Graphene nanoribbon electrodes for batteries and methods of making same

By employing partially reduced graphene nanoribbons with controlled oxygen-to-carbon ratios and MXene hybrids, the scalability and performance limitations of existing electrode materials are addressed, achieving enhanced conductivity and stability in ion batteries.

WO2026232218A1PCT designated stage Publication Date: 2026-11-12THE GOVERNING COUNCIL OF THE UNIV OF TORONTO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CA2026/050203
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-02-10
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing electrode materials for ion batteries, such as graphite and graphene, face limitations in scalability and performance due to their theoretical capacity and sluggish lithium-ion intercalation/deintercalation kinetics, necessitating improved production methods and alternative materials.

Method used

The use of partially reduced graphene nanoribbons (GOnRs) with controlled oxygen-to-carbon ratios and hybridization with MXene materials, along with specific conductive and non-conductive additives, to enhance conductivity and stability, is proposed.

Benefits of technology

This approach results in improved electron transfer and balanced lithium intake capacity, leading to superior overall conductivity and stability during charge-discharge cycles, addressing scalability and performance issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CA2026050203_12112026_PF_FP_ABST
    Figure CA2026050203_12112026_PF_FP_ABST
Patent Text Reader

Abstract

An electrode for a battery and a method for preparing the same are provided. The electrode is made of partially reduced graphene oxide nanoribbons (GOnRs) having an oxygen to carbon (O / C) ratio of greater than zero to less than 0.49, and optionally MXene. By reducing the GOnRs, e.g by annealing at different annealing temperatures, it is possible to tune the electrode's electrical properties.
Need to check novelty before this filing date? Find Prior Art

Description

GRAPHENE NANORIBBON ELECTRODES FOR BATTERIES AND METHODS OF MAKING SAME CROSS REFERENCE TO RELATED APPLICATION AND CLAIM OF PRIORITY

[0001] The present application claims priority to U.S. provisional patent application no.63,802,410 filed on May 8, 2025, the entire contents of which are hereby incorporated by reference.TECHNICAL FIELD

[0002] The present application relates to electrodes for batteries, and more particularly it relates to the use of modified graphene nanoribbons (GnRs) as electrode materials and hybrid materials of modified GnRs with MXenes as electrode materials.BACKGROUND

[0003] Existing vulnerabilities of the global supply chain for ion batteries, e.g. lithium-ion batteries (LIBs), has prompted extensive research into alternative electrode chemistries and structures, as the total market demand of for LIBs from ~700 GWh in 2022 is projected to increase to 4700 GWh by 2030. Case in point, this vulnerability is evident in the case of graphite, the dominant anode material for certain ion batteries, such as LIBs, where about two-thirds of the world's natural graphite and almost all coated spherical graphite used in electric vehicle (EV) batteries are produced in China. Despite its widespread use, graphite known for its two-dimensional (2D) plate-like structure, is limited by its theoretical maximum capacity of 372 mAh / g and its sluggish lithium-ion intercalation / deintercalation kinetics with an effective diffusion coefficient of 10-12to 10-14cm2 / s.

[0004] To address these, graphite has undergone various chemical and mechanical modifications, notably spheroidization, to provide isotropic electrochemical properties that improve cyclability. Despite these improvements, researchers continue to explore alternative carbon-based materials, including hard carbon, graphene and its derivatives, such as optimized graphene oxide and morphologically engineered graphene. Blending or decorating graphite / graphene with other geometrically diverse carbonaceous nanomaterials, such as carbon nanotubes (CNTs) and carbon nanofibers (CNFs), along with doping it with high-capacity particles and / or metal oxides like silicon (Si), iron oxide (Fe3O4), titanium oxide (TiO2), and tin oxide (SnO2), is another strategy to enhance performance.

[0005] The incorporation of graphitic layers in these hybrid electrodes is primarily aimed at exploiting the potential capacity of these particles by encapsulating them and forming a stable solid-electrolyte interphase (SEI) layer; otherwise, cyclic failure occurs due to continuous expansion and contraction during lithiation and delithiation processes.

[0006] Among these alternatives, graphene nanoribbon (GNR), which exhibit both quasi-one-dimensional (1D) and 2D characteristics, was introduced in 2010 as a promising candidate for ion battery electrodes, such as LIB anodes, due to their unique physicochemical properties. Multiple theoretical and experimental studies, including those utilizing in situ transmission electron microscopy (TEM), have shown that lithiation and delithiation processes predominantly occur at the nanoribbon edges and the surface of GnRs, where a stable SEI layer forms. These results indicate the formation of a combined mechanically robust and flexible network of nanoribbons, capable of withstanding cycling without brittle fracture, thus enhancing their potential application in batteries. However, research on GnRs as a negative electrode material for LIBs has been hindered by the scalability of production methods. Most techniques, such as bottom-up molecular synthesis, longitudinal unzipping of carbon nanotubes, oxygen plasma etching, and epitaxial growth, have been limited to small-scale production. This has reduced the material's commercial viability as a large-scale electrode for ion batteries, such as LIBs, sodium-ion batteries, aluminum-ion batteries, magnesium-ion batteries. According, improved electrode materials comprising GnRs, and methods of making the electrode materials, are desired.SUMMARY

[0007] Electrodes and methods for making the electrode are provided in this disclosure for batteries, e.g. Lithium-Ion Batteries (LIBs), sodium-ion batteries, aluminum-ion batteries, magnesium-ion batteries. The electrode materials are composed of partially reduced graphene nanoribbons (GnRs). In some aspects, the electrode materials are hybrid materials composed of GnRs and MXene. In another aspect, by varying the annealing temperature, the oxygen / carbon (0 / C) ratios of these materials may be tuned to optimize electrode performance. This disclosure provides that by tuning the 0 / C of these materials, it is possible to tune their electrical properties for use as battery electrodes. In some embodiments, hybrid materials according to this disclosure provide superior overall conductivity, leading to improved electron transfer during charge-discharge cycles. In addition, by modulating the thermal reduction temperature, this disclosure demonstrates that a balance between lithium intake capacity and conductivity may be achieved. A further understanding of the functional and advantageous aspects of the invention can be realized by reference to the following detailed description and drawings.

[0008] In an aspect, the disclosure describes an electrode for a battery. The electrode comprises: partially reduced graphene oxide nanoribbons (GOnRs) having an oxygen to carbon (0 / C) ratio of greater than zero to less than 0.49. In an embodiment, the 0 / C ratio ranges from about 0.03 to about 0.21. In another embodiment, the 0 / C ratio ranges fromabout 0.03 to about 0.12. In another embodiment, the 0 / C ratio ranges from about 0.07 to about 0.12. In another embodiment, the 0 / C ratio is about 0.12. In an embodiment, the battery is a lithium-ion battery, sodium-ion, aluminium-ion, or an magnesium-ion based batteries. In an specific embodiment, the battery is a lithium-ion battery.

[0009] In some embodiments, an oxygen content in the GOnRs ranges from about 2.6 wt.% to about 17.6 wt.%. In an example, the oxygen content is about 11.2%.

[0010] In some embodiments, the electrodes comprises MXene. In another embodiment, the MXene is Mn+iXnTx, where M is a transition metal, wherein M is at least one of Ti, Nb, V, Mo, Ta, Zr, Hf, Cr, and Sc; n is 1 , 2, 3, or 4; X is at least one of carbon and nitrogen; and Txis surface functional groups, wherein Txis at least one of -OH, -F, -Cl, -O. In an embodiment, M is at least one of Ti, V, Sc, and Nb. In another embodiment, the MXene is Ti3C2Txand Txis at least one of -OH, -F, -Cl, and -O. In another embodiment, Txis at least one of -OH, -F, and -O.

[0011] In some embodiments, a weight ratio of GOnRs : MXene in the electrode is in a range of about 2:5 to about 3:1. In another embodiment, the weight ratio of GOnRs : MXene in the electrode is about 3:1.

[0012] In some embodiments, the electrode comprises a conductive additive, where the conductive additive is at least one of carbon black, acetylene black, graphite (synthetic or natural), carbon nanotubes (CNTs), graphene I graphene oxide, carbon nanofibers (CNFs), vapor-grown carbon fibers (VGCFs), polyaniline (PANI), polypyrrole (PPy), and poly(3,4-ethylenedioxythiophene: polystyrene sulfonate (PDOT:PSS). In an embodiment, the conductive additive is carbon black.

[0013] In some embodiments, the electrode comprises a non-conductive binder, where the non-conductive binder at least one of of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), Styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyimides (PI), polytetrafluoroethylene (PTFE), poly(acrylonitrile) (PAN), chitosan, polyurethane (PU), and poly(methyl methacrylate) (PMMA). In an embodiment, the non-conductive binder is poly(vinylidene fluoride).

[0014] In some embodiments, the weight ratio of (GOnRs and MXene) : conductive additive : non-conductive binder in the electrode is about 9: 0.5 :0.5.

[0015] Embodiments may include combinations of the above features.

[0016] In another aspect, the disclosure describes a battery comprising an anode, a cathode, and a separator. The anode is the electrode according to this disclosure. In an embodiment, the cathode comprises at least one of Lithium Cobalt Oxide, Nickel ManganeseCobalt, Lithium Iron Phosphate, and Lithium Manganese Oxide. In another embodiment, the battery is a lithium-ion battery, sodium-ion, aluminium-ion, or an magnesium-ion based batteries. In another embodiment, the battery is a lithium-ion battery.

[0017] Embodiments may include combinations of the above features.

[0018] In another aspect, the disclosure describes an electrode material for a battery, the electrode material comprises: partially reduced graphene oxide nanoribbons (GOnRs) having an oxygen to carbon (0 / C) ratio of greater than zero to less than 0.49. In an embodiment, the 0 / C ratio ranges from about 0.03 to about 0.21. In another embodiment, the 0 / C ratio ranges from about 0.03 to about 0.12. In another embodiment, the 0 / C ratio ranges from about 0.07 to about 0.12. In another embodiment, the 0 / C ratio is about 0.12. In another embodiment, the battery is a lithium-ion battery, sodium-ion, aluminium-ion, or an magnesium-ion based batteries. In another embodiment, the battery is a lithium-ion battery.

[0019] In an embodiment, an electrode material for a lithium-ion battery is provided. The electrode material comprises: partially reduced graphene oxide nanoribbons (GOnRs) having an oxygen / carbon (0 / C) ratio of about 0.12 and an oxygen content of about 11.2%; Ti3C2Tx, wherein Txis -OH, -F, and -O; a conductive additive; and a non-conductive binder, wherein a weight ratio of GOnRs : MXene is about 3:1 and the weight ratio of (GOnRs and MXene) : conductive additive : non-conductive binder is about 9: 0.5 :0.5.

[0020] In an embodiment, the conductive additive is carbon black and the binder is poly(vinylidene fluoride).

[0021] In an embodiment, the electrode material comprises MXene. In an embodiment, the MXene is Mn+iXnTx, wherein M is a transition metal, M is at least one of Ti, Nb, V, Mo, Ta, Zr, Hf, Cr, Sc, n is 1, 2, 3, or 4, X is at least one of carbon and nitrogen, and Txis surface functional groups, wherein Txis at least one of -OH, -F, -Cl, and -O.

[0022] In some embodiments, a weight ratio of GOnRs : MXene is in a range of about 2:5 to about 3:1. In another embodiment, the weight ratio of GOnRs : MXene is about 3:1.

[0023] In some embodiments, the electrode material comprises a conductive additive, where the conductive additive is at least one of carbon black, acetylene black, graphite (synthetic or natural), carbon nanotubes (CNTs), graphene I graphene oxide, carbon nanofibers (CNFs), vapor-grown carbon fibers (VGCFs), polyaniline (PANI), polypyrrole (PPy), and poly(3,4-ethylenedioxythiophene: polystyrene sulfonate (PDOT:PSS). In an embodiment, the conductive additive is carbon black.

[0024] In some embodiments, the electrode material comprises a non-conductive binder, where the non-conductive binder at least one of of polyvinylidene fluoride (PVDF),carboxymethyl cellulose (CMC), Styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyimides (PI), polytetrafluoroethylene (PTFE), poly(acrylonitrile) (PAN), chitosan, polyurethane (PU), and poly(methyl methacrylate) (PMMA). In an embodiment, the non-conductive binder is poly(vinylidene fluoride).

[0025] In some embodiments, the weight ratio of (GOnRs and MXene) : conductive additive : non-conductive binder is about 9: 0.5 :0.5.

[0026] Embodiments may include combinations of the above features.

[0027] In another aspect the disclosure describes a method of preparing an electrode for a battery. The method comprises: reducing graphene oxide nanoribbons (GOnRs) until the oxygen to carbon (0 / C) ratio is in a range from greater than zero to less than 0.49 to form partially reduced graphene oxide nanoribbons (rGOnRs); mixing the GOnRs with a conductive additive and binder to form a mixture; and coating the mixture onto a current collector. In another embodiment, the battery is a lithium-ion battery, sodium-ion, aluminium-ion, or an magnesium-ion based batteries. In another embodiment, the battery is a lithium-ion battery.

[0028] In an embodiment, the method comprises annealing the GOnR to reduce the 0 / C ratio at a temperature ranging from 250°C to 1000°C to partially reduce the GOnRs.

[0029] In an embodiment, the method comprises mixing the partially reduced graphene oxide nanoribbons with MXene.

[0030] In an embodiment, the weight ratio of (rGOnRs and MXene) : conductive additive : non-conductive binder is about 9: 0.5 :0.5.

[0031] In an embodiment, the conductive additive is at least one of carbon black, acetylene black, graphite (synthetic or natural), carbon nanotubes (CNTs), graphene I graphene oxide, carbon nanofibers (CNFs), vapor-grown carbon fibers (VGCFs), polyaniline (PANI), polypyrrole (PPy), and poly(3,4-ethylenedioxythiophene: polystyrene sulfonate (PDOT:PSS). In another embodiment, the conductive additive is carbon black.

[0032] In an embodiment, the binder is a non-conductive binder comprising at least one of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), Styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyimides (PI), polytetrafluoroethylene (PTFE), poly(acrylonitrile) (PAN), chitosan, polyurethane (PU), and poly(methyl methacrylate) (PMMA). In another embodiment, the non-conductive binder is poly(vinylidene fluoride).

[0033] In an embodiment, the weight ratio of rGOnRs : MXene is within a range of about 2:5 to about 3:1.

[0034] In an embodiment, the weight ratio of rGOnRs : MXene is about 3: 1.

[0035] In an embodiment, the temperature is 250°C 500°C, 750°C or 1000°C.

[0036] In an embodiment, the temperature is 500°C.

[0037] In an embodiment, the partially reduced GOnRs have an oxygen to carbon (0 / C) ratio ranging from about 0.03 to about 0.21. In another embodiment, the 0 / C ratio ranges from about 0.03 to about 0.12. In another embodiment, the 0 / C ratio ranges from about 0.07 to about 0.12. In another embodiment, the 0 / C ratio is about 0.12.

[0038] In an embodiment, the MXene is Mn+iXnTx, where M is a transition metal, wherein M is at least one of Ti, Nb, V, Mo, Ta, Zr, Hf, Cr, and Sc, n is 1 , 2, 3, or 4, X is at least one of carbon and nitrogen, and Txis surface functional groups, wherein Txis at least one of -OH, -F, -Cl, and -O. In another embodiment, M is at least one of Ti, V, Sc, and Nb. In another embodiment, the MXene is Ti3C2Txand Txis at least one of -OH, -F, -O, and -Cl. In another embodiment, Txis at least one of -OH, -F, and -O.

[0039] Embodiments may include combinations of the above features.BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Embodiments disclosed herein will be more fully understood from the following detailed description thereof taken in connection with the accompanying drawings, which form a part of this application, and in which:

[0041] FIGS. 1Ato 1C show characterization results of an example electrodes according to this disclosure in example coin batteries, in which:

[0042] FIG. 1A shows a graphical illustration of X-ray Photoelectron Spectroscopy (XPS) survey spectra of graphene oxide nanoribbons (GOnRs) and reduced graphene oxide nanoribbons (rGOnRs) at various temperatures,

[0043] FIG. 1B shows a graphical illustration of powder X-ray Diffraction (XRD) patterns of the example electrode materials,

[0044] FIG. 1C shows a graphical illustration of the Raman spectra of GNR250, GNR500, GNR750, and GNR1000 example electrode materials.

[0045] FIG. 2 shows a graphical illustration of high-resolution C 1s XPS spectra of GOnR and the reduced powders at the specified temperatures.

[0046] FIG. 3 shows EDX results showing the oxygen content in example GOnR and reduced samples (the scale bars represent 25 pm).

[0047] FIGS. 4Ato 4C show graphical illustrations of galvanostatic charge-discharge (GOD) profiles, in which:

[0048] FIG. 4A shows initial (GOD) profiles of example electrode G250, G500, G750, and G1000 at 0.05 A / g over a potential range of 0.005-2.9 vs. Li / Li+,

[0049] FIG. 4B shows the 5th cycle GOD profiles at 0.05 A / g, and

[0050] FIG. 4C shows GOD profiles of example electrodes G250, G500, G750, and G1000 at 0.5 A / g.

[0051] FIG. 5 shows a graphical illustration of the rate-dependent capacities of example electrodes G250, G500, G750, and G1000 across a broad current density range of 0.05-5 A / g.

[0052] FIGS 6A and 6B show cyclic stability at 0.1 A / g over a potential range of 0.005-2.9 vs. Li / Li+, for: FIG. 6A example electrode G500, FIG. 6B example electrode G1000.

[0053] FIGS 7A to 7C show graphical illustration of the GOD profiles of: FIG. 7A example electrode G500 at 0.05 A / g, FIG. 7B example electrode G 1000 at 0.05 A / g, and FIG.7C shows a comparison of example electrodes G500 and G 1000 with each electrode composed of precoated graphite at 0.05 A / g (5th cycle).

[0054] FIG. 8A shows a graphical illustration of rate-dependent capacities of the half-cell battery cell made of the hybrid electrode (GM) across a wide current density range of 0.05-5 A / g, and

[0055] FIG. 8B shows a graphical illustration of the GOD profiles of hybrid electrode GM at 0.5 A / g.

[0056] FIG. 9 shows a schematic representation of a coil cell battery featuring the chemically tailored hybrid GNR / MXene electrode, accompanied by its SEM image and TEM images of the components.

[0057] FIG. 10 shows a schematic diagram illustrating a method for making an electrode for a battery, according to some embodiments.DETAILED DESCRIPTION

[0058] A detailed description is provided below to facilitate a thorough understanding of the disclosed embodiments and their interrelationships. It is understood that the description is not limited to any particular example set forth herein. Various embodiments and aspects of the disclosure are described with reference to the detailed discussion below. The following description and accompanying drawings are intended to be illustrative and are not to be construed as limiting the scope of the disclosure. Numerous specific details are provided topromote a complete understanding of the embodiments; however, in certain instances, well-known elements or techniques have not been described in detail so as not to obscure the disclosure.

[0059] The accompanying figures / drawings, which are not necessarily to scale and are incorporated into and form part of the present specification, illustrate various embodiments and aspects of the disclosure. In conjunction with the description provided herein, the drawings serve to explain the principles of the process preparing partially rGOnRs and GOnRs-based hybrid materials. The drawings are provided solely for illustrative purposes and are not intended to define or limit the scope of the disclosure.

[0060] According to the present disclosure, the inventors have discovered that annealing GOnRs to obtain a partial reduction plays a critical factor in modulating oxygen functional groups on GOnRs. In addition, they have discovered that hybridizing rGOnRs with MXene offers a potential solution. Among highly conductive nanoparticles, Ti3C2Tx— one of the most studied members of the MXene family — has shown great potential for addressing the shortcomings of reduced graphene oxide (rGO), despite its known relatively low capacity as an anode (~100 mAh / g at a 1C rate). The metallic conductivity of TisC2Tx(105— 106S / m) and its low Li+diffusion barrier (0.07 eV) are considered key factors that enhance the Li+intake capacity of the hybrid electrode material.

[0061] The present disclosure discloses modified GOnRs, e.g. using annealing where the ratio of carbon (C) to oxygen (O) is varied to tune the electrical properties of the GOnRs for use as battery electrodes.

[0062] DEFINITIONS

[0063] Although terms such as “maximize”, “minimize” and “optimize” may be used in the present disclosure, it should be understood that such terms may be used to refer to improvements, tuning and refinements which may not be strictly limited to maximal, minimal or optimal.

[0064] The term “connected” or "coupled to" may include both direct coupling (in which two elements that are coupled to each other and contact each other) and indirect coupling (in which at least one additional element is located between the two elements).

[0065] The term “substantially” as used herein may be applied to modify any quantitative representation which could permissibly vary without resulting in a change in the basic function to which it is related.

[0066] Terms such as "up to", "at least", "greater than", "less than", "more than", "or more", and the like, include the number recited and such terms refer to ranges that can besubsequently broken down into sub-ranges. In the same manner, all ratios recited herein also include all sub-ratios falling within the broader ratio.

[0067] The singular forms "a," "an," and "the" include the plural reference unless the context clearly dictates otherwise. The term "and / or" means any one of the items, any combination of the items, or all of the items with which this term is associated.

[0068] The term "about" can refer to a variation of± 5%, ± 10%, ± 20%, or± 25% of the value specified. For example, "about 50" percent can in some embodiments carry a variation from 45 to 55 percent. For integer ranges, the term "about" can include one or two integers greater than and / or less than a recited integer at each end of the range. Unless indicated otherwise herein, the term "about" is intended to include values and ranges proximate to the recited range that are equivalent in terms of the functionality of the composition, or the embodiment.

[0069] The terms, “comprises” and “comprising” are to be construed as being inclusive and open ended, and not exclusive. Specifically, when used in the specification and claims, the terms, “comprises” and “comprising” and variations thereof mean the specified features, steps or components are included. These terms are not to be interpreted to exclude the presence of other features, steps or components.

[0070] The term “exemplary” means “serving as an example, instance, or illustration,” and should not be construed as preferred or advantageous over other configurations disclosed herein.

[0071] It is to be understood that unless otherwise specified, any specified range or group is as a shorthand way of referring to each and every member of a range or group individually, as well as each and every possible sub-range or sub-group encompassed therein and similarly with respect to any sub-ranges or sub-groups therein. Unless otherwise specified, the present disclosure relates to and explicitly incorporates each and every specific member and combination of sub-ranges or sub-groups.

[0072] As used herein, the term "on the order of', when used in conjunction with a quantity or parameter, refers to a range spanning approximately one tenth to ten times the stated quantity or parameter.

[0073] As used herein, the coordinating conjunction “and / or” is meant to be a selection between a logical disjunction and a logical conjunction of the adjacent words, phrases, or clauses. Specifically, the phrase “X and / or Y” is meant to be interpreted as “one or both of X and Y” wherein X and Y are any word, phrase, or clause.

[0074] As used herein, the word “conductive” typically refers to electronic conductivity and ionic conductivity. In the present application the word “conductive” corresponds to onlyelectronic conductivity. However, instead of “ionic conductivity”, the better terms describing Li-ion transport in the developed electrodes are “ion transport” or “intercalation kinetics” rather than bulk ionic conductivity.

[0075] As used herein, the word “hybrid” refers to the developed electrode materials made by combining two different nanomaterials. The term "composite" is not used here to avoid confusion with its common definition, which refers to materials consisting of a major phase (matrix) and a minor phase, such as a filler or reinforcement. In this context, there is no matrix and additive in their conventional meanings.

[0076] As used herein the word “MXene” refers to a class of two-dimensional transition metal carbides, nitrides, or carbonitrides with the general formula Mn+iXnTx, where M is a transition metal (e.g., but not limited to, Ti, Nb, V, Mo, Ta, Zr, Hf, Cr, Sc or any combination thereof), X is carbon and / or nitrogen and Txis surface functional groups (e.g., -OH, -F, -O, -Cl or any combination thereof) and n is 1 , 2, 3, or 4. In this document, non-limiting example of a MXene being studied is specifically Ti3C2Tx.

[0077] Without limitation, the embodiments described herein are directed to modified GnRs as battery electrodes and hybrids formed with mixed GnRs and MXenes. As required, embodiments of the present invention are disclosed herein. However, the disclosed embodiments are merely exemplary, and it should be understood that the invention may be embodied in many various and alternative forms.

[0078] REDUCED GRAPHENE OXIDE NANORIBBONS (rGOnRs) AS ELECTRODE MATERIAL

[0079] The electrochemical performance of GnRs is strongly influenced by their atomic and crystalline structure, as well as their chemical composition. Structurally, aside from the influence of (002) interlayer spacing, studies have demonstrated that lithium binding energy is stronger in zigzag GnRs compared to armchair GnRs, with lithium adatoms preferring sites near the nanoribbon edges. This edge effect in GnRs offers a solution to a common issue with graphene, where its theoretical capacity often falls short in practice. While graphene can theoretically adsorb Li+on both sides, resulting in a Li2C6stoichiometry with a specific capacity of 744 mAhg-1, studies have shown that weak Li binding energy and strong Coulombic repulsion between Li+prevent full Li coverage. However, the unique geometry of GnR with its abundant edges may provide additional active sites for Li+intake. Regarding chemical attributes, studies to date indicate that GnRs produced via the longitudinal unzipping of multiwalled carbon nanotubes (MWCNTs) have shown enhanced performance due to the presence of oxygen-containing functional groups.

[0080] However, these oxidized GnRs, despite exhibiting an initial discharge capacity of ~1400 mAh / g, suffered from a low Coulombic efficiency (CE) of around 53% and poor cycling stability, with ~3% capacity losses per cycle. Similar trends have been observed in graphenebased electrodes, where oxygen functional groups (i.e., C=O and -COOH) can enhance capacity, but excessive oxygen content results in high irreversible capacity loss. Thus, this disclosure describes a balanced oxygen content in graphene materials which optimizes both capacity and stability.

[0081] Specifically, changing the oxygen to carbon ratio was found to change coulombic efficiency and discharge capacities. In some examples, described below, 0 / C ratios having higher initial discharge capacities may have lower initial coulombic efficiency suggesting a trade-off between initial capacity and cycle stability. Tuning the 0 / C ratios for certain use cases may be preferred.

[0082] In an aspect, an electrode for a battery is provided comprising partially reduced graphene oxide nanoribbons (rGOnRs). In some embodiments, the rGOnRs may have an oxygen to carbon (0 / C) ratio of greater than zero and less than 0.49 In some embodiments, the rGOnRs may have an oxygen to carbon (0 / C) ratio ranging from about 0.03 to about 0.21. According to another embodiment, the 0 / C ratio may range from about 0.03 to about 0.12 or the 0 / C ratio may range from about 0.07 to about 0.12. In an example, the 0 / C ratio may be about 0.12. The electrode material may have an oxygen content ranging from greater than zero to less than 32.5%, or in an embodiment, about 2.6 wt.% to about 17.6 wt.%. Alternatively, in an example, the oxygen content may be about 11.2%. In some embodiments, the battery is a lithium-ion battery, sodium-ion, aluminium-ion, or a magnesium-ion based batteries. In another embodiment, the battery is a lithium-ion battery.

[0083] As noted above, varying the 0 / C ratio of the rGOnRs may create a trade-off between capacity and cycle stability. According to this disclosure, it was determined that MXene may improve overall performance of batteries comprising electrodes having rGOnRs by minimizing performance trade-offs as the 0 / C ratio is varies. Notably, hybridization of reduced GnRs with MXene resulted in enhancement to high-rate capacity. These findings in the examples below underscore the effectiveness of combining thermally tuned GnRs with MXene to address performance trade-offs.

[0084] According to an embodiment, an electrode according to disclosure comprising rGOnRs may also comprise MXene forming hybrid electrode material. The MXene may be Mn+iXnTx, where M is a transition metal, M being Ti, Nb, V, Mo, Ta, Zr, Hf, Cr, Sc or any combination thereof, n is 1, 2, 3, or 4, X is carbon and / or nitrogen and Txis surface functional groups, Txbeing -OH, -F, -Cl, -O or any combination thereof. According to an embodiment, the transitionmetal, M, is selected from the group consisting of Ti, V, Sc, Nb and any combination thereof. In some embodiments, the MXene is Ti3C2Txand Txis -OH, -F, -Cl, -O or any combination thereof. In some embodiments, the MXene is Ti3C2Txand Txis -OH, -F, and -O.

[0085] According to an embodiment, when the electrode comprises MXene, the hybrid material may have a weight ratio of rGOnRs : MXene ranging from about 2:5 to about 3:1. This optimized ratio may improve electrochemical performance of graphene / MXene nanohybrids with various nanofiller loadings by reducing the trade-off between capacity and coulombic efficiency when tuning the 0 / C ratio of the electrode material.

[0086] According to an embodiment, the electrode material may comprise a conductive additive. The additive may comprise at least one of carbon black, acetylene black, graphite (synthetic or natural), carbon nanotubes (CNTs), graphene I graphene oxide, carbon nanofibers (CNFs), vapor-grown carbon fibers (VGCFs), polyaniline (PANI), polypyrrole (PPy), and poly(3,4-ethylenedioxythiophene: polystyrene sulfonate (PDOTPSS). According to an embodiment, the conductive additive may be carbon black.

[0087] According some embodiments, the electrode material may comprise a non-conductive binder. The binder may comprise at least one of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), Styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyimides (PI), polytetrafluoroethylene (PTFE), poly(acrylonitrile) (PAN), chitosan, polyurethane (PU), and poly(methyl methacrylate) (PMMA). According to an embodiment, the non-conductive binder may be poly(vinylidene fluoride).

[0088] According to an embodiment, the electrode material may have a weight ratio of (GOnRs and MXene) : conductive additive : non-conductive binder of about 9: 0.5 :0.5. In situations where the material is free of MXene, the weight ratio may be GOnRs : conductive additive : non-conductive binder and may be about 9: 0.5 :0.5.

[0089] A method of preparing an electrode material is provided. The method has the step of annealing GOnRs at a selected temperature. The selected temperature may range from 250°C to 1000°C to partially reduce the GOnRs. According to an embodiment, the temperature may be 250°C 500°C, 750°C or 1000°C. Alternatively, the selected temperature may be 500°C.

[0090] According to an embodiment, the step of annealing the GOnRs may result in partially reduced GOnRs having an oxygen / carbon (O / C) ratio ranging from about 0.03 to about 0.21. Alternatively, the O / C ratio may range from about 0.03 to about 0.12 or the O / C ratio may range from about 0.07 to about 0.12. According to another embodiment, the annealing step may result in a partially reduced GOnRs having an O / C ratio of about 0.12.

[0091] FIG. 9 shows an example lithium-ion battery 900 according to this disclosure. While a lithium-ion battery is illustrated in the non-limiting example shown in FIG. 9, electrodes according to this disclosure may be used in other batteries, for example sodium-ion, aluminium-ion, or magnesium-ion based batteries, because the chemical reactions in these alternative batteries are similar. Lithium-ion battery 900 comprises an electrode 901 according to this disclosure. In the illustrated example, electrode 901 is an anode. Lithium-ion battery 900 also comprises cathode 902 and separator / electrolyte 903 for a lithium-ion battery, e.g. polyethylene, polypropylene, or ceramics. The electrode 901, i.e. the anode, cathode 902, and separator / electrolyte 903 may be positioned within a housing which is shown as cap 904 and can 905. In this example, electrode 901 comprises reduced GOnRs 906 and MXene 907 according to this disclosure.

[0092] FIG. 10 shows a schematic diagram illustrating a method 1000 for making an electrode for a battery, according to some embodiments. In some embodiments, the battery is a lithium-ion battery, sodium-ion, aluminium-ion, or an magnesium-ion based batteries. In another embodiment, the battery is a lithium-ion battery.

[0093] At 1002, the method 1000 comprises reducing graphene oxide nanoribbons (GOnRs) until the oxygen to carbon (0 / C) ratio is in a range from greater than zero to less than 0.49 to form partially reduced graphene oxide nanoribbons (rGOnRs).

[0094] At 1004, method 1000 comprises mixing the GOnRs with a conductive additive and binder to form a mixture.

[0095] In an embodiment, the conductive additive is at least one of carbon black, acetylene black, graphite (synthetic or natural), carbon nanotubes (CNTs), graphene I graphene oxide, carbon nanofibers (CNFs), vapor-grown carbon fibers (VGCFs), polyaniline (PANI), polypyrrole (PPy), and poly(3,4-ethylenedioxythiophene: polystyrene sulfonate (PDOTPSS). In an example, the conductive additive is carbon black.

[0096] In an embodiment, the binder is a non-conductive binder comprising at least one of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), Styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyimides (PI), polytetrafluoroethylene (PTFE), poly(acrylonitrile) (PAN), chitosan, polyurethane (PU), and poly(methyl methacrylate) (PMMA). In an example, the binder is poly(vinylidene fluoride).

[0097] At 1006, method 1000 comprises coating the mixture onto a current collector.

[0098] According to an embodiment, method 1000 may also comprise the step of mixing the partially reduced GOnRs with MXene. The MXene is Mn+iXnTx, where M is a transition metal, M is at least one of Ti, Nb, V, Mo, Ta, Zr, Hf, Cr, and Sc, n is 1, 2, 3, or 4, X is at least one ofcarbon and nitrogen and Txis surface functional groups, where Txat least one of -OH, -F, -Cl, and -O. According to an embodiment, the method may use Ti3C2Txas MXene and Txis at least one of -OH, -F, -O, and -Cl. According to another embodiment, method 1000 may use Ti3C2Txas MXene and Txis at least one of -OH, -F, and -O.

[0099] According to an embodiment, method 1000 may provide rGOnRs, the conductive additive, and the binder in a weight ratio of about 9: 0.5 :0.5. According to another embodiment, method 1000 may provide the rGOnRs and MXene mixture, a conductive additive and a non-conductive binder in a weight ratio of about 9: 0.5 :0.5. In an example, the weight ratio of rGOnRs : MXene is about 3:1.

[0100] The present disclosure will now be illustrated using the following illustrative, non-liming examples. In these non-limiting examples, MXene is Ti3C2Tx.

[0101] Example 1 - Nanoparticle Synthesis

[0102] The following materials were used in the work: Ti3AIC2MAX phase powder (> 400 mesh), lithium fluoride (LiF; > 99%), hydrochloric acid (HCI; 37%), hydrogen peroxide (H2O2; 30%), phosphoric acid (H3PO4), sulfuric acid (H2SO4), and N-Methylpyrrolidone (NMP), all purchased from Sigma-Aldrich. Polyvinylidene fluoride (PVDF) binder was sourced as KUREHA KF POLYMER. For synthesizing GnRs, multi-walled carbon nanotubes (MWCNTs) with average diameter, length, and surface area of 9.5 nm, 1.5 pm, and 275 m2 / g was obtained from Nanocyl SA Belgium, and potassium permanganate (KMnO4) was purchased from EMD Chemicals. A 25 pm trilayer polypropylene / polyethylene / polypropylene microporous membrane (Celgard 2535) was used for battery assembly. The electrolyte, 1 M lithium hexafluorophosphate (LiPF6) in a 1:1:1 (v / v / v) mixture of ethylene carbonate (EC), dimethyl carbonate (DMC), and diethyl carbonate (DEC), was obtained from Sigma-Aldrich for half-cell operations.

[0103] GOnRs were synthesized through a chemical unzipping process. First, 1 g of MWCNTs was dispersed in a mixture of 180 mL sulfuric acid and 20 mL phosphoric acid and stirred for 1 hour at 0°C. Next, 5 g of potassium permanganate was gradually added over 30 minutes, followed by heating the mixture to 65°C over 1 hour and stirring for an additional 3 hours. After cooling, the mixture was poured into a 200 mL ice bath containing 10 mL hydrogen peroxide, and the resulting graphene oxide nanoribbons (GOnRs) were allowed to precipitate for 24 hours. The resulting slurry was dialyzed until the pH reached 6-7, then freeze-dried to obtain GONR powder. Athermal reduction process was conducted under an argon atmosphere in a tube furnace using an alumina ceramic crucible at temperatures of 250, 500, 750, and 1000°C to partially remove functional groups. The temperature profile included a heating rate of 3°C / min up to 500°C, and an additional step with a rate of 10°C / min for temperatures beyond 500°C, followed by cooling to room temperature.

[0104] MXene nanoflakes were synthesized by selectively etching the aluminum layer from Ti3AIC2using minimally intensive layer delamination (MILD) method. In atypical synthesis, 3.2 g of LiF was dissolved in 40 mL of 9 M HCI and stirred for 30 minutes at room temperature in a Teflon container. Then, 2 g of Ti3AIC2was gradually added over 15 minutes to control hydrogen bubbling due to the exothermic reaction. The mixture was stirred in a water bath at 37°C for 24 hours. The product was washed with distilled water and centrifuged at 8000 rpm for 10 minutes until the pH reached 5-6, resulting in a dark green supernatant, indicating the initiation of MXene flake delamination. To further delaminate the MXene, the mixture was sonicated for 1 hour under argon flow and then centrifuged at 3500 rpm for 45 minutes. The exfoliated MXene nanoflakes were collected and freeze-dried.

[0105] Example 2 - Battery Fabrication

[0106] Electrodes were prepared via slurry casting. A slurry was made by mixing the active materials (rGOnR powders reduced at various temperatures and MXene), carbon black (Super P®) as a conductive additive, and poly(vinylidene fluoride) in N-methyl-2-pyrrolidone as a non-conductive binder with a weight ratio of 9:0.5:0.5. The slurry was coated onto copper foil as the current collector and dried in a vacuum oven at 60°C for 24 hours. GNR-based electrodes were labeled based on their reduction temperature: “G250”, “G500”, “G750”, and “G1000”. In other words, “G250” has a reduction temperature of 250°C; “G500” has a reduction temperature of 500°C; “G500” has a reduction temperature of 500°C; “G750” has a reduction temperature of 750°C; and “G1000” has a reduction temperature of 1000°C. The GNR500 / MXene nanohybrid electrode with a 3:1 weight ratio was labeled "GM." This optimized ratio was selected based on findings regarding the electrochemical performance of graphene / MXene nanohybrids with various nanofiller loadings. See S. Xu, Y. DallAgnese, J. Li, Y. Gogotsi, W. Han, Chem. Eur. J. 2018, 24, 18556; and S. Xu, G. Wei, J. Li, W. Han, Y. Gogotsi, J. Mater. Chem. A 2017, 5, 17442, the entire contents of which are hereby incorporated by reference. Half-cell batteries were assembled using Li metal as the counter electrode, a trilayer microporous separator, and the 1 M LiPF6in EC / DMC / DEC electrolyte. All cells were assembled in an argon-filled glovebox with O2and H2O levels below 0.2 ppm.

[0107] The morphology of the synthesized nanoparticles and electrodes was characterized using scanning electron microscopy (SEM, Jeol JSM-IT100) and transmission electron microscopy (TEM, Talos™ L120C). Structural changes in GnRs were analyzed using X-ray diffraction (XRD, Philips APD3520) with Cu-Ka radiation (A = 1.54184 A) and Raman spectroscopy (Anton Paar Cora 5001). Surface chemistry was studied using X-rayphotoelectron spectroscopy (XPS, Thermo Fisher Scientific KAIpha). Elemental mapping was performed with a JEOL-6610 LV microscope equipped with an energy dispersive X-ray (EDX) spectroscopy probe (Oxford Instruments Xplore). Electrochemical tests were conducted at room temperature. Cycling and galvanostatic charge / discharge tests were performed between 0.005-2.9 vs. Li / Li+at current densities ranging from 0.05-5 A g-1using an MTI Battery Analyzer (BST8-MA).

[0108] The synthesis of graphene nanoribbons via chemical unzipping transformed the morphology from one-dimensional MWCNTs to two-dimensional nanoribbons. Following synthesis, the GOnRs were reduced in a preheated tubular furnace under an argon atmosphere to form reduced graphene oxide nanoribbons (rGOnRs). These rGOnRs retained some oxygen functional groups, which were analyzed using XPS and EDX to assess changes in oxygen functionalities throughout the reduction process.

[0109] XPS data reveals a gradual reduction in the oxygen-to-carbon (0 / C) atomic ratio from approximately 0.49 (in GONR) to 0.03 (in G1000) with increased reduction temperatures (FIG.1A). Powder X-ray diffraction analysis (FIG. 1B) demonstrates changes in the GnR stacking structure as a function of temperature. G250 displays a broad (002) diffraction peak at 29 = 24.6°, corresponding to an interlayer spacing (c / -spacing) of approximately 3.62 A (according to Bragg’s equation as d = A / 2sin9 where A is the wavelength of X-ray). See M. Salari, S. Habibpour, M. Hamidinejad, H. E. Naguib, A. Yu, C. B. Park, Mater. Horizons 2023, the entire contents of which are hereby incorporate by reference. As the reduction temperature increases, this peak gradually shifted to 29 = 25.9° with a c / -spacing of around 3.43 A for G1000. This trend demonstrates that removing oxygen functional groups effectively fine-tunes the crystalline properties of the graphitic structure in GnRs.

[0110] As shown in FIG. 1C, Raman spectroscopy was employed to characterize the carbonaceous material's chemical structure, revealing two primary peaks: the D mode at 1335 ± 5 cm-1, associated with defects, and the G mode at 1548 ± 5 cm-1, linked to the first-order scattering of the E2gmode from C-C bond stretching in graphitic carbon. Defects and disruptions in the sp2structure of MWCNTs during oxidation and reduction are effectively captured by this technique. The ID / IG intensity ratio serves as a measure of the carbon material’s structural integrity. Upon oxidizing and unzipping MWCNTs to form GOnRs, an ID / IG of 1.06 indicates edge structure formation in GOnRs, which increases D mode activation. Consistent with reports on reduced graphene oxide and GOnRs, further thermal reduction of GOnR elevates ID / IG ratio. Since smaller sp2aromatic domains contribute to the D mode, while G mode represents the general domain size, the rise in ID / IG after thermal reduction reflects the decrease in overall in-plane sp2domain size due to oxidation, as individual restored sp2domains become notably smaller. See C. Uthaisar, V. Barone, B. D. Fahlman, Carbon N. Y.2013, 61, 558; and S. Stankovich, D. A. Dikin, R. D. Piner, K. A. Kohlhaas, A. Kleinhammes, Y. Jia, Y. Wu, S. the entire contents of which are hereby incorporated by reference.

[0111] This explains the gradual increase in ID / IG from approximately 1.09 to 1.17 as the reduction temperature rises from 250 to 1000 °C.

[0112] High-resolution C 1s XPS spectra of GOnR in FIG. 2 is deconvoluted into four components: sp2-hybridized carbon (C=C) and sp3-hybridized carbon (C-C) at ~284.9 eV, hydroxyl / epoxy (C-O) groups at ~285.9 eV, carbonyl (C=O) groups at 287.9 eV, and carboxyl (COOH as O-C=O) groups at 291.5 eV. The intensities of all oxygen functionalities decrease with higher temperatures, while the C=C bond content increases. Notably, the dominant C-0 peak in GOnR diminishes significantly beyond 500 °C, indicating substantial removal of hydroxyl and epoxy groups. EDX analysis (FIG. 3) further confirms the reduction in oxygen functional groups, showing a pronounced decrease in oxygen content from 32.5% to 11.2%, and 2.6% in GONR, G500, and G1000, respectively. These findings suggest that reduction temperature is a critical factor for modulating oxygen functional groups on GnRs.

[0113] The electrochemical performance of the GnRs with different oxygen contents was evaluated in coin cell batteries. Galvanostatic charge-discharge (GOD) profiles at 0.05 A / g (FIG. 4A) showed that GnRs reduced at lower temperatures exhibited higher initial discharge capacities but lower initial Coulombic efficiencies (CE), suggesting a trade-off between initial capacity and cycle stability. For instance, G250 with an initial columbic efficiency of 44.2% shows larger initial capacity fade, attributed to solid electrolyte interphase (SEI) layer formation and the Li ions trapped in oxygen groups like carboxyl and epoxy, which normally causes irreversible capacity loss above 1 V versus Li / Li+. Compared to the initial discharge cycle in FIG. 4A, the GCD results for the 5thcycle at 0.05 A / g (FIG. 4B) show that G500 has a higher capacity (=576 mAh g-1) than the other samples, emphasizing the importance of oxygen group density and related structural changes (see FIGS. 1Ato 1C) in balancing Li+intake capacity with irreversible capacity loss. Although G500 performs best at a slower rate, G1000 achieves =335 mAh g-1at a higher rate of 0.5 A / g (FIG. 4C). This result highlights the trade-off between Li+intake capacity and conductivity as influenced by the functional groups, with electrical conductivity enabling higher discharge capacities at elevated charge-discharge rates.

[0114] Mechanistically, all GnR samples behave similarly to graphene materials, exhibiting a surface-controlled charge storage mechanism, as evidenced by the sloping charge-discharge profiles. These slopes suggest Li+adsorption on the numerous defective and edge sites of GnRs, while the relatively flat plateau below =0.3 V versus Li / Li+likely corresponds to diffusion-controlled Li+intercalation into the partially stacked GnR layers. FIG. 5 shows the cyclic discharge capacities at various rates, with G500 reaching the highest reversible capacity(=457 mAh g-1) at 0.05 A / g after experiencing cycles across a range of rates from 0.05 to 5 A / g. As expected, the capacity difference among electrodes becomes more pronounced at high rates, with G500 and G1000 achieving =120 and =197 mAh g-1, respectively, at 5 A / g. Although G1000 shows the most stable performance, G500's superior performance at low current rates makes it an energy-efficient candidate for synthesis, as the complete removal of oxygen-containing functional groups at the high temperature of 1000°C is an energy-intensive process.

[0115] Comparing the cyclic stability of G500 (FIGS. 6A and 7A) and G1000 (FIGS. 6B and 7B), G500 exhibits slightly higher capacity fade (CF) than G1000 (approximately CFG5OO=O.O8% vs CFGIOOO=O.O4% per cycle), aligning with the observed effects of oxygen functional groups on irreversible Li+affinity. Compared to commercial graphene nanoplatelets, which deliver 338 mAh g-1after 10 cycles at 0.05 A / g, G500 and G1000 exhibit significantly higher specific capacities of 514 and 478 mAh g-1, respectively, after 10 cycles at the same current density (FIG.7C). These results indicate the potential of GnR for scalable adoption as a high-capacity carbonaceous material for next-generation battery technologies, given the ongoing progress in mass-scale production of GNR, see for example F. Liu, Y. Hu, Z. Qu, X. Ma, Z. Li, R. Zhu, Y. Yan, B. Wen, Q. Ma, M. Liu, Proc. Natl. Acad. Sci. 2023, 120, e2303262120, the entire contents of which are hereby incorporated by reference.

[0116] Given the inherent trade-off in GnR structure for optimized Li+intake and high-rate performance, hybridization with MXene was postulated to address this balance. Comparing FIGS. 8A and 8B, GM demonstrates significantly improved performance, comparable to G1000, with approximately 47% and 36% improvement observed at high rates of 1 and 5 A g-1, respectively, over G500. With an average specific capacity of ~320 mAh g-1at 0.5 A g-1, the hybrid electrode also exhibits desirable cyclic stability (FIG. 8B) with CFGM ~0.12% per cycle.

[0117] These findings are explained considering the layered structure of similar systems, where graphene layers separate MXene sheets, preventing restacking and thereby enhancing ion transport and electroactive site accessibility for better Li-ion storage performance. A similar effect is expected in GnR / MXene nanohybrids, as the binding energy between MXene and graphene layers is exothermic, suggesting favorable interactions and structural stability. This interaction is sufficiently weak to maintain the distinctive electronic properties of each material, allowing the graphene layers to prevent MXene restacking without significantly altering their electroactive properties. Additionally, MXene naturally possesses surface functional groups (e.g., -OH, — O, -F) that enhance electrolyte infiltration and improve electrochemical interactions, contributing to tunning Li diffusion barrier and facilitating charge transfer.13543451See S. Xu, Y. Dall’Agnese, J. Li, Y. Gogotsi, W. Han, Chem. Eur. J. 2018, 24, 18556; Y.-T. Du,X. Kan, F. Yang, L.-Y. Gan, U. Schwingenschldgl, ACSAppl. Mater. Interfaces 2018, 10, 32867; and D. Song, Y. Du, W. Ma, X. Zhang, Int. J. Energy Res. 2021, 45, 3421, the entire contents of which are hereby incorporate by reference. The interfacial binding energy between MXene and G500 enables stronger Li-ion binding at the interface than on pure MXene or graphene alone, with the collective effect of both materials increasing Li-ion storage capacity. Considering GM’s cyclic stability (FIG. 8B), the hybrid MXene-GNR500 heterostructure is expected to achieve optimized ion adsorption, e.g. Li adsorption strength while maintaining high Li mobility. Further, the conductive heterostructures at MXene / rGOnR interfaces offer additional ion storage sites, e.g. lithium-ion storage sites, and facilitate efficient inserting / removal of ions into / from the electrode via e.g. lithiation and delithiation, sodiation and desodiation, etc. leading to superior electrochemical performance. A schematic of the developed GNR / MXene 906, 907 heterostructure, along with a SEM image of the components, is presented in Fig. 9 as fragmentary views of electrode 901 of battery 900.

[0118] While both materials' functional groups aid Li intake, MXene, due to its metallic conductivity caused by its titanium core, is less affected by these functional groups than G500, enabling faster charge transfer kinetics and sustaining high-rate capacity. Therefore, combined with MXene’s inherent conductivity, this hybrid structure offers superior overall conductivity, which is essential for efficient electron transfer during charge-discharge cycles.

[0119] This disclosure highlights the potential of thermally reduced GnRs, e.g. thermally reduce GnRs, as high-performance anode materials for lithium-ion batteries, with a focus on optimizing both capacity and rate capability through controlled oxygen content. By modulating the thermal reduction temperature, this disclosure demonstrates that a balance between lithium intake capacity and conductivity could be achieved. GnRs reduced at 500 °C exhibited high capacity at lower current densities, while GnRs reduced at 1000 °C delivered improved high-rate performance. Importantly, the hybridization of mildly reduced GnRs with MXene resulted in significant enhancements in high-rate capacity, with a 36% increase at 5 A / g, achieving an average capacity of approximately 320 mAh / g at 0.5 A / g. These findings underscore the effectiveness of combining thermally tuned GnRs with MXene to address performance trade-offs, suggesting that these hybrid materials are well-suited for nextgeneration battery applications, e.g. lithium-ion battery applications, requiring both high capacity and cycling stability.

[0120] IMPLEMENTATION DETAILS

[0121] The description above provides many example embodiments. Although each embodiment represents a single combination of inventive elements, other examples may include all possible combinations of the disclosed elements. Thus if one embodimentcomprises elements A, B, and C, and a second embodiment comprises elements B and D, other remaining combinations of A, B, C, or D, may also be used.

[0122] Although the embodiments have been described in detail, it should be understood that various changes, substitutions and alterations can be made herein without departing from the scope as defined by the appended claims.

[0123] Moreover, the scope of the present application is not intended to be limited to the particular embodiments of the process, machine, manufacture, composition of matter, means, methods and steps described in the specification. As one of ordinary skill in the art will readily appreciate from the disclosure of the present invention, processes, machines, manufacture, compositions of matter, means, methods, or steps, presently existing or later to be developed, that perform substantially the same function or achieve substantially the same result as the corresponding embodiments described herein may be utilized. Accordingly, the appended claims are intended to include within their scope such processes, machines, manufacture, compositions of matter, means, methods, or steps

[0124] As can be understood, the examples described above and illustrated are intended to be exemplary only. The scope is indicated by the appended claims.

[0125] The claims are not intended to include, and should not be interpreted to include, means-plus- or step-plus-function limitations, unless such a limitation is explicitly recited in a given claim using the phrase(s) “means for” or “step for,” respectively.

Claims

CLAIMS1. An electrode for a battery, the electrode comprising:partially reduced graphene oxide nanoribbons (GOnRs) having an oxygen to carbon (0 / C) ratio of greater than zero to less than 0.49.

2. The electrode according to claim 1 , wherein the O / C ratio ranges from about 0.03 to about 0.21.

3. The electrode according to claim 2, wherein the O / C ratio ranges from about 0.03 to about 0.12.

4. The electrode according to claim 3, wherein the O / C ratio ranges from about 0.07 to about 0.12.

5. The electrode according to claim 4, wherein the O / C ratio is about 0.12.

6. The electrode according to any one of claims 1 to 5, wherein an oxygen content in the GOnRs ranges from about 2.6 wt.% to about 17.6 wt.%.

7. The electrode material according to claim 6, wherein the oxygen content is about 11.2%.

8. The electrode according to any one of claims 1 to 7, comprising MXene.

9. The electrode according to claim 8, wherein the MXene is Mn+iXnTx, where M is a transition metal, wherein M is at least one of Ti, Nb, V, Mo, Ta, Zr, Hf, Cr, and Sc, n is 1, 2, 3, or 4, X is at least one of carbon and nitrogen, and Txis surface functional groups, wherein Txis at least one of -OH, -F, -Cl, and -O.

10. The electrode according to claim 9, wherein M is at least one of Ti, V, Sc, and Nb.

11. The electrode according to claim 10, wherein the MXene is Ti3C2Txand Txis at least one of -OH, -F, -Cl, and -O.

12. The electrode according to claim 11, wherein Txis at least one of -OH, -F, and -O.

13. The electrode according to any one of claims 1 to 12, wherein a weight ratio of GOnRs : MXene is in a ranging of about 2:5 to about 3: 1.

14. The electrode according to claim 13, wherein the weight ratio of GOnRs : MXene is about 3:1.

15. The electrode according to any one of claims 1 to 14, comprising a conductive additive, wherein the conductive additive is at least one of carbon black, acetylene black, graphite (synthetic or natural), carbon nanotubes (CNTs), graphene I graphene oxide, carbon nanofibers (CNFs), vapor-grown carbon fibers (VGCFs), polyaniline (PANI), polypyrrole (PPy), and poly(3,4-ethylenedioxythiophene: polystyrene sulfonate (PDOTPSS).

16. The electrode according to any one of claims 1 to 15, comprising a non-conductive binder, wherein the non-conductive binder is at least one of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), Styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyimides (PI), polytetrafluoroethylene (PTFE), poly(acrylonitrile) (PAN), chitosan, polyurethane (PU), and poly(methyl methacrylate) (PMMA).

17. The electrode according to claim 15 or 16, wherein the conductive additive is carbon black.

18. The electrode according to claim 16 or 17, wherein the non-conductive binder is poly(vinylidene fluoride).

19. The electrode according to any one of claims 16, 17 or 18, wherein the weight ratio of (GOnRs and MXene) : conductive additive : non-conductive binder is about 9: 0.5 :0.

5.

20. The electrode according to any one of claim 1-19, wherein the battery is a lithium-ion battery, a sodium-ion battery, an aluminium-ion battery, or an magnesium-ion battery.

21. The electrode according to claim 20, wherein the battery is a lithium-ion battery.

22. A battery comprising an anode, a cathode, and a separator, wherein the anode is the electrode of any one of claims 1-22.

23. The battery of claim 22 wherein the cathode comprises any one of Lithium Cobalt Oxide, Nickel Manganese Cobalt, Lithium Iron Phosphate, Lithium Manganese Oxide.

24. A method of preparing an electrode for a battery, the method comprising:reducing graphene oxide nanoribbons (GOnRs) until the oxygen to carbon (0 / C) ratio is in a range from greater than zero to less than 0.49 to form partially reduced graphene oxide nanoribbons (rGOnRs);mixing the GOnRs with a conductive additive and binder to form a mixture; and coating the mixture onto a current collector.

25. The method of claim 24, comprising annealing the GOnR to reduce the 0 / C ratio at a temperature ranging from 250°C to 1000°C to partially reduce the GOnRs.

26. The method according to any one of claims 24-25 comprising mixing the partially reduced graphene oxide nanoribbons with MXene.

27. The method according to claim 26, wherein the weight ratio of (rGOnRs and MXene) : conductive additive : non-conductive binder is about 9: 0.5 :0.5.

28. The method according to any one of claims 24-27, wherein the conductive additive is at least one of carbon black, acetylene black, graphite (synthetic or natural), carbon nanotubes (CNTs), graphene I graphene oxide, carbon nanofibers (CNFs), vapor-grown carbon fibers (VGCFs), polyaniline (PANI), polypyrrole (PPy), and poly(3,4-ethylenedioxythiophene: polystyrene sulfonate (PDOT:PSS).

29. The method according to any one of claims 24-28, wherein the binder is a non-conductive binder comprising at least one of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), Styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyimides (PI), polytetrafluoroethylene (PTFE), poly(acrylonitrile) (PAN), chitosan, polyurethane (PU), and poly(methyl methacrylate) (PMMA).

30. The method according to any one of claims 26-27, wherein the weight ratio ofrGOnRs : MXene is within a range of about 2:5 to about 3:1.

31. The method according to claim 30, wherein the weight ratio of rGOnRs : MXene is about 3:1.

32. The method according to according to any one of claims 24to 31 , wherein the temperature is 250°C 500°C, 750°C or 1000°C.

33. The method according to claim 32, wherein the temperature is 500°C.

34. The method according to according to any one of claims 24to 33, wherein the partially reduced GOnRs have an oxygen to carbon (O / C) ratio ranging from about 0.03 to about 0.21.

35. The method according to claim 34, wherein the O / C ratio ranges from about 0.03 to about 0.12.

36. The method according to claim 35, wherein the O / C ratio ranges from about 0.07 to about 0.12.

37. The method according to claim 36, wherein the O / C ratio is about 0.12.

38. The method according to any one of claims 24-37, wherein the MXene is Mn+iXnTx, where M is a transition metal, wherein M is at least one of Ti, Nb, V, Mo, Ta, Zr, Hf, Cr, and Sc, n is 1 , 2, 3, or 4, X is at least one of carbon and nitrogen, and Txis surface functional groups, wherein Txis at least one of -OH, -F, -Cl, and -O.

39. The method according to claim 38, wherein M is at least one of Ti, V, Sc, and Nb.

40. The method according to claim 39, wherein the MXene is Ti3C2Txand Txis at least one of -OH, -F, -O, and -Cl.

41. The method according to claim 40, wherein Txis at least one of -OH, -F, and -O.

42. The method according to any one of claims 24-41 , wherein the conductive additive is carbon black.

43. The method according to claim 24-42, wherein the non-conductive binder is poly(vinylidene fluoride).

44. The method according to any one of claims 24-43, wherein the battery is a lithium-ion battery, a sodium-ion battery, an aluminium-ion battery, or an magnesium-ion battery.

45. The electrode according to claim 44, wherein the battery is a lithium-ion battery.

46. An electrode material for an electrode of a lithium-ion battery, the electrode material comprising:partially reduced graphene oxide nanoribbons (GOnRs) having an oxygen to carbon (0 / C) ratio of greater than zero to less than 0.49.

47. The electrode material according to claim 46, wherein the 0 / C ratio ranges from about 0.03 to about 0.21.

48. The electrode material of claim 46, comprising MXene, a conductive additive, and a binder, wherein:the partially reduced graphene oxide nanoribbons (GOnRs) has an oxygen / carbon (0 / C) ratio of about 0.12 and an oxygen content of about 11.2%;the MXene is TisC2Tx, where Txis at least one of -OH, -F, and -O;a weight ratio of GOnRs : MXene is about 3:1 and the weight ratio of (GOnRs and MXene) : conductive additive : non-conductive binder is about 9: 0.5 :0.5.

49. The electrode material of claim 48, wherein the conductive additive is carbon black and the binder is poly(vinylidene fluoride).