Semiconductor power device with multi-layer gate stack
A multilayer gate stack with ALD and CVD layers, combined with PDA processes, addresses SiC MOSFET reliability and cost issues by reducing interface defects and contamination, enhancing performance and manufacturability.
Patent Information
- Application Number
- PCT/EP2025/062686
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-12
AI Technical Summary
Existing SiC MOSFETs face challenges in achieving high performance, reliability, and cost-effectiveness due to issues with gate oxide interface defects, high channel resistance, and contamination during thermal processes, particularly with ALD deposition methods.
A multilayer gate stack comprising a thin ALD layer for the interface, a thicker CVD or LPCVD layer for core dielectric, and an optional ALD capping layer, combined with high-temperature PDA processes to enhance film stability and reduce contamination.
This approach reduces channel resistance, enhances ruggedness, and improves reliability and manufacturability while lowering production costs by optimizing the gate oxide process.
Smart Images

Figure EP2025062686_12112026_PF_FP_ABST
Abstract
Description
[0001] SEMICONDUCTOR POWER DEVICE WITH MULTI-LAYER GATE STACK
[0002] TECHNICAL FIELD
[0003] The disclosure relates to the field of semiconductor and power devices, in particular Silicon Carbide (SiC) devices and SiC MOSFETs (Metal Oxide Semiconductor Field Effect Transistors) and gate dielectric layer design for such devices. The disclosure further relates to methods for manufacturing such devices. In particular, the disclosure relates to multilayer gate oxide SiC MOSFETs.
[0004] BACKGROUND
[0005] Silicon Carbide devices have emerged as the most viable candidate for next-generation, low-loss semiconductors due to their low ON resistance and superior high-temperature, high-frequency, and high-voltage performance, when compared to silicon. In particular, the optimization of the gate process module plays a crucial role in SiC MOSFETs to enable high performance and reliability. Gate oxide interface and bulk characteristics are determined by the oxide / dielectric deposition and post deposition annealing processes affecting interface trapped density and bulk oxide trapped charge. The detectivity correlated to the gate oxide process module has a significant impact on both electrical characteristics (channel mobility, switching, gate threshold voltage and leakage) and reliability (gate oxide breakdown, threshold voltage instabilities, hysteresis effects).
[0006] SUMMARY
[0007] This disclosure provides a solution for improving the SiC MOSFET gate characteristics with respect to performance, reliability and lifetime. At the same time the solution improves manufacturability issues and considerably reduces costs.
[0008] The foregoing and other objects are achieved by the features of the independent claims. Further implementation forms are apparent from the dependent claims, the description and the figures.
[0009] Embodiments of the disclosure present SiC MOSFETs designs with a multilayer gate stack. The stack is given by at least the first two layers (items A and B) of the following three different layers with the following characteristics (from SiC interface): A) First thin dielectric layer (SiO2 or high K) deposited by ALD to create a low detectivity interface with SiC; B) Second thicker layer (SiO2) deposited at high temperature by CVD or LPCVD to create a core dielectric layer with comparatively higher film quality (with reference to all the deposited layer options including for example PEC VD); and C) Third thin dielectric layer (SiO2 or high K) deposited by ALD to create a capping layer sealing the first two layers against dopant or contamination diffusion occurring during subsequent process steps (e.g. poly gate deposition or contacts annealing).
[0010] Suitable PDA processes in N2 or FG can be carried out at high temperature after each dielectric layer deposition to reduce the interface detectivity and improve film robustness through densification.
[0011] In some embodiments the capping layer (see point C above) is not included in the gate stack or is aligned to the first two dielectric layers to simplify the process flow.
[0012] In some further embodiments the gate stack is split such not to cover part of the JFET region between contiguous P wells, to reduce the capacitance increase derived from the possible use of high K dielectric layers in the gate stack (compatible only to planar MOSFET design).Most of the solutions presented hereinafter can be applied likewise to SiC planar and trench MOSFETs, regardless of the voltage class and current rating. For some embodiments for simplicity, design features and exemplar process flows will be provided only for SiC planar MOSFETs. However, the concept can be easily extended to trench MOSFETs. The solutions reported in this disclosure can also be applied to other semiconductor materials, especially wide band gap, where the high detectivity at the interface in the gate region and high electrical field in the gate dielectric layers can result critical for reliability or long-term stability.
[0013] Reference will be made to some limitations derived from the ALD deposition of dielectric layers like silicon oxides (SiO2), metallic oxides (e.g. HfO2, ZrO2), silicon nitrides and oxynitrides (SiN, SiOxNy) and metallic nitrides (e.g. AIN), as gate layers in SiC MOSFETs. In particular the embodiments presented in this disclosure resolve the following items reported in the literature: 1 ) Slow ALD deposition rate; 2) Need to fine tune PDA processes to make the interface characteristics stable; and 3) ALD layers permeability to contaminants or dopant diffusion during subsequent steps in the process flow (main reference to thermal deposition step like poly gate deposition or contacts annealing).
[0014] In order to describe the disclosure in detail, the following terms and notations will be used.
[0015] SiC Silicon Carbide
[0016] Dit Defect Interface Traps
[0017] RCH Channel Resistance
[0018] RON ON Resistance
[0019] MOSFET Metal Oxide Semiconductor Field Effect Transistor
[0020] ALD Atomic Layer Deposition
[0021] PECVD Plasma Enhanced Chemical Vapor Deposition
[0022] LPCVD Low Pressure Chemical Vapor Deposition
[0023] CVD Chemical Vapor Deposition
[0024] PDA Post Deposition Annealing
[0025] JFET Junction F ield Effect Transistor
[0026] FG Forming Gas
[0027] In this disclosure, SiC devices and SiC power devices are described. Such devices have emerged as the most viable candidate for next-generation, low-loss semiconductors due to their low ON resistance and superior high-temperature, high-frequency, and high-voltage performance, when compared to silicon. SiC power devices are currently used in smart appliances in domestic and commercial buildings, servers, power supply systems, renewable energy such as electric vehicles (SiC core market), wind power and solar photovoltaic, railway transportation, power grid converters and inverters. SiC power devices electrical characteristics, quality and final costs are determined by a number of processes, design and materials challenges. Addressing them is crucial to improve the performance / robustness / cost trade off in many use cases.
[0028] As alreadv pointed out, the optimization of the gate process module plays a crucial role in SiC MOSFETs to enable high performance and reliability. Gate oxide interface and bulk characteristics are determined by the oxide / dielectric deposition and post deposition annealing processes affecting interface trapped density and bulk oxide trapped charge. The detectivity correlated to the gate oxide process module has a significant impact on both electrical characteristics (channel mobility, switching, gate threshold voltage and leakage) and reliability (gate oxide breakdown, threshold voltage instabilities, hysteresis effects).The channel resistance RCH accounts for about 15%-25% the overall MOSFET RON (depending on voltage class and design). Therefore, RCH reduction, heavily affected by interface trapped density, is crucial to improve the conduction current density, with obvious benefits in terms of cost reduction and miniaturization. On the other hand, due to the very high SiC electrical breakdown strength, the electrical field inside the gate oxide layer is much higher than for example in Si MOSFETs, leading, together with the higher gate oxide defect density, to higher failure risks and poor ruggedness.
[0029] SiC planar MOSFET devices mostly use thermal or CVD SiO2 single layers connecting the N+ Source, P Well and N-doped JFET region (either N- drift layer or N doped current spread layer between P wells to reduce JFET resistance.
[0030] The two options used for gate oxide formation in SiC MOSFETs include thermal oxides or deposited oxides, including high K materials like metallic oxides. Thermal oxides deliver high gate oxide breakdown voltage, stable and higher gate threshold voltage, low leakage and excellent electrical characteristics stability with the process. Elowever, they show quite limited channel mobility, due to the high defect interface trapped density arising from the formation of carbon related defects at the SiC interface during the thermal oxidation process. On the other hand, deposited oxides (usually by CVD, LPCVD, PECVD, ALD) show higher channel mobility, due to the fact the SiC surface is not oxidized during the deposition process. Elowever, the quality of the oxide material is lower leading to low gate oxide breakdown voltage, lower and unstable gate threshold voltage, high leakage, hysteresis effects and process variations impact (especially for the post deposition annealing) on gate oxide characteristics (threshold voltage and leakage).
[0031] Deposited oxides (CVD, LPCVD, PECVD, ALD) represent a suitable alternative to thermal oxides in SiC MOSFETs, especially in trench designs where the oxide deposition conformity plays a crucial role for reliability. MOS capacitors have alreadv been produced with the SiO2 layer deposited by a high temperature (800C) LPCVD, followed by a PDA process in N2O. Low interface state density (Dit of 9.0xl0ncm-2 eV-1) was found at about 0.2 eV. In general, high T deposition processes using C-free precursors are considered valid alternatives to thermal SiO2 in commercial products, due to the relatively higher mobility (-50-60 cm2 / Vs) and good interface characteristics with SiC.
[0032] Oxides or other high K dielectric layers deposited at low temperature by ALD will be largely used in SiC MOSFETs in near future, due to the lower channel resistance enabled by the low defect density at SiC surface and better suitability to trench designs, given the high conformity and fine control of the deposition process. Moreover, ALD equipment allows the sequential deposition (without vacuum break) of a high number of different dielectric layers with precise control of their thickness and low probability of contamination offering in this way the possibility to design multilayer gate stacks finely tuned for different application requirements.
[0033] Nonetheless, ALD deposition also shows some limitations, currently hindering the use of ALD oxides in commercial devices. ALD is in fact a very slow deposition process (100-300 nm / h), resulting in a low throughput and high production costs. Moreover, as the ALD process is a low temperature process occurring at 200°C-300°C, it is critical that suitable post-deposition anneal (PDA) processes are used to form a permanent bond between the materials, and thereby improve the mobility of the resulting MOSFET. Finally, being ALD layers not densified due to the low T deposition process, they may potentially be subject to dopant or contamination diffusion during subsequent thermal processes (poly deposition, ohmic contacts annealing), resulting in poor lifetime and reliability.
[0034] Embodiments described in the following solve the above-described limitations by using only a very thin ALD layer (-1 nm-10 nm) as first interface layer in the gate stack. A third ALD capping layer is optional in some embodiments. This results in a considerably reduction of deposition time (compared to a standard 50 nm single ALD layer) by improving equipment throughput and reducing production costs.Embodiments described hereinafter allow using of multiple high temperature PDA processes after each dielectric layer deposition in the gate stack. This feature allows to reduce the interface detectivity and improve film stability via densification process. This helps to reduce channel resistance and enhance ruggedness.
[0035] Embodiments described hereinafter are based on a thin ALD capping layer (high K material) that is deposited on top of the first two dielectric layers in the gate stack to prevent interface and bulk contamination or doping during subsequent (thermal) process. This improves lifetime and reliability.
[0036] According to a first aspect, the disclosure relates to a semiconductor device, comprising: an n-type doped substrate acting as a drain contact; an n-type doped drift layer formed on the substrate; a p-type doped well formed in the n-type doped drift layer; an n-type doped source contact implanted in part of the p-type doped well; and a multi-layer gate stack that is overlapping the n-type doped drift layer, the p-type doped well and at least part of the n-type doped source contact to enable formation of a gate electrons channel in the p-type doped well between the n-type doped source contact and the drain contact; wherein the multilayer gate stack comprises at least a first dielectric layer and a second dielectric layer; wherein the first dielectric layer is an ALD, atomic layer deposition, dielectric layer creating an interface with the n-type doped drift layer, the p-type doped well and the at least part of the n-type doped source contact; wherein the second dielectric layer is deposited on the first dielectric layer; and wherein the multi-layer gate stack is configured to increase a channel mobility of the gate electrons channel.
[0037] The first ALD layer creates low detectivity interface with the layers below, e.g., SiC layers or other low bandgap material layers. The second dielectric layer creates core dielectric layer with high film quality. The gate stack can have two or more dielectric layers. For two dielectric layers, the manufacturing process can be simplified with benefits in terms of lower cycle time and costs. For two dielectric layers, these two dielectric layers can be patterned by a photolithographic process in the same step which reduces process time.
[0038] In an exemplary implementation of the semiconductor device, the first dielectric layer is thinner than the second dielectric layer.
[0039] By having a thinner first dielectric layer than a second dielectric layer, the deposition time can be reduced considering that only a thin ALD layer is deposited as first interfacial layer, instead of having only one single dielectric gate layer all deposited by ALD and whose deposition would require long time.
[0040] In an exemplary implementation of the semiconductor device, a thickness of the first dielectric layer is within a range of about Inm to lOnm and a thickness of the second dielectric layer is within a range of about 20nm to 40nm.
[0041] By such thin ALD dielectric layer, deposition time is in some cases considerably reduced by improving equipment throughput and reducing production costs. In particular, the deposition time is reduced considering that only a thin ALD layer is deposited as first interfacial layer, instead of having only one single dielectric gate layer all deposited by ALD and whose deposition would require long time. In this case there is a thin ALD layer requiring some time for deposition plus a second deposition layer supposed thicker whose deposition with other techniques like LPCVD requires less time, compared to ALD. Less deposition time refers to the case when there is one single thick dielectric layer all deposited by ALD which is a very slow deposition technique.
[0042] In an exemplary implementation of the semiconductor device, the first dielectric layer comprises one of the following layers: a Silicon oxide, SiO2, layer, a Silicon Nitride, Si3N4, layer, an Aluminum Nitride, AIN, layer, an Aluminum Oxide, A12O3, layer, a Zirconium Oxide, ZrO2, layer; and the second dielectric layer comprises a Silicon oxide, SiO2, layer.Such materials are well suited for deposition creating thin and robust dielectric layers.
[0043] In an exemplary implementation of the semiconductor device, the first dielectric layer is formed by ALD (i.e., atomic layer deposition) at low temperature in a range of about 200C to 300C; and the second dielectric layer is formed by CVD (i.e., chemical vapor deposition), or by LPCVD (i.e., liquid phase chemical vapor deposition) at high temperature in a range of about 700C to 950C.
[0044] PDA processes (at high temperature such as 1100C in N2 or FG, 60min) after each dielectric layer deposition reduces the interface detectivity and improves film stability and robustness via densification process. This helps to reduce channel resistance and enhance ruggedness.
[0045] In an exemplary implementation of the semiconductor device, the deposition of each dielectric layer is followed by a Post Deposition Annealing (PDA) process at high temperature in one or a combination of FG (i.e., Forming Gas), N2, NO or N2O.
[0046] PDA may be applied, for example, at high temperatures ranging from about 600 degrees Celsius to about 1100 degrees Celsius.
[0047] Such Post Deposition Annealing process can form a permanent bond between the materials, and thereby improve the mobility of the resulting MOSFET. ALD layers being not densified due to the low T deposition process could potentially be subject to dopant or contamination diffusion during subsequent thermal processes (poly deposition, ohmic contacts annealing), resulting in poor lifetime and reliability. PDA thus improves lifetime and reliability of the semiconductor device.
[0048] In an exemplary implementation of the semiconductor device, the first dielectric layer is aligned with the second dielectric layer.
[0049] When aligning the first dielectric layer with the second dielectric layer, only one photomask process is required which reduces processing complexity.
[0050] In an exemplary implementation of the semiconductor device, the multi-layer gate stack has a constant thickness; and each dielectric layer of the multi-layer gate stack has a respective constant thickness.
[0051] Such constant thickness multi-layer gate stack can be seen as a single layer with the same thickness over the layer. Besides, a constant thickness multi-layer gate stack can be easily manufactured.
[0052] In an exemplary implementation of the semiconductor device, the multi-layer gate stack comprises a third dielectric layer formed by an ALD dielectric layer, the third dielectric layer being deposited on the second dielectric layer.
[0053] A third dielectric layer as ALD dielectric layer can improve lifetime and reliability.
[0054] The third dielectric layer can create a cover or capping layer protecting the first two layers against dopant or contamination diffusion occurring during subsequent process steps, e.g., poly gate deposition or contacts annealing.
[0055] In an exemplary implementation of the semiconductor device, the third dielectric layer is aligned with the first and second dielectric layers or is fully covering the first and second dielectric layers to create a capping layer sealing the first dielectric layer and the second dielectric layer against dopant or contamination diffusion.The third dielectric layer prevents interface and bulk contamination or doping during subsequent (thermal) process.
[0056] When aligning the third dielectric layer with the first and second dielectric layers for creating a cover layer, only one photomask process is required which reduces processing complexity.
[0057] When creating a capping or sealing layer by the third dielectric layer, this layer can protect the first and second layers against dopant or contamination diffusion.
[0058] In the option not fully aligned (i.e., second photomask needed to pattern the third layer), the first two layers are protected also laterally from dopant diffusion from the sides of the first two layers.
[0059] In an exemplary implementation of the semiconductor device, a thickness of the third dielectric layer is within a range of about 5nmto lOnm.
[0060] A very thin third dielectric layer is sufficient to provide the protection functionality of such third dielectric layer.
[0061] In an exemplary implementation of the semiconductor device, the third dielectric layer comprises one of the following layers: a Silicon oxide, SiO2, layer, an Aluminum Oxide, A12O3, layer, a Zirconium Oxide, ZrO2, layer, a Hafnium Oxide, HfO2, layer; and the third dielectric layer is formed by ALD, atomic layer deposition at low temperatures in a range of about 200C to 300C.
[0062] Such materials are well suited for deposition creating thin and robust dielectric layers.
[0063] In an exemplary implementation of the semiconductor device, the deposition of each dielectric layer is followed by at least one Post Deposition Annealing, PDA, process at high temperature in one or a combination of FG (Forming Gas), N2, NO orN2O.
[0064] PDA may be applied, for example, at high temperatures ranging from about 600 degrees Celsius to about 1100 degrees Celsius.
[0065] Such Post Deposition Annealing process can form a permanent bond between the materials, and thereby improve the mobility of the resulting MOSFET. PDA thus improves lifetime and reliability of the semiconductor device.
[0066] PDA may be applied, for example, at high temperatures ranging from about 600 degrees Celsius to about 1100 degrees Celsius.
[0067] The term “at least one PDA process” covers the option where there is one PDA process after the deposition of each layer (so three PDA processes in total) or only one or only two PDA processes following the deposition of the first, second and third layer or first and second and second and third layers, respectively.
[0068] In an exemplary implementation of the semiconductor device, the multi-layer gate stack is partially opened in a JFET region of the n-type doped drift layer to form a multilayer split gate stack according to a split gate technology.
[0069] This so-called split gate technology helps to reduce power dissipation and improve the response at high frequency through the reduction of reverse transfer capacitance. This solution can be useful to compensate the increase of the capacitance, due to the use of high permittivity dielectric layers in the gate stack.In an exemplary implementation of the semiconductor device, the multilayer split gate stack comprises a first section and a second section which are separated from each other in the .11' FT region or connected to each other by the third dielectric layer formed in the JFET region.
[0070] When the third dielectric layer is formed in the JFET region between the first and second sections of the gate stack, this solution helps to achieve a better sealing effect for the gate stack against dopant or contamination diffusion occurring during subsequent thermal steps, as for example the highly doped polysilicon layer deposition used as gate contact t and ohmic contacts annealing with beneficial effects on lifetime and reliability.
[0071] In an exemplary implementation of the semiconductor device, the n-type doped substrate and the n-type doped drift layer comprise a high-bandgap semiconductor material, in particular silicon carbide or Gallium nitride.
[0072] The solution described here can be applied to SiC, GaN and other semiconductor materials, especially wide band gap, where the high detectivity at the interface in the gate region and high electrical field in the gate dielectric layers can result critical for reliability or long-term stability. The solution described in this disclosure improves reliability and long-term stability.
[0073] In an exemplary implementation of the semiconductor device, the semiconductor device is forming a planar MOSFET or a trench MOSFET.
[0074] The technology described here can be applied likewise to planar and trench MOSFETs, regardless of the voltage class and current rating.
[0075] According to a second aspect, the disclosure relates to a method for producing a semiconductor device, the method comprising: providing a p-type doped well formed in an n-type doped drift layer, an n-type doped source contact implanted in part of the p-type doped well and an n-type doped substrate acting as a drain contact; and forming a first dielectric layer and a second dielectric layer of a multilayer gate stack overlapping the n-type doped drift layer, the p-type doped well and at least part of the n-type doped source contact to enable formation of a gate electrons channel in the p-type doped well between the n-type doped source contact and the drain contact; wherein forming the first dielectric layer comprises forming an atomic layer deposition, ALD, dielectric layer, creating an interface with the n-type doped drift layer, the p-type doped well and the at least part of the n-type doped source contact; and wherein forming the second dielectric layer comprises depositing the second dielectric layer on the first dielectric layer for increasing a channel mobility of the gate electrons channel.
[0076] By such method a first ALD layer is formed which creates low defectivity interface with the layers below, e.g., SiC layers or other low bandgap material layers. Forming the second dielectric layer creates core dielectric layer with high film quality. The gate stack can be formed having two or more dielectric layers. For two dielectric layers, the manufacturing process, i.e., the method, can be simplified with benefits in terms of lower cycle time and costs. For two dielectric layers, these two dielectric layers can be patterned by a photolithographic process in the same step which reduces process time.
[0077] In an exemplary implementation of the method, the second dielectric layer is a deposited dielectric layer formed by Plasma Enhanced Chemical Vapor Deposition, PECVD, Low Pressure Chemical Vapor Deposition, LPCVD, or Chemical Vapor Deposition, CVD.
[0078] Deposited oxides (CVD, LPCVD, PECVD, ALD) represent a suitable alternative to thermal oxides in SiC MOSFETs, especially in trench designs (but also in planar designs) where the oxide deposition conformity plays a crucial role for reliability. Such manufacturing provides low interface state density. High T deposition processes using C-free precursors are validalternatives to thermal SiO2 in commercial products, due to the relatively higher mobility (-50-60 cm2 / V s) and good interface characteristics with SiC.
[0079] In an exemplary implementation of the method, forming the first dielectric layer comprises ALD, atomic layer deposition at low temperature in a range of about 200C to 300C; and forming the second dielectric layer comprises chemical vapor deposition, CVD, or liquid phase chemical vapor deposition, LPCVD, at high temperature in a range of about 700C to 950C.
[0080] The deposition of each dielectric layer may be followed by at least one Post Deposition Annealing, PDA, process at high temperature in one or a combination of FG, N2, NO or N2O. PDA may be applied, for example, at high temperatures ranging from about 600 degrees Celsius to about 1100 degrees Celsius.
[0081] In an exemplary implementation of the method, the method comprises: forming a third dielectric layer of the multilayer gate stack by ALD deposition on the second dielectric layer.
[0082] A third dielectric layer as ALD dielectric layer can improve lifetime and reliability.
[0083] The third dielectric layer can create a cover or capping layer protecting the first two layers against dopant or contamination diffusion occurring during subsequent process steps, e.g., poly gate deposition or contacts annealing.
[0084] In an exemplary implementation of the method, forming the third dielectric layer comprises ALD deposition at low temperature in a range of about 200C to 300C followed by post deposition annealing at high temperature.
[0085] The deposition of each dielectric layer may be followed by at least one Post Deposition Annealing, PDA, process at high temperature in one or a combination of FG (Forming Gas), N2, NO or N2O.
[0086] PDA may be applied, for example, at high temperatures ranging from about 600 degrees Celsius to about 1100 degrees Celsius. PDA may be applied, for example, for a duration between about 30 min and 4 hours.
[0087] BRIEF DESCRIPTION OF THE DRAWINGS
[0088] Further embodiments of the disclosure will be described with respect to the following figures, in which:
[0089] Figure 1 shows a cross section of a semiconductor device 100 in a planar MOSFET design (left-side picture) and a cross section of a semiconductor device 100b in a trench MOSFET design (right-side picture) according to a first embodiment;
[0090] Figure 2 shows a schematic process flow constituting a method 200 for producing a semiconductor device according to the disclosure;
[0091] Figure 3 shows a cross section of a semiconductor device 100 according to a second embodiment;
[0092] Figure 4 shows a cross section of a semiconductor device 100 according to a third embodiment;
[0093] Figure 5 shows a cross section of a semiconductor device 100 according to a fourth embodiment; and
[0094] Figure 6 shows a cross section of a semiconductor device 100 according to a fifth embodiment.DETAILED DESCRIPTION OF EMBODIMENTS
[0095] In the following detailed description, reference is made to the accompanying drawings, which form a part thereof, and in which is shown by way of illustration specific aspects in which the disclosure may be practiced. It is understood that other aspects may be utilized and structural or logical changes may be made without departing from the scope of the disclosure. The following detailed description, therefore, is not to be taken in a limiting sense, and the scope of the disclosure is defined by the appended claims.
[0096] It is understood that comments made in connection with a described method may also hold true for a corresponding device or system configured to perform the method and vice versa. For example, if a specific method step is described, a corresponding device may include a unit to perform the described method step, even if such unit is not explicitly described or illustrated in the figures. Further, it is understood that the features of the various exemplary aspects described herein may be combined with each other, unless specifically noted otherwise.
[0097] Figure 1 shows a cross section of a semiconductor device 100 in a planar MOSFET design (left-side picture) and a cross section of a semiconductor device 100b in a trench MOSFET design (right-side picture) according to a first embodiment.
[0098] The SiC MOSFET 100 according to the first embodiment has a multilayer gate oxide stack that may be formed by 3 different layers 111, 112, 113. A thin interfacial dielectric layer 111 can be deposited on the SiC surface by ALD at low temperature. The thickness is the nanometric range while several materials can be considered for deposition like SiO2, SiN, AIN, A12O3 or ZrO2. The ALD ability to produce accurate thicknesses and uniform surfaces in addition to high quality film production using various different material is exploited to create an almost defect free interface, with beneficial effects on the channel mobility and reliability.
[0099] The second layer 112 can be a deposited SiO2 by CVD or HT LPCVD (between 700C and 950C, according to the different deposition technique). The deposition can be carried out for example by LPCVD at a preferred temperature around 800 °C, starting from Dichlorosilane (DCS) and nitrogen-based vapor C-free precursors (SiH2C12 and N2O). The thickness of the layer 112 can be between 20 nm and 40 nm. The high temperature deposition technique in a C-free chemistry allows to form a core dielectric layer with comparatively higher film bulk quality with extremely low density of fixed and mobile charges, heavily affecting reliability.
[0100] The third layer 113 can be a thin dielectric layer deposited at low temperature by ALD with thickness in the nanometric range. This layer can be a metallic oxide like A12O3, ZrO2 or HfO2. This layer 113 acts as capping layer sealing the first two layers 111, 112 against dopant or contamination diffusion occurring during subsequent process steps (e.g. high temperature processes like poly gate deposition or ohmic contacts annealing) in order to further reduce defectivity and improve reliability. The same gate stack is fully compatible to planar and trench designs.
[0101] In the following, a basic design for this semiconductor device 100 is described for the planar architecture. However, this design is the same for the trench architecture.
[0102] The semiconductor device 100 comprises: an n-type doped substrate 102 acting as a drain contact; an n-type doped drift layer 103 formed on the substrate 102; a p-type doped well 104 formed in the n-type doped drift layer 103; an n-type doped source contact 106 implanted in part of the p-type doped well 104; and a multi-layer gate stack 111, 112, 113 that is overlapping the n-type doped drift layer 103, the p-type doped well 104 and at least part of the n-type doped source contact 106 to enableformation of a gate electrons channel 107 in the p-type doped well 104 between the n-type doped source contact 106 and the drain contact.
[0103] The multi-layer gate stack 111, 112, 113 comprises at least a first dielectric layer 111 and a second dielectric layer 112 (the third dielectric layer 113 shown in Figure 1 is optional).
[0104] The first dielectric layer 111 is an ALD (atomic layer deposition) dielectric layer creating an interface with the n-type doped drift layer 103, the p-type doped well 104 and the at least part of the n-type doped source contact 106. The second dielectric layer 112 is deposited on the first dielectric layer 111.
[0105] The multi-layer gate stack 111, 112, 113 is configured to increase a channel mobility of the gate electrons channel 107.
[0106] By using such ALD dielectric layer 111, the deposition time can be in some cases considerably reduced by improving equipment throughput and reducing production costs. In particular, the deposition time can be reduced considering that only a thin ALD layer 111 is deposited as first interfacial layer, instead of having only one single (thick) dielectric gate layer which is all deposited by ALD and whose deposition would require a long time. In this case there is a thin ALD layer requiring some time for deposition plus a second deposition layer supposed thicker whose deposition with other techniques like LPCVD requires less time, compared to ALD.
[0107] Less deposition time refers to the case when there is one single thick dielectric layer all deposited by ALD which is very slow deposition technique.
[0108] The first ALD layer 111 creates a low detectivity interface with the layers below, e.g., SiC layers or other low bandgap material layers.
[0109] The second dielectric layer 112 creates a core dielectric layer with high film quality.
[0110] The gate stack can have two or more dielectric layers. For two dielectric layers, the manufacturing process can be simplified with benefits in terms of lower cycle time and costs. For two dielectric layers, these two dielectric layers can be patterned by a photolithographic process in the same step which reduces process time.
[0111] The first dielectric layer 111 can be implemented thinner than the second dielectric layer 112. For example, a thickness of the first dielectric layer 111 can be within a range of about Inm to lOnm and a thickness of the second dielectric layer 112 can be within a range of about 20nm to 40nm.
[0112] The first dielectric layer 111 may, for example, comprise one of the following layers: a Silicon oxide (SiO2) layer, a Silicon Nitride (Si3N4) layer, an Aluminum Nitride (AIN) layer, an Aluminum Oxide (A12O3) layer, a Zirconium Oxide (ZrO2) layer. The second dielectric layer 112 may, for example, comprise a Silicon oxide (SiO2) layer.
[0113] The first dielectric layer 111 may be formed by ALD (atomic layer deposition) at low temperature in a range of about 200C to 300C, for example. The second dielectric layer 112 may be formed by CVD (chemical vapor deposition) or by LPCVD (liquid phase chemical vapor deposition) at high temperature in a range of about 700C to 950C, for example.PDA processes (at high temperature such as 1100C in N2 or FG, 60min) after each dielectric layer deposition reduce the interface detectivity and improve film stability and robustness via a densification process. This helps to reduce channel resistance and enhance ruggedness.
[0114] The deposition of each dielectric layer may be followed by a Post Deposition Annealing (PDA) process at high temperature in one or a combination of FG, N2, NO or N2O.
[0115] PDA may be applied, for example, at high temperatures ranging from about 600 degrees Celsius to about 1100 degrees Celsius.
[0116] The first dielectric layer 111 may be aligned with the second dielectric layer 112.
[0117] When aligning the first dielectric layer 111 with the second dielectric layer 112, only one photomask process is required which reduces processing complexity.
[0118] The multi-layer gate stack 111, 112, 113 may have a constant thickness. Each dielectric layer 111, 112, 113 of the multi-layer gate stack 111, 112, 113 may have a respective constant thickness.
[0119] The multi-layer gate stack 111, 112, 113 may comprise a third dielectric layer 113 as shown in Figure 1, that may be formed by an ALD dielectric layer. The third dielectric layer 113 may be deposited on the second dielectric layer 112 as shown in Figure 1.
[0120] The third dielectric layer as ALD dielectric layer can improve lifetime and reliability.
[0121] The third dielectric layer 113 creates a cover or capping layer protecting the first two layers 111, 112 against dopant or contamination diffusion occurring during subsequent process steps, e.g., poly gate deposition or contacts annealing.
[0122] The third dielectric layer 113 may be aligned with the first and second dielectric layers 111, 112 or may be fully covering the first and second dielectric layers 111, 112 to create a capping layer sealing the first dielectric layer 111 and the second dielectric layer 112 against dopant or contamination diffusion.
[0123] The third dielectric layer 113 prevents interface and bulk contamination or doping during subsequent (thermal) process.
[0124] When aligning the third dielectric layer 113 with the first and second dielectric layers 111, 112 for creating a cover layer, only one photomask process is required which reduces processing complexity.
[0125] When creating a capping or sealing layer by the third dielectric layer 113, this layer can protect the first and second layers 111, 112 against dopant or contamination diffusion.
[0126] In the option not fully aligned (i.e., second photomask needed to pattern the third layer), the first two layers 111, 112 are protected also laterally from dopant diffusion from the sides of the first two layers.
[0127] A thickness of the third dielectric lay er 113 can be within a range of about 5nm to 1 Onm, for example.The third dielectric layer 113 may comprise one of the following layers, for example: a Silicon oxide, SiO2, layer, an Aluminum Oxide, A12O3, layer, a Zirconium Oxide, ZrO2, layer, a Hafnium Oxide, HfO2, layer. The third dielectric layer 113 may be formed by ALD (atomic layer deposition) at low temperatures in a range of about 200C to 300C, for example.
[0128] The deposition of each dielectric layer may be followed by at least one Post Deposition Annealing, PDA, process at high temperature in one or a combination of FG, N2, NO or N2O, for example.
[0129] PDA may be applied, for example, at high temperatures ranging from about 600 degrees Celsius to about 1100 degrees Celsius.
[0130] The term “at least one PDA process” covers the option in which there is one PDA process after the deposition of each layer (so 3 PDA process in all) or only one or only two PDA processes following the deposition of first, second and third layer or first and second and second and third layers, respectively.
[0131] The multi-layer gate stack 111, 112, 113 may be partially opened in a JFET region 103a (see Figures 5 and 6 described below) of the n-type doped drift layer 103 to form a multilayer split gate stack Illa, 112a, 113a, 111b, 112b, 113b according to a split gate technology.
[0132] This so-called split gate technology helps to reduce power dissipation and improve the response at high frequency through the reduction of reverse transfer capacitance. This solution can be useful to compensate the increase of the capacitance, due to the use of high permittivity dielectric layers in the gate stack.
[0133] The multilayer split gate stack Illa, 112a, 113a, 11 lb, 112b, 113b (see Figures 5 and 6) may comprise a first section Illa, 112a, 113a and a second section 111b, 112b, 113b which are separated from each other in the JFET region 103a or connected to each other by the third dielectric layer 113a, 113b formed in the JFET region 103a.
[0134] When the third dielectric layer 113a, 113b is formed in the JFET region 103a between the first and second sections of the gate stack, this solution helps to achieve a better sealing effect for the gate stack against dopant or contamination diffusion occurring during subsequent thermal steps, as for example the highly doped polysilicon layer deposition used as gate contact t and ohmic contacts annealing with beneficial effects on lifetime and reliability.
[0135] The n-type doped substrate 102 and the n-type doped drift layer 103 may comprise a high-bandgap semiconductor material, in particular silicon carbide or Gallium nitride.
[0136] The solution described here can be applied to SiC, GaN and other semiconductor materials, especially wide band gap, where the high defectivity at the interface in the gate region and high electrical field in the gate dielectric layers can result critical for reliability or long-term stability. The solution described in this disclosure improves reliability and long-term stability.
[0137] Beside the layers mentioned above, the power device 100 shown in Figure 1 further comprises a drain contact metal 101 placed below the n-type doped substrate 102 acting with the drain contact metal 101 as the drain contact. AP+ contact 105 is implanted in another part of the p-type doped well 104 next to the n-type doped source contact 106. A poly silicon layer 108 is formed on top of the multi-layer gate stack 111, 112, 113, in particular here in F igure 1 on top of the third dielectric I aver I 13 : whereas in Figure 3 it may be formed on top of the second dielectric layer 112. An intermetal dielectric 109 is covering the poly silicon layer 108 and the multi-layer gate stack 111, 112, 113. A source metal contact 110 is formed above the n-type doped source contact 106, the P+ contact 105 and the intermetal dielectric 109.As shown in F igure 1 , the semiconductor device 100 can form a planar MOSFET 100 or a trench MOSFET 100b.
[0138] As mentioned above, the technology described here can be applied likewise to planar and trench MOSFETs, regardless of the voltage class and current rating.
[0139] Figure 2 shows a schematic process flow constituting a method 200 for producing a semiconductor device according to the disclosure.
[0140] The shown process flow can be applied for the integration of the multilayer gate stack previously described with respect to Figure 1 in a SiC planar MOSFET structure. Known methods not shown in Figure 2 can be used prior to the steps 1 to 5 shown in Figure 2 to define and activate all the implanted regions prior to the gate layers deposition and to create contacts, metallization and passivation regions after the gate oxide process module, i.e., after the steps 1 to 5 shown in Figure 2.
[0141] A high temperature surface pre-conditioning treatment can be optionally carried out at high temperature in inert atmosphere (N2, Ar) before the deposition of the first ALD layer 111 in the gate stack. Suitable post deposition annealing processes can be carried out at high temperature (approximately in 1000C-1300C range) after the deposition of each dielectric layer in the gate stack with the purpose to create stable interfaces (in particular that formed by the first layer and SiC), reduce the detectivity and densify the dielectric layers deposited at quite low temperatures. N2 can be used after the deposition of the ALD layers while FG (Forming Gas) or N2 can be used after the deposition of the CVD / LPCVD intermediate SiO2 layer. Nonetheless, high temperature PDA in different ambient can be applied, including for example NO, N2O, N3, POC13 or a mixture of these gases.
[0142] In the manufacturing of the semiconductor device according to the first embodiment, the third layer 113 may fully embed the first two layers 111, 112 and can be defined by a second photolithography and etching process while a first photolithographic process can be used to pattern the first two dielectric layers 111, 112 in the same step.
[0143] The method 200 shown in Figure 2 can be used for producing a semiconductor device, e.g., a semiconductor device 100, 100b as shown in Figure 1.
[0144] The method 200 comprises: providing 201 a p-type doped well 104 formed in an n-type doped drift layer 103, an n-type doped source contact 106 implanted in part of the p-type doped well 104 and an n-type doped substrate 102 acting as a drain contact. This process is shown by the first item (1).
[0145] The method 200 comprises: forming 202, 203 a first dielectric layer 111 and a second dielectric layer 112 of a multilayer gate stack 111, 112, 113 overlapping the n-type doped drift layer 103, the p-type doped well 104 and at least part of the n-type doped source contact 106 to enable formation of a gate electrons channel 107 in the p-type doped well 104 between the n-type doped source contact 106 and the drain contact. This process is shown by the first item (1 ) where forming the first dielectric layer 111 is shown and by the second item (2) where forming the second dielectric layer 112 is shown.
[0146] In the method 200, forming 202 the first dielectric layer 111 comprises forming an atomic layer deposition (ALD) dielectric layer, creating an interface with the n-type doped drift layer 103, the p-type doped well 104 and the at least part of the n-type doped source contact 106 as shown by the first item (1).
[0147] In the method 200, forming 203 the second dielectric layer 112 comprises depositing the second dielectric layer 112 on the first dielectric layer 111 for increasing a channel mobility of the gate electrons channel 107 as shown by the second item (2).The second dielectric layer 112 can be a deposited dielectric layer formed by Plasma Enhanced Chemical Vapor Deposition (PECVD), Low Pressure Chemical Vapor Deposition (LPCVD) or Chemical Vapor Deposition (CVD).
[0148] Forming 202 the first dielectric layer 111 may comprise ALD (atomic layer deposition) at low temperature in a range of about 200C to 300C. Forming 203 the second dielectric layer 112 may comprise chemical vapor deposition (CVD) or liquid phase chemical vapor deposition (LPCVD) at high temperature in a range of about 700C to 950C.
[0149] The deposition of each dielectric layer may be followed by at least one Post Deposition Annealing, PDA, process at high temperature in one or a combination of FG (Forming Gas), N2, NO or N2O.
[0150] PDA may be applied, for example, at high temperatures ranging from about 600 degrees Celsius to about 1100 degrees Celsius.
[0151] In this method 200, the subsequent items (3), (4) and (5) are optional and described in the following.
[0152] The method 200 may further comprise: forming 204 a third dielectric layer 113 of the multilayer gate stack 111, 112, 113 by ALD deposition on the second dielectric layer 112.
[0153] Forming 204 the third dielectric layer 113 may comprise ALD deposition at low temperature in a range of about 200C to 300C followed by post deposition annealing at high temperature. Before forming 204 the third dielectric layer 113, the first and second dielectric layers 111, 112 may be structured, e.g., in the region of the gate electrode as shown by item (3).
[0154] The deposition of each dielectric layer may be followed by at least one Post Deposition Annealing, PDA, process at high temperature in one or a combination of FG (Forming Gas), N2, NO or N2O.
[0155] PDA may be applied, for example, at high temperatures ranging from about 600 degrees Celsius to about 1100 degrees Celsius. PDA may be applied, for example, for a duration between about 30 min and 4 hours.
[0156] The third dielectric layer 113 may be structured, e.g., in the region of the gate electrode as shown by item (5).
[0157] Figure 3 shows a cross section of a semiconductor device 100 according to a second embodiment.
[0158] The semiconductor device 100 according to the second embodiment corresponds to the semiconductor device 100 according to the first embodiment, but no capping layer (i.e., third dielectric layer 113) is used. Only two PDA treatments may be carried out after the deposition of the first and second gate layers 111, 112.
[0159] In the second embodiment the manufacturing process can be simplified with benefits in terms of lower cycle time and costs. The second embodiment is compatible to both planar and trench MOSFET designs as shown in Figure 1.
[0160] Figure 4 shows a cross section of a semiconductor device 100 according to a third embodiment.
[0161] The semiconductor device 100 according to the third embodiment corresponds to the semiconductor device 100 according to the first embodiment, but only one photomask process is used to pattern the three aligned dielectric layers 111, 112, 113 in the gate stack. The PDA treatments can be reduced to two, the first after the deposition of the first ALD layer 111 , the second after the deposition of the second CVD or LPCVD and third ALD layers.In the third embodiment the manufacturing process can be simplified with benefits in terms of lower cycle time and costs. The third embodiment is compatible to both planar and trench MOSFET designs as shown in Figure 1.
[0162] Figure 5 shows a cross section of a semiconductor device 100 according to a fourth embodiment.
[0163] The semiconductor device 100 according to the fourth embodiment corresponds to the semiconductor device 100 according to the first embodiment, but the dielectric gate layers 111, 112, 113 are completely opened in an inner part of the JFET region 103a between contiguous P wells 104. The separated gate layers are referred to as Illa, 112a, 113a (left side gate stack) and 111b, 112b, 113b (right side gate stack). This so-called split gate technology helps to reduce power dissipation and improve the response at high frequency through the reduction of reverse transfer capacitance. This solution can be useful to compensate the increase of the capacitance, due to the use of high permittivity dielectric layers in the gate stack.
[0164] This structure can be combined with the second and third embodiments shown in Figures 3 and 4 for planar MOSFETs (missing 3rdlayer 113 in the stack or 3rdlayer 113 aligned to first and second layers 111, 112).
[0165] The fourth embodiment is compatible to the planar MOSFET design as shown in Figure 1 but requires design changes when being applied to the trench MOSFET.
[0166] Figure 6 shows a cross section of a semiconductor device 100 according to a fifth embodiment.
[0167] The semiconductor device 100 according to the fifth embodiment is an extension of the semiconductor device 100 according to the fourth embodiment shown in Figure 5. In the fifth embodiment shown here in Figure 6, only the dielectric capping layer 113 is not patterned in the JFET region 103a. This solution helps to achieve a better sealing effect for the gate stack against dopant or contamination diffusion occurring during subsequent thermal steps, as for example the highly doped poly silicon layer deposition used as gate contact and ohmic contacts annealing, with beneficial effects on lifetime and reliability.
[0168] The fifth embodiment is compatible to the planar MOSFET design as shown in Figure 1 but requires design changes when being applied to the trench MOSFET.
[0169] While a particular feature or aspect of the disclosure may have been disclosed with respect to only one of several implementations, such feature or aspect may be combined with one or more other features or aspects of the other implementations as may be desired and advantageous for any given or particular application. Furthermore, to the extent that the terms "include", "have", "with", or other variants thereof are used in either the detailed description or the claims, such terms are intended to be inclusive in a manner similar to the term "comprise". Also, the terms "exemplary", "for example" and "e.g." are merely meant as an example, rather than the best or optimal. The terms “coupled” and “connected”, along with derivatives may have been used. It should be understood that these terms may have been used to indicate that two elements cooperate or interact with each other regardless whether they are in direct physical or electrical contact, or they are not in direct contact with each other.
[0170] Although specific aspects have been illustrated and described herein, it will be appreciated by those of ordinary skill in the art that a variety of alternate and / or equivalent implementations may be substituted for the specific aspects shown and described without departing from the scope of the disclosure. This application is intended to cover any adaptations or variations of the specific aspects discussed herein.Although the elements in the following claims are recited in a particular sequence with corresponding labeling, unless the claim recitations otherwise imply a particular sequence for implementing some or all of those elements, those elements are not necessarily intended to be limited to being implemented in that particular sequence.
[0171] Many alternatives, modifications, and variations will be apparent to those skilled in the art in light of the above teachings. Of course, those skilled in the art readily recognize that there are numerous applications of the disclosure beyond those described herein. While the disclosure has been described with reference to one or more particular embodiments, those skilled in the art recognize that many changes may be made thereto without departing from the scope of the disclosure. It is therefore to be understood that within the scope of the appended claims and their equivalents, the disclosure may be practiced otherwise than as specifically described herein.
Claims
CLAIMS:
1. A semiconductor device (100), comprising:an n-type doped substrate (102) acting as a drain contact;an n-type doped drift layer (103) formed on the substrate (102);a p-type doped well (104) formed in the n-type doped drift layer (103);an n-type doped source contact (106) implanted in part of the p-type doped well (104); anda multi-layer gate stack (111, 112, 113) that is overlapping the n-type doped drift layer (103), the p-type doped well (104) and at least part of the n-type doped source contact (106) to enable formation of a gate electrons channel (107) in the p-type doped well (104) between the n-type doped source contact (106) and the drain contact;wherein the multi-layer gate stack (111, 112, 113) comprises at least a first dielectric layer (111) and a second dielectric layer (112);wherein the first dielectric layer (111) is an ALD, atomic layer deposition, dielectric layer creating an interface with the n-type doped drift layer (103), the p-type doped well (104) and the at least part of the n-type doped source contact (106);wherein the second dielectric layer (112) is deposited on the first dielectric layer (111); andwherein the multi-layer gate stack (111, 112, 113) is configured to increase a channel mobility of the gate electrons channel (107).
2. The semiconductor device (100) of claim 1,wherein the first dielectric layer (111) is thinner than the second dielectric layer (112).
3. The semiconductor device (100) of claim 1 or 2,wherein a thickness of the first dielectric layer (111) is within a range of about Inm to lOnm and a thickness of the second dielectric layer (112) is within a range of about 20nm to 40nm.
4. The semiconductor device (100) of any of the preceding claims,wherein the first dielectric layer (111) comprises one of the following layers: a Silicon oxide, SiO2, layer, a Silicon Nitride, Si3N4, layer, an Aluminum Nitride, AIN, layer, an Aluminum Oxide, A12O3, layer, a Zirconium Oxide, ZrO2, layer; andwherein the second dielectric layer (112) comprises a Silicon oxide, SiO2, layer.
5. The semiconductor device (100) of any of the preceding claims,wherein the first dielectric layer (111) is formed by ALD, atomic layer deposition at low temperature in a range of about 200C to 300C; andwherein the second dielectric layer (112) is formed by CVD, chemical vapor deposition, or by LPCVD, liquid phase chemical vapor deposition at high temperature in a range of about 700C to 950C.
6. The semiconductor device (100) of any of the preceding claims,wherein the deposition of each dielectric layer is followed by a Post Deposition Annealing, PDA, process at high temperature in one or a combination of FG, N2, NO or N2O.
7. The semiconductor device (100) of any of the preceding claims,wherein the first dielectric layer (111) is aligned with the second dielectric layer (112).
8. The semiconductor device (100) of any of the preceding claims,wherein the multi-layer gate stack (111, 112, 113) has a constant thickness; andwherein each dielectric layer (111, 112, 113) of the multi-layer gate stack (111, 112, 113) has a respective constant thickness.
9. The semiconductor device (100) of any of the preceding claims,wherein the multi-layer gate stack (111, 112, 113) comprises a third dielectric layer (113) formed by an ALD dielectric layer, the third dielectric layer (113) being deposited on the second dielectric layer (112).
10. The semiconductor device (100) of claim 9,wherein the third dielectric layer (113) is aligned with the first and second dielectric layers (111, 112) or is fully covering the first and second dielectric lay ers ( 111 , 112) to create a capping layer sealing the first dielectric lay er ( 111 ) and the second dielectric layer (112) against dopant or contamination diffusion.
11. The semiconductor device (100) of claim 9 or 10,wherein a thickness of the third dielectric layer (113) is within a range of about 5nm to lOnm.
12. The semiconductor device (100) of any of claims 9 to 11,wherein the third dielectric layer (113) comprises one of the following layers: a Silicon oxide, SiO2, layer, an Aluminum Oxide, A12O3, layer, a Zirconium Oxide, ZrO2, layer, a Hafnium Oxide, HfO2, layer; andwherein the third dielectric layer (113) is formed by ALD, atomic layer deposition at low temperatures in a range of about 200C to 300C.
13. The semiconductor device (100) of any of claims 9 to 12,wherein the deposition of each dielectric layer is followed by at least one Post Deposition Annealing, PDA, process at high temperature in one or a combination of FG, N2, NO or N2O.
14. The semiconductor device (100) of any of claims 9 to 13,wherein the multi-layer gate stack (111, 112, 113) is partially opened in a JFET region (103a) of the n-type doped drift layer (103) to form a multilayer split gate stack (Illa, 112a, 113a, 111b, 112b, 113b) according to a split gate technology.
15. The semiconductor device (100) of claim 14,wherein the multilayer split gate stack (Illa, 112a, 113a, 111b, 112b, 113b) comprises a first section (Illa, 112a, 113a) and a second section (111b, 112b, 113b) which are separated from each other in the JFET region (103a) or connected to each other by the third dielectric layer (113a, 113b) formed in the JFET region (103a).
16. The semiconductor device (100) of any of the preceding claims,wherein the n-type doped substrate (102) and the n-type doped drift lay er ( 103 ) comprise a high-bandgap semiconductor material, in particular silicon carbide or Gallium nitride.
17. The semiconductor device (100) of any of the preceding claims,forming a planar MOSFET or a trench MOSFET.
18. A method (200) for producing a semiconductor device (100), the method comprising:providing (201) a p-type doped well (104) formed in an n-type doped drift layer (103), an n-type doped source contact (106) implanted in part of the p-type doped well (104) and an n-type doped substrate (102) acting as a drain contact; andforming (202, 203) a first dielectric layer (111) and a second dielectric layer (112) of a multilayer gate stack (111, 112, 113) overlapping the n-type doped drift layer (103), the p-type doped well (104) and at least part of the n-type doped source contact (106) to enable formation of a gate electrons channel (107) in the p-type doped well (104) between the n-type doped source contact (106) and the drain contact;wherein forming (202) the first dielectric layer (111) comprises forming an atomic layer deposition, ALD, dielectric layer, creating an interface with the n-type doped drift layer (103), the p-type doped well (104) and the at least part of the n-type doped source contact (106); andwherein forming (203) the second dielectric layer (112) comprises depositing the second dielectric layer (112) on the first dielectric layer (111) for increasing a channel mobility of the gate electrons channel (107).
19. The method (200) of claim 18,wherein the second dielectric layer (112) is a deposited dielectric layer formed by Plasma Enhanced Chemical Vapor Deposition, PECVD, Low Pressure Chemical Vapor Deposition, LPCVD, or Chemical Vapor Deposition, CVD.1920. The method (200) of claim 18 or 19,wherein forming the first dielectric layer (111) comprises ALD, atomic layer deposition at low temperature in a range of about 200C to 300C; andwherein forming the second dielectric layer (112) comprises chemical vapor deposition, CVD, or liquid phase chemical vapor deposition, LPCVD, at high temperature in a range of about 700C to 950C.
21. The method (200) of any of claims 18 to 20, comprising:forming (204) a third dielectric layer (113) of the multilayer gate stack (111, 112, 113) by ALD deposition on the second dielectric layer (112).
22. The method (200) of claim 21,wherein forming the third dielectric layer (113) comprises ALD deposition at low temperature in a range of about 200C to 300C followed by post deposition annealing at high temperature.20