High-voltage-resistant polymer-based solid-state electrolyte, preparation method therefor, and use thereof

By using a thermal polymerization method involving cyanoacrylate monomers, lithium salts, crosslinking agents, and solvents, a polymer-based solid electrolyte with cyano polar functional groups is formed. This solves the problem of poor electrochemical stability of polymer electrolytes under high voltage, and enables stable operation and good performance of batteries under high voltage.

WO2026232696A1PCT designated stage Publication Date: 2026-11-12SOLID IONIC POWER TECHNOLOGY (WUHAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/108848
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2025-07-16
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing polymer electrolytes have low room-temperature ionic conductivity, narrow electrochemical window, and poor electrochemical stability, making it difficult to match them with high-voltage cathodes to prepare high-energy-density solid-state batteries.

Method used

A polymer-based solid electrolyte containing cyano group polar functional groups is formed by mixing cyanoacrylate monomers with lithium salt, crosslinking agent and solvent through thermal polymerization. The cyano group forms a stable interface with the positive electrode transition metal, which reduces solvent decomposition and improves oxidation stability.

Benefits of technology

It broadens the electrochemical window to approximately 5.1V, enabling stable operation above 4.5V, maintaining interfacial chemical stability, and is suitable for high-voltage cathode materials, thereby improving the physicochemical properties and electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025108848_12112026_PF_FP_ABST
    Figure CN2025108848_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Embodiments of the present invention relate to a high-voltage-resistant polymer-based solid-state electrolyte, a preparation method therefor, and an use thereof. The preparation method comprises: uniformly mixing a lithium salt, a polymer monomer, a crosslinking agent, and a solvent in proportion to obtain a polymer-based solid-state electrolyte precursor, wherein the polymer monomer comprises a cyanoacrylate monomer; and adding an initiator to the polymer-based solid-state electrolyte precursor, and then performing thermal polymerization to obtain a polymer-based solid-state electrolyte having a polar functional group, i.e., a cyano group, that is, the high-voltage-resistant polymer-based solid-state electrolyte. In the present invention, by using the cyanoacrylate monomer containing the cyano functional group, the cyano group can be effectively adsorbed and coordinated on a positive electrode transition metal to form a stable positive electrode-electrolyte interface, thereby reducing leakage of solvent molecules, effectively improving the oxidation stability of the electrolyte, enabling the electrolyte to be compatible with a high-voltage positive electrode material, and maintaining the chemical stability of the interface.
Need to check novelty before this filing date? Find Prior Art

Description

High-voltage resistant polymer-based solid electrolytes, their preparation methods and applications

[0001] This application claims priority to Chinese Patent Application No. 202510590876.4, filed on May 8, 2025, entitled "High Voltage Resistant Polymer-Based Solid Electrolyte and its Preparation Method and Application". Technical Field

[0002] This invention relates to the field of solid electrolyte materials, and more particularly to a high-voltage resistant polymer-based solid electrolyte, its preparation method, and its application. Background Technology

[0003] With the rapid development of electric vehicles and energy storage devices, the urgent demand for high-energy-density batteries is increasing daily. However, currently commercialized liquid lithium batteries not only struggle to achieve the ideal high energy density, but also pose serious safety hazards due to the flammability and explosiveness of the liquid electrolyte. Therefore, the development of solid-state lithium batteries has become a competitive arena for researchers and major new energy companies worldwide.

[0004] Solid-state electrolytes possess characteristics such as non-volatility, flame retardancy, high mechanical strength, and the ability to suppress lithium dendrite formation. Therefore, developing solid-state lithium batteries using solid-state electrolytes can effectively solve the problems of energy density and safety. Currently, inorganic solid-state electrolytes and polymer electrolytes have been extensively studied. Among them, inorganic solid-state electrolytes exhibit high room-temperature ionic conductivity (>10). -4 S cm -1 While polymer electrolytes offer advantages such as good flexibility, close contact with electrodes, ease of processing, and low cost, they also suffer from poor contact at the electrode interface, high sensitivity to oxygen and water, inherent brittleness, and poor interfacial expansion, thus limiting their further development. Polymer electrolytes are considered the most promising materials for preparing solid-state lithium batteries due to their good flexibility, close contact with electrodes, ease of processing, and low cost. However, polymer electrolytes also exhibit low room-temperature ionic conductivity, a narrow electrochemical window, and poor electrochemical stability. Therefore, using polymer electrolytes to match high-voltage cathodes to prepare high-energy-density solid-state batteries remains a significant challenge.

[0005] Therefore, there is an urgent need to design a polymer-based solid electrolyte with a wide electrochemical window and the ability to form a stable electrolyte-electrode interface at high voltage. Summary of the Invention

[0006] The purpose of this invention is to address the deficiencies of existing technologies by providing a high-voltage resistant polymer-based solid electrolyte, its preparation method, and its application. This high-voltage resistant polymer-based solid electrolyte exhibits good physicochemical properties and electrochemical performance at a cutoff voltage of 4.5V or higher.

[0007] To achieve the above objectives, in a first aspect, the present invention provides a method for preparing a high-voltage resistant polymer-based solid electrolyte, the method comprising:

[0008] Lithium salt, polymer monomer, crosslinking agent, and solvent are mixed uniformly in a certain proportion to obtain a polymer-based solid electrolyte precursor; wherein, the polymer monomer includes cyanoacrylate monomers;

[0009] An initiator is added to the polymer-based solid electrolyte precursor, and then thermal polymerization is carried out to obtain a polymer-based solid electrolyte with polar functional groups of cyano groups, which is the high-voltage resistant polymer-based solid electrolyte.

[0010] Preferably, the mass ratio of the polymer monomer to the solvent is 1:10-10:1; the mass of the crosslinking agent is 0.5%-3% of the mass of the polymer monomer; and the concentration of the lithium salt in the polymer-based solid electrolyte precursor is 0.5mol / L-2mol / L.

[0011] Preferably, the mass of the initiator is no more than 1% of the mass of the polymer-based solid electrolyte precursor.

[0012] Preferably, the temperature of the thermal polymerization is 45℃-80℃, and the time is 1 hour-24 hours.

[0013] Preferably, the lithium salt comprises one or more of lithium difluorooxalate borate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium difluorodioxamate phosphate.

[0014] The cyanoacrylate monomers include one or more of the following: 2-cyanoethyl acrylate, acrylonitrile, 2-ethyl cyanoacrylate, 2-cyanoethoxyethyl acrylate, cyanoethyl isobutylenoate, ethyl cyanoacrylate, propyl cyanoacrylate, pentyl cyanoacrylate, 3-amino-2-butenoic acid cyanoacetic acid, and ethyl 2-cyano-3-methylbutenoate.

[0015] The solvent includes carbonate compounds and / or sulfite compounds; the carbonate compounds include one or more of the following: dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, ethylene carbonate, propylene carbonate, and fluoroethylene carbonate;

[0016] The sulfite compounds include one or more of the following: dimethyl sulfite, dimethyl sulfate, diethyl sulfite, ethyl sulfite, and propylene sulfite;

[0017] The crosslinking agent is an acrylate compound, which includes one or more of the following: ethoxylated trimethylolpropane triacrylate, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and pentaerythritol triacrylate.

[0018] Preferably, the initiator is a free radical initiator; the free radical initiator includes one or more of azobisisobutyronitrile, azobisisoheptanenitrile, and benzoyl peroxide.

[0019] In a second aspect, the present invention provides a high-voltage resistant polymer-based solid electrolyte, wherein the high-voltage resistant polymer-based solid electrolyte is prepared by any of the preparation methods described in the first aspect above.

[0020] Thirdly, the present invention provides a solid-state battery, the solid-state battery comprising the high-voltage resistant polymer-based solid electrolyte described in the second aspect.

[0021] Preferably, the positive electrode active material of the solid-state battery includes one or two of layered oxide and polyanionic compound; the layered oxide includes one or two of lithium cobalt oxide and lithium nickel cobalt manganese oxide; the polyanionic compound includes lithium iron phosphate; and the negative electrode active material includes any one of graphite and lithium metal sheet.

[0022] Fourthly, the present invention provides a method for preparing the solid-state battery described in the third aspect, the method comprising:

[0023] Lithium salt, polymer monomer, crosslinking agent, and solvent are mixed uniformly in a certain proportion to obtain a polymer-based solid electrolyte precursor; wherein, the polymer monomer includes cyanoacrylate monomers;

[0024] An initiator is added to the polymer-based solid electrolyte precursor to obtain a liquid precursor to be polymerized;

[0025] The liquid precursor to be polymerized is injected into the space between the positive and negative electrodes inside the battery to be assembled, so that the liquid precursor to be polymerized fully wets the positive electrode, negative electrode and separator, and then the battery is encapsulated; or, the liquid precursor to be polymerized is dropped onto the positive electrode, negative electrode and separator of the battery to be assembled, and then the battery is encapsulated.

[0026] The battery is subjected to heat treatment to obtain the solid-state battery.

[0027] This invention provides a method for preparing a high-voltage resistant polymer-based solid electrolyte. By screening polymer monomers and solvents and optimizing precursor ratios, an in-situ polymerization process is used to prepare a polymer-based solid electrolyte suitable for high-voltage applications. By using cyanoacrylate monomers containing cyano functional groups, cyano groups can be effectively adsorbed and coordinated onto the positive electrode transition metal, forming a stable positive electrode-electrolyte interface, reducing solvent molecule leakage, and effectively improving the electrolyte's oxidation stability. Simultaneously, it reduces parasitic reactions between solvent molecules and the electrode, enabling the solid-state battery to operate stably at high voltages (≥4.5V). The polymerization of cyanoacrylate monomers forms a solid electrolyte containing polar groups. Because these polar functional groups have high electronegativity, they preferentially coordinate and adsorb onto the transition metal on the positive electrode, reducing the dissolution of the transition metal on the positive electrode side. The unique coordination structure formed by the polar functional groups in the cyanoacrylate monomers and the positive electrode reduces solvent decomposition, thereby increasing the electrolyte's oxidation potential. The high-voltage polymer-based solid electrolyte prepared by this invention exhibits good antioxidant properties and has an electrochemical window that is broadened to about 5.1V. It can match high-voltage cathode materials and maintain the chemical stability of the interface, thus exhibiting good physicochemical properties and electrochemical performance at a cutoff voltage of 4.5V or higher, and has good application prospects. Attached Figure Description

[0028] Figure 1 is a flowchart of the preparation method of the high-voltage resistant polymer-based solid electrolyte provided in the embodiment of the present invention;

[0029] Figure 2 shows the electrochemical window test curve of the high-voltage resistant polymer-based solid electrolyte provided in Example 1 of the present invention;

[0030] Figure 3 shows the electrochemical window test curve of the electrolyte provided in Comparative Example 1 of the present invention;

[0031] Figure 4 shows the leakage current test curves provided in Embodiment 2 and Comparative Example 1 of the present invention;

[0032] Figure 5 shows the electrochemical cycle performance of the solid-state battery with lithium cobalt oxide as the positive electrode provided in Example 2 of the present invention at a charging cutoff voltage of 4.5V.

[0033] Figure 6 shows the electrochemical cycling performance of the solid-state battery with lithium cobalt oxide as the positive electrode provided in Example 2 of the present invention at a charging cutoff voltage of 4.6V.

[0034] Figure 7 shows the battery cycle performance of the solid-state battery with lithium nickel cobalt manganese oxide as the positive electrode provided in Embodiment 2 of the present invention at a charging cutoff voltage of 4.7V.

[0035] Figure 8 is one of the XPS images of the interface between the high-voltage resistant polymer-based solid electrolyte and the positive electrode provided in Embodiment 2 of the present invention;

[0036] Figure 9 is the second XPS image of the interface between the high-voltage resistant polymer-based solid electrolyte and the positive electrode provided in Embodiment 2 of the present invention;

[0037] Figure 10 is one of the comparison diagrams of the electrochemical performance of the solid-state battery provided in Example 2 of the present invention and the coin cell provided in Comparative Example 1;

[0038] Figure 11 is a comparison of the electrochemical performance of the solid-state battery provided in Example 2 of the present invention and the coin cell provided in Comparative Example 1. Detailed Implementation

[0039] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments.

[0040] This invention provides a method for preparing a high-voltage resistant polymer-based solid electrolyte, the process of which is shown in Figure 1 and includes the following steps:

[0041] Step 110: Mix lithium salt, polymer monomer, crosslinking agent and solvent in proportion to obtain polymer-based solid electrolyte precursor;

[0042] The lithium salts include one or more of the following: lithium difluorooxalate borate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium difluorooxalate phosphate.

[0043] The polymer monomers include cyanoacrylate monomers. Cyanoacrylate monomers may include one or more of the following: 2-cyanoethyl acrylate, acrylonitrile, 2-ethyl cyanoacrylate, 2-cyanoethoxyethyl acrylate, cyanoethyl isobutylenoate, ethyl cyanoacrylate, propyl 2-cyanoacrylate, pentyl 2-cyanoacrylate, cyanoacetic acid of 3-amino-2-butenoic acid, and ethyl 2-cyano-3-methylbutenoate. Cyanoacrylate monomers can provide cyano groups to solid electrolytes, which have significant electronegativity and low highest occupied molecular orbitals, thus improving the oxidative stability of solid electrolytes and making them suitable for high-voltage (≥4.5V) cathodes.

[0044] The crosslinking agent can be an acrylate compound, specifically including one or more of the following: ethoxylated trimethylolpropane triacrylate, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and pentaerythritol triacrylate.

[0045] Solvents can include carbonate compounds and / or sulfite compounds. Carbonate compounds include one or more of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, ethylene carbonate, propylene carbonate, and fluoroethylene carbonate. Sulfite compounds include one or more of dimethyl sulfite, dimethyl sulfate, diethyl sulfite, ethylene sulfite, and propylene sulfite. Polar groups in the solvent can improve ionic conductivity, form hydrogen bonds or other interactions with the polymer backbone, enhance the mechanical strength of the solid electrolyte, and form ion transport channels, increasing ion mobility, etc. In particular, the sulfur-oxygen double bonds in sulfite compounds have high chemical reactivity and can react with other substances to form new interfacial layers. For example, during electrolyte decomposition, the sulfur-oxygen double bond can break to generate various products (sulfides), which can further react with the electrode surface to form a stable passivation layer, thereby enhancing the stability and functionality of the interface.

[0046] Specifically, firstly, one solvent can be used, or two solvents can be mixed. When the two solvents are carbonate compounds and sulfite compounds, the mass ratio of carbonate compounds to sulfite compounds can be 1:4.

[0047] Then, polymer monomers and crosslinking agents are added to the solvent and mixed for 2 hours at 30°C using mechanical stirring to obtain a mixed solution.

[0048] Finally, lithium salt was added to the mixed solution and mixed for 2 hours at 30°C using mechanical stirring to obtain the electrolyte precursor.

[0049] The mass ratio of polymer monomer to solvent can be 1:10-10:1, preferably 3:20-1:1. The mass of crosslinking agent can be 0.5%-3% of the mass of polymer monomer, preferably 1%-2%. The concentration of lithium salt in the polymer-based solid electrolyte precursor can be 0.5mol / L-2mol / L, preferably 1mol / L-2mol / L.

[0050] Step 120: An initiator is added to the polymer-based solid electrolyte precursor, and then thermal polymerization is carried out to obtain a polymer-based solid electrolyte with polar functional groups of cyano groups, which is a high-voltage resistant polymer-based solid electrolyte.

[0051] Specifically, this step can be carried out in a glove box where the water and oxygen content are both less than 0.1 ppm.

[0052] The initiator includes a free radical initiator. The mass of the initiator is no more than 1% of the mass of the polymer-based solid electrolyte precursor, preferably 0.2%-1%. The free radical initiator may include one or more of azobisisobutyronitrile, azobisisoheptanenitrile, and benzoyl peroxide.

[0053] The specific conditions for thermal polymerization are: temperature 45℃-80℃, time 1 hour-24 hours, preferably 60℃ for 2 hours. During the thermal polymerization process, the initiator decomposes to generate free radicals, which cause cyanoacrylate monomers to polymerize and form cyanoacrylate polymer chains. The crosslinking agent connects different cyanoacrylate polymer chains to form a network structure, resulting in a polymer-based solid electrolyte with polar functional groups, i.e., a high-voltage resistant polymer-based solid electrolyte. The polar functional groups are cyano and fluorinated groups.

[0054] This invention provides a method for preparing a high-voltage resistant polymer-based solid electrolyte. By screening polymer monomers and solvents and optimizing the precursor ratio, an in-situ polymerization process is used to prepare a polymer-based solid electrolyte suitable for high-voltage applications.

[0055] By using cyanoacrylate monomers containing cyano functional groups, cyano groups can be effectively adsorbed and coordinated onto the cathode transition metal, forming a stable cathode-electrolyte interface, reducing solvent molecule leakage, and effectively improving the oxidation stability of the electrolyte. Simultaneously, it reduces parasitic reactions between solvent molecules and the electrode, enabling the solid-state battery to operate stably at high voltages (≥4.5V). The cyanoacrylate monomers, after polymerization, form a solid electrolyte containing polar groups. Due to the high electronegativity of these polar functional groups, they preferentially coordinate and adsorb onto the transition metal on the cathode, reducing the dissolution of the transition metal on the cathode side. The unique coordination structure formed by the polar functional groups in the cyanoacrylate monomers and the cathode reduces solvent decomposition, thereby increasing the oxidation potential of the electrolyte. The high-voltage resistant polymer-based solid electrolyte prepared by this invention exhibits excellent oxidation resistance, with an electrochemical window widened to approximately 5.1V. It can be matched with high-voltage cathode materials, maintaining interfacial chemical stability, thus exhibiting good physicochemical properties and electrochemical performance above a cutoff voltage of 4.5V, and has promising application prospects.

[0056] The high-voltage polymer-based solid electrolyte provided in this invention can be applied to solid-state lithium metal batteries.

[0057] When applied to solid-state lithium metal batteries, solid-state batteries can be fabricated as follows:

[0058] Step 210: Mix lithium salt, polymer monomer, crosslinking agent and solvent in proportion to obtain polymer-based solid electrolyte precursor;

[0059] The polymer monomers include cyanoacrylate monomers;

[0060] Step 220: Add an initiator to the polymer-based solid electrolyte precursor to obtain the liquid precursor to be polymerized;

[0061] It should be noted that the materials used in steps 210 and 220 are the same as those used in the preparation of the high-voltage resistant polymer-based solid electrolyte, and the mixing methods and conditions are also the same, so they will not be repeated here.

[0062] Step 230: Inject the liquid precursor to be polymerized into the space between the positive and negative electrodes inside the battery to be assembled, so that the liquid precursor to be polymerized fully wets the positive electrode, negative electrode and separator, and then complete the battery encapsulation; or, drop the liquid precursor to be polymerized onto the positive electrode, negative electrode and separator of the battery to be assembled, and then complete the battery encapsulation.

[0063] Step 240: The battery is subjected to heat treatment to obtain a solid-state battery.

[0064] Those skilled in the art can refer to the following materials as needed to select the positive and negative electrode materials for solid-state batteries.

[0065] The positive electrode active material of solid-state batteries includes one or two of layered oxides and polyanionic compounds; the layered oxides include one or two of lithium cobalt oxide and lithium nickel cobalt manganese oxide; the polyanionic compounds include lithium iron phosphate; and the negative electrode active material includes any one of graphite and lithium metal sheets.

[0066] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0067] Example 1

[0068] This embodiment prepares a high-voltage resistant polymer-based solid electrolyte.

[0069] Preparation of the electrolyte precursor: Fluoroethylene carbonate (FEC) and dimethyl sulfite (DMS) were mixed in a mass ratio of 1:4; then, 2-cyanoethyl acrylate (CA) and 2% (by mass) of crosslinking agent ethoxylated trimethylolpropane triacrylate were added to the solvent in a mass ratio of 3:20 to the solvent, and the mixture was stirred at 30°C for about 2 hours to obtain a mixed solution; then, lithium difluorooxalate borate (LiDFOB) was added to the mixed solution at a mass ratio of 1 mol / L and stirred at 30°C for about 2 hours until completely dissolved, finally obtaining a homogeneous polymer-based solid electrolyte precursor.

[0070] Preparation of polymer-based solid electrolyte: 1% by mass of initiator azobisisobutyronitrile (AIBN) was added to the polymer-based solid electrolyte precursor obtained above, and the mixture was heated at 60°C for 2 hours to allow CA to fully polymerize, thereby obtaining a high-voltage resistant polymer-based solid electrolyte.

[0071] The high-voltage-resistant polymer-based solid electrolyte was used to assemble a semi-blocking battery for electrochemical window testing. The specific process is as follows: A stainless steel gasket was used as the working electrode and lithium metal was used as the reference electrode to assemble the semi-blocking battery. Linear sweep voltammetry (LSV) was performed, and the test was conducted from the open circuit voltage to the termination voltage of 7V at a scan rate of 1mV / s. The test equipment was a Gamry electrochemical workstation Interface 1000. The results are shown in Figure 2.

[0072] Example 2

[0073] This embodiment describes the preparation of a solid-state battery containing a high-voltage resistant polymer-based solid electrolyte.

[0074] Preparation of the electrolyte precursor: Fluoroethylene carbonate (FEC) and dimethyl sulfite (DMS) were mixed in a mass ratio of 1:4. Then, 2-cyanoethyl acrylate (CA) and 2% (by mass) of crosslinking agent ethoxylated trimethylolpropane triacrylate were added to the solvent in a mass ratio of 3:20. The mixture was stirred at 30°C for about 2 hours to obtain a mixed solution. Then, lithium difluorooxalate borate (LiDFOB) was added to the mixed solution at a mass of 1 mol / L and stirred at 30°C for about 2 hours until completely dissolved, finally yielding a homogeneous polymer-based solid electrolyte precursor.

[0075] The polymer-based solid electrolyte precursor prepared above was used to fabricate solid-state batteries, and relevant tests were conducted. The specific process is as follows:

[0076] Azobisisobutyronitrile (AIBN) initiator with a mass fraction of 1% was added to the polymer-based solid electrolyte precursor obtained above to form a liquid precursor to be polymerized. 15 μL of the liquid precursor to be polymerized was dropped onto the lithium cobalt oxide (LCO) positive electrode, and then a polypropylene separator was placed on top. Another 15 μL of the liquid precursor to be polymerized was dropped on to wet the separator. Then, a negative electrode lithium metal sheet, a gasket, and a spring were stacked. Finally, the assembled battery was placed in a heating device and heated at 60°C for 2 hours to allow CA to polymerize and form a high-voltage resistant polymer-based solid electrolyte. At the same time, an integrated stack including a positive electrode, electrolyte, separator, and negative electrode was formed in situ. Finally, the battery was encapsulated to obtain a solid-state battery, namely a Li||LCO battery.

[0077] First, the leakage current of the solid-state battery (Li||LCO battery) with lithium cobalt oxide (LCO) as the positive electrode was tested using the CT2001A battery testing system with a timed current method: the battery was charged to 4.2V, 4.3V, 4.4V, 4.5V, 4.6V, 4.7V, 4.8V, 4.9V and 5.0V and held at each voltage for 3 hours. The leakage current of the battery was observed to evaluate the actual oxidation stability of the electrolyte. The results are shown in Figure 4.

[0078] Secondly, the electrochemical performance of the above-mentioned solid-state battery (Li||LCO battery) with lithium cobalt oxide (LCO) as the positive electrode was characterized using a CT-4008Tn-mA battery testing system. The results are shown in Figure 5. At a charging cutoff voltage of 4.5V and a charge / discharge rate of 1C, the capacity retention after 400 cycles is 89.5%, and the discharge capacity is approximately 157.2 mAh / g. As shown in Figure 6, at a charging cutoff voltage of 4.6V and a charge / discharge rate of 1C, the capacity retention after 600 cycles is 84%, and the discharge capacity is approximately 168.9 mAh / g. This indicates that the polymer-based solid electrolyte can withstand high voltages.

[0079] Third, replace the above positive electrode with lithium nickel cobalt manganese oxide (LiNi). 0.8 Co 0.1 Mn 0.1 O2(NCM811) was used to assemble a solid-state battery, namely Li||NCM811 battery, according to the above steps. The electrochemical performance was characterized using a CT2001A battery testing system. The results are shown in Figure 7. At a charging cutoff voltage of 4.7V and a charge / discharge rate of 1C, the capacity retention rate after 200 cycles was 79.3%, and the discharge capacity was approximately 153.9mAh / g.

[0080] In summary, the solid-state battery prepared in this embodiment can maintain a good capacity retention rate during long-term charge and discharge at a cutoff voltage of 4.5V or higher, which also demonstrates that the polymer-based solid electrolyte is resistant to high voltage.

[0081] Fourth, the solid-state battery (Li||LCO battery) with the above positive electrode as lithium cobalt oxide (LCO) was charged and discharged for 10 cycles, and then the positive electrode of the battery was tested by X-ray photoelectron spectroscopy (XPS).

[0082] The X-ray photoelectron spectroscopy (XPS) instrument used is the AXIS Ultra DLD-600W instrument from Shimadzu Corporation of Japan, with a voltage of 15kV and a beam current of 15mA.

[0083] The test results are shown in Figures 8 and 9. The peak division of N in Figure 8 indicates that the -CN group in the polymer monomer used is indeed related to the Co in the positive electrode. 3+ Coordination occurred, which forms a stable positive electrode interface. The peak fractionation of F in Figure 9 indicates that the formed positive electrode interface contains LiF. LiF has high mechanical properties and chemical stability, which can effectively protect the positive electrode side and reduce side reactions caused by solvent decomposition.

[0084] Fifth, the cycle capacity retention of the solid-state battery (Li||LCO battery) with lithium cobalt oxide (LCO) as the cathode was tested. The capacity retention was tested after 500 cycles at a voltage of 3-4.5V and a charge / discharge rate of 0.5C, and the results are shown in Figure 10. The capacity retention was tested after 300 cycles at a voltage of 3-4.6V and a charge / discharge rate of 0.5C, and the results are shown in Figure 11.

[0085] Example 3

[0086] This embodiment describes the preparation of a solid-state battery containing a high-voltage resistant polymer-based solid electrolyte.

[0087] Preparation of the electrolyte precursor: Fluoroethylene carbonate (FEC) and dimethyl sulfite (DMS) were mixed in a mass ratio of 1:4. Then, 2-cyanoethyl acrylate (CA) and 2% (by mass) of crosslinking agent ethoxylated trimethylolpropane triacrylate were added to the solvent in a mass ratio of 1:4 to the solvent. The mixture was stirred at 30°C for about 2 hours to obtain a mixed solution. Then, lithium difluorooxalate borate (LiDFOB) was added to the mixed solution at a mass ratio of 2 mol / L and stirred at 30°C for about 2 hours until completely dissolved, finally yielding a homogeneous polymer-based solid electrolyte precursor.

[0088] Preparation of polymer-based solid electrolyte and assembly of solid-state battery: 1% by mass of azobisisobutyronitrile (AIBN) initiator was added to the electrolyte precursor obtained above to form a liquid precursor to be polymerized. 15 μL of the liquid precursor to be polymerized was dropped onto a lithium cobalt oxide (LCO) positive electrode, and then a polypropylene separator was placed on top. Another 15 μL of the liquid precursor to be polymerized was added to wet the separator. Then, a negative electrode lithium metal sheet, a gasket, and a spring were stacked. Finally, the assembled battery was placed in a heating device and heated at 60°C for 2 hours to allow CA to polymerize and form a high-voltage resistant polymer-based solid electrolyte. Simultaneously, an integrated stack including a positive electrode, electrolyte, separator, and negative electrode was formed in situ. Finally, the battery was encapsulated to obtain a solid-state battery.

[0089] Electrochemical performance was characterized using a CT-4008Tn-mA battery testing system. The results showed that the solid-state battery retained 88% of its capacity after 600 cycles at a charging cutoff voltage of 4.6V and a charge / discharge rate of 1C, with a discharge capacity of approximately 171.9mAh / g.

[0090] Example 4

[0091] This embodiment demonstrates the preparation of a solid-state battery containing a polymer-based solid-state electrolyte.

[0092] Preparation of the electrolyte precursor: Fluoroethylene carbonate (FEC) and dimethyl sulfite (DMS) were mixed in a mass ratio of 1:4. Then, 2-cyanoethyl acrylate (CA) and 2% (by mass) of crosslinking agent ethoxylated trimethylolpropane triacrylate were added to the solvent in a mass ratio of 7:20. The mixture was stirred at 30°C for about 2 hours to obtain a mixed solution. Then, lithium difluorooxalate borate (LiDFOB) was added to the mixed solution at a mass of 2 mol / L and stirred at 30°C for about 2 hours until completely dissolved, finally yielding a homogeneous polymer-based solid electrolyte precursor.

[0093] Preparation of polymer-based solid electrolyte and assembly of solid-state battery: 1% by mass of azobisisobutyronitrile (AIBN) initiator was added to the electrolyte precursor obtained above to form a liquid precursor to be polymerized. 15 μL of the liquid precursor to be polymerized was dropped onto a lithium cobalt oxide (LCO) positive electrode, and then a polypropylene separator was placed on top. Another 15 μL of the liquid precursor to be polymerized was added to wet the separator. Then, a negative electrode lithium metal sheet, a gasket, and a spring were stacked. Finally, the assembled battery was placed in a heating device and heated at 60°C for 2 hours to allow CA to polymerize and form a high-voltage resistant polymer-based solid electrolyte. Simultaneously, an integrated stack including a positive electrode, electrolyte, separator, and negative electrode was formed in situ. Finally, the battery was encapsulated to obtain a solid-state battery.

[0094] Electrochemical performance was characterized using a CT-4008Tn-mA battery testing system. The results showed that the solid-state battery retained 85% of its capacity after 200 cycles at a charging cutoff voltage of 4.7V and a charge / discharge rate of 1C, with a discharge capacity of approximately 170.3mAh / g.

[0095] Example 5

[0096] This embodiment demonstrates the preparation of a solid-state battery containing a polymer-based solid-state electrolyte.

[0097] Preparation of the electrolyte precursor: Fluoroethylene carbonate (FEC) and diethyl sulfite were mixed in a mass ratio of 1:4; then, 2-cyanoethoxyethyl acrylate and 2% (by mass) of trimethylolpropane triacrylate, a crosslinking agent, were added to the solvent in a mass ratio of 1:10 to the solvent. The mixture was stirred at 30°C for about 2 hours to obtain a mixed solution; then, lithium bis(fluorosulfonyl)imide lithium salt was added to the mixed solution at a rate of 2 mol / L, and the mixture was stirred at 30°C for about 2 hours until completely dissolved, finally obtaining a homogeneous polymer-based solid electrolyte precursor.

[0098] Preparation of polymer-based solid electrolyte and assembly of solid-state battery: Azobisisobutyronitrile (AIBN) initiator (0.5% by mass) was added to the electrolyte precursor obtained above to form a liquid precursor to be polymerized. 15 μL of the liquid precursor to be polymerized was dropped onto lithium nickel cobalt manganese oxide (LiNi). 0.8 Co 0.1 Mn 0.1 On the O2 (NCM811) positive electrode, a polypropylene separator is placed on top, and then 15 μL of the liquid precursor to be polymerized is added to wet the separator. Then, a negative electrode lithium metal sheet, a gasket, and a spring are stacked on top. Finally, the assembled battery is moved to a heating device and heated at 45°C for 8 hours to allow 2-cyanoethoxyethyl acrylate to polymerize and form a high-voltage resistant polymer-based solid electrolyte. At the same time, an integrated stack including a positive electrode, electrolyte, separator, and negative electrode is formed in situ. Finally, the battery is encapsulated to obtain a solid-state battery.

[0099] Example 6

[0100] This embodiment demonstrates the preparation of a solid-state battery containing a polymer-based solid-state electrolyte.

[0101] Preparation of the electrolyte precursor: Fluoroethylene carbonate (FEC) and propylene carbonate were mixed in a mass ratio of 1:4; propyl 2-cyanoacrylate and pentaerythritol tetraacrylate (1% by mass of the polymer monomer) were added to the solvent in a mass ratio of 1:10; the mixture was stirred at 30°C for about 2 hours to obtain a mixed solution; lithium bis(fluorosulfonyl)imide was then added to the mixed solution at a mass ratio of 0.5 mol / L; the mixture was stirred at 30°C for about 2 hours until completely dissolved, finally yielding a homogeneous polymer-based solid electrolyte precursor.

[0102] Preparation of polymer-based solid electrolyte and assembly of solid-state battery: Azobisisobutyronitrile (AIBN) initiator (0.2% by mass) was added to the electrolyte precursor obtained above to form a liquid precursor to be polymerized. 15 μL of the liquid precursor to be polymerized was dropped onto lithium nickel cobalt manganese oxide (LiNi). 0.8 Co 0.1 Mn 0.1 On the O2 (NCM811) positive electrode, a polypropylene separator is placed on top, and then 15 μL of the liquid precursor to be polymerized is added to wet the separator. Then, a negative electrode lithium metal sheet, a gasket, and a spring are stacked on top. Finally, the assembled battery is moved to a heating device and heated at 50°C for 5 hours to allow propyl 2-cyanoacrylate to polymerize and form a high-voltage resistant polymer-based solid electrolyte. At the same time, an integrated stack including a positive electrode, electrolyte, separator, and negative electrode is formed in situ. Finally, the battery is encapsulated to obtain a solid-state battery.

[0103] Comparative Example 1

[0104] This comparative example prepared an electrolyte that does not contain polymer monomers.

[0105] Preparation of electrolyte: Fluoroethylene carbonate (FEC) and dimethyl sulfite (DMS) were mixed in a mass ratio of 1:4 and stirred at 30°C for about 2 hours; then lithium difluorooxalate borate (LiDFOB) was added to the solvent at a rate of 1 mol / L and stirred at 30°C for about 2 hours until completely dissolved, finally obtaining a homogeneous electrolyte.

[0106] Subsequently, relevant tests were conducted using the electrolyte prepared above:

[0107] First, assemble a semi-blocking battery and test the electrochemical window:

[0108] A semi-blocking battery was assembled using a stainless steel gasket as the working electrode and lithium metal as the reference electrode, and linear sweep voltammetry (LSV) was performed. The test was conducted at a sweep rate of 1 mV / s from the open circuit voltage to the termination voltage of 7 V. The test equipment was a Gamry electrochemical workstation Interface 1000. The results are shown in Figure 3.

[0109] Second, assemble the button cells and conduct relevant tests:

[0110] Add 1% by mass of azobisisobutyronitrile (AIBN) initiator to the electrolyte obtained above to form a liquid precursor to be polymerized. Take 15 μL of the liquid precursor to be polymerized and drop it onto the lithium cobalt oxide (LCO) positive electrode, then cover it with a polypropylene separator, and add another 15 μL of the liquid precursor to be polymerized to wet the separator. Then, stack the negative electrode lithium metal sheet, gasket, and spring sheet. Finally, transfer the assembled battery to a heating device and heat it at 60°C for 2 hours to form a coin cell including a positive electrode, electrolyte, separator, and negative electrode.

[0111] First, the leakage current of the button cell was tested using the timed current method: the cell was charged to 4.2V, 4.3V, 4.4V, 4.5V, 4.6V, 4.7V, 4.8V, 4.9V and 5.0V and held at each voltage for 3 hours. The leakage current of the cell was observed to evaluate the actual oxidation stability of the electrolyte. The results are shown in Figure 4.

[0112] Secondly, the cycle capacity retention of the coin cells was tested. The capacity retention was tested after 500 cycles at a voltage of 3-4.5V and a charge / discharge rate of 0.5C, and the results are shown in Figure 10. The capacity retention was tested after 300 cycles at a voltage of 3-4.6V and a charge / discharge rate of 0.5C, and the results are shown in Figure 11.

[0113] The results of the same tests conducted in Example 2 and Comparative Example 1 were analyzed as follows:

[0114] Comparing Figures 2 and 3, it can be seen that the electrochemical window of the high-voltage resistant polymer-based solid electrolyte in Example 1 reaches 5.1V, while the electrochemical window of the electrolyte in Comparative Example 1 is 4.6V, which is lower than the electrochemical window of the polymer-based solid electrolyte in Example 1 of this application. This indicates that the high-voltage resistant polymer-based solid electrolyte in Example 1 of this application has a wider electrochemical window. This is because the polymer-based solid electrolyte contains polar functional groups such as cyano groups and fluorinated groups, which increase the oxidation potential of the electrolyte.

[0115] As shown in Figure 4, the solid-state battery of Example 1 of this invention, even when charged to 5V (total time in the figure is 27 hours), exhibits a leakage current of 33.3 μA, indicating that the polymer-based solid electrolyte has good oxidation stability. In contrast, the coin cell battery of Comparative Example 1, when charged to 4.7V, shows a leakage current of 70.5 μA, indicating that the oxidation stability of its electrolyte is only moderate. In summary, the oxidation stability of the electrolyte in Comparative Example 1 is far lower than that of the high-voltage resistant polymer-based solid electrolyte of Example 2 of this invention. It should be noted that Example 2 involves polymerizing the polymer-based solid electrolyte precursor of Example 1 in a battery system to obtain the polymer-based solid electrolyte, followed by relevant tests on the solid-state battery. The composition and properties of the polymer-based solid electrolyte in Example 2 are the same as those in Example 1.

[0116] As shown in Figure 10, the solid-state battery of Embodiment 2 of the present invention retains 98.4% of its capacity after 500 cycles, while the semi-blocking battery of Comparative Example 1 has reduced its capacity retention to 67.3% after 350 cycles. As shown in Figure 11, the solid-state battery of Embodiment 2 of the present invention retains 80.91% of its capacity after 300 cycles, while the coin cell battery of Comparative Example 1 begins to decline in capacity retention after 120 cycles, and the capacity retention drops to 67.3% after 175 cycles. This demonstrates that the solid-state battery of this application maintains a high capacity retention even after prolonged charge-discharge cycles at high voltage (≥4.5V).

[0117] This invention prepares a polymer-based solid electrolyte suitable for high voltage resistance by screening polymer monomers and solvents and optimizing precursor ratios using an in-situ polymerization process.

[0118] The high-voltage resistant polymer-based solid electrolyte prepared by this invention exhibits good physicochemical properties and electrochemical performance under a charging cutoff voltage of ≥4.5V, and can be applied to lithium batteries, showing good application prospects.

[0119] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a high-voltage resistant polymer-based solid electrolyte, characterized in that, The preparation method includes: Lithium salt, polymer monomer, crosslinking agent, and solvent are mixed uniformly in a certain proportion to obtain a polymer-based solid electrolyte precursor; wherein, the polymer monomer includes cyanoacrylate monomers; An initiator is added to the polymer-based solid electrolyte precursor, and then thermal polymerization is carried out to obtain a polymer-based solid electrolyte with polar functional groups of cyano groups, which is the high-voltage resistant polymer-based solid electrolyte.

2. The preparation method according to claim 1, characterized in that, The mass ratio of the polymer monomer to the solvent is 1:10-10:1; the mass of the crosslinking agent is 0.5%-3% of the mass of the polymer monomer; and the concentration of the lithium salt in the polymer-based solid electrolyte precursor is 0.5mol / L-2mol / L.

3. The preparation method according to claim 1, characterized in that, The mass of the initiator is no more than 1% of the mass of the polymer-based solid electrolyte precursor.

4. The preparation method according to claim 1, characterized in that, The thermal polymerization temperature is 45℃-80℃, and the time is 1 hour-24 hours.

5. The preparation method according to claim 1, characterized in that, The lithium salt includes one or more of lithium difluorooxalate borate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium difluorooxalate phosphate. The cyanoacrylate monomers include one or more of the following: 2-cyanoethyl acrylate, acrylonitrile, 2-ethyl cyanoacrylate, 2-cyanoethoxyethyl acrylate, cyanoethyl isobutylenoate, ethyl cyanoacrylate, propyl cyanoacrylate, pentyl cyanoacrylate, 3-amino-2-butenoic acid cyanoacetic acid, and ethyl 2-cyano-3-methylbutenoate. The solvent includes carbonate compounds and / or sulfite compounds; the carbonate compounds include one or more of the following: dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, ethylene carbonate, propylene carbonate, and fluoroethylene carbonate; The sulfite compounds include one or more of the following: dimethyl sulfite, dimethyl sulfate, diethyl sulfite, ethyl sulfite, and propylene sulfite; The crosslinking agent is an acrylate compound, which includes one or more of the following: ethoxylated trimethylolpropane triacrylate, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and pentaerythritol triacrylate.

6. The preparation method according to claim 1, characterized in that, The initiator is a free radical initiator; the free radical initiator includes one or more of azobisisobutyronitrile, azobisisoheptanenitrile, and benzoyl peroxide.

7. A high-voltage resistant polymer-based solid electrolyte, characterized in that, The high-voltage resistant polymer-based solid electrolyte is prepared by any of the preparation methods described in claims 1-6.

8. A solid-state battery, characterized in that, The solid-state battery includes the high-voltage resistant polymer-based solid electrolyte as described in claim 7.

9. The solid-state battery according to claim 8, characterized in that, The positive electrode active material of the solid-state battery includes one or two of layered oxides and polyanionic compounds; the layered oxides include one or two of lithium cobalt oxide and lithium nickel cobalt manganese oxide; the polyanionic compounds include lithium iron phosphate; and the negative electrode active material includes any one of graphite and lithium metal sheets.

10. A method for preparing a solid-state battery according to claim 8, characterized in that, The preparation method includes: Lithium salt, polymer monomer, crosslinking agent, and solvent are mixed uniformly in a certain proportion to obtain a polymer-based solid electrolyte precursor; wherein, the polymer monomer includes cyanoacrylate monomers; An initiator is added to the polymer-based solid electrolyte precursor to obtain a liquid precursor to be polymerized; The liquid precursor to be polymerized is injected into the space between the positive and negative electrodes inside the battery to be assembled, so that the liquid precursor to be polymerized fully wets the positive electrode, negative electrode and separator, and then the battery is encapsulated; or, the liquid precursor to be polymerized is dropped onto the positive electrode, negative electrode and separator of the battery to be assembled, and then the battery is encapsulated. The battery is subjected to heat treatment to obtain the solid-state battery.