Coated separator for lithium battery and preparation method therefor, and lithium battery

By coating the lithium-ion battery separator with a copolymer polymer material that has a low glass transition temperature and narrow particle size distribution, the problems of high energy consumption and low production yield in the prior art have been solved, achieving efficient bonding under low temperature and low pressure, and improving the safety and production efficiency of lithium batteries.

WO2026233161A1PCT designated stage Publication Date: 2026-11-12SHANGHAI ENERGY NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/093294
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-04-27
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing lithium-ion battery separators suffer from high energy consumption, low production yield, and are prone to short circuits during the bonding process, especially due to the production challenges caused by the high melting point and poor degradability of PVDF copolymers.

Method used

Using fluorine-free copolymer polymer materials, an adhesive coating is applied to the surface of the base film. The copolymer polymer materials with low glass transition temperature and narrow particle size distribution are combined with adhesives, inorganic heat-resistant fillers and surface additives to achieve low-temperature and low-pressure bonding between the lithium battery coated separator and the electrode.

Benefits of technology

It reduces energy consumption in the battery manufacturing process, improves production yield, avoids the generation of separator pinholes, and enhances the safety and adhesion of lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026093294_12112026_PF_FP_ABST
    Figure CN2026093294_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A coated separator for a lithium battery and a preparation method therefor, and a lithium battery, relating to the technical field of battery materials. When f(p,T) is 0.15-0.35, a bonding force between the coated separator for a lithium battery and an electrode sheet is greater than or equal to 1.0 N / m, wherein f(p,T)=1 / ln(p×T); p is the hot‑pressing pressure applied when the coated separator for a lithium battery is bonded to the electrode sheet, and 1 MPa≤p≤10 MPa; T is the hot-pressing temperature when the coated separator for a lithium battery is bonded to the electrode sheet, and 25°C≤T≤90°C. The bonding force between the coated separator for a lithium battery and the electrode sheet increases rapidly as the temperature rises or the pressure increases, so that a relatively large increase in bonding force can be achieved with a relatively small amount of energy. This not only facilitates reduction of energy consumption during battery preparation, but also avoids or reduces the probability of battery cell short-circuiting caused by pinholes formed in the separator due to excessively high composite pressure in battery production, thereby improving the production yield.
Need to check novelty before this filing date? Find Prior Art

Description

A lithium battery coated separator and its preparation method and lithium battery

[0001] Cross-references to related applications

[0002] This disclosure claims priority to Chinese Patent Application No. 202510580483.5, filed on May 7, 2025, entitled "A Lithium Battery Coated Separator and its Preparation Method and a Lithium Battery", the entire contents of which are incorporated herein by reference. Technical Field

[0003] This disclosure relates to the field of battery materials technology, and more specifically, to a lithium battery coated separator, its preparation method, and a lithium battery. Background Technology

[0004] In the structure of lithium-ion batteries, the separator is one of the key internal components. The separator not only isolates the positive and negative electrodes to prevent short circuits, but also blocks current conduction in the battery when it overheats through its pore-closing function. The performance of the separator determines the battery's interface structure, internal resistance, and other characteristics, directly affecting the battery's capacity, cycle performance, and safety performance. A high-performance separator plays a crucial role in improving the overall performance of the battery.

[0005] Currently, commercially available lithium-ion battery separators are mainly polyolefin separators based on polyethylene (PE) and / or polypropylene (PP), including single-layer PE separators, single-layer PP separators, and three-layer PP / PE / PP composite membranes. Existing polyolefin separator production processes can be divided into two main categories: dry process and wet process. Currently, 60% to 70% of the separator market mainly uses the wet process.

[0006] With the development of the electric vehicle industry, improving battery performance is becoming increasingly important. Existing polyvinylidene fluoride (PVDF) copolymer coated separators possess inherent adhesive properties, which can bond the separator and electrode together, improving battery rigidity. Therefore, PVDF copolymer coatings represent an important development direction. However, PVDF, a perfluorinated or polyfluoroalkyl substance, is difficult to degrade, posing a risk of restriction or ban. Furthermore, PVDF has a high melting point, requiring high temperature and pressure conditions to heat-press the electrode and separator together to achieve bonding. This results in high energy consumption during production, and the high pressure can easily cause pinholes in the separator, leading to short circuits in the battery cell and reducing production yield.

[0007] In view of this, this disclosure is hereby made.

[0008] Public content

[0009] The purpose of this disclosure includes providing a lithium battery coated separator, a method for preparing the same, and a lithium battery.

[0010] This disclosure can be implemented as follows:

[0011] In a first aspect, this disclosure provides a lithium battery coated separator, wherein when the hot-press response factor f(p,T) is 0.15 to 0.35, the adhesion force between the lithium battery coated separator and the electrode is ≥1.0 N / m; wherein f(p,T)=1 / ln(p×T), p is the hot-press pressure when the lithium battery coated separator is bonded to the electrode, in MPa, 1MPa≤p≤10MPa; T is the hot-press temperature when the lithium battery coated separator is bonded to the electrode, in °C, 25℃≤T≤90℃.

[0012] In an optional embodiment, the lithium battery coated separator includes a base film and an adhesive coating applied to the surface of the base film;

[0013] The adhesive coating contains a copolymer polymer material, and the glass transition temperature of the copolymer polymer material is less than or equal to the hot-pressing temperature when the lithium battery coated separator is bonded to the electrode.

[0014] In an optional embodiment, the copolymer polymer is obtained by copolymerizing at least two of styrene, acrylic acid, acrylate monomers, polyacrylate monomers, olefin monomers, acrylamide monomers, and vinyl acetate monomers.

[0015] In an optional embodiment, the copolymeric polymer material includes at least one of acrylate copolymers and thermoplastic elastomers.

[0016] In an optional embodiment, the thermoplastic elastomer includes at least one of SBS, SIS, SEBS, SEPS, TPV, TPB, and TPI.

[0017] In an optional embodiment, the glass transition temperature of the acrylate copolymer is 25°C to 90°C.

[0018] In an optional embodiment, the glass transition temperature of the acrylate copolymer is 50°C to 70°C.

[0019] In an optional embodiment, the glass transition temperature of the acrylate copolymer is 50°C to 60°C.

[0020] In an optional embodiment, the glass transition temperature of the thermoplastic elastomer is -70°C to 120°C.

[0021] In an optional embodiment, the copolymeric polymer material also has at least one of the following characteristics:

[0022] Feature 1: The copolymer polymer material is in particulate form, and the particle size of the copolymer polymer material is 0.3μm~0.8μm;

[0023] Feature 2: The copolymer polymer material is granular, and the (Dv) of the copolymer polymer material 90 -Dv 10 ) / Dv 50 ≤1.5 and >0.

[0024] In an optional embodiment, the copolymer polymer material (Dv) 90 -Dv 10 ) / Dv 50 >0 and <1.

[0025] In an optional embodiment, the copolymer polymer material (Dv) 90 -Dv 10 ) / Dv 50 The value ranges from 0.50 to 0.95.

[0026] In an optional embodiment, the adhesive coating further comprises at least one of an adhesive, an inorganic heat-resistant filler, and a surface additive.

[0027] In an optional embodiment, the adhesive includes at least one of polyacrylate resins, PVP, PVA, and modified SBR.

[0028] In an optional embodiment, the inorganic heat-resistant filler includes metal oxides.

[0029] In an optional embodiment, the inorganic heat-resistant filler includes at least one of alumina, boehmite, and barium titanate.

[0030] In an optional embodiment, the particle size of the inorganic heat-resistant filler is 0.1 μm to 2 μm.

[0031] In an optional embodiment, the surface additive includes at least one of a wetting agent and a dispersant.

[0032] In optional embodiments, the surface additives include at least one of acrylates, fatty alcohol polyoxyethylene ethers, silicones, and acrylic polymers.

[0033] In an optional embodiment, the base film includes a polyethylene base film, a polypropylene base film, or a composite base film of polyethylene and polypropylene.

[0034] And / or, the thickness of the base film is 2μm to 20μm;

[0035] And / or, the thickness of the adhesive coating is 0.5μm to 5μm.

[0036] Secondly, this disclosure provides a method for preparing a lithium battery coated separator as described in any of the foregoing embodiments, comprising the following steps: preparing an adhesive coating on the surface of a base film.

[0037] In an optional embodiment, the preparation of the adhesive coating includes: mixing the raw materials for the adhesive coating with water to obtain a slurry; coating the slurry onto the surface of the base film and drying it.

[0038] In an optional embodiment, the raw material for preparing the adhesive coating is a copolymer polymer.

[0039] In an optional embodiment, the raw materials for preparing the adhesive coating include at least one of an adhesive, an inorganic heat-resistant filler, a surface additive, and a copolymer polymer.

[0040] In an optional embodiment, the mass ratio of adhesive to copolymer polymer is (2-10):(4-15).

[0041] In an optional embodiment, the mass ratio of inorganic heat-resistant filler to copolymerized polymer material is (80-90):(4-15).

[0042] In an optional embodiment, the mass ratio of surface additive to copolymerized polymer is (0.1-3):(4-15).

[0043] In an optional embodiment, the raw materials for preparing the adhesive coating, by weight, include 2 to 10 parts of adhesive, 80 to 90 parts of inorganic heat-resistant filler, 0.1 to 3 parts of surface additives, and 4 to 15 parts of copolymer polymer material.

[0044] Thirdly, this disclosure provides a lithium battery, which includes an electrode and a lithium battery coated separator as described in any of the foregoing embodiments, wherein the lithium battery coated separator is adhered to the surface of the electrode.

[0045] The beneficial effects of this disclosure include:

[0046] The lithium battery coated separator proposed in this disclosure has the following characteristics: when f(p,T) is 0.15 to 0.35, the adhesion force between the lithium battery coated separator and the electrode is ≥1.0 N / m; where f(p,T)=1 / ln(p×T), p is the hot-pressing pressure when the lithium battery coated separator is bonded to the electrode, in MPa, 1MPa≤p≤10MPa; T is the hot-pressing temperature when the lithium battery coated separator is bonded to the electrode, in °C, 25℃≤T≤90℃.

[0047] The lithium battery coated separator that meets the above characteristics has a fast temperature response rate and pressure response. That is, the adhesion between the lithium battery coated separator and the electrode increases rapidly with the increase of temperature or pressure. Therefore, the lithium battery coated separator can achieve a significant increase in adhesion with less energy. On the one hand, it helps to reduce energy consumption in the battery manufacturing process. On the other hand, it can avoid or improve the probability of pinholes in the separator caused by excessive composite pressure in battery production, which may lead to short circuits in the cell, thereby improving the production yield. Attached Figure Description

[0048] To more clearly illustrate the technical solutions of the embodiments of this disclosure, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of this disclosure and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0049] Figure 1 is a schematic diagram of the adhesion effect between the lithium battery coated separator and the electrode when the particle size distribution of the copolymer polymer material is narrow.

[0050] Figure 2 is a schematic diagram of the adhesion effect between the lithium battery coated separator and the electrode when the particle size distribution of the copolymer polymer material is relatively wide. Detailed Implementation

[0051] To make the objectives, technical solutions, and advantages of the embodiments of this disclosure clearer, the technical solutions in the embodiments of this disclosure will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0052] The following provides a detailed description of the lithium battery coated separator, its preparation method, and the lithium battery itself.

[0053] This disclosure provides a lithium battery coated separator. When the hot-press response factor f(p,T) is 0.15 to 0.35, the adhesion force between the lithium battery coated separator and the electrode is ≥1.0 N / m. Wherein, f(p,T)=1 / ln(p×T), p is the hot-press pressure when the lithium battery coated separator is bonded to the electrode, in MPa, 1MPa≤p≤10MPa; T is the hot-press temperature when the lithium battery coated separator is bonded to the electrode, in °C, 25℃≤T≤90℃.

[0054] In some optional implementations, p can be 1MPa, 2MPa, 3MPa, 4MPa, 5MPa, 6MPa, 7MPa, 8MPa, 9MPa or 10MPa, or any other value or any range of value within the range of 1MPa to 10MPa.

[0055] In some optional implementations, T can be 25℃, 30℃, 35℃, 40℃, 45℃, 50℃, 55℃, 60℃, 65℃, 70℃, 75℃, 80℃, 85℃ or 90℃, or any other value or range within the range of 25℃ to 90℃.

[0056] In some optional embodiments, when the thermo-pressure response factor f(p,T) is 0.15 to 0.2, the adhesion force between the lithium battery coated separator and the electrode is ≥1.0 N / m.

[0057] In some preferred embodiments, when hot-pressed at 60°C and 3MPa, the adhesion between the lithium battery coated separator and the electrode is ≥1.0N / m; in some preferred embodiments, when hot-pressed at 85°C and 3MPa, the adhesion between the lithium battery coated separator and the electrode is ≥6.5N / m.

[0058] The lithium battery coated separator proposed in this disclosure, which meets the above characteristics, has a fast temperature response rate and pressure response. That is, the adhesion between the lithium battery coated separator and the electrode increases rapidly with the increase of temperature or pressure. Therefore, the lithium battery coated separator can achieve a significant increase in adhesion with less energy. On the one hand, it helps to reduce energy consumption in the battery manufacturing process, and on the other hand, it can avoid or improve the probability of pinholes in the separator caused by excessive composite pressure in battery production, which would lead to short circuits in the cell, thereby improving the production yield.

[0059] In this disclosure, the lithium battery coated separator includes a base film and an adhesive coating applied to the surface of the base film.

[0060] The adhesive coating contains a copolymer polymer. The glass transition temperature of this copolymer polymer is less than or equal to the hot-pressing temperature during the bonding of the lithium battery separator and the electrode.

[0061] In some alternative embodiments, the copolymeric polymer is fluorine-free. For example, the copolymeric polymer can be obtained by copolymerizing at least two of styrene, acrylic acid, acrylate monomers, polyacrylate monomers, olefin monomers, acrylamide monomers, and vinyl acetate monomers.

[0062] In some preferred embodiments, the copolymeric polymeric material includes at least one of acrylate copolymers and thermoplastic elastomers.

[0063] The glass transition temperature of the acrylate copolymer can be between 25°C and 90°C, such as 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, or 90°C, or any other value within the range of 25°C to 90°C. In some preferred embodiments, the glass transition temperature of the acrylate copolymer is 50°C to 70°C; in some even preferred embodiments, the glass transition temperature of the acrylate copolymer is 50°C to 60°C.

[0064] Thermoplastic elastomers may, by way of example but not limitation, include at least one of styrene-based thermoplastic elastomers (SBS), styrene-isoprene-styrene block copolymers (SIS), hydrogenated styrene-butadiene-styrene block copolymers (SEBS), styrene-ethylene / ethylene / propylene-styrene block copolymers (SEPS), thermoplastic elastomer dynamic vulcanizates (TPV), diene-based thermoplastic elastomers (TPB), and trans-isoprene rubber (TPI). The glass transition temperature of the thermoplastic elastomer can be from -70°C to 120°C, such as -70°C, -65°C, -60°C, -55°C, -50°C, -45°C, -40°C, -35°C, -30°C, -25°C, -20°C, -15°C, -10°C, 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, or 30°C, or other values ​​within the range of -70°C to 120°C.

[0065] The copolymer polymer material used in this disclosure is fluorine-free and has a low glass transition temperature. On the one hand, it avoids the problem of difficult degradation of fluorine-containing copolymers, and on the other hand, it can achieve bonding with the electrode at a lower hot pressing temperature.

[0066] In some alternative embodiments, the copolymer polymer material is in particulate form, and its particle size (D) V50 The particle size can be 0.1 μm to 2 μm, such as 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, or 2 μm, or any value within the range of 0.1 μm to 2 μm. In some typical embodiments, the particle size of the copolymer polymer is 0.5 μm to 0.8 μm.

[0067] If the particle size of the copolymer polymer is less than 0.1 μm, it is not conducive to distribution on the coating surface and cannot establish effective bonding sites with the electrode. If the particle size of the copolymer polymer is greater than 2 μm, it is not conducive to uniform distribution in the thickness direction of the coating surface, resulting in the surface part of the copolymer polymer being isolated and unable to establish contact sites.

[0068] In some alternative embodiments, the copolymer polymer material is in particulate form, and its (Dv) 90 -Dv 10 ) / Dv 50 ≤1.5 and >0, such as 1.5, 1.2, 1.0, 0.99, 0.95, 0.90, 0.85, 0.80, 0.75, 0.70, 0.65, 0.60, 0.55, 0.5, 0.4, 0.3, 0.2, 0.1, or 0.05, etc., or other values ​​within the range of ≤1.5 and >0. In some preferred embodiments, the (Dv) of the copolymer polymer material... 90 -Dv 10 ) / Dv 50 A value between 0.50 and 0.95, where <1 and >0, is preferred for better adhesion. If the copolymer polymer material's (Dv) 90 -Dv 10 ) / Dv 50 A value greater than 1.5 is not conducive to establishing an effective bond between the coated separator and the electrode in lithium batteries.

[0069] The above (Dv) 90 -Dv 10 ) / Dv 50 This can be understood as the particle size distribution. As shown in Figure 1, when the particle size distribution is narrow, the size of the copolymer polymer material is basically the same, which can effectively bond the lithium battery coated separator and the electrode at all positions. As shown in Figure 2, when the particle size distribution is wide, the size of the copolymer polymer material varies greatly. Some positions of the lithium battery coated separator and the electrode can be effectively bonded, while some positions cannot be effectively bonded.

[0070] In some typical embodiments, the copolymeric polymer is fluorine-free, and the glass transition temperature of the copolymeric polymer is 50°C to 70°C (more preferably 50°C to 60°C), (Dv 90 -Dv 10 ) / Dv 50 <1 and >0.

[0071] Continuing from the above, this disclosure utilizes copolymer polymer particles that are fluorine-free, have a low glass transition temperature, and a narrow particle size distribution, which can greatly improve the adhesion between the separator and the electrode, reduce the hot pressing temperature, and thus reduce production energy consumption.

[0072] It should be noted that traditional separators have high hot-pressing temperatures (at least 85°C and above, usually above 90°C) and require high energy. The solution provided in this disclosure can achieve the bonding effect of traditional separators at a hot-pressing temperature of 60°C to 80°C. This not only reduces energy consumption in the battery manufacturing process, but also avoids or improves the probability of short circuits in the battery cell caused by pinholes in the separator due to excessive composite pressure during battery production, thereby improving the production yield.

[0073] In this disclosure, the adhesive coating also contains at least one of an adhesive, an inorganic heat-resistant filler, and a surface additive.

[0074] The adhesive may, by way of example but not by way of limitation, include at least one of polyacrylate resins, polyvinylpyrrolidone (PVP), polyvinyl alcohol (PVA), and modified styrene-butadiene rubber (SBR).

[0075] Inorganic heat-resistant fillers may include metal oxides, such as at least one of alumina, boehmite, and barium titanate. The particle size of inorganic heat-resistant fillers may be 0.1 μm to 2 μm, such as 0.1 μm, 0.5 μm, 1 μm, 1.5 μm, or 2 μm, or other values ​​or ranges within the range of 0.1 μm to 2 μm.

[0076] Surface additives include at least one of wetting agents and dispersants. For example, surface additives may include at least one of acrylates, fatty alcohol polyoxyethylene ethers, silicones, and acrylic polymers. Among these, fatty alcohol polyoxyethylene ethers and silicones can act as wetting agents, and acrylates and acrylic polymers can act as dispersants.

[0077] It should be noted that the adhesives, inorganic heat-resistant fillers and surface additives in this disclosure are not limited to the contents disclosed above, and can also be set with reference to relevant prior art.

[0078] In this disclosure, the base film may include a polyethylene base film, a polypropylene base film, or a composite base film of polyethylene and polypropylene. The number of layers in the base film may be one, two, three, or more, depending on the actual needs.

[0079] In some alternative embodiments, the thickness of the base film can be 2μm to 20μm, such as 2μm, 5μm, 8μm, 10μm, 12μm, 15μm, 18μm or 20μm.

[0080] In some alternative embodiments, the thickness of the adhesive coating is 0.5 μm to 5 μm, such as 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm or 5 μm.

[0081] Accordingly, this disclosure also provides a method for preparing the above-mentioned lithium battery coated separator, including the following steps: preparing an adhesive coating on the surface of a base film.

[0082] In some alternative embodiments, the preparation of the adhesive coating includes: mixing the raw materials for the adhesive coating with water to obtain a slurry; coating the slurry onto the surface of the base film and drying it.

[0083] In some optional embodiments, the raw materials for preparing the adhesive coating are limited to copolymeric polymers. In other optional embodiments, the raw materials for preparing the adhesive coating may include at least one of an adhesive, an inorganic heat-resistant filler, and a surface additive, as well as a copolymeric polymer. For example, the raw materials may consist of an adhesive and a copolymeric polymer; or an inorganic heat-resistant filler and a copolymeric polymer; or a surface additive and a copolymeric polymer; or an adhesive, an inorganic heat-resistant filler, and a copolymeric polymer; or an inorganic heat-resistant filler, a surface additive, and a copolymeric polymer; or an adhesive, a surface additive, and a copolymeric polymer; or a combination of an adhesive, an inorganic heat-resistant filler, a surface additive, and a copolymeric polymer.

[0084] For example, the mass ratio of adhesive to copolymerized polymer can be (2-10):(4-15), the mass ratio of inorganic heat-resistant filler to copolymerized polymer can be (80-90):(4-15), and the mass ratio of surface additive to copolymerized polymer can be (0.1-3):(4-15).

[0085] In some typical embodiments, the raw materials may include, by weight, 2 to 10 parts of adhesive, 80 to 90 parts of inorganic heat-resistant filler, 0.1 to 3 parts of surface additives, and 4 to 15 parts of copolymer polymer material.

[0086] The adhesive can be 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts, or other values ​​within the range of 2 to 10 parts, for example, 4 to 7 parts.

[0087] The inorganic heat-resistant filler can be 80 parts, 82 parts, 84 parts, 86 parts, 88 parts or 90 parts, or other values ​​in the range of 80 parts to 90 parts, for example, 85.5 parts to 88.5 parts.

[0088] The surface additive can be 0.1 parts, 0.5 parts, 1 part, 1.5 parts, 2 parts, 2.5 parts, or 3 parts, or other values ​​within the range of 0.1 parts to 3 parts, for example, 1.5 parts to 3 parts. When the surface additive includes both a wetting agent and a dispersant, the mass ratio of the wetting agent to the dispersant is 2:1.

[0089] The copolymerized polymer material can be 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts, or other values ​​within the range of 4 parts to 15 parts, for example, 6 parts to 9 parts.

[0090] If the amount of copolymer polymer material used in the preparation raw materials is too small, it is not conducive to the process; if the amount of copolymer polymer material is too large, it is easy to cause membrane pore blockage, which will increase the membrane permeability and is not conducive to lithium ion transport.

[0091] It should be noted that the contents of this disclosure regarding the preparation and coating of slurry can be referred to the relevant prior art, and will not be elaborated or limited here.

[0092] In addition, this disclosure also provides a lithium battery including an electrode and the aforementioned lithium battery coated separator, wherein the lithium battery coated separator is adhered to the surface of the electrode.

[0093] In some alternative implementations, the electrode can be a positive electrode or a negative electrode. Both the positive and negative electrodes can be the same as those used in lithium batteries in the prior art, which will not be elaborated on here.

[0094] The features and performance of this disclosure will be further described in detail below with reference to embodiments.

[0095] Example 1

[0096] This embodiment provides a lithium battery coated separator, which is prepared by the following method:

[0097] Four parts of adhesive, 88.5 parts of inorganic heat-resistant filler, 0.5 parts of dispersant (sodium acrylate), 1 part of wetting agent (organosilicon), and 6 parts of copolymer polymer material were mixed with water to obtain a slurry with a solid content of 30%. The slurry was coated on the surface of the base film to a thickness of 2 μm and then dried.

[0098] The copolymer polymer material is polymethyl methacrylate (PMMA), purchased from Shenzhen Yanyi, with a glass transition temperature of 50.3℃ and a particle size of Dv. 50 : 0.5μm, (Dv 90 -Dv 10 ) / Dv 50The viscosity is 0.92. The adhesive is a polyacrylate resin, and the inorganic heat-resistant filler is alumina with a particle size of 0.3 μm. The base film is a 9 μm thick PE base film, specifically the ND9 diaphragm from Shanghai Enjie New Material Technology Co., Ltd. The coating speed is 100 m / min, and the drying temperature is 55℃.

[0099] Example 2

[0100] The difference between this embodiment and Example 1 is that the copolymer polymer material is polymethyl methacrylate (PMMA), purchased from Zhuhai Chenyu, with a glass transition temperature of 56.8℃ and a particle size of 0.8μm. (Dv) 90 -Dv 10 ) / Dv 50 It is 0.88.

[0101] Example 3

[0102] The difference between this embodiment and Example 1 is that the polymer material is replaced with a polymer prepared in the following manner.

[0103] Weigh 5g of PVP and add it to a flask containing 400g of anhydrous ethanol. Stir at room temperature until completely dissolved. Under nitrogen protection, heat to approximately 80°C and stir for 30 minutes. Add 38g of styrene, 62g of butyl acrylate, and 1g of AIBN as initiators, and continue stirring for 24 hours to obtain the polymer.

[0104] The polymer has a glass transition temperature of 54℃ and a particle size of 0.8μm. (Dv) 90 -Dv 10 ) / Dv 50 It is 1.5.

[0105] Example 4

[0106] The difference between this embodiment and Example 1 is that the polymer material is replaced with a polymer prepared in the following manner.

[0107] Weigh 5g of PVP and add it to a flask containing 400g of anhydrous ethanol. Stir at room temperature until completely dissolved. Under nitrogen protection, heat to approximately 80°C and stir for 30 minutes. Add 49g of styrene, 51g of butyl acrylate, and 1g of AIBN as initiators, and continue stirring for 24 hours to obtain the polymerization product.

[0108] The polymer has a glass transition temperature of 43℃ and a particle size of 0.45μm. (Dv) 90 -Dv 10 ) / Dv 50 It is 0.9.

[0109] Example 5

[0110] The difference between this embodiment and Example 1 is that the copolymer polymer material is hydrogenated SEBS, purchased from Kron Polymers, with a glass transition temperature of -60℃. After cryogenic grinding, the particle size is 0.5μm. (Dv) 90 -Dv 10 ) / Dv 50 It is 0.9.

[0111] Example 6

[0112] The difference between this embodiment and Embodiment 1 is that the polymer is replaced by 3 parts PMMA and 3 parts SBS instead of 6 parts PMMA.

[0113] Example 7

[0114] The difference between this embodiment and Embodiment 1 is that the polymer is replaced by 3 parts PMMA and 3 parts SIS instead of 6 parts PMMA.

[0115] Example 8

[0116] The difference between this embodiment and Embodiment 1 is that the polymer is replaced by 3 parts PMMA and 3 parts TPB instead of 6 parts PMMA.

[0117] Comparative Example 1

[0118] The difference between this comparative example and Example 1 is that the copolymer polymer is polymethyl methacrylate (PMMA), purchased from Zhuhai Chenyu, with a glass transition temperature of 73.7℃ and a particle size of 0.5μm. (Dv) 90 -Dv 10 ) / Dv 50 It is 0.88.

[0119] Comparative Example 2

[0120] The difference between this comparative example and Example 1 is that the polymer material is PVDF, purchased from Arkema, with a softening point of approximately 105°C (due to PVDF's semi-crystalline polymer nature, although its Tg is relatively low at -40°C, its softening temperature is relatively high. Since it only has an adhesive effect after softening, this comparative example considers the softening temperature of PVDF), and the particle size is 6 μm. (Dv) 90 -Dv 10 ) / Dv 50 It is 1.107.

[0121] Comparative Example 3

[0122] The difference between this comparative example and Example 1 is that the copolymer polymer is polymethyl methacrylate (PMMA), purchased from Zhuhai Chenyu, with a glass transition temperature of 73.7℃ and a particle size of 0.3μm. (Dv) 90 -Dv10 ) / Dv 50 It is 1.66.

[0123] Test case

[0124] The lithium battery coated separators obtained in Examples 1-8 and Comparative Examples 1-3 were hot-pressed to bond with the electrodes, and the adhesion strength between the electrodes and the lithium battery coated separators under different hot-pressing conditions was tested. The specific test method is as follows: The electrodes (double-sided coated positive electrodes, ternary material MCN523, electrode thickness of 120μm, aluminum foil thickness of 15μm) were stacked together with the lithium battery coated separators, and hot-pressed for 60s at a pressure of 1MPa-3MPa and a temperature of 60℃-85℃ to bond the separators and electrodes together. The bonded samples were cut into 25mm×200mm strips, and then the adhesion strength was tested on a universal tensile testing machine. The results are shown in Table 1.

[0125] Wherein, Adhesion 1 represents the adhesion force corresponding to hot pressing at 60℃ and 1MPa; Adhesion 2 represents the adhesion force corresponding to hot pressing at 60℃ and 3MPa; Adhesion 3 represents the adhesion force corresponding to hot pressing at 85℃ and 3MPa.

[0126] The hot-pressing response factor is approximately 0.244 at 60℃ and 1MPa, approximately 0.192 at 60℃ and 3MPa, and approximately 0.182 at 80℃ and 3MPa.

[0127] Air permeability testing method: The testing equipment is a Wang Yan-type air permeability meter. The battery separator is fixed, and a pressure of 0.05 MPa is applied to one side of the separator. Due to the micropores in the separator, this pressure gradually decreases. When 100 mL of air completely passes through the separator, the pressure equals atmospheric pressure. The time it takes for 100 ml of air to pass through the separator under 0.05 MPa pressure is recorded, in seconds / 100 cc. The shorter the pressure drop time, the better the air permeability of the separator, and vice versa. The air permeability increment of the coating is the difference in air permeability before and after coating.

[0128] Table 1 Comparison Results

[0129] As can be seen from Table 1, the lithium battery coated separators provided in Examples 1-8 have basically the same or better air permeability than Comparative Examples 1-3.

[0130] The lithium battery coated separators provided in Examples 1-8 exhibited adhesion strengths greater than 1 N / m to the electrodes when the thermo-pressure response factor f(p,T) was between 0.15 and 0.2. This indicates that the lithium battery coated separator has a fast temperature and pressure response rate, and its adhesion strength to the electrodes can be significantly increased with rising temperature or pressure, meaning that a large increase in adhesion strength can be achieved with relatively little energy.

[0131] The results from Examples 1-2 and Examples 6-8 show that when the glass transition temperature of PMMA is between 50°C and 60°C, and (Dv) 90 -Dv 10 ) / Dv 50 When the value is less than 1, it can achieve good adhesion under different hot-pressing conditions.

[0132] In Examples 6-8, the polymer used was PMMA combined with thermoplastic elastomer, and the resulting diaphragm could also achieve good adhesion under different hot-pressing conditions.

[0133] The results of Example 3 show that when the glass transition temperature of PMMA is between 50°C and 60°C, but (Dv) 90 -Dv 10 ) / Dv 50 When the value is greater than 1, the adhesion between the lithium battery coated separator and the electrode is significantly lower than that in Examples 1-2 after the corresponding lithium battery coated separator is hot-pressed with the electrode under higher hot-pressing temperature and pressure (85°C, 3MPa) or higher hot-pressing temperature and pressure (60°C, 1MPa).

[0134] As can be seen from the results of Example 4, when PMMA's (Dv) 90 -Dv 10 ) / Dv 50 <1 However, when the glass transition temperature is below 50°C, it can maintain high adhesion between the lithium battery coated separator and the electrode under various hot-pressing conditions. However, considering that PMMA in this comparative example has a low glass transition temperature, it is prone to melting during the drying process at temperatures above 60°C, resulting in a high increase in air permeability after coating and making subsequent storage and transportation more difficult. Therefore, PMMA with a glass transition temperature above 50°C is preferred, as in Examples 1 and 2.

[0135] The results of Comparative Example 1 show that when PMMA's (Dv) 90 -Dv 10 ) / Dv 50However, when the glass transition temperature is higher than 70℃, the corresponding lithium battery coated separator is hot-pressed with the electrode at 60℃ and 1MPa and 60℃ and 3MPa, and the adhesion between the lithium battery coated separator and the electrode is <1N / m, indicating poor adhesion.

[0136] The results of Comparative Example 2 show that when the copolymer polymer material uses Dv 50 With PVDF >0.8μm, after hot pressing the lithium battery coated separator with the electrode at 60℃ and 1MPa and 60℃ and 3MPa, the adhesion force between the lithium battery coated separator and the electrode is <1N / m, indicating poor adhesion.

[0137] The results of Comparative Example 3 show that when the copolymer polymer material (Dv) 90 -Dv 10 ) / Dv 50 With a glass transition temperature greater than 70°C and a value greater than 1.5, the adhesion between the coated separator and the electrode is low under various hot-pressing conditions.

[0138] In summary, the lithium battery coated separator proposed in this disclosure has the following characteristics: when f(p,T) is 0.15 to 0.35, the adhesion force between the lithium battery coated separator and the electrode is ≥1.0 N / m; where f(p,T)=1 / ln(p×T), p is the hot-pressing pressure when the lithium battery coated separator is bonded to the electrode, in MPa, 1MPa≤p≤10MPa; T is the hot-pressing temperature when the lithium battery coated separator is bonded to the electrode, in °C, 25℃≤T≤90℃.

[0139] The lithium battery coated separator that meets the above characteristics has a fast temperature response rate and pressure response. That is, the adhesion between the lithium battery coated separator and the electrode increases rapidly with the increase of temperature or pressure. Therefore, the lithium battery coated separator can achieve a significant increase in adhesion with less energy. On the one hand, it helps to reduce energy consumption in the battery manufacturing process. On the other hand, it can avoid or improve the probability of pinholes in the separator caused by excessive composite pressure in battery production, which may lead to short circuits in the cell, thereby improving the production yield.

[0140] The above description is merely a preferred embodiment of this disclosure and is not intended to limit this disclosure. Various modifications and variations can be made to this disclosure by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this disclosure should be included within the scope of protection of this disclosure. Industrial applicability

[0141] The adhesion between the lithium battery coated separator and the electrode provided in this disclosure increases rapidly with increasing temperature or pressure, enabling a greater increase in adhesion with less energy. This helps reduce energy consumption during battery manufacturing and avoids or reduces the probability of short circuits in the cell caused by pinholes in the separator due to excessive composite pressure during battery production, thereby improving production yield.

Claims

1. A lithium battery coated separator, characterized in that, When the hot-pressing response factor f(p,T) is 0.15 to 0.35, where f(p,T) = 1 / ln(p×T), p is the hot-pressing pressure when the lithium battery coated separator is bonded to the electrode, in MPa, 1MPa≤p≤10MPa; T is the hot-pressing temperature when the lithium battery coated separator is bonded to the electrode, in °C, 25 °C≤T≤90 °C.

2. The lithium battery coated separator according to claim 1, characterized in that, The lithium battery coated separator includes a base film and an adhesive coating applied to the surface of the base film; The adhesive coating contains a copolymer polymer material, and the glass transition temperature of the copolymer polymer material is less than or equal to the hot-pressing temperature when the lithium battery coated separator is bonded to the electrode.

3. The lithium battery coated separator according to claim 2, characterized in that, The copolymer polymer material is obtained by copolymerizing at least two of the following monomers: styrene, acrylic acid, acrylate monomers, polyacrylate monomers, olefin monomers, acrylamide monomers, and vinyl acetate monomers.

4. The lithium battery coated separator according to claim 3, characterized in that, The copolymer polymer material includes at least one of acrylate copolymers and thermoplastic elastomers.

5. The lithium battery coated separator according to claim 4, characterized in that, The thermoplastic elastomer includes at least one of SBS, SIS, SEBS, SEPS, TPV, TPB, and TPI.

6. The lithium battery coated separator according to claim 3, characterized in that, The glass transition temperature of the acrylate copolymer is 25℃~90℃.

7. The lithium battery coated separator according to claim 6, characterized in that, The glass transition temperature of the acrylate copolymer is 50℃~70℃.

8. The lithium battery coated separator according to claim 7, characterized in that, The glass transition temperature of the acrylate copolymer is 50℃~60℃.

9. The lithium battery coated separator according to claim 4 or 5, characterized in that, The glass transition temperature of the thermoplastic elastomer is -70℃ to 120℃.

10. The lithium battery coated separator according to any one of claims 2 to 9, characterized in that, The copolymer polymer material also has at least one of the following characteristics: Feature 1: The copolymer polymer material is in particulate form, and the particle size of the copolymer polymer material is 0.1μm to 2μm; Feature 2: The copolymer is in particulate form, and the copolymer material (Dv) 90 -Dv 10 ) / Dv 50 ≤1.5 and >0.

11. The lithium battery coated separator according to claim 10, characterized in that, The copolymer polymer material (Dv) 90 -Dv 10 ) / Dv 50 >0 and <1.

12. The lithium battery coated separator according to claim 11, characterized in that, The copolymer polymer material (Dv) 90 -Dv 10 ) / Dv 50 The value ranges from 0.50 to 0.

95.

13. The lithium battery coated separator according to any one of claims 2 to 12, characterized in that, The adhesive coating also contains at least one of an adhesive, an inorganic heat-resistant filler, and a surface additive.

14. The lithium battery coated separator according to claim 13, characterized in that, The adhesive includes at least one of polyacrylate resin, PVP, PVA, and modified SBR; And / or, the inorganic heat-resistant filler includes metal oxides; And / or, the surface aids include at least one of wetting agents and dispersants.

15. The lithium battery coated separator according to claim 14, characterized in that, The inorganic heat-resistant filler includes at least one of alumina, boehmite, and barium titanate. And / or, the particle size of the inorganic heat-resistant filler is 0.1 μm to 2 μm.

16. The lithium battery coated separator according to claim 13, characterized in that, The surface additives include at least one of acrylates, fatty alcohol polyoxyethylene ethers, organosilicones, and acrylic polymers.

17. The lithium battery coated separator according to any one of claims 2 to 16, characterized in that, The base film includes a polyethylene base film, a polypropylene base film, or a composite base film of polyethylene and polypropylene; And / or, the thickness of the base film is 2 μm to 20 μm; And / or, the thickness of the adhesive coating is 0.5 μm to 5 μm.

18. A method for preparing a lithium battery coated separator as described in any one of claims 1 to 17, characterized in that, Includes the following steps: An adhesive coating is prepared on the surface of the base film.

19. The preparation method according to claim 18, characterized in that, The preparation of the adhesive coating includes: mixing the raw materials for the adhesive coating with water according to the preset preparation materials to obtain a slurry; coating the slurry onto the surface of the base film and drying it.

20. The preparation method according to claim 19, characterized in that, The raw material for preparing the adhesive coating is a copolymer polymer.

21. The preparation method according to claim 19, characterized in that, The raw materials for preparing the adhesive coating include at least one of adhesive, inorganic heat-resistant filler, surface additives, and copolymer polymer.

22. The preparation method according to claim 21, characterized in that, The mass ratio of the adhesive to the copolymerized polymer is (2-10):(4-15); And / or, the mass ratio of the inorganic heat-resistant filler to the copolymer polymer is (80-90):(4-15); And / or, the mass ratio of the surface additive to the copolymer polymer is (0.1-3):(4-15).

23. A lithium battery, characterized in that, The lithium battery includes an electrode and a lithium battery coated separator as described in any one of claims 1 to 17, wherein the lithium battery coated separator is adhered to the surface of the electrode.