aspect, the strength is 2.5 N / mm 2 When a pressure of 1000 kJ / cm is applied to the porous membrane, the compressibility in the thickness direction of the porous membrane is 20% or less.

[0015] A porous membrane according to a third aspect of the present invention is a porous membrane containing, as a main component, a thermoplastic resin having a melting point of 180°C or more and 300°C or less, and having a compressive strength of 2.5 N / mm 2 When a pressure of 1000 kJ / cm is applied to the porous membrane, the compressibility in the thickness direction of the porous membrane is 20% or less.

[0016] In a fourth aspect of the present invention, for example, in the porous membrane according to any one of the first to third aspects, the thermoplastic resin includes a polymethylpentene resin.

[0017] In a fifth aspect of the present invention, for example, in a porous film according to any one of the first to fourth aspects, when a cross section of the porous film is observed, a plurality of the nodes are included along the thickness direction.

[0018] In a sixth aspect of the present invention, for example, in the porous membrane according to any one of the first to fifth aspects, the air permeability expressed in Gurley number is 1000 seconds / 100 mL or less.

[0019] In a seventh aspect of the present invention, for example, in the porous film according to any one of the first to sixth aspects, the porosity of the porous film is 25% or more.

[0020] A filter member according to an eighth aspect of the present invention comprises: a porous membrane according to any one of the first to seventh aspects; and a pressure-sensitive adhesive layer bonded to the porous membrane.

[0021] A component supply assembly according to a ninth aspect of the present invention is a component supply assembly comprising a filter member to be placed on a surface of an object having an opening, and a base sheet on which the filter member is placed, wherein the filter member comprises: a porous membrane having a shape that covers the opening when placed on the surface; and an adhesive layer bonded to the porous membrane, and the porous membrane is a porous membrane according to any one of the first to seventh aspects.

[0022] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described below with reference to the accompanying drawings, but is not limited to the following embodiments.

[0023] [Porous membrane] An example of the porous membrane of the present invention is shown in Figure 1A. The porous membrane 1 in Figure 1A contains a thermoplastic resin having a melting point of 180°C or more and 300°C or less as a main component. The "main component" refers to the component that is contained in the porous membrane in the largest amount by weight. With this configuration, the porous membrane 1 can be adhered to a device housing or the like, for example, not only by using an adhesive layer but also by heat fusion.

[0024] FIG. 1B is a schematic diagram showing an example of the surface of the porous membrane 1. The porous membrane 1 has a tortoiseshell structure formed by multiple nodes 1a and multiple fibrils 1b. As shown in FIG. 1B, the tortoiseshell structure is present throughout the porous membrane 1. This structure can suppress a decrease in the thickness of the porous membrane 1 due to compression when attached to a device housing, etc. Therefore, an appropriate attachment pressure can be ensured. The tortoiseshell structure can be confirmed, for example, by observing the main surface of the porous membrane 1 from the vertical direction. In this disclosure, the term "main surface" refers to the surface of a sheet-like or film-like member having the largest area. In addition, in this disclosure, the "main surface" and "surface" of the porous membrane 1 are used interchangeably.

[0025] In the present disclosure, the term "hexagonal structure formed by multiple nodes 1a and multiple fibrils 1b" refers to a structure that can be confirmed by observing the surface of the porous membrane 1 with a scanning electron microscope (SEM). This structure refers to a structure in which island regions 1c formed by multiple nodes 1a are irregularly connected and these island regions 1c are connected to each other by multiple fibrils 1b. Examples of island regions 1c include polygonal regions. The polygonal region does not necessarily have to have an outer shape composed of only straight lines; it also includes approximately polygonal regions in which some sides are curved, such as arcs. The polygon is, for example, a hexagon, but is not limited thereto and may be, for example, a pentagon or a rectangle. The hexagonal structure may include multiple island regions 1c and multiple fibrils 1b extending in multiple directions from each island region 1c. The island regions 1c may be connected to each other or overlap without the intervention of multiple fibrils 1b (see part I in Figure 1B). That is, there may not be multiple fibrils 1b between adjacent island regions 1c. Island regions 1c, which are aggregates of multiple nodes 1a, may be present together with nodes 1a (see part II in Figure 1B). Planar regions 1d may be present, formed by the dense collection of multiple fibrils 1b extending in multiple directions from each island region 1c (see part III in Figure 1B). When observing the surface of the porous membrane 1 with an SEM, it may not be clear at first glance whether the planar region 1d formed by the dense collection of multiple fibrils 1b is different from the island regions 1c formed by multiple nodes 1a. However, even in such cases, it is possible to distinguish between the island regions 1c and the planar region 1d by magnifying the observation image, for example, up to about 10,000 times. The island regions 1c may have a shape that is more raised than the planar region 1d. When observing the surface of the porous membrane 1 with an SEM, the longest diameter of the island regions 1c may be 0.5 μm or more, 1 μm or more, or even 2 μm or more.

[0026] In this disclosure, the term "tortoiseshell-like" is a term that focuses on the island-like regions 1c and describes how the island-like regions 1c are irregularly arranged like a turtle shell, but does not necessarily mean that the island-like regions 1c are densely arranged like a turtle shell.

[0027] The average spacing between adjacent island regions 1c is, for example, 0.1 μm or more and 30 μm or less. The lower limit of the average spacing between island regions 1c may be 0.5 μm or more, 1 μm or more, 2 μm or more, or even 4 μm or more. The upper limit of the average spacing between island regions 1c may be 20 μm or less, 15 μm or less, 10 μm or less, or even 8 μm or less.

[0028] The average area of ​​the island regions 1c is, for example, 0.1 μm 2 100 μm or more 2 The lower limit of the average area of ​​the island regions 1c is 0.5 μm 2 It may be 1 μm or more. 2 It may be 5 μm or more. 2 It may be 10 μm or more. 2 It may be 14 μm or more, 2 The upper limit of the average area of ​​the island regions 1c is 75 μm 2 It may be 65 μm or less, 2 It may be 55 μm or less, 2 It may be less than 50 μm, 2 It may be the following:

[0029] The average spacing between island regions of the porous membrane 1 can be determined by the method described below. Figure 20 is a schematic diagram illustrating how to determine the distance between island regions of the porous membrane 1 of Figure 1A. First, the surface of the porous membrane 1 is observed with an SEM (see, for example, Figure 1B). Next, the obtained SEM observation image (or a portion thereof) is binarized using image analysis software. Island regions are identified from the obtained binarized image, and the area of ​​each island region contained in the image is calculated. For each island region, the circle equivalent diameter is calculated from the calculated area. The circle equivalent diameter is the diameter of a perfect circle having the same area as the area of ​​the island region being measured. As shown in Figure 20, the distance L between island regions A and B is ABcan be calculated as the distance between the center of gravity c of island region A and the center of gravity c of island region B minus ½ of the circle equivalent diameter of island region A and ½ of the circle equivalent diameter of island region B. In this way, the distance between the island regions (L AB , L AC and L AD That is, the distance between the fourth and subsequent island regions (island region E) from island region A (L AE ) is not adopted. However, an island region (island region F) that overlaps with island region A in the image is excluded from the three island regions that are first to third closest in distance to island region A. The average of the distances between the island regions and the three island regions closest to island region A obtained in this way is considered to be the distance between island regions of island region A. The distance between island regions is obtained in the same manner for each island region included in the image. The average of the obtained distances between island regions can be considered to be the average spacing between island regions of the porous membrane 1. When identifying island regions, island regions that fall on the edges of the image are omitted from the analysis. As image analysis software, for example, ImageJ can be used.

[0030] The average area of ​​the island regions of the porous membrane 1 can be determined by the method described below. First, a binarized image is obtained using the same method as that described for the distance between island regions of the porous membrane 1, and nodes are identified from the binarized image. Island regions are identified from the obtained binarized image, and the area of ​​each island region contained in the image is calculated. The average value of the determined island region areas can be considered the average area of ​​the island regions of the porous membrane 1. However, the average area of ​​the island regions of the porous membrane 1 should be determined by measuring 30 or more island regions, for example, 50 to 200 island regions.

[0031] 10 to 12B and 13 to 14B show the results of SEM observations of the surfaces of the porous membranes of Examples 1 to 5, which will be described later. As shown in these observation images, the surfaces of the porous membranes of Examples 1 to 5 have a tortoiseshell structure formed by multiple nodes and multiple fibrils. Specifically, island-like regions 1c formed by multiple nodes 1a are irregularly connected, and these island-like regions 1c are connected to each other by multiple fibrils 1b.

[0032] When observing a cross section of the porous membrane 1, a plurality of nodes may be included along the thickness direction. The plurality of nodes may be present throughout the entire thickness direction of the porous membrane 1. With such a structure, a reduction in the thickness of the membrane due to compression when attached to a device housing or the like can be suppressed.

[0033] The nodes present in the thickness direction may be lumpy. That is, when a cross section of the porous membrane 1 is observed, multiple lumpy nodes may be present along the thickness direction. The lumpy nodes present in the thickness direction correspond to island regions when the surface of the porous membrane 1 is observed with an SEM.

[0034] The multiple agglomerated nodes may be uniformly present across the thickness direction of the porous membrane 1. Adjacent agglomerated nodes may be connected by multiple fibrils, or adjacent agglomerated nodes may be directly linked to each other without being connected by multiple fibrils.

[0035] 12C shows the results of SEM observation of the cross section of the porous membrane of Example 3, which will be described later. As shown in FIG. 12C, when the cross section of the porous membrane of Example 3 is observed, multiple cluster nodes are present along the thickness direction. The multiple cluster nodes are present throughout the entire thickness direction of the porous membrane.

[0036] The porous membrane 1 has a resistance of 2.5 N / mm 2The compressibility Rc of the porous membrane 1 in the thickness direction when a pressure of 1000 kJ / cm is applied is 20% or less. The compressibility Rc is a value per unit amount of resin. In this way, the porous membrane 1 is prevented from reducing in thickness due to compression when attached to a device housing or the like, so that an appropriate attachment pressure can be ensured.

[0037] The compressibility Rc can be determined by a compression test using a thermomechanical analyzer (TMA). Fig. 21 is a schematic cross-sectional view for explaining the compression test. First, the porous membrane 1 is cut into a strip of 10 mm width x 10 mm length to form a sample piece S. Next, in an environment of 25°C, a cylindrical indenter 90 of the TMA with a tip diameter of 1 mm is used to gradually apply a load from an initial load P1 (gf) (see Fig. 21(A)) to a maximum load P max (gf) (see FIG. 21B), the sample piece S was compressed at a loading rate of 50 gf / min. n A function F1 of the load (gf) and the deformation rate (%) in the compression direction is obtained. n The deformation rate (%) at (gf) is the ratio of the load P to the thickness T (μm) of the sample piece S at the initial load P (gf). n (gf) The thickness T of the sample piece S n (μm), where 100×T n Next, the function F1 is calculated by the area of ​​the indenter 90 (0.785 mm 2 ) to calculate the load per unit area Pa (gf / mm 2 ) and the deformation rate (%) into a function F2 (load Pa (gf / mm 2 ) = load P n (gf) / 102 / area of ​​indenter 90 (mm 2 )) Furthermore, taking into consideration the pores present in the porous membrane 1, the function F2 is converted per unit resin amount, and the load Pb (gf / mm 2 ) to obtain a function F3 of the deformation rate (%) at the load Pb (gf / mm 2 ) = Load Pa (gf / mm 2 ) / {(100-porosity) / 100}). In function F3, when the load Pb is 2.5 gf / mm 2 The deformation rate (%) at the time point is the rate of change R 2.5When defined as 100-R 2.5 The value obtained by the above is regarded as the compressibility Rc (%). The measurement conditions for the compression test are as follows: <Measurement conditions> Initial load P1: 2 gf Maximum load P max Loading speed: 50 gf / min

[0038] The compression ratio Rc may be 19.5% or less, or may be 19% or less. The lower limit of the compression ratio Rc is, for example, 5%.

[0039] As described above, the melting point of the thermoplastic resin contained in the porous membrane 1 is 180° C. or higher and 300° C. or lower. When the melting point of the thermoplastic resin is 180° C. or higher, sufficient heat resistance can be ensured in the porous membrane 1. When the melting point of the thermoplastic resin is 300° C. or lower, the porous membrane 1 can be produced by melt molding, for example.

[0040] The melting point of the thermoplastic resin may be 200°C or higher and 280°C or lower, and may further be 220°C or higher and 260°C or lower.

[0041] The thermoplastic resin having a melting point of 180°C or higher and 300°C or lower may be a fluorine-free thermoplastic resin. The fluorine-free thermoplastic resin may be a polyolefin resin. Polyolefin resins include polyethylene (PE) resin, polypropylene (PP) resin, and polymethylpentene (PMP) resin.

[0042] Examples of thermoplastic resins include polymethylpentene resins such as poly(4-methylpentene-1) resin (polymethylpentene resin) and poly(3-methylbutene-1) resin; polyethylene terephthalate resin; polybutylene terephthalate resin; polyethylene naphthalate resin; polyacetal resin; polyphenylene sulfide resin; polyether ether ketone resin; syndiotactic polystyrene resin; ethylene-carbon monoxide copolymer resin; polyamide resins such as nylon 6 resin and nylon 66 resin; cycloolefin polymer (COP) resin; polyphenylene ether (PPE) resin; polyetherimide (PEI) resin; and polyphenylene oxide (PPO) resin.

[0043] The thermoplastic resin may be a polymethylpentene resin. The polymethylpentene resin is a homopolymer or copolymer such as poly(4-methylpentene-1) resin and poly(3-methylpentene-1) resin. Examples of the copolymer include random copolymers and block copolymers. From the viewpoints of heat resistance and moldability, a homopolymer of poly(4-methylpentene-1) resin is preferred. Polymethylpentene resin has a melting point of 230°C to 240°C. Therefore, with this configuration, it is easy to obtain a porous film suitable for suppressing a reduction in thickness due to compression when attached to a device housing or the like.

[0044] The thermoplastic resin may be a poly(4-methylpentene-1) resin. Poly(4-methylpentene-1) resin refers to a homopolymer of 4-methylpentene-1 or a copolymer of 4-methylpentene-1 and at least one α-olefin. The composition ratio of 4-methylpentene-1 to the α-olefin contained in the copolymer can be adjusted so that the melting point is 180°C or higher.

[0045] The porous film 1 may contain additives such as a plasticizer and an antioxidant in addition to the thermoplastic resin.

[0046] The air permeability in the thickness direction of the porous membrane 1 may be 0.1 / 100 mL or more and 10,000 seconds / 100 mL or less, expressed as a Gurley number. In this specification, "Gurley number" refers to the air resistance (Gurley air permeability) measured in accordance with the Oken testing machine method specified in JIS P8117:2009. The lower limit of the air permeability of the porous membrane 1 may be 10 seconds / 100 mL or more, 30 seconds / 100 mL or more, 50 seconds / 100 mL or more, or even 70 seconds / 100 mL or more, expressed as a Gurley number. The upper limit of the air permeability of the porous membrane 1 may be 5,000 seconds / 100 mL or less, 1,000 seconds / 100 mL or less, or even 500 seconds / 100 mL or less, expressed as a Gurley number.

[0047] Even if the size of the porous membrane 1 is smaller than the recommended dimensions (50 mm x 50 mm) of the test piece for the Oken Testing Machine Method, the air resistance (Gurley air permeability) can be evaluated in accordance with the Oken Testing Machine Method by using a measuring jig.

[0048] The measurement jig has a shape and size that can be placed in the air permeability measurement section of the Oken tester, and is made of a thickness and material that will not deform due to the differential pressure applied to the test piece when measuring air permeability resistance. An example of the measurement jig is a 2 mm thick, 47 mm diameter SUS disk. A through hole with an opening smaller than the membrane to be evaluated is provided in the center of the surface of the measurement jig. The cross section of the through hole is typically circular, and the diameter is set so that the opening of the through hole is completely covered by the membrane to be evaluated. The diameter of the through hole can be, for example, 1 mm or 2 mm. Next, the porous membrane 1 to be evaluated is fixed to one side of the measurement jig so as to cover the opening. The fixation is performed so that during the air permeability resistance measurement, air passes only through the opening and the effective test portion of the porous membrane 1 to be evaluated (the portion overlapping with the opening when viewed from a direction perpendicular to the main surface of the fixed porous membrane 1), and the fixed portion does not obstruct the passage of air through the effective test portion of the porous membrane 1. To fix the porous membrane 1, a double-sided adhesive tape with a vent hole punched in the center, having a shape that matches the shape of the opening, can be used. The double-sided adhesive tape can be placed between the measurement jig and the porous membrane 1 so that the periphery of the vent hole matches the periphery of the opening. Next, the measurement jig with the porous membrane 1 fixed is set in the air permeability measurement section of the Oken tester so that the fixed surface of the porous membrane 1 is downstream of the air flow during measurement, and a test is performed using the Oken tester method, and the air permeability resistance indicated value t shown by the tester is recorded. Next, the recorded air permeability resistance indicated value t is measured using an effective test area of ​​6.452 [cm2] as specified in the Oken tester method. 2 ] per value t K In equation t K = {t × (area of ​​the effective test portion of the porous membrane 1 [cm 2 ]) / 6.452 [cm 2 ]}, and the resulting converted value t K can be the air resistance (Gurley air permeability) of porous membrane 1 measured according to Oken type testing machine method.It has been confirmed that the air resistance measured for porous membrane 1 that meets the recommended size (50mm x 50mm) of test piece of Oken type testing machine method without using measuring tool, and the air resistance measured after cutting porous membrane 1 into small pieces using measuring tool are well consistent, that is, the use of measuring tool does not substantially affect the measured value of air resistance.

[0049] The water pressure resistance of the porous membrane 1 may be 10 kPa or more, as evaluated by the water resistance test method B (high water pressure method) specified in JIS L1092:2009. The lower limit of the water pressure resistance of the porous membrane 1 may be 100 kPa or more, 130 kPa or more, or even 150 kPa or more. The upper limit of the water pressure resistance of the porous membrane 1 is, for example, 2000 kPa or less.

[0050] The water pressure resistance of the porous membrane 1 can be measured using a measuring tool in accordance with the above-mentioned water resistance test method as follows. An example of the measuring tool is a 47 mm diameter stainless steel (SUS) disk with a 2.0 mm diameter through-hole (having a circular cross section) in the center. This disk has a thickness that does not deform under the water pressure applied when measuring the water pressure resistance. Measurement of the water pressure resistance using this measuring tool can be carried out as follows.

[0051] The porous membrane 1 to be evaluated is fixed to one side of the measuring jig so as to cover the opening of the through-hole of the measuring jig. The porous membrane 1 is fixed so that water does not leak from the fixed portion of the membrane during water pressure resistance measurement. Double-sided adhesive tape with a water passage hole punched in the center, whose shape matches the shape of the opening, can be used to fix the porous membrane 1. The double-sided adhesive tape can be placed between the measuring jig and the porous membrane 1 so that the circumference of the water passage hole coincides with the circumference of the opening. Next, the measuring jig with the porous membrane 1 fixed is set in the testing device so that the surface opposite the fixed surface of the porous membrane 1 becomes the water pressure application surface during measurement, and the water pressure resistance is measured according to Water Resistance Test Method B (high water pressure method) specified in JIS L1092:2009. The water pressure resistance is measured based on the water pressure when water comes out from one point on the membrane surface of the porous membrane 1. The measured water pressure resistance can be used as the water pressure resistance of the porous membrane 1. The test device may have the same configuration as the water resistance test device exemplified in JIS L1092:2009 and have a test piece mounting structure on which the above-mentioned measuring jig can be set.

[0052] The porosity of the porous membrane 1 is, for example, 25% or more. The porosity of the porous membrane 1 may be 20% or more, or 35% or more. The porosity can be calculated by substituting the mass, thickness, area (area of ​​the main surface), and true density of the porous membrane 1 into the following formula (1).

[0053] Porosity (%) = {1 - (mass [g] / (thickness [cm] × area [cm 2 ]×True density [g / cm 3 ]))}×100 ...Formula (1)

[0054] The upper limit of the porosity of the porous film 1 is, for example, 95%. The upper limit of the porosity of the porous film 1 may be 90%.

[0055] The porous membrane 1 may be in the form of a sheet or a film. The thickness of the porous membrane 1 is, for example, 1 μm or more and 100 μm or less. Such a structure makes it easy to suppress a decrease in the thickness of the membrane due to compression when attached to a device housing or the like. The thickness of the porous membrane 1 may be 5 μm or more and 80 μm or less, or 10 μm or more and 70 μm or less.

[0056] The thickness of the porous membrane 1 can be determined by measuring the thickness at any five points on the porous membrane 1 using, for example, a dial gauge, and calculating the average value of these measured values. The thickness of the porous membrane 1 can also be determined by measuring the thickness at any five points on an SEM image of the cross section of the porous membrane 1 and calculating the average value of these measured values.

[0057] At least one of the main surfaces of the porous film 1 may be subjected to a surface modification treatment. Examples of the surface modification treatment include chemical treatment, sputter etching treatment, liquid repellent treatment, and plasma treatment. In the area subjected to the surface modification treatment, the bonding property of the porous film 1 is improved.

[0058] [Method for Producing Porous Membrane] The porous membrane 1 described above can be produced, for example, by the following method.

[0059] The method for producing the porous membrane 1 includes the steps of kneading a composition containing a thermoplastic resin having a melting point of 180°C or more and 300°C or less and a plasticizer to obtain a kneaded mixture (step S1), hot-pressing the kneaded mixture to obtain a pressed body (step S2), cooling the pressed body to obtain a molded body (step S3), stretching the molded body to obtain a sheet body (step S4), and extracting and removing the plasticizer from the sheet body (step S5).

[0060] Steps S1 to S3 correspond to a process for producing a precursor of the porous film 1. Steps S4 to S5 correspond to a process for growing a porous structure.

[0061] Step S1 is carried out, for example, at a temperature of 230° C. to 260° C. for 5 to 30 minutes.

[0062] As the thermoplastic resin having a melting point of 180° C. or more and 300° C. or less, a polymethylpentene resin can be used.

[0063] The composition containing a thermoplastic resin and a plasticizer may be mixed with a resin such as polyethylene, polypropylene, poly-1-butene, or cyclic polyolefin, as long as the properties of the porous membrane 1 are not affected.

[0064] The plasticizer is a non-volatile solvent that, when mixed with a thermoplastic resin such as polymethylpentene resin, forms a mixture at or above the melting point of the resin, and exhibits thermally induced phase separation when the mixture is cooled. The plasticizer may be in the form of a liquid or a solid at room temperature. A single plasticizer may be used, or two or more types of plasticizers may be mixed and used. Examples of such plasticizers include plasticizers having a kinematic viscosity of 50 to 150 mm at 40°C. 2 / s can be used.

[0065] The mixing ratio of the thermoplastic resin and the plasticizer is set so that a uniform mixture can be obtained in step S1 and a molded body can be formed in step S3. Specifically, the weight ratio of the thermoplastic resin in the composition containing the thermoplastic resin and the plasticizer is, for example, 20 wt% to 80 wt%, preferably 30 wt% to 70 wt%. By setting the weight ratio of the thermoplastic resin to 20 wt% or more, excessive reduction in viscosity of the composition can be avoided. By setting the weight ratio of the thermoplastic resin to 80 wt% or less, a good porous structure can be easily obtained.

[0066] The composition containing the thermoplastic resin and the plasticizer may further contain additives such as antioxidants, crystal nucleating agents, antistatic agents, flame retardants, lubricants, ultraviolet absorbers, colorants, and inorganic fillers for improving strength, depending on the purpose.

[0067] Step S2 is carried out for 2 to 30 minutes at a temperature of 230 to 260° C., for example. The thickness of the pressed body obtained in step S2 is, for example, 0.1 mm.

[0068] In step S3, the pressed body obtained in step S2 may be solidified by being cooled to a temperature sufficiently lower than the crystallization temperature of the thermoplastic resin, for example, by contacting it with a thermal conductor. Examples of the thermal conductor used for cooling include water, air, plasticizers, and metals. The thermal conductor used for cooling is preferably water.

[0069] In step S4, the molded body is stretched at least once in at least one axial direction. Stretching in at least one axial direction includes uniaxial stretching in the machine direction, uniaxial stretching in the transverse direction, simultaneous biaxial stretching, and sequential biaxial stretching. The molded body may be biaxially stretched sequentially or simultaneously. By step S4, pores are generated in the molded body.

[0070] The stretching temperature may be 20°C to 240°C, 50°C to 230°C, or even 100°C to 220°C in each of the longitudinal and transverse directions.

[0071] The stretching ratio in the longitudinal and / or transverse uniaxial directions may be 2.0 to 10.0 times, 2.0 to 8.0 times, or even 2.0 to 5.0 times.

[0072] The strain rate in the stretching may be 1% / sec to 10% / sec in the machine direction and / or the transverse direction, or 2% / sec to 8% / sec, or even 3% / sec to 5% / sec. When the strain rate is in the above range, breakage is unlikely to occur during stretching, further improving productivity. By having the strain rate in the above range, it is possible to obtain a stretching rate of 2.5 N / mm 2 It is easy to realize a porous film having a compressibility Rc of 20% or less in the thickness direction when a pressure of 1000 kJ / cm is applied.

[0073] In step S5, the plasticizer is extracted and removed from the sheet using, for example, an extraction solvent.

[0074] The extraction solvent is preferably a poor solvent for thermoplastic resins such as polymethylpentene resins, but a good solvent for plasticizers, and has a boiling point lower than the melting point of the porous membrane. Examples of such extraction solvents include hydrocarbons such as n-hexane and cyclohexane; halogenated hydrocarbons such as methylene chloride and 1,1,1-trichloroethane; alcohols such as ethanol and isopropanol; ethers such as diethyl ether and tetrahydrofuran; and ketones such as acetone and 2-butanone. Considering safety and other factors, alcohols and ketones are preferably used. Methyl ethyl ketone (MEK) may also be used as the extraction solvent.

[0075] Between step S4 and step S5, the sheet may be heat-set. Heat-set may be performed, for example, using a hot air circulating oven. Heat-set may reduce the thermal shrinkage of the sheet after stretching. The heat-set temperature is, for example, 50°C to 240°C. The heat-set temperature may be 100°C to 230°C, or may be 150°C to 220°C.

[0076] Heat setting may be performed after step S4, between steps S4 and S5, or both after steps S4 and S5. Examples of the heat setting method include fixing the film in the width direction with a tenter and continuously passing it through a heat treatment furnace, applying an appropriate tension and continuously passing it through a heat treatment furnace without fixing it in the width direction, and winding the film around a roll and feeding it into a heat treatment furnace in batches.

[0077] [Ventilation member] An example of the ventilation member of the present invention is shown in Figure 2. The ventilation member 2 (2A) in Figure 2 comprises a porous membrane 1. A first modification of the ventilation member in Figure 2 is shown in Figure 3. The ventilation member 2 (2B) in Figure 3 further comprises an air-permeable support material 3. The air-permeable support material 3 is laminated on the porous membrane 1. The air-permeable support material 3 can improve the strength and handleability of the ventilation member 2.

[0078] The breathable support material 3 typically has higher breathability in the thickness direction than the porous membrane 1. Examples of the breathable support material 3 include woven fabric, nonwoven fabric, net, and mesh. Examples of materials constituting the breathable support material 3 include polyesters such as polyethylene terephthalate (PET), polyolefins such as polyethylene (PE) and polypropylene (PP), and aramid resin. The shape of the breathable support material 3 may be the same as or different from the shape of the porous membrane 1 when viewed perpendicularly to the main surface of the ventilation member 2. The breathable support material 3 may have a shape corresponding to the peripheral portion of the porous membrane 1 when viewed perpendicularly to the main surface of the ventilation member 2. When the porous membrane 1 is circular, the shape is ring-shaped. The configuration and shape of the breathable support material 3 are not limited to the above examples.

[0079] The ventilation member 2B in Fig. 3 includes one breathable support material 3 arranged on one side of the porous membrane 1. The ventilation member 2 may include two or more breathable support materials 3. In the ventilation member 2, breathable support materials 3 may be arranged on both sides of the porous membrane 1. The porous membrane 1 and the breathable support material 3 may be joined by welding such as thermal welding or ultrasonic welding, an adhesive, or a pressure-sensitive adhesive.

[0080] The ventilation member 2 may include any layers and / or members other than those described above.

[0081] The thickness of the ventilation member 2 is, for example, 1 to 300 μm, and may be 50 to 200 μm.

[0082] The weight of the ventilation member 2 is, for example, 1.0 to 200.0 g / m 2 and 10.0 to 100.0 g / m 2 may be.

[0083] The ventilation member 2 can have the same properties as the porous membrane 1, for example, air permeability in the thickness direction and / or water pressure resistance.

[0084] The ventilation member 2 may be subjected to a liquid-repellent treatment and / or a coloring treatment.

[0085] The ventilation member 2 can be used as, for example, a filter member. However, the use of the ventilation member 2 is not limited to the above example.

[0086] The shape of the ventilation member 2, when viewed perpendicularly to the main surface of the ventilation member 2, is, for example, a polygon including a square and a rectangle, a circle, an ellipse, or a strip. The corners of the polygon may be rounded. However, the shape of the ventilation member 2 is not limited to the above examples. The strip-shaped ventilation member 2 may be wound to form a wound body. Furthermore, if necessary, it may be wound in a state where it is laminated with a release liner.

[0087] Fig. 4 shows a second modified example (wound body) of the ventilation member of Fig. 2. The wound body 10 shown in Fig. 4 includes the ventilation member 2A and release liner 11 of Fig. 2. The ventilation member 2A and the release liner 11 are bonded to each other by a pressure-sensitive adhesive layer 12. In the wound body 10, a release surface 13 formed when the release liner 11 is peeled from the ventilation member 2A is located between the ventilation member 2A and the pressure-sensitive adhesive layer 12. That is, in the wound body 10, when the release liner 11 is peeled off, the pressure-sensitive adhesive layer 12 is also peeled off from the ventilation member 2A, resulting in a ventilation member 2A that does not have the pressure-sensitive adhesive layer 12 formed on its surface.

[0088] The ventilation member 2A supplied by the roll 10 and having no pressure-sensitive adhesive layer 12 formed on its surface can be joined to the opening of the housing by any joining method. That is, the ventilation member 2A has a high degree of freedom in the method of joining to the opening of the housing. Joining methods include, for example, joining via a pressure-sensitive adhesive layer newly disposed on the surface of the ventilation member 2A, joining by thermal welding, and joining by ultrasonic welding.

[0089] The ventilation member 2A supplied by the wound body 10 can be processed into any shape as needed. That is, the ventilation member 2A has a high degree of freedom in terms of shape. However, "shape" also includes "size." The above means that the wound body 10 allows the ventilation member 2A that functions as a waterproof membrane to be supplied with a high degree of freedom in terms of the joining method to the opening of the housing and / or the shape.

[0090] Furthermore, with the wound body 10, misalignment between the ventilation member 2A and the release liner 11 during winding is suppressed by the pressure-sensitive adhesive layer 12. With the wound body 10, it is possible to suppress the occurrence of malfunctions (abnormal shape of the wound body) caused by tightness during winding, etc.

[0091] [Filter Element] An example of a filter element of the present invention is shown in Fig. 5. The filter element 4 (4A) in Fig. 5 has the above-described ventilation element 2 as a ventilation element that is breathable in the thickness direction and prevents the passage of foreign matter in that direction. The filter element 4A is a element that is placed on, for example, a surface of an object having an opening, and ensures ventilation through the opening while preventing the passage of foreign matter through the opening. In this case, the filter element 4A is usually placed so that the ventilation element 2 covers the opening of the object.

[0092] The filter member 4A includes an adhesive layer 5 disposed on one side of the ventilation member 2. The ventilation member 2 and the adhesive layer 5 are directly bonded to each other. The filter member 4A can be placed on the surface of an object via the adhesive layer 5.

[0093] When handling the filter member 4 or placing it on an object, a strong force may be applied to the filter member 4 in a specific direction. However, the ventilation member 2 has a tortoiseshell structure formed by multiple nodes and multiple fibrils, and is equipped with a porous membrane 1 that can suppress a decrease in membrane thickness due to compression. Therefore, for example, the filter member 4 can be manufactured without limiting the direction in which the ventilation member 2 (or porous membrane 1) is assembled into the filter member 4.

[0094] Examples of adhesives constituting the adhesive layer 5 include acrylic adhesives, silicone adhesives, urethane adhesives, epoxy adhesives, and rubber adhesives. When consideration must be given to using the filter member 4 at high temperatures, it is preferable to select an acrylic adhesive or a silicone adhesive, particularly a silicone adhesive, which have excellent heat resistance. The adhesive layer 5 may be a substrate-less double-sided adhesive tape. The adhesive may be a curable adhesive such as a phenolic resin, an epoxy resin, a urea resin, a polyurethane resin, a melamine resin, or a polyester resin.

[0095] The outer periphery of the ventilation member 2 and the outer periphery of the pressure-sensitive adhesive layer 5 are coincident when viewed perpendicularly to the main surface of the ventilation member 2. The shape of the pressure-sensitive adhesive layer 5 corresponds to the peripheral edge of the ventilation member 2 when viewed perpendicularly to the main surface of the ventilation member 2. The region of the ventilation member 2 to which the pressure-sensitive adhesive layer 5 is not bonded can be used as the ventilation region of the filter member 4A. However, the shape of the pressure-sensitive adhesive layer 5 is not limited to the above example.

[0096] The area of ​​the ventilation area is, for example, 40 mm 2 The filter member 4 having an area of ​​the ventilation region within this range is suitable for placement in an object having a small diameter opening, for example. The lower limit of the area of ​​the ventilation region is, for example, 0.008 mm 2 However, the area of ​​the ventilation region may be larger depending on the type of object on which the filter member 4 is placed.

[0097] Fig. 6 shows a first modified example of the filter member 4 in Fig. 5. The filter member 4 (4B) in Fig. 6 has the same configuration as the filter member 4A, except that it further includes a base material layer 6 disposed on one side of the ventilation member 2, and the ventilation member 2 and the pressure-sensitive adhesive layer 5 are bonded via the base material layer 6. The base material layer 6 can improve the strength and handleability of the filter member 4, and can prevent damage to the ventilation member 2 during handling or placement on an object.

[0098] Examples of materials constituting the base material layer 6 include polyolefins such as PE and PP, polyesters such as PET, silicone resins, polycarbonate, polyimide, polyamideimide, polyphenylene sulfide, polyether ether ketone (PEEK), polyvinyl chloride, fluororesins, and metals such as aluminum and stainless steel. Examples of fluororesins include PTFE, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), and tetrafluoroethylene-ethylene copolymer (ETFE). However, the materials constituting the base material layer 6 are not limited to the above examples.

[0099] The outer periphery of the ventilation member 2 and the outer periphery of the base material layer 6 are coincident when viewed perpendicularly to the main surface of the ventilation member 2. The shape of the base material layer 6 corresponds to the peripheral edge of the ventilation member 2 when viewed perpendicularly to the main surface of the ventilation member 2. The region of the ventilation member 2 to which the base material layer 6 is not joined can be used as the ventilation region of the filter member 4B. However, the shape of the base material layer 6 is not limited to the above example.

[0100] The ventilation member 2 and the base layer 6 may be joined with an adhesive or a adhesive, or may be joined by welding such as thermal welding or ultrasonic welding. The ventilation member 2 and the base layer 6 may be joined with an adhesive layer. The adhesive layer may have the same configuration as the adhesive layer 5. The base layer 6 and the adhesive layer 5 may be the base and adhesive layer of a single-sided adhesive tape or a double-sided adhesive tape, respectively.

[0101] Fig. 7 shows a second modification of the filter member 4 in Fig. 5. The filter member 4 (4C) in Fig. 7 has the same configuration as the filter member 4B, except that it further includes a base material layer 6 (6B) arranged on the other surface of the ventilation member 2. The ventilation member 2 is sandwiched between the pair of base material layers 6 (6A, 6B). This sandwiching structure can further improve the strength and handleability of the filter member 4.

[0102] FIG. 8 shows a third variation of the filter member 4 in FIG. 5 . The filter member 4 (4D) in FIG. 8 further includes a tab film 7, and has the same configuration as the filter member 4C, except that the base layer 6 (6B) and the tab film 7 are bonded to each other via a pressure-sensitive adhesive layer 5 (5B). The tab film 7 has a tab that protrudes outward beyond the outer periphery of the base layer 6B when viewed perpendicularly to the main surface of the base layer 6B. The filter member 4D can be handled or placed on the surface of an object by grasping the tab. The tab film 7 is typically removed when the filter member 4D is used. The tab film 7 can be made of the same material as the base layer 6. The tab film 7 is typically removed by grasping and lifting the tab. At this time, a strong force is applied to the ventilation member 2 in the lifting direction.

[0103] [Component Supply Assembly] The filter member 4 can be supplied, for example, by a component supply sheet. Fig. 9 shows an example of a component supply assembly that supplies the filter member 4. The component supply assembly 20 in Fig. 9 includes the filter member 4 to be placed on the surface of an object having an opening, and a base sheet 9 on whose surface the filter member 4 is placed. The component supply assembly 20 shown in Fig. 9 includes a filter member 4D as the filter member 4.

[0104] The filter member 4 (4D) is disposed on the base sheet 9 via the adhesive layer 5. The member supply assembly 20 can efficiently supply the filter member 4, for example, in the process of placing it on the surface of an object.

[0105] The filter member 4 may be disposed on the base sheet 9 via an adhesive layer provided on the surface of the base sheet 9 on which the filter member 4 is to be disposed. The adhesive layer on the surface on which the filter member 4 is to be disposed preferably has weak adhesiveness.

[0106] Although not shown in the drawings, a plurality of filter members 4 may be arranged on the surface of the base sheet 9 .

[0107] Examples of materials that make up the base sheet 9 include paper, metal, resin, and composite materials thereof. Examples of metal include stainless steel and aluminum. Examples of resin include polyester such as PET, and polyolefins such as PE and PP. However, the materials that make up the base sheet 9 are not limited to the above examples. The base sheet 9 may be in the form of a sheet or a strip. If the sheet 9 is in the form of a strip, the member supply assembly 20 may be wound to form a wound body.

[0108] Examples of objects on which the filter member 4 is disposed include the housing of an electronic device and the housing of a vehicle electrical component. The filter member 4 can be disposed on the outer surface and / or inner surface of the housing. In this case, the opening may be an air vent and / or a sound vent provided in the housing. Examples of electronic devices include wearable devices such as smart watches and wristbands; various cameras including action cameras and security cameras; information and communication devices such as mobile phones, smartphones, and tablets; virtual reality (VR) devices; augmented reality (AR) devices; and sensor devices. Examples of vehicle electrical components include lamps and ECUs. However, the objects are not limited to the above examples.

[0109] The foreign matter that is prevented from passing through by the arrangement of the filter member 4 is, for example, particles such as dust, and liquid water such as water droplets.

[0110] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.

[0111] [Example 1] Poly(4-methylpentene-1) resin (manufactured by Mitsui Chemicals, Inc., RT18, melting point: 232°C) was prepared as a thermoplastic resin. 2Liquid paraffin (MORESCO) with a 1000-µm viscosity (1000 µm / s) was prepared. Pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (BASF Japan) was prepared as an antioxidant. A mixture was obtained by mixing 50.0 wt% of thermoplastic resin, 49.8 wt% of plasticizer, and 0.2 wt% of antioxidant. The mixture was kneaded at 260°C for 30 minutes using a Labo Plastomill (Toyo Seiki Seisakusho) to obtain a uniform mixture. The mixture was then heat-pressed using a compression molding machine heated to 260°C to obtain a pressed body. The pressed body was sandwiched between a pair of polyimide plates and cooled by contacting it with 18°C ​​water to obtain a molded body.

[0112] Next, using a biaxial stretching machine, the molded body was subjected to simultaneous biaxial stretching under the conditions of a stretching temperature of 150°C and a stretching ratio of 2.5 times (longitudinal direction) x 2.5 times (transverse direction). The strain rate during stretching was 4% / sec (2.6 mm / sec) in both the longitudinal and transverse directions. This resulted in a sheet body. Finally, an extraction operation was performed by immersing the sheet body in MEK at room temperature for 2 minutes using methyl ethyl ketone (MEK) as the extraction solvent. This resulted in the extraction and removal of the plasticizer from the sheet body. The extraction operation was performed while the sheet body was fixed to a stainless steel frame to suppress shrinkage. In this way, the porous membrane of Example 1 was obtained.

[0113] FIG. 10 is a diagram (2500x magnification) showing the results of SEM observation of the surface of the porous membrane of Example 1.

[0114] [Example 2] A plasticizer having a kinematic viscosity of 68 mm at 40°C was used. 2 Liquid paraffin (MORESCO) with a viscosity of 1 / s was prepared. A mixture was obtained by mixing 70.0 wt% of thermoplastic resin, 29.8 wt% of plasticizer, and 0.2 wt% of antioxidant. The mixture was kneaded using a Labo Plastomill at 230°C for 30 minutes to obtain a uniform mixture. Except for these factors, the porous membrane of Example 2 was obtained by the same method as Example 1.

[0115] FIG. 11 is a diagram (2500x magnification) showing the results of SEM observation of the surface of the porous membrane of Example 2.

[0116] [Example 3] A plasticizer having a kinematic viscosity of 92 mm at 40°C was used. 2 / s of liquid paraffin (manufactured by MORESCO) was prepared. Except for these, the porous membrane of Example 3 was obtained in the same manner as in Example 1.

[0117] Fig. 12A is a diagram (2500x magnification) showing the results of SEM observation of the surface of the porous membrane of Example 3. Fig. 12B is a partially enlarged diagram (10000x magnification) of Fig. 12A. Fig. 12C is a diagram (1500x magnification) showing the results of SEM observation of the cross section of the porous membrane of Example 3.

[0118] [Example 4] A plasticizer having a kinematic viscosity of 68 mm at 40°C was used. 2 Liquid paraffin (manufactured by MORESCO) with a viscosity of 1 / s was prepared. A mixture was obtained by mixing 30.0 wt% thermoplastic resin, 69.8 wt% plasticizer, and 0.2 wt% antioxidant. The mixture was kneaded using a Labo Plastomill at 230°C for 30 minutes to obtain a uniform mixture. Simultaneous biaxial stretching was performed using a biaxial stretching machine at a stretching temperature of 150°C and a stretch ratio of 2.0 times (longitudinal direction) x 2.0 times (transverse direction). Except for these factors, the porous membrane of Example 4 was obtained by the same method as Example 1.

[0119] FIG. 13 is a diagram (2500x magnification) showing the results of SEM observation of the surface of the porous membrane of Example 4.

[0120] [Example 5] Use biaxial stretching machine to carry out simultaneous biaxial stretching under the conditions of stretching temperature 150 ℃, stretching ratio 2.0 times (longitudinal direction) × 2.0 times (transverse direction).Except this, by the same method as in Example 1, obtain the porous membrane of Example 5.

[0121] Fig. 14A is a diagram (2500x magnification) showing the results of SEM observation of the surface of the porous membrane of Example 5. Fig. 14B is a partially enlarged diagram (10000x magnification) of Fig. 14A.

[0122] Comparative Example 1 As a thermoplastic resin, poly(4-methylpentene-1) resin (manufactured by Mitsui Chemicals, Inc., MX002, melting point: 224°C) was prepared. 2Liquid paraffin (MORESCO) with a viscosity of 1 / s was prepared. A mixture was obtained by mixing 30.0 wt% of thermoplastic resin, 69.8 wt% of plasticizer, and 0.2 wt% of antioxidant. The mixture was kneaded using a Labo Plastomill at 230°C for 30 minutes to obtain a uniform mixture. Except for these factors, the membrane of Comparative Example 1 was obtained using the same method as in Example 1.

[0123] Fig. 15A is a diagram (2500x magnification) showing the results of SEM observation of the surface of the film of Comparative Example 1. Fig. 15B is a partially enlarged diagram (10000x magnification) of Fig. 15A. Fig. 15C is a diagram (2000x magnification) showing the results of SEM observation of the cross section of the film of Comparative Example 1.

[0124] Comparative Example 2 A membrane of Comparative Example 2 was obtained in the same manner as in Comparative Example 1, except that 50.0 wt % of a thermoplastic resin, 49.8 wt % of a plasticizer, and 0.2 wt % of an antioxidant were mixed to obtain a mixture.

[0125] FIG. 16 is a diagram (2500x magnification) showing the results of SEM observation of the surface of the film of Comparative Example 2.

[0126] Comparative Example 3 A membrane of Comparative Example 3 was obtained in the same manner as in Comparative Example 1, except that 70.0 wt % of a thermoplastic resin, 29.8 wt % of a plasticizer, and 0.2 wt % of an antioxidant were mixed to obtain a mixture.

[0127] FIG. 17 is a diagram (2500x magnification) showing the results of SEM observation of the surface of the film of Comparative Example 3.

[0128] The production conditions for Examples 1 to 5 and Comparative Examples 1 to 3 are shown in Table 1.

[0129]

[0130] Using the methods described above for the porous membranes, the Gurley air permeability, water pressure resistance, etc. were evaluated for the porous membranes of Examples 1 to 5 and the membranes of Comparative Examples 1 to 3. The evaluation results are shown in Table 2.

[0131]

[0132] [Example 6] The pressed body was sandwiched between polyimide plates and brought into contact with water at 90°C to cool the pressed body, thereby obtaining a molded body. Except for this, the membrane of Example 6 was obtained in the same manner as in Example 1.

[0133] [Example 7] The pressed body was sandwiched between polyimide plates and brought into contact with water at 5°C to cool the pressed body, thereby obtaining a molded body. Except for this, the membrane of Example 7 was obtained in the same manner as in Example 1.

[0134] Comparative Example 4 The membrane of Comparative Example 4 was obtained in the same manner as in Example 1, except that the pressed body was cooled by being left to stand at room temperature to obtain a molded body.

[0135] Table 3 shows the manufacturing conditions for Examples 6 to 7 and Comparative Example 4, along with the manufacturing conditions for Example 1. Fig. 19 shows the results of measuring the actual film temperatures from after hot pressing to cooling with a thermocouple at intervals of 100 ms for Example 1, Examples 6 to 7, and Comparative Example 4.

[0136] Fig. 18A is a diagram (2500x magnification) showing the results of SEM observation of the surface of the film of Comparative Example 4. Fig. 18B is a partially enlarged diagram (20000x magnification) of Fig. 18A.

[0137]

[0138] As can be seen from a comparison of Figures 10 to 12B and 13 to 14B with Figures 15A to 15B and 16 to 17, the porous membranes of Examples 1 to 5 had a tortoiseshell structure formed by multiple nodes and multiple fibrils. Specifically, in the porous membranes of Examples 1 to 5, island regions formed by multiple nodes were irregularly connected, and these island regions were connected to each other by multiple fibrils. In contrast, the membranes of Comparative Examples 1 to 3 did not have such a tortoiseshell structure. Because the membranes of Comparative Examples 1 to 3 did not have island regions, it was not possible to determine the average spacing between the island regions or the average area of ​​the island regions.

[0139] The porous membranes of Examples 1 to 5 contained multiple island regions and multiple fibrils extending in multiple directions from each island region. It was also confirmed that the island regions were connected or overlapped without the need for multiple fibrils (see, for example, Figure 14B). Some porous membranes contained a mixture of island regions, which were aggregates of multiple nodes, and nodes (see, for example, Figure 12B). Some porous membranes contained planar regions formed by the dense accumulation of multiple fibrils extending in multiple directions from each island region (see, for example, Figures 10 and 11).

[0140] On the other hand, the membranes of Comparative Examples 1 to 3 exhibited a structure that does not have clear nodes and fibrils, that is, a so-called cell structure.

[0141] The reason why a tortoiseshell structure was formed in the porous membranes of Examples 1 to 5, while a tortoiseshell structure was not formed in the membranes of Comparative Examples 1 to 3, is presumed to be as follows: The thermoplastic resin (RT18) used in Examples 1 to 5 and the thermoplastic resin (MX002) used in Comparative Examples 1 to 3 contain ethylene units as polymer chain units. MX002 is known to contain more ethylene units than RT18. Due to the difference in ethylene unit content, Examples 1 to 5 and Comparative Examples 1 to 3 differ in the compatibility between the thermoplastic resin and the plasticizer and the temperature range at which the thermoplastic resin precipitates as a solid phase, which is thought to have led to differences in the structure after phase separation. As a result, a tortoiseshell structure was ultimately obtained in Examples 1 to 5, while Comparative Examples 1 to 3 produced a cell structure without a tortoiseshell structure.

[0142] Furthermore, among Examples 6 to 7 and Comparative Example 4, in which the same RT18 thermoplastic resin as in Example 1 was used but the cooling conditions were changed, the tortoiseshell structure was confirmed in Examples 6 and 7, just like in Example 1 (not shown). On the other hand, in Comparative Example 4, in which air cooling was performed, the tortoiseshell structure was not confirmed (see Figures 18A and 18B). As shown in Figure 19, in Comparative Example 4, the cooling rate of the thermoplastic resin was relatively slow, which significantly promoted crystal growth and phase separation, and it is thought that the tortoiseshell structure was not formed. From these results, it is thought that the cooling conditions also affect the formation of the tortoiseshell structure.

[0143] 12C and 15C, multiple clustered nodes were uniformly present throughout the thickness of the porous membrane of Example 3. In contrast, no such structure was observed in the membrane of Comparative Example 1.

[0144] As shown in Table 2, the porous membranes of Examples 1 to 5 had a resistance of 2.5 N / mm 2 In contrast, the films of Comparative Examples 1 to 3 exhibited compressibility Rc of 21.4% to 42.5%.

[0145] From these results, it can be seen that the porous films of Examples 1 to 5 can suppress the reduction in film thickness caused by compression when attached to a device housing or the like.

[0146] The technology of the present invention can be applied to, for example, waterproof gas-permeable membranes, waterproof sound-permeable membranes, separators for electricity storage devices, and the like.

Claims

1. A porous membrane comprising as a main component a thermoplastic resin having a melting point of 180°C or more and 300°C or less, said porous membrane having a tortoiseshell structure formed by a plurality of nodes and a plurality of fibrils.

2. 2.5N / mm 2 The porous membrane according to claim 1 , wherein the compressibility of the porous membrane in the thickness direction when a pressure of 1000 g is applied thereto is 20% or less.

3. A porous membrane containing as its main component a thermoplastic resin having a melting point of 180°C or more and 300°C or less, and having a strength of 2.5 N / mm 2 A porous membrane, wherein a compressibility of the porous membrane in a thickness direction when a pressure of 1000 g is applied thereto is 20% or less.

4. The porous membrane according to any one of claims 1 to 3, wherein the thermoplastic resin comprises a polymethylpentene resin.

5. The porous membrane according to any one of claims 1 to 3, wherein a plurality of the nodes are included along the thickness direction when a cross section of the porous membrane is observed.

6. The porous membrane according to any one of claims 1 to 3, having an air permeability, expressed in Gurley number, of 1000 seconds / 100 mL or less.

7. The porous membrane according to any one of claims 1 to 3, wherein the porosity of the porous membrane is 25% or more.

8. A filter member comprising: a porous membrane according to any one of claims 1 to 7; and an adhesive layer bonded to the porous membrane.

9. A component supply assembly comprising a filter member to be placed on a surface of an object having an opening, and a base sheet with the filter member placed on a surface thereof, wherein the filter member comprises: a porous membrane having a shape that covers the opening when placed on the surface; and an adhesive layer bonded to the porous membrane, and the porous membrane is a porous membrane according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Olefin resin microporous biaxially oriented film, method for producing the same, heat-resistant olefin resin microporous biaxially oriented film, and method for producing the same

    JP2017095576A

  • Microporous membrane and its manufacturing method

    JP2005255876A

  • Heat resistant polyolefin microporous film and manufacturing method thereof

    JP2011184671A

  • Microporous membrane and cell separator including the same

    JP2011228056A

  • Surface-modified porous film and manufacturing method thereof

    JP2019150775A

Cited By

  • Porous film, method for producing porous film, ventilation member, and sheet for supplying member

    WO2025249338A1