Improved manufacture
By using soluble porogens and specialized fillers in additive manufacturing, the method addresses the challenge of uniform pore formation and absorption enhancement in foams, resulting in structurally sound and intricately designed acoustic and electromagnetic shielding materials.
Patent Information
- Application Number
- PCT/EP2026/062636
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-06
- Filing Date
- 2026-05-01
- Publication Date
- 2026-11-12
AI Technical Summary
Existing foam manufacturing methods struggle to achieve uniform pore sizes and homogeneous distribution, limiting structural strength and design intricacy, especially in additively manufactured foams for sound and electromagnetic absorption.
Employing a soluble porogen, such as alkali metal or alkali earth metal-based salts, in additive manufacturing processes like SLA or SLS to control pore size and density, combined with specialized fillers for enhanced sound and electromagnetic absorption.
Produces foams with less than 50% variation in pore thickness, enabling intricate designs and improved acoustic and electromagnetic absorption capabilities while maintaining structural integrity.
Smart Images

Figure EP2026062636_12112026_PF_FP_ABST
Abstract
Description
[0001] Improved manufacture
[0002] FIELD OF THE INVENTION
[0003] The invention relates to novel foam structures, methods of their preparation and used thereof. In particular, the invention provides novel methods of preparing additively manufactured high absorbing foams.
[0004] BACKGROUND OF THE INVENTION
[0005] Typically, foams are manufactured from a liquid monomer that is shaped through the application of a foaming agent during its polymerisation. In order to produce a foam containing a filler material the filler must first be mixed thoroughly with the monomer. A foaming agent is applied generating the final filled foam structure.
[0006] With respect to traditional and current foam manufacturing methods, it is difficult to control the size of the pores generated leading to an uneven or inconsistent pore sizes and limited homogeneous pore distribution, reducing the structural strength of the foam. It is also difficult using existing materials and methods to create intricate designs with a foam.
[0007] Additive manufacture is not typically the method used to manufacture foams, in recent years there has been an increase in ceramic foam production for the areas of orthopaedics in which porous bone analogue is produced to aid in natural bone recovery. Foams loaded with absorbent material, such as carbon, find use within the acoustics and construction dampening sound within rooms and shielding sensitive equipment from sound or electromagnetic radiation.
[0008] Two production methods show the most value for foam production, stereolithography (SLA) and selective laser sintering (SLS).
[0009] Stereolithography (SLA) 3D printing is widely used to create intricate and high-resolution structures from a liquid photopolymer resin. A laser system selectively cures the resin through a photo polymerisation reaction in a layered structure, which is followed by a wash in isopropanol and further curing under UV to achieve a higher strength structure. A range of materials can be used with this technology; including filler particles within a resin system see for example Manapat J.-Z.; Chen Q.; Ye P.;Advincula R.-C. 3D printing of polymer nanocomposites via stereolithography, Macromolecular Materials and Engineering, 2017, 9, 302.
[0010] For SLA printing, photopolymers are used, which are a blend of polyurethane acrylate, acrylate monomer and photoinitiator. An example composition used is 50% epoxy resin, 40% hexamethylene diacrylate, 5% N-(Dimethylcarbamoyl) glycine and 5% hydrocycyclohexyl phenyl ketone. The constituent parts are formulated to achieve specific properties in the final print, resulting in a very wide range of photopolymer resins that are available to be used.
[0011] Selective Laser Sintering (SLS) operates in a similar way to SLA, using a laser to produce high-resolution structures. Unlike SLA, SLS utilises a polymer powder as a feedstock material. The powder is heated by action of the laser and fused together into a 3D structure. For applications of SLS printing see Charoo N.-A.; Ali S.-F.-B; Mohamed E.-M; Kuttolamadom M.-A.; Ozjan T.; Khan M.-A.; Rahman Z.; Selective Laser Sintering 3D printing - an overview of the technology and pharmaceutical applications, Drug Development and Industrial Pharmacy, 2020, 46, 6, 869-877.
[0012] Various polymer powders are used in SLS printing techniques, including polyamide (nylon), polystyrene, polypropylene, TPU, PEEK and polycarbonate all of which can be mixed with functional additives such as fillers.
[0013] Novel and improved methods of producing high absorbing foams through additive manufacturing methods are needed.
[0014] SUMMARY OF INVENTION
[0015] Accordingly, the present invention provides methods for preparing high absorbing additively manufactured foams with uniform porosity thereby according to the appended claims.
[0016] In one embodiment various additive manufacturing methods can be employed to rapidly produce bespoke foams using a soluble substance of the dimensions of the desired pores, for example a salt such as sodium chloride (NaCI).
[0017] In one embodiment, the present invention provides a method of preparing an additively manufactured foam material through the use of a soluble porogen.By soluble porogen, we mean a water-soluble particle, typically an alkali metal / alkali earth metal-based salt.
[0018] In one embodiment the salts used have a particle size between 1-500 micron.
[0019] By salt, we mean a compound formed through the reaction of an acid and base in which the hydrogen of the acid is all or partially replaced by the base cation.
[0020] By high absorbing, we mean that the foams contain both an additional filler material and a specialised internal structure to increase the absorption of sounds and incident electromagnetic radiation.
[0021] In one embodiment the filler material comprises an inorganic compound or a mix thereof.
[0022] By specialised internal structure, we mean a unique internal geometry produced through the stereolithographic process, the geometry of which benefits the acoustic and electromagnetic (EM) absorbing effects of the filled foam.
[0023] By additively manufactured we mean that the foams were produced through a SLA resin process or a SLS powder bed process.
[0024] SLA and SLS 3D printing devices are commercially available and may be obtained from a number of suppliers.
[0025] By uniform porosity, we mean that pores are formed with less than a 50% variation in thickness, or less than 30% variation, or less than 10% variation.
[0026] By utilising a soluble porogen of known particle size it is possible to selectively control the pore size within a foam, by varying the loading of the porogen the density can also be controlled.
[0027] In one embodiment the porogen is selected from one or more of soluble salts of sodium, potassium, ammonium, copper, magnesium, lithium, ruthenium or any combination thereof, and in particular salts in the form of chlorides, sulphates, nitrates and bromides.
[0028] In one embodiment a dispersing aid is used to aid in homogenisation of the resin system, the dispersing aid is an organic surfactant that may be but is not limited to a polyacrylate salt, polymethylalkylsiloxane, polyethylene glycol, alkyl ammonium salts.In one embodiment, the pore size of the foam ranges from 1 -500 micrometres, or 20-400 micrometres, or 50-200micrometres or more specifically 10-150m icrometers. In one embodiment, the absorbing fillers may be carbon black, mica, silicon carbide, iron, silicon dioxide, graphite, spinels with general structure (A1B2O4) and Perovskites with general formula (AxCyBzDwO4). Where A, B, C and D relate to an elements that may be, but are not limited to, iron, copper, silver, gold, nickel, manganese, europium, neodymium, lithium, calcium, samarium, gadolinium, aluminium, lead, silicon, and zinc.
[0029] Brief Description of the Drawings
[0030] Figure 1 Schematic representation of resin system containing a soluble porogen dispersed within.
[0031] Figure 2 Schematic representation of SLA printing equipment used.
[0032] Figure 3 SEM microscopy of pore structure of foam sample.
[0033] DETAILED DESCRIPTION
[0034] Resin systems as shown in Figure 1 can be prepared, for example as detailed below.
[0035] A soluble porogen [1] with particle size ranging 20-100 micrometres and highly absorbing fillers [4] are dispersed within a photopolymer resin [2] using a stirrer. The viscosity of the resin system [3] is measured and dispersant is added to lower it to an acceptable level. The resin is printed as shown in Figure 2 into coupons measuring 20x30x8mm. The appropriate layer thickness and exposure durations for SLA printing were determined through UV penetration testing and UV-Vis spectrometry. The coupons are weighed then soaked in 60°C water for 74 hours before mass loss is measured. Samples are ground down to an appropriate size and the absorbing performance of the foam measured.
[0036] Foam samples were evaluated microscopically [SEM] as shown in Figure 3 to determine the surface pore sizes. As shown a range of pore sizes and distinct layers can be observed.In one embodiment the resin viscosity can be optimised as required.
[0037] In one embodiment the tensile properties can be optimised as required.
[0038] The benefits of foams prepared according to the invention include one or more of: a reduction in weight whilst maintaining structural properties, the ability to print more intricate structures, thermal and acoustic insulation and uses in a range of applications such as building design, radar control and improved crew comfort in vehicles.
[0039] Example Foam Preparations Follow:
[0040] Example 1
[0041] Sodium chloride 65g (table salt, Lidl UK) is ball milled at 500RPM for 30 minutes until a fine powder is produced, the powder is sieved to ensure the grain size was smaller than 100 micron. The salt is dispersed in 45ml of photopolymer resin (Elegoo standard - Translucent, Elegoo). To the mixture, 5g of dispersant is added (BYK 187, BASF). The system is mixed using a high shear mixer at 300RPM until a homogenous mixture is formed.
[0042] The resin system is printed using an SLA printer at 100 micron layer thickness, coupons are produced for testing. The porogen is dissolved out in a 60°C water bath for 74 hours.
[0043] Example 2
[0044] Sodium chloride 60g is ball milled at 500RPM for 30 minutes until a fine powder is produced. The salt is dispersed in 45ml of photopolymer resin (Elegoo standard -Translucent, Elegoo) and 5g of mica filler. To the mixture, 5g of dispersant is added (BYK 187, BASF). The system is mixed using a high shear mixer at 300RPM until homogenised. The resin system is printed through an SLA process and the produced parts are soaked in water at 60°C for 74 hours.Example 3
[0045] Sodium chloride 75.3g is ball milled at 500RPM for 30 minutes until a fine powder is produced. The salt is dispersed in 34ml of photopolymer resin (Elegoo standard-Translucent, Elegoo) to which 1 ,6g of carbon black is added. To the mixture 5.5g of dispersant (BYK 077, BASF) is added. The mixture is mixed in using a high shear mixer at 300RPM until homogenised. The resin system is printed through an SLA process and the produced parts are soaked in water at 60°C for 74 hours.
[0046] Example 4
[0047] Magnesium sulphate 60g is ball milled at 500rpm for 30 minutes until a fine powder is produced. The magnesium sulphate is dispersed in 40ml of photopolymer resin (Elegoo standard- Translucent, Elegoo). To the mixture 6g of dispersant (BYK 077, BASF) is added. The resin system is printing through an SLA process, the produced parts are soaked in water at 60°C for 74 hours. Foams produced have a small pore size.
[0048] Example 5
[0049] Copper nitrate 50g at 100 micron (Sigma Aldrich) was mixed into 50ml of photopolymer resin (Elegoo standard- Translucent, Elegoo). The resin system is printed through the SLA process and the resulting parts are soaked for 74h in 60°C water.
[0050] Example 6
[0051] Sodium chloride 50g (particle size distribution of 150 ±25 micron) with 150g of nylon 12 powder 65 micron (Formlabs). To the mixture, 50g of silicon carbide (Goodfellows) added and homogenised using a Turbula® mixer. The powder was loaded into a SLS printer and test parts were produced. The produced parts were soaked in water at 60°C for 74 hours. Foams produced have uniform pore channels.Leaching Trial
[0052] Sample Initial mass (g) Final mass (g) Mass loss % Pore size (pm) 1 10.89 5.3 51 50-55
[0053] 2 8.16 3.75 54 45-84
[0054] 3 11.32 4.73 58 90-125
[0055] 4 11.37 7.05 38 22-43
[0056]
[0057] Pore size was determined through microscopy (SEM) pore size relates closely to the particle size of porogen used. Mass lost relates to the loss of porogen through dissolution.
Claims
8CLAIMS1. A method of producing foams for acoustic absorptionwherein said foams are loaded with acoustic fillersand wherein the porosity of the foam is controlled through the use of a soluble porogen systemsaid system comprising a combination of soluble porogen and acoustic filler material in a polymer matrix.
2. A method according to any proceeding claim in which the polymer matrix is either a photopolymer resin in the presence of a dispersing aid or a thermoplastic polymer.
3. A method according to any proceeding claim in which the dispersing aid is selected from one or more of a polyacrylate salt, polymethylalkylsiloxane, polyethylene glycol and alkyl ammonium salts.
4. A method according to any proceeding claim wherein the soluble porogen is selected from water soluble salts.
5. A method according to any preceding claim wherein the water soluble salt is selected from one or more of sodium chloride, sodium nitrate, sodium sulphate, potassium chloride, potassium nitrate, potassium sulphate, copper nitrate, copper sulphate, copper chloride, magnesium sulphate, magnesium chloride, magnesium nitrate, ammonium chloride, ammonium nitrate and ammonium sulphate.
6. A method according to any proceeding claim wherein the acoustic filler material is an inorganic compound or functional particles or mixtures thereof.
7. A method according to claim 6 wherein the inorganic compound is selected from one or more of carbon black, zeolites, mica, silicon carbide or carbon nanotubes.
98. A method according to any proceeding claim in which the soluble porogen has particle size between 1-500 microns, or 125 - 175 microns, or 20-400 microns, or 50-200 microns or 10-150 microns or 20-100 microns.
9. A method according to claim 8 having a particle size of approximately 125 - 175 microns.
10. A method according to any preceding claim wherein sodium chloride with grain size smaller than 100 microns is dispersed in photopolymer resin using BYK dispersant.
11. A method according to any preceding claim wherein sodium chloride with particle size distribution of 150 ±25 microns is dispersed in photopolymer resin using BYK dispersant.
12. A method according to any preceding claim wherein magnesium sulphate of fine grain size is dispersed in photopolymer resin using BYK dispersant.
13. A method according to any proceeding claim in which foam material is further processed into a finished article.
14. A foam or foamed finished article obtainable by a method according to any preceding claim.
15. The use of a foam or foamed article according to claim 14 for acousticprotection.