Tubular ethylene acrylate copolymers and films produced therefrom
The tubular free-radical polymerization process with controlled acrylate content and temperature enhances melt strength and branching in ethylene acrylate copolymers, addressing limitations in existing configurations and improving film production stability and processability.
Patent Information
- Application Number
- PCT/ES2025/070258
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
Existing tubular polymerization reactor configurations for acrylate copolymers limit the development of branched polymer topologies and melt strength, and increasing temperature to enhance long-chain branching is risky due to side reactions and radical decomposition.
A tubular free-radical polymerization process with a moderate acrylate content and controlled reactor temperature range produces ethylene acrylate copolymers with high melt strength and adjustable crystallization temperature, resulting in improved melt rheology and processability.
The ethylene acrylate copolymers exhibit enhanced melt strength, shear flow, and long-chain branching, improving processability and stability for large bubble film applications.
Smart Images

Figure IMGF000009_0001 
Figure IMGF000010_0001 
Figure IMGF000010_0002
Abstract
Description
TUBULAR COPOLYMERS OF ETHYLENE ACRYLATE AND FILMS PRODUCED THEREOF TECHNICAL SECTOR
[0001] The embodiments described in this invention generally relate to acrylate copolymers manufactured by a tubular production optimization process for film applications. BACKGROUND OF THE INVENTION
[0002] Acrylate copolymers are often used in large bubble applications, including greenhouse films. While it is known in the art that tubular polymerization reactor configurations can provide such materials with longer ethylene sequence lengths and higher maximum melt temperatures for the same polar comonomer content, this plug-flow nature has been found to impede the development of branched polymer topologies and limit melt strength to a given melt rate. Furthermore, there is a limit to how much temperature can be increased to enhance long-chain branching in the presence of polar monomers due to the risk of side reactions and radical decomposition.
[0003] Consequently, there is a need for acrylate copolymers that have high melt strength and an adjustable crystallization temperature to improve melt rheology and processability for large bubble (film) applications. SUMMARY OF THE INVENTION
[0004] The embodiments of the present invention satisfy these needs by providing an ethylene acrylate copolymer produced by a tubular free-radical polymerization process, comprising a moderate acrylate content and reactor temperature range, resulting in melt strength and shear flow comparable to autoclave materials. The combination of the tubular production characteristics with a moderate acrylate content exhibits high melt strength, which correlates with an increased maximum melt temperature and improved long-chain branching. This combination of characteristics allows for improved processability and stability of the ethylene acrylate copolymer for large bubble (film) applications.
[0005] According to at least one embodiment of the present invention, ethylene acrylate copolymers produced by a tubular free-radical depolymerization process are provided. The ethylene acrylate copolymer comprises between 9 wt% and 15 wt% acrylate; a molecular weight distribution (MWD=Mw / Mn) less than or equal to 7.5, wherein Mw is the weight-average molecular weight and Mn is the number-average molecular weight measured by gel permeation chromatography (GPC); a melting point of at least 99 °C measured by differential scanning calorimetry (DSC); and a crystallization temperature (Tc) of at least 99 °C. g ) of at least 85 °C as measured by DSC.
[0006] These and other embodiments are described in more detail in the following Detailed Description of the invention. DETAILED DESCRIPTION OF THE INVENTION
[0007] The specific embodiments of the present invention will now be described. However, the invention can be incorporated in various ways and should not be interpreted as being limited to the embodiments set forth herein. Rather, these embodiments are provided to make this invention comprehensive and complete and to fully convey the scope of the subject matter to those skilled in the art.
[0008] The term "polymer" refers to a polymeric compound prepared by the polymerization of monomers, whether of the same or different types. Therefore, the generic term polymer encompasses the term "homopolymer," which generally refers to a polymer prepared from a single type of monomer, as well as "copolymer," which refers to a polymer prepared from two or more different monomers.
[0009] "Ethylene-based polymer" means a polymer comprising more than 50% by weight of units derived from the ethylene monomer. This includes polyethylene-based polymers, including polyethylene homopolymers or copolymers (i.e., units derived from two or more comonomers).
[0010] As used in this invention, "multilayer film" and "multilayer films" refer to a structure or structures having multiple layers. In contrast, "monolayer film" is a single-layer film.
[0011] The amount of a component (e.g., acrylate) is provided in this invention as a weight percent (% wt), based on the total weight of the ethylene acrylate copolymer (i.e., the product of the tubular free-radical polymerization process described herein), unless otherwise stated.
[0012] The ranges in this invention may be expressed from "approximately" a particular value and / or to "approximately" another particular value. When such a range is expressed, another embodiment includes from one particular value and / or to the other particular value. Similarly, when values are expressed as approximations, by using the antecedent "about," the particular value shall be understood to constitute another embodiment. It shall be further understood that the endpoints of each range are significant both in relation to and independently of the other endpoint.
[0013] The terms "comprises," "includes," "has," and their derivatives are not intended to exclude the presence of any additional component, step, or process, whether or not specifically disclosed. For the avoidance of doubt, all compositions claimed by using the term "comprises" may include any additive, adjuvant, or additional compound, whether polymeric or otherwise, unless otherwise stated. Conversely, the expression "consisting essentially of" excludes from the scope of any subsequent recitation any other component, step, or process, except those not essential to operability. The term "consisting of" excludes any component, step, or process that is not specifically delineated or enumerated.
[0014] Reference will now be made in detail to the embodiments of various ethylene acrylate copolymers and films comprising ethylene acrylate copolymers.
[0015] As described below, it was found that a combination of tubular production characteristics with a moderate acrylate content results in an ethylene acrylate copolymer with comparable melt strength and shear thinning properties to autoclave materials, with minimal risk of processing problems. Surprisingly, it was found that an ethylene acrylate copolymer must comprise an appropriate amount of polar comonomer (i.e., 9 wt% to 15 wt% acrylate) and a suitable comonomer distribution derived from the tubular free-radical polymerization process to provide a set of thermal and mechanical characteristics optimized for blown film production.
[0016] Ethylene acrylate copolymers
[0017] In one or more embodiments of the present invention, the ethylene acrylate copolymers are produced by a tubular free-radical polymerization process. In one or more embodiments, the ethylene acrylate copolymer comprises 9 wt% to 15 wt% acrylate; a molecular weight distribution (MWD=Mw / Mn) less than or equal to 7.5, wherein Mw is the weight mean molecular weight and Mn is the number mean molecular weight measured by gel permeation chromatography (GPC); a melting point of at least 99 °C measured by differential scanning calorimetry (DSC); and a crystallization temperature of at least 85 °C measured by DSC.
[0018] In one or more embodiments, the ethylene acrylate copolymer comprises 9 wt% to 15 wt% acrylate. It has been found that an ethylene acrylate copolymer comprising an acrylate comonomer of 9 wt% to 15 wt% comprises a suitable amount of polar acrylate comonomer to increase long-chain branching, reduce the risk of side reactions, and reduce the radical composition of the copolymer. For example, in embodiments, the ethylene acrylate copolymer comprises 9 wt% to 15 wt%; 9 wt% to 13 wt%; 9 wt% to 11 wt%; 11 wt% to 15 wt%; 13 wt% to 15 wt%; or even 12 wt% to 14 wt% acrylate comonomer, based on the total weight of the ethylene acrylate copolymer.
[0019] In one or more embodiments, the molecular weight distribution (MWD = Mw / Mn) of the ethylene acrylate copolymer is less than or equal to 7.5 as measured by conventional gel permeation chromatography (GPC). In further embodiments, the MWD of the ethylene acrylate copolymer is greater than or equal to 6.0. For example, in embodiments, the ethylene acrylate copolymer comprises a molecular weight distribution of greater than or equal to 6.0 to 6.5, from 6.5 to 7.0, or from 7.0 to less than or equal to 7.5. Not being limited by theory, it is believed that ethylene acrylate copolymers produced by the tubular free-radical polymerization process as described in this invention comprise a higher relative degree of heterogeneity along the polymer backbone and, therefore, a lower molecular weight distribution relative to the conventional ethylene acrylate copolymer produced by an autoclave.
[0020] In one or more embodiments, the melting point of the ethylene acrylate copolymer is at least 99 °C as measured by differential scanning calorimetry (DSC). In one or more embodiments, the melting point of the ethylene acrylate copolymer is 100 °C.
[0021] In one or more embodiments, the crystallization temperature of the ethylene acrylate copolymer is at least 85 °C as measured by differential scanning calorimetry (DSC). In one or more embodiments, the crystallization temperature of the ethylene acrylate copolymer is at least 86 °C, or at least 87 °C. In one or more embodiments, the crystallization temperature of the ethylene acrylate copolymer is 87 °C.
[0022] In one or more embodiments of the present invention, the ethylene acrylate copolymers comprise a C1-C6 acrylate. In some embodiments, the C1-C6 acrylate may comprise an unsubstituted or substituted C1-C6 acrylate. For example, the ethylene acrylate copolymers may include methyl acrylate, ethyl acrylate, and butyl acrylate, including combinations thereof. According to at least one embodiment of the present invention, the ethylene acrylate copolymers comprise n-butyl acrylate.
[0023] In one or more embodiments of the present invention, the ethylene acrylate copolymers comprise a density of 0.910 g / cc to 0.945 g / cc. For example, the ethylene acrylate copolymers may comprise a density of 0.910 g / cc to 0.940 g / cc, 0.910 g / cc to 0.935 g / cc, 0.910 g / cc to 0.930 g / cc, 0.920 g / cc to 0.940 g / cc, or 0.920 g / cc to 0.930 g / cc. According to at least one embodiment of the present invention, the ethylene acrylate copolymers comprise a density of 0.924 g / cc.
[0024] In one or more embodiments of the present invention, the ethylene acrylate copolymers comprise a melt strength (MS) that is greater than or equal to C-[(I2)D], where C is 13.5 maximum strength per grams eluted per 10 minutes (cN / (g / 10 min)), I2 is the melt strength measured according to ASTM D 1238 at 190 °C and a load of 2.16 kg, and D is -0.28. For example, in one or more embodiments of the present invention, the ethylene acrylate copolymers comprise a melt strength of at least 17.0 cN, at least 18.0 cN, at least 19.0 cN, at least 20.0 cN, or even at least 21.0 cN. In other embodiments, the melting strength is 17.0 cN to 25.0 cN, 17.0 cN to 20.0 cN, or 20.0 cN to 25.0 cN.
[0025] In one or more embodiments of the present invention, the ethylene acrylate copolymers comprise a melt flow index (flow rate) I2 less than or equal to 0.35 g / 10 min. For example, in one or more embodiments, the ethylene acrylate copolymers comprise a melt flow index I2 less than or equal to 0.30 g / 10 min, less than or equal to 0.27 g / 10 min, or less than or equal to 0.25 g / 10 min. Without being limited by theory, it is believed that the ethylene acrylate copolymers may comprise a melt flow index I2 greater than or equal to 0.20 g / 10 min. For example, in embodiments, the ethylene acrylate copolymers comprise greater than or equal to 0.21 g / 10 min, greater than or equal to 0.22 g / 10 min, or even greater than or equal to 0.23 g / 10 min. According to at least one embodiment, the melting index 12 is 0.24 g / 10 min.
[0026] In one or more embodiments of the present invention, the ethylene acrylate copolymers comprise a melt flow index (flow rate) less than or equal to 6.0 g / 10 min. For example, in one or more embodiments, the ethylene acrylate copolymers comprise a melt flow index less than or equal to 5.5 g / 10 min, less than or equal to 5.0 g / 10 min, or less than or equal to 4.5 g / 10 min. In other embodiments, the melt flow index is from 4.0 g / 10 min to 5.0 g / 10 min, or from 4.0 g / 10 min to 4.5 g / 10 min.
[0027] In one or more embodiments of the present invention, the ethylene acrylate copolymers comprise a melt flow ratio I10 / I2 of at least 17.0, where I10 and I2 are melt flow indices. For example, in one or more embodiments, the ethylene acrylate copolymers comprise a melt flow ratio I10 / I2 of at least 17.0, at least 17.5, or even at least 18.0. In other embodiments, the melt flow ratio I10 / I2 is from 17.0 to 25.0, or from 17.0 to 20.0.
[0028] In one or more embodiments of the present invention, the ethylene acrylate copolymers comprise a melt viscosity ratio (V0.1 / V100) of at least 35, where V0.1 is the viscosity measured at 0.1 radians / second (rad / s) and 190 °C and V100 is the viscosity measured at 100 rad / s and 190 °C. In one or more embodiments, the ethylene acrylate copolymers comprise a melt viscosity ratio of at least 40. In other embodiments, the melt viscosity ratio may range from 35 to 40, or from 36 to 38.
[0029] In one or more embodiments of the present invention, the ethylene acrylate copolymers comprise an average molecular weight z (M z) of less than 750,000 g / mol, less than 700,000 g / mol, less than 650,000 g / mol, or even less than 600,000 g / mol as measured by GPC. In other embodiments, the average molecular weight z can range from 500,000 g / mol to 750,000 g / mol, from 550,000 g / mol to 700,000 g / mol, or from 575,000 g / mol to 650,000 g / mol.
[0030] Blown films
[0031] According to at least one embodiment of the present invention, a film comprises the ethylene acrylate copolymer as described in this invention.
[0032] In one or more embodiments of the present invention, the film comprises a single-layer or multi-layer film. According to at least one embodiment, the film is a single-layer film.
[0033] In one or more embodiments, the single-layer film comprises a thickness of 10 micrometers (µm) to 250 µm. For example, in one or more embodiments, the single-layer film comprises a thickness of 50 µm or 250 µm.
[0034] In one or more embodiments of the present invention, the film is a greenhouse film.
[0035] In further embodiments, the blown film bubble is formed by a free-radical tubular polymerization process with an inflation ratio of 1:4 or 1:3. Furthermore, the formation of the single-layer blown film bubble can occur at a temperature of 170°C to 250°C, or 190°C to 230°C. The output rate can be from 10 kilograms per hour (kg / h) to 50 kg / h, or from 20 kg / h to 40 kg / h.
[0036] In one or more embodiments, the multilayer film comprises more than 65% by weight of ethylene acrylate copolymer. In some embodiments, the multilayer film comprises more than 70% by weight of ethylene acrylate copolymer. In addition, in some embodiments, the multilayer film comprises less than 80% by weight of ethylene acrylate copolymer.
[0037] Reference will now be made in detail to several embodiments of the present invention for an ethylene acrylate copolymer produced by a tubular free-radical polymerization process for manufacturing monolayer and multilayer films. In one or more embodiments, the process comprises the formation of a blown monolayer film.
[0038] TEST METHODS
[0039] The test methods include the following:
[0040] Impact from falling dart
[0041] To test dart drop impact, samples were measured according to ISO 7765-1 / 1998. Dart drop impact values were reported in grams (g).
[0042] Elmendorf Tear
[0043] To test the Elmendorf tear strength, samples were measured according to ASTM D1922-09. Elmendorf tear strength values were expressed in grams (g).
[0044] Film tenacity, tensile strength, and tensile elongation
[0045] To test film toughness, tensile strength at the elastic limit, tensile strength at break, and elongation at break, samples were measured according to ASTM D527-3. Film toughness values are reported in megajoules per cubic meter (MJ / m³). 3 The tensile strength at yield and tensile strength at break values are given in millipascals (MPa). Elongation at break is reported as a percentage (%).
[0046] fusion index and fusion flow ratio
[0047] To test the L-value, lio-value, and 110 / 12 melt flow ratio, ethylene acrylate copolymer samples were measured according to ASTM D1238 at 190 °C and 2.16 kg and 10 kg, respectively. The L-value and lio-value are expressed in grams eluted per 10 minutes (g / 10 min).
[0048] Melting resistance (MSI)
[0049] Melt strength tests were performed on a Góttfert Rheotester 2000 or Góttfert Rheograph 25 capillary rheometer paired with a Góttfert Rheotens 71.97 according to ASTM D1238 at 190 °C and 2.16 kg. The tests were performed isothermally using a die with an entry angle of 180°, a diameter of 2.0 millimeters (mm), and a length of 30 mm.
[0050] Before starting the test, the granulated sample was loaded into the capillary barrel and allowed to equilibrate at the test temperature for 10 minutes. During the test, the piston inside the barrel applied a constant force to the molten sample to achieve an apparent wall shear rate of 38.16 per second ( s l ), and the molten mass was extruded through the die at an exit velocity of approximately 9.7 mm / s. 100 mm below the die exit, the extrudate was guided through pairs of Rheotens wheels, which accelerated at a constant velocity of 2.4 mm / s. 2The extrudate's response to the applied tensile force was measured. The Rheotens wheel pairs were toothed and spaced 0.4 mm apart. Melt strength test results were documented in force-versus-Rheotens wheel speed graphs using the Excel macro RtensEvaluations2007. The melt strength value is reported as the maximum force (cN) before the extruded strand broke. The corresponding Rheotens wheel speed at the strand breakage point was documented as the pull limit.
[0051] Nuclear magnetic resonance (NMR) for comonomer quantification
[0052] Quantitative spectra of 13C were obtained using a DC cryoprobe installed on a 500 MHz spectrometer. The spectra obtained are referenced to the main signal of ethylene at 30 ppm. A 0.15 g × 0.20 g sample was dissolved in a solvent composed of 60% 1,1,2,2-tetrachloroethane-D2 (TCE-D2), 40% 1,1,2,2-tetrachloroethane-H2 (TCE-H2), 0.025 M chromium(III) acetylacetonate, and 100 ppm Irgafos® 168.
[0053] Differential scanning calorimetry (DSC)
[0054] DSC tests were performed on a TA Instruments (Q2000 / Discovery) machine equipped with a refrigerated cooling system (RCS) and an autosampler module at a nitrogen purge gas flow rate of 50 mL / min. Each sample was pressed into a thin film and melted in the press at approximately 190°C. The melted sample was then allowed to cool to room temperature (i.e., approximately 25°C). From the cooled sample, a 3-mg to 10-mg sample with a diameter of 6 mm was extracted from the cooled polymer, weighed, placed in a lightweight aluminum tray (i.e., containing 50 mg of calcium), and sealed. Analyses were then performed to determine the thermal properties of the samples. The thermal behavior of the samples was determined by increasing and decreasing the sample temperature to create a heat flow versus temperature profile.First, the sample was rapidly heated to 180 °C and held isothermally for 5 minutes to eliminate its thermal history. Next, the sample was cooled to -40 °C at a rate of 10 °C / minute and held isothermally at -40 °C for 5 minutes. Then, the sample was heated to 150 °C (i.e., the "second heat" ramp) at a rate of 10 °C / minute. The cooling and second heat curves were recorded. The cooling curve was analyzed by establishing reference endpoints from the start of crystallization at -20 °C. The heat curve was analyzed by establishing reference endpoints from -20 °C to the end of the melt. The determined values, including the maximum melting temperature (Tm), were analyzed. m ), the maximum crystallization temperature (Te), the heat of fusion (Hf) (in joules per gram) and the percentage (%) of crystallinity of the polyethylene samples were calculated using Equation 1: 100 (EC1) v
[0055] Density
[0056] The density measurements of the ethylene acrylate copolymers were performed in accordance with ASTM D792, Method B. Density values are expressed in grams per cubic centimeter (g / cc).
[0057] Conventional gel permeation chromatography (GPC)
[0058] The chromatographic system consisted of a PolymerChar GPC-IR® high-temperature GPC chromatograph (Valencia, Spain) equipped with an internal IR5 infrared detector. The autosampler oven compartment was set to 160 °C and the column compartment to 150 °C. The columns used were four 30 cm, 20 µm (µm) Agilent "Mixed A" linear mixed-bed columns. The chromatographic solvent used was 1,2,4-trichlorobenzene, composed of 200 ppm butylhydroxytoluene (BHT). The solvent source was sprayed nitrogen. The injection volume was 200 µL and the flow rate was 1.0 mL s / min.
[0059] The GPC column array was calibrated using Agilent EasiCal PS-1 (lot number 0006640482) and PS-2 (lot number 0006583993) narrow molecular weight distribution polystyrene standards with molecular weights ranging from 580,000 g / mol to 6,545,000 g / mol. The standards were purchased from Agilent Technologies. The polystyrene standards were prepared by placing two spatulas for each standard into a nitrogen-sprayed, septate-cap vial, and adding 8 mL of solvent through a PolymerChar high-temperature autosampler. The standards were dissolved for 2 hours at 160 °C under gentle stirring. The standard maximum molecular weights of polystyrene were converted to molecular weights of polyethylene using Equation 2 (as described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)): where M is the molecular weight, A is equivalent to 0.4113 and B is equal to 1.0.
[0061] A third-order polynomial was used to adjust the respective polyethylene equivalent calibration points.
[0062] To monitor for deviations over time, a flow marker (decane) was introduced into each sample using a micropump controlled by the PolymerChar GPC-IR system. This flow marker (FM) was used to linearly correct the pump flow rate (nominal flow rate) for each sample by aligning the RV of the respective decane peak within the sample (RV (FM Sample)) with the decane peak within the narrow standards calibration (RV (FM calibrated)). Any change over time in the decane marker peak was assumed to correspond to a linear change in the flow rate (effective flow rate) throughout the run. After calibrating the system based on a flow marker peak, the effective flow rate (relative to the narrow standards calibration) was calculated using Equation 3. Processing of the flow marker peak was performed using PolymerChar GPCONe™ software.An acceptable flow correction is such that the effective flow rate must be within ±0.5% of the nominal flow rate.
[0064] The total plate count for the GPC column array was performed using decane, which was introduced into the blank sample via a micropump controlled by the PolymerChar GPC-IR system. The plate count for the chromatographic system must exceed 18,000 for the four 30 cm, 20 µm Agilent "Mixed A" linear mixed-bed columns.
[0065] The samples were prepared semi-automatically using PolymerChar "Instrument Control" software, in which the samples were fixed at a weight of 2 mg / ml, and the solvent (comprising 200 ppm of BHT) was added to a septate vial with a septum cap that had been pre-sprayed with nitrogen, via the PolymerChar high-temperature autosampler. The samples were dissolved for 3 hours at 160 °C under "low-speed" stirring.
[0066] The calculations for Mn, Mw, and Mz were based on GPC results using the internal IR5 infrared detector of the PolymerChar GPC-IR chromatograph according to Equations 3-5, using PolymerChar GPCOne™ software, the baseline subtracted IR chromatogram at each equally spaced data collection point (i), and the equivalent molecular weight of polyethylene obtained from the narrow standard calibration curve for point (i) of Equation 1. The baseline was plotted using PolymerChar GPCOne™ software in a straight line from a point just before the sample retention volume to a point after the sample retention volume but before the n-decane peak, where this point lies at the minimum signal value of the IR5 detector measurement channel.The two integration limits for joining the baseline subtracted chromatogram are found at the intersection of the baseline with the IR5 detector measurement channel signal before the maximum retention volume and the retention volume point that corresponds to a PE equivalent molecular weight value, according to ASTM-D6474-99, of 500 g / mol determined from Equation 2 using the narrow standard molecular weight calibration curve of polystyrene. (EC 5)
[0069] (EC 6)
[0070] Dynamic mechanical spectroscopy (DMS) frequency sweep
[0071] All DMS frequency tests were performed on either an ARES-G2 rheometer or a DHR-3 rheometer, both manufactured by TA Instruments. Data analysis was performed using TA Instruments' TRIOS software.
[0072] Prior to testing, the test specimens were placed in a 1.5-inch diameter cavity with a thickness of 3.10 mm and compression molded in a hydraulic press for 6.5 minutes at a temperature of 190 °C and a pressure of 25,000 pounds. After cooling to room temperature at a rate of 10 °C / min, the specimens were removed for theological testing.
[0073] The DMS frequency sweep was performed using parallel 25 mm plates at frequencies ranging from 0.1 rad / s to 100 rad / s. The test gap between the plates was 1.8 mm, and a strain was used that satisfied linear viscoelastic conditions. Each test was conducted under a nitrogen atmosphere and isothermal conditions at 190 °C. To initiate the DMS test, the rheometer oven was first allowed to equilibrate at 190 °C for at least 30 minutes before loading the sample into the test geometry. The sample was then equilibrated in the oven, with the door closed, for 1 minute. The test gap was set to 1.8 mm, and the sample was allowed 5 minutes to relax the resulting normal force. The oven was then quickly opened, and the sample was trimmed to remove any lumps. The DMS measurement was initiated after the oven was resealed.During the test, the shear elastic modulus (G'), viscous modulus (G") and complex viscosity were also measured.
[0074] EXAMPLES
[0075] The following examples illustrate features of the present invention, but are not intended to limit its scope. The following experiments compared the performance of a conventional ethylene acrylate copolymer and a novel ethylene acrylate copolymer, both produced from the optimized tubular production process as described in this invention.
[0076] Ethylene acrylate copolymers
[0077] The following copolymers were used for these experiments:
[0078] Comparative Example 1 (CE1) is REPSOL EBANTIX® E13O3, a conventional ethylene-butylate copolymer that is commercially available from Repsol. The properties of CE1 are provided in Table 2.
[0079] Inventive Example (IE1) is an ethylene-butyl acrylate copolymer produced according to the free-radical tubular polymerization process as described in this invention. The processing conditions for the free-radical tubular polymerization are provided in Table 1. The properties of IE1 are provided in Table 2 together with the properties of CE1.
[0080] Table 1. Conditions of the tubular free radical process.
[0081] Table 2. Properties of Inventive Example 1 (IE1) and Comparative Example 1 (CE1).
[0082] As can be seen in Table 2, the melting and crystallization temperatures of IE1 are higher than those of CE1. Furthermore, IE1 was found to exhibit a higher melting temperature (Tm), which has been shown to improve processability when producing large bubble films.
[0083] Furthermore, IE1, comprising an ethylene acrylate copolymer produced by a tubular free-radical polymerization process, exhibits melt strength and shear thinning comparable to CE1. The comparable melt strength of the polymers produced by the tubular process (i.e., IE1) relative to the polymers produced in an autoclave (i.e., CE1) indicates improved long-chain branching. It is known in the art that improved long-chain branching is beneficial for increasing film stability in bubble applications (as described in Barry Morris, Chapter 13, pages 542-543). Additionally, IE1 exhibits a higher melt temperature relative to CE1, demonstrating improved processability when producing large bubble films. Furthermore, IE1 shows a lower average mass compared to CE1.Unconstrained by theory, a lower average mass can improve film optics by reducing film haze (as described in Barry Morris, Chapter 12, pages 516-517). This combination of characteristics allows for improved processability and stability of ethylene acrylate copolymer resin for large bubble (film) applications.
[0084] Film manufacturing
[0085] Monolayer films with a thickness of 50 pm and 200 pm were processed on an extrusion line using the manufacturing conditions summarized in Table 3 below.
[0086] Table 3. Manufacturing conditions for single-layer blown films.
[0087] Table 4. Mechanical properties of monolayer blown films comprising inventive example 1 (IE1) at 50 pm and 200 pm.
[0088] It will be evident that modifications and variations are possible without departing from the scope of the invention as defined in the appended claims. More specifically, although some aspects of the present invention are identified herein as preferred or particularly advantageous, it is envisaged that the present invention is not necessarily limited to these aspects.
Claims
CLAIMS 1. An ethylene acrylate copolymer produced by a tubular free-radical polymerization process, wherein the ethylene acrylate copolymer comprises: 9 to 15% by weight of acrylate; a molecular weight distribution (MWD=Mw / Mn) less than or equal to 7.5, where Mw is the weight mean molecular weight and Mn is the number mean molecular weight measured by gel permeation chromatography (GPC); and a melting temperature of at least 99 °C as measured by differential scanning calorimetry (DSC).
2. The ethylene acrylate copolymer of claim 1, wherein the acrylate comprises a C1-C6 acrylate.
3. The ethylene acrylate copolymer of any of claims 1 and 2, wherein the acrylate further comprises n-butyl acrylate.
4. The ethylene acrylate copolymer of any of claims 1-3, wherein the ethylene acrylate copolymer further comprises a density of 0.910 g / cc to 0.945 g / cc.
5. The ethylene acrylate copolymer of any of claims 1-4 wherein the ethylene acrylate copolymer comprises from 12% by weight to 14% by weight acrylate.
6. The ethylene acrylate copolymer of any of claims 1-5, further comprising a melt strength (MS) greater than or equal to C-[(h)D], where C is the maximum strength on grams eluted per 10 minutes (cN / (g / 10 min)), E is the melt index measured according to ASTM D 1238 at 190 °C and a load of 2.16 kg, and D is -0.
28.
7. The ethylene acrylate copolymer of any of claims 1-6, further comprising a melt index ratio I10 / I2 of at least 17.0, wherein I10 and I2 are melt indices measured according to ASTM D 1238 at 190 °C and a loading of 2.16 kg and 10 kg, respectively.
8. The ethylene acrylate copolymer of any of claims 1-7 further comprises a melt viscosity ratio (Vo,i / Vioo) of at least 35, wherein Vo,i is the viscosity measured at 0.1 radians / second (rad / s) and 190 °C and Vioo is the viscosity measured at 100 rad / s and 190 °C.
9. The ethylene acrylate copolymer of any of claims 1-8 further comprising an average molecular weight z (M z ) of less than 750,000 g / mol, as measured.
10. The ethylene acrylate copolymer of any of claims 1-9 further comprises a crystallization temperature of at least 85 °C as measured by DSC.
11. The ethylene acrylate copolymer of any of claims 1-10 further comprises a melt strength (MS) of 17.0 maximum strength (cN) at 25.0 cN.
12. A film comprising the ethylene acrylate copolymer of any of the preceding claims.
13. The film of claim 12, in which the film is a single-layer film.
14. The film of claim 12, in which the film is a multi-layered film.
15. The film of any of claims 12 to 14, wherein the film is a greenhouse film.