Single metal-ceramic substrate and method for dividing a metal-ceramic substrate to produce a single metal-ceramic substrate

The use of localized laser heating to reduce the thickness of metal-ceramic substrates at their outer circumference facilitates automatic and damage-free division, addressing the inefficiencies of traditional cutting methods by ensuring precise and efficient separation.

WO2026233832A1PCT designated stage Publication Date: 2026-11-12ROGERS GERMANY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/062474
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-04-30
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing methods for cutting metal-ceramic substrates often cause damage and require mechanical intervention, leading to inefficiencies and potential defects in the cutting process.

Method used

A metal-ceramic single substrate with a reduced thickness at its outer circumference, achieved through localized heating using laser light, allows for automatic division without mechanical intervention, ensuring fast and reliable singulation.

Benefits of technology

The method enables precise and efficient separation of metal-ceramic substrates with reduced damage, eliminating the need for mechanical breaking and active cooling, thereby improving the quality and speed of the cutting process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026062474_12112026_PF_FP_ABST
    Figure EP2026062474_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A single metal-ceramic substrate (1) for use as a printed circuit board, wherein the single metal-ceramic substrate (1) comprises a ceramic element (20) and a component metallization (20) arranged one above the other in a stacking direction (S), wherein the ceramic element (20) has, at least in sections, in an edge region delimiting the single metal-ceramic substrate (1) in a plane extending perpendicular to the stacking direction (S), a thickness which is reduced relative to the thickness in a central region of the ceramic element (20).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Rogers Germany GmbH MSP Ref: 49669 PT-WO PM / SK

[0002] Metal-ceramic single substrate and method for dividing a metal-ceramic substrate to produce a Meta II ceramic single substrate

[0003] The present invention relates to a metal-ceramic substrate and electronic modules, which are well known from the prior art, for example as power electronics modules. Such electronic modules typically utilize switchable or controllable electronic components that are interconnected via conductor tracks on a common metal-ceramic substrate. Essential components of the metal-ceramic substrate are an insulating layer, which in the case of the metal-ceramic substrate is made of a ceramic-containing material, and a metallization layer, which is preferably structured to form conductor tracks and is formed on one side of the metal-ceramic substrate.

[0004] Typically, a metal-ceramic substrate is produced as a large card, which is then separated into smaller metal-ceramic substrates, i.e., individual metal-ceramic substrates, either before or after structuring. These large cards are processed using laser light to create predetermined breaking lines and / or separation points. The individual metal-ceramic substrates can then be separated from the large card, for example, by manual breaking. The use of ultrashort pulse lasers has proven advantageous in this process, as described, for example, in WO 2017 / 108950 A1.

[0005] Based on this prior art, the present invention aims to improve, in particular simplify, the cutting of metal-ceramic substrates and to reduce any damaging influence on the metal-ceramic substrate during cutting.

[0006] This problem is solved by a metal-ceramic single substrate according to claim 1, and a method according to claim 9. Further embodiments can be found in the dependent claims and the description. 49669 PT-WO PM / SK © According to a first aspect, a metal-ceramic single substrate is provided for use as a printed circuit board, wherein the metal-ceramic single substrate comprises a ceramic element and a component metallization arranged one above the other in the stacking direction, wherein the ceramic element in a peripheral region that limits the metal-ceramic single substrate in a plane perpendicular to the stacking direction has, at least section by section, a thickness that is reduced compared to the thickness in a central region of the ceramic element.

[0007] Compared to previously known metal-ceramic single substrates, this metal-ceramic single substrate is characterized by its reduced thickness at the outer circumference of the ceramic element and thus at the outer circumference of the metal-ceramic single substrate. This thickness reduction of the ceramic element is due to local heating, which was used to automatically divide a large-format metal-ceramic substrate into individual metal-ceramic substrates without mechanical intervention or cooling. It has been shown that a corresponding thickness reduction of the ceramic element occurs with a sufficiently high heat input, particularly using laser light. Simultaneously, it has also been found that the use of high light energy and the correspondingly high heat input enables comparatively fast and reliable singulation.The reduction in outer circumference is therefore a sign of a very fast and process-reliable singulation of the metal-ceramic substrates into individual metal-ceramic substrates, which in turn can then be used as part of a power module.

[0008] It is intended that in an area with reduced thickness (compared to the thickness in the central area), the reduced thickness is essentially constant. By "essentially constant," a person skilled in the art understands in particular that no deviations of more than 15%, preferably more than 10%, and most preferably more than 5% from the mean value occur. Thus, the area with reduced thickness is not a section that could be assigned to a predetermined breaking line, especially a notch-shaped predetermined breaking line. The area with reduced thickness is specifically free of melting and amorphous phases. Melting and amorphous phases are the result of an optically embedded predetermined breaking line, which is not part of the area with reduced thickness.In particular, a stepped transition is formed between the area with reduced thickness and the central area, with an outer surface of the ceramic element in the area with reduced thickness running essentially parallel to the main extension plane. Specifically, it is provided that the area with reduced thickness is free of an inclined outer surface of the ceramic element facing the component metallization. This also serves to delineate predetermined breaking lines or remnants of a predetermined breaking line.

[0009] In this context, the term "edge region" refers in particular to the area formed at the outermost perimeter of the metal-ceramic substrate, extending over up to 5%, preferably up to 2.5%, and most preferably up to 2% of the total surface area of ​​a top and / or bottom surface of the metal-ceramic substrate. It is not essential that the reduced thickness extends over the entire edge region, i.e., over the entire width and area of ​​the edge region. It is also conceivable that the reduced thickness is only present as a portion of this edge region. Alternatively, the thickness reduction extends over the entire edge region.

[0010] Preferably, the edge region is formed by a region on the outermost perimeter of the metal-ceramic single substrate and extends over 2% to 10%, preferably 3% to 7.5% and particularly preferably 3.5% to 5% of the total area of ​​a top and / or bottom surface of the metal-ceramic substrate.

[0011] Preferably, the width of the area with reduced thickness of the ceramic element, measured perpendicular to the stacking direction, is defined as having a value between 5 pm and 20 pm, preferably between 7 pm and 17 pm, and most preferably between 10 pm and 15 pm.

[0012] Furthermore, it is preferably provided that the area of ​​reduced thickness has a thickness reduction compared to the central area of ​​up to 10 pm, preferably up to 8 pm and particularly preferably up to 5 pm.

[0013] In particular, the central area is to be understood as the area that does not belong to the periphery, i.e., lies outside the periphery.

[0014] According to a preferred embodiment, the ceramic element has optical properties in its edge region that differ from those of the ceramic element in its central region. In particular, a color change is observed in the area that was heated, especially with laser light. However, a change in reflectivity can also occur, such that a portion of the edge region, particularly the area treated with light from the second laser source, appears matte compared to the rest of the ceramic element. Thus, correspondingly manufactured metal-ceramic substrates can be identified by their visually detectable properties when heated with light in the area of ​​a predetermined breaking line in the metal-ceramic substrate, in the form of a large card, causing a fracture and subsequent separation.

[0015] Preferably, the metal-ceramic substrate has a sidewall region that bounds the metal-ceramic substrate in a plane parallel to its main extension plane, wherein the sidewall region comprises a first sidewall section running substantially parallel to the stacking direction and a second section running obliquely to the stacking direction. This profile of the sidewall region indicates that a predetermined breaking line, in particular a predetermined breaking line created by means of laser pulses, was initially generated. This line is still visible on the metal-ceramic substrate even after the predetermined breaking, particularly in a cross-sectional view through the metal-ceramic substrate.The outer edge of the metal-ceramic area is therefore angled, or has a corresponding slope, which proves advantageous, for example, because it reduces a sharp edge on the outer circumference of the ceramic element.

[0016] Preferably, the second sidewall section adjoins a surface of the ceramic element opposite the component metallization. Such an arrangement is particularly likely if the predetermined breaking line is located on the side opposite the component metallization and heating occurs, for example, directly at the predetermined breaking line or on the surface of the ceramic element facing the component metallization. However, it is also conceivable that the metal-ceramic substrate has two inclined sidewall sections, each adjoining the surface of the ceramic element, in particular the surface facing the component metallization and the surface facing the back metallization and / or a heat sink element.49669 PT-WO PM / SK © The backside metallization serves, in particular during the manufacturing process, to prevent deflections of the metal-ceramic substrate that would otherwise be caused by thermomechanical stresses. Such thermomechanical stresses result from the different coefficients of thermal expansion for the metal on one side and the ceramic element on the other. This leads to a corresponding thermomechanical stress in the interface area, which is preferably compensated by the thermomechanical stress in the interface area of ​​the backside metallization in order to provide the flattest possible metal-ceramic substrate.

[0017] Preferably, a first extension of the first sidewall section, dimensioned in a direction parallel to the stacking direction, and a second extension of the second sidewall section, also dimensioned parallel to the stacking direction, are provided, wherein the ratio of the first extension to the second extension is between 0.1 and 1, preferably between 0.2 and 0.8, and most preferably between 0.25 and 0.6. It has proven advantageous that, particularly when using high light energy, which leads in particular to a reduction in thickness at the outer circumference of the ceramic element, a correspondingly smaller depth for a predetermined breaking line is also required. Accordingly, less chamfered outer edges, especially second sidewall sections, can be realized in the ceramic element.

[0018] Preferably, an amorphous phase is formed on the ceramic element in a region adjacent to the second side wall section, and this phase is spatially limited along the outer circumference of the ceramic element. Preferably, several amorphous phases are formed on the outer circumference, which are interrupted along a direction that follows the outer circumference of the ceramic element. It has been found that predetermined fracture lines generated with ultrashort pulse lasers are particularly advantageous for fracture. These lasers, in turn, generate amorphous phases along a defined and produced predetermined fracture line, which are interrupted along the direction of the predetermined fracture line, provided the respective pulses have sufficient energy. With such comparatively high-energy pulses, the removal of ceramic material to generate the predetermined fracture line can be achieved particularly quickly.After fracture to separate the metal-ceramic substrates, these amorphous phases are still perceptible on the outer circumference of the ceramic element.49669 PT-WO PM / SK © Preferably, the area of ​​reduced thickness of the ceramic element extends over a width in a direction perpendicular to the stacking direction, with a width-to-thickness ratio of less than 1, preferably less than 0.6, and most preferably less than 0.3. It has been advantageously found that even areas of correspondingly small width, which require heating, are sufficient to produce a successful fracture. This is reflected in the pronounced area of ​​reduced thickness of the ceramic element on the separated metal-ceramic substrate.

[0019] Preferably, the distance between the component metallization and the outer circumference of the metal-ceramic substrate is greater than 150 pm, preferably greater than 220 pm, and particularly preferably greater than 300 pm. Such a dimensioning of the distance proves particularly advantageous because, especially during the breaking process, a sufficient distance between the heat and the metallizations is ensured to prevent the bond between the metal layer and the ceramic element from being stressed when the heat is introduced for breaking.

[0020] Another aspect is a method for singulating a metal-ceramic substrate to produce a single metal-ceramic substrate according to the present invention, comprising

[0021] Providing a metal-ceramic substrate, wherein the metal-ceramic substrate comprises at least a metal layer and a ceramic element,

[0022] - Formation of a predetermined breaking line, in particular by the removal of ceramic material from the ceramic element and

[0023] Local heating of the ceramic element in the area of ​​the predetermined breaking line using laser light.

[0024] All the advantages and properties described for the metal-ceramic single substrate can be applied analogously to the metal-ceramic substrate and the process for producing a metal-ceramic substrate.

[0025] Preferably, the metal-ceramic substrate is divided by exposing it to a temperature between 5°C and 45°C, and in particular without active cooling, and the separation is carried out without mechanical and / or manual intervention on the metal-ceramic substrate.49669 PT-WO PM / SK © In contrast to methods known from the prior art, active cooling, in particular shock cooling after local heating, is deliberately omitted. Specifically, the local heating is carried out in such a way that the metal-ceramic substrates, intended as large cards, are broken or divided without the need for cooling, in particular shock cooling. Furthermore, the breaking occurs without mechanical means or by manual breaking. In this way, the metal-ceramic substrates are divided particularly gently.Surprisingly, it has been found that, particularly by introducing sufficient heat during local heating, it is not necessary to fracture the created predetermined breaking point through targeted, especially active, cooling. This approach proves particularly advantageous because the bond between the metal layer and the ceramic element is subjected to less stress from the strong temperature change. This strong temperature change, otherwise caused by the active cooling required in the prior art methods, is precisely what is avoided. Therefore, it proves to be particularly reliable and gentle to cut the metal-ceramic substrates without cooling in order to divide them into individual metal-ceramic substrates.

[0026] Preferably, for local heating, heat from the laser light is introduced into the ceramic element via a longitudinally extended surface, the longitudinally extended surface preferably running substantially parallel to a predetermined fracture line direction. It is further provided that the laser light follows an oscillating motion for heating and / or that multiple laser light sources are used for heating and / or that the laser light is guided through an optical element for beam shaping. In particular, it is provided that an illuminated area resulting from the local heating by the laser light is not circular, but, for example, has an elliptical cross-section. This is achieved, for example, by moving the laser light back and forth, i.e., in an oscillating motion, along the predetermined fracture line direction, i.e., the direction of travel.An optical (imaging) element for beam cross-section shaping, such as a cylindrical lens, could also be conceivable, shaping the beam in such a way that an elliptical cross-section is formed. In other words, in addition to the relative movement between the substrate and the laser light, an additional, particularly oscillating, movement of the laser light is provided to illuminate and heat a longitudinally extended area locally and for a defined period of time.

[0027] It is also conceivable that a correspondingly elongated area for heating could be achieved using several laser spots positioned side by side and overlapping. This elongation ensures that a sufficiently large area is used for heat input, in order to force the desired fracture. In particular, this approach ensures that a sufficiently large area is illuminated without illuminating the component's metallization, which spatially limits the area available for heating the ceramic element. It is also conceivable that a desired elliptical path could be achieved by appropriately tilting the laser light.

[0028] Preferably, an illuminated area intended for heating is designed such that the surface has a first major axis and a minor second axis measured perpendicular to the major axis, wherein the ratio of the first axis to the second axis is greater than 1.5, preferably greater than 2, and particularly preferably greater than 2.5. This results in a particularly preferably longitudinally extended illuminated area on the ceramic element, which is advantageous for the desired and successful local heating of the ceramic element in the region of the predetermined breaking line.

[0029] Preferably, the laser light used for heating is adjusted such that the heat input is below the melting point of the ceramic element. It is therefore advantageous, on the one hand, to introduce sufficient heat to ensure successful fracture even if the fracture is initiated without further cooling. On the other hand, it should be avoided that the ceramic element or parts thereof melt uncontrollably, thereby impairing its function, in particular its electrical insulation capacity and / or its mechanical strength. It is evident to those skilled in the art that the corresponding energy inputs depend on the ceramic element, and in particular on its absorption behavior, especially as a function of the laser light used.

[0030] Preferably, the material removal from the ceramic element is carried out on a first side of the ceramic element, and the heating of the ceramic element is performed on a second side opposite the first side. This allows for corresponding treatment of opposite sides without the respective treatment steps interfering with each other. Furthermore, precisely the area located below the predetermined fracture line, i.e., the area actually intended to fracture, can be heated. Thus, as much energy as possible is introduced into the area that is actually relevant to the fracture behavior of the ceramic element.

[0031] The described method, which combines the generation of local thermomechanical stress with the generated predetermined fracture lines, proves particularly advantageous because it enables the automatic separation or splitting of the ceramic element. Consequently, manual breaking or breaking caused by mechanical action on the ceramic element can be avoided. This reduces the probability of a defective fracture, as, for example, the possibility of incorrect force application during fracture is eliminated. Furthermore, potential scratches that can be caused by manual or mechanical breaking are avoided. Finally, it also prevents fingerprints or similar marks that might be left on the metal-ceramic substrate, especially on the at least one metal layer, during manual breaking.This is therefore an essentially non-contact process that can be automated and results in the desired division of the metal-ceramic substrate into individual metal-ceramic substrates. A person skilled in the art would preferably not consider clamping the metal-ceramic substrate, particularly for holding it in place, as the application of a mechanical tool, especially since such a clamping tool is primarily intended for holding the large card and / or the metal-ceramic substrate. Such a clamping tool can, for example, be equipped with a vacuum element to act on the large card.

[0032] In particular, it is a metal-ceramic single substrate used as a printed circuit board (PCB) in which a metallization, i.e., a component metallization, is formed on the component side, which, due to its structuring, has several electrically isolated metallization sections. These metallization sections form, for example, connection surfaces or pads or conductive traces of the PCB. 49669 PT-WO PM / SK © Preferably, the ceramic element comprises AI2O3, SisN4, AIN, an HPSX ceramic (i.e., a ceramic with an AI2O3 matrix comprising an x ​​percent proportion of ZrC>2, for example, AI2O3 with 9% ZrCh = HPS9 or AI2O3 with 25% ZrCh = HPS25), SiC, BeO, MgO, high-density MgO (> 90% of the theoretical density), or TSZ (tetragonally stabilized zirconia) as the ceramic material.In particular, the ceramic element has a thermal conductivity greater than 100 W / mK, preferably greater than 120 W / mK, or most preferably greater than 130 W / mK. It is also conceivable that the ceramic element is designed as a composite or hybrid ceramic, in which several ceramic layers, each differing in their material composition, are arranged one above the other and joined together to form an insulating element in order to combine various desired properties.

[0033] Suitable materials for component metallization and / or backside metallization include copper, aluminum, molybdenum, tungsten, and / or their alloys such as CuZr, AlSi, or AlMgSi, as well as laminates such as CuW, CuMo, CuAl, and / or AICu or MMC (metal matrix composite), such as CuW, CuMo, or AlSiC. Preferably, the component metallization is identical to the backside metallization in terms of material or differs from it. Furthermore, it is preferably provided that the component metallization and / or the backside metallization is surface-modified on the manufactured metal-ceramic substrate, particularly as component metallization. Surface modification could include, for example, sealing with a precious metal, especially silver and / or gold, or (electroless) nickel or EN IG (electroless nickel immersion gold), or edge sealing of the metallization to suppress crack formation or propagation.For example, the metal used for the component metallization differs from the metal used for the reverse side metallization.

[0034] The bonding of the metal layer, i.e., the component metallization and / or the backside metallization, to the ceramic element can be achieved, for example, via a DCB process, an AM B process, a diffusion bond, in particular ADB, and / or hot isostatic pressing.

[0035] A "DCB process" (Direct Copper Bond Technology) or a "DAB process" (Direct Aluminum Bond Technology) is understood by those skilled in the art to be a process that serves, for example, to bond metal layers or sheets (e.g., copper sheets or foils or aluminum sheets or foils) to each other and / or to ceramic or ceramic layers, using metal or copper sheets or foils that have a layer or coating (fused-on layer) on their surface sides. In this process, described, for example, in US 3,744,120 A or in DE 2319854 C2, this layer or coating (fused-on layer) forms a eutectic with a melting temperature below that of the metal (e.g.,copper), so that by placing the foil on the ceramic and by heating all layers they can be joined together, namely by melting the metal or copper essentially only in the area of ​​the fusion layer or oxide layer.

[0036] Preferably, the ceramic layer and the metal layer are joined by means of a direct metal bonding process, hot isostatic pressing, a soldering process and / or a diffusion bonding process.

[0037] In particular, the DCB method then includes, for example, the following procedural steps:

[0038] • Oxidizing a copper foil in such a way that a uniform copper oxide layer is formed;

[0039] • Applying the copper foil to the ceramic layer;

[0040] • Heating the composite to a process temperature between approximately 1025 and 1083°C, e.g. to approximately 1071°C;

[0041] • Cool to room temperature.

[0042] An active soldering process, e.g., for joining metal layers or foils, especially copper layers or foils, to ceramic material, is a process specifically used for producing metal-ceramic substrates. At a temperature between approximately 600 and 1000°C, a bond is created between a metal foil, for example, copper foil, and a ceramic substrate, for example, aluminum nitride ceramic, using a hard solder. In addition to a main component such as copper, silver, and / or gold, this hard solder also contains an active metal. This active metal, which is, for example, at least one element (49669 PT-WO PM / SK ©) from the group Hf, Ti, Zr, Nb, Ce, forms a bond between the solder and the ceramic through a chemical reaction. The bond between the solder and the metal is a metallic brazing joint. Alternatively, a thick-film bonding process is also conceivable.Preferably, a separate active metal layer is used for bonding, which is introduced, for example, as a solder system between the ceramic element and the metal layer in addition to a solder base material layer.

[0043] Preferably, an ADB (active diffusion bonding) process is used, which includes, for example, the following steps:

[0044] - Providing a ceramic element and a metal layer,

[0045] - Providing a gas-tight container that encloses the ceramic element, wherein the container is preferably formed from or comprises the metal layer,

[0046] - Formation of the metal-ceramic substrate by bonding the metal layer to the ceramic element using hot isostatic pressing,

[0047] In order to form the metal-ceramic substrate, at least in sections an active metal layer or a contact layer comprising an active metal is arranged between the metal layer and the ceramic element to support the bonding of the metal layer to the ceramic element. The container is preferably formed as a metal container consisting of a metal layer and / or another metal layer. Alternatively, it is also conceivable that a glass container is used.

[0048] In hot isostatic pressing, it is specifically designed that bonding occurs through heating under pressure, ensuring that the metal layer of the metal container, particularly the subsequent metal layer of the metal-ceramic substrate and any eutectic layer present there, does not enter the molten phase. Accordingly, hot isostatic pressing requires lower temperatures than a direct metal bonding process, especially a direct bonding process.

[0049] In contrast to bonding a metal layer to a ceramic layer using a solder material, which typically involves temperatures below the melting point of at least one metal layer, the present method advantageously eliminates the need for a solder base material and requires only an active metal. Furthermore, the use of pressure during hot isostatic pressing proves beneficial because it reduces air inclusions or voids between the metal layer and the ceramic element. This, in turn, reduces or even eliminates the formation of voids in the resulting metal-ceramic substrate. This positively impacts the bond quality between the metal layer of the metal container and the ceramic element.Furthermore, it is advantageously possible to simplify the "second etching" and avoid solder residues and silver migration.

[0050] The active metal layer comprises a comprehensive contact layer of active metal exceeding 15 wt.%.

[0051] Hot isostatic pressing is known, for example, from EP 3080055 B1, the content of which is hereby explicitly referenced with regard to hot isostatic pressing.

[0052] According to a preferred embodiment of the present invention, it is provided that in the manufactured metal-ceramic substrate a bonding layer is formed between the component metallization and the ceramic element, wherein an adhesion promoter layer of the bonding layer has a surface resistance greater than 0.5 ohms / sq, preferably greater than 1 ohm / sq and particularly preferably greater than 2 ohms / sq or even greater than 15 ohms / sq, in particular greater than 20 ohms / sq.

[0053] The surface resistance is directly related to the proportion of active metal in the adhesion promoter layer, which is crucial for bonding the at least one metal layer to the ceramic element. The surface resistance increases with a decreasing proportion of active metal in the bonding layer. A correspondingly high surface resistance therefore corresponds to a low proportion of active metal in the adhesion promoter layer.

[0054] The surface resistance does not depend on a single parameter, but can be influenced by the interplay of several parameters. For example, the purity of the active metal, the thickness of the bonding layer, and / or the surface roughness of the ceramic element also contribute to determining the surface resistance. In particular, high surface resistances can only be achieved through the interaction of at least two parameters.49669 PT-WO PM / SK © It has been found that an increasing proportion of active metal promotes the formation of brittle, intermetallic phases, which in turn is detrimental to the pull-off strength of the metal layer from the insulating layer. In other words, the desired surface resistances describe bonding layers whose pull-off strength is improved, i.e., increased, due to the reduced formation of brittle intermetallic phases.

[0055] A structuring is preferably incorporated into the at least one metal layer prior to the formation of the predetermined breaking line by removing material from the bonded at least one metal layer.

[0056] According to a preferred embodiment of the present invention, the ablation of ceramic materials is achieved using light from a first laser source and / or the local heating of the ceramic element in the region of the predetermined fracture line is achieved using light from a second laser source. It is preferably provided that the first and second light sources differ from one another, particularly with regard to wavelength, intensity, and / or operating mode; i.e., they can be pulsed or continuous wave (CW) radiation. Alternatively, it is conceivable that the first and / or the second laser source are lasers of the same type, but operated, for example, at different wavelengths and / or intensities, perhaps by varying the light cross-section. For example, it is conceivable that the first and / or the second laser source is a YAG, fiber, or CO2 laser.

[0057] The first laser source is preferably an ultrashort pulse laser source, in particular a source that generates pulse durations of less than 100 ns, preferably less than 100 ps, ​​and most preferably less than 1 ps. It has been found that particularly favorable amorphous phases can be generated at the edge of the predetermined breaking point with such ultrashort pulse lasers, which have a positive effect on the fracture behavior and, in particular, prevent undesired fracture behavior and fracture patterns when the individual metal-ceramic substrates break apart. The second laser source, which is used for heating, is in particular a laser source that generates pulses greater than 1 ns or a laser that operates in continuous wave mode. Thus, the first laser source is different from the second laser source, differing in particular with respect to its pulse duration.The pulse length of the second laser source is at least 10 times, preferably at least 50 times, and particularly preferably 70 times greater than the pulse length of the first laser source. This allows sufficient thermal energy to be introduced into the ceramic element with the second laser source to achieve the desired self-refracting effect, while the first light source generates a predetermined fracture line, which, together with the thermal heating, has proven particularly suitable for controlled and therefore process-reliable cutting.

[0058] In particular, the first light source is designed to cause material removal from the ceramic element, especially from its top or outer surface, while the second light source is configured or designed to cause only heating without material removal. It is also conceivable that the second light source is selected to contribute at least a small amount of material removal. For example, it is also conceivable that the first light source is used to at least partially create the predetermined breaking point and also to heat or preheat the ceramic element. Furthermore, it is conceivable that the predetermined breaking point is created using a chemical or mechanical process.

[0059] Preferably, the first laser source is an ultrashort pulse (USP) laser source that provides light pulses with a pulse duration of 0.01 to 800 ps, ​​preferably 1 to 500 ps, ​​and particularly preferably 10 to 50 ps. It has proven particularly advantageous to produce predetermined fracture lines or fracture points using such pulses, especially at processing speeds between 0.2 and 8 m / s. These predetermined fracture lines exhibit a particularly favorable ratio between molten ceramic and crack formation within the fracture lines, thereby ensuring particularly reliable and successful fracturing along the fracture lines without causing damage to the individual metal-ceramic substrate during fracturing.

[0060] Preferably, the area heated by means of the laser light, in particular the second laser source, is smaller than 5 mm. 2 , preferably smaller than 2 mm 2 and especially preferably smaller than 0.7 mm2 Preferably, the area heated by the light is larger than 0.2 mm. 2 , preferably larger than 1 mm 2 and especially preferably larger than 1.5 mm 2.49669 PT-WO PM / SK © Preferably, the removal of ceramic material is carried out on a first side of the ceramic element and the heating of the ceramic element is carried out on a second side opposite the first side, and / or the predetermined breaking line is interrupted or continuous. In the case of opposite processing, particularly when creating the predetermined breaking line on one side and generating the thermomechanical stress on the other side, it is advantageously possible to realize the predetermined breaking line and the separation or cutting process in the ceramic element as simultaneously or in parallel as possible. Alternatively or additionally, it is conceivable that the heating takes place on the same side as the creation of the predetermined breaking line.In this case, a common holding element can be used to create the predetermined breaking line and to subsequently separate the ceramic element by combining heating and cooling it in a locally restricted area.

[0061] Furthermore, the predetermined breaking line can be designed, for example, as a notch or V-shaped feature and / or have varying depths along its direction, and may even be interrupted. For instance, the predetermined breaking line could be a perforation or, alternatively, a continuous notch that defines the desired separation path.

[0062] Furthermore, it is preferably provided that the generation of the predetermined breaking line and / or the heating takes place after structuring the metal-ceramic substrate, i.e., after the at least one metal layer has been structured in such a way that conductor tracks and / or connection surfaces have been generated on the component side.

[0063] Furthermore, it is preferably provided that a predetermined breaking line with a depth of less than 50 pm, preferably less than 20 pm, and particularly preferably less than 15 pm, is created by removing ceramic material. It is also preferably provided that a predetermined breaking line with a depth greater than 1 pm, preferably greater than 4 pm, and particularly preferably greater than 8 pm, is created by removing ceramic material. It has been found that predetermined breaking lines with a shallow depth are necessary or required, meaning that the predetermined breaking lines need not be as deep as those usually created to guarantee a clean break or to improve mechanical stability during subsequent handling. This saves time in the manufacturing process when creating the predetermined breaking line. In addition, it saves the energy required to create the predetermined breaking line.49669 PT-WO PM / SK ©.

[0064] Preferably, a maximum temperature change of more than 1,000 °C / s, preferably more than 10,000 °C / s and particularly preferably more than 50,000 °C / s is achieved during heating. The correspondingly high temperature change allows the desired thermomechanical stresses to be generated in the target area, which cause or result in automatic fracture.

[0065] Preferably, the metal-ceramic substrate is fixed, at least temporarily, and preferably throughout the entire separation or division process, for example, by means of a vacuum. The skilled person defines the entire division process as the process that begins with the creation of the predetermined breaking line and ends with the removal of the individual metal-ceramic substrates. By appropriate fixing and the application of the vacuum, additional stress can also be generated in the metal-ceramic substrate, which leads to the desired fracture or separation being produced automatically.

[0066] Further advantages and features will become apparent from the following description of preferred embodiments of the invention with reference to the accompanying figures. Individual features of the individual embodiments can be combined with one another within the scope of the invention.

[0067] It shows:

[0068] Fig. 1: Schematic representation of a method for singulating metal-ceramic substrates according to a first exemplary embodiment of the present invention,

[0069] Fig. 2: Schematic representation of a method for singulating metal-ceramic substrates according to a second exemplary embodiment of the present invention and

[0070] Fig. 3a, 3b. Sectional views through a metal-ceramic substrate (Fig. 3a) and a metal-ceramic single substrate (Fig. 3b)

[0071] Figure 1 schematically illustrates a method for providing a metal-ceramic single substrate 1, which is separated from a metal-ceramic substrate 1049669 PT-WO PM / SK © provided as a large card, according to a first preferred embodiment of the present invention. Such a metal-ceramic single substrate 1 preferably serves as a carrier for electronic or electrical components that can be bonded to the metal-ceramic single substrate 1. Essential components of such a metal-ceramic single substrate 1 are a ceramic element 20 extending along a principal extension plane HSE and at least one metal layer 21 bonded to the ceramic element 20. The ceramic element 20 is made of at least one material comprising a ceramic.The at least one metal layer 21 and the ceramic element 20 are arranged one above the other along a stacking direction S perpendicular to the principal extension plane HSE and, in a finished state, are at least partially bonded to one another via a bonding surface. Preferably, the at least one metal layer 21 is then structured to form conductive tracks or connection points for the electrical components. For example, this structuring is etched into the at least one metal layer 21. However, a permanent bond, in particular a material-bonded bond, must first be formed between the at least one metal layer 21 and the ceramic element 20.

[0072] To permanently bond the metal layer 21 to the ceramic element 21, a system for producing the metal-ceramic substrate 10, particularly in a DCB or DAB bonding process, comprises a furnace in which a stacked arrangement of the ceramic element 20 and the at least one metal layer 21 is heated, thereby achieving the bond. For example, the at least one metal layer 21 is made of copper, and the at least one metal layer 21 and the ceramic element 20 are joined together using a DCB (Direct Copper Bonding) process. Alternatively, the at least one metal layer 21 can be bonded to the ceramic element 20 using an active soldering process, an ADB (Active Diffusion Bonding) process, hot isostatic pressing, or a thick-film process.

[0073] After bonding, in particular by means of a DCB process, a soldering process, active diffusion bonding, hot isostatic pressing and / or a thick-film process, the metal-ceramic substrate 10 is structured and provided as a large sheet. Such large sheets are to be separated in the subsequent process to provide individual metal-ceramic substrates 1. Preferably, for such separation, the large sheet is processed using laser light from a first laser source, in particular using ultrashort pulse laser light (not shown here).49669 PT-WO PM / SK © It is possible to create a predetermined breaking line 7 along which the large sheet is broken in the subsequent process to form the individual metal-ceramic substrates 1. An ultrashort pulse laser is understood by those skilled in the art to be, in particular, laser sources that emit laser pulses whose pulse lengths are less than one nanosecond.Preferably, the pulse duration is between 0.01 and 100 ps. Furthermore, it is conceivable that the pulse duration is in the femtosecond range, i.e., the pulse length is 0.1 to 100 ps. For example, the metal-ceramic substrate 1 is arranged in a holding element, at least during the production of the predetermined breaking line, and preferably during the entire cutting process.

[0074] It is specifically provided that the metal-ceramic substrate 1 is fixedly arranged by means of the holding element for the production of the predetermined breaking line 7. To create a predetermined breaking line 7 in the metal-ceramic substrate 1, which in particular has a specific course, i.e., along a predetermined breaking line direction, across the metal-ceramic substrate 1, it is provided that the laser light or a laser beam from the first laser source is moved across the metal-ceramic substrate 1. In other words, instead of moving the metal-ceramic substrate 1 relative to the laser light or its orientation, it is preferably provided that the orientation of the laser light or laser beam from the first laser source for forming the predetermined breaking line 7 is such that the laser light moving across the metal-ceramic substrate 1 creates a predetermined breaking line 7 at the respective points of impact.The laser light from the first laser source, passing over the metal-ceramic substrate 1, has a processing speed between 0.1 and 2 m / s, and preferably between 0.8 and 1.5 m / s. Alternatively, it is conceivable that the metal-ceramic substrate 1 is displaced to change the position of the laser light 10 striking the metal-ceramic substrate 1. In particular, the first laser source is designed to effect material removal from the ceramic element 20, for example, by appropriately adjusting the wavelength of the light and / or the light intensity. Alternatively, it is also conceivable that the predetermined breaking line 7 is produced by means of a mechanical or chemical process.

[0075] At the point in time shown in Figure 1 of the process for cutting or processing the metal-ceramic substrate, the predetermined breaking line 7 has already been created. The predetermined breaking line 7 shown in Figure 1 has a V- or notch-shaped form in a sectional view, which runs perpendicular to the principal extension plane HSE and perpendicular to the direction of the predetermined breaking line 7. Furthermore, the predetermined breaking line 7 has a first depth T, which is dimensioned particularly along the stacking direction S. It is conceivable that, in particular, the first depth T is modulated or varied along a predetermined breaking line direction along which the predetermined breaking line 7 extends, or is essentially constant, i.e., deviates by no more than 5%, particularly preferably no more than 2.5%, and particularly preferably no more than 1% from a mean value of the first depth T along the predetermined breaking line direction.For example, it is conceivable that a jagged or wavy course along the direction of the predetermined breaking line is provided for a floor of predetermined breaking line 7.

[0076] In particular, the trench bottom of the predetermined fracture line 7, which is set back from the outer surface of the ceramic element 20, assumes a linear shape and is height-modulated, especially along the predetermined fracture line direction VR. Height modulation is preferably understood by those skilled in the art to mean a deviation of more than 5% of the average depth T from the first depth T averaged along the direction VR. If there are no deviations from the first depth T greater than 5% of the average depth, the depth T is assumed to be essentially constant. For example, the depth T of the predetermined fracture line 7 can also be constant.

[0077] To enable the automation of the cutting of the metal-ceramic substrate 10 into individual metal-ceramic substrates 1, it is provided that the ceramic element 20 is subjected to a targeted local thermomechanical stress in the area where the predetermined breaking line 7 is formed. It has been shown that it is sufficient to selectively introduce heat locally in the area of ​​the predetermined breaking line 7, in particular by means of light from a second laser source. This induces thermomechanical stresses in the ceramic element 20 such that a fracture occurs in the correspondingly treated area of ​​the predetermined breaking line 7, especially along the predetermined breaking line 7. The ceramic element 20 is thereby selectively heated briefly in a spatially limited area.

[0078] It has been found that it is advantageous if a predetermined breaking line 7 already exists to prevent uncontrolled breakage, particularly breakage that does not occur along the desired dividing line. In other words, the predetermined breaking line 7 embedded in the ceramic element 20 specifies the direction along which the automated breakage occurs, which in turn is triggered by the process sequence in which the ceramic element 20 is locally heated. 49669 PT-WO PM / SK © In the embodiment shown in Figure 1, the ceramic element 20 is heated in the area of ​​the predetermined breaking point 7 by means of laser light 15 from a second laser source. It is specifically designed that the second laser source is configured such that it can generate heat input or a temperature increase in the ceramic element 20 in the irradiated area, but does not cause material removal.For example, by appropriately selecting the wavelength and / or intensity, the desired heat input can be achieved without any material removal.

[0079] In the embodiment shown in Figure 1, the laser light 15 from the second laser source is directed towards the side of the ceramic element 20 opposite the predetermined breaking point 7. Alternatively, it is conceivable that the light 15 from the second laser source is directed towards the same side of the ceramic element 20, particularly in the areas where the predetermined breaking point 7 is also embedded. Furthermore, it is preferred that the heating takes place in a locally confined sub-area of ​​the ceramic element 20 in which the predetermined breaking point 7 is located and / or which is sufficiently far removed from the at least one metal layer 21 of the metal-ceramic substrate 10.

[0080] For example, it is provided that a distance A between the light 15, in particular a laser beam, and the at least one metal layer 21 is at least 200 pm. This advantageously prevents the thermomechanical stress generated in the region of the predetermined breaking line 7 from impairing or even damaging the bond between the at least one metal layer 21 and the ceramic element 20 in the metal-ceramic substrate 10.

[0081] Furthermore, it is provided that the first depth T of the predetermined breaking line 7 is reduced compared to those required to effect purely manual division of the metal-ceramic substrate 10 into the individual metal-ceramic substrates 1. For example, the first depth T or the mean depth of the predetermined breaking line 7 is less than 130 pm, preferably less than 100 pm, and particularly preferably less than 70 pm. Preferably, the ratio of a first depth T or a mean depth to the thickness of the ceramic element 20 is less than 50%, preferably less than 30%, and particularly preferably less than 20% of the thickness of the ceramic element 30.

[0082] The automatic separation of the ceramic element 20 reduces cycle time and the likelihood of uneven breakage due to inconsistent force application during manual breaking is advantageously reduced. Specifically, it is intended that the automatically separated metal-ceramic substrates 10 are removed from the holding element, and in particular, that they are automatically removed and packaged. This eliminates the need to manually break and package the individual metal-ceramic substrates 1. This also prevents fingerprints that would otherwise be unintentionally generated on the individual metal-ceramic substrates 1.

[0083] Figure 2 shows a metal-ceramic substrate 10 in the form of a large card according to a second exemplary embodiment of the present invention. In particular, the metal-ceramic substrate 10, designed as a large card, comprises several individual metal-ceramic substrates 1, each separated from the others by predetermined breaking lines 7. The individual metal-ceramic substrates 1 are enclosed or surrounded by a frame element 4, which is formed as a closed perimeter around the outermost circumference of the large card or the metal-ceramic substrate 1. The frame element 4 is also separated from the individual metal-ceramic substrates 1 by a predetermined breaking line 7. The top view shown in Figure 2 is directed towards the side of the metal-ceramic substrate 10 on which the predetermined breaking lines 7 have already been created. As in Figure 1, a state is shown in which the predetermined breaking lines 7 have already been created.In particular, the predetermined breaking lines 7 exhibit amorphous phases that do not form continuously along the predetermined breaking line 7, but rather are uninterrupted. Specifically, these phases are statistically distributed across the large map, i.e., not distributed according to a recurring pattern across the large map or the metal-ceramic substrate. Furthermore, the lengths of the continuous amorphous phases also differ from one another. In addition, an elongated surface 30 is included in Figure 2, which is illuminated by light from the second laser source in this snapshot of the figure. Heat is introduced here. The ceramic element 20 is heated locally in the region of the predetermined breaking line 7. During the heating process, the elongated surface 30 migrates along the predetermined breaking line 7, specifically along the direction of the predetermined breaking line.The longitudinally extended surface 30, which in particular has an elliptical cross-section, serves the purpose of introducing thermal energy into the ceramic element 20 in order to generate thermomechanical stresses that cause spontaneous fracture of the ceramic element 20, i.e., without mechanical or manual intervention, without the introduction of an active cooling element. A correspondingly longitudinally extended surface 30, which is illuminated, can be realized, for example, by an oscillating, i.e., back-and-forth movement of the laser spot. An alternative possibility for realizing the longitudinally extended surface 30 is the use of several superimposed laser spots. It has been found that the longitudinally extended surface 30 makes it possible to introduce sufficient thermal energy to achieve targeted heating without the need for active cooling of the Meta II ceramic substrate 1.This longitudinally extended surface can also be realized, for example, by an arrangement of lenses forming an optical element. The optical element is inserted into the light beam path and, due to its imaging properties, changes the shape of the light cross-section. For pulsed applications, components are preferably used that can correct the pulse duration if necessary.

[0084] The longitudinal extent of the surface 30 results in particular from the fact that the lateral extent of the area to be heated is limited by the position of the metal sections 21, from which the laser light is spaced, or rather, that its illumination does not lead to heating of the ceramic element 20. Therefore, a corresponding elliptical shape is advantageous in order to introduce sufficient heat into the ceramic element 20. Preferably, the longitudinally extended surface 30 is extended along a direction that runs essentially parallel to the predetermined breaking line direction. In particular, the longitudinally extended surface 30 has a first axis and a second axis perpendicular to the first axis, wherein the ratio of the second axis to the first axis is less than 0.5, preferably less than 0.3, and preferably less than 0.2. This results in a particularly elliptical or, more precisely, rectangular shape of the longitudinally extended direction.The first axis preferably runs parallel to the longitudinal extent of the predetermined breaking line 7, i.e., the predetermined breaking line direction. Furthermore, the representation of this large map includes a so-called chamfer. This refers to corner areas, in particular rhombus- or quadrilateral intermediate areas between several adjacent corners of metal-ceramic individual substrates 1. These necessitate an angled predetermined breaking line direction, especially in the area where corner points of the metal-ceramic individual substrates abut each other. In the embodiment shown here, the corner direction in the form of a chamfer 17 results in a change in the predetermined breaking line direction of 30°–70°, particularly 45°, compared to the predetermined breaking line direction along the longitudinal edges of the metal-ceramic individual substrates 1.It has been found that a corresponding chamfer 17 is advantageous for the fracture behavior and can also be used as a stop for further processing of the metal-ceramic single substrate 1.49669 PT-WO PM / SK © Preferably, the predetermined fracture line 7, which has a first depth T particularly outside the corner areas of the metal-ceramic single substrates 1, has a second depth in the fiber area that is greater than the first depth T, especially because these areas are prone to uncontrolled and undirected breaking, while the other predetermined fracture lines 7 located outside the corner areas can provide a certain stability with the first depth, which allows for safe and stable transport of the metal-ceramic substrates 10 in the form of large cards.Furthermore, the predetermined breaking line 7 between the frame element 4 and the individual metal-ceramic substrates 1 has a second and / or third depth, which is also greater than the first depth T. This allows the frame element 4 to be advantageously removed first, and only then, with the correspondingly advantageous spatial freedom, the individual metal-ceramic substrates 1 to be further broken. It is conceivable that at least at the frame element 4, mechanical breaking is further supported, since imprints from tools and / or fingers are irrelevant for subsequent processes.

[0085] Preferably, at least two predetermined breaking lines 7, in particular opposing predetermined breaking lines 7, extend to the outermost edge of the large card to delineate the frame element 4. This avoids the probability of errors when separating the frame element 4. Preferably, only two predetermined breaking lines 7 are provided, extending continuously across the entire large card.

[0086] Figure 3a shows a cross-sectional view through the metal-ceramic substrate 1 in the form of a large map. It is evident to those skilled in the art that, after fracture, the individual metal-ceramic substrates 1 in Figure 3a exhibit a profile in the cross-sectional view that corresponds to half of the layer view shown here, in particular up to the dividing line indicated below the predetermined fracture line 7. In Figure 3a, a predetermined fracture line 7 is formed with an amorphous phase 2. In particular, an amorphous phase 2 forms as a deposit on the upper surface of the ceramic element 20. As already mentioned in connection with Figure 2, this phase is distributed across the individual predetermined fracture line profiles or along the respective predetermined fracture line directions when ultrashort pulse lasers are used. Such amorphous phases 2 occur particularly when light pulses with high light energy are used.If lower-energy light pulses are used, the initial depth of the predetermined fracture line 7 must be increased to enable successful and reliable fracturing without active cooling.49669 PT-WO PM / SK © Figure 3b shows a sectional view where a second light source 12 was used during heating. This light source's energy is significantly above the threshold that leads to ablation of the ceramic element 20 or a physical change in its surface texture. Consequently, a stepped profile is visible on the top surface of the ceramic element 20 and on the side of the ceramic element 20 facing the secondary light source 12. This is due to the corresponding erosion of the ceramic element 20 by the light from the secondary light source.Additionally, it is conceivable that the laser light causes a modification to the upper surface of the ceramic element 20, which faces the secondary light source during processing. Such a change, particularly an optical change, could be, for example, a color change or a matting. This allows the identification, even after the predetermined fracture, of those metal-ceramic substrates 1 that were subjected to the corresponding cutting process, as they are clearly attributable to the use of a heating second laser light 12, which has resulted in the form of a recess in the edge region, i.e., a step-like progression of the ceramic element 20 at the edge region and / or a discoloration or optical modification of the ceramic element 20 in the edge region.

[0087] In particular, Figure 3b shows a side wall region SB that bounds the metal-ceramic single substrate 1 at its outer circumference. This side wall region SB has a first side wall section S1 and a second side wall section S2, which are arranged one above the other when viewed in the stacking direction S. The second side wall section S2 runs essentially parallel to the stacking direction S, while the first side wall section S1 runs obliquely to the stacking direction S. The first side wall section S1 is the result of a predetermined breaking line 7 introduced into the ceramic element 20 and is still recognizable on the manufactured, i.e., divided, metal-ceramic single substrate 1. Furthermore, a region 4 with reduced thickness and, in particular, with optically altered properties extends over a width extending from the outer circumference.This width B is preferably in such a ratio to the thickness D of the ceramic element 20 that this ratio takes on a value that is less than 1, preferably 0.75 and particularly preferably less than 0.55.

[0088] 1 metal-ceramic single substrate

[0089] 2 amorphous phase4 frame element

[0090] 6 Area with reduced thickness 7 Break line

[0091] 10 Metal-ceramic substrate 12 Second laser source

[0092] 15 lights

[0093] 17th phase

[0094] 20 ceramic elements

[0095] 21 Metal layer

[0096] 30 area

[0097] T first depth

[0098] HSE Main Extension Plane S Stacking Direction

[0099] SB side wall area

[0100] 51 first side wall section 52 second side wall section B width

[0101] A distance

[0102] Thickness

Claims

49669 PT-WO PM / SK © Claims 1. Metal-ceramic single substrate (1) for use as a printed circuit board, wherein the metal-ceramic single substrate (1) comprises a ceramic element (20) and a component metallization a, which are arranged one above the other in the stacking direction (S), wherein the ceramic element (20) has, at least in sections, a thickness that is reduced compared to the thickness in a central area of ​​the ceramic element (20) in a peripheral region which limits the metal-ceramic single substrate (1) in a plane perpendicular to the stacking direction (S).

2. Metal-ceramic single substrate according to claim 1, wherein the ceramic element (20) has optical properties in the edge region that differ from those that the ceramic element (20) has in the central region.

3. Metal-ceramic single substrate (1) according to one of the preceding claims, wherein in a region with reduced thickness the reduced thickness is substantially constant.

4. Metal-ceramic single substrate (1) according to one of the preceding claims, wherein the area with reduced thickness is free from an obliquely oriented outer surface of the ceramic element (20) which faces the component metallization.

5. Metal-ceramic single substrate (1) according to one of the preceding claims, wherein the edge region is formed by a region on the outermost outer circumference of the metal-ceramic single substrate (1) and extends over 2% to 10%, preferably 3% to 7.5% and particularly preferably 3.5% to 5% of the total area of ​​a top and / or bottom surface of the metal-ceramic single substrate (1).

6. Metal-ceramic single substrate (1) according to one of the preceding claims, wherein the metal-ceramic single substrate (1) has a side wall region (SB) that limits the metal-ceramic single substrate (1) in a plane parallel to the main extension plane (HSE) of the metal-ceramic single substrate (S), wherein the side wall region (SB) has a first side wall section (S1) extending substantially parallel to the stacking direction (S) and a second side section (S2) extending obliquely to the stacking direction (S).

7. Metal-ceramic single substrate (1) according to one of the preceding claims, wherein the second side wall section (S2) adjoins a surface side of the ceramic element (20) that is opposite the component metallization (21).

8. Metal-ceramic single substrate (1) according to one of the preceding claims, wherein a first extension of the first side wall section (S1) dimensioned in a direction parallel to the stacking direction (S) and a second extension of the second side wall section (S2) dimensioned in a direction parallel to the stacking direction (S) is provided, wherein a ratio of the first extension to the second extension is a ratio between 0.1 and 1, preferably between 0.2 and 0.8 and particularly preferably between 0.25 and 0.

6.

9. Metal-ceramic single substrate (1) according to one of the preceding claims, wherein an amorphous phase (2) is formed on the ceramic element (20) in an area adjacent to the second side wall section (S2), which is spatially limited along an outer circumference of the ceramic element (20).

10. Metal-ceramic single substrate (1) according to one of the preceding claims, wherein the area of ​​the ceramic element (20) with reduced thickness extends in a direction perpendicular to the stacking direction (S) over a width (B), wherein the ratio of the width to the thickness of the ceramic element (20) assumes a value that is less than 1, preferably less than 0.6 and particularly preferably less than 0.3 .

11. Metal-ceramic single substrate (1) according to one of the preceding claims, wherein a distance (A) of the component metallization (21) to the outer circumference of the metal-ceramic single substrate is greater than 40 pm, preferably greater than 60 pm and particularly preferably greater than 70 pm. 49669 PT-WO PM / SK © 12. Method for singulating a metal-ceramic substrate for producing a metal-ceramic single substrate according to one of the preceding claims, comprising - Providing a metal-ceramic substrate (10) wherein the metal-ceramic substrate (10) comprises at least a metal layer (21) and a ceramic element (20), - Forming a target book line (7), in particular by removing ceramic material from the ceramic element (20) and - local heating of the ceramic element (20) in the area of ​​the predetermined breaking line (7) using laser light (15).

13. Method according to claim 12, wherein the metal-ceramic substrate (10) is separated by exposing it to a temperature between 5 °C and 45 °C and in particular without active cooling, and wherein the separation is carried out without mechanical and / or manual action on the metal-ceramic substrate (10).

14. Method according to claim 12 or 13, wherein for local heating a heat input of the laser light (15) is introduced into the ceramic element (20) via a longitudinally extended surface, wherein the longitudinally extended surface preferably runs substantially parallel to a predetermined fracture line direction and wherein the laser light (15) follows an oscillating movement sequence for heating and / or several laser light sources are used for heating and / or laser light (15) is guided through an optical element for beam shaping.

15. Method according to one of claims 12 to 14, wherein the removal of ceramic materials is carried out using light from a first laser source and / or the local heating of the ceramic element in the region of the predetermined breaking line is carried out using light from a second laser source.