Hot-melt self-adhesive composition

A self-adhesive hot melt composition using styrenic block copolymers and natural tackifying resins addresses co-extrusion issues in multilayer packaging, ensuring strong adhesion and seal integrity for resealable films, suitable for chilled or frozen food packaging.

WO2026233836A1PCT designated stage Publication Date: 2026-11-12BOSTIK SA(FR)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/062484
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-05
Filing Date
2026-04-30
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing multilayer packaging materials face challenges in co-extrusion due to the mismatch in melt flow indices of hot melt pressure sensitive adhesives (HMPSA) and thermoplastic polymers like polyolefins, leading to non-uniform appearance and poor adhesion properties, especially when subjected to repeated opening and closing cycles or low temperatures.

Method used

A self-adhesive hot melt composition comprising styrenic block copolymers and naturally derived tackifying resins with controlled melt flow index and glass transition temperature, allowing co-extrusion with polyolefins while maintaining good adhesion and seal integrity.

Benefits of technology

The composition ensures a uniform, resealable film with strong adhesion and seal integrity, even under freezing conditions, without toxic effects on users or the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000029_0001_TABLE
    Figure IMGF000029_0001_TABLE
  • Figure IMGF000030_0001_TABLE
    Figure IMGF000030_0001_TABLE
  • Figure IMGF000030_0002_TABLE
    Figure IMGF000030_0002_TABLE
Patent Text Reader

Abstract

The invention relates to a hot-melt self-adhesive composition comprising: - at least one mixture M of styrenic block copolymers, said mixture comprising, on the basis of its total weight; - from 5% to 100% by weight of at least one triblock copolymer; and - from 0% to 95% by weight of at least one diblock copolymer; said mixture having a melt flow index of less than or equal to 20 g / 10 min and preferably less than or equal to 18 g / 10 min (200°C, 5 kg) - at least one tackifying resin of natural origin having a Gardner color of less than or equal to 1.5, said composition having a melt flow index of less than or equal to 60 g / 10 min (190°C, 2.16 kg) and being characterized by a total polystyrene content of between 5% and 15% by weight relative to the total weight of said composition.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Self-adhesive hot melt composition

[0002] Scope of the invention

[0003] The present invention relates to a self-adhesive hot melt composition, a multilayer structure, a manufacturing process and the use of the multilayer structure, as well as a resealable package.

[0004] Technical background

[0005] Multilayer (or laminated) products are used in many fields for packaging a wide variety of goods, particularly in the food, cosmetics, and detergent industries. Depending on the requirements, these products can be flexible or rigid. Flexible packaging is a common example. These products are generally made of different materials (composite multilayer products). Materials can include paper, metal, or thermoplastic polymers.

[0006] The characteristics and properties of multilayer articles will depend, in particular, on the materials used to create the layers. Thus, it is common to combine layers made of different materials to obtain multilayer articles, most often composite multilayer articles, which combine the characteristics and properties of the different individual layers and therefore have specific characteristics and properties.

[0007] Among multi-layered products are resealable packages used in the food industry and retail for packaging food, particularly fresh produce. These packages typically consist of a container (or receptacle) and a lid (or sealing film) that are hermetically sealed together by heat sealing. After the lid is opened and some of the food in the receptacle is consumed, the user can reposition the lid on the receptacle to essentially re-seal the package, thus preserving the remaining portion of the product. Repeated opening and resealing is also possible.

[0008] The container for these packages typically consists of a thermoformed plastic sheet with a flat base on which the food product rests and a flat, band-shaped rim. This rim, usually parallel to the base, is heat-sealed to the lid, which is made of a multi-layered film. When the consumer opens the package, the lidding film is manually separated from the container at the flat band around its rim. This exposes the adhesive layer that was originally part of the lidding film.

[0009] A simple manual press then allows the packaging to be resealed, once the lid has been repositioned on the receptacle in accordance with its position in the packaging before opening.

[0010] In most resealable packaging available on the market, the lidding film is a multilayer structure that includes a layer comprising a self-adhesive hot melt adhesive (or HMPSA for "Hot Melt Pressure Sensitive Adhesive") bonding a complexable layer and a heat-sealable layer.

[0011] The HMPSA composition typically comprises one or more tackifying resins and one or more styrenic block copolymers. Applied in a molten state, it solidifies upon cooling, forming an adhesive layer that ensures the bonding of the complexable and heat-sealable layers.

[0012] The complexable layer can be complexed with other layers to produce the lidding film, for example with a rigid layer to improve the mechanical strength of said film.

[0013] The heat-sealable layer allows the lidding film to be sealed onto the receptacle by heat sealing.

[0014] The laminating and heat-sealable layers can be based on thermoplastic polymers such as polyolefins like polyethylene and / or polypropylene. These polymers have a low melt flow index (MFI), while HMPSA compositions generally have a high MFI. Because of these differences, it is difficult to co-extrude these different materials (particularly by bubble blowing) to obtain a lidding film with a uniform appearance.

[0015] However, a very low MFI for the HMPSA composition implies very cohesive properties, which are in opposition to the adhesive properties needed to obtain a resealable lidding film.

[0016] The present invention aims to provide a self-adhesive, heat-fusible composition that can be co-extruded (for example, by bubble blowing), particularly with a polyolefin such as polyethylene and / or polypropylene, while maintaining good adhesion properties, so that the lidding film using said composition can withstand several opening / closing cycles while maintaining a good seal. Furthermore, the present invention aims to provide a self-adhesive, heat-fusible composition that ensures a good seal even when resealable packages are placed in a freezer.

[0017] It is also desirable that the self-adhesive hot melt composition according to the invention is not toxic to either the user or the environment.

[0018] Summary of the invention

[0019] The present invention relates to a self-adhesive, hot-melt composition comprising:

[0020] - at least one mixture M of styrenic block copolymers, said mixture comprising, on the basis of its total weight;

[0021] - from 5% to 100% by weight of at least one triblock copolymer; and - from 0% to 95% by weight of at least one diblock copolymer;

[0022] said mixture having a hot melt flow index MFR less than or equal to 20 g / 10min and preferably less than or equal to 18 g / 10min (200°C, 5kg),

[0023] - at least one tackifying resin of natural origin having a Gardner color less than or equal to 1.5,

[0024] said composition having a hot melt index MFI less than or equal to 60 g / 10 min (190°C, 2.16kg) and being characterized by a total polystyrene content of between 5 and 15% by weight relative to the total weight of said composition.

[0025] In one embodiment, at least one mixture M of styrenic block copolymers comprises, on the basis of its total weight, 10 to 60% by weight of at least one triblock copolymer and 40 to 90% by weight of at least one diblock copolymer.

[0026] In embodiments, the composition according to the invention has a glass transition temperature less than or equal to 4°C, preferably less than or equal to 0°C.

[0027] In some embodiments, the content of mixture M in the composition ranges from 50% by weight to 75% by weight relative to the total weight of the composition, and in a preferred embodiment, the content of mixture M ranges from 52% to 73% by weight relative to the total weight of the composition.

[0028] In preferred embodiments, the triblock copolymer is a styrene-isoprene-styrene (SIS) triblock copolymer and the diblock copolymer is a styrene-isoprene (SI) diblock copolymer. In some embodiments, the weight ratio "m" of the mixture M relative to the total weight of the composition is given by the relation (ax MFR + b)% < m < 75%, where:

[0029] MFR is the hot fluidity index of mixture M (200°C, 5kg); a is between 1 and 1.35 preferably between 1.1 and 1.3, for example between 1.15 and 1.25 or 1.2;

[0030] b is between 50 and 60, preferably between 52 and 55.

[0031] Preferably, the ratio "m" is defined by the relation such that (1.11 x MFR + 52)% < m < 75%, for example by the relation (1.2 x MFR + 55)% < m < 75%.

[0032] In some embodiments, at least one tackifying resin of natural origin is chosen from:

[0033] - natural and modified rosins, such as gum rosin, wood rosin, tall oil rosin, distilled rosin, hydrogenated rosin, dimerized rosin, polymerized rosin,

[0034] - natural and modified rosin esters, including glycerol and pentaerythritol esters such as glycerol esters of pale wood rosin, glycerol esters of polymerized rosin, pentaerythritol esters of pale wood rosin, pentaerythritol esters of tall oil rosin, phenolically modified pentaerythritol esters of rosin, and

[0035] their mixtures.

[0036] In embodiments, the total content of at least one tackifying resin in the composition according to the invention is between 25% by weight and 50% by weight relative to the total weight of the composition, and preferably between 27% and 48%.

[0037] In some embodiments, the composition according to the invention further comprises one or more additives.

[0038] Preferably, the composition according to the invention does not include a plasticizer.

[0039] In some embodiments, the naturally sourced tackifying resin has a Gardner color less than or equal to 1, for example less than or equal to 0.5 or equal to 0.

[0040] In embodiments, the composition according to the invention has a Gardner color less than or equal to 2, preferably less than or equal to 1.5, more preferably less than or equal to 1, for example less than or equal to 0.5 or equal to 0. In embodiments, the composition is obtained in the form of granules, with dimensions between 1mm and 10mm.

[0041] In some embodiments, said granules are coated with an anti-caking agent such as talc, wax, silica, kaolin, allowing to obtain individually separated granules.

[0042] In some embodiments, the granules are spherical or ovoid in shape.

[0043] Another object of the invention relates to a multilayer structure comprising:

[0044] an adhesive layer consisting of the self-adhesive, hot-melt composition according to the invention,

[0045] a heat-sealable layer, and

[0046] a complexifiable layer,

[0047] in which the adhesive layer is located between the heat-sealable layer and the complexable layer.

[0048] Another object of the invention relates to a method of manufacturing the multilayer structure according to the invention by lamination or by coextrusion, in particular by coextrusion by bubble blowing.

[0049] The invention further relates to a resealable package comprising the multilayer structure according to the invention.

[0050] The invention also relates to the use of the multilayer structure according to the invention for the manufacture of a resealable package, preferably for food, in particular for chilled or frozen food.

[0051] Description of the invention

[0052] Unless otherwise stated, in this description, percentages by weight are relative to the total weight of the composition and the standards mentioned throughout the application are those in force at the date of filing the application.

[0053] Self-adhesive hot melt composition

[0054] The term "hot melt" is used in this text to indicate that the composition is solid at room temperature (e.g., between 18°C ​​and 25°C) and needs to be heated to melt before being applied to a substrate. Mixture M

[0055] The composition according to the invention comprises a mixture M of styrenic block copolymers comprising at least one triblock copolymer and optionally at least one diblock copolymer. "Styrenic block copolymers" means block copolymers comprising at least one polystyrene block (whether wholly or partly block, such as gradient copolymers, preferably entirely block). The styrenic block copolymers may be linear or branched (e.g., star, brush, or comb), preferably linear.

[0056] Advantageously, mixture M comprises between 5% and 100% by weight of at least one triblock copolymer and between 0% and 95% by weight of at least one diblock copolymer relative to the total weight of mixture M, preferably between 10% and 85% by weight of at least one triblock copolymer and between 15% and 90% by weight of at least one diblock copolymer.

[0057] Within the framework of the invention, the ranges of values ​​are understood to include the limits. For example, the range "between 0% and 25%" includes, in particular, the values ​​0% and 25%.

[0058] Preferably, the triblock copolymer is a styrene-isoprene-styrene (SIS) triblock copolymer. Preferably, the diblock copolymer is a styrene-isoprene (SI) diblock copolymer.

[0059] The styrenic block copolymers of mixture M can have a number-average molar mass between 50,000 g / mol and 600,000 g / mol. The number-average molar mass can be determined by size-exclusion chromatography, particularly with polystyrene standards.

[0060] Preferably, the mixture M consists solely of styrene-isoprene-styrene and styrene-isoprene block copolymers, and does not include other styrenic block copolymers (in particular those having at least one ethylene, propylene, butylene or butadiene block).

[0061] Mixture M has a melt flow index (MFR) less than or equal to 20 g / 10 min (200°C, 5kg), and preferably less than or equal to 18 g / 10 min (200°C, 5kg).

[0062] MFR can, for example, be measured according to the ASTM D-1238 standard (specifically procedure A).

[0063] Styrenic block copolymers suitable for implementing the invention include, for example, the JH9520 copolymer from Ningbo Jinhai Chenguang Chemical Corporation, the Quintac 3520 copolymer from Zeon, the EL9520 copolymer from Hexas, the D1111KT copolymer from Kraton, the YH4023 copolymer from Sinopec, the Vector 4116ND copolymer from TSRC, the D1113PT copolymer from Kraton, the JH8161 copolymer from JinHai, and the YH1126 copolymer from Sinopec. The content of mixture M in the composition according to the invention may be between 50% by weight and 75% by weight relative to the total weight of the composition, preferably between 52% by weight and 73% by weight relative to the total weight of the composition.

[0064] Tackifying resin

[0065] The composition according to the invention comprises at least one tackifying resin of natural origin, which may be selected from:

[0066] - natural and modified rosins, such as gum rosin, wood rosin, tall oil rosin, distilled rosin, hydrogenated rosin, dimerized rosin, polymerized rosin,

[0067] - natural and modified rosin esters, including glycerol and pentaerythritol esters such as glycerol esters of pale wood rosin, glycerol esters of polymerized rosin, pentaerythritol esters of pale wood rosin, pentaerythritol esters of tall oil rosin, phenolically modified pentaerythritol esters of rosin, and

[0068] - their mixtures.

[0069] Preferably, the tackifying resin of natural origin is derived from pine wood. Ideally, the tackifying resin is certified for food contact.

[0070] Naturally derived tackifying resins can have a softening temperature of at least 80°C, preferably between 80°C and 150°C, and more preferably between 90°C and 140°C. The softening temperature can be measured by a ball and ring method, for example according to ASTM E28.

[0071] The weight-average molecular weight of the tackifying resin can vary between 200 g / mol and 5000 g / mol, preferably between 300 g / mol and 3000 g / mol. The weight-average molecular weight can be measured by size-exclusion chromatography, particularly with polystyrene standards.

[0072] The naturally occurring tackifying resin may have a viscosity of at least 180 mPa.s, preferably at least 220 mPa.s, at 177°C as measured according to ASTM D2196. Such a viscosity of the tackifying resin contributes to giving the composition its hot flow index.

[0073] The total content of at least one naturally derived tackifying resin in the composition according to the invention may be between 25% and 50% by weight relative to the total weight of the composition, preferably between 27% and 48% by weight. Preferably, the naturally derived tackifying resin has a Gardner color value of 1.5 or less, preferably 1 or less, for example, 0.5 or 0 or less. The Gardner color may be measured according to ISO 6271-2 (Part 2) or ISO 4630, preferably ISO 4630. Thus, the final color of the composition according to the invention is less pronounced than compositions incorporating a petroleum-derived tackifying resin such as C5 or O9 type resins.In particular, the composition according to the invention may have a Gardner color less than or equal to 2, preferably less than or equal to 1.5, more preferably less than or equal to 1, for example less than or equal to 0.5 or equal to 0. The final packaging thus does not have any particular mark or color indicating the presence of the composition according to the invention.

[0074] Such tackifying resins have a low odor, thus preventing or limiting the odor of the composition according to the invention and the associated volatile compounds from interacting with the initial odor of the product, particularly food products. Furthermore, the tackifying resins included in the composition according to the invention have little or no taste, which prevents a pronounced flavor transfer to food when the composition according to the invention is used on food packaging.

[0075] Tackifying resins suitable for implementing the invention include, for example, Sylvalite 9100 resins from Kraton.

[0076] Additives

[0077] The composition according to the invention may further comprise one or more additives, for example selected from fillers, ultraviolet stabilizers (or antioxidants), additional polymers other than styrenic block copolymers, rheological agents, core-bark type impact modifiers, pigments, and mixtures thereof.

[0078] The total content of additives in the composition according to the invention can be up to 10% by weight relative to the total weight of the composition.

[0079] The filler can be chosen from organic fillers, mineral fillers, and mixtures thereof.

[0080] As an example of mineral fillers, one can cite any mineral filler commonly used in the field of adhesive compositions. These fillers typically come in the form of particles of various geometries. They can be, for example, spherical, fibrous, or have an irregular shape. The mineral filler can be chosen from clays (such as talc), quartz, carbonate fillers (notably calcium carbonate, which can be coated with fatty acids (the latter preferably being precipitated), kaolins, gypsum, silica, hollow mineral microspheres (notably hollow glass microspheres, such as those made of sodium and calcium borosilicate or aluminosilicate), zeolites, and mixtures thereof.

[0081] The mineral feed can be untreated or treated, for example with an organic acid including stearic acid.

[0082] The average particle size of the mineral charge can range from 10 nm to 400 pm, preferably from 20 nm to 100 pm, more preferably from 30 nm to 10 pm.

[0083] In this text and unless otherwise indicated, the average particle size advantageously corresponds to the d50 particle size, i.e. the maximum size of 50% of the smallest particles by volume, and can be measured with a particle size analyzer, in particular by laser diffraction, for example on a MALVERN type device (for example according to ISO 13320).

[0084] As an example of an organic filler, one can cite any organic filler, especially polymeric, commonly used in the field of adhesive compositions.

[0085] The organic filler can be selected from polyvinyl chloride (PVC), polyolefins, ethylene vinyl acetate (EVA), expandable or non-expandable thermoplastic polymer hollow microspheres (such as vinylidene chloride / acrylonitrile hollow microspheres), aramid fibers (such as Kevlar®), and mixtures thereof.

[0086] The average particle size of the organic load may be less than or equal to 15 pm, preferably between 5 and 15 pm.

[0087] The filler content can be up to 10% by weight relative to the total weight of the composition according to the invention, preferably up to 5% by weight.

[0088] Ultraviolet (UV) stabilizers are typically introduced to prevent degradation resulting from a reaction with oxygen that can form under the influence of heat or light. UV stabilizers may include antioxidants capable of scavenging free radicals.

[0089] The UV stabilizer (or antioxidant) can be chosen from among benzotriazoles, benzophenones, phosphites (such as tris(2,4-di-tert-butylphenyl)phosphite, tris-(p-nonylphenyl)phosphite), so-called hindered phenols (such as ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], 2,2'-methylenebis(6-(tert-butyl)-4-methylphenol), 2,2'-methylenebis(6-(tert-butyl)-4-ethylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-methylenebis(4,6-di(tert-butyl)phenol), 4,4'-methylenebis(2,6-di(tert-butyl)phenol, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,6-di(tert-butyl)-4-methylphenol), so-called sterically hindered amines (such as bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate (CAS No: 41556-26-7), methyl 1,2,2,6,6-pentamethyl-4-piperidyl sebacate (CAS No: 82919-37-7), 4,4'-bis(α,α-dimethylbenzyl)diphenylamine),and their mixtures.

[0090] The UV stabilizer (or antioxidant) content can be up to 5% by weight relative to the total weight of the composition according to the invention, preferably up to 3% by weight.

[0091] Additional polymers other than styrenic block copolymers include, for example, polyolefins (including polyethylene, polypropylene, polyisobutylene, polybutadiene, etc., functionalized or not), ethylene-vinyl acetate copolymers, acrylic copolymers (functionalized or not) and / or acrylic block copolymers.

[0092] By "acrylic block copolymer" is meant a block copolymer comprising at least one acrylic block, that is to say, comprising at least one block consisting of a polymer obtained from at least one acrylic monomer. By "acrylic monomer" is meant in particular a monomer comprising a group of formula -X-(C=O)-C(R')=CH2, in which R' represents a hydrogen atom or a methyl radical, and -X- represents -O- or -NR"- with R" representing a hydrogen atom or an alkyl radical (cyclic, linear or branched) comprising from 1 to 22 carbon atoms, preferably from 1 to 14, more preferably from 1 to 8. Preferably, -X- represents -O-.

[0093] The content of additional polymers can be up to 5% by weight relative to the total weight of the composition according to the invention.

[0094] The rheological agent can be chosen from among thixotropic agents, for example from:

[0095] fumed silica (hydrophilic and / or hydrophobic),

[0096] - urea derivatives resulting from the reaction of a diisocyanate monomer, preferably aromatic such as diphenylmethylene diisocyanate (in particular 4,4'-MDI), with a primary aliphatic amine such as butylamine,

[0097] Castor oil-derived waxes, such as THIXCIN® R by ELEMENTIS, and amide waxes, preferably micronized, such as CRAYVALLAC® SLT by ARKEMA,

[0098] beeswax (especially CAS 8006-40-4 and / or 8012-89-3), and their mixtures.

[0099] By "waxes derived from castor oil" we mean waxes obtained from castor oil, in particular hydrogenated castor oil.

[0100] The term "amide waxes" refers to waxes comprising one or more compounds with at least one amide group. In particular, amide waxes can be obtained from organic acid(s) (e.g., fatty acid(s)) and (di)amine(s).

[0101] The amide waxes are preferably micronized, that is to say, they have an average particle size of less than or equal to 1 mm. Advantageously, the amide waxes have an average particle size of less than or equal to 500 pm, preferably less than or equal to 100 pm, more preferably less than or equal to 15 pm.

[0102] The content of rheological agent can be up to 10% by weight relative to the total weight of the composition according to the invention.

[0103] Core-shell impact modifiers can generally be described as polymeric substances, typically in particulate form, comprising a core (inner part) consisting of a core polymer and a shell (outer part) consisting of a shell polymer. One or more intermediate polymer layers may be included between the core and shell polymers.

[0104] The core polymer may comprise a polymer (homopolymer and / or copolymer) of a conjugated diene comprising from 4 to 12, preferably from 4 to 8, carbon atoms (such as isoprene and / or butadiene), and / or a polymer (homopolymer and / or copolymer) of an acyclic alkyl (meth)acrylate in which the alkyl chain (linear or branched) comprises from 1 to 12, preferably from 1 to 8, carbon atoms (such as butyl acrylate).

[0105] The bark polymer may comprise a polymer (homopolymer and / or copolymer) of an acyclic alkyl (meth)acrylate in which the alkyl chain (linear or branched) comprises from 1 to 12 carbon atoms, preferably from 1 to 8 carbon atoms, more preferably from 1 to 4 carbon atoms, such as methyl methacrylate.

[0106] When one or more intermediate polymer layers are present, each intermediate polymer may comprise a polymer (homopolymer and / or copolymer) of an acyclic alkyl (meth)acrylate in which the alkyl chain (linear or branched) comprises from 1 to 12 carbon atoms, preferably from 1 to 8 carbon atoms, more preferably from 1 to 4 carbon atoms, such as methyl methacrylate. Each intermediate polymer may be identical to or different from the shell polymer.

[0107] The bark polymer and / or intermediate polymer (if present) may further comprise functional groups different from the groups derived from the polymerization of an acyclic alkyl (meth)acrylate (i.e., different from the acyclic alkyl esters remaining after polymerization of said alkyl (meth)acrylate). These functional groups can be selected from epoxy groups (such as the glycidyl group), carboxylic acid groups, carboxamide groups (such as N,N-dialkylcarboxamide groups, notably N,N-dimethylcarboxamide), alkoxy groups (such as methoxy, ethoxy), amine groups (e.g. primary amine), cycloalkyl ester groups (e.g. C8-C12 cycloalkyl such as isobornyl ester, 3,3,5-trimethylcyclohexyl, tert-butylcyclohexyl and / or (octahydro-4,7-methano-1H-indenyl)methyl), and mixtures thereof.

[0108] Each of the core, shell and intermediate polymers can be crosslinked. The crosslinking agent(s) / monomer(s) can be selected from polyfunctional vinylaromatic compounds such as divinylbenzene and divinyltoluene, polyhydric alcohols such as ethylene glycol di(meth)acrylate and 1,3-butanediol di(meth)acrylate, tri(meth)acrylates, allyl carboxylates such as allyl acrylate and allyl methacrylate, and di- and triallylic compounds such as diallyl phthalate, diallyl sebacate and triallyl triazine.

[0109] The volume-average diameter of the functionalized core-shell filler can range from 10 to 900 nm. The volume-average diameter can be measured by dynamic light scattering (DLS).

[0110] Examples of commercially available core-shell fillers include Clearstrength® (e.g., Clearstrength® XT100) or Durastrength® sold by Arkema, or Paraloid™ (Paraloid™ 2650A, Paraloid™ 2691A) sold by Dow.

[0111] The core-bark type impact modifier content can be up to 15% by weight relative to the total weight of the composition according to the invention.

[0112] The pigment can be chosen from organic pigments, inorganic pigments, and mixtures thereof. For example, the pigment can be chosen from phthalocyanine-based pigments (such as copper phthalocyanine, halogenated copper phthalocyanine, metal-free phthalocyanine), anthraquinone-based pigments (such as 1-methylamino-4-o-tolylaminoanthraquinone, 1,4-diisopropyl aminoanthraquinone, 1,4-diaminoanthraquinone, 1,4-dibutyl-aminoanthraquinone, 1-amino-4-anilinoanthraquinone), quinacridone-based pigments, perylene-based pigments, thioindigo-based pigments, quinophthalone-based pigments, titanium dioxide, carbon black, manganese ferrite, and mixtures thereof.

[0113] The pigment content can be up to 3% by weight relative to the total weight of the composition according to the invention.

[0114] Other features

[0115] Advantageously, the weight ratio of the mixture M of styrene block copolymers comprising at least one triblock copolymer and optionally at least one diblock copolymer, preferably a styrene-isoprene-styrene (SIS) triblock copolymer and a styrene-isoprene (SI) diblock copolymer, relative to the tackifying resin is between 50 / 50 and 75 / 25, preferably between 55 / 45 and 65 / 35.

[0116] Preferably, the ratio "m" by weight of mixture M relative to the total weight of the composition is given by the relation (ax MFR + b)% < m 75%, in which:

[0117] MFR is the hot fluidity index of mixture M (200°C, 5kg);

[0118] - a is between 1 and 1.35 preferably between 1.1 and 1.3, for example between 1.15 and 1.25 or 1.2;

[0119] b is between 50 and 60, preferably between 52 and 55.

[0120] In particular, the ratio "m" can be between (1.11 x MFR + 52)% < m < 75%, for example (1.2 x MFR + 55)% < m < 75%.

[0121] Advantageously, the composition according to the invention does not include any other styrenic block copolymers than those of mixture M.

[0122] According to one embodiment, the composition according to the invention comprises: - between 50% by weight and 75% by weight of a mixture M of styrene block copolymers comprising at least one styrene-isoprene-styrene triblock copolymer and at least one styrene-isoprene diblock copolymer, preferably between 5% and 100% by weight of at least one styrene-isoprene-styrene triblock copolymer and between 0% and 95% by weight of at least one styrene-isoprene diblock copolymer relative to the total weight of mixture M,

[0123] - between 25% by weight and 50% by weight of at least one tackifying resin, and - optionally up to 10% by weight of one or more additives, for example chosen from fillers, ultraviolet stabilizers (or antioxidants), additional polymers other than styrenic block copolymers, rheological agents, core-bark type impact modifiers, pigments, and mixtures thereof,

[0124] in which the weight ratio of M mixture / tackifying resin is between 50 / 50 and 75 / 25, preferably between 55 / 45 and 65 / 35.

[0125] Preferably, the composition according to the invention consists essentially of the ingredients mentioned above. By "consists essentially of" means that the composition according to the invention comprises less than 5% by weight of ingredients other than the aforementioned ingredients, relative to the total weight of said composition, preferably less than 2% by weight, and even more preferably less than 1% by weight.

[0126] The ingredients of this embodiment and their particular contents are as described above, including preferred embodiments and characteristics.

[0127] In preferred embodiments, the composition according to the invention comprises:

[0128] - between 50% by weight and 75% by weight of a mixture M of styrene block copolymers comprising at least one styrene-isoprene-styrene triblock copolymer and at least one styrene-isoprene diblock copolymer, preferably consisting of between 5% and 100% by weight of at least one styrene-isoprene-styrene triblock copolymer and between 0% and 95% by weight of at least one styrene-isoprene diblock copolymer relative to the total weight of mixture M,

[0129] - between 25% by weight and 50% by weight of at least one tackifying resin of natural origin, preferably derived from pine wood, and

[0130] - optionally up to 10% by weight of one or more additives, for example chosen from fillers, ultraviolet stabilizers (or antioxidants), additional polymers other than styrenic block copolymers, rheological agents, core-shell type impact modifiers, pigments, and mixtures thereof,

[0131] in which the ratio of the mixture M, denoted "m", is given by the relation (1.11 x MFR + 52)% < m < 75% with respect to the total weight of the composition, where "MFR" is the hot melt index (200°C, 5kg) of said mixture M. For example, "m" is defined by the relation (1.2 x MFR + 55)% < m < 75%.

[0132] Preferably, the composition according to the invention consists essentially of the ingredients mentioned above. The ingredients of this embodiment and their particular contents are as described above, including the preferred embodiments and characteristics.

[0133] Advantageously, the composition according to the invention has a fifth-opening adhesion strength by T-peel greater than or equal to 0.3 N / cm for a thickness of 15 µm of said composition between two polyethylene substrates. The fifth-opening adhesion strength can, for example, be measured in accordance with Example 1.

[0134] Advantageously, the composition according to the invention has a hot melt flow rate at 190°C and 2.16 kg of 60 g / 10 min or less, preferably 50 g / 10 min or less, for example 40 g / 10 min or less, 20 g / 10 min or less, or 15 g / 10 min or less. The hot melt flow rate can be measured in accordance with ASTM D1238-10 (Procedure A).

[0135] Advantageously, the composition according to the invention has a glass transition temperature Tg less than or equal to 4°C, preferably less than or equal to 0°C. The glass transition temperature Tg can be determined by Dynamic Mechanical Analysis, for example as described in Example 1.

[0136] Such a low glass transition temperature allows the composition according to the invention to be used for products or packaging intended to be stored at low temperatures, for example food packaging intended to be refrigerated or frozen.

[0137] The composition according to the invention is generally in a molten state at a temperature of 150°C or lower, preferably 140°C or lower, and more preferably 130°C or lower. The molten state can, for example, be characterized by the intersection temperature of the elastic modulus G' and viscous modulus curves on a temperature-versus-temperature plot obtained using Dynamic Mechanical Analysis (DMA). DMA conditions are given in Example 1 below.

[0138] A low crossing temperature allows the fluid resin to remain at a low temperature, which allows for energy savings during the preparation and implementation of the composition according to the invention.

[0139] The composition according to the invention is therefore particularly suitable for packaging or products that need to be kept at low temperatures, for example frozen food products or products kept in a refrigerator. The composition according to the invention can be in the form of granules, preferably ovoid or spheroidal in shape, with an average size of between 1 mm and 10 mm, preferably between 2 and 6 mm.

[0140] The average size of the granules can be measured using calipers. These granules are preferably coated with a layer of a sliding and / or anti-blocking agent at a rate of 0.5% to 1.5% maximum by weight relative to the total weight of the granules.

[0141] The sliding and / or anti-blocking agent may be chosen from among organic and / or inorganic sliding and / or anti-blocking agents. For example, the sliding and / or anti-blocking agent may be chosen from erucamide, oleamide, docosanamide, stearamide, palmitamide, ethylene bis-stearamide, ethylene bis-oleamide, silica, talc, calcium carbonate, glass beads, and mixtures thereof, in particular talc.

[0142] The composition according to the invention can be prepared by a process comprising:

[0143] - a hot mixing stage for the ingredients, for example between 90°C and 200°C, preferably using a twin-screw extruder, then

[0144] - a cutting step of the extruded mixture, preferably at the exit of the die, then

[0145] - a cooling step, for example at room temperature (23°C). Preferably, the cutting step is carried out in such a way as to obtain granules (in particular of ovoidal or spheroidal shape) with an average size of between 1 mm and 10 mm, preferably between 2 and 6 mm.

[0146] For example, the cutting stage of the extruded mixture can be underwater cutting followed by centrifugation and then a drying stage of the resulting granules.

[0147] Multilayer structure

[0148] The present invention also relates to a multilayer structure comprising:

[0149] - an adhesive layer consisting of the self-adhesive, hot-melt composition according to the invention,

[0150] - a heat-sealable layer, and

[0151] - a complexifiable layer,

[0152] in which the adhesive layer is located between the heat-sealable layer and the laminating layer. Adhesive layer

[0153] The self-adhesive hot melt composition according to the invention is as described above, including preferred embodiments and features.

[0154] The adhesive layer can have a thickness between 5 µm and 50 µm, preferably between 7 µm and 25 µm.

[0155] Heat-sealable layer

[0156] The heat-sealable layer allows the multilayer structure to be sealed to a substrate when heated (for example, the perimeter of a container), particularly at temperatures between 80°C and 180°C, preferably between 100°C and 160°C. Thus, the heat-sealable layer advantageously has a softening temperature between 80°C and 180°C. This softening temperature can be measured according to ASTM E28-67.

[0157] The heat-sealable layer may be based on a thermoplastic polymer. In particular, the heat-sealable layer comprises at least 90% by weight of one or more thermoplastic polymers relative to the total weight of said layer, preferably at least 95% by weight, more preferably at least 99% by weight.

[0158] The thermoplastic polymer can be chosen from:

[0159] - polyethylene (PE),

[0160] - polypropylene (PP),

[0161] - polyamide (PA),

[0162] - a polyester polymer, for example comprising at least one motif derived from a cyclic or acyclic diol (preferably acyclic) and at least one motif derived from a cyclic dicarboxylic acid (preferably aromatic), in particular polyethylene terephthalate (PET) or one of its derivatives (for example further comprising a motif derived from isophthalic acid),

[0163] - an ethylene copolymer, for example a maleic anhydride grafted copolymer, an ethylene and propylene copolymer, an ethylene and vinyl acetate (EVA) copolymer, an ethylene and vinyl alcohol (EVOH) copolymer, an ethylene and an alkyl acrylate copolymer such as methyl acrylate (EMA) or butyl acrylate (EBA),

[0164] - polystyrene (PS),

[0165] - polyvinyl chloride (PVC),

[0166] - polyvinylidene fluoride (PVDF),

[0167] - a lactic acid polymer (PLA),

[0168] - a polyhydroxyalkanoate (PHA), and

[0169] - their mixtures. Preferably, the thermoplastic polymer is chosen from polyethylene, polypropylene, a polyester polymer, an ethylene-propylene copolymer, and mixtures thereof, more preferably from polyethylene, polypropylene, an ethylene-propylene copolymer, and mixtures thereof, and even more preferably polyethylene.

[0170] The heat-sealable layer may also include one or more additives, for example chosen from UV stabilizers (or antioxidants), sliding and / or anti-blocking agents, anti-fog agents, anti-static agents, and mixtures thereof.

[0171] The total content of additive(s) may be up to 10% by weight relative to the total weight of the heat-sealable layer, preferably up to 5% by weight, more preferably up to 1% by weight.

[0172] The UV stabilizer (or antioxidant) can be chosen from among benzotriazoles, benzophenones, phosphites (such as tris(2,4-di-tert-butylphenyl)phosphite, tris-(p-nonylphenyl)phosphite), so-called hindered phenols (such as rethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], 2,2-methylenebis(6-(tert-butyl)-4-methylphenol), 2,2'-methylenebis(6-(tert-butyl)-4-ethylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-methylenebis(4,6-di(tert-butyl)phenol), 4,4'-methylenebis(2,6-di(tert-butyl)phenol, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,6-di(tert-butyl)-4-methylphenol), so-called hindered amines (such as bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, methyl 1,2,2,6,6-pentamethyl-4-piperidyl sebacate and 4,4'-bis(a,a-dimethylbenzyl)diphenylamine), and mixtures thereof.

[0173] The sliding and / or anti-blocking agent can be chosen from organic and / or inorganic sliding and / or anti-blocking agents. For example, the sliding and / or anti-blocking agent can be chosen from erucamide, oleamide, docosanamide, stearamide, palmitamide, ethylene bis-stearamide, ethylene bis-oleamide, silica, talc, calcium carbonate, glass beads, and mixtures thereof.

[0174] The anti-fog agent may be chosen from sorbitan esters, glycerol esters, poly(oxyethylene) esters, alkylbenzene sulfonates, and mixtures thereof; said esters are in particular fatty acid(s) esters.

[0175] The antistatic agent can be chosen from alkali metal sulfonates, polyether-modified polydiorganosiloxanes, polyalkylphenylsiloxanes, tertiary amines, glycerol monostearate, mixtures of glycerol monostearate and tertiary amines, and mixtures thereof. The heat-sealable layer is advantageously breakable.

[0176] The heat-sealable layer can be pre-cut over all or part of its thickness, for example using a laser or a cutting plate.

[0177] The heat-sealable layer can be bi-oriented.

[0178] The bi-orientation of one (or more) layer(s) can be achieved by stretching the layer(s) under heating (e.g., infrared, at a temperature above 100°C) in the machine direction (also called axial) and by stretching under heating (e.g., between 100°C and 135°C) in the direction perpendicular to the machine direction (also called transverse). The layer(s) can then be heated up to 220°C and relaxed at 220-170°C in the transverse direction. The stretch factor can be between 2.0 and 4.0 (particularly around 3.0) in the machine direction, and between 3.0 and 4.0 (particularly around 3.4) in the transverse direction.

[0179] By "approximately X", we are aiming for more or less 10% of the value of X.

[0180] The heat-sealable layer may have undergone surface treatment, such as embossing (preferably hot), plasma treatment like corona treatment, atmospheric pressure plasma treatment, flame plasma treatment, chemical plasma treatment, etc.

[0181] The heat-sealable layer can have a thickness between 0.1 pm and 100 pm, preferably between 1 pm and 50 pm.

[0182] Complexable layer

[0183] The complexable layer can be complexed (or bonded, or laminated, preferably bonded) with other layers, for example with a rigid layer to improve the mechanical strength of the multilayer structure.

[0184] The complexable layer may be based on a thermoplastic polymer. In particular, the complexable layer comprises at least 90% by weight of one or more thermoplastic polymers relative to the total weight of said layer, preferably at least 95% by weight, more preferably at least 99% by weight.

[0185] The thermoplastic polymer can be chosen from:

[0186] - polyethylene (PE),

[0187] - polypropylene (PP),

[0188] - polyamide (PA),

[0189] - a polyester polymer, for example comprising at least one cyclic or acyclic diol-derived motif (preferably acyclic) and at least one cyclic dicarboxylic acid-derived motif (preferably aromatic), in particular polyethylene terephthalate (PET) or one of its derivatives (for example further comprising an isophthalic acid-derived motif, preferably PET,

[0190] - an ethylene copolymer, for example a maleic anhydride grafted copolymer, an ethylene and propylene copolymer, an ethylene and vinyl acetate (EVA) copolymer, an ethylene and vinyl alcohol (EVOH) copolymer, an ethylene and an alkyl acrylate copolymer such as methyl acrylate (EMA) or butyl acrylate (EBA),

[0191] - polystyrene (PS),

[0192] - polyvinyl chloride (PVC),

[0193] - polyvinylidene fluoride (PVDF),

[0194] - a lactic acid polymer (PLA),

[0195] - a polyhydroxyalkanoate (PHA), and

[0196] - their mixtures.

[0197] Preferably, the thermoplastic polymer is chosen from polyethylene, polypropylene, a polyester polymer, an ethylene-propylene copolymer, and mixtures thereof, more preferably from polyethylene, polypropylene, an ethylene-propylene copolymer, and mixtures thereof, and even more preferably polyethylene.

[0198] The complexable layer may also include one or more additives, for example chosen from UV stabilizers (or antioxidants), sliding and / or anti-blocking agents, antistatic agents, and mixtures thereof.

[0199] The total content of additive(s) may be up to 10% by weight relative to the total weight of the complexable layer, preferably up to 5% by weight, more preferably up to 1% by weight.

[0200] The UV stabilizer (or antioxidant) can be chosen from among benzotriazoles, benzophenones, phosphites (such as tris(2,4-di-tert-butylphenyl)phosphite, tris-(p-nonylphenyl)phosphite), so-called hindered phenols (such as rethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], 2,2-methylenebis(6-(tert-butyl)-4-methylphenol), 2,2'-methylenebis(6-(tert-butyl)-4-ethylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-methylenebis(4,6-di(tert-butyl)phenol), 4,4'-methylenebis(2,6-di(tert-butyl)phenol, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,6-di(tert-butyl)-4-methylphenol), so-called hindered amines (such as bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, methyl 1,2,2,6,6-pentamethyl-4-piperidyl sebacate and 4,4'-bis(a,a-dimethylbenzyl)diphenylamine), and mixtures thereof.

[0201] The sliding and / or anti-blocking agent can be chosen from organic and / or inorganic sliding and / or anti-blocking agents. For example, the sliding and / or anti-blocking agent can be chosen from erucamide, oleamide, docosanamide, stearamide, palmitamide, ethylene bis-stearamide, ethylene bis-oleamide, silica, talc, calcium carbonate, glass beads, and mixtures thereof.

[0202] The antistatic agent may be chosen from alkali metal sulfonates, polyether-modified polydiorganosiloxanes, polyalkylphenylsiloxanes, tertiary amines, glycerol monostearate, mixtures of glycerol monostearate and tertiary amines, and mixtures thereof.

[0203] The complexable layer can be bi-oriented.

[0204] The complexable layer may have undergone surface treatment, such as embossing (preferably hot), plasma treatment such as corona treatment, atmospheric pressure plasma treatment, flame plasma treatment, chemical plasma treatment, etc.

[0205] The complexable layer can have a thickness between 0.1 pm and 100 pm, preferably between 1 pm and 50 pm.

[0206] Additional layers

[0207] The multilayer structure according to the invention may also include one or more additional layers (in addition to the adhesive, heat-sealable and complexable layers described above).

[0208] For example, the multilayer structure according to the invention may include: one or more additional layers on the heat-sealable layer (preferably between the adhesive layer and the heat-sealable layer), and / or one or more additional layers on the complexable layer (between the adhesive layer and the complexable layer, and / or on the surface not directed towards the adhesive layer, preferably between the adhesive layer and the complexable layer).

[0209] In this text, "heat-sealable film" means the assembly formed by the heat-sealable layer and the additional layer(s) on the heat-sealable layer, and "complexable film" means the assembly formed by the complexable layer and the additional layer(s) on the complexable layer.

[0210] Advantageously, the heat-sealable layer has a free side (not covered by another layer); it is therefore an outer layer. When the multilayer structure is used as the lid of a resealable package, the lid is heat-sealed to the receptacle via the heat-sealable layer.

[0211] It is possible that one or more of the additional layers may also be heat-sealable layers, identical or different from the heat-sealable layer as described above.

[0212] Each additional layer may be based on a thermoplastic polymer. In particular, each additional layer comprises at least 90% by weight of one or more thermoplastic polymers relative to the total weight of said layer, preferably at least 95% by weight, more preferably at least 99% by weight.

[0213] The thermoplastic polymer can be chosen from:

[0214] - polyethylene (PE),

[0215] - polypropylene (PP),

[0216] - polyamide (PA),

[0217] - a polyester polymer, for example comprising at least one motif derived from a cyclic or acyclic diol (preferably acyclic) and at least one motif derived from a cyclic dicarboxylic acid (preferably aromatic), in particular polyethylene terephthalate (PET) or one of its derivatives (for example further comprising a motif derived from isophthalic acid),

[0218] - an ethylene copolymer, for example a maleic anhydride grafted copolymer, an ethylene and propylene copolymer, an ethylene and vinyl acetate (EVA) copolymer, an ethylene and vinyl alcohol (EVOH) copolymer, an ethylene and an alkyl acrylate copolymer such as methyl acrylate (EMA) or butyl acrylate (EBA),

[0219] - polystyrene (PS),

[0220] - polyvinyl chloride (PVC),

[0221] - polyvinylidene fluoride (PVDF),

[0222] - a lactic acid polymer (PLA),

[0223] - a polyhydroxyalkanoate (PHA), and

[0224] - their mixtures.

[0225] Each additional layer may further include one or more additives, for example chosen from UV stabilizers (or antioxidants), sliding and / or anti-blocking agents, antistatic agents, and mixtures thereof.

[0226] The total content of additive(s) may be up to 10% by weight relative to the total weight of each additional layer, preferably up to 5% by weight, more preferably up to 1% by weight.The UV stabilizer (or antioxidant) can be chosen from among benzotriazoles, benzophenones, phosphites (such as tris(2,4-di-tert-butylphenyl)phosphite, tris-(p-nonylphenyl)phosphite), so-called hindered phenols (such as ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], 2,2'-methylenebis(6-(tert-butyl)-4-methylphenol), 2,2'-methylenebis(6-(tert-butyl)-4-ethylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-methylenebis(4,6-di(tert-butyl)phenol), 4,4'-methylenebis(2,6-di(tert-butyl)phenol, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,6-di(tert-butyl)-4-methylphenol), so-called hindered amines (such as bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, methyl 1,2,2,6,6-pentamethyl-4-piperidyl sebacate and 4,4'-bis(a,a-dimethylbenzyl)diphenylamine), and mixtures thereof.

[0227] The sliding and / or anti-blocking agent can be chosen from organic and / or inorganic sliding and / or anti-blocking agents. For example, the sliding and / or anti-blocking agent can be chosen from erucamide, oleamide, docosanamide, stearamide, palmitamide, ethylene bis-stearamide, ethylene bis-oleamide, silica, talc, calcium carbonate, glass beads, and mixtures thereof.

[0228] The antistatic agent may be chosen from alkali metal sulfonates, polyether-modified polydiorganosiloxanes, polyalkylphenylsiloxanes, tertiary amines, glycerol monostearate, mixtures of glycerol monostearate and tertiary amines, and mixtures thereof.

[0229] Each additional layer can be bi-oriented.

[0230] Each additional layer may have undergone a surface treatment, such as embossing (preferably hot), plasma treatment such as corona treatment, atmospheric pressure plasma treatment, flame plasma treatment, chemical plasma treatment, etc.

[0231] Each additional layer can have a thickness between 0.1 pm and 100 pm, preferably between 1 pm and 50 pm.

[0232] The heat-sealable film can have a thickness between 2 µm and 150 µm, preferably between 3 µm and 100 µm.

[0233] The complexable film can have a thickness between 5 pm and 150 pm, preferably between 10 pm and 100 pm.

[0234] The heat-sealable film is advantageously tearable.

[0235] Heat-sealable film can be pre-cut through all or part of its thickness, for example using a laser or a cutting plate. Heat-sealable film can be bi-oriented.

[0236] The complexable film can be bi-oriented.

[0237] Other features

[0238] One or more of the layers of the multilayer structure according to the invention can be covered in whole or in part by an ink.

[0239] According to one embodiment, the multilayer structure according to the invention comprises:

[0240] - an adhesive layer having a thickness between 5 µm and 50 µm, consisting of the self-adhesive, hot-melt composition according to the invention,

[0241] - a heat-sealable and breakable layer, preferably based on a thermoplastic polymer selected from polyethylene, polypropylene, a polyester polymer, an ethylene-propylene copolymer, and mixtures thereof,

[0242] - a complexable layer, preferably based on a thermoplastic polymer selected from polyethylene, polypropylene, a polyester polymer, an ethylene-propylene copolymer, and mixtures thereof, and

[0243] - optionally one or more additional layers,

[0244] in which the adhesive layer is located between the heat-sealable layer and the complexable layer.

[0245] The layers of this embodiment are as described above, including preferred embodiments and features.

[0246] The multilayer structure according to the invention can be used as a lid for packaging comprising a receptacle. In this case, it is understood that the multilayer structure does not include the receptacle.

[0247] Manufacturing process for the multilayer structure

[0248] The present invention also relates to a method of manufacturing the multilayer structure according to the invention by lamination or by coextrusion, in particular by bubble blowing coextrusion.

[0249] According to a first embodiment, the manufacturing process for the multilayer structure according to the invention comprises:

[0250] - a step of coating an adhesive comprising the self-adhesive hot-melt composition according to the invention onto a surface of a first film, then - a step of laminating (bonding) a surface of a second film onto the coated surface of the first film,

[0251] in which one of the films includes the heat-sealable layer or is bonded to the heat-sealable layer after the laminating step, and in which one of the films includes the complexable layer or is bonded to the complexable layer after the laminating step.

[0252] The multilayer structure, the self-adhesive hot-melt composition, the heat-sealable layer, and the laminating layer are as described above, including preferred embodiments and characteristics. In particular, the heat-sealable layer preferably has a free face.

[0253] The first film and the second film can each be single-layer or multi-layer.

[0254] The coating step can be carried out on all or part of the surface of the first film, preferably in a continuous or substantially continuous manner.

[0255] To facilitate the coating of the hot melt self-adhesive composition, the adhesive preferably comprises an organic solvent, for example butanone, toluene, xylene, benzene, monochlorobenzane, dichloromethane, 2-nitropropane, nitroethane, nitrobenzene, dichlorobenzene, dioxolane, tetrahydrofuran, an ester (ethyl acetate, n-butyl acetate, 2-ethoxyethyl acetate), cyclohexanone and / or dioxane, in particular an ester such as ethyl acetate, n-butyl acetate, 2-ethoxyethyl acetate, etc.

[0256] The solvent content can be between 10% and 95% by weight relative to the total weight of the adhesive, preferably between 50% and 90% by weight.

[0257] When the adhesive contains a solvent, the manufacturing process for the multilayer structure according to the invention advantageously includes an adhesive drying step after the coating step and before the laminating step. The drying step can be carried out at a temperature between 18°C ​​and 100°C, preferably between 20°C and 90°C, for a period sufficient to allow the solvent to evaporate.

[0258] When one or more additional layers (as described above) are present in the multilayer structure, they can be obtained by co-extrusion, coating and / or by lamination with one or more layers of the multilayer structure.

[0259] According to a second embodiment, the manufacturing process of the multilayer structure according to the invention includes a co-extrusion step of the self-adhesive heat-fusible composition according to the invention and the constituent materials of the heat-sealable and complexable layers.

[0260] The multilayer structure, the self-adhesive hot-melt composition, the heat-sealable layer, the complexable layer, and the additional layers are as described above, including preferred embodiments and characteristics. In particular, the heat-sealable layer preferably has a free face.

[0261] When one or more additional layers (as described above) are present in the multilayer structure, they can be obtained by co-extrusion, coating and / or by lamination with one or more layers of the multilayer structure.

[0262] The coextrusion device is preferably a bubble blow coextrusion device (also known as "sheath blow coextrusion"). As is known to those skilled in the art, this process comprises:

[0263] - the melting, in separate extruders, of the compositions and materials constituting the adhesive, heat-sealable and laminating layers, and optionally any additional layers, then

[0264] - the passage of the corresponding flows through a set of annular and concentric dies, so as to form a multi-layered tubular bubble, in the order corresponding to that desired for the final structure, then - the radial expansion (relative to the annular die) and the stretching (in the axial direction) of the bubble, then

[0265] - the cooling of the bubble.

[0266] The geometric characteristics of the dies, as well as process parameters such as the radial expansion rate and the stretching speed, are set to obtain the desired thickness for the various constituent layers of the multilayer structure. For a more detailed description of the bubble blow coextrusion process, reference is made to US patent application 2013 / 0029553.

[0267] Resealable packaging

[0268] The present invention also relates to a resealable package comprising the multilayer structure according to the invention.

[0269] In particular, the resealable packaging includes a receptacle and a lid made up of the multilayer structure according to the invention.

[0270] Advantageously, the lid is heat-sealed around the perimeter of the receptacle. The receptacle is preferably made of a plastic polymer, for example, chosen from:

[0271] - polyethylene (PE),

[0272] - polypropylene (PP),

[0273] - polyamide (PA), - polyethylene terephthalate (PET),

[0274] - an ethylene copolymer, for example a maleic anhydride grafted copolymer, an ethylene and propylene copolymer, an ethylene and vinyl acetate (EVA) copolymer, an ethylene and vinyl alcohol (EVOH) copolymer, an ethylene and an alkyl acrylate copolymer such as methyl acrylate (EMA) or butyl acrylate (EBA),

[0275] - polystyrene (PS),

[0276] - polyvinyl chloride (PVC),

[0277] - polyvinylidene fluoride (PVDF),

[0278] - a lactic acid polymer (PLA),

[0279] - a polyhydroxyalkanoate (PHA), and

[0280] - their mixtures.

[0281] The total content of thermoplastic polymer(s) may be at least 90% by weight relative to the total weight of the receptacle, preferably at least 95% by weight, more preferably at least 99% by weight.

[0282] The receptacle may also include one or more additives, for example chosen from UV stabilizers (or antioxidants), sliding and / or anti-blocking agents, pigments, antistatic agents, and mixtures thereof.

[0283] The total content of additive(s) may be up to 10% by weight relative to the total weight of the receptacle, preferably up to 5% by weight, more preferably up to 1% by weight.

[0284] The UV stabilizer (or antioxidant) can be chosen from among benzotriazoles, benzophenones, phosphites (such as tris(2,4-di-tert-butylphenyl)phosphite, tris-(p-nonylphenyl)phosphite), so-called hindered phenols (such as ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], 2,2-methylenebis(6-(tert-butyl)-4-methylphenol), 2,2'-methylenebis(6-(tert-butyl)-4-ethylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-methylenebis(4,6-di(tert-butyl)phenol), 4,4'-methylenebis(2,6-di(tert-butyl)phenol, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,6-di(tert-butyl)-4-methylphenol), so-called hindered amines (such as bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, methyl 1,2,2,6,6-pentamethyl-4-piperidyl sebacate and 4,4'-bis(a,a-dimethylbenzyl)diphenylamine), and mixtures thereof.

[0285] The sliding and / or anti-blocking agent can be chosen from among organic and / or inorganic sliding and / or anti-blocking agents. For example, the sliding and / or anti-blocking agent can be chosen from erucamide, oleamide, docosanamide, stearamide, palmitamide, ethylene bis-stearamide, ethylene bis-oleamide, silica, talc, calcium carbonate, glass beads, and mixtures thereof.

[0286] The pigment can be chosen from organic pigments, inorganic pigments, and mixtures thereof. For example, the pigment can be chosen from manganese ferrite, titanium dioxide, carbon black, iron oxide, aluminum, talc, and mixtures thereof, in particular titanium dioxide, carbon black, and mixtures thereof.

[0287] The antistatic agent may be chosen from alkali metal sulfonates, polyether-modified polydiorganosiloxanes, polyalkylphenylsiloxanes, tertiary amines, glycerol monostearate, mixtures of glycerol monostearate and tertiary amines, and mixtures thereof.

[0288] Use of the multilayer structure

[0289] The present invention also relates to the use of the multilayer structure according to the invention for the manufacture of a resealable package, preferably for food, in particular for chilled or frozen food.

[0290] Advantageously, the multilayer structure is used as the lid of the resealable packaging.

[0291] Preferably, the resealable packaging is as described above, including preferred embodiments and features.

[0292] All the embodiments described above can be combined with one another. In particular, the various aforementioned components of the composition, and especially the preferred embodiments, can be combined with one another.

[0293] Figures

[0294] Fig. 1 is a graph showing the evolution of the % of SIS to be introduced into the formulation with Sylvalite9100 as a function of the MFR of said SIS, to obtain a final MFI of at least 60 g / 10min, or 40 g / 10min according to the invention.

[0295] Fig. 2 is a graph showing the evolution of the adhesion strength for an example of composition according to the invention.

[0296] Fig. 3 shows photos of samples of compositions K, J and E. Examples

[0297] The following examples are given purely to illustrate the invention and should not be interpreted as limiting its scope.

[0298] Example 1: Ingredients and measurement methods

[0299] Ingredients used

[0300] The following ingredients were used.

[0301] The tackifying resins used in Example 2 are Sylvalite 9100 resin, Kraton RE100-S resin, and NINGBO JINHAI CHENGUANG CHEMICAL CORPORATION JH3204 resin. Sylvalite 9100 resin is derived from pine wood. RE100-S resin is derived from tall oil. JH3204 resin is a C5 hydrocarbon resin. The characteristics of Sylvalite 9100 resin are as follows:

[0302] Table 1

[0303] Properties Test Method Sylvalite 9100 Sylvalite RE100S

[0304] AQCM point 003 104 98 softening (°C)

[0305] KO H (mg / g) AQCM 001 8 5 Color (Hazen, 1:1 AQCM 002 88 /

[0306] in toluene)

[0307] Color (Gardner, 1:1 AQCM 002 0.9 2

[0308] in toluene)

[0309] Brookfield viscosity at AQCM 004 23100 9920

[0310] 125°C (mPa.s)

[0311] Brookfield viscosity at AQCM 004 1570 940

[0312] 150°C (mPa.s)

[0313] Brookfield viscosity at AQCM 004 240 173

[0314] 177°C (mPa.s)

[0315] AQCM temperature 218 55 48 glass transition Tg

[0316] (°C)

[0317]

[0318] The characteristics of JH3204 resin are as follows:

[0319] Table 2 Properties JH3204 Typical Value

[0320] Softening point (°C) 96-104

[0321] Color (Index of 20)

[0322] yellowing)

[0323] Gardner Colour 2.6

[0324] Brookfield viscosity at 160°C: 1570

[0325] (mPa.s)

[0326] Brookfield viscosity at 177°C 240

[0327] (mPa.s)

[0328] Transition temperature 55

[0329] vitreous Tg (°C)

[0330]

[0331] The styrenic block copolymers used are JH9520 from Ningbo Jinhai Chenguang Chemical Corporation, Vector 4116ND from TSRC, and D1111KT from Kraton. Their technical characteristics are as follows:

[0332] Table 3

[0333] V4116ND JH9520 D1111KT Meltdown ratio at 9-15°C (measured 3.5 - 9.5 (measured 6.5) 2-4 (measured 2.3) hot (MFR) 13.6)

[0334] (200°C-5kg)

[0335] % of triblock SIS 42-48 19-25 82

[0336] (by weight

[0337] relative to the weight of the

[0338] copolymer)

[0339] % of SI diblock (in 52 - 58 75 - 81 18 weight relative to

[0340] to the weight of

[0341] copolymer)

[0342] % of styrene (by weight 15-17, 13-17, 20-24)

[0343] to the weight of

[0344] copolymer)

[0345]

[0346] Measurement Methods: The melt flow index (MFI) was measured according to ASTM D1238-10 (Procedure A). Briefly, a sample of the composition to be tested was introduced into a plastometer, and the temperature was then raised to 190°C. A weight of 2.16 kg was then placed on the sample. The material flowing through the die for a specified time was weighed to determine the MFI. The MFI is expressed in g / 10 min at 190°C for a weight of 2.16 kg. The melt flow rate (MFR) was measured using the same protocol as the MFI, except that the temperature was raised to 200°C and the weight used was 5 kg. The MFR is expressed in g / 10 min at 200°C for a weight of 5 kg.

[0347] A Dynamic Mechanical Analysis (DMA) was performed on a sample of the composition to be tested using an ARES rheometer (marketed by TA Instruments), with a temperature sweep and a "plane-plane" type sample holder geometry (parallel plates spaced 1.6 mm apart, each 10 mm in diameter). Briefly, the sample to be analyzed was placed on the designated sample holder. The temperature was raised to 190°C to achieve a melt, then a temperature ramp down to -40°C was applied simultaneously with a shear rate of 10 rad / s. The temperature ramp rate was -8°C / min for temperatures from 190°C to 0°C, and -5°C / min for temperatures from 0°C to -40°C.The sample's response to mechanical stress was recorded every 15 seconds, and then the glass transition temperature (Tg) was determined to be the temperature at which the maximum of the tan 5 peak is observed.

[0348] The elastic modulus G' (also called the conservation modulus) and the loss factor (tan 5) were determined at 24°C, during the temperature decrease.

[0349] The strength of the 5th's adherence èmeThe opening was determined as follows. According to a first method, a sample of approximately 2 to 3 grams of each composition was placed between two polypropylene substrates (polypropylene / polyethylene terephthalate composite, 12 µm / 50 µm respectively; the PP face being in direct contact with the formulation under consideration). The sandwich was then placed under a heated press at 120°C and 240 bar for 3 minutes. A film 200 µm thick was obtained at the end of this first step. The film was then placed under the same conditions, but this time at 6400 bar, to obtain a final film thickness between 10 and 20 µm. The heat-sealed areas thus defined the test specimens used for adhesion and resealability measurements. 1 cm x 15 cm specimens were cut from the film. According to a second method, the adhesion strength of the 5 èmeThe opening was determined as follows: the composition was first dissolved in ethyl acetate to obtain a 20% wt. solution. This solution was then dispensed onto a 20 µm thick polyethylene (PE) substrate using a Mayer bar. After evaporation of the solvent at room temperature (approximately 23°C), the substrate was placed in an oven at 70°C for 1 h, whereupon a second 20 µm thick PE substrate was deposited on top of the coated and dried adhesive composition layer (15 µm thick), and the stack was held under a hydraulic press at 25 kN for 24 h. Subsequently, a PE / PET complex (20µm / 55µm, respectively) was laminated to each side of the stack (PE face on PE substrates), then heat-sealed between 1cm x 15cm jaws heated to 130°C for 1 second and under a pressure of 600N. The heat-sealed areas thus define the test specimens used for adhesion and resealability measurements.

[0350] Adhesion measurements were performed at 23°C on a dynamometer (Instron) by peeling the T-shaped test specimens at a speed of 300 mm / minute. Each specimen was opened and resealed (manually) five times; the adhesion strength at the fifth opening is considered relevant for comparing the compositions and for the intended applications. The adhesion strength was measured once a plateau value was reached for each opening and averaged over a 10 cm opening.

[0351] Example 2: Comparative Table

[0352] Compositions comprising a mixture of styrenic block copolymer and tackifying resin derived from pine wood are listed below, as well as compositions for comparison with one or more resins derived from C5 petroleum cuttings. The compositions are prepared using any technique well known to those skilled in the art, with the following proportions of SIS triblock copolymer / resin:

[0353] Table 4

[0354] MFI Adhesion g / 10 Resin Temperature

[0355] Copolymè 5th min Tg of tackifier

[0356] re (%) opening (190°C, (°C) crossing (%)

[0357] (N / cm) 2.16kg) (°C) A V4116ND Sylvalite

[0358] 0.59 42 -27 119 (inv) (70) 9100 (30)

[0359]

[0360] V4116ND Sylvalite

[0361] B > 0.59 73 -13.4 117.3 (65) 9100 (35)

[0362] V4116ND Sylvalite

[0363] C > 0.59 117 -7 115 (63) 9100 (37)

[0364] D JH9520 Sylvalite

[0365] 0.6 45.8 -14.9 114.4 (inv) (63) 9100 (37)

[0366] E JH9520 Sylvalite

[0367] 0.85 55 -13.3 112.8 (inv) (60) 9100 (40)

[0368] JH9520 Sylvalite

[0369] F > 0.85 92 -5.9 109.7 (57) 9100 (43)

[0370] G D1111KT Sylvalite

[0371] 0.74 35 -9.3 128.6 (inv) (60) 9100 (40)

[0372] H D1111KT Sylvalite 0.74 <

[0373] 40.5 -6.8 126 (inv) (57) 9100 (43) <1.34

[0374] I D1111KT Sylvalite

[0375] 1.34 55.5 -1 123 (inv) (55) 9100 (45)

[0376]

[0377] The comparative formulations are compositions B, C and F. The compositions incorporating a styrenic block copolymer according to the invention in Table 4 have a melt flow index (MFI) of less than 60 g / 10 min.

[0378] All the tested formulations exhibit a glass transition temperature below 0°C for the various resin / copolymer ratios studied, as does the comparative formulation J (-8°C). Furthermore, the crossover temperature of the elastic and viscous moduli of each formulation made with Sylvalite9100 resin is significantly lower than that of formulation J (Tx = 147°C) comprising a C5-type petroleum-based resin. The compositions according to the invention are therefore suitable for forming at lower temperatures than traditional compositions incorporating tackifying resins derived from hydrocarbons. This results in significant energy savings, thereby enhancing the ecological and bio-based nature of the compositions according to the invention.

[0379] Finally, all formulations according to the invention exhibit adhesion greater than 0.3 N / cm for a formulation thickness of 15 pm.

[0380] Furthermore, the viscosity of composition I was measured using a Brookfield-type method at 200°C and 1 rpm (rotations per minute): the measured value was 150 Pa·s (or 150,000 cP). This value is underestimated due to the air bubbles present in composition I, which is highly viscous.

[0381] Example 3: Appearance and odor of the compositions

[0382] The odor properties of the compositions are evaluated as follows: 50 grams of each composition or reference resin are placed individually in glass jars, which are then hermetically sealed for 24 hours. A panel of 5 to 10 people is selected. Each sample is presented to them blindly (one independent set of samples per person), and a score from 0 to 5 (0 = no odor, 5 = very strong odor) is assigned to each sample. The panel results are averaged for each sample and reported in the corresponding tables. For this example, the tackifying resin MWW65, a hydrogenated C5 type resin known for its low odor, and the tackifying resin M650F, a hydrocarbon-based C5 type resin, are used as test controls. The MWW65 and M650F resins are manufactured by BOSTIK. The comparative compositions are compositions J and K, whose formulation is as follows:

[0383] Composition J: 60% JH9520 polymer + 40% JH3204 resin; and composition K: 60% JH9520 polymer + 40% RES100 resin.

[0384] Comparison with MWW65 resin

[0385] Mean Standard deviation

[0386] MVWV65

[0387] 1.5 0.5

[0388] (reference)

[0389] Composition D 2 0.7

[0390] Composition E 1.6 0.6

[0391]

[0392] Comparison with M650F resin

[0393] Average Standard deviation M650F (reference) 2.5 0.5

[0394] Composition D 1.6 0.4

[0395] Composition E 2 0.6

[0396]

[0397] Comparison with M650F resin

[0398] Average Standard deviation M650F (reference) 3.5 1

[0399] Composition K 4.2 0.3

[0400]

[0401] The compositions according to the invention, in particular compositions D and E, therefore have a low odor, particularly suitable for use as an adhesive for packaging intended for consumer goods such as cosmetics and food products.

[0402] Example 4: Transfer of taste to food

[0403] The flavor transfer of each composition is evaluated as follows: a composition or control film, a few hundred micrometers thick, is obtained using a conventional method such as lamination or heat press. The film is then placed in direct contact with butter and chocolate for one week at refrigerated temperature (approximately 6°C), after which the film is removed from the food. A panel of 5 to 10 people is selected, and each food pair for each sample is presented to them blindly for tasting. An independent set of samples is prepared for each person. The control films are made of M 650F resin and a reference food that has not been exposed to an HMPSA film. A score from 0 to 5 (0 = no noticeable flavor compared to the food that has not been exposed to the film, 5 = very pronounced flavor) is assigned to each sample by the panelist.The panel results are then averaged for each sample and reported in the corresponding tables.

[0404] Comparison with M650F resin

[0405] Average Standard deviation M650F (reference) 1.3 1.5

[0406] Composition D 1.2 1.1

[0407] Composition E 1 0.9

[0408]

[0409] Comparison with M650F resin

[0410] Average Standard deviation M650F (reference) 2.6 1

[0411] Composition K 3.4 0.7

[0412]

[0413] The compositions according to the invention, particularly compositions D and E, therefore have a taste that transfers very little into food. The compositions according to the invention are thus particularly suitable for use as adhesives for food packaging.

[0414] Example 5: Color

[0415] Composition J has a pronounced yellow color. Composition K has a more pronounced yellow color than composition J, while composition E has a very pale yellow color. The polymer / resin ratios are identical in all three compositions.

Claims

Demands 1. Self-adhesive, hot-melt composition comprising: - at least one mixture M of styrenic block copolymers, said mixture comprising, on the basis of its total weight; - 5% to 100% by weight of at least one triblock copolymer; and - 0% to 95% by weight of at least one diblock copolymer; said mixture having a melt flow index MFR less than or equal to 20 g / 10min and preferably less than or equal to 18 g / 10min (200°C, 5kg); - at least one tackifying resin of natural origin having a Gardner color less than or equal to 1.5, said composition having a hot melt index MFI less than or equal to 60 g / 10 min (190°C, 2.16kg) and being characterized by a total polystyrene content of between 5 and 15% by weight relative to the total weight of said composition.

2. Composition according to claim 1 having a glass transition temperature less than or equal to 4°C, preferably less than or equal to 0°C.

3. Composition according to any one of claims 1 or 2 comprising an amount of mixture M of 50% by weight to 75% by weight relative to the total weight of the composition, and preferably of 52% to 73% by weight relative to the total weight of the composition.

4. Composition according to any one of the preceding claims wherein the triblock copolymer is a styrene-isoprene-styrene (SIS) triblock copolymer and the diblock copolymer is a styrene-isoprene (SI) diblock copolymer.

5. Composition according to any one of the preceding claims, wherein the ratio "m" by weight of mixture M relative to the total weight of the composition is given by the relation (ax MFR + b)% < m < 75%, wherein: MFR is the hot flow index of mixture M (200°C, 5kg); a is between 1 and 1.35, preferably between 1.1 and 1.3; b is between 50 and 60, preferably between 52 and 55.

6. A composition according to any one of the preceding claims, wherein at least one tackifying resin of natural origin is selected from: - natural and modified rosins, such as gum rosin, wood rosin, tall oil rosin, distilled rosin, hydrogenated rosin, dimerized rosin, polymerized rosin, - esters of natural and modified rosins, in particular glycerol and pentaerythritol esters such as glycerol esters of pale wood rosin, glycerol esters of polymerized rosin, pentaerythritol esters of pale wood rosin, pentaerythritol esters of tall oil rosin, pentaerythritol esters of phenolically modified rosin, and - their mixtures.

7. Composition according to any one of the preceding claims, wherein the total content of at least one tackifying resin is between 25% by weight and 50% by weight relative to the total weight of the composition.

8. Composition according to any one of the preceding claims, further comprising one or more additives.

9. Composition according to any one of the preceding claims not comprising a plasticizer.

10. Composition according to any one of the preceding claims wherein the naturally sourced tackifying resin has a Gardner colour less than or equal to 1.

11. Composition according to any one of the preceding claims having a Gardner colour less than or equal to 2, preferably less than or equal to 1.5, more preferably less than or equal to 1.

12. Multilayer structure comprising: - an adhesive layer consisting of the self-adhesive, hot-melt composition according to any one of claims 1 to 11, - a heat-sealable layer, and - a complexifiable layer, in which the adhesive layer is located between the heat-sealable layer and the complexable layer.

13. Method of manufacturing the multilayer structure according to claim 12 by lamination or by co-extrusion, in particular by bubble blow co-extrusion.

14. Resealable packaging comprising the multilayer structure according to claim 12.

15. Use of the multilayer structure according to claim 12 for the manufacture of a resealable package, preferably for food, in particular for chilled or frozen food.