Polyamide composition
A blend of semi-aromatic polyamides with a reinforcing agent and flame retardant addresses moisture absorption and processing issues, enhancing mechanical strength and heat aging resistance in electronic and electrical appliances.
Patent Information
- Application Number
- PCT/CN2026/093872
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-06
- Filing Date
- 2026-04-29
- Publication Date
- 2026-11-12
AI Technical Summary
Polyamide compositions used in electronic and electrical appliances face challenges with moisture absorption leading to mechanical property degradation, high melt viscosity affecting processability, and inadequate heat aging resistance, making them difficult to process and prone to defects.
A polyamide composition comprising a blend of two semi-aromatic polyamides with specific glass transition temperatures, a reinforcing agent, and a flame retardant, formulated in a specific weight ratio, to enhance moisture resistance, flowability, and heat aging performance.
The composition achieves significantly improved moisture absorption resistance, good processing flowability, and refined heat aging resistance, suitable for applications in connectors and transformer shells.
Smart Images

Figure PCTCN2026093872-FTAPPB-I100001 
Figure PCTCN2026093872-FTAPPB-I100002 
Figure PCTCN2026093872-FTAPPB-I100003
Abstract
Description
POLYAMIDE COMPOSITIONTECHNICAL FIELD
[0001] The present invention relates to a polyamide composition with significantly improved moisture absorption resistance performance, good flowability for processing, expected mechanical strength as well as refined heat aging resistance performance, which is highly promising for application in the field of electronic and electrical appliances, such as connectors, capacitors, transformer shells, or the like.BACKGROUND
[0002] Polyamide compositions are frequently used for technical construction materials since they exhibit good toughness, rigidity and heat resistance, i.e. good retention of mechanical properties such as tensile strength at break and Charpy impact strength, high heat distortion temperature (HDT) and minimum distortion during injection molding. Application areas of these polyamide compositions include, for example, interior and exterior parts in automotive sector and in other transport means, housing materials for appliances and equipment for telecommunications, entertainment electronics, household appliances, mechanical engineering equipments, and heating equipments and fasting parts for installations.
[0003] For electronic and electrical appliances, such as connectors, excellent mechanical properties and low moisture absorption performance is eagerly expected and needed to ensure no crack during assembly process and no electrical and electronics (E&E) failure during end use. The moisture may exist during different stages of the polymer processing; it also may be absorbed from the surrounding atmosphere during delivery, storage, and use of the final products. It is known that moisture is always an inducement for negative impacts on a range of polyamide’s properties, in particular mechanical properties, such as elastic modulus and strength.
[0004] Processability (i.e. good melt flowability) is also critical, as many of those parts are combined with metal insert. Thus, a polyamide material shall have good flowability to ensure easy processing and no defects during processing. However, polyamide compositions with high thermal stability (i.e. high heat distortion temperature) typically exhibit high melt viscosity and therefore have lower melt flow rate. Thus, the polyamide compositions having high thermal stability are difficult to be processed and it is necessary to carry out the processing at a relatively high temperature.
[0005] CN107073875A discloses a composite structure having a surface, which has at least a portion made of a surface resin composition, and comprising a woven glass fiber fabric, said woven glass fiber fabric being fully impregnated with a matrix resin composition, wherein the matrix resin composition comprises a blend of PA6T / DT and PA66 / 6T, preferably with a weight ratio between from about 30: 70 to about 70: 30, more preferably with a weight ratio of about 50: 50. However, due to the intrinsic shape of the woven glass fiber fabric, the final composite material prepared by using PA6T / DT and PA66 / 6T blend for impregnating a woven glass fiber fabric is merely suitably presented in the form of a sheet or laminate structure. Also, this disclosure is silent on the properties of moisture absorption resistance or flowability for processing.SUMMARY OF THE INVENTION
[0006] An object of this invention is to develop a polyamide composition, which could have at least one of the following expected properties: improved moisture absorption resistance performance, good flowability for processing, expected mechanical strength, as well as refined heat aging resistance performance. Surprisingly, it has been found by the inventors that the above object can be achieved by providing a polyamide composition, comprising the following components:
[0007] a) a first semi-aromatic polyamide having a glass transition temperature of from 70℃ to 145℃;
[0008] b) a second semi-aromatic polyamide having a glass transition temperature of from 110℃ to 160℃, which is different from the first semi-aromatic polyamide;
[0009] c) at least one reinforcing agent;
[0010] d) at least one flame retardant; and
[0011] e) optionally at least one further additive;
[0012] wherein the weight ratio of the component a) to the component b) is in the range of (2.4 -10) : 1, preferably in the range of (2.5 -8) : 1.
[0013] In one embodiment of the invention, the first semi-aromatic polyamide is at least one polyamide derived from a linear aliphatic C4-C12 diamine and an aromatic C5-C12 dicarboxylic acid, or derived from a linear aliphatic C4-C10 diamine, at least one aromatic C5-C12 dicarboxylic acid and a linear aliphatic C4-C10 dicarboxylic acid, or derived from two different linear aliphatic C4-C10 diamines and at least one aromatic C5-C12 dicarboxylic acid.
[0014] In one embodiment of the invention, the second semi-aromatic polyamide is at least one polyamide derived from at least one linear aliphatic C4-C10 diamine, a branched aliphatic C4-C10 diamine, and at least one aromatic C5-C12 dicarboxylic acid.
[0015] In one embodiment of the invention, the enthalpy of fusion of the first semi-aromatic polyamide (ΔHf1) and the enthalpy of fusion of the second semi-aromatic polyamide (ΔHf2) are each independently more than 15 kJ / kg, preferably more than 20 kJ / kg.
[0016] In a preferable embodiment of the invention, the difference of the enthalpy of fusion between the first semi-aromatic polyamide and the second semi-aromatic polyamide (ΔHf1-ΔHf2) is in the range of from 1 to 45 kJ / kg, preferably from 3 to 40 kJ / kg.
[0017] In a preferable embodiment of the invention, the molar percentage of the branched aliphatic C4-C10 diamine is in the range of from 40 mol%to 60 mol%, preferably in the range of from 45 mol%to 55 mol%, based on the total amount of the diamine in the second semi-aromatic polyamide.
[0018] In a preferable embodiment of the invention, the branched aliphatic C4-C10 diamine is at least one selected from the group consisting of methyl substituted linear aliphatic C3-C9 diamine, and the at least one aromatic C5-C12 dicarboxylic acid is one or more selected from the group consisting of terephthalic acid, isophthalic acid, phthalic acid, and any combinations thereof.
[0019] In a preferable embodiment of the invention, the second semi-aromatic polyamide is at least one selected from the group consisting of PA6T / DT, PA5T / 6T / DT, PA5T / DT, PA6T / 6I / DT, PA4T / 6T / DT, PA4T / 10T / DT, PA4T / 4I / 6T / 6I / DT / DI or any combinations thereof.
[0020] In one embodiment of the invention, the first semi-aromatic polyamide is at least one selected from the group consisting of PA5T, PA6T, PA9T, PA10T, PA11T, PA12T or any combinations thereof.
[0021] In another embodiment of the invention, the first semi-aromatic polyamide is derived from a linear aliphatic C4-C10 diamine, at least one aromatic C5-C12 dicarboxylic acid and a linear aliphatic C4-C10 dicarboxylic acid, and the molar percentage of the aromatic C5-C12 dicarboxylic acid is in the range of from 50 mol%to 70 mol%, preferably in the range of from 55 mol%to 65 mol%, based on the total amount of the dicarboxylic acid in the first semi-aromatic polyamide.
[0022] In a preferable embodiment of the invention, the first semi-aromatic polyamide is at least one selected from the group consisting of PA610 / 6T, PA66 / 6T, PA6T / 66, PA5T / 56, PA66 / 6T / 6I, PA1010 / 10T, and any combinations thereof.
[0023] In yet another embodiment of the invention, the first semi-aromatic polyamide is derived from two different linear aliphatic C4-C10 diamines and at least one aromatic C5-C12 dicarboxylic acid, and wherein the two different linear aliphatic C4-C10 diamines are a linear aliphatic C4-C5 diamine and a linear aliphatic C6-C10 diamine, respectively, and the molar percentage of the linear aliphatic C4-C5 diamine is in the range of from 40 mol%to 60 mol%, preferably in the range of from 45 mol%to 55 mol%, based on the total amount of the diamine in the first semi-aromatic polyamide.
[0024] In a preferable embodiment of the invention, the first semi-aromatic polyamide is at least one selected from the group consisting of PA6T / 5T, PA4T / 6T or any combinations thereof.
[0025] In one embodiment of the invention, the first semi-aromatic polyamide has a melting temperature between 260℃ and 320 ℃, preferably between 270 ℃ and 310 ℃, and the second semi-aromatic polyamide has a melting temperature between 290℃ and 310 ℃, preferably between 295 ℃ and 305 ℃.
[0026] In one embodiment of the invention, the sum of the first semi-aromatic polyamide and the second semi-aromatic polyamide is in the range of 30-90 wt%, preferably 35-80 wt%, more preferably 40-70 wt%, in particular 43-60 wt%, based on the total weight of the polyamide composition.
[0027] In one embodiment of the invention, the polyamide composition comprises
[0028] a) 25 wt%to 65 wt%, preferably 28 wt%to 62 wt%, more preferably 30 wt%to 60 wt%of the first semi-aromatic polyamide;
[0029] b) 3 wt%to 30 wt%, preferably 4 wt%to 25 wt%, more preferably 5 wt%to 20 wt%, of the second semi-aromatic polyamide;
[0030] c) 10 wt%to 55 wt%, preferably 15 wt%to 50 wt%, more preferably 20 wt%to 45 wt%of the reinforcing agent; and
[0031] d) 10 wt%to 30wt%, preferably 12 wt%to 25wt%, more preferably 13 wt%to 20 wt%of the flame retardant;
[0032] based on the total weight of the polyamide composition.
[0033] In one embodiment of the invention, the reinforcing agent is at least one selected from the group consisting of glass fibers, carbon fibers, graphite fibers, aramid fibers, potassium titanate fibers, and any combinations thereof.
[0034] In one embodiment of the invention, the flame retardant is at least one selected from the group consisting of phosphorus-containing flame retardants, nitrogen-containing flame retardants, halogenated flame retardants, and any combinations thereof.
[0035] In one embodiment of the invention, the polyamide composition has a water uptake of no more than 1.60%, such as from 0.50 %to 1.60 %, determined according to ISO 62.
[0036] Another object of this invention is to provide a molded article, comprising the polyamide composition according to the present invention.
[0037] It has been surprisingly found that the inventive polyamide compositions comprising components (a) - (e) would showcase at least one of the following expected properties: significantly improved moisture absorption resistance performance, good flowability for processing, expected mechanical strength, as well as refined heat aging resistance performance, which is highly promising for application in the field of electronic and electrical appliances, such as connectors, capacitors, transformer shells, or the like.
[0038] It was found by the present inventors that the combination of the first semi-aromatic polyamide and the second semi-aromatic polyamide according to the invention results in a synergistic effect which provides the unique combination of properties described herein.DETAILED DESCRIPTION OF THE INVENTION
[0039] In the following passages, different aspects of the invention are defined in more detail. Each aspect so defined may be combined with any other aspect or aspects unless clearly indicated to the contrary. In particular, any feature indicated as being preferred or advantageous may be combined with any other feature or features indicated as being preferred or advantageous.
[0040] Furthermore, whereas some embodiments described herein include some but not other features included in other embodiments, combinations of features of different embodiments are meant to be within the scope of the invention, and form different embodiments, as would be understood by those familiar with the art. For example, in the following claims, any of the claimed embodiments can be used in any combination.
[0041] Before the polyamide compositions of the invention are described, it is to be understood that this invention is not limited to the particular compositions described, since such compositions may vary. It is also to be understood that the terminology used herein is not intended to be limiting, since the scope of the present invention will be limited only by the appended claims. Unless defined otherwise, all technical and scientific terms used herein have the meaning commonly understood by a person skilled in the art to which the invention belongs.
[0042] As used herein, the term “comprising” should not be interpreted as being restricted to the features, elements or components listed thereafter; it does not exclude other features, elements or components. It is thus to be interpreted as specifying the presence of the stated features, elements or components as referred to, but does not preclude the presence or addition of one or more other features, elements or components, or groups thereof. Thus, the scope of the expression “acomposition comprising components A and B” should not be limited to compositions consisting only of components A and B; rather, it means that with respect to the present invention, the only relevant components of the polyamide composition are A and B. The term “comprising” and its variants such as “comprises” and “comprised of” as used herein are synonymous with “including” , “includes” , “containing” , and “contains” ; and these terms are inclusive or open-ended and do not exclude additional, non-recited features, elements and components.
[0043] As used herein, the articles “a” , “an” and “the” may refer to one or to more than one (i.e., to at least one) of the grammatical object of the article. By way of example, “acomponent” means one component or more than one component.
[0044] If the term "about" is used before a quantitative value, the present teachings also include the specific quantitative value itself, unless specifically stated otherwise. As used herein the term "about" refers to a ± 10 %variation from the nominal value unless specifically stated otherwise. As used herein, the term "melting point" in reference to a polyamide refers to the melting point of the pure resin as determined with differential scanning calorimetry (DSC) at a scan rate of 10℃ / min in the first heating scan, wherein the melting point is taken at the maximum of the endothermic peak. When selecting polyamides for the scope of the current invention, always the peak of the melting endotherm of the first heating scan of the single polyamide is used. As used herein, a scan rate is an increase of temperature per unit time. Sufficient energy must be supplied to maintain a constant scan rate of 10℃ / min until a temperature of at least 30℃ above the melting point is reached.
[0045] As used herein, the term “enthalpy of fusion (ΔHf) ” is the measured enthalpy in [kJ / kg] of the semi-aromatic polyamide polymer, determined by differential scanning calorimetry (DSC, Q200 instrument, TA Instruments) in accordance with DIN EN ISO 11357 at a cooling rate of 10 K / min in the range from 340 ℃ to 20 ℃ under a nitrogen atmosphere.
[0046] Unless otherwise identified, all percentages (%) are “percent by weight" .
[0047] Unless otherwise identified, the temperature refers to room temperature and the pressure refers to ambient pressure.
[0048] The present invention provides a polyamide composition, comprising the following components:
[0049] a) a first semi-aromatic polyamide having a glass transition temperature of from 70℃ to 145℃;
[0050] b) a second semi-aromatic polyamide having a glass transition temperature of from 110℃ to 160℃, which is different from the first semi-aromatic polyamide;
[0051] c) at least one reinforcing agent;
[0052] d) at least one flame retardant; and
[0053] e) optionally at least one further additive;
[0054] wherein the weight ratio of the component a) to the component b) is in the range of (2.4 -10) : 1, preferably in the range of (2.5 -8) : 1.
[0055] Component (a) a first semi-aromatic polyamide
[0056] The first semi-aromatic polyamide according to the present invention is at least one polyamide derived from a linear aliphatic C4-C12 diamine and an aromatic C5-C12 dicarboxylic acid, or derived from a linear aliphatic C4-C10 diamine, at least one aromatic C5-C12 dicarboxylic acid and a linear aliphatic C4-C10 dicarboxylic acid, or derived from two different linear aliphatic C4-C10 diamines and at least one aromatic C5-C12 dicarboxylic acid.
[0057] The term “linear aliphatic C4-C12 diamine” should be understood to mean a linear aliphatic diamine having 4-12 carbon atoms. Examples of the linear aliphatic diamines include, but not limited to, 1, 4-butane diamine, 1, 5-pentane diamine, 1, 6-hexane diamine, 1, 8-octanediamine, 1, 9-nonanediamine, 1, 10-decanediamine, 1, 11-undecanediamine, 1, 12-dodecanediamine and mixtures thereof, preferably 1, 4-butane diamine, 1, 5-pentane diamine, 1, 6-hexane diamine, 1, 8-octanediamine, 1, 10-decanediamine and mixtures thereof, more preferably 1, 4-butane diamine, 1, 5-pentane diamine, 1, 6-hexane diamine and mixtures thereof.
[0058] The term “aromatic C5-C12 dicarboxylic acid” should be understood to mean an aromatic dicarboxylic acid having 5-12 carbon atoms. Examples of the aromatic dicarboxylic acid include, but not limited to, terephthalic acid, isophthalic acid, naphthalene dicarboxylic acids and / or diphenyl dicarboxylic acids, more preferably terephthalic acid, a mixture of terephthalic and isophthalic, naphthalene dicarboxylic acid, a mixture of terephthalic and naphthalene dicarboxylic acid, most preferably terephthalic acid.
[0059] The term “linear aliphatic C4-C10 diamine” should be understood to mean a linear aliphatic diamine having 4-10 carbon atoms. Examples of the linear aliphatic diamines include, but not limited to, 1, 4-butane diamine, 1, 5-pentane diamine, 1, 6-hexane diamine, 1, 8-octanediamine, 1, 9-nonanediamine, 1, 10-decanediamine and mixtures thereof, preferably 1, 5-pentane diamine, 1, 6-hexane diamine, 1, 8-octanediamine, 1, 9-nonanediamine and mixtures thereof, more preferably 1, 5-pentane diamine, 1, 6-hexane diamine and mixtures thereof.
[0060] The term “linear aliphatic C4-C10 dicarboxylic acid” should be understood to mean a linear aliphatic dicarboxylic acid having 4-10 carbon atoms. Examples of the linear aliphatic dicarboxylic acid include, but not limited to, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid and mixtures thereof, more preferably adipic acid, azelaic acid, sebacic acid and mixtures thereof, most preferably adipic acid.
[0061] Preferably, the first semi-aromatic polyamide has a glass transition temperature (Tg1) of from 70℃ to 145℃, preferably from 75℃ to 142℃, more preferably from 80℃ to 140℃.
[0062] Preferably, the enthalpy of fusion of the first semi-aromatic polyamide (ΔHf1) is more than 15 kJ / kg, preferably more than 20 kJ / kg, and preferably less than 85 kJ / kg, more preferably less than 80 kJ / kg, most preferably less than 75 kJ / kg.
[0063] In one preferred embodiment according to the present invention, the first semi-aromatic polyamide is at least one selected from the group consisting of PA5T, PA6T, PA9T, PA10T, PA11T, PA12T or any combinations thereof.
[0064] In another preferred embodiment according to the present invention, the first semi-aromatic polyamide is derived from a linear aliphatic C4-C10 diamine, at least one aromatic C5-C12 dicarboxylic acid and a linear aliphatic C4-C10 dicarboxylic acid, and the molar percentage of the aromatic C5-C12 dicarboxylic acid is in the range of from 50 mol%to 70 mol%, preferably in the range of from 55 mol%to 65 mol%, based on the total amount of the dicarboxylic acid in the first semi-aromatic polyamide.
[0065] Preferably, the first semi-aromatic polyamides may be at least one selected from the group consisting of PA610 / 6T, PA66 / 6T, PA6T / 66, PA5T / 56, PA66 / 6T / 6I, PA1010 / 10T, and any combinations thereof.
[0066] In the present application, the polyamide 66 / 6T and the polyamide 6T / 66 comprise the same repeating units but differ in that polyamide 66 / 6T comprises a higher amount of repeating units derived from adipic acid (6) compared to repeating units derived from terephthalic acid (T) , whereas polyamide 6T / 66 comprises a higher amount of repeating units derived from terephthalic acid (T) compared to repeating units derived from adipic acid (6) .
[0067] In one preferred embodiment according to the present invention, the first semi-aromatic polyamide is derived from two different linear aliphatic C4-C10 diamines and at least one aromatic C5-C12 dicarboxylic acid, and wherein the two different linear aliphatic C4-C10 diamines are a linear aliphatic C4-C5 diamine and a linear aliphatic C6-C10 diamine, respectively, and the molar percentage of the linear aliphatic C4-C5 diamine is in the range of from 40 mol%to 60 mol%, preferably in the range of from 45 mol%to 55 mol%, more preferably 50 mol%, based on the total amount of the diamine in the first semi-aromatic polyamide.
[0068] Preferably, the first semi-aromatic polyamides may be at least one selected from the group consisting of PA6T / 5T, PA4T / 6T or any combinations thereof.
[0069] In one preferred embodiment according to the present invention, the first semi-aromatic polyamide has a melting temperature (Tm1) between 260℃ and 320 ℃, preferably between 270 ℃ and 310 ℃, more preferably between 275 ℃ and 308 ℃.
[0070] Most preferably, the first semi-aromatic polyamide according to the present invention is at least one selected from the group consisting of PA9T, PA6T / 66, PA6T / 5T, PA66 / 6T and mixtures thereof.
[0071] In one preferred embodiment according to the present invention, the content of the first semi-aromatic polyamide in the polyamide composition is in the range of from 25 wt%to 65wt%, preferably from 28 wt%to 62 wt%, more preferably from 30 wt%to 60 wt%, most preferably from 32 wt%to 55 wt%, in particular from 35 wt%to 50 wt%, based on the total weight of the polyamide composition. According to the present invention, for example, the first semi-aromatic polyamide may be present in an amount of 25 wt%, 26 wt%, 27 wt%, 28 wt%, 30 wt%, 31 wt%, 32 wt%, 34 wt%, 35 wt%, 36 wt%, 38 wt%, 40 wt%, 42 wt%, 43 wt%, 45 wt%, 46 wt%, 47 wt%, 48 wt%, 50 wt%, 51 wt%, 52 wt%, 54 wt%, 55 wt%, 57 wt%, 58 wt%, 59 wt%, 60 wt%, 62 wt%, 63 wt%, 64 wt%, or 65 wt%, or within a range of any two values aforesaid.
[0072] Component (b) a second semi-aromatic polyamide
[0073] The second semi-aromatic polyamide according to the present invention is at least one polyamide derived from at least one linear aliphatic C4-C10 diamine, a branched aliphatic C4-C10 diamine, and at least one aromatic C5-C12 dicarboxylic acid.
[0074] The term “branched aliphatic C4-C10 diamine” should be understood to mean a branched aliphatic diamine having 4-10 carbon atoms. Examples of the branched aliphatic diamines include, but not limited to, 2-methyl-1, 5-pentane diamine, 3-methyl-1, 5-pentane diamine, 2-methyl-1, 8-octanediamine, 5-methyl-1, 9-nonanediamine, 2, 4, 4-trimethylhexamethylene diamine, 2, 2, 4-trimethylhexamethylene diamine, 2, 4-dimethyloctanediamine and mixtures thereof, preferably 2-methyl-1, 5-pentane diamine, 3-methyl-1, 5-pentane diamine, 2-methyl-1, 8-octanediamine, 2, 4, 4-trimethylhexamethylene diamine, 2, 2, 4-trimethylhexamethylene diamine and mixtures thereof.
[0075] The terms “linear aliphatic C4-C10 diamine” and “aromatic C5-C12 dicarboxylic acid” have the same meaning as mentioned above.
[0076] Specifically, preferred examples of the second semi-aromatic polyamide may be at least one selected from the group consisting of PA6T / DT, PA5T / 6T / DT, PA5T / DT, PA6T / 6I / DT, PA4T / 6T / DT, PA4T / 10T / DT, PA4T / 4I / 6T / 6I / DT / DI or any combinations thereof. More preferably, the second semi-aromatic polyamide is PA6T / DT.
[0077] Preferably, the second semi-aromatic polyamide has a glass transition temperature (Tg2) of from 110℃ to 160℃, preferably from 130℃ to 150℃, more preferably from 135℃ to 145℃.
[0078] More preferably, the glass transition temperature of the second semi-aromatic polyamide is greater than that of the first semi-aromatic polyamide, preferably greater than 0.5 –70 ℃, more preferably greater than 0.6 –60 ℃.
[0079] Preferably, the enthalpy of fusion of the second semi-aromatic polyamide (ΔHf2) is more than 15 kJ / kg, preferably more than 20 kJ / kg, and preferably less than 60 kJ / kg, more preferably less than 50 kJ / kg.
[0080] Preferably, the difference of the enthalpy of fusion between the first semi-aromatic polyamide and the second semi-aromatic polyamide (ΔHf1-ΔHf2) is in the range of from 1 to 45 kJ / kg, preferably from 3 to 40 kJ / kg, more preferably from 5 to 30 kJ / kg.
[0081] Preferably, the second semi-aromatic polyamide has a melting temperature (Tm2) between 290℃ and 310 ℃, preferably between 295 ℃ and 305 ℃.
[0082] In one embodiment according to the present invention, the molar percentage of the branched aliphatic C4-C10 diamine is in the range of from 40 mol%to 60 mol%, preferably in the range of from 45 mol%to 55 mol%, based on the total amount of the diamine in the second semi-aromatic polyamide.
[0083] In one embodiment according to the present invention, the branched aliphatic C4-C10 diamine is at least one selected from the group consisting of methyl substituted linear aliphatic C3-C9 diamine, and the at least one aromatic C5-C12 dicarboxylic acid is one or more selected from the group consisting of terephthalic acid, isophthalic acid, phthalic acid, and any combinations thereof. The term linear aliphatic C3-C9 diamine has a similar meaning to that of the term linear aliphatic C4-C10 diamine.
[0084] In one embodiment according to the present invention, the sum of the percent by weight of the first semi-aromatic polyamide and the second semi-aromatic polyamide is in the range of 30-90 wt%, preferably 35-80 wt%, more preferably 40-70 wt%, in particular 45-60 wt%, based on the total weight of the polyamide composition.
[0085] In one preferred embodiment according to the present invention, the content of the second semi-aromatic polyamide in the polyamide composition is in the range of from 3 wt%to 30wt%, preferably from 4 wt%to 25 wt%, more preferably from 5 wt%to 20 wt%, most preferably from 6 wt%to 18 wt%, in particular from 7 wt%to 15 wt%, based on the total weight of the polyamide composition. According to the present invention, for example, the second semi-aromatic polyamide may be present in an amount of 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 18 wt%, 20 wt%, 21 wt%, 22 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, or 30 wt%, or within a range of any two values aforesaid.
[0086] In one preferred embodiment according to the present invention, the weight ratio of the component a) to the component b) is in the range of (2.4-10) : 1, preferably in the range of (2.5 -8) : 1, more preferably in the range of (2.5 -7) : 1.
[0087] Examples of the semi-aromatic polyamides in the polyamide composition described herein can be commercially available or prepared by known methods in the art. For example, the first and second semi-aromatic polyamide according to the present invention can be prepared by any known polymerization method, in particular through melt polycondensation reaction of the dicarboxylic acid component according to the present invention in the determined molar amounts and the diamine component according to the present invention which is used in stoichiometric amounts with respect to the dicarboxylic acid component. Alternatively, a salt of at least one of the dicarboxylic acids and at least a part of the diamine can be prepared in a first step which is then fed into a polycondensation equipment to obtain the respective polyamides, according to one of technologies well known in the art (e.g. as described in Nylon Plastics Handbook, edited by Melvin Kohan, Hanser Verlag, 1995) .
[0088] According to the present invention, the first semi-aromatic polyamide and the second semi-aromatic polyamide may be semi-crystalline polyamides.
[0089] The meaning of the term “semi-crystalline polyamide” is known to a person skilled in the art. Usually, the term is intended to denote a polyamide comprising a crystallizable and an amorphous portion in the skeleton, i.e., an amorphous polymeric material which contains randomly entangled chains and a crystalline material which contains domains in which the polymer chains are packed in an ordered array, where these crystalline domains are embedded in an amorphous polymer matrix portion. In particular, the semi-crystalline polyamide in the solid state contains a fraction of regularly organized, crystalline polymeric domains in which polymer chains are packed in an ordered array (e.g. lamellae, spherulites) . Crystalline domains coexist with a fraction of amorphous, non-crystallized polymer domains. The semi-crystalline fraction shows a melting and a crystallization point range, and a melting and a crystallization enthalpy as well. Such values can be easily detected by experts in the field, e.g. by DSC analysis or by X-ray diffraction. The amorphous phase does not show any melting or crystallization point.
[0090] Preferably, the aromatic C5-C12 dicarboxylic acids used in the first semi-aromatic polyamide and the second the semi-aromatic polyamide may be the same or different from each other.
[0091] In one preferred embodiment of the invention, the first semi-aromatic polyamide is at least one selected from the group consisting of PA9T, PA6T / 66, PA6T / 5T, PA66 / 6T and mixtures thereof, and the second semi-aromatic polyamide is PA6T / DT.
[0092] Additionally, the first semi-aromatic polyamide and second semi-aromatic polyamide used in the present application should not be limited to the ones prepared from virgin crude oil monomers and could be completely or at least partially biobased or derived from waste stream or recycling activities, i.e., the polyamide used in the present application may be prepared or obtained based on renewable materials, secondary raw materials or recycled raw materials through existing known methods.
[0093] Component c) at least one reinforcing agent
[0094] According to the present invention, at least one reinforcing agent may be added into the polyamide composition. The reinforcing agent may be in the form of a proper shape, such as fiber, whisker, or flake, preferably in the form of fiber. Preferred fiber reinforcing agents may be glass fibers, carbon fibers, graphite fibers, aramid fibers, and potassium titanate fibers, particular preference being given to glass fibers. These can be used as rovings or in the commercially available forms of chopped glass.
[0095] The nature of glasses constituting the glass fibers for the polyamide composition of the present invention is not particularly limited, and may include E glass fibers, D glass fibers, boron free glass fibers, T glass, NE glass, C glass, S glass, S2 glass and R glass, and the like. Glass fibers may contain sizing agents on their surface in order to guarantee their cohesion when in continuous or chopped strand forms, and particularly to provide adhesion at the interface with the polyamide matrix.
[0096] Glass fibers can be comprised in the polyamide composition in form of continuous roving bundles or in form of chopped strands. Once glass fibers are mixed with the polyamides in a mixing device, e.g. an extruder, the glass fibers break into shorter fibrils with a given length distribution determined by the type and amount of glass fibers, by the extruder screw profile and by the processing conditions.
[0097] In one embodiment of the invention, the at least one glass fiber is introduced to the polyamide composition in form of at least one chopped glass fiber, in particular a chopped glass fiber having an initial number-average fiber length of 0.1 to 10 mm and an average diameter of 1 to 25 μm, preferably 10 to 15 μm. The number-average fiber length of the at least one glass fiber in the final polyamide composition is typically in the range of from 200 to 1000 μm.
[0098] The at least one glass fiber may comprise at least one glass fiber having a substantially circular cross section (herein also further referred to as circular glass fiber) and / or at least one glass fiber having a substantially non-circular cross section (herein also further referred to as flat glass fiber) .
[0099] In one embodiment of the present invention, the polyamide composition comprises at least one circular glass fiber.
[0100] In another embodiment of the present invention, the polyamide composition comprises at least one flat glass fiber.
[0101] The polyamide composition according to the present invention comprises 10 to 55 wt%, preferably 15 to 50 wt%, more preferably 20 to 45 wt%, especially 25 to 42 wt%, of at least one reinforcing agent, based on the total weight of the polyamide composition. According to the present invention, for example, the at least one reinforcing agent may be present in an amount of 10 wt%, 12 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 28 wt%, 30 wt%, 32 wt%, 36 wt%, 38 wt%, 40 wt%, 42 wt%, 45 wt%, 48 wt%, 50 wt%, 52 wt%, or 55 wt%, or within a range of any two values aforesaid.
[0102] Component d) at least one flame retardant
[0103] Suitable flame retardants in the context of the present invention may be at least one selected from the group consisting of phosphorus-containing flame retardants, nitrogen-containing flame retardants and halogenated flame retardants.
[0104] Suitable phosphorus-containing flame retardants may be one or more selected from the group consisting of dialkyl phosphinate, hypophosphite, phosphate, phosphonate, phosphazene, and any combinations thereof. Preferably, the phosphorus-containing flame retardants are halogen-free flame-retardant based on alkyl phosphinates. The phosphorus-containing flame retardant comprises aluminum dialkylphosphinate, such as aluminum diethylphosphinate and a mixture of aluminum diethylphosphinate and aluminum hypophosphite.
[0105] Suitable flame retardants are additionally nitrogen-containing flame retardants such as melamine compounds. Suitable examples are melamine cyanurates, for example reaction products of preferably equimolar amounts of melamine and cyanuric acid or isocyanuric acid.
[0106] Further suitable compounds (often also referred to as salts or adducts) are melamine sulfate, melamine, melamine borate, oxalate, primary phosphate, secondary phosphate, and pyrophosphate, melamine neopentyl glycol borate, and polymeric melamine phosphate (CAS No. 56386-64-2 and 218768-84-4) .
[0107] Suitable halogenated flame retardants may be at least one selected from the group consisting of brominated epoxy resin, brominated polycarbonate, brominated polystyrene, brominated polyacrylic, and any combinations thereof.
[0108] The polyamide composition according to the present invention comprises 10 to 30 wt%, preferably 12 to 25 wt%, more preferably 13 to 20 wt%, of at least one flame retardant, based on the total weight of the polyamide composition. According to the present invention, for example, the at least one flame retardant may be present in an amount of 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 18 wt%, 20 wt%, 21 wt%, 22 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, or 30 wt%, or within a range of any two values aforesaid.
[0109] Component e) optionally at least one further additive
[0110] In the present invention, the polyamide composition optionally comprises at least one further additive, which is beneficial to improve the performance of the polyamide composition. The other additives used for the polyamide composition may be any processing agent suitable for preparing a polyamide composition and commonly known to those skilled in the art.
[0111] Preferably, the other additives may comprise a lubricant, an antioxidant, a nucleating agent, a flow enhancer, a colorant, a dispersant, a stabilizer, or any combinations thereof. Preferably, the other additives are at least one selected from the group comprising a lubricant, an antioxidant, a nucleating agent, a colorant, or any combinations thereof.
[0112] In a preferable embodiment of the invention, the other additives may comprise a lubricant, an antioxidant, a nucleating agent and a colorant. Customary and known lubricants, antioxidants, nucleating agents and colorants for polyamide can be used for producing the polyamide compositions of the present invention. The above-mentioned additives can be used alone or in any combination in any desired mixing ratio.
[0113] Where the other additives are present, the total amount of all the other additives, based on the total weight of the polyamide composition, is 0.2-10 wt%, preferably 0.5 to 8 wt%, more preferably 0.6 to 5 wt%, most preferably 0.7 to 3 wt%. In the present invention, for example, the total amount of all the other additives, based on the total weight of the polyamide composition, may be 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 1.0 wt%, 1.2 wt%, 1.5 wt%, 1.8 wt%, 2.0 wt%, 2.2 wt%, 2.4 wt%, 2.5 wt%, 2.7 wt%, 2.8 wt%, 3.0 wt%, 3.2 wt%, 3.5 wt%, 3.6 wt%, 3.8 wt%, 4.0 wt%, 4.1 wt%, 4.4 wt%, 4.5 wt%, 4.6 wt%, 5.0 wt%, 5.2 wt%, 5.6 wt%, 6.4 wt%, 6.7 wt%, 7.2 wt%, 7.5 wt%, 8.0 wt%, 8.4 wt%, 8.7 wt%, 9.0 wt%, 9.2 wt%, 9.4 wt%, 9.5 wt%, 9.6 wt%, or 10.0 wt%, or within a range of any two values aforesaid.
[0114] As antioxidants, customary and known antioxidants for polyamide production are optionally used for producing the polyamide compositions of the present invention. The antioxidant is preferably selected from sterically hindered phenolic antioxidants. Examples of the antioxidant may be products under the trade name of (available from BASF) , such as 1098. Typically, the total amount of the antioxidant is preferably from 0.02 to 5.0 %by weight, more preferably from 0.05 to 3.0%by weight, more preferably from 0.1 to 1.5%by weight, based on the total weight of the polyamide compositions.
[0115] As lubricants, customary and known lubricants for polyamide production are optionally used for producing the polyamide compositions of the present invention. The lubricant is preferably selected from those lubricants which can significantly improve the filler dispersion or provide lubricating effects in all kinds of molded (e.g., injection molded) polyamides. Suitable examples of the lubricants are stearamide type lubricant or salts (such as calcium salt) of long chain, saturated, linear carboxylic acids (such as montanic acids) , or any combinations thereof. Typically, the total amount of the lubricant is preferably from 0.05 to 3.0 %by weight, more preferably from 0.1 to 2.0%by weight, based on the total weight of the polyamide compositions.
[0116] As nucleating agents, customary and known nucleating agents for polyamide production are optionally used for producing the polyamide compositions of the present invention. The nucleating agent is preferably at least one selected from inorganic nucleating agents. Suitable examples of the nucleating agents are talcum powder, nanosilicon dioxide, nanometer titania and the like. Typically, the total amount of the nucleating agent is preferably from 0.02 to 2.0 %by weight, more preferably from 0.05 to 1.0%by weight, based on the total weight of the polyamide compositions.
[0117] As flow enhancers, customary and known flow enhancers for polyamide production are optionally used for producing the polyamide compositions of the present invention. Typically, the total amount of the flow enhancer is preferably from 0.05 to 3.0 %by weight, more preferably from 0.1 to 2.0%by weight, based on the total weight of the polyamide compositions.
[0118] As colorants, customary and known colorants for polyamide production are optionally used for producing the polyamide compositions of the present invention. Suitable examples of the colorants are organic black pigments, aniline black, carbon black and the like. Typically, the total amount of the colorant is preferably from 0.05 to 5.0 %by weight, more preferably from 0.1 to 3.0%by weight, based on the total weight of the polyamide compositions.
[0119] As dispersants, customary and known dispersants for polyamide production are optionally used for producing the polyamide compositions of the present invention. Typically, the total amount of dispersants is preferably from 0.05 to 3.0 %by weight, more preferably from 0.1 to 2.0%by weight, based on the total weight of the polyamide compositions.
[0120] As stabilizers, customary and known stabilizers for polyamide production are optionally used for producing the polyamide compositions of the present invention. Typically, the total amount of stabilizers is preferably from 0.05 to 3.0 %by weight, more preferably from 0.1 to 2.0%by weight, based on the total weight of the polyamide compositions.
[0121] In a preferable embodiment of the invention, the polyamide composition comprises:
[0122] a) 25 wt%to 65 wt%, preferably 28 wt%to 62 wt%, more preferably 30 wt%to 60 wt%of the first semi-aromatic polyamide;
[0123] b) 3 wt%to 30 wt%, preferably 4 wt%to 25 wt%, more preferably 5 wt%to 20 wt%of the second semi-aromatic polyamide;
[0124] c) 10 wt%to 55 wt%, preferably 15 wt%to 50 wt%, more preferably 20 wt%to 45 wt%of the reinforcing agent; and
[0125] d) 10 wt%to 30wt%, preferably 12 wt%to 25wt%, more preferably 13 wt%to 20 wt%of the flame retardant;
[0126] based on the total weight of the polyamide composition.
[0127] Preferably, the polyamide composition as described herein has a water uptake of no more than 1.60 %, for example, from 0.50%to 1.60 %, preferably from 0.55%to 1.50 %, under 70℃ and 62 RH %after 14 days, determined according to ISO 62.
[0128] Preferably, the polyamide composition as described herein has a MVR (melt volume rate) of from 7 to 40 mL / 10 minutes, preferably from 9 to 38 mL / 10 minutes, particularly preferably from 12 to 27 mL / 10 minutes, determined according to ISO 1133 at a temperature of 325 ℃, with a load of 2.16 kg, or has a MVR of 40 to 55 mL / 10 minutes, preferably from 41 to 50 mL / 10 minutes, particularly preferably from 42 to 49 mL / 10 minutes, determined according to ISO 1133 at a temperature of 300 ℃, with a load of 5 kg.
[0129] Preferably, the polyamide composition as described herein has a tensile strength of from 140 MPa to 200 MPa, preferably from 150 MPa to 185 MPa, particularly preferably from 167 MPa to 182 MPa, determined according to ISO 527-1-2012.
[0130] The present invention also provides a method for preparing the polyamide composition according to the present invention, comprising the following steps:
[0131] S1) compounding components (a) - (b) and (d) - (e) to form a mixture, and then feeding the mixture and component (c) into an extruder,
[0132] S2) melting the materials in the extruder to form a melt, and then extruding the melt and optionally pelletizing, to obtain the polyamide composition.
[0133] The general preparation process may be as follows: all raw materials except the reinforcing agent are mixed together in a stirrer to form a mixture. Then, the mixture is fed into an extruder at the main throat and the reinforcing agent is fed at downstream using a side feeder to keep good mechanical property. The raw materials are melt-extruded under a temperature of greater than 300℃ (such as 300-320℃) , then optionally pelletized and dried, so as to obtain a thermoplastic polyamide composition, preferably in a pellet form for storage or further application.
[0134] The present invention also provides a molded article, comprising at least one polyamide composition according to the present invention.
[0135] In the present invention, the inventive polyamide materials are especially suitable for the applications in the field of electronic and electrical appliances, such as connectors, capacitors, transformer shells, or the like.
[0136] EXAMPLES
[0137] The following non-limiting examples illustrate various features and characteristics of the present invention, the scope of the present invention should not be construed as limited thereto.
[0138] The following starting materials (i.e., raw materials) were used:
[0139] PA6T / 66: purchased from Mitsui. The PA6T / 66 is based on hexamethylenediamine, terephthalic acid (T) and adipic acid. The PA6T / 66 has a Tm of about 305 ℃, a Tg of about 86 ℃, and a fusion enthalpy of about 53 kJ / kg.
[0140] PA6T / 5T: home-made. The PA6T / 5T is based on terephthalic acid (T) , hexamethylenediamine and 1, 5-pentanediamine. The molar relative percentage between hexamethylenediamine and 1, 5-pentanediamine in the polymer is 50: 50 mol / mol. The PA6T / 5T has a Tm of about 305 ℃, a Tg of about 139℃, and a fusion enthalpy of about 64 kJ / kg.
[0141] PA66 / 6T: purchased from DOMO chemicals. The PA66 / 6T is based on hexamethylenediamine, terephthalic acid (T) and adipic acid. The PA66 / 6T has a Tm of about 280℃, a Tg of about 80℃, and a fusion enthalpy of about 55 kJ / kg.
[0142] PA6T / DT: home-made. The PA6T / DT is based on terephthalic acid (T) , hexamethylenediamine and 2-methyl-1, 5-pentanediamine. The molar relative percentage between hexamethylenediamine and 2-methyl-1, 5-pentanediamine in the polymer is 50: 50 mol / mol. The PA6T / DT has a Tm of about 300 ℃, a Tg of about 140 ℃, and a fusion enthalpy of about 37 kJ / kg.
[0143] PA9T: purchased from Kuraray. The PA9T has a Tm of about 305 ℃, a Tg of about 120 ℃, and a fusion enthalpy of about 74 kJ / kg.
[0144] Flame retardant: Exolit OP 1230, Aluminum diethylphosphinate, CAS#: 225789-38-8, Clariant Produkte (Deutschland) GmbH, Chemiepark Knapsack, 50351 Hürth, water content % (w / w) < 0.2, average particle size (D50) 20-40 μm.
[0145] Exolit OP 1400, Halogen-free flame-retardant mixture based on di-alkyl-phosphinates (Clariant Plastics &Coatings (Deutschland) GmbH) .
[0146] Glass fiber: ECSHP3610 EC10-3.5, purchased from Nippon Electric Glass Co., Ltd;
[0147] ECS301 HP-3-M4, purchased from Chongqing Polycomp International Corp. ;
[0148] Antioxidant: Irganox 1098, purchased from BASF;
[0149] Lubricant: Ethylene bis stearamide (EBS) , purchased from CRODA.
[0150] Measurement standard for property test
[0151] Tensile strength, tensile modulus and elongation at break were measured according to ISO 527-1-2012. Test specimens of type 1 having a thickness of 4 mm described in ISO 527-1-2012 were used. Charpy notched impact strength and Charpy unnotched impact strength were measured according to ISO 179-1-2010 via edgewise impact. The test specimens for Charpy unnotched test were type 1 specimen with the dimensions of 80 × 10 × 4 mm (length × width × thickness) . The test specimens for Charpy notched test were type 1 with notched type A. The test specimens were pretreated in air under a relative humidity of 50%at 23 ℃ for 16 hours.
[0152] The flexural strength corresponds to the maximum stress in the bending test. The bending test is a three -point bending test according to ISO 178.
[0153] Heat resistance of the specimens was determined according to ISO 75 (HDT A) (with a load of 1.8 MPa, temperature rise of 50 K per hour, on ISO specimens) .
[0154] MVR was determined according to ISO 1133 at a temperature of 300-325 ℃, with a load of 2.16-5 kg.
[0155] Water uptake was determined according to ISO 62.
[0156] The flame retardancy of the molding compositions was determined firstly by the UL 94V method (Underwriters Laboratories Inc. Standard of Safety, "Test for Flammability of Plastic Materials for Parts in Devices and Appliances" , p. 14 to p. 18, Northbrook 1998) at 0.4 mm thickness, 1.0mm thickness, or 1.5 mm thickness.
[0157] Heat aging test was conducted according to ISO 2578-1993 in air under 180 ℃ for a period of time as indicated in Table 5 below.
[0158] The test specimens used were made according to the following general procedure for preparing the test specimens.
[0159] General procedure for preparing the test specimens
[0160] Test specimens were prepared in accordance with the formulations as shown in following Tables. All raw materials except glass fiber were mixed together in, for example, a Tubula T50A high-speed stirrer and then fed into, for example, a Coperion ZSK26 MC twin-screw extruder at the throat, and the glass fiber was fed at downstream using a side feeder, then melt-extruded under a temperature of 320 ℃, and pelletized and dried at a temperature of 100 ℃ for 6 hours, thus obtaining dried pellets.
[0161] The dried pellets were then processed in an injection molding machine (Haitian MA900 II) with a clamping force of 900 kN at a melting temperature of 320℃ and a molding temperature of 140℃ to provide a test specimen.
[0162] The test specimens obtained were measured for the properties as described above. The formulations for preparing the test specimens and the test results thereof are summarized in following tables.
[0163] The mechanical properties, water uptake resistance and processability of Comparative Examples C1-C5 and Inventive Examples A1-A6 were shown in Tables 1-4. It can be seen that the mechanical properties, water uptake resistance and processability of the Inventive Examples based on the combination of the first semi-aromatic polyamide and the second semi-aromatic polyamide were superior compared with the Comparative Examples based on the first semi-aromatic polyamide or the second semi-aromatic polyamide alone. The combination of the first semi-aromatic polyamide and the second semi-aromatic polyamide was believed to result in synergistic effects which provide this unique combination of advantageous properties.
[0164] Table 1
[0165] *RH%represents Relative Humidity%.
[0166] From the above test results in Table 1, it can be seen that, as compared with the Comparative Examples C1 and C2 using one polyamide (i.e. PA6T / 66 or PA6T / DT) as the matrix resin, the present application Examples A1 and A2, in which a blend of two different semi-aromatic polyamides (i.e. PA6T / 66 and PA6T / DT) plays as the matrix resin, showed significantly decreased water uptake (meaning improved water absorption resistance performance) under the condition of elevated temperature and high relative humidity, and distinctly increased MVR value (meaning improved flowability under melted status which contributes to excellent processability) , while at the same time showcasing improved mechanical properties, in particular in terms of impact strength, tensile strength, and flexural strength, which indicated that the combination of two inventive polyamides may exert surprisingly synergistic effects on the final material. This may be attributed to a proper difference between the enthalpy of fusion of PA6T / 66 and PA6T / DT, resulting in a good thermodynamic compatibility which may contribute to a satisfied uniform melting blend during preparation.
[0167] Table 2
[0168] *RH%represents Relative Humidity%.
[0169] Similarly, it can also be seen from the above Table 2 that the combination of two proper semi-aromatic polyamides (i.e. PA6T / 5T and PA6T / DT) could result in a polyamide composition with significantly decreased water uptake (meaning improved water absorption resistance performance) under the condition of elevated temperature and high relative humidity, and distinctly increased MVR value (meaning improved flowability under melt status which contributes to excellent processability) , while at the same time showcasing improved mechanical properties, in particular in terms of Charpy unnotched impact strength, tensile strength, and flexural strength, which indicated that the combination of two inventive polyamides may exert surprisingly synergistic effects on the final material. This may be attributed to a proper difference between the enthalpy of fusion of PA6T / 5T and PA6T / DT, resulting in a good thermodynamic compatibility which may contribute to a satisfied uniform melting blend during preparation.
[0170] Table 3
[0171] *RH%represents Relative Humidity%.
[0172] Likewise, it can also be seen from the above Table 3 that the combination of two inventive polyamides (i.e. PA66 / 6T and PA6T / DT) could result in a polyamide composition with decreased water uptake (meaning improved water absorption resistance performance) under the condition of elevated temperature and high relative humidity, and distinctly increased MVR value (meaning improved flowability under melt status which contributes to excellent processability) , while at the same time showcasing improved mechanical properties, in particular in terms of impact strength, tensile modulus, tensile strength, and flexural strength, which indicated that the combination of two inventive polyamides may exert surprisingly synergistic effects on the final material. This may be attributed to a proper difference between the enthalpy of fusion of PA66 / 6T and PA6T / DT, resulting in a good thermodynamic compatibility which may contribute to a satisfied uniform melting blend during preparation.
[0173] Table 4
[0174] *RH%represents Relative Humidity%.
[0175] Based on the above Table 4, the present application Example A6, in which a proper amount of PA6T / DT was incorporated into the matrix resin (i.e., PA9T) , showcased significantly decreased water uptake, under an elevated temperature and a high relative humidity, and increased MVR value compared with Comparative Example C5. Surprisingly, in addition to the refinement of water uptake resistance as well as processability, Example A6 also exhibited improved mechanical properties particularly in terms of impact strength, tensile strength, and flexural strength. This may be attributed to a proper difference between the enthalpy of fusion of PA9T and PA6T / DT, resulting in a good thermodynamic compatibility which may contribute to a satisfied uniform melting blend during preparation.
[0176] Table 5
[0177] *RH%represents Relative Humidity%.
[0178] Furthermore, in view of Table 5, the present application Examples A7-A9 surprisingly exhibited superior tensile strength retentions after heat aging compared with Comparative Examples C6-C8, in addition to the improved water uptake resistance, processability as well as mechanical properties. This indicates that the composition according to the present application could also possess improved heat aging resistance performance. This may be attributed to a proper difference between the enthalpy of fusion of PA66 / 6T and PA6T / DT, resulting in a good thermodynamic compatibility which may contribute to a satisfied uniform melting blend during preparation.
[0179] The structures, materials, compositions, and methods described herein are intended to be representative examples of the invention, and it will be understood that the scope of the invention is not limited by the scope of the examples. Those skilled in the art will recognize that the invention may be practiced with variations on the disclosed structures, materials, compositions and methods, and such variations are regarded as within the ambit of the invention. Thus, it is intended that the present invention cover such modifications and variations as come within the scope of the appended claims and their equivalents.
Claims
1.A polyamide composition, comprising the following components:a) a first semi-aromatic polyamide having a glass transition temperature of from 70℃ to 145℃;b) a second semi-aromatic polyamide having a glass transition temperature of from 110℃ to 160℃, which is different from the first semi-aromatic polyamide;c) at least one reinforcing agent;d) at least one flame retardant; ande) optionally at least one further additive;wherein the weight ratio of the component a) to the component b) is in the range of (2.4 -10) : 1, preferably in the range of (2.5 -8) : 1.2.The polyamide composition according to claim 1, wherein the first semi-aromatic polyamide is at least one polyamide derived from a linear aliphatic C4-C12 diamine and an aromatic C5-C12 dicarboxylic acid, or derived from a linear aliphatic C4-C10 diamine, at least one aromatic C5-C12 dicarboxylic acid and a linear aliphatic C4-C10 dicarboxylic acid, or derived from two different linear aliphatic C4-C10 diamines and at least one aromatic C5-C12 dicarboxylic acid.3.The polyamide composition according to claim 1 or 2, wherein the second semi-aromatic polyamide is at least one polyamide derived from at least one linear aliphatic C4-C10 diamine, a branched aliphatic C4-C10 diamine, and at least one aromatic C5-C12 dicarboxylic acid.4.The polyamide composition according to any one of claims 1 to 3, wherein the enthalpy of fusion of the first semi-aromatic polyamide (ΔHf1) and the enthalpy of fusion of the second semi-aromatic polyamide (ΔHf2) are each independently more than 15 kJ / kg, preferably more than 20 kJ / kg.5.The polyamide composition according to any one of claims 1 to 4, wherein the difference of the enthalpy of fusion between the first semi-aromatic polyamide and the second semi-aromatic polyamide (ΔHf1-ΔHf2) is in the range of from 1 to 45 kJ / kg, preferably from 3 to 40 kJ / kg.6.The polyamide composition according to any one of claims 3 to 5, wherein the molar percentage of the branched aliphatic C4-C10 diamine is in the range of from 40 mol%to 60 mol%, preferably in the range of from 45 mol%to 55mol%, based on the total amount of the diamine in the second semi-aromatic polyamide.7.The polyamide composition according to claim 6, wherein the branched aliphatic C4-C10 diamine is at least one selected from the group consisting of methyl substituted linear aliphatic C3-C9 diamine, and the at least one aromatic C5-C12 dicarboxylic acid is one or more selected from the group consisting of terephthalic acid, isophthalic acid, phthalic acid, and any combinations thereof.8.The polyamide composition according to claim 7, wherein the second semi-aromatic polyamide is at least one selected from the group consisting of PA6T / DT, PA5T / 6T / DT, PA5T / DT, PA6T / 6I / DT, PA4T / 6T / DT, PA4T / 10T / DT, PA4T / 4I / 6T / 6I / DT / DI or any combinations thereof.9.The polyamide composition according to any one of claims 1 to 8, wherein the first semi-aromatic polyamide is at least one selected from the group consisting of PA5T, PA6T, PA9T, PA10T, PA11T, PA12T or any combinations thereof.10.The polyamide composition according to any one of claims 1 to 8, wherein the first semi-aromatic polyamide is derived from a linear aliphatic C4-C10 diamine, at least one aromatic C5-C12 dicarboxylic acid and a linear aliphatic C4-C10 dicarboxylic acid, and the molar percentage of the aromatic C5-C12 dicarboxylic acid is in the range of from 50 mol%to 70 mol%, preferably in the range of from 55 mol%to 65 mol%, based on the total amount of the dicarboxylic acid in the first semi-aromatic polyamide.11.The polyamide composition according to claim 10, wherein the first semi-aromatic polyamide is at least one selected from the group consisting of PA610 / 6T, PA66 / 6T, PA6T / 66, PA5T / 56, PA66 / 6T / 6I, PA1010 / 10T, and any combinations thereof.12.The polyamide composition according to any one of claims 1 to 8, wherein the first semi-aromatic polyamide is derived from two different linear aliphatic C4-C10 diamines and at least one aromatic C5-C12 dicarboxylic acid, and wherein the two different linear aliphatic C4-C10 diamines are a linear aliphatic C4-C5 diamine and a linear aliphatic C6-C10 diamine, respectively, and the molar percentage of the linear aliphatic C4-C5 diamine is in the range of from 40 mol%to 60 mol%, preferably in the range of from 45 mol%to 55 mol%, based on the total amount of the diamine in the first semi-aromatic polyamide.13.The polyamide composition according to claim 12, wherein the first semi-aromatic polyamide is at least one selected from the group consisting of PA6T / 5T, PA4T / 6T or any combinations thereof.14.The polyamide composition according to any one of claims 1 to 13, wherein the first semi-aromatic polyamide has a melting temperature between 260℃ and 320 ℃, preferably between 270 ℃ and 310 ℃, and the second semi-aromatic polyamide has a melting temperature between 290℃ and 310 ℃, preferably between 295 ℃ and 305 ℃.15.The polyamide composition according to any one of claims 1 to 14, wherein the sum of the first semi-aromatic polyamide and the second semi-aromatic polyamide is in the range of 30-90 wt%, preferably 35-80 wt%, more preferably 40-70 wt%, in particular 43-60 wt%, based on the total weight of the polyamide composition.16.The polyamide composition according to any one of claims 1 to 15, wherein the polyamide composition comprisesa) 25 wt%to 65 wt%, preferably 28 wt%to 62 wt%, more preferably 30 wt%to 60 wt%of the first semi-aromatic polyamide;b) 3 wt%to 30 wt%, preferably 4 wt%to 25 wt%, more preferably 5 wt%to 20 wt%of the second semi-aromatic polyamide;c) 10 wt%to 55 wt%, preferably 15 wt%to 50 wt%, more preferably 20 wt%to 45 wt%of the reinforcing agent; andd) 10 wt%to 30wt%, preferably 12 wt%to 25wt%, more preferably 13 wt%to 20 wt%of the flame retardant;based on the total weight of the polyamide composition.17.The polyamide composition according to any one of claims 1 to 16, wherein the reinforcing agent is at least one selected from the group consisting of glass fibers, carbon fibers, graphite fibers, aramid fibers, potassium titanate fibers, and any combinations thereof.18.The polyamide composition according to any one of claims 1 to 17, wherein the flame retardant is at least one selected from the group consisting of phosphorus-containing flame retardants, nitrogen-containing flame retardants, halogenated flame retardants, and any combinations thereof.19.The polyamide composition according to any one of claims 1 to 18, wherein the polyamide composition has a water uptake of no more than 1.60 %under 70℃and 62 RH %after 14 days, determined according to ISO 62.20.Molded article, comprising the polyamide composition according to any one of claims 1 to 19.