Method for steam-assisted dry-gel synthesis of zeolite material on nonwoven substrate
The steam-assisted dry-gel synthesis directly grows zeolite crystals on nonwoven substrates, addressing the inefficiencies of traditional methods by minimizing wastewater and enabling efficient zeolite-coated substrates for gas sorption applications.
Patent Information
- Application Number
- PCT/EP2026/062024
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-05
- Filing Date
- 2026-04-27
- Publication Date
- 2026-11-12
AI Technical Summary
Existing zeolite synthesis methods require pre-formed zeolite powder and binders to adhere to substrates, which is inefficient and generates wastewater.
A method for steam-assisted dry-gel synthesis directly grows zeolite crystals on nonwoven substrates using a precursor mixture, eliminating the need for pre-formed zeolite powder and binders, and allowing for wastewater minimization and recycling.
This method enables the formation of high-bonded zeolite coatings on nonwoven substrates with improved control and reduced wastewater, facilitating the assembly of structured sorption materials for gas sorption.
Smart Images

Figure EP2026062024_12112026_PF_FP_ABST
Abstract
Description
[0001] Method for steam-assisted dry-gel synthesis of zeolite material on nonwoven substrate
[0002] TECHNICAL FIELD
[0003] The present disclosure relates to dry-gel zeolite synthesis, steam-assisted zeolite synthesis, dry-gel coatings, and sorbent materials.
[0004] BACKGROUND ART
[0005] Zeolite synthesis typically involves a hydrothermal process where a mixture of silica, alumina, water, and an alkaline agent is heated under controlled conditions. Initially, a precursor gel is prepared by mixing sources of silica and alumina with water and an alkaline agent. This gel is then typically aged to allow initial nucleation reactions to occur, often improving the efficacy of the synthesis. The aged gel is transferred to an autoclave and undergoes hydrothermal treatment at elevated temperatures, usually between 100-200°C, for several hours to days, promoting the crystallization of the zeolite structure. After the hydrothermal treatment, the mixture is cooled, and the solid zeolite crystals are separated from the liquid by filtration. The crystals are then washed to remove any remaining impurities and dried to obtain the final product. In some cases, the zeolite may undergo additional activation steps, such as calcination, ionexchange, or metal impregnation, to enhance its properties for specific applications. This process results in the formation of zeolites with a highly ordered, porous structure, making them useful for applications in catalysis, adsorption, and ion-exchange. Based on precise control over the synthesis conditions the zeolite properties may be tailored to suit various industrial needs.
[0006] There is a need to provide additional solutions and methods for performing zeolite synthesis, particularly those that facilitate the preparation of uniform coatings on substrates.
[0007] SUMMARY OF THE INVENTIONExisting solutions apply zeolites to surfaces for adsorption / catalysis and utilize a binder to hold the pre-formed zeolite powder to the surface. The inventors have discovered a method for growing zeolite crystals directly on a nonwoven substrate from a zeolite precursor mixture, thus removing the need to utilize pre-formed zeolite powder and binders.
[0008] One object of the invention is to provide an alternative synthesis of zeolite material on nonwoven substrates.
[0009] This has in accordance with the present disclosure been achieved by means of method for steam-assisted dry-gel synthesis of zeolite material on nonwoven substrate. The method comprises
[0010] - preparing a zeolite precursor mixture comprising zeolite precursor, a structuredirecting agent, and water;
[0011] - applying said zeolite precursor mixture onto a nonwoven substrate;
[0012] - evaporating water from said applied zeolite precursor mixture applied onto the nonwoven substrate; and
[0013] - performing steam-assisted hydrothermal treatment of the nonwoven substrate with applied zeolite precursor mixture, whereby the zeolite precursor mixture forms zeolite material on the nonwoven substrate.
[0014] This has the advantage of allowing a dry-gel synthesis of zeolites on a nonwoven substrate with a high amount of bonded zeolite. This further allows wastewater to be minimized and may allow recovery and recycling of any wastewater for the next synthesis.
[0015] In some embodiments, performing the hydrothermal treatment comprises arranging the nonwoven substrate with the applied zeolite precursor mixture in a sealed container in which water is provided separately from the applied zeolite precursor mixture, such that steam generated from said separately provided water causes the zeolite precursor mixture to form the zeolite material on the nonwoven substrate.
[0016] In some embodiments, evaporating water from said applied zeolite precursor mixture comprises forming an evaporated zeolite precursor mixture having a molar ratio between H2O and SiO2 in the range of 1 to 4.In some embodiments, applying said zeolite precursor mixture onto the nonwoven substrate comprises performing wet corrugation and / or preparing for a patterned surface to form.
[0017] In some embodiments, the method comprises pre-treating the nonwoven substrate for applying the zeolite precursor mixture and / or synthesis of zeolite material.
[0018] This has the advantage of allowing improved control of the application of zeolite precursor mixture onto the nonwoven substrate, and the subsequent formation of zeolite material.
[0019] In some embodiments, the method comprises evaporating water from the zeolite precursor mixture prior to applying said zeolite precursor mixture onto the nonwoven substrate, wherein the evaporated zeolite precursor mixture has a viscosity of at least 20 centipoise.
[0020] In some embodiments, the method comprises forming a three-dimensional sorption material from the nonwoven substrate with applied zeolite precursor mixture, and performing hydrothermal treatment of said formed three-dimensional sorption material. This has the advantage of allowing assembly of structured sorption material prior to performing hydrothermal treatment, whereby the steps of assembling the nonwoven substrate with, typically thixotropic, zeolite / binder mixtures are minimized.
[0021] In some embodiments, the method comprises washing the nonwoven substrate with synthesised zeolite material after performing hydrothermal treatment.
[0022] In some embodiments, the method comprises performing calcination of the formed zeolite material by heat treatment.
[0023] In some embodiments, performing hydrothermal treatment comprises measuring the coated nonwoven substrate with the applied zeolite precursor mixture, and controlling at least one parameter of the hydrothermal treatment based on said measurement, wherein said at least one parameter of the hydrothermal treatment comprises temperature, pressure, and / or the duration of at least one part of the hydrothermal treatment.In some embodiments, the zeolite precursor comprises ground silica gel, and / or wherein the structure-directing agent comprises tetrapropylammonium hydroxide, TPAOH.
[0024] The present disclosure further relates to a three-dimensional sorption material for gas sorption, comprising:
[0025] - a nonwoven substrate comprising glass fibres; and
[0026] - zeolite material directly bonded to surfaces of the glass fibres,
[0027] wherein the three-dimensional sorption material comprises a plurality of channels arranged to allow fluid flow through the three-dimensional sorption material, and wherein the zeolite material constitutes at least 40 wt% of the dry weight of the nonwoven substrate with formed zeolite.
[0028] The present disclosure further relates to a rotary sorberfor gas sorption, the rotary sorber comprising
[0029] - the three-dimensional sorption material,
[0030] - a rotary sorber housing arranged to house the three-dimensional sorption material. The present disclosure further relates to a device for removing species from a gas flow, the device comprising
[0031] - the rotary sorber,
[0032] - an actuator arranged to rotate the rotary sorber,
[0033] - a first adsorption zone arranged to guide process gas flow through the rotary sorber, and
[0034] - a first desorption zone arranged to guide regenerating gas flow through the rotary sorber,
[0035] wherein the actuator is arranged to rotate the three-dimensional sorption material of the rotary sorber between the first adsorption zone and the first desorption zone.
[0036] BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Fig. 1a-d schematically shows a device comprising a rotary sorber with sorption material comprising zeolite material.
[0038] Fig. 2 illustrates a flowchart for synthesis of zeolite material on nonwoven substrate.Fig. 3 shows a method for steam-assisted dry-gel synthesis of zeolite material on nonwoven substrate.
[0039] DETAILED DESCRIPTION
[0040] Throughout the figures, same reference numerals refer to same parts, concepts, and / or elements. Consequently, what will be said regarding a reference numeral in one figure applies equally well to the same reference numeral in other figures unless explicitly stated otherwise.
[0041] Terms and expressions
[0042] The term zeolite material relates to the finished material upon performing zeolite synthesis. Herein the term is used both to refer to the material after steam-assisted hydrothermal treatment, both before and after any steps of washing and calcination. The term zeolite precursor relates to a material or compound that serves as the initial building block in the synthesis of zeolites. Zeolite precursors typically comprise the essential elements, such as silicon and aluminium, used in the formation of the zeolite's crystalline structure during the synthesis process.
[0043] The term MFI zeolites relates to a specific framework type of zeolitic molecular sieves, wherein the term MFI stands for Mobil Five, and comprises, e.g., Zeolite Socony Mobil 5 (ZSM-5) and silicalite-1 (S-1) materials.
[0044] The term structure-directing agent, SDA, relates to species arranged to promote formation of a crystalline framework of the zeolite during synthesis. Herein the term is used broadly to include species having an influence on the rate of formation, morphology, and performance properties of the resulting zeolite. Typically, at least one structure-directing agent for zeolite synthesis comprises a cationic salt with a hydroxide anion.
[0045] The term dry-gel relates to a process where the precursor mixture contains significantly less water compared to conventional synthesis methods, such as being a hydrogel.The term nonwoven substrate relates to fabric-like materials made from fibres or filaments that are bonded together by mechanical, chemical, or thermal methods, without being woven or knitted.
[0046] The term steam-assisted hydrothermal treatment of a zeolite precursor mixture relates to exposure to water under autogenous pressures at a controlled temperature to facilitate the crystallization of zeolite material. Typically, hydrothermal treatment further relates to controlling pressure and humidity.
[0047] The term three-dimensional sorption material relates to a multi-part structure comprising substrate material. Typically, three-dimensional sorption material comprises substrate material with formed zeolite material having channels for fluid to flow through said three-dimensional sorption material. Herein, the term three-dimensional sorption material is also used for multi-part structures of substrate material coated with zeolite precursor mixture prior to hydrothermal treatment. Herein “three-dimensional” relates to the structure being more complex than a sheet or strip of sorption material.
[0048] The expression “zeolite material directly bonded to fibres of the nonwoven substrate” relates to zeolite material that is formed on, and adheres to, surfaces of fibres or filaments of the nonwoven substrate without relying on pre-formed zeolite particles being held on the substrate by a dedicated binder. In preferred examples, zeolite crystals are formed directly on exposed fiberglass filaments of the nonwoven substrate.
[0049] The expression “without a dedicated binder” relates to zeolite material being retained on the nonwoven substrate without the need for a separate binder phase intended to hold pre-formed zeolite particles on the substrate. In such embodiments, the zeolite material itself provides the bonding to the nonwoven substrate.
[0050] The expression “dry weight of the nonwoven substrate with formed zeolite” relates to the weight of the nonwoven substrate and the zeolite material after removal of free liquid, such as after drying.
[0051] Fig. 1a-d schematically shows a device comprising a rotary sorberwith sorption material comprising zeolite material. Fig. 1a shows an example device utilizing a rotary sorber. Fig. 1b shows a rotary sorber comprising sorption material. Fig. 1c illustrates across-section of a sorption material. Fig. 1d illustrates the sorption material comprising a substrate covered with zeolite material.
[0052] Fig. 1a shows schematically an example device 100 for removing species from a gas flow 101,102, wherein the device 100 comprises a rotatable rotary sorber 110 comprising three-dimensional sorption material 111. Fig. 1 a shows a process gas flow 101,102, arranged to interact with the three-dimensional sorption material 111 by passing through the rotary sorber 110 in a first volume. A regenerating gas flow 103,104 is arranged to reactivate the three-dimensional sorption material 111 by passing through the rotary sorber 110 in a second volume. In fig. 1a a structure 106 at the rotary sorber 110 is arranged to separate the gas flows going through the first volume and the second volume.
[0053] The device 100 further comprises an actuator 120 arranged to rotate the rotary sorber 110, whereby a part of the three-dimensional sorption material 111 alternates between exposure to the process gas flow 101,102 and to the regenerating gas flow 103,104 in the first and second volumes respectively.
[0054] It is to be understood that the regenerating gas flow 103,104 may be different from the process gas flow 101,102 in one or more properties, such as temperature, pressure, flow rate, humidity, or composition. In some examples, the device 100 is arranged to control the temperature, pressure, humidity, flow rate and / or gas flow composition in the first and / or second volume.
[0055] Fig. 1b shows schematically an example rotary sorber 110 comprising a housing 112 and three-dimensional sorption material 111. The three-dimensional sorption material 111 is arranged to, in an active state, remove species from a gas flow. The rotary sorber 110 may be arranged to be a replaceable component in a device or system for removing species from a gas flow, such as the device shown in fig. 1a.
[0056] Fig. 1 c shows schematically an example three-dimensional sorption material 111. The example sorption material 111 comprises channels for gas flow formed by flat sheets 11 T of sorption material 111 separated by wavy sheets 111” of sorption material 111. In fig. 1c the perspective view is a side-view of the sheets 111’, 111” that looks into said channels for gas flow, which corresponds to the direction of gas flow through said sorption material 111.It is to be understood that the examples shown in fig. 1a-c correspond to established approaches for using sorption materials 111 in order to remove species from a gas flow. The embodiments of the present disclosure may be implemented in examples such as those shown in fig. 1a-c.
[0057] Fig. 1d illustrates a zoomed in view of the example sorption material 111 of fig. 1c. The sorption material 111 comprises a substrate material 210 covered in zeolite material 220. In fig. 1d the two flat sheets are shown as separated from the wavy sheet for readability, whereas they would typically be direct contact and / or attached in a sorption material 111.
[0058] In some examples, the sorption material 111 is formed by coating flat sheets and wavy sheets of substrate material with zeolite material 220, and thereafter assembling said coated sheets together.
[0059] Fig. 2 illustrates an example flowchart for synthesis of zeolite material 220 on nonwoven substrate 210. The flowchart 200 begins with mixing of zeolite precursor 201 and a surface directing agent 202, SDA, with water to forms a zeolite precursor mixture 203.
[0060] The zeolite precursor mixture 203 is applied to the surface of a nonwoven substrate 210. Thereafter, the amount of water in the zeolite precursor mixture 203 is reduced by evaporation.
[0061] Finally, the nonwoven substrate 210 with zeolite precursor mixture 203 undergoes steam-assisted hydrothermal treatment, whereby the zeolite precursor mixture 203 forms zeolite material 220 on the nonwoven substrate 210.
[0062] It is to be understood that additional steps may be added in-between the shown steps and / or after the last step of the example flowchart 200, such as washing or calcination. Fig. 3 shows an example method for steam-assisted dry-gel synthesis of zeolite material on nonwoven substrate. The method 300 comprises
[0063] - preparing 310 a zeolite precursor mixture comprising zeolite precursor, a structuredirecting agent, and water;
[0064] - applying 330 said zeolite precursor mixture onto a nonwoven substrate;
[0065] - evaporating 340 water from said zeolite precursor mixture;- performing 360 steam-assisted hydrothermal treatment of the nonwoven substrate with applied zeolite precursor mixture, whereby the zeolite precursor mixture forms zeolite material on the nonwoven substrate.
[0066] It is to be understood that for the traditional approach the coating that is applied to a substrate comprises pre-formed zeolite particles and binders for binding said zeolite particles to the substrate. In the method of fig. 3 the nonwoven substrate is coated with a zeolite precursor mixture and the zeolite material is instead formed on the substrate. In some examples, preparing 310 the zeolite precursor mixture comprising a zeolite precursor and a structure-directing agent comprises utilizing grinding to form the zeolite precursor mixture. Typically, the step of preparing 310 comprises mixing to form an aqueous solution.
[0067] In some examples, applying 330 said zeolite precursor mixture onto the nonwoven substrate comprises performing 332 wet corrugation and / or preparing for a patterned surface to form. In some examples, performing 332 wet corrugation and / or preparing for a patterned surface to form comprises corrugating at least some nonwoven substrate. In a three-dimensional sorption material, the corrugated nonwoven substrates may correspond to the wavy sheets 111” of sorption material 111 shown in fig. 1c, whereas untreated nonwoven substrates may correspond to the flat sheets 11 T of sorption material 111 in fig. 1c. In some examples, performing 332 wet corrugation comprises corrugating and / or embossing nonwoven substrate that is coated with zeolite precursor mixture.
[0068] In some examples, applying 330 said zeolite precursor mixture onto the nonwoven substrate comprises obtaining corrugated nonwoven substrate with a repeating pattern, such as by embossing the nonwoven substrate. In some examples, said repeating pattern is a smooth sinusoidal wave pattern or a triangular wave pattern. In some of these examples, the repeating pattern has, for a repeating unit such as a wave, a ratio between height and width in the range of 0.1 to 4. In some of these examples, the ratio between height and width is in the range of 0.2 to 2, or in the range of 0.4 to 1.For example, applying 330 said zeolite precursor mixture onto the nonwoven substrate may comprises applying zeolite precursor mixture as a wave pattern with a wave height in the range of 1 to 2.6 mm, with a wave width in the range of 2.5 to 4.2 mm. In some examples, applying 330 said zeolite precursor mixture onto the nonwoven substrate comprises applying zeolite precursor mixture in a repeating pattern of zeolite precursor mixture thickness.
[0069] In some examples, applying 330 said zeolite precursor mixture onto the nonwoven substrate comprises immersing said nonwoven substrate in said zeolite precursor mixture.
[0070] In some examples, applying 330 said zeolite precursor mixture onto the nonwoven substrate comprises applying zeolite precursor mixture by utilizing embossing.
[0071] In some examples, applying 330 said zeolite precursor mixture onto the nonwoven substrate comprises embossing a pattern onto the nonwoven substrate prior to covering the nonwoven substrate with said zeolite precursor mixture.
[0072] In some examples, applying 330 said zeolite precursor mixture onto the nonwoven substrate comprises utilizing a robotic device to coat said nonwoven substrate with zeolite precursor mixture.
[0073] In some examples, applying 330 said zeolite precursor mixture onto a nonwoven substrate comprises applying 50 to 2000 g / m2of zeolite precursor mixture. In some of these examples, applying zeolite precursor mixture in the range of 100 to 1000 g / m2, 200 to 800 g / m2, or 400 to 600 g / m2.
[0074] In some examples, applying 330 said zeolite precursor mixture onto a nonwoven substrate comprises applying a dry weight of 20 to 1000 g / m2of zeolite precursor mixture. In some of these examples, applying zeolite precursor mixture in the dry weight range of 40 to 500 g / m2, 100 to 300 g / m2, or 150 to 200 g / m2.
[0075] In some examples, nonwoven substrate comprises fiberglass paper. In some example, the nonwoven substrate consists of fiberglass paper.
[0076] In a preferred embodiment, 5 g of zeolite precursor mixture is coated onto every 1 g of fiberglass paper.In some examples, applying 330 said zeolite precursor mixture comprises submersing the nonwoven substrate into the zeolite precursor mixture, spray the nonwoven substrate, or pouring the zeolite precursor mixture the nonwoven substrate.
[0077] In some examples, applying 330 said zeolite precursor mixture comprises forming a three-dimensional sorption material (not shown) of the nonwoven substrate, and pouring the precursor mixture over three-dimensional sorption material.
[0078] For nonwoven substrate being flat sheets of fiberglass paper substrate, a preferred technique for applying zeolite precursor mixture is to drag the fiberglass paper through a trough filled with the zeolite precursor mixture. Excess precursor mixture may be removed from a flat nonwoven substrate, after submersion or spraying, using a wiper to scrap off any excess. For a three-dimensional sorption material, such as a honeycomb matrix, the solution is preferably allowed to drain out of the bottom of the channels, which may be assisted by forcing air through the channels to push out excess solution.
[0079] In some examples, the nonwoven substrate has a thickness in the range of 30 to 1000 pm. In some of these examples, the thickness is in the range of 60 to 600 pm, 100 to 300 pm, or 150 to 200 pm.
[0080] In some examples, the nonwoven substrate has a bulk density in the range of 5 to 200 g / m2. In some of these examples, the bulk density is in the range of 10 to 100 g / m2, 20 to 50 g / m2.
[0081] In some examples, the nonwoven substrate has at most 20 wt% of organic content functioning as adhesive binder for the nonwoven substrate. In some of these examples, the organic content functioning as adhesive binder for the nonwoven substrate is at most 15 wt%, or at most 12 wt%. For example, a fiberglass paper may have an organic content of 11%.
[0082] In some examples, the method 300 comprises pre-treating 331 the nonwoven substrate for applying the zeolite precursor mixture and / or synthesis of zeolite material. In some examples, pre-treating 331 the nonwoven substrate comprises coating the nonwoven substrate in colloidal silica. Coating with colloidal silica may improve zeolite binding to the substrate for nonwoven substrates that lack a silica surface. In someexamples, pre-treating 333 the nonwoven substrate comprises cleaning the nonwoven substrate with an organic solvent, whereby impurities are removed.
[0083] In some examples, pre-treating 331 the nonwoven substrate comprises coating the nonwoven substrate with a polymer. In some of these examples, the polymer comprises polyvinyl alcohol (PVA), polyethylene glycol (PEG), polydimethylsiloxane (PDMS), polyacrylic acid (PAA), polyvinylpyrrolidone (PVP), and / or polystyrene (PS). In some examples, evaporating 340 water from said zeolite precursor mixture comprises forming an evaporated zeolite precursor mixture with at most 60 wt% water. In some of these examples, the water content of the evaporated zeolite precursor mixture is at most 55 wt%, at most 50 wt%, at most 45 wt%, at most 40 wt%, at most 30 wt%, or at most 25 wt%.
[0084] In some examples, evaporating 340 water from said zeolite precursor mixture comprises forming an evaporated zeolite precursor mixture with a molar ratio between H2O and SiO2 in the range of 1 to 4. In some of these examples, said molar ratio is between 1.2 and 3, or 1.5 and 2.5. For example, a molar ratio of 2 typically corresponds to about 20 wt% water.
[0085] It is to be understood that the step of evaporating 340 water from said zeolite precursor mixture may be performed while applying 330 said zeolite precursor mixture onto a nonwoven substrate.
[0086] In some examples, performing 360 the hydrothermal treatment comprises arranging the nonwoven substrate with the applied zeolite precursor mixture in a sealed container in which water is provided separately from the applied zeolite precursor mixture, such that steam generated from said separately provided water causes the zeolite precursor mixture to form the zeolite material on the nonwoven substrate.
[0087] In some examples, the method comprises forming 350 a three-dimensional sorption material (not shown) of the nonwoven substrate with applied zeolite precursor mixture, and performing 360 hydrothermal treatment of said formed three-dimensional sorption material. In some of these examples, the formed three-dimensional sorption material comprises channels and / or openings arranged to allow fluid flow through the formed three-dimensional sorption material.In some examples, performing 360 hydrothermal treatment comprises applying a temperature of at least 75°C for at least 24 hours. In some of these examples, the temperature is at least 80°C, at least 90°C, at least 100°C, at least 120°C, at least 125°C, or at least 130°C. In some of these examples, the temperature is at most 200°C. In some of these examples, the duration is at least 2 days, at least 3 days, or at least 5 days. In some of these examples, the duration is at most 14 days.
[0088] In some examples, performing 360 hydrothermal treatment comprises utilizing a sealed container and having an autogenous pressure that is based on the applied temperature.
[0089] In some examples, performing 360 hydrothermal treatment comprises cyclic temperature variations configured to promote formation of zeolite material.
[0090] In some examples, performing 360 hydrothermal treatment comprises using a microwave-assisted hydrothermal process. A microwave-assisted hydrothermal process relates to a hydrothermal process that utilizes microwave radiation to provide heat.
[0091] In some examples, performing 360 hydrothermal treatment comprises utilizing a pressure in the range of 1 to 10 bar, or in the range of 3 to 6 bar.
[0092] In a preferred embodiment, the performing 360 hydrothermal treatment comprises utilizing a sealed container with a small amount of water, such as 0.5 moles of H2O per mole of SiO2, and applying 125°C for 3 days.
[0093] In some examples, performing 360 hydrothermal treatment comprises measuring the coated nonwoven substrate with the applied zeolite precursor mixture and controlling at least one parameter of the hydrothermal treatment based in said measurement. In some of these examples, said at least one parameter of the hydrothermal treatment comprises temperature, pressure, and / or the duration of at least one part of the hydrothermal treatment. In some examples, performing 360 hydrothermal treatment comprises measuring the coated nonwoven substrate during the hydrothermal treatment.
[0094] In some of these examples, measuring the coated nonwoven substrate with the applied zeolite precursor mixture during hydrothermal treatment comprises measuringcrystallinity of formed zeolite material by utilizing X-ray diffraction. Typically, a sample is extracted from setup used for hydrothermal treatment and measured separately. It is to be understood that typically zeolite crystallization is highly repeatable, therefore once hydrothermal treatment conditions that yield a desirable result have been identified, the benefits of measurements during the hydrothermal treatment are greatly diminished.
[0095] In some examples, the zeolite precursor comprises ground silica gel, colloidal silica, tetraethyl orthosilicate, and / or sodium silicate solution.
[0096] It is to be understood that silica colloids are consumed during hydrothermal treatment to form the zeolite material, whereas silica colloids when used as a binder networks already crystallized zeolite powders to hold the zeolite powder onto a substrate. The present disclosure describes a method for directly growing zeolites on a nonwoven substrate, such as fiberglass, without such binders present in the final product.
[0097] In some examples, the zeolite precursor comprises aluminium sulphate, sodium aluminate, pseudoboehmite, alumina, aluminium isopropoxide, and / or aluminium hydroxide.
[0098] In some examples, at least part of the zeolite precursor is provided to the zeolite precursor mixture as a powder. In some of these examples, the zeolite precursor is in powder form.
[0099] In some examples, the structure-directing agent comprises tetrapropylammonium hydroxide (TPAOH), tetramethylammonium hydroxide (TEAOH), tetramethylammonium hydroxide (TMAOH), and / or hexamethyleneimine (HMI). In some of these examples, the structure-directing agent is comprised in an aqueous solution.
[0100] In some example, the structure-directing agent comprises, or is arranged to form, a cationic salt with a hydroxide anion.
[0101] In some examples, the structure-directing agent comprises, or is arranged to form, a cationic salt with a halogen anion, such as a chloride, bromide, or iodide anion.
[0102] In some example, the structure-directing agent is an organic and / or inorganic species.In some examples, the zeolite precursor mixture or the structure-directing agent comprises tripropylamine, dipropylamine, 1,5-diaminopentane, 1,6-diaminohexane, ethylenediamine, morpholine, propanolamine, pentaerythritol, ethanolamine, dipropylenetriamine, methyl quinuclide, dihexamethylenetriamine, triethylenetetramine, diethylenetetramine, glycerol, 1-alkyl-4-azonibicyclo[2,2,2]octane-4-oxide halide, n-propylamine, hexanediol, dibutylamine, and / or isopropylamine.
[0103] In some examples, the zeolite precursor mixture comprises sodium hydroxide, and / or potassium hydroxide, arranged to dissolve the zeolite precursor. In some of these examples, the structure-directing agent comprises sodium hydroxide, and / or potassium hydroxide, wherein the structure-directing agent is arranged to dissolve the zeolite precursor.
[0104] In some examples, the zeolite precursor mixture has a molar ratio between the structure-directing agent and SiO2 in the range of 0 to 2. In some of these examples, said molar ratio is in the range of 0.05 to 1 , in the range of 0.1 to 0.8, and / or in the range of 0.15 to 0.6.
[0105] In some examples, the zeolite precursor mixture has a molar ratio between TPA2O and SiO2 in the range of 0 to 2. In some of these examples, said molar ratio is in the range of 0.02 to 1 , in the range of 0.5 to 0.8, and / or in the range of 0.10 to 0.6.
[0106] In some examples, the zeolite precursor mixture consists of the zeolite precursor, the structure-directing agent, and water. In some of these examples, the zeolite precursor mixture consists of SiO2, TPA2O and water.
[0107] In some examples, preparing 310 a zeolite precursor mixture comprises mixing zeolite precursor, a structure-directing agent, and water results in a molar ratio between water and SiO2 in the range of 3 to 40. In some of these examples, said molar ratio is in the range of 6 to 30, and / or in the range of 10 to 20.
[0108] In a preferred embodiment, the zeolite precursor mixture contains SiO2, SDA2O and H2O in a molar ratio of 1 SiO2, 0.2 SDA2O and 15 H2O.
[0109] For conventional MFI type zeolite synthesis, a synthesis mixture would for example have a molar ratio of 1 SiO2, 0.33 AI2O3, 0.5 Na2O, 0.5 SDA2O, and 80 H2O.It is to be understood that the term SDA2O relates to the structure-directing agent in a form that it may be added to the synthesis mixture.
[0110] In some examples, the zeolite precursor mixture comprises trivalent cations. In some of these examples, the zeolite precursor mixture comprises Al3+, Fe3+, Ga3+, or B3+. In some of these examples, the molar ratio between SiO2 and said trivalent cation(s) is at most 2000, at most 1000, or at most 500.
[0111] In some examples, preformed zeolite powders may be added to the zeolite precursor mixture as seed crystals where the seed zeolite is in the range of 0-20 wt% of the silica content. In some of these examples, said seed zeolite is in the range of 2 to 10 wt%, and / or in the range of 3 to 6 wt%.
[0112] In some examples, the nonwoven substrate comprises a nonwoven fabric. In some of these examples, the nonwoven substrate is a nonwoven fabric.
[0113] In some examples, the nonwoven substrate comprises glass fibres, natural fibres, and / or synthetic fibres.
[0114] In some examples, the nonwoven substrate comprises glass fibres. In some of these examples, the nonwoven substrate consists of glass fibres. In some examples, the nonwoven substrate is and / or comprises fibreglass paper.
[0115] In some examples, the nonwoven substrate is a support material with a fiberglass surface. In some of these examples, the fiberglass surface is a structured fiberglass surface.
[0116] In some examples, the nonwoven substrate comprises glass fibres, polyester, polypropylene, aramid, and / or cellulose-based material.
[0117] In some examples, the nonwoven substrate is electrospun, wetlaid, airlaid, hydroentangled, meltblown, extruded and / or spunbond.
[0118] In a preferred embodiment, the nonwoven substrate is fiberglass paper. The glass fibres have the advantage of the silica surface of the glass becoming etched during the zeolite synthesis, thereby creating nucleation sites to grow the zeolite crystals directly on the exposed fiberglass filaments. For alternatives, such as cellulose fibre paper or a nonwoven polymer paper, such as polyimide, PET, PLA, may require additional pre-Y1
[0119] treatments, like coating in colloidal silica, in order to achieve a similar performance as fiberglass paper.
[0120] It is to be understood that the synthesis of zeolites of the present disclosure is performed without the need for a dedicated binder and / or pH modulation species. In some examples, the synthesis of zeolite material is performed on a nonwoven substrate without the utilization of colloidal binders. In some examples, the formed zeolite precursor mixture contains zeolite precursor, SDA, and water. In some of these examples, zeolite material is synthesized from the zeolite precursor mixture containing zeolite precursor, SDA, and water.
[0121] It is to be understood that conventional coated sorption materials commonly rely on pre-formed zeolite particles and a binder for attaching the particles to a substrate. In contrast, embodiments of the present disclosure provide zeolite material formed on the nonwoven substrate itself, whereby zeolite material is directly bonded to fibres of the nonwoven substrate.
[0122] In some examples, the synthesized zeolite material comprises at least one of the following zeolite structures:
[0123] - Linde Type A, LTA;
[0124] - Linde Type L, LTL;
[0125] - Faujasite, FAU;
[0126] - Zeolite P, GIS;
[0127] - Erionite, ERI;
[0128] - Zeolite Socony Mobil - 12, MTW;
[0129] - Beta, BEA;
[0130] - Ferrierite, FER;
[0131] - Mordenite, MOR; and / or
[0132] - Chabazite, CHA.
[0133] In some examples, performing 360 hydrothermal treatment of the nonwoven substrate with applied zeolite precursor mixture results in a nonwoven substrate with formed zeolite being hydrophobic and being arranged to remove volatile organic compounds, VOCs, in favour of water vapor.In some examples, performing 360 hydrothermal treatment of the nonwoven substrate with applied zeolite precursor mixture results in a nonwoven substrate with formed zeolite having a dry weight of at least 40 wt% zeolite.
[0134] In some examples, three-dimensional sorption material comprises nonwoven substrate with formed zeolite having a dry weight of at least 40 wt% zeolite.
[0135] In some examples, the method 300 comprises evaporating 320 water from the zeolite precursor mixture prior to applying 330 said zeolite precursor mixture onto the nonwoven substrate. In some of these examples, the evaporated zeolite precursor mixture has a viscosity of at least 10 centipoise. In some of these examples, the zeolite precursor mixture has a viscosity of at least 20, at least 40, at least 60, at least 80, or at least 100 centipoise prior to applying 330 said zeolite precursor mixture onto the nonwoven substrate.
[0136] In a preferred embodiment, the evaporated zeolite precursor mixture has a viscosity of 80 centipoise, and after applying evaporated zeolite precursor mixture to the nonwoven substrate, a three-dimensional sorption material is formed from said nonwoven substrate, such as the sorption material 111 shown in fig. 1c.
[0137] Evaporating 320 water from the zeolite precursor mixture prior to applying 330 said zeolite precursor mixture onto the nonwoven substrate allows for the viscosity to match the application technique, and may further allow for more formed zeolite material per unit area of the nonwoven substrate. Additionally, proper viscosity improves the adhesion between substrate sheets by zeolite formation, such as the sorption material 111 shown in Fig. 1d.
[0138] In some examples, the method 300 comprises washing 370 the nonwoven substrate with synthesised zeolite material after performing 360 hydrothermal treatment. In some examples, washing comprises washing with an aqueous solution, such as water. In some examples, washing 370 the nonwoven substrate further comprises drying the nonwoven substrate with synthesised zeolite material.
[0139] In some examples, washing 370 the nonwoven substrate comprises washing with water and / or an organic solvent. Utilizing water may help to remove excess salts.It is to be understood that washing 370 may remove any loose zeolite matter, any excess precursor silica mixture, and / or any excess hydroxide.
[0140] In some examples, washing 370 the nonwoven substrate comprises performing ultrasonic cleaning.
[0141] In some examples, the method 300 comprises performing ion-exchange of the formed zeolite material by washing with or immersing in an aqueous salt solution.
[0142] In some examples, the method 300 comprises metal impregnation of the formed zeolite material by washing with or immersing in a solution of dissolved metal precursors.
[0143] In some examples, the method 300 comprises performing calcination 380 of the formed zeolite material by heat treatment. In some of these examples, calcination 380 comprises heating the nonwoven substrate with synthesised zeolite material to at least 300°C.
[0144] Calcination 380 relates to purging the zeolite material of organic species from the structure directing agents that have become trapped within the pores of the zeolite material.
[0145] In some examples, performing calcination 380 is performed in a controlled atmosphere with specific gas compositions.
[0146] It is to be understood that the steps of washing 370 and performing calcination 380 are performed after the zeolite material has formed and serve as a clean-up of the zeolite material. That is to say, the synthesis of zeolite material occurs while performing 360 hydrothermal treatment.
[0147] In some examples, the method 300 does not utilize an organic structure directing agent, whereby the step of calcination 380 may be omitted from the washing 370 and performing calcination 380 to clean-up the zeolite material.
[0148] Returning to fig. 1a-d and fig 2.
[0149] The invention further relates to a three-dimensional sorption for gas sorption, comprising:
[0150] - a nonwoven substrate comprising glass fibres; and- zeolite material directly bonded to surfaces of the glass fibres,
[0151] wherein the three-dimensional sorption material comprises a plurality of channels arranged to allow fluid flow through the three-dimensional sorption material, and wherein the zeolite material constitutes at least 40 wt% of the dry weight of the nonwoven substrate with formed zeolite.
[0152] In some of these examples, the nonwoven substrate 210 with zeolite material 220 is produced according to the method 300 for steam-assisted dry-gel synthesis of zeolite material on nonwoven substrate.
[0153] In some examples three-dimensional sorption material 111 is arranged to remove volatile organic compounds from air.
[0154] In some examples, the nonwoven substrate is fiberglass paper.
[0155] In some examples, the zeolite material is present without a dedicated binder.
[0156] In some examples, the channels are formed by flat sheets of the nonwoven substrate separated by corrugated sheets of the nonwoven substrate.
[0157] In some examples, the three-dimensional sorption material 111 comprises a plurality of channels, wherein the channels are arranged for fluid and bringing fluid in contact with the zeolite material, such as shown in the example sorption material 111 in fig. 1a-d. In some examples three-dimensional sorption material 111 is a stack comprising sheets of nonwoven substrate 210 with zeolite material 220 produced according to the method 300 for steam-assisted dry-gel synthesis of zeolite material on nonwoven substrate. In some of these examples, the stack is assembled prior to performing hydrothermal treatment of the zeolite precursor mixture. In some of these examples, the stacks are held together by the formed zeolite material. In some of these examples, the stack comprises corrugated sheets of nonwoven substrate 210 with zeolite material.
[0158] The invention further relates to a rotary sorberfor gas sorption, the rotary sorber 110 comprising three-dimensional sorption material 111 and a rotary sorber housing 112 arranged to house the three-dimensional sorption material 111. In some of these examples, the three-dimensional sorption material 111 comprises nonwoven substrate210 with zeolite material 220 produced according to the method 300 for steam-assisted dry-gel synthesis of zeolite material on nonwoven substrate.
[0159] In some examples, rotary sorber 110 for gas sorption is arranged to remove volatile organic compounds from air.
[0160] The invention further relates to a device for removing species from a gas flow, the device 100 comprising
[0161] - said rotary sorber 110 comprising the three-dimensional sorption material 111, - an actuator 120 arranged to rotate the rotary sorber 110,
[0162] - a first adsorption zone arranged to guide process gas flow 101 ,102 through the rotary sorber 110, and
[0163] - a first desorption zone arranged to guide regenerating gas flow 103,104 through the rotary sorber 110,
[0164] wherein the actuator 120 is arranged to rotate the three-dimensional sorption material 111 of the rotary sorber 120 between the first adsorption zone and the first desorption zone.
[0165] In some examples, the device 100 for removing species from a gas flow is arranged to remove volatile organic compounds from air.
[0166] Experimental method examples of conventional approaches and the approach of the present disclosure.
[0167] Conventional method for producing MFI zeolite powder:
[0168] Synthesized from mixtures of a silica source, water, and an organic structure directing agent, oSDA; specifically, tetrapropylammonium hydroxide orTPAOH. Optionally, sodium hydroxide and / or an aluminium source, such as sodium aluminate, aluminium hydroxide, can be added to adjust the ratio of charged species in the precursor mixture.
[0169] Typical molar ratios, per mole of SiO2, in an MFI zeolite precursor mixture may be around 1 SiO2 / 0.005 AI2O3 / 0.1 Na2O / 0.1 TPA2O / 25 H2O.
[0170] This zeolite precursor mixture is then sealed within a PTFE-lined high-pressure autoclave and heated to >140°C for at least 3 days under autogenous pressure.It is to be understood that, for the conventional method, the zeolite precursor mixture forms zeolite particles in solution, and has not been coated on a substrate. The goal of the conventional method is to produce zeolite powder.
[0171] Afterwards, the zeolite powder must be separated from the mother liquor. Mother liquor being the liquid phase that remains after the crystallization of zeolites from the zeolite precursor mixture. This is done by filtering, washing with water, drying, and then being calcined in air to >500°C to remove the oSDA.
[0172] Conventional dry-gel synthesis zeolite production method:
[0173] Dry-gel methods improve upon conventional aqueous synthesis methods by removing the solvent and minimizing the amount of wastewater produced.
[0174] In a dry-gel synthesis, the same zeolite precursor mixture is prepared but the water is removed by evaporation at -80-100°C and then ground into a powder. The dry powder typically contains a water molar ratio less than 2 H2O / 1 SiO2.
[0175] This powder is placed in an autoclave and a small amount of additional water, such as -0.5 moles of H2O per mole of SiO2, is added to the container and kept separate from the dry powder.
[0176] This water is used to generate steam that aides in the crystallization of zeolites from the dry powder. In this way, the container does not need to be high-pressure rated as the amount of water is significantly reduced from a conventional aqueous synthesis. The sealed container is heated to 140°C for at least 3 days, whereby crystalline zeolite powder is formed.
[0177] Afterwards, the formed crystalline zeolite powder is washed with water, dried, and then calcined in air to >500°C to remove the organic structure directing agent, oSDA.
[0178] Example of direct synthesis of silicalite-1 zeolites on fiberglass paper, pure Si-MFI, corresponding to the present disclosure:
[0179] A variation of a dry-gel synthesis method developed to crystallize MFI zeolites directly on fiberglass paper, without the need for colloidal or polymer binders.A pure Si-MFI (silicalite-1) zeolite precursor mixture was prepared by addition of 11 ,0g of finely ground silica gel to 39.0g of a 40wt% aqueous solution of tetrapropylammonium hydroxide, TPAOH; 15.6g of TPAOH and 23.4g of water, resulting in approximately 50g of zeolite precursor mixture with a molar composition of 1 SiO2 / 0.2 TPA2O / 15 H2O.
[0180] The zeolite precursor mixture was then stirred until the silica fully dissolved resulting in a clear solution.
[0181] Water was removed via evaporation at 80°C to produce a thickened solution, with viscosity around 100 centipoise. This moderate temperature drying accomplishes two key factors: obtaining the proper viscosity for wet corrugation and aging the synthesis gel which generates viable nuclei that facilitate zeolite crystallization.
[0182] Fiberglass paper, total weight of ~6g, was then dredged in the zeolite precursor mixture and excess was wiped away to create an even coating.
[0183] The coated paper was then fully dried at 80°C to a final water content of about 2 moles of H2O per mole of SiO2, resulting in about 20 wt% water remaining.
[0184] The dried paper was then suspended above ~2g of water in a PTFE-lined autoclave, sealed, and heated at 140°C for 5 days.
[0185] The products were then washed with water, recovered by filtration, and then dried at 125°C.
[0186] Crystallinity of the zeolite was confirmed by X-ray diffraction.
[0187] Crystalline products were then calcined in air at 550°C to remove the oSDA.
[0188] After calcination, crystallinity of the zeolite may be checked again by measuring X-ray diffraction and vapor sorption capacities for water and 2-propanol isotherms.
[0189] Example of an alternative approach corresponding to the present disclosure. Direct synthesis of ZSM-5 zeolites on fiberglass paper, Al-containing MFI.
[0190] The same direct synthesis dry-gel synthesis procedure as above, except an amount of Al and Na precursors were added to the zeolite precursor mixture as follows:Aluminium containing MFI zeolites, ZSM-5, were prepared by adding 11.4g of finely ground silica gel to 38.5g of a 40wt% aqueous solution of tetrapropylammonium hydroxide, TPAOH, comprising 15.4g of TPAOH and 23.1g of water.
[0191] 1 ,54g of sodium hydroxide was then dissolved in 23.1 g of water.
[0192] 0.075g of aluminium hydroxide AI(OH)s was then added to the solution of sodium hydroxide and stirred until dissolved.
[0193] The aluminium containing solution was then added to the silica containing solution under stirring resulting in approximately 51 ,5g of zeolite precursor mixture with a molar composition of 1 SiC / 0.005 AI2O3 / 0.1 Na2O / 0.2 TPA2O / 15 H2O.
[0194] Stirring the zeolite precursor mixture until homogeneous, resulting in a white, opaque mixture.
[0195] Alternative approach corresponding to the present disclosure. Direct synthesis of faujasite zeolites on fiberglass paper, zeolite Y:
[0196] A similar direct synthesis procedure was followed, but for the synthesis of zeolite Y directly on fiberglass paper.
[0197] Faujasite zeolites, zeolite Y, were prepared by adding 25.6g of finely ground silica gel to 24.4g of a 38wt% aqueous solution of sodium aluminate, comprising NaAICk; 4.78g of AI2O3, 4.59g of Na2O, and 15.1g of water, resulting in approximately 50g of zeolite precursor mixture with a molar composition of 1 SiCk / 0.20 AI2O3 / 0.32 Na2O / 8.4 H2O. The zeolite precursor mixture was then stirred until the silica fully dissolved resulting in a clear solution.
[0198] Water was removed via evaporation at 80°C to produce a thickened solution, resulting in a viscosity around 80 centipoise.
[0199] Fiberglass paper, total weight of ~5g, was then dredged in the zeolite precursor mixture and excess was wiped away to create an even coating.
[0200] The coated paper was then fully dried at 80°C to a final water content of about 2 moles of H2O per mole of SiO2, resulting in about 20 wt% water remaining.The dried paper was then suspended above ~2g of water in a PTFE-lined autoclave, sealed, and heated at 140°C for 72 hours. The products were then washed with water, recovered by filtration, and then dried at 125°C.
[0201] Confirmed crystallinity of the zeolite by X-ray diffraction, and measure vapor sorption capacities by water isotherms.
[0202] Example of forming three-dimensional sorption material for gas sorption - wet corrugation:
[0203] Draw two separate sheets of fiberglass paper through a trough containing the zeolite precursor mixture, Sheet A and Sheet B.
[0204] Wipe of excess synthesis mixture from both sheets.
[0205] Sheet A then goes to the corrugator to form the wavy sheet, corresponding to the wavy sheets 111” of sorption material 111 in fig. 1c. This happens with two toothed corrugated rollers, one on each side, to “pinch” Sheet A into the desired form.
[0206] At the outlet of the corrugator, Sheet A will transition to a single toothed corrugated roller where the waves of Sheet A are still in the teeth of the corrugated roller.
[0207] Sheet B, corresponding to the flat sheets 11 T of sorption material 111 in fig 1c, is then pressed against the exposed portion of Sheet A using a smooth roller to form the final element. This element is comprised of corrugated Sheet A attached to flat Sheet B. The elements are then stacked and pressed together to form a media block with an array of parallel channels / flutes.
[0208] The stacked media block will then be dried, steamed, washed, and dried / calcined again to form the three-dimensional sorption material for gas sorption, corresponding to the sorption material 111 in fig 1c.
[0209] Example of forming three-dimensional sorption material for gas sorption - dry corrugation:A singular element was formed from two separate sheets of nonwoven fiberglass paper, Sheet A and Sheet B, by passing to a corrugator unit. Sheet A undergoes corrugation between two toothed rollers to form the wavy sheet, while Sheet B is kept flat but parallel lines of adhesive are applied to the surface of Sheet B. At the outlet of the toothed roller, Sheet A is pressed in contact with Sheet B such that Sheet A and Sheet B are adhered together. The element comprised of corrugated Sheet A attached to flat Sheet B is then cured to set the adhesive.
[0210] The dry, uncoated elements are then stacked and pressed together using an aluminium housing to form a media block with an array of parallel channels / flutes approximately 100mm x 100mm x 120mm.
[0211] A pure Si-MFI (silicalite-1) zeolite precursor mixture was prepared by addition of 43.8g of finely ground silica gel to 156.2g of a 40wt% aqueous solution of tetrapropylammonium hydroxide, TPAOH; 62.5g of TPAOH and 93.7g of water, resulting in approximately 200g of zeolite precursor mixture with a molar composition of 1 SiO2 / 0.2 TPA2O / 15 H2O.
[0212] The zeolite precursor mixture was then stirred until the silica fully dissolved resulting in a clear solution.
[0213] Water was removed via evaporation at 80°C to produce a thickened solution, with viscosity around 40 centipoise.
[0214] The zeolite precursor mixture was then poured over the uncoated, media block such that the precursor mixture was allowed to flow through and out of the parallel channels. Excess synthesis mixture was removed by forcing air through the channels.
[0215] The coated media block was then fully dried at 80°C to a final water content of about 2.5 moles of H2O per mole of SiO2, resulting in about 25 wt% water remaining.
[0216] The dried block was then suspended above ~15g of water in a stainless-steel autoclave, sealed, and heated at 100°C for 48 hours. The product media block was then washed with water, recovered by filtration, and then dried at 125°C.
[0217] Crystallinity of the zeolite was confirmed by X-ray diffraction and the final dry zeolite content was determined to be about 50 wt%.Crystalline products were then calcined in air at 550°C to remove the oSDA. After calcination, crystallinity of the zeolite was confirmed by measuring X-ray diffraction and vapor sorption capacities for water and 2-propanol isotherms.
Claims
28CLAIMS1. A method for steam-assisted dry-gel synthesis of zeolite material on nonwoven substrate,the method (300) comprising- preparing (310) a zeolite precursor mixture (203) comprising zeolite precursor (201), a structure-directing agent (202), and water;- applying (330) said zeolite precursor mixture (203) onto a nonwoven substrate (210);- evaporating (340) water from said applied zeolite precursor mixture (204) applied onto the nonwoven substrate (210); and- performing (360) steam-assisted hydrothermal treatment of the nonwoven substrate (210) with applied zeolite precursor mixture (203), whereby the zeolite precursor mixture (203) forms zeolite material (220) on the nonwoven substrate (210).
2. The method according to claim 1, wherein performing (360) the hydrothermal treatment comprises arranging the nonwoven substrate with the applied zeolite precursor mixture in a sealed container in which water is provided separately from the applied zeolite precursor mixture, such that steam generated from said separately provided water causes the zeolite precursor mixture to form the zeolite material on the nonwoven substrate.
3. The method according to claim 1 or 2, wherein evaporating (340) water from said applied zeolite precursor mixture (204) comprises forming an evaporated zeolite precursor mixture having a molar ratio between H2O and SiO2 in the range of 1 to 4.
4. The method according to any preceding claim, wherein applying (330) said zeolite precursor mixture onto the nonwoven substrate comprises performing (332) wet corrugation and / or preparing for a patterned surface to form.
5. The method according to any preceding claim, wherein the method (300) comprises pre-treating (331) the nonwoven substrate for applying the zeolite precursor mixture and / or synthesis of zeolite material (220).
6. The method according to any preceding claim, wherein the method (300) comprises evaporating (320) water from the zeolite precursor mixture (204) prior to applying (330) said zeolite precursor mixture onto the nonwoven substrate (210), wherein the evaporated zeolite precursor mixture (204) has a viscosity of at least 20 centipoise.
7. The method according to any preceding claim, wherein the method (300) comprises forming (350) a three-dimensional sorption material from the nonwoven substrate (210) with applied zeolite precursor mixture (204), and performing (360) hydrothermal treatment of said formed three-dimensional sorption material.
8. The method according to any preceding claim, wherein the method (300) comprises washing (370) the nonwoven substrate with synthesised zeolite material (220) after performing (360) hydrothermal treatment.
9. The method according to any preceding claim, wherein the method (300) comprises performing calcination (380) of the formed zeolite material (220) by heat treatment.
10. The method according to any preceding claim, wherein performing (360) hydrothermal treatment comprises measuring the coated nonwoven substrate (210) with the applied zeolite precursor mixture (203), and controlling at least one parameter of the hydrothermal treatment based on said measurement, wherein said at least one parameter of the hydrothermal treatment comprises temperature, pressure, and / or the duration of at least one part of the hydrothermal treatment.
11. The method according to any preceding claim, wherein the zeolite precursor comprises the ground silica gel, and / or wherein the structure-directing agent comprises tetrapropylammonium hydroxide, TPAOH.
12. A three-dimensional sorption material for gas sorption, comprising:- a nonwoven substrate comprising glass fibres; and- zeolite material directly bonded to surfaces of the glass fibres,wherein the three-dimensional sorption material comprises a plurality of channels arranged to allow fluid flow through the three-dimensional sorption material, and wherein the zeolite material constitutes at least 40 wt% of the dry weight of the nonwoven substrate with formed zeolite.
13. A rotary sorber for gas sorption, the rotary sorber (110) comprising- the three-dimensional sorption material (111) according to claim 12,- a rotary sorber housing (112) arranged to house the three-dimensional sorption material (111).
14. A device for removing species from a gas flow, the device (100) comprising- the rotary sorber (110) according to claim 13,- an actuator (120) arranged to rotate the rotary sorber (110),- a first adsorption zone arranged to guide process gas flow (101,102) through the rotary sorber (110), and- a first desorption zone arranged to guide regenerating gas flow (103, 104) through the rotary sorber (110),wherein the actuator (120) is arranged to rotate the three-dimensional sorption material of the rotary sorber (110) between the first adsorption zone and the first desorption zone.
15. The device according to claim 14, wherein the process gas flow (101,102) is an airflow.