Finishing layer for a decorative covering element and a decorative covering element

By optimizing the print layer with specific pigments and a base ink layer, and using calcium-zinc stabilizers and UV absorbers, the finishing layers achieve improved whiteness, realism, and consistent color perception, addressing the issues of dullness, blurriness, and yellowing in decorative elements.

WO2026234542A1PCT designated stage Publication Date: 2026-11-12UNILIN BVBA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2026/054383
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-10-22
Filing Date
2026-05-04
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Finishing layers of decorative covering elements often appear dull, blurry, and exhibit a yellow shine, especially with high-contrast features, and are influenced by lighting conditions and observer angles, particularly when using PVC layers that degrade over time.

Method used

Incorporating a print layer with specific amounts of titanium dioxide or alternative white pigments, a base ink layer, and optimizing the wear and lacquer layers to enhance whiteness, contrast, and resistance to yellowing, while using calcium-zinc stabilizers and UV absorbers to maintain color stability and reduce angle-dependent perception.

Benefits of technology

The solution improves the whiteness, realism, and sharpness of decorative elements, reduces yellowing, and ensures consistent color perception regardless of lighting conditions and angles, providing enhanced durability and aesthetic appeal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2026054383_12112026_PF_FP_ABST
    Figure IB2026054383_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a finishing layer (6) for a decorative covering element (1) comprising a print layer (7), wherein the print layer (7) comprises at least synthetic material and pigments (12), wherein said synthetic material is preferably thermoplastic material, characterized in that said pigments (12) are titanium dioxide particles or white pigments other than titanium dioxide particles, wherein the print layer (12) comprises said pigments in an amount of at least 5 phr, preferably at least 7.5 phr, more preferably at least 10 phr, even more preferably at least 12.5 phr. The invention further also relates to alternative finishing layers (6) for a decorative covering element (1) as well as a decorative covering element (1).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Finishing layer for a decorative covering element and a decorative covering element.

[0002] The present invention relates to finishing layers for decorative covering elements as well as to such decorative covering elements.

[0003] Finishing layers of current decorative covering elements typically comprise a print layer with possibly a wear layer placed above the print layer. In the case where it is desired to provide the decorative covering element with a decorative appearance or a decor, one or more decorative ink layers may be provided between the print layer and the wear layer. Optionally, a lacquer layer may be arranged on top of the wear layer for increased scratch and wear resistance. Decorative covering elements typically comprise a substrate below a said finishing layer.

[0004] The inventors found that a finishing layer of the prior art, in particular a decor of such a finishing layer, is often not perceived as intended, for example it may appear dull and / or blurry. This is especially the case where it is desired to incorporate high-contrast features such as for example decorative patterns on a white background. Furthermore, finishing layers of the prior art tend to produce a yellow shine, which may alter the perception of the finishing layer as well as the realism of the decor if present. This is especially the case when the print layer and / or wear layer of the finishing layer is a PVC layer, in particular a PVC plastisol layer, which over the course of time tends to degrade and turn yellow.

[0005] Another factor that may affect how a finishing layer, in particular its decor if present, is perceived are the lighting conditions, for example light coming from a lightbulb in the case of indoor lighting or from the sun in the case of outdoor lighting may alter how the finishing layer and its possible decor may be perceived. The specific lighting conditions may be further altered by the relative positioning between the light source, the decorative covering element, and the observer. For example, a person standing up will perceive a decor of a decorative covering element differently when it is on a wall or on a floor because of the difference in the angle of observation. It is desired that the perception ofthe finishing layer and / or the decor is substantially independent from the lighting conditions.

[0006] According to a first object, the present invention provides alternative finishing layers to the finishing layers of the prior art, which according to preferred embodiments may overcome one or more of the shortcomings of finishing layers of the prior art. According to a second object, the present invention also provides an alternative decorative covering element to the decorative covering elements of the prior art, which according to preferred embodiments may overcome one or more of the shortcomings of decorative covering elements of the prior art.

[0007] According to its first independent aspect, the present invention is a finishing layer for a decorative covering element comprising a print layer, wherein the print layer comprises at least synthetic material and pigments, wherein the synthetic material is preferably thermoplastic material, with the characteristic that said pigments are titanium dioxide particles or white pigments other than titanium dioxide particles, wherein the print layer comprises said pigments in an amount of at least 5 phr, preferably at least 7.5 phr, more preferably at least 10 phr, even more preferably at least 12.5 phr. To their surprise, the inventors have found that these amounts of said pigments in the print layer improve the whiteness of the finishing layer, even when additional layers, such as a wear layer and / or lacquer layer, are placed above the finishing layer. Furthermore, significant improvements in the realism of a decor comprising one or more colors above the print layer may be obtained, and the high level of whiteness of the print layer may increase the perceived contrast of these one or more colors, and may even increase the apparent sharpness of the decor. This may be of particular interest in the case of stone decors or fantasy decors, where it may be desired to have an intense white color. Especially in the case where more than 7.5 phr of said pigments is used, good results may be obtained. The inventors have obtained very good results when using 15 phr of said pigments. In a preferred embodiment, said pigments are present in an amount of at most 50 phr, preferably at most 40 phr, more preferably at most 30 phr, most preferably at most 25 phr or at most 20 phr. This ensures that the print layer has an excellent whiteness, while limiting the cost of production.Such white pigments other than titanium dioxide may for example be zinc oxide, calcium carbonate, barium sulphate and / or lithopone. It is noted that, in the case that said pigments comprise a combination of different types of titanium dioxide and / or white pigments other than titanium dioxide, the amount referred to above preferably relates to the total combined amount of all these pigments. In a preferred embodiment, the print layer is free or essentially free from white pigments other than titanium dioxide particles. This may provide a better control and reduce the variability on the obtained or obtainable whiteness of the print layer. It may also reduce the complexity of the formulation. This may further facilitate stock keeping.

[0008] In a preferred embodiment, the titanium dioxide particles and / or white pigments other than titanium dioxide particles have a relative tinting strength of at least 60, preferably at least 75, more preferably at least 85. Preferably, the relative tinting strength is at least 95, more preferably at least 100. This may improve the intensity of the print layer’s whiteness. Preferably, the titanium dioxide particles and / or white pigments other than titanium dioxide particles have a brightness L* of at least 85, more preferably at least 90, even more preferably at least 95 or at least 98. This may increase the brightness of the white color, making the whiteness more intense. Preferably, the titanium dioxide particles and / or white pigments other than titanium dioxide particles have a tone b* of at most 4, preferably at most 3, even more preferably at most 2, most preferably at most 1. This reduces the yellowness of the pigment, such that a more neutral whiteness may be obtained. The relative tinting strength, the brightness L* and the tone b* may be determined according to the norm DIN 53775, preferably using a spectrophotometer.

[0009] Preferably, the print layer is arranged to receive a possible base ink layer, one or more possible decorative ink layers, a possible wear layer and / or a possible lacquer layer on its top side. The side of the print layer opposite to its top side is the bottom side of the print layer. In the context of the present invention, “above” means that a certain element has a position which has a higher coordinate on a reference axis running through the print layer, preferably orthogonal to the print layer, from the bottom side of the print layer tothe top side of the print layer, “below” means that a certain element has a position which has a lower coordinate on said reference axis.

[0010] According to a preferred embodiment, the synthetic material of the print layer is or comprises flexible synthetic material. Preferably, the synthetic material is or comprises PVC, preferably flexible PVC. PVC means polyvinyl chloride in the present invention. The print layer may be obtained by curing of a plastisol. Said plastisol is preferably applied in an amount between 50 and 600 g / m2, preferably between 150 and 450 g / m2, more preferably between 200 and 400 g / m2, for example 290 g / m2. The print layer may be foamed or unfoamed, however is preferably unfoamed.

[0011] Throughout this application, PVC preferably has a K-value between 50 and 90.

[0012] In the context of the present invention, a flexible synthetic material, such as flexible PVC, means a synthetic material that comprises 40 or more than 40 phr plasticizers. Semi-rigid or semi-flexible synthetic materials, for example semi-rigid or semi-flexible PVC, means a synthetic material that comprises between 10 and 40 phr plasticizers, whereas rigid synthetic material, such as rigid PVC, comprises less than or exactly 10 phr plasticizer. Throughout this application, the notation “phr” means “parts per hundred parts of resin” wherein the resin is the amount of said synthetic material. For example, in the case where the synthetic material is PVC, “phr” is counted per 100 parts of PVC.

[0013] Generally, in the context of the present invention, plasticizers are inter alia esters of carboxylic acids (for example esters of phthalic acid, iso- or terephthalic acid, trimellitic acid and adipic acid), for example diisononyl phthalate (DINP), dioctyl terephthalate (DOTP), diisononyl-l,2-cyclohexanedicarboxylate (DINCH), esters of phosphoric acid, for example triaryl or trialkaryl phosphates, for example tricresyl phosphate, chlorinated or unchlorinated hydrocarbons, ethers, polyesters, polyglycols, sulfonamides, or combinations thereof.

[0014] In a preferred embodiment, the synthetic material comprises fillers, preferably in an amount above 10 wt%, more preferably above 40 wt%. The amount of fillers ispreferably at most 90 wt%, more preferably at most 80 wt%. These weight percentages are expressed with respect to the total weight of the print layer. In a preferred embodiment, the synthetic material comprises fillers in an amount of at least 50 phr, preferably at least 75 phr, more preferably at least 90 phr. The inventors have obtained an excellent balance between cost and mechanical performance for an amount of filler of 95 phr. Preferably, said fillers comprise inorganic fillers such as talcum, calcium carbonate, lime and / or chalk. A preferred filler is calcium carbonate.

[0015] Preferably, the print layer is cellulose-free. In a preferred embodiment, the print layer is cellulose-free and comprises flexible or semi-rigid thermoplastic material, for example flexible or semi-rigid PVC, and fillers, for example calcium carbonate.

[0016] The print layer preferably has a thickness of at least 0.05 mm, preferably at least 0.15 mm, more preferably at least 0.2 mm. In a preferred embodiment, the print layer has a thickness of 0.18 mm. In other preferred embodiments, the print layer may have a thickness of between 0.09 and 0.6 mm, for example between 0.4 and 0.6 mm. With these thicknesses of the print layer, the print layer may be opaque or essentially opaque, and an excellent whiteness may thus be obtained. This provides an excellent print layer on which further layers, for example decorative ink layers, may be applied.

[0017] Preferably, the print layer comprises one or more components selected from the list of phosphite, barium-zinc stabilizer, calcium-zinc stabilizer and epoxidized soybean oil. These components may provide an improved thermal stability to the print layer, such that, even during high-temperature steps of the production, the stability of the whiteness of the print layer may be guaranteed. Preferably, the print layer comprises phosphite, barium-zinc stabilizer, calcium-zinc stabilizer and / or epoxidized soybean oil, wherein each is present in an amount between 0 and 5 phr, preferably between 0 and 3 phr.

[0018] The finishing layer preferably comprises one or more decorative ink layers above the print layer. Thanks to the enhanced whiteness of the print layer, the decorative ink layers may come more to the foreground and may appear more realistic. Furthermore, the enhanced whiteness of the print layer may increase the sharpness of the decor formed bythe decorative ink layers, possibly in combination with the print layer. Furthermore, thanks to the consistency of the whiteness of the print layer, there may be less variation in the obtained decor and the perception of the decor may be better predictable.

[0019] According to its second independent aspect, the invention is a finishing layer for a decorative covering element comprising a print layer, with the characteristic that the finishing layer further comprises a base ink layer above, preferably directly above, the print layer, wherein the base ink layer is a layer of ink, preferably a layer of blue ink. To their surprise, the inventors found that the application of said base ink layer may enhance the realism of the colors of further layers, for example decorative ink layers, in the finishing layer. They have found that, by including said base ink layer, especially when said base ink layer is a layer of blue ink, that the yellowing of the print layer and / or possibly a wear layer may be effectively counterbalanced, such that said yellowing may not be perceived with the naked eye. The inventors believe that, in this case, this is a result of the fact that blue and yellow act as complementary colors that cancel each other out when viewed in combination.

[0020] It is noted that “blue” in the context of this application is not intended to be interpreted as limiting, but blue may equally encompass blue-like colors such as for example azure, cyan, teal, turquoise, periwinkle, navy, cerulean, indigo, violet.

[0021] According to a particular embodiment, said base ink layer is a layer of ink with a color different from blue, for example brown or green. This may be of particular interest when it is desired to obtain specific decors. For instance, if a wood decor is desired, it may be beneficial to apply said base ink layer in the form of a layer of brown ink, which may lead to ink savings. Furthermore, it is conceivable that a material of the finishing layer over time turns towards an aging color different from yellow, such that it may be beneficial to apply said base ink layer with a color that is the complementary color of this aging color.

[0022] It is remarked that, according to the second independent aspect of the invention, the base ink layer is applied above the print layer and below possible decorative ink layers, wearlayers and / or lacquer layers. Further, it is preferred that the base ink layer is applied directly onto the print layer, however, it is not excluded that one or more preparatory layers are applied in between, for example for improved adherence of the base ink layer.

[0023] According to a first embodiment, the print layer comprises one or more colored pigments, preferably at least blue or cyan pigments. According to a second embodiment, the finishing layer further comprises one or more wear layers above the print layer, wherein at least one, and preferably each, of said one or more wear layers comprises one or more colored pigments, preferably at least blue or cyan pigments. It is remarked that, according to a variant of the second independent aspect, which may be in accordance with this first and / or second embodiment, the finishing layer may be free from a said base ink layer. Preferred embodiments of the second independent aspect are equally applicable for this variant as far as this does not lead to contradictions, and the same benefits may be obtained.

[0024] Preferred embodiments and their benefits for the finishing layer of the first independent aspect of the invention may equally be applied to the finishing layer of the second independent aspect of the invention. It is noted that, herein, it is preferred that the print layer comprises pigments in an amount as described in relation to the first independent aspect, however, that this is not strictly necessary.

[0025] A particularly preferred embodiment is where the base ink layer, in particular in the form of a layer of blue ink, is arranged above, preferably directly above, the print layer of the first independent aspect. The inventors found that the layer of blue ink strengthens the apparent whiteness of the print layer, providing an even better contrast for further ink layers. Additionally, the increased apparent whiteness improves the finishing layer’s resistance to apparent yellowing of one or more of its layers. Said apparent yellowing is important, especially in the case of PVC layers, in particular PVC plastisol layers. This problem of apparent yellowing is greatly reduced thanks to this particularly preferred embodiment. Furthermore, the increased apparent whitness thanks to the layer of blue ink may reduce the required amount of titanium dioxide or white pigment other thantitanium dioxide in the print layer while maintaining equal or similar levels of whiteness, which may thus provide cost savings.

[0026] In a preferred embodiment, the base ink layer covers at least 25%, preferably at least 50%, more preferably at least 75%, most preferably at least 95%, of the entire surface area of the print layer. The base ink layer may be an all-over layer, covering the entire surface area or essentially the entire surface area of the print layer. This has the benefit that its application may be less complex and that it may be applied independently of any desired decor that may be applied later. According to another preferred embodiment, the base ink layer is applied in one or more predetermined areas on the print layer, wherein preferably said predetermined areas are in register with the decor that may be applied. This may result in cost savings. It is remarked that said base ink layer may be a uniform layer or a collection of dots that may provide the impression of being a uniform layer. Said collection of dots may be the result of analogue printing, for example rotogravure printing, or of digital printing, for example digital inkjet printing. Preferably, in the case where the base ink layer is a collection of dots that provide the impression of being a uniform layer, said collection of dots is present in an amount of at least 300 dpi, preferably at least 600 dpi or at least 1000 or 1500 dpi. This may make the base ink layer appear more like a uniform layer.

[0027] Preferably, the base ink layer is applied by analog printing, preferably by rotogravure printing, however, the base ink layer may likewise be applied by digital printing, for example by digital inkjet printing. Especially in the case where the base ink layer is an all-over layer, or covers at least 50% of the surface area of the print layer, it is preferred that the base ink layer is applied by means of analog printing. This may result in significant cost savings.

[0028] The base ink layer preferably comprises a water-based ink. This has the benefit that only a limited amount of harmful substances, such as volatile organic compounds, may be released by the base ink layer, providing a more safe working environment. It is remarked that, if the base ink layer comprises more than one ink, that each of these inks may be a water-based ink.Preferably, the base ink layer is or comprises a pigmented ink. Said pigmented ink preferably comprises one or more pigments selected from C.I. Pigment Blue 15:1, C.I. Pigment Blue 15:3, C.I. Pigment Blue 15:4, C.I. Pigment Blue 29, C.I. Pigment Blue 60, C.I. Pigment Violet 19, C.I. Pigment Violet 23, C.I. Pigment Violet 32, C.I. Pigment Red 122. Suitable inks are commercially available on the market. According to a preferred embodiment, the pigmented ink comprises the pigments C.I. Pigment Blue 15:3 and C.I. Pigment Red 122. The inventors found that such a base ink layer provides very good results, even when the pigmented ink of the base ink layer comprises a mixture of blue and red pigments. In a preferred embodiment, said pigmented ink comprises pigments in an amount between 0.1 and 50 wt%, preferably between 1 and 40 wt%, more preferably between 5 and 20 wt%. The inventors obtained excellent results with these values, especially when the pigmented ink comprises a mixture of blue and red pigments. Preferably, said pigmented ink further comprises binder in an amount between 50 and 99.9 wt%, more preferably between 60 and 99 wt%, most preferably between 80 and 95 wt%. Weight percentages in relation to the base ink layer are preferably based on dry weight.

[0029] In a preferred embodiment, the base ink layer comprises a mixture of a pigmented ink and a non-pigmented ink. This pigmented ink is preferably a pigmented ink as already described earlier. In this case, the base ink layer preferably comprises said pigmented ink in an amount of at most 2 wt%, more preferably at most 1 wt%, even more preferably at most 0.5 wt%, most preferably at most 0.1 wt%, for example 0.05 wt%. Preferably, said non-pigmented ink represents at least 98 wt%, more preferably at least 99 wt%, even more preferably at least 99.5 wt%, most preferably at least 99.9 wt%, for example 99.95 wt%, of the base ink layer. Such low amount of pigmented ink may ensure that the base ink layer remains almost completely transparent, while adding a subtle hint of color, for example blue, to the decor and / or the print layer. The inventors observed that a mixture of blue and red pigments in the pigmented ink provides excellent results, especially when the pigmented ink is present in an amount of at most 2 wt% in the base ink layer. The inventors have found that, when the print layer comprises titanium dioxide particles and / or white pigments other than titanium dioxide particles, such as in the firstindependent aspect of the invention, that the whiteness of the print layer is enhanced by the base ink layer being a layer of blue ink comprising said amounts of pigmented ink. For clarity, it is noted that a mixture of a pigmented ink and a non -pigmented ink, in the context of the invention, is considered to be a pigmented ink.

[0030] The base ink layer may have a thickness between 1 and 50 micrometers, preferably between 2 and 20 micrometer, more preferably between 5 and 10 micrometers. The base ink layer may be applied in an amount between 1 and 50 g / m2, preferably between 2 and 20 g / m2, more preferably between 5 and 10 g / m2.

[0031] According to a particularly preferred embodiment, the finishing layer is a finishing layer in accordance with the first independent aspect, wherein the finishing layer comprises a layer of blue ink directly above the print layer, wherein the layer of blue ink comprises at most 0.05 wt% of a pigmented ink comprising C.I. Pigment Blue 15:3 and C.I. Pigment Red 122 in an amount between 5 and 20 wt%. The inventors obtained excellent results in terms of whiteness and resistance against apparent yellowing, even when further layers such as decorative ink layers, wear layers and / or lacquer layers, are applied.

[0032] The ink - or inks - of the base ink layer preferably comprises an acrylate-based binder. This may provide excellent adhesion properties, a high flexibility, and high print quality. Especially in the case where the finishing layer and / or the decorative covering element is intended to be wound up or woundable on a roll, said high flexibility is of interest. Said ink - or inks - of the base ink layer may further also comprise a PVC latex, which may beneficially improve adherence to PVC-based or PVC-containing layers, for instance to a PVC print layer and / or to a PVC wear layer.

[0033] In a preferred embodiment, the finishing layer comprises one or more decorative ink layers above said base ink layer. It is clear that, in the context of this application, the decor may be formed by the print layer and / or the base ink layer and / or the decorative ink layers, possibly even in combination with one or more wear layers.In preferred embodiments according to the first independent aspect and the second independent aspect, the finishing layer preferably comprises a wear layer arranged above the print layer, above the possible base ink layer and above the possible one or more decorative ink layers, wherein the wear layer has a thickness of at least 0.15 mm, preferably of at least 0.4 mm, more preferably of at least 0.5 mm. Preferably, the wear layer has a thickness between 0.15 mm and 1.0 mm, for example between 0.2 mm and 0.55 mm.

[0034] The wear layer preferably comprises fillers in an amount of less than 50 wt%, preferably less than 30 wt%, more preferably less than 15 wt%. According to a particularly preferred embodiment, the wear layer is free from fillers. Preferably, the wear layer is translucent or transparent such that any decorative features formed below the wear layer remain visible. The wear layer preferably comprises flexible or semi-rigid thermoplastic material, preferably flexible or semi-rigid PVC.

[0035] In a preferred embodiment, the wear layer comprises epoxidized soybean oil. The wear layer may instead or in combination therewith comprise one or more of phosphites, calcium-zinc stabilizers and barium-zinc stabilizers. This may improve the thermal stability of the wear layer, such that the wear layer does not or to a lesser degree become yellow during its production, for example because of high temperatures in an oven or during lamination. The wear layer then preferably comprises epoxidized soybean oil, phosphites, calcium-zinc stabilizers and / or barium-zinc stabilizers in an amount between 0 and 10 phr each, preferably between 0 and 5 phr each, more preferably between 0 and 3.5 phr each.

[0036] The wear layer preferably comprises one or more UV absorbers and / or one or more radical scavengers. UV absorbers absorb UV radiation such that the material of the wear layer, for example the flexible or semi-rigid PVC, does not degrade. Examples of UV absorbers may be benzotriazole, benzophenone and high performance triazine. Radical scavengers on the other hand react with free radicals to neutralize them, such that they may prevent degradation of the wear layer. Examples of radical scavengers may include antioxidants and / or hindered amine light stabilizers (HALS) - such as derivatives oftetramethylpiperdine. Examples of antioxidants may be phenolic antioxidants, in particular primary phenolic antioxidants, thioesters, in particular secundary thioesters, and / or phosphites, in particular secundary phosphites. Examples of HALS may be derivatives of tetramethylpiperdine - such as Tinuvin 123 available from the company BASF -, imadizolidinone-based HALS and / or azetidinone-based HALS. UV absorbers and radical scavengers may be beneficial since they protect the wear layer, as well as the underlying layers such as the print layer, the possible one or more decorative ink layers, and the possible base ink layer, from UV radiation, such that the risk of their colors changing over time is limited. Their presence may thus further reduce the risk of yellowing and / or improve the realism of the colors by avoiding color fading, safeguarding the aesthetical qualities of the finishing layer. Said UV absorbers and / or radical scavengers are preferably present in the wear layer in an amount of between 0 and 10 phr each, preferably between 0 and 5 phr each, more preferably between 0 and 3 phr each. In particular, hindered amine light stabilizers are preferably present in an amount of between 0 and 5 wt%, preferably between 0.5 and 2 wt%.

[0037] It is noted that the presence of a calcium-zinc stabilizer in the wear layer in itself also forms an inventive concept. Therefore, according to its third independent aspect, the invention is a finishing layer for a decorative covering element comprising a print layer and a wear layer arranged above said print layer, with the characteristic that the wear layer comprises a calcium-zinc stabilizer. The inventors have found that said calciumzinc stabilizer is highly efficient in protecting the wear layer from discolorations during the production process, even when high temperatures are reached such as in an oven or during thermal processes such as thermal pressing processes. In other words, the calcium-zinc stabilizer aids in avoiding discoloration, such as yellowing, of the wear layer. Where the finishing layer comprises a decor, the presence of said calcium-zinc stabilizer may thus also help in maintaining the realism of the decor. Furthermore, the inventors found that said calcium-zinc stabilizer may provide excellent properties in terms of transparency, such that decorative features below the wear layer may be perceived clearly with little to no disturbances and / or blurring.Preferred embodiments and their benefits for the finishing layer of the first independent aspect and / or the second independent aspect of the invention may equally be applied to the finishing layer of the third independent aspect of the invention. It is remarked that, in finishing layers according to the third independent aspect of the invention, the wear layer is applied above the print layer and, if present, also above the one or more decorative ink layers and the possible base ink layer.

[0038] Preferably, the calcium-zinc stabilizer is or is obtained from a solid calcium-zinc stabilizer. Preferably, said solid calcium-zinc stabilizer is at least partially dissolved, for example in plasticizer. This improves the ease of incorporating said solid calcium-zink stabilizer into the formulation of the wear layer.

[0039] In a preferred embodiment, the wear layer is a single layer comprising said calcium-zinc stabilizer. The inventors observed that this may provide an excellent transparency and / or may maximize consistency between production batches.

[0040] In a preferred embodiment, the wear layer comprises a first wear layer arranged above the print layer and a second wear layer arranged above the first wear layer, wherein at least the first wear layer comprises said, preferably solid, calcium-zinc stabilizer. By dividing the wear layer into multiple layers, it may be possible to finetune the compositions of each of these multiple layers such that optimal properties, for instance adherence and / or transparency properties, may be obtained.

[0041] Preferably, the first wear layer comprises said calcium-zinc stabilizer in an amount of at least 0.2 phr, preferably at least 0.5 phr, more preferably at least 1.5 phr, even more preferably at least 2.5 phr or 3 phr. With this amount of calcium-zinc stabilizer, particular solid calcium-zinc stabilizer, the inventors obtained excellent results in terms of transparency and thermal stability. The inventors have obtained excellent results with an amount of 1 phr calcium-zinc stabilizer in the first wear layer.

[0042] Preferably, the first wear layer and / or the second wear layer comprises a synthetic material, preferably a thermoplastic material such as PVC. Said synthetic material ispreferably a flexible or semi-rigid synthetic material such as flexible or semi-rigid PVC. Preferably, the first wear layer and / or the second wear layer are free from fillers.

[0043] Preferably, the second wear layer is free or essentially free from calcium-zinc stabilizer, in particular from solid calcium-zinc stabilizer. The inventors found that a calcium-zinc stabilizer, in particular a solid calcium-zinc stabilizer, may provide limited adherence to a possible lacquer layer. Thus, the absence of said calcium-zinc stabilizer in the second wear layer may provide beneficial adherence properties for a possible lacquer layer to be arranged above the second wear layer. In this context, “essentially free” means that the second wear layer may comprise said calcium-zinc stabilizer in an amount below 1 phr, preferably below 0.5 phr, more preferably below 0.1 phr or even below 0.01 phr.

[0044] In a preferred embodiment, the second wear layer comprises a barium-zinc stabilizer, preferably in an amount of at least 0.01 phr, more preferably at least 0.1 phr, even more preferably at least 0.5 phr, most preferably at least 0.75 phr. Preferably, the barium-zinc stabilizer is a liquid barium-zinc stabilizer. The inventors found that said barium-zinc stabilizer, in particular said liquid barium-zinc stabilizer, while providing excellent adherence properties for a possible lacquer layer, still provides very good properties in terms of transparency, such that decorative features below the wear layer may be perceived clearly with little to no disturbances and / or blurring.

[0045] In a preferred embodiment, the first wear layer and / or the second wear layer, preferably both the first wear layer and the second wear layer, comprises a phosphite costabilizer, preferably in an amount of at least 0.05 phr, more preferably at least 0.2 phr, even more preferably at least 0.5 phr or 1 phr. The phosphite costabilizer may provide a good thermal stability, especially when used in combination with the aforementioned calcium-zinc stabilizer or the aforementioned barium-zinc stabilizer.

[0046] According to some embodiments, the thickness of the first wear layer and the thickness of the second wear layer are substantially equal. This may provide a good balance between obtaining an excellent transparency on the one hand and obtaining a good adherence with a possible lacquer layer above the wear layer on the other hand.“substantially equal” in this context preferably means that the difference between the thickness of the first wear layer and the thickness of the second wear layer is less than 50%, preferably less than 35%, more preferably less than 20% or even less than 10% of the thickness of the first wear layer. According to alternative embodiments, the first wear layer is thicker than the second wear layer, preferably at least 10% thicker, more preferably at least 20% thicker, even more preferably at least 30% thicker, most preferably at least 50% thicker than the second wear layer. This may provide excellent transparency of the wear layer while still providing sufficient adherence for a possible lacquer layer above the wear layer. The inventors have obtained good results with a first wear layer having a thickness of about 0.3 mm and a second wear layer having a thickness of about 0.2 mm. According to further alternative embodiments, the second wear layer is thicker than the first wear layer, preferably at least 10% thicker, more preferably at least 20% thicker, even more preferably at least 30% thicker, most preferably at least 50% thicker than the first wear layer. This may provide excellent adherence for a possible lacquer layer above the wear layer while still maintaining a good transparency of the wear layer.

[0047] In preferred embodiments according to the first, second and third independent aspects, the finishing layer preferably comprises a lacquer layer arranged on top of the wear layer, wherein the lacquer layer preferably comprises or consists of polyurethane, preferably a UV cured or UV curable polyurethane. The lacquer layer may further improve the wear and scratch resistance of the finishing layer, and may provide the finishing layer at its outer side with a non-sticky surface.

[0048] Preferably, the lacquer layer has a thickness of up to 10 micrometer, preferably up to 20 micrometer, more preferably up to 30 micrometer. The lacquer layer is preferably applied in an amount of up to 10 g / m2, preferably up to 20 g / m2, more preferably up to 30 g / m2.

[0049] The lacquer layer preferably comprises one or more UV absorbers and / or one or more radical scavengers. UV absorbers absorb UV radiation such that the material of the lacquer layer, does not degrade. Examples of UV absorbers may be benzotri azole,benzophenone and high performance triazine. Radical scavengers on the other hand react with free radicals to neutralize them, such that they may prevent degradation of the lacquer layer. Examples of radical scavengers may include antioxidants and / or hindered amine light stabilizers (HALS) - such as derivatives of tetramethylpiperdine. Examples of antioxidants may be phenolic antioxidants, in particular primary phenolic antioxidants, thioesters, in particular secundary thioesters, and / or phosphites, in particular secundary phosphites. Examples of HALS may be derivatives of tetramethylpiperdine - such as Tinuvin 123 available from the company BASF -, imadizolidinone-based HALS and / or azetidinone-based HALS. UV absorbers and radical scavengers may be beneficial since they protect the lacquer layer, as well as the underlying layers such as the print layer, the possible one or more decorative ink layers, the possible base ink layer, and the one or more wear layers, from UV radiation, such that the risk of their colors changing over time is limited. Their presence may thus further reduce the risk of yellowing and / or improve the realism of the colors by avoiding fading of the colors, safeguarding the aesthetic appearance of the finishing layer. Said UV absorbers and / or radical scavengers are preferably present in the lacquer layer in an amount of between 0 and 10 phr each, preferably between 0 and 5 phr each. More preferably between 0 and 3 phr each. In particular, hindered amine light stabilizers are preferably present in an amount of between 0 and 5 wt%, preferably between 0.5 and 2 wt%.

[0050] The inventors observed that the lacquer layer may appear milky or white when looked at from an angle, and that, as a result, the finishing layer and a possible decor may not be perceived as intended. This is especially the case when looking from an angle of above 45° with respect to the perpendicular to the lacquer layer, and this effect becomes more prominent with increasing angle. Thus, there is a large difference in the way that a decor may be perceived, depending on the angle of observation. The inventors found that this is linked to the gloss level of the lacquer layer. In order to obtain a more angleindependent perception of the finishing layer, it may be desired to have a matte lacquer layer. Therefore, in accordance with its fourth independent aspect, the invention is a finishing layer for a decorative covering element comprising a print layer, a wear layer arranged on or above said print layer and a lacquer layer arranged on said wear layer atthe side opposite the print layer, with the characteristic that the lacquer layer has a gloss level measured at an angle of 85° of at most 10, preferably at most 6, more preferably at most 3, most preferably at most 2 and / or a gloss level measured at an angle of 60° of at most 10, preferably at most 6, more preferably at most 4, most preferably at most 3, wherein the gloss level is measured with a Rhopoint Novo-Gloss 20 / 60 / 85 glossmeter. The inventors obtained excellent results with a lacquer layer having such gloss levels, with little to no influence from the observation angle on the perception of the finishing layer. Such finishing layers are thus highly suitable to be provided with a decor since the realism of the possible colors and / or inks is optimally maintained, independent of the angle of observation.

[0051] It is noted that, in the context of this application, angles related to gloss levels are defined with respect to the perpendicular to the lacquer layer. The Rhopoint Novo-Gloss 20 / 60 / 85 glossmeter may perform its measurements according to a multitude of standards including DIN 67530, ISO 2813, and ASTM D523.

[0052] Preferred embodiments and their benefits for the finishing layer of the first independent aspect and / or the second independent aspect and / or the third independent aspect of the invention may equally be applied to the finishing layer of the fourth independent aspect of the invention.

[0053] Preferably, the lacquer layer comprises one or more from the list of matting agents, viscosity controlling agents, and photo-initiators. Examples of suitable photo-initiators are hydroxyaetophenones, alkyl aminoacetophenones, benzil ketals and dialkoxyacetophenones, benzoin ethers, phosphine oxides, (substituted) benzophenones, thioxanthones, anthraquinones, benzoylformate esters and camphorquinone. Examples of suitable matting agents are silica, calcium carbonate, talc, and micronized duromeric plastics such as polymethyl urea or polyamide. Said viscosity controlling agents may comprise thickeners and / or dilutants. Examples of suitable thickeners are polyurethane thickeners such as Hydrophobically Ethoxylated Urethane (HEUR) thickeners, Polyacrylate thickeners, Hydrophobically-modified polyacrylate thickeners such as hydrophobically-modified Alkali-Swellable Emulsion (HASE) thickeners,Hydrophobically-modified polyether thickeners (HMPE), Cellulose ethers or Hydrophobically-modified cellulose ethers such as Hydrophobically-modified Hydroxyethyl Cellulose (HMHEC). Examples of suitable dilutents are mono-, di-, tri- or tetra-functional acrylate monomers such as: 2-Ethylhexyl Acrylate (2-EHA), Phenoxyethyl Acrylate (PEA), Cyclic Trimethylolpropane Formal Acrylate (CTFA), 4-tert-Butylcyclohexyl Acrylate (TBCHA), Lauryl Acrylate (LA), 1,6-Hexanediol Diacrylate (HDDA), Dipropylene Glycol Diacrylate (DPGDA), Tripropylene Glycol Diacrylate (TPGDA), Glyceryl Propoxy Triacrylate (GPTA), Ethoxylated Trimethylolpropane Triacrylate (TMP(EO)TA), Propoxylated Trimethylolpropane Triacrylate (TMP(PO)TA) and / or Pentaerythritol Tetraacrylate (PETIA).

[0054] Preferably, the lacquer layer is cured by a type of UV radiation other than excimer radiation. The inventors have found, to their surprise, that it is possible to achieve the aforementioned gloss levels by types of UV radiation other than excimer radiation, for example by curing with radiation from a Mercury UV lamp. This significantly simplifies the process, as no inert environment is required, and the lacquer layer may be cured throughout its entire thickness more easily. Preferably, the lacquer layer is essentially free from micro-wrinkles.

[0055] According to a first particular embodiment of the first independent aspect, the finishing layer comprises a print layer, an optional base ink layer above the print layer, a wear layer arranged above said base ink layer, and a lacquer layer arranged on said wear layer at the side opposite the print layer, with the characteristics that the print layer comprises at least synthetic material and pigments, wherein said synthetic material is preferably thermoplastic material, wherein said pigments are titanium dioxide particles or white pigments other than titanium dioxide particles, wherein the print layer comprises said pigments in an amount of at least 5 phr, preferably at least 7.5 phr, more preferably at least 10 phr, even more preferably at least 12.5 phr; wherein the optional base ink layer is situated preferably directly above the print layer and wherein the optional base ink layer is a layer of ink, preferably a layer of blue ink; wherein the wear layer comprises a calcium-zinc stabilizer; and wherein the lacquer layer has a gloss level measured at an angle of 85° of at most 10, preferably at most 6, more preferably at most 3, mostpreferably at most 2 and / or a gloss level measured at an angle of 60° of at most 10, preferably at most 6, more preferably at most 4, most preferably at most 3, wherein the gloss level is measured with a Rhopoint Novo-Gloss 20 / 60 / 85 glossmeter.

[0056] The benefit of the first particular embodiment is on the one hand that an excellent background with very high whiteness is obtained such that possible decors applied thereon may be perceived more vibrant, while on the other hand discolorations of the different layers and changes of colors may be prevented. It is clear that the first particular embodiment combines multiple features described above in a synergistic manner.

[0057] According to a second particular embodiment of the first independent aspect, the finishing layer comprises a print layer, an optional base ink layer above the print layer, one or more decorative ink layers above said print layer or above said optional base ink layer, a wear layer arranged above said base ink layer, and a lacquer layer arranged on said wear layer at the side opposite the print layer, with the characteristics that the print layer comprises at least synthetic material and pigments, wherein said synthetic material is preferably thermoplastic material, wherein said pigments are titanium dioxide particles or white pigments other than titanium dioxide particles, wherein the print layer comprises said pigments in an amount of at least 5 phr, preferably at least 7.5 phr, more preferably at least 10 phr, even more preferably at least 12.5 phr; wherein the optional base ink layer is situated preferably directly above the print layer and wherein the optional base ink layer is a layer of ink, preferably a layer of blue ink; wherein the wear layer comprises a calcium-zinc stabilizer, wherein the wear layer comprises a first wear layer arranged above the print layer and a second wear layer arranged above the first wear layer, wherein at least the first wear layer comprises said calcium-zinc stabilizer; and wherein the lacquer layer has a gloss level measured at an angle of 85° of at most 10, preferably at most 6, more preferably at most 3, most preferably at most 2 and / or a gloss level measured at an angle of 60° of at most 10, preferably at most 6, more preferably at most 4, most preferably at most 3, wherein the gloss level is measured with a Rhopoint Novo-Gloss 20 / 60 / 85 glossmeter.The benefit of the second particular embodiment is that the decorative appearance of the finishing layer, which is at least formed by the one or more decorative ink layers, may be highly realistic thanks to the whiteness of the print layer and the optional base ink layer. Furthermore, thanks to the wear layer having a high transparency and excellent adherence to the lacquer layer, and the lacquer layer having a low gloss level, the decorative appearance may be perceived almost unaltered through the wear layer and the lacquer layer, independently from the angle of observation. As such, the second particular embodiment provides a synergistic combination of features described in relation to the first, second, third and fourth independent aspect.

[0058] In preferred embodiments according to any of the first, second, third, and fourth independent aspect, the finishing layer may have a structured upper surface. Said structured surface may comprise a relief which is preferably in register with a decor of the finishing layer.

[0059] It is clear that the finishing layer of the first, second, third, and fourth independent aspect, may be used as finishing layer of a decorative covering element. Therefore, in accordance with its fifth independent aspect, the invention is a decorative covering element, preferably a floor or wall covering element, wherein the decorative covering element comprises a substrate and a finishing layer attached to the substrate, with the characteristic that the finishing layer is a finishing layer as in any one of the first, second, third, and fourth independent aspect. As such, a decorative covering element may be obtained with excellent properties, such as vibrant colors, high realism, resistance against yellowing, and the decor being perceived similar for all angles of observation.

[0060] It is noted that the print layer herein may relate to one or more preparatory layers which may be directly printed. Said preparatory layers may be applied to a carrier. According to an alternative, said print layer may be a prefabricated foil arranged to be directly printed on, possibly with one or more preparatory layers.

[0061] Preferably, the substrate comprises one or more flexible or semi-rigid synthetic material layers, preferably thermoplastic material layers such as PVC layers. In someembodiments, the flexible or semi-rigid PVC layer or layers may comprise at least 50 phr plasticizer, preferably at least 60 phr, or even at least 70 phr. Said flexible or semi-rigid PVC layer or layers may comprise a reinforcing layer, for example a textile reinforcing layer, for example a glass-fiber fleece or cloth. The reinforcing layer preferably has a weight per unit area of between 10 and 150 g / m2, preferably between 20 and 100 g / m2, for example 40 g / m2. The flexible or semi-rigid PVC layer may comprise fillers in an amount of at least 10 wt%, preferably at least 30 wt%, more preferably at least 50 wt% or 60 wt%. The flexible or semi-rigid PVC layer may comprise fillers in an amount of at least 90 phr, preferably at least 100 phr, more preferably at least 120 phr. In a preferred embodiment, the fillers of one or more of said flexible or semi-rigid PVC layer or layers comprise biofiller, such as for example egg shell-based filler. This increases the circularity and sustainability of the decorative covering element.

[0062] The flexible or semi-flexible PVC of the substrate may be applied as a layer of PVC plastisol, with a first PVC layer being PVC plastisol impregnated in the reinforcing layer, and one or more layers of PVC plastisol applied on this impregnated reinforcing layer. Preferably, the thickness of the impregnated reinforcing layer is between 0.2 and 0.6 mm, preferably between 0.25 and 0.5 mm, for example 0.35 mm.

[0063] The flexible or semi-rigid PVC layer or layers may or may not be foamed, and in the foamed state preferably relate to a foam with closed cells. This foam may be foamed mechanically (for example by introducing gas or air bubbles), by chemical foaming with a blowing agent (for example azodi carbonamide or ADCA), or by incorporation of expandable or expanded cells (for example Expancell). Preferably, the first PVC layer impregnating the reinforcing layer is not foamed whereas one or more of said PVC layers applied on the impregnated reinforcing layer may be foamed. Preferably, the total thickness of said PVC layers applied on the impregnated reinforcing layer is between 0.3 and 5 mm, preferably between 0.5 and 3 mm, for example 1 mm.

[0064] In some embodiments, the substrate comprises a flexible or semi-rigid synthetic material layer being in contact with the print layer of the finishing layer, wherein the flexible or semi-rigid synthetic material layer comprises titanium dioxide particles or whitepigments other than titanium dioxide particles, preferably in an amount of at least 1 phr, more preferably at least 3 phr, even more preferably at least 5 phr. The flexible or semirigid synthetic material layer preferably comprises titanium dioxide particles or white pigments other than titanium dioxide particles in an amount of at most 10 phr, preferably at most 7 phr, most preferably at most 6 phr. The inventors observed that this may improve the realism and / or contrast of a decor while maintaining excellent processability. The inventors obtained excellent results with amounts between 4 and 6 phr, in particular amounts of 5 phr or around 5 phr.Preferably, the substrate further comprises a backing layer, wherein the backing layer preferably comprises or consists of a layer of synthetic material, preferably a layer of thermoplastic material, for example flexible or semi-rigid PVC. The backing layer preferably has a thickness of more than 0.5 mm, for example between 0.5 mm and 5 mm, for example between 0.75 mm and 2.5 mm. The backing layer may comprise fillers in an amount of up to 30 wt%, preferably up to 50 wt% or up to 60 wt%. In some embodiments, the backing layer may comprise more than 50 phr of plasticizer. In other embodiments, the backing layer is a textile backing layer, preferably with a weight per unit area of at least 30 g / m2, preferably at least 60 g / m2, more preferably at least 100 g / m2, for example 120 g / m2. In some embodiments, the textile backing layer is a polyester backing layer. In alternative embodiments, the textile backing layer is a polypropylene backing layer or a polyethylene backing layer. Such backing layers have the benefit that they have a relatively low melting temperature, and can thus be recycled more easily, in particular together with the rest of the decorative covering element.

[0065] The substrate may further comprise a calendered layer. The calendered layer may be a layer of thermoplastic material, preferably of PVC. The inventors found that a calendered layer may improve the mechanical performance of the decorative covering element, for example may improve the tear resistance. Preferably, the calendered layer comprises plasticizer in an amount of at least 25 phr, more preferably at least 30 phr or at least 35 phr. Preferably, the calendered layer comprises plasticizer in an amount of at most 60 phr, more preferably at most 50 phr, more preferably at most 45 phr. The inventors obtained good results with plasticizer amounts of 36 phr and 41 phr. Preferably the calendered layer comprises fillers, such as calcium carbonate and / or chalk, in an amountof at most 350 phr, more preferably at most 300 phr, even more preferably at most 275 phr or at most 265 phr. Preferably the calendered layer comprises fillers, such as calcium carbonate and / or chalk, in an amount of at least 150 phr, more preferably at least 200 phr, even more preferably at least 225 phr or at least 245 phr. The inventors found that these amounts of fillers, especially in combination with the aforementioned amounts of plasticizer, provide a mechanically performant layer for a decorative covering element while being sufficiently malleable during production. Good combinations were found to be 36 phr of plasticizer with a filler amount of 260 phr, and 41 phr of plasticizer with a filler amount of 250 phr. Preferably, the calendered layer has a thickness of at most 2 mm, more preferably at most 1.5 mm, even more preferably at most 1 mm. Preferably, the calendered layer has a thickness of at least 0.25 mm, more preferably at least 0.4 mm, even more preferably at least 0.5 mm or 0.6 mm. This may provide a very good balance between the increase in mechanical properties thanks to the presence of the calendered layer and the weight of the decorative covering element. The calendered layer may be applied between the print layer and the one or more flexible or semi-rigid synthetic material layers and / or between layers of the one or more flexible or semi-rigid synthetic material layers and / or between the one or more flexible or semi-rigid synthetic material layers and the backing layer and / or at the bottom side of the backing layer. Preferably, the calendered layer is applied between the one or more flexible or semi-rigid synthetic material layers and the backing layer and / or at the bottom side of the backing layer. This may be the preferred location for the calendered layer in order to maintain excellent walking comfort.

[0066] According to some embodiments, the decorative covering element may have a weight per unit area between 1500 g / m2and 3000 g / m2Preferably, the weight per unit area is selected between 1900 g / m2and 2600 g / m2, such as between 2050 g / m2and 2500 g / m2. Decorative covering elements with said weights per unit area have the advantage that their weight helps in more stable laying on a supporting structure, certainly if this is provided with non-permanent glue.According to some embodiments, the decorative covering element may have a thickness between 1 mm and 8 mm, preferably between 1 and 6 mm, more preferably between 1.5 and 4 mm.

[0067] According to a first possibility, the decorative covering element may have a width of at most 6 m, preferably at most 4 m, more preferably at most 2.5 m, even more preferably at most 2 m or even at most 1.5 m. Of course, the decorative covering element may also have a width of less than 2 m, for example of 1 m, 0.5 m or 0.2 m. The decorative covering element may have a length of various dozens of meters, for example between 20 and 50 meters.

[0068] According to a second possibility, the decorative covering element may have a substantially rectangular or square surface with a long side less than 3 m and greater than 0.4 m, or at least 0.8 m, and a short side less than 0.5 m and greater than 0.08 m. The long side is preferably in the range from 0.4 to 2.5 m, such as in the range from 0.4 to 2 m. The short side is preferably in the range from 0.1 to 0.45 m, such as in the range from 0.15 to 0.45 m.

[0069] According to some embodiments, the decorative covering element may be sheet vinyl or sheet vinyl cut to panel-shaped sizes.

[0070] According to some embodiments, the decorative covering element may be a floor covering element, a wall covering element or a ceiling covering element. According to a preferred embodiment, the decorative covering element is a floor covering element. It is noted that decorative covering elements of the invention are particularly suitable as floor covering elements thanks to their wear-resistant build-up, in particular thanks to the presence of the wear layer and / or lacquer layer.

[0071] The inventors found that the yellowing of a decorative covering element, in particular of its finishing layer, may also be linked to the migration of particular components from the bottom side of the decorative covering element to the top side of the decorative covering element. For example, in the case where the decorative covering element is glued to asubstructure, for example a subfloor, the inventors observed that some compounds, e.g. organic compounds, of the glue, may migrate to the finishing layer and cause undesired yellowing of the print layer and / or of the wear layer. The inventors observed that providing a migration barrier in the decorative covering element may effectively avoid or reduce this migration, thereby avoiding or reducing the associated yellowing or apparent yellowing. Therefore, in accordance with its sixth independent aspect, the invention is a decorative covering element, preferably a floor or wall covering element, wherein the decorative covering element comprises a substrate and a finishing layer attached to the substrate, with the characteristic that the decorative covering element comprises a migration barrier.

[0072] Preferably, the substrate comprises one or more flexible or semi-rigid synthetic material layers and / or a backing layer. These one or more flexible or semi-rigid synthetic material layers and / or backing layer are preferably in accordance with the one or more flexible or semi-rigid synthetic material layers and / or the backing layer described in relation to the fifth independent aspect. Preferred embodiments of the fifth independent aspect also apply to the sixth independent aspect as long as this does not lead to contradictions. Preferably, the finishing layer of the decorative covering element is in accordance with any one of the first, second, third, and fourth independent aspect and their preferred embodiments, without necessarily comprising a minimum amount of pigments as defined in relation to the first independent aspect. This has the benefit that a decorative covering element may be obtained with excellent properties, such as vibrant colors, high realism and resistance against yellowing.

[0073] Here below, several practical embodiments of such a migration barrier are described, without being limitative. Preferably, one or a combination of two or more of these possible embodiments are applied, which may provide excellent migration barrier properties and may avoid yellowing through migration.

[0074] In general, the inventors observed that the provision of a textile backing layer and / or one or more foamed layers - for example where one or more of the one or more flexible or semi-rigid synthetic material layers is foamed - may reduce migration. For the severalpractical embodiments, the inventors observed the biggest improvement in migration barrier efficiency for decorative covering elements that are free from a textile backing layer and / or of foamed layers in the substrate. This thus forms a preferred embodiment of the sixth independent aspect of the invention, however, is not essential.

[0075] In a first practical embodiment, the migration barrier is a coating comprising polyvinyl alcohol (PVOH), wherein one or more of the layers of the decorative covering element is provided with said coating. Preferably, said coating is provided on the print layer, on one or more of the one or more flexible or semi-rigid synthetic material layers and / or on the backing layer. It is noted that “on” herein may refer to applying the coating at the top side and / or at the bottom side of the respective layer. The inventors observed that applying the coating at these locations may significantly improve the migration barrier efficiency, effectively avoiding or at least reducing yellowing. Preferably, said coating is provided at the bottom side of the backing layer, especially in the case where the backing layer is a PVC-based backing layer and / or where the substrate - or at least the one or more flexible or semi-rigid synthetic material layers - is free from foamed layers. Especially in this case, the inventors observed that the presence of such a coating may be critical to avoid migration and its associated effects. Additionally, applying the coating to the bottom side of the backing layer may require the least amount of necessary changes to an already existing production line, as such production lines are often already provided with a coating or printing station to coat or print on the bottom side of the backing layer.

[0076] Preferably, said coating is a single-layered coating, however, the coating may also be multi-layered. Preferably, the total thickness of said coating is at least 1 micrometer, preferably at least 5 micrometer, more preferably at least 15 micrometer, even more preferably at least 50 micrometer or even at least 75 micrometer. The total thickness of said coating is preferably at most 100 micrometer, preferably at most 85 micrometer, most preferably at most 75 micrometer or at most 60 micrometer. The thickness of the coating preferably is in the range of 1-85 micrometer, preferably in the range of 5-75 micrometer, more preferably 10-60 micrometer, most preferably 15-50 micrometer. It was observed by the inventors that these coating thickness values provide good migration barrier efficiencies. These thickness values preferably relate to the thicknessof the coating after removal, for example by evaporation, of water and / or solvent. When applied, said coating preferably comprises a mixture of water, said PVOH, and an optional wetting agent. This may significantly increase the easy of application of the coating. This mixture preferably comprises at least 50 wt% water, preferably at least 60 wt%, more preferably at least 70 wt%, even more preferably at least 80 wt%, most preferably at least 90 wt% or even at least 95 wt%. The mixture preferably comprises at least 1 wt% PVOH, preferably at least 2 wt%, more preferably at least 4 wt% or at least 5 wt%. The mixture preferably comprises at most 50 wt% PVOH, preferably at most 40 wt%, more preferably at most 30 wt%, even more preferably at most 25 wt% or at most 20 wt%. This may provide a good balance between on the one hand the ease of application of the coating and on the other hand the migration barrier efficiency of the coating. The optional wetting agent may be of the polyether-siloxane type such as a poly dimethylsiloxane poly ether. The mixture preferably comprises at least 1.5 wt% of the optional wetting agent, preferably at least 2 wt%, more preferably at least 3 wt%, even more preferably at least 5 wt% or at least 10 wt%. In particular when applied to PVC-based layers, for example foamed PVC layers, it may be beneficial to apply such amounts of wetting agent in order for the coating to provide excellent adhesion and migration barrier efficiency. In some embodiments, the mixture comprises at least 0.05 wt% of the optional wetting agent, preferably at least 0.1 wt%, more preferably at least 0.2 wt%, even more preferably at least 0.3 wt% or at least 0.35 wt%. It was observed that such amounts of wetting agent may provide excellent applicability of the coating, which may provide a uniform and efficient migration barrier.

[0077] In a first preferred example, said PVOH comprises an adhesion compound, wherein said adhesion compound preferably accounts for at least 40 wt% of the PVOH, preferably at least 45 wt%, more preferably at least 50 wt%, even more preferably at least 60 wt% or at least 65 wt%. In alternative embodiments, said adhesion compound accounts for at most 1 wt%, preferably at most 2 wt%, more preferably at most 5 wt% or at most 6 wt% of the PVOH. Surprisingly, it was found that coatings having such compositions may provide excellent adherence to synthetic material layers, especially to PVC layers, while also providing excellent migration barrier properties. It is noted that, while good adhesion to PVC-based layers may be obtained, it is not necessary that the coating is directlyapplied to a PVC-based layer. For example, the coating may be applied to layers of synthetical material different from PVC, for example layers of polypropylene (PP) or polyethylene terephthalate (PET). It is also not excluded that first a primer is applied before the coating is applied, such that the coating is applied to the primer. Such a primer may provide the surface intended to receive the coating with appropriate surface properties for the coating to adhere. As such, desired properties may be obtained thanks to the primer, while the coating then provides the adhesion to the primer as well as excellent migration barrier efficiency. Said adhesion compound may be a compound selected from silane, polyethyleneimine (PEI), epoxy silanes, MAH-grafted polymers (maleic anhydride grafted polymers), Hexamethoxymethylmelamine (HMMM) such as Cymel 323 from the company Allnex, tannins and lignin. Said adhesion compound, in particular silane compound, may comprise at least one amine functional group, which may provide even better adherence properties to the coating, especially for adherence to PVC layes, in particular to filled PVC layers.

[0078] In a second preferred example, the coating comprises PVOH and a polyisocyanate derivative. Said polyisocyanate derivative was found to promote adhesion to synthetic material layers, especially to PVC-based layers. Good adhesion may even be obtained to filled PVC-based layers. It is noted that, while good adhesion to PVC-based layers is obtained, it is not necessary that the coating is directly applied to a PVC-based layer. For example, the coating may be applied to layers of material, preferably synthetic material, different from PVC, for example layers of polypropylene (PP) or polyethylene terephthalate (PET). It is also not excluded that first a primer is applied before the coating is applied, such that the coating is applied to the primer. As such, desired properties may be obtained thanks to the primer, while the coating then provides the adhesion to the primer as well as excellent migration barrier efficiency. Said polyisocyanate derivative may be obtained through reaction of a polyisocyanate with hydroxyl groups of the PVOH. Preferably said PVOH has a hydrolysis degree of at most 99.5 mol%, preferably of at most 99 mol%, more preferably at most 98 mol%, even more preferably at most 95 mol% or at most 90 mol%. The weight of the polyisocyanate derivative is preferably at least 30% of the weight of the PVOH, preferably at least 40%, more preferably at least 45%, even more preferably at least 50%, most preferably at least 55% or at least 60%. Inalternative embodiments, the weight of the polyisocyanate derivative is preferably at most 10% of the weight of the PVOH, preferably at most 6%, more preferably at most 5%, even more preferably at most 4%, most preferably at most 3% or even at most 2%. The inventors observed that these weight ratios may provide excellent migration barrier properties on the one hand and excellent adhesion properties on the other hand.

[0079] In a second practical embodiment, the migration barrier is a coating comprising a modified polyvinyl alcohol (modified PVOH), wherein one or more of the layers of the decorative covering element is provided with said coating. Said modified PVOH may be a PVOH modified by carboxyl modification, by crosslinking with glutaraldehyde, with borax or with citric acid, or by graft polymerisation with acrylonitril. These modifications may provide a coating with excellent migration barrier properties, especially when applied on a PVC-based layer. Preferred features described in relation to the coating of the first practical embodiment may also apply to the coating of the second practical embodiment, as long as this does not lead to contradictions.

[0080] In a third practical embodiment, the migration barrier is a coating comprising an ethylene vinyl alcohol (EVOH) or a modified ethylene vinyl alcohol (modified EVOH), wherein one or more of the layers of the decorative covering element is provided with said coating. Said modified EVOH may be an EVOH modified by carboxyl modification, by crosslinking with glutaraldehyde, with borax or with citric acid, or by graft polymerisation with acrylonitril. These modifications may provide the coating with excellent migration barrier properties, especially when applied on a PVC-based layer. Most preferably, said modified EVOH is an EVOH modified by copolymerisation with aromatic monomers, such as styrene or acrylonitril, which the inventors found to be very suitable to increase the migration barrier efficiency of coatings comprising EVOH or modified EVOH. Preferred features described in relation to the coating of the first practical embodiment may also apply to the coating of the third practical embodiment, as long as this does not lead to contradictions.

[0081] In a fourth practical embodiment, the migration barrier is a coating comprising polyacrylic acid, polyaspartic acid, acrylic copolymers - such as ethylene acrylic acidcopolymer (EAA) or ethylene methacrylic acid copolymer (EMAA)

[0082]

[0083] and / or poly vinylidene chloride (PVDC), wherein one or more layers of the decorative covering element is provided with said coating. Preferred features described in relation to the coating of the first practical embodiment may also apply to the coating of the fourth practical embodiment, as long as this does not lead to contradictions.

[0084] In a fifth practical embodiment, the migration barrier is a layer comprising a composition comprising lamellar fillers, preferably said lamellar fillers having an aspect ratio of at least 500, preferably at least 1000, more preferably at least 3000, even more preferably at least 4000, most preferably at least 5000 or at least 6000. The aspect ratio of a said lamellar filler refers to the ratio of the diameter - or equivalent diameter - of the lamellar filler with respect to the thickness of the lamellar filler. The inventors observed that lamellar fillers having such high aspect ratios may be very efficient in avoiding or reducing migration and its associated effects, which is theorized to be a result of the lamellar fillers significantly increasing the length of the path that the migrating components need to travel. The lamellar fillers preferably have their thickness direction substantially parallel to the thickness direction of the decorative covering element. The lamellar fillers may have a thickness of at most 500 nanometer, preferably at most 100 nanometer, more preferably at most 10 nanometer, even more preferably at most 1 nanometer or even at most 0.5 nanometer. The lamellar fillers may have a diameter -or equivalent diameter - of at most 20 micrometer, preferably at most 10 micrometer, more preferably at most 5 micrometer, most preferably at most 1 micrometer. Good results have been obtained with lamellar fillers having a thickness in the range of 0.5-1.5 nanometer, in particular 0.9-1.0 nanometer, and a diameter - or equivalent diameter - in the range of 1 to 10 micrometer, in particular in the range of 3 to 5 micrometer. The lamellar fillers are preferably clay -based lamellar fillers, which are preferably present in a substantially dry or dried state. Clay is preferably used as this allows to obtain lamellar fillers having suitable dimensions to provide excellent migration barrier properties. The lamellar fillers preferably have a residual moisture content of at most 5%, preferably at most 2%, even more preferably at most 1%. It was observed that such residual moisture contents may improve the migration barrier efficiency of the layer comprising lamellarfillers. Preferably, said composition comprising lamellar fillers further comprises a dispersing agent selected from:

[0085] - Polyacrylate-based dispersant, comprising polyacrylic acid or one or more of its copolymers;

[0086] - Polyurethane-based dispersant, comprising polyurethane block copolymers; - Hyperdispersant, comprising tailored block copolymers with pigment-affinic anchoring groups;

[0087] - Phosphate ester-based dispersant, comprising one or more phosphate esters or one or more of their salts;

[0088] Amino-functional dispersant, comprising amine-modified polymers or copolymers;

[0089] Controlled flocculation agents, comprising a solution of a phosphoric acid salt of long-chain carboxylic acid polyamine amides.

[0090] The dispersing agent provides a good rheology to the composition comprising lamellar fillers such that the lamellar fillers may form an efficient migration barrier. Said dispersing agent preferably represents between 0 and 30 wt% of the composition comprising lamellar fillers, more preferably between 1 and 20 wt%, even more preferably between 5 and 15 wt%. The composition comprising lamellar fillers preferably also comprises a plasticizer in an amount between 10 and 80 wt%, preferably between 20 and 70 wt%, more preferably between 30 and 60 wt%. It may be preferred that the composition comprises at most 60 wt%, at most 40 wt% or at most 20 wt% of lamellar fillers. Said plasticizer is preferably selected from Diisononyl Phthalate (DINP), Diisodecyl Phthalate (DIDP), Dioctyl Terephthalate (DOTP), and Diisononyl Cyclohexane-l,2-dicarboxylate (DINCH). Most preferably, however, the plasticizer is selected from DOTP, DINCH and other non-phtalate plasticizers as these are safer and provide less health risks.

[0091] Said lamellar fillers may be employed in one or more of the layers of the decorative covering element and / or as a coating on one or more of the layers of the decorative covering element.Preferably, the print layer, the one or more flexible or semi-rigid synthetic material layers and / or to the backing layer, in particular where the backing layer is PVC-based, comprises said composition comprising lamellar fillers. This may facilitate the introduction of the lamellar fillers into the decorative covering element and may not require additional steps and equipment for the manufacturing process as the lamellar fillers may be incorporated into the composition of the corresponding layer. It may be preferred that the aforementioned composition comprising lamellar fillers comprises at most 60 wt%, at most 40 wt% or at most 20 wt% of lamellar fillers. Very good results were obtained where the layer comprising the composition comprising lamellar fillers is a PVC-based layer, especially for PVC-based layers having a K-value of between 20 and 100, in particular between 50 and 90, since the inventors found that such PVC based layers already reduce the amount of migration. This is of high interest in the case of a PVC-based print layer, which forms one of the last layers that may stop the migration from reaching the wear layer. Furthermore, it may be preferred that the layer comprising the composition comprising lamellar fillers relates to the print layer and / or to the one or more flexible or semi-rigid synthetic material layers and / or to the backing layer, wherein the backing layer is unfoamed. The inventors found that unfoamed layers have a lower migration barrier efficiency than foamed layers, such that it is extremely beneficial that one or more of the aforementioned layers comprises said lamellar fillers in order to improve the overall migration barrier efficiency. Of course, it is not excluded that the backing layer is foamed, which may further improve the overall migration barrier efficiency.

[0092] Said layer comprising the composition comprising lamellar fillers may be a coating, wherein this coating is preferably applied to the bottom side of the wear layer and / or to the top side of the print layer and / or to the bottom side of the print layer. Said coating may also be applied between the print layer and the one or more flexible or semi-rigid synthetic material layers and / or between layers of the one or more flexible or semi-rigid synthetic material layers and / or between the one or more flexible or semi-rigid synthetic material layers and the backing layer and / or at the bottom side of the backing layer. Most preferably, the coating is applied to the top side of the print layer, in particular before application of the possible one or more decorative ink layers. Thus, the coating ispreferably arranged between the print layer and the possible one or more decorative ink layers. This may provide a more seamless incorporation of such coating into an already existing production line, since printing equipment for applying the possible one or more decorative ink layers, is already present and may also be used for applying this coating. Said coating preferably has a thickness of at least 1 micrometer or at least 2 micrometer, preferably at least 5 micromer, more preferably at least 10 micrometer, more preferably at least 15 micrometer, even more preferably at least 20 micrometer or at least 30 micrometer. Said coating preferably has a thickness of at most 50 micrometer, more preferably at most 40 micrometer, even more preferably at most 30 micrometer. With such coating thicknesses, the inventors observed that the lamellar fillers may orient themselves suitably in order to provide excellent barrier properties, while not or barely affecting other properties such as for example bonding properties. Additionally, when the coating is to be applied on top of the print layer - and preferably below the possible one or more decorative ink layers - it is desired to apply such limited thicknesses as these thicknesses may be efficiently provided by already present printing equipment in an existing production line, thus requiring little to no investments for adaptations. Preferably, the coating further comprises a resin such as for example PVC, which may improve the adherence of the coating to further layers, for example further PVC layers.

[0093] In a sixth practical embodiment, the migration barrier is a layer comprising barrier fillers. Said barrier fillers preferably relate to microspheres, preferably hollow microspheres. These barrier fillers have the benefit that they may, in a similar manner as the lamellar fillers described before, increase the length of the path that the migrating compounds need to travel before reaching the wear layer. Preferably, these barrier fillers are lightweight, meaning that their mass density is lower than the average mass density of the layer comprising said barrier fillers. As such, the barrier fillers reduce the weight of the decorative covering element, thereby facilitating handling of the decorative covering element. Preferred barrier fillers are hollow glass microspheres, closed-cell expanded perlite and hollow ceramic microspheres such as the microspheres known under the name Fillite. The barrier fillers preferably have a diameter - or equivalent diameter - of at most 500 micrometer, preferably of at most 350 micrometer, more preferably of at most 150 micrometer, even more preferably at most 100 micrometer, most preferably at most50 micrometer or at most 10 micrometer. These sizes allow the barrier fillers to become sufficiently closely packed, thereby increasing the length of the path that the migrating compounds need to travel before reaching the wear layer. The inventors obtained very good results with barrier fillers having a diameter - or equivalent diameter - of between 50 and 250 micrometer, in particular of 150 micrometer. The layer comprising barrier fillers preferably relates to one or more of the one or more flexible or semi-rigid synthetic material layers - in particular to the one or more flexible or semi-rigid synthetic material layers that is free from a reinforcing layer -, however it may also relate to the print layer and / or to the backing layer, in particular when the backing layer comprises PVC. The inventors observed that foaming of a layer may reduce migration, however, may also reduce mechanical properties - such as indentation and compression strength - of the foamed layer and / or of the decorative covering element. Therefore, in a preferred embodiment, the layer comprising barrier fillers is an unfoamed layer. This has the benefit that the barrier fillers may provide good migration barrier efficiency while maintaining good mechanical properties. In an alternative preferred embodiment, the layer comprising barrier fillers is a foamed layer, wherein the foaming may be at least partially obtained by a foaming agent such as azodi carbonamide (ADCA). This may provide very light decorative covering elements that have excellent migration barrier properties. Preferably, the diameter - or equivalent diameter - of the barrier fillers is within 50% of the diameter - or equivalent diameter - of the cells of the foamed layer, preferably within 30%, more preferably within 20%, even more preferably within 10% or within 5%. It was observed by the inventors that this may provide an excellent migration barrier efficiency, which is theorized to be because the barrier fillers may arrange themselves in a very good packing with respect to the cells of the foam, thereby further increasing the length of the path that the migrating components have to travel. In a preferred embodiment, the foamed layer comprising the barrier fillers is a layer of the one or more flexible or semi-rigid synthetic material layers, in particular a PVC layer applied on an impregnated reinforcing layer.

[0094] In a seventh practical embodiment, the migration barrier is a reinforcing layer comprising reinforcing material and a binder. Said reinforcing material may be glass fibers bonded together by said binder. Preferably, said reinforcing layer is a glass-fiber fleece. Saidreinforcing layer preferably has a surface weight, which preferably relates to the combined weight of the reinforcing material and the binder, of at least 5 g / m2, preferably of at least 15 g / m2, more preferably of at least 30 g / m2, even more preferably of at least 40 g / m2, most preferably of at least 50 g / m2. Said reinforcing layer preferably has a surface weight of at most 100 g / m2, preferably of at most 85 g / m2, more preferably of at most 75 g / m2, most preferably of at most 60 g / m2. It was observed by the inventors that reinforcing layers having such surface weights may provide both structural stability and excellent migration barrier properties. Preferably, the binder represents between 5% and 80% of the combined weight of the reinforcing material and the binder, more preferably between 10% and 50%, even more preferably between 20% and 35%, for example 25% or 31.5%. With these ratios, the inventors observed that excellent migration barrier efficiency may be obtained. Said binder preferably is or comprises PVOH, modified PVOH, EVOH, modified EVOH and / or a component as described in relation to the fourth practical embodiment. With respect to PVOH, modified PVOH and modified EVOH, the above described modifications for the first, second and third practical embodiments may also be applied here. Preferably, the reinforcing layer of the seventh practical embodiment relates to the reinforcing layer of the one or more flexible or semirigid synthetic material layers.

[0095] As mentioned already, it is possible, and even preferred, to combine two or more of the aforementioned practical embodiments. For example, excellent migration barrier results may be obtained with a decorative covering element provided with (i) a coating comprising a composition comprising lamellar fillers on top of the print layer - and preferably below the optional one or more decorative ink layers -, (ii) a glass-fiber fleece provided with PVOH or another binder which preferably relates to an impregnated glassfiber fleece of the one or more flexible or semi-rigid synthetic material layers, (iii) barrier fillers in an unfoamed or foamed layer of the substrate, and / or (iv) a coating in accordance with any of the first to fourth practical embodiment on the - preferably back side of the - backing layer and / or on one or more of the one or more flexible or semirigid synthetic material layers.In an eighth practical embodiment, the migration barrier is a calendered layer. The calendered layer may be a layer of thermoplastic material, preferably of PVC. Without being bound by theory, the inventors believe that the migration barrier properties of the calendered layer may be a result of its closely spaced polymer chains which are relatively immobile, which may then restrict the amount of migration through the calendered layer. Preferably, the calendered layer comprises plasticizer in an amount of at least 25 phr, more preferably at least 30 phr or at least 35 phr. Preferably, the calendered layer comprises plasticizer in an amount of at most 60 phr, more preferably at most 50 phr, more preferably at most 45 phr. The inventors obtained good results with plasticizer amounts of 36 phr and 41 phr. The inventors observed that the polymer chains of the calendered layer may become less mobile and / or more closely spaced with such amounts of plasticizer, which may provide optimal efficiency of the calendered layer as migration barrier. Preferably the calendered layer comprises fillers, such as calcium carbonate and / or chalk, in an amount of at most 350 phr, more preferably at most 300 phr, even more preferably at most 275 phr or at most 265 phr. Preferably the calendered layer comprises fillers, such as calcium carbonate and / or chalk, in an amount of at least 150 phr, more preferably at least 200 phr, even more preferably at least 225 phr or at least 245 phr. This amount of fillers may be preferred in order for the thermoplastic material to remain sufficiently workable, especially when using the aforementioned plasticizer amounts. Good combinations were found to be 36 phr of plasticizer with a filler amount of 260 phr, and 41 phr of plasticizer with a filler amount of 250 phr. Preferably, the calendered layer has a thickness of at most 2 mm, more preferably at most 1.5 mm, even more preferably at most 1 mm. Preferably, the calendered layer has a thickness of at least 0.25 mm, more preferably at least 0.4 mm, even more preferably at least 0.5 mm or 0.6 mm. This may provide an excellent balance between on the one hand the efficiency as migration barrier and on the other hand the cost of manufacturing and incorporating such a calendered layer. The calendered layer may be applied between the print layer and the one or more flexible or semi-rigid synthetic material layers and / or between layers of the one or more flexible or semi-rigid synthetic material layers and / or between the one or more flexible or semi-rigid synthetic material layers and the backing layer and / or at the bottom side of the backing layer. Preferably, the calendered layer is applied between the one or more flexible or semi-rigid synthetic material layers and the backing layer and / orat the bottom side of the backing layer. This may be the preferred location for the calendered layer in order to maintain excellent walking comfort because the calendered layer may be rather compact, for example because of low plasticizer amounts.

[0096] In a nineth practical embodiment, the migration barrier is a thermoplastic layer comprising plasticizer in an amount below 50 phr, preferably below 30 phr, more preferably below 20 phr, even more preferably below 10 phr or below 5 phr, wherein the migration barrier is arranged below the print layer. The inventors theorize that this may lead to a plasticizer flow towards the migration barrier, for example from layers arranged above the migration barrier, and that this plasticizer flow may slow down or even halt the migration of the components of the glue. The migration barrier may be arranged between the print layer and the one or more flexible or semi-rigid synthetic material layers and / or between layers of the one or more flexible or semi-rigid synthetic material layers and / or between the one or more flexible or semi-rigid synthetic material layers and the backing layer and / or at the bottom side of the backing layer. Preferably, the migration barrier is arranged between the one or more flexible or semi-rigid synthetic material layers and the backing layer and / or at the bottom side of the backing layer. This may optimize the working of the migration barrier since there is only or mainly a downwords flow of plasticizer, which migrates in the opposite direction of the component or components of the glue. Preferably, this thermoplastic layer comprises or is based on PVC. The thermoplastic layer may comprise filler such as calcium carbonate and / or chalk, preferably in an amount of at most 250 phr, more preferably at most 150 phr, most preferably at most 100 phr or at most 50 phr. Preferably, the thermoplastic layer has a thickness of at most 2 mm, more preferably at most 1.5 mm, even more preferably at most 1 mm. Preferably, the thermoplastic layer has a thickness of at least 0.25 mm, more preferably at least 0.4 mm, even more preferably at least 0.5 mm or 0.6 mm.

[0097] It is remarked that the coating referred to in any one of the aforementioned practical embodiments may preferably be arranged between the print layer and the possible one or more decorative ink layers. In such case, the coating is preferably applied by a printing device, for example by an analogue printing device such as by rotogravure printing. Theprinting device for applying the coating is preferably the same printing device used for applying the one or more decorative ink layers. This may provide an easy incorporation of such coating into an already existing production line, since printing equipment for applying the possible one or more decorative ink layers, is typically already present and may also be used for applying this coating.

[0098] It is remarked that each of the aforementioned first to nineth practical embodiments are preferably applied to a PVC layer having a K-value of between 20 and 100, in particular between 50 and 90. This may relate to a coating applied to such a PVC layer and / or to such a PVC layer comprising one of the fillers described in the fifth and sixth practical embodiments. The inventors found that PVC having such K-values may already reduce migration, such that this may provide for excellent migration barrier properties.

[0099] According to a seventh independent aspect, the invention is a decorative covering element, preferably a floor or wall covering element, wherein the decorative covering element comprises a substrate and a finishing layer attached to the substrate, wherein the substrate comprises a calendered layer comprising thermoplastic material, with the characteristic that the thermoplastic material of the calendered layer comprises recycled thermoplastic material. This has the benefit that recycled material may be efficiently incorporated into a decorative covering element, which may improve sustainability and reduce production costs.

[0100] Preferably, the substrate comprises one or more flexible or semi-rigid synthetic material layers and / or a backing layer. These one or more flexible or semi-rigid synthetic material layers and / or backing layer are preferably in accordance with the one or more flexible or semi-rigid synthetic material layers and / or the backing layer described in relation to the fifth independent aspect. Preferred embodiments of the fifth and / or sixth independent aspect also apply to the seventh independent aspect as long as this does not lead to contradictions. Preferably, the finishing layer of the decorative covering element of the seventh independent aspect is in accordance with any one of the first, second, third, or fourth independent aspect and their preferred embodiments, without necessarily comprising a minimum amount of pigments as defined in relation to the first independentaspect. This has the benefit that a decorative covering element may be obtained with excellent properties, such as vibrant colors, high realism and resistance against yellowing.

[0101] The calendered layer may be applied between the finishing layer and the one or more flexible or semi-rigid synthetic material layers and / or between layers of the one or more flexible or semi-rigid synthetic material layers and / or between the one or more flexible or semi-rigid synthetic material layers and the backing layer and / or at the bottom side of the backing layer. Preferably, the calendered layer is applied between the one or more flexible or semi-rigid synthetic material layers and the backing layer and / or at the bottom side of the backing layer. This may be the preferred location for the calendered layer in order to maintain excellent walking comfort. The calendered layer preferably has a thickness of at most 2 mm, more preferably at most 1 mm, even more preferably at most 0.75 mm. The calendered layer preferably has a thickness of at least 0.1 mm, more preferably at least 0.3 mm, most preferably at least 0.5 mm.

[0102] Preferably, the thermoplastic material and / or the recycled thermoplastic material of the calendered layer comprises or substantially consists of the same thermoplastic material, preferably PVC.

[0103] In a preferred embodiment, the thermoplastic material of the calendered layer comprises at least 25 wt%, preferably at least 50 wt%, more preferably at least 60 wt% or at least 70 wt% of recycled thermoplastic material. Preferably, the thermoplastic material of the calendered layer substantially consists or entirely consists of recycled thermoplastic material.

[0104] Preferably, the recycled thermoplastic material originates at least partially from decorative covering elements such as floor products, wall products, and / or ceiling products. This may provide excellent circularity of dcorative covering elements. Preferably, the recycled thermoplastic material originates partially or entirely from decorative covering elements in accordance with the fifth independent aspect and / or sixth independent aspect.Preferably, the decorative covering element is a sheet vinyl.

[0105] According to an eighth independent aspect, the invention is a method for manufacturing a decorative covering element, preferably a floor or wall covering element, wherein the decorative covering element comprises a substrate and a finishing layer attached to the substrate, wherein the substrate comprises a calendered layer comprising thermoplastic material, wherein the method comprises at least the steps of:

[0106] providing thermoplastic material, preferably PVC;

[0107] providing recycled thermoplastic material, preferably recycled PVC; mixing the thermoplastic material with the recycled thermoplastic material to form a mixture;

[0108] optionally adding plasticizer and / or fillers and / or additives to the mixture; forming a calendered layer from said mixture;

[0109] arranging a finishing layer above said calendered layer.

[0110] It is clear that the method of the eighth independent aspect is ideally suited for manufacturing a decorative covering element in accordance with the seventh independent aspect. Preferred embodiments of the seventh independent aspect may also form preferred embodiments of the eighth independent aspect, as long as this does not lead to contradictions.

[0111] Preferably, the step of providing recycled thermoplastic material comprises the step of grinding and / or comminuting recycled thermoplastic material, preferably into particles having a particle size distribution percentile D90 value of less thanat most 6 mm, preferably at most 4 mm, more preferably less than 2,5 mm and / or a D50 percentile value or less than 1,75 mm. This may provide a substantially uniform mixture. The particle size may be determined by laser granulometry, which may be performed in accordance with ISO 13320:2020. This is a dynamic light scattering technique using a laser with an emission wavelength of 632.8 nm, measuring at a scattering angle of 90 degrees. This technique may be performed, for example, with a Malvern® Mastersizer 2000 or with a Malvern® Mastersizer 3000.Preferably, the step of forming the calendered layer comprises the step of heating the mixture until the mixture is in a semi-molten or molten state. Preferably, the step of forming the calendered layer comprises the step of calendering the semi-molten or molten mixture through heated calendering rollers. Thanks to these steps, virgin and recycled thermoplastic material may be intimately connected, such that the calendered layer resulting from the process may show uniform properties.

[0112] It is noted that, according to every aspect of the invention, the print layer preferably forms the bottom layer of the finishing layer, and that when applied, this print layer is adjacent to the substrate of the decorative covering element. Preferably, the top side of the finishing layer forms the top side of the decorative covering element.

[0113] For better illustration of the features of the invention, some preferred embodiments are described hereunder, as examples without any limiting character, referring to the appended drawings, in which:

[0114] Figure 1 shows a top view of a portion of a decorative covering element of the invention;

[0115] Figure 2 shows an enlarged view of the cross-section indicated by the line II-II on Figure 1;

[0116] Figures 3 shows an enlarged view of the area indicated with F3 in Figure 2; Figures 4 to 7 show, in a similar view as Figure 3, different embodiments for a finishing layer according to the invention.

[0117] Figure 1 represents a portion of a decorative covering element 1. The width B of such decorative covering element 1 can vary between 2 and 6 meters and is preferably up to 3.5 m or 4 m. The length L can be various dozens of meters, for example, between 20 and 50 meters. The decor of the decorative covering element 1 of the example represents a number of panel-shaped elements 2, each having a wood decor. Of course, other decors such as a stone decor or a fantasy decor are equally possible. The decorative covering element 1 of the example has a structured upper surface comprising relief features 3 that may be in register with the wood decor, as well as lowered edge regions 4 at the edgesbetween said panel-shaped elements 2. These lowered edge regions 4 may aid in providing a more realistic imitation, in this case of wooden panels or wooden boards.

[0118] The cross-sectional view of Figure 2 clearly shows that the decorative covering element 1 comprises a substrate 5 and a finishing layer 6 arranged above the substrate 5. The finishing layer 6 of this example, seen in more detail in Figure 3, comprises, from bottom to top, a print layer 7, an optional base ink layer 8, one or more decorative ink layers 9, a wear layer 10, and a lacquer layer 11.

[0119] The print layer 7 of the example comprises unfoamed, flexible PVC and pigments, wherein the pigments 12 are titanium dioxide particles and / or white pigments other than titanium dioxide particles. Said pigments 12 are present in the print layer 7 in a total amount of at least 7.5 phr, more preferably at least 10 phr, even more preferably at least 12.5 phr. The pigments 12 may for example be present in an amount of 15 phr. The print layer 7 comprises plasticizer in an amount of more than 40 phr, preferably even more than 50 phr. The print layer 7 further comprises fillers, preferably calcium carbonate, in an amount above 75 phr, preferably above 90 phr. Said fillers may also be or comprise talcum, lime and / or chalk. The print layer 7 has a thickness of at least 0.05 mm, preferably at least 0.15 mm, more preferably at least 0.2 mm. It is remarked that the thickness of each layer is intended to be understood as the average thickness, not taking into account local deviations, for example due to a structured upper surface. In this example, the print layer 7 comprises between 0.1 and 2 phr of calcium-zinc stabilizer in order to improve its thermal stabilization. In certain embodiments, the print layer 7 may also comprise one or more components selected from the list of phosphite, barium-zinc stabilizer, and epoxidized soybean oil.

[0120] In this example, as can be clearly seen on Figure 3, the optional base ink layer 8 is present and is arranged directly above the print layer 7. Preferably, the base ink layer 8 is a layer of blue ink, such that apparent yellowing of other layers, for example of the wear layer 10 or the print layer 7, may be counteracted and remain hidden to the naked eye. In the example, the base ink layer 8 covers the entire surface area of the print layer 7, i.e. it is an all-over layer. The ink used for the base ink layer 8 may be a water-based inkcomprising an acrylate-based binder and pigments, preferably C.I. Pigment Blue 15:3 and C.I. Pigment Red 122. Preferably, the base ink layer 8 comprises a pigmented ink in an amount of at most 2 wt%, more preferably at most 1 wt%, even more preferably at most 0.5 wt%, most preferably at most 0.1 wt%, for example 0.05 wt%, and a nonpigmented ink in an amount of at least 98 wt%, more preferably at least 99 wt%, even more preferably at least 99.5 wt%, most preferably at least 99.9 wt%, for example 99.95. Preferably, the pigmented ink comprises pigments, preferably C.I. Pigment Blue 15:3 and C.I. Pigment Red 122, in an amount between 0.5 and 50 wt%, preferably between 1 and 40 wt%, more preferably between 5 and 20 wt%, and binder in an amount between 50 and 99.5 wt%, more preferably between 60 and 99 wt%, most preferably between 80 and 95 wt%. Preferably, these weight percentages are based on dry weight. The base ink layer 8 has a thickness between 5 and 10 micrometers in this example. Preferably, the base ink layer 8 comprises a PVC latex, which improves the adherence between the base ink layer 8 and adjacent layers comprising PVC, such as the print layer 7 and / or the one or more decorative ink layers 9.

[0121] The one or more decorative ink layers 9 in this example are arranged above the print layer 7 with the base ink layer 8 between these layers. The one or more decorative ink layers 9, in combination with the print layer 7 and the base ink layer 8, form the decor of the finishing layer 6. Thanks to the whiteness of the print layer 7, the colors of the one or more decorative ink layers 9 may be more vibrant, and a more realistic impression of real wood may be obtained. Said one or more decorative ink layers 9 preferably comprise a PVC latex, which improves the adherence between the one or more decorative ink layers 9 and adjacent layers comprising PVC, for example the wear layer 10.

[0122] As can be clearly seen on Figure 3, the wear layer 10 of the example comprises a first wear layer 10A arranged above the one or more decorative ink layers 9 and a second wear layer 10B arranged above the first wear layer 10 A. Both the first wear layer 10A and the second wear layer 10B are unfoamed, flexible or semi-rigid PVC layers, preferably comprising more than 20 phr of plasticizer, more preferably more than 30 phr. Both the first wear layer 10A and the second wear layer 10B are free from fillers. In the example, the first wear layer 10A comprises a solid calcium-zinc stabilizer in an amountof at least 0.2 phr, preferably at least 0.5 phr, more preferably at least 1.5 phr, even more preferably at least 2.5 phr or 3 phr. The second wear layer 10B is preferably free from calcium-zinc stabilizer, but comprises a liquid barium-zinc stabilizer in an amount of at least 0.01 phr, more preferably at least 0.1 phr, even more preferably at least 0.5 phr, most preferably at least 0.75 phr. Further, the first wear layer 10A and the second wear layer 10B comprise a phosphite costabilizer in an amount of at least 0.05 phr, more preferably at least 0.2 phr, even more preferably at least 0.5 phr or 1 phr. The inventors found that this combination of stabilizers in a first wear layer 10A and a second wear layer 10B provides excellent results in terms of transparency, thermal stability, and adherence to the lacquer layer. Preferably, the thickness of the first wear layer 10A and the thickness of the second wear layer 10B are substantially equal, for example the first wear layer 10A has a thickness of 0.3 mm and the second wear layer 10B has a thickness of 0.2 mm or 0.22 mm. The wear layer 10, more particularly the first wear layer 10A and / or the second wear layer 10B, may further comprise UV absorbers, antioxidants and / or hindered amine light stabilizers.

[0123] The lacquer layer 11 of the example comprises or consists of polyurethane, preferably a UV cured or UV curable polyurethane. The lacquer layer 11 preferably has a gloss level measured at an angle of 85° of at most 10, preferably at most 6, more preferably at most 3, most preferably at most 2 and / or a gloss level measured at an angle of 60° of at most 10, preferably at most 6, more preferably at most 4, most preferably at most 3, wherein the gloss level is measured with a Rhopoint Novo-Gloss 20 / 60 / 85 glossmeter. Such low gloss levels beneficially allow the decor of the finishing layer 6 to be perceived the same from different angles of observation, thus providing a more realistic impression. In the example, the lacquer layer 11 comprises one or more from the list of matting agents, viscosity controlling agents, and photo-initiators. The lacquer layer 11 has a thickness of up to 10 micrometer, preferably up to 20 micrometer, more preferably up to 30 micrometer. The lacquer layer 11 may further comprise UV absorbers, antioxidants and / or hindered amine light stabilizers. Preferably, the lacquer layer 11 is cured by a type of UV radiation other than excimer radiation, for example by radiation from a Mercury UV lamp. The lacquer layer 11 is preferably essentially free from micro-wrinkles.The substrate 5 of the example of Figures 1-3 comprises, from bottom to top, a backing layer 13, a second PVC layer 14 and a reinforcing layer 15 impregnated with a first PVC layer.

[0124] The backing layer 13 of the example is preferably a textile backing layer with a weight per unit area of at least 30 g / m2, preferably at least 60 g / m2, more preferably at least 100 g / m2, for example 120 g / m2. Alternatively, the backing layer 13 may be or may comprise a layer of flexible or semi-rigid PVC. In this case, the backing layer 13 may comprise fillers in an amount of up to 30 wt%, preferably up to 50 wt% or up to 60 wt%.

[0125] The second PVC layer 14 is arranged on top of the backing layer 13, and is a layer of foamed, flexible PVC. The foam is preferably foam with closed cells. The second PVC layer 14 may comprise plasticizer in an amount of at least 50 phr plasticizer, preferably at least 60 phr, or even at least 70 phr. The second PVC layer 14 may further comprise fillers in an amount of at least 10 wt%, preferably at least 30 wt%, more preferably at least 50 wt% or 60 wt%, and / or in an amount of at least 90 phr, preferably at least 100 phr, more preferably at least 120 phr. Preferably, said fillers for the second PVC layer 14 comprise a biofiller such as an egg shell-based filler. The second PVC layer 14 is preferably applied as a PVC plastisol layer, and preferably has a thickness between 0.5 and 3 mm, for example 1 mm.

[0126] The reinforcing layer 15 is preferably a glass-fiber fleece or cloth with a weight per unit area of between 10 and 150 g / m2, preferably between 20 and 100 g / m2, for example 40 g / m2. The first PVC layer impregnating the reinforcing layer 15 is a layer of unfoamed, flexible PVC and may have a plasticizer content of at least 50 phr plasticizer, preferably at least 60 phr, or even at least 70 phr. The first PVC layer may further comprise fillers in an amount of at least 10 wt%, preferably at least 30 wt%, more preferably at least 50 wt% or 60 wt%, and / or in an amount of at least 90 phr, preferably at least 100 phr, more preferably at least 120 phr. The first PVC layer is preferably applied as a PVC plastisol layer. Preferably, the combined thickness of the first PVC layer and the reinforcing layer 15 is between 0.2 and 0.6 mm, preferably between 0.25 and 0.5 mm, for example 0.35 mm.Preferably, the decorative covering element 1 comprises a migration barrier (not shown) in accordance with the sixth independent aspect of the invention. For example, the migration barrier may be a layer comprising a composition comprising lamellar fillers in accordance with the fifth particular embodiment of the sixth independent aspect. Preferably, said layer comprising a composition comprising lamellar fillers is a coating on top of the print layer 7, and possibly on top of and / or below one or more layers of the one or more flexible or semi-rigid synthetic material layers 14, 15. Said lamellar fillers preferably have a diameter - or equivalent diameter - of between 3 and 5 micrometer and a thickness of between 0.9 and 1 nanometer. The lamellar fillers are preferably claybased and have a residual moisture content of at most 5%, preferably at most 1%. Said composition comprising lamellar fillers preferably comprises a dispersing agent in an amount between 1 and 20 wt%, a plasticizer in an amount between 20 and 70 wt%, and lamellar fillers in an amount of at most 20 wt%. The plasticizer is preferably selected from DOTP and DINCH. The dispersing agent is preferably a dispersing agent described in relation to the fifth practical embodiment of the sixth independent aspect of the invention. Preferably, the coating has a thickness between 2 and 25 micrometer, preferably between 5 and 15 micrometer.

[0127] Preferably, the decorative covering element comprises a calendered layer (not shown) comprising PVC between the backing layer 13 and the second PVC layer 14. The calendered layer preferably has a thickness of at most 1.5 mm, preferably at most 1 mm. The calendered layer preferably has a thickness of at least 0.5 mm, preferably at least 0.6 mm or at least 0.75 mm. Preferably, the calendered layer comprises plasticizer in an amount of at least 25 phr, more preferably at least 30 phr or at least 35 phr. Preferably, the calendered layer comprises plasticizer in an amount of at most 60 phr, more preferably at most 50 phr, more preferably at most 45 phr. Preferably the calendered layer comprises fillers, such as calcium carbonate and / or chalk, in an amount of at most 350 phr, more preferably at most 300 phr, even more preferably at most 275 phr or at most 265 phr. Preferably the calendered layer comprises fillers, such as calcium carbonate and / or chalk, in an amount of at least 150 phr, more preferably at least 200 phr, even more preferably at least 225 phr or at least 245 phr.The decorative covering element 1 may have a weight per unit area between 1500 g / m2and 3000 g / m2, preferably, between 1900 g / m2and 2600 g / m2, such as between 2050 g / m2and 2500 g / m2. The decorative covering element 1 of the example has a thickness T between 1 mm and 8 mm, preferably between 1 and 6 mm, more preferably between 1.5 and 4 mm, for example about 2 mm.

[0128] The decorative covering element 1 may be a floor covering element, a wall covering element or a ceiling covering element.

[0129] Figures 4 to 7 show alternative embodiments for the finishing layer 6 described in relation to Figures 1-3. In Figure 4, the finishing layer 6 consists of a print layer 7, a wear layer 10 and a lacquer layer 11. The print layer 7 is identical to the print layer of Figures 1-3. The wear layer 10 of the example of Figure 4 consists of only one layer. In this example, the wear layer 10 has a thickness between 0.12 and 0.8 mm, preferably between 0.2 and 0.6 mm. The wear layer 10 is free from fillers. The wear layer 10 comprises flexible PVC, and possibly one or more of epoxidized soybean oil, phosphites, calciumzinc stabilizers and barium-zinc stabilizers, preferably at least a calcium-zinc stabilizer. The wear layer 10 preferably further comprises UV absorbers, antioxidants and / or hindered amine light stabilizers. The lacquer layer 11 of this example consists of a UV cured polyurethane, and possibly comprises UV absorbers, antioxidants and / or hindered amine light stabilizers. The lacquer layer 11 has a thickness of up to 10 micrometer, preferably up to 20 micrometer, more preferably up to 30 micrometer. This example provides a finishing layer 6 with a deep white color, with the further benefit that the white color is well maintained throughout the years thanks to the good resistance against yellowing and UV radiation of the wear layer 10 and the lacquer layer 11.

[0130] Figure 5 provides a further alternative embodiment for a finishing layer 6 according to the invention. The example of Figure 5 differs from the example of Figure 4 in that the print layer 7 comprises a lower amount of pigments 12, in particular titanium dioxide particles and / or white pigments other than titanium dioxide particles, in that the finishing layer 6 comprises a base ink layer 8 and one or more decorative ink layers 9 arrangedabove the base ink layer 8, and in that the finishing layer 6 does not comprise a lacquer layer 11. In this example, the base ink layer 8 is a layer of blue ink as described in relation to the example of Figures 1-3. Even though the print layer 7 has a limited whiteness, the layer of blue ink enhances the whiteness, such that the decor formed in the finishing layer 6 may still have vibrant colors with an excellent realism. The layer of blue ink further counter-balances the yellowing that may occur due to degradation over time of the PVC layers.

[0131] Figure 6 shows yet another alternative embodiment for a finishing layer 6 according to the invention, which differs from the example of Figure 5 in that the finishing layer 6 does not comprise a base ink layer 8, and in that the wear layer 10 comprises a first wear layer 10A and a second wear layer 10B. The first wear layer 10A and the second wear layer 10B in this example are identical to those described in relation to Figure 1. In this example, the print layer 7 preferably comprises the pigments that have been described in relation to the base ink layer 8 for Figures 1-3. As a result, no additional layer needs to be applied, however, the same vibrant colors an excellent realism may be obtained with this example.

[0132] Figure 7 shows an enlarged view of the finishing layer 6 as described in relation to Figures 1-3. In this figure, the relative thicknesses of the first wear layer 10A and the second wear layer 10B are different from that in Figures 1-3. In this example, the first wear layer 10A is at least 20%, preferably at least 50%, more preferably at least 100%, thicker than the second wear layer 10B. For example, the first wear layer 10A may have a thickness of 0.4 mm whereas the second wear layer 10B has a thickness of 0.15 mm or 0.2 mm. This provides an excellent balance between optimal transparency and thermal stability on the one hand, and sufficient adherence for the lacquer layer 11 on the other hand.

[0133] It is clear that, although several embodiments and / or materials for providing embodiments in accordance with the present invention have been discussed, various amendments or modifications can be applied without deviating from the scope of this invention as defined by the claims. The present invention is by no means limited to theembodiments described above, but can be realized in accordance with different variants without departing from the scope of the present invention.

Claims

Claims1.- A finishing layer (6) for a decorative covering element (1) comprising a print layer (7), wherein the print layer (7) comprises at least synthetic material and pigments (12), wherein said synthetic material is preferably thermoplastic material, characterized in that said pigments (12) are titanium dioxide particles or white pigments other than titanium dioxide particles, wherein the print layer (7) comprises said pigments (12) in an amount of at least 5 phr, preferably at least 7.5 phr, more preferably at least 10 phr, even more preferably at least 12.5 phr.2.- The finishing layer of claim 1, wherein the synthetic material is or comprises PVC, preferably flexible PVC.3.- The finishing layer of any one of the claims 1 to 2, wherein the synthetic material comprises fillers, preferably in an amount above 10 wt%, more preferably above 40 wt%.4.- The finishing layer of claim 3, wherein the fillers comprise inorganic fillers such as talcum, calcium carbonate, lime and / or chalk.5.- The finishing layer of any one of the preceding claims, wherein the print layer (7) has a thickness of at least 0.05 mm, preferably at least 0.15 mm, more preferably at least 0.2 mm.6.- The finishing layer of any one of the preceding claims, wherein the print layer (7) comprises one or more components selected from the list of phosphite, barium-zinc stabilizer, calcium -zinc stabilizer and epoxidized soybean oil.7.- The finishing layer of any one of the preceding claims, wherein the finishing layer (6) comprises one or more decorative ink layers (9) above the print layer (7).8.- A finishing layer (6) for a decorative covering element (1) comprising a print layer (7), characterized in that the finishing layer (6) further comprises a base ink layer (8) above, preferably directly above, the print layer (7), wherein the base ink layer (8) is a layer of ink, preferably a layer of blue ink.9.- The finishing layer of claim 8, wherein the finishing layer (6) is a finishing layer (6) in accordance with any one of the claims 1 to 7.10.- The finishing layer of claim 8 or 9, wherein the base ink layer (8) covers at least 25%, preferably at least 50%, more preferably at least 75%, most preferably at least 95%, of the entire surface area of the print layer (7).11.- The finishing layer of any one of the claims 8 to 10, wherein the base ink layer (8) comprises a water-based ink.12.- The finishing layer of any one of the claims 8 to 11, wherein the ink is or comprises a pigmented ink.13.- The finishing layer of claim 12, wherein the pigmented ink comprises one or more pigments selected from C.I. Pigment Blue 15:1, C.I. Pigment Blue 15:3, C.I. Pigment Blue 15:4, C.I. Pigment Blue 29, C.I. Pigment Blue 60, C.I. Pigment Violet 19, C.I. Pigment Violet 23, C.I. Pigment Violet 32, C.I. Pigment Red 122.14.- The finishing layer of claim 12 or 13, wherein the base ink layer (8) comprises said pigmented ink in an amount of at most 2 wt%, preferably at most 0.5 wt%, more preferably at most 0.1 wt%, even more preferably at most 0.05%.15.- The finishing layer of any one of the claims 8 to 14, wherein the ink comprises an acrylate-based binder.16.- The finishing layer of any one of the claims 8 to 15, wherein the finishing layer (6) comprises one or more decorative ink layers (9) above said base ink layer (8).17.- The finishing layer of any one of the preceding claims, wherein the finishing layer (6) comprises a wear layer (10) arranged above the print layer (7), above the possible base ink layer (8) and above the possible one or more decorative ink layers (9), wherein the wear layer (10) has a thickness of at least 0.15 mm, preferably of at least 0.4 mm, more preferably of at least 0.5 mm.18.- The finishing layer of claim 17, wherein the wear layer (10) is free from fillers.19.- The finishing layer of any one of the claims 17 or 18, wherein the wear layer (10) is translucent or transparent.20.- The finishing layer of any one of the claims 17 to 19, wherein the wear layer (10) comprises flexible or semi-rigid thermoplastic material, preferably flexible or semi-rigid PVC.21.- The finishing layer of any one of the claims 17 to 20, wherein the wear layer (10) comprises epoxidized soybean oil.22.- The finishing layer of any one of the claims 17 to 21, wherein the wear layer (10) comprises one or more UV absorbers and / or one or more radical scavengers.23.- A finishing layer (6) for a decorative covering element (1) comprising a print layer (7) and a wear layer (10) arranged above said print layer (7), characterized in that the wear layer (10) comprises a calcium-zinc stabilizer.24.- The finishing layer of claim 23, wherein the finishing layer (6) is a finishing layer (6) in accordance with any one of the claims 1 to 22.25.- The finishing layer of claim 23 or 24, wherein the calcium-zinc stabilizer is or is obtained from a solid calcium-zinc stabilizer.26.- The finishing layer of any one of the claims 23 to 25, wherein the wear layer (10) comprises a first wear layer (10A) arranged above the print layer (7) and a second wear layer (10B) arranged above the first wear layer (10B), wherein at least the first wear layer (IOA) comprises said calcium-zinc stabilizer.27.- The finishing layer of claim 26, wherein the first wear layer (10A) comprises said calcium-zinc stabilizer in an amount of at least 0.2 phr, preferably at least 0.5 phr, more preferably at least 1.5 phr, even more preferably at least 2.5 phr or 3 phr.28.- The finishing layer of claim 26 or 27, wherein the first wear layer (10A) and / or the second wear layer (10B) comprises a synthetic material, preferably a thermoplastic material such as PVC.29.- The finishing layer of any one of the claims 26 to 28, wherein the second wear layer (IOB) is free or essentially free from calcium-zinc stabilizer.30.- The finishing layer of any one of the claims 26 to 29, wherein the second wear layer (10B) comprises a barium-zinc stabilizer, preferably in an amount of at least 0.01 phr,more preferably at least 0.1 phr, even more preferably at least 0.5 phr, most preferably at least 0.75 phr.31.- The finishing layer of claim 30, wherein the barium-zinc stabilizer is a liquid bariumzinc stabilizer.32.- The finishing layer of any one of the claims 26 to 31, wherein the first wear layer (10A) and / or the second wear layer (10B) comprises a phosphite costabilizer, preferably in an amount of at least 0.05 phr, more preferably at least 0.2 phr, even more preferably at least 0.5 phr or 1 phr.33.- The finishing layer of any one of the claims 26 to 32, wherein the thickness of the first wear layer (10A) and the thickness of the second wear layer (10B) are substantially equal.34.- The finishing layer of any one of the claims 26 to 32, wherein the first wear layer (10A) is thicker than the second wear layer (10B), preferably at least 10% thicker, more preferably at least 20% thicker, even more preferably at least 30% thicker, most preferably at least 50% thicker than the second wear layer (10B).35.- The finishing layer of any one of the claims 17 to 34, wherein the finishing layer (6) comprises a lacquer layer (11) arranged on top of the wear layer (10), wherein the lacquer layer (11) preferably comprises or consists of polyurethane, preferably a UV cured or UV curable polyurethane.36.- The finishing layer of claim 35, wherein the lacquer layer (11) has a thickness of up to 10 micrometer, preferably up to 20 micrometer, more preferably up to 30 micrometer.37.- The finishing layer of claim 35 or 36, wherein the lacquer layer (11) comprises one or more UV absorbers and / or one or more radical scavengers.38.- A finishing layer (6) for a decorative covering element (1) comprising a print layer (7), a wear layer (10) arranged on said print layer (7) and a lacquer layer (11) arranged on said wear layer (10) at the side opposite the print layer (7), characterized in that the lacquer layer (11) has a gloss level measured at an angle of 85° of at most 10, preferably at most 6, more preferably at most 3, most preferably at most 2 and / or a gloss level measured at an angle of 60° of at most 10, preferably at most 6, more preferably at most 4, most preferably at most 3, wherein the gloss level is measured with a Rhopoint Novo-Gloss 20 / 60 / 85 glossmeter.39.- The finishing layer of claim 38, wherein the finishing layer (6) is a finishing layer (6) in accordance with any one of the claims 1 to 37.40.- The finishing layer of claim 38 or 39, wherein the lacquer layer (11) comprises one or more from the list of matting agents, viscosity controlling agents, and photo-initiators.41.- The finishing layer of any one of the claims 38 to 40, wherein the lacquer layer (11) is cured by a type of UV radiation other than excimer radiation.42.- The finishing layer of claim 41, wherein the lacquer layer (11) is essentially free from micro-wrinkles.43.- A decorative covering element (1), preferably a floor or wall covering element, wherein the decorative covering element (1) comprises a substrate (5) and a finishing layer (6) attached to the substrate (5), characterized in that the finishing layer (6) is a finishing layer (6) as in any one of the preceding claims.44.- The decorative covering element of claim 43, wherein the substrate (5) comprises one or more flexible or semi-rigid synthetic material layers (14), preferably thermoplastic material layers such as PVC layers.45.- The decorative covering element of claim 44, wherein the flexible or semi-rigid PVC layer or layers comprise a reinforcing layer (15), for example a textile reinforcing layer, for example a glass-fiber fleece or cloth.46.- The decorative covering element of claim 44 or 45, wherein the flexible or semirigid PVC layer (14) comprises fillers in an amount of at least 10 wt%, preferably at least 30 wt%, more preferably at least 50 wt% or 60 wt%.47.- The decorative covering element of any one of the claims 43 to 46, wherein the substrate (5) further comprises a backing layer (13), wherein the backing layer (13) preferably comprises or consists of a layer of synthetic material, preferably a layer of thermoplastic material, for example flexible or semi-rigid PVC.48.- A decorative covering element, possibly in accordance with any one of the claims 43 to 47, preferably a floor or wall covering element, wherein the decorative covering element comprises a substrate and a finishing layer attached to the substrate, characterized in that the decorative covering element comprises a migration barrier.49.- The decorative covering element of claim 48, wherein the substrate comprises one or more flexible or semi-rigid synthetic material layers and / or a backing layer.50.- The decorative covering element of claim 48 or 49, wherein the migration barrier comprises one or more of the following features:- the migration barrier is a coating comprising polyvinyl alcohol (PVOH), wherein one or more of the layers of the decorative covering element is provided with said coating;- the migration barrier is a coating comprising a modified polyvinyl alcohol (modified PVOH), wherein one or more of the layers of the decorative covering element is provided with said coating;- the migration barrier is a coating comprising an ethylene vinyl alcohol (EVOH) or a modified ethylene vinyl alcohol (modified EVOH), wherein one or more of the layers of the decorative covering element is provided with said coating; - the migration barrier is a coating comprising polyacrylic acid, polyaspartic acid, acrylic copolymers - such as ethylene acrylic acid copolymer (EAA) or ethylene methacrylic acid copolymer (EMAA) -, and / or polyvinylidene chloride (PVDC), wherein one or more layers of the decorative covering element is provided with said coating;- the migration barrier is a layer comprising a composition comprising lamellar fillers, preferably said lamellar fillers having an aspect ratio of at least 500, preferably at least 1000, more preferably at least 3000, even more preferably at least 4000, most preferably at least 5000 or at least 6000;the migration barrier is a layer comprising barrier fillers;- the migration barrier is a reinforcing layer comprising reinforcing material and a binder;- the migration barrier is a calendered layer;- the migration barrier is a thermoplastic layer comprising plasticizer in an amount below 50 phr, preferably below 30 phr, more preferably below 20 phr, even more preferably below 10 phr or below 5 phr, wherein the migration barrier is arranged below the print layer.51 A decorative covering element, preferably a floor or wall covering element, wherein the decorative covering element comprises a substrate and a finishing layer attached to the substrate, wherein the substrate comprises a calendered layer comprising thermoplastic material, with the characteristic that the thermoplastic material of the calendered layer comprises recycled thermoplastic material.52.- The decorative covering element of claim 51, wherein the decorative covering element is in accordance with any one of the claims 43 to 50.53.- A method for manufacturing a decorative covering element, preferably a floor or wall covering element, wherein the decorative covering element comprises a substrate and a finishing layer attached to the substrate, wherein the substrate comprises a calendered layer comprising thermoplastic material, wherein the method comprises at least the steps of:providing thermoplastic material, preferably PVC;- providing recycled thermoplastic material, preferably recycled PVC;mixing the thermoplastic material with the recycled thermoplastic material to form a mixture;optionally adding plasticizer and / or fillers and / or additives to the mixture; forming a calendered layer from said mixture;- arranging a finishing layer above said calendered layer.54.- The method of claim 53, wherein the decorative covering element is a decorative covering element in accordance with claim 51 or 52.