Disordered rock salt li 3v 2o 5 fast-charging negative electrode material, preparation method therefor and use thereof
The method of preparing disordered rock salt Li3V2O5 material by solvothermal method solves the safety and complexity problems of existing preparation methods, realizes the preparation of efficient and stable fast-charging anode material, and improves the structural stability and fast-charging performance of the material.
Patent Information
- Application Number
- PCT/CN2026/078099
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-02-10
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for preparing Li3V2O5 materials suffer from problems such as harsh chemical lithiation reaction conditions, poor safety, difficulties in storage and transportation, and complex electrochemical lithiation processes.
Disordered rock salt Li3V2O5 material was prepared by a solvothermal method. By dispersing a vanadium source in an organic solvent and reacting it with a lithium source and a reducing agent, and performing two solvothermal treatments, the use of high-risk organic lithium reagents and battery assembly/disassembly steps was avoided. The reaction parameters were adjusted to control the material composition and morphology.
A simple and efficient method for preparing Li3V2O5 materials was achieved, avoiding lattice defects, improving the structural stability and high-current charge-discharge capability of the material, and exhibiting excellent fast-charging performance.
Smart Images

Figure CN2026078099_12112026_PF_FP_ABST
Abstract
Description
A disordered rock salt Li3V2O5 fast-charging negative electrode material, its preparation method and application Technical Field
[0001] This invention belongs to the field of fast-charging anode materials for lithium-ion batteries, specifically relating to a disordered rock salt Li3V2O5 fast-charging anode material, its preparation method, and its application. Background Technology
[0002] The anode material is a decisive factor affecting charging speed. The slow lithium intercalation process and low lithium intercalation potential of commercial graphite anodes lead to severe lithium plating problems during fast charging. Disordered rock salt Li3V2O5 anode material, with its extremely fast charging speed, low lithium intercalation potential, and cycle stability, is considered a highly promising fast-charging anode material. However, existing preparation methods for Li3V2O5 still have some problems. Currently, Li3V2O5 is mainly prepared by chemical or electrochemical lithiation of V2O5. Chemical lithiation requires the use of highly reactive organic lithium reagents, and the reaction must be carried out in an environment isolated from water and oxygen. Furthermore, organic lithium reagents are flammable and explosive, requiring stringent storage and transportation conditions. Electrochemical lithiation involves fabricating V2O5 into electrode sheets, assembling them with lithium metal to form a battery, and then discharging at a specific voltage to complete the excess lithium ion intercalation into V2O5. After the reaction is complete, the battery is disassembled to obtain the Li3V2O5 material. Electrochemical lithiation involves battery assembly and disassembly, making the process complex. Summary of the Invention
[0003] To overcome the shortcomings of the prior art, the present invention aims to provide a disordered rock salt Li3V2O5 fast-charging anode material, its preparation method and application, and to solve the problems of harsh chemical lithiation reaction conditions, poor safety, difficult storage and transportation, and complex electrochemical lithiation process in the existing preparation process.
[0004] This invention is achieved through the following technical solution:
[0005] A method for preparing a disordered rock salt Li3V2O5 fast-charging negative electrode material includes the following steps:
[0006] S1. Disperse the vanadium source in an organic solvent to obtain a solution A with a vanadium source concentration of 0.01 mol / L-0.2 mol / L. After stirring solution A evenly, carry out the first solvothermal reaction at 180~240℃ for 0.5~12h.
[0007] S2. After the first solvothermal reaction is completed, a lithium source and a reducing agent are added to the resulting solution in sequence, and the mixture is stirred continuously to obtain a precursor solution.
[0008] The molar ratio of the vanadium source to the lithium source is (1:1.4) to (1:1.6), and the concentration of the reducing agent is 0.1-0.5 mol / L.
[0009] S3. The precursor solution is subjected to a second solvothermal reaction at 200~250℃ for 12~72h;
[0010] S4. After the second solvothermal reaction is completed, the obtained product is cooled, centrifuged, washed, dried, and ground to obtain disordered rock salt Li3V2O5 fast-charging negative electrode material.
[0011] Furthermore, in step S1, the vanadium source is any one of ammonium metavanadate, vanadium chloride, vanadium acetylacetonate, and vanadium pentoxide, and the organic solvent is any one of ethanol, isopropanol, ethylene glycol, and methanol.
[0012] Furthermore, in step S2, the lithium source is any one of lithium hydroxide and its hydrate, lithium chloride, lithium nitrate, and lithium acetate, and the reducing agent is any one of hydrazine hydrate and hydroxylamine hydrochloride.
[0013] Furthermore, the molar ratio of the vanadium source to the lithium source is preferably 1:1.48-1:1.52.
[0014] Furthermore, in step S4, the drying method is to dry in a vacuum drying oven at 80°C for 12 hours.
[0015] Furthermore, steps S1 and S2 are performed under closed conditions that isolate oxygen.
[0016] Furthermore, steps S1 and S2 are carried out in an air atmosphere, and step S3 involves bubbling the precursor solution with an inert gas to remove oxygen before the second solvothermal reaction.
[0017] Furthermore, the inert gas is one or more of argon, nitrogen, and helium.
[0018] A disordered rock salt Li3V2O5 fast-charging negative electrode material was obtained according to the above preparation method. The disordered rock salt Li3V2O5 fast-charging negative electrode material has a regular blocky morphology and a thickness of 1~5 μm.
[0019] A lithium-ion battery comprising the aforementioned disordered rock salt Li3V2O5 fast-charging negative electrode material.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0021] This invention is the first to prepare disordered rock salt Li3V2O5 material via a solvothermal method. The process is simple and yields high output. The preparation process does not require the use of high-risk organic lithium reagents and avoids the cumbersome battery assembly and disassembly steps of electrochemical lithiation, allowing direct preparation of Li3V2O5 material. By controlling the process parameters of the solvothermal reaction, the composition, morphology, and microstructure of the obtained material can be controlled. The Li3V2O5 prepared by the method of this invention has a regular cubic morphology and good structural stability. At the same time, the (200) crystal face is fully exposed, which helps to promote the rapid insertion / extraction of lithium ions. The Li3V2O5 prepared by the method of this invention has high crystallinity, which can avoid the lattice defects generated by existing chemical lithiation and electrochemical lithiation methods, and helps to improve the cycle stability and high current charge / discharge capability of the material. Attached Figure Description
[0022] Figure 1 is the XRD pattern of the negative electrode material obtained in Example 1 of the present invention;
[0023] Figure 2 is a SEM image of the negative electrode material obtained in Example 1 of the present invention. Detailed Implementation
[0024] The present invention will be further described in detail below with reference to specific embodiments. These descriptions are for explanation purposes only and are not intended to limit the scope of the invention.
[0025] The first aspect of this disclosure provides a negative electrode material, the phase of which is Li3V2O5. The Li3V2O5 is a lithium-rich disordered rock salt phase, composed of lithium, vanadium and oxygen. The disordered rock salt Li3V2O5 fast-charging negative electrode material has a regular blocky morphology and a thickness of 1~5 μm.
[0026] A second aspect of this disclosure provides a method for preparing the above-mentioned negative electrode material, the technical solution of which is as follows:
[0027] A method for preparing a disordered rock salt Li3V2O5 fast-charging anode material involves dispersing a vanadium source in an organic solvent to obtain a solution A with a vanadium source concentration of 0.01 mol / L to 0.2 mol / L. After stirring evenly, a first solvothermal reaction is carried out at 180–240 °C for 0.5–12 h. After the reaction is completed, the reaction vessel is opened, and a lithium source and a reducing agent are added. The mixture is stirred continuously to obtain a precursor solution. The precursor solution is then subjected to a second solvothermal reaction at 200–250 °C for 12–72 h. After the reaction is completed, the mixture is cooled, centrifuged, washed, dried, and ground to obtain the fast-charging anode material.
[0028] Furthermore, the vanadium source is any one of ammonium metavanadate, vanadium chloride, vanadium acetylacetonate, and vanadium pentoxide, and the organic solvent is any one of ethanol, isopropanol, ethylene glycol, and methanol.
[0029] Furthermore, the lithium source is any one of lithium hydroxide and its hydrate, lithium chloride, lithium nitrate, and lithium acetate; the molar ratio of the vanadium source to the lithium source is (1:1.4) to (1:1.6).
[0030] Furthermore, the reducing agent is either hydrazine hydrate or hydroxylamine hydrochloride.
[0031] Furthermore, the operation is carried out under closed conditions that isolate oxygen.
[0032] Furthermore, the operation is carried out in an air atmosphere, and the precursor solution is deoxygenated by bubbling with an inert gas before the second solvothermal reaction.
[0033] Furthermore, the inert gas used in the bubbling operation is one or more of argon, nitrogen, and helium;
[0034] Furthermore, the drying method is to dry in a vacuum drying oven at 80°C for 12 hours.
[0035] A third aspect of this disclosure provides a negative electrode, comprising the negative electrode material described in the first aspect of this disclosure.
[0036] The negative electrode material provided in this disclosure includes a copper foil current collector and a negative electrode coating, wherein the negative electrode coating includes the negative electrode material, a conductive agent, and a binder;
[0037] Furthermore, based on the total weight of the negative electrode coating, the content of the negative electrode material is 60-90% by weight, the content of the conductive agent is 30-10% by weight, and the balance is the negative electrode binder;
[0038] Furthermore, the thickness of the negative electrode coating is 15~100 μm, preferably 20-50 μm.
[0039] In this disclosure, the negative electrode conductive agent and binder can be materials conventionally selected in the art. For example, the conductive agent can be one or more of acetylene black, Super P, Ketjen black, multi-walled carbon nanotubes, and single-walled carbon nanotubes; the binder can be one or more of carboxymethyl cellulose, polyacrylic acid, and polyvinylidene fluoride. The solvent is deionized water or N-methylpyrrolidone; the negative electrode coating can be obtained using conventional slurry coating methods, and the coating can be performed using conventional operations.
[0040] A fourth aspect of this disclosure provides a lithium-ion battery including the negative electrode described in the third aspect of this disclosure.
[0041] The lithium-ion battery also includes a positive electrode, a separator, and an electrolyte, which can be of conventional types selected in the art. For example, the positive electrode can be a lithium sheet, lithium cobalt oxide, lithium iron phosphate, ternary materials, etc.; the separator can be a Celgard 2400 polypropylene membrane and polyethylene, etc.; the electrolyte includes a lithium salt, a solvent, and additives, wherein the lithium salt can be lithium fluorophosphate, the electrolyte solvent can be ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, etc., and the additives can be fluoroethylene carbonate, lithium fluorosulfonate, etc.
[0042] In this disclosure, the lithium-ion battery is assembled using methods conventional in the art.
[0043] Example 1
[0044] (1) Weigh 2 mmol of analytical grade ammonium metavanadate and disperse it in 70 mL of anhydrous ethanol. The concentration is 0.0286 mol / L. After stirring for 0.5 h, a pale yellow transparent solution A is formed. Transfer solution A to a polystyrene liner with a stainless steel outer vessel for the first solvothermal reaction at 240 °C for 1 h.
[0045] (2) After the reaction is completed and cooled to room temperature, open the reaction vessel in the glove box; add 3 mmol of lithium hydroxide monohydrate to the reaction vessel, wherein the molar ratio of ammonium metavanadate to lithium hydroxide monohydrate is 1:1.5; continue stirring for 0.5 h to obtain suspension B; add 1 mL of hydrazine hydrate with a concentration of 0.23 mol / L to suspension B, and continue stirring for 0.5 h to obtain precursor solution C;
[0046] (3) The above steps (1) and (2) are carried out under closed conditions that isolate oxygen. The polystyrene liner containing the precursor solution C is placed into the stainless steel outer vessel for the second solvothermal reaction. The reaction temperature is 200℃ and the time is 60h.
[0047] (4) After the reaction is completed and cooled to room temperature, the precipitate is separated by centrifugation and washed with anhydrous ethanol. The washed product is placed in a vacuum drying oven and dried at 80°C for 12 hours. The dried sample is then ground to obtain the Li3V2O5 fast-charging negative electrode material.
[0048] The XRD pattern of the negative electrode material obtained in this embodiment is shown in Figure 1. As can be seen from Figure 1, the diffraction peak positions are completely consistent with those of the previously reported Li3V2O5, indicating that the Li3V2O5 material was successfully prepared.
[0049] The SEM image of the negative electrode material obtained in this embodiment is shown in Figure 2. As can be seen from Figure 2, the material exhibits a regular blocky morphology with a thickness of 3.5 μm. It has higher structural stability, which is beneficial to improving the cycle life of the battery.
[0050] Example 2
[0051] This embodiment refers to the method in Embodiment 1, but differs from Embodiment 1 in that:
[0052] The vanadium source used was vanadium chloride, the lithium source used was lithium chloride, and the organic solvent was isopropanol. The remaining processes were the same as in Example 1, and the negative electrode material was prepared.
[0053] Example 3
[0054] This embodiment refers to the method in Embodiment 1, but differs from Embodiment 1 in that:
[0055] The lithium source used was lithium nitrate, and the first solvothermal reaction was carried out at 180 °C for 12 h. The remaining processes were the same as in Example 1, and the negative electrode material was prepared.
[0056] Example 4
[0057] This embodiment refers to the method in Embodiment 1, but differs from Embodiment 1 in that:
[0058] The vanadium source used was vanadium acetylacetone, and the second solvothermal reaction was carried out at 250°C for 12 hours. The remaining processes were the same as in Example 1, and the negative electrode material was prepared.
[0059] Example 5
[0060] This embodiment refers to the method in Embodiment 1, but differs from Embodiment 1 in that:
[0061] The second solvothermal reaction was carried out at 200°C for 72 hours. Steps (1) and (2) were carried out in an air atmosphere. In step (3), nitrogen was used to bubble the precursor to remove oxygen for 10 minutes. The rest of the process was the same as in Example 1, and the negative electrode material was prepared.
[0062] Comparative Example 1
[0063] This comparative example follows the method described in Example 1, except that the first solvothermal reaction is omitted, and lithium hydroxide and hydrazine hydrate are directly added to the ammonium metavanadate solution to carry out the second solvothermal reaction. The remaining operations are the same as in Example 1, resulting in a non-disordered rock salt phase mixture.
[0064] The XRD pattern of the material obtained in this comparative example is shown in Figure 1. As can be seen from Figure 1, the obtained product is a non-disordered rock salt phase material, and the phase is a mixture of V2O3 and Li3VO4. Compared with Example 1, this demonstrates that the stepwise solvothermal technology disclosed in this invention is the key to preparing Li3V2O5 disordered rock salt materials.
[0065] Test case
[0066] This test example illustrates the application effect of the negative electrode material prepared in Example 1 in lithium-ion batteries.
[0067] Using N-methylpyrrolidone as a solvent, the negative electrode material obtained in Example 1, acetylene black (conductive agent), and polyvinylidene fluoride (binder) were mixed evenly at a mass ratio of 6:3:1 to obtain a slurry. This slurry was then coated onto a copper foil current collector and placed in a vacuum drying oven at 80°C for 12 hours to obtain the negative electrode. This negative electrode includes a negative electrode coating, in which the negative electrode material content is 60% by weight, the conductive agent content is 30% by weight, and the binder content is 10% by weight.
[0068] The battery uses lithium foil as the positive electrode, Celgard 2400 polypropylene membrane as the battery separator, and a mixed solution of 1 mol / L lithium hexafluorophosphate in ethylene carbonate (EC) and dimethyl carbonate (DMC) (solvent volume ratio of 1:1) as the electrolyte.
[0069] The above-mentioned positive and negative electrode materials, separator and electrolyte are assembled into CR2032 coin cells using conventional methods in the art.
[0070] The electrochemical performance of the Li3V2O5 anode material was tested using the Xinwei Battery Testing System. The assembled coin cells were discharged at room temperature with a constant current density of 100 mA / g to 0.01 V, and then charged with a constant current density of 100 mA / g to 2.0 V. The discharge specific capacity and charge specific capacity of the first cycle were recorded. Cyclic testing was performed using this process, and the capacity retention after 100 cycles was calculated.
[0071] Rate performance test: The assembled coin cells were discharged to 0.01V at a constant current density of 100 mA / g at room temperature, and then charged to 2.0V at a constant current density of 100 mA / g. The charging capacity and time required at different current densities were recorded.
[0072] The test results of the negative electrode material obtained in Example 1 in lithium-ion batteries are summarized in Tables 1 and 2 below.
[0073] Table 1 Cycle performance of the negative electrode material obtained in Example 1 in lithium-ion batteries
[0074] Initial discharge specific capacity (mAh / g) Initial charge specific capacity (mAh / g) 100-cycle discharge specific capacity (mAh / g) 100-cycle charge specific capacity (mAh / g) 133.05 176.03 276.83 277.07
[0075] Table 2 Rate performance and time required to complete one charge of the negative electrode material obtained in Example 1 in lithium-ion batteries
[0076] Current density (A / g) Specific charging capacity (mAh / g) Time required to complete one charge 0.1279.02h 46min 0.2255.91h 10min 0.5230.228min 1215.413min 2194.96min 5136.01.65min
[0077] The test data shows that the material has a low initial charge-discharge capacity, but after 100 cycles, the capacity stabilizes at 277 mAh / g, demonstrating stable cycle performance. More importantly, the test data at high current densities indicate that the material prepared in this invention has excellent fast-charging performance; for example, at a current density of 5 A / g, it can be fully charged in just 1.65 minutes, demonstrating superior fast-charging performance. Example 6
[0078] (1) Weigh 0.35 mmol of vanadium pentoxide and disperse it in 70 mL of ethylene glycol at a concentration of 0.005 mol / L. Stir for 0.5 h to form suspension A. Transfer suspension A to a polystyrene liner with a stainless steel outer vessel and react at 200 °C for 8 h.
[0079] (2) After the reaction is completed and cooled to room temperature, open the reaction vessel in the glove box; add 1.12 mmol of lithium nitrate to the reaction vessel, wherein the molar ratio of vanadium pentoxide to lithium nitrate is 0.5:1.6; continue stirring for 0.5 h to obtain suspension B; add 0.43 mL of hydrazine hydrate with a concentration of 0.1 mol / L to suspension B, and continue stirring for 0.5 h to obtain precursor C;
[0080] (3) Steps (1) and (2) are carried out in an air atmosphere. The precursor solution C is deoxygenated by bubbling with nitrogen for 10 minutes. The polystyrene liner containing the precursor solution C is placed into a stainless steel outer vessel for a second solvothermal reaction at a temperature of 250°C for 12 hours.
[0081] (4) After the reaction is completed and cooled to room temperature, the precipitate is separated by centrifugation and washed with anhydrous ethanol. The washed product is placed in a vacuum drying oven and dried at 80°C for 12 hours. The dried sample is then ground to obtain the Li3V2O5 fast-charging negative electrode material. Example 7
[0082] (1) Weigh 14 mmol of vanadium acetylacetonate and disperse it in 70 mL of methanol to a concentration of 0.2 mol / L. After stirring for 0.5 h, a blue-green transparent solution A is formed. Transfer solution A to a polystyrene liner with a stainless steel outer vessel and react at 180 °C for 12 h.
[0083] (2) After the reaction is completed and cooled to room temperature, open the reaction vessel in the glove box; add 20.72 mmol of lithium acetate to the reaction vessel, wherein the molar ratio of vanadium acetylacetonate to lithium acetate is 1:1.48; continue stirring for 0.5 h to obtain suspension B; add 2.43 g of hydroxylamine hydrochloride with a concentration of 0.5 mol / L to suspension B, and continue stirring for 0.5 h to obtain precursor C;
[0084] (3) Steps (1) and (2) are carried out in an air atmosphere. The precursor solution C is deoxygenated by helium bubbling for 10 min. The polystyrene liner containing the precursor solution C is placed into a stainless steel outer vessel for a second solvothermal reaction at a temperature of 220°C for 72 h.
[0085] (4) After the reaction is completed and cooled to room temperature, the precipitate is separated by centrifugation and washed with anhydrous ethanol. The washed product is placed in a vacuum drying oven and dried at 80°C for 12 hours. The dried sample is then ground to obtain the Li3V2O5 fast-charging negative electrode material. Example 8
[0086] (1) Weigh 7 mmol of vanadium chloride and disperse it in 70 mL of isopropanol at a concentration of 0.1 mol / L. Stir for 0.5 h to form suspension A. Transfer suspension A to a polystyrene liner with a stainless steel outer vessel and react at 220 °C for 0.5 h.
[0087] (2) After the reaction is completed and cooled to room temperature, open the reaction vessel in the glove box; add 9.8 mmol of lithium chloride to the reaction vessel, wherein the molar ratio of vanadium chloride to lithium chloride is 1:1.4; continue stirring for 0.5 h to obtain suspension B; add 1.39 mL of hydrazine hydrate with a concentration of 0.4 mol / L to suspension B, and continue stirring for 0.5 h to obtain precursor C;
[0088] (3) After steps (1) and (2) are carried out under closed conditions in the absence of oxygen, the polystyrene liner containing the precursor solution C is placed into the stainless steel outer vessel for a second solvothermal reaction at a temperature of 240°C for 40 hours.
[0089] (4) After the reaction is completed and cooled to room temperature, the precipitate is separated by centrifugation and washed with anhydrous ethanol. The washed product is placed in a vacuum drying oven and dried at 80°C for 12 hours. The dried sample is then ground to obtain the Li3V2O5 fast-charging negative electrode material. Example 9
[0090] (1) Weigh 14 mmol of vanadium acetylacetonate and disperse it in 70 mL of ethylene glycol to a concentration of 0.2 mol / L. After stirring for 0.5 h, a pale yellow transparent solution A is formed. Transfer solution A to a polystyrene liner with a stainless steel outer vessel and react at 200 °C for 8 h.
[0091] (2) After the reaction is completed and cooled to room temperature, open the reaction vessel in the glove box; add 21.28 mmol of lithium nitrate to the reaction vessel, wherein the molar ratio of vanadium acetylacetonate to lithium nitrate is 1:1.52; continue stirring for 0.5 h to obtain suspension B; add 1.49 mL of hydroxylamine hydrochloride with a concentration of 0.5 mol / L to suspension B, and continue stirring for 0.5 h to obtain precursor C;
[0092] (3) After steps (1) and (2) are carried out under closed conditions in the absence of oxygen, the polystyrene liner containing the precursor solution C is placed into the stainless steel outer vessel for a second solvothermal reaction at a temperature of 220°C for 72 hours.
[0093] (4) After the reaction is completed and cooled to room temperature, the precipitate is separated by centrifugation and washed with anhydrous ethanol. The washed product is placed in a vacuum drying oven and dried at 80°C for 12 hours. The dried sample is then ground to obtain the Li3V2O5 fast-charging negative electrode material.
Claims
1. A method for preparing a disordered rock salt Li3V2O5 fast-charging negative electrode material, characterized in that, Includes the following steps: S1. Disperse the vanadium source in an organic solvent to obtain a solution A with a vanadium source concentration of 0.01 mol / L-0.2 mol / L. After stirring solution A evenly, carry out the first solvothermal reaction at 180~240℃ for 0.5~12h. S2. After the first solvothermal reaction is completed, a lithium source and a reducing agent are added to the resulting solution in sequence, and the mixture is stirred continuously to obtain a precursor solution. The molar ratio of the vanadium source to the lithium source is (1:1.4) to (1:1.6), and the concentration of the reducing agent is 0.1-0.5 mol / L. S3. The precursor solution is subjected to a second solvothermal reaction at 200~250℃ for 12~72h; S4. After the second solvothermal reaction is completed, the obtained product is cooled, centrifuged, washed, dried, and ground to obtain disordered rock salt Li3V2O5 fast-charging negative electrode material.
2. The preparation method of a disordered rock salt Li3V2O5 fast-charging negative electrode material according to claim 1, characterized in that, In step S1, the vanadium source is any one of ammonium metavanadate, vanadium chloride, vanadium acetylacetonate, and vanadium pentoxide, and the organic solvent is any one of ethanol, isopropanol, ethylene glycol, and methanol.
3. The preparation method of a disordered rock salt Li3V2O5 fast-charging negative electrode material according to claim 1, characterized in that, In step S2, the lithium source is any one of lithium hydroxide and its hydrate, lithium chloride, lithium nitrate, and lithium acetate, and the reducing agent is any one of hydrazine hydrate and hydroxylamine hydrochloride.
4. The preparation method of a disordered rock salt Li3V2O5 fast-charging negative electrode material according to claim 1, characterized in that, The preferred molar ratio of the vanadium source to the lithium source is 1:1.48 to 1:1.
52.
5. The preparation method of a disordered rock salt Li3V2O5 fast-charging negative electrode material according to claim 1, characterized in that, In step S4, the drying method is to dry in a vacuum drying oven at 80°C for 12 hours.
6. The preparation method of a disordered rock salt Li3V2O5 fast-charging negative electrode material according to claim 1, characterized in that, Steps S1 and S2 are performed under closed conditions that isolate oxygen.
7. The preparation method of a disordered rock salt Li3V2O5 fast-charging negative electrode material according to claim 1, characterized in that, Steps S1 and S2 are carried out in an air atmosphere, and step S3 involves bubbling the precursor solution with an inert gas to remove oxygen before the second solvothermal reaction.
8. The preparation method of a disordered rock salt Li3V2O5 fast-charging negative electrode material according to claim 7, characterized in that, The inert gas is one or more of argon, nitrogen, and helium.
9. A disordered rock salt Li3V2O5 fast-charging negative electrode material obtained by the preparation method according to any one of claims 1-8, characterized in that, The disordered rock salt Li3V2O5 fast-charging negative electrode material has a regular blocky morphology and a thickness of 1~5 μm.
10. A lithium-ion battery, characterized in that, It contains the disordered rock salt Li3V2O5 fast-charging negative electrode material as described in claim 8.