Vitrimer epoxy and method of synthesizing vitrimer epoxy
The synthesis of vitrimer epoxy with dynamic covalent acetal linkages addresses the recyclability and stability issues of thermoset polymers by allowing for reprocessability and stress relaxation, enhancing sustainability in applications requiring mechanical strength and thermal stability.
Patent Information
- Application Number
- PCT/IN2026/050689
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Priority Date
- 2025-05-08
- Filing Date
- 2026-04-15
- Publication Date
- 2026-11-12
AI Technical Summary
Thermoset polymers are non-recyclable and non-reprocessable due to their irreversible cross-linked structure, leading to significant waste generation and environmental pollution, while thermoplastics lack high-temperature dimensional stability and chemical resistance.
A vitrimer epoxy is synthesized with dynamic covalent acetal linkages that form a cross-linked network, allowing for reprocessability and maintaining mechanical strength and thermal stability through trans-acetalization reactions.
The vitrimer epoxy exhibits permanent crosslinking characteristics at lower temperatures for mechanical strength and dimensional stability, while enabling stress relaxation and reprocessing at elevated temperatures, facilitating recycling and reshaping without compromising structural integrity.
Smart Images

Figure IN2026050689_12112026_PF_FP_ABST
Abstract
Description
VITRIMER EPOXY AND METHOD OF SYNTHESIZING VITRIMER EPOXYTECHNICAL FIELD
[0001] The present disclosure relates to a field of thermoset polymers. Moreover, the present disclosure relates to a vitrimer epoxy, and a method of synthesizing vitrimer epoxy.BACKGROUND
[0002] Thermoset polymers are permanently cross-linked polymers widely used in various industrial applications due to their superior mechanical properties, thermal stability, and chemical resistance. The thermoset polymers are useful in electrical applications, including circuit breakers, switch gears, switchboards, transformers, and reclosers. However, the irreversible cross-linked structure of the thermoset polymers makes them non-recyclable and non-reprocessable, resulting in significant waste generation, environmental pollution, and increased landfill burden. The challenge of thermoset disposal and waste management remains a vital issue in sustainable material development.
[0003] The challenge of thermoset disposal and waste management can be solved by using existing thermoplastics. The existing thermoplastics offer recyclability and reprocessability through melting and reshaping, but they lack high-temperature dimensional stability and chemical resistance like thermoset polymers. Thus, there exists a technical problem of how to develop a vitrimer epoxy that retains the mechanical strength and thermal stability of thermoset polymers while enabling recyclability and reprocessability like thermoplastics.
[0004] Therefore, in light of the foregoing discussion, there exists a need to overcome the aforementioned drawbacks.SUMMARY
[0005] The present disclosure provides a vitrimer epoxy and a method of synthesizing vitrimer epoxy. The present disclosure addresses the technical problem of how to enhance the mechanical strength, thermal stability, and reprocessability of vitrimer epoxy while maintaining structural integrity and durability under varying environmental conditions . An aim of the present disclosure is to provide a solution that overcomes at least partially the problems encountered in the prior art and provides an improved vitrimer epoxy and an improved method of synthesizing vitrimer epoxy featuring a dynamic covalent acetal exchange network that enables reprocessability while maintaining high mechanical strength and thermal stability.
[0006] One or more objectives of the present disclosure is achieved by the solutions provided in the enclosed independent claims. Advantageous implementations of the present disclosure are further defined in the dependent claims.
[0007] In one aspect, the present disclosure provides a vitrimer epoxy comprising:a virgin epoxy resin; andan acetal-containing hardener in an amount of 5-50 weight percent relative to the virgin epoxy resin,wherein the vitrimer epoxy contains dynamic covalent acetal linkages that form a cross-linked network, wherein the cross-linked network possesses dynamic bond exchange capability via trans-acetalization reactions when heated above a predetermined temperature threshold, resulting in a material exhibiting permanent crosslinking characteristics at temperatures below the predetermined temperature threshold and stress relaxation with retained structural integrity at temperatures above the predetermined temperature threshold.
[0008] The vitrimer epoxy exhibits a combination of mechanical durability and reprocessability by incorporating an acetal-containing hardener at 5-50 weight percent relative to the virgin epoxy resin. The vitrimer epoxy forms dynamiccovalent acetal linkages throughout the cross-linked network. The vitrimer epoxy exhibits a unique dual-nature behaviour dependent on temperature conditions. At normal operating temperatures below the predetermined threshold, the vitrimer epoxy exhibits permanent crosslinking characteristics similar to high-performance thermosets, providing exceptional mechanical strength and dimensional stability. When heated above the predetermined temperature threshold, the cross-linked network undergoes controlled bond exchange via trans-acetalization reactions, enabling stress relaxation while maintaining overall structural integrity. Unlike existing thermosets, which remain permanently rigid until degradation, the vitrimer epoxy can be reshaped, repaired, and recycled without sacrificing the mechanical properties associated with crosslinked materials such as existing thermosets.
[0009] In another aspect, the present disclosure provides a method for synthesizing a vitrimer epoxy, comprising:preheating a virgin epoxy resin;adding an acetal-containing hardener to a preheated virgin epoxy resin to obtain an intermediate mixture;degassing the intermediate mixture for a predetermined time to obtain a degassed mixture; andcuring the degassed mixture through a staged thermal cycle to obtain the vitrimer epoxy, wherein the vitrimer epoxy contains dynamic covalent acetal linkages that form a cross-linked network, wherein the cross-linked network possesses dynamic bond exchange capability via trans acetalization reactions when heated above a predetermined temperature threshold, resulting in a material exhibiting permanent crosslinking characteristics at temperatures below the predetermined temperature threshold and stress relaxation with retained structural integrity at temperatures above the predetermined temperature threshold.
[0010] The method for synthesizing a vitrimer epoxy achieves all the advantages and technical effects of the vitrimer epoxy formed in the present disclosure.
[0011] It is to be appreciated that all the aforementioned implementation forms can be combined. All steps that are performed by the various entities described in the present application, as well as the functionalities described to be performed by the various entities, are intended to mean that the respective entity is adapted to or configured to perform the respective steps and functionalities. It will be appreciated that features of the present disclosure are susceptible to being combined in various combinations without departing from the scope of the present disclosure as defined by the appended claims.
[0012] Additional aspects, advantages, features, and objects of the present disclosure would be made apparent from the drawings and the detailed description of the illustrative implementations construed in conjunction with the appended claims that follow.BRIEF DESCRIPTION OF THE DRAWINGS
[0013] The summary above, as well as the following detailed description of illustrative embodiments, is better understood when read in conjunction with the appended drawings. For the purpose of illustrating the present disclosure, exemplary constructions of the disclosure are shown in the drawings. However, the present disclosure is not limited to specific methods and instrumentalities disclosed herein. Moreover, those in the art will understand that the drawings are not to scale. Wherever possible, like elements have been indicated by identical numbers.
[0014] Embodiments of the present disclosure will now be described, by way of example only, with reference to the following diagrams wherein:FIG.l is a flowchart illustrating a method for synthesizing a vitrimer epoxy, in accordance with an embodiment of the present disclosure;FIG. 2 is a graphical representation illustrating a Fourier transform infrared (FTIR) spectroscopy comparison between different epoxies, in accordance with an embodiment of the present disclosure;FIG. 3 is a flowchart illustrating a reaction mechanism for the formation of a flexible vitrimer epoxy, in accordance with an embodiment of the present disclosure;FIG. 4 is a graphical representation illustrating the Fourier transform infrared (FTIR) spectroscopy analysis of two distinct epoxy formulations, in accordance with an embodiment of the present disclosure;FIG. 5 is a graphical representation illustrating a relationship between stress and strain for flexible vitrimer epoxy, in accordance with an embodiment of the present disclosureFIG. 6A is a flowchart for synthesizing rigid vitrimer epoxy, in accordance with an embodiment of the present disclosure;FIG. 6B is a graphical representation illustrating the Fourier transform infrared (FTIR) spectroscopy analysis of different configurations of vitrimer epoxies, in accordance with an embodiment of the present disclosure;FIG. 6C is a graphical representation illustrating the Fourier transform infrared (FTIR) spectroscopy analysis of different configurations of vitrimer epoxies, in accordance with an embodiment of the present disclosure;FIG. 7 is a graphical representation illustrating force-displacement curves for various acetal-modified rigid vitrimer epoxy formulations, in accordance with an embodiment of the present disclosure;FIG. 8 is a graphical representation illustrating a tensile strength of various acetal-based rigid vitrimer epoxy formulations, in accordance with an embodiment of the present disclosure;FIG. 9 is a graphical representation illustrating the Fourier transform infrared (FTIR) spectroscopy analysis of two acetal-modified epoxy formulations with varying composition ratios, in accordance with an embodiment of the present disclosure;FIG. 10 is a graphical representation illustrating tensile strength of various acetal-modified epoxy formulations, in accordance with an embodiment of the present disclosure;FIG. 11 is a graphical representation illustrating a differential scanning calorimetry (DSC) analysis of various acetal-modified epoxy formulations, in accordance with an embodiment of the present disclosure;FIG. 12 is a graphical representation illustrating a thermogravimetric analysis (TGA) of two acetal-modified epoxy formulations, in accordance with an embodiment of the present disclosure;FIG. 13 is a graphical representation illustrating a dynamic mechanical analysis (DMA) of various epoxy formulations, in accordance with an embodiment of the present disclosure;FIG. 14 is a graphical representation illustrating a storage modulus at room temperature of three epoxy formulations, in accordance with an embodiment of the present disclosure;FIG. 15 is a graphical representation illustrating the force-displacement curves for various epoxy formulations, in accordance with embodiments of the present disclosure;FIG. 16 is a graphical representation illustrating the tensile strength comparison between various epoxy formulations, in accordance with embodiments of the present disclosure;FIG. 17 is a graphical representation illustrating the force-displacement curves for various acetal-based vitrimer epoxy formulations, in accordance with embodiments of the present disclosure; andFIG. 18 is a graphical representation illustrating the tensile strength comparison between three distinct epoxy formulations, in accordance with embodiments of the present disclosure.
[0015] In the accompanying drawings, an underlined number is employed to represent an item over which the underlined number is positioned or an item to which the underlined number is adjacent. A non-underlined number relates to an item identified by a line linking the non-underlined number to the item. When a number is non-underlined and accompanied by an associated arrow, the nonunderlined number is used to identify a general item at which the arrow is pointing.DETAILED DESCRIPTION OF EMBODIMENTS
[0016] The following detailed description illustrates embodiments of the present disclosure and ways in which they can be implemented. Although some modes of carrying out the present disclosure have been disclosed, those skilled in the art would recognize that other embodiments for carrying out or practicing the present disclosure are also possible.
[0017] FIG.l is a flowchart illustrating a method for synthesizing a vitrimer epoxy, in accordance with an embodiment of the present disclosure. With reference to FIG. 1, there is shown a flowchart illustrating the method 100 for synthesizing a vitrimer epoxy. The method 100 includes steps 102 to 108. There is provided the method 100 for synthesizing the vitrimer epoxy.
[0018] At step 102, the method 100 includes preheating a virgin epoxy resin. The virgin epoxy resin is a thermosetting polymer comprising epoxide functional groups, such as Araldite CY 228-1, which has not been previously cured or processed. The virgin epoxy resin can also comprise diglycidyl ether of bisphenol A (DGEBA) as epoxide functional group. Here, curing refers to a chemical reaction process where the liquid epoxy resin is converted into a hard, infusible, and insoluble three-dimensional network through crosslinking reactions. The preheating involves heating the virgin epoxy resin to a predefined temperature while stirring for a predefined time using equipment such as a hot plate with magnetic stirring capability. In an implementation, the preheating of the virgin epoxy resin is carried out at a temperature between 40-80 degrees Celsius with stirring at 200-400 rpm for 20-30 minutes. The temperature range between 40-80 degrees Celsius and stirring at 200-400 rpm for 20-30 minutes provides a reduction in the viscosity of the virgin epoxy resin while preventing thermal degradation. The controlled stirring between 200-400 rpm facilitates uniform heat distribution throughout the virgin epoxy resin while minimizing air entrapment. For example, at a stirring speed of 200 rpm, the movement of the virgin epoxy resin is relatively slow and gentle. The stirring speed of 200 rpm ensures that heat is gradually and uniformly distributed throughout the virgin epoxy resin. However, because themixing speed is low, the time required to achieve complete heat distribution is longer. Additionally, the slow stirring motion minimizes turbulence, which helps in reducing air entrapment in the virgin epoxy resin.
[0019] In another example, at 350 rpm, the stirring speed is moderate, meaning that the virgin epoxy resin undergoes more movement, leading to faster heat distribution compared to 200 rpm. Therefore, ensuring that the heat spreads effectively while still keeping air entrapment relatively low. In another example, at 400 rpm, the stirring speed is high. The virgin epoxy resin experiences more rapid movement, leading to quicker heat distribution. However, if the stirring is too aggressive, it might introduce some turbulence, increasing the risk of air bubbles forming within the virgin epoxy resin. The stirring at 400 rpm is carefully controlled to prevent defects in the vitrimer epoxy formed. The process of preheating creates suitable conditions for the subsequent incorporation of an acetal-containing hardener to improve the final quality and performance of the vitrimer epoxy.
[0020] The preheating prepares the virgin epoxy resin for trans-acetalization and dynamic covalent bond exchange by reducing the viscosity and enhancing the miscibility of the virgin epoxy resin. The preheating temperature and duration are controlled to achieve suitable processing conditions without initiating premature crosslinking. The preheated virgin epoxy resin serves as the primary polymer matrix that will incorporate the dynamic covalent bonds required for the vitrimer properties.
[0021] At step 104, the method 100 includes adding the acetal-containing hardener to the preheated virgin epoxy resin to obtain an intermediate mixture. The acetal-containing hardener refers to a chemical compound containing both amine groups and acetal groups, which serves as the crosslinking agent for the virgin epoxy resin while simultaneously introducing dynamic covalent bonds. The crosslinking agent refers to a molecule capable of reacting with functional groups on multiple polymer chains to form bridges between the chains, creating a three-dimensional network. The process of adding the acetal-containing hardener involves measuring the acetal-containing hardener relative to the virgin epoxy resinand gradually incorporating the acetal-containing hardener into the preheated virgin epoxy resin while maintaining a predefined temperature for a predefined time. The acetal groups present in the acetal-containing hardener position themselves within the virgin epoxy resin network during curing, creating sites for bond exchanges when exposed to increased temperatures. The proper dispersion and incorporation of the acetal-containing hardener in the intermediate mixture improves the distribution of dynamic linkages throughout the virgin epoxy resin. Thereby determining the recyclability characteristics of the vitrimer epoxy formed. The control of hardener concentration relative to the epoxy resin establishes the balance between rigid thermoset properties and thermoplastic-like behaviour.
[0022] In an implementation, the acetal-containing hardener includes amino acetaldehyde dimethyl acetal in an amount of 5-50 weight percent relative to the virgin epoxy resin. Amino acetaldehyde dimethyl acetal is a specialized compound containing primary amine groups (-NH2) at one end and two methoxy groups (-OCH3) connected to the same carbon atom, forming the characteristic acetal structure (-C(OR)2"). The epoxy groups in the virgin epoxy resin are characterized by a three-membered ring containing an oxygen atom bonded to two carbon atoms. During the reaction with epoxy groups, the primary amine groups initiate ringopening of the epoxide to form a secondary amine group and hydroxyl group, while the acetal structure remains intact. The intact acetal structure allows the cured material to undergo trans-acetalization reactions when heated above a specific temperature threshold. The trans-acetalization involves the exchange of alkoxy groups between different acetal functions, effectively breaking and reforming chemical bonds while maintaining the overall network connectivity. The chemical reaction enables the vitrimer epoxy to be reshaped, repaired, and recycled without losing structural integrity. The selection of amino acetaldehyde dimethyl acetal enables suitable crosslinking via the amine groups while establishing the acetal linkages required for trans-acetalization reactions. The concentration range of 5-50 weight percent allows for customization of the cross-link density and the proportion of dynamic bonds in the vitrimer epoxy formed, directly influencing the balance between mechanical rigidity and reprocessability characteristics in the vitrimerepoxy formed. In another implementation, the acetal containing-hardener includes amino acetaldehyde diethyl acetal, 4-aminobutyraldehyde dimethyl acetal, 3-aminobenzaldehyde ethylene acetal, 2-methyl-l,3-dioxolan-2-yl methanamine, 3-(2-methyl-l,3-dioxolan-2-yl)-l-propanamine, methyl amino acetaldehyde dimethyl acetal, n-(2,2-dimethoxy ethyl) prop-2-enamide, 2-(cbz-amino)acetaldehyde dimethyl acetal, n-(2,2-dimethoxyethyl)-4-methoxy- 1 ,3 -benzodioxole-5 -methanamine, n-(2,2-dimethoxyethyl)-4-methylbenzenesulfonamide, hydroxy acetaldehyde dimethyl acetal, hydroxy acetaldehyde diethyl acetal, 2-hydroxy-2-phenylpropionaldehyde dimethyl acetal, 2-methyl-3-hydroxypentanal dimethyl acetal, 4-(2,2-dimethoxy ethyl) phenol, 4-(hydroxymethyl)benzaldehyde dimethyl acetal, 4-amino-3-(2,2-dimethoxy-ethyl) phenol, 3-(l,3-dioxolan-2-yl) phenol, 1,3-dioxolane-2-methanol, (2-methyl-l,3-dioxolan-4-yl) methanol, 2-ethyl-l,3-dioxolane-4-methanol, 2-ethyl-2-methyl- 1 ,3-dioxolane-4-methanol, 2 -methyl -2-phenyl- 1 ,3-dioxolane-4-methanol, 2-ethyl-2-phenyl- 1 ,3-dioxolane-4-methanol, 4-(2-ethyl-l,3-dioxolan-2-yl) phenol, 2,2-dimethyl-l,3-dioxolane-4-methanol, 2,2-diethyl-l,3-dioxolane-4-methanol, 2-methyl-l,3-dioxolane-2-methanol, 2-(2-methyl- 1 ,3 -dioxolan-2-yl)- 1 , 1 -diphenylethanol, 2-ethyl -2 -methyl- 1 ,3 -dioxolane-4-methanol, 2-(dimethyl amino)-4-(2-methyl-l,3-dioxolan-2-yl) phenol, 2-isobutyl-2-methyl- 1 ,3 -dioxolane-4-methanol, 2,2-bis(propan-2-yl)- 1 ,3 -dioxolan-4-yl] methanol, 2-[2-(l -hydroxy-2 -nitroethyl) phenyl] acetaldehyde dimethyl acetal, 1-(2,2-dimethoxyethyl)-5-methoxy-6-(methoxycarbonyl)-4-oxo-l,4-dihydropyridine -3 -carboxylic acid.
[0023] In an implementation, the acetal-containing hardener is used in an amount of 30-50 weight percent relative to the virgin epoxy resin to produce a flexible vitrimer epoxy having a tensile strength of 15-25 mega pascal (MPa). The flexible vitrimer epoxy refers to a variant of the vitrimer epoxy composition with enhanced pliability and elongation properties, suitable for applications requiring impact resistance and resilience. The process of producing flexible vitrimer epoxy involves increasing the proportion of acetal-containing hardener to 30-50 weight percent relative to the virgin epoxy resin, which creates a polymer network with a higher concentration of dynamic acetal linkages and comparatively lower cross-linkdensity. The mixing of the acetal -containing hardener in the virgin epoxy resin must be performed in a precisely controlled instrument, such as a mechanical stirrer, planetary mixer, or high-shear mixer, to ensure uniform dispersion of the hardener within the epoxy resin.
[0024] The acetal-containing hardener facilitates the formation of a polymer network characterized by an increased concentration of dynamic acetal linkages. The dynamic acetal linkages enable bond exchange reactions, thereby enhancing the reprocessability and adaptability of the vitrimer epoxy material. For example, when the acetal-containing hardener is used at 30 weight percent relative to the virgin epoxy resin, the vitrimer epoxy network maintains a higher cross-link density compared to higher proportions of the acetal-containing hardener. The vitrimer epoxy formed is flexible but retains structural rigidity. The tensile strength is closer to 25 MPa, indicating a balance between strength and flexibility.
[0025] In another example, when the acetal-containing hardener is used at 40 weight percent relative to the virgin epoxy resin, the increased proportion of the acetal-containing hardener reduces the cross-link density further, increasing the number of dynamic acetal linkages. As a result, the vitrimer epoxy formed becomes more flexible, and the tensile strength is slightly lower approximately ranging between 25 MPa to 20 MPa. The composition provides a balance between mechanical strength and adaptability, making the formed vitrimer epoxy suitable for applications requiring moderate flexibility.
[0026] In another example, when the acetal-containing hardener is used at 50 weight percent relative to the virgin epoxy resin, the vitrimer epoxy formed contains the highest proportion of dynamic acetal linkages, leading to lower cross-link density. The vitrimer epoxy formed is highly flexible with tensile strength ranging between 20 MPa to 15 MPa. Additionally, the controlled increase in the hardener proportion reduces the overall cross-link density, imparting flexibility to the vitrimer epoxy formed. The process parameters, including temperature, stirring rate, and reaction time, are kept suitable to achieve a homogenous distribution of the acetal-containing hardener and ensure the desired mechanical and thermalproperties of the flexible vitrimer epoxy formed. The quantity of acetal-containing hardener mixed with the virgin epoxy resin to form the flexible vitrimer epoxy creates a network with increased dynamic bond content and reduced cross-link density, resulting in improved flexibility and elongation properties of the vitrimer epoxy formed. The tensile strength range of 15-25 MPa provides suitable structural integrity for applications requiring resilience and impact resistance while maintaining adequate recyclability characteristics.
[0027] At step 106, the method 100 includes degassing the intermediate mixture for a predetermined time to obtain a degassed mixture. The degassing refers to the process of removing entrapped air bubbles and volatile compounds from a polymer mixture through the application of vacuum or other pressure reduction techniques such as thermal reduction and membrane degasification. The entrapped air bubbles and volatile compounds may create voids or defects in the final cured material. The degassing involves placing the intermediate mixture containing the epoxy resin and acetal-containing hardener in a vacuum chamber and applying reduced pressure for a predetermined gassing time. In an implementation, the reduced pressure is applied for 15-30 minutes. Air bubbles trapped during the mixing process expand under vacuum conditions and rise to the surface of the mixture, where the bubbles burst and are removed. The process of degassing improves the structural integrity and mechanical properties of the vitrimer epoxy formed by eliminating stress concentration points. The predetermined degassing time is suitable for the complete removal of air while preventing excessive exposure that might initiate premature curing reactions. Therefore, degassing the intermediate mixture enhances the structural integrity and mechanical properties of the vitrimer epoxy by eliminating voids and stress concentration points, ensuring a defect-free final material.
[0028] At step 108, the method 100 includes curing the degassed mixture through a staged thermal cycle to obtain the vitrimer epoxy. The staged thermal cycle refers to a programmed heating regimen with multiple temperature plateaus configured to improve the curing process for the vitrimer epoxy. In an implementation, the staged thermal cycle includes sequential heating at 80°C, 100°C, 120°C, and 140°C, eachtemperature maintained for 2-4 hours. The degassed mixture is placed in a laboratory oven or similar heating equipment with precise temperature control capabilities, followed by programming a sequence of temperature increases with specified hold times at each level. The initial curing phase at 80°C serves as a critical initiation stage where the reaction between the epoxy groups and the acetal-containing hardener begins at a controlled rate. The sequential heating at 80°C enables the formation of preliminary crosslinks without inducing excessive reaction exotherm that might otherwise lead to thermal runaway or structural defects. At this temperature, the amino groups of the hardener initiate the nucleophilic attack on the epoxide rings, forming the foundation of the polymer network while maintaining sufficient mobility for optimal component distribution throughout the matrix.
[0029] Following the initial phase, the temperature elevation to 100°C represents a strategic advancement in the curing profile. At this temperature, the reaction kinetics are accelerated to promote further crosslinking while simultaneously initiating the dynamic bond exchange mechanisms characteristic of vitrimer chemistry. The 100°C plateau facilitates the establishment of secondary crosslinks and allows for stress relaxation within the forming network, which is essential for minimizing residual stresses that could compromise mechanical properties in the final product. The subsequent increase to 120°C marks the transition to advanced curing, where the network densification occurs more rapidly. The temperature is particularly significant as it exceeds the glass transition temperature of the partially cured vitrimer epoxy, enabling chain mobility that allows unreacted functional groups to find reaction partners more readily. The dynamic exchange reactions between hydroxyl groups and acetal moieties become more pronounced at 120°C temperature, establishing the reversible covalent bonds that will enable the reprocessability character of the vitrimer epoxy.
[0030] The final stage at 140°C represents the post-curing phase that is essential for achieving maximum crosslink density and optimal mechanical properties. At elevated temperature of 140°C, any residual unreacted functional groups have sufficient mobility and energy to participate in the crosslinking reactions, ensuringcomplete conversion. Additionally, 140°C temperature further promotes the establishment of the dynamic exchange network that defines the vitrimer character, balancing the seemingly contradictory requirements of high mechanical strength and reprocessability. The maintenance of temperature for 2-4 hours ensures that the vitrimer epoxy achieves the desired tensile strength in the range of 70-85 MPa while retaining the capacity for controlled bond rearrangement under appropriate conditions.
[0031] The staged thermal curing process facilitates the formation of a crosslinked network containing dynamic covalent acetal linkages. The temperature-controlled stages allow for ideal network formation while establishing the acetal exchange capability within vitrimer epoxy. During curing, the epoxy resin forms permanent crosslinks while simultaneously incorporating the dynamic bonds that enable the unique vitrimer epoxy properties. The resulting vitrimer epoxy exhibits permanent crosslinking characteristics at temperatures below a predetermined threshold while demonstrating stress relaxation with retained structural integrity when heated above the threshold. The dual-nature behaviour of the vitrimer epoxy distinguishes the vitrimer epoxy from existing thermosets and enables recyclability through grinding and reprocessing.
[0032] In an implementation, the method 100 is used for producing a rigid vitrimer epoxy. For producing the rigid vitrimer epoxy, the method 100 includes preheating the virgin epoxy resin, followed by the controlled addition of the acetal-containing hardener to the preheated virgin epoxy resin (as explained in steps 102 and 104). The mixing of virgin epoxy resin and the acetal-containing hardener is conducted under predefined conditions such as temperature, stirring speed, and time period for mixing to ensure homogeneous dispersion of the acetal-containing hardener within the epoxy resin, thereby forming the intermediate mixture.
[0033] In an implementation, the method 100 further includes adding silica microparticles having a particle size of less than 45 micrometres in an amount of 50-80 weight percent relative to the total composition after adding the acetal-containing hardener. The silica microparticles are inorganic fillers composed ofsilicon dioxide (SiC ) with dimensions less than 45 micrometres. The silica microparticles act as reinforcing fillers that improve the mechanical properties and provide electrical insulation characteristics essential for applications in electrical components. A quantity of silica microparticles is measured corresponding to 50-80 weight percent of the total composition and gradually incorporated into the total composition.
[0034] When the silica microparticles are added after the acetal-containing hardener, several beneficial phenomena occur. First, the hardener creates an initial network structure that can better suspend and distribute the silica particles throughout the composition. If the silica were added before the hardener, it might agglomerate or settle unevenly before the network formation begins. The posthardener addition ensures more uniform distribution and ultimately superior mechanical properties in the final product.
[0035] For example, when silica microparticles are added at 50 weight percent relative to the total composition. At this concentration, the silica provides significant reinforcement while maintaining good flowability of the mixture. The acetal-containing hardener has already begun establishing cross-links in the polymer matrix, creating a scaffolding that supports the even distribution of the silica particles. This results in a composition with enhanced strength and durability while retaining workability during application. The 50-weight percent silica content represents the lower threshold where sufficient reinforcement is achieved without compromising other desirable properties.
[0036] In another example, when silica microparticle content is at 65 weight percent, the composition achieves an optimal balance between strength enhancement and processability. The previously added acetal-containing hardener has initiated a network that can effectively incorporate this higher silica loading. The developing polymer matrix supports the silica particles in a three-dimensional arrangement that prevents settling or separation. This mid-range concentration delivers superior tensile strength and dimensional stability compared to the 50-weight percent formulation, while still allowing adequate flow characteristicsduring application. The interparticle distances are reduced compared to the lower concentration, creating more effective load transfer throughout the material.
[0037] When silica microparticles are incorporated at 80 weight percent, the composition exhibits excessively high viscosity, which adversely affects the processability and uniform dispersion of the silica microparticles. At this high fdler loading, the remaining 20 weight percent of the virgin epoxy resin and acetal-containing hardener is insufficient to effectively encapsulate and bind the silica microparticles, even with the network-forming ability of the acetal-containing hardener. The lack of adequate content of the virgin epoxy resin and the acetal-containing hardener leads to poor interfacial bonding, increased risk of agglomeration, and compromised structural cohesion of the vitrimer epoxy.
[0038] In another implementation, materials such as Alumina (Aluminium Oxide, AI2O3), Magnesium Hydroxide (Mg(0H)2), Aluminium trihydroxide (ATH, Al(0H)3), Talc (Magnesium Silicate, Mg3Si40io(OH)2), Mica (Muscovite or Phlogopite), Zinc Borate (2ZnO AB2O3 3.5H2O), Calcium Carbonate (CaCO ). Nanoclay (Montmorillonite), Titanium Dioxide (Ti02), Zinc Oxide (ZnO), and Silicon Carbide (SiC) may be used as alternatives to silica microparticles.
[0039] The intermediate mixture and the silica microparticles are then mixed using precisely controlled instrument, such as a mechanical stirrer, planetary mixer, or high-shear mixer, to ensure uniform dispersion of the silica microparticles within the intermediate mixture. In an implementation, the high shear mixture is rotated at 100-400 rpm for 20 minutes -40 minutes at 40 degrees Celsius -80 degrees Celsius, resulting in a compounded mixture. The silica microparticles have a size of less than 45 micrometres, ensuring uniform dispersion within the intermediate mixture and minimising stress concentration points in the rigid vitrimer epoxy formed. The vitrimer epoxy supports a high filler content of 50-80 weight percent due to the well-balanced viscosity characteristics. Therefore, resulting in a composite material with stable dimensions, reduced thermal expansion, and improved electrical insulation while remaining reusable.
[0040] The compounded mixture undergoes bath sonication for 15-30 minutes at a predefined frequency of 40 kHz and power of 200 W. The bath sonication is a non-contact technique in which the container holding the compounded mixture is placed in a water bath through which ultrasonic waves are transmitted. The ultrasonic generator operates at 40 kHz with a power output of 200 W, providing sufficient acoustic energy to process the highly viscous mixture without causing premature curing reactions. The bath Bonification allows acoustic energy to pass through the container walls and act on the compounded mixture without direct contact with an ultrasonic probe. The absence of direct contact of the ultrasonic probe with the compounded mixture helps maintain cleanliness and prevents contamination, making bath sonication beneficial for sensitive formulations.
[0041] The selection of a 40 kHz frequency is vital for the effective dispersion of silica microparticles within the vitrimer epoxy formulation. The frequency of 40 kHz produces larger and more energetic cavitation bubbles, which are particularly effective for breaking up and dispersing dense, inorganic materials such as silica. Compared to higher frequencies, which generate smaller cavitation bubbles, lower frequencies improve particle dispersion in high-viscosity formulations. The 200 W power setting ensures adequate energy transfer to break down silica agglomerates while preventing excessive heating that could accelerate crosslinking reactions prematurely.
[0042] The timing of the bath sonication step is carefully controlled to optimize dispersion. Sonication is performed after adding the acetal-containing hardener but before introducing the accelerator. This sequence allows the hardener to initiate preliminary crosslinking, which helps stabilize the dispersed silica particles within the epoxy matrix. Performing sonication at this stage ensures that the silica particles remain well-integrated in the formulation while the mixture retains sufficient fluidity for effective dispersion. The ultrasonic waves efficiently break down silica clusters, preventing uneven distribution and ensuring a homogeneous particle dispersion.
[0043] Following bath sonication, the mixture undergoes additional high-shear mixing at a speed of 100-400 rpm while maintaining a temperature range of 40-80°C. The additional high shear mixing preserves the uniform dispersion achieved during sonication, further incorporating silica particles into the developing vitrimer network, thereby forming a resulting formulation. The resulting formulation is then prepared for degassing and moulding, ensuring consistent material properties and optimal performance in the final vitrimer epoxy product.
[0044] In an implementation, the method 100 further includes adding an accelerator to the intermediate mixture prior to degassing. The accelerator refers to a chemical compound that increases the rate of reaction between the virgin epoxy resin and acetal-containing hardener, providing efficient network formation at moderate temperatures and shorter cure times. The accelerator may be added in the intermediate mixture or the resulting formulation depending upon whether we want to synthesize rigid vitrimer epoxy without improved electrical properties or to synthesize rigid vitrimer epoxy with improved electrical properties, respectively.
[0045] In an implementation, the accelerator includes l-(3-aminopropyl) imidazole in an amount of 2.5-20 weight percent relative to the virgin epoxy resin. l-(3-aminopropyl) imidazole is a catalytic compound containing both an imidazole ring and an aminopropyl side chain, providing multiple nucleophilic centres for initiating and accelerating epoxy ring-opening reactions. The incorporation involves adding a measured quantity of 1 -(3 -aminopropyl) imidazole corresponding to 2.5-20 weight percent relative to the virgin epoxy resin into the intermediate mixture, followed by thorough mixing to achieve uniform distribution. The 1 -(3 -aminopropyl) imidazole functions as a highly effective catalyst for epoxy ring-opening reactions due to the presence of dual nucleophilic sites. The l-(3-aminopropyl) imidazole (also known as imidazole moiety) initiates the chemical reaction with epoxy groups, while the aminopropyl group provides additional catalytic functionality. The structure of 1 -(3 -aminopropyl) imidazole enables efficient network formation at moderate curing temperatures while providing uniform incorporation of the acetal linkages throughout the vitrimer epoxy formed.In another implementation, the accelerator may comprise 1 -methyl imidazole, 2-methylimidazole, 2-ethyl-5 -methyl- Ih-imidazole, l-benzyl-2-methylimidazole, 2-aminoimidazole, hydroxy methylimidazole, 1 -(2 -hydroxyethyl) imidazole, l-(p-hydroxyphenyl)imidazole, hydroxymethyl-5 -methyl imidazole, 2 -hydroxy- Ih-imidazole-4-carboxylic acid, l-methylimidazole-5 -carboxylic acid, ethyl 1-methyl-lh-imidazole-5-carboxylate, l-methylimidazole-4, 5 -dicarboxylic acid, ethyl 2-amino-lh-imidazole-4-carboxylate, 2-amino-3-methyl-3h-imidazole-4-carboxylic acid ethyl ester, methyl 1 -benzyl- lh-imidazole-5 -carboxylate, ethyl 5-methyl-2-phenyl- lh-imidazole-4-carboxylate, ethyl 1 -benzyl-5 -methyl- lh-imidazole-4-carboxylate, lh-imidazole-4-carboxamide, 1 -methyl- lh-imidazole-4-carboxamide, 5-amino- 1-methyl- lh-imidazole-4-carboxamide, 5-amino- 1 -propyl- Ih-imidazole-4-carboxamide, 5-hydroxy-lh-imidazole-4-carboxamide, histidine, histamine.
[0046] In an implementation, for synthesizing the rigid vitrimer epoxy without improved electrical properties accelerator is added into the intermediate mixture of epoxy resin and acetal-containing hardener, followed by thorough mixing to ensure uniform distribution throughout the intermediate mixture. The accelerator catalyses the ring-opening reactions of the epoxy groups by providing nucleophilic attack sites that lower the activation energy barrier for the crosslinking process. The accelerated reaction kinetics enables thorough incorporation of the acetal-containing hardener into the rigid vitrimer epoxy formed. The addition of the accelerator improves cross-linking and provides complete incorporation of the acetal-containing hardener into the polymer network. The accelerator facilitates uniform network formation throughout the intermediate mixture, preventing localized variations in cross-link density that may compromise mechanical properties. The precise control over the curing process provided by the accelerator ensures the formation of permanent crosslinks and dynamic acetal linkages throughout the final vitrimer epoxy.
[0047] In an implementation, the acetal-containing hardener is used in an amount of 10-20 weight percent, and the accelerator is used in an amount of 5-11 weight percent relative to the virgin epoxy resin to produce a rigid vitrimer epoxy havinga tensile strength of 70-85 megapascal (MPa). The rigid vitrimer epoxy refers to a variant of the vitrimer epoxy with high mechanical strength and stiffness, suitable for structural applications requiring high load-bearing capacity.
[0048] In an implementation, the acetal-containing hardener is incorporated at 10 weight percent, while the accelerator is used at 11 weight percent relative to the virgin epoxy resin. At this formulation, the lower concentration of the acetal-containing hardener (amino acetaldehyde dimethyl acetate) results in fewer initial crosslinking points within the polymer network. However, the higher accelerator concentration (aminopropyl imidazole) facilitates the curing reaction, ensuring efficient network formation. This balance leads to a structured vitrimer epoxy network, where the limited acetal functionality contributes to rigidity while the accelerator promotes rapid and effective crosslinking. The tensile strength achieved with this formulation is approximately 72 MPa, which is within the claimed range of 70-85 MPa. The formulation demonstrates the feasibility of using a lower hardener concentration while maintaining the necessary mechanical strength and vitrimer properties through enhanced catalyst activity.
[0049] In another implementation, the acetal-containing hardener is increased to 15 weight percent, while the accelerator remains at 11 weight percent relative to the virgin epoxy resin. This composition establishes an optimal balance between crosslink density and dynamic bond exchange capability, resulting in a vitrimer epoxy with superior mechanical properties. The increased concentration of the acetal-containing hardener facilitates the formation of additional crosslinking sites, reinforcing the polymer network while preserving the reprocessability characteristic of vitrimers. The accelerator ensures efficient curing, promoting a well-integrated and uniform structure. The formulation achieves a tensile strength of approximately 82 MPa, representing the highest mechanical performance within the claimed range. This ratio provides a vitrimer epoxy composition with enhanced rigidity, stability, and reprocessability, making it suitable for structural applications requiring high mechanical integrity.
[0050] In another implementation, the acetal-containing hardener is incorporated at 20 weight percent, while the accelerator remains at 11 weight percent relative to the virgin epoxy resin. The higher concentration of acetal-containing hardener increases the availability of dynamic covalent bonds, allowing for greater molecular rearrangement and bond exchange within the vitrimer network. This formulation maintains sufficient crosslinking to ensure rigidity and structural integrity, achieving a tensile strength of approximately 73 MPa, which remains within the claimed range of 70-85 MPa. However, as the concentration of the acetal-containing increases, the material exhibits a shift towards a more dynamic and flexible polymer network. When the acetal-containing hardener concentration is increased further, the formulation undergoes structural modifications that result in reduced mechanical strength and increased susceptibility to deformation. The controlled selection of the acetal-containing hardener concentration within the 10-20 weight percent range ensures that the vitrimer epoxy exhibits optimal mechanical performance while maintaining the desired level of dynamic bond exchange for reprocessability.
[0051] Further, the degassing process removes entrapped air bubbles and volatile compounds using vacuum or pressure reduction techniques. The intermediate mixture is placed in the vacuum chamber, and reduced pressure is applied for 15-30 minutes, allowing air bubbles to expand, rise to the surface, and burst. The degassing eliminates voids and stress concentration points, enhancing the structural integrity and mechanical properties of the rigid vitrimer epoxy formed while preventing premature curing reactions.
[0052] The staged thermal cycle for curing involves sequential heating at 80°C, 100°C, 120°C, and 140°C, each maintained for 2-4 hours. The initial phase at 80°C enables controlled crosslinking, while 100°C accelerates reaction kinetics and facilitates stress relaxation. At 120°C, network densification occurs, enhancing dynamic bond exchange, and 140°C ensures complete conversion, achieving high tensile strength and vitrimer properties in the rigid vitrimer epoxy.
[0053] The thermal curing process establishes a crosslinked network with dynamic covalent acetal linkages, ensuring structural integrity at lower temperatures while enabling stress relaxation and reprocessability when heated above a threshold. The dual behaviour of the rigid vitrimer epoxy, having stress relaxation and reprocessability, differentiates the rigid vitrimer epoxy from existing thermoset polymers.
[0054] The vitrimer epoxy is formed by combining the virgin epoxy resin, such as ARALDITE CY 228-1, with the acetal -containing hardener in an amount ranging from 5-50 weight percent relative to the virgin epoxy resin. The selection of the virgin epoxy resin provides a strong polymer backbone, while the acetal-containing hardener introduces dynamic covalent acetal linkages. The acetal-containing hardener reacts with epoxy groups to establish a crosslinked network within the vitrimer epoxy network. For example, in a formulation containing 15 weight percent acetal-containing hardener, the rigid vitrimer epoxy exhibits a tensile strength of approximately 82 MPa. The tensile strength exhibits mechanical properties comparable to existing thermoset polymers. The formation of a stable crosslinked network ensures high mechanical integrity, making the rigid vitrimer epoxy suitable for applications requiring structural durability, including electrical insulation components and structural composites.
[0055] The incorporation of dynamic covalent acetal linkages enables trans-acetalization reactions, which occur when the virgin epoxy resin is heated above a predetermined temperature threshold (approximately ranging between 80-100°C).The occurrence of trans-acetalization allows bond exchange within the vitrimer epoxy network without degrading the polymer backbone. The capability to undergo bond exchange facilitates stress relaxation while preserving structural integrity, enhancing the reprocessability of the vitrimer epoxy. For example, in vitrimer epoxy samples, up to 93% of the original tensile strength is maintained after multiple reprocessing cycles, indicating effective bond exchange while retaining mechanical properties. Unlike existing thermoset polymers, which remain permanently rigid and degrade overtime, vitrimer epoxy enables reshaping, repair,and recycling, making vitrimer epoxy suitable for sustainable material applications in aerospace, automotive, and electrical industries.
[0056] At temperatures below the predetermined threshold, the vitrimer epoxy exhibits characteristics of a permanently crosslinked thermoset, ensuring excellent dimensional stability and load-bearing capacity under normal operating conditions. The retention of structural integrity at lower temperatures enables vitrimer epoxy to maintain performance in applications that require reliability, such as high-voltage insulation panels and reinforced composites. When heated above the threshold temperature, stress relaxation occurs due to bond exchange between hydroxyl groups and acetal linkages. The occurrence of bond exchange enables vitrimer epoxy to be remolded or recycled while maintaining overall integrity. The permanent crosslinking at lower temperatures, combined with stress relaxation and reprocessability at elevated temperatures, provides an effective solution for extending the lifecycle of existing thermoset polymers that are non-recyclable.
[0057] FIG. 2 is a graphical representation illustrating Fourier transform infrared (FTIR) spectroscopy comparison between different epoxies, in accordance with an embodiment of the present disclosure. FIG 2 is described in conjunction with elements from FIG 1. With reference to FIG. 2, there is shown a graphical representation 200 representing Fourier transform infrared (FTIR) spectroscopy comparison between different epoxies. The graphical representation 200 depicts the absorption of infrared light by permanent epoxy and uncured epoxy at different wavelengths, typically measured in wavenumbers. The transmittance percentage is represented on the ordinate axis. The wavenumber is measured in centimetres inverse (cm ') on the abscissa axis. Transmittance percentage quantifies the amount of light that passes through a sample or material, expressed as a percentage of the original light intensity. The wavenumber is defined as the number of wavelengths per unit distance. The graphical representation 200 includes a curve 202 depicting the behaviour of permanent epoxy and the curve 204 depicting the behaviour of uncured epoxy. Each peak or band in the curve 202 and the curve 204 correspondsto the vibration of specific chemical bonds within the corresponding epoxy formulation.
[0058] The curve 202, representing a broad absorption dip is observed approximately ranging between 3000 cm1to 3500 cm which corresponds to the O-H stretching vibrations, indicating the formation of hydroxyl groups due to the ring -opening reaction of epoxide groups during curing. The structural transformation confirms the successful crosslinking of the epoxy resin, converting the epoxy resin into a permanent polymer network. Additionally, a decrease in absorption intensity is noticeable, approximately ranging between 900 cm1to 1000 cm '. which corresponds to the disappearance of the characteristic C-0 stretching vibrations of the epoxide ring, further verifying the curing process. The fingerprint region 208, approximately ranging between 1000 cm1to 1500 cm '. reveals multiple sharp absorption bands associated with C-O, C-C, and C-H bending and stretching vibrations, reflecting the structural reorganization that occurs during cross-linking.
[0059] The curve 204, representing a sharp absorption dip, observed approximately ranging between 2800 cm1to 3100 cm '. which corresponds to the C-H stretching vibrations of the epoxide ring. Another significant absorption feature is present, approximately ranging between 850 cm1to 950 cm '. attributed to the C-0 stretching vibrations of the oxirane ring, confirming the presence of unreacted epoxy groups. The fingerprint region 208, approximately ranging between 1000 cm1to 1500 cm '. exhibits intense and well-defined absorption dips, which correspond to the molecular vibrations of epoxy functional groups and backbone structures that remain unaltered due to the absence of cross-linking.
[0060] The analysis of curve 202 and curve 204 indicates the structural changes occurring during the curing process. The disappearance of the epoxide ring -related absorption dips in curve 202, particularly in a region 206, approximately ranging between 850 cm1to 950 cm '. confirms the consumption of reactive epoxy groups in the crosslinking reaction. The emergence of a broad absorption dip in a region 206, approximately ranging between 3000 cm to 3500 cm in curve 202, whichis absent in curve 204, signifies the formation of hydroxyl groups resulting from epoxide ring -opening. The fingerprint region 208 of curve 202 also exhibits shifts in peak positions and intensities, indicating modifications in the polymer backbone due to the formation of a permanent, crosslinked network. Therefore, the analysis of the curve 202 and the curve 204 confirms that the permanent epoxy undergoes a structural transformation that enhances stability and mechanical integrity, distinguishing the permanent epoxy from the uncured epoxy, which retains reactive functionalities.
[0061] FIG. 3 is a flowchart illustrating a reaction mechanism for the formation of flexible vitrimer epoxy, in accordance with an embodiment of the present disclosure. FIG. 3 is described in conjunction with FIGs. 1 to 2. With reference to FIG. 3, there is shown a flowchart 300 that includes a series of operations from 302 to 306.
[0062] At operation 302, the initial reaction components are shown, comprising an amino acetal hardener with terminal NIL group and dimethoxy functionality (OCH3 groups) positioned to react with an epoxy group (represented as R with an oxirane ring). After that, at operation 304, the nucleophilic attack of the amino group (NIL) on the epoxy ring occurs, resulting in ring -opening of the oxirane. An intermediate reaction product 308 shows the formed secondary amine (NH) linkage between the acetal moiety and the epoxy group (R), with the characteristic hydroxyl group (OH) that forms during epoxy ring opening.
[0063] Finally, at operation 306, the dynamic exchange reaction characteristic of the vitrimer chemistry is established. The operation 306 illustrates the reversible reaction equilibrium between the hydroxyl-containing intermediate and another acetal group, illustrating the formation of new acetal linkages through trans-acetalization. The chemical structures presented in operation 306 illustrate the reversible nature of the chemical reaction, with the double arrow (« ) indicating the dynamic exchange between the two formed products. The hydroxyl group (HO) from the opened epoxy reacts with the acetal, displacing a methoxy group (H3CO) and forming a new acetal linkage. The new acetal linkage formed establishes thedynamic covalent network that enables the vitrimer properties of the resulting epoxy system.
[0064] FIG. 4 is a graphical representation illustrating Fourier transform infrared (FTIR) spectroscopy analysis of two distinct epoxy formulations, in accordance with an embodiment of the present disclosure. FIG 4 is described in conjunction with elements from FIGs 1 to 3. With reference to FIG. 4, there is shown a graphical representation 400 representing Fourier transform infrared (FTIR) spectroscopy analysis of two distinct epoxy formulations. Specifically, the graphical representation 400 depicts the absorption of infrared light by two distinct epoxy formulations at different wavelengths, typically measured in wavenumbers. The transmittance percentage is represented on the ordinate axis. The wavenumber is measured in centimetres inverse (cm ') on the abscissa axis. The graphical representation 400 includes a curve 402 depicting the behaviour of unmodified epoxy and the curve 404 depicting the behaviour of an epoxy modified with 40% acetal hardener.
[0065] The curve 402 exhibits a broad absorption dip at approximately ranging between 3000 cm1to 3500 cm '. which corresponds to O-H stretching vibrations. The broad dip signifies the formation of hydroxyl groups due to the ring-opening reaction of epoxide groups. The emergence of hydroxyl -related absorption confirms successful chemical interaction between the epoxy and the acetal-containing hardener, useful in forming a dynamic covalent network.
[0066] Additionally, another absorption dip is observed, approximately ranging between 2800 cm1to 3000 cm '. corresponding to C-H stretching vibrations. The stretching vibrations arise from the hydrocarbon backbone of the polymer network, providing analysis of the structural modifications occurring during polymerization. A series of sharp absorption dips appears in a fingerprint region 408, particularly approximately ranging between 1000 cm1to 1300 cm which corresponds to C-O-C stretching vibrations associated with acetal groups. The presence of the sharp absorption dips in the fingerprint region 408 confirms the successful incorporation of acetal functionalities into the polymer backbone, establishing dynamicexchangeable bonds vital for the vitrimer epoxy. Furthermore, additional absorption dips occur approximately ranging between 1500 cm1to 1800 cm which correspond to C=C and C=O stretching vibration absorption features indicating structural reorganization due to crosslinking, further reinforcing the presence of a modified polymeric network with improved stability.
[0067] The curve 404 exhibits an absorption dip in the region 406, approximately ranging between 3000 cm1to 3500 cm indicating a lower concentration of hydroxyl groups. The reduced intensity of the absorption dip confirms that minimal epoxide ring-opening has occurred, highlighting the absence of chemical modification with an acetal-based curing agent. Another absorption dip is observed in the region 406, approximately ranging between 2800 cm1to 3000 cm '. which corresponds to C-H stretching vibrations of the epoxy structure. The absorption dips are similar to the corresponding absorption dips in the curve 402, indicating the presence of hydrocarbon-based functional groups.
[0068] A distinct absorption dip appears in the region 406, approximately ranging between 850 cm to 950 cm '. corresponding to C-0 stretching vibrations of the oxirane (epoxide) ring. The presence of the distinct absorption dip confirms the retention of unreacted epoxy groups, verifying the absence of extensive curing or modification in the curve 404. The fingerprint region 408, approximately ranging between 1000 cm1to 1500 cm '. exhibits well-defined absorption dips corresponding to C-0 and C-C vibrations. The fingerprint region 408 and the region 406 indicate the presence of an unmodified epoxy framework, with fewer structural variations compared to the curve 402.
[0069] The spectral features of curve 402 and curve 404 provide insights into the structural transformations of the unmodified epoxy and the epoxy modified with 40% acetal hardener. The presence of a strong hydroxyl-related absorption dip in the curve 402, which is less pronounced in the curve 404, confirms the successful chemical reaction between the epoxy and acetal components, leading to hydroxyl formation. The absence of an epoxide ring-related absorption dip in curve 402,which remains visible in curve 404, further verifies the consumption of epoxy functional groups during curing.
[0070] FIG. 5 is a graphical representation illustrating a relationship between stress and strain for flexible vitrimer epoxy, in accordance with an embodiment of the present disclosure. FIG 5 is described in conjunction with elements from FIGs 1 to 4. With reference to FIG. 5, there is shown a graphical representation 500 representing the relationship between stress and strain for vitrimer epoxy. The graphical representation 500 includes a curve 502 depicting the mechanical response of the flexible vitrimer epoxy when subjected to tensile deformation. The strain percentage is represented on the abscissa axis. The stress is measured in megapascal (MPa) on the ordinate axis. The stress is the force applied to a material per unit area. On the other hand, the strain is the deformation that results from the force applied.
[0071] The curve 502 exhibits an initial region 504 showing a sharp increase in stress, reaching a peak stress approximately ranging between 18 MPa to 22 MPa at a strain approximately ranging between 8% to 12%. The initial region 504 signifies the elastic deformation. In the initial region 504, the flexible vitrimer epoxy exhibits a proportional increase in stress with strain, governed by the inherent stiffness of the molecular structure of the flexible vitrimer epoxy. The sharp rise in stress in the initial region 504 indicates a rapid resistance to applied force, characteristic of a significant initial modulus.
[0072] Following the initial region 504, the curve 502 undergoes a drop in stress to a range approximately ranging between 12 MPa to 15 MPa, occurring within a strain range of approximately ranging between 15% to 30%. The decline represents a yielding phase, where molecular chain reorganization or localized deformation mechanisms, such as necking or bond slippage, reduce the resistance to applied force. The presence of the dip suggests a transition from elastic to plastic deformation, where intermolecular forces begin to realign under sustained loading.
[0073] Beyond the yielding phase, the curve transitions into a plateau region 506, where stress remains relatively stable within a range of approximately ranging between 13 MPa to 16 MPa, extending over a strain range of approximately ranging between 40% to 160%. The plateau region 506 is indicative of strain hardening and molecular alignment, where polymer chains of the flexible vitrimer epoxy reorient along the stress, offering sustained resistance without a significant increase in applied stress. The gradual upward trend observed within the plateau region 506 suggests strain-induced reinforcement due to molecular orientation, secondary crystallization, or alignment of fibrillar structures in the flexible vitrimer epoxy.
[0074] At a strain level approximately ranging between 160% to 180%, the stress exhibits a peak 508 before undergoing a sudden drop to near-zero stress values, signifying material failure. The peak 508 before failure indicates a final resistance phase where maximum alignment or secondary interactions temporarily enhance the mechanical integrity of the flexible vitrimer epoxy. The subsequent rapid decline in stress to near zero corresponds to catastrophic failure, where the flexible vitrimer epoxy loses its structural continuity due to chain scission, void formation, or fracture propagation.
[0075] The graphical representation 500 indicates that the flexible vitrimer epoxy exhibits moderate yield strength, high ductility, and substantial energy absorption capacity, making the flexible vitrimer epoxy suitable for applications requiring flexibility, resilience, and toughness. The plateau region 506 extending over abroad strain range indicates the ability to undergo large deformations without significant stress variation, a characteristic beneficial for shock absorption, flexible structural components, and high-strain applications. The presence of a pronounced failure point suggests that once the material surpasses a critical strain limit, failure occurs abruptly, indicating the necessity for controlled strain conditions in functional applications.
[0076] FIG. 6A is a flowchart for synthesizing rigid vitrimer epoxy, in accordance with an embodiment of the present disclosure. FIG. 6A is described in conjunctionwith elements of FIGs. 1 to 5. With reference to FIG. 6A, there is shown a flowchart 600A that includes a series of operations from 602A to 612A.
[0077] At operation 602A, an imidazole compound having an aminoalkyl side chain is reacted with an epoxide -containing compound represented by “R”, where “R” is an alkyl or aryl group. For example, at operation 602, the aminoalkyl side chain is reacted with an epoxide-containing compound represented by “R”, where “R” is an alkyl or aryl group. After that, at operation 604A, a nucleophilic addition occurs wherein the nitrogen atom of the imidazole ring attacks the epoxy group of the epoxide-containing compound represented by “R”. The epoxide-containing compound undergoes ring opening, forming an intermediate product with the R group now attached to the imidazole compound.
[0078] At operation 606A, the intermediate product undergoes further reaction to form a modified imidazole compound with the R group attached, along with a reacting molecule i.e. amino acetaldehyde dimethyl acetal containing methoxy (3HCO) groups. As the reaction continues to operation 608A, the intermediate product is transformed into another product, now with a dimethoxy-containing fragment.
[0079] At operation 610A, a transition state is reached where the epoxy oxygen of the “R” group interacts with the nitrogen atom adjacent to the dimethoxy moiety. The transition state is a specific point of high energy within the pathway of a reaction, representing the configuration where bonds are in the process of being broken and formed. The epoxy oxygen of the “R” group forms a bond with the nitrogen atom adjacent to the dimethoxy moiety. Finally, at operation 612A, the reaction concludes with the formation of the target compound containing the “R group”, a hydroxyl group, and dimethoxy functionalities. The chemical structure of the final compound is shown in the block of operation 612A. The chemical structure establishes the foundation for the dynamic covalent acetal linkages that will allow for bond exchange reactions in a cured vitrimer epoxy system.
[0080] FIG. 6B is a graphical representation illustrating Fourier transform infrared (FTIR) spectroscopy analysis of different configurations of vitrimer epoxies, in accordance with an embodiment of the present disclosure. FIG 6B is described in conjunction with elements from FIGs 1 to 6A. With reference to FIG.6B, there is shown a graphical representation 600B representing Fourier transform infrared (FTIR) spectroscopy analysis of different configurations of vitrimer epoxies. The graphical representation 600B includes a curve 602B depicting the behaviour of uncured epoxy resin, a curve 604B depicting the behaviour of an epoxy formulation containing 20% amino acetaldehyde dimethyl acetal hardener and 11% aminopropyl imidazole, a curve 606B depicting the behaviour of an epoxy formulation containing 10% hardener and 11% aminopropyl imidazole, a curve 608B depicting the behaviour of an epoxy formulation containing 15% hardener and 11% aminopropyl imidazole, and a curve 610B depicting the behaviour of an epoxy flexible vitrimer formulation containing 40% hardener and no aminopropyl imidazole. The transmittance percentage is represented on the ordinate axis. The wavenumber is measured in centimetres inverse (cm ' ) on the abscissa axis.
[0081] The curve 602B does not contain any hardener or catalyst. The transmittance remains relatively flat across the curve 602B. The curve 602B exhibits characteristic peaks in a region 612B, approximately ranging between 3000 to 2800 cm '. corresponding to C-H stretching vibrations. The curve 602B maintains high transmittance at approximately ranging between 3400-3200 cm '. indicating the absence of hydroxyl (O-H) groups. The curve 602B exhibits that the epoxide rings remain intact, and hydroxyl groups have not yet formed.
[0082] The curve 604B exhibits a reduction in transmittance at approximately between 3400-3200 cm1as compared to the curve 602B, forming a broad absorption band characteristic of hydroxyl (O-H) stretching vibrations. The formation of a broad absorption band indicates that the epoxide rings have undergone opening, leading to the formation of hydroxyl groups. Additionally, characteristic peaks appear in region 612B, approximately in the range of 3000-2800 cm ', corresponding to aliphatic C-H stretching vibrations. The presence of hydroxyl groups confirms the successful curing of the epoxy formulation.
[0083] The curve 606B exhibits a moderately strong hydroxyl absorption band in the region corresponding to 3400-3200cm However, the intensity of the absorption band is lower than that of the curve 604B, suggesting partial curing or a lower extent of hydroxyl group formation. The characteristic peaks in the region 612B corresponding to aliphatic C-H stretching vibrations remain visible in the range of 3000-2800 cm The reduced intensity of the hydroxyl absorption band indicates that curve 606B has undergone curing but to a lesser extent compared to the formulation represented by curve 604B.
[0084] The curve 608B exhibits a hydroxyl absorption band in the region 612B corresponding to 3400-3200 cm '. with an intensity between that of curves 606B and 604B. The epoxy formulation has undergone a moderate degree of curing, resulting in the formation of hydroxyl groups. The characteristic peaks in the region 612B, approximately ranging between 3000-2800 cm '. corresponding to aliphatic C-H stretching vibrations, remain present. The intensity of the hydroxyl absorption band suggests that the curve 608B achieves an optimal balance between curing and mechanical properties as compared to the curve 602B, curve 604B, and curve 606B.
[0085] The curve 610B exhibits the most pronounced hydroxyl absorption band for wavenumber corresponding to 3400-3200 cm '. indicating extensive hydroxyl group formation due to epoxide ring opening. The presence of a strong hydroxyl absorption band suggests increased hydrogen bonding within the formulation, contributing to its flexible nature. The characteristic peaks corresponding to aliphatic C-H stretching vibrations remain visible in the range of 3000-2800 cm The increased hydroxyl content in the curve 610B correlates with the enhanced flexibility as compared to the curve 602B, curve 604B, curve 606B and curve 608B.
[0086] The graphical representation 600B confirms the successful curing of vitrimer epoxy formulations through the appearance of hydroxyl groups, with varying intensities depending on the hardener content. The curve 602B maintainshigh transmitance in the region 612B, approximately between 3400 to 3200 cmindicating the absence of hydroxyl groups, while all modified formulations (i.e. the curve 604B, curve 606B, curve 608B and the curve 610B) exhibit hydroxyl absorption bands, signifying epoxide ring opening and subsequent curing. The curve 604B shows the strongest hydroxyl absorption, suggesting extensive curing, while the curve 606B and the curve 608B display intermediate hydroxyl intensities, aligning with respective curing extents. The curve 608B is identified as the optimal composition for achieving high mechanical strength, whereas the curve 610B, with the highest hydroxyl content, demonstrates increased flexibility due to enhanced hydrogen bonding and dynamic covalent bond exchange.
[0087] FIG. 6C is a graphical representation illustrating Fourier transform infrared (FTIR) spectroscopy analysis of different configurations of vitrimer epoxies, in accordance with an embodiment of the present disclosure. FIG 6C is described in conjunction with elements from FIGs 1 to 6B. With reference to FIG.6C, there is shown a graphical representation 600C representing Fourier transform infrared (FTIR) spectroscopy analysis of different configurations of vitrimer epoxies. The graphical representation 600C includes a curve 602C depicting the behaviour of uncured epoxy resin, a curve 604C depicting the behaviour of an epoxy formulation containing 20% amino acetaldehyde dimethyl acetal hardener and 11% aminopropyl imidazole, a curve 606C depicting the behaviour of an epoxy formulation containing 10% hardener and 11% aminopropyl imidazole, a curve 608C depicting the behaviour of an epoxy formulation containing 15% hardener and 11% aminopropyl imidazole, and a curve 610C depicting the behaviour of an epoxy flexible vitrimer formulation containing 40% hardener and no aminopropyl imidazole. The transmittance percentage is represented on the ordinate axis. The wavenumber is measured in centimetres inverse (cm ') on the abscissa axis.
[0088] The curve 602C exhibits a prominent peak in the region 612C at approximately 915 cm '. which is indicative of the C-O-C stretching vibration of the oxirane (epoxide) ring. The oxirane ring, consisting of a three-membered structure with one oxygen atom and two carbon atoms, possesses substantialpotential energy, rendering it highly reactive. The presence of the peak at 915 cm1confirms the integrity of the epoxy groups, indicating that the epoxy resin remains unreacted. Additionally, the curve 602C exhibits characteristic peaks in a region 614C associated with the molecular backbone of the epoxy resin, including C-C bending vibrations in the range of 850-750 cm
[0089] The curve 604C exhibits the complete disappearance of the oxirane peak at 915 cm '. providing conclusive evidence that the curing reaction has been completed. During the curing process, the oxirane rings undergo opening due to reactions with amino groups of the acetal-containing hardener, leading to the formation of C-N bonds and hydroxyl (-OH) groups. The curve 604C further exhibits new absorption bands in the region 614C (at around 850-750 cm"), corresponding to C-C stretching vibrations, C-H out of plane bending vibrations, and additional vibrational modes associated with the newly formed crosslinked network. The absence of the oxirane peak confirms that the 20% hardener concentration, in combination with 11% aminopropyl imidazole catalyst, facilitated the complete conversion of epoxide groups, resulting in a fully cured vitrimer network.
[0090] The curve 606C exhibits the complete absence of the oxirane peak at 915 cm1, indicating that the curing reaction has progressed to full conversion of epoxide groups. However, variations in spectral features, particularly in the intensity and shape of peaks within the region 614C, reflect differences in crosslink density and network structure due to the lower hardener content. The formulation corresponding to the curve 606C exhibits incomplete curing under lower-temperature conditions, necessitating an extended curing cycle to achieve complete conversion of epoxide groups.
[0091] The curve 608C exhibits that the complete absence of the oxirane peak at 915 cm1confirms the successful curing of the epoxy formulation. The spectral pattern exhibits distinctive absorption bands within the fingerprint region, corresponding to the specific chemical structure of this formulation. The formulation associated with curve 608C demonstrates optimized mechanicalproperties, including a tensile strength of approximately 82 MPa, indicative of an optimal balance between crosslink density, network flexibility, and dynamic bond exchange capability. Variations in peak intensities relative to curve 604C and curve 606C indicate structural differences contributing to enhanced mechanical performance.
[0092] The curve 610C exhibits the complete disappearance of the oxirane peak at 915 cm '. confirming that all epoxide rings have undergone a reaction despite the absence of a catalyst. The spectral pattern of curve 610C differs substantially from the other cured formulations, particularly within the region 614C, which reflects the distinct network structure of flexible vitrimer epoxy. The increased hardener content results in a network with reduced crosslink density, increased linear segment formation, and greater chain mobility, thereby imparting flexibility to the material. The curve 610C exhibits a tensile strength of approximately 19.8 MPa and an elongation capacity of up to 170%, making it suitable for applications requiring high flexibility rather than rigidity.
[0093] The peak at approximately 915 cm *, corresponding to the oxirane (epoxide) ring, serves as a vital diagnostic marker in epoxy curing reactions. The disappearance of the peak at approximately 915 cm1provides direct evidence of reaction progression, confirming the complete conversion of epoxide groups upon curing. The oxirane peak further serves as a verification parameter in quality control assessments, ensuring that the final cured material attains optimal mechanical, thermal, and chemical properties. Additionally, the ability to monitor variations in this peak facilitates formulation validation, allowing for the evaluation of different hardener-to-catalyst ratios in achieving complete epoxide conversion. Furthermore, the structural transformation resulting from oxirane ring opening directly correlates with mechanical performance, wherein vitrimer epoxies exhibit hydroxyl group formation, enabling dynamic bond exchange reactions that confer reprocessability characteristics.
[0094] FIG. 7 is a graphical representation illustrating force -displacement curves for various acetal-modified rigid vitrimer epoxy formulations, in accordance withan embodiment of the present disclosure. FIG. 7 is described in conjunction with elements from FIGs 1 to 6C. With reference to FIG. 7, there is shown a graphical representation 700 illustrating force-displacement curves for various acetal-modified epoxy formulations. The force measured in Newton (N) is represented on the ordinate axis. The displacement measured in millimetres (mm) is represented on the abscissa axis. The graphical representation 700 includes a curve 702 representing a vitrimer epoxy with 10% acetal -containing hardener mixed with 11 % accelerator, a curve 704 representing a vitrimer epoxy with 15% acetal -containing hardener mixed with 11% accelerator, a curve 706 representing a vitrimer epoxy with 20% acetal-containing hardener mixed with 11% accelerator, and a curve 708 representing huntsman epoxy.
[0095] The curve 702 exhibits the highest force capacity among the other curves (704, 706, 708), reaching a maximum force of approximately ranging between 700-750N at a displacement of approximately ranging between 1.0-1.1mm. The curve 702 exhibits a relatively smooth elasticity (as illustrated by the straight-line characteristics of the curve 702 till displacement of approximately 0.6-0.8 mm) followed by a well-defined peak (illustrated by a dotted box 710) before failure occurs at approximately 1.3mm displacement. The performance of the curve 702 likely results from the balance between crosslinking density and dynamic bond exchanges enabled by the 10% acetal-containing hardener mixed with 11% accelerator.
[0096] The curve 704 exhibits a slightly lower maximum force capacity of approximately ranging between 500-550N at approximately 1.0-1.1mm displacement. The rigid vitrimer epoxy illustrated by the curve 704 has suitable ductility but experiences a reduction in force compared to the curve 702. The reduction in force indicates that increasing the content of acetal-containing hardener to 15% may introduce additional flexibility but reduces the load-bearing capacity of the rigid vitrimer epoxy formed. The curve 704 maintains a similar profile to the curve 702 but with reduced magnitude.
[0097] The curve 706 exhibits a further reduction in maximum force capacity to approximately ranging between 450-500N at a displacement of approximately 0.8-0.9mm. The rigid vitrimer epoxy illustrated by the curve 706 exhibits a very low range of elasticity and achieves earlier failure, with displacement at break occurring at approximately 1.0mm. The progressive decrease in force capacity with increasing content of the acetal-containing hardener indicates that higher concentrations of acetal groups may compromise the mechanical integrity of the formed vitrimer epoxy.
[0098] The curve 708 shows distinctive mechanical behaviour compared to the curve 702, the curve 704 and the curve 706. The curve 708 exhibits a lower maximum force of approximately ranging between 400-450N indicating the brittle nature of the of the huntsman epoxy. The curve 708, lacking the dynamic bonds found in the acetal-modified rigid vitrimer epoxy formulations, exhibits failure at a displacement of approximately 0.6-0.8 mm, whereas the curve 702 shows failure at a displacement of approximately 1-1.4 mm, indicating better elongation capability. Due to the permanent crosslink network structure, the curve 708 cannot be reprocessed and recycled and also has a relatively lower maximum force as compared to the curve 702, curve 704 and the curve 706.
[0099] FIG. 8 is a graphical representation illustrating a tensile strength of various acetal-based rigid vitrimer epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 8 is described in conjunction with elements from FIGs 1 to 7. With reference to FIG. 8, there is shown a graphical representation 800 illustrating the tensile strength for various acetal-based rigid vitrimer epoxy formulations. The tensile strength measured in megapascals (MPa) is represented on the ordinate axis. The various acetal -based rigid vitrimer epoxy formulations are labelled along the abscissa axis. The graphical representation 800 includes a bar 802 representing tensile strength for huntsman epoxy, a bar 804 representing tensile strength for a vitrimer epoxy with 10% acetal-containing hardener mixed with 11% accelerator, a bar 806 representing tensile strength for a vitrimer epoxy with 15% acetal-containing hardener mixed with 11% accelerator, a bar 808 representingtensile strength for a vitrimer epoxy with 20% acetal-containing hardener mixed with 11% accelerator, and a bar 810 representing tensile strength for a vitrimer epoxy with 40% acetal-containing hardener and no accelerator. The accelerator used in the graphical representation 800 is an aminopropyl imidazole catalyst. The bar 802 represents the huntsman epoxy, exhibiting a tensile strength of approximately 58 MPa. The bar 802 serves as the reference point against which the bar 804, bar 806, bar 808 and bar 810 are compared.
[0100] The bar 804 exhibits an increase in tensile strength to approximately 72 MPa as compared to bar 802. The approximately 24% improvement in the tensile strength of the rigid vitrimer epoxy formulation illustrated by the bar 804 as compared to the bar 802 indicates that incorporating 10% content of the acetal-containing hardener with 11% accelerator improves the mechanical properties of the rigid vitrimer epoxy formed while introducing dynamic crosslinking capabilities. The bar 806 achieves the highest tensile strength among all various acetal-based rigid vitrimer epoxy formulations at approximately ranging between 78 to 82 MPa. The bar 806 exhibits 41% increase in tensile strength as compared to the bar 802. The optimal mechanical performance of the acetal-based rigid vitrimer epoxy formulation associated with the bar 806 provides an ideal balance between existing crosslinking and dynamic acetal exchange networks.
[0101] The bar 808 exhibits a decrease in tensile strength as compared to the bar 802, approximately ranging between 48-52 MPa. The reduction in tensile strength indicates that increasing the content of the acetal-containing hardener beyond 15% begins to compromise the mechanical integrity of the rigid vitrimer epoxy formed, likely due to excessive network flexibility or incomplete curing. The bar 810 exhibits the lowest tensile strength among the bar 802, bar 804, bar 806, and bar 808, approximately ranging between 13-18 MPa. The reduction in tensile strength indicates the reduction in mechanical properties, indicating that the high content of the acetal-containing hardener (40%) without the accelerator results in insufficient crosslinking density and network formation.
[0102] The graphical representation 800 exhibits a comparative analysis between the various acetal-based rigid vitrimer epoxy formulations. The comparative analysis exhibits the relationship between formulation parameters (acetal-containing hardener and accelerator) and mechanical performance, indicating that the vitrimer epoxy with 15% acetal-containing hardener mixed with 11% accelerator achieves an optimal balance of strength and recyclability through dynamic bond exchanges.
[0103] FIG. 9 is a graphical representation illustrating Fourier transform infrared (FTIR) spectroscopy analysis of two acetal-modified epoxy formulations with varying composition ratios, in accordance with an embodiment of the present disclosure. FIG. 9 is described in conjunction with elements from FIGs 1 to 8. With reference to FIG. 9, there is shown a graphical representation 900 representing FTIR spectroscopy analysis of two distinct acetal-modified epoxy formulations. The transmittance percentage is represented on the ordinate axis. The wavenumber is measured in centimetres inverse (cm ') on the abscissa axis. The graphical representation 900 includes a curve 902 representing the FTIR spectrum of a vitrimer epoxy formulation containing 10% amino acetaldehyde dimethyl acetal and 5% aminopropyl imidazole relative to the virgin epoxy resin. The graphical representation 900 further includes a curve 904 representing the FTIR spectrum of a vitrimer epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 5% aminopropyl imidazole relative to the virgin epoxy resin.
[0104] The curve 902 exhibits characteristic absorption bands, including a broad hydroxyl stretching region (illustrated by the dotted box 908), approximately ranging between 3000-3500 cm '. indicating the presence of hydroxyl groups formed during the epoxy ring-opening reaction. The curve 902 further exhibits distinctive C-H stretching vibrations (illustrated by the dotted box 910) approximately ranging between 2700-2900 cm '. carbonyl stretching bands approximately ranging between 1700-1800 cm '. and various C-O-C stretching and bending modes in the fingerprint region below 1500 cm
[0105] The curve 904 exhibits similar functional group signatures as compared to the curve 902 but with subtle differences in peak intensities and positions. In the fingerprint region 906 the curve 904 exhibits various C-O-C stretching and bending modes at approximately ranging between 1500 and 500 cm The broad hydroxyl stretching region 908 at approximately ranging between 3000-3500 cm indicating the presence of hydroxyl groups formed during the epoxy ring-opening reaction, is similar to the curve 902. The variations observed in fingerprint region 906, when comparing curve 904 to curve 902, indicate structural modifications in the network of the vitrimer epoxy formulation, containing 15% amino acetaldehyde dimethyl acetal and 5% aminopropyl imidazole relative to the virgin epoxy resin. The increased concentration of acetal groups provides the structural modifications. Therefore, the changes in crosslinking density and intermolecular interactions are reflected in the spectral shifts and intensity variations of C-O-C stretching and bending modes within the range of 1500 to 500 cm . The curve 902 and the curve 904 show the absence or significant reduction of the characteristic epoxide ring absorption peak at approximately 912 cm '. confirming successful ring-opening and crosslinking reactions in both the curve 902 and the curve 904.
[0106] FIG. 10 is a graphical representation illustrating the tensile strength of various acetal -modified epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 10 is described in conjunction with elements from FIGs 1 to 9. With reference to FIG. 10, there is shown a graphical representation 1000 representing the tensile strength values in megapascals (MPa) for five distinct epoxy formulations. The tensile strength (MPa) is represented on the ordinate axis. The different epoxy formulations are labelled along the abscissa axis. The graphical representation 1000 includes a bar 1002 representing the huntsman epoxy, a bar 1004 representing a vitrimer epoxy formulation containing 10% amino acetaldehyde dimethyl acetal and 11% aminopropyl imidazole catalyst, a bar 1006 representing a vitrimer epoxy formulation containing 10% amino acetaldehyde dimethyl acetal and 5% aminopropyl imidazole catalyst, a bar 1008 representing a vitrimer epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 11% aminopropyl imidazole catalyst and a bar 1010 representing a vitrimerepoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 5% aminopropyl imidazole catalyst. The bar 1002 exhibits a tensile strength of approximately 58 MPa. The huntsman epoxy serves as the reference standard for evaluating the performance enhancements achieved through acetal modification as illustrated in bar 1004, bar 1006, bar 1008 and bar 1010. The bar 1004 demonstrates a tensile strength of approximately 72 MPa, representing a significant 24% improvement in the tensile strength of the vitrimer epoxy formulation illustrated by the bar 1004 as compared to the bar 1002. The enhancement in the tensile strength indicates that the combination of dynamic acetal bonds and 11% aminopropyl imidazole catalyst improves the mechanical properties of the vitrimer epoxy formed while introducing dynamic crosslinking capabilities.
[0107] The bar 1006 exhibits a tensile strength of approximately 67 MPa, which is slightly lower than the bar 1004 but higher than the bar 1002. The bar 1006 indicates that while the reduction in the quantity of aminopropyl imidazole catalyst from 11% to 5% affects mechanical properties, the vitrimer epoxy formulation maintains substantial strength advantages over the Huntsman epoxy. The bar 1008 achieves the highest tensile strength among all the various acetal-modified epoxy formulations shown by the bar 1002, bar 1004, bar 1006, bar 1008 and the bar 1010 at approximately 82 MPa. The increased value of tensile strength indicates that increasing acetal content to 15% while maintaining a high catalyst concentration (11%) creates an ideal balance of conventional and dynamic crosslinking mechanisms. The bar 1010 demonstrates a tensile strength of approximately 73 MPa, which is lower than the bar 1008 but still substantially stronger than the Huntsman epoxy. The vitrimer epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 5% aminopropyl imidazole catalyst achieves a balance of mechanical performance and enhanced reprocessability through the dynamic acetal exchange mechanism while utilizing less quantity of the catalyst.
[0108] FIG. 11 is a graphical representation illustrating differential scanning calorimetry (DSC) analysis of various acetal-modified epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 11 is described inconjunction with elements from FIGs 1 to 10. With reference to FIG. 11, there is shown a graphical representation 1100 depicting the thermal behaviour of various acetal -modified epoxy formulations. The heat flow measured in watt per gram (W / g) is represented on the ordinate axis, while the temperature measured in degrees Celsius (°C) is shown on the abscissa axis. The differential scanning calorimetry (DSC) is a thermal analysis technique used to measure heat flow associated with phase transitions in polymeric materials. The DSC is employed to evaluate the curing behaviour, glass transition temperature, and thermal stability of the various acetal -modified epoxy formulations. As the temperature increases, variations in heat flow indicate exothermic or endothermic events corresponding to curing reactions, molecular rearrangements, or thermal degradation. The thermal analysis provides insights into the network architecture, crosslinking efficiency, and reprocessability of the various acetal-modified epoxy formulations. The graphical representation 1100 includes a curve 1102 representing the permanent epoxy, the curve 1104 representing an acetal-modified epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 11% aminopropyl imidazole, and the curve 1106 representing an acetal-modified epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 5% aminopropyl imidazole.
[0109] The curve 1102 exhibits a smooth thermal profile with a gradually decreasing heat flow as temperature increases. The behaviour of the curve 1102 is characteristic of a conventional thermosetting polymer with permanent crosslinks that limit molecular mobility during thermal transitions. The curve 1104 exhibits a distinct thermal response compared to the curve 1102, with subtle transitions observed in aregion 1108. The variations in the region 1108 represent the activation of dynamic bond exchange facilitated by the acetal groups and catalysed by the aminopropyl imidazole. The curve 1106 exhibits thermal behaviour intermediate between the curve 1102 and the curve 1104. The behaviour of the curve 1106 indicates that the 5% aminopropyl imidazole influences not only mechanical properties but also thermal transitions and dynamic exchange rates. The region 1108 indicates the temperature range where differences in dynamic behaviour are most apparent among the curve 1102, curve 1104 and the curve 1106.
[0110] FIG. 12 is a graphical representation illustrating thermogravimetric analysis (TGA) of two acetal-modified epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 12 is described in conjunction with elements from FIGs 1 to 11. With reference to FIG. 12, there is shown a graphical representation 1200 depicting the thermal decomposition behaviour of two distinct acetal-modified epoxy formulations. The weight percentage (%) is represented on the ordinate axis, while the temperature (°C) is represented on the abscissa axis. Thermogravimetric analysis (TGA) is a technique used to assess the thermal stability and decomposition characteristics of polymeric materials by measuring weight loss as a function of temperature. The TGA provides insights into the degradation profile of the two acetal-modified epoxy formulations, indicating the temperatures at which thermal decomposition begins and progresses. The weight loss observed at different temperature ranges corresponds to various stages of material breakdown, such as solvent evaporation, bond dissociation, and complete degradation of the polymer network. The graphical representation 1200 includes a curve 1202 representing the acetal-modified epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 5% aminopropyl imidazole, and the curve 1204 representing the acetal-modified epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 11% aminopropyl imidazole.[oni] The curve 1202 exhibits an initial weight retention of approximately ranging between 95-100% at lower temperatures. As the temperature increases, a significant weight loss occurs within the range of approximately 250°C to 400°C, indicating the primary thermal degradation phase. The primary thermal degradation phase occurs due to the breakdown of the polymer structure, resulting from the dissociation of acetal and imidazole-linked crosslinks. Beyond 400°C, the weight stabilizes, suggesting that most of the volatile degradation products have been released, and the remaining residue primarily consists of thermally stable char.
[0112] The curve 1204 follows a similar degradation pattern as compared to the curve 1202 but exhibits differences in thermal stability. The onset of decomposition occurs at a slightly lower temperature compared to the curve 1202, indicating thatthe 11% aminopropyl imidazole content may influence the thermal crosslinking density or bond dissociation characteristics. The major weight loss phase extends within the range of approximately 250°C to 400°C, but the final residual weight fraction is slightly lower, suggesting a reduced char yield. The curve 1204 implies that 11% aminopropyl imidazole content may lead to modifications in the polymer degradation mechanism, affecting the thermal performance and structural integrity of the formulation.
[0113] A line 1206 representing the thermal decomposition temperature at 5% weight loss (Td5%) which is observed around 279°C, while a line 1206 representing the temperature at 30% weight loss 1208 (Td30%) occurs at approximately 349°C.The thermal decomposition temperature parameters are vital for determining the upper-temperature limits for processing and application of the acetal-modified epoxy formulations. The thermal decomposition temperature indicates the suitability of the acetal-modified epoxy formulations for moderately high-temperature applications while maintaining dynamic bond exchange capabilities.
[0114] FIG. 13 is a graphical representation illustrating dynamic mechanical analysis (DMA) of various epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 13 is described in conjunction with elements from FIGs 1 to 12. With reference to FIG. 13, there is shown a graphical representation depicting the temperature-dependent viscoelastic properties of various epoxy formulations. The storage modulus measured in megapascal (MPa) is represented on the ordinate axis, while the temperature measured in degrees Celsius (°C) is represented on the abscissa axis. The dynamic mechanical analysis (DMA) is a technique used to evaluate the viscoelastic behaviour of polymeric materials by measuring the response to an applied oscillatory force over a range of temperatures. The DMA provides insights into the stiffness, elasticity, and mechanical damping characteristics of various epoxy formulations. The storage modulus represents the ability of the material to store mechanical energy, indicating structural rigidity, while variations in modulus with temperature reflect phase transitions, such as the glass transition temperature, which marks the shift from a rigid to a more flexiblestate. The graphical representation 1300 includes a curve 1302, representing the permanent epoxy, the curve 1304, representing the acetal-modified epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 11% aminopropyl imidazole, and the curve 1306, representing an epoxy formulation, which incorporates 15% acetal, 5% catalyst, and 65% silica fdler.
[0115] The curve 1302 exhibits an initial storage modulus of approximately 2000 MPa at 20°C. The curve 1302 exhibits a gradual, nearly linear decrease in storage modulus with increasing temperature until approximately 90°C, followed by a more pronounced decline through the glass transition region 1308. The pronounced decline in the curve 1302 indicates a broad distribution of relaxation times, characteristic of permanent crosslinked networks in the permanent epoxy.
[0116] The curve 1304 exhibits an initial storage modulus of approximately ranging between 2200-2400 MPa at 20°C but undergoes the earliest and most rapid decline in storage modulus with increasing temperature among the curve 1302, 1304 and the curve 1306. The storage modulus for the curve 1304 decreases steeply between 40-70°C, indicating a lower glass transition temperature and enhanced molecular mobility facilitated by the dynamic acetal bonds and higher catalyst concentration.
[0117] The curve 1306 exhibits the highest initial storage modulus of approximately ranging between 2500-2800 MPa at 20°C. The value of storage modulus indicates the substantial reinforcing effect of silica fdler on mechanical rigidity. The curve 1306 maintains high modulus values up to approximately 80°C, after which the curve 1306 experiences a relatively steep decline through the glass transition region 1310, eventually reaching complete softening around 120°C.
[0118] FIG. 14 is a graphical representation illustrating the storage modulus at room temperature of three epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 14 is described in conjunction with elements from FIGs 1 to 13. With reference to FIG. 14, there is shown a graphical representation 1400 representing the storage modulus values in megapascals (MPa) for threedistinct epoxy formulations measured at room temperature. The storage modulus (MPa) is represented on the ordinate axis. The different epoxy formulations are labelled along the abscissa axis. The graphical representation 1400 includes a bar 1402 representing the permanent epoxy, a bar 1404 representing the epoxy formulation with 15% amino acetaldehyde dimethyl acetal and 5% aminopropyl imidazole catalyst, and a bar 1406 representing the epoxy formulation with 15% amino acetaldehyde dimethyl acetal and 11% aminopropyl imidazole catalyst.
[0119] The bar 1402 exhibits a storage modulus of approximately ranging between 1900-2000 MPa at room temperature. The bar 1402 serves as the reference standard for evaluating the viscoelastic performance of the bar 1404 and the bar 1406.
[0120] The bar 1404 demonstrates a storage modulus of approximately ranging between 2100-2200 MPa, representing an 8% improvement over the bar 1402. The increase in the value of storage modulus for the bar 1404 indicates that the combination of 15% amino acetaldehyde dimethyl acetal and 5% aminopropyl imidazole catalyst creates a network structure in the epoxy formulation that has improved rigidity as compared to the bar 1402 while maintaining dynamic characteristics.
[0121] The bar 1406 achieves the highest storage modulus of approximately ranging between 2200-2300 MPa, representing a 15% improvement over the bar 1402 and a 6% increase compared to the bar 1404. The bar 1406 indicates that an increase in catalyst concentration from 5% to 11% improves both the formation of the initial network structure and the dynamic bond exchange processes in the forming epoxy, resulting in enhanced mechanical rigidity at room temperature.
[0122] FIG. 15 is a graphical representation illustrating force-displacement curves for various epoxy formulations, in accordance with embodiments of the present disclosure. FIG. 15 is described in conjunction with elements from FIGs 1 to 14.
[0123] With reference to FIG. 15, there is shown a graphical representation 1500 depicting force-displacement characteristics of two distinct epoxy formulations. The force measured in Newton (N) is represented on the ordinate axis, against displacement measured in millimetres (mm) represented on the abscissa axis. The graphical representation 1500 includes a curve 1502 representing the permanent epoxy formulation and a curve 1504 representing the 65% silica-fdled high-performance epoxy (HPE) formulation.
[0124] The curve 1502 exhibits a gradual increase in force, reaching a maximum force of approximately ranging between 500-600 N at a displacement of approximately 0.6 mm. The curve 1502 exhibits elastic characteristics for a range approximately between 0-600N. The curve 1502 is used as a reference curve to compare the elasticity and stiffness with the curve 1504. The curve 1504 exhibits a steeper initial slope as compared to the curve 1502, thereby indicating a higher stiffness and elastic modulus. The curve 1504 reaches a significantly higher maximum force as compared to the curve 1502 of approximately 650 N at a displacement of approximately 0.4 mm before experiencing a sudden drop in force at point 1506, characteristic of brittle fracture behaviour. The value of maximum force indicates that the improved mechanical performance can be attributed to the reinforcement effect of the 65% silica filler in the epoxy. The 65% silica filler creates a rigid three-dimensional network structure within the epoxy matrix.
[0125] The significant disparity in mechanical performance between the curve 1502 and the curve 1504 exhibits the effect of silica filler incorporation on the force displacement characteristics of epoxy formulation. The acetal exchange -based vitrimer combined with silica loading results in superior load-bearing capacity, which is useful in high-performance structural applications requiring enhanced mechanical properties while maintaining recyclability.
[0126] FIG. 16 is a graphical representation illustrating tensile strength comparison between various epoxy formulations, in accordance with embodiments of the present disclosure. FIG. 16 is described in conjunction with elements from FIGs 1 to 15. With reference to FIG. 16, there is shown a graphical representation1600 comparing the tensile strength values in megapascals (MPa) for various epoxy formulations. The tensile strength (MPa) is represented on the ordinate axis ranging, while the various epoxy formulations are labelled along the abscissa axis. The graphical representation 1600 includes a bar 1602 representing the permanent Huntsman epoxy formulation and a bar 1604 representing the 65% silica-filled permanent epoxy (PE) formulation.
[0127] The bar 1602 represents the tensile strength of the permanent Huntsman epoxy, which falls within the range of approximately 50 MPa to 60 MPa. The value of tensile strength establishes the baseline mechanical performance of the epoxy material without any additional modifications. The tensile strength refers to the maximum stress the epoxy material can withstand while being stretched or pulled before breaking. The measured tensile strength of the permanent Huntsman epoxy indicates the ability of the permanent Huntsman epoxy to resist mechanical deformation under tensile loads.
[0128] The bar 1604 represents the tensile strength of the 65% silica-filled permanent epoxy (PE) formulation, exhibiting a higher value of approximately ranging between 70-80 MPa. The increase in tensile strength indicates an enhancement of approximately 25% as compared to the bar 1602. The improvement in the mechanical performance of the bar 1604 can be attributed to the reinforcing effect of the 65% silica-filled permanent epoxy (PE) formulation, which enhances load distribution, increases intermolecular interactions, and improves the overall structural integrity of the epoxy formed. The silica particles serve as stress-transfer elements, distributing applied tensile loads throughout the polymer network and impeding crack propagation pathways, thereby enhancing the overall mechanical integrity of the epoxy formed.
[0129] FIG. 17 is a graphical representation illustrating force-displacement curves for various acetal-based vitrimer epoxy formulations, in accordance with embodiments of the present disclosure. FIG. 17 is described in conjunction with elements from FIGs 1 to 16. With reference to FIG. 17, there is shown a graphical representation 1700 depicting force-displacement characteristics for various acetal-based vitrimer epoxy formulations. The force measured in Newton (N) is represented on the ordinate axis. The displacement measured in millimetres (mm) is represented on the abscissa axis. The graphical representation 1700 includes a curve 1702 representing an epoxy formulation containing 15% hardener and 11% aminopropyl imidazole and a curve 1704 representing an epoxy formulation containing the 65% silica-fdled with 15% hardener and 11% aminopropyl imidazole.
[0130] The curve 1702 exhibits a gradual increase in force with displacement, reaching a maximum force of approximately 700-800 N at a displacement of about 1.0 mm before experiencing a moderate decrease in force. The behaviour of the curve 1702 is characteristic of ductility with significant deformation capability of the epoxy formulation containing 15% hardener and 11% aminopropyl imidazole. The deformation capability of the curve 1702 is due to the dynamic covalent acetal exchange networks present in the epoxy formulation containing 15% hardener and 11% aminopropyl imidazole.
[0131] The curve 1704 exhibits a steeper initial slope, indicating higher stiffness as compared to the curve 1702. The curve 1704 reaches a maximum force of approximately ranging between 750-800 N at a lower displacement of about 0.5 mm, followed by an abrupt decrease in force. The behaviour of the curve 1704 indicates a transition to a more brittle fracture region starting from point 1706 upon the incorporation of 65% silica fdler in the vitrimer epoxy formulation containing 15% hardener and 11% aminopropyl imidazole.
[0132] FIG. 18 is a graphical representation illustrating tensile strength comparison between three distinct epoxy formulations, in accordance with embodiments of the present disclosure. FIG. 18 is described in conjunction with elements from FIGs 1 to 17. With reference to FIG. 18, there is shown a graphical representation 1800 for three distinct epoxy formulations. The tensile strength (MPa) is represented on the ordinate axis. The different epoxy formulations are labelled along the abscissa axis. The graphical representation 1800 includes a bar 1802 representing an epoxy formulation containing 15% hardener and 11%aminopropyl imidazole, a bar 1804 representing an epoxy formulation containing 65% silica-filled with 15% hardener and 11% aminopropyl imidazole, and bar 1806 representing an epoxy formulation containing 65% silica in Huntsman PE formulations.
[0133] The bar 1802 exhibits the highest tensile strength among the bar 1802, bar 1804 and bar 1806 at approximately 82 MPa. The bar 1802 exhibits the mechanical properties of the vitrimer epoxy formed using an acetal-containing hardener. The increased tensile strength indicates the superior mechanical performance of the bar 1802 as compared to the bar 1804 and the bar 1806. The high value of tensile strength indicates the strong crosslinking network formed by the acetal-containing hardener. The presence of aminopropyl imidazole enhances intermolecular interactions in the vitrimer epoxy, contributing to improved load-bearing capacity and structural integrity under tensile stress.
[0134] The bar 1804 exhibits a lower tensile strength of approximately 73 MPa, indicating an approximately 11% decrease in tensile strength as compared to the bar 1802. The introduction of silica as a fdler affects the mechanical properties of the vitrimer epoxy, leading to a reduction in tensile strength compared to the formulation represented by the bar 1802. The measured tensile strength of the bar 1804 indicates that while silica provides reinforcement, the silica may also affect the flexibility and stress distribution, leading to a compromise in the overall tensile performance of the formed vitrimer epoxy.
[0135] The bar 1806 exhibits a tensile strength of approximately 74 MPa. The observed tensile strength indicates that the vitrimer epoxy retains a significant portion of mechanical properties while benefiting from the enhancements in durability and thermal stability provided by the silica microparticles.
[0136] The graphical representation 1800 indicates that the bar 1804 and the bar 1806 shows similar tensile strength approximately ranging between 72-75 MPa. The bar 1804 and the bar 1806 have 65% silica filled indicating that the introduction of dynamic covalent bonds in the bar 1804 does not compromise the mechanicalintegrity of the thermoset polymer, even at high filler loadings, while simultaneously imparting valuable reprocessability characteristics that are absent in the huntsman PE formulation.
[0137] Modifications to embodiments of the present disclosure described in the foregoing are possible without departing from the scope of the present disclosure as defined by the accompanying claims. Expressions such as "including", "comprising", "incorporating", "have", "is" used to describe and claim the present disclosure are intended to be construed in a non-exclusive manner, namely allowing for items, components or elements not explicitly described also to be present. Reference to the singular is also to be construed to relate to the plural. The word "exemplary" is used herein to mean "serving as an example, instance or illustration". Any embodiment described as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments and / or to exclude the incorporation of features from other embodiments. The word "optionally" is used herein to mean "is provided in some embodiments and not provided in other embodiments" . It is appreciated that certain features of the present disclosure, which are, for clarity, described in the context of separate embodiments, may also be provided in combination in a single embodiment. Conversely, various features of the present disclosure, which are, for brevity, described in the context of a single embodiment, may also be provided separately or in any suitable combination or as suitable in any other described embodiment of the disclosure.
Claims
CLAIMSWe claim:
1. A vitrimer epoxy comprising :a virgin epoxy resin; andan acetal-containing hardener in an amount of 5-50 weight percent relative to the virgin epoxy resin,wherein the vitrimer epoxy contains dynamic covalent acetal linkages that form a cross-linked network, wherein the cross-linked network possesses dynamic bond exchange capability via trans-acetalization reactions when heated above a predetermined temperature threshold, resulting in a material exhibiting permanent crosslinking characteristics at temperatures below the predetermined temperature threshold and stress relaxation with retained structural integrity at temperatures above the predetermined temperature threshold.
2. The vitrimer epoxy as claimed in claim 1, further comprising an accelerator in an amount of 2.5-20 weight percent relative to the virgin epoxy resin.
3. The vitrimer epoxy as claimed in claim 2, wherein the accelerator comprises 1 -(3 -aminopropyl) imidazole.
4. The vitrimer epoxy as claimed in claim 1, wherein the acetal- containing hardener comprises amino acetaldehyde dimethyl acetal.
5. The vitrimer epoxy as claimed in claim 1, wherein the acetal- containing hardener is present in an amount of 10-20 weight percent relative to the virgin epoxy resin to produce a rigid vitrimer epoxy having a tensile strength of 70-85 MPa.
6. The vitrimer epoxy as claimed in claim 1, wherein the acetal- containing hardener is present in an amount of 30-50 weight percent relative to the virgin epoxy resin to produce a flexible vitrimer epoxy having a tensile strength of 15-25 MPa.
7. The vitrimer epoxy as claimed in claim 1, further comprising silica microparticles having a particle size of less than 45 micrometres in an amount of 50-80 weight percent relative to the total composition.
8. A method (100) for synthesizing a vitrimer epoxy, the method (100) comprising:preheating a virgin epoxy resin;adding an acetal-containing hardener to a preheated virgin epoxy resin to obtain an intermediate mixture;degassing the intermediate mixture for a predetermined time to obtain a degassed mixture; andcuring the degassed mixture through a staged thermal cycle to obtain the vitrimer epoxy, wherein the vitrimer epoxy contains dynamic covalent acetal linkages that form a cross-linked network, wherein the cross-linked network possesses dynamic bond exchange capability via trans acetalization reactions when heated above a predetermined temperature threshold, resulting in a material exhibiting permanent crosslinking characteristics at temperatures below the predetermined temperature threshold and stress relaxation with retained structural integrity at temperatures above the predetermined temperature threshold.
9. The method (100) as claimed in claim 8, further comprising adding an accelerator to the intermediate mixture prior to degassing.
10. The method (100) as claimed in claim 9, wherein the accelerator comprises 1 -(3 -aminopropyl) imidazole in an amount of 2.5-20 weight percent relative to the virgin epoxy resin.
11. The method (100) as claimed in claim 9, wherein the acetal-containing hardener is used in an amount of 10-20 weight percent and the accelerator is used in an amount of 5-11 weight percent relative to the virgin epoxy resin to produce a rigid vitrimer epoxy having a tensile strength of 70-85 MPa.
12. The method (100) as claimed in claim 8, wherein the preheating of the virgin epoxy resin is carried out at a temperature between 40-80 degrees Celsius with stirring at 200-400 rpm for 20-30 minutes.
13. The method (100) as claimed in claim 8, wherein the acetal -containing hardener comprises amino acetaldehyde dimethyl acetal in an amount of 5-50 weight percent relative to the virgin epoxy resin.
14. The method (100) as claimed in claim 8, wherein the staged thermal cycle comprises sequential heating at 80°C, 100°C, 120°C, and 140°C, each temperature maintained for 2-4 hours.
15. The method (100) as claimed in claim 8, further comprising adding silica microparticles having a particle size of less than 45 micrometres in an amount of 50-80 weight percent relative to the total composition after adding the acetal -containing hardener.
16. The method (100) as claimed in claim 8, wherein the acetal-containing hardener is used in an amount of 30-50 weight percent relative to the virgin epoxy resin to produce a flexible vitrimer epoxy having a tensile strength of 15-25 MPa.