Smelting process and device for high-grade nickel-based superalloy

By combining vacuum induction smelting and plasma beam refining, and utilizing the batch addition of rare elements in powder form and inert gas protection, the problems of rare element loss and impurity introduction were solved, thereby improving the uniformity and quality of high-temperature alloy composition.

WO2026232724A1PCT designated stage Publication Date: 2026-11-12SHANGHAI ERAUM ALLOY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/119722
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2025-09-08
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The traditional smelting process for adding rare elements leads to excessive losses and the introduction of impurities, affecting the uniformity of the internal composition of high-temperature alloys and reducing the quality of high-grade nickel-based high-temperature alloys.

Method used

The process combines vacuum induction smelting and plasma beam refining. Rare elements in powder form are added in batches by reciprocating oscillation and mixed under inert gas protection. A rare element crushing and adding device is used to improve mixing uniformity and reduce losses.

Benefits of technology

It effectively reduces the loss of rare elements, improves the uniformity of the internal components of high-temperature alloys and the quality of the final product, and shortens the smelting time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025119722_12112026_PF_FP_ABST
    Figure CN2025119722_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A smelting process and device for a high-grade nickel-based superalloy. The smelting process comprises the following steps: S1, raw material preparation; S2, vacuum induction smelting; and S3, plasma beam refining: using a plasma beam refining device to perform reciprocating plasma beam scanning on a molten alloy in S2, and further removing impurities from a superalloy; and S4, addition of rare elements: when the plasma beam refining in S3 is completed, adding prepared rare elements to the molten superalloy, wherein during the addition of the rare elements, the molten superalloy is synchronously controlled to be directionally stirred, and the rare elements in a powder state are added to a furnace in portions in a reciprocating manner and come into contact and mix with the molten superalloy. The process shortens the overall smelting time, reduces the loss of rare elements, and improves the quality of a final high-grade nickel-based superalloy product.
Need to check novelty before this filing date? Find Prior Art

Description

A smelting process and equipment for high-grade nickel-based superalloys Technical Field

[0001] This invention relates to the field of alloy manufacturing technology, and in particular to a smelting process and smelting equipment for a high-grade nickel-based superalloy. Background Technology

[0002] GH163 is a Ni~Cr~Co based precipitation hardening wrought superalloy with a service temperature of up to 850℃. GH163 alloy has good oxidation resistance, high yield strength and creep strength below 800℃, low tendency for strain failure cracks, and good resistance to thermal fatigue.

[0003] The addition of multiple rare earth elements can more effectively refine the grains, reduce grain boundary defects, and improve the density and uniformity of GH163 high-temperature alloy, thereby further improving the alloy's corrosion resistance and mechanical properties.

[0004] In the traditional smelting process, the timing and method of adding rare elements can lead to excessive loss of rare elements and introduce too many impurities. At the same time, since rare elements account for a low mass proportion, the concentrated block addition method will also increase the overall stirring and mixing time, affecting the uniformity of the internal components of the final high-temperature alloy and the quality of the final high-temperature alloy product. Summary of the Invention

[0005] To address the aforementioned problems, this invention provides a smelting process and equipment for high-grade nickel-based superalloys. This invention shortens the overall smelting time, reduces the loss of rare elements, and improves the quality of the final high-grade nickel-based superalloy.

[0006] To solve the above problems, the technical solution adopted by the present invention is as follows:

[0007] A smelting process for a high-grade nickel-based superalloy includes the following steps: S1, raw material preparation: preparing raw materials according to the composition of the high-grade nickel-based superalloy; S2, vacuum induction smelting: adding the raw materials from step S1 into a vacuum smelting furnace for high-temperature smelting to initially remove impurities and obtain a molten superalloy; S3, plasma beam refining: using a plasma beam refining device to perform a reciprocating plasma beam scan on the molten alloy liquid from step S2 to further remove impurities from the superalloy; S4, addition of rare elements: after the plasma beam refining in step S3, adding the prepared rare elements into the molten superalloy; wherein, during the addition of rare elements, the molten superalloy is simultaneously controlled to be directionally stirred, and the powdered rare elements are added to the furnace in batches by reciprocating oscillation to contact and mix with the molten superalloy.

[0008] Powdered rare elements can react more quickly with molten high-temperature alloys. By adding powdered rare elements into the furnace through reciprocating oscillation, the rare element powder can come into contact with high-temperature alloys at different locations, increasing the contact area, improving the uniformity of distribution, enhancing the mixing effect, and improving the uniformity of the distribution of different components within the final alloy.

[0009] Preferably, the high-grade nickel-based superalloy comprises, by mass percentage: C 0.04~0.08%, Mo 5.60~6.10%, Cu 0~0.20%, Si 0~0.40%, Mn 0~0.60%, Co 19.0~21.0%, Cr 22.0~25.0%, Ti 1.90~2.40%, Ag 0~0.005%, P 0~0.015%, W 1.0~2.0%; rare element additions include: Ce 0.1~0.15%, La 0.02~0.05%; the remainder is Ni, some impurities, and necessary metallic or non-metallic elements; wherein the purity of Ni, Mo, Co, Cr, and Ti is not less than 99.5%, and the purity of the remaining alloy materials is not less than 99%.

[0010] Preferably, in step S3, the vacuum level inside the furnace is controlled to reach 10⁻² ~ 10⁻³ Pa, and a segmented heating strategy is adopted. First, the molten high-temperature alloy is restored to a temperature of not less than 1300°C at a lower heating rate, and then all metals are kept above the melting point at a higher heating rate. Then, a refining process is carried out, and the refining temperature is increased to between 1550°C and 1700°C.

[0011] Preferably, the refining time in step S3 is between 35 and 55 minutes, and an inert gas is used for protection during the plasma beam refining process.

[0012] Preferably, the rare element powder is pulverized in batches. The first pulverization is carried out outside the furnace, which pulverizes the blocky rare element into millimeter-level particles. The second grinding and pulverization is carried out inside the furnace, which further grinds and pulverizes the rare element particles obtained in the first pulverization to the micron level.

[0013] Preferably, the rare elements are crushed into particles no larger than 5 mm in the first crushing process, and then ground into particles between 100 and 400 micrometers in the second grinding process.

[0014] A smelting device for high-grade nickel-based superalloys, used in the aforementioned smelting process, includes a rare element crushing and adding device. The rare element crushing and adding device includes a limiting base, with a grinding body mounted on the upper end of the limiting base. A drive shaft is rotatably connected to the inner wall of the grinding body, and a grinding roller is mounted on the lower end of the drive shaft. The first end of the drive shaft penetrates the grinding body and is fixedly connected to a feeding pipe. A hollow conveying channel is formed on the inner wall of the drive shaft and communicates with the feeding pipe. A guide opening is opened on the side wall of the drive shaft and communicates with the interior of the grinding body. An air blowing device is mounted on the upper end of the grinding body. Simultaneously, the drive shaft drives the grinding roller to grind and the feeding pipe to oscillate, while the air blowing device blows protective gas towards the inner wall of the grinding body to form a protective airflow. This protective airflow carries micron-sized rare element powder into the hollow conveying channel and finally discharges it from the feeding pipe to contact and mix with the molten superalloy.

[0015] Preferably, the air blowing device includes two sets of symmetrically arranged strip-shaped air nozzles, and also includes a connecting main pipe, which is connected to two connecting branch pipes. The two connecting branch pipes are respectively connected to the corresponding strip-shaped air nozzles, and a control valve is provided at the connection point between the connecting main pipe and the two connecting branch pipes.

[0016] Preferably, the blowing direction of the strip-shaped air nozzle is tangent to the arc of the inner wall of the grinding body, and the opening of the guide opening faces away from the grinding roller.

[0017] Preferably, the second end of the drive shaft passes through the grinding body and is connected to the electrical control device. The delivery tube includes a first tube and a second tube. The second tube and the first tube are electrically retractable via a control component. The electrical control device is electrically connected to the control component.

[0018] The beneficial effects of this invention are as follows:

[0019] Compared with existing technologies, the composite process of vacuum induction smelting and plasma beam refining can minimize impurities in high-temperature alloys. After plasma beam refining, rare elements are added to the furnace in batches in powder form and mixed with the molten high-temperature alloy in a reciprocating oscillating manner. This can maximize the mixing effect of rare elements with high-temperature alloys, ensure the uniform and stable distribution of rare elements, shorten the overall smelting time, reduce the loss of rare elements, and improve the quality of the final high-grade nickel-based high-temperature alloy. Attached Figure Description

[0020] Figure 1 is a process flow diagram of the present invention.

[0021] Figure 2 is a schematic diagram of the internal structure of the furnace body of the present invention.

[0022] Figure 3 is an enlarged structural diagram of point A in Figure 2 of the present invention.

[0023] Figure 4 is a three-dimensional structural schematic diagram of the rare element crushing and adding device of the present invention.

[0024] Figure 5 is a side view of the structure of Figure 4 of the present invention.

[0025] Figure 6 is a schematic cross-sectional view of the structure in Figure 5 of the present invention along the B-B direction.

[0026] In the diagram: 100, furnace body; 200, rare element crushing and adding device; 210, feeding pipe; 211, first pipe body; 212, second pipe body; 220, limiting base; 230, grinding body; 231, grinding shell; 232, grinding roller; 233, connecting frame; 234, drive shaft; 2341, hollow conveying channel; 2342, guide opening; 240, air blowing device; 241, strip-shaped air blowing nozzle; 242, connecting branch pipe; 243, control valve; 244, connecting main pipe. Detailed Implementation

[0027] The present invention will be further described below with reference to the accompanying drawings and embodiments.

[0028] GH163 is a Ni~Cr~Co based precipitation hardening wrought superalloy with a service temperature of up to 850℃. GH163 alloy has good oxidation resistance, high yield strength and creep strength below 800℃, low tendency for strain failure cracks, and good resistance to thermal fatigue.

[0029] The alloy is mainly suitable for manufacturing plate welded structural components and load-bearing components for the main combustion chamber and afterburner of aero engines. It has been used to manufacture aero engine flame tubes, afterburner bodies, mounting edges, mounting bases and pipes, etc.

[0030] Applications such as combustion chambers and flame tubes in extreme conditions require high corrosion resistance of alloys. To improve the corrosion resistance of GH163 high-temperature alloy, a new high-grade nickel-based high-temperature alloy is proposed, which, by mass percentage, comprises: C 0.04~0.08%, Mo 5.60~6.10%, Cu 0~0.20%, Si 0~0.40%, Mn 0~0.60%, Co 19.0~21.0%, Cr 22.0~25.0%, Ti 1.90~2.40%, Ag 0~0.005%, P 0~0.015%, W 1.0~2.0%, and rare element additions including Ce 0.1~0.15%, La 0.02~0.05%, with the remainder being Ni, some impurities, and necessary metallic or non-metallic elements.

[0031] By increasing the lower limit of Cr content from 19.0% to 22.0% and the upper limit to 25.0%, the higher Cr content can form a thicker and more stable dense oxide film on the outer surface of GH163 high-temperature alloy, further enhancing the ability to block the intrusion of corrosive media, thereby significantly improving the corrosion resistance of the alloy in various corrosive environments.

[0032] Adding 1 to 2% W element, which has a high melting point and good chemical stability, can be dissolved in the alloy matrix to improve the high-temperature strength and hardness of GH163 high-temperature alloy. At the same time, tungsten works synergistically with elements such as chromium and molybdenum to optimize the structure and properties of the oxide film on the alloy surface, thereby enhancing the alloy's corrosion resistance in high-temperature and highly corrosive environments.

[0033] The amount of Ce added is increased to 0.1-0.15%, and 0.02-0.05% of La is added at the same time. The composite addition of multiple rare earth elements can more effectively refine the grains, reduce grain boundary defects, and improve the density and uniformity of GH163 high-temperature alloy, thereby further improving the corrosion resistance and mechanical properties of the alloy.

[0034] To meet the production requirements of the aforementioned alloys, referring to Figures 1-6, a smelting process for high-grade nickel-based superalloys is provided, specifically including the following steps:

[0035] Step 1: Raw material preparation: Prepare raw materials according to the composition of the new high-grade nickel-based superalloy, wherein the purity of the main alloy materials (including Ni, Mo, Co, Cr, and Ti) is not less than 99.5%, and the purity of the remaining alloy materials is not less than 99%.

[0036] Step 2: Vacuum induction smelting. The above alloy materials (except for rare elements) are added to a vacuum smelting furnace for high-temperature smelting. Continuous induction smelting in a relatively vacuum environment can effectively reduce the gas content in the alloy liquid, such as some hydrogen, nitrogen, oxygen or their compounds; it can also effectively reduce the impurity content. The smelting temperature is controlled between 1480℃ and 1550℃ to ensure that the elements are fully melted and uniformly mixed. During the smelting process, existing electromagnetic stirring equipment can also be used for electromagnetic stirring to control the full flow of the molten alloy, accelerate the mixing of different components, and make the components more fully mixed, thereby improving the quality of the final high-temperature alloy.

[0037] Step 3: Plasma beam refining; Use plasma beam refining equipment to perform reciprocating plasma beam scanning on the molten alloy liquid from Step 2. Spiral or grid scanning can also be selected to ensure that the molten alloy liquid is fully refined by plasma beam.

[0038] Plasma beam refining can further remove impurities from the molten alloy, optimize the alloy's performance, and especially prepare for the subsequent addition of rare elements. It avoids excessive burning of rare elements, prevents the formation of harmful phases and deterioration of the microstructure, and ensures the corrosion resistance of the final high-temperature alloy.

[0039] It should be noted that the molten high-temperature alloy here needs to be transferred from smelting and melting to plasma beam equipment for plasma beam scanning. Before plasma beam scanning, the status of the relevant equipment, as well as related cooling systems, vacuum systems, plasma guns, and other equipment, need to be carefully checked to avoid accidents during the plasma beam scanning process.

[0040] Before plasma beam scanning, loading and vacuuming are required. During loading, the quantity and rate of loading must be controlled to avoid material accumulation and insufficient loading. At the same time, the loading time should be controlled to avoid excessive oxidation due to prolonged exposure to air. After loading, the plasma beam equipment is evacuated to control the vacuum level inside the furnace to 10⁻² ~ 10⁻³ Pa. The vacuum level change curve is closely monitored to promptly detect and eliminate any possible air leaks.

[0041] In the large-scale melting of nickel-based superalloys, a segmented heating strategy is adopted. First, the molten superalloy is heated back to at least 1300°C at a relatively low heating rate to ensure uniform heating within the molten alloy. Then, a higher heating rate is used to maintain all metals above their melting points. Following this, a refining process is carried out, with the refining temperature increased to between 1550°C and 1700°C to accelerate the removal of impurities. The refining time needs to be adjusted appropriately based on the scale and specific composition of the superalloy, ranging from 35 to 55 minutes. During the refining process, the temperature distribution within the furnace needs to be monitored, and the scanning process adjusted promptly based on the temperature distribution.

[0042] In the process of plasma beam refining, inert gas protection is also required. Appropriate inert gas is introduced to prevent the high-temperature alloy liquid from being oxidized during the refining process. The slag on the surface is removed regularly, and the floating impurities are discharged in time to avoid the accumulation of impurities.

[0043] Step 4: Addition of rare elements; After the plasma beam refining in Step 3 is completed, the prepared rare elements Ce and La are added to the molten high-temperature alloy. Before adding the rare elements, it is necessary to ensure that all elements in the high-temperature alloy are fully melted and mixed. After adding the rare elements, it is also necessary to continuously control the high-temperature alloy to ensure that the rare elements are evenly distributed after addition.

[0044] It is important to note that during the addition of rare elements, contact with air should be avoided to prevent oxidation. Inert gas protection can also be used by introducing inert gas into the feeding device to prevent the introduction of new impurities.

[0045] It is also important to note that rare elements should be added in batches, slowly and evenly. It is preferable to crush the rare elements into powder and add the powdered rare elements into the molten high-temperature alloy in batches to further ensure the uniformity of rare element addition.

[0046] When adding rare element powder in a single batch, the molten high-temperature alloy in the furnace is stirred in a directional manner. While stirring, rare element powder is continuously added to the surface of the high-temperature alloy in a reciprocating oscillating manner to ensure that the rare element powder can more evenly contact and mix with the molten high-temperature alloy in different areas. A certain time interval is given between each batch of rare element powder additions. During this time interval, the electromagnetic stirring of the molten high-temperature alloy is strengthened to control sufficient disturbance between the upper and lower layers of the molten high-temperature alloy, further improving the full contact between the powdered rare elements and the molten high-temperature alloy in different locations.

[0047] Preferably, before adding the rare element powder, the rare element can be preheated. The rare element adding device can be extended into the furnace, and the rare element powder can be fully preheated by the high temperature atmosphere in the furnace. This reduces the temperature difference between the rare element powder and the high-temperature alloy, and avoids local temperature fluctuations in the alloy liquid, which would affect the uniformity of the alloy.

[0048] Preferredly, rare elements are ground and pulverized to a size between 100 and 400 micrometers. Controlling the grinding of rare elements to this range can further shorten the melting time of rare element powder, enabling rapid melting within a high-temperature range. This results in a high heat transfer rate and a large specific surface area, further achieving rapid pulverization and uniform distribution of high-temperature alloys and rare element powders.

[0049] The rare element powder here is pulverized in batches. The first pulverization is carried out outside the furnace. The first pulverization crushes the lumpy rare elements into particles no larger than 5 mm. This facilitates rapid processing and avoids over-pulverization, which could cause oxidation or agglomeration of the rare element powder outside the furnace, thus preventing the introduction of more impurities and affecting the subsequent addition effect. At the same time, pulverizing to this particle size facilitates subsequent secondary pulverization and grinding, which shortens the overall processing time.

[0050] The second grinding and pulverization is carried out in the furnace, further grinding and pulverizing the rare element particles obtained from the first pulverization to the micron level, which facilitates the subsequent addition of rare elements and improves the effect of their full reaction. The second grinding and pulverization process and the addition process are carried out in an inert atmosphere in the furnace. The ground and pulverized rare element powder is directly added to the furnace to react with the molten high-temperature alloy, avoiding the introduction of impurities and oxidation, and improving the quality of the finished high-temperature alloy.

[0051] To achieve the grinding and addition of the aforementioned rare element powder, a smelting device for high-grade nickel-based high-temperature alloys is also provided, including a rare element grinding and adding device 200. This device grinds and pulverizes millimeter-sized rare element particles into micron-sized rare element powders, and then feeds the ground and pulverized rare element powders into the furnace body 100 to contact and mix with the molten high-temperature alloy.

[0052] Specifically, the smelting equipment for high-grade nickel-based high-temperature alloys includes a limiting base 220, with a grinding body 230 at the upper end of the limiting base 220. The grinding body 230 grinds the granular rare element particles into rare element powder. A drive shaft 234 is rotatably connected to the inner wall of the grinding body 230. A grinding roller 232 is provided at the lower end of the drive shaft 234. The first end of the drive shaft 234 passes through the grinding body 230 and is fixedly connected to a feeding pipe 210. The rare element powder obtained by grinding is fed into the furnace body 100 through the feeding pipe 210 to contact and mix with the molten high-temperature alloy.

[0053] A hollow conveying channel 2341 is formed on the inner wall of the drive shaft 234 and communicates with the feeding pipe 210. A guide opening 2342 is opened on the side wall of the drive shaft 234 and communicates with the interior of the grinding body 230. An air blowing device 240 is provided at the upper end of the grinding body 230. An air blowing device 240 is formed inside the grinding body 230 through the air blowing device 240. While the drive shaft 234 drives the grinding roller 232 to grind and drives the feeding pipe 210 to swing, the air blowing device 240 blows protective gas toward the inner wall of the grinding body 230 to form a protective airflow. The protective airflow carries the micron-level rare element powder into the hollow conveying channel 2341 and finally discharges it from the feeding pipe 210 to contact and mix with the molten high-temperature alloy.

[0054] The aforementioned rare element crushing and adding device 200 is installed at the top of the furnace body. The entire device, especially the feeding pipe 210, is made of high-temperature resistant material and can withstand the high temperature inside the furnace body. At the same time, setting the entire structure inside the furnace body 100 can preheat the rare elements.

[0055] During the generation of the protective airflow, it is necessary to control the furnace body 100 to be in a state of relative negative pressure. The gas blown out by the blowing device 240 can flow directionally within the grinding body 230. During the flow, the rare element powder ground to the micron level is blown up. The protective airflow can flow directionally under the action of negative pressure. The protective airflow can carry the rare element powder through the guide opening 2342 and the hollow conveying channel 2341 in sequence and finally be discharged from the end of the feeding pipe 210. The discharged rare element powder can directly contact and mix with the molten high-temperature alloy below, thus completing the feeding of rare elements.

[0056] The aforementioned protective gas flow is an inert protective gas to prevent the introduction of oxygen from the air, which would cause oxidation of the alloy. It also avoids the introduction of impurities in the final stage, thus ensuring the quality of the final finished alloy.

[0057] Specifically, the blowing device 240 includes two sets of symmetrically arranged strip-shaped blowing nozzles 241, and a connecting main pipe 244. The connecting main pipe 244 is connected to two connecting branch pipes 242, which are respectively connected to the corresponding strip-shaped blowing nozzles 241. A control valve 243 is provided at the connection between the connecting main pipe 244 and the two connecting branch pipes 242. The control valve 243 can control the flow direction of the protective airflow, and can control it to be discharged from the left or right strip-shaped blowing nozzles 241, forming an alternating protective airflow and improving the internal turbulence effect. The frequency of the protective gas blowing and switching can be consistent with the frequency of the grinding roller 232 swinging and grinding. During the movement of the grinding roller 232, the strip-shaped blowing nozzles 241 with the opposite movement direction are controlled to blow out the protective airflow. The blown protective airflow can blow up the rare element powder that has just been ground and finally discharge it from the corresponding channel.

[0058] The preferred strip-shaped air nozzle 241 has its blowing direction tangential to the inner wall arc of the grinding body 230, allowing the blown airflow to flow along the inner wall of the grinding body 230, thus improving the effect on the rare element powder. At the same time, the guide opening 2342 faces away from the grinding roller 232. By setting the guide opening 2342 on the upper side, the rare element powder and rare element particles can be effectively separated, ensuring that the rare element powder is in contact with the molten high-temperature alloy. This increases the specific area of ​​rare element contact, improves the final mixing effect of rare elements with the high-temperature alloy, and improves the quality of the finished high-grade nickel-based high-temperature alloy.

[0059] Furthermore, the second end of the drive shaft 234 passes through the grinding body 230 and is connected to the electrical control equipment. The feeding tube 210 includes a first tube body 211 and a second tube body 212. The second tube body 212 and the first tube body 211 are electrically retractable through a control component. The electrical control equipment is electrically connected to the control component. Through the above structural design, while the feeding tube 210 swings back and forth, the second tube body 212 can be controlled to contract regularly relative to the first tube body 211. After the feeding tube 210 swings to the extreme positions on both sides, the second tube body 212 is controlled to extend. When the feeding tube 210 moves towards the middle position, the second tube body 212 is controlled to contract. During the swinging process, through the above adjustment settings, the second tube body 212 can be positioned on the side close to the surface of the high-temperature alloy to blow out and mix the rare element powder, ensuring the quality of the final alloy and reducing the loss of rare element powder.

[0060] The telescopic control of the second tube 212 can be achieved by setting the drive structure on the side away from the second tube 212. It can be a traditional electric telescopic structure or a pneumatic telescopic structure. The outer side is protected by a heat-insulating structure to reduce the wear and tear on the related structures in the high-temperature environment and ensure the long-term and accurate telescopic control.

[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A process for smelting a high-grade nickel-based superalloy, characterized in that, Includes the following steps: S1. Raw material preparation: Prepare raw materials according to the composition of high-grade nickel-based high-temperature alloys; S2. Vacuum induction smelting: The raw materials from step S1 are added to a vacuum smelting furnace for high-temperature smelting to initially remove impurities and obtain a molten high-temperature alloy. S3. Plasma beam refining: Plasma beam refining equipment is used to reciprocate the plasma beam scanning towards the molten alloy liquid in S2 to remove impurities in the high-temperature alloy again. S4. Addition of rare elements: After plasma beam refining in S3, the prepared rare elements are added to the molten high-temperature alloy. Among them, when adding rare elements, the molten high-temperature alloy is stirred in a directional manner simultaneously. The powdered rare elements are added to the furnace in batches by reciprocating oscillation to contact and mix with the molten high-temperature alloy.

2. A process for smelting a high-grade nickel-based superalloy as claimed in claim 1, wherein, High-grade nickel-based superalloys, specifically including (by weight percentage): The alloy composition is as follows: C 0.04~0.08%, Mo 5.60~6.10%, Cu 0~0.20%, Si 0~0.40%, Mn 0~0.60%, Co 19.0~21.0%, Cr 22.0~25.0%, Ti 1.90~2.40%, Ag 0~0.005%, P 0~0.015%, W 1.0~2.0%; rare elements include Ce 0.1~0.15%, La 0.02~0.05%; the remainder consists of Ni, some impurities, and necessary metallic or non-metallic elements; the purity of Ni, Mo, Co, Cr, and Ti is not less than 99.5%, and the purity of the remaining alloy materials is not less than 99%.

3. The process for smelting of high-grade nickel-based superalloys as claimed in claim 1, wherein, In step S3, the vacuum level inside the furnace is controlled to reach 10⁻² ~ 10⁻³ Pa. A segmented heating strategy is adopted. First, the molten high-temperature alloy is restored to a temperature of not less than 1300°C at a lower heating rate. Then, all metals are kept above the melting point at a higher heating rate. The refining process is then carried out, and the refining temperature is increased to between 1550°C and 1700°C.

4. The process for smelting of high-grade nickel-based superalloys as claimed in claim 1 wherein, The refining time in step S3 is between 35 and 55 minutes, and an inert gas is used for protection during the plasma beam refining process.

5. The process for smelting of high-grade nickel-based superalloys as claimed in claim 1, wherein, The rare element powder is pulverized in batches. The first pulverization is carried out outside the furnace, which pulverizes the lumpy rare elements into millimeter-level particles. The second grinding and pulverization is carried out inside the furnace, which further grinds and pulverizes the rare element particles obtained in the first pulverization to the micron level.

6. A process for smelting a high-grade nickel-based superalloy as claimed in claim 5, wherein, The rare elements are crushed into particles no larger than 5 mm in the first crushing process, and then ground into particles between 100 and 400 micrometers in the second grinding process.

7. A melting apparatus of a high-grade nickel-based superalloy, characterized by comprising: The smelting process for the high-grade nickel-based superalloy as described in any one of claims 1 to 6 includes a rare element crushing and adding device (200). The rare element crushing and adding device (200) includes a limiting base (220), a grinding body (230) is provided at the upper end of the limiting base (220), a drive shaft (234) is rotatably connected to the inner wall of the grinding body (230), a grinding roller (232) is provided at the lower end of the drive shaft (234), the first end of the drive shaft (234) passes through the grinding body (230) and is fixedly connected to an feeding pipe (210), and a hollow conveying channel (2210) is formed on the inner wall of the drive shaft (234). 341) Connected to the delivery pipe (210), the drive shaft (234) has a flow guide opening (2342) on its side wall, which is connected to the inside of the grinding body (230). The upper end of the grinding body (230) is provided with an air blowing device (240). While the drive shaft (234) drives the grinding roller (232) to grind and drives the delivery pipe (210) to swing, the air blowing device (240) blows protective gas toward the inner wall of the grinding body (230) to form a protective airflow. The protective airflow carries the micron-level rare element powder into the hollow conveying channel (2341) and finally discharges from the delivery pipe (210) to contact and mix with the molten high-temperature alloy.

8. The apparatus for smelting a high-grade nickel-based superalloy according to claim 7, wherein The air blowing device (240) includes two sets of symmetrically arranged strip-shaped air blowing nozzles (241) and a connecting main pipe (244). The connecting main pipe (244) is connected to two connecting branch pipes (242). The two connecting branch pipes (242) are respectively connected to the corresponding strip-shaped air blowing nozzles (241). A control valve (243) is provided at the connection point between the connecting main pipe (244) and the two connecting branch pipes (242).

9. The apparatus for smelting a high-grade nickel-based superalloy according to claim 8, wherein The blowing direction of the strip-shaped air nozzle (241) is tangent to the arc of the inner wall of the grinding body (230), and the opening of the guide opening (2342) faces away from the grinding roller (232).

10. The apparatus for smelting a high-grade nickel-based superalloy according to claim 7, wherein The second end of the drive shaft (234) passes through the grinding body (230) and is connected to the electrical control device. The delivery tube (210) includes a first tube body (211) and a second tube body (212). The second tube body (212) and the first tube body (211) are electrically retractable through a control component. The electrical control device is electrically connected to the control component.