Method for producing a multilayer adhesive element
A multi-layer adhesive element with a barrier layer composed of copolyamides or copolyolefins addresses storage stability issues at elevated temperatures, ensuring consistent adhesive performance and bond strength.
Patent Information
- Application Number
- PCT/EP2026/061994
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-06
- Filing Date
- 2026-04-27
- Publication Date
- 2026-11-12
AI Technical Summary
Adhesive elements experience adverse storage stability at elevated temperatures, particularly in demanding applications, leading to deterioration of adhesive properties, especially when using foamed carriers and resin-containing adhesives, which affects their performance on non-surface-activated substrates.
A multi-layer adhesive element is designed with a specific barrier layer between the adhesive resin-containing layer and the foamed carrier layer, using copolyamides or copolyolefins with defined glass transition temperatures to prevent resin migration and maintain adhesive properties during storage at elevated temperatures.
The solution ensures that the adhesive elements maintain excellent adhesive properties after prolonged exposure to high temperatures, reducing the need for additional release liners and enhancing bond strength under mechanical loads.
Smart Images

Figure EP2026061994_12112026_PF_FP_ABST
Abstract
Description
[0001] Method for producing a multi-layer adhesive element
[0002] Description
[0003] The invention relates to a multilayer adhesive element and a method for producing such a multilayer adhesive element. It also discloses the use of a barrier layer between an adhesive resin-containing layer and a foamed carrier layer of a multilayer adhesive element to improve the storage stability of the multilayer adhesive element at elevated temperatures.
[0004] Joining separate components is a key process in manufacturing technology. Alongside other methods, such as welding and soldering, bonding—that is, joining using an adhesive—is of particular importance today. An alternative to using formless adhesives, such as those applied from a tube, are adhesive tapes, whose adhesive effect is based on the adhesive compounds used. The use of adhesive tapes offers numerous advantages, making this technology ideal for use in many industries, such as electronics and automotive.
[0005] Nowadays, adhesive elements are specifically adapted to the requirements of each application. Consequently, many industrially used adhesive elements are high-performance products whose physicochemical, mechanical, and especially adhesive properties are subject to stringent demands.
[0006] An important technological development in this area is the use of adhesive tapes with a porous, particularly foamed, backing layer, as this can have a particularly beneficial effect on the mechanical properties of the resulting adhesive elements, especially at low temperatures. Furthermore, the specific tailoring of the adhesive compound to the application requirements also plays a crucial role. The adhesive compounds used can be adjusted across a broad spectrum of properties through various chemical parameters, especially the choice of polymers and additives. Adhesive compounds that utilize resins to optimize bonding properties are particularly relevant for high-performance applications.Such adhesives are particularly useful for adhesive elements that are intended to achieve excellent adhesion on difficult substrates even without prior surface treatment (also known as "primerless").
[0007] Even though high-performance adhesive elements can often be produced using methods known from the prior art, these methods are also perceived as disadvantageous in other respects. The high demands on application properties apply not only to the initial bonding of a new adhesive element, but also to the fact that the adhesive elements must maintain the desired property profiles over a long period. A particular challenge here is that the properties of many adhesive elements, especially after prolonged storage at elevated temperatures of, for example, 70 °C or more, are not sufficiently stable. As a result, after such storage, the adhesive elements may not meet the high demands placed upon them, or may only do so to a limited extent.
[0008] It has been found that adverse storage stability at elevated temperatures is observed particularly in adhesive elements designed for demanding applications, such as primerless bonding, by using a foamed carrier and resin-containing adhesives. The deterioration of adhesive properties during prolonged storage at elevated temperatures is especially significant in such adhesive elements.
[0009] The primary objective of the present invention was to eliminate or at least reduce the disadvantages of the prior art.
[0010] In particular, it was an object of the present invention to provide a multi-layer adhesive element with which excellent adhesive properties can be achieved even after several days of storage at elevated temperatures, wherein the adhesive properties should preferably not change or at least only change to a small extent during storage at elevated temperatures, especially in the range of 70 to 100 °C.
[0011] It was an object of the present invention that the multilayer adhesive elements to be specified should have inherently advantageous adhesive properties that should make them particularly suitable for demanding adhesive applications, especially for use on non-surface-activated substrate surfaces (“primerless”), and especially also on surfaces with a low surface energy, such as clear coats, as used, for example, in the automotive industry.
[0012] A further objective of the present invention was that the bonds produced with the multilayer adhesive elements to be specified should also exhibit advantageous adhesive properties even after prolonged exposure at 100 °C.
[0013] A further objective of the present invention was to ensure that the multilayer adhesive elements to be specified could be manufactured in the most time- and cost-efficient manner possible, preferably using equipment that is already in use today for the production of corresponding multilayer adhesive elements.
[0014] Against this background, a further object of the present invention was to provide an advantageous method by which the multilayer adhesive elements to be specified could be produced in a time- and cost-efficient manner.
[0015] In this respect, it was a desirable requirement that the specified process should in particular reduce the need for separating liners used in the process, which would otherwise be generated as waste in the process, so that the process according to the invention should be advantageous from both ecological and economic points of view.
[0016] A further object of the present invention was that the multilayer adhesive elements to be specified should exhibit a particularly advantageous bond strength, whereby the adhesion between the individual layers of the multilayer adhesive elements meets the requirements even under high mechanical loads, and especially at elevated temperatures. In this respect, a further object of the present invention was that the method to be provided should make it possible to produce multilayer adhesive elements which have excellent bond strength between the individual layers.
[0017] The inventors of the present invention have now found that the problems described above can surprisingly be solved by providing a multi-layer adhesive element comprising an adhesive resin-containing adhesive mass and a foamed carrier layer, and by arranging a specific barrier layer between the adhesive mass and the carrier layer, which is formed using one or more specific barrier plastics as defined in the claims.
[0018] A particularly advantageous manufacturing process for producing multi-layered adhesive elements can be achieved if the foamed plastic layer of the carrier layer is not produced separately in a prior step on conventional release liners, but rather the foamed carrier layer is formed directly on the barrier layer. This not only advantageously reduces the need for additional release liners in the manufacturing process, but also results in a particularly favorable bond strength between the carrier layer and the barrier layer.
[0019] The aforementioned problems are thus solved by the subject matter of the invention as defined in the claims. Preferred embodiments of the invention are described in the dependent claims and the following descriptions.
[0020] Such embodiments, which are hereinafter referred to as preferred, are combined in particularly preferred embodiments with features of other embodiments referred to as preferred. Combinations of two or more of the embodiments referred to below as particularly preferred are therefore especially preferred. Also preferred are embodiments in which a feature of one embodiment, referred to as preferred to any degree, is combined with one or more further features of other embodiments, which are referred to as preferred to any degree. Features of preferred methods and uses result from the features of preferred multilayer adhesive elements.
[0021] Insofar as specific quantities or proportions of an element, for example, the adhesive resins, as well as preferred embodiments of the element, are disclosed below, the specific quantities or proportions of the preferably embodiments of the elements are also disclosed. Furthermore, it is disclosed that, among the corresponding specific total quantities or proportions of the elements, at least some of the elements may be preferably embodiments, and in particular, that preferably embodiments may, within the specific total quantities or proportions, again be present in specific quantities or proportions.
[0022] Particularly preferred embodiments of the invention are disclosed in the exemplary embodiments. Particularly preferred embodiments of the invention have two or more, preferably three or more, and most preferably four or more, of the preferred features of the invention disclosed below, which are also implemented in the exemplary embodiments.
[0023] The invention relates to a multi-layered adhesive element comprising:
[0024] i) a first adhesive layer, wherein the first adhesive layer comprises a first adhesive compound, wherein the first adhesive compound comprises one or more adhesive resins,
[0025] ii) a carrier layer, wherein the carrier layer comprises a foamed plastic layer, and ill) a first barrier layer arranged between the first adhesive layer and the carrier layer, wherein the first barrier layer comprises one or more barrier plastics selected from the group consisting of
[0026] iii.i) Copolyamides with a glass transition temperature, measured by DSC, of 5 °C or more, and
[0027] iii.ii) Copolyolefins of at least one first olefin with 2 to 5 carbon atoms and at least one second olefin with 6 to 12 carbon atoms.
[0028] The invention relates to a multilayer adhesive element. It can be considered advantageous that the multilayer adhesive element according to the invention can, in principle, be provided in various forms, including, for example, die-cut versions. However, for the vast majority of cases, adhesive tapes are preferred, particularly from a manufacturing perspective. Accordingly, a multilayer adhesive element according to the invention is preferably an adhesive tape. For many applications, a multilayer adhesive element according to the invention is additionally or alternatively preferred, wherein the multilayer adhesive element has an average thickness in the range of 150 to 3000 pm, preferably in the range of 300 to 2000 pm.
[0029] The advantages of the use of the first barrier layer according to the invention are already evident in single-sided adhesive elements. However, the advantages are particularly pronounced when the teaching according to the invention is applied to double-sided adhesive elements, in which cases barrier layers are preferably used between the two adhesive layers. For most applications, a multi-layer adhesive element according to the invention is therefore preferred, wherein the multi-layer adhesive element is a single-sided or double-sided, preferably a double-sided, adhesive element. A multi-layer adhesive element according to the invention is also preferred, wherein the multi-layer adhesive element additionally comprises:
[0030] iv) a second adhesive layer, wherein the second adhesive layer comprises a second adhesive compound, the second adhesive compound comprising one or more resins, and
[0031] v) a second barrier layer arranged between the second adhesive layer and the carrier layer, wherein the second barrier layer comprises one or more of the barrier plastics.
[0032] An important component of the multilayer adhesive elements according to the invention is the carrier layer. A preferred multilayer adhesive element according to the invention is one in which the carrier layer, preferably the carrier layer and the foamed plastic layer, have an average thickness in the range of 150 to 4000 pm, preferably in the range of 200 to 2000 pm.
[0033] According to the invention, the carrier layer comprises a foamed plastic layer. At least theoretically, it would be conceivable for the carrier layer to have one or more further layers in addition to the foamed plastic layer, with which, for example, the mechanical properties of the carrier layer could be further adapted to the respective application. However, for the vast majority of cases, it is relevant that the carrier layer should consist as largely as possible of the foamed plastic layer, which is particularly advantageous from a manufacturing perspective and also prevents the bond strength between individual sub-layers of the carrier layer from becoming a weak point in the multi-layer adhesive element. Accordingly, a multi-layer adhesive element according to the invention is conceivable, wherein the carrier layer comprises one or more further sub-layers in addition to the foamed plastic layer.However, a multi-layer adhesive element according to the invention is preferred, wherein the carrier layer consists of a mass fraction of 70% or more, preferably 90% or more, particularly preferably 95% or more, and most particularly preferably 98% or more, of the foamed plastic layer, based on the mass of the carrier layer.
[0034] According to the invention, the plastic layer is a foamed plastic layer. The use of so-called syntactically foamed plastics is preferred. A multilayer adhesive element according to the invention is therefore preferred, wherein the foamed plastic layer is a syntactically foamed plastic layer, and the foamed plastic layer preferably comprises expanded microballoons or hollow spheres, preferably glass hollow spheres.
[0035] In syntactically foamed plastic layers, hollow bodies, such as pre-expanded microballoons, are incorporated into the matrix material, whereby the created cavities are separated from each other and from the matrix material by a membrane.
[0036] The term "microballoons" refers to elastic, and therefore expandable in their ground state, microhollow spheres with a thermoplastic polymer shell. These spheres are usually filled with low-boiling liquids or liquefied gas. Common shell materials include polyacrylonitrile, PVDC, PVC, and poly(meth)acrylates. The low-boiling liquids used are typically short-chain hydrocarbons, such as isobutane or isopentane, which are often contained within the polymer shell as a liquefied gas under pressure.
[0037] Microballoons are commercially available in a variety of embodiments, which can be characterized essentially by their size (mostly 6 to 45 pm diameter d50 in the unexpanded state) and the initial expansion temperatures required (e.g., 75 to 220 °C). Unexpanded microballoons are available, for example, as aqueous dispersions with a microballoon mass fraction of approximately 40 to 45%, or as polymer-bonded products, for example in ethylene vinyl acetate, with a microballoon mass fraction of approximately 65%, as well as in dry form. A multilayer adhesive element according to the invention is generally preferred, wherein the foamed plastic layer has an average porosity in the range of 1 to 65%, preferably in the range of 10 to 55%.
[0038] The inventors of the present invention have found that particularly high-performance multilayer adhesive elements can be obtained by using a poly(meth)acrylate-based plastic for the foamed carrier layer, where the term (meth)acrylate, in accordance with the understanding of those skilled in the art, denotes both acrylates and methacrylates, and corresponding plastics may also comprise other monomers, in particular (meth)acrylic acid. A multilayer adhesive element according to the invention is therefore preferred, wherein the foamed plastic layer comprises one or more (co)polymers selected from the group consisting of poly(meth)acrylates.
[0039] Although it is theoretically possible to produce the foamed plastic layer from the melt, for example by means of extrusion coating, particularly advantageous results with regard to the bond strength between the barrier layer and the formed foamed plastic layer have been achieved when the foamed plastic layer is formed by means of initiator-based crosslinking, in particular radiation-based crosslinking, as is further disclosed below with regard to the process according to the invention. Accordingly, a multilayer adhesive element according to the invention is preferred, wherein the foamed plastic layer can be produced or is produced by crosslinking a crosslinkable composition, preferably a radiation-crosslinkable composition, and particularly preferably a UV-radiation-crosslinkable composition.Preferably, or alternatively, a multilayer adhesive element according to the invention is used, wherein the crosslinkable composition comprises:
[0040] i) one or more crosslinkable compounds, preferably crosslinkable (meth)acrylate compounds,
[0041] ii) one or more initiator compounds, preferably photoinitiator compounds, iii) one or more fillers selected from the group consisting of hollow spheres, in particular glass hollow spheres, pre-expanded microballoons and expandable microballoons, preferably expandable microballoons and pre-expanded microballoons. As further disclosed below with reference to the process according to the invention, it is particularly advantageous to form the support layer or its foamed plastic layer directly on the respective barrier layer during production, which not only allows for a particularly time- and cost-efficient process but also results in advantageous bond strength.A multi-layer adhesive element according to the invention is therefore preferred, wherein the carrier layer, preferably via the foamed plastic layer, is materially bonded to the first barrier layer, and / or wherein the connection between the carrier layer and the first barrier layer, preferably between the foamed plastic layer and the first barrier layer, can be produced by crosslinking a crosslinkable composition used in the production of the carrier layer that contacts the first barrier layer.A multilayer adhesive element according to the invention is preferred, either additionally or alternatively, wherein the carrier layer, preferably via the foamed plastic layer, is bonded to the second barrier layer, and / or wherein the connection between the carrier layer and the second barrier layer, preferably between the foamed plastic layer and the second barrier layer, can be established by crosslinking a crosslinkable composition used in the manufacture of the carrier layer and contacting the second barrier layer. The functionality of the multilayer adhesive element to act as an adhesive element is ensured according to the invention by the first adhesive layer, or, in the case of double-sided adhesive elements, by the first and second adhesive layers.Although it would theoretically be conceivable to provide further layers between the adhesive layer and the barrier layer, it is particularly preferred, in view of the manufacturing effort and costs as well as the resulting bond strength, to form the adhesive layers directly on the barrier layer. A multilayer adhesive element according to the invention is preferred, wherein the first adhesive layer is materially bonded to the first barrier layer, and / or wherein the second adhesive layer is materially bonded to the second barrier layer.
[0042] It can be seen as an advantage of the present invention that it is not fundamentally limited with regard to the method by which the adhesive layer is brought together with the other components of the multilayer adhesive element. In particular, it is possible to coat the barrier layer with the respective adhesive, which can in principle be done directly on the barrier layer by means of solvent coating or by first producing a corresponding adhesive layer, which can then be laminated onto the barrier layer. However, in the inventors' opinion, particularly advantageous embodiments result, especially with regard to the achievable bond strengths, when the adhesive layer is obtained directly on the respective barrier layer by crosslinking a corresponding crosslinkable adhesive composition.A multi-layer adhesive element according to the invention is therefore preferred, wherein the connection between the first barrier layer and the first adhesive layer can be established by crosslinking a first adhesive composition used in the production of the first adhesive layer and contacting the first barrier layer, and / or wherein the connection between the first barrier layer and the first adhesive layer can be established by coating the first barrier layer with the first adhesive compound, wherein the coating is preferably carried out by coating with the first adhesive compound from a solvent or by laminating the first adhesive layer.Preferably, or alternatively, a multi-layer adhesive element according to the invention is used, wherein the connection between the second barrier layer and the second adhesive layer can be established by crosslinking a second, crosslinkable adhesive composition used in the production of the second adhesive layer and contacting the second barrier layer, and / or wherein the connection between the second barrier layer and the second adhesive layer can be established by coating the second barrier layer with the second adhesive compound, wherein the coating is preferably carried out by coating with the second adhesive compound from a solvent or by laminating the second adhesive layer.
[0043] For essentially all embodiments, it is particularly preferred to use pressure-sensitive adhesives for the adhesive layers, thus creating a pressure-sensitive adhesive element. Such pressure-sensitive adhesive elements can advantageously be removed without leaving any residue after application, if necessary. A multi-layer adhesive element according to the invention is therefore preferred, wherein the first adhesive layer and / or the second adhesive layer, preferably both the first and second adhesive layers, are pressure-sensitive adhesive layers, and / or wherein the first adhesive and / or the second adhesive layer, preferably both the first and second adhesive layers, are pressure-sensitive adhesives.
[0044] In accordance with professional understanding, a pressure-sensitive adhesive is an adhesive that possesses tacky properties, meaning the ability to form a permanent bond to a substrate even under relatively light pressure. Corresponding pressure-sensitive tapes are generally permanently tacky even at room temperature, meaning they exhibit a certain viscosity and tackiness, allowing them to wet the surface of a substrate even with minimal pressure. While not bound to this theory, it is often assumed that a pressure-sensitive adhesive can be considered an extremely highly viscous liquid with an elastic component, which consequently exhibits characteristic viscoelastic properties that lead to the permanent tackiness and pressure-sensitive adhesion described above.It is assumed that, in the case of suitable pressure-sensitive adhesives, mechanical deformation leads to both viscous flow processes and the development of elastic restoring forces. The viscous flow component serves to achieve adhesion, while the elastic properties are particularly necessary for achieving cohesion. The relationships between rheology and pressure-sensitive tack are known in the prior art and are described, for example, in "Satas, Handbook of Pressure Sensitive Adhesives Technology", Third Edition, (1999), pages 153 to 203. To characterize the degree of elastic and viscous components, the storage modulus (G') and the loss modulus (G") are usually used, which can be determined by means of dynamic mechanical analysis (DMA), for example, using a rheometer, as disclosed, for example, in WO 2015 / 189323 A1.Within the scope of the present invention, an adhesive mass is preferably understood to be adhesive and thus a pressure-sensitive adhesive mass if, at a temperature of 23 °C in the deformation frequency range of 10° to 10. 1 rad / sec G' and G" each at least partially in the range of 10 3 up to 10 7 Pa lie.
[0045] With regard to the dimensioning of the adhesive layers, a multi-layer adhesive element according to the invention is preferred, wherein the first adhesive layer and / or the second adhesive layer, preferably the first adhesive layer and the second adhesive layer, have an average layer thickness in the range of 20 to 100 pm, preferably in the range of 30 to 70 pm.
[0046] Although it would theoretically be conceivable to include other components in the adhesive layers besides the respective adhesives, for example, macroscopically dispersed fillers in the adhesives, it is particularly preferred to form the adhesive layers as largely as possible from the respective adhesive. A multilayer adhesive element according to the invention is therefore preferred, wherein the first adhesive layer consists of the first adhesive by mass of 70% or more, preferably 90% or more, particularly preferably 95% or more, and most preferably 98% or more, based on the mass of the first adhesive layer, and / or wherein the second adhesive layer consists of the second adhesive by mass of 70% or more, preferably 90% or more, particularly preferably 95% or more, and most preferably 98% or more, based on the mass of the second adhesive layer.
[0047] For the use of the multilayer adhesive elements according to the invention, poly(meth)acrylate- and synthetic rubber-based adhesives have proven to be particularly effective, although it is also possible in principle to use mixtures of these polymers. A preferred multilayer adhesive element according to the invention is one in which the first adhesive and / or the second adhesive, preferably both the first and second adhesives, consists of one or more adhesive (co)polymers selected from the group consisting of poly(meth)acrylates and synthetic rubbers, preferably poly(meth)acrylates, to a mass fraction of 40% or more, preferably 60% or more.
[0048] According to the above definition, the first adhesive, and in the case of double-sided adhesive tapes preferably also the second adhesive, comprises one or more adhesive resins. Adhesive resins are widely known in the field of technology and are generally used to optimize the adhesive properties of an adhesive. Corresponding adhesive resins are commercially available from numerous suppliers under this term. A person skilled in the art distinguishes between adhesive resins and polymeric compounds based on their general technical knowledge, in particular on the basis of the weight-average molar mass Mw, measured by GPC, which for resins is 15,000 g / mol or less, preferably 10,000 g / mol or less, and particularly preferably 5,000 g / mol or less, and thus below the values of adhesive (co)polymers.A multilayer adhesive element according to the invention is preferred, the adhesive resins being selected from the group consisting of resins with a weight-average molar mass Mw in the range of 1000 to 15000 g / mol, preferably in the range of 1500 to 10000 g / mol, and particularly preferably in the range of 2000 to 5000 g / mol. The determination by gel permeation chromatography (GPC) is carried out within the scope of the present invention in accordance with paragraph 37 of DE 102022124903 A1.
[0049] With regard to the chemical nature of the adhesive resins, a multilayer adhesive element according to the invention is preferred, wherein the adhesive resins are selected from the group consisting of non-hydrogenated, partially or fully hydrogenated resins based on rosin or rosin derivatives, terpene phenol resins, resins based on methacylates, hydrogenated polymers of dicyclopentadiene, non-hydrogenated, partially, selectively or fully hydrogenated hydrocarbon resins based on C5, C5 / C9 and C9 monomer streams, and polyterpene resins based on α-pinene and / or β-pinene and / or β-limonene.
[0050] The inventors have succeeded in identifying preferred ranges for the content of adhesive resins. A preferred option is a multilayer adhesive element according to the invention, wherein the first adhesive mass comprises one or more adhesive resins in a combined mass fraction in the range of 1 to 60%, preferably in the range of 5 to 40%, based on the mass of the first adhesive mass, and / or wherein the second adhesive mass comprises one or more adhesive resins in a combined mass fraction in the range of 1 to 60%, preferably in the range of 5 to 40%, based on the mass of the second adhesive mass.
[0051] Particularly for applications where both adhesive layers of double-sided, multi-layer adhesive elements are designed for contacting similar or even identical substrates, the first and second adhesives can be of the same type. However, especially high-performance multi-layer adhesive elements for the highly practical bonding of different substrates are obtained when chemically different adhesives are used, tailored to the specific properties of the various substrates.A multi-layer adhesive element according to the invention is therefore preferred, wherein the first adhesive and the second adhesive are chemically different adhesives, wherein the first adhesive and the second adhesive preferably differ at least with regard to the chemical nature of the adhesive (co-)polymers used and / or the amount of the adhesive (co-)polymers used and / or the chemical nature of the adhesive resins used and / or the amount of the adhesive resins used, preferably at least with regard to the chemical nature of the adhesive (co-)polymers used.
[0052] According to the invention, one or two barrier layers are provided between the adhesive layer(s) and the carrier layer, in particular its foamed plastic layer. Without wishing to be bound by this theory, the inventors assume, based on conducted experiments, that the adverse effect on the adhesive properties observed in multilayer adhesive elements known from the prior art during continued storage at elevated temperatures is at least partially due to the migration of the adhesive resin from the adhesive compound into the carrier layer. This causes the resin content in the adhesive compound to change over time, and consequently no longer corresponds to that intended for the respective application, resulting in the properties of the adhesive compound deviating from the desired specification.The barrier layer provided according to the invention serves to prevent the migration of the adhesive resin from the adhesive compound into the substrate layer, even at elevated temperatures of, for example, 70 °C or higher. This is also the origin of the term "barrier layer" used in the present invention. For the sake of clarity, the temperature of 70 °C, which is particularly relevant in the industry as a test condition, is used here.A multilayer adhesive element according to the invention is therefore preferred, wherein at least one of the adhesive resins, preferably the majority of the adhesive resins relative to the mass of the adhesive resins, and particularly preferably all of the adhesive resins in the first adhesive compound, exhibits a lower diffusion coefficient at 70 °C in the barrier plastic than in the adhesive (co)polymers of the first adhesive compound, and / or wherein at least one of the adhesive resins, preferably the majority of the adhesive resins relative to the mass of the adhesive resins, and particularly preferably all of the adhesive resins in the second adhesive compound, exhibits a lower diffusion coefficient at 70 °C in the barrier plastic than in the adhesive (co)polymers of the second adhesive compound. The diffusion coefficient can, in principle, be determined using any method known and available to those skilled in the art, provided that the same method is used for both measurements in accordance with the principles of good faith.
[0053] A multi-layer adhesive element according to the invention is preferred with regard to adjusting the barrier effect, wherein the multi-layer adhesive element is designed such that the first barrier layer hinders diffusion of the adhesive resins of the first adhesive mass into the carrier layer in such a way that, after 10 days of heat storage at 70 °C, less than 20%, preferably less than 10%, particularly preferably less than 5%, and most preferably less than 1% of the adhesive resins from the first adhesive mass diffuse into the carrier layer, based on the initial mass of the adhesive resins in the first adhesive mass, and / or wherein the multi-layer adhesive element is designed such that the second barrier layer hinders diffusion of the adhesive resins of the second adhesive mass into the carrier layer in such a way that, after 10 days of heat storage at 70 °C, less than 20%, preferably less than 10%, particularly preferably less than 5%, and most preferably less than 1%, diffuses from the adhesive resins of the first adhesive mass into the carrier layer.The adhesive resins from the second adhesive compound diffuse into the carrier layer, relative to the initial mass of the adhesive resins in the second adhesive compound. This characteristic can be easily determined by a person skilled in the art in routine tests by examining the composition of the adhesive compound before and after the corresponding storage, which is possible using standard analytical chemistry methods. In this respect, a person skilled in the art can use any suitable method available to them, since the mass fraction of the adhesive resin is not a measurable quantity that depends on the measurement conditions. The inventors fundamentally aimed for the corresponding barrier layers to achieve the desired barrier effect even at low average thicknesses, which is advantageously possible with the identified barrier plastics. Accordingly, a multilayer adhesive element according to the invention is preferred, wherein the first barrier layer and / or the second barrier layer,The first barrier layer and the second barrier layer preferably have an average thickness in the range of 1 to 30 pm, preferably in the range of 2 to 10 pm.
[0054] Extensive experiments conducted by the inventors have shown that the desired requirements can only be met by very specific materials. Within the scope of the present invention, these materials are referred to as "barrier plastics" in light of their intended use in the barrier layer.
[0055] Based on the inventors' experiments, the desired barrier effect is shown, at least to a sufficient degree, only for copolyamides with a specific glass transition temperature and specific copolyolefins in which at least two specific olefins are reacted with each other to form the copolyolefin.
[0056] Within the scope of the present invention, the glass transition temperature is determined by differential scanning calorimetry (DSC) as described in DIN EN ISO 11357:2023. For this purpose, approximately 5 mg of an untreated polymer sample is weighed into an aluminum crucible (volume 25 pL) and sealed with a perforated lid. A Netzsch DSC 204 F1 is used for the measurement. The instrument is operated under nitrogen for inerting. The sample is first cooled to -150 °C, then heated to +300 °C at a rate of 10 K / min and cooled again to -150 °C. The subsequent second heating cycle, which is crucial for determining the glass transition temperature, is again performed at 10 K / min, and the change in heat capacity is recorded. Glass transitions are identified as steps in the thermogram.Determining the glass transition temperature from DSC measurements is straightforward for a person skilled in the art and is described in more detail, for example, in EP 2832811 A1.
[0057] The first category of suitable barrier plastics are copolyamides, whereby the inventors have found that their suitability for function as a barrier plastic appears to depend significantly on the glass transition temperature. Therefore, a multilayer adhesive element according to the invention is preferred, wherein the barrier plastics are selected from the group consisting of copolyamides with a glass transition temperature, measured by DSC, of 5 °C or more.
[0058] When using suitable copolyamides, a multilayer adhesive element according to the invention is preferred, wherein the glass transition temperature of the copolyamides is 15 °C or more, preferably 20 °C or more.
[0059] In the inventors' experiments, copolyamides combining one or more dicarboxylic acids with one or more diamine compounds proved particularly advantageous, with copolyamides comprising two or more different dicarboxylic acids and two or more different diamine compounds being considered especially advantageous. A multilayer adhesive element according to the invention is therefore preferred, wherein the copolyamides are selected from the group consisting of copolyamides of one or more dicarboxylic acids with one or more diamines, preferably of two or more dicarboxylic acids with two or more diamine compounds.
[0060] In this respect, the inventors have succeeded in identifying preferred embodiments and mass ratios of the compounds for the dicarboxylic acids and the diamines. A preferred embodiment is a multilayer adhesive element according to the invention, wherein the dicarboxylic acids are selected from the group consisting of dicarboxylic acids with 6 to 14 carbon atoms, preferably 8 to 12, carbon atoms, and / or wherein the dicarboxylic acids comprise a dicarboxylic acid A with 6 to 9, preferably 8, carbon atoms and a dicarboxylic acid B with 10 to 14, preferably 12, carbon atoms. A preferred embodiment is additionally or alternatively a multilayer adhesive element according to the invention, wherein the mass ratio of dicarboxylic acids A to dicarboxylic acids B is in the range of 1:20 to 1:1, preferably in the range of 1:15 to 1:5, and particularly preferably in the range of 1:12 to 1:8.Preferably, or alternatively, a multilayer adhesive element according to the invention is used, wherein the diamine compounds are selected from the group consisting of linear aliphatic and cycloaliphatic diamine compounds with 4 to 8 carbon atoms, preferably 4 to 6 carbon atoms, and / or wherein the diamine compounds comprise a linear aliphatic diamine compound C with 5 to 8 carbon atoms and a cycloaliphatic diamine compound D with 4 to 6 carbon atoms. Preferably, or alternatively, a multilayer adhesive element according to the invention is used, wherein the mass ratio of the diamine compounds C to the diamine compounds D is in the range of 1:15 to 1:1, preferably in the range of 1:12 to 1:2, and particularly preferably in the range of 1:8 to 1:3.
[0061] Particularly preferred is a multilayer adhesive element according to the invention which realizes several of these features, i.e., a multilayer adhesive element according to the invention, wherein the copolyamides are selected from the group consisting of copolyamides of two or more dicarboxylic acids with two or more diamine compounds. The dicarboxylic acids comprise a dicarboxylic acid A with 6 to 9, preferably 8, carbon atoms and a dicarboxylic acid B with 10 to 14, preferably 12, carbon atoms. The diamine compounds comprise a linear aliphatic diamine compound C with 5 to 8 carbon atoms and a cycloaliphatic diamine compound D with 4 to 6 carbon atoms.
[0062] Particularly preferred is a multilayer adhesive element according to the invention, wherein the copolyamides are selected from the group consisting of copolyamides of two or more dicarboxylic acids with two or more diamine compounds.
[0063] wherein the dicarboxylic acids comprise a dicarboxylic acid A with 6 to 9, preferably 8, carbon atoms and a dicarboxylic acid B with 10 to 14, preferably 12, carbon atoms, wherein the mass ratio of the dicarboxylic acids A to the dicarboxylic acids B is in the range of 1:20 to 1:1, preferably in the range of 1:15 to 1:5, particularly preferably in the range of 1:12 to 1:8,
[0064] wherein the diamine compounds comprise a linear aliphatic diamine compound C with 5 to 8 carbon atoms and a cycloaliphatic diamine compound D with 4 to 6 carbon atoms, wherein the mass ratio of the diamine compounds C to the diamine compounds D is in the range of 1:15 to 1:1, preferably in the range of 1:12 to 1:2, and particularly preferably in the range of 1:8 to 1:3. In the inventors' experiments, it has been shown that, based on empirical tests, copolyamides identified as particularly suitable not only exhibit a specific glass transition temperature, but also show a specific crystallization temperature in DSC. A multilayer adhesive element according to the invention is therefore preferred, wherein one or more of the copolyamides have a crystallization temperature, determined by DSC, in the range of 40 to 70 °C, preferably in the range of 45 to 65 °C.
[0065] As an alternative to copolyamides, the inventors were able to identify specific copolyolefins suitable for achieving the desired barrier effect in their own experiments. A multilayer adhesive element according to the invention is preferred, wherein one or more barrier polymers are selected from the group consisting of copolyolefins of at least one first olefin with 2 to 5 carbon atoms and at least one second olefin with 6 to 12 carbon atoms.
[0066] The inventors have succeeded in identifying particularly preferred ranges for the olefins used and their mass fractions. A preferred option is a multilayer adhesive element according to the invention, wherein the first olefin has 2 to 4, preferably 2 or 3, particularly preferably 2, carbon atoms. A preferred additional or alternative option is a multilayer adhesive element according to the invention, wherein the second olefin has 6 to 10, preferably 7 or 8, particularly preferably 8, carbon atoms.Preferably, or alternatively, a multilayer adhesive element according to the invention is used, wherein the mass fraction of monomer units of the copolyolefins derived from first olefins is in the range of 60 to 90%, preferably in the range of 65 to 85%, particularly preferably in the range of 70 to 80%, based on the mass of the copolyolefins, and / or wherein the mass fraction of monomer units of the copolyolefins derived from second olefins is in the range of 10 to 40%, preferably in the range of 15 to 35%, particularly preferably in the range of 20 to 30%, based on the mass of the copolyolefins.
[0067] Furthermore, the inventors' experiments have shown that, unlike copolyamides, copolyolefins can exhibit a lower glass transition temperature. A multilayer adhesive element according to the invention is preferred, wherein the copolyolefins have a glass transition temperature, measured by DSC, of -70 °C or more, preferably -65 °C or more, and particularly preferably -60 °C or more. Suitable copolyamides and copolyolefins for use in such multilayer adhesive elements are commercially available from various manufacturers, who offer them for different applications, especially as hot melt adhesives. In light of the above definition, a person skilled in the art can select suitable materials from the portfolios of known polymer suppliers.Furthermore, it can be seen as an advantage of the present invention that the copolyamides and copolyolefins can be produced from relatively basic monomers that are readily available commercially. For their own production, those skilled in the art can rely on established processes for the polymerization of copolyamides and copolyolefins, which are among the most industrially relevant polymerization processes.
[0068] Even though – analogous to the preceding explanations regarding the carrier layer and the adhesive layers – it would theoretically be conceivable for the barrier layers to comprise additional components besides the specific barrier plastics, such as fillers, it is particularly preferable, in view of the manufacturing effort of the corresponding barrier layers and the achievable barrier effect, to form the corresponding barrier layers as largely as possible from the barrier plastics. Accordingly, a multi-layered adhesive element according to the invention is preferred, wherein the first barrier layer and / or the second barrier layer, preferably the first barrier layer and the second barrier layer, consist of barrier plastics to a mass fraction of 70% or more, preferably 90% or more, particularly preferably 95% or more, and most preferably 98% or more, based on the mass of the respective barrier layer.
[0069] The barrier layers to be used according to the invention can advantageously be produced from the barrier plastics in various ways and can potentially, for example, also be obtained in layer form from commercial suppliers. For example, it is possible to produce corresponding barrier layers by extrusion of the barrier plastics, at least up to a thickness of approximately 5 pm. In the inventors' opinion, however, a particularly advantageous manufacturing process for the barrier layers results when the barrier plastics are formed into barrier layers by means of a solvent coating.A multi-layer adhesive element according to the invention is therefore preferred, wherein the first barrier layer and / or the second barrier layer, preferably the first barrier layer and the second barrier layer, are produced or can be produced by forming the barrier plastic(s) in a solvent-based process, preferably by applying a solution or a dispersion of the barrier plastics in a solvent with subsequent removal of the solvent(s).
[0070] In principle, when using double-sided adhesive elements, it is conceivable to use different barrier plastics for the various barrier layers, for example, by using copolyamides in one case and copolyolefins in the other. This can be particularly advantageous when using different adhesive compounds, in which case a person skilled in the art can determine through routine experiments which of the two barrier plastics exhibits the better barrier effect for the intended application. However, especially from the perspective of manufacturing logistics, it is preferable for many embodiments to use the same barrier plastic or the same mixture of barrier plastics for the barrier layers as much as possible.A multi-layer adhesive element according to the invention is therefore preferred, wherein the first barrier layer and the second barrier layer are formed from the same barrier plastics to a mass fraction of 90% or more, preferably 95% or more, particularly preferably 98% or more, and most preferably substantially 100%.
[0071] As disclosed above, the barrier layers can in principle comprise two or more of the specific barrier plastics. This advantageously makes it possible to tailor the physicochemical and mechanical properties of the barrier layer specifically to the respective application requirements. However, with regard to manufacturing effort and material logistics, it is advantageous to form the barrier layers as far as possible from only one barrier plastic. A multilayer adhesive element according to the invention is therefore preferred, wherein the first barrier layer and the second barrier layer consist of a single barrier plastic to a mass fraction of 90% or more, preferably 95% or more, particularly preferably 98% or more, and most preferably substantially 100%.
[0072] The invention also relates to a method for producing a multilayer adhesive element, preferably a multilayer adhesive element according to the invention, comprising the following process steps:
[0073] a) Manufacturing or providing a first barrier layer, wherein the first barrier layer comprises one or more barrier plastics selected from the group consisting of
[0074] iii.i) Copolyamides with a glass transition temperature, measured by DSC, of 5 °C or more, and
[0075] iii.ii) Copolyolefins of at least one first olefin with 2 to 5 carbon atoms and at least one second olefin with 6 to 12 carbon atoms,
[0076] b) Manufacturing or providing a crosslinkable composition,
[0077] c) Application of the crosslinkable composition to the first barrier layer, and
[0078] d) Crosslinking of the crosslinkable composition to form a foamed plastic layer during the formation of a carrier layer.
[0079] The method according to the invention is intended for the production of multilayer adhesive elements and, in particularly preferred embodiments, serves to produce the multilayer adhesive elements according to the invention.
[0080] The above-defined method serves to produce a multilayer adhesive element with one or more adhesive layers. Analogous to the preceding descriptions, it is also preferred for the method according to the invention, for essentially all embodiments, to tailor the method to the production of a double-sided adhesive tape, in which case a second barrier layer is used. Therefore, a method according to the invention is preferred, additionally comprising, prior to process step d), the following process steps:
[0081] e) Manufacturing or providing a second barrier layer, wherein the second barrier layer comprises one or more of the barrier plastics, and
[0082] f) Applying the second barrier layer to the crosslinkable composition applied to the first barrier layer.
[0083] As explained above, the barrier layers can advantageously be produced in a variety of ways. A preferred method according to the invention is one in which the first barrier layer is produced by coating a web-shaped release material using solvent coating or melt coating, and / or in which the second barrier layer is produced by coating a web-shaped release material using solvent coating or melt coating. The focus of the method according to the invention is above on the formation of the foamed plastic layer, in the case of the formation of the support layer on the first barrier layer or between the first barrier layer and the second barrier layer.The corresponding direct formation of the foamed plastic layer is a central element of the inventive method, through which, in particular, an advantageous bond strength between the barrier layers and the foamed plastic layer is achieved, as well as the advantageous reduction of the need for separating liners to be used in the manufacturing process.
[0084] In contrast, the application of the adhesive layers is possible in principle in many ways. For example, it is conceivable that the single-sided or double-sided adhesive layers could be applied after the barrier layer and substrate layer have been created, for instance, by solvent coating or lamination. However, the inventors believe that particularly efficient processes result when the barrier layer and the corresponding adhesive layer are joined together to form a base composite before the final molding.A preferred method according to the invention is therefore one in which the first barrier layer is produced or provided in process step a) as part of a first initial composite comprising the first barrier layer and a first adhesive layer contacting the first barrier layer, wherein the first adhesive layer comprises a first adhesive compound, wherein the first adhesive compound comprises one or more adhesive resins, and / or wherein the second barrier layer is produced or provided in process step e) as part of a second initial composite comprising the second barrier layer and a second adhesive layer contacting the second barrier layer, wherein the second adhesive layer comprises a second adhesive compound, wherein the second adhesive compound comprises one or more adhesive resins.
[0085] Building on the foregoing, this can in principle be achieved by a variety of methods generally known to those skilled in the art, with the production of the adhesive layers by crosslinking a crosslinkable adhesive composition being particularly preferred. A preferred method according to the invention is one in which the first initial composite is produced or provided by crosslinking a first, crosslinkable adhesive composition used in the production of the first adhesive layer and contacting the first barrier layer, wherein the crosslinking is preferably carried out by means of radiation-induced crosslinking, particularly preferably UV-induced crosslinking, and / or wherein the first initial composite is produced or provided by coating the first barrier layer with the first adhesive compound, wherein the coating is preferably carried out by coating with the first adhesive compound from a solvent or by laminating the first adhesive layer.A preferred or alternative method according to the invention is wherein the second starting composite is produced or provided by crosslinking a second, crosslinkable adhesive composition used in the production of the second adhesive layer and contacting the second barrier layer, wherein the crosslinking is preferably carried out by means of radiation-induced crosslinking, particularly preferably UV-induced crosslinking, and / or wherein the second starting composite is produced or provided by coating the second barrier layer with the second adhesive, wherein the coating is preferably carried out by coating with the second adhesive from a solvent or by laminating the second adhesive layer.
[0086] According to the inventive method, a crosslinkable composition is produced or provided. This crosslinkable composition serves to form the foamed plastic layer, which constitutes part or all of the carrier layer, through crosslinking. Although it is conceivable to initiate the crosslinking of the crosslinkable composition in another way, the inventors believe that radiation crosslinking is particularly suitable for producing the desired high-performance foamed plastic layer. A preferred method according to the invention is therefore one in which the crosslinkable composition is a radiation-crosslinkable composition, preferably a UV-radiation-crosslinkable composition. A further or alternative preferred method according to the invention is one in which the crosslinkable composition comprises:
[0087] i) one or more crosslinkable compounds, preferably crosslinkable (meth)acrylate compounds,
[0088] ii) one or more initiator compounds, preferably photoinitiator compounds, and ill) one or more fillers selected from the group consisting of hollow spheres, expandable microballoons and pre-expanded microballoons, preferably expandable microballoons and pre-expanded microballoons.
[0089] A preferred or alternative method according to the invention is a crosslinking of the crosslinkable composition contacting the first barrier layer, preferably the crosslinkable composition contacting the first barrier layer and the second barrier layer, by means of radiation-induced crosslinking, preferably by means of UV radiation-induced crosslinking.
[0090] Particularly in the production of web-shaped adhesive elements, the barrier layer or the corresponding initial composite can be guided on a web-shaped release material, for example a release liner, which makes it possible, for example, to guide it through a production line in which the crosslinkable composition is first applied and then crosslinked to form a foamed plastic layer, for example by passing it past suitable UV LEDs.A preferred method according to the invention is therefore one in which the first barrier layer, preferably the first starting composite, is guided on a first web-shaped release material, preferably a PET liner, at least in process steps a) and b), wherein the first web-shaped release material is preferably provided with a release coating, and / or wherein the second barrier layer, preferably the second starting composite, is guided on a second web-shaped release material, preferably a PET liner, at least in process steps d), wherein the second web-shaped release material is preferably provided with a release coating.
[0091] A preferred method is additionally or alternatively a method according to the invention, wherein the first web-shaped separation material and / or the second web-shaped separation material, preferably the first web-shaped separation material and the second web-shaped separation material, has an average thickness in the range of 30 to 150 pm.
[0092] Furthermore, the use of a barrier layer between an adhesive resin-containing adhesive layer and a foamed carrier layer of a multilayer adhesive element, preferably an adhesive element according to the invention, to improve the storage stability of the multilayer adhesive element at elevated temperatures is disclosed.
[0093] wherein the first barrier layer comprises one or more barrier plastics selected from the group consisting of
[0094] iii.i) Copolyamides with a glass transition temperature, measured by DSC, of 5 °C or more, and
[0095] iii.ii) Copolyolefins of at least one first olefin having 2 to 5 carbon atoms and at least one second olefin having 6 to 12 carbon atoms. Preferred embodiments of the invention are explained and described in more detail below with reference to the accompanying figures. These figures show:
[0096] Fig. 1 shows a schematic cross-sectional view through a multilayer adhesive element according to the invention in a preferred embodiment; and
[0097] Fig. 2 shows a schematic representation of the method according to the invention in a preferred embodiment;
[0098] Fig. 1 shows a (not to scale) schematic cross-sectional view through a multilayer adhesive element 10 according to the invention in a preferred embodiment, which can be produced using the method according to the invention, which is shown in Fig. 2.
[0099] The multilayer adhesive element 10 shown is designed as a double-sided multilayer adhesive element 10 and accordingly comprises a first adhesive layer 12 and a second adhesive layer 20, each having a thickness of approximately 50 pm. In the example shown in Fig. 1, the first adhesive layer 12 and the second adhesive layer 20 each consist essentially entirely of a (meth)acrylate-based pressure-sensitive adhesive compound, which each comprises an adhesive resin, for example, a hydrocarbon resin, an AC resin, rosin, or a terpene phenol resin, wherein the composition of the first adhesive compound and the second adhesive compound differ, since the two adhesive compounds have each been optimized for bonding to different substrates.
[0100] In the example of Fig. 1, a web-shaped release material 26, 28 in the form of a typical PET release liner is arranged on the first adhesive layer 12 and the second adhesive layer 20, which is peeled off before later use.
[0101] The core of the multilayer adhesive element 10 is the carrier layer 14, which in the example shown consists entirely of a foamed plastic layer 16 with a porosity of approximately 30% and a thickness of approximately 1 mm, which can be determined by optical evaluation of a cross-section through the foamed plastic layer 16. The foamed plastic layer 16 is a syntactically foamed plastic layer 16 using expandable microballoons, in which the expanded microballoons are embedded in a poly(meth)acrylate-based plastic. A first barrier layer 18 is arranged between the first adhesive layer 12 and the carrier layer 14, and is materially bonded to both of them. Similarly, the second barrier layer 22, arranged between the second adhesive layer 20 and the carrier layer 14, is also materially bonded to the two adjacent layers in the example shown.
[0102] In the example of Fig. 1, the first barrier layer 18 and the second barrier layer 22 are each essentially made entirely of the same barrier plastic and have a thickness of about 5 pm.
[0103] Particularly high-performance multilayer adhesive elements 10 were achieved by the inventors, for example, using the barrier plastics B1 to B3 listed in Table 1, especially in comparison to an alternative plastic V1.
[0104] Table 1 - Barrier plastics
[0105] (Tg = glass transition temperature, Tc = crystallization temperature)
[0106] No. Material Tg Tc
[0107] / °C / °C
[0108] B1 Commercially available copolyamide, trade name: 28 54
[0109] “Platamid M1276”, from Arkema Aliphatic
[0110] Copolyamide, made from 65% dodecanedioic acid, 7%
[0111] Octanedioic acid, 24% piperazine and 4%
[0112] Hexamethylenediamine
[0113] B2 Commercially available copolyamide, trade name 36
[0114] “Fixatti 803V”, from Fixatti
[0115] B3 Commercially available copolyolefins, trade name: -54
[0116] “Engage 8200”; from Dow; made from copolyolefins
[0117] Made from 75% ethylene and 25% octene.
[0118] V1 Commercially available polyamide, trade name: -4 - “Technomelt 6240”, from Henkel.
[0119]
[0120] The inventors investigated the adhesive strength of multilayer adhesive elements 10, which comprise the aforementioned materials B1 to B3 or V1 in the barrier layers 18, 22, and compared them with an adhesive element that completely dispenses with the use of corresponding barrier layers 18, 22.
[0121] The adhesive strengths were determined analogously to ISO 29862-2019 at 23 °C and 50% relative humidity, with a peel speed of 300 mm / min and a peel angle of 180°. Contrary to the standard, substrates coated with automotive clear coat were used. The multilayer adhesive elements 10 were applied using a roller machine with a rolling pressure of 2 kg. Prior to measurement, the corresponding samples were aged for 10 days at a temperature of 70 °C.
[0122] The results for the aged samples are summarized in Table 2 below.
[0123] Table 2 - Adhesive strength after 10 days of aging at 70 °C
[0124] Barrier layer, adhesive strength, failure pattern
[0125] / (N / cm)
[0126] B1 42 Cohesive failure in
[0127] the support position
[0128] B2 42 Cohesive failure in
[0129] the support position
[0130] B3 42 Cohesive failure in
[0131] the support position
[0132] V1 21 Adhesive failure at
[0133] substrate
[0134] No 21 Adhesive Failures at
[0135] substrate
[0136]
[0137] The advantages of the multilayer adhesive elements 10 with barrier layers B1 to B3 are clearly evident, with the adhesive strengths obtained after aging essentially corresponding to those of the unaged samples and demonstrating that the advantageous adhesive strengths will also be evident after even longer aging and / or after aging at higher temperatures. In contrast, the intermediate layer made of Technomelt 6240 exhibits essentially no barrier effect.
[0138] Fig. 2 shows a schematic representation of a preferred method according to the invention for the production of the multilayer adhesive element 10 of Fig. 1.
[0139] Figure 2 schematically illustrates the introduction of a first output assembly 30 into the system. This assembly comprises the first barrier layer 18, which was previously produced from the barrier plastic, for example, by extrusion or solvent coating. In the output assembly 30, the first barrier layer 18 is already bonded to the first adhesive layer 12, which was, for example, laminated to the first barrier layer 18. To ensure efficient guidance through the system, the first output assembly 30 with the first adhesive layer 12 rests on a first web-shaped release material 26, which acts as a release liner.
[0140] Figure 2 shows how a crosslinkable composition 24 is applied to the first starting composite 30 so that it contacts the first barrier layer 18. In the example shown, the crosslinkable composition 24 comprises crosslinkable (meth)acrylate compounds and suitable photoinitiators to initiate crosslinking after irradiation with UV radiation. Furthermore, the crosslinkable composition 24 in the example shown includes pre-expanded microballoons, which enable the desired syntactic foaming to be achieved.
[0141] After the application of the crosslinkable composition 24, it is covered with a second initial composite 32, which comprises the second adhesive layer 20 and the second barrier layer 22 and is guided on a second web-shaped release material 28 analogously to the first initial composite 30.
[0142] In the resulting layer structure, the crosslinkable composition 24 is then crosslinked using UV radiation sources 34 to obtain the foamed plastic layer 16, thereby producing the multilayer adhesive element 10. Reference numeral list 10 multilayer adhesive element
[0143] 12 first adhesive layer
[0144] 14 Support position
[0145] 16 foamed plastic lay
[0146] 18 first barrier layer
[0147] 20 second adhesive layer
[0148] 22 second barrier layer
[0149] 24 crosslinkable composition
[0150] 26 first web-shaped separation material 28 second web-shaped separation material 30 first initial composite
[0151] 32 second output group
[0152] 34 UV radiation source
Claims
Claims 1. Multilayer adhesive element (10), comprising: i) a first adhesive layer (12), wherein the first adhesive layer (12) comprises a first adhesive compound, the first adhesive compound comprising one or more adhesive resins, ii) a support layer (14), wherein the support layer (14) comprises a foamed plastic layer (16), and ill) a first barrier layer (18) arranged between the first adhesive layer (12) and the carrier layer (14), wherein the first barrier layer (18) comprises one or more barrier plastics selected from the group consisting of iii.i) Copolyamides with a glass transition temperature, measured by DSC, of 5 °C or more, and iii.ii) Copolyolefins of at least one first olefin with 2 to 5 carbon atoms and at least one second olefin with 6 to 12 carbon atoms.
2. Multilayer adhesive element (10) according to claim 1, wherein the multilayer adhesive element (10) further comprises: iv) a second adhesive layer (20), wherein the second adhesive layer (20) comprises a second adhesive compound, the second adhesive compound comprising one or more resins, and v) a second barrier layer (22) arranged between the second adhesive layer (20) and the carrier layer (14), wherein the second barrier layer (22) comprises one or more of the barrier plastics.
3. Multilayer adhesive element (10) according to one of claims 1 or 2, wherein the foamed plastic layer (16) is a syntactically foamed plastic layer, wherein the foamed plastic layer (16) preferably comprises expanded microballoons or hollow spheres, preferably glass hollow spheres. 4.Multilayer adhesive element (10) according to one of claims 1 to 3, wherein the connection between the carrier layer (14) and the first barrier layer (18), preferably between the foamed plastic layer (16) and the first barrier layer (18), can be produced by crosslinking a crosslinkable composition (24) used in the production of the carrier layer (14) and contacting the first barrier layer (18), and / or wherein the connection between the carrier layer (14) and the second barrier layer (22), preferably between the foamed plastic layer (16) and the second barrier layer (22), can be produced by curing a crosslinkable composition (24) used in the production of the carrier layer (14) and contacting the second barrier layer (22).
5. Multilayer adhesive element (10) according to one of claims 1 to 4, wherein the first adhesive and / or the second adhesive, preferably the first adhesive and the second adhesive, consists of one or more adhesive (co)polymers selected from the group consisting of poly(meth)acrylates and synthetic rubbers, preferably poly(meth)acrylates, to a mass fraction of 40% or more, preferably 60% or more.
6. Multilayer adhesive element (10) according to any one of claims 1 to 5, wherein the adhesive resins are selected from the group consisting of non-hydrogenated, partially or fully hydrogenated resins based on rosin or rosin derivatives, terpene phenol resins, resins based on methacylates, hydrogenated polymers of dicyclopentadiene, non-hydrogenated, partially, selectively or fully hydrogenated hydrocarbon resins based on C5, C5 / C9 and C9 monomer streams, and polyterpene resins based on α-pinene and / or β-pinene and / or β-limonene.
7. Multilayer adhesive element (10) according to any one of claims 1 to 6, wherein the first adhesive mass comprises one or more adhesive resins in a combined mass fraction in the range of 1 to 60%, preferably in the range of 5 to 40%, based on the mass of the first adhesive mass, and / or wherein the second adhesive composition comprises one or more adhesive resins in a combined mass fraction in the range of 1 to 60%, preferably in the range of 5 to 40%, based on the mass of the second adhesive composition.
8. Multilayer adhesive element (10) according to any one of claims 1 to 7, wherein the first barrier layer (18) and / or the second barrier layer (22), preferably the first barrier layer (18) and the second barrier layer (22), have an average thickness in the range of 1 to 30 pm, preferably in the range of 2 to 10 pm.
9. Multilayer adhesive element (10) according to any one of claims 1 to 8, wherein the copolyamides are selected from the group consisting of copolyamides of one or more dicarboxylic acids with one or more diamines, preferably of two or more dicarboxylic acids with two or more diamine compounds.
10. Multilayer adhesive element (10) according to claim 9, wherein the dicarboxylic acids are selected from the group consisting of dicarboxylic acids having 6 to 14 carbon atoms, preferably 8 to 12 carbon atoms, comprising and / or wherein the diamine compounds are selected from the group consisting of linear aliphatic and cycloaliphatic diamine compounds with 4 to 8 carbon atoms, preferably 4 to 6 carbon atoms.
11. Multilayer adhesive element (10) according to any one of claims 1 to 10, wherein the first olefin comprises 2 to 4, preferably 2 or 3, particularly preferably 2, carbon atoms, and / or wherein the second olefin comprises 6 to 10, preferably 7 or 8, particularly preferably 8, carbon atoms.
12. Multilayer adhesive element (10) according to any one of claims 1 to 11, wherein the mass fraction of monomer units of the copolyolefins derived from first olefins is in the range of 60 to 90%, preferably in the range of 65 to 85%, particularly preferably in the range of 70 to 80%, based on the mass of the copolyolefins, and / or wherein the mass fraction of monomer units of the copolyolefins derived from second olefins is in the range of 10 to 40%, preferably in the range of 15 to 35%, particularly preferably in the range of 20 to 30%, based on the mass of the copolyolefins.
13. Method for producing a multilayer adhesive element (10), preferably a multilayer adhesive element (10) according to one of claims 1 to 12, comprising the process steps: a) Establishing or providing an initial barrier layer (18), wherein the first barrier layer (18) comprises one or more barrier plastics selected from the group consisting of iii.i) Copolyamides with a glass transition temperature, measured by DSC, of 5 °C or more, and iii.ii) Copolyolefins of at least one first olefin having 2 to 5 carbon atoms and at least one second olefin having 6 to 12 carbon atoms, b) Producing or providing a crosslinkable composition (24), c) Applying the crosslinkable composition (24) to the first barrier layer (18), and d) Crosslinking of the crosslinkable composition (24) to form a foamed plastic would take place (16) in the formation of a support layer (14).
14. The method of claim 13, further comprising, prior to process step d), the following process steps: e) Manufacturing or providing a second barrier layer (22), wherein the second barrier layer (22) comprises one or more of the barrier plastics, and f) Applying the second barrier layer (22) to the crosslinkable composition (24) applied to the first barrier layer (18).
15. Method according to one of claims 13 or 14, wherein the first barrier layer (18) is produced or provided in process step a) as part of a first initial composite (30), comprising the first barrier layer (18) and a first adhesive layer (12) contacting the first barrier layer (18), wherein the first adhesive layer (12) comprises a first adhesive compound, wherein the first adhesive compound comprises one or more adhesive resins, and / or wherein the second barrier layer (22) is produced or provided in process step e) as part of a second initial composite (30), comprising the second barrier layer (22) and a second adhesive layer (20) contacting the second barrier layer (22), wherein the second adhesive layer (20) comprises a second adhesive compound, wherein the second adhesive compound comprises one or more adhesive resins.