Manufacturing method for metal composite pipe, and pipeline
By setting an alloy powder layer and performing gradient heating and protective atmosphere treatment during the manufacturing process of metal composite pipes, the problem of low bonding strength in existing metal composite pipes is solved, achieving efficient and low-cost metallurgical bonding, which is suitable for pipe manufacturing in highly corrosive environments.
Patent Information
- Application Number
- PCT/CN2026/095012
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
Existing metal composite pipe manufacturing processes suffer from low bonding strength, high cost, low production efficiency, and complex processes, making it difficult to meet production needs in highly corrosive media and harsh environments.
By setting an alloy powder layer between the first and second pipes, and then pressing and heating it to remelt the alloy layer to form a metallurgical bond, the temperature gradient and protective atmosphere are controlled during the bonding process to ensure the interfacial bonding strength between the alloy layer and the two pipes.
It achieves high-strength interface bonding, adapts to performance consistency at different angles and positions, reduces manufacturing costs and improves production efficiency, avoids delamination, and has good machinability.
Smart Images

Figure CN2026095012_12112026_PF_FP_ABST
Abstract
Description
Manufacturing methods and pipelines of metal composite pipes Technical Field
[0001] This invention belongs to the field of metal pipe manufacturing, and particularly relates to a method for manufacturing a metal composite pipe and the pipe itself. Background Technology
[0002] In industrial production, especially in scenarios involving highly corrosive media or harsh environments such as thermal combustion, chemical engineering, marine engineering, and oil and gas extraction, pipeline systems in production equipment are constantly exposed to combined corrosive factors such as acidic and alkaline media, high-salt spray environments, or high temperatures and pressures. Traditional single-layer metal pipelines often suffer from wall thinning, stress cracking, and even media leakage due to surface corrosion, seriously threatening production safety and significantly increasing pipeline maintenance frequency.
[0003] To improve production safety and reduce maintenance costs, metal composite pipes are commonly used in existing technologies to construct pipeline systems in the aforementioned production scenarios. Metal composite pipes consist of at least two layers: a base pipe layer and a corrosion-resistant layer. The base pipe layer is mainly used to provide rigidity, while the corrosion-resistant layer wraps around the outer surface of the base pipe layer or covers the inner surface of the base pipe layer to provide corrosion protection. If both the inner and outer surfaces of the base pipe layer are covered with corrosion-resistant layers, then such pipes with corrosion-resistant treatment on both the inside and outside can cope with harsh working scenarios where both the external environment and internal transmission are corrosive.
[0004] The forming processes of metal composite pipes can be broadly categorized into mechanical composite processes and metallurgical composite processes. Mechanical composite processes involve using specific cold forming methods to tightly bond the inner and outer metal layers together to form the composite pipe. While this method has lower manufacturing costs, the bonding strength between the two metal layers is also low, making them prone to delamination and unsuitable for expansion joints and bends. Therefore, to meet the production demands in scenarios involving highly corrosive media or harsh environments, as mentioned earlier, metal composite pipes formed using mechanical composite processes are increasingly being replaced by those formed using metallurgical composite processes. Metallurgical composite processes, on the other hand, involve using hot forming methods to create atomic diffusion between the base pipe and the outer / lined pipe interface. This results in the outer pipe tightly wrapping the base pipe, or the inner cavity of the base pipe tightly bonding with the liner, forming the metal composite pipe. The outer / lined pipe corresponds to the corrosion-resistant layer described earlier.
[0005] Traditional metallurgical composite processes each have their own drawbacks. For example, in hot rolling forming, most easily oxidized ferrous metal materials cannot be combined through rolling; in hot extrusion forming, the formed surface is rough, the uniformity of the pipe end wall thickness is poor, and since the bonding effect depends on the element interface diffusion within a very short time during extrusion, it is usually affected by the presence of oxide films, and the problem of interface stress concentration is difficult to overcome; in centrifugal casting combined with hot extrusion, the metal combination is limited, interlayer inclusion defects are prone to occur, and the uniformity of the pipe end wall thickness is poor; in centrifugal aluminothermic forming, if there is no subsequent hot deformation, it is limited to use in the cast state, the composition of the cladding layer is difficult to control, and the coarse cast structure of the cladding layer prevents the mechanical properties of the cladding metal from being fully utilized; in explosive welding forming, its productivity is low and the production process is highly dangerous; in cladding (surfacing) composite forming, the production cost is high, the process is complex, and the material combination of the pipes that can be produced has compatibility limitations.
[0006] Therefore, the current technical challenge is to provide a manufacturing process for metal composite pipes that can meet expectations in terms of manufacturing cost, production efficiency, and the strength of the finished pipe. Summary of the Invention
[0007] To overcome the aforementioned deficiencies in the prior art, the present invention provides a method for manufacturing a metal composite pipe, the method comprising:
[0008] A first pipe and a second pipe are provided, both of which are made of metal. The first pipe has a first surface and the second pipe has a second surface.
[0009] Alloy powder is attached to the first surface or the second surface to form an alloy layer covering the first surface or the second surface;
[0010] The first tube and the second tube are coaxially sleeved together, with the first surface facing the second surface, and the alloy layer is placed between the first surface and the second surface to form a multilayer tube;
[0011] The multilayer tube is subjected to a compression composite process to form an interference fit between the first tube and the second tube;
[0012] The multilayer tube is heated to bring the temperature of the alloy layer to its remelting temperature.
[0013] The multilayer tube is cooled to obtain a metal composite tube, wherein the alloy layer in the metal composite tube forms a metallurgical bond with the first surface and the second surface respectively, and the first tube material forms an interface bond with the second tube material through the alloy layer.
[0014] According to one aspect of the present invention, the step of heating the multilayer tube in the manufacturing method includes: placing the multilayer tube in a heating furnace and heating the multilayer tube as a whole; or sequentially transferring multiple sections of the multilayer tube to the heating furnace for segmented heating along a predetermined feeding direction.
[0015] According to another aspect of the invention, in the manufacturing method, the step of overall heating or segmented heating includes: controlling the power of the heating furnace so that the temperature of the heated section located in the heating furnace in the multilayer tube increases in a gradient manner.
[0016] According to another aspect of the present invention, in the manufacturing method, the gradient heating includes the following stages: a first stage, continuously heating the heated section until the temperature of the heated section reaches a first temperature; a second stage, continuing to heat the heated section until the temperature of the heated section reaches a second temperature; and a third stage, continuing to heat the heated section until the temperature of the heated section reaches the remelting temperature.
[0017] According to another aspect of the invention, in the manufacturing method, the first temperature is not higher than 750°C; the second temperature is greater than the first temperature and less than the remelting temperature.
[0018] According to another aspect of the invention, in the manufacturing method, when the multilayer tube is heated as a whole or in segments, the multilayer tube rotates about its central axis, and / or the induction coil group of the heating furnace rotates around the multilayer tube.
[0019] According to another aspect of the invention, in the manufacturing method, when the multilayer tube is subjected to the overall heating or the segmented heating, a clamping force is applied to the outside of the multilayer tube.
[0020] According to another aspect of the present invention, in the manufacturing method, when the multilayer tube is subjected to overall heating or segmented heating, the inner cavity of the multilayer tube is sealed and a protective gas is injected into the inner cavity so that the gas pressure value in the inner cavity is not lower than a predetermined threshold.
[0021] According to another aspect of the invention, in the manufacturing method, the predetermined threshold ranges from 0.1 MPa to 10 MPa.
[0022] According to another aspect of the present invention, the step of cooling the multilayer tube in the manufacturing method includes: providing a spray device or an air-cooling device at the outlet of the multilayer tube to cool the multilayer tube.
[0023] According to another aspect of the invention, after the cooling treatment, the manufacturing method further includes: tempering the metal composite tube.
[0024] According to another aspect of the invention, before attaching the alloy powder, the manufacturing method further includes: roughening the surface of the first surface or the second surface carrying the alloy powder.
[0025] According to another aspect of the invention, in the manufacturing method, the melting point of the alloy layer is lower than the melting points of the first pipe and the second pipe; the thickness of the alloy layer ranges from 0.01 mm to 0.5 mm, and the thickness of the first pipe and the second pipe is at least twice the thickness of the alloy layer.
[0026] According to another aspect of the invention, in the manufacturing method, the first tube is sleeved on the outside of the second tube, the first surface is the inner surface of the first tube, and the second surface is the outer surface of the second tube; the alloy powder is sprayed onto the first surface or the second surface.
[0027] According to another aspect of the present invention, in the manufacturing method, the step of compressing and bonding the multilayer tube includes: sealing a cavity formed by the inner surface of the second tube and injecting a pressurizing medium into the cavity, so that the second tube undergoes plastic expansion deformation and then adheres tightly to the first tube; the material of the first tube includes any or all of carbon steel and iron-based alloys; the material of the second tube includes any, any combination or all of alloy steel, 316L stainless steel, nickel-based alloys, cobalt-based alloys and titanium alloys; the material of the alloy layer includes any, any combination or all of nickel-based alloys, cobalt-based alloys or iron-based alloys doped with boron and / or silicon.
[0028] According to another aspect of the invention, in the manufacturing method, the second tube is sleeved on the outside of the first tube, the first surface is the outer surface of the first tube, and the second surface is the inner surface of the second tube; the alloy powder is sprayed onto the first surface or the second surface.
[0029] According to another aspect of the present invention, in the manufacturing method, the step of compressing and bonding the multilayer tube includes: setting a mandrel in a cavity formed by the inner surface of the first tube, and applying radial pressure to the outer surface of the second tube, so that the second tube undergoes plastic diameter reduction deformation and then adheres tightly to the first tube; the material of the first tube includes any or all of carbon steel and iron-based alloys; the material of the second tube includes any, any combination or all of alloy steel, 316L stainless steel, nickel-based alloys, cobalt-based alloys and titanium alloys; the material of the alloy layer includes any, any combination or all of nickel-based alloys, cobalt-based alloys or iron-based alloys doped with boron and / or silicon.
[0030] In addition, the present invention also provides a pipe for waste incineration equipment or oil and gas transmission equipment, wherein the pipe is constructed partially or entirely using a metal composite pipe prepared by the manufacturing method described above.
[0031] The manufacturing method of the metal composite pipe provided by this invention involves setting an alloy layer between a first pipe and a second pipe and remelting it. This alloy layer forms a metallurgical bond with both the first and second pipes, thereby creating an interfacial bond between the first pipe and the second pipe through the alloy layer. The resulting metal composite pipe can meet the performance consistency requirements of various pipe diameters, lengths, and angles. Due to the high strength of the metallurgical bond, the first and second pipes have sufficient interfacial bonding strength, making it difficult for the layers of the metal composite pipe to separate even after subsequent plastic deformation machining processes, such as bending or diameter reduction. Compared to existing metallurgical composite processes for manufacturing metal composite pipes, the manufacturing method of this invention has advantages such as simple process, low cost, strong compatibility, high safety, and high yield. Attached Figure Description
[0032] Other features, objects, and advantages of the invention will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings:
[0033] Figure 1 is a flowchart illustrating a specific embodiment of the manufacturing method of the metal composite pipe according to the present invention;
[0034] Figure 2 is a schematic cross-sectional view of an alternative embodiment of an internally corrosion-resistant metal composite pipe prepared according to the manufacturing method shown in Figure 1.
[0035] Figure 3 is a schematic diagram of an optional embodiment of step S200 shown in Figure 1;
[0036] Figure 4 is a schematic diagram of another optional embodiment of step S200 shown in Figure 1;
[0037] Figure 5 is a schematic diagram of an optional embodiment of step S300 shown in Figure 1;
[0038] Figure 6 is a schematic diagram of an optional embodiment of step S400 shown in Figure 1;
[0039] Figure 7 is a schematic diagram of a preferred embodiment of the compression composite process described in step S400 of Figure 1;
[0040] Figure 8 is a schematic diagram of an optional embodiment of steps S500 and S600 shown in Figure 1;
[0041] Figure 9 is a schematic cross-sectional view of an optional embodiment of the externally corrosion-resistant metal composite pipe prepared according to the manufacturing method shown in Figure 1;
[0042] Figure 10 is a schematic diagram of an alternative embodiment of step S400 shown in Figure 1;
[0043] Figure 11 is a schematic diagram of another preferred embodiment of step S400 shown in Figure 1.
[0044] The same or similar reference numerals in the accompanying drawings represent the same or similar parts. Detailed Implementation
[0045] To better understand and explain this invention, a further detailed description will be provided below with reference to the accompanying drawings. This invention is not limited to these specific embodiments. Rather, any modifications or equivalent substitutions made to this invention should be covered within the scope of the claims.
[0046] It should be noted that numerous specific details are provided in the following detailed embodiments. Those skilled in the art should understand that the present invention can be practiced without these specific details. In the various detailed embodiments given below, structures and components well-known in the art are not described in detail in order to highlight the spirit of the invention.
[0047] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.
[0048] In the description of this embodiment, the terms "upper," "lower," "right," etc., refer to the orientation or positional relationship shown in the accompanying drawings. They are used only for ease of description and simplification of operation, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the present invention. In addition, the terms "first" and "second" are used only for distinction in description and have no special meaning.
[0049] The following description, in conjunction with the accompanying drawings, details various specific embodiments of the present invention. It should be noted that the accompanying drawings are merely illustrative of the technical solutions and core concepts of the present invention. The shapes and dimensions of the components in the specific embodiments shown in the accompanying drawings are not strictly based on the form of an actual product, and the shape and size proportions of the actual product may differ from those of the specific embodiments shown in the accompanying drawings. Therefore, the specific embodiments shown in the drawings should not be construed as the sole limitation on the actual product corresponding to the present invention, nor should they be used as the sole basis for determining shape and size comparisons in patent infringement cases.
[0050] Please refer to Figure 1, which is a flowchart illustrating a specific embodiment of the manufacturing method of a metal composite pipe according to the present invention. As shown in Figure 1, the manufacturing method of a metal composite pipe provided by the present invention includes the following steps:
[0051] Step S100: Provide a first pipe and a second pipe, both of which are made of metal. The first pipe has a first surface and the second pipe has a second surface.
[0052] Step S200: Attach alloy powder to the first surface or the second surface to form an alloy layer covering the first surface or the second surface;
[0053] Step S300: The first tube and the second tube are coaxially sleeved together, with the first surface facing the second surface, and the alloy layer is placed between the first surface and the second surface to form a multilayer tube;
[0054] Step S400: The multilayer tube is subjected to a compression composite process to make the first tube and the second tube form an interference fit;
[0055] Step S500: The multilayer tube is heated to bring the temperature of the alloy layer to its remelting temperature.
[0056] Step S600: Cool the multilayer tube to obtain a metal composite tube. The alloy layer in the metal composite tube forms a metallurgical bond with the first surface and the second surface, respectively, and the first tube material forms an interface bond with the second tube material through the alloy layer.
[0057] Specifically, one objective of this invention is to provide a method for manufacturing a metal composite pipe. The metal composite pipe obtained by this method has at least a corrosion-resistant metal layer and a base pipe layer, and the corrosion-resistant layer and the base pipe layer have sufficient interfacial bonding strength. This ensures that the metal composite pipe is less prone to delamination due to insufficient internal interfacial bonding strength during subsequent plastic deformation machining processes. Typically, the corrosion-resistant layer has a thinner thickness and better ductility than the base pipe layer.
[0058] Performing steps S100 to S600 as shown in Figure 1 yields two different types of metal composite pipes: an internally corrosion-resistant metal composite pipe and an externally corrosion-resistant metal composite pipe. For the internally corrosion-resistant metal composite pipe, typically used for closed transport of highly corrosive media (e.g., high-temperature flue gas discharge, oil and gas transport, transport of highly oxidizing media), the corrosive substances are primarily located inside the pipe. Therefore, the internally corrosion-resistant metal composite pipe needs to have corrosion resistance in its inner cavity; that is, the corrosion-resistant layer should be formed on the inner wall of the base pipe layer. For the externally corrosion-resistant metal composite pipe, typically used for closed transport of neutral media under conditions of numerous corrosive factors in the external environment (e.g., deep-sea oil and gas pipelines, underwater cooling pipes, fluidized bed walls, waste incineration combustion chamber walls), the corrosive substances are primarily located on the outside of the pipe. Therefore, the externally corrosion-resistant metal composite pipe needs to have corrosion resistance on its outer surface; that is, the corrosion-resistant layer should be formed on the outer wall of the base pipe layer.
[0059] In step S100, the second pipe can be selected to correspond to the corrosion-resistant layer, and the first pipe can be selected to correspond to the base pipe layer. In step S200, the alloy layer can be formed on the base pipe layer or on the corrosion-resistant layer. Preferably, the alloy layer can be formed by spraying alloy powder onto the target plane using a powder coating process. The powder coating process includes, but is not limited to, electrostatic spraying, thermosetting spraying, and fluidized bed dip coating.
[0060] Taking the selection of the second pipe material corresponding to the corrosion-resistant layer and the manufacturing objective of obtaining the internally anti-corrosion metal composite pipe as an example, the steps of each step in the specific embodiment shown in FIG1 will be explained. Please refer to FIG2. FIG2 is a cross-sectional structural schematic diagram of an optional embodiment of the internally anti-corrosion metal composite pipe prepared according to the manufacturing method shown in FIG1. As shown in FIG2, the internally anti-corrosion metal composite pipe 101 includes a first pipe material 110, a second pipe material 120 and an alloy layer 130, wherein the alloy layer 130 forms a metallurgical bond with the first pipe material 110 and the second pipe material 120 respectively, the first pipe material 110 forms an interface bond with the second pipe material 120 through the alloy layer 130, the first pipe material 110 is sleeved on the outside of the second pipe material 120, and the first pipe material 110 and the second pipe material 120 can be seamless pipes or welded pipes made by welding sheet metal coils.
[0061] Please refer to Figure 3. Figure 3 is a schematic diagram of an optional embodiment of step S200 shown in Figure 1. As shown in Figure 3, when electrostatic spraying or thermosetting spraying is selected to form the alloy layer 130, if the diameter of the first tube 110 is large enough to accommodate the nozzle 201 extending into the first tube 110 for powder spraying, then in step S200, the alloy powder can be sprayed onto the first surface 111 of the first tube 110, that is, an alloy layer 130 covering the first surface 111 is formed. At this time, the first surface 111 is the inner surface of the first tube 110.
[0062] Please refer to Figure 4. Figure 4 is a schematic diagram of another optional embodiment of step S200 shown in Figure 1. As shown in Figure 4, when electrostatic spraying or thermosetting spraying is selected to form the alloy layer 130, if the diameter of the first pipe 110 is small and insufficient to accommodate the nozzle 201 to enter the interior of the first pipe 110 for powder spraying, then in step S200, the alloy powder can be sprayed onto the second surface 121 of the second pipe 120, that is, an alloy layer 130 covering the second surface 121 is formed. At this time, the second surface 121 is the outer surface of the second pipe 120.
[0063] Typically, in order to enable the alloy powder to adhere better to the first surface 111 or the second surface 121, the first surface 111 or the second surface 121 may be roughened before the alloy powder is attached. Since the first tube 110 and the second tube 120 are both made of metal, the roughening process is preferably carried out by sandblasting or shot blasting.
[0064] Regardless of whether step S200 is implemented using the embodiment shown in FIG3 or FIG4, after the alloy layer 130 is formed, the first tube 110 and the second tube 120 need to be coaxially fitted in step S300. More specifically, the first tube 110 is fitted over the outside of the second tube 120. Please refer to FIG5, which is a schematic diagram of an optional embodiment of step S300 shown in FIG1. As shown in FIG5, after the first tube 110 and the second tube 120 are coaxially fitted, a multilayer tube 102 is formed, wherein the inner surface of the first tube 110 faces the outer surface of the second tube 120, and the alloy layer 130 is located between the inner surface of the first tube 110 and the outer surface of the second tube 120.
[0065] Next, step S400 is performed to compress and composite the multilayer tube 102, forming an interference fit between the first tube 110 and the second tube 120. One purpose of step S400 is to ensure a tight fit between the first tube 110, the alloy layer 130, and the second tube 120. The first tube 110 and the second tube 120 compress the alloy layer 130 to obtain an alloy layer 130 of substantially uniform thickness, and to expel as much oxygen as possible between the first tube 110 and the alloy layer 130, or between the second tube and the alloy layer 130. The heat treatment performed on the multilayer tube 102 in step S500 helps improve the temperature uniformity of the alloy layer 130 and also prevents the formation of oxide scale, thus ensuring the remelting effect of the alloy layer 130. Another purpose of performing step S400 is to correct the manufacturing deviation of the second tube 120 through the interference fit, so that the first tube 110 and the second tube 120 can be coaxially fitted to meet the requirements, and avoid the first tube 110 and the second tube 120 being misaligned, which would affect the final yield.
[0066] Please refer to Figure 6, which is a schematic diagram of an optional embodiment of step S400 shown in Figure 1. As shown in Figures 4 and 6, in step S200, the alloy layer 130 is formed on the outer surface (i.e., the second surface 121) of the second tube 120. After the first tube 110 is fitted onto the outside of the second tube 120 in step S300, the outer diameter of the second tube 120 may still be smaller than the inner diameter of the first tube 110. This results in a gap 140 between the first tube 110 and the second tube 120 in the multilayer tube 102. Therefore, the multilayer tube 102 needs to be compressed and composited to obtain a multilayer tube 102 with each layer tightly bonded together. The preferred method of the compression composite treatment is to plastically expand the diameter of the second pipe 120, and the preferred method of plastic expansion is hydraulic expansion. The specific steps include: sealing the cavity formed by the inner surface of the second pipe 120, and injecting a pressurizing medium into the cavity, so that the second pipe 120 undergoes plastic expansion deformation and adheres tightly to the first pipe 110. Please refer to Figure 7, which is a schematic diagram of a preferred embodiment of the compression composite treatment in step S400 shown in Figure 1. As shown in Figure 7, end caps 202 are provided at both ends of the multilayer pipe 102 to seal the inner cavity of the second pipe 120. A pressurizing medium delivery pipe 203 is provided through one end cap 202. By injecting a pressurizing medium into the inner cavity, the pressurizing medium can be water or hydraulic oil. The pressurized medium increases the pressure within the inner cavity, causing the second pipe 120 to undergo plastic deformation and its diameter to increase. This results in the alloy layer 130 formed on the outer surface of the second pipe 120 adhering tightly to the inner surface of the first pipe 110. Due to the tension of the second pipe 120, the first pipe 110 also undergoes elastic deformation. When the pressure is released from the inner cavity, the first pipe 110 shrinks and rebounds, tightly wrapping around the second pipe 120, which has already undergone plastic expansion deformation. More preferably, the pressurized medium delivery pipe 203 is connected to an external pressure control system, which can control the upper limit of the pressure within the inner cavity, ensuring that the first pipe 110 only undergoes elastic deformation without plastic deformation. In other embodiments, the plastic expansion can also be achieved using a skew rolling mill.
[0067] Further, in step S500, the multilayer tube 102 is heat-treated to bring the temperature of the alloy layer 130 to the remelting temperature. Ideally, during this heat treatment, the alloy layer 130 as a whole should reach the remelting temperature in a controllable and uniform manner, while the strength and surface properties of the first tube 110 and the second tube 120 should not be damaged. In other words, it is desirable that when the alloy layer 130 is heated to the remelting temperature, the temperatures of the first tube 110 and the second tube 120 have not yet reached their corresponding melting points. Therefore, it is preferable that the melting point of the alloy layer 130 is lower than the melting points of the first tube 110 and the second tube 120. If the melting point of the alloy layer 130 is greater than that of the first pipe 110 and the second pipe 120, the first pipe 110 and the second pipe 120 will melt before the alloy layer 130 forms a metallurgical bond with the first pipe 110 and the second pipe 120. During the subsequent recooling process, the first pipe 110 and the second pipe 120 may become embrittled, resulting in cracks. Porosity, coarse grains, stress accumulation and other adverse effects may also occur inside, causing the first pipe 110 and the second pipe 120 to lose toughness and strength.
[0068] In most cases, due to manufacturing cost considerations, the first pipe 110 and the second pipe 120 are typically manufactured using different materials. For example, in this embodiment, the second pipe 120 is chosen to correspond to the corrosion-resistant layer, and the first pipe 110 is chosen to correspond to the base pipe layer. The second pipe 120 can be formed using a higher-cost material to resist chemical corrosion and impact corrosion of the medium transported inside, while the first pipe can be formed using a lower-cost material, mainly to provide the mechanical properties of the metal composite pipe to resist tensile forces, pressures, and impact forces applied inside and outside the metal composite pipe. Of course, regardless of the materials chosen for the first pipe 110 and the second pipe 120, the melting point of the alloy layer 130 is preferentially lower than that of the first pipe 110 and the second pipe 120. The melting point of the alloy layer 130 can be adjusted by reasonably proportioning the various materials in the alloy powder, for example, by adding boron or silicon to the metal alloy to prepare the alloy powder. In this embodiment, preferably, the material of the first pipe 110 includes any or all of carbon steel and iron-based alloys; the material of the second pipe 120 includes any, any combination or all of alloy steel, 316L stainless steel, nickel-based alloys, cobalt-based alloys and titanium alloys; and the material of the alloy layer 130 includes any, any combination or all of nickel-based alloys, cobalt-based alloys or iron-based alloys doped with boron and / or silicon. The implementer of this embodiment can select the material of the second pipe 120 according to the type of corrosive medium. For example, austenitic stainless steel (e.g., 316L stainless steel) can be selected to deal with salt spray corrosion, duplex stainless steel can be selected to deal with scouring corrosion and chloride ion corrosion, Hastelloy nickel-based alloys can be selected to deal with high-temperature flue gas corrosion, acidic gas corrosion, and boiling strong acid corrosion, TA2 titanium alloy can be selected to deal with brine corrosion and chloride ion stress corrosion, and Stellite cobalt-based alloy can be selected to deal with the coexistence of chemical corrosion and wear corrosion. Therefore, the selection of the material of the second pipe 120 is highly related to the working scenario of the internal anti-corrosion metal composite pipe 101, and can be flexibly selected according to the actual situation. This invention does not limit this.
[0069] From the perspective of material conservation, through repeated experiments, it was verified that when the thickness of the alloy layer 130 is between 0.01 mm and 0.5 mm, it is sufficient to ensure that the alloy layer 130 can stably and controllably form a metallurgical bond with the first tube 110 and the second tube 120 respectively, ultimately enabling the first tube 110 to form a metallurgical bond with sufficient strength through the alloy layer 130 and the second tube 120. Furthermore, further experiments verified that when the thickness of the first tube 110 and the second tube 120 is set to be at least twice the thickness of the alloy layer 130, because the first tube 110 and the second tube 120 have sufficient thickness, even if there are slight deviations in temperature control or heating time during the remelting process of the alloy layer 130, it is not easy for the components of the alloy layer 130 to excessively diffuse into the first tube 110 and the second tube 120. Excessive diffusion may cause overall or local elemental imbalances or metallographic deterioration in the first tube 110 and the second tube 120. For example, the diffusion of boron or silicon may lead to grain boundary brittleness or elemental segregation, thereby reducing the overall performance of the first tube 110 and the second tube 120. Preferably, the thickness of the first tube 110 is in the range of 3 mm to 20 mm, and the thickness of the second tube 120 is in the range of 1 mm to 3 mm.
[0070] As explained earlier, when performing the heat treatment in step S500 on the multilayer tube 102, the ideal state is that the alloy layer 130 as a whole can controllably and uniformly reach the remelting temperature. Typically, the steps for heat treatment of the multilayer tube 102 include: placing the multilayer tube 102 in a heating furnace for overall heating; or sequentially transferring multiple sections of the multilayer tube 102 to the heating furnace for segmented heating along a predetermined feeding direction. Overall heating is suitable for cases where the axial length of the multilayer tube 102 is short. For cases where the axial length of the multilayer tube 102 is long, segmented heating is obviously more suitable. Segmented heating can be achieved by arranging multiple heating furnaces along the feeding path of the multilayer tube 102, or by feeding the multilayer tube 102 segment by segment into a heating furnace for heating discretely over time. Experiments have shown that both overall heating and segmented heating, which cause the temperature of the heated section in the multilayer tube 102 located in the heating furnace to increase in a gradient manner, help to improve the remelting effect of the alloy layer 130.
[0071] Preferably, the gradient heating includes the following stages: a first stage, continuously heating the heated section until the temperature of the heated section reaches a first temperature; a second stage, continuing to heat the heated section until the temperature of the heated section reaches a second temperature; and a third stage, continuing to heat the heated section until the temperature of the heated section reaches the remelting temperature.
[0072] According to the specific material selection of the first pipe 110, the second pipe 120 and the alloy layer 130 listed in this embodiment, the melting point of the first pipe 110 is the same as or similar to the melting point of elemental iron, that is, not higher than 1538°C. The melting point of the second pipe 120 usually falls in the range of 1290°C to 1450°C. The melting point of the alloy layer 130 is preferably adjusted to fall in the range of 850°C to 1100°C. Correspondingly, the first temperature is not higher than 750°C, and the second temperature is greater than the first temperature and less than the remelting temperature.
[0073] Preferably, in order to improve the temperature consistency of the heated section, a constant temperature holding treatment can be performed on the heated section after the temperature reaches a preset temperature. Preferably, in the first stage, after the temperature of the heated section reaches the first temperature, the heated section is held for a first time; in the second stage, after the temperature of the heated section reaches the second temperature, the heated section is held for a second time; in the third stage, after the temperature of the heated section reaches the remelting temperature, the heated section is held for a third time. Preferably, the first time, the second time, and the third time do not exceed 600 seconds. It should be noted that the constant temperature heat preservation treatment can be achieved by periodically placing the heated section in the heating furnace to keep the heated section continuously in the heating furnace and maintain a constant temperature. However, this is not the only method of constant temperature heat preservation treatment. On the contrary, the multilayer tube 102 can be driven by the feeding wheel, feeding roller and other equipment on the production line to move along the predetermined feeding direction. By reasonably setting the movement speed of the multilayer tube 102, the heated section can be heated to the first temperature, the second temperature or the remelting temperature in the heating furnace, and the circulation time of the heated section in the heating furnace can be regarded as the heat preservation time of the heated section.
[0074] Based on the consideration of precise control of heating temperature, the heating furnace can be implemented using a medium-frequency induction heating furnace. The medium-frequency induction heating furnace includes one or more heating coils, and each heating coil is equipped with a thermometer for real-time monitoring and feedback of temperature information. The operating current frequency of the heating coil is preferably set in the range of 500Hz to 12000Hz.
[0075] To prevent delamination between the alloy layer 130 and the first tube 110 during the heating process of the multilayer tube 102, preferably, when heating the multilayer tube 102 as a whole or in segments, a clamping force can be applied to the outside of the multilayer tube 102. For example, a set of suitable clamping rollers can be used to force the first tube 110 to undergo non-plastic diameter reduction deformation. This will make the first tube 110 and the alloy layer 130 fit more tightly, and the alloy layer 130 will be more likely to form a metallurgical bond with the first tube 110.
[0076] Please refer to Figure 8, which is a schematic diagram of an optional embodiment of steps S500 and S600 shown in Figure 1. As shown in Figure 8, the multilayer tube 102 is fed into the heating furnace 205 for the overall heating or the segmented heating. At this time, the induction coil group of the heating furnace 205 is fixed, and the multilayer tube 102 rotates around its central axis. This helps the multilayer tube 102 to be heated evenly in the heating furnace 205. In other embodiments, the induction coil group of the heating furnace 205 can be set to rotate around the multilayer tube 102, and the multilayer tube 102 can also be rotated around its central axis at the same time, which also helps the multilayer tube 102 to be heated evenly.
[0077] Because the first tube 110 and the second tube 120 are usually made of different metal materials, they often have different coefficients of thermal expansion. During the overall heating or the segmented heating process, delamination frequently occurs between the first tube 110 and the second tube 120, especially for certain special dimensions of the tube diameter and wall thickness. This delamination phenomenon makes it difficult for the interfacial bonding strength of the first tube 110 and the second tube 120 to reach the expected value. Through implementation, it has been found that when performing the overall heating or the segmented heating of the multilayer tube 102, if the inner cavity of the multilayer tube 102 is sealed and a protective gas (preferably an inert gas) is injected into the inner cavity to ensure that the gas pressure in the inner cavity is not lower than a predetermined threshold, the frequency of delamination can be greatly reduced. During the heating process of the multilayer tube 102, the protective gas inside the cavity expands simultaneously, forcing the second tube 120 to undergo an expansion-diameter elastic deformation. This causes the second tube 120 to push the alloy layer 130 closer to the inner surface of the first tube 110. Especially after the alloy layer 130 reaches its remelting temperature, the liquid alloy layer 130, under the expansion and compression of the protective gas, can fully contact the first tube 110 and the second tube 120, forming a higher-quality metallurgical bond with both. Furthermore, when an inert gas is preferably used as the protective gas, the formation of oxide scale on the inner surface of the second tube 120 can be reduced. If the gas pressure in the cavity is too low, sufficient pressure cannot be achieved to force the second tube 120 to undergo an expansion-diameter elastic deformation. If the gas pressure in the cavity is too high, there is a certain degree of danger. Tests have shown that the optimal solution is when the predetermined threshold falls within the range of 0.1 MPa to 10 MPa.
[0078] In step S600, the heated multilayer tube 102 is cooled to obtain the internally corrosion-resistant metal composite tube 101 as shown in FIG2. Preferably, as shown in FIG8, the step of cooling the multilayer tube 102 includes: setting a rapid cooling device 206 at the outlet of the multilayer tube 102 to cool the multilayer tube 102. The rapid cooling device 206 is typically a spray device with water as the cooling medium or an air-cooling device with gas as the cooling medium. In other embodiments, the multilayer tube 102 can also be cooled by natural placement cooling.
[0079] Preferably, in order to refine the grains and eliminate internal stress, thereby improving the performance of the internal anti-corrosion metal composite pipe 101, after the cooling treatment in step S600, the following preferred step can also be performed: tempering treatment of the internal anti-corrosion metal composite pipe 101.
[0080] The internally corrosion-resistant metal composite pipe 101 prepared by implementing the various embodiments of steps S100 to S600 has sufficient bonding strength between its first pipe 110 and second pipe 120. This bonding strength can approach the shear strength of the first pipe 110 and the second pipe 120, typically above 300 MPa, and can reach up to about 450 MPa.
[0081] The specific implementation methods formed by combining the various embodiments shown in Figures 2 to 8 above are descriptions of steps S100 to S600 under the premise that the second pipe 120 is aligned with the corrosion-resistant layer and the manufacturing objective is to obtain the internally corrosion-resistant metal composite pipe 101 as shown in Figure 2. If the manufacturing objective is to obtain the externally corrosion-resistant metal composite pipe as described above, some technical details in steps S100 to S600 differ from the specific implementation methods formed by combining the various embodiments shown in Figures 2 to 8, and need to be adjusted according to the structural characteristic that the corrosion-resistant layer in the externally corrosion-resistant metal composite pipe is formed outside the base pipe layer.
[0082] Please refer to Figure 9, which is a cross-sectional structural schematic diagram of an optional embodiment of the externally corrosion-resistant metal composite pipe prepared according to the manufacturing method shown in Figure 1. As shown in Figure 9, the externally corrosion-resistant metal composite pipe 103 includes a first pipe 110, a second pipe 120, and an alloy layer 130. The alloy layer 130 forms a metallurgical bond with the first pipe 110 and the second pipe 120 respectively. The first pipe 110 forms an interface bond with the second pipe 120 through the alloy layer 130. The second pipe 120 is sleeved on the outside of the first pipe 110. The first pipe 110 and the second pipe 120 can be seamless pipes or welded pipes made by welding sheet metal coils.
[0083] Based on the embodiment shown in FIG9, the second pipe 120 is selected to correspond to the corrosion-resistant layer of the external anti-corrosion metal composite pipe 103, and the first pipe 110 is selected to correspond to the base pipe layer of the external anti-corrosion metal composite pipe 103. Steps S100 to S600 will be described on this premise.
[0084] When forming the alloy layer 130 in step S200, referring to the explanation of the two optional embodiments of S200 above, it is only necessary to form the alloy layer 130 between the first pipe 110 and the second pipe 120. Accordingly, when selecting to use electrostatic spraying or thermosetting spraying to form the alloy layer 130, if the diameter of the second pipe 120 is small, the alloy layer 130 can be formed on the outer surface of the first pipe 110 (corresponding to the first surface of the first pipe 110); if the diameter of the second pipe 120 is large, the alloy layer 130 can be formed on the inner surface of the second pipe 120 (corresponding to the second surface of the second pipe 120).
[0085] Accordingly, before forming the alloy layer 130, roughening treatment is preferably performed on the outer surface of the first pipe 110 or the inner surface of the second pipe 120, depending on the formation location of the alloy layer 130.
[0086] After step S200 is executed, in step S300, the first pipe 110 and the second pipe 120 are coaxially sleeved. More specifically, the second pipe 120 is sleeved outside the first pipe 110 to form a multilayer pipe 104 as shown in FIG10. Please refer to FIG10, which is a schematic diagram of an alternative embodiment of step S300 shown in FIG1. In the multilayer pipe 104 shown in FIG10, since the second pipe 120 corresponds to the corrosion-resistant layer of the outer anti-corrosion metal composite pipe 103 and the first pipe 110 corresponds to the base pipe layer of the outer anti-corrosion metal composite pipe 103, the second pipe 120 usually has a thinner thickness and better ductility than the first pipe 110. Therefore, when performing the compression composite treatment on the multilayer pipe 104 in step S400, the embodiment shown in FIG6 and FIG7 is usually not considered. That is, the compression composite treatment in step S300 is not considered by plastically expanding the diameter of the first pipe 110. Instead, consideration should be given to how to make the second tube 120 plastically shrink in diameter and then tightly adhere to the outer surface of the first tube 110. Therefore, preferably, the pressing and bonding process in step S300 includes: setting a mandrel in the cavity formed by the inner surface of the first tube 110, and applying radial pressure to the outer surface of the second tube 120, so that the second tube 120 plastically shrinks in diameter and then tightly adheres to the first tube 110.
[0087] Please refer to Figure 11, which is a schematic diagram of another preferred embodiment of step S400 shown in Figure 1. As shown in Figures 10 and 11, in step S200, the alloy layer 130 is formed on the outer surface of the first pipe 110, and after the second pipe 120 is fitted onto the outside of the first pipe 110 in step S300, the second pipe 120 and the first pipe 110 are not tightly fitted. Therefore, the multilayer pipe 104 needs to be compressed and composited to obtain a multilayer pipe 104 with each layer tightly fitted. As described above, the preferred method of the compression and composite treatment in step S400 is to plastically reduce the diameter of the second pipe 120. During the plastic reduction process, the radial pressure applied to the outer surface of the second pipe fitting 120 forces it to undergo plastic reduction deformation. Simultaneously, to prevent the first pipe 110 from easily deforming and thus maintain the required diameter of the external anti-corrosion metal composite pipe 103, a mandrel 204 is installed within the cavity formed by the inner surface of the first pipe 110. The mandrel 204 is typically made of hard alloy. Due to the presence of the mandrel 204, even if a sufficiently large radial pressure has been applied to the outer surface of the second pipe fitting 120, the first pipe 110 is less likely to undergo irreversible plastic reduction deformation. The radial pressure can be achieved using the extrusion pressure between the reduction die and the second pipe 120 during the cold drawing process, or by applying extrusion pressure to the second pipe 120 using a spinning machine, or by using a preset air pressure difference, hydraulic pressure difference, or other static pressure applied to the outer surface of the second pipe 120. Those skilled in the art can select the appropriate method for achieving the radial pressure based on the diameter and material of the second pipe 120.
[0088] After step S400 is executed, the multilayer tube 104 also needs to undergo further heating treatment in step S500 to bring the temperature of the alloy layer 130 to the remelting temperature. Preferably, through repeated experiments, it has been verified that when the thickness of the alloy layer 130 is between 0.01 mm and 0.5 mm, it is sufficient to ensure that the alloy layer 130 can stably and controllably form a metallurgical bond with the first tube 110 and the second tube 120 respectively, ultimately allowing the first tube 110 to form a metallurgical bond with sufficient strength through the alloy layer 130 and the second tube 120. Furthermore, further experiments have verified that when the thickness of the first tube 110 and the second tube 120 is set to be at least twice the thickness of the alloy layer 130, since the first tube 110 and the second tube 120 have sufficient thickness, even if there are slight deviations in temperature control or heating time during the remelting of the alloy layer 130, it is not easy for the components of the alloy layer 130 to excessively diffuse into the first tube 110 and the second tube 120. In this embodiment, preferably, the material of the first pipe 110 includes any or all of carbon steel and iron-based alloys; the material of the second pipe 120 includes any, any combination of, or all of alloy steel, 316L stainless steel, nickel-based alloys, cobalt-based alloys, and titanium alloys; the material of the alloy layer 130 includes any, any combination of, or all of nickel-based alloys, cobalt-based alloys, or iron-based alloys doped with boron and / or silicon. The selection of the material of the second pipe 120 is highly related to the working environment of the external anti-corrosion metal composite pipe 103 and can be flexibly selected according to actual conditions; this invention does not limit this selection. Preferably, the thickness of the first pipe 110 ranges from 3 mm to 20 mm, and the thickness of the second pipe 120 ranges from 1 mm to 3 mm.
[0089] Preferably, the heat treatment step S500 includes: placing the multilayer tube 104 in a heating furnace and heating the multilayer tube 104 as a whole; or sequentially transferring multiple sections of the multilayer tube 104 to the heating furnace for segmented heating along a predetermined feeding direction. Whether it is overall heating or segmented heating, causing the temperature of the heated section of the multilayer tube 104 located in the heating furnace to increase in a gradient manner helps to improve the remelting effect of the alloy layer 130.
[0090] Preferably, the gradient heating includes the following stages: a first stage, continuously heating the heated section until its temperature reaches a first temperature; a second stage, continuing to heat the heated section until its temperature reaches a second temperature; and a third stage, continuing to heat the heated section until its temperature reaches the remelting temperature. According to the specific material selection of the first pipe 110, the second pipe 120, and the alloy layer 130 listed in this embodiment, the melting point of the first pipe 110 is the same as or close to the melting point of elemental iron, i.e., not higher than 1538°C. The melting point of the second pipe 120 typically falls within the range of 1290°C to 1450°C. The melting point of the alloy layer 130 is preferably adjusted to fall within the range of 850°C to 1100°C. Correspondingly, the first temperature is not higher than 750°C, and the second temperature is greater than the first temperature but less than the remelting temperature.
[0091] Preferably, in order to improve the temperature consistency of the heated section, a constant temperature holding treatment can be performed on the heated section after the temperature reaches a preset temperature. Preferably, in the first stage, after the temperature of the heated section reaches the first temperature, the heated section is held for a first time; in the second stage, after the temperature of the heated section reaches the second temperature, the heated section is held for a second time; in the third stage, after the temperature of the heated section reaches the remelting temperature, the heated section is held for a third time. Preferably, the first time, the second time, and the third time do not exceed 600 seconds. It should be noted that the constant temperature heat preservation treatment can be achieved by periodically placing the heated section in the heating furnace to keep the heated section continuously in the heating furnace and maintain a constant temperature. However, this is not the only method of constant temperature heat preservation treatment. On the contrary, the multilayer tube 104 can be driven by the feeding wheel, feeding roller and other equipment on the production line to move along the predetermined feeding direction. By reasonably setting the movement speed of the multilayer tube 104, the heated section can be heated to the first temperature, the second temperature or the remelting temperature in the heating furnace, and the circulation time of the heated section in the heating furnace can be regarded as the heat preservation time of the heated section.
[0092] Similar to the principle mentioned above, based on the consideration of precise control of the heating temperature, the heating furnace can be implemented using a medium-frequency induction heating furnace. The medium-frequency induction heating furnace includes one or more heating coils, each equipped with a temperature sensor for real-time monitoring and feedback of temperature information. The operating current frequency of the heating coils is preferably set within the range of 500Hz to 12000Hz.
[0093] To prevent delamination between the alloy layer 130 and the second tube 120 during the heating process of the multilayer tube 104, preferably, when heating the multilayer tube 104 as a whole or in segments, a clamping force can be applied to the outside of the multilayer tube 104. For example, a set of suitable clamping rollers can be used to press the outer surface of the second tube 120. This will make the second tube 120 and the alloy layer 130 fit more tightly, and the alloy layer 130 will be more likely to form a metallurgical bond with the second tube 120.
[0094] More preferably, when the multilayer tube 104 is subjected to the overall heating or the segmented heating, rotating the multilayer tube 104 about its central axis, and / or arranging the induction coil of the heating furnace to rotate around the multilayer tube 104, helps to ensure uniform heating of the multilayer tube 104.
[0095] Preferably, when the multilayer tube 104 is subjected to overall heating or segmented heating, the inner cavity of the multilayer tube 104 is sealed, and a protective gas is injected into the inner cavity to ensure that the gas pressure in the inner cavity is not lower than a predetermined threshold. This helps to suppress the separation and delamination of the second tube 120 and the first tube 110, and also helps to reduce the formation of oxide scale on the inner surface of the first tube 110. Tests have shown that the optimal solution is when the predetermined threshold falls within the range of 0.1 MPa to 10 MPa.
[0096] In step S600, the heated multilayer tube 104 is cooled to obtain the externally corrosion-resistant metal composite tube 103 as shown in Figure 9. Preferably, the cooling process includes: installing a rapid cooling device at the outlet of the multilayer tube 104 to cool it. This rapid cooling device is typically a spray device using water as the cooling medium or an air-cooling device using gas as the cooling medium. In other embodiments, natural cooling can also be used to cool the multilayer tube 104.
[0097] Preferably, in order to refine the grains and eliminate internal stress, thereby improving the performance of the external anti-corrosion metal composite pipe 103, after the cooling treatment in step S600, the following preferred step can also be performed: tempering treatment of the external anti-corrosion metal composite pipe 103.
[0098] It should be particularly noted that the embodiments shown in Figures 2 to 9, and the embodiments shown in Figures 8 to 11, are all based on the premise that the second pipe provided in step S100 corresponds to the corrosion-resistant layer of the metal composite pipe, to illustrate how the metal composite pipe is obtained after performing each step of the specific implementation shown in Figure 1. Accordingly, the material of the second pipe is selected from metal alloys with corrosion-resistant functions, including any, any combination or all of alloy steel, 316L stainless steel, nickel-based alloys, cobalt-based alloys and titanium alloys. At the same time, the material of the first pipe provided in step S100 is selected from metal alloys with lower cost, including any or all of carbon steel and iron-based alloys. However, those skilled in the art will understand that if the materials of the first pipe and the second pipe are interchanged, it is equivalent to assigning the first pipe to the corrosion-resistant layer of the metal composite pipe. This means that the first pipe and the second pipe are simply mirror images swapped in the entire manufacturing process of the metal composite pipe. Referring to the various embodiments shown in Figures 2 to 9 and the various embodiments shown in Figures 8 to 11, using the description and explanation of the second pipe to describe and explain the first pipe, and using the description and explanation of the first pipe in the above embodiments to describe and explain the second pipe, a complete technical solution can also be obtained.
[0099] It is particularly important to emphasize that although the various operations of the method for manufacturing the metal composite tube of the present invention are described in a specific order in Figure 1, this does not require or imply that these operations must be performed in that specific order, or that all of the operations shown must be performed to achieve the desired result. Rather, the steps depicted in the flowchart can be performed in a different order. Additionally or alternatively, certain steps may be omitted, multiple steps may be combined into one step, and / or one step may be broken down into multiple steps.
[0100] In addition, the present invention also provides a pipe for waste incineration equipment or oil and gas transmission equipment, wherein the pipe is partially or entirely constructed using a metal composite pipe prepared by the manufacturing method described above. For example, the inner anti-corrosion metal composite pipe 101 is used to construct the flue gas exhaust pipe of the waste incineration equipment, and the outer anti-corrosion metal composite pipe 103 is used to construct the underwater cooling pipe of the oil and gas transmission equipment.
[0101] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered illustrative and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. All variations within the meaning and scope of equivalents of the claims are embraced within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims. Furthermore, it is clear that the word "comprising" does not exclude other components, elements, or steps, and the singular does not exclude the plural.
[0102] The manufacturing method of the metal composite pipe provided by this invention involves setting an alloy layer between a first pipe and a second pipe and remelting it. This alloy layer forms a metallurgical bond with both the first and second pipes, thereby creating an interfacial bond between the first pipe and the second pipe through the alloy layer. The resulting metal composite pipe can meet the performance consistency requirements of various pipe diameters, lengths, and angles. Due to the high strength of the metallurgical bond, the first and second pipes have sufficient interfacial bonding strength, making it difficult for the layers of the metal composite pipe to separate even after subsequent plastic deformation machining processes, such as bending or diameter reduction. Compared to existing metallurgical composite processes for manufacturing metal composite pipes, the manufacturing method of this invention has advantages such as simple process, low cost, strong compatibility, high safety, and high yield.
[0103] The above-disclosed embodiments are merely some preferred embodiments of the present invention and should not be construed as limiting the scope of the present invention. Equivalent variations made in accordance with the claims of the present invention are still within the scope of the present invention.
Claims
1. A method for manufacturing a metal composite pipe, the method comprising: A first pipe and a second pipe are provided, both of which are made of metal. The first pipe has a first surface and the second pipe has a second surface. Alloy powder is attached to the first surface or the second surface to form an alloy layer covering the first surface or the second surface; The first tube and the second tube are coaxially sleeved together, with the first surface facing the second surface, and the alloy layer is placed between the first surface and the second surface to form a multilayer tube; The multilayer tube is subjected to a compression composite process to form an interference fit between the first tube and the second tube; The multilayer tube is heated to bring the temperature of the alloy layer to its remelting temperature. The multilayer tube is cooled to obtain a metal composite tube, wherein the alloy layer in the metal composite tube forms a metallurgical bond with the first surface and the second surface respectively, and the first tube material forms an interface bond with the second tube material through the alloy layer.
2. The manufacturing method according to claim 1, wherein the step of heat-treating the multilayer tube includes: The multilayer tube is placed in a heating furnace and heated as a whole; or Along a predetermined feeding direction, multiple sections of the multilayer tube are sequentially transferred to a heating furnace for segmented heating.
3. The manufacturing method according to claim 2, wherein, The steps of overall heating or segmented heating include: The power of the heating furnace is controlled so that the temperature of the heated section in the multilayer tube located in the heating furnace increases in a gradient manner.
4. The manufacturing method according to claim 3, wherein, The gradient increase includes the following stages: In the first stage, the heated section is continuously heated until the temperature of the heated section reaches a first temperature; In the second stage, the heated section is heated further until the temperature of the heated section reaches the second temperature. In the third stage, the heated section is heated until its temperature reaches the remelting temperature.
5. The manufacturing method according to claim 4, wherein: The first temperature is not higher than 750℃; The second temperature is greater than the first temperature and less than the remelting temperature.
6. The manufacturing method according to claim 2, wherein: When the multilayer tube is heated as a whole or in segments, the multilayer tube rotates around its central axis, and / or the induction coil group of the heating furnace rotates around the multilayer tube.
7. The manufacturing method according to claim 2, wherein: When the multilayer tube is subjected to overall heating or segmented heating, a clamping force is applied to the outside of the multilayer tube.
8. The manufacturing method according to claim 2, wherein: When the multilayer tube is heated as a whole or in segments, the inner cavity of the multilayer tube is sealed and a protective gas is injected into the inner cavity to ensure that the gas pressure in the inner cavity is not lower than a predetermined threshold.
9. The manufacturing method according to claim 8, wherein: The predetermined threshold ranges from 0.1 MPa to 10 MPa.
10. The manufacturing method according to claim 1, wherein, The steps for cooling the multilayer tube include: A spray device or air-cooling device is installed at the outlet of the multi-layer tube to cool the multi-layer tube.
11. The manufacturing method according to claim 10, wherein after the cooling treatment, the manufacturing method further comprises: The metal composite tube is subjected to tempering treatment.
12. The manufacturing method according to claim 1, wherein before attaching the alloy powder, the manufacturing method further comprises: The surface of the first or second surface carrying the alloy powder is roughened.
13. The manufacturing method according to any one of claims 1 to 12, wherein: The melting point of the alloy layer is lower than that of the first pipe and the second pipe; The thickness of the alloy layer ranges from 0.01 mm to 0.5 mm, and the thickness of the first pipe and the second pipe is at least twice the thickness of the alloy layer.
14. The manufacturing method according to claim 13, wherein: The first pipe is sleeved on the outside of the second pipe, the first surface is the inner surface of the first pipe, and the second surface is the outer surface of the second pipe; The alloy powder is sprayed onto the first surface or the second surface.
15. The manufacturing method according to claim 14, wherein, The steps for compressing and bonding the multilayer tube include: The cavity formed by the inner surface of the second pipe is sealed, and a pressurized medium is injected into the cavity, causing the second pipe to undergo plastic expansion deformation and then adhere tightly to the first pipe. The material of the first pipe includes any or all of carbon steel and iron-based alloys; The material of the second pipe includes any one, any combination of, or all of the following: alloy steel, 316L stainless steel, nickel-based alloys, cobalt-based alloys, and titanium alloys. The alloy layer is made of any, any combination of, or all of the following: nickel-based alloys, cobalt-based alloys, or iron-based alloys doped with boron and / or silicon.
16. The manufacturing method according to claim 13, wherein: The second pipe is sleeved on the outside of the first pipe, the first surface is the outer surface of the first pipe, and the second surface is the inner surface of the second pipe; The alloy powder is sprayed onto the first surface or the second surface.
17. The manufacturing method according to claim 16, wherein, The steps for compressing and bonding the multilayer tube include: A mandrel is provided in the cavity formed by the inner surface of the first tube, and radial pressure is applied to the outer surface of the second tube, so that the second tube undergoes plastic diameter reduction deformation and then adheres tightly to the first tube. The material of the first pipe includes any or all of carbon steel and iron-based alloys; The material of the second pipe includes any one, any combination of, or all of the following: alloy steel, 316L stainless steel, nickel-based alloys, cobalt-based alloys, and titanium alloys. The alloy layer is made of any, any combination of, or all of the following: nickel-based alloys, cobalt-based alloys, or iron-based alloys doped with boron and / or silicon.
18. A pipe for a waste incineration facility or an oil and gas transmission facility, wherein the pipe is partially or wholly constructed using a metal composite pipe prepared by the manufacturing method as described in claims 1 to 17.