laminate
High viscosity resins applied as coatings on laminate sheets before pressing address formaldehyde emissions and safety risks in laminate production, achieving efficient and safe laminate manufacturing with improved bonding and reduced delamination.
Patent Information
- Application Number
- PCT/IB2026/054386
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2026-03-18
- Filing Date
- 2026-05-04
- Publication Date
- 2026-11-12
AI Technical Summary
Existing laminates, particularly those using melamine and phenol formaldehyde resins, contribute to formaldehyde emissions and pose safety risks during production and use, and their production can be challenging.
The use of high viscosity resins, such as those with viscosities of at least 50 mPa s at 20 °C and 1.013 bar, applied as coatings on laminate sheets before pressing, eliminates the need for impregnation baths and ensures sufficient bonding without delamination, using protein-containing components like flour or lignin-based resins.
This method produces laminates with reduced formaldehyde emissions, improved safety, and enhanced production efficiency by ensuring even resin distribution and internal bonding, thus minimizing delamination risks.
Smart Images

Figure IB2026054386_12112026_PF_FP_ABST
Abstract
Description
[0001] Laminate
[0002] The present invention relates to laminates. Said laminates are made up of at least two sheets which are laminated together with one or more resins. More in particular, said invention relates to High Pressure Laminates (HPL). When said HPL are produced in a continuous manner, these HPL can be indicated as continuously Pressed Laminates (CPL). HPL / CPL are used among other things in the production of furniture, e.g. kitchen furniture and cabinets, and this to form a decorative surface. HPL and CPL can also be used for the production of floor panels or wall panels. Said invention also relates to compact laminate. Compact laminate is preferably entirely assembled from paper / cardboard and one or more resins and optionally one or more lacquers. Said invention can also relate to Direct Pressure Laminates (DPL), which comprise a substrate, such as a particle board substrate or a wood fiber substrate, and two or more sheets laminated to said substrate. Said laminate can also be an edge tape / edge band for taping / edgebanding the edges of panels, e.g. for edgebanding the edges of panels comprising a substrate upon which preferably a HPL / CPL is glued.
[0003] The laminates can possess additional features such as flame-retardant properties, waterproof properties and anti-static properties.
[0004] High Pressure Laminates (HPL) are built up from several sheets, preferably resin-impregnated sheets. HPL is produced by pressing the various layers of the HPL together under temperature and pressure, which results in curing of the resin. HPL is glued on substrates by means of a suitable glue. The HPL is for example glued on a chipboard (also indicated as particle board), MDF (Medium Density Fiberboard) or HDF (High Density Fiberboard), plywood or on boards that comprise several sheets of paper / cardboard impregnated with for example a phenol-formaldehyde resin and that have been pressed together. A suitable glue must be selected, depending on the type of substrate.In the case of Direct Pressure Laminates (DPL), layers similar to layers used in the production of HPL, for example resin-impregnated papers, are pressed directly under temperature and pressure on a substrate. The mutual bonding of the various layers occurs at the same moment, by means of the resin that the layer or layers of the DPL comprise.
[0005] Compact laminate is preferably constructed with layers of resin-impregnated kraft papers which are sandwiched between resin-impregnated decorative papers, e.g. printed papers and / or dyed papers and / or papers with a uniform color, and which are optionally further sandwiched between protective layers, e.g. wear layers, such as resin-impregnated papers and / or lacquer layers and / or UV-cured layers. Said different layers are pressed together to form said compact laminate.
[0006] For the above-mentioned laminates, resins comprising formaldehyde, such as melamine resins (melamine formaldehyde resins, MF resins) and / or phenol resins (phenol formaldehyde resins, PF resins) are often used. The drawback of said resins is that they can be the cause of high formaldehyde emissions and / or use of said resins during production poses safety risks. Formaldehyde-free resins have been and are being sought for the production of above-mentioned laminates. Melamine-free resins and also phenol-free resins have been and are being sought for the production of above-mentioned laminates. These formaldehyde-free resins and / or melamine-free resins often have drawbacks with regard to MF resins or PF resins. For example production can be more challenging and / or the characteristics of the produced laminate can be inferior.
[0007] One aim of the invention is to have laminates that solve one or more of the abovementioned problems. It is a specific aim to have laminates that do not contribute to formaldehyde emissions and which do not entail safety risks during production or during use of said laminates. Preferably said laminates comprise at least one resin which is free from formaldehyde and / or melamine and / or phenol, and this with the laminates still having the desired properties. One aim of the invention is to have methods for manufacturing a laminate, wherein the production is less challenging.The invention, according to a first aspect, relates to a method for manufacturing a laminate, said laminate being made up of at least two sheets which are laminated together with one or more resins, wherein at least one of said one or more resins is a first resin, said first resin preferably having a viscosity of at least 50 mPa s, at 20 °C and 1.013 bar, wherein the method comprises a lamination step wherein a stack of at least two or more sheets is formed and pressed together to laminate said sheets together, wherein at least one of said two or more sheets in said stack, has a side coated with said first resin, said side preferably facing a subsequent sheet in said stack. To produce laminates comprising two or more sheets which have been laminated together by means of one or more resins, said sheets are normally impregnated with a respective said resin, after which a stack is formed comprising resin-impregnated sheets. The limitation of this, is that impregnation equipment, such as impregnation baths are needed, and also that only use can be made of resins which are able to impregnate paper by using an impregnation bath and / or that use should be made of specific impregnation conditions. By coating said at least one of said two or more sheets with said first resin, the need of impregnating said sheet before forming said stack becomes redundant. Surprisingly it was found that a high viscosity resin, for example having a viscosity of at least 50 mPa s at 20°C and 1,013 bar, can be used to coat a said sheet before forming said stack and still said high viscosity resin is able to connect with another sheet during said pressing to form a laminate having a sufficient internal bond and which is not sensitive to delamination. Further it was found that a said high viscosity resin can be well applied evenly to said sheet and remain its position until the pressing starts, as such resulting in good quality laminate. Surprisingly, it was also found that said first resin, as a result of the pressing conditions, can at least partially impregnate a said sheet. After coating a said side of the sheet with the first resin, said first resin, before said lamination step, can be partially cured to bring it in a so-called B-stage. To bring the first resin in said B-stage, use can made of heat, for example use can made of an oven or radiation, e.g. near infrared radiation. However, said partially curing can also be omitted and is preferably omitted.
[0008] Preferably said first resin has a viscosity of at least 50 mPa s, at 20 °C and 1.013 bar, more preferably at least 100 mPa s, at 20 °C and 1.013 bar, most preferably at least 500mPa s, at 20 °C and 1.013 bar. The first resin can have a viscosity of at least 1000 mPa s, or at least 2000 mPa s or at least 5000 mPa s, at 20 °C and 1.013 bar.
[0009] In a preferred embodiment both opposite sides of at least one of said two or more sheets in said stack is coated with said first resin. By coating said two sides of at least one sheet, sufficient resin is present for also partially impregnating said sheet, preferably for even fully impregnating said sheet. The risk of delamination is thus lowered. Further because of said high viscosity, it is also possible to coat said side of the sheet facing downwards and this without the risk of the first resin coming loose during formation of said stack.
[0010] In a very preferred embodiment the first resin comprises a protein-containing component, said protein-containing component being for example flour or blood meal. Proteincontaining components are bio-based and free from melamine, phenol and formaldehyde. However proteins tend to increase the viscosity. Since said first resin is coated, said higher viscosity is no longer a problem and protein-containing resins, for example protein-based resins, can be used to manufacture said laminates in an efficient manner.
[0011] Further preferably, the dry matter weight of said first resin comprises at least 30 wt% of said protein-containing component, preferably at least 50 wt%. The first resin can then be indicated as a protein-based resin.
[0012] In an embodiment said first resin comprises lignin. Said first resin can be a lignin-based resin. Preferably said lignin-based resin is free from phenol. Preferably said lignin-based resin is free from melamine and formaldehyde. Preferably the dry matter weight of said first resin comprises at least 30 wt% of lignin, preferably at least 50 wt%.
[0013] In an embodiment, said first resin comprises a yeast.
[0014] In an embodiment the first resin is a water-based epoxy resin or a water-based polyurethane resin, said resin comprising bio-based fillers, wherein said bio-based fillers are insoluble in water and have an average particle size D90 value by mass of between 10 and 1000 μm. The average particle size D90 values are preferably smaller than 1000pm, more preferably smaller than 700 pm. The average particle size D90 values can be between 100 μm and 500 μm. The average particle size can be measured by various techniques known in the art. Particularly for larger granules, the particle size can possibly be determined by sieving techniques, for example as described in EN 933-2:2020. The particle size of smaller particles can be determined by laser granulometry, in particular, the median particle size D90 may be determined using laser granulometry, which may be performed in accordance with ISO 13320:2020.
[0015] The bio-based fillers are preferably of vegetable, microbial or animal origin. Nonlimiting examples of vegetable fillers are lignocellulosic by-products of oil pressing (press cakes from for example sugar beets or beer manufacturing), wood flour, bark, straw of various grains, flax shives, leaves, seeds. Non-limiting examples of microbial fillers are microalgae, activated sludge, microbial waste of fermentation processes. Nonlimiting examples of animal fillers are bone meal, fish scales, fish bones, exoskeletons of crustaceans and insects. Preferably, the various fillers are not soluble in water or oil and they are available in granular form.
[0016] In a preferred embodiment
[0017] -a discontinuous press, such as a single daylight press or a multidaylight press, is used for pressing together to laminate said sheets together, wherein pressing takes place at a maximum temperature of at least 150 °C, preferably at least 160 °C, more preferably at least 180° and most preferably at least 200 °C, and a maximum pressure of at least 40 kg / cm2, preferably at least 60 kg / cm2, more preferably at least 60 kg / cm2, most preferably at least 80 kg / cm2, for example 100 or 120 kg / cm2, and wherein the pressing has a duration of at least 30 seconds, for example 3 minutes, or;
[0018] -a continuous press, such as a double belt press, is used for pressing together to laminate said sheets together, wherein pressing takes place at a maximum temperature of at least 150 °C, preferably at least 190 °C, more preferably at least 200 °C, for example 195 °C or 220 °C or 240 °C, and a maximum pressure of at least 25 kg / cm2, preferably at least 40 kg / cm2, more preferably at least 60 kg / cm2, for example 70 or 90 or 110 kg / cm2, and wherein the pressing has a duration of at least 30 seconds, preferably at least 1 minute, more preferably at least 3 minutes.It has been found that with such pressing conditions, the first resin coated on a said side of the sheet, has sufficient time and flowability to be pressed by said press into the sheet, such as to impregnate said sheet, resulting in a good quality laminate.
[0019] The invention according to a second aspect is a method for manufacturing a laminate, said laminate being made up of at least two sheets which are laminated together with one or more resins, wherein at least one of said one or more resins is a first resin, said first resin being an emulsion comprising particles and a wetting agent, wherein the method comprises a lamination step wherein a stack of at least two or more sheets is formed and pressed together to laminate said sheets together, wherein at least one of said at least two sheets has a side coated with said first resin, said side preferably facing a subsequent sheet in said stack. To produce laminates comprising two or more sheets which have been laminated together by means of one or more resins, said sheets are normally impregnated with a respective said resin, after which a stack is formed comprising resin-impregnated sheets. The limitation of this, is that impregnation equipment, such as impregnation baths are needed, and also that only use can be made of resins which are able to impregnate paper by using an impregnation bath and / or that use should be made of specific impregnation conditions. By coating said at least one of said two or more sheets with said first resin, the need of impregnating said sheet before forming said stack becomes redundant. Surprisingly it was found that said emulsions can be used to coat a said sheet before forming said stack and still said particles allow to connect with another sheet during said pressing to form a laminate having a sufficient internal bond and which is not sensitive to delamination. Further it was found that said resin can be well applied evenly to said sheet and remain its position until the pressing starts, as such resulting in good quality laminate. The wetting agent ensures that the particles are evenly spread upon the said side of the sheet. Surprisingly, it was also found that said particles of the first resin, as a result of the pressing conditions, can at least partially impregnate a said sheet.
[0020] The second aspect can also be according to the first aspect. The first resin can for example have a viscosity of at least 50 mPa s at 20 °C and 1,013 bar.Preferably both opposite sides of at least one of said two or more sheets in said stack is coated with said first resin. By coating two sides of at least one sheet, sufficient particles are present for also partially impregnating said sheet, preferably for even fully impregnating said sheet. The risk of delamination is thus lowered. Further because of said wetting agent, it is also possible to coat said side of the sheet facing downwards and this without the risk of the first resin coming loose during formation of said stack.
[0021] In a preferred embodiment the emulsion is a water-based emulsion and the D50value ofthe particle size distribution by volume of the particles in water is less than 200micrometers, preferably less than 100 micrometers, more preferably less than 50micrometers, even more preferably less than 30 micrometers. The D50value of the particle size distribution by volume can be measured by laser diffraction (Beckman Coulter laser diffraction device LS 13320). The D50value is the particle size – expressedin microns – wherein 50 % of the particles are smaller than this value. These embodiments provide better glue stability, good glue efficiency and homogeneous spreading of the particles upon said side of the sheet. A preferred embodiment of the second aspect of the invention is characterized in that the D90value of the particle sizedistribution by volume of the particles in water, measured in by laser diffraction, is lessthan 200 micrometers, preferably less than 100 micrometers. The D90value is the particlesize – expressed in microns – wherein 90 % of the particles are smaller than this value.
[0022] Preferably the wetting agent is chosen from the list of: alcohols, solvents, sulfates –such as sodium dodecyl sulfate–. For example the wetting agent can be ethanol, isopropanol, butanol or amino alcohol. The wetting agent can be a glycol ether, an acetate or acetone.
[0023] Preferably the dry matter weight of the first resin comprises at most 15 wt% wetting agent, preferably at most 3 wt%, for example between 1 and 2 wt%.
[0024] The invention according to a third aspect, relates to a method for manufacturing a laminate, said laminate being made up of at least two sheets which are laminated togetherwith one or more resins, wherein the method comprises a lamination step, said lamination step comprising:
[0025] -providing at least two sheets;
[0026] -a stacking substep wherein said at least two sheets are placed on top of each other in a continuous manner -for example wherein said two sheets are continuously unrolled on top of each other- followed by
[0027] -a pressing sub step wherein said at least two sheets which are placed on top of each other, are pressed and laminated together,
[0028] and wherein during said stacking substep, one or more sides of said sheets, are coated with a curable first resin, said first resin being cured in the pressing substep.
[0029] Preferably, between said stacking substep and said pressing substep, there is no curing of the resin, for example said resin is not exposed to heat and / or radiation before said pressing substep. Curing then only takes place in said pressing substep. The benefit here is that additional infrastructure, such as ovens and / or radiation devices, can be omitted. To produce laminates comprising two or more sheets which have been laminated together by means of one or more resins, said sheets are normally impregnated with a respective said resin and said resin is partially cured to obtain non-sticky sheets. The result is resin-impregnated sheets in the so-called B-stage. After this a stack is formed comprising only resin-impregnated sheets. The limitation of this is, that additional intermediate curing is needed and thus infrastructure such as ovens to obtain this curing. By making use of the method of the third aspect of the invention, this intermediate curing can be omitted, of course this is not excluded. When no intermediate curing is present, said curable first resin is able to penetrate the said sheet in the beginning of said pressing substep in a good manner.
[0030] The third aspect can also be according to the second aspect or the first aspect. The third aspect can also be according to the first and second aspect.
[0031] Preferably said at least two sheets are supplied on roll, wherein during said stacking substep, said sheets are unrolled and coated with said curable first resin, and placed on top of each other. This is an efficient and fast manner to coat a said sheet. Only one sideof said sheet can be coated with said curable first resin. Both said sides can also be coated with said curable first resin. If both sides are coated and / or two or more of said sheets are coated, the respective curable resins can or cannot have the same composition. If different curable resins are used having different resins, the curable resins can be Taylor-made for each respective sheet.
[0032] In a specific embodiment at least one of said provided sheets comprises a resin-impregnated sheet, wherein a said resin-impregnated sheet is or is not coated during said stacking substep. Depending on the used sheets, the position of said sheet in the laminate, the used resins, it can be desirable to provide one or more resin-impregnated sheets. In this manner one can choose between impregnation and coating and choose the most optimum way to obtain said laminate. For example the laminate can be a decorative laminate comprising a printed decorative paper and one or more structural sheets, for example kraft papers. One can for example choose to impregnate said decorative sheet with a translucent resin before said stacking substep, and to coat sides of said structural sheets with said first resin during the stacking substep. Also a resin-impregnated sheet can be coated in the stacking substep and this for example to promote adhesion with a subsequent sheet.
[0033] In a specific embodiment at least one of said provided sheets is a sheet free from resin, wherein said sheet free from resin, is or is not coated during said stacking substep. As stated above one can choose between impregnation and coating and choose the most optimum way to obtain said laminate. By coating a sheet free from resin, it is also ensured that this sheet will adhere well to another sheet or to two other sheets.
[0034] In an embodiment the laminated together sheets are rolled up forming a laminate on roll, or are cutted into smaller sheets of laminate.
[0035] A said sheet can be a paper, a cardboard, a veneer, a textile or a glass fiber scrim.
[0036] In a preferred embodiment at least two sheets which are subsequently unrolled on top of each other in said stacking substep, are resin-impregnated sheets, which are impregnatedwith a type of resin which differs from the first resin, wherein during said stacking substep, at least one side of said at least two sheets facing each other, is coated with said curable first resin. By having different resins, resins for impregnating and resins for coating, one can also provide the laminate with desired features. For example said first resin can comprise flame-retardant additives, water resistant additives and / or antimicrobial additives and this to respectively provide the laminate with fire-resistant, water resistant and / or antimicrobial properties.
[0037] The invention according to a fourth aspect relates to a method for manufacturing a laminate, said laminate being made up of at least two sheets which are laminated together with one or more resins, wherein at least one of said one or more resins is a first resin, said first resin preferably having a viscosity of at least at least 50 mPa s, at 20 °C and 1.013 bar, wherein the method comprises an impregnation step wherein at least one of said two sheets is impregnated with said first resin by vacuum and / or by pressure to form an resin-impregnated sheet, wherein a stack is formed and pressed together to laminate said sheets together, wherein said stack comprises at least said resin-impregnated sheet. With vacuum and / or by pressure, for example by pressing said at least one sheet in the presence of said first resin, said first resin, despite its high viscosity, can impregnate said sheet.
[0038] The fourth aspect can also be according to one or more of the first, second or third aspect. For example some sheets can be coated with a said resin, while other sheets are impregnated by vacuum and / or pressure with a said resin. It is also possible that a said sheet is impregnated with a said resin by vacuum and / pressure and further coated with the same or another resin.
[0039] Preferably said first resin has a viscosity of at least 50 mPa s, at 20 °C and 1.013 bar, more preferably at least 100 mPa s, at 20 °C and 1.013 bar, most preferably at least 500 mPa s, at 20 °C and 1.013 bar. The first resin can have a viscosity of at least 1000 mPa s, or at least 2000 mPa s or at least 5000 mPa s, at 20 °C and 1.013 bar.In an embodiment the first resin comprises a protein-containing component, said proteincontaining component being for example flour or blood meal. Protein-containing components are bio-based and free from melamine and formaldehyde. However proteins tend to increase the viscosity. Since said first resin is applied trough vacuum and / or pressure for impregnation said sheet, said higher viscosity is no longer a problem and protein-containing resins, for example protein-based resins, can be used to manufacture said laminates in an efficient manner.
[0040] Further preferably the dry matter weight of said first resin comprises at least 30 wt% of said protein-containing component, preferably at least 50 wt%. The first resin can then be indicated as a protein-based resin.
[0041] In a specific embodiment said first resin comprises lignin. Said first resin can be a ligninbased resin. Preferably said lignin-based resin is free from phenol. Said lignin-based resin is preferably free from melamine and formaldehyde.
[0042] In an embodiment, said first resin comprises a yeast.
[0043] The first resin can also be a water-based epoxy resin comprising bio-based fillers or a water-based polyurethane resin comprising bio-based fillers, wherein said bio-based fillers are insoluble in water and have an average particle size D90 value by mass of between 10 and 1000 μm. The bio-based fillers are preferably of vegetable, microbial or animal origin. Non-limiting examples of vegetable fillers are lignocellulosic by-products of oil pressing (press cakes from for example sugar beets or beer manufacturing), wood flour, bark, straw of various grains, flax shives, leaves, seeds. Non-limiting examples of microbial fillers are microalgae, activated sludge, microbial waste of fermentation processes. Non-limiting examples of animal fillers are bone meal, fish scales, fish bones, exoskeletons of crustaceans and insects. Preferably, the various fillers are not soluble in water or oil and they are available in granular form.
[0044] The invention according to a fifth aspect, relates to a method for manufacturing a laminate, said laminate being made up of at least two sheets which are laminated together with one or more resins, wherein at least one of said one or more resins is a first resin,said first resin preferably having a viscosity of at least at least 50 mPa s, at 20 °C and 1.013 bar, wherein the method comprises an impregnation step wherein at least one of said two sheets is impregnated with said first resin by moving the sheet through and / or along an impregnation bath comprising said first resin, said first resin being present in said impregnation batch having a temperature of at least 30 °C, preferably at least 40 °C, more preferably at least 50 °C, wherein a stack is formed and pressed together to laminate said sheets together, wherein said stack comprises at least said resin-impregnated sheet. By raising the temperature of the first resin, the viscosity of the first resin can be lowered, and by making use of an impregnation batch, the first resin has sufficient time to impregnate said sheet. For example said sheet can be guided into the first resin present inside said impregnation bath and thus pass through the first resin. Additionally or alternatively the first resin can be applied to the sheet with the aid of a lick roller which is in contact with the first resin in said impregnation bath. Preferably the temperature of the first resin is at most 70 °C, such that no unwanted precuring occurs. Increasing the temperature not only aids with impregnation, but can also significantly increase impregnation speed.
[0045] The fifth aspect can also be according to one or more of the first, second, third or fourth aspect. For example some sheets can be coated with a said resin, while other sheets are impregnated by said heated first resin. It is also possible that a said sheet is impregnated with a said heated first resin and further coated with the same or another resin.
[0046] Preferably the first resin has a viscosity of at least 50 mPa s, at 20 °C and 1.013 bar, preferably of at least 100 mPa s, more preferably of at least 500 mPa s, most preferably of at least 2000 mPa s. Especially with such viscosities, raising the temperature can have a significant effect upon the speed of impregnation.
[0047] In a specific embodiment the first resin comprises a protein-containing component, said protein-containing component being for example flour or blood meal. To prevent denaturation of the proteins, the temperature of the first resin is preferably at most 60°C, more preferably at most 50 °C.Further preferably the dry matter weight of said first resin comprises at least 30 wt% of said protein-containing component, preferably at least 50 wt%.
[0048] In a specific embodiment said first resin comprises lignin. For example the first resin can be a lignin-based resin, which is preferably free from phenol, melamine and formaldehyde.
[0049] In an embodiment, said first resin comprises a yeast.
[0050] In an embodiment the first resin is a water-based epoxy or polyurethane resin comprising bio-based fillers, wherein said bio-based fillers are insoluble in water and have an average particle size D90 value by mass of between 10 and 1000 μm. The bio-based fillers are preferably of vegetable, microbial or animal origin. Non-limiting examples of vegetable fillers are lignocellulosic by-products of oil pressing (press cakes from for example sugar beets or beer manufacturing), wood flour, bark, straw of various grains, flax shives, leaves, seeds. Non-limiting examples of microbial fillers are microalgae, activated sludge, microbial waste of fermentation processes. Non-limiting examples of animal fillers are bone meal, fish scales, fish bones, exoskeletons of crustaceans and insects. Preferably, the various fillers are not soluble in water or oil and they are available in granular form.
[0051] The invention, according to a sixth aspect, relates to a method for manufacturing a laminate, with said laminate being made up of at least two sheets which are laminated together with one or more resins, wherein at least one of said one or more resins is a first resin, wherein the method comprises an impregnation step wherein at least one of said two sheets is impregnated with said first resin by moving the sheet through and / or along an impregnation bath comprising said first resin for forming a resin-impregnated sheet, and wherein said method subsequently comprises a coating step wherein said resin-impregnated sheet is coated with said first resin for forming a coated resin-impregnated sheet, wherein a stack is formed and pressed together to laminate said sheets together, wherein said stack comprises at least said coated resin-impregnated sheet, wherein one or more of the following features are preferably present:- said first resin being present in said impregnation batch has a temperature of at least 30 °C, preferably at least 40 °C, more preferably at least 50 °C;
[0052] -a wetting agent is added to said first resin being present in said impregnation bath; -said first resin being present in said impregnation batch is diluted, preferably diluted by water.
[0053] The sixth aspect can also be according to one or more of the first, second, third, fourth or fifth aspect.
[0054] By making use of impregnation and coating, and by further taking one or more additional measures when impregnating, it can be ensured that sufficient resin can present for said sheet to form good laminates and it can be ensured that the sheet is sufficiently or even completely impregnated by said first resin. Alternatively, instead of an impregnation bath, use can also be made of vacuum / pressure to impregnate said sheet.
[0055] Said first resin preferably has a viscosity of at least 50 mPa s, at 20 °C and 1.013 bar, more preferably of at least 100 mPa s, more preferably of at least 500 mPa s, most preferably of at least 2000 mPa s.
[0056] Said first resin can comprise a protein-containing component, said protein-containing component being for example flour or blood meal. Further the dry matter weight of said first resin can comprise at least 30 wt% of said protein-containing component, preferably at least 50 wt%. Said first resin can be as described for such a resin in the other aspects of the invention.
[0057] Said first resin can comprise lignin and can be lignin-based resin as described for the other aspects.
[0058] Said first resin can comprise a yeast.
[0059] Said first resin can be a water-based epoxy or polyurethane resin comprising bio-based fillers, wherein said bio-based fillers are insoluble in water and have an average particlesize D90 value by mass of between 10 and 1000 μm. Said first resin can be as described for such a resin in the other aspects of the invention.
[0060] The invention according to a seventh aspect relates to a method for manufacturing a laminate, said laminate being made up of at least two sheets which are laminated together with one or more resins, wherein at least one of said one or more resins is a first resin, and wherein at least one of said two sheets is a paper sheet, wherein said paper sheet is treated with said first resin, for example is coated and / or impregnated with said first resin, and forms a resin-treated paper sheet, characterized in that said paper sheet has one or more of the following properties:
[0061] -a Gurley value of between 15 and 60 seconds;
[0062] -a Bendtsen roughness value of between 70 and 150 ml / min;
[0063] -a Bendtsen porosity value of between 850 and 1350 ml / min;
[0064] -a Bekk smoothness value of between 100 and 400 seconds;
[0065] -at least one smoothened surface;
[0066] -a residual moisture content of between 11 and 13 wt%;
[0067] -a weight of between 100 and 180 gsm, preferably of between 130 and 170 gsm.
[0068] Known problems with laminates is unwanted warping after production and unwanted dimpled / restless surfaces which resemble to texture of an orange peel or similar. Surprisingly the inventors found that said problems can be solved by altering the characteristics of at least one sheet used to form the laminates, especially when said paper sheets form the structural sheets of the laminate, e.g. the structural sheets of a decorative laminate comprising at least a decorative sheet and structural sheets. Especially if one wants to produce such laminates according to a continuous process, e.g. with a continuous press -for example a double belt press-, a combination of one or more of the abovementioned features has been found to show superior results.
[0069] Said method preferably comprises a lamination step wherein a stack of said sheets is formed and pressed together. Said paper sheet is preferably impregnated with said first resin, such that said resin-treated paper sheet is a resin-impregnated paper sheet.The Gurley value (value of penetrability) is preferably according to ISO 5636-5:2013. The surface roughness according to Bendtsen is preferably carried out according to ISO 8791-2. The Bendtsen porosity can be determined according to ISO 5636-3:2013. The Bekk smoothness can be determined according to ISO 5627:1995.
[0070] For example said paper sheet can be edge tape / edgebanding base paper. An edge tape / edgebanding base paper typically has at least one smoothened surface. Said smoothened surface can be obtained with the aid of a Yankee cylinder and / or a calender roller. Preferably, for said decorative laminates, at least the surface directed to said decorative sheet has been smoothened, and more preferably both said surfaces are smoothened. Further edge tape / edgebanding base paper preferably has finer fibers and a uniform fiber distribution. Said edge tape / edgebanding base paper can have a Bendtsen roughness value of between 70 and 150 ml / min and / or a Bendtsen porosity value of between 850 and 1350 ml / min. Said edge tape / edgebanding base paper preferably also has a significant flexibility.
[0071] In a preferred embodiment the first resin comprises polyamides, which are obtained by polymerization of amino acids, and further carbohydrates. Impregnating said paper sheet with said first resin, will result in laminates with less risk of unwanted warping and / or dimpled / restless surfaces.
[0072] In a preferred embodiment the laminate is a decorative laminate comprising a decorative paper and one or more structural sheets, wherein said resin-treated paper sheet forms a said structural sheet. The inventor founds that the characteristics of the structural sheets are important if one wants to avoid warping and / or dimpled / restless surfaces. For example the decorative laminate can comprise from top to bottom:
[0073] -optionally a resin-impregnated translucent paper
[0074] -a resin-impregnated decorative paper, e.g. a resin-impregnated printed paper and / or a resin-impregnated uniformly coloured paper;
[0075] -one, two, three or more resin-impregnated papers, wherein said resin is the first resin and said papers are edge tape / edgebanding base papers.The invention also relates to a laminate comprising such a specific paper sheet as structural sheet, e.g. comprising for example an edge tape / edgebanding base paper which forms a structural sheet.
[0076] The seventh aspect can also be according to one or more of the first, second, third, fourth, fifth or sixth aspect.
[0077] For all the above-mentioned aspects, said laminate can be a decorative laminate comprising a decor, wherein at least one of said two sheets is a decorative sheet comprising said decor and wherein at least one of said two sheets is a structural sheet, wherein said structural sheet of the laminate is coated and / or impregnated with said first resin. Said first resin is used to attach a said structural sheet to another sheet, for example the decorative sheet or another structural sheet. Said decor can be a printed decor. Said decor can also be a unicolor.
[0078] Further said decorative sheet can be impregnated and / or coated with a transparent resin, preferably chosen from the list of a melamine resin, an acrylate resin, polyester resin, a polyacrylate resin, or polyurethane resin.
[0079] For all the above-mentioned aspects at least one sheet can be a paper having a weight of less than 50 gsm, preferably less than 25 gsm and / or having a Gurley value of less than 15 s, preferably less than 5 s, for example less than 3 s. The Gurley value (value of penetrability) is preferably according to ISO 5636-5:2013. With the aid of thin papers and / or high permeability papers, high viscosity resins and / or resin emulsions can well penetrate said paper and provide high quality laminates, even if said resins are only present in a said stack as a coating upon a side or both sides of a said paper. Said low Gurley value is especially beneficial for structural sheets.
[0080] For all the above-mentioned aspects, said first resin can comprise flame-retardants. Said flame-retardants are preferably ammonium phosphates or ammonium sulphates. Surprisingly it was found that a mixture of ammonium polyphosphates (APP) is very suitable. Alternatively or in addition, diammonium phosphate (DAP, (NH4)2HPO4canbe used. Preferably a said first resin comprises at least 5 wt% of such flame-retardants, preferably at least 10 wt%, more preferably at least 20 wt%, based on dry matter weight.
[0081] The invention also relates to resin-treated sheets, wherein said sheets have been treated with a first resin, for example have been coated and / or impregnated with a first resin. Said first resin can be resins as described in any of the abovementioned aspects. Said treating with the first resin can be as described in the any of the above mentioned aspects. Advantages and embodiments apply mutatis mutandis for these resin-treated sheets according to the invention. Said resin-treated sheets can be used to form laminates as described above. Said resin-treated sheets can be attached to wood-based substrates such as particle boards or wood fiber boards.
[0082] For example the first resin of the resin-treated sheet can have, when applying this first resin to form said resin-treated sheet, a viscosity of at least 50 mPa s, at 20 °C and 1.013
[0083] Said first resin can comprise a protein-containing component, said protein-containing component being for example flour or blood meal.
[0084] Said first resin can comprise lignin.
[0085] Said first resin can comprise a yeast.
[0086] Said first resin can be water-based epoxy or polyurethane resin, comprising bio-based fillers, wherein said bio-based fillers are insoluble in water and have an average particle size D90 value by mass of between 10 and 1000 μm.
[0087] Said resin-treated sheet can be coated with said first resin, on one side and preferably on both sides. Said resin-treated sheet can be impregnated with said first resin. Said resin-treated sheet can be impregnated and coated with said first resin.
[0088] Said first resin can comprise a wetting agent chosen from the list of: alcohols, solvents, sulfates –such as sodium dodecyl sulfate–.Impregnating with said first resin can be done by vacuum and / or by pressure, or can be done in an impregnation bath with first resin having a temperature of at least 30°C.
[0089] Impregnation and coating with said first resin can be done, by taking specific measures for impregnating: e.g. heated first resin, adding wetting agents or diluting.
[0090] The invention also relates to the laminates made according to one or more of the first, second, third, fourth, fifth, sixth or seventh aspect. Impregnation with said first resin can be the result of said pressing, for example if said first resin during the manufacturing of the laminate is coated upon a side of a said sheet, said pressing can bring about impregnation.
[0091] Said laminates can for example comprise at least three said sheets, with from top to bottom, a first paper impregnated with a first transparent resin, one or more second papers impregnated with said first resin, and a third paper impregnated with a second transparent resin, said first and second transparent resin preferably being the same transparent resin and the one or more second papers preferably being kraft papers.
[0092] Said laminates can for example comprise from top to bottom, optionally a first transparent paper impregnated with a first transparent resin, a second decorative paper impregnated with a second transparent resin, and one or more third papers impregnated with said first resin, a fourth decorative paper impregnated with a third transparent resin, and optionally a fifth transparent paper impregnated with a fourth transparent resin, wherein said transparent resins are preferably the same transparent resins or preferably at least from the same type, and the one or more third papers preferably being kraft papers.
[0093] Said laminates can for example comprise at least three said sheets, from top to bottom, optionally a first transparent paper impregnated with a first transparent resin, a second decorative paper impregnated with a second transparent resin, and one or more third papers impregnated with said first resin, wherein said first transparent resin and saidsecond transparent resin are preferably the same resins or preferably at least resins of the same type. Said third papers are preferably kraft papers.
[0094] Said laminates can comprise from bottom to top, one or more first papers impregnated with said first resin, a second decorative paper impregnated with a first transparent resin and coated at its surface opposite said first papers with one or more transparent resins, wherein said transparent resins are preferably the same resins or at least resins of the same type.
[0095] Said laminates can comprise a core formed by at least three said sheets, said sheets preferably being paper, e.g. kraft paper, and said sheets preferably being impregnated with said first resin, and at least one top layer, said top layer comprising a digital print applied upon said core.
[0096] The laminates can comprise a top side and bottom side opposite said top side, wherein at least said bottom side or at least said top side is formed by a coating layer, wherein said coating layer is preferably chosen from the list of: primers, hotmelt glues, ethylene vinyl acetate (EVA) glue, lacquers.
[0097] Said laminates can comprise a core formed by at least three said sheets, said sheets preferably being papers, e.g. kraft papers, and said sheets preferably being impregnated with said first resin, and at least one top layer, said top layer comprising a lacquer, such as a polyurethane lacquer.
[0098] For all the above-mentioned aspects at least one sheet can be a paper having a weight of less than 50 gsm, preferably less than 25 gsm and / or having a Gurley value of less than 5 s, preferably less than 3 s. The Gurley value (value of penetrability) is preferably according to ISO 5636-5:2013. With the aid of thin papers and / or high permeability papers, high viscosity resins and / or resin emulsions can well penetrate said paper and provide high quality laminates, even if said resins are only present is a said stack as a coating upon a side or both sides of a said paper.In a specific embodiment according to one or more of the above mentioned aspects, the first resin can comprise polyamides which are obtained by polymerization of amino acids.
[0099] For one or more of the above mentioned aspects, said at least two sheets are preferably chosen from the list of papers, cardboards, textiles, glass fiber sheets. Said laminates can further comprise substrates -such as particle board and wood fiberboard-. Said at least two sheets can be the same sheets, or can be different sheets. Preferably at least one of said at least two sheets is a paper. More preferably at least one of said two sheets is a kraft paper. Preferably this kraft paper has a weight of between 80 and 300 grams per square meter (gsm), for example 120 gsm or 155 gsm or 200 gsm. Said kraft paper is preferably impregnated with said first resin. Kraft paper is often used for the production of HPL, CPL and compact laminate. For example HPL and CPL typically comprise two or three kraft papers and at least one decorative paper, wherein the kraft paper provides the HPL / CPL with the desired strength. Kraft paper is often used to form the core of a compact laminate, wherein said core then typically comprises between 5 and 40 kraft papers, for example between 10 and 20 kraft papers. Said kraft papers most often form structural sheets of the laminate. Of course other papers and / or cardboards can be used as structural sheets. Also more preferably, at least one of said two sheets is a decorative paper, e.g. a paper with a decor printed upon it and / or a paper with a uniform color and / or a dyed paper. The decorative paper is for example a white paper with a decor printed upon it or a yellow paper (or other colored paper) with a decor printed upon it, or a paper with a uniform color upon which no decor is printed. Preferably the decorative paper has a weight between 40 and 120 grams per square meter, for example 120 grams per square meter. Said decorative paper, in a said stack prior to pressing, can be impregnated with a resin and then preferably has an impregnated weight of between 120 and 300 grams per square meter, more preferably between 150 and 220 grams per square meter, for example 200 grams per square meter. Also in a specific embodiment, at least one of said two sheets is a translucent / transparent paper. Translucent and transparent are used interchangeably throughout this application. Said translucent paper is preferably part of a wear layer that is located on top of the decorative paper to protect said decorative paper. Instead of having a sheet to form an additional wear layer, said wear layer can be formedby applying one or more layers, e.g. coating one or more layers, upon the resin-impregnated decorative paper, for example by applying one or more lacquer layers and / or one or more UV-curable layers. For example such a wear layer can be formed by coating one or more acrylate resins, polyester resins and / or polyurethane resins, upon the resin impregnated decorative paper. A said wear layer can or cannot comprise hard particles, such as corundum.
[0100] With acrylate resins can be indicated polyacrylate resins. With polyester resins can be indicated unsaturated polyester resins. With melamine resins are preferably indicated melamine formaldehyde resins, but can also be indicated melamine urea formaldehyde resins.
[0101] Cardboards can be part of a compact laminate.
[0102] Textiles can be woven sheets or non-woven sheets, wherein said textiles comprise organic material, such as cotton fibers, silk fibers, flax fibers or wool, and / or comprise synthetic material, such as polyester fibers, polyamides fibers and / or comprise glass wool or rockwool.
[0103] The at least two sheets can comprise one or more glass fiber sheets (such as glass fiber scrims or nets).
[0104] Said laminate can further comprise a substrate, such as a particle board substrate or a wood fiber board substrate (such as an MDF or HDF). Preferably, if such a substrate is present, said laminate only comprises one substrate, wherein said substrate can be onelayered or multi-layered. For example, the laminate can be a DPL, for example a floor panel laminate comprising from top to bottom:
[0105] -a decorative top layer, preferably comprising a translucent paper which functions as wear layer and a printed paper which functions as a decorative layer, or preferably comprising a protective top layer, e.g. a top layer comprising one or more lacquer layers and / or one or more UV-cured acrylate / polyester layers and a printed paper which functions as a decorative layer;-a substrate, such as a wood fiber board or a particle board;
[0106] -optionally a balancing layer, said balancing layer preferably comprising a paper impregnated with said first resin.
[0107] For example the laminate can be a DPL, for example a furniture panel comprising from top to bottom:
[0108] -a decorative layer, comprising at least one paper;
[0109] -a substrate, such as a wood fiber board or a particle board;
[0110] -a decorative layer, comprising at least one paper.
[0111] Above-mentioned substrates can also comprise thermoplastic material and / or mineral fillers, such as chalk or magnesiumoxide (MgO). For example said substrate can comprise wood fibers, glue and mineral fillers such as MgO. For example said substrate can be a filled synthetic composite comprising thermoplastic material and mineral fillers and optionally plasticizers.
[0112] Pressing can occur with press elements, such as press plates and press rolls and belt presses, wherein at least one of said press elements can have a structure and this to provide laminates with the desired structure. For example, if the laminate imitates wood, it can provide a wood structure, or if the laminate imitates stone, it can provide a stone structure. To provide the laminate with the desired surface structure, alternatively, or additionally, use can be made of a structured release film / foil which is pressed together with the laminate and removed after pressing, and / or use can be made of excimer technology and / or use can be made of digital printing of a structure.
[0113] Said one or more resins can comprise only said first resin, wherein then preferably said at least two sheets have been impregnated / coated with said first resin.
[0114] The sheets are laminated together with one or more resins, wherein said one or more resins comprise a first resin. To form said laminate, said one or more resins are provided in a state wherein said one or more resins are not cured or are only partially cured. When forming said laminate, said one or more resins are cured or further cured. For example,firstly said two or more sheets are treated with said one or more resins, e.g. impregnated and / or coated with said one or more resins. Said one or more resins which are used to impregnate and / or coat said two or more sheets are then preferably uncured or with a low degree of curing. Said impregnated and / or coated sheets are then laminated together which results in further curing of the one or more resins. Here, cured resin means that the resin has undergone curing during forming of the laminate, it is sufficiently dry and it bonds the sheets together sufficiently so as to produce the desired laminate. This does not mean per se that the resin is cured completely. Here, a cured resin may or may not be a fully cured resin. If the description mentions a laminate comprising one or more resins, being a laminate which is already manufactured, said one or more resins are one or more cured resins. The laminate therefore comprises a cured first resin.
[0115] In a specific embodiment, the first resin comprises anti-static additives. Preferably the weight ratio of anti-static additives to the dry matter weight of the first resin is at most 0,03.
[0116] In a specific embodiment, the first resin comprises flame-retardants. Preferably the weight ratio of flame-retardants to the dry matter weight of the first resin is at most 0, 15, for example is 0,03.
[0117] In a preferred embodiment the first resin comprises water-repellent additives, wherein these water-repellent additives are preferably chosen from the list of
[0118] -a silicon containing compound, such as fumed silica or silanes or polysiloxanes;
[0119] -a metallic soap;
[0120] -a thermoplastic material;
[0121] -inorganic fillers such as CaCO3, talc, vermiculite.
[0122] Preferably the weight ratio of water-repellent additives to the dry matter weight of the first resin is at most 0,03. Because of said water-repellent additives, the laminate comprising said first resin can have good water resistant properties, for example can be less prone to swelling. Said thermoplastic material can be chosen from the list of polyvinyl butyral (PVB), ethylene vinyl acetate (EVA), polyvinyl alcohol (PVA), polybutylene succinate (PBS), polyvinyl chloride (PVC), polymethyl methacrylate(PMMA), polyurethane (PU), polypropylene (PP) and polyethylene (PE). Said metallic soaps preferably comprise an aliphatic chain comprising at least 8 carbons, more preferably at least 12 carbons and most preferably at least 16 carbons. More preferably said metallic soaps also comprise one, two or more shorter aliphatic chains, e.g. aliphatic chains with at most 6 carbons, preferably at most 4 carbons. Said metallic soaps can be obtained from animal fats or plant / vegetable fats. The metallic soaps are preferably zinc metallic soaps or calcium metallic soaps or magnesium metallic soaps. An example of possible metallic soaps is zinc stearate. Metallic soaps can contribute to the water resistance of a board comprising said glue, but can also enhance the soap resistance of a said board.
[0123] In a specific embodiment the first resin comprises one or more of the list of:
[0124] -pH regulators such as bases, e.g. potassium carbonate, or acids;
[0125] -dialdehydes such as glyoxal or Strecker aldehyde;
[0126] -metal ions, e.g. (Cu2+, Mg2+, Al3+, Fe3+, Ca2+);
[0127] -polyimines.
[0128] Preferably the weight ratio of above-mentioned molecules to the dry matter weight of the first resin is at most 0,03.
[0129] In a specific embodiment the first resin comprises antibacterial additives.
[0130] The above-mentioned wetting agents, water-repellent additives, anti-static additives, flame-retardant additives, antibacterial additives, pH regulators, dialdehydes, metal ions, polyimines, are all possible additives of the first resin. Of course, combinations of different additives are possible, depending on the requirement needed for said first resin. Further preferably said additives are present in amount of between 1% and 25% by weight based upon the dry matter weight of the first resin, for example 5 wt% or 15 wt%, more preferably of between 2 wt% and 3 wt%.
[0131] The first resin, when being used to make said laminate, preferably comprises water as solvent. During the coating and / or impregnation of said sheets with said first resin to form said laminate, the water ensures that said sheets are wetted, and there can be goodimpregnation of the sheets. With the aid of this first resin, the sheets can be bonded together very well, owing to the good contact between the first resin and the said sheets. Said first resin preferably has a dry matter content of between 30 and 60 wt%, for example of between 40 and 48 wt%, such that the first resin has the desired viscosity and is able to penetrate said sheet in a good manner. Of course, the laminate comprises the cured first resin, such that the dry matter content will be different for the laminate.
[0132] Preferably, if for example said laminates are HPL / CPL or compact laminate, said sheets are chosen from the list of: paper, cardboard, textiles, metal sheets, glass fiber sheets. For example said sheets can only comprise papers, wherein then preferably the type of papers are chosen in function of its position and function in the laminate. For example, laminates can comprise sheets which provide structural integrity and strength, decorative layers with for example at least one decorative sheet and wear-resistant layers with for example at least one translucent sheet. For structural integrity and strength, use can be made of kraft papers or cardboards or glass fiber scrims or edge tape / edge banding base papers. Said kraft papers can have a weight - before impregnation- between 80 and 300 gsm, for example 120 gsm or 155 gsm or 200 gsm. Said kraft papers can or cannot comprise a certain amount of recycled material. For example said kraft papers can comprise recycled material, e.g. can comprise at least 10 wt%, 20 wt%, 30 wt%, 50 wt%, 70 wt% or 100 wt% of recycled material. For decorative layers use can be made of white paper (for example for decors with light colors e.g. light wood decors, stone decors, fantasy decors) or of yellowish paper (for example for dark wood decors). Said decorative papers can be printed papers (analog printed paper or digital printed papers). Said decorative papers can also have a uniform color and can for example be a coloured paper, e.g. red, green, pink, blue, etc. paper. Said decorative papers preferably comprise a paper with a weight between 40 and 120 gsm. For wear-resistant layers, use can be made of transparent / translucent papers, such that decorative layers which have a said wearresistant layer on top, are still visible. For wear-resistant layers, in addition to a transparent / translucent paper, or instead of transparent / translucent paper, use can be made of one or more lacquer layers and / or one or more UV-cured layers, e.g. one can further coat a resin-impregnated decorative paper with an acrylate resin or a polyester resin or a polyurethane resin. Said transparent / translucent paper preferably is a paperwith a weight between 20 and 80 gsm. Of course, papers or other sheets with one or more of above-mentioned features or below-mentioned features can also be used for a DPL laminate comprising for example a particle board or wood fiberboard substrate.
[0133] For example the laminate can comprise a textile, such as a woven or non-woven sheet to provide the laminate with additional structural integrity. For example the laminate can comprise a glass fiber sheet to enhance the fire resistant properties of the laminate. For example the laminate can comprise a metal sheet, such as an aluminum sheet, to enhance the fire resistant properties of the laminate. The laminate can comprise a cardboard, to enhance the structural integrity and strength of the laminate and to have the desired thickness.
[0134] Said pressing together of the one or more of the above-mentioned aspects is preferably heat pressing, e.g. pressing wherein heat is supplied. For this use can be made of a discontinue process which makes use of a single daylight press or a multidaylight press. Use can also be made of a continuous process wherein for example a continuous double belt press is used. By supplying heat, curing can take place in a faster manner.
[0135] During said pressing together, the one or more resins liquefy such that the resins of the different sheets can flow into each other and adhere to each other.
[0136] Coating of a said sheet with said first resin can be done by, for example spray coating or a roller or a transfer disk.
[0137] Said first resin, when being used to form said laminate, is preferably water-based and has a dry matter content of between 30 and 60 wt%, for example of between 40 and 48 wt%, such that the first resin has the desired viscosity and is able to penetrate said sheet in a good manner.
[0138] Preferably a said sheet is impregnated / coated with said first resin in such a way, that the amount of first resin is between 60 and 120 gsm sheet, for example 70 gsm or 80 gsm or 90 gsm or 100 gsm.The invention according to the eighth aspect also relates to laminates having specific resins. Said specific resins are described below. Said laminates can or cannot be made according to one or more of the first, second, third, fourth, fifth, sixth or seventh aspect of the invention. The specific resins of the eight aspect of the invention can thus be used for the first, second, third, fourth, fifth, sixth or seventh aspect of the invention.
[0139] The invention also relates to a laminate made up of at least two sheets which are laminated together with one or more resins, wherein said one or more resins comprise a first resin, said first resin comprising a protein-containing component chosen from the list of blood meal, plant flour, plant seeds, such as epoxidized flax seed, and wherein said first resin preferably comprises a wetting agent.
[0140] Said wetting agent can be chosen from the list of alcohols, solvents and sulfates –such as sodium dodecyl sulfate–. If said wetting agent is present, the dry matter weight of the first resin comprises preferably at most 15 wt% of said wetting agent, preferably at most 10 wt%, for example 3 wt%. Preferably the wetting agent is chosen from the list of alcohols, solvents, sulfates -such as sodium dodecyl sulfate. For example the wetting agent can be ethanol, isopropanol, butanol or amino alcohol. The wetting agent can be a glycol ether, an acetate or acetone.
[0141] The invention also relates to a laminate made up of at least two sheets which are laminated together with one or more resins, wherein said one or more resins comprise a first resin, said first resin comprising bio-aromatics derived from a lignin source. Said bio-aromatics can provide the first resin with the desired viscosity and reactivity.
[0142] Further preferably said first resin comprises further an aldehyde, such as formaldehyde or hydroxymethylfurfural, and / or comprises a dialdehyde, such as glutaraldehyde or glyoxal. This enhances the reactivity of the first resin comprising bio-aromatics derived from a lignin source.The invention also relates to a laminate made up of at least two sheets which are laminated together with one or more resins, wherein said one or more resins comprise a first resin, said first resin being a lignin-based resin. Said first resin can be a lignin-based resin free from phenol.
[0143] The invention also relates to a laminate made up of at least two sheets which are laminated together with one or more resins, wherein said one or more resins comprise a first resin, said first resin comprising a furan containing compound, such as humins or polyfurfuralcohol.
[0144] The invention also relates to a laminate made up of at least two sheets which are laminated together with one or more resins, wherein said one or more resins comprise a first resin, said first resin comprising a yeast.
[0145] The invention also relates to a laminate made up of at least two sheets which are laminated together with one or more resins, wherein said one or more resins comprise a first resin, said first resin comprising polycarboxylic acid. Preferably said first resin further comprises a crosslinker including, for example di-, tri- or polyamines.
[0146] The invention also relates to a laminate made up of at least two sheets which are laminated together with one or more resins, wherein said one or more resins comprise a first resin, said first resin comprising cardanol. Preferably said first resin further comprises a crosslinker, for example aldehydes such as formaldehyde, glyoxal, glutaraldehyde or furaldehyde.
[0147] The above-mentioned laminates of the eight aspect of the invention can be made according to one or more of the first, second, third, fourth, fifth, sixth or seventh aspect of the invention. Also said laminates can comprise one or more features as described for said first, second, third, fourth, fifth, sixth and / or seventh aspect of the invention.
[0148] For better illustration of the features of the invention, some preferred embodiments are described hereunder, as examples without any limiting character, referring to the appended drawings, in which:Fig.1 shows an example of a part of a method according to the invention, wherein laminate is produced in a continuous pressing operation;
[0149] Fig. 2 shows an example of a laminate according to the invention, which can be made according to the method shown in figure 1.
[0150] Figure 2 shows an example of a laminate 1 according to the invention. Said laminate 1 is made up of five papers, which are laminated together with at least two types of resins, said two types of resins at least comprising a first resin 9.
[0151] Said first resin 9 can have one or more of the following features
[0152] - a viscosity of at least 50 mPa s, at 20 °C and 1.013 bar, preferably at least 100 mPa s, more preferably at least 500 mPa s, most preferably at least 1000 mPa s;
[0153] - an emulsion comprising particles, the emulsion preferably being a water-based emulsion and the D50value of the particle size distribution by volume of the particles in water is less than 200 micrometers, preferably less than 100 micrometers, more preferably less than 50 micrometers, even more preferably less than 30 micrometers,
[0154] The main components of said first resin 9 can be one of the following and / or the first resin 9 is:
[0155] -polyamides, which are obtained by polymerization of amino acids, and further carbohydrates. Said first resin 9 can for example have the following composition (based on dry matter weight):
[0156] • between 30 and 40 wt% of polylysine, said polylysine preferably comprising at least 80 wt% of hyperbranched polylysine;
[0157] • between 50 and 70 wt% of carbohydrates, preferably chosen from the list of fructose and / or glucose and / or invert sugar;
[0158] • between 0 and 20 wt%, or between 1 and 10 wt%, of additives as indicated in the description above and / or other components, said other components being for example the result of the production of said polylysine.
[0159] -a protein-containing component, said protein-containing component being for example flour or blood meal, wherein the dry matter weight of said first resin 9 comprises at least
[0160]
[0161] preferably at least 70 wt%, and preferably a wetting agent chosen from the list of: alcohols, solvents and sulfates –such as sodium dodecyl sulfate–.;
[0162] -lignin;
[0163] -a water-based epoxy resin or water-based polyurethane resin, said resin comprising biobased fillers, wherein said bio-based fillers are insoluble in water and have an average particle size D90 value of between 10 and 1000 μm.
[0164] - bio-aromatics derived from a lignin source;
[0165] - an aldehyde, such as formaldehyde or hydroxymethylfurfural, and / or a dialdehyde, such as glutaraldehyde or glyoxal;
[0166] - polycarboxylic acid;
[0167] - cardanol;
[0168] - a furan containing compound, such as humins or polyfurfuralcohol;
[0169] Said abovementioned compositions of the first resin can apply to all the described aspects of the invention.
[0170] Said first resin 9 can have one or more of the following additives:
[0171] -a wetting agent;
[0172] -anti-static additives;
[0173] -flame-retardant additives;
[0174] -a silicon containing compound, such as fumed silica or silanes or polysiloxanes;
[0175] -a metallic soap;
[0176] -a thermoplastic material;
[0177] -inorganic fillers such as CaCO3, talc, vermiculite;
[0178] -pH regulators such as bases, e.g. potassium carbonate, or acids;
[0179] -dialdehydes such as glyoxal or Strecker aldehyde;
[0180] -metal ions, e.g. (Cu2+, Mg2+, Al3+, Fe3+, Ca2+);
[0181] -polyimines.
[0182] Said abovementioned additives of the first resin can apply to all the described aspects of the invention.Said laminate 1 comprises from top to bottom, a translucent paper 4 impregnated with a first translucent resin, a decorative paper 3 impregnated with a second translucent resin and three kraft papers 2 impregnated with said first resin 9. In other words, from top to bottom, said laminate 1 comprises respectively a wear layer, a decorative layer and three structural layers. Said first translucent resin can or cannot be the same resin as the second translucent resin, however said resins are preferably of the same type and are chosen from the list of: melamine resins, such as MF resins, (poly)acrylate resins, polyurethane resins and unsaturated polyester resins. Said laminate 1 can be a HPL formed by a discontinuous process, e.g. with a single daylight press or with a multi daylight press. Said laminate 1 is preferably a CPL made by a continuous process, for example by a process as partially shown in figure 1. Said decorative paper 3 can be a printed paper or can be a uniformly coloured paper. Instead of said kraft papers 2, edge tape / edgebanding base paper can be used.
[0183] Fig. 2 shows an example of a step of a method according to the invention, wherein laminate 1 is produced in a continuous pressing operation. One or more of said sheets can be impregnated before pressing occurs (see further), wherein said impregnation can or cannot occur as described in the third aspect of the invention. One or more of said sheets are provided as not-impregnated sheets.
[0184] As can be seen in figure 1, papers are unrolled from five rolls of paper rolls 20, 30, 40, being respectively three rolls of kraft papers 20, one roll of decorative paper 30 and one roll of translucent paper 40. Preferably said rolls of kraft papers 20 are not impregnated with a resin, although this is not excluded. Preferably said roll of decorative paper 30 is impregnated with said second translucent resin and also preferably said roll of translucent paper 40 is impregnated with said first translucent resin. The resins present in said rolls of decorative paper 30 and translucent paper 40 are preferably in a B-stage, e.g. a semicured state, such that they are not tacky.
[0185] As can be seen in figure 1, the rolls of kraft papers 20 are coated with said first resin 9, namely an upper side of the lowermost roll of kraft paper 20 is coated with said first resin 9 and for the other rolls of kraft paper 20, one or both sides are coated with said first resin9. As can be seen in figure 1, said coating can be done with different types of applicators 10, for example with spraying devices 10 or with a transfer wheel 10. Of course other types of applicators can be used. After said coating of the rolls of kraft paper 20, the papers are laid on top of each other. Optionally a release film 5 is also unrolled from a roll 6 and placed on top of said unrolled papers. This release film 5 comprises a texture. The various papers are pressed together in a continuous pressing operation 7 at elevated temperature and pressure, wherein the resins from the different papers flow into each other and are (further) cured, as such laminating the papers together. A laminate 1 is produced thereby. The release film 5 presses a texture into the surface of the laminate 1. The release film 5 is then rolled up again and forms again a roll 6, which can be reused. After the pressing operation the laminate 1 may be cooled, abraded and the edges trimmed. Preferably a chopping or cutting tool 8 can chop or cut the produced laminate into said laminates 1 according to the invention and for example shown in figure 2.
[0186] Instead of cutting or chopping the laminate after the continuous pressing operation into sheets, it is also possible to roll up the laminate. In this way, a roll of laminate can be obtained.
[0187] The present invention is by no means limited to the embodiments described above, but such products may be produced according to several variants while remaining within the scope of the present invention.
Claims
Claims1.- A method for manufacturing a laminate, said laminate (1) being made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, wherein at least one of said one or more resins is a first resin (9), said first resin (9) preferably having a viscosity of at least 50 mPa s, at 20 °C and 1.013 bar, wherein the method comprises a lamination step wherein a stack of at least two or more sheets is formed and pressed together to laminate said sheets together, wherein at least one of said two or more sheets in said stack, has a side coated with said first resin (9), said side preferably facing a subsequent sheet in said stack.2.- The method according to claim 1, wherein both opposite sides of at least one of said two or more sheets in said stack, are coated with said first resin (9).3.- The method according to claim 1 or 2, wherein the first resin (9) has a viscosity of at least 50 mPa s, at 20 °C and 1.013 bar, preferably of at least 100 mPa s, more preferably of at least 500 mPa s, most preferably of at least 2000 mPa s.4.- The method according to any of the preceding claims, wherein the first resin (9) comprises a protein-containing component, said protein-containing component being for example flour or blood meal.5.- The method according to claim 4, wherein the dry matter weight of said first resin (9) comprises at least 30 wt% of said protein-containing component, preferably at least 50 wt%.6.- The method according to any of the preceding claims 1 to 3, wherein said first resin (9) comprises lignin.7.- The method according to any of the preceding claims 1 to 3, wherein the first resin (9) is a water-based epoxy or polyurethane resin, comprising bio-based fillers, wherein said bio-based fillers are insoluble in water and have an average particle size D90 value by mass of between 10 and 1000 μm.8.- The method according to any of the preceding claims, wherein-a discontinuous press, such as a single daylight press or a multidaylight press, is used for pressing together, to laminate said sheets together, wherein said pressing takes place at a maximum temperature of at least 150 °C, preferably at least 160°C, more preferably at least 180 °C, most preferably at least 200 °C, and a maximum pressure of at least 40 kg / cm2, preferably at least 80 kg / cm2, most preferably at least 100 kg / cm2and wherein the pressing has a duration of at least 30 seconds, for example at least 3 minutes; or -a continuous press (7), such as a double belt press, is used for pressing together, to laminate said sheets together, wherein said pressing takes place at a maximum temperature of at least 150 °C, preferably at least 190 °C, most preferably at least 200 °C, and a maximum pressure of at least 25 kg / cm2, preferably at least 40 kg / cm2, most preferably at least 60 kg / cm2, and wherein the pressing has a duration of at least 30 seconds, preferably at least 1 minute, more preferably at least 3 minutes.9.- A method for manufacturing a laminate, optionally according to any of the preceding claims 1 to 8, said laminate (1) being made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, wherein at least one of said one or more resins is a first resin (9), said first resin (9) being an emulsion comprising particles and comprising a wetting agent, wherein the method comprises a lamination step wherein a stack of at least two or more sheets is formed and pressed together to laminate said sheets together, wherein at least one of said at least two sheets has a side coated with said first resin (9), said side preferably facing a subsequent sheet in said stack10.- The method according to claim 9, wherein both opposite sides of at least one of said two or more sheets in said stack, are coated with said first resin (9).11.- The method according to claim 9 or 10, wherein the emulsion is a water-based emulsion and the D50value of the particle size distribution by volume of the particles in water is less than 200 micrometers, preferably less than 100 micrometers, more preferably less than 50 micrometers, even more preferably less than 30 micrometers.12.- The method according to any of the preceding claims 9 to 11, wherein the wetting agent is chosen from the list of: alcohols, solvents, sulfates –such as sodium dodecyl sulfate–.13.- A method for manufacturing a laminate, optionally according to any of the preceding claims 1 to 12, said laminate (1) being made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, wherein the method comprises a lamination step, said lamination step comprising:-providing at least two sheets;-a stacking substep wherein said at least two sheets are placed on top of each other in a continuous manner, for example wherein said two sheets are continuously unrolled on top of each other, followed by-a pressing sub step wherein said at least two sheets which are placed on top of each other, are pressed and laminated together,and wherein during said stacking substep, one or more sides of said sheets, are coated with a curable first resin (9), said first resin (9) being cured in the pressing substep.14.- The method according to claim 13, wherein said at least two sheets are supplied on roll, wherein during said stacking sub step said sheets are unrolled and coated with said curable first resin (9) and placed on top of each other.15.- The method according to claim 13 or 14, wherein at least one of said provided sheets is a resin-impregnated sheet, for example a resin-impregnated sheet on roll.16.- The method according to claim 15, wherein a said resin-impregnated sheet is coated during said stacking substep.17.- The method according to any of the claims 13 to 16, wherein at least one of said provided sheets is a sheet free from resin.18.- The method according to claim 17, wherein a said sheet free from resin, is coated during said stacking substep.19.- The method according to any of the claim 13 to 18, wherein the laminated together sheets are rolled up forming a laminate on roll, or are cutted into smaller sheets of laminate.20.- The method according to any of the claims 13 to 19, wherein a said sheet is a paper, a veneer, a textile or a glass fiber scrim.21.- The method according to any of the claims 13 to 20, wherein at least two sheets which are subsequently unrolled on top of each other in said stacking substep are resin-impregnated sheets, which are impregnated with a type of resin different from said first resin (9), wherein during said stacking sub step, at least one side of said at least two sheets facing each other, is coated with the curable first resin (9).22.- A method for manufacturing a laminate, optionally according to any of the preceding claims 1 to 21, said laminate (1) being made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, wherein at least one of said one or more resins is a first resin (9), said first resin (9) preferably having a viscosity of at least at least 50 mPa s, at 20 °C and 1.013 bar, wherein the method comprises an impregnation step wherein at least one of said two sheets is impregnated with said first resin (9) by vacuum and / or by pressure to form a resin-impregnated sheet, wherein a stack is formed and pressed together to laminate said sheets together, wherein said stack comprises at least said resin-impregnated sheet.23.- The method according to claim 22, wherein the first resin (9) has a viscosity of at least 50 mPa s, at 20 °C and 1.013 bar, preferably of at least 100 mPa s, more preferably of at least 500 mPa s, most preferably of at least 2000 mPa s.24.- The method according to claim 22 or 23, wherein the first resin (9) comprises a protein-containing component, said protein-containing component being for example flour or blood meal.25.- The method according to claim 24, wherein the dry matter weight of said first resin (9) comprises at least 30 wt% of said protein-containing component, preferably at least 50 wt%.26.- The method according to claim 22 or 23, wherein said first resin (9) comprises lignin.27.- The method according to claim 22 or 23, wherein the first resin (9) is a waterbased epoxy or polyurethane resin comprising bio-based fillers, wherein said bio-based fillers are insoluble in water and have an average particle size D90 value by mass of between 10 and 1000 μm.28.- A method for manufacturing a laminate, optionally according to any of the preceding claims 1 to 27, said laminate (1) being made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, wherein at least one of said one or more resins is a first resin (9), said first resin (9) preferably having a viscosity of at least at least 50 mPa s, at 20 °C and 1.013 bar, wherein the method comprises an impregnation step wherein at least one of said two sheets is impregnated with said first resin (9) by moving the sheet through and / or along an impregnation bath comprising said first resin (9), said first resin (9) being present in said impregnation batch having a temperature of at least 30 °C, preferably at least 40 °C, more preferably at least 50 °C, wherein a stack is formed and pressed together to laminate said sheets together, wherein said stack comprises at least said resin-impregnated sheet.29.- The method according to claim 28, wherein the first resin (9) has a viscosity of at least 50 mPa s, at 20 °C and 1.013 bar, preferably of at least 100 mPa s, more preferably of at least 500 mPa s, most preferably of at least 2000 mPa s.30.- The method according to claim 28 or 29, wherein the first resin (9) comprises a protein-containing component, said protein-containing component being for example flour or blood meal.31.- The method according to claim 30, wherein the dry matter weight of said first resin (9) comprises at least 30 wt% of said protein-containing component, preferably at least 50 wt%.32.- The method according to claim 28 or 29, wherein said first resin (9) comprises lignin.33.- The method according to claim 28 or 29, wherein the first resin (9) is a waterbased epoxy or polyurethane resin comprising bio-based fillers, wherein said bio-based fillers are insoluble in water and have an average particle size D90 value by mass of between 10 and 1000 μm.34.- A method for manufacturing a laminate, optionally according to any of the preceding claims 1 to 33, said laminate (1) being made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, wherein at least one of said one or more resins is a first resin (9), wherein the method comprises an impregnation step wherein at least one of said two sheets is impregnated with said first resin (9) by moving the sheet through and / or along an impregnation bath comprising said first resin (9) for forming a resin-impregnated sheet, and wherein said method subsequently comprises a coating step wherein said resin-impregnated sheet is coated with said first resin (9) for forming a coated resin-impregnated sheet, wherein a stack is formed and pressed together to laminate said sheets together, wherein said stack comprises at least said coated resin-impregnated sheet, wherein one or more of the following features are present:-said first resin (9) being present in said impregnation batch has a temperature of at least 30 °C, preferably at least 40 °C, more preferably at least 50 °C;-a wetting agent is added to said first resin (9) being present in said impregnation bath; -said first resin (9) being present in said impregnation batch is diluted, preferably diluted by water.35.- The method according to claim 34, wherein the first resin (9) has a viscosity of at least 50 mPa s, at 20 °C and 1.013 bar, preferably of at least 100 mPa s, more preferably of at least 500 mPa s, most preferably of at least 2000 mPa s.36.- The method according to claim 34 or 35, wherein the first resin (9) comprises a protein-containing component, said protein-containing component being for example flour or blood meal.37.- The method according to claim 36, wherein the dry matter weight of said first resin (9) comprises at least 30 wt% of said protein-containing component, preferably at least 50 wt%.38.- The method according to claim 34 or 35, wherein said first resin (9) comprises lignin.39.- The method according to claim 34 or 35, wherein the first resin (9) is a waterbased epoxy or polyurethane resin comprising bio-based fillers, wherein said bio-based fillers are insoluble in water and have an average particle size D90 value by mass of between 10 and 1000 μm.40.- A method for manufacturing a laminate, optionally according to any of the preceding claims 1 to 39, said laminate (1) being made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, wherein at least one of said one or more resins is a first resin (9), and wherein at least one of said two sheets is a paper sheet, wherein said paper sheet is treated with said first resin, for example is coated and / or impregnated with said first resin, and forms a resin-treated paper sheet, characterized in that said paper sheet has one or more of the following properties:-a Gurley value of between 15 and 60 seconds;-a Bendtsen roughness value of between 70 and 150 ml / min;-a Bendtsen porosity value of between 850 and 1350 ml / min;-a Bekk smoothness value of between 100 and 400 seconds;-at least one smoothened surface;-a residual moisture content of between 11 and 13 wt%;-a weight of between 100 and 180 gsm, preferably of between 130 and 170 gsm.41.- The method according to claim 40, wherein the first resin (9) comprises polyamides, which are obtained by polymerization of amino acids, and further carbohydrates.42.- The method according to claim 40 or 41, wherein said laminate is a decorative laminate comprising a decorative paper and one or more structural sheets, wherein said resin-treated paper sheet forms a said structural sheet.43.- The method according to any of the preceding claims, wherein said laminate (1) is a decorative laminate comprising a decor, wherein at least one of said two sheets is a decorative sheet (3) comprising said decor and wherein at least one of said two sheets is a structural sheet (2), wherein said structural sheet is coated and / or impregnated with said first resin (9).44.- The method according to claim 43, wherein said decorative sheet (3) is impregnated and / or coated with a transparent resin, preferably chosen from the list of a melamine resin, an acrylate resin, polyester resin or polyurethane resin.45.- The method according to any of the preceding claims, wherein at least one sheet is a paper having a weight of less than 50 gsm, preferably less than 25 gsm and / or having a Gurley value of less than 15 s, preferably less than 5 s, more preferably less than 3 s.46.- The method according to any of the preceding claims, wherein-a discontinuous press, such as a single daylight press or a multidaylight press, is used for pressing together, to laminate said sheets together, wherein said pressing takes place at a maximum temperature of at least 150 °C, preferably at least 160°C, more preferably at least 180 °C, most preferably at least 200 °C, and a maximum pressure of at least 40 kg / cm2, preferably at least 80 kg / cm2, most preferably at least 100 kg / cm2and wherein the pressing has a duration of at least 30 seconds, for example at least 3 minutes; or -a continuous press (7), such as a double belt press, is used for pressing together, to laminate said sheets together, wherein said pressing takes place at a maximum temperature of at least 150°C, preferably at least 190 °C, most preferably at least 200 °C,and a maximum pressure of at least 25 kg / cm2, preferably at least 40 kg / cm2, most preferably at least 60 kg / cm2, and wherein the pressing has a duration of at least 30 seconds, preferably at least 1 minute, more preferably at least 3 minutes.47.- A laminate, wherein the laminate (1) is made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, characterized in that said one or more resins comprise a first resin (9), said first resin (9) comprising a protein-containing component chosen from the list of: blood meal, plant flour, plant seeds, such as epoxidized flax seed, and wherein said first resin (9) preferably comprises a wetting agent.48.- The laminate according to claim 47, wherein the wetting agent is chosen from the list of: alcohols, solvents and sulfates –such as sodium dodecyl sulfate–.49.- A laminate, wherein the laminate (1) is made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, characterized in that said one or more resins comprise a first resin (9), said first resin (9) comprising bio-aromatics derived from a lignin source.50.- The laminate according to claim 49, wherein the first resin (9) further comprises an aldehyde, such as formaldehyde or hydroxymethylfurfural, and / or comprises a dialdehyde, such as glutaraldehyde or glyoxal.51.- A laminate, wherein the laminate (1) is made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, characterized in that said one or more resins comprise a first resin (9), said first resin (9) being a lignin-based resin.52.- A laminate, wherein the laminate (1) is made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, characterized in that said one or more resins comprise a first resin (9), said first resin (9) comprising a furan containing compound, such as humins or polyfurfuralcohol.53.- A laminate, wherein the laminate (1) is made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, characterized in that said one or more resins comprise a first resin (9), said first resin (9) comprising polycarboxylic acid.54.- A laminate, wherein the laminate (1) is made up of at least two sheets (2, 3, 4) which are laminated together with one or more resins, characterized in that said one or more resins comprise a first resin (9), said first resin (9) comprising cardanol.55.- A laminate according to any of the preceding claims 47 to 54, wherein the laminate (1) is made by method according to any of the preceding claims 1 to 46.