Etching method for silicon-containing organic dielectric layer, and semiconductor processing device

Through the alternating etching steps, different proportions of oxygen and fluorine gas are used to etch the silicon-containing organic dielectric layer, which solves the problem of uneven morphology at the bottom of the trench or through holes, and achieves a smoother morphology and better electronic device performance.

WO2025082211A1PCT designated stage expired Publication Date: 2025-04-24BEIJING NAURA MICROELECTRONICS EQUIP CO LTD

Patent Information

Application Number
PCT/CN2024/122875
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-16
Filing Date
2024-09-30
Publication Date
2025-04-24

AI Technical Summary

Technical Problem

When etching the silicon-containing organic dielectric layer, micro-trenches or uneven morphology are prone to appear at the bottom of the trench or through-hole, resulting in too concentrated electric field stress and affecting the performance of electronic devices.

Method used

The silicon-containing organic dielectric layer is etched using at least two etching steps alternately, the first etching step uses an etching gas containing at least oxygen gas, and the second etching step uses an etching gas containing at least oxygen gas and fluorine gas to adjust the gas flow ratio of the fluorine element to the oxygen element to adjust the etching rate of different elements and reduce micro grooves or protrusions at the bottom of the trench or through holes.

Benefits of technology

Through the alternating etching steps, adjusting the proportion of the etching gas can make the bottom of the trench or through holes have a smooth morphology, avoiding excessive concentration of electric field stress, and improving the performance of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024122875_24042025_PF_FP_ABST
    Figure CN2024122875_24042025_PF_FP_ABST
Patent Text Reader

Abstract

The present application discloses an etching method for a silicon-containing organic dielectric layer, and a semiconductor processing device. A silicon-containing organic dielectric layer is etched by cyclically and alternately performing at least two etching steps, wherein the at least two etching steps comprise a first etching step and a second etching step, etching gas adopted in the first etching step at least comprises oxygen-containing gas, and etching gas adopted in the second etching step at least comprises oxygen-containing gas and fluorine-containing gas, so that the first etching step and the second etching step can be carried out cyclically and alternately, a gas flow rate ratio of the fluorine-containing gas to the oxygen-containing gas is adjusted, the etching rates of different elements in the silicon-containing organic dielectric layer can be adjusted, and thus micro trenches or protrusions at the bottoms of trenches or through holes of the silicon-containing organic dielectric layer can be reduced, so that the bottoms of the trenches or through holes have a smooth morphology, and the situation that the performance of an electronic device is affected due to the fact that the electric field stress at the bottoms of trenches or through holes is too concentrated can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Etching method of silicon-containing organic dielectric layer and semiconductor process equipment Technical Field

[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to an etching method for a silicon-containing organic dielectric layer and semiconductor process equipment. Background Art

[0002] With the rapid development of integrated circuits, silicon-containing organic materials such as benzocyclobutene (BCB) are being widely used as dielectric materials in electronic devices across various fields due to their wide curing temperature range, low curing temperature, low dielectric constant, improved adhesion, and superior hydrophobicity. However, when etching silicon-containing organic dielectric layers made from BCB and other silicon-containing organic materials, micro-trenching or uneven topography often occurs at the bottom of the etched trenches or through-holes. This results in excessive concentration of electric field stress at the bottom of the trenches or through-holes, affecting the performance of the electronic devices.

[0003] Summary of the Invention

[0004] The present application discloses an etching method for a silicon-containing organic dielectric layer and a semiconductor process equipment, which can reduce microgrooves or protrusions at the bottom of a groove or through-hole etched by the silicon-containing organic dielectric layer, so that the bottom of the groove or through-hole has a smooth morphology.

[0005] In a first aspect, the present application discloses a method for etching a silicon-containing organic dielectric layer, comprising: etching the silicon-containing organic dielectric layer using at least two etching steps that alternate in a cycle; wherein the at least two etching steps include a first etching step and a second etching step, the etching gas used in the first etching step includes at least an oxygen-containing gas, and the etching gas used in the second etching step includes at least an oxygen-containing gas and a fluorine-containing gas.

[0006] In some optional examples, during the alternating cycle of at least two etching steps, the ratio of fluorine element to oxygen element is greater than 0 and less than or equal to 15, or the content of fluorine element is 0; or in the first etching step, the ratio of fluorine element to oxygen element is less than 0.01, or the content of fluorine element is 0.

[0007] In some optional examples, the gas flow rate range of the oxygen-containing gas used in the first etching step is 5 sccm to 200 sccm; and / or the gas flow rate range of the oxygen-containing gas used in the second etching step is 5 sccm to 200 sccm, and the gas flow rate range of the fluorine-containing gas used in the second etching step is 5 sccm to 20 sccm.

[0008] In some optional examples, the material of the silicon-containing organic dielectric layer includes BCB, the oxygen-containing gas includes at least one of O2, CO2, CO and SO2, and the fluorine-containing gas includes at least one of SF6, CF4, C4F8, CHF3, NF3, SF6, CH2F2 and C2F6.

[0009] In some optional examples, the etching gas used in the first etching step and the second etching step further includes an inert gas; the inert gas includes at least one of Ar, He and Ne.

[0010] In some optional examples, the gas flow rate of the inert gas used in the first etching step is in the range of 5 sccm to 200 sccm, and the gas flow rate of the inert gas used in the second etching step is in the range of 5 sccm to 200 sccm.

[0011] In some optional examples, during the alternating process of at least two etching steps, the ratio of fluorine element to inert element is greater than 0 and less than or equal to 60, or the content of fluorine element is 0; or

[0012] In the first etching step, the ratio of fluorine element to inert element is less than 0.01, or the content of fluorine element is 0.

[0013] In some optional examples, during the alternating process of at least two etching step cycles, the gas flow rate of the oxygen-containing gas remains unchanged, the gas flow rate of the inert gas remains unchanged, and the gas flow rate change curve of the fluorine-containing gas presents a pulse waveform.

[0014] In some optional examples, the process time range of the first etching step is 0.2s to 8s, and / or the process time range of the second etching step is 0.2s to 5s.

[0015] In some optional examples, the chamber pressure range used in the first etching step is 2 mTorr to 30 mTorr; and / or the chamber pressure range used in the second etching step is 2 mTorr to 30 mTorr.

[0016] In some optional examples, the at least two etching steps also include at least one third etching step, and the at least one third etching step is located between the first etching step and the second etching step, and the flow rate of the etching gas used in the third etching step is smaller than the flow rate of the etching gas used in the first etching step and the second etching step.

[0017] In the second aspect, the present application discloses a semiconductor process equipment, including a process chamber, an air inlet assembly, an upper electrode assembly, a lower electrode assembly and a control device, the control device including at least one memory and at least one processor, the memory storing a computer program, the processor executing the computer program to implement the etching method of the silicon-containing organic dielectric layer as described above.

[0018] The present application discloses an etching method and semiconductor process equipment for a silicon-containing organic dielectric layer. The silicon-containing organic dielectric layer is etched using at least two cyclically alternating etching steps. The at least two etching steps include a first etching step and a second etching step. The etching gas used in the first etching step includes at least an oxygen-containing gas, and the etching gas used in the second etching step includes at least an oxygen-containing gas and a fluorine-containing gas. Thus, by cyclically alternating the first etching step and the second etching step, the gas flow ratio of the fluorine-containing gas to the oxygen-containing gas can be adjusted, thereby adjusting the etching rate of different elements in the silicon-containing organic dielectric layer. Furthermore, microgrooves or protrusions at the bottom of grooves or through-holes in the silicon-containing organic dielectric layer can be reduced, resulting in a smooth morphology at the bottom of the grooves or through-holes. This prevents excessive concentration of electric field stress at the bottom of the grooves or through-holes, which can affect the performance of electronic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the background technology, the drawings required for use in the embodiments of the present application or the background technology will be described below.

[0020] FIG1 is a SEM image of a trench of a silicon-containing organic dielectric layer etched by a current etching method.

[0021] 2 to 8 are schematic cross-sectional views of electronic devices in various steps of an etching method for a silicon-containing organic dielectric layer disclosed in an embodiment of the present application.

[0022] FIG9 is a SEM image of a groove with an uneven bottom surface disclosed in an embodiment of the present application.

[0023] FIG10 is an SEM image of a groove having a micro-groove morphology at the bottom disclosed in an embodiment of the present application.

[0024] FIG. 11 is a SEM image of a groove etched by an etching method for a silicon-containing organic dielectric layer disclosed in an embodiment of the present application.

[0025] FIG12 is an SEM image of a trench with a bow-shaped sidewall disclosed in an embodiment of the present application.

[0026] Figure 13 is a schematic diagram of the curve of the gas flow rate changes of oxygen-containing gas (such as O2), fluorine-containing gas (such as SF6) and inert gas (such as Ar) over time in an etching method of a silicon-containing organic dielectric layer disclosed in an embodiment of the present application.

[0027] Figure 14 is a curve showing the change in the flow ratio of fluorine-containing gas (such as SF6) and inert gas (such as Ar) over time in an etching method for a silicon-containing organic dielectric layer disclosed in an embodiment of the present application, and a schematic diagram of a curve showing the change in the flow ratio of fluorine-containing gas (such as SF6) and oxygen-containing gas (such as O2) over time.

[0028] FIG15 is a schematic structural diagram of a semiconductor process equipment disclosed in an embodiment of the present application. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0030] As shown in FIG1 , when a silicon-containing organic dielectric layer made of silicon-containing organic materials such as BCB is etched using current etching methods, sub-trench or uneven topography is likely to appear at the bottom of the etched trench or through-hole, resulting in excessive concentration of electric field stress at the bottom of the trench or through-hole, thereby affecting the performance of the electronic device.

[0031] The inventors have discovered that an imbalance in the etching rates of different elements in the silicon-containing organic dielectric layer is the primary cause of microgrooves or uneven topography. For example, if the etching rate of Si in the silicon-containing organic dielectric layer is higher than that of CH, an uneven topography will appear at the bottom of the silicon-containing organic dielectric layer. If the etching rate of Si is lower than that of CH, microgrooves will appear at the bottom of the silicon-containing organic dielectric layer.

[0032] Based on this, the present application discloses a method for etching a silicon-containing organic dielectric layer, comprising:

[0033] The silicon-containing organic dielectric layer is etched using at least two cyclically alternating etching steps, and the etching gas used in at least one of the at least two cyclically alternating etching steps includes an oxygen-containing gas, and the etching gas used in at least one etching step includes an oxygen-containing gas and a fluorine-containing gas, so that the bottom of the groove or through hole of the silicon-containing organic dielectric layer has a smooth morphology.

[0034] As an optional implementation of the disclosure of this application, an embodiment of this application discloses a method for etching a silicon-containing organic dielectric layer, the etching method comprising:

[0035] The silicon-containing organic dielectric layer is etched using at least two etching steps that are cyclically alternating, wherein the at least two etching steps include a first etching step and a second etching step, the etching gas used in the first etching step includes at least an oxygen-containing gas, and the etching gas used in the second etching step includes at least an oxygen-containing gas and a fluorine-containing gas.

[0036] In the embodiments of the present application, electronic devices prepared using silicon-containing organic dielectric layers can be used in fields such as wireless communication base stations, satellite navigation, and mobile communications. The electronic devices can be power amplifiers, rectifiers, oscillators, phase-locked devices, controllers, and memories, etc.

[0037] As shown in FIG2 , the electronic device may include, for example, a substrate 101 and a silicon-containing organic dielectric layer 11 located on one side of the substrate 101 . In some optional embodiments, a metal layer 102 and an isolation layer 103 may be further included between the substrate 101 and the silicon-containing organic dielectric layer 11 .

[0038] The substrate 101 may include a gallium arsenide (GaAs) substrate, a silicon substrate, a germanium substrate or a silicon germanium substrate, etc., the metal layer 102 may include an Au metal layer, etc., the isolation layer 103 may include a silicon nitride layer, etc., and the material of the silicon-containing organic dielectric layer 11 includes BCB.

[0039] In some embodiments of the present application, when etching the silicon-containing organic dielectric layer 11, first, as shown in FIG3 , an anti-reflective layer 12 and a patterned photoresist layer 13 are sequentially formed on the surface of the silicon-containing organic dielectric layer 11 facing away from the substrate 101. The anti-reflective layer 12 may be made of silicon nitride or silicon oxynitride. A mask having a preset mask pattern may be used to expose the entire surface of the photoresist layer to transfer the mask pattern to the photoresist layer. The photoresist layer is then developed to form the patterned photoresist layer 13.

[0040] Then, as shown in FIG4 , the anti-reflective layer 12 is etched using the patterned photoresist layer 13 as a mask, so that the mask pattern is transferred to the anti-reflective layer 12. The anti-reflective layer 12 can alleviate or eliminate the standing wave effect of the photoresist layer 13, thereby increasing the accuracy of the transfer of the mask pattern from the mask plate to the photoresist layer. Of course, in some embodiments of the present application, the anti-reflective layer 12 may not be included, and this will not be discussed in detail here.

[0041] 5 , the patterned photoresist layer 13 is used as a mask, and the silicon-containing organic dielectric layer 11 is etched by a first etching step so that the depth of the groove 110 is a first preset depth h1. Then, as shown in FIG6 , the silicon-containing organic dielectric layer 11 is etched by a second etching step so that the depth of the groove 110 is a second preset depth h2, where h2 is greater than h1. Then, as shown in FIG7 , the silicon-containing organic dielectric layer 11 is etched by the first etching step so that the depth of the groove 110 is a third preset depth h3, where h3 is greater than h2. Then, as shown in FIG8 , the silicon-containing organic dielectric layer 11 is etched by a second etching step so that the depth of the groove 110 is a fourth preset depth h4, where h4 is greater than h3. This cycle is repeated until the depth of the groove 110 reaches the desired depth, thereby forming the desired groove or through-hole. It should be noted that, in the embodiment of the present application, at least two etching steps for etching the silicon-containing organic dielectric layer 11 both adopt a dry etching process, such as a plasma etching process.

[0042] In some embodiments, the anti-reflection layer 12 can be etched first, and then the silicon-containing organic dielectric layer 11 can be etched using the first etching step. Of course, the present application is not limited to this. In other embodiments, the anti-reflection layer 12 can be etched while the silicon-containing organic dielectric layer 11 is etched using the first etching step. This will not be repeated here.

[0043] In some embodiments of the present application, the silicon-containing organic dielectric layer 11 can be etched first using a first etching step, and then the silicon-containing organic dielectric layer 11 can be etched using a second etching step. However, the present application is not limited to this. In other embodiments, the silicon-containing organic dielectric layer 11 can be etched first using a second etching step, and then the silicon-containing organic dielectric layer 11 can be etched using the first etching step. The details will not be repeated here.

[0044] In some embodiments of the present application, the oxygen-containing gas includes at least one of O2, CO2, CO, and SO2, and the fluorine-containing gas includes at least one of SF6, CF4, C4F8, CHF3, NF3, SF6, CH2F2, and C2F6. Furthermore, in some embodiments, the oxygen-containing gas includes O2, and the fluorine-containing gas includes SF6. Based on this, in some embodiments, the etching gas in the first etching step includes O2, and the etching gas in the second etching step includes O2 and SF6.

[0045] Since the etching gas used in the first etching step includes at least an oxygen-containing gas (such as O2), the etching gas used in the first etching step is substantially fluorine-free, the flow ratio of fluorine to oxygen is less than 0.01, or the fluorine content is zero, and the etching gas used in the second etching step includes at least an oxygen-containing gas (such as O2) and a fluorine-containing gas (such as SF6), and the first etching step and the second etching step are cyclically performed, the first etching step and the second etching step can be cyclically performed alternately, for example, by intermittently introducing fluorine-containing gas and adjusting the gas flow ratio of fluorine-containing gas to oxygen-containing gas in the process chamber to adjust the ratio of fluorine to oxygen in the process chamber, thereby adjusting the etching rate of different elements in the silicon-containing organic dielectric layer 11, thereby reducing micro-grooves or protrusions at the bottom of the grooves or through-holes etched in the silicon-containing organic dielectric layer 11, so that the bottom of the grooves or through-holes has a smooth morphology, thereby preventing excessive concentration of electric field stress at the bottom of the grooves or through-holes that affects the performance of electronic devices.

[0046] In some embodiments of the present application, during the alternating cycles of at least two etching steps, the ratio of fluorine to oxygen in the process chamber is greater than 0 and less than or equal to 15, or the fluorine content is zero, to achieve a smoother morphology at the bottom of the trench or via. It is understood that in some embodiments, because the first etching step does not include a fluorine-containing gas, i.e., the fluorine content is zero, the fluorine to oxygen ratio is zero when the first etching step is performed during the alternating cycles of at least two etching steps. In other embodiments, the first etching step may also include a small amount of fluorine-containing gas, for example, a fluorine to oxygen ratio of less than 0.01. In some embodiments, the fluorine to oxygen ratio can be greater than 0 and less than or equal to 15, or the fluorine content can be zero, by setting the SF6 to O2 gas flow ratio to greater than 0 and less than or equal to 5, or by setting the SF6 gas flow rate to zero. Of course, the present application is not limited to this. In actual applications, the flow ratio range of the fluorine-containing gas to the oxygen-containing gas can be adjusted based on the composition of the fluorine-containing gas and the oxygen-containing gas, which will not be further described here.

[0047] It can be understood that, in some embodiments, the etching gas used in the first etching step does not include fluorine-containing gas (such as SF6), or in other words, the gas flow rate of the fluorine-containing gas (such as SF6) used in the first etching step is 0. However, the present application is not limited to this. In other embodiments, the etching gas used in the first etching step may also include fluorine-containing gas (such as SF6), but it is necessary to ensure that the gas flow rate of the fluorine-containing gas (such as SF6) in the etching gas used in the first etching step is less than the gas flow rate of the fluorine-containing gas (such as SF6) in the etching gas used in the second etching step. In other words, as long as it is ensured that during the alternating cycle of at least two etching steps, the ratio of fluorine element to oxygen element in the process chamber is greater than 0 and less than or equal to 15, or the content of fluorine element is 0, it can be sufficient.

[0048] The following uses BCB material as an example to explain the principle of adjusting the etching rate of different elements in the silicon-containing organic dielectric layer 11. The molecular formula of BCB is C4H 12 OSi2, the BCB etching process includes etching of CH elements and etching of Si elements. Fluorine-containing gases (such as SF6) dissociate under a high-frequency electromagnetic field to produce F ions and F-containing radicals, which etch Si elements, resulting in gaseous SiFx. F ions and F-containing radicals etch CH elements, resulting in gaseous CFx and HFx. Oxygen-containing gases (such as O2) dissociate to produce O ions and O-containing radicals, which etch Si elements, resulting in non-volatile SiOx deposits that hinder the etching of Si elements. O ions and O-containing radicals etch CH elements, generating volatile gaseous substances CO, CO2, and HO. In other words, the etching rate of oxygen-containing gases (such as O2) on Si is lower than that of fluorine-containing gases (such as SF6) on Si.

[0049] It can be seen from the molecular formula of BCB that the content of Si element in BCB is relatively small, the content of CH element is relatively large, and the generation rate of SiFx is greater than the generation rate of CFx and HFx. Therefore, if only fluorine-containing gas such as SF6 is used to etch BCB, or if the gas flow ratio of fluorine-containing gas (such as SF6) to oxygen-containing gas (such as O2) is greater than 5, the etching rate of Si element will be greater than the etching rate of CH element, which will not only significantly reduce the etching rate of BCB material, but also cause the bottom of the groove or through-hole of BCB to have an uneven morphology as shown in Figure 9, resulting in excessive concentration of electric field stress at the bottom of the groove or through-hole, affecting the performance of electronic devices.

[0050] If only oxygen-containing gas (such as O2) is used to etch BCB, or if the gas flow ratio of fluorine-containing gas (such as SF6) to oxygen-containing gas (such as O2) is greater than and close to 0, or the gas flow of fluorine-containing gas (such as SF6) is 0, the etching rate of Si element will be lower than the etching rate of CH element, and the bottom of the groove or through-hole of BCB will have a micro-groove morphology as shown in Figure 10, resulting in excessive concentration of electric field stress at the bottom of the groove or through-hole, affecting the performance of the electronic device.

[0051] The BCB is etched by using a first etching step and a second etching step that are cyclically alternating. The first etching step and the second etching step can be performed cyclically alternatingly, for example, fluorine-containing gas (such as SF6) is intermittently introduced, and the gas flow ratio of fluorine-containing gas (such as SF6) to oxygen-containing gas (such as O2) in the process chamber is adjusted, for example, the flow ratio range of SF6 to O2 is greater than 0 and less than or equal to 15, or the gas flow of SF6 is 0, so that the ratio of fluorine element to oxygen element can be adjusted, and the etching rate of Si element and the etching rate of CH element can be balanced, which not only ensures that the etching rate of BCB meets the requirements, but also makes the bottom of the groove or through-hole of BCB have a smooth morphology as shown in Figure 11, thereby avoiding excessive concentration of electric field stress at the bottom of the groove or through-hole that affects the performance of the electronic device.

[0052] In other words, the etching rates of oxygen and fluorine on Si are different, and the etching rates of oxygen and fluorine on CH are also different. For example, the etching rate of fluorine on Si is greater than that of oxygen, and the etching rate of fluorine on CH is less than that of oxygen. By intermittently introducing fluorine-containing gas (such as SF6) to adjust the gas flow ratio of fluorine-containing gas (such as SF6) and oxygen-containing gas (such as O2) in the process chamber, the flow ratio of fluorine and oxygen can be adjusted, and then the etching rate of Si and the etching rate of CH can be adjusted, so that the etching rate of Si and the etching rate of CH are balanced.

[0053] Of course, in some embodiments, the gas flow ratio of fluorine-containing gas (such as SF6) and oxygen-containing gas (such as O2) in the process chamber can be adjusted by adjusting the gas flow and / or process time of the first etching step and / or the second etching step, or the flow ratio of fluorine element and oxygen element in the process chamber can be adjusted.

[0054] It should be noted that although the second etching step is used to etch the BCB, the etching rate of the Si element and the etching rate of the CH element can be adjusted by adjusting the gas flow ratio of the fluorine-containing gas (such as SF6) and the oxygen-containing gas (such as O2) in the second etching step. However, as shown in Figure 12, this will cause the sidewalls of the trench or through-hole to have a bowing morphology, making adjacent trenches or through-holes have the risk of cross-linking or short circuiting. The use of the first etching step and the second etching step in a cyclic alternation can effectively avoid the presence of F ions and F-containing radicals in the chamber, thereby avoiding the bowing morphology on the sidewalls of the trench or through-hole.

[0055] In some embodiments of the present application, the gas flow rate range of the oxygen-containing gas (such as O2) used in the first etching step is 5 sccm to 200 sccm; and / or, the gas flow rate range of the oxygen-containing gas (such as O2) used in the second etching step is 5 sccm to 200 sccm, and the gas flow rate range of the fluorine-containing gas (such as SF6) is 5 sccm to 20 sccm.

[0056] In some embodiments of the present application, the first etching step employs a process time ranging from 0.2s to 8s, and / or the second etching step employs a process time ranging from 0.2s to 5s. This not only facilitates the control of the etching gas, but also facilitates achieving a smooth morphology at the bottom of the trench or through-hole in the silicon-containing organic dielectric layer.

[0057] It should be noted that if the process time used in the first etching step and the second etching step is less than 0.2s, it will exceed the shortest controllable gas intake time, which is not conducive to gas control. If the process time used in the second etching step is greater than 5s, the flow ratio of SF6 and O2 will be greater than 5, resulting in an uneven morphology at the bottom of the BCB groove or through-hole. If the process time used in the first etching step is greater than 8s, the flow ratio of SF6 and O2 will be greater than and close to 0, or the SF6 gas flow rate will be 0, resulting in a micro-groove morphology at the bottom of the BCB groove or through-hole.

[0058] In some embodiments of the present application, the chamber pressure used in the first etching step is in the range of 2 mTorr to 30 mTorr, and / or the chamber pressure used in the second etching step is in the range of 2 mTorr to 30 mTorr. Based on this, it is possible to avoid the etching effect of the silicon-containing organic dielectric layer being affected by excessive or insufficient chamber pressure. In some embodiments, the chamber pressure used in the first etching step is the same as the chamber pressure used in the second etching step.

[0059] In some embodiments of the present application, the upper RF power used in the first etching step is in the range of 300 W to 2500 W, and the lower RF power is in the range of 100 W to 1200 W, and / or the upper RF power used in the second etching step is in the range of 300 W to 2500 W, and the lower RF power is in the range of 100 W to 1200 W. In some embodiments, the upper RF power used in the first etching step is the same as the upper RF power used in the second etching step, and the lower RF power used in the first etching step is the same as the lower RF power used in the second etching step.

[0060] In some specific examples, the first etching step uses an oxygen-containing gas (such as O2) with a gas flow rate of 32 sccm, a process time range of 3 seconds, a chamber pressure range of 4 mTorr, an upper RF power range of 300 W, and a lower RF power range of 100 W. The second etching step uses an oxygen-containing gas (such as O2) with a gas flow rate range of 32 sccm, a fluorine-containing gas (such as SF6) with a gas flow rate range of 8 sccm, a process time range of 2 seconds, a chamber pressure range of 4 mTorr, an upper RF power range of 300 W, and a lower RF power range of 100 W.

[0061] In some embodiments of the present application, the etching gas used in the first etching step and the second etching step further includes an inert gas, and the inert gas includes at least one of Ar, He, and Ne. In some embodiments, the etching gas used in the first etching step and the second etching step further includes the inert gas Ar. In this case, the etching gas used in the first etching step includes Ar and O2, and the etching gas used in the second etching step includes Ar, O2, and SF6.

[0062] Since the Ar radicals and Ar ions generated by the dissociation of inert gases such as Ar under a high-frequency electromagnetic field play a role of physical bombardment and do not participate in chemical reactions, they can not only remove the polymers generated during the etching process, but also improve the verticality of the side walls of the trenches or through-holes formed by etching, thereby avoiding cross-linking of adjacent through-holes due to excessively low verticality, resulting in short circuits of signals transmitted by conductors in the trenches or through-holes, etc.

[0063] In some embodiments of the present application, the gas flow rate of the oxygen-containing gas (such as O2) used in the first etching step is in the range of 5 sccm to 200 sccm, the gas flow rate of the inert gas such as Ar is in the range of 5 sccm to 200 sccm, the process time is in the range of 0.2 s to 8 s, the chamber pressure is in the range of 2 mTorr to 30 mTorr, the upper RF power is in the range of 300 W to 2500 W, and the lower RF power is in the range of 100 W to 1200 W. The gas flow rate of the oxygen-containing gas (such as O2) used in the second etching step is in the range of 5 sccm to 200 sccm, the gas flow rate of the fluorine-containing gas (such as SF6) is in the range of 5 sccm to 20 sccm, the gas flow rate of the inert gas such as Ar is in the range of 5 sccm to 200 sccm, the process time is in the range of 0.2 s to 5 s, the chamber pressure is in the range of 2 mTorr to 30 mTorr, the upper RF power is in the range of 300 W to 2500 W, and the lower RF power is in the range of 100 W to 1200 W.

[0064] In some specific examples, the first etching step uses an oxygen-containing gas (such as O2) with a gas flow rate of 32 sccm, an inert gas (such as Ar) with a gas flow rate of 10 sccm, a process time of 3 s, a chamber pressure of 4 mTorr, an upper RF power of 300 W, and a lower RF power of 100 W. The second etching step uses an oxygen-containing gas (such as O2) with a gas flow rate of 32 sccm, a fluorine-containing gas (such as SF6) with a gas flow rate of 8 sccm, an inert gas (such as Ar) with a gas flow rate of 10 sccm, a process time of 2 s, a chamber pressure of 4 mTorr, an upper RF power of 300 W, and a lower RF power of 100 W.

[0065] In some embodiments, during the alternating cycles of at least two etching steps, the ratio of fluorine to inert elements in the process chamber is greater than 0 and less than or equal to 60, or the fluorine content is zero, thereby achieving a smoother, rounded corner morphology at the bottom of the trench or through-hole. Similarly, because the first etching step does not include a fluorine-containing gas or has an extremely low fluorine content, i.e., the ratio of fluorine to inert elements is less than 0.01, or the fluorine content is zero, during the alternating cycles of at least two etching steps, the ratio of fluorine to inert elements is greater than 0 and less than or equal to 0.01, or the fluorine content is zero when the first etching step is performed. In some embodiments, the ratio of fluorine to inert elements can be greater than 0 and less than or equal to 60, or the fluorine content can be zero, by setting the flow rate ratio of fluorine-containing gas (e.g., SF6) to inert gas (e.g., Ar) to greater than 0 and less than or equal to 10, or by setting the flow rate of fluorine-containing gas (e.g., SF6) to zero.

[0066] During the alternating cycles of at least two etching steps, the time-varying curves of the flow rates of an oxygen-containing gas (e.g., O2), a fluorine-containing gas (e.g., SF6), and an inert gas (e.g., Ar) are shown in FIG13 , where V1 represents the SF6 gas flow rate, V2 represents the Ar gas flow rate, V3 represents the O2 gas flow rate, T1 represents the process time of the second etching step, and T2 represents the process time of the first etching step. During the alternating cycles of at least two etching steps, the time-varying curves of the flow rate ratio of a fluorine-containing gas (e.g., SF6) to an inert gas (e.g., Ar) and the time-varying curves of the flow rate ratio of a fluorine-containing gas (e.g., SF6) to an oxygen-containing gas (e.g., O2) are shown in FIG14 . During the alternating cycles of at least two etching steps, the flow rate of the oxygen-containing gas (e.g., O2) remains constant, the flow rate of the inert gas (e.g., Ar) remains constant, and the flow rate curve of the fluorine-containing gas (e.g., SF6) exhibits a pulse waveform.

[0067] Because after the gas is stopped from being introduced into the process chamber, it takes a certain amount of time for the gas in the process chamber to become zero. Therefore, the flow ratio of the fluorine-containing gas (such as SF6) to the inert gas (such as Ar) and the flow ratio of the fluorine-containing gas (such as SF6) to the oxygen-containing gas (such as O2) are dynamically changing. The slope of the curve of the flow ratio of the fluorine-containing gas (such as SF6) to the inert gas (such as Ar) changing with time is greater than 0 and less than or equal to 10, or the gas flow of the fluorine-containing gas (such as SF6) changes to 0. The slope of the curve of the flow ratio of the fluorine-containing gas (such as SF6) to the oxygen-containing gas (such as O2) changing with time is greater than 0 and less than or equal to 5, or the gas flow of the fluorine-containing gas (such as SF6) changes to 0.

[0068] In some embodiments of the present application, at least two etching steps include only a first etching step and a second etching step, that is, the silicon-containing organic dielectric layer 11 is etched only by cyclically alternating the first etching step and the second etching step. However, the present application is not limited thereto. In other embodiments, the at least two etching steps may further include at least one third etching step, and the at least one third etching step may be located between the first etching step and the second etching step, or between the second etching step and the first etching step. The flow rate of the etching gas used in the third etching step may be less than the flow rate of the etching gas used in the first etching step and the second etching step. The flow rate of the etching gas in the third etching step may be 0, that is, no gas is introduced into the process chamber in the third etching step, or a vacuum process may be performed in the process chamber in the third etching step.

[0069] As another optional implementation of the contents disclosed in the present application, an embodiment of the present application further discloses a semiconductor process equipment, which includes but is not limited to an inductively coupled plasma etching equipment or a capacitively coupled plasma etching equipment.

[0070] In some optional embodiments, as shown in FIG15 , taking the inductively coupled plasma etching equipment as an example, the semiconductor process equipment includes a process chamber 1, an air inlet assembly 2, an exhaust assembly (not shown in the figure), an upper electrode assembly, a lower electrode assembly and a control device (not shown in the figure), etc.

[0071] The gas inlet assembly 2 is used to introduce gas, including process gas, into the process chamber 1 . The control device is used to control the opening or closing of the electronic valve of the gas inlet assembly 2 to control the gas inlet assembly 2 to start or stop introducing gas into the process chamber 1 .

[0072] The exhaust assembly is used to extract gases from the process chamber 1, including byproduct gases generated by the etching reaction. The control device can also be used to control the opening or closing of the electronic valve of the exhaust assembly to control whether the exhaust assembly starts or stops extracting gases from the process chamber 1. Furthermore, the control device can also be used to control the valve position of the electronic valve of the gas inlet assembly 2 and the valve position of the electronic valve of the exhaust assembly to control the chamber pressure of the process chamber 1.

[0073] The upper electrode assembly includes an upper RF power supply 31, a first matcher 32 electrically connected to the upper RF power supply 31, and an RF coil 33 electrically connected to the first matcher 32. The upper RF power supply 31 can be electrically connected to the RF coil 33 in the process chamber 1 via the first matcher 32, and is configured to apply RF power to the RF coil 33, so that the RF coil 33 couples the RF power into the process chamber 1 through the dielectric window 5, ionizing the gas in the process chamber 1 into plasma 6. The control device can also be configured to control the amount of RF power applied to the RF coil 33 by the upper RF power supply 31 via the first matcher 32.

[0074] The lower electrode assembly includes a lower RF power supply 41, a second matching device 42 electrically connected to the lower RF power supply 41, and a carrier 43 electrically connected to the second matching device 42. The carrier 43 includes, among other things, an electrostatic chuck. The lower RF power supply 41 is electrically connected to the carrier 43 via the second matching device 42, and is used to apply bias power to the carrier 43 to accelerate the plasma. The carrier 43 is used to support the device 7 to be fabricated and to heat or cool the device 7 to be fabricated.

[0075] The technical features of the above embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0076] The above embodiments merely represent several implementation methods of this specification. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that a person of ordinary skill in the art may make various modifications and improvements without departing from the spirit of this specification, and these modifications and improvements fall within the scope of protection of this specification. Therefore, the scope of protection of the patent in this specification shall be based on the appended claims.

Claims

1. A method for etching a silicon-containing organic dielectric layer, characterized in that: include: Etching the silicon-containing organic dielectric layer using at least two etching steps that are cyclically alternating; The at least two etching steps include a first etching step and a second etching step, the etching gas used in the first etching step includes at least an oxygen-containing gas, and the etching gas used in the second etching step includes at least an oxygen-containing gas and a fluorine-containing gas.

2. The etching method according to claim 1, characterized in that: In the process of alternating at least two etching steps, the ratio of fluorine to oxygen is greater than 0 and less than or equal to 15, or the content of fluorine is 0; or In the first etching step, the ratio of fluorine element to oxygen element is less than 0.01, or the content of fluorine element is 0.

3. The etching method according to claim 1 or 2, characterized in that: The gas flow rate of the oxygen-containing gas used in the first etching step is in the range of 5 sccm to 200 sccm; The gas flow rate of the oxygen-containing gas used in the second etching step is in the range of 5 sccm to 200 sccm, and the gas flow rate of the fluorine-containing gas used in the second etching step is in the range of 5 sccm to 20 sccm.

4. The etching method according to claim 1, characterized in that: The material of the silicon-containing organic dielectric layer includes BCB, the oxygen-containing gas includes at least one of O2, CO2, CO and SO2, and the fluorine-containing gas includes at least one of SF6, CF4, C4F8, CHF3, NF3, SF6, CH2F2 and C2F6.

5. The etching method according to claim 1, characterized in that: The etching gas used in the first etching step and the second etching step also includes an inert gas; the inert gas includes at least one of Ar, He and Ne.

6. The etching method according to claim 5, characterized in that: The gas flow rate of the inert gas used in the first etching step is in the range of 5 sccm to 200 sccm; the gas flow rate of the inert gas used in the second etching step is in the range of 5 sccm to 200 sccm.

7. The etching method according to claim 5, characterized in that: In the process of alternating at least two etching steps, the ratio of fluorine element to inert element is greater than 0 and less than or equal to 60, or the content of fluorine element is 0; or In the first etching step, the ratio of fluorine element to inert element is less than 0.01, or the content of fluorine element is 0.

8. The etching method according to claim 5, characterized in that: During the alternating cycle of at least two etching steps, the gas flow rate of the oxygen-containing gas remains unchanged, the gas flow rate of the inert gas remains unchanged, and the gas flow rate variation curve of the fluorine-containing gas presents a pulse waveform.

9. The etching method according to claim 1, characterized in that: The process time range of the first etching step is 0.2s to 8s; and / or The process time range of the second etching step is 0.2s to 5s.

10. The etching method according to claim 1, characterized in that: The chamber pressure range used in the first etching step is 2mTorr to 30mTorr; and / or The chamber pressure range used in the second etching step is 2 mTorr to 30 mTorr.

11. The etching method according to claim 1, characterized in that: The at least two etching steps also include at least one third etching step, which is located between the first etching step and the second etching step, and the flow rate of the etching gas used in the third etching step is smaller than the flow rate of the etching gas used in the first etching step and the second etching step.

12. A semiconductor process equipment, comprising a process chamber, an air intake assembly, an upper electrode assembly, a lower electrode assembly and a control device, characterized in that: The control device comprises at least one memory and at least one processor, wherein the memory stores a computer program, and the processor executes the computer program to implement the etching method of the silicon-containing organic dielectric layer according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Dielectric material BCB removing method

    CN101211777A

  • Method for sealing wafer-level micro-cavity based on BCB (benzocyclobutene) glue

    CN102963864A

  • Method for etching silicon through hole

    CN104576506A

  • Etching method of BCB material

    CN105390386A

  • Etching method of silicon-containing organic dielectric layer and semiconductor process equipment

    CN117174582A

Cited By

  • Manufacturing method of metal through hole and semiconductor structure

    CN120767255A