Epitaxial structure of semiconductor laser and preparation method therefor
By optimizing the composition and thickness of each layer of materials in the epitaxial structure, especially by adjusting the content of aluminum, gallium and indium in the barrier layer, the problem of insufficient carrier confinement was solved, the output efficiency and high-temperature performance of the semiconductor laser were improved, and it is suitable for mass production.
Patent Information
- Application Number
- PCT/CN2025/111154
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2025-07-29
- Publication Date
- 2026-11-12
AI Technical Summary
In the epitaxial structure design of semiconductor laser chips, the carrier confinement is not high, resulting in limited improvement in output efficiency. Furthermore, the lattice matching of the epitaxial structure is poor, making it unsuitable for large-scale, mass production.
By adjusting the material composition and thickness of each layer in the epitaxial structure, especially by adjusting the content of aluminum, gallium and indium in the first and second barrier layers, the aluminum content of the first waveguide layer, the first barrier layer, the second barrier layer and the second waveguide layer is optimized to ensure that the conduction band and valence band difference reaches a specific value, thereby balancing the confinement effect on electrons and holes and forming a better lattice match.
It achieves the optimal state of carrier confinement capability, improves the output efficiency of semiconductor lasers and the output power and electro-optic conversion efficiency at high temperature power, and is suitable for large-scale, mass production.
Smart Images

Figure CN2025111154_12112026_PF_FP_ABST
Abstract
Description
Epitaxial Structure and Fabrication Method of Semiconductor Lasers
[0001] Cross-references to related applications
[0002] This disclosure claims priority to Chinese Patent Application No. 2025105937184, filed on May 9, 2025, entitled "Epipolar Structure of Semiconductor Laser and Preparation Method Thereof", the entire contents of which are incorporated herein by reference. Technical Field
[0003] This disclosure relates to the field of semiconductor technology, and in particular to an epitaxial structure of a semiconductor laser and its fabrication method. Background Technology
[0004] In the epitaxial structure design of semiconductor laser chips, a design method is adopted to insert a thin high-bandgap carrier blocking layer between low-bandgap waveguide layers to confine carriers (especially electrons) within the quantum well as much as possible. However, in the current process of adjusting the epitaxial structure design, the degree of carrier confinement is often insufficient, and the output efficiency of semiconductor lasers cannot be significantly improved. Summary of the Invention
[0005] In view of this, the present disclosure provides an epitaxial structure of a semiconductor laser and a method for fabricating the same. The epitaxial structure design of the semiconductor laser disclosed herein can balance the confinement of electrons and holes, so that the confinement capability of the epitaxial structure for charge carriers reaches the optimal state, and the output efficiency of the semiconductor laser is greatly improved. At the same time, the lattice matching state between the layers of the epitaxial structure is good, which is suitable for large-scale, batch production.
[0006] The technical solution provided in this disclosure is as follows:
[0007] In a first aspect, embodiments of this disclosure provide an epitaxial structure for a semiconductor laser, comprising: a first waveguide layer, a first barrier layer, a first potential barrier layer, a quantum well layer, a second potential barrier layer, a second barrier layer, and a second waveguide layer stacked from bottom to top.
[0008] The first conduction band difference ΔEc11 between the second blocking layer and the second barrier layer is greater than 70 meV, the second valence band difference ΔEv21 between the first blocking layer and the first barrier layer is greater than 240 meV, the first valence band difference ΔEv11 between the second blocking layer and the second waveguide layer is equal to a meV, and the second conduction band difference ΔEc21 between the first blocking layer and the first waveguide layer is equal to b meV, where a ≤ 0 and b ≤ 0.
[0009] In one optional embodiment, the aluminum content in the first waveguide layer is greater than the aluminum content in the first barrier layer; and the aluminum content in the second waveguide layer is greater than the aluminum content in the second barrier layer.
[0010] In an optional embodiment, the first waveguide layer is Al. x2 Ga 1-x2 As, 0.2≤x2≤0.4;
[0011] The first barrier layer is Ga x3 In 1-x3 P, x3≥0.55;
[0012] The first barrier layer is Al x4 Ga 1-x4 As, 0.05≤x4≤0.20;
[0013] The second barrier layer is Al x6 Ga 1-x6 As, 0.05≤x6≤0.20;
[0014] The second barrier layer is Al x7 Ga y7 In 1-x7-y7 As, 1-x7-y7<0.2, 0.25≤x7≤0.45;
[0015] The second waveguide layer is Al x8 Ga 1-x8 As, 0.20≤x8≤0.30.
[0016] In an optional embodiment, the epitaxial structure of the semiconductor laser further includes: a first confinement layer disposed below the first waveguide layer and a second confinement layer disposed above the second waveguide layer;
[0017] The first confinement layer is A1 x1 Ga 1-x1 As, 0.25≤x1≤0.80;
[0018] The quantum well layer is In x5 Ga 1-x5 As, 0 ≤ x5 ≤ 0.25;
[0019] The second confinement layer is Al x9 Ga 1-x9 As, 0.35≤x9≤0.90.
[0020] In one optional embodiment, the thickness of the first confinement layer is 1.5-3 micrometers, the thickness of the first waveguide layer is 0.3-1.5 micrometers, the thickness of the first barrier layer is 0.004-0.030 micrometers, the thickness of the first potential barrier layer is 0.003-0.060 micrometers, the thickness of the quantum well layer is 0.006-0.010 micrometers, the thickness of the second potential barrier layer is 0.003-0.060 micrometers, the thickness of the second barrier layer is 0.004-0.030 micrometers, the thickness of the second waveguide layer is 0.3-1.0 micrometers, and the thickness of the second confinement layer is 0.5-2 micrometers.
[0021] In an optional embodiment, the first waveguide layer is Al. m1 Ga n1 In 1-m1-n1 As, 0.25≤m1≤0.45, 0.05≤n1≤0.20;
[0022] The first barrier layer is Ga m2 In 1-m2 P, 0.60≤m2≤0.85;
[0023] The first barrier layer is Al m3 Ga n3 In 1-m3-n3 As, 0.20≤m3≤0.40, 0.10≤n3≤0.25;
[0024] The second barrier layer is Al m5 Ga n5 In 1-m5-n5 As, 0.20≤m5≤0.40, 0.10≤n5≤0.25;
[0025] The second barrier layer is Al m6 In 1-m6 As, 0.45≤m6≤0.60;
[0026] The second waveguide layer is Al m7 Ga n7 In 1-m7-n7 As, 0.35≤m7≤0.50, 0.10≤n7≤0.20.
[0027] In an optional embodiment, the epitaxial structure of the semiconductor laser further includes: a first confinement layer disposed below the first waveguide layer and a second confinement layer disposed above the second waveguide layer;
[0028] The quantum well layer is Al. m4 Ga n4 In 1-m4-n4As, 0.02≤m4≤0.10, 0.30≤n4≤0.50;
[0029] Both the first and second confinement layers are InP.
[0030] In one optional embodiment, the thickness of the first confinement layer is 1.5-3 micrometers, the thickness of the first waveguide layer is 0.3-1.5 micrometers, the thickness of the first barrier layer is 0.004-0.030 micrometers, the thickness of the first potential barrier layer is 0.003-0.060 micrometers, the thickness of the quantum well layer is 0.006-0.012 micrometers, the thickness of the second potential barrier layer is 0.003-0.060 micrometers, the thickness of the second barrier layer is 0.004-0.030 micrometers, the thickness of the second waveguide layer is 0.1-1.0 micrometers, and the thickness of the second confinement layer is 0.5-2.5 micrometers.
[0031] Secondly, embodiments of this disclosure also provide a method for fabricating an epitaxial structure of a semiconductor laser, comprising:
[0032] A first waveguide layer, a first barrier layer, a first potential barrier layer, a quantum well layer, a second potential barrier layer, a second barrier layer, and a second waveguide layer are grown and stacked on a substrate.
[0033] During the growth of the first waveguide layer, the first barrier layer, the first potential barrier layer, the second potential barrier layer, the second barrier layer, and the second waveguide layer: the contents of aluminum and gallium in the first waveguide layer, the first potential barrier layer, the second potential barrier layer, and the second waveguide layer are adjusted; the contents of gallium and indium in the first barrier layer are adjusted; and the contents of aluminum and indium in the second barrier layer are adjusted, so that the first conduction band difference ΔEc11 between the second barrier layer and the second potential barrier layer is >70meV, the second valence band difference ΔEv21 between the first barrier layer and the first potential barrier layer is >240meV, the first valence band difference ΔEv11 between the second barrier layer and the second waveguide layer is ΔEv11 = a meV, and the second conduction band difference ΔEc21 between the first barrier layer and the first waveguide layer is ΔEc21 = b meV, where a≤0 and b≤0.
[0034] In one optional embodiment, the first confining layer is an AlGaAs material;
[0035] The first waveguide layer is made of AlGaAs material;
[0036] The first barrier layer is made of GaInP material;
[0037] The first barrier layer is made of AlGaAs material;
[0038] The quantum well layer is made of InGaAs material;
[0039] The second barrier layer is made of AlGaAs material;
[0040] The second barrier layer is made of AlGaInAs material;
[0041] The second waveguide layer is made of AlGaAs material;
[0042] The second confinement layer is made of AlGaAs material.
[0043] In an alternative embodiment, during the growth of the first waveguide layer Al x2 Ga 1-x2 When using As, the growth thickness is controlled between 0.5 and 1.5 μm, and the growth rate is between 0.1 and 0.7 nm / s, wherein the Al content range satisfies: 0.2 ≤ x2 ≤ 0.4.
[0044] During the growth of the first barrier layer Al x4 Ga 1-x4 When using As, the growth thickness is controlled between 0.003 and 0.060 μm, and the growth rate is between 0.02 and 0.1 nm / s, wherein the Al content range satisfies: 0.05 ≤ x4 ≤ 0.20;
[0045] During the growth of the second barrier layer Al x6 Ga 1-x6 When using As, the growth thickness is controlled between 0.003 and 0.060 μm, and the growth rate is between 0.02 and 0.1 nm / s, wherein the Al content range satisfies: 0.05 ≤ x6 ≤ 0.20;
[0046] During the growth of the second waveguide layer Al x8 Ga 1-x8 When using As, the growth thickness is controlled between 0.3 and 1.0 μm, the growth rate is between 0.1 and 0.7 nm / s, and the Al content range satisfies: 0.20 ≤ x8 ≤ 0.30.
[0047] In one alternative embodiment, it includes:
[0048] During the growth of the first barrier layer Ga x3 In 1-x3 When P is used, the growth thickness is controlled between 0.004 μm and 0.020 μm, the growth rate is between 0.02 and 0.1 nm / s, and the In content range satisfies: x3 ≥ 0.55; after the first barrier layer has grown, the injection of the reaction source is stopped for 15-20 seconds, and the temperature in the chamber is kept constant.
[0049] as well as,
[0050] During the growth of the second barrier layer Al x7Ga y7 In 1-x7-y7 When As is used, the growth thickness is controlled between 0.004 μm and 0.030 μm, the growth rate is between 0.02 and 0.1 nm / s, and the In content range satisfies: 1 - x⁷ - y⁷ < 0.2; the second barrier layer Al x7 Ga y7 In 1-x7-y7 After As growth is complete, stop injecting the reaction source for 15-20 seconds and keep the temperature inside the chamber constant.
[0051] In one alternative embodiment, it includes:
[0052] When forming the first barrier layer, the growth temperature is selected as 680℃-750℃, the growth thickness is controlled at 0.003~0.060μm, and the growth rate is 0.02~0.1nm / s;
[0053] When forming the second barrier layer, the growth temperature is selected as 680℃-750℃, the growth thickness is controlled at 0.003~0.060μm, and the growth rate is 0.02~0.1nm / s.
[0054] In an alternative embodiment, when performing quantum well layer In x5 Ga 1-x5 During As deposition, the deposition temperature in the chamber is controlled to be reduced to 580-640℃, the growth thickness is controlled to be 0.006-0.01μm, and the growth rate is 0.02-0.1nm / s, wherein the In content satisfies: 0≤x5≤0.25;
[0055] After the quantum well layer is formed, the reaction source is stopped for 15-20 seconds, and the temperature is kept constant.
[0056] In an optional embodiment, the epitaxial structure of the semiconductor laser further includes: a first confinement layer disposed below the first waveguide layer and a second confinement layer disposed above the second waveguide layer;
[0057] The first waveguide layer is Al m1 Ga n1 In 1-m1-n1 As, 0.25≤m1≤0.45, 0.05≤n1≤0.20;
[0058] The first barrier layer is Ga m2 In 1-m2 P, 0.60≤m2≤0.85;
[0059] The first barrier layer is Al m3 Ga n3 In 1-m3-n3As, 0.20≤m3≤0.40, 0.10≤n3≤0.25;
[0060] The quantum well layer is Al m4 Ga n4 In 1-m4-n4 As, 0.02≤m4≤0.10, 0.30≤n4≤0.50;
[0061] The second barrier layer is Al m5 Ga n5 In 1-m5-n5 As, 0.20≤m5≤0.40, 0.10≤n5≤0.25;
[0062] The second barrier layer is Al m6 In 1-m6 As, 0.45≤m6≤0.60;
[0063] The second waveguide layer is Al m7 Ga n7 In 1-m7-n7 As, 0.35≤m7≤0.50, 0.10≤n7≤0.20;
[0064] Both the first and second confinement layers are InP.
[0065] In an alternative embodiment, during the growth of the first waveguide layer Al m1 Ga n1 In 1-m1-n1 When using As, the growth thickness is controlled between 0.3 and 1.5 μm, and the growth rate is between 0.05 and 0.8 nm / s. The content ranges of Al and Ga satisfy: 0.25 ≤ m1 ≤ 0.45 and 0.05 ≤ n1 ≤ 0.20.
[0066] During the growth of the first barrier layer Ga m2 In 1-m2 When P is used, the growth thickness is controlled between 0.004 μm and 0.030 μm, the growth rate is between 0.02 and 0.8 nm / s, and the In content range meets the following: 0.60 ≤ m2 ≤ 0.85. After the first barrier layer has grown, the injection of the reaction source is stopped for 15-20 seconds, and the temperature in the chamber is kept constant.
[0067] During the growth of the first barrier layer Al m3 Ga n3 In 1-m3-n3 When using As, the growth thickness is controlled between 0.003 and 0.060 μm, and the growth rate is between 0.02 and 0.8 nm / s. The content ranges of Al and Ga satisfy: 0.20 ≤ m3 ≤ 0.40 and 0.10 ≤ n3 ≤ 0.25.
[0068] In the process of quantum well layer Al m4 Ga n4 In 1-m4-n4 During As deposition, the deposition temperature in the chamber is controlled to be reduced to 580-700℃, the growth thickness is controlled to be 0.006-0.012μm, and the growth rate is 0.02-0.1nm / s. The contents of Al and Ga satisfy the following conditions: 0.02≤m4≤0.10 and 0.30≤n4≤0.50. After the quantum well layer is formed, the reaction source is stopped for 15-20 seconds, and the temperature is kept constant.
[0069] During the growth of the second barrier layer Al m5 Ga n5 In 1-m5-n5 When using As, the growth thickness is controlled between 0.003 and 0.060 μm, and the growth rate is between 0.02 and 0.8 nm / s. The content ranges of Al and Ga satisfy: 0.20 ≤ m5 ≤ 0.40 and 0.10 ≤ n5 ≤ 0.25.
[0070] During the growth of the second barrier layer Al m6 In 1-m6 When As is grown, the growth thickness is controlled between 0.004 μm and 0.030 μm, the growth rate is between 0.02 and 0.8 nm / s, and the Al content range meets the following: 0.45 ≤ m6 ≤ 0.60. After the second barrier layer has grown, the injection of the reaction source is stopped for 15-20 seconds, and the temperature in the chamber is kept constant.
[0071] During the growth of the second waveguide layer Al m7 Ga n7 In 1-m7-n7 When using As, the growth thickness is controlled between 0.1 and 1.0 μm, the growth rate is between 0.05 and 0.8 nm / s, and the content ranges of Al and Ga satisfy: 0.35 ≤ m7 ≤ 0.50 and 0.10 ≤ n7 ≤ 0.20.
[0072] In one alternative embodiment, it includes:
[0073] When forming the first barrier layer, the growth temperature is selected as 630℃-750℃, the growth thickness is controlled at 0.003~0.060μm, and the growth rate is 0.02~0.8nm / s;
[0074] When forming the second barrier layer, the growth temperature is selected as 630℃-750℃, the growth thickness is controlled at 0.003~0.060μm, and the growth rate is 0.02~0.8nm / s.
[0075] The epitaxial structure design of the semiconductor laser provided in this disclosure effectively balances the confinement of electrons and holes, optimizing the carrier confinement capability and significantly improving the output efficiency of the semiconductor laser. Simultaneously, the adaptive adjustment of the indium content in the first blocking layer (hole blocking layer) and the second blocking layer (electron blocking layer), along with the adjustment of the aluminum and gallium content in the first waveguide layer, first barrier layer, second barrier layer, and second waveguide layer, ensures that the indium content remains within a suitable range. This results in good lattice matching between the layers in the epitaxial structure, making it suitable for large-scale, mass production. Furthermore, the improved temperature characteristics and higher internal quantum efficiency of the semiconductor laser design in this embodiment contribute to achieving higher output power, particularly with significant improvements in output power and electro-optical conversion efficiency under high-temperature power conditions, greatly expanding the application directions of semiconductor lasers.
[0076] To make the above-mentioned objects, features and advantages of this disclosure more apparent and understandable, preferred embodiments are described below in detail with reference to the accompanying drawings. Attached Figure Description
[0077] To more clearly illustrate the technical solutions of the embodiments of this disclosure, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of this disclosure and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0078] Figure 1 is a schematic diagram of the energy band structure of a typical epitaxial structure with a carrier blocking layer;
[0079] Figure 2 is a schematic diagram of the energy band structure of an epitaxial structure provided in an embodiment of this disclosure;
[0080] Figure 3 is a schematic diagram of the energy band structure of an epitaxial structure provided in another embodiment of this disclosure;
[0081] Figure 4 shows the substrate and buffer layer, and the epitaxial structure of the semiconductor laser grown thereon, provided in one embodiment of this disclosure.
[0082] Reference numerals: N-type confinement layer 01, N-type waveguide layer 02, N-type hole blocking layer 03, N-type barrier layer 04, quantum well 05, P-type barrier layer 06, P-type electron blocking layer 07, P-type waveguide layer 08, P-type confinement layer 09, substrate 1, buffer layer 10, epitaxial structure 100: first confinement layer 11, first waveguide layer 12, first barrier layer 13, first barrier layer 14, quantum well layer 15, second barrier layer 16, second barrier layer 17, second waveguide layer 18, second confinement layer 19, capping layer 20. Detailed Implementation
[0083] The technical solutions of the embodiments of this disclosure will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this disclosure, and not all embodiments. The components of the embodiments of this disclosure described and shown in the accompanying drawings can be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of this disclosure provided in the accompanying drawings is not intended to limit the scope of the claimed disclosure, but merely represents selected embodiments of this disclosure. All other embodiments obtained by those skilled in the art based on the embodiments of this disclosure without inventive effort are within the scope of protection of this disclosure. It should be noted that similar reference numerals and letters in the following drawings indicate similar items; therefore, once an item is defined in one drawing, it does not need to be further defined and explained in subsequent drawings. Furthermore, in the description of this disclosure, the terms "first," "second," etc., are used only to distinguish descriptions and should not be construed as indicating or implying relative importance.
[0084] Through a series of studies conducted by the applicant, it was found that: In the epitaxial structure design of semiconductor lasers, the typical bandgap design of GaAs / AlGaAs-based epitaxial structures with carrier blocking layers is shown in Figure 1. From left to right, they are the N-region formed by N-type doping, the quantum well 05 (QW), and the P-region formed by P-type doping. The N-region includes an N-type confinement layer 01, an N-type waveguide layer 02, an N-type hole blocking layer 03, and an N-type barrier layer 04 (also called a waveguide layer). The N-type barrier layer 04 generally has the same composition as the N-type waveguide layer 02. The quantum well 05 (QW) can be made of GaAs, InGaAs, or InAlGaAs materials. The required bandgap needs to be designed according to different wavelength requirements, while considering the influence of quantum well strain on gain and growth quality, and selecting a suitable quantum well material. The P-region includes a P-type barrier layer 06 (also called a waveguide layer), a P-type electron blocking layer 07, a P-type waveguide layer 08, and a P-type confinement layer 09. The P-type confinement layer 09 generally has the same composition as the P-type barrier layer 06.
[0085] As shown in Figure 1, the typical epitaxial bandgap design with a carrier blocking layer has two characteristics: the P-type electron blocking layer 07 restricts the movement of electrons from the N-region to the P-region, and also restricts the movement of holes from the P-region to the quantum well 05 to some extent; the N-type hole blocking layer 03 restricts the movement of holes from the P-region to the N-region, and also restricts the movement of electrons from the N-region to the quantum well 05 to some extent. Therefore, it is necessary to balance the first conduction band difference ΔE between the P-type electron blocking layer 07 and the P-type barrier layer 06. c1 The first valence band difference ΔE between the P-type electron blocking layer 07 and the P-type waveguide layer 08 v1To improve the first conduction band difference ΔE c1 At the same time, it does not cause an excessively high first valence band difference ΔE v1 The objective is to simultaneously balance the second conduction band difference ΔE between the N-type hole blocking layer 03 and the N-type waveguide layer 02. c2 The second valence band difference ΔE between the N-type hole blocking layer 03 and the N-type barrier layer 04 v2 To increase the second valence band difference ΔE v2 At the same time, it does not cause an excessively high second conduction band difference ΔE c2 The purpose.
[0086] In addition, the applicant's research found that in the process of adjusting the proportion of each element in the epitaxial structure, it is not possible to simply pursue the band difference. It is also necessary to match the In content in the P-type electron blocking layer O7 and the N-type hole blocking layer O3 to avoid the In content being relatively high, which would prevent it from achieving a good matching state with the AlGaAs material, thus making the epitaxial material growth more difficult and unfavorable for large-scale, batch production.
[0087] Based on the above research conclusions, the applicant provides an epitaxial structure design as shown in Figures 2, 3, and 4. This epitaxial structure includes, from bottom to top, a first waveguide layer 12, a first barrier layer 13 (hole blocking layer), a first barrier layer 14, a quantum well layer 15, a second barrier layer 16, a second barrier layer 17 (electron blocking layer), and a second waveguide layer 18, stacked sequentially. In Figure 2, the first waveguide layer 12 is made of AlGaAs, the first barrier layer 13 (hole blocking layer) is made of GaInP, the first barrier layer 14 is made of AlGaAs, the quantum well layer 15 is made of InGaAs, the second barrier layer 16 is made of AlGaAs, the second barrier layer 17 (electron blocking layer) is made of AlGaInAs, and the second waveguide layer 18 is made of AlGaAs.
[0088] Referring to Figure 4, the epitaxial structure 100 can be formed on an N-type GaAs substrate or an InP substrate. A buffer layer 10 can be formed before forming the epitaxial structure 100 on the substrate 1. When forming the epitaxial structure 100 on the N-type substrate 1, the first confinement layer 11 is an N-type confinement layer, the first waveguide layer 12 is an N-type waveguide layer, the first barrier layer 13 is a hole blocking layer, the first barrier layer 14 is an N-type barrier layer, the quantum well layer 15, the second barrier layer 16 is a P-type barrier layer, the second barrier layer 17 is an electron blocking layer, the second waveguide layer 18 is a P-type waveguide layer, and the second confinement layer 19 is a P-type confinement layer.
[0089] In an optional embodiment, as shown in FIG2, an N-type epitaxial structure 100 is formed on a GaAs substrate, including a first confinement layer 11 below the first waveguide layer 12 and a second confinement layer 19 above the second waveguide layer 18. The first confinement layer 11 is made of AlGaAs material, the first waveguide layer 12 is made of AlGaAs material, the first barrier layer 13 is made of GaInP material, the first barrier layer 14 is made of AlGaAs material, the quantum well layer 15 is made of InGaAs material, the second barrier layer 16 is made of AlGaAs material, the second barrier layer 17 is made of AlGaInAs material, the second waveguide layer 18 is made of AlGaAs material, and the second confinement layer 19 is made of AlGaAs material.
[0090] The material combinations in the above embodiments are only typical and practically feasible alternatives. In other embodiments, the material combinations are variable; for example, the quantum well structure could also be an InAlGaAs structure.
[0091] By adjusting the contents of aluminum and gallium in the first waveguide layer 12, the first barrier layer 14, the second barrier layer 16, and the second waveguide layer 18, adjusting the contents of gallium and indium in the first blocking layer 13 (hole blocking layer), and adjusting the contents of aluminum, gallium, and indium in the second blocking layer 17 (electron blocking layer), the following conditions are met: the first conduction band difference ΔEc11 between the second blocking layer 17 (electron blocking layer) and the second barrier layer 16 is greater than 70 meV; the second valence band difference ΔEv21 between the first blocking layer 13 (hole blocking layer) and the first barrier layer 14 is greater than 240 meV; the first valence band difference ΔEv11 between the second blocking layer 17 (electron blocking layer) and the second waveguide layer 18 is equal to a meV; and the second conduction band difference ΔEc21 between the first blocking layer 13 (hole blocking layer) and the first waveguide layer 12 is equal to b meV, where a ≤ 0 and b ≤ 0.
[0092] In this embodiment, by first adjusting the content of aluminum and gallium in the second barrier layer 16 and the second waveguide layer 18, and then adjusting the content of aluminum, gallium, and indium in the second blocking layer 17 (electron blocking layer), a second blocking layer 17 (electron blocking layer) with stronger electron blocking effect can be obtained. Simultaneously, it ensures that holes in the valence band can smoothly pass through the second blocking layer 17 (electron blocking layer) into the quantum well layer 15 (first valence band difference ΔEv11≈0). As shown in Table 1 below, the stronger electron blocking effect is manifested in the fact that the first conduction band difference ΔEc11 between the second blocking layer 17 (electron blocking layer) and the second barrier layer 16 is >70meV, which is superior to the first conduction band difference in the prior art (ΔEc1≈60meV).
[0093] Table 1 shows the variations in elemental content and bandgap of the second barrier layer 16, the second blocking layer 17, and the second waveguide layer 18.
[0094] Similarly, by first adjusting the content of aluminum and gallium in the first waveguide layer 12 and the first barrier layer 14, and then adjusting the content of gallium and indium in the first blocking layer 13 (hole blocking layer), a first blocking layer 13 (hole blocking layer) with stronger hole blocking effect can be obtained. At the same time, it can be ensured that electrons in the conduction band can pass smoothly through the first blocking layer 13 (hole blocking layer) into the quantum well layer 15 (i.e., ensuring that the second conduction band difference ΔEc21≈0). As shown in Table 2 below, the stronger hole blocking effect is reflected in the fact that the second valence band difference ΔEv21 between the first blocking layer 13 (hole blocking layer) and the first barrier layer 14 is >240meV, which is better than the second valence band difference in the prior art (ΔEv2≈200meV).
[0095] Table 2 shows the variations in elemental content and bandgap of the first waveguide layer 12, the first barrier layer 13, and the first energy barrier layer 14.
[0096] Therefore, the epitaxial structure design of the semiconductor laser in this disclosure can effectively balance the confinement of electrons and holes, achieving optimal carrier confinement and significantly improving the output efficiency of the semiconductor laser. Simultaneously, the adjustment of gallium and indium content in the first blocking layer 13 (hole blocking layer) and the second blocking layer 17 (electron blocking layer), relying on the adjustment of aluminum and gallium content in the first waveguide layer 12, the first barrier layer 14, the second barrier layer 16, and the second waveguide layer 18, allows gallium and indium to be maintained within appropriate ranges. This ensures good lattice matching between layers in the epitaxial structure, making it suitable for large-scale, mass production. Furthermore, the higher temperature characteristics and higher internal quantum efficiency of the epitaxial structure design of the semiconductor laser in this embodiment contribute to achieving higher output power, especially significantly improving output power and electro-optical conversion efficiency under high-temperature power conditions, greatly expanding the application directions of semiconductor lasers.
[0097] In an optional embodiment, the aluminum content in the first waveguide layer 12 may be greater than the aluminum content in the first barrier layer 14; and the aluminum content in the second waveguide layer 18 may be greater than the aluminum content in the second barrier layer 16.
[0098] In this embodiment, the aluminum content in the first waveguide layer 12 is greater than that in the first barrier layer 14. This allows for the design of a larger second valence band difference ΔEv21 between the first barrier layer 13 (hole blocking layer) and the first barrier layer 14 when adjusting the different contents of gallium and indium in the first barrier layer 13 (hole blocking layer), while ensuring that the second conduction band difference ΔEc21 between the first barrier layer 13 (hole blocking layer) and the first waveguide layer 12 is ΔEc21 = b meV, where b ≤ 0.
[0099] Similarly, the aluminum content in the second waveguide layer 18 is greater than that in the second barrier layer 16. This allows for the design of a larger first conduction band difference ΔEc11 between the second barrier layer 17 (electron blocking layer) and the second barrier layer 16 when adjusting the content of aluminum, gallium, and indium in the second barrier layer 17 (electron blocking layer), while ensuring that the first valence band difference ΔEv11 between the second barrier layer 17 (electron blocking layer) and the second waveguide layer 18 is ΔEv11 = a meV, where a ≤ 0.
[0100] In an optional embodiment, and more specifically, the first waveguide layer 12 can be configured as Al. 0.3 Ga 0.7 As, the first barrier layer 14 is Al. 0.1 5Ga 0.85 As, and, the second waveguide layer 18 is Al 0.25 Ga 0.75 As, the second barrier layer 16 is Al 0.1 Ga 0.9 As.
[0101] In an optional embodiment, the first waveguide layer 12 is Al. x2 Ga 1-x2 As, 0.2≤x2≤0.4, for example, x2 can be set to 0.2, 0.26, 0.30, 0.35, 0.4 or other values.
[0102] The first blocking layer 13 (hole blocking layer) is Ga x3 In 1-x3 P, x3≥0.55, for example, x3 can be set to 0.57, 0.6, 0.75, 0.8, 0.9, 0.95 or other values.
[0103] The first barrier layer 14 is Al x4 Ga 1-x4 As, 0.05≤x4≤0.20, for example, x4 can be set to 0.06, 0.07, 0.10, 0.11, 0.13, 0.15, 0.17, 0.19 or other values.
[0104] The second barrier layer 16 is Al x6 Ga 1-x6 As, 0.05≤x6≤0.20, for example, x6 can be set to 0.07, 0.09, 0.10, 0.12, 0.14, 0.15, 0.18, 0.19 or other values.
[0105] The second blocking layer 17 (electron blocking layer) is Al x7 Ga y7 In 1-x7-y7 As, 1-x7-y7<0.2, 0.25≤x7≤0.45, for example, x7 can be set to 0.40, and y7 can be set to 0.45.
[0106] The second waveguide layer 18 is Al x8 Ga 1-x8 As, 0.20≤x8≤0.30, for example, x8 can be set to 0.2, 0.25, 0.28 or other values.
[0107] The reduction in Al content in the first barrier layer 14 and the second barrier layer 16 leads to a reduction in In content in the first barrier layer 13 (hole blocking layer) and the second barrier layer 17 (electron blocking layer). The reduction in In content is beneficial for the growth of epitaxial materials; therefore, the epitaxial structure design in the embodiments of this disclosure can greatly reduce the difficulty of epitaxial growth.
[0108] The low Al content (between 0.05-0.15%) in the first barrier layer 14 and the second barrier layer 16 allows the first blocking layer 13 (hole blocking layer) and the second blocking layer 17 (electron blocking layer) to achieve a higher bandgap difference with a lower In content, resulting in better carrier confinement. The bandgap differences ΔEc11 and ΔEc21 in Figure 2 can easily be higher than typical designs (ΔEc11 > 70 meV and ΔEc21 > 240 meV). Simultaneously, the second blocking layer 17 (electron blocking layer) significantly reduces or eliminates hole blocking, and the first blocking layer 13 (hole blocking layer) significantly reduces or eliminates electron blocking. This effectively improves carrier injection efficiency and carrier confinement capability, while also allowing for greater growth tolerance.
[0109] Optionally, the lower Al content in the first barrier layer 14 and the second barrier layer 16 reduces the series resistance of the overall semiconductor laser design, enabling lower voltage and higher electro-optical conversion efficiency.
[0110] The epitaxial structure design disclosed herein fundamentally solves the problem of voltage increase and low efficiency caused by using high Al content materials in the first barrier layer 14 and the second barrier layer 16 to ensure low carrier leakage in the original high-temperature structure design. This design can both suppress carrier leakage at high temperatures and achieve high power output, and ensure low voltage to achieve high efficiency. Therefore, the design is very beneficial for both high and room temperature applications, and can form a laser that operates stably and efficiently over a wide temperature range, providing huge tolerance for use in different application environments.
[0111] In this embodiment, the above-mentioned value ranges are all verified by the applicant through epitaxial growth design. They can balance the confinement effect on electrons and holes, so that the epitaxial structure can achieve the best confinement ability of charge carriers, and the output efficiency of semiconductor laser is greatly improved. At the same time, the gallium and indium contents in the first blocking layer 13 (hole blocking layer) and the second blocking layer 17 (electron blocking layer) are kept within a suitable range, and the lattice matching state between the layers in the epitaxial structure is good, which is suitable for large-scale, batch production.
[0112] In an optional embodiment, the first limiting layer 11 is Al. x1 Ga 1-x1 As, 0.25 ≤ x1 ≤ 0.80, for example, x1 can be 0.27, 0.29, 0.32, 0.37, 0.39, 0.42, 0.47, 0.51, 0.58, 0.63, 0.69, 0.72, 0.76, 0.79, 0.80 or other values. The quantum well layer 15 is In. x5 Ga 1-x5 As, 0 ≤ x5 ≤ 0.25. The second confinement layer 19 is Al. x9 Ga 1-x9 As, 0.35≤x9≤0.90, for example, x9 can be 0.37, 0.39, 0.43, 0.57, 0.69, 0.73, 0.80, 0.84, 0.87, 0.89, 0.90 or other values.
[0113] In this embodiment, the contents of the first confinement layer 11, the quantum well layer 15, and the second confinement layer 19 are further designed to form a complete epitaxial structure of a high-power semiconductor laser.
[0114] In an optional embodiment, the thickness of the first confinement layer 11 can be set to 1.5-3 micrometers, the thickness of the first waveguide layer 12 can be set to 0.3-1.5 micrometers, the thickness of the first blocking layer 13 (hole blocking layer) can be set to 0.004-0.030 micrometers, the thickness of the first barrier layer 14 can be set to 0.003-0.060 micrometers, the thickness of the quantum well layer 15 can be set to 0.006-0.010 micrometers, the thickness of the second barrier layer 16 can be set to 0.003-0.060 micrometers, the thickness of the second blocking layer 17 (electron blocking layer) can be set to 0.004-0.030 micrometers, the thickness of the second waveguide layer 18 can be set to 0.3-1.0 micrometers, and the thickness of the second confinement layer 19 can be set to 0.5-2 micrometers.
[0115] In this disclosure, the Al content (band gap) in the first confinement layer 11, the first waveguide layer 12, the second waveguide layer 18, and the second confinement layer 19 changes synchronously with the quantum well layer 15 (wavelength, quantum well band gap).
[0116] Specifically, the quantum well band gap Eg is negatively correlated with the wavelength. Therefore, the longer the wavelength of the quantum well layer, the smaller the quantum well band gap Eg. The corresponding band gap Eg of the waveguide layer and the barrier layer also decreases, which can satisfy the effective band gap difference, reduce the resistance, and achieve higher efficiency.
[0117] More specifically, the lasing wavelength of a semiconductor laser chip depends on the energy level difference between the conduction band bottom (first sub-electron level) and the valence band top (first sub-hole level) of the quantum well in the epitaxial structure, ideally satisfying the following:
[0118] Where λ is the lasing wavelength, h is Planck's constant, c is the speed of light, and E c-h For the effective band gap from the bottom of the conduction band to the top of the valence band, E c1 For the first electron sublevel at the bottom of the conduction band, E h1 It is the first sub-energy level of the hole at the top of the valence band.
[0119] The strain of a quantum well satisfies the following formula:
[0120] Among them, E c-hh For the effective band gap of a compressive strain quantum well, the band gap from the first sublevel of the conduction band to the first sublevel of the heavy hole band is E. g (x) represents the band gap of the quantum well under no strain condition, which is related to the material composition and content, a c For the conduction band deformation potential of the quantum well, a v b is the valence band and conduction band deformation potential of the quantum well, c is the tangential deformation potential, and c is the tangential band deformation potential. 11 and c 12 For the elastic modulus, ε / / The strain is in the plane of the quantum well layer. Therefore, when designing the epitaxial structure 100, the bandgap of the quantum well layer 15 is first designed based on the target wavelength, and then the matching design of the barrier, waveguide and confinement layer is carried out.
[0121] The design method described above can be used in all feasible wavelength bands of GaAs semiconductor lasers. The specific structure can achieve similar effects by proportionally varying or fine-tuning the bandgap of the quantum well structure corresponding to the operating wavelength. Therefore, Table 3 below provides an example of forming a 950nm wavelength band on an N-type GaAs substrate for reference. The specific structural information is as follows:
[0122] Table 3 shows examples of variations in elemental content and bandgap in the 950nm band formed on N-type GaAs substrates.
[0123] The epitaxial structure can also be formed on a p-type GaAs substrate. A buffer layer can be formed before forming the epitaxial structure on the substrate. When forming the above-mentioned epitaxial structure on a p-type substrate, the first confinement layer 11 is a p-type confinement layer, and Al... x11 Ga 1-x11 As, 0.35≤x11≤0.90; the first waveguide layer 12 is a P-type waveguide layer Al x12 Ga 1-x12 As, 0.20≤x12≤0.30; the first barrier layer 13 is an electron barrier layer Al. x13 Ga y13 In 1-x13-y13 As, 1-x13-y13<0.2, 0.25≤x13≤0.45; the first barrier layer 14 is a P-type barrier layer Al. x14 Ga 1-x14 As, 0.05 ≤ x14 ≤ 0.15; quantum well layer 15 is In x15 Ga 1-x15 As, 0≤x15≤0.25; the second barrier layer 16 is an N-type barrier layer, Al x16 Ga 1-x16 As, 0.05≤x16≤0.15; the second blocking layer 17 is a hole blocking layer, Ga x17 In 1-x17 P, x17≥0.55; the second waveguide layer 18 is an N-type waveguide layer, Al x18 Ga 1-x18 As, 0.2≤x18≤0.4; the second confinement layer 19 is an N-type confinement layer Al. x19 Ga 1-x19 As, 0.25≤x19≤0.80.
[0124] In another embodiment of this disclosure, FIG3 illustrates an N-type epitaxial structure 100 formed on an InP substrate, showing its energy band diagram. The N-type epitaxial structure 100 includes: a first confinement layer 11 made of InP material, a first waveguide layer 12 made of AlGaInAs material, a first barrier layer 13 made of GaInP material, a first barrier layer 14 made of AlGaInAs material, a quantum well layer 15 made of AlGaInAs material, a second barrier layer 16 made of AlGaInAs material, a second barrier layer 17 made of AlInAs material, a second waveguide layer 18 made of AlGaInAs material, and a second confinement layer 19 made of InP material. The material combinations in the above embodiments are only a typical and practically feasible preferred combination. In other embodiments, the material combinations are variable.
[0125] In an optional embodiment, the first waveguide layer is 12Al. m1 Ga n1 In 1-m1-n1 As, 0.25≤m1≤0.45, 0.05≤n1≤0.20; specifically, m1 = 0.4, n1 = 0.09 can be set. The first barrier layer 13 is Ga. m2 In 1-m2 P, 0.60≤m2≤0.85; specifically, m2 can be set to 0.69. The first barrier layer 14 is Al. m3 Ga n3 In 1-m3-n3 As, 0.20≤m3≤0.40, 0.10≤n3≤0.25; specifically, m3 = 0.35, n3 = 0.27 can be set. The second barrier layer 16 is Al. m5 Ga n5 In 1-m5-n5 As, 0.20≤m5≤0.40, 0.10≤n5≤0.25; specifically, m5 = 0.32, n5 = 0.18 can be set. The second barrier layer 17 is Al. m6 In 1-m6 As, 0.45≤m6≤0.60; specifically, m6 can be set to 0.58. The second waveguide layer 18 is Al. m7 Ga n7 In 1-m7-n7 As, 0.35≤m7≤0.50, 0.10≤n7≤0.20; specifically, m7 = 0.40, n7 = 0.19 can be set. Quantum well layer 15 is Al. m4 Ga n4 In 1-m4-n4 As, 0.02≤m4≤0.10, 0.30≤n4≤0.50; specifically, m4 = 0.07, n4 = 0.42 can be set. The first restriction layer 11 and the second restriction layer 19 are both InP.
[0126] In one optional embodiment, the thickness of the first confinement layer 11 is 1.5-3 micrometers, the thickness of the first waveguide layer 12 is 0.3-1.5 micrometers, the thickness of the first barrier layer 13 is 0.004-0.030 micrometers, the thickness of the first barrier layer 14 is 0.003-0.060 micrometers, the thickness of the quantum well layer 15 is 0.006-0.012 micrometers, the thickness of the second barrier layer 16 is 0.003-0.060 micrometers, the thickness of the second barrier layer 17 is 0.004-0.030 micrometers, the thickness of the second waveguide layer 18 is 0.1-1.0 micrometers, and the thickness of the second confinement layer 19 is 0.5-2.5 micrometers.
[0127] In a specific embodiment, Table 4 below provides an example of forming a 1480nm wavelength band on an N-type InP substrate for reference. The specific structural information is as follows:
[0128] Table 4 shows examples of variations in elemental content and bandgap in the 1480nm band formed on N-type InP substrates.
[0129] This disclosure also provides a method for fabricating an epitaxial structure of a semiconductor laser.
[0130] The growth sources used in the epitaxial growth process include: Group III high-purity organometallic compound sources: trimethylgallium (TMGa), trimethylaluminum (TMAl) and trimethylindium (TMIn); Group V high-purity organometallic compound sources: arsine (AsH3) and phosphine (PH3); doping sources: (ethyl)silane (used to form N-type doping) and tetrabromomethane (CBr4) (used to form P-type doping).
[0131] S1. Provide a substrate 1, and form a buffer layer 10 on the substrate 1. The material of the substrate 1 is GaAs or InP. The buffer layer formed on the substrate can buffer the stress between the substrate and the upper layer structure, improve the lattice matching degree, and improve the connection performance between the substrate and the epitaxial structure of the semiconductor laser.
[0132] S2. A first confinement layer 11 is formed on the buffer layer by metal-organic chemical vapor deposition (MOCVD) or molecular beam epitaxy. The first confinement layer 11 is Al. x1 Ga 1-x1 As material. In one embodiment, the first confinement layer 11 is an N-type confinement layer, grown using a TMAl source, a TMGa source, and an AsH3 source, wherein the Al content ranges from 0.25 to 0.80, i.e., 0.25 ≤ x1 ≤ 0.80, the growth thickness is controlled between 1.5 and 3.0 μm, and the growth rate is 0.1 to 1.0 nm / s.
[0133] S3. Using a TMAl source, a TMGa source, and an AsH3 source, a first waveguide layer 12 is formed on the first confinement layer 11. The material of the first waveguide layer 12 is Al. x2 Ga 1-x2 The growth layer is composed of As, where the Al content ranges from 0.20 to 0.30, the growth thickness is controlled between 0.5 and 1.5 μm, and the growth rate is 0.1 to 0.7 nm / s. In a specific embodiment, the first waveguide layer 12 is made of Al. 0.2 Ga 0.8 As, the temperature for growing the first waveguide layer 12 is 680℃-750℃, preferably in the range of 700℃-710℃.
[0134] S4. In the same deposition chamber, a first blocking layer 13 (hole blocking layer) is epitaxially grown on the first waveguide layer 12 using a TMIn source, a TMGa source, and a PH3 source. The material of the first blocking layer 13 (hole blocking layer) is GaInP, wherein the In content is greater than or equal to 0.55%, the growth thickness is controlled between 0.004 μm and 0.030 μm, and the growth rate is between 0.02 and 0.1 nm / s. Since the first blocking layer 13 (hole blocking layer) contains In, In will precipitate at high temperatures. The precipitated In will form a p-type confinement layer of In material at the interface, which will affect the performance of the semiconductor laser. Therefore, when forming the first blocking layer 13 (hole blocking layer), the temperature must be strictly controlled, and the growth temperature should be controlled at around 600℃, for example, between 580℃ and 640℃, to prevent In precipitation.
[0135] After the first blocking layer 13 (hole blocking layer) is formed, the injection of the reaction source is stopped for 15-20 seconds to keep the temperature inside the cavity constant. This ensures that even if a small amount of In is deposited after the first blocking layer 13 (hole blocking layer) is formed, it will not mix with the first waveguide layer 12 to form the layer structure.
[0136] In this step, the growth temperature and interface switching conditions of the first barrier layer 13 (cavity barrier layer) are strictly controlled to ensure the steepness of the interface and the quality of the material.
[0137] S5. Using a TMAl source, a TMGa source, and an AsH3 source, a first barrier layer 14 is formed on the first barrier layer 13 (hole blocking layer). The material of the first barrier layer 14 is In. x4 Ga 1-x4 The growth layer is composed of As, with an Al content ranging from 0.05 to 0.20, a growth thickness controlled between 0.003 and 0.060 μm, and a growth rate between 0.02 and 0.1 nm / s. The growth temperature of the first barrier layer 14 is selected as 680℃-750℃.
[0138] S6. After forming the first barrier layer 14, the deposition temperature in the control chamber is reduced to 580-640℃, and the quantum well layer 15 is deposited within this range. The quantum well layer 15 is grown on the first barrier layer 14 using a TMIn source, a TMGa source, and an AsH3 source. The material of the quantum well layer 15 is In. x5 Ga 1-x5 As, where the In content is approximately 0.12%, the growth thickness is controlled at 0.006–0.01 μm, and the growth rate is 0.02–0.1 nm / s. Since the quantum well layer 15 is an In-containing material, the temperature must be lower than that for In-free materials to prevent In precipitation. After the quantum well layer 15 is formed, the reaction source is stopped, and the temperature is kept constant for 15–20 seconds.
[0139] In step S7, a second barrier layer 16 is formed above the quantum well 15 using TMAl, TMGa, and AsH3 sources. The material of the second barrier layer 16 is AlGaAs, where the Al content ranges from 0.05 to 0.20%, the growth thickness is controlled between 0.003 and 0.060 μm, and the growth rate is 0.02 to 0.1 nm / s. The second barrier layer 16 does not contain In and is made of the same material as the first waveguide layer 12, with a growth temperature of 680℃-750℃. When forming the second barrier layer 16, x6 ranges between 0.05 and 0.20.
[0140] S8. The temperature inside the control chamber is reduced to 580℃-640℃. A second barrier layer 17 (electron blocking layer) is grown on the second barrier layer 16 using TMIn, TMAl, TMGa, and AsH3 sources. The material of the second barrier layer 17 (electron blocking layer) is AlGaInAs, where the In content is within the range of 0.20%, the growth thickness is controlled between 0.004 and 0.020 μm, and the growth rate is between 0.02 and 0.1 nm / s. After the second barrier layer 17 (electron blocking layer) is formed, the gas source is stopped for 15-20 seconds. Stopping the gas source for a period of time ensures that even if In is precipitated, it will not form a mixed layer structure with the upper layer structure.
[0141] S9. Increase the temperature and use a TMAl source, a TMGa source, and an AsH3 source to form a second waveguide layer 18 above the second blocking layer 17 (electron blocking layer). The material of the second waveguide layer 18 is AlGaAs, with an Al content ranging from 0.20% to 0.30%, a growth thickness controlled from 0.3% to 1.0 μm, and a growth rate of 0.1% to 0.7 nm / s. For example, the second waveguide layer 18 can be Al... 0.2 Ga 0.8 As. The temperature for growing the second waveguide layer 18 is 680℃-750℃, preferably within the range of 700℃-710℃.
[0142] S10. Using a TMAl source, a TMGa source, and an AsH3 source, a second confinement layer 19 is grown above the second waveguide layer 18. The second confinement layer 19 is AlGaAs, wherein the Al content ranges from 0.35% to 0.80%, the growth thickness is controlled from 0.5% to 2.0 μm, and the growth rate is 0.1% to 1.0 nm / s. The growth temperature of the second confinement layer 19 can be controlled to be the same as that of the second waveguide layer 18. The material composition ratio of the second confinement layer 19 is controlled by controlling the amount of reaction source gas introduced. In a specific embodiment, the second confinement layer 19 is Al. 0.4 Ga 0.6 As.
[0143] S11. A capping layer 20 is formed above the second confinement layer 19 using a TMGa source and an AsH3 source. The capping layer 20 is GaAs. The growth thickness of the capping layer 20 is 0.01 μm to 0.04 μm, and the growth rate is 0.1 to 0.5 nm / s.
[0144] The preparation method disclosed herein has the following advantages:
[0145] (1) The reduction of Al content in the first barrier layer 14 and the second barrier layer 16 on both sides of the quantum well layer 15 (the Al content is between 0.05 and 0.15) leads to a reduction of In content in the carrier blocking layer 13 (the In content in the first blocking layer, i.e. the hole blocking layer, is ≤0.45, and the In content in the second blocking layer 17 and the electron blocking layer is <0.20), which can greatly reduce the difficulty of epitaxial growth.
[0146] (2) By reducing the Al content in the first barrier layer 14 and the second barrier layer 16 on both sides of the quantum well layer 15, the valence band potential of the second barrier layer 16 on the side of the second barrier layer 17 (electron barrier layer) is less than the valence band potential of the second waveguide layer 18; the conduction band potential of the first barrier layer 14 on the side of the first barrier layer 13 (hole barrier layer) is less than the conduction band potential of the first waveguide layer 12; thus, the blocking effect of the second barrier layer 17 (electron barrier layer) on holes is reduced to a very low level or even non-existent, and the blocking effect of the first barrier layer 13 (hole barrier layer) on electrons is reduced to a very low level or even non-existent, which can effectively improve the carrier injection efficiency and carrier confinement capability.
[0147] (3) Reducing the Al content in the first barrier layer 14 and the second barrier layer 16 located on both sides of the quantum well layer 15 will reduce the series resistance of the overall epitaxial structure design, which can achieve a smaller voltage (here, a smaller voltage means a decrease in voltage under the same current. Specifically, refer to the formula: V=V0+I*Rs, where V0 is the turn-on voltage and Rs is the series resistance. Under the same current I, the series resistance Rs decreases and the voltage V decreases), thus achieving higher photoelectric conversion efficiency.
[0148] (4) The formation temperature of the indium-containing second barrier layer 17 (electron barrier layer), the first barrier layer 13 (hole barrier layer), and the quantum well layer 15 is lower than that of the other layers, which can prevent In precipitation. After these three layers are formed, the introduction of the reaction source needs to be controlled with a certain period of interruption and the temperature needs to be kept constant. This can prevent In precipitation from affecting the upper layer structure and from forming a mixed structure with the upper layer structure.
[0149] In another embodiment of this disclosure, the substrate 1 is InP, and a method for fabricating an epitaxial structure of a semiconductor laser is provided. The method includes sequentially growing a buffer layer 10, a first confinement layer 11, a first waveguide layer 12, a first barrier layer 13, a first potential barrier layer 14, a quantum well layer 15, a second barrier layer 16, a second barrier layer 17, a second waveguide layer 18, a second confinement layer 19, and a capping layer 20 on the InP substrate.
[0150] During the growth of the first waveguide layer Al m1 Ga n1 In 1-m1-n1 When using As, the growth thickness is controlled between 0.3 and 1.5 μm, and the growth rate is between 0.05 and 0.8 nm / s. The content ranges of Al and Ga satisfy: 0.25 ≤ m1 ≤ 0.45 and 0.05 ≤ n1 ≤ 0.20.
[0151] During the growth of the first barrier layer Ga m2 In 1-m2 When P is used, the growth thickness is controlled between 0.004 μm and 0.030 μm, the growth rate is between 0.02 and 0.8 nm / s, and the In content range is 0.60 ≤ m2 ≤ 0.85. After the first barrier layer is grown, the injection of the reaction source is stopped for 15-20 seconds, and the temperature in the chamber is kept constant.
[0152] During the growth of the first barrier layer Al m3 Ga n3 In 1-m3-n3 When using As, the growth thickness is controlled between 0.003 and 0.060 μm, and the growth rate is between 0.02 and 0.8 nm / s. The content ranges of Al and Ga satisfy: 0.20 ≤ m³ ≤ 0.40 and 0.10 ≤ n³ ≤ 0.25, respectively. When forming the first barrier layer, the growth temperature is selected as 630℃-750℃, the growth thickness is controlled between 0.003 and 0.060 μm, and the growth rate is between 0.02 and 0.8 nm / s.
[0153] In the process of quantum well layer Al m4 Ga n4 In 1-m4-n4During As deposition, the deposition temperature in the chamber is controlled to be reduced to 580-700℃, the growth thickness is controlled to be 0.006-0.012μm, and the growth rate is 0.02-0.1nm / s. The contents of Al and Ga satisfy: 0.02≤m4≤0.10 and 0.30≤n4≤0.50. After the quantum well layer is formed, the reaction source is stopped for 15-20 seconds, and the temperature is kept constant.
[0154] During the growth of the second barrier layer Al m5 Ga n5 In 1-m5-n5 When using As, the growth thickness is controlled between 0.003 and 0.060 μm, and the growth rate is between 0.02 and 0.8 nm / s. The content ranges of Al and Ga satisfy: 0.20 ≤ m⁵ ≤ 0.40 and 0.10 ≤ n⁵ ≤ 0.25, respectively. When forming the second barrier layer, the growth temperature is selected as 630℃-750℃, the growth thickness is controlled between 0.003 and 0.060 μm, and the growth rate is between 0.02 and 0.8 nm / s.
[0155] During the growth of the second barrier layer Al m6 In 1-m6 When As is grown, the growth thickness is controlled between 0.004 μm and 0.030 μm, the growth rate is between 0.02 and 0.8 nm / s, and the Al content range is: 0.45 ≤ m6 ≤ 0.60. After the second barrier layer is grown, the injection of the reaction source is stopped for 15-20 seconds, and the temperature in the chamber is kept constant.
[0156] During the growth of the second waveguide layer Al m7 Ga n7 In 1-m7-n7 When using As, the growth thickness is controlled between 0.1 and 1.0 μm, the growth rate is between 0.05 and 0.8 nm / s, and the content ranges of Al and Ga satisfy: 0.35 ≤ m7 ≤ 0.50 and 0.10 ≤ n7 ≤ 0.20.
[0157] This disclosure also relates to a semiconductor laser, including a substrate 1 and an epitaxial structure 100 disposed on the surface of the substrate. The epitaxial structure 100 is the epitaxial structure 100 as described in any of the above embodiments, or an epitaxial structure obtained by any of the above methods for preparing the epitaxial structure 100.
[0158] The epitaxial structure and semiconductor laser disclosed herein utilize the following methods to adjust the content of aluminum and gallium in the first waveguide layer 12, the first barrier layer 14, the second barrier layer 16, and the second waveguide layer 18; the content of gallium and indium in the first blocking layer 13 (hole blocking layer); and the content of aluminum, gallium, and indium in the second blocking layer 17 (electron blocking layer). These methods result in the following: a first conduction band difference ΔEc11 between the second blocking layer 17 (electron blocking layer) and the second barrier layer 16 > 70 meV; a second valence band difference ΔEv21 between the first blocking layer 13 (hole blocking layer) and the first barrier layer 14 > 240 meV; a first valence band difference ΔEv11 between the second blocking layer 17 (electron blocking layer) and the second waveguide layer 18 = a meV; and a second conduction band difference ΔEc21 between the first blocking layer 13 (hole blocking layer) and the first waveguide layer 12 = b meV, where a ≤ 0 and b ≤ 0.
[0159] The inventors discovered that differences in polarization intensity, lattice matching, and doping efficiency of material systems determine drastically different EBL design logics. Traditional GaN-based EBLs (electron blocking layers) are a necessary means to compensate for material shortcomings, while the epitaxial structure of the semiconductor laser disclosed herein and the GaAs-based EBLs (electron blocking layers) used in the semiconductor laser may become redundant designs in terms of performance and cost.
[0160] GaN materials (especially InGaN quantum wells) exhibit significant lattice mismatch and piezoelectric polarization effects, leading to a tilted energy band in the quantum well. Electrons readily leak from the active region into the p-type layer. Simultaneously, the p-type doping efficiency in GaN is low, and hole mobility is far lower than that of electrons, resulting in low hole injection efficiency. To overcome the strong polarization effect and hole injection barrier of InGaN / GaN quantum wells, GaN-based laser chips must employ an electron blocking layer (EBL) structure (such as a p-AlGaN layer). This high conduction band barrier blocks electron leakage. During design, it is not necessary to minimize the blocking effect of the electron blocking layer on holes; instead, the energy band gradient can be adjusted by optimizing the composition, thickness, and doping design of the p-type transition compensation layer and the electron blocking layer (p-AlGaN layer), thereby improving hole injection efficiency.
[0161] The GaAs-based structure disclosed herein naturally forms a high potential barrier through the band shift of the heterojunction (e.g., the increase in Al content significantly improves the conduction and valence band shifts), which can effectively confine charge carriers. Furthermore, the polarization electric field is weak, the quantum well band is flat, and the leakage risk is low. Simultaneously, p-type GaAs has high doping efficiency, and its hole mobility is far superior to GaN, resulting in more complete hole injection and insignificant electron-hole asymmetry issues. Therefore, when using an electron / hole blocking layer design in a GaAs-based structure, it is necessary to additionally address defects caused by lattice mismatch, decreased hole injection efficiency, and doping compatibility issues. The electron blocking layer design needs to reduce the hole blocking effect of the layer to an extremely low level (<20 meV). Therefore, reducing the blocking effect of the electron blocking layer on holes and reducing the blocking effect of the hole blocking layer on electrons are key aspects of GaAs-based EBL design.
[0162] Furthermore, the material combinations for GaN-based and GaAs-based structures differ. The GaN-based structure uses a QW layer with an InGaN waveguide layer, an AlGaN EBL, and an AlGaN confinement layer. The GaAs-based structure uses a QW layer with an AlGaAs waveguide layer, an InAlGaAs EBL, an AlGaAs waveguide layer, and an AlGaAs confinement layer.
[0163] The above description is merely a preferred embodiment of this disclosure and is not intended to limit this disclosure. Various modifications and variations can be made to this disclosure by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this disclosure should be included within the scope of protection of this disclosure. It should be noted that similar reference numerals and letters in the following figures indicate similar items; therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.
[0164] The above description is merely a specific embodiment of this disclosure, but the scope of protection of this disclosure is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this disclosure should be included within the scope of protection of this disclosure. Therefore, the scope of protection of this disclosure should be determined by the scope of the claims. Industrial applicability
[0165] By adopting the above scheme, the epitaxial structure design of the semiconductor laser can effectively balance the confinement of electrons and holes, achieving optimal carrier confinement and significantly improving the output efficiency of the semiconductor laser. Simultaneously, the adaptive adjustment of the indium content in the first blocking layer (hole blocking layer) and the second blocking layer (electron blocking layer), relying on the adjustment of the aluminum and gallium content in the first waveguide layer, first barrier layer, second barrier layer, and second waveguide layer, ensures that the indium content remains within a suitable range. This results in good lattice matching between the layers in the epitaxial structure, making it suitable for large-scale, mass production. Furthermore, the higher temperature characteristics and higher internal quantum efficiency of the epitaxial structure design of the semiconductor laser in this embodiment contribute to achieving higher output power, especially with a significant improvement in output power and electro-optical conversion efficiency under high-temperature power conditions, greatly expanding the application directions of semiconductor lasers.
Claims
1. An epitaxial structure for a semiconductor laser, comprising: The first waveguide layer, the first barrier layer, the first barrier layer, the quantum well layer, the second barrier layer, the second barrier layer and the second waveguide layer are stacked from bottom to top, characterized in that: The first conduction band difference between the second barrier layer and the second barrier layer is ΔEc11> 70meV, the second valence band difference between the first barrier layer and the first barrier layer is ΔEv21> 240meV, the first valence band difference between the second barrier layer and the second waveguide layer is ΔEv11= a meV, and the second conduction band difference between the first barrier layer and the first waveguide layer is ΔEc21= b meV, wherein a≤0, b≤0.
2. The epitaxial structure of the semiconductor laser according to claim 1, characterized in that, The content of aluminum in the first waveguide layer is greater than the content of aluminum in the first barrier layer; and the content of aluminum in the second waveguide layer is greater than the content of aluminum in the second barrier layer.
3. The epitaxial structure of a semiconductor laser according to any one of claims 1-2, characterized in that, The first waveguide layer is Al x2 Ga 1-x2 As, 0.2≤x2≤0.4; The first barrier layer is Ga x3 In 1-x3 P, x3≥ 0.55; The first barrier layer is Al x4 Ga 1-x4 As, 0.05≤x4≤0.20; The second barrier layer is Al x6 Ga 1-x6 As, 0.05≤x6≤0.20; The second barrier layer is Al x7 Ga y7 In 1-x7-y7 As, 1-x7-y7 < 0.2, 0.25 < x7 < 0.45 The second waveguide layer is Al x8 Ga 1-x8 As, 0.20≤x8≤0.
30.
4. The epitaxial structure of a semiconductor laser according to any one of claims 1 to 3, characterized in that The epitaxial structure of the semiconductor laser further comprises a first limiting layer disposed below the first waveguide layer and a second limiting layer disposed above the second waveguide layer. The first confinement layer is Al x1 Ga 1-x1 As, 0.25≤x1≤0.80; The quantum well layer is In x5 Ga 1-x5 As, 0≤x5≤0.25; The second confinement layer is Al x9 Ga 1-x9 As, 0.35≤x9≤0.
90.
5. The epitaxial structure of a semiconductor laser according to claim 4, wherein The thickness of the first limiting layer is 1.5-3 microns, the thickness of the first waveguide layer is 0.3-1.5 microns, the thickness of the first barrier layer is 0.004-0.030 microns, the thickness of the first barrier layer is 0.003-0.060 microns, the thickness of the quantum well layer is 0.006-0.010 microns, the thickness of the second barrier layer is 0.003-0.060 microns, the thickness of the second barrier layer is 0.004-0.030 microns, the thickness of the second waveguide layer is 0.3-1.0 microns, and the thickness of the second limiting layer is 0.5-2 microns.
6. The epitaxial structure of a semiconductor laser according to any one of claims 1 to 2, characterized in that The epitaxial structure of the semiconductor laser further comprises a first limiting layer disposed below the first waveguide layer and a second limiting layer disposed above the second waveguide layer. The first confinement layer is Al x11 Ga 1-x11 As, 0.35≤x11≤0.90; The first waveguide layer is Al x12 Ga 1-x12 As, 0.20≤x12≤0.30; The first barrier layer is Al x13 Ga y13 In 1-x13-y13 As, 1-x13-y13 < 0.2, 0.25 < x13 < 0.45; The first barrier layer is Al x14 Ga 1-x14 As, 0.05≤x14≤0.15; The quantum well layer is In x15 Ga 1-x15 As, 0≤x15≤0.25; The second barrier layer is Al x16 Ga 1-x16 As, 0.05≤x16≤0.15; The second barrier layer is Ga x17 In 1-x17 P, x17≥ 0.55; The second waveguide layer is Al x18 Ga 1-x18 As, 0.2≤x18≤0.4; The second confinement layer is Al x19 Ga 1-x19 As, 0.25≤x19≤0.
80.
7. The epitaxial structure of a semiconductor laser according to any one of claims 1 to 2, characterized in that The first waveguide layer is Al m1 Ga n1 In 1-m1-n1 As, 0.25≤m1≤0.45, 0.05≤n1≤0.20; The first barrier layer is Ga m2 In 1-m2 P, 0.60≤m2≤0.85; The first barrier layer is Al m3 Ga n3 In 1-m3-n3 As, 0.20≤m3≤0.40, 0.10≤n3≤0.25; The second barrier layer is Al m5 Ga n5 In 1-m5-n5 As, 0.20≤m5≤0.40, 0.10≤n5≤0.25; The second barrier layer is Al m6 In 1-m6 As, 0.45≤m6≤0.60; The second waveguide layer is Al m7 Ga n7 In 1-m7-n7 As, 0.35≤m7≤0.50, 0.10≤n7≤0.
20.
8. The epitaxial structure of a semiconductor laser according to claim 7, wherein The epitaxial structure of the semiconductor laser further comprises a first limiting layer disposed below the first waveguide layer and a second limiting layer disposed above the second waveguide layer. The quantum well layer is Al m4 Ga n4 In 1-m4-n4 As, 0.02≤m4≤0.10, 0.30≤n4≤0.50; The first limiting layer and the second limiting layer are both InP.
9. An epitaxial structure for a semiconductor laser according to any of claims 6 to 8, characterised in that, The thickness of the first limiting layer is 1.5-3 microns, the first waveguide layer is 0.3-1.5 microns, the thickness is 0.004-0.030 microns, the thickness of the first barrier layer, the thickness of the first barrier layer is 0.003-0.060 microns; the thickness of the quantum well layer is 0.006-0.012 microns, the thickness of the second barrier layer is 0.003-0.060 micron, the thickness of the second barrier layer is 0.004-0.030 microns; the thickness of the second waveguide layer is 0.1-1.0 microns, and the thickness of the second limiting layer is 0. 5-2.5 microns.
10. A method of fabricating an epitaxial structure of a semiconductor laser, characterized by, Comprising: Growth of a first waveguide layer, a first barrier layer, a first barrier layer, a quantum well layer, a second barrier layer, a second barrier layer, a second waveguide layer stacked on a substrate; In the growth of the first waveguide layer, the first barrier layer, the first barrier layer, the second barrier layer, the second barrier layer and the second waveguide layer: the content of aluminum element and gallium element in the first waveguide layer, the first barrier layer, the second barrier layer and the second waveguide layer is adjusted, the content of gallium element and indium element in the first barrier layer is adjusted, and the content of aluminum element and indium element in the second barrier layer is adjusted, so that the first conduction band difference ΔEc11 between the second barrier layer and the second barrier layer is greater than 70meV, the second valence band difference ΔEv21 between the first barrier layer and the first barrier layer is greater than 240meV, the first valence band difference ΔEv11 between the second barrier layer and the second waveguide layer is a meV, and the second conduction band difference ΔEc21 between the first barrier layer and the first waveguide layer is b meV, a≤0, b≤0.
11. The method of claim 10, wherein the method further comprises: The epitaxial structure of the semiconductor laser further comprises: a first limiting layer arranged below the first waveguide layer and a second limiting layer arranged above the second waveguide layer. The first limiting layer is AlGaAs material. The first waveguide layer is AlGaAs material. The first barrier layer is GaInP material. The first barrier layer is GaInP material. The first barrier layer is GaInAs material. The second barrier layer is AlGaInAs material. The second barrier layer is AlGaInAs material. The second waveguide layer is AlGaInAs material. The second limiting layer is AlGaInAs material.
12. The preparation method of the epitaxial structure of the semiconductor laser according to claim 11, characterized in that: When growing the first waveguide layer Al x2 Ga 1-x2 As, the thickness is controlled at 0.5-1.5 μm, and the growth rate is 0.1-0.7 nm / s, wherein the content of Al satisfies: 0.2≤x2≤0.
4. When growing the first barrier layer Al x4 Ga 1-x4 As, the thickness is controlled at 0.003-0.060 μm, and the growth rate is 0.02-0.1 nm / s, wherein the content of Al satisfies: 0.05≤x4≤0.
20. When growing the second barrier layer Al x6 Ga 1-x6 As, the thickness is controlled at 0.003-0.060 μm, and the growth rate is 0.02-0.1 nm / s, wherein the content of Al satisfies: 0.05≤x6≤0.
20. When growing the second waveguide layer Al x8 Ga 1-x8 As, the thickness is controlled at 0.3-1.0 μm, the growth rate is 0.1-0.7 nm / s, and the content of Al is in the range of 0.20≤x8≤0.
30.
13. The method of claim 12, wherein the method further comprises: including: In the growth of the first barrier layer Ga x3 In 1-x3 P, the thickness is controlled in the range of 0.004 μm to 0.020 μm, the growth rate is 0.02 to 0.1 nm / s, and the content of In is in the range of x3≥0.55; after the growth of the first barrier layer, the injection of the reaction source is stopped for 15 to 20 seconds, and the temperature in the chamber is kept unchanged; and, During the growth of the second barrier layer Al x7 Ga y7 In 1-x7-y7 When As is used, the growth thickness is controlled between 0.004 μm and 0.030 μm, the growth rate is between 0.02 and 0.1 nm / s, and the In content range satisfies: 1 - x⁷ - y⁷ < 0.2; the second barrier layer Al x7 Ga y7 In 1-x7-y7 After As growth is complete, stop injecting the reaction source for 15-20 seconds and keep the temperature inside the chamber constant.
14. The method of claim 12, wherein the method further comprises: including: When forming the first barrier layer, the growth temperature is selected to be 680-750℃, the growth thickness is controlled to be 0.003-0.060μm, and the growth rate is 0.02-0.1nm / s; When forming the second barrier layer, the growth temperature is selected to be 680-750℃, the growth thickness controlled to be 0.003-0.060μm, and the growth rate is controlled to be 0.02-0.1nm / s.
15. The method of claim 14, wherein the method further comprises: In x5 Ga 1-x5 During the deposition of quantum well layer In x5Ga x5As, the deposition temperature in the chamber is controlled to decrease to 580-640℃, the thickness is controlled to be 0.006-0.01 μm, and the growth rate is 0.02-0.1 nm / s, wherein the content of In satisfies: 0≤x5≤0.
25. After forming the quantum well layer, the reaction source is stopped for 15-20 seconds, and the temperature is kept unchanged.
16. The method of claim 9, wherein the method further comprises: The epitaxial structure of the semiconductor laser further comprises: a first limiting layer arranged below said first waveguide layer and a second limiting layer arranged above said second waveguide layer; The first limiting layer is InP material. The first waveguide layer is AlGaInAs material. The first barrier layer is GaInP material. The first barrier layer is GaAs material. The first barrier layer is GaInP material. The second barrier layer is AlGaInAs material. The second barrier layer is AlInAs material. The second waveguide layer is AlGaInAs material. The second limiting layers are InP.
17. The method of claim 16, wherein the method further comprises: The first waveguide layer is Al m1 Ga n1 In 1-m1-n1 As, 0.25≤m1≤0.45, 0.05≤n1≤0.20; The first barrier layer is Ga m2 In 1-m2 P, 0.60≤m2≤0.85; The first barrier layer is Al m3 Ga n3 In 1-m3-n3 As, 0.20≤m3≤0.40, 0.10≤n3≤0.25; The quantum well layer is Al m4 Ga n4 In 1-m4-n4 As, 0.02≤m4≤0.10, 0.30≤n4≤0.50; The second barrier layer is Al m5 Ga n5 In 1-m5-n5 As, 0.20≤m5≤0.40, 0.10≤n5≤0.25; The second barrier layer is Al m6 In 1-m6 As, 0.45≤m6≤0.60; The second waveguide layer is Al m7 Ga n7 In 1-m7-n7 As, 0.35≤m7≤0.50, 0.10≤n7≤0.20; The first limiting layer and the second limiting layer are both InP.
18. The preparation method of the epitaxial structure of the semiconductor laser according to claim 17, characterized in that, In growing the first waveguide layer Al m1 Ga n1 In 1-m1-n1 As, the thickness is controlled to be 0.3-1.5 μm, and the growth rate is 0.05-0.8 nm / s, wherein the content range of Al and Ga satisfies: 0.25≤m1≤0.45, 0.05≤n1≤0.
20. In the growth of the first barrier layer Ga m2 In 1-m2 P, the thickness is controlled in the range of 0.004 μm to 0.030 μm, the growth rate is 0.02 to 0.8 nm / s, and the content of In is in the range of 0.60≤m2≤0.85; after the growth of the first barrier layer, the injection of the reaction source is stopped for 15 to 20 seconds, and the temperature in the chamber is kept unchanged. The thickness of the first barrier layer Al m3 Ga n3 In 1-m3-n3 As is controlled to be 0.003-0.060 μm, and the growth rate is 0.02-0.8 nm / s, wherein the content range of Al and Ga satisfies: 0.20≤m3≤0.40, 0.10≤n3≤0.
25. In the quantum well layer Al m4 Ga n4 In 1-m4-n4 During the deposition of As, the deposition temperature in the chamber is controlled to decrease to 580-700°C, the thickness is controlled to be 0.006-0.012 μm, and the growth rate is 0.02-0.1 nm / s, wherein the content of Al and Ga satisfies: 0.02≤m4≤0.10, 0.30≤n4≤0.50; after the quantum well layer is formed, the supply of the reaction source is stopped for 15-20 seconds, and the temperature is kept unchanged; In growing the second barrier layer Al m5 Ga n5 In 1-m5-n5 As, the growth thickness is controlled to be 0.003-0.060 μm, and the growth rate is 0.02-0.8 nm / s, wherein the content range of Al and Ga satisfies: 0.20≤m5≤0.40, 0.10≤n5≤0.
25. In growing the second barrier layer Al m6 In 1-m6 As time, the thickness is controlled in 0.004 μm~0.030 μm, the growth rate is 0.02~0.8 nm / s, the content range of Al satisfies: 0.45≤m6≤0.60;After the second barrier layer is grown, the injection of the reaction source is stopped for 15-20 seconds, and the temperature in the chamber is kept unchanged; The thickness of the second waveguide layer Al m7 Ga n7 In 1-m7-n7 As is controlled to be 0.1-1.0 μm, the growth rate is 0.05-0.8 nm / s, and the content range of Al and Ga satisfies: 0.35≤m7≤0.50, 0.10≤n7≤0.
20.
19. The method of claim 18, wherein the method further comprises: including: In forming the first barrier layer, the growth temperature is selected to be 630-750 DEG C, the growth thickness is controlled to be 0.003-0.060 μm, and the growth rate is 0.02-0.8 nm / s; In forming the second barrier layer, the growth temperature is selected to be 630-750 DEG C, the growth thickness is controlled to be 0.003-0.060 μm, and the growth rate is 0.02-0.8 nm / s.