Stretch hood film structure

The multilayer film structure with ethylene/a-olefin copolymers addresses the recyclability challenge of non-polyethylene films by achieving high mechanical properties suitable for stretch hood processes.

WO2026234489A1PCT designated stage Publication Date: 2026-11-12NOVA CHEM (INT) SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2026/054079
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-05
Filing Date
2026-04-24
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing multilayer films for stretch hood processes containing non-polyethylene materials pose challenges in mechanical recycling and there is a need for all-polyethylene film structures that maintain elasticity, holding force, and toughness.

Method used

A multilayer film structure comprising an inner layer and skin layers made of ethylene/a-olefin copolymers with specific density and melt index ranges, characterized by melting peaks and heat of fusion, to achieve high machine-direction elastic recovery, holding force, and tear resistance.

Benefits of technology

The film structure provides enhanced mechanical properties, including machine-direction elastic recovery, holding force, and tear resistance, while being fully recyclable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000001_0001
    Figure IMGF000001_0001
  • Figure IMGF000001_0002
    Figure IMGF000001_0002
  • Figure IMGF000003_0001
    Figure IMGF000003_0001
Patent Text Reader

Abstract

A multilayer film structure, comprising: an inner layer; a first skin layer; and a second skin layer. The inner layer comprises a first ethylene / α-olefin copolymer composition, wherein the first ethylene / α-olefin copolymer composition comprises about 55 weight percent of ethylene or greater than 55 weight percent of ethylene. The first ethylene / α-olefin copolymer composition has: a density, ρ1, of from about 0.880 g / cm3 to about 0.913 g / cm3, as determined in accordance with ASTM D792; and a melt index I2 1 of from about 0.1 dg / min to about 2 dg / min, as determined in accordance with ASTM D1238 at 190°C and at a loading 2.16 kg. The first skin layer and a second skin layer, each independently comprises a second ethylene / α-olefin copolymer composition, the second ethylene / α-olefin copolymer composition having a melt index, I2 2, of from about 0.1 dg / min to about 2 dg / min, as determined in accordance with ASTM D1238 at 190°C and at a loading 2.16 kg, and a density, ρ2, of from about 0.910 g / cm3 to about 0.935 g / cm3, as determined in accordance with ASTM D792. The first ethylene / α-olefin copolymer composition and the second ethylene / α-olefin copolymer composition may further be characterized by defined thermal and fractionation characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] STRETCH HOOD FILM STRUCTURE

[0002] TECHNICAL FIELD

[0003] The present disclosure generally relates to multilayer films structures, and in particular, relates to multilayer films structures suitable for stretch hood processes.

[0004] BACKGROUND ART

[0005] Stretch hood is a process for unitizing packaged goods with minimal heat requirements and high packaging speeds. Suitable multilayer film designs for this process typically include three-layer films that rely on ethylene-vinyl acetate (EVA) copolymers, ethyl ene-butyl acrylate (EBA) copolymers, and ethyl ene-propylene copolymers (with a propylene content » 50 wt.%) to achieve a balance of elasticity, holding force, and toughness / abuse resistance properties. Multilayered films containing more than 10% by weight of non-polyethylene materials are known to pose challenges in polyethylene mechanical recycling processes. Thus, despite advancements in stretch hood technology, there remains a significant need to develop new film structures, particularly those that address the demand for all-polyethylene film structures.

[0006] SUMMARY OF INVENTION

[0007] Provided in a first aspect is a multilayer film structure, comprising: an inner layer; a first skin layer; and a second skin layer. The inner layer of the first aspect comprises a first ethylene / a-olefin copolymer composition. The first ethylene / a-olefin copolymer composition of the first aspect comprises about 55 weight percent of ethylene or greater than 55 weight percent of ethylene, and has a density,1, of from about 0.880 g / cm3to about 0.913 g / cm3, as determined in accordance with ASTM D792 and a melt index I21of from about 0.1 dg / min to about 2 dg / min, as determined in accordance with ASTM DI 238 at 190°C at a loading 2.16 kg. The first ethylene / a-olefin copolymer composition of the first aspect is further characterized by at least one melting peak, as determined by differential scanning calorimetry, at a temperature greater than a first density-adjusted temperature,

[0008]

[0009] Ta(pl), the first density-adjusted temperature being defined according to Ta(

[0010]

[0011] pl) = 103xpl- 800.

[0012] The first skin layer and the second skin layer of the first aspect each independently comprise a second ethylene / a-olefin copolymer composition. The second ethylene / a-olefin copolymer composition of the first aspect has a melt index, I22, of from about 0.1 dg / min to about 2 dg / min, as determined in accordance with ASTM DI 238 at 190°C at a loading2.16 kg, and a density, / )2, of from about 0.910 g / cm3to about 0.935 g / cm3, as determined in accordance with ASTM D792.

[0013] In some embodiments of the first aspect, the inner layer is a core layer.

[0014] In some embodiments of the first aspect, the first ethylene / a-olefin copolymer composition and the second ethylene / a-olefin copolymer composition each independently comprise one or more than one C4 to C10 a-olefin.

[0015] In some embodiments of the first aspect, the first ethylene / a-olefin copolymer composition and the second ethylene / a-olefin copolymer composition each independently comprise one or more than one a-olefin selected from the group consisting of octene, hexene and mixtures thereof.

[0016] In some embodiments of the first aspect, the density of second ethylene / a-olefin copolymer composition, / )2, is greater than the density of the first ethylene / a-olefin copolymer composition, / )1.

[0017] In some embodiments of the first aspect, the first ethylene / a-olefin copolymer composition further has a heat of fusion, as determined by differential scanning calorimetry, of greater than about 10 J / g and less than about 35 J / g above the first density-adjusted temperature, Tapl).

[0018] In some embodiments of the first aspect, the first ethylene / a-olefin copolymer composition has at least one melting peak, as determined by differential scanning calorimetry, at a temperature less than the first density-adjusted temperature, 7 i / ( / )1).

[0019] In some embodiments of the first aspect, the first ethylene / a-olefin copolymer composition is an in-situ blend comprising a first homogeneously-branched ethylene / a-olefin copolymer and a first heterogeneously-branched ethylene / a-olefin copolymer.

[0020] In some embodiments of the first aspect, the first ethylene / a-olefin copolymer composition has a poly dispersity index, Mw / Mnof from about 2.5 to 5, as determined by conventional gel permeation chromatography.

[0021] In some embodiments of the first aspect, the first ethylene / a-olefin copolymer composition has a ratio of z-average molecular weight to weight-average molecular weight, Mz / Mw of from about 2 to 4, as determined by conventional gel permeation chromatography.

[0022] In some embodiments of the first aspect, the density of the first ethylene / a-olefin copolymer composition, p has a value ranging from greater than or equal to 0.895 g / cm3to less than or equal to 0.910 g / cm3, as determined in accordance with ASTM D792.

[0023] In some embodiments of the first aspect, the second ethylene / a-olefin copolymer composition has at least one melting peak, as determined by differential scanning calorimetry,at a temperature greater than a second density-adjusted temperature, Ta(2), the second density-adjusted temperature being defined according to

[0024]

[0025] Ta(p2) = I 03 / / r - 800.

[0026] In some embodiments of the first aspect, the second ethylene / a-olefin copolymer composition has at least one melting peak, as determined by differential scanning calorimetry, at a temperature less than the second density-adjusted temperature, Ta(2).

[0027] In some embodiments of the first aspect, the second ethylene / a-olefin copolymer composition further has a heat of fusion, as determined by differential scanning calorimetry, of greater than about 10 J / g and less than about 45 J / g above the second density-adjusted temperature, Ta(2).

[0028] In some embodiments of the first aspect, the multilayer film structure is a blown multilayer film structure, and wherein the multilayer film structure is characterized by at least one of the following features: a machine-direction elastic recovery of greater than 50%, as determined by ASTM D5459; a machine-direction holding force of greater than 10 N, as determined by ASTM D5459; a machine-direction tear propagation resistance of greater than 0.5 pound-force, as determined by ASTM D1938; a machine-direction tear resistance of greater than 300 g / mil, as determined by ASTM DI 922; and a machine-direction stress at yield of greater than 7 MPa as determined by ASTM D882.

[0029] In some embodiments of the first aspect, at least one of the first skin layer and the second skin layer is in adhering contact with the inner layer.

[0030] In some embodiments of the first aspect, a ratio of the first skin layer thickness to the inner layer thickness and a ratio of the second skin layer thickness to the inner layer thickness are independently greater than 1:1.

[0031] In some embodiments of the first aspect, a ratio of the inner layer thickness to an overall thickness of the multilayer film structure is less than 1 :2.

[0032] In some embodiments of the first aspect, the inner layer is an all-polyethylene film layer.

[0033] In some embodiments of the first aspect, the multilayer film structure is an allpolyethylene structure.

[0034] Provided in a second aspect is a multilayer film structure, comprising: an inner layer; a first skin layer; and a second skin layer. The inner layer of the second aspect comprises a first ethylene / a-olefin copolymer composition. The first ethylene / a-olefin copolymer composition of the second aspect comprises about 55 weight percent of ethylene or greater than 55 weight percent of ethylene, and has a density,1, of from about 0.880 g / cm3to about 0.913 g / cm3, as determined in accordance with ASTM D792 and a melt index I21of fromabout 0.1 dg / min to about 2 dg / min, as determined in accordance with ASTM D1238 at 190°C at a loading 2.16 kg.

[0035] The first skin layer and the second skin layer of the second aspect each independently comprise a second ethyl ene / a-olefin copolymer composition The second ethylene / a-olefin copolymer composition of the second aspect has a melt index, I22, of from about 0.1 dg / min to about 2 dg / min, as determined in accordance with ASTM DI 238 at 190°C at a loading 2.16 kg and a density,2, of from about 0.910 g / cm3to about 0.935 g / cm3, as determined in accordance with ASTM D792. The second ethylene / a-olefin copolymer composition of the second aspect is further characterized by a single melting peak, as determined by differential scanning calorimetry, and a temperature rising elution fractionation, TREF, profile comprising at least two peaks within a temperature range of from about 75°C to about 100°C.

[0036] In some embodiments of the second aspect, the inner layer is a core layer.

[0037] In some embodiments of the second aspect, the first ethylene / a-olefin copolymer composition and the second ethylene / a-olefin copolymer composition each independently comprise one or more than one C4 to C10 a-olefin.

[0038] In some embodiments of the second aspect, the first ethylene / a-olefin copolymer composition and the second ethylene / a-olefin copolymer composition each independently comprise one or more than one a-olefin selected from the group consisting of octene, hexene and mixtures thereof.

[0039] In some embodiments of the second aspect, the second ethylene / a-olefin copolymer composition has a poly dispersity index, Mw / Mnof from about 3 to 6, as determined by conventional gel permeation chromatography.

[0040] In some embodiments of the second aspect, the second ethylene / a-olefin copolymer composition has a ratio of z-average molecular weight to weight-average molecular weight, Mz / Mw of from about 2 to 4, as determined by conventional gel permeation chromatography.

[0041] In some embodiments of the second aspect, the density of the second ethylene / a-olefin copolymer composition,2, has a value ranging from greater than or equal to 0.913 g / cm3to less than or equal to 0.925 g / cm3, as determined in accordance with ASTM D792.

[0042] In some embodiments of the second aspect, the single melting peak of the second ethylene / a-olefin copolymer composition occurs at a temperature less than a second density-adjusted temperature, 7 (2), the second density-adjusted temperature being defined according to Ta(p2) = I 03* r - 800.

[0043] In some embodiments of the second aspect, the multilayer film structure is a blown multilayer film structure, and wherein the multilayer film structure is characterized by at leastone of the following features: a machine-direction elastic recovery of greater than 50%, as determined by ASTM D5459; a machine-direction holding force of greater than 10 N, as determined by ASTM D5459; a machine-direction tear propagation resistance of greater than 0.75 pound-force, as determined by ASTM D1938; a machine-direction tear resistance of greater than 300 g / mil, as determined by ASTM DI 922; and a machine-direction stress at yield of greater than 4 MPa as determined by ASTM D882.

[0044] In some embodiments of the second aspect, the first ethylene / a-olefin copolymer composition has a single melting peak, as determined by differential scanning calorimetry.

[0045] In some embodiments of the second aspect, the first ethylene / a-olefin copolymer composition has a single melting peak, as determined by differential scanning calorimetry. In these embodiments, the multilayer film structure, when prepared by film blowing, may be characterized by at least one of the following features: a machine-direction elastic recovery of greater than 50%, as determined by ASTM D5459; a machine-direction holding force of greater than 10 N, as determined by ASTM D5459; a machine-direction tear propagation resistance of greater than 1.5 pound-force, as determined by ASTM D1938; a machinedirection tear resistance of greater than 350 g / mil, as determined by ASTM DI 922; and a machine-direction stress at yield of greater than 5 MPa as determined by ASTM D882.

[0046] In some embodiments of the second aspect, at least one of the first skin layer and the second skin layer is in adhering contact with the inner layer.

[0047] In some embodiments of the second aspect, a ratio of the first skin layer thickness to the inner layer thickness and a ratio of the second skin layer thickness to the inner layer thickness are independently greater than 1:1.

[0048] In some embodiments of the second aspect, a ratio of the inner layer thickness to an overall thickness of the multilayer film structure is less than 1 :2.

[0049] In some embodiments of the second aspect, the inner layer is an all-polyethylene film layer.

[0050] In some embodiments of the second aspect, the multilayer film structure is an allpolyethylene structure.

[0051] Definition of Terms

[0052] Other than in the examples or where otherwise indicated, all numbers or expressions referring to quantities of ingredients, extrusion conditions, etc., used in the specification and claims are to be understood as modified in all instances by the term “about”. Accordingly, unless indicated to the contrary, the numerical parameters set forth in the following specification and attached claims are approximations that can vary depending upon thedesired properties that the various embodiments desire to obtain. At the very least, and not as an attempt to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should at least be construed in light of the number of reported significant digits and by applying ordinary rounding techniques. The numerical values set forth in the specific examples are reported as precisely as possible. Any numerical values, however, inherently contain certain errors necessarily resulting from the standard deviation found in their respective testing measurements.

[0053] It should be understood that any numerical range recited herein is intended to include all sub-ranges subsumed therein. For example, a range of “1 to 10” is intended to include all sub-ranges between and including the recited minimum value of 1 and the recited maximum value of 10; that is, having a minimum value equal to or greater than 1 and a maximum value of equal to or less than 10. Because the disclosed numerical ranges are continuous, they include every value between the minimum and maximum values. Unless expressly indicated otherwise, the various numerical ranges specified in this application are approximations.

[0054] All compositional ranges expressed herein are limited in total to and do not exceed 100 percent (volume percent or weight percent) in practice. Where multiple components can be present in a composition, the sum of the maximum amounts of each component can exceed 100 percent, with the understanding that, and as those skilled in the art readily understand, the amounts of the components actually used will conform to the maximum of 100 percent.

[0055] In order to form a more complete understanding of this disclosure the following terms are defined and should be used with the accompanying figures and the description of the various embodiments throughout.

[0056] As used herein, the term “monomer” refers to a small molecule that may chemically react and become chemically bonded with itself or other monomers to form a polymer.

[0057] As used herein, the term “a-olefin” or “alpha-olefin” is used to describe a monomer having a linear hydrocarbon chain having a double bond at one end of the chain and containing from n = 3 to 20 carbon atoms with a chemical formula Cn n, an equivalent term is “linear a-olefin”

[0058] As used herein, the terms “polyethylene”, “polyethylene polymer” or “ethylene polymer”, refers to macromolecules produced from ethylene monomer and optionally at least one a-olefin monomer; regardless of the specific catalyst or specific process used to make the ethylene polymer. Common polyethylenes include high density polyethylene (HDPE), medium density polyethylene (MDPE), linear low density polyethylene (LLDPE), very low density polyethylene (VLDPE), ultralow density polyethylene (ULDPE), plastomer andelastomers. The term polyethylene also includes combinations of, or blends of, the polyethylenes described above. An ethylene polymer in its polymerized form will include greater than 50 weight percent (based on the weight of the ethylene polymer) of ethylene monomeric units.

[0059] As used herein, the term “ethylene homopolymer” refers to a subset of polymers within the “ethylene polymer” group that are produced using only ethylene as a polymerizable monomer.

[0060] The term “ ethyl ene / a-olefin copolymer” refers to a subset of polymers within the “ethylene polymer” group that are produced from ethylene and at least one a-olefin. Thus, as used herein, the term “ethylene / a-olefin copolymer” includes ethylene polymers prepared from two polymerizable monomeric units (i.e., ethylene and one a-olefin) and ethylene polymers prepared from more than two polymerizable monomeric units (i.e., ethylene and two or more than two a-olefins).

[0061] The term “thermoplastic polymer” refers to a polymer that becomes liquid when heated, will flow under pressure and solidify when cooled. Thermoplastic polymers include ethylene polymers as well as other polymers used in the plastic industry; non-limiting examples of other polymers commonly used in film applications include barrier resins (e.g., EVOH), tie resins, polyethylene terephthalate (PET), polyamides, ethylene-vinyl acetate copolymers (EVA) and the like.

[0062] As used herein the term “monolayer film” refers to a film containing a single layer of one or more than one thermoplastic polymer.

[0063] As used herein the term “multilayer film” or “multilayer film structure” refers to a film composed of more than one thermoplastic layer, or optionally non-thermoplastic layers. Non-limiting examples of non-thermoplastic materials include metals (foil) or cellulosic (paper) products. One or more of the thermoplastic layers within a multilayer film (or film structure) may be comprised of more than one thermoplastic.

[0064] As used herein, the term “all polyethylene film layer” refers to a film layer, either as a monolayer film or as one layer within a multilayer film structure, that contains at least 90% by weight, based on the total weight of the film layer, of one or more than one type of ethylene polymers.

[0065] As used herein, the term “all polyethylene multilayer film structure” refers to a multilayer film structure containing greater than or equal to 90% of one or more than one ethylene polymer based on the total weight of the multilayer film structure excluding the nonthermoplastic layers (if present).DESCRIPTION OF EMBODIMENTS

[0066] In the present disclosure, the multilayer film structure will include an inner layer positioned between a first skin layer and a second skin layer. The inner layer includes a first ethylene / a-olefin copolymer composition. Each of the first skin layer and the second skin layer independently includes a second ethylene / a-olefin copolymer composition.

[0067] Inner Laver

[0068] In the present disclosure, the inner layer may be a core layer or a non-core layer. As used herein, the term “core layer” refers to the central layer in a multilayer structure which is exactly positioned at the center of the structure. As used herein, the term “non-core layer” refers to an intermediate layer that is not centrally positioned between the first skin layer and the second skin layer.

[0069] In the present disclosure, the inner layer includes a first ethylene / a-olefin copolymer composition.

[0070] In some embodiments, the inner layer consists essentially of the first ethylene / a-olefin copolymer composition.

[0071] In some embodiments, the inner layer comprises greater than 10 wt.% and less than or equal to 100 wt.% of the first ethylene / a-olefin copolymer composition, based on the total weight of the inner layer. In some embodiments, the inner layer comprises greater than 25 wt.% and less than or equal to 100 wt.% of the first ethylene / a-olefin copolymer composition, based on the total weight of the inner layer. In some embodiments, the inner layer comprises greater than 50 wt.% and less than or equal to 100 wt.% of the first ethylene / a-olefin copolymer composition, based on the total weight of the inner layer. In some embodiments, the inner layer comprises greater than 70 wt.% and less than or equal to 100 wt.% of the first ethylene / a-olefin copolymer composition, based on the total weight of the inner layer. In some embodiments, the inner layer comprises greater than 80 wt.% and less than or equal to 100 wt.% of the first ethylene / a-olefin copolymer composition, based on the total weight of the inner layer. In some embodiments, the inner layer comprises greater than 85 wt.% and less than or equal to 100 wt.% of the first ethylene / a-olefin copolymer composition, based on the total weight of the inner layer. In some embodiments, the inner layer comprises greater than or equal to 90 wt.% and less than or equal to 100 wt.% of the first ethylene / a-olefin copolymer composition, based on the total weight of the inner layer. In some embodiments, the inner layer comprises greater than or equal to 93 wt.% and less than or equal to 100 wt.% of the first ethylene / a-olefin copolymer composition, based on the total weight of the inner layer. In some embodiments, the inner layer comprises greater than or equal to 95 wt.% and less thanor equal to 100 wt.% of the first ethylene / a-olefin copolymer composition, based on the total weight of the inner layer. In some embodiments, the inner layer comprises greater than or equal to 97 wt.% and less than or equal to 100 wt.% of the first ethylene / a-olefin copolymer composition, based on the total weight of the inner layer. In some embodiments, the inner layer comprises greater than or equal to 98 wt.% and less than or equal to 100 wt.% of the first ethylene / a-olefin copolymer composition, based on the total weight of the inner layer.

[0072] The first ethylene / a-olefin copolymer composition comprises about 55 weight percent of ethylene or greater than 55 weight percent of ethylene. In some embodiments, the first ethylene / a-olefin copolymer composition comprises about 55 weight percent of ethylene or greater than 55 weight percent of ethylene and less than 90 weight percent of ethylene. In some embodiments, the first ethylene / a-olefin copolymer composition comprises about 60 weight percent of ethylene or greater than 60 weight percent of ethylene and less than 90 weight percent of ethylene. In some embodiments, the first ethylene / a-olefin copolymer composition comprises about 65 weight percent of ethylene or greater than 65 weight percent of ethylene and less than 90 weight percent of ethylene. In some embodiments, the first ethylene / a-olefin copolymer composition comprises about 70 weight percent of ethylene or greater than 70 weight percent of ethylene and less than 90 weight percent of ethylene. In some embodiments, the first ethylene / a-olefin copolymer composition comprises about 75 weight percent of ethylene or greater than 75 weight percent of ethylene and less than 90 weight percent of ethylene. In some embodiments, the first ethylene / a-olefin copolymer composition comprises about 80 weight percent of ethylene or greater than 80 weight percent of ethylene and less than 90 weight percent of ethylene.

[0073] The first ethylene / a-olefin copolymer composition has a density,1, of from about 0.880 g / cm3to about 0.913 g / cm3, or from about 0.880 g / cm3to about 0.910 g / cm3, about 0.885 g / cm3to about 0.910 g / cm3, about 0.890 g / cm3to about 0.910 g / cm3, about 0.895 g / cm3to about 0.910 g / cm3, about 0.900 g / cm3to about 0.910 g / cm3.

[0074] The first ethylene / a-olefin copolymer composition has a melt index I21of from about 0.1 dg / min to about 2 dg / min, or from about 0.2 dg / min to about 2 dg / min, from about 0.3 dg / min to about 2 dg / min, from about 0.4 dg / min to about 2 dg / min, from about 0.5 dg / min to about 2 dg / min, from about 0.5 dg / min to about 1.5 dg / min.

[0075] In some embodiments, the first ethylene / a-olefin copolymer composition is further characterized by at least one melting peak, as determined by differential scanning calorimetry, at a temperature greater than a first density-adjusted temperature,

[0076]

[0077] Ta(pl), the first density-adjusted temperature being defined according to Ta(

[0078]

[0079] pl) = 103xpl- 800. In these embodiments,the first ethylene / a-olefin copolymer composition may further have a heat of fusion, as determined by differential scanning calorimetry, of greater than about 10 J / g and less than about 30 J / g above the first density-adjusted temperature, p'). In these embodiments, the first ethylene / a-olefin copolymer composition may further have at least one melting peak, as determined by differential scanning calorimetry, at a temperature less than the first density-adjusted temperature, Ta(

[0080]

[0081] pl).

[0082] In some other embodiments, the ethylene / a-olefin copolymer composition may be characterized by a single melting peak, as determined by differential scanning calorimetry.

[0083] The first ethylene / a-olefin copolymer composition comprises one or more than one ethylene / a-olefin copolymer. The one or more than one ethylene / a-olefin copolymer may be brought together by any known method including in-situ blending and post-reactor blending. As used herein, the term “in-situ blending” refers to a blending process in which the blend is formed while polymerization is occurring and is herein distinguished from a physical postreactor blending process. The term “post-reactor blending” refers to a blending process in which the blend is formed by combining two or more than two blend components (e.g., by solution blending and melt blending) wherein each one of the blend components is already polymerized and recovered from the polymerization process — the recovery operations can include catalyst deactivation, phase separation, devolatilizing unreacted monomers and / or process solvent, pelletization, etc. — before being combined with the other blend component(s).

[0084] In some embodiments, the first ethylene / a-olefin copolymer composition is an in-situ blend comprising a first homogeneously branched ethylene / a-olefin copolymer and a first heterogeneously branched ethylene / a-olefin copolymer. An in-situ blend may be produced through a process involving a single polymerization reactor or a process involving mor than one polymerization reactor. As used herein, the term “homogeneously branched ethylene / a-olefin copolymer” refers to a subset of ethylene / a-olefin copolymers group that are produced using single-site catalysts. Non-limiting examples of single-site catalysts include metallocene catalysts, phosphinimine catalysts, and constrained geometry catalysts, all of which are well known in the art. As used herein, the term “heterogeneously branched ethylene / a-olefin copolymer” refers to a subset of ethylene / a-olefin copolymers that are produced using a heterogeneous catalyst system. A non-limiting example of heterogeneous catalysts includes Ziegler-Natta catalysts which are well known in the art. In these embodiments, the first homogeneously branched ethylene / a-olefin copolymer may have a poly dispersity index, Mw / Mn, of less than 2.8; and the first heterogeneously branched ethylene / a-olefin copolymermay have a poly dispersity index greater than the poly dispersity index of the first homogeneously branched ethylene / a-olefin copolymer.

[0085] The first ethylene / a-olefin copolymer composition may further comprise one or more than one antioxidant. In some embodiments, the first ethylene / a-olefin copolymer composition comprises a primary antioxidant and a secondary antioxidant. Non-limiting examples of suitable primary antioxidants include IRGANOX® 1010 (CAS 6683-19-8) and IRGANOX 1076 (CAS 2082-79-3); both available from BASF Corporation. Anon-limiting example of suitable secondary antioxidant is IRGAFOS® 168 (CAS 31570-04-4), available from BASF Corporation.

[0086] In some embodiments, the first ethylene / a-olefin copolymer composition has a poly dispersity index, Mw / Mnof from about 2.5 to about 5, as determined by conventional gel permeation chromatography.

[0087] In some embodiments, the first ethylene / a-olefin copolymer composition has a ratio of z-average molecular weight to weight-average molecular weight, Mz / Mwof from about 2 to about 4, as determined by conventional gel permeation chromatography.

[0088] In some embodiments, the first ethylene / a-olefin copolymer composition comprises one or more than one C4 to C10 a-olefin.

[0089] In some embodiments, the first ethylene / a-olefin copolymer composition comprises one or more than one a-olefin selected from the group consisting of octene, hexene and mixtures thereof.

[0090] The First and Second Skin Layers

[0091] The first skin layer and the second skin layer are the outermost layers in the multilayer film structure.

[0092] The first skin layer and the second skin layer each independently comprise a second ethylene / a-olefin copolymer composition.

[0093] In some embodiments, the first skin layer comprises greater than 10 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the first skin layer. In some embodiments, the first skin layer comprises greater than 10 wt.% and less than 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the first skin layer. In some embodiments, the first skin layer comprises greater than 20 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the first skin layer. In some embodiments, the first skin layer comprises greater than 30 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weightof the first skin layer. In some embodiments, the first skin layer comprises greater than 40 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the first skin layer. In some embodiments, the first skin layer comprises greater than 50 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the first skin layer. In some embodiments, the first skin layer comprises greater than 60 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the first skin layer. In some embodiments, the first skin layer comprises greater than 70 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the first skin layer. In some embodiments, the first skin layer comprises greater than 80 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the first skin layer. In some embodiments, the first skin layer comprises greater than 85 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the first skin layer. In some embodiments, the first skin layer comprises greater than 90 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the first skin layer. In some embodiments, the first skin layer comprises greater than 93 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the first skin layer.

[0094] In some embodiments, the second skin layer comprises greater than 10 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the second skin layer. In some embodiments, the second skin layer comprises greater than 20 wt.% and less than or equal to 100 wt.% of the second ethyl ene / a-olefin copolymer composition, based on the total weight of the second skin layer. In some embodiments, the second skin layer comprises greater than 30 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the second skin layer. In some embodiments, the second skin layer comprises greater than 40 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the second skin layer. In some embodiments, the second skin layer comprises greater than 50 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the second skin layer. In some embodiments, the second skin layer comprises greater than 60 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the second skin layer. In some embodiments, the second skin layercomprises greater than 70 wt.% and less than or equal to 100 wt.% of the second ethyl ene / a-olefin copolymer composition, based on the total weight of the second skin layer. In some embodiments, the second skin layer comprises greater than 80 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the second skin layer. In some embodiments, the second skin layer comprises greater than 85 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the second skin layer. In some embodiments, the second skin layer comprises greater than 90 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the second skin layer. In some embodiments, the second skin layer comprises greater than 93 wt.% and less than or equal to 100 wt.% of the second ethylene / a-olefin copolymer composition, based on the total weight of the second skin layer.

[0095] The second ethylene / a-olefin copolymer composition has a melt index, I22, of from about 0.1 dg / min to about 2 dg / min, or from about 0.2 dg / min to about 2 dg / min, from about 0.3 dg / min to about 2 dg / min, from about 0.4 dg / min to about 2 dg / min, from about 0.5 dg / min to about 2 dg / min, from about 0.5 dg / min to about 1.5 dg / min.

[0096] The second ethylene / a-olefin copolymer composition has a density, / )2, of from about 0.910 g / cm3to about 0.935 g / cm3, or from about 0.912 g / cm3to about 0.935 g / cm3, or from about 0.912 g / cm3to about 0.932 g / cm3, or from about 0.912 g / cm3to about 0.930 g / cm3, or from about 0.913 g / cm3to about 0.930 g / cm3, or from about 0.913 g / cm3to about 0.928 g / cm3, or from about 0.913 g / cm3to about 0.926 g / cm3, or from about 0.913 g / cm3to about 0.925 g / cm3, or from about 0.913 g / cm3to about 0.922 g / cm3, or from about 0.913 g / cm3to about 0.920 g / cm3.

[0097] In some embodiments, the density of second ethylene / a-olefin copolymer composition, / )2, is greater than the density of the first ethylene / a-olefin copolymer composition, / )1.

[0098] In some embodiments, the second ethylene / a-olefin copolymer composition has at least one melting peak, as determined by differential scanning calorimetry, at a temperature greater than a second density-adjusted temperature, 7 (2), the second density-adjusted temperature being defined according

[0099]

[0100] to 7L( / )2) = I03 / / )2- 800. In these embodiments, the second ethylene / a-olefin copolymer composition may further have at least one melting peak, as determined by differential scanning calorimetry, at a temperature less than the second density-adjusted temperature, 7 ( / )2). In these embodiments, the second ethylene / a-olefin copolymer composition may further have a heat of fusion, as determined by differentialscanning calorimetry, of greater than aboutlO J / g and less than about 40 J / g above the second density-adjusted temperature, 7 (2).

[0101] In some other embodiments, the second ethylene / a-olefin copolymer composition has a single melting peak, as determined by differential scanning calorimetry. In these embodiments, the second ethylene / a-olefin copolymer composition has a temperature rising elution fractionation, TREF, profile comprising at least two peaks within a temperature range of from about 75°C to about 100°C. In these embodiments, the single melting peak of the second ethylene / a-olefin copolymer composition may occur at a temperature less than the second density-adjusted temperature, 7 (2).

[0102] The second ethylene / a-olefin copolymer composition comprises one or more than one ethylene / a-olefin copolymer. The one or more than one ethylene / a-olefin copolymer may be brought together by any known method including in-situ blending and post-reactor blending. As used herein, the term “in-situ blending” refers to a blending process in which the blend is formed while polymerization is occurring and is herein distinguished from a physical postreactor blending process. The term “post-reactor blending” refers to a blending process in which the blend is formed by combining two or more than two blend components (e.g., by solution blending and melt blending) wherein each one of the blend components is already polymerized and recovered from the polymerization process — the recovery operations can include catalyst deactivation, phase separation, devolatilizing unreacted monomers and / or process solvent, pelletization, etc. — before being combined with the other blend component(s).

[0103] The second ethylene / a-olefin copolymer composition may further comprise one or more than one antioxidant.

[0104] In some embodiments, the second ethylene / a-olefin copolymer composition comprises one or more than one C4 to C10 a-olefin.

[0105] In some embodiments, the second ethylene / a-olefin copolymer composition comprises one or more than one a-olefin selected from the group consisting of octene, hexene and mixtures thereof.

[0106] At least one of the first skin layer and the second skin layer may further comprise an anti-blocking additive. Non-limiting examples of anti-blocking additives include talc, diatomaceous earth, synthetic silica, kaolin, calcium carbonate, ceramic microspheres. As used herein, the term “anti-blocking additive” refers to any substance that reduces unwanted tendency of film layers to adhere to each other or to other surfaces (e.g., processing equipment).In some embodiments, at least one of the first skin layer and the second skin layer may further comprise an anti-blocking additive. Non-limiting examples of anti-blocking additives include talc, diatomaceous earth, synthetic silica, kaolin, calcium carbonate, ceramic microspheres. As used herein, the term “anti-blocking additive” refers to any substance that reduces unwanted tendency of film layers to adhere to each other or to other surfaces (e.g., processing equipment).

[0107] In some embodiments, at least one of the first skin layer and the second skin layer may further comprise a slip agent selected from oleamide, erucamide, stearamide and behenamide.

[0108] In some embodiments, at least one of the first skin layer and the second skin layer may further comprise a polymer process aid including one or more of a fluoroelastomer and polyethylene glycol.

[0109] Multilayer Film Structure

[0110] The multilayer film structure of the present disclosure can be formed using a variety of techniques known in the art. A non-limiting example of a process to prepare the multilayer film structure includes blown processes. In the blown film extrusion process, an extruder heats, melts, mixes and conveys a thermoplastic or a blend of thermoplastics. Once molten, the thermoplastic is forced through an annular die to produce a thermoplastic tube. In the case of coextrusion, multiple extruders are employed to produce a multilayer thermoplastic tube. The temperature of the extrusion process is primarily determined by the thermoplastic or thermoplastic blend being processed, for example the melting temperature or glass transition temperature of the thermoplastic and the desired viscosity of the melt. In the case of polyolefins, typical extrusion temperatures are from 330°F to 550°F (166°C to 288°C). Upon exit from the annular die, the thermoplastic tube is inflated with air, cooled, solidified and pulled through a pair of nip rollers. Due to air inflation, the tube increases in diameter forming a bubble of desired size. Due to the pulling action of the nip rollers the bubble is stretched in the machine direction. Thus, the bubble is stretched in two directions: the transverse direction (TD) where the inflating air increases the diameter of the bubble; and the machine direction (MD) where the nip rollers stretch the bubble. In the blown film process, air is also blown on the external bubble circumference to cool the thermoplastic as it exits the annular die. The final width of the film is determined by controlling the inflating air or the internal bubble pressure; in other words, increasing or decreasing bubble diameter. Film thickness is controlled primarily by increasing or decreasing the speed of the nip rollers to control thedraw-down rate. After exiting the nip rollers, the bubble or tube is collapsed and may be slit in the machine direction thus creating sheeting.

[0111] The multilayer film structure of the present disclosure may have a thickness ranging from greater than (>) 1 mil to less than (<) 10 mil. In some embodiments, multilayer film structure has a thickness ranging from about 2 mil to about 8 mil, or from about 2.5 mil to about 8 mil, or from about 2.5 mil to about 6 mil, or from about 3 mil to about 6 mil.

[0112] In some embodiments, the multilayer film structure has 3 to 11 layers.

[0113] In some embodiments, the multilayer film structure is a three-layer structure, or a five-layer structure, or a seven-layer structure, or a nine-layer structure, or an eleven-layer structure.

[0114] The multilayer film structures of the present disclosure may be used to form a stretch hood.

[0115] In some embodiments, the thickness of the inner layer within the multilayer film structure may be 20%, in other cases about 30%, in other cases about 35%, in other cases about 40%, in other cases about 45%, in other cases about 50%, in other cases about 55%, in other cases about 60%, in other cases about 65%, in other cases about 70%, in other cases about 75%, and in still other cases about 80% of the total multilayer film thickness.

[0116] In some embodiments, a ratio of the inner layer thickness to the total thickness of the multilayer film structure is less than 1:2 — i.e., the thickness of the inner layer within the multilayer film structure is less than 50% of the total multilayer film thickness. In some embodiments, a ratio of the inner layer thickness to the total thickness of the multilayer film structure is from 1:2 to 1:3 — i.e., the thickness of the inner layer within the multilayer film structure is from 30% to 50%.

[0117] In some embodiments, a ratio of the first skin layer thickness to the inner layer thickness and a ratio of the second skin layer thickness to the inner layer thickness are independently greater than 1:1 — i.e., the first skin layer and the second skin layer are individually thicker than the inner layer.

[0118] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a machine-direction holding force of greater than 10 N.

[0119] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a machine-direction holding force of greater than 10 N and less than 20 N, or greater than 10 N and less than 18 N, or greater than 10 N and less than 15 N.In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a machine-direction elastic recovery of greater than 50%.

[0120] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a machine-direction elastic recovery of greater than 50% and less than 90%, or greater than 50% and less than 85%, or greater than 50% and less than 80%.

[0121] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a machine-direction permanent deformation of greater than 5% and less than 50%, or greater than 10% and less than 50%, or greater than 10% and less than 45%, or greater than 10% and less than 40%, or greater than 10% and less than 35%, or greater than 10% and less than 30%, or greater than 10% and less than 25%.

[0122] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a transverse-direction holding force of greater than 10 N.

[0123] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a transverse-direction holding force of greater than 10 N and less than 20 N, or greater than 10 N and less than 18 N, or greater than 10 N and less than 16 N.

[0124] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a transverse-direction elastic recovery of greater than 50%.

[0125] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a machine-direction elastic recovery of greater than 50% and less than 90%, or greater than 50% and less than 85%, or greater than 50% and less than 80%.

[0126] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a transverse-direction permanent deformation of greater than 10% and less than 50%, or greater than 10% and less than 40%, or greater than 10% and less than 35%, or greater than 10% and less than 30%.

[0127] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a dart impact of greater than 100 g / mil.

[0128] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a dart impact of greater than 150 g / mil.In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a dart impact of greater than 300 g / mil.

[0129] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a dart impact of greater than 400 g / mil.

[0130] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a dart impact of greater than 100 g / mil and less than 1000 g / mil, or greater than 150 g / mil and less than 1000 g / mil, or greater than 300 g / mil and less than 1000 g / mil, or greater than 400 g / mil and less than 1000 g / mil, greater than 400 g / mil and less than 800 g / mil.

[0131] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a machine-direction Elmendorf tear resistance of greater than 200 g / mil and less than 600 g / mil, or greater than 200 g / mil and less than 550 g / mil, or greater than 200 g / mil and less than 450 g / mil.

[0132] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a transverse-direction Elmendorf tear resistance of greater than 300 g / mil and less than 700 g / mil, or greater than 300 g / mil and less than 650 g / mil, or greater than 300 g / mil and less than 600 g / mil.

[0133] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has an energy at break of from 18 J / mm to 42 J / mm, or from 18 J / mm to 40 J / mm, or from 18 J / mm to 35 J / mm, or from 18 J / mm to 32 J / mm.

[0134] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a machine-direction Trouser tear propagation resistance of greater than 0.5 pound-force to less than 4 pound-force, or greater than 0.75 pound-force to less than 3.5 pound-force, or greater than 1 pound-force to less than 3.2 poundforce, or greater than 1 pound-force to less than 3 pound-force.

[0135] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a transverse-direction Trouser tear propagation resistance of greater than 0.6 pound-force to less than 5 pound-force, or greater than 1 poundforce to less than 5 pound-force, or greater than 1.5 pound-force to less than 4.5 pound-force, or greater than 1.5 pound-force to less than 4 pound-force, or greater than 1.5 pound-force to less than 3.5 pound-force, or greater than 1.5 pound-force to less than 3 pound-force.In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has an elongation at break of greater than 600% in both machine-direction and transverse-direction.

[0136] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure has a machine-direction stress at yield of from greater than 5 MPa and less than 10 MPa, or greater than 5 MPa and less than 9 MPa, or greater than 6 MPa and less than 9 MPa, or greater than 6 MPa and less than 8.5 MPa.

[0137] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure is characterized by at least one of the following features: a machine-direction elastic recovery of greater than 50%, as determined by ASTM D5459; a machine-direction holding force of greater than IO N, as determined by ASTM D5459; a machine-direction Trouser tear propagation resistance of greater than 0.5 poundforce, as determined by ASTM DI 938; a machine-direction Elmendorf tear resistance of greater than 300 g / mil, as determined by ASTM DI 922; and a machine-direction stress at yield of greater than 7 MPa as determined by ASTM D882.

[0138] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure is characterized by at least one of the following features: a machine-direction elastic recovery of greater than 50% and less than 90%, as determined by ASTM D5459; a machine-direction holding force of greater than 10N and less than 20 N, as determined by ASTM D5459; a machine-direction Trouser tear propagation resistance of greater than 0.5 pound-force and less than 4 pound-force, as determined by ASTM D1938; a machine-direction Elmendorf tear resistance of greater than 300 g / mil and less than 700 g / mil, as determined by ASTM DI 922; a machine-direction stress at yield of greater than 7 MPa and less than 10 MPa, as determined by ASTM D882; and a tensile energy at break of greater than 25 J / mm to less than 42 J / mm, as determined by ASTM D882.

[0139] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure is characterized by at least one of the following features: a machine-direction elastic recovery of greater than 50%, as determined by ASTM D5459; a machine-direction holding force of greater than 10 N, as determined by ASTM D5459; a machine-direction Trouser tear propagation resistance of greater than 0.75 poundforce, as determined by ASTM DI 938; a machine-direction Elmendorf tear resistance of greater than 300 g / mil, as determined by ASTM DI 922; and a machine-direction stress at yield of greater than 4 MPa as determined by ASTM D882.In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure is characterized by at least one of the following features: a machine-direction elastic recovery of greater than 50% and less than 90%, as determined by ASTM D5459; a machine-direction holding force of greater than ION and less than 20 N, as determined by ASTM D5459; a machine-direction Trouser tear propagation resistance of greater than 0.75 pound-force and less than 4 pound-force, as determined by ASTM D1938; a machine-direction Elmendorf tear resistance of greater than 300 g / mil and less than 700 g / mil, as determined by ASTM DI 922; and a machine-direction stress at yield of greater than 4 MPa and less than 10 MPa, as determined by ASTM D882.

[0140] In some embodiments, the multilayer film structure is a blown multilayer film structure, and the multilayer film structure is characterized by at least one of the following features: a machine-direction elastic recovery of greater than 50%, as determined by ASTM D5459; a machine-direction holding force of greater than 10 N, as determined by ASTM D5459; a machine-direction Trouser tear propagation resistance of greater than 1.5 poundforce, as determined by ASTM DI 938; a machine-direction Elmendorf tear resistance of greater than 350 g / mil, as determined by ASTM DI 922; and a machine-direction stress at yield of greater than 5 MPa as determined by ASTM D882.

[0141] In some embodiments, each of the first ethylene / a-olefin copolymer composition and the second ethylene / a-olefin copolymer composition has a single melting peak, as determined by differential scanning calorimetry. In these embodiments, the first ethylene / a-olefin copolymer composition has a temperature rising elution fractionation, TREF, profile comprising at least two peaks within a temperature range of from about 75°C to about 100°C. These embodiments include sub-embodiments where the multilayer film structure is a blown multilayer film structure, and the multilayer film structure is characterized by a tensile energy at break of greater than 25 J / mm to less than 42 J / mm, as determined by ASTM D882. The blown film sub-embodiments may further be characterized by at least one of the following features: a machine-direction elastic recovery of greater than 50% and less than 90%, as determined by ASTM D5459; a machine-direction holding force of greater than 10N and less than 20 N, as determined by ASTM D5459; a machine-direction Trouser tear propagation resistance of greater than 1.5 pound-force and less than 6 pound-force, as determined by ASTM DI 938; a machine-direction Elmendorf tear resistance of greater than 350 g / mil and less than 800 g / mil, as determined by ASTM DI 922; and a machine-direction stress at yield of greater than 5 MPa and less than 10 MPa, as determined by ASTM D882.EXAMPLES

[0142] General Testing Procedures

[0143] Prior to testing, each specimen was conditioned for at least 24 hours at 23±2°C and 50 ±10% relative humidity and subsequent testing was conducted at 23±2°C and 50 ±10% relative humidity. Herein, the term “ASTM conditions” refers to a laboratory that is maintained at 23±2°C and 50±10% relative humidity. ASTM refers to the American Society for Testing and Materials.

[0144] Polymer Density

[0145] Ethylene / a-olefin copolymer composition density in the solid state was determined using ASTM D792. Density measurements were performed on compression molded specimens molded at 165°C and at a cooling rate of 15 degrees per minute.

[0146] Polymer Melt Index

[0147] Ethylene / a-olefin copolymer composition melt index was determined using ASTM D1238. Melt indexes, I2, le and I21 were measured at 190°C, using a weights of 2160 g, 6480 g and 21600 g, respectively. In the present disclosure, the term “stress exponent” is defined by the following relationship: Stress Exponent = logio (L5 / I2) / logio (6480 / 2160); wherein E and I2 are the melt indexes measured at 190°C using 6480 g and 2160 g loads, respectively.

[0148] Conventional Gel Permeation Chromatography (GPC)

[0149] A polymer sample (about 15 mg) was weighed into the sample vial and loaded onto the auto-sampler of the Polymer Char GPC-IR5 unit. The vial was filled with 8 ml 1,2,4-tri chlorobenzene (TCB), heated to the desired dissolution temperature (e.g., 160°C) with a shaking for 120 minutes. The antioxidant 2,6-di-tert-butyl-4-methylphenol (BHT) was added to TCB in order to stabilize the polymer against oxidative degradation. The BHT concentration was 250 ppm. Sample solutions were chromatographed at 140°C on a Polymer Char GPC-IR5 chromatography unit equipped with four Shodex GPC columns (HT803, HT804, HT805 and HT806) using TCB as the mobile phase with a flow rate of 1.0 mL / minute, with an Infrared IR5 as the concentration detector. BHT was added to the mobile phase at a concentration of 250 ppm to protect GPC columns from oxidative degradation. The sample injection volume was 200 pL. The GPC columns were calibrated with narrow distribution polystyrene standards. The polystyrene molecular weights were converted to polyethylene molecular weights using the Mark-Houwink equation, as described in the ASTM standard test method D6474. The GPC raw data were processed with Excel spreadsheet, to produce molar mass averages (Mn, Mw, Mz) and molar mass distribution(e.g., poly dispersity, Mw / Mn). In the polyethylene art, a commonly used term that is equivalent to GPC is SEC, i.e., size exclusion chromatography.

[0150] Differential Scanning Calorimetry

[0151] Melting peak(s) (in °C) and heat of fusion (in J / g) within pre-defined temperature interval(s) were determined using differential scanning calorimetry (DSC) as follows: the instrument was first calibrated with indium; after the calibration, a polymer specimen is equilibrated at -50°C and then the temperature was increased to 200°C at a heating rate of 10°C / min; the melt was then kept isothermally at 200°C for five minutes; the melt was then cooled to -50°C at a cooling rate of 10°C / min and kept at -50°C for five minutes; the specimen was then heated to 200°C at a heating rate of 10°C / min. The DSC melting peaks(s) and heat of fusion within pre-defined temperature interval(s) were reported from the second heating cycle.

[0152] Comonomer Content: Fourier Transform Infrared (FTIR) Spectroscopy

[0153] The quantity of the a-olefinic comonomer in the disclosed ethylene / a-olefin copolymer compositions were determined by FTIR and reported as the weight percent of the a-olefinic comonomer. This test was completed according to ASTM D6645-01 (2001), employing a compression molded polymer plaque and a Thermo-Nicolet 750 Magna-IR Spectrophotometer. The polymer plaque was prepared using a compression molding device (Wabash-Genesis Series press) according to ASTM D4703-16 (April 2016).

[0154] Temperature Rising Elution Fractionation

[0155] The composition distribution branching of the disclosed ethylene / a-olefin copolymer compositions were assessed using a CRYSTAF / TREF 200+ unit equipped with an IR detector in the TREF mode. The acronym “TREF” refers to Temperature Rising Elution Fractionation. The TREF was supplied by Polymer Char S. A. (Valencia Technology Park, Gustave Eiffel, 8, Paterna, E-46980 Valencia, Spain). A polymer sample (80 to 100 mg) was placed into the reactor vessel of the TREF. The reactor vessel was filled with 35 ml of 1,2, 4-tri chlorobenzene (TCB) and the polymer was dissolved by heating the solution to 150°C for 2 hours. An aliquot (1.5 mL) of the solution was then loaded into the TREF column which was packed with stainless steel beads. The column, loaded with sample, was allowed to stabilize at 110°C for 45 minutes. The polymer was then crystallized from solution, within the column, by dropping the temperature to 30°C at a cooling rate of 0.09°C per minutes. The column was then equilibrated for 30 minutes at 30°C. The crystallized polymer was then eluted from the column with TCB flowing through the column at 0.75 mL / minute, while the column was slowly heated from 30°C to 120°C at a heating rate of 0.25°C / minute. The raw TREF datawere processed using Polymer Char software, an Excel spreadsheet and TREF software developed in-house.

[0156] Film Tensile

[0157] The following film tensile properties were determined using ASTM D882-12 (August 1, 2012): tensile strength at break (MPa), elongation at break (%), tensile stress at yield (MPa), tensile elongation at yield (%) and tensile energy to break (J / mm). Tensile properties were measured in both the machine direction (MD) and the transverse direction (TD) of the blown films.

[0158] Film Dart Impact

[0159] Film dart impact strength was determined using ASTM DI 709-09 Method A (May 1, 2009). In this disclosure the dart impact test employed a 1.5 inch (38 mm) diameter hemispherical headed dart.

[0160] Film Tear Resistance

[0161] Film tear resistance in grams per thickness of film in mils was determined by ASTM D1922-09 (May 1, 2009); an equivalent term for the tear resistance test is “Elmendorf tear”. Film tear resistance was measured in both the machine direction (MD) and the transverse direction (TD) of the films.

[0162] Film Tear Propagation Resistance

[0163] Film tear propagation resistance in pound-force was determined by ASTM D1938-19 (May 9, 2019); an equivalent term for the tear propagation resistance test is “Trouser tear” or “T-Tear”. Film tear propagation resistance was measured in both the machine direction (MD) and the transverse direction (TD) of the films.

[0164] Holding Force, Elastic Recovery, Permanent Deformation and Elasticity

[0165] Holding force, elastic recovery and permanent deformation were determined by ASTM D5459-95 (December 1, 2020). A specimen of dimensions 1 inch (width) x 13 inch (length) was cut out of film sample using punch press and a mold of appropriate dimensions for the determination of the elastic recovery, permanent deformation, holding force and elasticity in MD and TD directions on an Instron 4203 Universal Testing Instrument. The specimen was initially elongated to a pre-defined strain level of 30% at 1000 mm / min. The specimen was then held at this strain level for 15 seconds during which time stress relaxation was allowed. Subsequently, the crosshead was reversed to a lower strain level of 25% at the same speed as the initial elongation step. The specimen was then held for 5 minutes at the strain level of 25% to allow for the holding force to stabilize. The final holding force was recorded at the end of the 5-minute wait period. After recording the final holding force, thecrosshead was returned slowly, and the strain is recorded at the point at which the force is zero. Elastic recovery and permanent deformation were then calculated as described in the standard method specified in ASTMD5459-95 (December 1, 2020). In the present disclosure, elasticity of the specimen was determined by dividing the minimum stress observed during the reversal of the crosshead to a strain level of 25% by the maximum stress observed during the initial elongation of the specimen to a strain level of 30%.

[0166] The following ethylene / a-olefin copolymer composition and multilayer film structures are presented for the purpose of illustrating selected embodiments of this disclosure — it being understood that the examples presented do not limit the claims presented.

[0167] Ethylene / a-Olefin Copolymer Compositions

[0168] Ethylene / a-olefin copolymer compositions 1 A, IB and 2 were each made in a pilotscale “in-series” multi-reactor solution polymerization process where the ethylene / a-olefin copolymer composition was made by forming a first ethylene / a-olefin copolymer in a first reactor (Rl); and forming a second ethylene / a-olefin copolymer in a second reactor (R2); where Rl and R2 were configured in series with one another. Multi -reactor, solution phase polymerization process operated in series has been described in U.S. Pat. Appl. Pub. No.

[0169] 2019 / 0135958, U.S. Pat. Appl. Pub. No. 2018 / 0305531 and U.S. Pat. Appl. Pub. No.

[0170] 2021 / 0032450.

[0171] In an “in-series” reactor system the exit stream from a first polymerization reactor (Rl) flows directly into a second polymerization reactor (R2). Both Rl and R2 were continuously stirred reactors (CSTRs). The process was operated continuously by feeding fresh process solvent, ethylene, 1 -octene and hydrogen to the first and second reactors and in the removal of product. Methylpentane was used as the process solvent (a commercial blend of methylpentane isomers). Monomer (ethylene) and comonomer (1 -octene) were purified prior to addition to the reaction using conventional feed preparation systems (such as contact with various absorption media to remove impurities such as water, oxygen and polar contaminants). The reactor feeds were pumped to the reactors at the ratios shown in Table 1.

[0172] Table 1 shows the reactor conditions used to make each of the ethylene / a-olefin copolymer compositions in ethylene / a-olefin copolymer compositions 1 A, IB and 2. Table 1 includes process parameters, such as the ethylene and 1 -octene splits between the reactors (Rl and R2), the reactor temperatures, the ethylene conversions, the amounts of hydrogen, ethylene and 1 -octene concertation in the fresh feed to reactors, CSTR reactors (Rl and R2) agitation speeds, etc.In ethylene / a-olefin copolymer composition 1A, the following bridged metallocene catalyst components were used to prepare a first homogeneously-branched ethylene / a-olefin copolymer in the first CSTR reactor (Rl) and to prepare a second homogeneously-branched ethylene / a-olefin copolymer in the second CSTR reactor (R2): component A, diphenylmethylene(cyclopentadienyl)(2,7-di-t-butylfuorenyl)hafnium dimethide [(2,7-tBu2Flu)Ph2C(Cp)HfMe2] (abbreviated as CpF in Table 1); component M, methylaluminoxane (MMAO-07); component B, trityl tetrakis(pentafluoro-phenyl)borate (trityl borate); and component P, 2,6-di-tert-butyl-4-ethylphenol (BHEB). Methylaluminoxane (MMAO-07); and 2,6-di-tert-butyl-4-ethylphenol are premixed in-line and then combined with diphenylmethylene(cyclopentadienyl)(2,7-di-t-butylfuorenyl)hafnium dimethide and trityl tetrakis(pentafluoro-phenyl)borate just before entering the polymerization reactors (Rl and R2). The following catalyst component solvents were used: methylpentane for components M and P; and xylene for component A and B. The efficiency of the bridged metallocene catalyst formulation was optimized by adjusting the quantity of component A added to Rl and R2 [Rl catalyst (ppm) and R2 catalyst (ppm) as recited in Table 1] and the mole ratios of the catalyst components — i.e., [M] / [A], [P] / [M] and [B] / [A] — as tabulated in Table 1.

[0173] In ethylene / a-olefin copolymer composition IB, the following single site catalyst components were used to prepare a first homogeneously-branched ethylene / a-olefin copolymer in the first reactor (Rl): component A, diphenylmethylene(cyclopentadienyl)(2,7-di-t-butylfuorenyl)hafnium dimethide [(2,7-tBu2Flu)Ph2C(Cp)Hf e2] (abbreviated as CpF in Table 1); component M, methylaluminoxane (MMAO-07); component B, trityl tetrakis(pentafluoro-phenyl)borate (trityl borate); and component P, 2,6-di-tert-butyl-4-ethylphenol (BHEB). Methylaluminoxane (MMAO-07); and 2,6-di-tert-butyl-4-ethylphenol are premixed in-line and then combined with diphenylmethylene(cyclopentadienyl)(2,7-di-t-butylfuorenyl)hafnium dimethide and trityl tetrakis(pentafluoro-phenyl)borate just before entering the polymerization reactor (Rl). The following catalyst component solvents were used: methylpentane for components M and P; and xylene for component A and B. The efficiency of the single site catalyst formulation was optimized by adjusting the quantity of component A added to Rl [Rl catalyst (ppm) as recited in Table 1] and the mole ratios of the catalyst components — i.e., [M] / [A], [P] / [M] and [B] / [A] — as tabulated in Table 1.

[0174] In ethylene / a-olefin copolymer composition IB, an in-line Ziegler-Natta (ZN) catalyst formulation catalyst was used to prepare a second heterogeneously-branched ethylene / a-olefin copolymer in the second reactor (R2). The in-line Ziegler-Natta catalyst formulationhad the following components: butyl ethyl magnesium [component v]; tertiary butyl chloride [component vi]; titanium tetrachloride [component vii]; diethyl aluminum ethoxide [component viii]; and tri ethyl aluminum [component ix]. Methylpentane was used as the catalyst component solvent and the in-line Ziegler-Natta catalyst formulation was prepared using the following steps and then injected into the second reactor (R2). In step one, a solution of tri ethylaluminum and butyl ethyl magnesium (Mg: Al = 20, mol:mol) was combined with a solution of tertiary butyl chloride and allowed to react for about 30 seconds to produce a MgCh support. In step two, a solution of titanium tetrachloride was added to the mixture formed in step one and allowed to react for about 14 seconds prior to injection into second reactor (R2). The in-line Ziegler-Natta catalyst was activated in the reactor by injecting a solution of diethyl aluminum ethoxide into R2. The efficiency of the in-line Ziegler-Natta catalyst formulation was optimized by adjusting the quantity of titanium tetrachloride added to the reactor — recited as R2 catalyst (ppm) in Table 1 and the mole ratios of the catalyst components — i.e., [vi] / [v], [viii] / [vii] and [ix] / [vii] — as tabulated in Table 1.

[0175] In ethyl ene / a-olefin copolymer composition 2, the following unbridged single site catalyst components were used to prepare a first homogeneously-branched ethylene / a-olefin copolymer in the first CSTR reactor (Rl) and to prepare a second homogeneously-branched ethylene / a-olefin copolymer in the second CSTR reactor (R2): component A*, cyclopentadienyl tri(tertiary butyl)phosphinimine titanium (Cp[(t-Bu)3PN]TiC12] (abbreviated as PIC in Table 1); component M*, methylaluminoxane (MMAO-07); component B*, trityl tetrakis(pentafluoro-phenyl)borate (trityl borate); and component P*, 2,6-di-tert-butyl-4-ethylphenol (BHEB). Methylaluminoxane (MMAO-07); and 2,6-di-tert-butyl-4-ethylphenol are premixed in-line and then combined with cyclopentadienyl tri(tertiary butyl)phosphinimine titanium and trityl tetrakis(pentafluoro-phenyl)borate just before entering the polymerization reactors (Rl and R2). The following catalyst component solvents were used: methylpentane for components M* and P*; and xylene for component A* and B*. The efficiency of the unbridged single site catalyst formulation was optimized by adjusting the quantity of component A* added to Rl and R2 [Rl catalyst (ppm) and R2 catalyst (ppm) as recited in Table 1] and the mole ratios of the catalyst components — i.e., [M*] / [A*], [P*] / [M*] and [B*] / [A*] — as tabulated in Table 1.

[0176] In operating the continuous solution polymerization process shown in Table 1, the total amount of ethylene supplied to the process were portioned or split between the three reactors Rl and R2. In Table 1, this operational variable was called the ethylene split (ES),i.e., ESRland ESR2referred to the weight percent of ethylene injected in R1 and R2, respectively; with the proviso that E^1+ ESR2= 100%.

[0177] 1 -Octene was also added to the continuous solution polymerization process and was proportioned or split between R1 and R2. In Table 1, this operational variable was called the octene-1 split (OS), i.e., < 5R1and (AS'R2referred to the weight percent of octene-1 comonomer that was injected in R1 and R2, respectively; with the proviso that (AS'R I+ (AS'R2= 100%.

[0178] In operating the continuous solution polymerization process shown in Table 1, the total amount of ethylene converted in each reactor is monitored. The termRIreferred to the percent of the ethylene added to R1 that was converted into a first ethylene a / olefin copolymer by the catalyst formulation. Similarly,R2represented the percent of the ethylene added to R2 that was converted into the second ethylene a / olefin copolymer.

[0179] Polymerization in the continuous solution polymerization process was terminated by adding a catalyst deactivator to the third reactor exit stream. A multi-stage phase separation process was employed to recover the ethyl ene / a-olefin copolymer composition from the process solvent in which the third reactor exit stream was heated and passed through multiple V / L separators configured in series with one another. The polymer-rich stream exiting the last V / L separator, which contained from 94.5 to 96.5 weight percent of the ethylene / a-olefin copolymer composition, was fed to a twin-screw extruder for addition of additives and pelletization.

[0180] Ethylene / a-olefin copolymer composition 1A (EaOCC 1A) had a density of 0.905 g / cm3, a melt index I2 of 0.85 dg / min, a melt flow ratio I21 / I2 of 50, a stress exponent of 1.540, a second heating DSC thermogram with a single melting peak at 98°C, and a heat of fusion above 105°C (= 103*0.905-800) of 7.9 J / g. Ethylene / a-olefin copolymer composition 1 Awas an ethylene / 1 -octene copolymer composition and contained 17 wt.% of 1 -octene as determined by FTIR.

[0181] Ethylene / a-olefin copolymer composition IB (EaOCC IB) had a density of 0.908 g / cm3, a melt index I2 of 0.85 dg / min, a melt flow ratio I21 / I2 of 30, a stress exponent of 1.365, a second heating DSC thermogram with three melting peaks at 91, 119 and 122°C, and a heat of fusion above 108°C (= 103*0.908-800) of 33.3 J / g. Ethylene / a-olefin copolymer composition IB had a Mw / Mnof 3.2 and Mz / Mwof 2.3. Ethylene / a-olefin copolymer composition IB was an ethylene / 1 -octene copolymer composition and contained 15 wt.% of 1 -octene as determined by FTIR.

[0182] Ethylene / a-olefin copolymer composition 2 (EaOCC 2) had a density of 0.916 g / cm3, a melt index I2 of 0.65 dg / min, a melt flow ratio I21 / I2 of 28, a stress exponent of 1.260, asecond heating DSC thermogram with a single peak at 111°C, and a heat of fusion above 116°C (= 103x0.916-800) of 4.1 J / g. Despite having a single melting peak, as determined by the DSC method, ethylene / a-olefin copolymer composition 2 was observed to have two TREF peaks at 81°C and 96°C. Ethylene / a-olefin copolymer composition 2 had a Mw / Mnof 3.3 and Mz / Mwof2.4.

[0183] Table 1 : Continuous Solution Polymerization Process Parameters for Ethylene / a-Olefin Copolymer Compositions (EaOCCs) 1 A, IB and 2,

[0184] 1A IB 2

[0185] R1 Ethylene Split, ESR1(wt.%) 38.0 45.0 49.9

[0186] R2 Ethylene Split, ESR2(wt.%) 62.0 55.0 50.0

[0187] R1 1 -Octene Split, OSR1(wt.%) 39.0 31.0 90.0

[0188] R2 1 -Octene Split, OSR2(wt.%) 61.0 69.0 10.0

[0189] R1 Ethylene Concentration (wt.%) 9.9 11.7 10.4

[0190] R2 Ethylene Concentration (wt.%) 12.9 14.7 12.9

[0191] R1 Hydrogen (ppm) 3.8 4.1 0.7

[0192] R2 Hydrogen (ppm) 5.0 2.6 0.8

[0193] R1 Catalyst Concentration (ppm) 0.5* 0.7* 0.1* R1 Catalyst CpFt CpFt PICJR1 ([M] / [A]) mole ratio 50 25 —

[0194] R1 ([P] / [M]) mole ratio 0.4 0.2 —

[0195] R1 ([B] / [A]) mole ratio 1.2 1.36 —

[0196] R1 ([M*] / [A*]) mole ratio — — 100

[0197] R1 ([P*] / [M*]) mole ratio — — 0.3

[0198] R1 ([B*] / [A*]) mole ratio — — 1.2

[0199] R2 Catalyst Concentration (ppm) 0.8* 5.3 ** 0.3*

[0200] R2 Catalyst CpF1' in-line ZN PICJR2 ([M] / [A]) mole ratio 50 — —

[0201] R2 ([P] / [M]) mole ratio 0.4 — —

[0202] R2 ([B] / [A]) mole ratio 1.2 — —

[0203] R2 ([M*] / [A*]) mole ratio — — 25

[0204] R2 ([P*] / [M*]) mole ratio — — 0.3

[0205] R2 ([B*] / [A*]) mole ratio — — 1.27

[0206] R2 ([vi] / [v]) mole ratio — 2.05 —

[0207] R2 ([viii] / [vii]) mole ratio — 1.51 —

[0208] R2 ([ix] / [vii]) mole ratio — 0.37 —

[0209] R1 Inlet Temperature (°C) 30.0 24.0 24.1

[0210] R2 Inlet Temperature (°C) 30.0 25.0 20.1 Overall 1-Octene / Ethylene (w / w) 0.3 0.7 0.8

[0211]

[0212] 1 -Octene Purity (wt.%) 71.2 70.0 67.7R1 Agitator (rpm) 236.1 236.0 235.9

[0213] R2 Agitator (rpm) 169.2 169.2 169.2

[0214] QR1(%) 76.9 77.3 77.2

[0215] QR2(%) 85.9 85.8 88.2

[0216] R1 Mean Temperature (°C) 142.7 158.2 137.9

[0217]

[0218] R2 Mean Temperature (°C) 190.4 203.4 186.1

[0219] * Concentration of component A or A*;

[0220] ** Concentration of component vii; and

[0221] t (2,7-tBu2Flu)Ph2C(Cp)HfMe2.

[0222] tCp[(t-Bu)3PN]TiCl2

[0223] Multilayer Film Structures

[0224] Three-layer coextruded blown films were fabricated using a Brampton 3-layer blown film line. This line was equipped with three extruders such that A / B / C coextruded film structures in which A, B and C represent distinct thermoplastic layers can be produced. Layer A was a sealant layer. Layer B was a sublayer sandwiched between the sealant layer A and a skin layer C. All three extruders had a consistent barrel diameter (D) of 1.75 inch (4.45 cm) and barrel length (L) with an extruder barrel length to diameter ratio of 30 (L / D). The 3-layer blown film die was a pancake design and the exit lip diameter was 4 inch (10.2 cm). A Saturn I air ring was used to quench the extrudate. The following operating conditions were used to generate three layer blown film samples: Blow-up-ratio (BUR) of 2.5:1; 4 inch (10.2 cm) die; 50 mil (0.127 cm) die gap; and frost line height was 18 inch (45.72 cm). The temperature set points and the actual melt temperatures at the die exit on the 3-layer blown film line are shown in Tables 2a to 2f.

[0225] In these structures, EaOCC 1 A was the ethylene / a-olefin copolymer composition 1 A; EaOCC IB was the ethylene / a-olefin copolymer composition IB; EaOCC 2 was the ethylene / a-olefin copolymer composition 2; EaOCC 3 was an ethylene / 1 -octene copolymer composition commercially available from NOVA Chemicals Corporation under the trade name SURPASS® VPsK914 with a nominal melt index I2 of 0.85 dg / min and a nominal density of 0.913 g / cm3; EaOCC 4 was an ethylene / 1 -octene copolymer composition commercially available from NOVA Chemicals Corporation under the trade name SURPASS® SPsll6 with a nominal melt index I2 of 1.0 dg / min and a nominal density of 0.916 g / cm3; and EaOCC 5 was an ethylene / 1 -octene copolymer composition commercially available from NOVA Chemicals Corporation under the trade name SURPASS® SPsK919 with a nominal melt index I2 of 0.85 dg / min and a nominal density of 0.919 g / cm3. EaOCC 3 had a second heating DSC thermogram with three melting peaks at 98°C, 119°C and 122°C, and a heat of fusion above 113°C (= 1000x0.913 - 800) of 30 J / g. EaOCC 4 had a second heating DSC thermogram with two melting peaks at 120°C and 122°C, and a heat of fusionabove 116°C (= 1000x0.916 - 800) of 33 J / g. EaOCC 5 had a second heating DSC thermogram with three melting peaks at 105°C, 118°C and 121°C, and a heat of fusion above 119°C (= 1000x0.919 - 800) of 15 J / g.

[0226] In Tables 2a to 2f, the first skin layer and the second skin layer each included a polymer process aid (PPA) masterbatch (MB). The PPA MB was a 5 wt.% masterbatch of 3M™ DYNAMAR™ FX5920A in a LLDPE (melt index h of 1 dg / min and density of 0.920 g / cm3) carrier resin. Both the first and second skin layers further included a 4: 1 mixture of an antiblocking additive (AB) masterbatch (MB) and a Slip masterbatch (MB). The AB MB was a 25 wt.% masterbatch of Diatomaceous Earth in an LLDPE carrier resin having a final density of 1.086 g / cm3. The Slip MB was a 5 wt.% Erucamide in LLDPE with a final density of 0.923 g / m3.

[0227] Table 2a: Blown Film Coextrusion Process Conditions.

[0228] Structure 1 Structure 2 Structure 3 Structure Thickness (mil) 4.5 4.5 4.5 Coextruded Structure A / B / C A / B / C A / B / C First Skin Layer (A) 94.0 wt.% EaOCC 2 94.0 wt.% EaOCC 2 94.0 wt.% EaOCC 2

[0229] + 3.5 wt.% PPA MB + 3.5 wt.% PPA MB + 3.5 wt.% PPA MB + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip MBs MBs MBs First Skin Layer Thickness % 35% (1.58 mil) 25% (1.12 mil) 20% (0.90 mil) Inner Layer (B) 100 wt.% EaOCC 1A 100 wt.% EaOCC 1A 100 wt.% EaOCC 1A Inner Layer Thickness % 30% (1.35 mil) 50% (2.25 mil) 60% (2.70 mil) Second Skin Layer (C) 93.5 wt.% EaOCC 2 93.5 wt.% EaOCC 2 93.5 wt.% EaOCC 2

[0230] + 4.0 wt.% PPA MB + 4.0 wt.% PPA MB + 4.0 wt.% PPA MB + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip MBs MBs MBs Second Skin Layer % 35% (1.57 mil) 25% (1.12 mil) 20% (0.90 mil) Feed Throat Temperature 65 / 65 / 65 65 / 65 / 65 65 / 65 / 65 (Setpoint)* (°F)

[0231] Barrel Zone 1 - Setpoint* (°F) 370 / 370 / 370 370 / 370 / 370 370 / 370 / 370 Barrel Zone 2 - Setpoint* (°F) 390 / 390 / 390 390 / 390 / 390 390 / 390 / 390 Barrel Zone 3 - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Barrel Zone 4 - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Screen - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Adaptor - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Die Module - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Melt Temperature - Actual* (°F) 439 / 408 / 428 424 / 416 / 417 416 / 418 / 414 Output Rate* (Ib / h) 26.4 / 22.3 / 26.3 18.9 / 37.3 / 18.9 15.1 / 44.8 / 15.1 Extruder RPM* 45.7 / 23.8 / .49.2 34.7 / 34.6 / 34.7 28.6 / 40.6 / 31.1 Barrel Pressure* (psig) 4883 / 2664 / 4841 4284 / 3151 / 3901 3756 / 3247 / 3461 Line Speed (feet per minute) 22.2 22.4 22.5

[0232] 15.76 15.71 15.64

[0233]

[0234] Layflat - Actual (inch)

[0235] * Values are listed in order of extruder A / extruder B / extruder C.Table 2b: Blown Film Coextrusion Process Conditions.

[0236] Structure 4 Structure 5 Structure 6 Structure Thickness (mil) 4.5 4.5 4.5 Coextruded Structure A / B / C A / B / C A / B / C First Skin Layer (A) 94.0 wt.% EaOCC 2 94.0 wt.% EaOCC 2 94.0 wt.% EaOCC 2

[0237] + 3.5 wt.% PPA MB + 3.5 wt.% PPA MB + 3.5 wt.% PPA MB + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip MBs MBs MBs First Skin Layer Thickness % 15% (0.68 mil) 35% (1.57 mil) 25% (1.13 mil) Inner Layer (B) 100 wt.% EaOCC 1A 100 wt.% EaOCC IB 100 wt.% EaOCC IB Inner Layer Thickness % 70% (3.17 mil) 30% (1.35 mil) 50% (2.27 mil) Second Skin Layer (C) 92.2 wt.% EaOCC 2 93.5 wt.% EaOCC 2 93.5 wt.% EaOCC 2

[0238] + 4.2 wt.% PPA MB + 4.0 wt.% PPA MB + 4.0 wt.% PPA MB + 3.6 wt.% AB / Slip + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip MBs MBs MBs Second Skin Layer % 15% (0.68 mil) 35% (1.57 mil) 25% (1.13 mil) Feed Throat Temperature 65 / 65 / 65 65 / 65 / 65 65 / 65 / 65 (Setpoint)* (°F)

[0239] Barrel Zone 1 - Setpoint* (°F) 370 / 370 / 370 370 / 370 / 370 370 / 370 / 370 Barrel Zone 2 - Setpoint* (°F) 390 / 390 / 390 390 / 390 / 390 390 / 390 / 390 Barrel Zone 3 - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Barrel Zone 4 - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Screen - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Adaptor - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Die Module - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Melt Temperature - Actual* (°F) 410 / 420 / 409 443 / 412 / 431 428 / 418 / 421 Output Rate* (Ib / h) 11.3 / 52.2 / 11.3 26.4 / 22.5 / 26.5 18.9 / 37.5 / 18.9 Extruder RPM* 22.5 / 47.2 / 24.8 45.5 / 21.9 / 45.4 32.6 / 33.1 / 34.7 Barrel Pressure* (psig) 3294 / 3437 / 3015 4957 / 2934 / 4787 4037 / 3526 / 3885 Line Speed (feet per minute) 22.5 22.5 22.4 Layflat - Actual (inch) 15.60 15.74 15.63

[0240]

[0241] * Values are listed in order of extruder A / extruder B / extruder C.

[0242] Table 2c: Blown Film Coextrusion Process Conditions.

[0243] Structure 7 Structure 8 Structure 9 Structure Thickness (mil) 4.5 4.5 4.5 Coextruded Structure A / B / C A / B / C A / B / C First Skin Layer (A) 94.0 wt.% EaOCC 2 94.0 wt.% EaOCC 2 94.5 wt.% EaOCC 3

[0244] + 3.5 wt.% PPA MB + 3.5 wt.% PPA MB + 3.0 wt.% PPA MB + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip MBs MBs MBs First Skin Layer Thickness % 20% (0.90 mil) 15% (0.68 mil) 35% (1.58 mil) Inner Layer (B) 100 wt.% EaOCC IB 100 wt.% EaOCC IB 100 wt.% EaOCC 1A Inner Layer Thickness % 60% (2.71 mil) 70% (3.17 mil) 30% (1.35 mil) Second Skin Layer (C) 93.5 wt.% EaOCC 2 93.1 wt.% EaOCC 2 93.5 wt.% EaOCC 3

[0245] + 4.0 wt.% PPA MB + 4.2 wt.% PPA MB + 4.0 wt.% PPA MB + 2.5 wt.% AB / Slip + 2.7 wt.% AB / Slip + 2.5 wt.% AB / Slip MBs MBs MBs Second Skin Layer % 20% (0.90 mil) 15% (0.68 mil) 35% (1.58 mil)

[0246]

[0247] Feed Throat Temperature 65 / 65 / 65 65 / 65 / 65 65 / 65 / 65 (Setpoint)* (°F)

[0248] Barrel Zone 1 - Setpoint* (°F) 370 / 370 / 370 370 / 370 / 370 370 / 370 / 370 Barrel Zone 2 - Setpoint* (°F) 390 / 390 / 390 390 / 390 / 390 390 / 390 / 390 Barrel Zone 3 - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Barrel Zone 4 - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Screen - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Adaptor - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Die Module - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Melt Temperature - Actual* (°F) 418 / 422 / 414 411 / 424 / 409 440 / 408 / 430 Output Rate* (Ib / h) 15.1 / 44.9 / 15.1 11.4 / 52.5 / 11.4 26.3 / 22.3 / 26.3 Extruder RPM* 28.0 / 37.3 / 28.6 21.3 / 43.2 / 21.5 44.1 / 19.9 / 43.7 Barrel Pressure* (psig) 3749 / 3619 / 3516 3262 / 3812 / 2871 4624 / 2552 / 4501 Line Speed (feet per minute) 22.5 22.5 22.3

[0249] 15.59 15.56 15.67

[0250]

[0251] Layflat (inch)

[0252] * Values are listed in order of extruder A / extruder B / extruder C.

[0253] Table 2d: Blown Film Coextrusion Process Conditions.

[0254] Structure 10 Structure 11 Structure 12 Structure Thickness (mil) 4.5 4.5 4.5 Coextruded Structure A / B / C A / B / C A / B / C First Skin Layer (A) 94.5 wt.% EaOCC 3 94.0 wt.% EaOCC 3 94.0 wt.% EaOCC 3

[0255] + 3.0 wt.% PPA MB + 3.5 wt.% PPA MB + 3.5 wt.% PPA MB + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip MBs MBs MBs First Skin Layer Thickness % 20% (0.91 mil) 35% (1.56 mil) 20% (0.91 mil) Inner Layer (B) 100 wt.% EaOCC 1A 100 wt.% EaOCC IB 100 wt.% EaOCC IB Inner Layer Thickness % 60% (2.72 mil) 30% (1.34 mil) 60% (2.72 mil) Second Skin Layer (C) 93.5 wt.% EaOCC 3 93.5 wt.% EaOCC 3 93.5 wt.% EaOCC 3

[0256] + 4.0 wt.% PPA MB + 4.0 wt.% PPA MB + 4.0 wt.% PPA MB + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip MBs MBs MBs Second Skin Layer % 20% (0.91 mil) 35% (1.56 mil) 20% (0.91 mil) Feed Throat Temperature 65 / 65 / 65 65 / 65 / 65 65 / 65 / 65 (Setpoint)* (°F)

[0257] Barrel Zone 1 - Setpoint* (°F) 370 / 370 / 370 370 / 370 / 370 370 / 370 / 370 Barrel Zone 2 - Setpoint* (°F) 390 / 390 / 390 390 / 390 / 390 390 / 390 / 390 Barrel Zone 3 - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Barrel Zone 4 - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Screen - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Adaptor - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Die Module - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Melt Temperature - Actual* (°F) 418 / 417 / 414 439 / 408 / 433 419 / 421 / 416 Output Rate* (Ib / h) 15.1 / 44.9 / 15.1 26.4 / 22.5 / 26.4 15.1 / 45.0 / 15.1 Extruder RPM* 25.3 / 38.3 / 25.0 43.1 / 19.4 / 43.8 24.4 / 38.4 / 24.0 Barrel Pressure* (psig) 3676 / 3206 / 3532 4701 / 2905 / 4883 3695 / 3876 / 3593 Line Speed (feet per minute) 22.6 22.6 22.5

[0258] 15.55 15.74 15.69

[0259]

[0260] Layflat (inch)

[0261] * Values are listed in order of extruder A / extruder B / extruder C.Table 2e: Blown Film Coextrusion Process Conditions.

[0262] Structure 13 Structure 14 Structure 15 Structure Thickness (mil) 4.5 4.5 4.5 Coextruded Structure A / B / C A / B / C A / B / C First Skin Layer (A) 94.0 wt.% EaOCC 4 94.0 wt.% EaOCC 4 93.9 wt.% EaOCC 5

[0263] + 3.5 wt.% PPA MB + 3.5 wt.% PPA MB + 3.6 wt.% PPA MB + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip + 2.5 wt.% AB / Slip MBs MBs MBs First Skin Layer Thickness % 20% (0.89 mil) 20% (0.90 mil) 20% (0.90 mil) Inner Layer (B) 100 wt.% EaOCC 1A 100 wt.% EaOCC IB 100 wt.% EaOCC 1A Inner Layer Thickness % 60% (2.67 mil) 60% (2.69 mil) 60% (2.71 mil) Second Skin Layer (C) 93.5 wt.% EaOCC 4 93.4 wt.% EaOCC 4 93.2 wt.% EaOCC 5

[0264] + 4.0 wt.% PPA MB + 4.0 wt.% PPA MB + 4.0 wt.% PPA MB + 2.5 wt.% AB / Slip + 2.6 wt.% AB / Slip + 2.8 wt.% AB / Slip MBs MBs MBs Second Skin Layer % 20% (0.89 mil) 20% (0.90 mil) 20% (0.90 mil) Feed Throat Temperature 65 / 65 / 65 65 / 65 / 65 65 / 65 / 65 (Setpoint)* (°F)

[0265] Barrel Zone 1 - Setpoint* (°F) 370 / 370 / 370 370 / 370 / 370 370 / 370 / 370 Barrel Zone 2 - Setpoint* (°F) 390 / 390 / 390 390 / 390 / 390 390 / 390 / 390 Barrel Zone 3 - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Barrel Zone 4 - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Screen - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Adaptor - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Die Module - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Melt Temperature - Actual* (°F) 412 / 416 / 409 414 / 421 / 410 413 / 416 / 412 Output Rate* (Ib / h) 15.1 / 44.8 / 15.1 15.1 / 44.9 / 15.1 15.1 / 44.6 / 15.1 Extruder RPM* 25.2 / 38.3 / 24.9 25.3 / 35.7 / 25.8 25.2 / 38.9 / 27.0 Barrel Pressure* (psig) 2900 / 2988 / 2899 2951 / 3417 / 2874 3153 / 3113 / 3102 Line Speed (feet per minute) 22.4 22.4 22.4

[0266] 15.91 15.77 15.58

[0267]

[0268] Layflat (inch)

[0269] * Values are listed in order of extruder A / extruder B / extruder C.

[0270] Table 2f: Blown Film Coextrusion Process Conditions.

[0271] Structure 16 Structure 17 Structure 18 Structure Thickness (mil) 4.5 4.5 4.5 Coextruded Structure A / B / C A / B / C A / B / C First Skin Layer (A) 94.0 wt.% EaOCC 5 94.0 wt.% EaOCC 94.0 wt.% EaOCC + 3.5 wt.% PPA MB 1A + 3.5 wt.% PPA IB +3.5 wt.% PPA + 2.5 wt.% AB / Slip MB + 2.5 wt.% MB +2.5 wt.% MBs AB / Slip MBs AB / Slip MBs First Skin Layer Thickness % 20% (0.89 mil) 20% (0.90 mil) 20% (0.90 mil) Inner Layer (B) 100 wt.% EaOCC 100 wt.% EaOCC 100 wt.% EaOCC IB 1A IB Inner Layer Thickness % 60% (2.67 mil) 60% (2.71 mil) 60% (2.69 mil) Second Skin Layer (C) 93.5 wt.% EaOCC 5 93.5 wt.% EaOCC 93.5 wt.% EaOCC + 4.0 wt.% PPA MB 1A + 4.0 wt.% PPA IB +4.0 wt.% PPA + 2.5 wt.% AB / Slip MB + 2.5 wt.% MB +2.5 wt.%

[0272]

[0273] MBs AB / Slip MBs AB / Slip MBsSecond Skin Layer % 20% (0.89 mil) 20% (0.90 mil) 20% (0.90 mil) Feed Throat Temperature 65 / 65 / 65 65 / 65 / 65 65 / 65 / 65 (Setpoint)* (°F)

[0274] Barrel Zone 1 - Setpoint* (°F) 370 / 370 / 370 370 / 370 / 370 370 / 370 / 370 Barrel Zone 2 - Setpoint* (°F) 390 / 390 / 390 390 / 390 / 390 390 / 390 / 390 Barrel Zone 3 - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Barrel Zone 4 - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Screen - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Adaptor - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Die Module - Setpoint* (°F) 400 / 400 / 400 400 / 400 / 400 400 / 400 / 400 Melt Temperature - Actual* (°F) 412 / 421 / 411 409 / 416 / 409 414 / 423 / 410 Output Rate* (Ib / h) 15.1 / 44.8 / 15.1 15.0 / 44.8 / 15.0 15.0 / 45.0 / 15.0 Extruder RPM* 24.6 / 36.9 / 26.0 22.2 / 37.4 / 23.0 21.0 / 38.6 / 23.1 Barrel Pressure* (psig) 3102 / 3507 / 3066 2852 / 2873 / 2710 3080 / 3520 / 2980 Line Speed (feet per minute) 22.5 22.4 22.5

[0275] 15.78 15.64 15.69

[0276]

[0277] Layflat - Actual (inch)

[0278] * Values are listed in order of extruder A / extruder B / extruder C.

[0279] Tables 3a, 3b and 3c summarize the physical properties of the Structures 1 to 18. With reference to Tables 3a-c, Structures 11, 12, 14 and 16 had an improved energy at break when compared to Structures 9, 10, 13 and 15. Structures 11, 12, 14 and 16 included EaOCC IB in the inner layer which had a melting peak at

[0280]

[0281] 122°C > Ta(pl) = 108°C. EaOCC IB was further characterized by a melting peak at 91 °C < Ta(pl) = 108°C, and a heat of fusion of 33.3 J / g above Ta(plStructures 11, 12, 14 and 16 included EaOCC 3, EaOCC 4 and EaOCC 5 in both skins layers. The ethyl ene / a-olefin copolymer compositions in EaOCC 3, EaOCC 4 and EaOCC 5 had at least one melting peak above 7 (2). The ethylene / a-olefin copolymer compositions in EaOCC 3, EaOCC 4 and EaOCC 5 further had a heat of fusion above / ( / >2) of greater than 10 J / g and less than 40 J / g.

[0282] With reference to Tables 3a-c, Structures 1 to 4 had an improved energy at break when compared to Structures 5 to 8. Structures 1 to 4 included EaOCC 1A in the inner layer and EaOCC 2 in the skin layers. Noticeably, the ethylene / a-olefin copolymer compositions in EaOCC 1A and EaOCC 2 both exhibited a single melting peak in a second heating thermogram.Table 3a: Physical Properties of the Multilayer Film Structures 1-6,

[0283] Structure Structure Structure Structure Structure Structure 1 2 3 4 5 6 MD Thickness Avg (mil) 4.57 4.53 4.63 4.50 4.57 4.33 MD Thickness SD (mil) 0.15 0.12 0.12 0.10 0.06 0.15 MD Max Force Avg (N) 24.65 22.68 22.28 20.01 26.7 23.58 MD Max Force SD (N) 0.69 0.1 0.86 0.73 0.12 0.58 MD Holding Force Avg (N) 14.82 14.17 14.21 13.05 15.23 13.78 MD Holding Force SD (N) 0.35 0.14 0.42 0.40 0.05 0.33 MD Elasticity Avg ( — ) 0.60 0.62 0.64 0.65 0.57 0.58 MD Elasticity (SD) Avg ( — ) 0.00 0.00 0.01 0.00 0.00 0.00 MD Elastic Recovery Avg (%) 74.36 77.83 79.1 80.09 66.6 66.66 MD Elastic Recovery SD (%) 0.11 0.48 0.59 0.32 0.2 0.29 MD Permanent Deformation 25.64 22.17 20.9 19.91 33.4 33.34 Avg (%)

[0284] MD Permanent Deformation 0.11 0.48 0.59 0.32 0.2 0.29 SD (%)

[0285] TD Thickness Avg (mil) 4.6 4.57 4.7 4.43 4.5 4.53 TD Thickness SD (mil) 0.1 0.06 0.17 0.06 0.17 0.06 TD Max Force Avg (N) 24.58 22.95 22.28 20.41 25.18 24.06 TD Max Force SD (N) 0.19 0.33 0.47 0.71 0.47 0.21 TD Holding Force Avg (N) 14.95 14.37 14.31 13.29 14.53 14.04 TD Holding Force SD (N) 0.14 0.17 0.23 0.43 0.26 0.2 TD Elasticity Avg ( — ) 0.61 0.63 0.64 0.65 0.58 0.58 TD Elasticity (SD) ( — ) 0.00 0.00 0.00 0.00 0.00 0.00 TD Elastic Recovery Avg (%) 74.54 77.14 79.32 80.48 67.57 67.84 TD Elastic Recovery SD (%) 0.47 0.25 0.06 0.19 0.27 0.96 TD Permanent Deformation 25.46 22.86 20.68 19.52 32.43 32.16 Avg (%)

[0286] TD Permanent Deformation 0.47 0.25 0.06 0.19 0.27 0.96 SD (%)

[0287] Dart (g / mil) 434 474 634 635 373 445 MD Tear* Resistance (g / mil) 506 439 405 359 375 361 TD Tear* Resistance (g / mil) 566 527 490 521 491 448 TD Elongation at Break (%) 850 811 798 800 857 844 MD Elongation at Break (%) 824 770 791 767 812 837 Tensile Energy to Break (J / mm) 35.4 31.4 34 33.2 25.1 24.9 MD Stress at Yield 7.4 6.5 5.8 6.7 8.1 8 MD Tear* * Propagation (Ibf) 1.93 1.79 1.83 1.73 0.683 0.612

[0288]

[0289] TD Tear* * Propagation (Ibf) 2.08 1.94 2.04 1.84 0.707 0.708 * Elmendorf tear; and

[0290] ** Trouser tear.Table 3b: Physical Properties of the Multilayer Film Structures 7-12,

[0291] Structure Structure Structure Structure Structure Structure 7 8 9 10 11 12 MD Thickness Avg (mil) 4.33 4.17 4.5 4.57 4.5 4.63 MD Thickness SD (mil) 0.15 0.06 0.1 0.06 0.1 0.15 MD Max Force Avg (N) 23.18 21.87 23.41 20.97 23.75 23.65 MD Max Force SD (N) 0.13 0.74 0.29 0.40 0.83 0.43 MD Holding Force Avg (N) 13.47 12.84 13.77 13.1 13.31 13.5 MD Holding Force SD (N) 0.02 0.35 0.11 0.37 0.50 0.35 MD Elasticity Avg ( — ) 0.58 0.59 0.59 0.62 0.56 0.57 MD Elasticity (SD) Avg ( — ) 0 0 0 0.01 0 0 MD Elastic Recovery Avg (%) 66.44 68.26 68.88 76.62 61.72 64.19 MD Elastic Recovery SD (%) 0.65 0.58 0.19 0.99 1.1 1.14 MD Permanent Deformation 33.56 31.74 31.12 23.38 38.28 35.81 Avg (%)

[0292] MD Permanent Deformation 0.65 0.58 0.19 0.99 1.1 1.14 SD (%)

[0293] TD Thickness Avg (mil) 4.33 4.17 4.67 4.63 4.60 4.60 TD Thickness SD (mil) 0.15 0.06 0.06 0.06 0.10 0.00 TD Max Force Avg (N) 22.83 20.77 23.12 21.08 23.6 23.08 TD Max Force SD (N) 0.49 0.84 0.15 0.21 0.19 0.86 TD Holding Force Avg (N) 13.3 12.31 13.75 13.23 13.18 13.21 TD Holding Force SD (N) 0.31 0.47 0.09 0.18 0.11 0.44 TD Elasticity Avg ( — ) 0.58 0.59 0.59 0.63 0.56 0.57 TD Elasticity (SD) ( — ) 0.00 0.00 0.00 0.00 0.00 0.00 TD Elastic Recovery Avg (%) 68.21 68.42 71.3 77.61 63.79 67.04 TD Elastic Recovery SD (%) 0.57 1.48 0.89 0.32 1.57 0.45 TD Permanent Deformation 31.79 31.58 28.7 22.39 36.21 32.96 Avg (%)

[0294] TD Permanent Deformation 0.57 1.48 0.89 0.32 1.57 0.45 SD (%)

[0295] Dart (g / mil) 567 660 682 697 697 697 MD Tear* Resistance (g / mil) 359 331 493 479 432 385 TD Tear* Resistance (g / mil) 409 425 623 523 496 480 TD Elongation at Break (%) 795 796 902 878 889 882 MD Elongation at Break (%) 806 769 893 895 891 866 Tensile Energy to Break (J / mm) 29 30.6 24.2 27.2 27.5 31.2 MD Stress at Yield 7.8 7.5 7.6 6.8 7.7 7.5 MD Tear* * Propagation (Ibf) 0.557 0.523 0.63 0.61 0.593 0.587 TD Tear* * Propagation (Ibf) 0.652 0.600 0.653 0.705 0.641 0.651

[0296]

[0297] * Elmendorf tear; and

[0298] ** Trouser tear.Table 3c: Physical Properties of the Multilayer Film Structures 13-18,

[0299] Structure Structure Structure Structure Structure Structure 13 14 15 16 17 18 MD Thickness Avg (mil) 4.47 4.43 4.53 4.50 4.50 4.50 MD Thickness SD (mil) 0.15 0.21 0.06 0.00 0.00 0.00 MD Max Force Avg (N) 21.31 24.08 22.78 24.7 17.85 21.74 MD Max Force SD (N) 0.45 0.48 0.14 0.19 0.26 0.67 MD Holding Force Avg (N) 12.91 13.44 13.52 13.61 12.05 12.72 MD Holding Force SD (N) 0.23 0.28 0.22 0.15 0.1 0.35 MD Elasticity Avg ( — ) 0.61 0.56 0.59 0.55 0.68 0.59 MD Elasticity (SD) Avg ( — ) 0 0 0.01 0 0 0 MD Elastic Recovery Avg (%) 73.13 61.07 71.86 59.78 83.24 67.27 MD Elastic Recovery SD (%) 0.23 0.3 1.22 1.04 0.11 0.82 MD Permanent Deformation 26.87 38.93 28.14 40.22 16.76 32.73 Avg (%)

[0300] MD Permanent Deformation 0.23 0.3 1.22 1.04 0.11 0.82 SD (%)

[0301] TD Thickness Avg (mil) 4.43 4.4 4.47 4.4 4.5 4.5 TD Thickness SD (mil) 0.15 0.12 0.06 0.17 0 0 TD Max Force Avg (N) 20.78 23.1 21.29 23.84 17.62 20.82 TD Max Force SD (N) 0.77 0.5 0.62 0.67 0.19 0.38 TD Holding Force Avg (N) 12.64 12.8 12.69 13.25 11.96 12.2 TD Holding Force SD (N) 0.58 0.29 0.5 0.32 0.14 0.2 TD Elasticity Avg ( — ) 0.61 0.55 0.6 0.56 0.68 0.59 TD Elasticity (SD) ( — ) 0.01 0 0.01 0 0 0 TD Elastic Recovery Avg (%) 73.62 61.91 72.21 62.61 83.42 67.87 TD Elastic Recovery SD (%) 1.73 0.94 1.42 0.66 0.21 0.38 TD Permanent Deformation 26.38 38.09 27.79 37.39 16.58 32.13 Avg (%)

[0302] TD Permanent Deformation 1.73 0.94 1.42 0.66 0.21 0.38 SD (%)

[0303] Dart (g / mil) 435 682 433 462 3318 3318 MD Tear* Resistance (g / mil) 367 354 387 342 310 318 TD Tear* Resistance (g / mil) 448 476 508 442 390 445 TD Elongation at Break (%) 893 862 881 846 854 796 MD Elongation at Break (%) 829 812 857 802 816 808 Tensile Energy to Break 26.4 29.4 25.5 29.7 29.2 35.9 (J / mm)

[0304] MD Stress at Yield 6.5 7.1 7 7.6 5.1 6.2 MD Tear* * Propagation (Ibf) 0.581 0.607 0.585 0.549 0.59 0.556

[0305]

[0306] TD Tear* * Propagation (Ibf) 0.765 0.702 0.752 0.676 0.926 0.641 * Elmendorf tear; and

[0307] ** Trouser tear.

[0308] INDUSTRIAL APPLICABILITY

[0309] The present disclosure provides multilayer film structures suitable for stretch hood processes.

Claims

CLAIMS1. A multilayer film structure, comprising:an inner layer, the inner layer comprising a first ethylene / a-olefin copolymer composition, wherein the first ethylene / a-olefin copolymer composition comprises about 55 weight percent of ethylene or greater than 55 weight percent of ethylene, and wherein the first ethylene / a-olefin copolymer composition has:a density,1, of from about 0.880 g / cm3to about 0.913 g / cm3, as determined in accordance with ASTM D792;a melt index I21of from about 0.1 dg / min to about 2 dg / min, as determined in accordance with ASTM D1238 at 190°C and at a loading 2.16 kg; andat least one melting peak, as determined by differential scanning calorimetry, at a temperature greater than a first density-adjusted temperature, Ta(plthe first density-adjusted temperature being defined according to Ta(pl) = 103xpl- 800; and a first skin layer and a second skin layer, the first skin layer and the second skin layer each independently comprising a second ethylene / a-olefin copolymer composition, the second ethylene / a-olefin copolymer composition having a melt index, I22, of from about 0.1 dg / min to about 2 dg / min, as determined in accordance with ASTM D1238 at 190°C and at a loading 2.16 kg, and a density, p2, of from about 0.910 g / cm3to about 0.935 g / cm3, as determined in accordance with ASTM D792.

2. The multilayer film structure of claim 1, wherein the inner layer is a core layer.

3. The multilayer film structure of claim 1 or 2, wherein the first ethylene / a-olefin copolymer composition and the second ethylene / a-olefin copolymer composition each independently comprise one or more than one C4 to C10 a-olefin.

4. The multilayer film structure of claim 1 or 2, wherein the first ethylene / a-olefin copolymer composition and the second ethylene / a-olefin copolymer composition each independently comprise one or more than one a-olefin selected from the group consisting of octene, hexene and mixtures thereof.

5. The multilayer film structure of any one of claims 1-4, wherein the density of second ethylene / a-olefin copolymer composition, p1, is greater than the density of the first ethylene / a-olefin copolymer composition, pl.

6. The multilayer film structure of any one of claims 1-5, wherein the first ethylene / a-olefin copolymer composition further has a heat of fusion, as determined by differentialscanning calorimetry, of greater than about 10 J / g and less than about 35 J / g above the first density-adjusted temperature, a(p').

7. The multilayer film structure of any one of claims 1-6, wherein the first ethylene / a-olefin copolymer composition has at least one melting peak, as determined by differential scanning calorimetry, at a temperature less than the first density-adjusted temperature, Ta(pl).

8. The multilayer film structure of any one of claims 1-7, wherein the first ethylene / a-olefin copolymer composition is an in-situ blend comprising a first homogeneously-branched ethylene / a-olefin copolymer and a first heterogeneously-branched ethylene / a-olefin copolymer.

9. The multilayer film structure of any one of claims 1-8, wherein the first ethylene / a-olefin copolymer composition has a poly dispersity index, Mw / Mnof from about 2.5 to 5, as determined by conventional gel permeation chromatography.

10. The multilayer film structure of any one of claims 1-9, wherein the first ethylene / a-olefin copolymer composition has a ratio of z-average molecular weight to weight-average molecular weight, Mz / Mwof from about 2 to 4, as determined by conventional gel permeation chromatography.

11. The multilayer film structure of any one of claims 1-10, wherein the density of the first ethylene / a-olefin copolymer composition, p has a value ranging from greater than or equal to 0.895 g / cm3to less than or equal to 0.910 g / cm3, as determined in accordance with ASTM D792.

12. The multilayer film structure of any one of claims 1-11, wherein the second ethylene / a-olefin copolymer composition has at least one melting peak, as determined by differential scanning calorimetry, at a temperature greater than a second density-adjusted temperature, a(p2), the second density-adjusted temperature being defined according to Ta(p2) = 103x2- 800.

13. The multilayer film structure of claim 12, wherein the second ethylene / a-olefin copolymer composition has at least one melting peak, as determined by differential scanning calorimetry, at a temperature less than the second density-adjusted temperature, 7k( / z2).

14. The multilayer film structure of claim 12 or 13, wherein the second ethylene / a-olefin copolymer composition further has a heat of fusion, as determined by differential scanning calorimetry, of greater than about 10 J / g and less than about 45 J / g above the second density-adjusted temperature, 7 (2).

15. The multilayer film structure of any one of claims 1-14, wherein the multilayer film structure is a blown multilayer film structure, and wherein the multilayer film structure is characterized by at least one of the following features:a machine-direction elastic recovery of greater than 50%, as determined by ASTMD5459;a machine-direction holding force of greater than 10 N, as determined by ASTMD5459;a machine-direction Trouser tear propagation resistance of greater than 0.5 poundforce, as determined by ASTM D1938;a machine-direction Elmendorf tear resistance of greater than 300 g / mil, as determined by ASTM DI 922; anda machine-direction stress at yield of greater than 7 MPa as determined by ASTMD882.

16. The multilayer film structure of any one of claims 1-15, wherein at least one of the first skin layer and the second skin layer is in adhering contact with the inner layer.

17. The multilayer film structure of any one of claims 1-16, wherein a ratio of the first skin layer thickness to the inner layer thickness and a ratio of the second skin layer thickness to the inner layer thickness are independently greater than 1:1.

18. The multilayer film structure of any one of claims 1-17, wherein a ratio of the inner layer thickness to an overall thickness of the multilayer film structure is less than 1 :2.

19. The multilayer film structure of any one of claims 1-18, wherein the inner layer is an all-polyethylene film layer.

20. The multilayer film structure of any one of claims 1-19, wherein the multilayer film structure is an all-polyethylene structure.

21. A multilayer film structure, comprising:an inner layer, the inner layer comprising a first ethylene / a-olefin copolymer composition, wherein the first ethylene / a-olefin copolymer composition comprises about 55 weight percent of ethylene or greater than 55 weight percent of ethylene, and wherein the first ethylene / a-olefin copolymer composition has:a density,1, of from about 0.880 g / cm3to about 0.913 g / cm3, as determined in accordance with ASTM D792; anda melt index I21of from about 0.1 dg / min to about 2 dg / min, as determined in accordance with ASTM D1238 at 190°C at a loading 2.16 kg; anda first skin layer and a second skin layer, the first skin layer and the second skin layer each independently comprising a second ethylene / a-olefin copolymer composition, wherein the second ethylene / a-olefin copolymer composition has:a melt index, I22, of from about 0.1 dg / min to about 2 dg / min, as determined in accordance with ASTM D1238 at 190°C at a loading 2.16 kg;a density,2, of from about 0.910 g / cm3to about 0.935 g / cm3, as determined in accordance with ASTM D792;a single melting peak, as determined by differential scanning calorimetry; and a temperature rising elution fractionation, TREF, profile comprising at least two peaks within a temperature range of from about 75°C to about 100°C.

22. The multilayer film structure of claim 21, wherein the inner layer is a core layer.

23. The multilayer film structure of claim 21 or 22, wherein the first ethylene / a-olefin copolymer composition and the second ethylene / a-olefin copolymer composition each independently comprise one or more than one C4 to C10 a-olefin.

24. The multilayer film structure of claim 21 or 22, wherein the first ethylene / a-olefin copolymer composition and the second ethylene / a-olefin copolymer composition each independently comprise one or more than one a-olefin selected from the group consisting of octene, hexene and mixtures thereof.

25. The multilayer film structure of any one of claims 21-24, wherein the second ethylene / a-olefin copolymer composition has a poly dispersity index, Mw / Mnof from about 3 to 6, as determined by conventional gel permeation chromatography.

26. The multilayer film structure of any one of claims 21-25, wherein the second ethylene / a-olefin copolymer composition has a ratio of z-average molecular weight to weightaverage molecular weight, Mz / Mwof from about 2 to 4, as determined by conventional gel permeation chromatography.

27. The multilayer film structure of any one of claims 21-26, wherein the density of the second ethylene / a-olefin copolymer composition,2, has a value ranging from greater than or equal to 0.913 g / cm3to less than or equal to 0.925 g / cm3, as determined in accordance with ASTM D792.

28. The multilayer film structure of any one of claims 21-27, wherein the single melting peak of the second ethylene / a-olefin copolymer composition occurs at a temperature less than a second density-adjusted temperature, 7 (p2), the second density-adjusted temperature being defined according to Taip2) = IO3* / )2- 800.

29. The multilayer film structure of any one of claims 21-28, wherein the multilayer film structure is a blown multilayer film structure, and wherein the multilayer film structure is characterized by at least one of the following features:a machine-direction elastic recovery of greater than 50%, as determined by ASTMD5459;a machine-direction holding force of greater than 10 N, as determined by ASTMD5459;a machine-direction Trouser tear propagation resistance of greater than 0.75 poundforce, as determined by ASTM D1938;a machine-direction Elmendorf tear resistance of greater than 300 g / mil, as determined by ASTM DI 922; anda machine-direction stress at yield of greater than 4 MPa as determined by ASTMD882.

30. The multilayer film structure of any one of claims 21-28, wherein the first ethylene / a-olefin copolymer composition has a single melting peak, as determined by differential scanning calorimetry.

31. The multilayer film structure of claim 30, wherein the multilayer film structure is a blown multilayer film structure, and wherein the multilayer film structure is characterized by at least one of the following features:a machine-direction elastic recovery of greater than 50%, as determined by ASTMD5459;a machine-direction holding force of greater than 10 N, as determined by ASTMD5459;a machine-direction Trouser tear propagation resistance of greater than 1.5 poundforce, as determined by ASTM D1938;a machine-direction Elmendorf tear resistance of greater than 350 g / mil, as determined by ASTM DI 922; anda machine-direction stress at yield of greater than 5 MPa as determined by ASTMD882.

32. The multilayer film structure of any one of claims 21-31, wherein at least one of the first skin layer and the second skin layer is in adhering contact with the inner layer.

33. The multilayer film structure of any one of claims 21-32, wherein a ratio of the first skin layer thickness to the inner layer thickness and a ratio of the second skin layer thickness to the inner layer thickness are independently greater than 1:1.

34. The multilayer film structure of any one of claims 21-33, wherein a ratio of the inner layer thickness to an overall thickness of the multilayer film structure is less than 1:2.

35. The multilayer film structure of any one of claims 21-34, wherein the inner layer is an all-polyethylene film layer.

36. The multilayer film structure of any one of claims 21-36, wherein the multilayer film structure is an all-polyethylene structure.