Low-cost and environmentally-friendly polyimide separator and preparation method therefor, and electrochemical device
By using environmentally friendly modifiers to react with polyamic acid, the structure of polyimide separators is improved, solving the problems of mechanical strength and environmental pollution. This enables the preparation of high-performance, low-cost separators, thereby enhancing the stability and safety of batteries.
Patent Information
- Application Number
- PCT/CN2025/094003
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-12
AI Technical Summary
Existing polyimide separators have low mechanical strength and elongation at break, and their preparation process involves high costs and environmental pollution, affecting the performance and safety of lithium-ion batteries.
By using environmentally friendly modifiers such as PBAT, PLA, PBS, PCL, PVA, and PVB to react with polyamic acid, the mechanical strength, elongation, and electrical conductivity of the polyimide membrane are improved, thereby reducing production costs and environmental impact.
It significantly improves the mechanical strength, elongation, and conductivity of polyimide separators, enhances the long-cycle stability and safety of batteries, and reduces production costs and environmental pollution, making it suitable for industrial production.
Smart Images

Figure CN2025094003_12112026_PF_FP_ABST
Abstract
Description
Low-cost, environmentally friendly polyimide membrane, its preparation method and electrochemical device Technical Field
[0001] This application relates to a low-cost, environmentally friendly polyimide membrane, its preparation method, and an electrochemical device, belonging to the field of polyimide membrane preparation technology. Background Technology
[0002] Currently, commercially available separators primarily use polyolefins, including polyethylene (PE) and polypropylene (PP), as base materials due to their excellent chemical stability and low cost. However, the non-polar structure of polyolefin microporous membranes results in poor hydrophilicity, leading to slow lithium-ion migration and negative rate capability, particularly at high current densities. Furthermore, the severe thermal shrinkage of polyolefin membranes at high temperatures significantly limits the application of lithium-ion batteries, as it can cause internal short circuits, fires, and even explosions, as seen in numerous electric vehicle fires and energy storage power station explosions.
[0003] In order to fundamentally avoid and eliminate the above-mentioned drawbacks, some new high-performance polymer membranes have been researched and developed. Among these membranes, polyimide membranes treated by phase inversion or electrospinning and thermal imidization exhibit superior performance due to their high porosity, electrolyte wettability, thermal stability and special three-dimensional network structure that suppresses lithium dendrites.
[0004] However, low tensile strength and low elongation at break have become significant weaknesses of polyimide separators, mainly due to the following two reasons:
[0005] 1. The monomers used in the synthesis of polyimide are relatively rigid, which makes the film brittle and has a low elongation.
[0006] 2. Nanofibers produced by electrospinning technology exhibit direct, loose overlap and a lack of cross-linking structures, which can lead to instability in the pore structure and instability in the cycling process.
[0007] Furthermore, the current preparation of polyimide separators still faces challenges such as high production costs and severe environmental pollution. Therefore, significantly improving the mechanical strength and elongation at break of polyimide separators, and enhancing their original performance while reducing costs and environmental pollution, is of great significance for the long-cycle stability of batteries. Summary of the Invention
[0008] To address the aforementioned issues, a low-cost, environmentally friendly method for preparing polyimide separators is provided. This method, while resolving environmental pollution problems and reducing production costs, can stabilize the pore structure of the polyimide separator, improve its mechanical strength and elongation at break, and enhance its rate performance and cycle life in batteries.
[0009] According to one aspect of this application, a method for preparing a low-cost, environmentally friendly polyimide separator is provided, comprising the following steps:
[0010] (1) Add diamine monomers and dianhydride monomers in a molar ratio of 1:(1-1.1) to a solvent and react to obtain a solution containing polyamic acid;
[0011] (2) Add a modifier to the polyamic acid-containing solution to obtain a slurry, wherein the modifier is selected from at least one of polybutylene terephthalate (PBAT), polylactic acid (PLA), polybutylene succinate (PBS), polycaprolactone (PCL), polyvinyl alcohol (PVA), and polyvinyl butyral (PVB).
[0012] (3) The slurry is coated or electrospinned to form a wet film, the wet film is immersed in a cleaning solution and dried to obtain the final product.
[0013] The reaction structural formulas of the diamine monomer and dianhydride monomer in step (1) of the above preparation method are as follows:
[0014] The reaction structure of polyamic acid and modifier in step (2) is as follows:
[0015] This application employs an environmentally friendly and low-cost method for modifying polyimide lithium-ion battery separators, requiring comprehensive consideration of material selection, modification technology, preparation process, cost control, and environmental impact. In this preparation method, the polyamic acid formed by the reaction of diamine monomers and dianhydride monomers is end-capped with amide groups. Therefore, the polyamic acid can react with the hydroxyl groups in the modifier, thereby introducing the modifier into the polyimide separator. Through the mechanisms of hydrogen bonding and van der Waals forces, it can improve the mechanical strength, elongation, thermal stability, and electrical conductivity of the polyimide separator. Furthermore, the modifier used is an environmentally friendly one, which can reduce environmental pollution and production costs, facilitating industrial-scale application.
[0016] Specifically, the Mn of PBAT is 50,000-200,000 g / mol, that of PLA is 20,000-80,000 g / mol, that of PBS is 20,000-100,000 g / mol, that of PCL is 20,000-80,000 g / mol, that of PVA is 10,000-150,000 g / mol, and that of PVB is 30,000-300,000 g / mol.
[0017] If the molecular weight of the above-mentioned modifier is too high, the porosity will be low, making preparation difficult; if the molecular weight is too low, the film formation will be poor, resulting in a decrease in the mechanical properties and heat resistance of the membrane.
[0018] In addition, the proportion of the modifier added in this application is not high and the molecular weight selected is also within the range commonly used in film making. It will not change the properties of the original polyimide membrane too much, but rather make the polyimide membrane arrange a rigid structure to make it more flexible.
[0019] Optionally, in step (2), the amount of the modifier is 5%-25% of the weight of polyamic acid.
[0020] The modifier achieves the best modification effect at the above dosage. As the amount of modifier increases, the porosity of the polyimide membrane can be increased, thereby improving its electrolyte absorption rate. However, when the amount of modifier exceeds 25% of the weight of polyamic acid, the heat resistance of the membrane will decrease.
[0021] Optionally, the reaction temperature in step (2) is 40-80℃ and the reaction time is 6-10h.
[0022] The aforementioned reaction temperature can improve the reaction efficiency of polyamic acid and modifier, thereby shortening the reaction time, saving time and costs, and facilitating large-scale industrial production. If the reaction temperature is too high or the reaction time is too long, the polymer will form a random structure, which will reduce the dimensional stability and mechanical strength of the membrane and may cause uneven pore size distribution, thus affecting the wettability of the electrolyte and the lithium-ion transport performance. If the reaction temperature is too low or the reaction time is too short, the polymer chain segments will be too short or amorphous, which will not only make it difficult to form a uniform and continuous porous structure, but may also reduce the thermal stability and tensile strength of the membrane and increase the risk of thermal runaway.
[0023] Optionally, in step (3), the soaking temperature is 25-65℃ and the soaking time is 10min.
[0024] The soaking process in step (3) removes unreacted modifiers. The soaking temperature is in the range of 25-65℃. The higher the temperature, the lower the solubility of the polymer, causing the polymer to precipitate from the solution more quickly. This promotes a faster phase separation process, making the pore structure on the membrane surface or inside more porous, resulting in higher membrane porosity. However, when the soaking temperature is higher than 65℃, the mobility of the polymer chains is enhanced, making the molecules more flexible, resulting in a more porous membrane structure with larger pores or more tiny holes. Although this structural change may improve the wettability of the electrolyte, it also makes the porosity and pore size distribution difficult to control, reduces the structural stability of the membrane, and makes it difficult to form a continuous and uniform porous network. This weakens the mechanical strength, thermal stability, and ion selective permeability required in lithium batteries, adversely affecting the overall performance and safety of the battery.
[0025] Optionally, the cleaning solution in step (3) is at least one of alcohol, water, ethylene glycol, and tetrahydrofuran.
[0026] Optionally, the reaction temperature in step (1) is 22-25℃ and the reaction time is 6-12h.
[0027] In step (1), if the reaction temperature is too high, the molecular weight will decrease, which is not conducive to improving the mechanical strength of the membrane. If the reaction temperature is too low or the time is too short, the reaction will be insufficient, the molecular weight of the membrane will decrease, and thus affect the performance of the membrane.
[0028] Optionally, the diamine monomer is selected from at least one of N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-diphenyl]-4,4'-diyl)bis(4-aminobenzamide), 4,4'-diaminobenzoylaniline, 3,5-diaminobenzoic acid, 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid, 4,4'-diaminodiphenyl ether, p-phenylenediamine, 4,4-diaminodiphenylmethane, 2,2'-bis(trifluoromethyl)diaminobiphenyl, 3,3'-dihydroxybenzidine, and 9,9-bis(4-aminophenyl)fluorene;
[0029] The dianhydride monomer is selected from at least one of hexafluorodianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, pyromellitic dianhydride, 4,4'-oxobisphthalic anhydride, 3,3',4,4'-benzophenone tetracarboxylic acid dianhydride, and 3,3,4,4-diphenylsulfone tetracarboxylic acid dianhydride.
[0030] Optionally, the solvent in step (1) is selected from at least one of dimethylacetamide (DMAc), m-cresol, tetrahydrofuran (THF), N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), chloroform, 3-methoxy-N,N-dimethylpropionamide and γ-butyrolactone (GBL).
[0031] Optionally, inert gases are introduced for protection during the reactions in steps (1) and (2), including nitrogen, argon, helium, neon, krypton, and xenon.
[0032] Optionally, the coating in step (3) includes dip coating, gravure coating, and spray coating.
[0033] Optionally, the drying in step (3) is to dry at 100°C for 10 min, and then at 250°C for 10 min.
[0034] Step (3) enables the membrane to undergo cross-linking or curing at low temperatures to reduce energy consumption and costs.
[0035] According to a second aspect of this application, a low-cost, environmentally friendly polyimide membrane prepared by any of the above-described preparation methods is provided.
[0036] Optionally, the polyimide diaphragm has a tensile strength of 20-60 MPa and an elongation of 10-60%.
[0037] Optionally, the polyimide membrane has an electrolyte absorption rate of 250-550% and an ionic conductivity of 0.30-0.80 ms / cm.
[0038] Optionally, the polyimide diaphragm has a tensile strength of 22.1-53 MPa and an elongation of 13.5-58%.
[0039] Optionally, the polyimide membrane has an electrolyte absorption rate of 250-514% and an ionic conductivity of 0.373-0.720 ms / cm.
[0040] Optionally, the thickness of the polyimide diaphragm is 5-30 μm, and optionally 10-15 μm.
[0041] For example, the thickness of the polyimide membrane can be 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, or any value in between.
[0042] According to a third aspect of this application, an electrochemical device is provided, comprising a positive electrode, a negative electrode, and a membrane, the membrane being located between the positive electrode and the negative electrode, the membrane being prepared by any of the preparation methods described above.
[0043] Optionally, the electrochemical device is one of a lithium secondary battery, a supercapacitor, a fuel cell, a sodium-sulfur battery, or a vanadium redox flow battery;
[0044] Optionally, the lithium secondary battery is selected from one of lithium-ion secondary batteries, lithium metal secondary batteries, lithium-air secondary batteries, and lithium-sulfur secondary batteries;
[0045] Optionally, the lithium-ion secondary battery includes a polymer lithium-ion secondary battery and an electrolyte support material for a solid-state battery.
[0046] The beneficial effects of this application include, but are not limited to:
[0047] 1. The method for preparing a low-cost, environmentally friendly polyimide separator according to this application achieves a balance between high performance and economic benefits by selecting environmentally friendly modifiers and processes, optimizing the production process, controlling costs, and minimizing environmental impact, thereby developing a battery separator that meets the needs of the modern market.
[0048] 2. The low-cost, environmentally friendly polyimide membrane preparation method of this application can solve the environmental pollution problem in the current preparation of polyimide membranes, reduce production costs, facilitate product process control, and has high economic benefits and environmental value.
[0049] 3. The low-cost, environmentally friendly polyimide separator preparation method of this application can significantly improve the mechanical strength, elongation, thermal stability and electrical conductivity of the polyimide separator, thereby improving the long-cycle stability of the battery.
[0050] 4. The low-cost, environmentally friendly polyimide separator according to this application can reduce the environmental impact and cost of the production process while ensuring excellent mechanical and electrochemical properties, and is suitable for industrial production.
[0051] 5. The low-cost, environmentally friendly polyimide separator according to this application can improve its rate performance and cycle life in batteries, while reducing production costs and environmental impact; and can meet the safety requirements of high-capacity, high-power power batteries for high-current charging and discharging and operation under harsh environments. Attached Figure Description
[0052] The accompanying drawings, which are included to provide a further understanding of this application and form part of this application, illustrate exemplary embodiments and are used to explain this application, but do not constitute an undue limitation of this application. In the drawings:
[0053] Figure 1 is a schematic diagram showing the morphology and wettability (contact angle) of the PVA-25% material and the comparative material 1 involved in Embodiment 2 of this application.
[0054] Figure 2 is a schematic diagram of the bending resistance test of the PVA-25% material and the comparative material 1 involved in Embodiment 2 of this application. Detailed Implementation
[0055] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.
[0056] Unless otherwise specified, all raw materials used in the embodiments of this application were purchased commercially. In the following embodiments, the Celgard 2325 diaphragm was purchased from Celgard Corporation.
[0057] Unless otherwise specified, the methods used in the embodiments of this application are conventional methods in the prior art.
[0058] The testing method for the diaphragm in the following embodiments is as follows:
[0059] 1. Membrane thickness: The thickness of different membranes was measured using a micrometer (accuracy 0.01 mm). Five points were randomly selected on the sample, and the average value was taken.
[0060] 2. Porosity: Immerse the diaphragm in n-octanol for 2 hours, then calculate the porosity using the formula:
[0061] P(%) = (Mw - Md) / ρVd x100, where ρ is the density of n-octanol and Vd is the geometric volume of the membrane, and Mw and Md are the mass of n-octanol absorbed by the membrane and the mass of the membrane itself.
[0062] 3. Electrolyte absorption rate: The diaphragm was immersed in the electrolyte (LiPF6 EC:DEC (v / v = 50 / 50)) for 2 hours to saturate the electrolyte in the diaphragm. The mass of the diaphragm before and after absorbing the electrolyte was measured and calculated using the following formula:
[0063] EU = [(W-Wo) / Wo] × 100%, where Wo and W are the masses of the diaphragm before and after absorbing the electrolyte.
[0064] 4. Ionic conductivity: Measured using electrochemical impedance spectroscopy (EIS) at 25°C in an electrochemical fixture. During the measurement, the electrolyte-impeded membrane is clamped between two stainless steel (SS) plate electrodes, and the impedance spectrum is recorded and analyzed. The test frequency range is 0.1-105 Hz, and the amplitude is 0.2 mV. Then, the ionic conductivity is calculated according to the following formula: σ=d / (Rb×S);
[0065] Where d and S are the thickness of the film and the contact area between the film and the stainless steel plate, respectively, and Rb is the intercept of the Nyquist plot on the real axis, which refers to the volume resistance.
[0066] 5. Wetting angle: Using a contact angle meter, cut the sample into 1cm*3cm pieces and fix the four corners flat on a glass slide. Take 2 microliters of EC / DEC electrolyte and place it below the separator membrane for analysis.
[0067] 6. Heat Shrinkage Rate: First, the membrane to be tested is cut into rectangular pieces of 4cm × 2.5cm and dried at 105℃ for 1 hour. Then, it is placed in a drying room at 150℃ for 1 hour. To more accurately determine the shrinkage rate, the area is compared using Autodesk mapping. The formula for calculating the heat shrinkage rate of the membrane is: (A1-A2) / A1×100%, where A1 is the area of the membrane before the test, and A2 is the area of the membrane after the test.
[0068] 7. Mechanical strength: A 1cm*10cm sample is tested using a tensile testing machine at a tensile speed of 1mm / s. This method can quickly obtain test data, and the sample's resistance to force can be observed directly at the time of testing. The test curve is mostly represented by a force-displacement curve.
[0069] 8. Positive electrode (NMC532): Place the positive and negative electrode materials and 70 μL of EC / DEC electrolyte onto the diaphragm to be tested, then press them onto the button cell and let them stand for 8 hours to confirm that the open-circuit voltage (OCV, open critical voltage) is stable. Starting from the open-loop voltage, use constant current mode to input the charging and discharging current and cutoff voltage (2.5V / 4.3V) for 100-cycle testing.
[0070] The modifiers used in this application, with Mn values of 50,000-200,000 g / mol for PBAT, 20,000-80,000 g / mol for PLA, 20,000-100,000 g / mol for PBS, 20,000-80,000 g / mol for PCL, 10,000-150,000 g / mol for PVA, and 30,000-300,000 g / mol for PVB, all fall within the aforementioned ranges and can achieve the scheme described in this application.
[0071] The modifiers used in the following examples have the following specific Mn values: PBAT = 50,000 g / mol, PLA = 40,000 g / mol, PBS = 50,000 g / mol, PCL = 68,000 g / mol, PVA = 88,000 g / mol, and PVB = 30,000 g / mol.
[0072] Example 1
[0073] This embodiment relates to a low-cost, environmentally friendly method for preparing a polyimide separator, comprising the following steps:
[0074] (1) Under nitrogen atmosphere, 4.90 g of 3,5-diaminobenzoic acid, 18 g of N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-diphenyl]-4,4'-diyl)bis(4-aminobenzamide) and 287.15 g of DMAc were added to a 500 ml three-necked flask and stirred at 22 °C for 30 min. After the 3,5-diaminobenzoic acid and N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-diphenyl]-4,4'-diyl)bis(4-aminobenzamide) were completely dissolved, 20 g of diphenyl ether tetracarboxylic dianhydride was added and the reaction was stirred at 22 °C for 6 h to obtain a solution containing the intermediate polyamic acid.
[0075] (2) Add different modifiers accounting for 10% of the weight of polyamic acid to the solution containing polyamic acid and stir until dissolved. Raise the temperature to 60°C and stir for 8 hours to obtain a slurry.
[0076] (3) Cool the slurry to room temperature and coat it onto a PET substrate with a release force of 150gf / 25mm. Then immerse it in a cleaning solution for 10 minutes to remove the modifier. The immersion temperature is 25℃. Finally, peel the removed wet film off the substrate surface and put it into a tunnel oven. First, dry it at 100℃ for 10 minutes, and finally dry it at 250℃ for 10 minutes to obtain a polyimide separator.
[0077] The different modifiers are PBAT (sample code PBAT-10), PCL (sample code PCL-10), PVA (sample code PVA-10), PBS (sample code PBS-10), and PVB (sample code PVB-10).
[0078] The performance of the three types of separators was tested, and the commercially available Celgard 2325 separator was used as Comparison 1, and the separator obtained without adding PVA in step (2) was used as Comparison 2. The results are shown in Table 1.
[0079] Table 1
[0080] As shown in Table 1, the electrolyte absorption rate of samples prepared with different environmentally friendly modifiers (PBAT-10, PCL-10 and PVA-10) increased by 1.8-3.23 times compared with commercially available separators as the content of carboxylic acid and hydroxyl groups increased, and the contact angle decreased significantly. The ionic conductivity was also increased by about 108% compared with commercially available separators (Celgard 2325 vs. PVA-10) due to the introduction of carboxylic acid and hydroxyl groups.
[0081] After stacking a bare cell by sequentially adding a positive electrode, different separators, and a negative electrode, and assembling them into a button-type lithium-ion battery, stability tests were conducted. The battery with the Celgard 2325 separator showed a sharp decrease in capacity at high-rate charge-discharge (1C), lower than that of the polyimide separator prepared in this application. This is due to its poor electrolyte adsorption, resulting in lower capacity. The difference in capacity between PVA-10 and Comparative 1 batteries after 100 days was 26.1%. In the test of Comparative 2 battery, at 100... th The reason why the hourly capacity is lower than 1.34 is that the lack of modifiers will lead to a decrease in the porosity of the separator, resulting in poor long-cycle stability during battery charge and discharge tests.
[0082] Example 2
[0083] This embodiment relates to a low-cost, environmentally friendly method for preparing a polyimide separator, comprising the following steps:
[0084] (1) Under nitrogen atmosphere, 7.72 g of 4,4'-diaminobenzoyl aniline, 9.25 g of 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid and 247.47 g of NMP were added to a 500 ml three-necked flask and stirred at 22 °C for 30 min. After 4,4'-diaminobenzoyl aniline and 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid were completely dissolved, 20 g of pyromellitic dianhydride was added and the reaction was stirred at 22 °C for 4 h to obtain a solution containing the intermediate polyamic acid.
[0085] (2) PVA was added to the polyamic acid solution at a weight percentage of 5%, 15% and 25% of the polyamic acid, and stirred continuously for 60 min. The sample codes were PVA-5%, PVA-15% and PVA-25%, respectively. The temperature was raised to 60℃ and stirred for 8 h to obtain the slurry.
[0086] (3) Cool the slurry to room temperature, take an appropriate amount of slurry with a syringe, install the syringe on the injection pump, connect the needle, and clamp the positive electrode of the high voltage electrostatic generator to the needle and connect the negative electrode to the receiving screen. Lay aluminum foil on the roller; set the spinning rate, adjust the spinning voltage and spinning distance, and perform electrostatic spinning; after spinning, remove the aluminum foil from the roller, and then soak it in the cleaning solution for 10 minutes to remove the modifier. The soaking temperature is 30℃. Finally, peel the wet film after removal from the aluminum foil surface and put it into the tunnel oven. First, dry it at 100℃ for 10 minutes, and finally dry it at 250℃ for 10 minutes to obtain the polyimide separator.
[0087] The performance of the three types of separators was tested, and the commercially available Celgard 2325 separator was used as Comparison 1, and the separator obtained without adding PVA in step (2) was used as Comparison 2. The results are shown in Table 2.
[0088] Table 2
[0089] Table 2 shows that the electrolyte absorption rate of samples prepared with different PVA addition amounts (PVA-5%, PVA-15%, and PVA-25%) increased by 2.89-4.24 times compared to commercially available separators as the addition amount increased, and the contact angle decreased significantly. This indicates that increasing the PVA content can improve the open porosity and thus the electrolyte absorption rate. The ionic conductivity also increased by approximately 60%-176% compared to commercially available separators due to the introduction of hydroxyl groups. With the increase of PVA, the tensile strength increased from 18.3 MPa (Comparison 2) to 33.4 MPa (PVA-25%), and the elongation at break increased by 112%.
[0090] After stacking a bare cell by sequentially adding a positive electrode, different separators, and a negative electrode, and assembling them into a button-type lithium-ion battery, stability tests were conducted. The battery with the Celgard 2325 separator showed a sharp decrease in capacity at high-rate charge-discharge (1C), lower than that of the polyimide separator prepared in this application. This is due to its poor electrolyte adsorption, resulting in lower capacity. The difference in capacity between PVA-25 and Comparative 1 battery after 100 days reached 34.4%. In the test of Comparative 2 battery, at 100... th The reason why the hourly capacity is lower than 1.64 is that the absence of PVA leads to a decrease in the porosity of the separator and the lack of hydroxyl groups affects the wettability of the electrolyte, resulting in poor long-cycle stability during battery charge and discharge tests.
[0091] Figure 1 shows the morphology and wettability (contact angle) of PVA-25% material and control material 1. Figure 1(a) is a micrograph of PVA-25% material, Figure 1(b) is a contact angle test diagram of PVA-25% material, Figure 1(c) is a micrograph of control material 1, and Figure 1(d) is a contact angle test diagram of control material 1. According to Figure 1, it can be seen that the pores of PVA-25% material are more uniform and more conducive to the absorption of electrolyte.
[0092] Figure 2(A) shows the sample images of PVA-25% material before, during and after bending, and Figure 2(B) shows the sample images of Comparison 1 material before, during and after bending. According to the comparison of Figure 2(A) and Figure 2(B), the diaphragm of this application has good bending resistance and is easier to use in industrial applications.
[0093] Example 3
[0094] This embodiment relates to a low-cost, environmentally friendly method for preparing a polyimide separator, comprising the following steps:
[0095] (1) Under nitrogen atmosphere, 4.90 g of 3,5-diaminobenzoic acid, 18 g of N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-diphenyl]-4,4'-diyl)bis(4-aminobenzamide) and 287.15 g of DMSO were added to a 500 ml three-necked flask, and stirred at 22 °C for 30 min. After the 3,5-diaminobenzoic acid and N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-diphenyl]-4,4'-diyl)bis(4-aminobenzamide) were completely dissolved, 20 g of diphenyl ether tetracarboxylic dianhydride was added, and the reaction was stirred at 22 °C for 6 h to obtain a solution containing the intermediate polyamic acid.
[0096] (2) Add PLA at a weight percentage of 10% of polyamic acid to the solution containing polyamic acid and stir until dissolved. Raise the temperature to 60°C and stir for 8 hours to obtain a slurry.
[0097] (3) Cool the slurry to room temperature and coat it onto a PET substrate with a release force of 150gf / 25mm. Then immerse it in a cleaning solution for 10 minutes to remove the modifier. The immersion temperatures are 25℃, 45℃ and 65℃ respectively. The sample codes are PLA-25, PLA-45 and PLA-65 respectively. Finally, peel the wet film off the substrate surface and put it into a tunnel oven. First, dry it at 100℃ for 10 minutes, and finally dry it at 250℃ for 10 minutes to obtain the polyimide separator.
[0098] The performance of the three types of diaphragms was tested, and the commercially available Celgard 2325 diaphragm was used as Comparison 1, and the diaphragm obtained without adding PLA in step (2) was used as Comparison 2. The results are shown in Table 3.
[0099] Table 3
[0100] As shown in Table 3, the electrolyte absorption rate of samples (PLA-25, PLA-45, and PLA-65) prepared at different immersion temperatures increased by 3.23-3.5 times compared to commercially available diaphragms as the temperature increased, and the contact angle decreased significantly. This indicates that increasing the temperature can improve the porosity and thus the electrolyte absorption rate. The ionic conductivity was also increased by about 117% compared to commercially available diaphragms (Celgard 2325 vs. PLA-65) due to the introduction of hydroxyl groups.
[0101] After stacking the positive electrode, different separators, and negative electrode to form a bare cell and assembling it into a button-type lithium-ion battery, stability tests were conducted. The battery composed of Celgard 2325 separator showed a sharp drop in capacity under high-rate charge and discharge (1C), which was lower than that of the polyimide separator prepared in this application. This was due to its poor electrolyte adsorption, resulting in poor capacity. The difference in capacity between PLA-65 and Comparative 1 battery after 100 days reached 32.48%.
[0102] In the full-battery test of Comparison 2, at 100 th The reason why the hourly capacity is lower than 1.43 is that the lack of modifiers will lead to a poorer opening rate of the separator, resulting in poor long-cycle stability during battery charge and discharge tests.
[0103] Example 4
[0104] This embodiment relates to a low-cost, environmentally friendly method for preparing a polyimide separator, comprising the following steps:
[0105] (1) Under nitrogen atmosphere, 3.49 g of p-phenylenediamine, 6.39 g of 4,4-diaminodiphenylmethane, and 287.15 g of DMSO were added to a 500 ml three-necked flask, and stirred at 25 °C for 30 min. After the p-phenylenediamine and 4,4-diaminodiphenylmethane were completely dissolved, 18.98 g of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride was added, and the reaction was stirred at 25 °C for 12 h to obtain a solution containing the intermediate polyamic acid.
[0106] (2) Add different modifiers accounting for 10% of the weight of polyamic acid to the solution containing polyamic acid and stir until dissolved. Raise the temperature to 80°C and stir for 6 hours to obtain a slurry.
[0107] (3) Cool the slurry to room temperature and coat it onto a PET substrate with a release force of 150gf / 25mm. Then immerse it in a cleaning solution for 10 minutes to remove the modifier. The immersion temperature is 25℃. Finally, peel the wet film off the substrate surface and put it into a tunnel oven. First, dry it at 100℃ for 10 minutes, and finally dry it at 250℃ for 10 minutes to obtain a polyimide separator.
[0108] The different modifiers were PBS (sample code PBS-10) and PVB (sample code PVB-10).
[0109] The performance of the two types of diaphragms was tested, and the commercially available Celgard 2325 diaphragm was used as control 1, and the diaphragm obtained without adding PBS in step (2) was used as control 2. The results are shown in Table 4.
[0110] Table 4
[0111] As shown in Table 4, the electrolyte absorption rate of samples prepared with different environmentally friendly modifiers (PBS-10, PVB-10) increased by 1.17-3.23 times compared with commercially available membranes as the content of carboxylic acid and hydroxyl groups increased, and the contact angle decreased significantly. The ionic conductivity was also increased by about 39% compared with commercially available membranes (Celgard 2325 vs. PVB-10) due to the introduction of carboxylic acid and hydroxyl groups.
[0112] After stacking the positive electrode, different separators, and negative electrode in sequence to form a bare cell and assembling it into a button-type lithium-ion battery, stability tests were conducted. The battery composed of Celgard 2325 separator showed a sharp drop in capacity under high-rate charge and discharge (1C), which was lower than that of the polyimide separator prepared in this application. This was due to its poor electrolyte adsorption, resulting in poor capacity. The difference in capacity between PVB-10 and Comparative 1 after 100 days was 19.74%.
[0113] Taking the addition of 25% as an example, the original membrane price is RMB 500-1500 / kg, and the price of the environmentally friendly modifier is RMB 20-300 / kg, so the production cost can be reduced by about 20%-24%.
[0114] The above description is merely an embodiment of this application, and the scope of protection of this application is not limited to these specific embodiments, but is determined by the claims of this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the technical concept and principles of this application should be included within the scope of protection of this application.
Claims
1. A method for preparing a low-cost, environmentally friendly polyimide separator, characterized by, The preparation method comprises the following steps: (1) adding diamine monomers and dianhydride monomers in a molar ratio of 1:(1-1.1) into a solvent to obtain a solution containing polyamic acid by reaction; (2) adding a modifier selected from at least one of polybutylene terephthalate adipate, polylactic acid, polybutylene succinate, polycaprolactone, polyvinyl alcohol and polyvinyl butyral into the solution containing polyamic acid to obtain a slurry; (3) forming a wet film by coating or electrospinning the slurry, and then immersing the wet film in a cleaning solution for treatment, and drying to obtain the polyimide separator.
2. The production method according to claim 1, characterized by, In step (2), the amount of the modifier is 5%-25% by weight of the polyamic acid.
3. The production method according to claim 1, characterized by, The reaction temperature in step (2) is 40-80°C, and the reaction time is 6-10h.
4. The method of claim 1, wherein, In step (3), the immersion temperature is 25-65°C, and the immersion time is 10min.
5. The preparation method according to claim 1, characterized in that, The reaction temperature in step (1) is 22-25°C, and the reaction time is 6-12h.
6. The method of claim 1, wherein, The diamine monomers are selected from at least one of N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide), 4,4'-diaminobenzanilide, 3,5-diaminobenzoic acid, 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid, 4,4'-diamino diphenyl ether, p-phenylenediamine, 4,4-diaminodiphenyl methane, 2,2'-bis(trifluoromethyl)diaminobiphenyl, 3,3'-dihydroxybenzidine, 9,9-bis(4-aminophenyl)fluorene; The dianhydride monomers are selected from at least one of hexafluorodianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, pyromellitic dianhydride, 4,4'-oxybisphthalic anhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3,4,4-diphenyl sulfone tetracarboxylic dianhydride.
7. The low-cost and environmentally friendly polyimide separator prepared by the preparation method of any one of claims 1-6.
8. The low cost, environmentally friendly polyimide separator of claim 7, wherein, The tensile strength of the polyimide separator is 20-60MPa, and the elongation at break is 10-60%.
9. The low cost, environmentally friendly polyimide separator of claim 7, wherein, The electrolyte absorption rate of the polyimide separator is 250-550%, and the ionic conductivity is 0.30-0.80ms / cm.
10. An electrochemical device, characterized by, The electrochemical device is one of a lithium secondary battery, a supercapacitor, a fuel cell, a sodium-sulfur battery, and a vanadium flow battery.
11. The electrochemical device of claim 10, wherein, The lithium secondary battery is one of a lithium ion secondary battery, a lithium metal secondary battery, a lithium air secondary battery, and a lithium sulfur secondary battery.
12. The electrochemical device of claim 11, wherein, The lithium ion secondary battery includes a polymer lithium ion secondary battery and an electrolyte support material of a solid-state battery.
13. The electrochemical device of claim 12, wherein,