Polyurethane foam, and cushioning material, sealing material, and heat insulating material using said polyurethane foam
A biomass-derived polyurethane foam with specific properties addresses the need for resilience and softness by combining biomass and petroleum-derived polyols, achieving high elongation and environmental sustainability.
Patent Information
- Application Number
- PCT/JP2025/016769
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
There is a growing demand for polyurethane foam that is both highly resilient and soft, particularly for applications such as cushioning materials in electronic devices and sealing materials in batteries, yet biomass-derived materials with these properties have not been adequately developed.
A polyurethane foam composition using a combination of biomass-derived polyols with specific molecular weights and petroleum-derived polyols, along with other additives, is formulated to achieve a hysteresis loss rate of 20% or less, a glass transition temperature of -10°C or lower, and a density of 100 kg/m³, ensuring high resilience and softness.
The resulting polyurethane foam exhibits an elongation rate of 50% or more, making it suitable for cushioning, sealing, and insulating applications while maintaining a high biomass content, thus contributing to environmental sustainability.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Polyurethane foam, cushioning material, sealing material, and heat insulating material using the polyurethane foam.
[0001] This technology relates to polyurethane foam. More specifically, it relates to polyurethane foam, and to cushioning materials, sealing materials, and thermal insulation materials using said polyurethane foam.
[0002] Polyurethane foam is widely used in a variety of fields, from furniture such as sofas and chairs, bedding such as mattresses and pillows, clothing such as underwear, daily necessities such as dishwashing sponges and cleaning sponges, vehicle and aircraft interior products such as car seats, electronic devices such as mobile phones, cameras, and televisions, electrical appliances such as home appliances, toys, and general merchandise. Furthermore, various developments are underway to improve quality and add new functions according to each field and purpose.
[0003] Furthermore, in recent years, technologies that utilize biomass raw materials in polyurethane foam as so-called carbon-neutral renewable resources have attracted attention in order to contribute to the formation of a sustainable society. For example, Patent Document 1 proposes a polyurethane foam that can contribute to environmental sustainability by using biomass-derived polyether polyols with a weight-average molecular weight of 1200 or more and biomass-derived polyols with a molecular weight of 300 or less.
[0004] Furthermore, Reference 2 proposes a technology to obtain polyurethane foam with excellent mechanical properties, which can suppress phase separation over long periods at room temperature and relatively high temperature environments, by using component (A): a polyester polyol, which is a condensate of a plant-derived fatty acid that may be condensed and a polyhydric alcohol; component (B): a polyether polyol; and component (C): a polyoxyethylene adduct of a hydroxyl group-containing fatty acid ester.
[0005] Japanese Patent Publication No. 2024-173204 Japanese Patent Publication No. 2016-183249
[0006] In recent years, there has been a growing demand for polyurethane foam that can be used as cushioning material to absorb vibrations and shocks in electronic devices such as mobile phones, cameras, and televisions, as well as in electrical equipment such as home appliances; as sealing material for various batteries; and as sealing and insulating material around batteries and electronic control units in electric vehicles. For these applications, the foam needs to be both highly resilient and soft, but a polyurethane foam using biomass raw materials possessing these properties had not yet been developed.
[0007] Therefore, the primary objective of this technology is to provide a highly resilient yet soft polyurethane foam using biomass raw materials.
[0008] This technology first provides a polyurethane foam obtained from a raw material composition containing a polyol component, wherein the polyol component contains a biomass-derived polyol, the hysteresis loss rate measured in accordance with JIS K 6254 is 20% or less, the glass transition temperature is -10°C or lower, and the density is 100 kg / m³. 3 More than 500kg / m 3 The following polyurethane foam is provided. In this technology, the biomass-derived polyol may contain a first biomass-derived polyol with a number average molecular weight of 1500 or more, and a second biomass-derived polyol with a molecular weight or number average molecular weight of 100 or more and 1000 or less. The polyurethane foam according to this technology may have an elongation rate of 50% or more, as measured in accordance with JIS K6251:2010. In this technology, the polyol component may contain a petroleum-derived polyol with a molecular weight or number average molecular weight of 100 or more and 1000 or less. In addition, the polyol component may contain a polymer polyol. The polyurethane foam according to this technology may have a biomass content of 20% or more. The polyurethane foam according to this technology can be used as a cushioning material, a sealing material, or a heat insulating material.
[0009] The following describes preferred embodiments for implementing this technology. The embodiments described below are examples of typical embodiments of this technology, and any combination of these embodiments is possible. Furthermore, this does not mean that the scope of this technology will be narrowed.
[0010] 1. Raw Material Composition for Polyurethane Foam Production The polyurethane foam according to this technology is obtained from a raw material composition containing a polyol component and an isocyanate. The raw material composition used in the production of polyurethane foam according to this technology may also contain foam stabilizers, catalysts, antioxidants, fillers, hygroscopic agents, blowing agents, etc., as needed.
[0011] The polyurethane foam according to this technology can be manufactured using any general polyurethane foam manufacturing method, as described later, but it is particularly preferable to manufacture it using the mechanical floss method. That is, the composition used in the manufacture of the polyurethane foam according to this technology can be suitably used as a composition for mechanical floss. Each component will be described in detail below.
[0012] (1) Polyol The polyurethane foam relating to this technology is characterized by containing a biomass-derived polyol as a polyol component. Furthermore, depending on the physical properties and applications of the polyurethane foam to be manufactured, it is also possible to freely select and use one or more types of polyols commonly used in polyurethane foams.
[0013] (1-1) Biomass-derived polyols The biomass-derived polyols that can be used in this technology may be one or more biomass-derived polyols that can be used in the manufacture of polyurethane foam, as long as the function and effect of this technology are not impaired. Examples of biomass-derived polyols that can be used in this technology include biomass-derived polyether polyols and biomass-derived polyester polyols.
[0014] Examples of biomass-derived polyether polyols include 1,3-propanediol derived from plants and animals such as corn, 1,2,3-propanetriol (glycerin) derived from plants and animals, or condensates thereof. Among these, in this technology, condensates of 1,3-propanediol derived from plants and animals are preferred as biomass-derived polyether polyols, and condensates of 1,3-propanediol derived from corn are more preferred.
[0015] Examples of biomass-derived polyester polyols include natural oils and fats such as castor oil, soybean oil, palm oil, palm kernel oil, coconut oil, cashew nut shell liquid (CNSL), olive oil, cottonseed oil, safflower oil, sesame oil, sunflower oil, and linseed oil, or their derivatives (for example, modified natural oil polyols, unmodified natural oil polyols, etc.). Among these, in this technology, natural oils and fats or their derivatives are preferred as biomass-derived polyester polyols, castor oil or its derivatives are more preferred, and castor oil-modified polyols are even more preferred.
[0016] The molecular weight of the biomass-derived polyol that can be used in this technology is not particularly limited as long as it does not impair the action or effect of this technology, but it is preferable to use in combination a first biomass-derived polyol with a number average molecular weight of 1500 or more and a second biomass-derived polyol with a molecular weight or number average molecular weight of 100 or more and 1000 or less. By using a first biomass-derived polyol and a second biomass-derived polyol in combination, it is possible to produce a polyurethane foam that is soft yet highly resilient, despite having a high biomass content.
[0017] When using both a first biomass-derived polyol and a second biomass-derived polyol in combination, the ratio of these polyols is not particularly limited and can be freely determined according to the properties and purpose of each biomass-derived polyol.
[0018] For example, when biomass-derived polyether polyols are used as the first biomass-derived polyol and the second biomass-derived polyol, the lower limit of the content of the second biomass-derived polyol, when the content of the first biomass-derived polyol is set to 1, is, for example, 0.1 times or more, preferably 0.15 times or more, and more preferably 0.2 times or more. The upper limit of the content of the second biomass-derived polyol, when the content of the first biomass-derived polyol is set to 1, is, for example, 2.0 times or less, preferably 1.7 times or less, and more preferably 1.5 times or less.
[0019] For example, when biomass-derived polyester polyols are used as the first biomass-derived polyol and the second biomass-derived polyol, the lower limit of the content of the second biomass-derived polyol, when the content of the first biomass-derived polyol is set to 1, is, for example, 0.05 times or more, preferably 0.07 times or more, and more preferably 0.1 times or more. The upper limit of the content of the second biomass-derived polyol, when the content of the first biomass-derived polyol is set to 1, is, for example, 1.0 times or less, preferably 0.7 times or less, and more preferably 0.5 times or less.
[0020] The content of biomass-derived polyols in the polyol component used in this technology can be freely set as long as it does not impair the function or effect of this technology. The lower limit of the biomass-derived polyol content in 100 parts by mass of the polyol component used in this technology is, for example, 35 parts by mass or more, preferably 40 parts by mass or more, more preferably 45 parts by mass or more, and even more preferably 50 parts by mass or more. By setting the biomass-derived polyol content in the polyol component within this range, this technology can improve the biomass content of the polyurethane foam produced, further reduce the environmental burden, and further contribute to the formation of a sustainable society.
[0021] The upper limit of the biomass-derived polyol content in 100 parts by mass of the polyol component used in this technology may be 100 parts by mass, but for example, it may be 95 parts by mass or less, preferably 90 parts by mass or less, more preferably 85 parts by mass or less, and even more preferably 80 parts by mass or less. In this technology, by setting the biomass-derived polyol content in the polyol component within this range, it is possible to suppress a decrease in the physical properties of the polyurethane foam produced.
[0022] For example, when using a biomass-derived polyether polyol as the biomass-derived polyol, the lower limit of the biomass-derived polyol content in 100 parts by mass of the polyol component is, for example, 45 parts by mass or more, preferably 50 parts by mass or more, more preferably 55 parts by mass or more, and even more preferably 60 parts by mass or more. The upper limit of the biomass-derived polyol content in 100 parts by mass of the polyol component is, for example, 95 parts by mass or less, preferably 90 parts by mass or less, more preferably 85 parts by mass or less, and even more preferably 80 parts by mass or less.
[0023] For example, when using a biomass-derived polyester polyol as the biomass-derived polyol, the lower limit of the biomass-derived polyol content in 100 parts by mass of the polyol component is, for example, 35 parts by mass or more, preferably 40 parts by mass or more, more preferably 45 parts by mass or more, and even more preferably 50 parts by mass or more. The upper limit of the biomass-derived polyol content in 100 parts by mass of the polyol component may be 100 parts by mass or less, but for example, 80 parts by mass or less, preferably 75 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 65 parts by mass or less.
[0024] (1-2) Polyols other than biomass-derived polyols In this technology, polyols other than biomass-derived polyols can also be used in combination. Examples of polyols other than biomass-derived polyols include polyester polyols, polyether polyols, polyester ether polyols, polycarbonate polyols, polymer polyols, etc.
[0025] In this technology, it is preferable to use a petroleum-derived polyol with a molecular weight or number average molecular weight of 100 or more and 1000 or less as a polyol other than biomass-derived polyol. By using a petroleum-derived polyol with a molecular weight or number average molecular weight of 100 or more and 1000 or less, the elongation rate of the polyurethane foam produced can be improved.
[0026] When using petroleum-derived polyols other than biomass-derived polyols, specifically those with a molecular weight or number average molecular weight of 100 or more and 1000 or less, their content can be freely set as long as it does not impair the function or effects of this technology. The lower limit of the content of petroleum-derived polyols with a molecular weight or number average molecular weight of 100 or more and 1000 or less in 100 parts by mass of the polyol component used in this technology is, for example, 1.0 part by mass or more, preferably 5.0 parts by mass or more, and more preferably 10 parts by mass or more. In this technology, by setting the content of petroleum-derived polyols with a molecular weight or number average molecular weight of 100 or more and 1000 or less in the polyol component to this range, the reactivity during polyurethane foam production can be improved, and the physical properties of the polyurethane foam produced can be further improved.
[0027] The upper limit of the content of petroleum-derived polyols with a molecular weight or number average molecular weight of 100 or more and 1000 or less in 100 parts by mass of the polyol component used in this technology is, for example, 40 parts by mass or less, preferably 30 parts by mass or less, and more preferably 25 parts by mass or less. In this technology, by setting the content of petroleum-derived polyols with a molecular weight or number average molecular weight of 100 or more and 1000 or less in the polyol component to this range, the biomass content of the polyurethane foam produced can be improved, the environmental burden can be reduced, and further contributions to the formation of a sustainable society can be made.
[0028] (1-2-1) Polyester Polyols In this technology, it is preferable to use polyester polyols as polyols other than biomass-derived polyols. By using polyester polyols, the elongation of the polyurethane foam produced can be improved.
[0029] Examples of polyester polyols include polylactone polyols and polycaprolactone polyols obtained by ring-opening polymerization of lactone monomers such as ε-caprolactone and methylvalerolactone; aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, and azelaic acid; aliphatic carboxylic acids such as ricinoleic acid; aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid; and alicyclic dicarboxylic acids such as hexahydrophthalic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid. Alternatively, examples include polyester polyols such as polypropylene glycol obtained by a dehydration condensation reaction of these acid esters or acid anhydrides with ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, 1,8-octanediol, 1,9-nonanediol, etc., or mixtures thereof. Among these, polycaprolactone polyols are preferred in this technology.
[0030] When using polyester polyol as a polyol other than biomass-derived polyol, its content can be freely set as long as it does not impair the function and effects of this technology. The lower limit of the polyester polyol content in 100 parts by mass of the polyol component used in this technology is, for example, 1.0 part by mass or more, preferably 5.0 parts by mass or more, and more preferably 10 parts by mass or more. In this technology, by setting the polyester polyol content in the polyol component within this range, the reactivity during polyurethane foam production can be improved, and the physical properties of the polyurethane foam produced can be further improved.
[0031] The upper limit of the polyester polyol content in 100 parts by mass of the polyol component used in this technology is, for example, 40 parts by mass or less, preferably 30 parts by mass or less, and more preferably 25 parts by mass or less. By setting the polyester polyol content in the polyol component within this range, this technology can improve the biomass content of the polyurethane foam produced, reduce environmental impact, and further contribute to the formation of a sustainable society.
[0032] (1-2-2) Polymer Polyols In this technology, it is preferable to use polymer polyols as polyols other than biomass-derived polyols. By using polymer polyols, the elongation of the polyurethane foam produced can be improved.
[0033] Polymer polyols are those obtained by polymerizing ethylenically unsaturated monomers in a polyol, or by emulsifying and dispersing polymers of ethylenically unsaturated monomers in a polyol. Specifically, examples include those obtained by graft polymerization of acrylonitrile, styrene, etc., into a polyol, or those obtained by dispersing polystyrene or polyacrylonitrile in a polyol.
[0034] When polymer polyols are used as polyols other than biomass-derived polyols, their content can be freely set as long as it does not impair the function and effects of this technology. The lower limit of the polymer polyol content in 100 parts by mass of the polyol component used in this technology is, for example, 1.0 part by mass or more, preferably 2.0 parts by mass or more, and more preferably 3.0 parts by mass or more. In this technology, by setting the polymer polyol content in the polyol component within this range, the reactivity during polyurethane foam production can be improved, and the physical properties of the polyurethane foam produced can be further improved.
[0035] The upper limit of the content of the polymer polyol in 100 parts by mass of the polyol component used in the present technology is, for example, 40 parts by mass or less, preferably 30 parts by mass or less, and more preferably 25 parts by mass or less. In the present technology, by setting the content of the polymer polyol in the polyol component within this range, the biomass degree of the produced polyurethane foam can be improved, the environmental load can be reduced, and further contribution can be made to the formation of a sustainable society.
[0036] For example, when a biomass-derived polyether polyol is used as the biomass-derived polyol, the lower limit of the content of the polymer polyol in 100 parts by mass of the polyol component is, for example, 5.0 parts by mass or more, preferably 6.0 parts by mass or more, and more preferably 7.0 parts by mass or more. The upper limit of the content of the polymer polyol in 100 parts by mass of the polyol component is, for example, 20 parts by mass or less, preferably 15 parts by mass or less, more preferably 12 parts by mass or less, and even more preferably 10 parts by mass or less.
[0037] For example, when a biomass-derived polyester polyol is used as the biomass-derived polyol, the lower limit of the content of the polymer polyol in 100 parts by mass of the polyol component is, for example, 1.0 part by mass or more, preferably 2.0 parts by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 4.0 parts by mass or more. The upper limit of the content of the polymer polyol in 100 parts by mass of the polyol component is, for example, 40 parts by mass or less, preferably 35 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 25 parts by mass or less.
[0038] (1-2-3) Polyether Polyol In the present technology, a polyether polyol can be used as a polyol other than the biomass-derived polyol. In particular, when a biomass-derived polyester polyol is used as the biomass-derived polyol, it is preferable to use a polyether polyol as the polyol other than the biomass-derived polyol. By using the polyether polyol, the glass transition point of the produced polyurethane foam can be shifted to the low temperature side, and a polyurethane foam that is more resilient and yet softer can be produced.
[0039] Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol and the like, which are obtained by polymerizing cyclic ethers such as ethylene oxide (EO), propylene oxide (PO), and tetrahydrofuran with an initiator, as well as copolyethers thereof. They can also be obtained by polymerizing the above cyclic ethers using polyhydric alcohols such as glycerin and trimethylolethane.
[0040] When a polyether polyol is used as the polyol other than the biomass-derived polyol, its content can be freely set as long as the actions and effects of the present technology are not impaired. The lower limit of the content of the polyether polyol in 100 parts by mass of the polyol component used in the present technology is, for example, 1.0 part by mass or more, preferably 3.0 parts by mass or more, and more preferably 5.0 parts by mass or more. In the present technology, by setting the content of the polyether polyol in the polyol component within this range, the flexibility of the produced polyurethane foam can be improved, and the glass transition point can be further lowered.
[0041] The upper limit of the content of the polyether polyol in 100 parts by mass of the polyol component used in the present technology is, for example, 40 parts by mass or less, preferably 35 parts by mass or less, and more preferably 30 parts by mass or less. In the present technology, by setting the content of the polyether polyol in the polyol component within this range, the biomass degree of the produced polyurethane foam can be improved, the environmental load can be reduced, and further contributions can be made to the formation of a sustainable society.
[0042] (1-2-4) Polyester ether polyols Examples of polyester ether polyols include aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, and azelaic acid; aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid; alicyclic dicarboxylic acids such as hexahydrophthalic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid; or those obtained by a dehydration condensation reaction of these acid esters or acid anhydrides with glycols such as diethylene glycol or propylene oxide adducts, or mixtures thereof.
[0043] (1-2-5) Polycarbonate polyols Examples of polycarbonate polyols include those obtained by reacting at least one polyhydric alcohol such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, 1,8-octanediol, 1,9-nonanediol, and diethylene glycol with diethylene carbonate, dimethyl carbonate, diethyl carbonate, etc.
[0044] (1-2-6) Biodegradable Polyols In this technology, biodegradable polyols can also be used with consideration for the environment. As biodegradable polyols that can be used in this technology, one or more types of biodegradable polyols that can be used in the manufacture of polyurethane foam can be freely selected and used, as long as the purpose and effects of this technology are not impaired. Examples include polyglycolic acid (PGA), polylactic acid (PLA), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), polycaprolactone (PCL), polyethylene glycol (PEG), polyvinyl alcohol (PVA), and polyhydroxyalkanoic acid (PHA).
[0045] (1-2-7) Resin Modifiers In this technology, resin modifiers can be used. In particular, when biomass-derived polyether polyols are used as biomass-derived polyols, it is preferable to use resin modifiers.
[0046] Resin modifiers are used to improve the various physical properties of the polyurethane foam being manufactured. For example, when using a resin modifier to improve the flossability of the polyurethane foam being manufactured, it is preferable to use a resin modifier that contains polymer particles having a core-shell structure.
[0047] Polymer particles having a core-shell structure specifically refer to rubber particles in which a particulate core component, mainly composed of a crosslinked rubber-like polymer, is coated with a shell component by graft polymerization of a polymer different from the core component onto its surface. Examples of the core component include crosslinked rubber particles. The type of rubber used for the crosslinked rubber particles is not limited and includes, for example, butadiene rubber, acrylic rubber, silicone rubber, butyl rubber, nitrile rubber, styrene rubber, synthetic natural rubber, and ethylene propylene rubber. Examples of the shell component include polymers polymerized from one or more monomers selected from the group consisting of acrylic acid esters, methacrylic acid esters, and aromatic vinyl compounds.
[0048] The shell component is preferably graft polymerized onto the core component and chemically bonded to the polymer constituting the core component. Furthermore, considering dispersibility with polyols, it is preferable that the core-shell rubber particles include a methyl methacrylate-butadiene-ethylene copolymer (MBS) polymer.
[0049] The lower limit of the particle size (volume-average particle diameter) of the polymer particles used in the resin modifier is, for example, 10 nm or more, preferably 50 nm or more, more preferably 100 nm or more, and even more preferably 200 nm or more. The upper limit of the particle size (volume-average particle diameter) of the polymer particles used in the resin modifier is, for example, 2000 nm or less, preferably 800 nm or less, more preferably 600 nm or less, and even more preferably 400 nm or less.
[0050] The lower limit of the polymer particle content used in the resin modifier is, for example, 1.0 part by mass or more, preferably 1.5 parts by mass or more, and more preferably 2.0 parts by mass or more, when the polyol component used in this technology is 100 parts by mass or less, preferably 8.0 parts by mass or less, and more preferably 6.0 parts by mass or less, when the polyol component used in this technology is 100 parts by mass or less.
[0051] The polymer particles used in the resin modifier are preferably used in the raw material composition as a polymer particle dispersion in a polyol that functions as a solvent, in order to facilitate mixing with polyols and the like. When a polyol is used as the solvent, this polyol should be included in the polyol contained in the raw material composition.
[0052] The polyol that functions as a solvent is not particularly limited, but examples include polypropylene glycol. The lower limit of the number-average molecular weight of the polypropylene glycol used as a solvent is, for example, 300 or more, preferably 350 or more. The upper limit of the number-average molecular weight of the polypropylene glycol used as a solvent is, for example, 600 or less, preferably 500 or less. The mass ratio of polymer particles to polypropylene glycol (polymer particles:polypropylene glycol) in the polymer particle dispersion is preferably, for example, 40:60 to 50:50.
[0053] The lower limit of the resin modifier content is, for example, 1.0 part by mass or more, preferably 2.0 parts by mass or more, and more preferably 3.0 parts by mass or more, when the polyol component used in this technology is 100 parts by mass. The upper limit of the resin modifier content is, for example, 20 parts by mass or less, preferably 15 parts by mass or less, and more preferably 10 parts by mass or less, when the polyol component used in this technology is 100 parts by mass.
[0054] (2) Isocyanates The isocyanates that can be used in this technology may be freely selected from one or more types of isocyanates that can be used in the manufacture of polyurethane foam, as long as the purpose and effects of this technology are not impaired. For example, aliphatic isocyanates such as hexamethylene diisocyanate, isophorone diisocyanate, and dicyclohexylmethane diisocyanate; aromatic isocyanates such as toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate, xylylene diisocyanate, and polymeric polyisocyanate; and modified polyisocyanates obtained by modifying these. Among these, in this technology, it is preferable to use diphenylmethane diisocyanate (MDI) or modified MDI as the isocyanate, more preferably polymeric MDI (crude MDI) or carbodiimide-modified MDI, and even more preferably polymeric MDI (crude MDI).
[0055] The isocyanate index of the polyurethane foam is not particularly limited, as long as it does not impair the function and effects of this technology. In this technology, the lower limit of the isocyanate index is, for example, 75 or higher, preferably 80 or higher, more preferably 85 or higher, even more preferably 90 or higher, and particularly preferably 95 or higher. By setting the lower limit of the isocyanate index within this range, the deterioration of the compression residual strain of the manufactured polyurethane foam can be suppressed, preventing the polyurethane foam from sagging and improving its cushioning performance.
[0056] The upper limit of the isocyanate index is, for example, 120 or less, preferably 115 or less, and more preferably 110 or less. By setting the upper limit of the isocyanate index within this range, the elongation of the polyurethane foam can be improved, while suppressing increased hardness and preventing a decrease in flexibility.
[0057] In this technology, the isocyanate index is calculated using the formula: [(Isocyanate equivalent in the polyurethane foam manufacturing composition / Equivalent of active hydrogen in the polyurethane foam manufacturing composition) × 100].
[0058] (3) Foam stabilizers Foam stabilizers can be used in the manufacture of polyurethane foam according to this technology. By using foam stabilizers, higher quality polyurethane foam can be manufactured.
[0059] As foam stabilizers that can be used in this technology, one or more types of foam stabilizers that can be used in the manufacture of polyurethane foam can be freely selected and used, as long as they do not impair the function or effect of this technology. Examples include silicone-based foam stabilizers, fluorine-containing compound-based foam stabilizers, surfactants, etc. Examples of silicone-based foam stabilizers include those mainly composed of siloxane chains, those in which siloxane chains and polyether chains form a linear structure, those that are branched and separated, and those in which polyether chains are modified into a pendant-like structure of siloxane chains. Among these, it is preferable to use a silicone-based foam stabilizer as the foam stabilizer in this technology.
[0060] The amount of foam stabilizer in the composition used to manufacture the polyurethane foam according to this technology can be freely set as long as it does not impair the function and effects of this technology. The lower limit of the foam stabilizer content in the composition is, for example, 1.0 part by mass or more, preferably 2.0 parts by mass or more, and more preferably 3.0 parts by mass or more, per 100 parts by mass of polyol. The upper limit of the foam stabilizer content in the composition is, for example, 20 parts by mass or less, preferably 18 parts by mass or less, and more preferably 15 parts by mass or less, per 100 parts by mass of polyol.
[0061] (4) Catalysts Catalysts may be used in the production of polyurethane foam according to this technology. As for catalysts that can be used in this technology, one or more catalysts that can be used in the production of polyurethane foam may be freely selected and used, as long as they do not impair the action or effect of this technology.
[0062] Examples of catalysts include metal catalysts (organometallic catalysts) such as organoiron compounds (iron acetylacetonate, etc.), organonickel compounds (nickel acetylacetonate, nickel octoate, nickel naphthenate, etc.), organotin compounds (tin(II) octoate (tin 2-ethylhexanoate, stanus octoate, etc.), organobismuth compounds (bismuth octoate, bismuth naphthenate, etc.), organolead compounds (lead octanoate, lead naphthenate, etc.), organocobalt compounds (cobalt acetylacetonate, cobalt octoate, cobalt naphthenate, etc.), organozirconium compounds (zirconium acetylacetonate, etc.), and organozinc compounds, as well as triethylamine, triethylenediamine (TEDA), tetramethylguanidine, diethanolamine, bis(2-dimethylaminoethyl) ether, N,N,N Examples of amine catalysts include ',N'',N''-pentamethyldiethylenetriamine, imidazole compounds, piperazine amines such as dimethylpiperazine, N-methyl-N'-(2-dimethylamino)ethylpiperazine, and N-methyl-N'-(2-hydroxyethyl)piperazine, morpholine amines such as N-methylmorpholine and N-ethylmorpholine, and amines referred to as DBU congeners such as 1,8-diazabicyclo-[5,4,0]-undecene-7 (DBU), 1,5-diazabicyclo-[4,3,0]-nonene-5 (DBN), 1,8-diazabicyclo-[5,3,0]-decene-7 (DBD), and 1,4-diazabicyclo-[3,3,0]octene-4 (DBO). Among these, the use of organoiron compounds is preferred in this technology, and the use of iron acetylacetonate is more preferred.
[0063] The amount of catalyst in the composition used to manufacture the polyurethane foam according to this technology can be freely set as long as it does not impair the function and effects of this technology. In this technology, the lower limit of the catalyst content in the composition is, for example, 0.1 parts by mass or more, preferably 0.2 parts by mass or more, and more preferably 0.3 parts by mass or more, per 100 parts by mass of polyol. By setting the lower limit of the catalyst content in the composition within this range, various reactions during manufacturing can be controlled, and as a result, polyurethane foam with excellent mechanical properties and appearance can be obtained.
[0064] In this technology, the upper limit of the catalyst content in the composition is, for example, 10 parts by mass or less, preferably 9.0 parts by mass or less, and more preferably 8.0 parts by mass or less, per 100 parts by mass of polyol. By setting the upper limit of the catalyst content in the composition within this range, it is possible to prevent destabilization of various reactions during manufacturing. As a result, polyurethane foam with excellent mechanical properties and appearance can be obtained.
[0065] (5) Antioxidants Antioxidants can be used in the production of polyurethane foam according to this technology. As antioxidants that can be used in this technology, one or more antioxidants that can be used in the production of polyurethane foam can be freely selected and used, as long as they do not impair the action or effect of this technology. For example, one or more antioxidants can be freely combined and used from phenolic (monophenolic, thiobisphenolic, hindered phenolic), naphthylamine, diphenylamine, p-phenyldiamine, quinoline, hydroquinone derivatives, phosphite esters, etc. Among these, it is preferable to use a phenolic antioxidant as the antioxidant in this technology.
[0066] The amount of antioxidant in the composition used to manufacture the polyurethane foam according to this technology can be freely set as long as it does not impair the function and effects of this technology. In this technology, the lower limit of the antioxidant content in the composition is, for example, 0.01 parts by mass or more, preferably 0.03 parts by mass or more, and more preferably 0.05 parts by mass or more, per 100 parts by mass of polyol. By setting the lower limit of the antioxidant content in the composition within this range, the discoloration prevention effect by preventing scorching can be improved.
[0067] In this technology, the upper limit of the antioxidant content in the composition is, for example, 5.0 parts by mass or less, preferably 3.0 parts by mass or less, and more preferably 1.0 part by mass or less, per 100 parts by mass of polyol. By setting the upper limit of the antioxidant content in the composition within this range, cost reduction can be achieved.
[0068] (6) Fillers The fillers that can be used in this technology may be freely selected from one or more types of fillers that can be used in the manufacture of polyurethane foam, as long as they do not impair the purpose and effects of this technology. When polyurethane foam is manufactured by the mechanical floss method described later, the fillers also function as nucleating agents (foaming starting points). Examples include metal hydroxides such as calcium carbonate, aluminum hydroxide, and magnesium hydroxide, alumina trihydrate, silica, talc, calcium carbonate, and clay. Among these, metal hydroxides are preferred as fillers in this technology, and aluminum hydroxide is more preferred among metal hydroxides.
[0069] The amount of filler in the composition used to manufacture the polyurethane foam according to this technology can be freely set as long as it does not impair the function or effect of this technology. In this technology, the lower limit of the filler content in the composition is, for example, 1.0 part by mass or more, preferably 2.0 parts by mass or more, and more preferably 3.0 parts by mass or more, per 100 parts by mass of polyol. The upper limit of the filler content in the composition is, for example, 20 parts by mass or less, preferably 15 parts by mass or less, and more preferably 12 parts by mass or less, per 100 parts by mass of polyol.
[0070] (7) Desiccants Desiccants can be used in the production of polyurethane foam according to this technology. By using desiccants, unintended foaming can be prevented due to moisture in the reaction atmosphere or contained in the material. In particular, it is preferable to use desiccants when producing polyurethane foam by the mechanical floss method. As for desiccants that can be used in this technology, one or more types of desiccants that can be used with polyurethane foam can be freely selected and used as long as they do not impair the action or effect of this technology. Examples of desiccants include zeolite, silica gel, calcium oxide, activated carbon, potassium hydroxide, sodium hydroxide, lithium hydroxide, etc. Among these, it is preferable to use zeolite as the desiccant in this technology.
[0071] The amount of hygroscopic agent in the composition used for manufacturing polyurethane foam according to this technology can be freely set as long as it does not impair the function or effect of this technology. In this technology, the lower limit of the hygroscopic agent content in the composition is, for example, 0.1 parts by mass or more, preferably 0.3 parts by mass or more, and more preferably 0.5 parts by mass or more, per 100 parts by mass of polyol. The upper limit of the hygroscopic agent content in the composition is, for example, 10 parts by mass or less, preferably 7 parts by mass or less, and more preferably 5 parts by mass or less, per 100 parts by mass of polyol.
[0072] (8) Foaming gas Foaming gas can be used in the manufacture of polyurethane foam according to this technology. As for the foaming gas that can be used in this technology, one or more types of foaming gas that can be used in the manufacture of polyurethane foam can be freely selected and used, as long as they do not impair the function or effect of this technology.
[0073] Examples of foaming gases include dry air and inert gases such as nitrogen. The mixing ratio of the foaming gas with other raw materials can be freely set according to the intended use of the polyurethane foam being manufactured, as long as it does not impair the purpose and effects of this technology. In this technology, the mixing ratio of the foaming gas with other raw materials can be set to, for example, 50% or more by volume, preferably 55% or more by volume, and more preferably 60% or more by volume, of the total 100% by volume of the foaming gas and other raw materials.
[0074] In this technology, the upper limit of the mixing ratio of the foaming gas with other raw materials can be set to, for example, 95% or less by volume, or 90% or less by volume, out of 100% of the total volume of the foaming gas and other raw materials.
[0075] (9) Foaming Agents As described later, the polyurethane foam according to this technology can be manufactured by the mechanical flossing method, in which case it is possible to manufacture the polyurethane foam according to this technology even without a foaming agent. However, it is also possible to use a foaming agent in this technology. That is, the polyurethane foam according to this technology can also be manufactured by a method using a foaming agent other than the mechanical flossing method. As for the foaming agents that can be used in this technology, one or more foaming agents that can be used in the manufacture of polyurethane foam can be freely selected and used, as long as they do not impair the purpose and effects of this technology.
[0076] The blowing agent that can be used in this technology can be either a chemical blowing agent or a physical blowing agent. Examples of chemical blowing agents include reactive blowing agents that generate carbon dioxide gas and cause foaming by reacting with water or the aforementioned isocyanates such as formic acid and acetic acid, physical blowing agents such as volatile hydrocarbons, and organic or inorganic thermal decomposition type chemical blowing agents. Examples of inorganic blowing agents include sodium bicarbonate, ammonium carbonate, sodium carbonate, ammonium bicarbonate, ammonium nitrite, sodium borohydride, and anhydrous monosodium citrate.
[0077] Examples of physical blowing agents include chlorofluorocarbons (HCFCs) and hydrofluorocarbons (HFCs), hydrofluoroolefins (HFOs), hydrocarbons such as heptane, hexane, pentane, and cyclopentane, and carbon dioxide.
[0078] The amount of foaming agent in the composition used to manufacture polyurethane foam according to this technology can be freely set as long as it does not impair the function and effects of this technology. In this technology, the foaming agent content in the composition is, for example, 10 parts by mass or less, preferably 7.0 parts by mass or less, and more preferably 5.0 parts by mass or less, per 100 parts by mass of polyol. By setting the upper limit of the foaming agent content in the composition within this range, it is possible to suppress formation defects due to excessive foaming and also contribute to cost reduction.
[0079] (10) In addition, in the manufacture of polyurethane foam relating to this technology, one or more other components that can be used in the manufacture of polyurethane foam may be freely selected and used as other components, as long as they do not impair the function or effect of this technology.
[0080] Examples of components that can be used in the manufacture of polyurethane foam related to this technology include flame retardants, pigments, stabilizers, plasticizers, colorants, crosslinking agents, antibacterial agents, dispersants, and ultraviolet absorbers.
[0081] 2. Polyurethane foam The polyurethane foam relating to this technology can be manufactured using the composition described above.
[0082] (1) Biomass content As demonstrated in the examples described later, this technology makes it possible to produce high-quality polyurethane foam even when using biomass-derived polyols. Therefore, it is possible to improve the biomass content of the produced polyurethane foam and contribute to environmental preservation and the formation of a sustainable society. The biomass content of the polyurethane foam according to this technology can be, for example, 20% or more, preferably 25% or more, and more preferably 30% or more.
[0083] In this technology, the biomass percentage is calculated using the following formula: Biomass percentage (%) = {(Weight of biomass material × Biomass percentage of biomass material / 100) / Total weight of raw materials} × 100
[0084] (2) Density The polyurethane foam relating to this technology has a density of 100 kg / m³ 3 More than 500kg / m 3 The following characteristics apply: The polyurethane foam relating to this technology has a density of 100 kg / m³. 3 As such, it can be suitably used as a cushioning material for vibration and shock absorption in electronic devices such as mobile phones, cameras, and televisions, as well as electrical equipment such as home appliances, as a sealing material for various batteries, as a sealing material around the battery and electronic control unit of electric vehicles, as well as as a heat insulating material.
[0085] The lower limit of the density of the polyurethane foam related to this technology is 100 kg / m³. 3If the value is at least the above, the effects of the present technology can be exhibited, and it is preferably 120 kg / m 3 or more, more preferably 130 kg / m 3 or more, still more preferably 140 kg / m 3 or more, even more preferably 150 kg / m 3 or more.
[0086] The upper limit of the density of the polyurethane foam according to the present technology is 500 kg / m 3 If the value is at most the following, the effects of the present technology can be exhibited, and it is preferably 450 kg / m 3 or less, more preferably 400 kg / m 3 or less. By setting the density of the polyurethane foam within this range, the flexibility of the polyurethane foam is not impaired (hardening is prevented), and cushioning properties can be imparted.
[0087] In the present technology, the density is a value measured by a method conforming to JIS K6401:2011.
[0088] (3) Hysteresis loss rate The hysteresis loss rate of the polyurethane foam according to the present technology is 20% or less. Since the hysteresis loss rate of the polyurethane foam according to the present technology is 20% or less, it can exhibit high resilience performance equal to or higher than that of a general polyurethane foam using petroleum-derived raw materials, even though a biomass-derived raw material is used.
[0089] As long as the hysteresis loss rate of the polyurethane foam according to the present technology is 20% or less, the functions and effects of the present technology can be exhibited, and it is preferably 19% or less, more preferably 18% or less, still more preferably 17% or less, even more preferably 16% or less, and particularly preferably 15% or less.
[0090] In this technology, the hysteresis loss rate is a value measured according to the method conforming to JIS K 6254. More specifically, the SS curve (stress-strain curve) used to calculate the hysteresis loss rate is measured according to the method conforming to JIS K 6254, and the hysteresis loss rate is calculated from the measurement results of the SS curve using the calculation formula described in section 6.8.3 of JIS K 6400-2.
[0091] (4) Glass transition temperature The glass transition temperature of the polyurethane foam according to this technology is characterized by being -10°C or lower. Because the polyurethane foam according to this technology has a glass transition temperature of -10°C or lower, changes in hardness at low temperatures can be suppressed.
[0092] The glass transition temperature of the polyurethane foam according to this technology can exhibit its effects and properties if it is -10°C or lower, but preferably -15°C or lower, and more preferably -20°C or lower.
[0093] In this technology, the glass transition temperature is the value measured by the method described in the examples below.
[0094] (5) Elongation The elongation of the polyurethane foam according to this technology can be freely set as long as it does not impair the function or effect of this technology. The lower limit of the elongation of the polyurethane foam according to this technology is, for example, 40% or more, preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more. The upper limit of the elongation of the polyurethane foam according to this technology is, for example, 300% or less, preferably 250% or less, and more preferably 200% or less.
[0095] In this technology, the elongation was measured using a method compliant with JIS K6251:2010.
[0096] (6) Thickness The thickness of the polyurethane foam relating to this technology can be freely set as long as it does not impair the purpose or effect of this technology. However, even when the thickness of the polyurethane foam relating to this technology is 10 mm or less, it will still be soft while being highly resilient.
[0097] The lower limit of the thickness of the polyurethane foam related to this technology can be freely set as long as it does not impair the purpose or effect of this technology, but for example, it is 0.05 mm or more, preferably 0.1 mm or more, and more preferably 0.2 mm or more. By setting the thickness of the polyurethane foam within this range, better rebound properties can be achieved.
[0098] The upper limit of the thickness of the polyurethane foam related to this technology can also be freely set as long as it does not impair the purpose or effect of this technology, but for example, it is 10 mm or less, preferably 7.0 mm or less, and more preferably 5.0 mm or less.
[0099] (7) Applications The polyurethane foam relating to this technology can be used in all fields and for all purposes by taking advantage of its high quality. For example, it can be suitably used in furniture such as sofas and chairs, bedding such as mattresses and pillows, clothing such as underwear, daily necessities such as tableware and cleaning sponges, vehicle and aircraft interior products such as car seats, building joint materials, building cushioning materials, building sealants, home appliance sealants, electrical equipment cushioning materials, electronic equipment cushioning materials, electrical equipment sealants, electronic equipment sealants, various battery sealants, soundproofing materials, packaging materials, vehicle insulation materials, vehicle battery sealants, vehicle electronic control unit sealants, condensation prevention materials, interior materials, home appliance insulation materials, pipe insulation materials, various covers, cushioning materials, toys, miscellaneous goods, etc.
[0100] 3. Method for Manufacturing Polyurethane Foam The polyurethane foam according to this technology can be manufactured by mixing the components of the composition described above to prepare a composition, and then foaming the prepared composition using a known method. The specific methods for the composition preparation process, the foaming process, etc., can be freely combined and adopted using general methods, as long as they do not impair the function and effect of this technology.
[0101] In the polyurethane foam manufacturing method according to this technology, it is particularly preferable to employ the mechanical flossing method. By employing the mechanical flossing method, density can be easily adjusted compared to the chemical foaming method, and high-density polyurethane foam can be manufactured. Furthermore, thin polyurethane foam can also be manufactured.
[0102] As for the specific method of the mechanical flossing method, a general mechanical flossing method can be used as long as it does not impair the function and effect of this technology. For example, the raw materials other than the isocyanate and foaming gas of the aforementioned composition are added to the mixing head at timings according to the type and purpose of each raw material, and mixed to prepare an intermediate composition. The prepared intermediate composition is then mixed with isocyanate while simultaneously adding the foaming gas, stirring until homogeneous, and then heated and cured on release paper or in a mold to produce polyurethane foam.
[0103] Furthermore, this technology can have the following configuration: [1] A polyurethane foam obtained from a raw material composition containing a polyol component, wherein the polyol component contains a biomass-derived polyol, the hysteresis loss rate measured in accordance with JIS K 6254 is 20% or less, the glass transition temperature is -10°C or lower, and the density is 100 kg / m³ 3 More than 500kg / m 3 The polyurethane foam is as follows: [2] The polyurethane foam according to [1], wherein the biomass-derived polyol comprises a first biomass-derived polyol having a number average molecular weight of 1500 or more, and a second biomass-derived polyol having a molecular weight or number average molecular weight of 100 or more and 1000 or less. [3] The polyurethane foam according to [1] or [2], wherein the elongation measured in accordance with JIS K6251:2010 is 50% or more. [4] The polyurethane foam according to any one of [1] to [3], wherein the polyol component comprises a petroleum-derived polyol having a molecular weight or number average molecular weight of 100 or more and 1000 or less. [5] The polyurethane foam according to any one of [1] to [4], wherein the polyol component comprises a polymer polyol. [6] The polyurethane foam according to any one of [1] to [5], wherein the biomass content is 20% or more. [7] A cushioning material, a sealing material, or a heat insulating material using the polyurethane foam according to any one of [1] to [6].
[0104] [8] A polyurethane foam obtained from a raw material composition containing a polyol component, wherein the polyol component contains a biomass-derived polyol, and the biomass-derived polyol comprises a first biomass-derived polyol having a number average molecular weight of 1500 or more, and a second biomass-derived polyol having a molecular weight or number average molecular weight of 100 or more and 1000 or less. [9] The polyurethane foam according to [8], wherein the polyol component contains a petroleum-derived polyol having a molecular weight or number average molecular weight of 100 or more and 1000 or less.
[10] The polyurethane foam according to [8] or [9], wherein the polyol component contains a polymer polyol.
[0105]
[11] The polyurethane foam according to any one of [8] to
[10] , wherein the biomass-derived polyol contains a biomass-derived ether polyol.
[12] The polyurethane foam according to
[11] , wherein the raw material composition contains a resin modifier.
[13] The polyurethane foam according to
[12] , wherein the resin modifier contains polymer particles having a core-shell structure.
[0106]
[14] The polyurethane foam according to any one of [8] to
[10] , wherein the biomass-derived polyol contains a biomass-derived ester polyol.
[15] The polyurethane foam according to
[14] , wherein the polyol component contains a petroleum-derived polyether polyol.
[0107] The present technology will be described in more detail below based on the following examples. The examples described below are representative examples of the present technology and should not be interpreted as narrowing the scope of the present technology.
[0108] (1) Raw material biomass-derived ether polyol 1: Condensate of 1,3-propanediol derived from corn, hydroxyl value 199 mg KOH / g, number of functional groups 2, number average molecular weight 500, biomass content 100% Biomass-derived ether polyol 2: Condensate of 1,3-propanediol derived from corn, hydroxyl value 59 mg KOH / g, number of functional groups 2, number average molecular weight 2000, biomass content 100% Biomass-derived ester polyol 1: Castor oil-modified polyol, hydroxyl value 50 mg KOH / g, number of functional groups 2.2, number average molecular weight 2500, biomass content 100% Biomass-derived ester polyol 2: Deodorized and refined castor oil, hydroxyl value 163 mg KOH / g, number of functional groups 2.7, number average molecular weight 929, biomass content 100% Biomass-derived ester polyol 3: Castor oil-modified polyol, hydroxyl value 225 mg KOH / g, number of functional groups 2.5, number average molecular weight 623, biomass content 70% Polyester polyol 1: Polycaprolactone-based polyester polyol, hydroxyl value 212 mg KOH / g, number of functional groups 2, number average molecular weight 529 Polyester polyol 2: Polyadipate-based polyester polyol, hydroxyl value 212 mg KOH / g, number of functional groups 2, number average molecular weight 529 Resin modifier: Dispersion of methyl methacrylate butadiene styrene copolymer (MBS resin) particles dispersed in polypropylene glycol, hydroxyl value 171 mg KOH / g, number of functional groups 2, number average molecular weight 400 Polymer polyol 1: hydroxyl value 30.6 mg KOH / g, number of functional groups 2, number average molecular weight 3000 Polymer polyol 2: Hydroxyl value 43.5 mg KOH / g, number of functional groups 3, number average molecular weight 3000 Polyether polyol 1: Hydroxyl value 39.8 mg KOH / g, number of functional groups 2, number average molecular weight 2819 Polyether polyol 2: Hydroxyl value 28.1 mg KOH / g, number of functional groups 2, number average molecular weight 4000 Polyether polyol 3: Hydroxyl value 23.8 mg KOH / g, number of functional groups 3, number average molecular weight 7000 Polyether polyol 4: Hydroxyl value 56 mg KOH / g, number of functional groups 2, number average molecular weight 2000 Polyether polyol 5: Hydroxyl value 50.3 mg KOH / g, number of functional groups 3, number average molecular weight 3346 Polyether polyol 6: Hydroxyl value 280 mg KOH / g, number of functional groups 3, number average molecular weight 600Chain extender: Dipropylene glycol, hydroxyl value 837 mg KOH / g, number of functional groups 2, molecular weight 134 Foam stabilizer: Silicone-based foam stabilizer, hydroxyl value 40 mg KOH / g, number of functional groups 1, number average molecular weight 1400 Catalyst 1: Iron acetylacetonate Catalyst 2: Nickel acetylacetonate Antioxidant: Phenolic antioxidant Filler: Aluminum hydroxide Desiccant: Synthetic zeolite Isocyanate 1: Polymeric MDI, NCO% = 31.5, number of functional groups 2.4, number average molecular weight 320 Isocyanate 2: Carbodiimide-modified MDI, NCO% = 30.88, number of functional groups 2.15, number average molecular weight 292
[0109] (2) Manufacturing of polyurethane foam Each component shown in Table 1 below was prepared in the mixing ratios shown in Table 1 below to obtain the mixed raw materials for each example and each comparative example. Next, the mixed raw materials were put into a mixing head and mixed while stirring until homogeneous with foaming gas (inert gas: nitrogen). After that, the mixed raw materials were applied to a continuously supplied release paper to the thickness shown in Table 1 below and heated and cured at 200°C to produce a sheet of polyurethane foam.
[0110] (2) Measurement and evaluation of physical properties
[0111] [Biomass Content] The biomass content was calculated using the following formula: Biomass Content (%) = {(Weight of biomass material × Biomass content of biomass material / 100) / Total weight of raw materials} × 100
[0112] [Density] The density was measured according to the method compliant with JIS K6401:2011.
[0113] [Tensile Strength] Tensile strength was measured according to the method in accordance with JIS K6251:2010.
[0114] [Elongation Rate] The elongation rate was measured using a method compliant with JIS K6251:2010.
[0115] [Tear Strength] Tear strength was measured according to the method in accordance with JIS K 6252:2007.
[0116] [Compression Hardness] The 25% and 40% compression hardness were measured using a method compliant with JIS K6254:2010.
[0117] [Compression Residual Strain] The compression residual strain was measured using a method compliant with JIS K6401:2011.
[0118] [Glass Transition Point] Test equipment: Using an ARES-G2 rheometer manufactured by TA Instruments, the temperature at the peak of tanδ (glass transition point) was measured under the following conditions: temperature range: -40°C to 80°C (heating rate: 3°C / min), mode: parallel plate mode (φ8 mm), strain: 0.5%, frequency: 1.0 Hz.
[0119] [Hysteresis Loss Rate] The hysteresis loss rate was measured using a method compliant with JIS K 6254.
[0120] (3) Results The results are shown in Table 1 below.
[0121] (4) Discussion As shown in Reference Examples 1-4 and Comparative Examples 1-4 in Table 1, compared to general polyurethane foam made from petroleum-derived polyols, polyurethane foam made from biomass-derived polyols had a higher glass transition temperature (Comparative Example 1), poor flossability, and high density (Comparative Examples 2 and 3). On the other hand, in this technology, despite using biomass-derived polyols, the foam has good flossability and a moderate density, so it has softness equivalent to or better than Reference Examples 1-4 made from petroleum-derived polyols, and because the glass transition temperature is below -10°C, the hardness change can be reduced even at low temperatures, and because it has a low hysteresis loss rate, it was possible to manufacture polyurethane foam with high rebound performance equivalent to or better than Reference Examples 1-4 made from petroleum-derived polyols.
[0122] Comparing the examples, it was found that Examples 1 to 9, which used petroleum-derived polyols with a molecular weight or number-average molecular weight of 100 or more and 1000 or less, showed improved elongation compared to Example 10, which used only biomass-derived polyols.
[0123] Furthermore, in Comparative Example 4, where a petroleum-derived polyester polyol was added to Example 10, which used only a biomass-derived polyol, the elongation improved, but the hysteresis loss rate increased, resulting in a decrease in resilience. On the other hand, as shown in Examples 1 to 9, by using a petroleum-derived polymer polyol, we succeeded in improving the elongation rate while maintaining a low hysteresis loss rate.
Claims
1. A polyurethane foam obtained from a raw material composition containing a polyol component, wherein the polyol component contains a biomass-derived polyol, the hysteresis loss rate measured in accordance with JIS K6254 is 20% or less, the glass transition temperature is -10°C or lower, and the density is 100 kg / m³. 3 More than 500kg / m 3 The following is polyurethane foam.
2. The polyurethane foam according to claim 1, wherein the biomass-derived polyol comprises a first biomass-derived polyol having a number average molecular weight of 1500 or more, and a second biomass-derived polyol having a molecular weight or number average molecular weight of 100 or more and 1000 or less.
3. The polyurethane foam according to claim 1, wherein the elongation rate measured in accordance with JIS K 6251:2010 is 50% or more.
4. The polyurethane foam according to claim 3, wherein the polyol component contains a petroleum-derived polyol having a molecular weight or number average molecular weight of 100 or more and 1000 or less.
5. The polyurethane foam according to claim 1, wherein the polyol component contains a polymer polyol.
6. The polyurethane foam according to claim 1, wherein the biomass content is 20% or more.
7. A cushioning material, sealing material, or heat insulating material using the polyurethane foam described in any one of claims 1 to 6.