Method for recycling thermoset polymers

The use of vitrimer epoxy with dynamic covalent acetal linkages enables the recycling of thermoset polymers, maintaining mechanical strength and thermal stability while allowing recyclability and reprocessability, addressing the non-recyclability of thermoset polymers and environmental waste issues.

WO2026234688A1PCT designated stage Publication Date: 2026-11-12INDIAN INSTITUTE OF SCIENCE +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IN2026/050691
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-04-15
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Thermoset polymers are non-recyclable and non-reprocessable due to their irreversible cross-linked structure, leading to significant waste generation and environmental pollution, while thermoplastics lack the mechanical strength and thermal stability of thermoset polymers.

Method used

A method involving the use of vitrimer epoxy with dynamic covalent acetal linkages, which allows for recycling by grinding into particles, incorporating these particles into preheated virgin epoxy resin, and curing through a staged thermal cycle to maintain mechanical properties and enable recyclability.

Benefits of technology

The method achieves a sustainable closed-loop system with efficient reprocessing and retention of mechanical properties, minimizing material degradation and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IN2026050691_12112026_PF_FP_ABST
    Figure IN2026050691_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A method (100) for recycling thermoset polymers includes providing a vitrimer epoxy containing a virgin epoxy resin crosslinked with an acetal-containing hardener, where the vitrimer epoxy has dynamic covalent acetal linkages The 5 method (100) further includes grinding the vitrimer epoxy into ground particles, preheating a virgin epoxy resin, and incorporating the ground particles into the preheated virgin epoxy resin. An acetal-containing hardener is then added to the mixture of virgin epoxy resin and ground particles. The method (100) also involves degassing the resulting mixture and curing the degassed mixture through a staged 10 thermal cycle. The resulting recycled material maintains the mechanical properties of the original vitrimer epoxy.
Need to check novelty before this filing date? Find Prior Art

Description

METHOD FOR RECYCLING THERMOSET POLYMERSTECHNICAL FIELD

[0001] The present disclosure relates to a field of thermoset polymers. Moreover, the present disclosure relates to a method for recycling thermoset polymers.BACKGROUND

[0002] Thermoset polymers are permanently cross-linked polymers widely used in various industrial applications due to their enhanced mechanical properties, thermal stability, and chemical resistance. The thermoset polymers are useful in electrical applications, including circuit breakers, switch gears, switchboards, transformers, and reclosers. However, the irreversible cross-linked structure of the thermoset polymers makes them non-recyclable and non-reprocessable, resulting in significant waste generation, environmental pollution, and increased landfill burden. The challenge of recycling and reprocessing the thermoset polymer remains a vital issue in sustainable material development.

[0003] The challenge of recycling and reprocessing the thermoset polymer may be solved by using existing thermoplastics. The existing thermoplastics offer recyclability and reprocessability through melting and reshaping, but they lack high-temperature dimensional stability and chemical resistance like thermoset polymers. Thus, there exists a technical problem of how to recycle a thermoset polymer that retains the mechanical strength and thermal stability of thermoset polymers while enabling recyclability and reprocessability like thermoplastics.

[0004] Therefore, in light of the foregoing discussion, there exists a need to overcome the aforementioned drawbacks.SUMMARY

[0005] The present disclosure provides a method for recycling thermoset polymers. The present disclosure addresses the technical problem of how to recycle a thermoset polymer that retains the mechanical strength and thermal stability of thermoset polymers while enabling recyclability and reprocessability like thermoplastics. An aim of the present disclosure is to provide a solution that overcomes at least partially the problems encountered in the prior art and provides an improved method of recycling thermoset polymers featuring a reversible crosslinking network that enables efficient reprocessing, enhanced mechanical properties retention, and compatibility with industrial-scale recycling processes while minimizing material degradation and environmental impact.

[0006] In one aspect, the present disclosure provides a method for recycling thermoset polymers, the method comprising:providing the vitrimer epoxy comprising a virgin epoxy resin crosslinked with an acetal-containing hardener, wherein the vitrimer epoxy contains dynamic covalent acetal linkages;grinding the vitrimer epoxy into ground particles;preheating a virgin epoxy resin;incorporating the ground particles into the preheated virgin epoxy resin; adding an acetal-containing hardener to the mixture of virgin epoxy resin and ground particles;degassing the resulting mixture; andcuring the degassed mixture through a staged thermal cycle, wherein the resulting recycled material maintains mechanical properties of the original vitrimer epoxy.

[0007] The method for recycling thermoset polymers creates a sustainable closed-loop system by utilising the dynamic bond exchange capabilities of vitrimer epoxy. Incorporating dynamic covalent acetal linkages enables efficient reprocessingthrough grinding into particles suitable for reintegration. The combination of the optimal particle size and weight percentage of ground particles creates an ideal balance of interfacial surface area and polymer network integrity, maximizing the potential for dynamic bond exchange while maintaining processing feasibility. Adding the ground particles into preheated virgin epoxy resin ensures uniform dispersion and compatibility with the vitrimer epoxy formed, with the particle dimensions specifically optimized to allow effective infiltration by the preheated virgin epoxy resin. Further, the addition of acetal-containing hardener establishes chemical integration pathways through trans-acetalization reactions, enhancing the interfacial bonding between recycled thermoset polymer and the virgin epoxy resin. The recycling of the thermoset polymer is further optimized through catalyst concentration, which balances reaction kinetics with polymer network stability. The degassing eliminates entrapped air, preventing void formation and ensuring the structural integrity of the recycled thermoset polymer, which is useful when incorporating higher percentages of ground particles. The staged thermal curing process facilitates dynamic bond exchange, allowing seamless integration of the ground particles while maintaining the mechanical performance of the recycled thermoset polymer.

[0008] Additional aspects of the present disclosure would be made apparent from the drawings and the detailed description of the illustrative implementations construed in conjunction with the appended claims that follow.BRIEF DESCRIPTION OF THE DRAWINGS

[0009] The summary above, as well as the following detailed description of illustrative embodiments, is better understood when read in conjunction with the appended drawings. For the purpose of illustrating the present disclosure, exemplary constructions of the disclosure are shown in the drawings. However, the present disclosure is not limited to specific methods and instrumentalities disclosed herein. Moreover, those in the art will understand that the drawings are not to scale. Wherever possible, like elements have been indicated by identical numbers.

[0010] Embodiments of the present disclosure will now be described, by way of example only, with reference to the following diagrams wherein:FIG.l is a flowchart illustrating a method for recycling thermoset polymers, in accordance with an embodiment of the present disclosure;FIG. 2 is a graphical representation illustrating a tensile strength of various regrind epoxy formulations, in accordance with an embodiment of the present disclosure; FIG. 3 is a flowchart illustrating a reaction mechanism for the formation of a recycled thermoset polymer, in accordance with an embodiment of the present disclosure;FIG. 4 is a graphical representation illustrating a tensile strength of various regrind epoxy formulations, in accordance with an embodiment of the present disclosure; FIG. 5 is a graphical representation illustrating force-displacement curves for various regrind epoxy formulations, in accordance with an embodiment of the present disclosure;FIG. 6 is a graphical representation illustrating the tensile strength of various regrind epoxy formulations, in accordance with an embodiment of the present disclosure;FIG. 7 is a graphical representation illustrating the tensile strength of various regrind epoxy formulations, in accordance with an embodiment of the present disclosure;FIG. 8 is a graphical representation illustrating dynamic mechanical analysis (DMA) of various epoxy formulations, in accordance with an embodiment of the present disclosure;FIG. 9 is a graphical representation illustrating dynamic mechanical analysis (DMA) of various epoxy formulations, in accordance with an embodiment of the present disclosure; andFIG. 10 is a graphical representation illustrating the tan delta curves from dynamic mechanical analysis (DMA) of various epoxy formulations, in accordance with an embodiment of the present disclosure.

[0011] In the accompanying drawings, an underlined number is employed to represent an item over which the underlined number is positioned or an item to which the underlined number is adjacent. A non-underlined number relates to an item identified by a line linking the non-underlined number to the item. When a number is non-underlined and accompanied by an associated arrow, the nonunderlined number is used to identify a general item at which the arrow is pointing. DETAILED DESCRIPTION OF EMBODIMENTS

[0012] The following detailed description illustrates embodiments of the present disclosure and ways in which they can be implemented. Although some modes of carrying out the present disclosure have been disclosed, those skilled in the art would recognize that other embodiments for carrying out or practicing the present disclosure are also possible.

[0013] FIG.l is a flowchart illustrating a method for recycling thermoset polymers, in accordance with an embodiment of the present disclosure. With reference to FIG. 1, there is shown a flowchart illustrating a method 100 for recycling thermoset polymers. The method 100 includes steps 102 to 114.

[0014] At step 102, the method 100 includes providing a vitrimer epoxy comprising a virgin epoxy resin crosslinked with an acetal-containing hardener. The vitrimer epoxy refers to a thermoset polymer material that possesses both permanent crosslinks and reversible bond exchange capabilities due to the incorporation of acetal functional groups. The virgin epoxy resin is a thermosetting polymer comprising epoxide functional groups, such as Araldite CY 228-1, which has not been previously cured or processed. The virgin epoxy resin can also comprise diglycidyl ether of bisphenol A (DGEBA) as epoxide functional group. Here, curing refers to a chemical reaction process where the liquid epoxy resin is converted into a hard, infusible, and insoluble three-dimensional network through crosslinking reactions. The acetal-containing hardener refers to a chemical compound containing both amine groups and acetal groups, which serves as the crosslinking agent for the virgin epoxy resin while simultaneously introducingdynamic covalent bonds. The crosslinking agent refers to a molecule capable of reacting with functional groups on multiple polymer chains to form bridges between the chains, creating a three-dimensional network. The vitrimer epoxy is used as the starting material for recycling thermoset polymers, exhibiting the unique dynamic crosslinked structure of the vitrimer epoxy that enables reprocessability. The dynamic covalent acetal linkages within the vitrimer epoxy enable the vitrimer epoxy to undergo controlled bond rearrangements at high temperatures without compromising the overall network integrity. The capacity for bond exchange while maintaining network integrity differentiates vitrimer epoxy from existing thermosets and makes recycling feasible. The vitrimer epoxy material exhibits permanent crosslinking characteristics at normal operating temperatures but gains dynamic bond exchange capabilities when heated above a specific temperature.

[0015] At step 104, the method 100 includes grinding the vitrimer epoxy into ground particles. Grinding refers to the process of mechanical size reduction of the vitrimer epoxy that transforms the vitrimer epoxy into small particles suitable for reincorporation into new polymer formulations such as thermoset polymer. The grinding process utilizes mechanical equipment such as ball mills, cryogenic grinders, or similar size-reduction machinery to apply shear forces that fracture the vitrimer epoxy into smaller particles suitable for reprocessing. The vitrimer epoxy is first broken into coarse fragments using mechanical crushers, then further reduced to predetermined particle size through grinding to achieve suitable particle size distributions. The particle size distribution impacts the recyclability and final properties of the recycled thermoset polymer. The ground particles retain the chemical functionality of the acetal linkages useful for reprocessing through trans-acetalization reactions.

[0016] In an implementation, the ground particles have a size between 60-600 micrometres and are incorporated in an amount of 5-30 weight percent relative to the virgin epoxy resin. The specified size range provides suitable dispersion throughout the virgin epoxy resin while providing sufficient surface area for effective bond exchange during curing. The 5-30 weight percent loading rangeallows for significant waste reduction while maintaining the mechanical integrity of the final product. The particle size distribution influences the rheological properties of the uncured mixture and affects processing parameters such as degassing efficiency and flow characteristics. The upper limit of 30 weight percent represents the maximum loading that maintains processability without compromising the final mechanical properties of the recycled thermoset polymer.

[0017] In an implementation, the ground particles have a size between 66-125 micrometres and are incorporated in an amount of 20 weight percent relative to the virgin resin. For example, when the ground particles with a size of 66 micrometres are incorporated at 20 weight percent into the formulation of the vitrimer epoxy with 15% acetal hardener and 11% accelerator, the formulation allows for effective interfacial bonding between the recycled thermoset polymer and the vitrimer epoxy. The particle size of 66 micrometres creates a larger surface area for the dynamic acetal exchange reactions to occur between the ground particles and the particle network in the vitrimer epoxy. In another example, when the ground particles with a size of 125 micrometres are incorporated at 20 weight percent of the virgin epoxy formulation, the vitrimer epoxy maintains suitable processability while achieving sufficient interfacial bonding through the dynamic acetal exchange bonding. The ground particle size of 125 micrometres provides a balance between processing requirements and the mechanical performance of the recycled thermoset polymer. In another example, when the ground particles with a size of 100 micrometres are incorporated at 20 weight percent, providing sufficient surface area for the dynamic covalent bond exchanges while maintaining reasonable viscosity. The interaction between the ground particles and the particle network of the virgin epoxy resin occurs through the hydroxyl groups and the acetal groups, allowing for suitable formation of the recycled thermoset polymer. The specific loading of 20 weight percent provides the optimized balance between maximizing recycled thermoset polymer and maintaining mechanical performance.

[0018] At step 106, the method 100 includes preheating the virgin epoxy resin. The preheating involves heating the virgin epoxy resin to a predefined temperaturewith temperature control while stirring for a predefined time using equipment such as a hot plate with magnetic stirring capability. The temperature control during preheating helps to achieve proper viscosity without initiating unwanted reactions. Further, the preheating of the virgin epoxy resin reduces the viscosity of the virgin epoxy resin to facilitate the incorporation of ground particles and subsequent mixing with the acetal-containing hardener. In an implementation, the preheating of the virgin epoxy resin is carried out at a temperature between 40-80 degrees Celsius (°C) with stirring at 200-400 rotations per minute (rpm) for 20-30 minutes. The preheated virgin epoxy resin serves as the base material that will bond with the ground particles through the dynamic exchange reactions.

[0019] For example, at a stirring speed of 200 rpm, the movement of the virgin epoxy resin is relatively slow and gentle. The stirring speed of 200 rpm ensures that heat is gradually and uniformly distributed throughout the virgin epoxy resin. However, because the mixing speed is low, the time required to achieve complete heat distribution is longer. Additionally, the slow stirring motion minimizes turbulence, which helps in reducing air entrapment in the virgin epoxy resin. In another example, at 350 rpm, the stirring speed is moderate, meaning that the virgin epoxy resin undergoes more movement, leading to faster heat distribution compared to 200 rpm. Therefore, ensuring that the heat spreads effectively while still keeping air entrapment relatively low. In another example, at 400 rpm, the stirring speed is high. The virgin epoxy resin experiences more rapid movement, leading to quicker heat distribution. However, if the stirring is too aggressive, it might introduce some turbulence, increasing the risk of air bubbles forming within the virgin epoxy resin. The stirring at 400 rpm is carefully controlled to prevent defects in the vitrimer epoxy formed. The process of preheating creates suitable conditions for the subsequent incorporation of an acetal-containing hardener to improve the final quality and performance of the vitrimer epoxy.

[0020] At step 108, the method 100 includes incorporating the ground particles into the preheated virgin epoxy resin. The measured quantity of ground particles relative to the virgin epoxy resin is incorporated into the preheated virgin epoxyresin while maintaining continuous stirring at 200-400 rpm and a temperature between 40-80°C. In an implementation, the incorporation of the ground particles into the preheated virgin epoxy resin can be performed using a high-shear mixer, planetary mixer, or twin-screw extruder to ensure uniform dispersion of ground particles in the preheated virgin epoxy resin. The elevated temperature of the preheated virgin epoxy resin facilitates suitable encapsulation of the ground particles by reducing the viscosity of the virgin epoxy resin. After incorporation of the ground particles into the preheated virgin epoxy resin, a compounded mixture is formed.

[0021] In an implementation, the compounded mixture undergoes bath sonication for 15-30 minutes at a predefined frequency ranging between 40-80 kHz and a power of approximately around 200 W. The bath sonication is a non-contact technique in which the container holding the compounded mixture is placed in a water bath through which ultrasonic waves are transmitted. In an example, the ultrasonic generator operates at 40 kHz with a power output of 200 W, providing sufficient acoustic energy to process the highly viscous mixture without causing premature curing reactions. The bath Bonification allows acoustic energy to pass through the container walls and act on the compounded mixture without direct contact with an ultrasonic probe. The absence of direct contact of the ultrasonic probe with the compounded mixture helps maintain cleanliness and prevents contamination. The frequency of 40 kHz produces larger and more energetic cavitation bubbles, which are effective for breaking up and dispersing dense ground particles. The formation and collapse of tiny bubbles in a liquid due to high-frequency sound waves is known as ultrasonic cavitation. Compared to higher frequencies (approximately ranging from 80 kHz to 200 kHz), which generate smaller cavitation bubbles, lower frequencies (approximately ranging from 20 kHz to 40 kHz) improve particle dispersion in high-viscosity formulations. The 200 W power setting ensures adequate energy transfer to break down silica agglomerates while preventing excessive heating that could accelerate crosslinking reactions prematurely.

[0022] The bath sonication is performed to enhance the dispersion of the ground particles in the virgin epoxy resin, prevent agglomeration, and improve the uniformity of the compounded mixture. The ultrasonic cavitation generated at 40 kHz assists in reducing the ground particle clustering by creating localized pressure variations, which help distribute the ground particles evenly throughout the virgin epoxy resin. Additionally, the bath sonication aids in degassing by removing entrapped air bubbles, thereby reducing void formation in the recycled thermoset polymer. By ensuring homogeneous dispersion, the bath sonication contributes to the retention of the mechanical properties of the vitrimer epoxy, facilitating efficient reprocessing and maintaining the performance characteristics of the recycled thermoset polymer.

[0023] Following the bath sonication, the compounded mixture undergoes additional high-shear mixing to reinforce the uniform dispersion of the ground particles within the virgin epoxy resin. The high-shear mixing is conducted at a controlled speed, approximately ranging from 100 to 400 rpm, ensuring thorough integration of the ground particles into the particle network of the virgin epoxy resin. The applied shear forces further break down any residual particle agglomerates that may persist after bath sonication, promoting a homogeneous mixture. The controlled agitation enhances the interaction between the ground particles and the virgin epoxy resin, optimizing their distribution and preventing phase separation.

[0024] At step 110, the method 100 includes adding an acetal-containing hardener to the mixture of the virgin epoxy resin and ground particles. The measured quantity of acetal-containing hardener is incorporated into the compounded mixture of the preheated virgin epoxy resin and the ground particles while maintaining controlled stirring. In an implementation, the measured quantity of acetal-containing hardener is incorporated into the compounded mixture using a precision digital weighing balance to ensure accurate dosing relative to the weight of the virgin epoxy resin. Once the hardener is weighed, the hardener is gradually added to the mixture of preheated virgin epoxy resin and ground particles under continuous mechanicalstirring using an overhead stirrer equipped with a high-torque motor and a four-blade impeller. The acetal-containing hardener provides reactive amine groups that form crosslinks with the virgin epoxy resin and with epoxy groups on the ground particles. The acetal groups from the acetal-containing hardener form new dynamic linkages within the thermoset polymer, adding to the existing bonds in the ground particles. The addition of acetal-containing hardener provides additional reactive sites for complete network formation between virgin epoxy resin and recycled thermoset polymer, improving the integration of ground particles into the thermoset polymer formed.

[0025] In an implementation, the acetal-containing hardener includes amino acetaldehyde dimethyl acetal in an amount of 5-50 weight percent relative to the virgin epoxy resin. The amino acetaldehyde dimethyl acetal provides both amine functionality for crosslinking with epoxy groups and acetal groups for dynamic exchange reactions. In another implementation, the acetal containing-hardener includes amino acetaldehyde diethyl acetal, 4-aminobutyraldehyde dimethyl acetal, 3-aminobenzaldehyde ethylene acetal, 2-methyl-l,3-dioxolan-2-yl methanamine, 3-(2-methyl-l,3-dioxolan-2-yl)-l-propanamine, methyl amino acetaldehyde dimethyl acetal, n-(2,2-dimethoxy ethyl) prop-2-enamide, 2-(cbz-amino)acetaldehyde dimethyl acetal, n-(2,2-dimethoxyethyl)-4-methoxy-l,3-benzodioxole-5-methanamine, n-(2,2-dimethoxyethyl)-4-methylbenzenesulfonamide, hydroxy acetaldehyde dimethyl acetal, hydroxy acetaldehyde diethyl acetal, 2 -hydroxy-2 -phenylpropionaldehyde dimethyl acetal, 2-methyl-3-hydroxypentanal dimethyl acetal, 4-(2,2-dimethoxy ethyl) phenol, 4-(hydroxymethyl)benzaldehyde dimethyl acetal, 4-amino-3-(2,2-dimethoxy-ethyl) phenol, 3-(l,3-dioxolan-2-yl) phenol, l,3-dioxolane-2-methanol, (2-methyl-l,3-dioxolan-4-yl) methanol, 2-ethyl-l,3-dioxolane-4-methanol, 2-ethyl-2-methyl-l,3-dioxolane-4-methanol, 2 -methyl -2 -phenyl- 1 ,3-dioxolane-4-methanol, 2-ethyl-2-phenyl-l,3-dioxolane-4-methanol, 4-(2-ethyl-l,3-dioxolan-2-yl) phenol, 2,2-dimethyl- 1 ,3 -dioxolane-4-methanol, 2,2-diethyl- 1 ,3 -dioxolane-4-methanol, 2-methyl- 1 ,3 -dioxolane-2 -methanol, 2-(2 -methyl- 1 ,3 -dioxolan-2-yl)- 1,1-diphenylethanol, 2-ethyl-2-methyl-l,3-dioxolane-4-methanol, 2-(dimethyl amino)-4-(2-methyl- 1 ,3 -dioxolan-2-yl) phenol, 2-isobutyl -2 -methyl- 1 ,3 -dioxolane-4-methanol, 2,2-bis(propan-2-yl)-l,3-dioxolan-4-yl] methanol, 2-[2-(l -hydroxy-2 -nitroethyl) phenyl] acetaldehyde dimethyl acetal, l-(2,2-dimethoxyethyl)-5-methoxy-6-(methoxycarbonyl)-4-oxo- l,4-dihydropyridine-3 -carboxylic acid. The concentration range of 5-50 weight percent allows for customization based on the desired mechanical properties and processing characteristics. The amino group reacts with the epoxide rings of the virgin epoxy resin to form the primary crosslinked network structure. The acetal functionality enables the trans-acetalization reactions that integrate the ground particles into the new network during curing.

[0026] In an implementation, the method 100 further includes adding an accelerator to the compounded mixture prior to degassing. The accelerator refers to a chemical compound that increases the rate of reaction between the virgin epoxy resin and acetal-containing hardener, providing efficient network formation at moderate temperatures and ensuring efficient curing in the presence of ground particles. The addition of accelerator allows for the complete conversion of epoxy groups at moderate temperatures and reasonable cure times. The accelerator catalyses both the primary network formation in the compounded mixture and the dynamic exchange reactions with the ground particles. The inclusion of the accelerator improves the integration of ground particles into the particle network of the compounded mixture by facilitating the trans -acetalization reactions between the virgin epoxy resin and the ground particles, forming a resulting mixture.

[0027] In an implementation, the accelerator includes I-(3-aminopropyl) imidazole in an amount of 2.5-20 weight percent relative to the virgin epoxy resin. I-(3-aminopropyl) imidazole acts as a highly efficient catalyst for epoxy-amine reactions through the nucleophilic attack of the imidazole moiety. In another implementation, the accelerator may comprise 1 -methyl imidazole, 2-methylimidazole, 2-ethyl-5 -methyl- Ih-imidazole, l-benzyl-2-methylimidazole, 2-aminoimidazole, hydroxy methylimidazole, 1 -(2 -hydroxyethyl) imidazole, l-(p-hydroxyphenyl)imidazole, hydroxymethyl-5 -methyl imidazole, 2 -hydroxy- Ih-imidazole-4-carboxylic acid, l-methylimidazole-5 -carboxylic acid, ethyl 1-methyl-lh-imidazole-5-carboxylate, l-methylimidazole-4, 5 -dicarboxylic acid, ethyl 2-amino-lh-imidazole-4-carboxylate, 2-amino-3-methyl-3h-imidazole-4-carboxylic acid ethyl ester, methyl 1 -benzyl- lh-imidazole-5 -carboxylate, ethyl 5-methyl-2-phenyl- lh-imidazole-4-carboxylate, ethyl 1 -benzyl-5 -methyl- lh-imidazole-4-carboxylate, lh-imidazole-4-carboxamide, 1 -methyl- lh-imidazole-4-carboxamide, 5-amino- 1-methyl- lh-imidazole-4-carboxamide, 5-amino- 1 -propyl- Ih-imidazole-4-carboxamide, 5-hydroxy-lh-imidazole-4-carboxamide, histidine, histamine. The concentration range of 2.5-20 weight percent allows for the optimization of cure kinetics based on the specific formulation and processing requirements. The imidazole functionality provides rapid initiation of the crosslinking reaction, while the amine group offers additional catalytic activity. The specific structure of l-(3-aminopropyl) imidazole promotes uniform network formation throughout the mixture of virgin epoxy and the ground particles.

[0028] At step 112, the method 100 includes degassing the resulting mixture. The degassing refers to the process of removing entrapped air bubbles and volatile compounds from a polymer mixture through the application of vacuum or other pressure reduction techniques such as thermal reduction and membrane degasification. The entrapped air bubbles and volatile compounds may create voids or defects in the final cured material. In an implementation, the degassing involves placing the mixture of virgin epoxy resin, ground particles, and the acetal-containing hardener in a vacuum chamber and applying reduced pressure for a predefined time. In another implementation, the degassing can also be performed using a planetary centrifugal mixer equipped with a vacuum function. The planetary centrifugal mixer simultaneously mixes and degasses the compounded mixture by subjecting the compounded mixture to high-speed rotation and revolution under reduced pressure, thereby eliminating entrapped air and volatile gases efficiently. The degassing removes entrapped air bubbles and volatile compounds that may create voids or defects in the thermoset polymer formed. The degassing isperformed due to the irregular shape of ground particles, which can trap additional air during mixing. The degassing improves structural integrity by eliminating air bubbles that would otherwise create stress concentration points and compromise the mechanical properties of the recycled thermoset polymer. The removal of such air bubbles provides consistent curing reactions throughout the recycled thermoset polymer. Thereby, improving the integration of ground particles into the particle network of the virgin epoxy resin. Further, the degassing provides homogeneity in the recycled thermoset polymer.

[0029] At step 114, the method 100 includes curing the degassed mixture through the staged thermal cycle. The curing process involves placing the degassed mixture in a laboratory oven or similar heating equipment with precise temperature control capabilities, followed by subjecting the degassed mixture to a sequence of temperature increases with predefined hold times. In an implementation, the staged thermal cycle progresses from 50°C to 150°C, with each temperature level maintained for 1-3 hours, resulting in a total curing duration of 6-10 hours. The initial curing phase at 50°C allows for the gradual activation of the acetal -containing hardener, preventing uncontrolled exothermic reactions. The initial curing phase aids in the uniform diffusion of reactive components in the resulting mixture and minimizes localized heat buildup, ensuring an even reaction profile throughout the resulting mixture. Following the initial phase, the temperature is increased to 80°C, initiating preliminary crosslink formation between the epoxy groups and the acetal-containing hardener. At 80°C, nucleophilic attack by amino groups on the epoxy rings begins, creating an initial polymeric framework. The moderate heat level prevents premature vitrification while ensuring sufficient mobility of the reactive species for uniform crosslinking.

[0030] The temperature is increased to 100°C to accelerate reaction kinetics, strengthening the crosslinked network while allowing stress relaxation to minimize internal strain in the recycled thermoset polymer. The 100°C temperature facilitates dynamic bond exchange through trans-acetalization, allowing stress-induced rearrangements that enhance the long-term durability of the recycled thermosetpolymer. Further, at 120°C, the curing process transitions into an advanced stage where the thermoset polymer surpasses its glass transition temperature, resulting in increased chain mobility. The increased chain mobility ensures that residual reactive groups effectively participate in crosslinking, improving network density. The reversible covalent bond formation between hydroxyl groups and acetal moieties intensifies, solidifying the reprocessability of the vitrimer epoxy while enhancing its mechanical performance.

[0031] The temperature is then elevated to 140°C, marking the post-curing phase. At the post-curing phase, the polymer network reaches near-complete crosslinking, with any remaining functional groups reacting to maximize mechanical strength. The thermoset polymer undergoes further stabilization, ensuring the formation of a well-structured, resilient polymer matrix. The dynamic bond exchange mechanism remains active, preserving the ability of the recycled thermoset polymer to undergo future reprocessing without significant degradation. A final curing step at 150°C is applied to ensure complete thermal stabilization and to drive any remaining reactions to completion. The final curing step eliminates residual unreacted groups, providing the recycled thermoset polymer with optimal tensile strength, impact resistance, and thermal stability. The final temperature held at 150°C for 1-2 hours ensures that the recycled thermoset polymer achieves full mechanical potential while retaining its adaptable characteristics.

[0032] The staged thermal curing facilitates controlled network formation between the polymer network of the virgin epoxy resin and the ground particles while simultaneously promoting trans-acetalization reactions between the virgin epoxy resin and the ground particles. During the curing process, the acetal groups in both the acetal-containing hardener and the ground particles participate in dynamic exchange reactions, effectively integrating the ground particles into the polymer network of the virgin epoxy resin. The carefully controlled temperature stages allow for suitable network development while minimizing internal stresses, which is useful in recycled thermoset polymers containing ground particles with different thermal expansion characteristics.

[0033] In an implementation, the recycled material maintains at least 70% of the tensile strength of a corresponding material made entirely from the virgin epoxy resin. The high strength retention demonstrates the effectiveness of the dynamic exchange reactions in integrating the ground particles into the vitrimer epoxy. The 70% strength retention threshold represents a significant achievement in thermoset recycling, far exceeding what would be possible with conventional thermosetting resins. The mechanical performance retention validates the vitrimer approach to thermoset recycling and enables closed-loop material circularity. The ability to maintain substantial mechanical properties while incorporating recycled content addresses a long-standing challenge in polymer sustainability and offers apractical solution for reducing thermoset waste.

[0034] For enhancing the mechanical, thermal, and chemical resistance of the recycled thermoset polymer, silica microparticles are added. The method 100 follows the initial step of preheating the virgin epoxy resin (as explained in the step 106). The preheated virgin epoxy resin is added with a predetermined quantity of the acetal -containing hardener (as explained in the step 110).

[0035] In an implementation, the method 100 further includes adding silica microparticles having a particle size of less than 45 micrometres in an amount of 50-80 weight percent relative to the total composition. The silica microparticles function as reinforcing fdlers that enhance mechanical properties and provide electrical insulation characteristics. In an example, an intermediate mixture is prepared by incorporating 50 weight percent silica microparticles relative to the total composition. The virgin epoxy resin is preheated to 60°C, and ground vitrimer epoxy particles are added while stirring continuously. The mixture undergoes bath sonication at 40 kHz and 200 W for 20 minutes to ensure uniform dispersion. Following bath sonication, high-shear mixing at 200 rpm is performed while maintaining a temperature of 50°C. The silica microparticles are gradually introduced under controlled agitation to prevent agglomeration. The addition of silica microparticles improves the mechanical strength and dimensional stability ofthe recycled thermoset polymer while maintaining sufficient flexibility for effective stress relaxation and dynamic bond exchange of the recycled thermoset polymer.

[0036] In another example, 65 weight percent silica microparticles are added relative to the total composition. The virgin epoxy resin is preheated to 70°C, and the ground particles are incorporated under continuous stirring. The mixture of the preheated virgin epoxy resin and the ground particles undergoes the bath sonication at 40 kHz and 200 W for 25 minutes, ensuring even dispersion of the ground particles within the preheated virgin epoxy. After the bath sonication, high-shear mixing at 300 rpm is conducted while maintaining the temperature at 65°C to facilitate better interaction between the silica microparticles and the polymer matrix of the mixture of the preheated virgin epoxy resin and the ground particles. The silica microparticles are gradually introduced, allowing controlled incorporation and homogeneous dispersion. The addition of 65 weight percent silica significantly enhances thermal stability, hardness, and tensile strength while maintaining a reasonable degree of processability.

[0037] In yet another example, the intermediate mixture is formulated with 80 weight percent silica microparticles relative to the total composition. The virgin epoxy resin is heated to 75 °C, followed by the incorporation of ground particles under constant stirring. The intermediate mixture undergoes bath sonication at 40 kHz and 200 W for 30 minutes to achieve maximum dispersion. The high-shear mixing at 400 rpm is then performed at a maintained temperature of 80°C, ensuring thorough particle distribution within the polymer matrix. The silica microparticles are introduced in stages to prevent excessive viscosity buildup. The high filler loading of 80 weight percent leads to a densely packed composite with superior mechanical strength, high thermal conductivity, and excellent dimensional stability. The particle size of less than 45 micrometres ensures uniform dispersion within the polymer matrix without interfering with the integration of the ground vitrimer particles. The high loading of 50-80 weight percent is particularly beneficial for electrical applications requiring specific dielectric properties. The silicamicroparticles contribute to dimensional stability and reduced thermal expansion while maintaining the recyclability of the vitrimer system.

[0038] After adding the silica microparticles, the ground particles of the vitrimer epoxy are added, and the bath sonication is performed on the resulting mixture for 15-30 minutes at a predefined frequency of 40 kHz and power of 200 W. After performing the bath sonication, the accelerator is added to the resulting mixture prior to degassing. The next step includes degassing the resulting mixture (as explained in the step 112). The degassed mixture is cured from 50°C to 150°C for 6 to 10 hours.

[0039] The steps 102 to 114 are only illustrative, and other alternatives can also be provided where one or more steps are added, one or more steps are removed, or one or more steps are provided in a different sequence without departing from the scope of the claims herein.

[0040] FIG. 2 is a graphical representation 200 illustrating a tensile strength of various regrind epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 2 is described in conjunction with elements from FIG. 1. The tensile strength measured in megapascals (MPa) is represented on the ordinate axis. The graphical representation 200 includes a bar 202 representing tensile strength for a vitrimer epoxy with 15% acetal -containing hardener mixed with 11% accelerator, a bar 204 representing tensile strength for a vitrimer epoxy with 5 weight percent of vitrimer epoxy regrind particles with particle size greater than 450 micrometers, a bar 206 representing tensile strength for a vitrimer epoxy with 5 weight percent of regrind particles with a size range of 250-450 micrometers, a bar 208 representing tensile strength for a vitrimer epoxy with 5 weight percent of regrind particles with a size range of 125-250 micrometers, and a bar 210 representing tensile strength for a vitrimer epoxy with 5 weight percent of regrind particles with a size range of 66-125 micrometers.

[0041] The bar 202 exhibits a tensile strength of 82 MPa, indicating the excellent mechanical properties of the vitrimer epoxy without any recycled content. The bar202 serves as a reference point against which the performance of all regrind epoxy formulations (indicated by the bar 204, the bar 206, the bar 208, and the bar 210) is compared.

[0042] The bar 204 exhibits a tensile strength of 40 MPa, which is the lowest tensile strength among the bar 202, the bar 206, the bar 208 and the bar 210. The tensile strength of the bar 204 is approximately 49% of the bar 202. The significant reduction in tensile strength can be attributed to the large particle size creating substantial stress concentration points within the polymer network of the bar 204 and providing insufficient surface area for effective interfacial bonding through acetal exchange reactions between the regrind particles and the virgin epoxy resin. The bar 206 exhibits a tensile strength of 53 MPa, which is approximately 65% of the bar 202. The moderate improvement in tensile strength compared to the bar 204 demonstrates the inverse relationship between particle size and mechanical performance. The regrind particles with a size range of 250-450 micrometres in the bar 206 provide better distribution throughout the polymer matrix and increased surface area for dynamic covalent bonding compared to the larger particles in the bar 204.

[0043] The bar 208 exhibits a tensile strength of 58 MPa, which is approximately 71% of the bar 202. The further improvement in tensile strength compared to the bar 206 continues to demonstrate the trend of enhanced mechanical properties with decreasing particle size. The regrind particles with size range of 125-250 micrometres in the bar 208 facilitate improved stress distribution and improved acetal exchange reactions at the interfaces between the regrind particles and the virgin epoxy resin. The bar 210 exhibits a tensile strength of 76 MPa, which is approximately 93% of the bar 202. The bar 210 demonstrates the highest tensile strength among all regrind-containing formulations. The mechanical performance can be attributed to the fine particle size range of 66-125 micrometres, which provides optimal interfacial interaction through maximized surface area, enabling extensive acetal exchange reactions while minimizing stress concentration effects within the polymer network.

[0044] Among the various regrind epoxy formulations, the bar 210 represents the most suitable composition for practical applications where mechanical integrity is vital. The graphical representation 200 indicates that the regrind particles within the size range of 66-125 micrometres enable the most effective integration of recycled vitrimer epoxy while maintaining excellent mechanical properties.

[0045] FIG. 3 is a flowchart 300 illustrating a reaction mechanism for the formation of a recycled thermoset polymer, in accordance with an embodiment of the present disclosure. FIG. 3 is described in conjunction with FIGs. 1 to 2. With reference to FIG. 3, there is shown the flowchart 300 that includes a series of operations from 302 to 308.

[0046] At operation 302, the chemical structure of a virgin epoxy resin containing bisphenol-A units with terminal epoxide groups alongside an amino acetal hardener undergoes an initial curing reaction. The initial curing reaction occurs when the amine group from the amino acetal hardener opens the epoxy ring through a nucleophilic attack. The amino acetal hardener is characterized by its primary amine (NIL) functional group and two methoxy groups (OCH3) attached to a central carbon, which is vital for the subsequent dynamic exchange reactions.

[0047] At operation 304, the initial curing reaction generates a secondary amine (NH) linkage and a hydroxyl (OH) group at the site of the epoxide group. The hydroxyl group is useful for the subsequent dynamic exchange reactions that enable the vitrimer properties.

[0048] At operation 306, the formed hydroxyl group formed after the initial curing reaction reacts with another acetal group. Another acetal group is received from the ground particles after grinding the vitrimer epoxy received as manufacturing waste, resulting in the exchange of methoxy groups. The reversible trans-acetalization reaction allows the vitrimer epoxy network to undergo bond rearrangement without changing the total number of crosslinks. The trans-acetalization reaction results in the formation of a new acetal linkage and the release of a methoxy group (H3CO).

[0049] At operation 308, a completed network structure of the recycled thermoset polymer is established following the occurrence of multiple dynamic bond exchange reactions. The different polymer chains (indicated by wavy lines) become interconnected through the newly formed acetal linkages. The network architecture of the recycled thermoset polymer enables the recycled thermoset polymer to maintain structural integrity and enables the reprocessability of the recycled thermoset polymer.

[0050] FIG. 4 is a graphical representation 400 illustrating a tensile strength of various regrind epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 4 is described in conjunction with elements from FIGs. 1 to 3. The tensile strength measured in megapascals (MPa) is represented on the ordinate axis. The graphical representation 400 includes a bar 402 representing tensile strength for a vitrimer epoxy with 15% acetal-containing hardener mixed with 11% accelerator, a bar 404 representing tensile strength for a vitrimer epoxy with 5 weight percent of vitrimer epoxy regrind particles with a particle size range of 66-125 micrometres, a bar 406 representing tensile strength for a vitrimer epoxy with 10 weight percent of regrind particles with a size range of 66-125 micrometres, a bar 408 representing tensile strength for a vitrimer epoxy with 20 weight percent of regrind particles with a size range of 66-125 micrometres, and a bar 410 representing tensile strength for a vitrimer epoxy with 30 weight percent of regrind particles with a size range of 66-125 micrometres.

[0051] The bar 402 exhibits the highest tensile strength, indicating that the polymer network of the vitrimer epoxy with 15% acetal-containing hardener mixed with 11% accelerator remains intact with a well -maintained crosslinking structure, ensuring suitable mechanical properties. The absence of regrind particles prevents potential disruptions in the molecular network, leading to maximized stress-bearing capacity and overall tensile integrity.

[0052] The bar 404 exhibits a slight reduction in tensile strength, approximately ranging from 80-75 MPa, as compared to the bar 402, indicating that theintroduction of a small amount of regrind particles does not significantly compromise the mechanical stability of the polymer network. The regrind particles are reintegrated within the polymer network while maintaining adequate crosslinking, allowing the regrind epoxy formulation to retain a substantial portion of the strength of the vitrimer epoxy.

[0053] The bar 406 exhibits a further decline in tensile strength, approximately ranging from 70-65 MPa, as compared to the bar 402 and the bar 404. The decrease in tensile strength indicates an increasing proportion of heterogeneous regrind particles disrupting the polymer network. As the content of the regrind particle increases, the regrind epoxy formulation experiences slightly reduced stress distribution efficiency, leading to localized weaknesses that affect the overall tensile strength of the recycled thermoset polymer.

[0054] The bar 408 exhibits a tensile strength approximately ranging between 65-55 MPa, indicating a reduction in tensile strength as compared to the bar 402, the bar 406 and the bar 408. However, despite the observed decrease, a tensile strength approximately ranging between 65-55 MPa remains a considerable value for various practical applications, such as structural or semi-structural components where moderate mechanical performance is acceptable. Additionally, the bar 408 indicates the capability of the vitrimer epoxy system to incorporate up to 20% by weight of regrind epoxy material which is considered as production waste into fresh formulations while retaining the mechanical properties of the thermoset polymer.

[0055] The bar 410 exhibits the lowest tensile strength, approximately ranging from 50-40 MPa, as compared to the bar 402, the bar 404, the bar 406 and the bar 408. The decline in tensile strength indicates the adverse effects of excessive regrind incorporation. The reduction in tensile strength with increasing regrind content is consistent with the expected behaviour of the reprocessed thermoset polymer.

[0056] Among the various regrind formulations, the bar 408 achieves a balance between material recyclability and mechanical performance, exhibiting only amoderate decrease in tensile strength (approximately ranging between 65-55 MPa) while maintaining the structural integrity. The bar 408 indicates that incorporating 20 weight percent of regrind particles is feasible for sustainable vitrimer epoxy applications without significantly compromising mechanical properties.

[0057] FIG. 5 is a graphical representation 500 illustrating force-displacement curves for various regrind epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 5 is described in conjunction with elements from FIGs. 1 to 4. The force measured in Newton (N) is represented on the ordinate axis. The displacement measured in millimetres (mm) is represented on the abscissa axis. The graphical representation 500 includes a curve 502 representing force for a 65% silica filled vitrimer epoxy with 15% acetal-containing hardener mixed with 11% accelerator, a curve 504 representing force for a vitrimer epoxy with 15% acetal-containing hardener mixed with 11% accelerator, and a curve 506 representing force for 10% regrind based vitrimer epoxy with 15% acetal-containing hardener mixed with 11% accelerator.

[0058] The curve 502 exhibits a steep initial slope, indicating high stiffness due to the 65% silica filler content. The curve 502 reaches a maximum force of approximately ranging from 700-750 N at a displacement of around 0.4 mm. After reaching a value of maximum force, the curve 502 indicates an abrupt drop in force, indicating a brittle failure region 508. The 65% loading of silica microparticles increases the stiffness of the vitrimer epoxy but reduces its ability to undergo plastic deformation before failure. The high force value achieved by the curve 502 exhibits excellent load-bearing capability, making the curve 502 suitable for applications requiring high strength and minimal deformation under load.

[0059] The curve 504 exhibits a more gradual slope compared to the curve 502, indicating lower initial stiffness due to the absence of silica fillers. The curve 504 reaches a maximum force of approximately ranging from 750-800 N at displacement of around 1.0 mm. After achieving a maximum force, the curve 504 follows a more gradual decrease in force up to approximately a displacement of 1.4mm before reaching a brittle failure region 510. The extended displacement range after the curve 504 reaches the maximum force indicates the higher ductility and toughness of the curve 504 as compared to the curve 502.

[0060] The curve 506 exhibits an intermediate behaviour between the curve 502 and the curve 504. The initial slope is steeper than the curve 504 but less steep than the curve 502, indicating moderate stiffness. The curve 506 reaches a maximum force of approximately ranging from 500-550 N at a displacement of around 0.8 mm, followed by failure. The incorporation of 10% regrind material results in a material with moderate stiffness and ductility, demonstrating the successful integration of recycled content while maintaining acceptable mechanical performance.

[0061] Among the curve 502, the curve 504 and the curve 506, the curve 504 exhibits the most favourable balance of force-displacement characteristics for applications requiring both strength and toughness. While the curve 504 does not provide the immediate stiffness like the curve 502, it achieves the highest maximum force and sustains the largest displacement before failure, indicating suitable energy absorption capacity and damage tolerance. The combination of high strength and enhanced ductility makes the curve 504 particularly well-suited for applications where impact resistance and the ability to withstand deformation without catastrophic failure are vital performance requirements. The curve 506 represents a viable compromise for applications where sustainability considerations must be balanced with mechanical performance.

[0062] FIG. 6 is a graphical representation 600 illustrating a tensile strength of various regrind epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 6 is described in conjunction with elements from FIGs. 1 to 5. The tensile strength measured in megapascals (MPa) is represented on the ordinate axis. The graphical representation 600 includes a bar 602 representing tensile strength for a vitrimer epoxy with 15% acetal-containing hardener mixed with 11% accelerator, a bar 604 representing tensile strength for 65% silica filledvitrimer epoxy with 15% acetal -containing hardener mixed with 11% accelerator, a bar 606 representing tensile strength for a 65% silica fdled huntsman epoxy, a bar 608 representing tensile strength for a 65% vitrimer epoxy with 10 weight percent of regrind particles, and a bar 610 representing tensile strength for a vitrimer epoxy with 10 weight percent of regrind particles.

[0063] The bar 602 exhibits a tensile strength of approximately ranging from SO-85 MPa. The bar 602 has the highest tensile strength among the bar 604, the bar 606, the bar 608, and the bar 610, indicating suitable mechanical properties. The tensile strength of the bar 602 can be attributed to the efficient crosslinking network formed by the acetal exchange, creating a robust polymer structure with well-distributed stress transfer capabilities throughout the vitrimer epoxy.

[0064] The bar 604 exhibits a tensile strength of approximately ranging between 70-75 MPa. The bar 604 has a slight reduction in tensile strength compared to the bar 602, achieving approximately 89% of the tensile strength. The incorporation of 65% silica microparticle content modifies the mechanical properties of the vitrimer epoxy by introducing rigid particles that can both reinforce the polymer network and introduce stress concentration points. The relatively high tensile strength maintained despite the significant filler loading demonstrates good compatibility between the silica particles and the vitrimer matrix.

[0065] The bar 606 exhibits a tensile strength of approximately ranging from 70-74 MPa. The bar 606 has approximately 90% of the tensile strength compared to the bar 602, indicating that the incorporation of the dynamic acetal exchange does not compromise the mechanical strength when compared to the bar 604 while providing reprocessing characteristics to vitrimer epoxy formed.

[0066] The bar 608 exhibits the lowest tensile strength at approximately 54 MPa compared to the bar 602, the bar 604, the bar 606 and the bar 610. However, the formulation of 65% vitrimer epoxy with 10 weight percent of regrind particles represents a well-balanced combination in which 10 weight percent of regrind particles are incorporated to address sustainability considerations, while silicamicroparticles are added to enhance electrical properties. Despite the inclusion of the regrind particles, the tensile strength remains within an acceptable range for the thermoset polymer, making such formulation suitable for various applications such as electronic encapsulation, structural adhesives, and composite laminates in consumer and industrial products.

[0067] The bar 610 exhibits a tensile strength of approximately ranging from 60-68 MPa. The bar 610 achieves tensile strength of approximately 83% compared to the bar 602. The improved performance compared to the bar 608 indicates that the curing reaction between the polymer network and the regrind particles effectively facilitates bonding between vitrimer epoxy and regrind particles, enabling efficient stress transfer across the interfaces between the polymer network and regrind particles.

[0068] Among the bar 602, the bar 604, the bar 606, the bar 608 and the bar 610, the bar 602 exhibits the suitable tensile strength indicating that while the addition of fillers and recycled content offers practical and sustainability benefits, they do come with some compromises to mechanical performance. However, the relatively small reduction in tensile strength in the bar 604, the bar 606 and the bar 610 indicates that the modified vitrimer epoxy formulations still maintain adequate mechanical integrity for many practical applications. The bar 608 and the bar 610 indicate that an effective balance between performance and sustainability can be achieved by incorporating regrind particles in the formation of the vitrimer epoxy.

[0069] FIG. 7 is a graphical representation 700 illustrating a tensile strength of various regrind epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 7 is described in conjunction with elements from FIGs. 1 to 6. The tensile strength measured in megapascals (MPa) is represented on the ordinate axis. The graphical representation 700 includes a bar 702 representing tensile strength for a vitrimer epoxy with 15% acetal-containing hardener mixed with 11% accelerator, a bar 704 representing tensile strength for a vitrimer epoxy with 5 weight percent of regrind particles with a size range of 66-125 micrometres,a bar 706 representing tensile strength for a vitrimer epoxy with 10 weight percent of regrind particles with a size range of 66-125 micrometres, a bar 708 representing tensile strength for a vitrimer epoxy with 20 weight percent of regrind particles with a size range of 66-125 micrometres, and a bar 710 representing tensile strength for a vitrimer epoxy with 20 weight percent of regrind particles with a size range of 66-125 micrometres after second reprocessing cycle.

[0070] The bar 702 exhibits the highest tensile strength of approximately ranging from 75-82 MPa. The absence of regrind particles ensures maximum crosslink density within the polymer network, allowing for efficient load distribution and high mechanical stability. The polymeric structure remains intact, with minimal disruptions, leading to optimal tensile strength.

[0071] The bar 704 exhibits a slight reduction in tensile strength compared to the bar 702, indicating that a small proportion of regrind particles does not affect the structural integrity of the vitrimer epoxy formed. The polymer network still maintains a relatively high degree of crosslinking, and the regrind particles are effectively incorporated within the virgin epoxy and acetal-containing hardener mixture without causing significant defects.

[0072] The bar 706 exhibits a further decrease in tensile strength, approximately ranging from 65-70 MPa, indicating an increased heterogeneity in the polymer network. As the regrind content increases from 5 to 10 weight percent, stress transfer efficiency across the recycled thermoset polymer decreases, leading to localized weak points that compromise the mechanical strength.

[0073] The bar 708 exhibits a tensile strength of approximately ranging between 55-60 MPa, indicating a moderate decrease compared to the bar 702, the bar 704, and the bar 706. However, the tensile strength remains within a functionally acceptable range for several applications such as moulded electrical housings, interior panels in automotive components, cable trays, appliance casings, and general -purpose tooling. The formulation represented by the bar 708 has 20 weightpercent of regrind particles indicating a reintegration of the vitrimer epoxy regrind back into high-performance thermoset polymer.

[0074] The bar 708 exhibits a significant drop in tensile strength, approximately ranging from 55-60 MPa, indicating disruption of the polymer network due to the increased quantity of regrind particles from 10 to 20 weight percent, resulting in poorer load distribution and reduced mechanical performance of the recycled thermoset polymer. The increasing number of regrind particles may introduce voids and interfacial inconsistencies, leading to structural deficiencies.

[0075] The bar 710 exhibits a tensile strength of approximately ranging from 50 to 55 MPa and is slightly lower than the bar 708. The second reprocessing cycle was conducted to simulate the real-world scenario of recycling production scrap, which typically consists of a heterogeneous mixture of multiple manufacturing batches. In industrial production, leftover or defective epoxy-based materials from different processing stages accumulate as scrap. Such epoxy-based materials often vary in composition, curing conditions, and ageing effects, making reprocessing more complex than working with a single, uniform batch. The drop in tensile strength is minimal as compared to the bar 708, indicating effective reprocessing using the vitrimer epoxy formulation associated with the bar 710.

[0076] FIG. 8 is a graphical representation 800 illustrating dynamic mechanical analysis (DMA) of various epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 8 is described in conjunction with elements from FIGs 1 to 7. With reference to FIG. 8, there is shown the graphical representation 800 depicting the temperature-dependent viscoelastic properties of various epoxy formulations. The storage modulus measured in megapascal (MPa) is represented on the ordinate axis, while the temperature measured in degrees Celsius (°C) is represented on the abscissa axis. The dynamic mechanical analysis (DMA) is a technique used to evaluate the viscoelastic behaviour of polymeric materials by measuring the response to an applied oscillatory force over a range of temperatures. The DMA provides insights into the stiffness, elasticity, and mechanical dampingcharacteristics of various epoxy formulations. The storage modulus represents the ability of the material to store mechanical energy, indicating structural rigidity, while variations in modulus with temperature reflect phase transitions, such as the glass transition temperature, which marks the shift from a rigid to a more flexible state. The graphical representation 800 includes a curve 802, representing the huntsman epoxy, the curve 804, representing the acetal-modified epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 5% aminopropyl imidazole, and the curve 806, representing the acetal-modified epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 11% aminopropyl imidazole.

[0077] The curve 802 exhibits an initial storage modulus of approximately ranging from 1800-2000 MPa at 30°C and maintains relatively high values up to around 100°C. After 100 degrees Celsius, the curve 802 shows a gradual decline that extends to approximately 120°C before approaching zero. The region of this extended decline is called a plateau region 808, and gradual transition indicates a broad glass transition temperature range. The maintained value of storage modulus at 100 to 120 degrees Celsius indicates the thermal stability of the curve 802, which preserves the structural integrity of the vitrimer epoxy across a wide temperature range due to its rigid, permanent covalent crosslinks that restrict polymer chain mobility even as temperature increases.

[0078] The curve 804 exhibits an initial storage modulus of approximately ranging from 2000-2400 MPa at 30°C. The curve 804 exhibits a relatively sharp decline in storage modulus beginning at approximately 40°C, with the storage modulus approaching zero by approximately 65 °C. The rapid decrease in storage modulus indicates a narrow glass transition temperature range and indicates that the lower concentration of aminopropyl imidazole catalyst (5%) allows for more pronounced dynamic exchange reactions at lower temperatures. The early onset of storage modulus reduction exhibits the enhanced chain mobility facilitated by the dynamic acetal exchange, which enables stress relaxation and network reconfiguration at lower temperatures as compared to the curve 802.

[0079] The curve 806 exhibits initial storage modulus approximately ranging from 2000-2400 MPa at 30°C. The curve 806 structural rigidity up to approximately 60°C before experiencing a relatively sharp decline in storage modulus, approaching zero by approximately 80°C. The extended temperature stability compared to the curve 804 indicates that the higher concentration of aminopropyl imidazole catalyst (11%) likely increases the crosslink density or alters the kinetics of the dynamic exchange reactions, resulting in improved thermal stability while still facilitating network reconfiguration at temperatures lower than the curve 802.

[0080] The curve 802 offers thermal stability but cannot undergo network reconfiguration, making it non-recyclable. In contrast, the curve 804 and the curve 806 demonstrate temperature-dependent modulus profiles consistent with materials capable of dynamic bond exchange, enabling reprocessability and recycling. The curve 806 represents an optimized balance between thermal stability and reprocessability, maintaining structural integrity to higher temperatures than the curve 804 while still facilitating the dynamic acetal exchange reactions that enable recycling at practically achievable processing temperatures.

[0081] FIG. 9 is a graphical representation 900 illustrating dynamic mechanical analysis (DMA) of various epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 9 is described in conjunction with elements from FIGs 1 to 8. The storage modulus measured in megapascal (MPa) is represented on the ordinate axis, while the temperature measured in degrees Celsius (°C) is represented on the abscissa axis. The graphical representation 900 includes a curve 902, representing the huntsman epoxy, the curve 904, representing the acetal-modified epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 11% aminopropyl imidazole, and the curve 906, representing the 65% silica fdled acetal -modified epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 5% aminopropyl imidazole.

[0082] The curve 902 exhibits an initial storage modulus of approximately ranging from 1500-2000 MPa at 30°C. The curve 902 further exhibits a gradualdecline in storage modulus with increasing temperature, maintaining substantial stiffness up to approximately 80°C before experiencing a more pronounced decrease. The storage modulus approaches zero around 120°C, indicating the completion of the glass transition. The gradual decline in the storage modulus indicates a wide glass transition temperature range approximately ranging from 80-120°C, which is suitable for applications requiring stable mechanical properties under fluctuating temperature conditions.

[0083] The curve 904 exhibits an initial storage modulus of approximately ranging from 2000-2500 MPa at 30°C. As compared to the curve 902, the curve 904 indicates higher stiffness. However, the curve 904 exhibits a more rapid decline in storage modulus with increasing temperature approximately ranging from 40-100°C, with a steep drop beginning around 40°C and approaching zero by approximately 100°C. The steep drop in the value of storage modulus indicates a narrower glass transition temperature range and indicates that the dynamic acetal exchange reactions become increasingly active as temperature rises, facilitating network reorganization and stress relaxation. The lower temperature at which this formulation loses its rigidity demonstrates its enhanced reprocessability compared to conventional epoxy, though at the cost of reduced thermal stability.

[0084] The curve 906 exhibits an initial storage modulus approximately ranging from 2500-3000 MPa at 30°C due to the reinforcing effect of the silica particles. The storage modulus remains relatively stable until approximately 60°C, after which the curve 906 experiences a significant decline, reaching near-zero values around 110°C. The high silica content significantly enhances the stiffness of the curve 906, while the reduced catalyst concentration (5% compared to 11% in the curve 904) appears to moderate the rate of dynamic exchange reactions, resulting in improved thermal stability compared to the curve 902. The combination of high initial storage modulus and extended temperature stability make the curve 906 suitable for applications requiring both structural rigidity and recyclability.

[0085] Among the curve 902, the curve 904 and the curve 906, the curve 906 exhibits a useful DMA profile for applications requiring both high stiffness and reasonable thermal stability. The initial storage modulus of approximately ranging from 2500-3000 MPa provides excellent rigidity, while the thermal stability up to approximately 80°C before significant softening occurs makes the curve 906 suitable for a wide range of practical applications. The retention of dynamic bond exchange capabilities, despite the high filler content, is indicated by the complete modulus reduction at a high temperature of approximately ranging between 100-120 °C, indicating that reprocessability is preserved. The curve 906 is well-suited for applications in electronic packaging, structural components, and other areas where both performance and sustainability are vital considerations.

[0086] FIG. 10 is a graphical representation 1000 illustrating the tan delta curves from dynamic mechanical analysis (DMA) of various epoxy formulations, in accordance with an embodiment of the present disclosure. FIG. 10 is described in conjunction with elements from FIGs 1 to 9. With reference to FIG. 10, there is shown the graphical representation 1000 depicting the damping behaviour of various epoxy formulations as a function of temperature. The tan delta value is represented on the ordinate axis, while the temperature measured in degrees Celsius (°C) is represented on the abscissa axis. The tan delta is the ratio of the loss modulus to the storage modulus, indicating the energy dissipation capacity of the epoxy formulation and is commonly used to identify the glass transition temperature (Tg), which corresponds to the peak of the tan delta curve. The graphical representation 1000 includes a curve 1002, representing the huntsman epoxy, the curve 1004, representing the acetal-modified epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 11% aminopropyl imidazole, and the curve 1006, representing the 65% silica filled acetal-modified epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 11% aminopropyl imidazole.

[0087] The curve 1002 exhibits a tan delta peak 1008 centred at approximately ranging from 120-130°C. The high temperature indicates a glass transition temperature of 128°C, indicating the thermal stability characteristic of the curve1002. The tan delta peak 1008 is moderately broad with a maximum tan delta value of approximately ranging from 0.6-0.7, indicating suitable but not excessive damping capacity. The breadth of the tan delta peak 1008 correlates with the wide glass transition range, confirming the gradual transition of the epoxy formulation associated with the curve 902 from a glassy state to a rubbery state. The high glass transition temperature makes the curve 902 suitable for applications requiring dimensional stability at elevated temperatures, although it lacks the capability for reprocessing due to its permanent crosslink structure.

[0088] The curve 1004 exhibits a tan delta peak 1010 centred at approximately ranging from 70-80°C, with the highest maximum value of tan delta compared with the curve 1002 and the curve 1006 at approximately ranging from 0.65-0.72. The relatively low temperature of the tan delta peak 1010 confirms the earlier onset of the glass transition observed in the storage modulus for the curve 904 in the FIG. 9. The high tan delta value, as compared to the curve 1002, indicates suitable damping capacity, indicating energy dissipation properties useful for vibration damping applications. The narrower peak width of the tan delta peak 1010 compared to the curve 1002 reflects a more homogeneous network structure

[0089] The curve 1006 exhibits a tan delta peak 1012 centred at approximately ranging from 90-110°C, with a maximum value of approximately ranging from 0.7-0.8. The glass transition temperature positions the curve 1106 between the curve 1102 and the curve 1104 in terms of thermal stability. The high maximum tan delta value, approximately ranging from 0.7-0.8, despite the silica content, indicates that the dynamic acetal exchange compensates for the reduced damping capacity of the 65% silica fdled acetal -modified epoxy formulation containing 15% amino acetaldehyde dimethyl acetal and 11% aminopropyl imidazole. The rightward shift of the tan delta peak compared to the curve 1004 indicates that the silica filler and catalyst concentration restrict polymer chain mobility, requiring higher thermal energy to activate sufficient chain motion for the glass transition.

[0090] Modifications to embodiments of the present disclosure described in the foregoing are possible without departing from the scope of the present disclosure as defined by the accompanying claims. Expressions such as "including", "comprising", "incorporating", "have", "is" used to describe and claim the present disclosure are intended to be construed in a non-exclusive manner, namely allowing for items, components or elements not explicitly described also to be present. Reference to the singular is also to be construed to relate to the plural. The word "exemplary" is used herein to mean "serving as an example, instance or illustration". Any embodiment described as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments and / or to exclude the incorporation of features from other embodiments. The word "optionally" is used herein to mean "is provided in some embodiments and not provided in other embodiments" . It is appreciated that certain features of the present disclosure, which are, for clarity, described in the context of separate embodiments, may also be provided in combination in a single embodiment. Conversely, various features of the present disclosure, which are, for brevity, described in the context of a single embodiment, may also be provided separately or in any suitable combination or as suitable in any other described embodiment of the disclosure.

Claims

CLAIMSWe claim:

1. A method (100) for recycling thermoset polymers, the method (100) comprising:providing a vitrimer epoxy comprising a virgin epoxy resin crosslinked with an acetal-containing hardener, wherein the vitrimer epoxy contains dynamic covalent acetal linkages;grinding the vitrimer epoxy into ground particles;preheating the virgin epoxy resin;incorporating the ground particles into the preheated virgin epoxy resin; adding an acetal-containing hardener to the mixture of virgin epoxy resin and ground particles;degassing the resulting mixture; andcuring the degassed mixture through a staged thermal cycle, wherein the resulting recycled material maintains mechanical properties of the original vitrimer epoxy.

2. The method (100) as claimed in claim 1, further comprising adding an accelerator to the mixture prior to degassing.

3. The method (100) as claimed in claim 2, wherein the accelerator comprises l-(3-aminopropyl) imidazole in an amount of 2.5-20 weight percent relative to the virgin epoxy resin.

4. The method (100) as claimed in claim 1 , wherein the ground particles have a size between 60-600 micrometres and are incorporated in an amount of 5-30 weight percent relative to the virgin epoxy resin.

5. The method (100) as claimed in claim 4, wherein the ground particles have a size between 66-125 micrometres and are incorporated in an amount of 20 weight percent relative to the virgin epoxy resin.

6. The method (100) as claimed in claim 1, wherein the acetal-containing hardener comprises amino acetaldehyde dimethyl acetal in an amount of 5-50 weight percent relative to the virgin epoxy resin.

7. The method (100) as claimed in claim 1, further comprising adding silica microparticles having a particle size of less than 45 micrometres in an amount of 50-80 weight percent relative to the total composition.

8. The method (100) as claimed in claim 1, wherein the recycled material maintains at least 70% of the tensile strength of a corresponding material made entirely from the virgin epoxy resin.