Treatment of contaminated gases comprising nitrogen oxide and chromium contaminants

The gas treatment system with a Cr capture material upstream or downstream of the SCR catalyst addresses the deactivation issue by removing Cr contaminants, ensuring efficient NOx reduction and reducing catalyst volume requirements.

WO2026234374A1PCT designated stage Publication Date: 2026-11-12JOHNSON MATTHEY PLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/GB2026/050765
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-09-05
Filing Date
2026-05-07
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

SCR catalysts used to treat NOx-contaminated gases are poisoned and deactivated by Cr contaminants, leading to reduced NOx reduction efficiency and increased costs due to the need for larger catalyst volumes.

Method used

A gas treatment system with a Cr capture material located upstream or downstream of the SCR catalyst to remove Cr contaminants before they reach the catalyst, thereby protecting the SCR catalyst from deactivation.

Benefits of technology

The system effectively captures Cr contaminants, preserving the efficiency of the SCR catalyst and reducing the need for larger catalyst volumes, thus maintaining NOx reduction efficiency and lowering costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000028_0001_TABLE
    Figure IMGF000028_0001_TABLE
  • Figure IMGF000029_0001_TABLE
    Figure IMGF000029_0001_TABLE
  • Figure IMGF000030_0001_TABLE
    Figure IMGF000030_0001_TABLE
Patent Text Reader

Abstract

A gas treatment system for treating a contaminated gas comprising NOx and Cr contaminants comprises a SCR catalyst that is located to receive a flow of the contaminated gas and a Cr capture material that is located to capture at least some of the Cr contaminants from the contaminated gas upstream of the SCR catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] TREATMENT OF CONTAMINATED GASES COMPRISING NITROGEN OXIDE AND CHROMIUM CONTAMINANTS

[0002] Field of the invention

[0003] This invention relates to the treatment of contaminated gases comprising nitrogen oxide (NOx) and chromium (Cr) contaminants. The invention discloses a gas treatment system for treating a contaminated gas comprising NOx and Cr contaminants. The invention also discloses a method of treating a contaminated gas comprising NOx and Cr contaminants. The invention extends to a process for producing a hydrogen containing gas and to a process for producing ethylene.

[0004] Background to the invention

[0005] In many industrial processes, particularly those in which process components are exposed to high temperatures, oxygen, water vapor or corrosive environments, process components such as piping, vessels, reactors, and heat exchangers are exposed to conditions that can lead to the leaching of metals, including Cr, from the material of construction of these process components into gases that are produced in the process.

[0006] Cr, which is often present in alloys such as stainless steel and other corrosion-resistant materials used for the construction of process components, is essential for maintaining the strength, durability, and resistance to corrosion of process equipment. However, under certain operational conditions, such as those described above, Cr can leach from these materials, as volatile or gaseous Cr species, into process gas streams, resulting in potentially harmful contamination of process gases and / or waste or effluent gases.

[0007] One of the most significant concerns of Cr contamination is its potential to interfere with the performance of sensitive components in downstream processes. For example, Cr contaminants are known to poison catalysts. Loss of catalyst activity is often attributed to deposition of chromium oxide species on the catalyst surface and in the pores of the catalyst.Another group of harmful gas contaminants that is produced in many industrial processes as a result of high temperature reaction between nitrogen (N2) and oxygen (O2), typically above 1000°C, more specifically above 1200°C, includes nitrogen oxides (NOx).

[0008] In certain cases, industrial gases that are contaminated with NOx contaminants can also be contaminated with Cr contaminants, considering the high temperature origin of both of these types of contaminants. This is particularly problematic in steam-methane reforming (SMR) processes. The SMR process reacts a hydrocarbon, such as methane, with steam (H2O) to produce a mixture of hydrogen (H2) and carbon monoxide (CO), generically known as synthesis gas (syngas). Harmful NOx emissions are produced as a byproduct in the off gas, or flue gas, of SMR processes. To reduce NOx emissions, selective catalytic reduction (SCR) is used to treat the off gas of SMR processes.

[0009] Since Cr contaminants are usually present in such gases in concentrations that are orders of magnitude lower than the concentration of NOx contaminants, more attention is given to NOx abatement than Cr abatement.

[0010] One way of treating such gases, to abate the NOx contamination thereof, is to reduce the NOx contaminants to N2 and water (H2O) in the presence of ammonia, over a SCR catalyst. Such catalysts are, however, poisoned and deactivated by Cr deposits thereon, which naturally has a significantly negative impact on the NOx reduction efficiency of SCR catalysts when treating NOx contaminated gases that also contain Cr contaminants.

[0011] The current practice in addressing the abovementioned challenge of Cr poisoning of SCR catalysts in treating gases contaminated with both NOx and Cr contaminants, is to increase the volume of the SCR catalyst, e.g. doubling it, to account for the deactivation and meet emission regulations and catalyst lifetime requirements. This necessarily has a knock-on effect on cost and on process and equipment design specifications.

[0012] The present invention finds application in addressing to the abovementioned challenge of Cr contaminant driven deactivation of SCR catalysts that are used to treat NOx contaminated gases that also comprise Cr contaminants.Summary of the invention

[0013] In one aspect, the invention provides a gas treatment system for treating a contaminated gas comprising NOx and Cr contaminants, the gas treatment system comprising a SCR catalyst that is located to receive a flow of the contaminated gas and a Cr capture material that is located to capture at least some of the Cr contaminants from the contaminated gas upstream of the SCR catalyst.

[0014] In an embodiment of the invention, the Cr capture material is located to capture at least some of the Cr contaminants from the contaminated gas upstream of injecting a reductant for the SCR catalyst into the contaminated gas.

[0015] In an embodiment of the invention, the Cr capture material is located to capture at least some of the Cr contaminants from the contaminated gas downstream of injecting a reductant for the SCR catalyst into the contaminated gas.

[0016] In an embodiment of the invention, the contaminated gas includes a reductant for the SCR catalyst and no reductant injection is provided for, i.e. SCR reductant injection is absent from the system.

[0017] In another aspect, the invention provides a method of treating a contaminated gas comprising NOx and Cr contaminants, the method comprising contacting a flow of the contaminated gas that is supplied to a SCR catalyst with a Cr capture material upstream of the SCR catalyst such that the Cr capture material captures at least some of the Cr contaminants from the contaminated gas upstream of the SCR catalyst.

[0018] In an embodiment of the invention, the contaminated gas is contacted with the Cr capture material upstream of injecting a reductant for the SCR catalyst into the contaminated gas.

[0019] In an embodiment of the invention, the contaminated gas is contacted with the Cr capture material downstream of injecting a reductant for the SCR catalyst into the contaminated gas.

[0020] In an embodiment of the invention, the contaminated gas includes a reductant for the SCR catalyst and no reductant injection is therefore performed.In another aspect, the invention provides a process for producing syngas and optionally hydrogen, the process including

[0021] subjecting a mixture of hydrocarbon and steam to steam methane reforming, thus producing a reformed gas mixture comprising hydrogen and carbon monoxide and an off gas comprising NOx and Cr contaminants; and

[0022] contacting a flow of the off gas with a Cr capture material upstream of a SCR catalyst such that the Cr capture material captures at least some of the Cr contaminants from the off gas upstream of the SCR catalyst.

[0023] The off gas may be a contaminated gas as provided for in relation to the system and method of the invention.

[0024] Contacting the flow of the off gas with the Cr capture material may be provided for and / or performed in accordance with the system and method aspects of the invention.

[0025] The process may include subjecting the reformed gas mixture to water gas shift and recovering carbon dioxide from a product thereof to product, thus producing a crude hydrogen product gas which can subsequently be purified to produce a purified hydrogen product gas.

[0026] In another aspect, the invention provides a process for producing ethylene, the process including

[0027] subjecting a mixture of hydrocarbon and steam to steam cracking, thus producing a cracked gas mixture comprising ethylene and an off gas comprising NOx and Cr contaminants; and

[0028] contacting a flow of the off gas with a Cr capture material upstream of a SCR catalyst such that the Cr capture material captures at least some of the Cr contaminants from the off gas upstream of the SCR catalyst.

[0029] The off gas may be a contaminated gas as provided for in relation to the system and method of the invention.

[0030] Contacting the flow of the off gas with the Cr capture material may be provided for and / or performed in accordance with the system and method aspects of the invention.Brief description of the drawings

[0031] The invention will now be described in more detail, including with reference to the accompanying non-limiting diagrammatic drawings, in which:

[0032] Figure 1 shows, by way of non-limiting example, one embodiment of a gas treatment system according to the invention, providing for Cr capture upstream of SCR reductant injection;

[0033] Figure 2 shows, by way of non-limiting example, another embodiment of a gas treatment system according to the invention, providing for Cr capture downstream of SCR reductant injection; and

[0034] Figure 3 shows, by way of non-limiting example, a further embodiment of a gas treatment system according to the invention, providing for Cr capture in the absence of SCR reductant injection.

[0035] Detailed description of the invention

[0036] Each aspect or embodiment of the invention as defined herein may be combined with any other aspect(s) or embodiment(s) unless clearly indicated to the contrary. In particular, any features indicated as being preferred or advantageous may be combined with any other features indicated as being preferred or advantageous.

[0037] In this specification, the term “Cr contaminants” refers to any undesired volatile or gaseous Cr species that is / are contained in a gas that is contaminated by the presence of such a species. Typically, in the context of the invention, such Cr species may include metallic Cr vapour and / or other volatile or gaseous Cr species, including Cr(VI) species, Cr(lll) species, and / or organometallic Cr species. Specific examples include chromium oxyhydroxides, such as CrC>2(OH)2, CrO2OH, and CrO(OH)2, and chromium oxides, such as CrO, CrC>2, and CrCh.

[0038] Furthermore, in this specification, the term “NOx” refers to nitrogen-based gas contaminants. Examples of NOx contaminants comprise nitric oxide (NO) and nitrogen dioxide (NO2). It will be understood by persons skilled in the art that NOx contaminants are pollutants that are most commonly abated by reduction thereof over SCR catalysts using a reductant. Typical reductants include ammonia (NH3), hydrogen (H2), and hydrocarbons, e.g. HC or HC10-20. Asindicated in the background to the invention, SCR catalysts are poisoned by Cr contaminants when such contaminants are present in the gases that are treated over such catalysts.

[0039] In the present invention, it was found that SCR catalyst poisoning by Cr contaminants in a NOx contaminated gas that is treated using a SCR catalyst can conveniently be limited by providing a Cr capture material upstream of the SCR catalyst, in a flow of the contaminated gas that is directed to the SCR catalyst, thereby to capture at least some of the Cr contaminants from the contaminated gas upstream of the SCR catalyst.

[0040] In addition, it was found that, under certain conditions, particularly subject to the temperature of the contaminated gas, the Cr capture material may conveniently be placed downstream of the injection of a reductant for the SCR catalyst into the contaminated gas, when such injection is needed. Advantageously, this allows for the Cr capture material to be placed closer to the SCR catalyst and, thus, for fresh contamination that may occur downstream of the Cr capture material and upstream of the SCR catalyst to be limited or avoided. A risk of such contamination downstream of the Cr capture material and upstream of the SCR catalyst would be appreciated to be a possibility when provision is made for SCR reductant injection between the Cr capture material and the SCR catalyst.

[0041] The term “upstream” as used in this specification indicates a location or direction in towards the source of the flow of the contaminated gas. By contrast, the term “downstream” as used herein indicates a location or direction away from the source of the flow of the contaminated gas.

[0042] Furthermore, in this specification, the term “capture” as used in relation to Cr contaminants means to remove one or more Cr contaminants from the contaminated gas. Such removal, in the context of the invention, would involve absorption and / or adsorption of one or more Cr contaminants by the Cr capture material and / or chemical reaction between Cr contaminants and the Cr capture material. Thus, the Cr capture material traps Cr of captured Cr contaminants either as the same Cr species that is present in the contaminated gas or as a different Cr species, thereby removing the Cr from the contaminated gas. Typically, the Cr is captured as Cr compounds or loose Cr species such as monomers and polymers including dimers, trimers, and tetramers.The Cr capture material of the invention may provide what is known in the art as a Cr trap or a Cr getter. In this specification, it should therefore be understood that the Cr capture material may therefore be regarded as providing a Cr trap or a Cr getter.

[0043] In one aspect, the invention provides a gas treatment system for treating a contaminated gas comprising NOx and Cr contaminants, the gas treatment system comprising a SCR catalyst that is located to receive a flow of the contaminated gas and a Cr capture material that is located to capture at least some of the Cr contaminants from the contaminated gas upstream of the SCR catalyst.

[0044] The term “contaminated gas” is predominantly used in this specification both with reference to the gas that is supplied to the Cr capture material and the gas that is supplied to the SCR catalyst after it has been contacted with the Cr capture material.

[0045] It will be understood, however, that the contaminated gas that is supplied to the SCR catalyst would be lean or free of Cr contaminants after having been contacted with the Cr capture material. This difference is emphasised with reference to the drawings only, in which the gas that is supplied to the Cr capture material is referred to as a contaminated gas while the gas that is supplied to the SCR catalyst is referred to as a Cr contaminant lean gas.

[0046] In the rest of the specification, the term “contaminated gas” is used both with reference to the gas that is supplied to the Cr capture material and the gas that is supplied to the SCR catalyst after it has been contacted with the Cr capture material. The context would dictate whether such a reference is to a contaminated gas that comprises both Cr and NOx contaminants or is lean or free of Cr contaminants but still has NOx contaminants.

[0047] In an embodiment of the invention, the Cr capture material may be located to capture at least some of the Cr contaminants from the contaminated gas upstream of injecting a reductant for the SCR catalyst into the contaminated gas.

[0048] In such an embodiment, the contaminated gas may be at a temperature at or above 300°C, more preferably at or above 400°C. It is not excluded, however, that the contaminated gas may, in such an embodiment, be at a temperature below 400°C, or below 300°C. For example, the contaminated gas may be at a temperature in the range of 200°C to 400°C, such as 200°C to 300°C.In an embodiment of the invention, the Cr capture material is located to capture at least some of the Cr contaminants from the contaminated gas downstream of injecting a reductant for the SCR catalyst into the contaminated gas.

[0049] In such an embodiment, the contaminated gas may be at a temperature below 400°C, e.g. below 300°C, preferably in the range of 200°C to 400°C, more preferably in the range of 200°C to 300°C.

[0050] It will be understood by persons skilled in the art that SCR reductants, most commonly ammonia (NH3) or a NH3 precursor such as urea (NH2CONH2), react selectively with NOx over SCR catalysts in excess amounts of oxygen (O2). The reductant may therefore be NH3 or a NH3 precursor such as urea.

[0051] Other suitable reductants may include hydrogen and hydrocarbons.

[0052] Reductant injection into gaseous SCR catalyst feeds, such as the contaminated gas of the present invention, is typically performed using a reductant injection grid, which is configured to achieve a predetermined concentration of reductant in the gas that would be treated by the SCR catalyst. The design and operation of such injection grids are within the knowledge and skill of persons skilled in the art.

[0053] In some cases, a gaseous SCR catalyst feed comprises a reductant, in which case no reductant injection is required. This is within the scope of the invention. Such a situation may, for example, occur when there is an unburnt fuel, such as hydrogen or hydrocarbons, in a gaseous SCR catalyst feed, which hydrogen or hydrocarbons can then act as reductant for the SCR. Thus, when the contaminated gas is produced comprising a reductant for the SCR catalyst, such as hydrogen or hydrocarbons, the system may omit providing for the injection of a reductant for the SCR catalyst into the flow of the contaminated gas.

[0054] Locating the Cr capture material upstream of the injection of the reductant into the contaminated gas would in relevant cases assist in avoiding oxidation of the reductant by the Cr capture material before the reductant reaches the SCR catalyst. This would be particularly preferred if the temperature of the contaminated gas that is supplied to the SCR catalyst is above 300°C, more preferably above 400°C, as indicated above. The feature of the inventionthat the Cr capture material is located ahead of the injection of the reductant not limited to such temperatures of the contaminated gas, however. It may be applied at lower temperatures too, as indicated above.

[0055] As also indicated above, depending on the temperature of the contaminated gas, the Cr capture material may in an embodiment of the invention instead be located downstream of the injection of the reductant into the contaminated gas.

[0056] Furthermore, as also indicated above, when the contaminated gas includes a reductant for the SCR catalyst, there may be no provision made for injection of a reductant for the SCR catalyst into the flow of contaminated gas.

[0057] The SCR catalyst comprises a catalytically active material capable of reducing NOx contaminants in the contaminated gas to N2 and O2 in the presence of a suitable reductant such as that described above. Typically, such catalytically active materials are selected from zeolites, such as copper (Cu) zeolites and iron (Fe) zeolites, copper (Cu), cobalt (Co), nickel (Ni), lanthanum (La), manganese (Mn), iron (Fe), vanadium (V), silver (Ag), and cerium (Ce), neodymium (Nd), praseodymium (Pr), titanium (Ti), chromium (Cr), zinc (Zn), tin (Sn), niobium (Nb), molybdenum (Mo), hafnium (Hf), yttrium (Y), and tungsten (W). Such catalytic materials are typically loaded or supported on molecular sieve support materials, such as Fe-zeolites or Cu-zeolites, and disposed on substrates, such as ceramic or metallic flow-through or filter substrates. Other possible substrates include fibres such as glass fibres or fibre glass, fibre mats, electric glass (“E-glass”), or corrugated glass paper.

[0058] The design of SCR catalysts is well known to persons skilled in the art, and the SCR catalyst of the invention may therefore be any SCR catalyst appropriate for abatement of NOx contaminants in the contaminated gas, mindful of relevant process operating conditions which a skilled person would be able to apply routinely.

[0059] In an embodiment of the invention, the SCR catalyst is a V-W-Ti catalyst, for example an extruded V-W-Ti catalyst or a washcoated V-W-Ti catalyst.

[0060] The number of channels, their diameters and wall thickness of a catalyst substrate determine the cell density of the catalyst, expressed as cells per square inch (CPSI). A SCR with a high CPSI (CPSI >200) is often preferred due to the increased available surface area for thecatalytic reaction to occur. However, the inventor of the present invention has found that the SCR in the system according to the invention exhibits improved performance where the SCR substrate has a substrate with a low CPSI due to the resultant lower back-pressure across the catalyst. Accordingly, it is preferred that the SCR according to the present invention has a CPSI of less than 200 CPSI, preferably less than 100 CPSI, preferably less than 70 CPSI, even more preferably 64 CPSI or less.

[0061] It will be appreciated that, to capture at least some of the Cr contaminants from the contaminated gas, the Cr capture material, like the SCR catalyst, would preferably also be located to receive the flow of the contaminated gas, and to do so upstream of the SCR catalyst, more preferably also upstream of injecting a reductant for the SCR catalyst into the contaminated gas.

[0062] The location of the Cr capture material upstream of the SCR catalyst, and in some embodiments also upstream of the SCR reductant injection, is preferably as close as possible to the SCR catalyst. Thus, the Cr capture material is preferably located immediately upstream of the SCR catalyst, or immediately upstream of the SCR reductant injection when relevant. As noted above, it is in this regard advantageous, when SCR reductant injection is provided for, that the Cr capture material be provided downstream of such reductant injection in accordance with the invention. Thus, re-entering of Cr contaminants into the flow of contaminated gas that is fed to the SCR catalyst can be limited or avoided, particularly if the contaminated gas is at a temperature that could cause such contamination to occur afresh through leaching from a SCR catalyst feed conduit along which the contaminated gas is conveyed downstream of the Cr capture material.

[0063] The contaminated gas is preferably an industrial gas, i.e. it may be a gas of (i.e. that is produced in and / or emanates from) an industrial process. In this regard, reference is made to feed gases, off gases or flue gases, and process gases of industrial processes. The term “process gases” in this context refers to gases produced in industrial processes other than off gases or flue gases. As will be understood by persons skilled in the art, off gases or flue gases of industrial processes are typically gases that contain byproducts or waste products of such processes, e.g. combustion products.

[0064] In accordance with the invention, the contaminated gas that is treated according to the invention comprises both NOx and Cr contaminants. It follows that the contaminated gas ispreferably a gas of an industrial process that causes both NOx contamination and Cr contamination of one or more gases of the process. In other words, the relevant gases are cocontaminated with NOx and Cr contaminants. Such contamination may occur simultaneously or sequentially.

[0065] Persons skilled in the art would know that, in industrial contexts, NOx contamination of industrial gases most typically results from the reaction of N2 with O2 in high temperature environments, e.g. above 1000°C and more typically above 1200°C, which has also been alluded to above. This may occur, for example, in process combustion environments, such as those that are associated with boilers, burners, high temperature reactors, and furnaces. In other words, the contaminated gas may, in an embodiment of the invention, be produced by the combustion of a fuel, such as hydrogen or hydrocarbons.

[0066] Persons skilled in the art would also know that Cr contamination of industrial gases typically occurs as a result of Cr leaching from process components such as equipment including one or more of piping, vessels, reactors, heat exchanges, etc., under high temperature conditions, which has also been alluded to above. Such process components would particularly be those that are made of or have process-exposed surfaces comprising Cr metal alloys.

[0067] In this specification, the term “high temperature” in the context of the cause of Cr contamination refers to any temperature that is sufficiently high to cause leaching of Cr from solid alloys thereof, such as stainless steel. Typically, such temperatures would be above 300°C, e.g. above 400°C, or above 500°C, or above 600°C, typically up to, but not necessarily limited to 700°C or even 1000°C.

[0068] In an embodiment of the invention, Cr contamination of the contaminated gas may be at a concentration of from 0.5ppb to 20ppb.

[0069] For the contaminated gas to cause Cr leaching from solid alloys thereof, the contaminated gas would typically also need to comprise oxygen. For example, when the contaminated gas comprises oxygen, the contaminated gas may comprise less than 3 vol% oxygen.

[0070] For the contaminated gas to cause Cr leaching from solid alloys thereof, the contaminated gas would typically also need to comprise water. For example, when the contaminated gascomprises water, the contaminated gas may comprise from 1 vol% to 30 vol% water, for example 3 vol% to 20 vol% water, or 3 vol% to 10 vol% water, for example 8 vol% water.

[0071] One industrial process that produces a Cr and NOx contaminated gas, as an off gas or flue gas, is the steam reforming of methane in a steam methane reformer (SMR). The off gas from SMR contains NOx that is formed as a result of the heat of combustion in the SMR’s furnace in which N2 and O2 may be present, particularly if air is used as oxidising gas. In addition, the operating temperature of SMR is sufficiently high, being in the order of 700°C to 1000°C, to cause the leaching of Cr contaminants from the SMR, e.g. from tubes and / or fins thereof, into the off gas.

[0072] In one embodiment of the invention, the contaminated gas is therefore a NOx and Cr contaminated gas of SMR, e.g. that emanates from SMR. Such a gas is preferably an off gas or flue gas of the SMR, more specifically of the SMR furnace. The Cr contaminants of the contaminated gas may in such a case originate from tubes of the SMR, i.e. the reformer tubes thereof, and / or from fins of a convection section of the SMR, which are typically constructed of chromium containing alloys such as stainless steel.

[0073] As noted in the background section, SMR is used to react a hydrocarbon, such as methane, with steam (H2O) to produce a mixture of hydrogen (H2) and carbon monoxide (CO), generically known as synthesis gas (syngas). Harmful NOx emissions are produced as a byproduct in the off gas, or flue gas, of the SMR, specifically of the SMR furnace.

[0074] Without limiting the invention or being bound to theory, the applicant notes that it is reported in literature that oxidation resistance of stainless steels and many other high-temperature nickel-based alloys containing chromium is provided by a protective Cr2Os surface layer. The Cr2C>3 normally forms spontaneously upon exposure to oxidizing conditions at high temperatures. For a high pressure Cr / Ni alloy, this oxide is not pure C^Os but consists of a relatively thick layer of C^Ch closest to the metal, topped by a thin external layer consisting of a mixed manganese-iron chromate (Mn,Fe)Cr2C>4 spinel.

[0075] An oxide such as C^Ch undergoes what is termed an oxidative vaporization at high temperature and reverts to its original form upon condensation. At least some of the C^Ch converts into products like Cr, CrO, CrC>2, and molecular and atomic oxygen in the vapor phase in the absence of oxygen from an outside source. When external oxygen is present, e.g. in aflue gas containing excess air, which is typically the case in SMRs, CrCh is also produced, and the equilibrium is shifted among the various oxide species. With accompanying flue gas water vapor in addition to the oxygen, gaseous hydroxides and oxyhydroxides such as CrC>2(OH)2, CrO2OH, and CrO(OH)2 are formed as well.

[0076] Persons skilled in the art would know that SMR’s most prominently find application in hydrogen and / or syngas production processes. While syngas is a product produced by SMR, hydrogen may be recovered from such a syngas product by employing a water-gas shift reaction to increase the hydrogen content of the syngas product and convert carbon monoxide to carbon dioxide and separating the carbon dioxide to produce a crude hydrogen product that is subsequently purified. The SMR may therefore form part of a hydrogen or syngas production process or plant.

[0077] In some applications, SMR that produces a NOx and Cr contaminated gas, to be treated according to the invention, may be usefully employed, along with other process components such as one or more water-gas shift reactors, in the production of hydrogen as a fuel gas for an electrochemical system that uses such a fuel gas. The gas treatment system may therefore be provided in a hydrogen production process comprising SMR, which process produces hydrogen as a fuel gas for an electrochemical system that is coupled to the process to receive hydrogen as a fuel gas from the process.

[0078] Another industrial process that produces gases contaminated with Cr and NOx is the ethylene production process. The contaminated gas may therefore be a gas of an ethylene production process. In other words, the contaminated gas may emanate from an ethylene production process.

[0079] In the ethylene production process, NOx is produced primarily through the combustion that is involved in heating and generating steam for cracking hydrocarbons like ethane, propane, or naphtha in steam crackers.

[0080] The contaminated gas of the invention may be at a temperature in a range of from 200°C to 700°C, or 300°C to 650°C, or 400°C to 650°C. As set out earlier in this specification, certain ranges within these limits may be typical for certain configurations of the system, specifically referring to the location of SCR reductant injection.The Cr capture material is preferably provided by a catalyst article that comprises a substrate that has the Cr capture material. Thus, locating the Cr capture material to capture at least some of the Cr contaminants from the contaminated gas would in effect involve locating the substrate having the Cr capture material, i.e. the catalyst article, to such an effect. In a preferred embodiment the substrate that has the Cr capture material has a cell density of 300 CPSI or less, preferably 200 CPSI or less, preferably 100 CPSI or less, more preferably less than 70 CPSI, for example 46 CPSI to 64 CPSI.

[0081] The term “article” or “catalyst article” as used herein therefore encompasses a substrate having the Cr capture material.

[0082] The catalyst article is preferably configured and located such that substantially all of the contaminated gas contacts the catalyst article, e.g. flows through or across the catalyst article, and thus comes into contact with the Cr capture material.

[0083] One suitable substrate is a ceramic or metallic flow-through or filter substrate, preferably being monolithic. For example, it may be in the form of a honeycomb monolith. The term “substrate” as used herein is therefore used to include, for example, a ceramic or metallic flow-through honeycomb, or a filter block, e.g. a wall flow filter. The substrate may vary in its material composition, size and configuration, cell shape and density, and wall thickness.

[0084] When the substrate is ceramic, the ceramic substrate may be of any suitable refractory material, e.g., alumina, silica, titania, ceria, zirconia, magnesia, zeolites, silicon nitride, silicon carbide, zirconium silicates, magnesium silicates, aluminosilicates and metallo aluminosilicates (such as cordierite and spodumene), or a mixture or mixed oxide of any two or more thereof. Cordierite, a magnesium aluminosilicate, is particularly preferred. Preferably, the substrate comprises cordierite. However, the composition of the substrate is not particularly limited.

[0085] When the substrate is metallic, the metallic substrate may be made of any suitable metal, and in particular heat-resistant metals and metal alloys such as titanium and stainless steel as well as ferritic alloys containing iron, nickel, chromium, and / or aluminium in addition to other trace metals.The substrate may have the Cr capture material disposed thereon. The terms “disposed thereon” and “disposed on” as used herein may encompass either having the Cr capture material directly disposed on the substrate, i.e. with no intervening material, and / or indirectly disposed on the substrate, i.e. with intervening material, e.g. supported on a support material.

[0086] The Cr capture material may be dispersed on a surface of the support material. If the support material is porous, the Cr capture material may, additionally or alternatively, be present within pores of the support material. How the Cr capture material may be disposed on the substrate is, however, not particularly important for the purpose of the present invention.

[0087] The substrate preferably has the Cr capture material disposed thereon as a washcoat.

[0088] The term “washcoat” as used in this specification is well-known in the field and refers to an adherent coating that is applied to a substrate usually during the production of a catalyst.

[0089] Alternatively, or additionally, substrate may be pelletised. In this regard, it is provided that it is also possible for the capture material itself to be pelletised, i.e. not to be supported on a pelletised substrate.

[0090] Alternatively, or additionally, the substrate may be made from extrudate comprising the Cr capture material. In one embodiment, the substrate may be an “all-active extrudate” wherein the substrate comprises an extrusion of the Cr capture material, i.e. wherein the substrate itself is active as the Cr capture material.

[0091] Alternatively, or additionally, the substrate may comprise a fibrous material.

[0092] The Cr capture material may be any material that is capable of capturing a gaseous Cr contaminant from a gas containing such a contaminant, within the meaning of the term “capture” as hereinbefore defined.

[0093] One suitable Cr capture material is an Fe-loaded molecular sieve.

[0094] Conveniently, the Fe-loaded molecular sieve may capture at least some of the Cr contaminants as one or more Cr(lll) species in contrast to other Cr capture materials that typically capture Cr contaminants as Cr(VI) species.The term “molecular sieve” as used herein in the context of the Fe-loaded molecular sieve is well known to the skilled person and may encompass crystalline or quasi-crystalline materials which can be, for example aluminosilicates (zeolites) or silico-alumino-phosphates (SAPOs). Such molecular sieves are constructed of repeating SiC>4, AIO4, and optionally PO4 tetrahedral units linked together, for example in rings, to form frameworks having regular intra-crystalline cavities and channels of molecular dimensions. The specific arrangement of tetrahedral units (ring members) gives rise to the molecular sieve’s framework, and by convention, each unique framework is assigned a unique three-letter code (e.g., “CHA”) by the International Zeolite Association (IZA).

[0095] Molecular sieves may exist as "H+-form" or “NH4+form” molecular sieves, for example. The term "H+-form" in relation to a molecular sieve refers to a molecular sieve having an anionic framework wherein the charge of the framework is counterbalanced by protons (i.e. H+cations). The term “NH4+form” in relation to a molecular sieve refers to a molecular sieve having an anionic framework wherein the charge of the framework is counterbalanced by ammonium cations (NH4+cations). When metal-loaded (e.g. Fe), these molecular sieves are no longer considered to be in their "H+-form" or “NH4+form”.

[0096] Molecular sieves (e.g. zeolites) may also be categorised by pore size, e.g. a maximum number of tetrahedral atoms present in a molecular sieve’s framework. As defined herein, a “smallpore” molecular sieve, such as CHA, contains a maximum ring size of eight tetrahedral atoms, whereas a “medium-pore” molecular sieve, e.g. MFI, contains a maximum ring size of ten tetrahedral atoms; and a “large-pore” molecular sieve, such as BEA, contains a maximum ring size of twelve tetrahedral atoms. In the present invention, small-, medium, and large-pore molecular sieves are defined as such in accordance with these generally understood definitions.

[0097] The molecular sieve of the Fe-loaded molecular sieve of the invention is not limited to a molecular sieve of any specific pore size. It is also not required for the molecular sieve to comprise only one type of molecular sieve. The invention therefore encompasses embodiments in which the Cr capture material comprises Fe loaded on two or more different small-, medium-, or large-pore molecular sieves.The term “different small-, medium-, or large-pore molecular sieves” may encompass that the framework (i.e. the Framework Type Code) of the molecular sieve, or another property of the molecular sieve, such as the SAR, is different. The term SAR stands for “silica-to-alumina ratio” and, as used herein, may encompass the molar ratio of silicon to aluminium present in the molecular sieve framework, calculated on the basis of the silica (SiC>2) and the alumina (AI2O3), rather than the silicon and aluminium atoms. Of course, in the chemical structure of the molecular sieve framework, the silicon and aluminium will not typically be present in the form of discrete silica and alumina. The SAR is a term commonly used in the art and would be understood by the skilled person.

[0098] The molecular sieve preferably comprises a zeolite.

[0099] The term “Fe-loaded” as used herein may encompass that the molecular sieve is metal-promoted with Fe, wherein the Fe may be loaded into the molecular sieve. In a metal-loaded molecular sieve, the loaded metal is a type of “extra-framework metal”, that is, a metal that resides within the molecular sieve and / or on at least a portion of the molecular sieve surface. This definition does not include atoms constituting the framework of the molecular sieve.

[0100] Metal-loaded molecular sieves, in general, and methods of manufacturing such metal-loaded molecular sieves, are known to the skilled person. For example, several methods have been mentioned in the literature for preparing metal-loaded molecular sieves, in particular metal-loaded zeolites. The direct synthesis of metal-loaded zeolites is a complicated process and depends on the synthesis conditions (see M. Moliner, ISRN Materials Science, 2012, Article ID 789525). An alternative is to use a commercial zeolite support and to subsequently add metal by post-synthesis treatment of the zeolite, for example, by wet impregnation, wet ion exchange or solid-state ion exchange.

[0101] Known wet ion-exchange methods for the addition of metal to molecular sieves (e.g. zeolites) typically employ soluble metal salts, such as metal acetates, metal sulphates or metal chlorides, as the active metal precursor, wherein the active metal precursor is reacted with the molecular sieve in aqueous solution. In order to accelerate ion-exchange, such processes typically require a heating step, wherein the mixture may be heated to a temperature in the range 70 to 80°C for up to several hours.The Fe-loaded molecular sieve may be substantially free of metals other than Fe-loaded thereon. The term “substantially free of” as used herein in the context of the Fe-loaded molecular sieve may encompass that the molecular sieve comprises less than 0.1 wt.%, more preferably less than 0.05 wt.%, even more preferably less than 0.01 wt.% and still more preferably less than 0.001 wt.% of any metal other than Fe loaded thereon, based on the total weight of the Fe-loaded molecular sieve. More preferably, the Fe-loaded molecular sieve does not comprise any metals other than Fe loaded thereon.

[0102] In other words, Fe is preferably the only metal that is loaded on the molecular sieve.

[0103] Of course, there is a chance that other metals may be present on the Fe-loaded molecular sieve, for example if a catalyst article comprising the Fe-loaded molecular sieve has other layers or zones disposed thereon that comprise different components which contain metals other than Fe. This may, in one embodiment, include to provide for oxidation of contaminants other than Cr in the contaminated gas, or to provide one or more other, different, Cr capture materials in addition to the Fe-loaded molecular sieve. In such cases, the other metals may typically be transferred due to physical contact. The characterisation of the present invention that the Fe-loaded molecular sieve, as a Cr capture material, is free of other metals than Fe is not intended to exclude such embodiments of incidental transfer.

[0104] The Cr capture material species can be selected from one or more alkaline earth metals, one or more transition metals, and combinations thereof.

[0105] It should be noted, however, that the exclusion of other metals than Fe from being loaded on the Fe-loaded molecular sieve relates only to a case in which the Fe-loaded molecular sieve, as such, is provided as or as an independent part of the Cr capture material. As discussed in more detail below, the invention includes an embodiment in which the Cr capture material comprises or consists of other metals, such as one or more alkaline earth metals, supported on a support material that may be a Fe-loaded molecular sieve. In such an embodiment, the gas treatment system would comprise Fe-loaded molecular sieve support materials that support one or more other metals than Fe, such as one or more alkaline earth metals. The abovementioned exclusion therefore does not exclude such embodiments of Cr capture materials from the scope of the invention.Another suitable Cr capture material is, as alluded to above, an alkaline earth metal. The Cr capture material may therefore comprise one or more alkaline earth metals. For example, the Cr capture material may preferably comprise barium (Ba), strontium (Sr), calcium (Ca), magnesium (Mg), or combinations of two or more thereof.

[0106] The one or more alkaline earth metals may be supported on a support material. That is, the Cr capture material may comprise the one or more alkaline earth metals disposed on the support material.

[0107] In being “disposed on” the support material, the one or more alkaline earth metals is preferably disposed directly on, i.e. directly supported on, the support material. The alkaline earth metal may in this regard be dispersed on a surface of the support material. If the support material is porous, the alkaline earth metal may be present within pores of the support material.

[0108] One suitable support material is a refractory inorganic oxide. Suitable refractory inorganic oxides may be selected from the group consisting of alumina, silica, titania, zirconia, ceria, zinc oxide, tin oxide, magnesium oxide, yttrium oxide, tantalum oxide, hafnium oxide, lanthanum oxide and a mixed or composite oxide thereof, e.g. a mixed oxide or a composite oxide of two or more thereof such as ceria-zirconia. Preferably, the refractory oxide support material is selected from ceria-zirconia, alumina, and a mixture thereof. The alumina may be gamma phase alumina, theta phase alumina, alpha phase alumina, delta (5), eta (q) and kappa (K) or a mixture thereof.

[0109] In some cases, it is desirable or necessary to modify the properties of inorganic refractory oxides with a dopant, to make it suitable or enhance its properties for use as a support material. The invention therefore provides that the inorganic refractory oxide may be a doped inorganic refractory oxide, in which case it is doped with a modifying element (dopant).

[0110] The alkaline earth metal may be loaded on the refractory oxide by any suitable method. Such methods would be within the knowledge of a person skilled in the art. For example, the alkaline earth metal may be loaded on the refractory oxide by impregnating the support material with the alkaline earth metal by incipient wetness, mechanochemistry (e.g. by milling of a mixture of the dry materials), or washcoat adsorption techniques.Another suitable support material is a molecular sieve. For example, the support material may be a zeolite, such as a small, medium or large pore zeolite. The zeolite may preferably be a small pore zeolite, for example having a framework type selected from AEI, AFX, CHA, LTA or ERI, a medium pore zeolite, for example having a framework type selected from FER, MEL, MFI, STI and STT, or a large pore zeolite, for example having a framework type selected from AFI, BEA, MAZ, MOR, Y, FAU and OFF. In an embodiment, the support material may be an Fe-zeolite or a Cu-zeolite.

[0111] As alluded to earlier in this specification, Fe-zeolite is one possible support material for the alkaline earth metal. In this sense, the Fe-zeolite acts as a support material, but may also have Cr capture functionality. This may, in an embodiment of the invention, be in addition to having Fe-zeolite, as such, comprised as an independent component of the Cr capture material.

[0112] The alkaline earth metal may be loaded on the molecular sieve by any suitable method. Such methods would be within the knowledge of a person skilled in the art. For example, the alkaline earth metal may be loaded on the molecular sieve by means of precipitation or ion exchange.

[0113] The support material may be substantially free of metals other than the one or more alkaline earth metals loaded thereon. This excludes metals that are a part of the support material as such, for example Fe and Cu, respectively, that are disposed on Fe-zeolites and Cu-zeolites.

[0114] The term “substantially free of” as used herein in the context of the support material supporting one or more alkaline earth metals may encompass that the molecular sieve comprises less than 0.1 wt.%, more preferably less than 0.05 wt.%, even more preferably less than 0.01 wt.% and still more preferably less than 0.001 wt.% of any metal other the one or more alkaline earth metals loaded thereon, excluding metals inherently part of the support material such as Fe and Cu in Fe-zeolites and Cu-zeolites respectively, based on the total weight of the support material supporting the one or more alkaline earth metals. More preferably, the Fe-loaded molecular sieve does not comprise any metals other than the one or more alkaline earth metals supported thereon.

[0115] In other words, the one or more alkaline earth metals is / are preferably the only metal / s that loaded on the molecular sieve, other than those metals that form an inherent part of the support material such as Fe or Cu in Fe-zeolites and Cu-zeolites respectively.Of course, there is a chance that other metals may be present on the support material supporting the one or more alkaline earth metals, for example if a catalyst article comprising the support material supporting the one or more alkaline earth metals has other layers or zones disposed thereon that comprise different components which contain metals other than the one or more alkaline earth metals. This may, in one embodiment, include to provide for oxidation of contaminants other than Cr in the contaminated gas, or to provide one or more other, different, Cr capture materials in addition to the one or more alkaline earth metals. In such cases, the other metals may typically be transferred due to physical contact. The characterisation of the present invention that the support material supporting the one or more alkaline earth metals, as a Cr capture material, is free of other metals than the one or more alkaline earth metals is not intended to exclude such embodiments of incidental transfer.

[0116] The one or more alkaline earth metals may be disposed on the support material as one or more alkaline earth metal species. Such alkaline earth metal species may include one or a combination of two or more of barium (Ba), strontium (Sr), magnesium (Mg), and calcium (Ca).

[0117] The gas treatment system may comprise only one species of Cr capture material. Thus, in such an embodiment, the Cr capture material may consist of one of the Fe-loaded molecular sieve and the one or more alkaline earth metals supported on a suitable support material, thus being free of the other thereof.

[0118] When the gas treatment system comprises only one species of Cr capture material and the Cr capture material is provided by a catalyst article, the substrate of the catalyst article would have only one species of Cr capture material disposed thereon, being free of other species of Cr capture material.

[0119] Furthermore, when the gas treatment system comprises only one species of Cr capture material and the Cr capture material is provided by a catalyst article, the gas treatment system may be free of any additional substrate that has another, different, Cr capture material disposed thereon.

[0120] In being “free” of any additional Cr capture materials, the gas treatment system may have substantially no such additional Cr capture materials located in a conduit that provides the flow of the contaminated gas. Such a conduit may, for example, be an exhaust or effluent or off gas conduit, which conveys the contaminated gas away from a source thereof, in which casethere would be substantially no such additional Cr capture materials between the source of the gas and a downstream end, e.g. an outlet end, of the conduit.

[0121] The gas treatment system may, alternatively, comprise more than one species of Cr capture material. Thus, in such an embodiment, the Cr capture material may comprise both the Reloaded molecular sieve and the one or more alkaline earth metals.

[0122] In such a case, the Cr capture material may be provided by a catalyst article comprising a substrate having both the Fe-loaded molecular sieve and the one or more alkaline earth metals disposed thereon, and / or by separate catalyst articles comprising separate substrates respectively having the Fe-loaded molecular sieve or the one or more alkaline earth metals disposed thereon.

[0123] When both the Fe-loaded molecular sieve and the alkaline earth metal are disposed on the same substrate, the Fe-loaded molecular sieve and the alkaline earth metal may be so disposed in a mixed layer on the substrate and / or in separate layers of the substrate that at least partly overlay each other or that are provided in separate regions of the substrate and that comprise one of the species of Cr capture material to the exclusion of the other.

[0124] The gas treatment system may be free of any catalytically active materials other than that which provides the Cr capture material and the SCR catalyst. In particular, the gas treatment system may be free of any oxidation catalysts, e.g. PGM oxidation catalysts.

[0125] In being “free” of any catalytically active materials other than that which provides the Cr capture material and the SCR catalyst, the gas treatment system may have substantially no such other catalytically active materials located in a conduit that provides the flow of the contaminated gas. As noted earlier, such a conduit may, for example, be an exhaust or effluent or off gas conduit, which conveys the contaminated gas away from a source thereof, in which case there would be substantially no other catalytically active materials between the source of the gas and a downstream end, e.g. an outlet end, of the conduit.

[0126] In use, contaminated gas would therefore be received by the Cr capture material upstream of the SCR catalyst, more preferably upstream of the injection of reductant into the contaminated gas upstream of the SCR catalyst and would capture at least some Cr contaminants from the contaminated gas. Thus, the contaminated gas that is passed to the SCR catalyst has areduced concentration of, or is free of, Cr contaminants. In this way, Cr poisoning of the SCR catalyst is limited or avoided, which allows for the SCR catalyst to be designed accordingly, with reduced attention, or no attention, being given to possible Cr poisoning in such design.

[0127] As has been indicated earlier, the contaminated gas with the Cr capture material therefore produces a Cr contaminant lean gas, which may be Cr contaminant lean or Cr contaminant free.

[0128] Such a Cr contaminant lean gas would subsequently be supplied to and contacted with the SCR catalyst, to abate NOx contaminants in the Cr contaminant lean gas and thus produce a cleaned gas.

[0129] In another aspect, the invention provides a method of treating a contaminated gas comprising NOx and Cr contaminants, the method comprising contacting a flow of the contaminated gas that is supplied to a SCR catalyst with a Cr capture material upstream of the SCR catalyst, such that the Cr capture material captures at least some of the Cr contaminants from the contaminated gas upstream of the SCR catalyst.

[0130] The contaminated gas is preferably contacted with the Cr capture material ahead of injecting a reductant for the SCR catalyst into the contaminated gas. Such an approach may be motivated by the considerations discussed in relation to the gas treatment system of the invention.

[0131] The contaminated gas, the SCR catalyst, the reductant for the SCR catalyst, and the Cr capture material may, each independently and in combination, be as described according to the gas treatment system of the invention.

[0132] Being located to receive the flow of the contaminated gas, the Cr capture material would preferably be located in a conduit that has the flow of the contaminated gas. In this regard, the Cr capture material may, in respect of a particular process or system, be located in one or more such conduits, correspondingly to receive one or more such flows of contaminated gas at one or more locations in the system or process.

[0133] In an embodiment of the invention, the method includes injecting a reductant for the SCR catalyst into the flow of contaminated gas, wherein the flow of contaminated gas is contactedwith the Cr capture material upstream of injecting a reductant for the SCR catalyst into the contaminated gas.

[0134] In such an embodiment of the invention, the contaminated gas may be at a temperature at or above 300°C, more typically at or above 400°C. It is not excluded, however, that the contaminated gas may in such an embodiment be at a temperature below 400°C, or below 300°C, for example in the range of 200°C to 400°C, such as in the range of 200°C to 300°C.

[0135] In an embodiment of the invention, the method includes injecting a reductant for the SCR catalyst into the flow of contaminated gas, wherein the flow of contaminated gas is contacted with the Cr capture material downstream of injecting a reductant for the SCR catalyst into the contaminated gas.

[0136] In such an embodiment of the invention, the contaminated gas may be at a temperature below 400°C or below 300°C, preferably in the range of 200°C to 400°C, more preferably in the range of 200°C to 300°C.

[0137] In an embodiment of the invention, no reductant for the SCR catalyst is injected into the flow of contaminated gas, i.e. the method excludes injecting a reductant for the SCR into the flow of contaminated gas. This would, as discussed earlier, typically be the case when the contaminated gas is produced including a reductant for the SCR catalyst. Examples include hydrogen or hydrocarbons.

[0138] Contacting the contaminated gas with the Cr capture material produces a Cr contaminant lean gas, which may be Cr contaminant lean or Cr contaminant free.

[0139] The Cr contaminant lean gas would subsequently be supplied to and contacted with the SCR catalyst, to abate NOx contaminants in the Cr contaminant lean gas and thus produce a cleaned gas.

[0140] In another aspect, the invention provides a process for producing syngas and optionally hydrogen, the process including

[0141] subjecting a mixture of hydrocarbon and steam to steam methane reforming, thus producing a reformed gas mixture comprising hydrogen and carbon monoxide and an off gas comprising NOx and Cr contaminants; andcontacting a flow of the off gas with a Cr capture material upstream of a SCR catalyst such that the Cr capture material captures at least some of the Cr contaminants from the off gas upstream of the SCR catalyst.

[0142] The off gas may be a contaminated gas as provided for in relation to the system and method of the invention.

[0143] Contacting the flow of the off gas with the Cr capture material may be provided for and / or performed in accordance with the system and method aspects of the invention.

[0144] The process may include subjecting the reformed gas mixture to water gas shift and recovering carbon dioxide from a product thereof to product, thus producing a crude hydrogen product gas which can subsequently be purified to produce a purified hydrogen product gas.

[0145] In another aspect, the invention provides a process for producing ethylene, the process including

[0146] subjecting a mixture of hydrocarbon and steam to steam cracking, thus producing a cracked gas mixture comprising ethylene and an off gas comprising NOx and Cr contaminants; and

[0147] contacting a flow of the off gas with a Cr capture material upstream of a SCR catalyst such that the Cr capture material captures at least some of the Cr contaminants from the off gas upstream of the SCR catalyst.

[0148] The off gas may be a contaminated gas as provided for in relation to the system and method of the invention.

[0149] Contacting the flow of the off gas with the Cr capture material may be provided for and / or performed in accordance with the system and method aspects of the invention.

[0150] Selected embodiments of the invention will now be described, by way of example only, with reference to the drawings.

[0151] Referring to the drawings, and specifically Figure 1, reference numeral 10 generally indicates one embodiment of a gas treatment system according to the invention.The system 10 includes a Cr capture material in accordance with the invention as herein described, generally represented by reference numeral 12, and a SCR catalyst, generally represented by reference numeral 14.

[0152] The Cr capture material 12 is located upstream of the SCR catalyst 14, relative to a direction of a flow of a contaminated gas. Such a flow of a contaminated gas, comprising Cr and NOx contaminants, is supplied to the Cr capture material 12 along line 16. The contaminated gas emanates from a source thereof, which may be as hereinbefore described. For example, the source may be SMR.

[0153] The contaminated gas is contacted with the Cr capture material 12 and Cr contaminants in the contaminated gas are thus captured from the contaminated gas, producing a Cr contaminant lean gas, which may be Cr contaminant lean or Cr contaminant free. A flow of the Cr contaminant lean gas leaves the Cr capture material 12 along line 18.

[0154] A reductant for the SCR catalyst 14, preferably being ammonia or urea, is injected, from a source 20 thereof and along line 22, into the flow of the Cr contaminant lean gas in line 18. Such injection is thus performed downstream of the Cr capture material 12.

[0155] The flow of the Cr contaminant lean gas, including the reductant for the SCR catalyst 14, is then supplied, along line 18, to the SCR catalyst 14 and is contacted with the SCR catalyst 14, thus abating NOx contaminants in the contaminated gas and producing a cleaned gas.

[0156] A flow of the cleaned gas leaves the SCR catalyst 14 along line 24, which typically vents to the atmosphere.

[0157] In the system 10, the contaminated gas is typically at a temperature above 300°C, more typically at or above 400°C, although lower temperatures are not excluded.

[0158] For the higher temperatures, however, providing for the SCR reductant injection to be performed downstream of the Cr capture material 12 is particularly preferred, to avoid oxidation of the SCR reductant by the Cr capture material 12 at such higher temperatures.1

[0159] Referring to Figure 2, reference numeral 100 generally indicates another embodiment of a gas treatment system according to the invention. Components of the system 100 that are shared with the system 10 are indicated by the same reference numerals used in Figure 1.

[0160] In the system 100, the SCR reductant is injected into the flow of contaminated gas in line 12, rather than being injected into the flow of the Cr contaminant lean gas in line 18. Thus, such injection is performed upstream of the Cr capture material 12, rather than being performed downstream of it.

[0161] Such injection of the SCR reductant upstream of the Cr capture material 12, in accordance with the invention, is preferred at lower temperatures, typically being temperatures below 400°C or below 300°C, preferably in the range of 200°C to 400°C, more preferably in the range of 200°C to 300°C.

[0162] Referring to Figure 3, reference numeral 200 generally indicates another embodiment of a gas treatment system according to the invention. Components of the system 200 that are shared with the system 10 are indicated by the same reference numerals used in Figure 1.

[0163] In the system 200, there is no provision made for injecting a SCR reductant upstream of the SCR catalyst 14, whether into the flow of contaminated gas in line 12 or into the flow of Cr contaminant lean gas in line 18.

[0164] In the system 200, injection of a SCR reductant is omitted since the contaminated gas in line 12 already includes a SCR reductant. Typically, such a reductant is hydrogen or hydrocarbons.

[0165] For example, where the contaminated gas is produced from the combustion of hydrogen or hydrocarbons, there may be sufficient non-combusted hydrogen or hydrocarbons in the contaminated gas for the SCR catalyst 14 to abate NOx in the contaminated gas without the addition of further reductant.

[0166] Example

[0167] The effect of the presence of a Cr enriched Cr capture material in the flow path of an ammonia reductant for a SCR catalyst was simulated to determine the feasibility of SCR reductantinjection upstream of a Cr capture material that is, in turn, upstream of a SCR catalyst. The advantages of being able to do so have been discussed above.

[0168] A coated chromium source was prepared on a 400 cells per square inch (CPSI) cordierite substrate, using a washcoat method.

[0169] The washcoat, with respect to the substrate, contained C^Ch at 1 ,6g / in3loading.

[0170] The substrate having the washcoat was calcined at 1200°C for 4hrs.

[0171] The core of the substrate was 1” (2.5 cm) diameter by 3” (7.6 cm) length.

[0172] Two of the abovementioned Cr loaded substrates were longitudinally arranged in series, such that one provided an inlet end of the arrangement thereof and the other provided an outlet end of the arrangement thereof.

[0173] A gas comprising 50ppm ammonia (NH3), 10 vol% O2, 8 vol% H2O, 3 vol% CO2, and balanced by N2 was supplied to the substrates, entering the substrates through the inlet end and leaving the substrates through the outlet end at a rate of 75 SLPM (standard litre per minute).

[0174] Ammonia conversion, over the substrates were measured at steady state temperature points. The results are shown in Table 1.

[0175] Table 1 : Results of NH3 conversion over Cr loaded substrate.

[0176] Outlet NOXProduced (ppm)

[0177] Inlet T (°C) NH3Conversion (%)

[0178] Inlet to SCR

[0179] 214 4.4 0

[0180] 249 2.6 0.2

[0181] 296 9.3 3.0

[0182] 344 37.8 14.0

[0183] 401 77.1 30.3

[0184] 451 86.4 34.4

[0185]

[0186] 500 91.3 39.9

[0187] Surprisingly, at lower temperatures, the extent to which ammonia is oxidised by the Cr of the Cr loaded substrate is sufficiently low that reductant injection upstream of the Cr capturematerial in a gas treatment system according to the invention, see for example Figure 2, would be feasible.

[0188] Thus, under suitable temperature conditions, the Cr capture material may conveniently be placed downstream of the injection of a reductant for the SCR catalyst into the contaminated gas, when such injection is needed. Advantageously, this allows for the Cr capture material to be placed closer to the SCR catalyst and, thus, for fresh contamination that may occur downstream of the Cr capture material and upstream of the SCR catalyst to be limited or avoided. A risk of such contamination downstream of the Cr capture material and upstream of the SCR catalyst would be appreciated to be a possibility when provision is made for SCR reductant injection between the Cr capture material and the SCR catalyst

[0189] The effect of Cr ageing on a SCR’s NOx conversion performance was also investigated.

[0190] An extruded SCR catalyst, with 300 cells per square inch (CPSI) was prepared containing AEI zeolite, copper, clays, and fibres.

[0191] The core of the substrate was 1” (2.5 cm) diameter by 2” (5 cm) length.

[0192] The effect of Cr ageing on NOx conversion was simulated by positioning the extruded SCR catalyst 2mm downstream of a Cr-source at an operating temperature of 450°C. A gas comprising air and 3 vol% H2O was supplied to the extruded SCR catalyst, entering the substrate through an inlet end and leaving the substrates through an outlet end at a rate of 14 SLPM for 24 hours. The temperature was then increased to 650°C and the flow rate of the gas was increased to 21.5 SLPM for an additional 90 hours to Cr age SCR catalyst in the presence of Cr (i.e. Cr ageing of the catalyst).

[0193] The extruded SCR catalyst was tested in a reactor at operating temperatures from 200°C to 450°C: The various operating conditions to which the SCR was subjected to are provided in Table 2.

[0194] Table 2: Operating conditions.

[0195] Condition GHSV [tr1] NO [ppm] NH3[ppm] O2[%] H2O [%] Fresh 225,000 50 50 3 17.5 Cr Aged 225,000 50 50 3 17.5

[0196]

[0197] The NOx conversion as measured at the operating conditions of Table 2 are shown in Table 3. It can be seen that the Cr exposure on a SCR catalyst has a detrimental effect on a SCR’s NOx conversion performance. It can be seen that NOx conversion achieved by a Cr aged SCR is consistently lower than the NOx conversion achieved by a fresh SCR, i.e. a SCR that has not been subjected to Cr ageing. It is therefore an objective of the present invention to alleviate this problem and to increase the NOx conversion in the presence of Cr contaminants.

[0198] Table 3: NOx conversion at fresh and Cr Aged conditions.

[0199] NOx Conversion (%)

[0200] Condition 200°C 250°C 300°C 350°C 400°C 450°C Fresh 23.1 44.3 55.7 58.4 60.7 56.9 Cr Aged 16.1 41.0 48.7 48.2 48.4 43.3

[0201]

[0202] The performance of a Cr getter at different temperatures were evaluated. A Cr getter was prepared on a 400 CPSI cordierite substrate and coated on a 4.16”x3” (10.6cm x 7.6cm) block. The Cr getter was prepared by preparing separate batches of a 3wt% lanthanum stabilized alumina slurry, 58wt% ceria-42wt% zirconia mixed oxide slurry, and a 72wt% zirconia 21.5wt% ceria, 1.5wt% lanthanum oxide and 5wt% neodymium oxide slurry. Following that, blending La-alumina, Ce-Zr, and Ce-Zr-La-Nd slurries in a 1.0: 1.2: 1.5 ratio. After blending 300 g / ft3(10.6 g / l) of barium acetate was added to the blended washcoat then a binder was added and the slurry was mixed. This was followed by the addition of 300g / ft3(10 g / l) strontium nitrate while mixing. Finally, the solids content and viscosity was adjusted appropriately to produce a washcoat slurry. The 400 CPSI cordierite substrate was coated with the washcoat slurry, dried and calcined. A 1”x1” (2.5 cm x 2.5 cm) core was taken and used for testing.

[0203] The chromium capture information at various temperatures is shown in Table 4.

[0204] Table 4: Cr Capture data is shown in the table at various Getter temperatures.

[0205] Inlet Cr Transpiration Rate (pg / hour) 45.5 40.1 45.5 50.5 50.5 GHSV of Cr-Getter (1 / hour) 100,000 100,000 100,000 100,000 100,000 Cr-Getter Temperature (°C) 200 485 550 615 800 Time on Stream (hours) 150 300 150 100 100

[0206]

[0207] Cr Capture (%) 82.1 90.4 94 96.5 95.9The performance of a Cr getter on a 64 CPSI cordierite substrate was evaluated. The Cr getter was coated on a 150x150x150mm (15 cm x 15 cm x 15 cm) 64 PSI cordierite square block. The Cr getter was prepared by slurrying a 5% Si doped alumina washcoat. To that washcoat 300g / ft3of barium acetate and 300g / ft3of strontium nitrate were added to the slurry, while mixing. A binder was subsequently added, and the slurry was allowed to mix. The 64 CPSI cordierite substrate was then coated with the washcoat slurry, dried and calcined. A 1”x3” (2.5 cm x 7.6 cm) core was taken and used for testing.

[0208] The Cr getter was tested under conditions similar to SMR conditions, with the water content being increased to 15%, which significantly increased the inlet Cr transpiration rate into the Cr Getter up to 119.4 pg / hour. The chromium capture data is shown in Table 5.

[0209] Even with the lower cell density coated Cr-Getter, the capture efficiency is still found to be greater than 90% and highly effective. This surprising result means that the system according to the invention can operate with low back-pressure, which the inventor has found leads to improved system efficiency and performance.

[0210] Table 5: Cr Capture data is shown in the table at 550 °C.

[0211] Inlet Cr Transpiration Rate (pg / hour) 119.4

[0212] GHSV of Cr-Getter (1 / hour) 30,000

[0213] Cr-Getter Temperature (°C) 550

[0214] Time on Steam (hours) 150

[0215]

[0216] Cr Capture (%) 92.1

Claims

Claims1. A gas treatment system for treating a contaminated gas comprising NOx and Cr contaminants, the gas treatment system comprising a SCR catalyst that is located to receive a flow of the contaminated gas and a Cr capture material that is located to capture at least some of the Cr contaminants from the contaminated gas upstream of the SCR catalyst.

2. The gas treatment system according to claim 1 , wherein the Cr capture material is located to capture at least some of the Cr contaminants from the contaminated gas upstream of injecting a reductant for the SCR catalyst into the contaminated gas.

3. The gas treatment system according to claim 2, wherein the contaminated gas is at a temperature at or above 400°C.

4. The gas treatment system according to claim 1 , wherein the Cr capture material is located to capture at least some of the Cr contaminants from the contaminated gas downstream of injecting a reductant for the SCR catalyst into the contaminated gas.

5. The gas treatment system according to claim 4, wherein the contaminated gas is at a temperature below 400°C, preferably in the range of 200°C to 400°C, more preferably in the range of 200°C to 300°C.

6. The gas treatment system according to any one of claims 1 to 5, wherein the contaminated gas comprises less than 3 vol% oxygen and from 10 vol% to 30 vol% water.

7. The gas treatment system according to any one of claims 1 to 6, wherein the contaminated gas emanates from SMR of a hydrogen production process or from an ethylene production process.

8. The gas treatment system according to any one of claims 1 to 7, wherein the Cr capture material comprises one or more Cr capture material species selected from one or more alkaline earth metals, one or more transition metals or combinations thereof.

9. The gas treatment system according to any one of claims 1 to 8, wherein the Cr capture material is provided by a catalyst article comprising a substrate having a cell densityof 300 CPSI or less, preferably 200 CPSI or less, preferably 100 CPSI or less, more preferably less than 70 CPSI.

10. A method of treating a contaminated gas comprising NOxand Cr contaminants, the method comprising contacting a flow of the contaminated gas that is supplied to a SCR catalyst with a Cr capture material upstream of the SCR catalyst such that the Cr capture material captures at least some of the Cr contaminants from the contaminated gas upstream of the SCR catalyst.

11. The method according to claim 10, which includes injecting a reductant for the SCR catalyst into the flow of contaminated gas and wherein the flow of contaminated gas is contacted with the Cr capture material upstream of injecting a reductant for the SCR catalyst into the contaminated gas.

12. The gas treatment system according to claim 11, wherein the contaminated gas is at a temperature at or above 400°C.

13. The gas treatment system according to claim 10, which includes injecting a reductant for the SCR catalyst into the flow of contaminated gas and wherein the flow of contaminated gas is contacted with the Cr capture material downstream of injecting a reductant for the SCR catalyst into the contaminated gas.

14. The gas treatment system according to claim 13, wherein the contaminated gas is at a temperature below 400°C, preferably in the range of 200°C to 400°C, more preferably in the range of 200°C to 300°C.

15. The gas treatment system according to any one of claims 10 to 14, wherein the contaminated gas comprises less than 3 vol% oxygen and from 15 vol% to 20 vol% water.