Molded body

The molded body with multi-stage protrusions addresses the inefficiencies of conventional cushioning materials by providing effective shock absorption and reducing waste, allowing for versatile packaging solutions.

WO2026234857A1PCT designated stage Publication Date: 2026-11-12KOBAYASHI & CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2025/043207
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2025-12-11
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Conventional cushioning materials for packaging, such as synthetic resin bubble wrap and cardboard retaining members, are bulky, generate waste, and fail to adequately absorb shocks during transportation, making it difficult to package diverse products on the same line.

Method used

A molded body with multi-stage protrusions formed from a resin composition containing biomass material and thermoplastic resin, designed to absorb shocks by collapsing under impact, featuring a recovery rate of 40% or more and cross-sectional areas decreasing in a plan view.

Benefits of technology

The molded body effectively mitigates impact from drops and vibrations, reducing material waste and enabling packaging of varied products on a single line with enhanced shock absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2025043207_12112026_PF_FP_ABST
    Figure JP2025043207_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a molded body having excellent shock absorbing properties with regard to a packaged object, such as a product, that is packaged in a container, when the container is dropped or a large vibration is applied thereto during transport. The present invention provides a molded body having a plurality of protrusions formed in a distributed manner therein, wherein the plurality of protrusions include a multi-level protrusion, the multi-level protrusion has a multi-level structure, and in the multi-level protrusion, the cross-sectional areas, in plan view of the molded body, of respective upper surfaces of the levels constituting the multi-level structure decrease toward the direction in which the protrusions protrude, and the recovery is 40% or greater, said recovery being calculated on the basis of the amount of displacement of the upper surface of the uppermost level of the multi-level protrusion before and after a compression test in which compression is performed by applying a load to the upper surface of the uppermost level from above.
Need to check novelty before this filing date? Find Prior Art

Description

Molded body

[0001] This technology relates to molded articles, and more specifically, to molded articles having shock-absorbing properties.

[0002] To facilitate the transportation of goods and products, and to prevent damage during transport, cushioning material is placed in the gaps between the goods or products and the container during packaging. Conventionally, cushioning materials used in packaging have included synthetic resin bubble wrap with multiple air-filled hollow sections, air cushions, loose-leaf cushioning material, kraft paper, mirror mat, paper cushion, and stretch film. Synthetic resin bubble wrap can be bulky and difficult to handle when storing or disposing of it due to the hollow sections. In addition, air cushions, loose-leaf cushioning material, kraft paper, mirror mat, paper cushion, and stretch film inevitably generate a lot of material waste, requiring effort in purchasing materials and securing storage space. To reduce material waste, a corrugated cardboard packaging container equipped with a retaining member to hold the goods or products in place inside the container has been proposed (Patent Document 1).

[0003] Utility Model Registration No. 3160273 Publication

[0004] However, the technology described in Patent Document 1 requires the preparation of cushioning material that conforms to the size and shape of the goods or products, and since the retaining member is made of cardboard, it does not adequately absorb shock when the goods or products are subjected to impact from being dropped during transportation, resulting in damage to the goods or products. Furthermore, in recent years, there has been a demand to fix and package a wide variety of products with different shapes and sizes within a container on the same packaging line, but the technology described in Patent Document 1 has the problem that it is difficult to package them on the same packaging line because cushioning material that conforms to the product is required. The present invention aims to provide a molded body that has excellent shock absorption properties for the packaged object, such as goods, when the container is dropped or subjected to large vibrations during transportation.

[0005] The present invention provides a molded body formed by a plurality of scattered protrusions, wherein the plurality of protrusions include multi-stage protrusions, the multi-stage protrusions have a multi-stage structure, the cross-sectional area of ​​the upper surface of each stage constituting the multi-stage structure decreases in a plan view of the molded body in the direction in which the protrusions protrude, and the recovery rate calculated based on the amount of displacement of the upper surface of the uppermost stage before and after a compression test in which a load is applied from above to the uppermost stage of the multi-stage protrusions is 40% or more. Furthermore, the molded body may be formed from a resin composition containing a biomass material and a thermoplastic resin. In a plan view of the molded body, the cross-sectional shape of the upper surface of each stage constituting the multi-stage structure may be circular. In a plan view of the molded body, the cross-sectional shape of the upper surface of each stage constituting the multi-stage structure may be concentric circles. In a plan view of the molded body, the cross-sectional shape of the upper surface of each stage constituting the multi-stage structure may be polygonal. The multi-stage structure may be a three-stage structure. When a load is applied to the upper surface of the uppermost step of the multi-stage protrusion, each step constituting the multi-stage protrusion may be crushed. The average thickness of the molded body may be 0.3 mm to 1.2 mm. In the multi-stage protrusion, recesses may be formed along the outer circumference direction of the upper surface of each step. The recesses may be formed on the upper surfaces of steps other than the upper surface of the uppermost step of the multi-stage protrusion. The cross-sectional shapes of the upper surfaces of each step constituting the multi-stage structure may be the same or different from each other. In a plan view of the molded body, the cross-sectional area of ​​the upper surface of the lowest step of the multi-stage protrusion is larger than the cross-sectional area of ​​the upper surface of the step adjacent to the lowermost step on the side of the uppermost step of the multi-stage protrusion.The present invention also provides a molded body molded to the shape of an object to be packaged, wherein, when the object to be packaged is placed in the molded body from the opening toward the bottom, a plurality of protrusions are formed on the bottom side that comes into contact with the object to be packaged, the plurality of protrusions include multi-stage protrusions, the multi-stage protrusions have a multi-stage structure, the cross-sectional area of ​​the upper surface of each stage constituting the multi-stage structure decreases in a plan view of the molded body in the direction in which the protrusions protrude, and the recovery rate calculated based on the amount of displacement of the upper surface of the uppermost stage before and after a compression test in which a load is applied from above to the upper surface of the uppermost stage of the multi-stage protrusions is 40% or more. The molded body may be formed from a resin composition containing a biomass material and a thermoplastic resin. In a plan view of the molded body, the cross-sectional shape of the upper surface of each stage constituting the multi-stage structure may be circular. In a plan view of the molded body, the cross-sectional shape of the upper surface of each stage constituting the multi-stage structure may be concentric circles. In a plan view of the molded body, the cross-sectional shape of the upper surface of each step constituting the multi-stage structure may be polygonal. The multi-stage structure may be a three-stage structure. When a load is applied to the upper surface of the uppermost step of the multi-stage protrusion, each step constituting the multi-stage protrusion may be crushed. The average thickness of the molded body may be 0.3 mm to 1.2 mm. In the multi-stage protrusion, a recess may be formed along the outer circumference direction of the upper surface of each step. The recess may be formed on the upper surface of steps other than the step containing the uppermost step of the multi-stage protrusion. In a plan view of the molded body, the cross-sectional shapes of the upper surfaces of each step constituting the multi-stage structure may be the same or different from each other. In a plan view of the molded body, the cross-sectional area of ​​the upper surface of the lowest step of the multi-stage protrusion is larger than the cross-sectional area of ​​the upper surface of the step adjacent to the lowermost step on the side of the uppermost step of the multi-stage protrusion. The lowest step of the multi-stage protrusion may be formed in the corner of the bottom of the molded body.

[0006] The present invention provides a molded body that offers excellent shock absorption when a container is dropped or subjected to significant vibration during transportation, for example, when a product is packed inside the container.

[0007] This is a perspective view of a molded body 10 with multiple protrusions 11 scattered thereon according to this embodiment. This is a plan view of a molded body 10 with multiple protrusions 11 scattered thereon according to this embodiment. This is a cross-sectional view taken along line A-A in Figure 2. This is a plan view photograph showing how the protrusions 11 are crushed when the object to be packaged P falls and collides with the protrusions 11 of the molded body. This is an oblique the state of the protrusions 11 after the object P has been removed, after the protrusions 11 have been crushed when the object to be packaged P falls and collides with the protrusions 11 of the molded body. This is a plan view of a molded body 20 with multiple protrusions 21 scattered thereon according to this embodiment. This is an enlarged perspective view of a protrusion 21. This is a cross-sectional view taken along line A-A in Figure 7. This is an enlarged plan view of a multi-stage protrusion in which recesses are formed along the outer circumference direction of the upper surface of each stage. This photograph shows the sample S placed between the movable plate UP and the fixed plate LP of a compression testing machine (Strograph VE20D, manufactured by Toyo Seiki Co., Ltd.) with an initial gap of 40 mm before applying a load. The height H of the uppermost surface of the protrusion before the compression test. b and the height H of the uppermost end surface of the protrusion after the compression test aThis is a diagram showing the following. This is a two-layer sheet composed of layer A and layer B according to this embodiment. This is a three-layer sheet composed of layer A, layer B, and layer A according to this embodiment. This is a three-layer sheet composed of layer A, layer B, and layer C according to this embodiment. This is a plan view of the bottom 30 of a molded body with a plurality of protrusions 31 scattered thereon. This is an enlarged perspective view of the protrusions 31. This is a cross-sectional view taken along line A-A in Figure 16. This is an enlarged plan view of a multi-stage protrusion in which recesses are formed along the outer circumference direction of the upper surface of each stage. This is a cross-sectional view showing the relationship between the packaged object contained from the opening of the molded body toward the bottom, the bottom of the molded body, the protrusions, and the side surface of the molded body. This is a plan view photograph of the sheet molded in Example 1. This is a plan view photograph of a circular two-stage protrusion 41 contained in a cut-out sample. This is a plan view photograph of a rectangular three-stage protrusion 42 contained in a cut-out sample. This is a plan view photograph of a circular three-stage protrusion 43 contained in a cut-out sample. This is a plan view photograph of a circular three-stage protrusion 44 contained in a cut-out sample. This is a photograph of the four-tiered circular protrusion 45 formed at the corner of the bottom of the molded body. This is a cross-sectional view of the four-tiered circular protrusion 45 formed at the corner of the bottom of the molded body. This is a graph showing the relationship between the amount of compressive displacement and the compressive load when the three-tiered circular protrusion contained in the cut-out sample is compressed.

[0008] Preferred embodiments of the present invention will be described below. The embodiments described below represent typical embodiments of the present invention, and the scope of the present invention is not limited to these embodiments.

[0009] The present invention will be described in the following order: 1. First Embodiment (An Example of a Molded Article) (1) Structure of the Molded Article (2) Method of Manufacturing the Molded Article (3) Applications 2. Second Embodiment (Another Example of a Molded Article) (1) Structure of the Molded Article (2) Method of Manufacturing the Molded Article (3) Applications 3. Examples

[0010] 1. First Embodiment (An Example of a Molded Body)

[0011] (1) Structure of the Molded Body The structure of the molded body of this embodiment will be described below with reference to the drawings. In this specification, the "direction perpendicular to the object when it is placed on a horizontal surface with the surface on which the object is placed facing upward" is called the "thickness direction," and the "any direction in a plane perpendicular to the thickness direction" is called the "plane direction." Also, the "view of the object when it is placed on a horizontal surface with the surface on which the object is placed facing upward, from the vertical upper side in the thickness direction" is called a "plan view." Furthermore, the "uppermost step of the multi-stage protrusion" is the "uppermost step of the multi-stage protrusion that protrudes upward from the molded body," and the "lowest step of the multi-stage protrusion" is the "lowest step of the multi-stage protrusion on the opposite side from the uppermost step."

[0012] The molded body of this embodiment is formed by a plurality of scattered protrusions. These protrusions include multi-stage protrusions having a multi-stage structure. In the multi-stage protrusions, the cross-sectional area of ​​the upper surface of each stage constituting the multi-stage structure decreases in a plan view of the molded body in the direction in which the protrusions protrude. Furthermore, the molded body of this embodiment has a recovery rate of 40% or more, calculated based on the amount of displacement of the upper surface of the uppermost stage of the multi-stage protrusion before and after a compression test in which a load is applied from above to the upper surface of the uppermost stage of the multi-stage protrusion.

[0013] Figure 1 is a perspective view of a molded body 10 with a plurality of protrusions 11 scattered thereon according to this embodiment. Figure 2 is a plan view of the molded body 10 with a plurality of protrusions 11 scattered thereon according to this embodiment. Figure 3 is a cross-sectional view taken along line A-A in Figure 2. As shown in Figure 1, the molded body 10 has a plurality of protrusions 11 scattered thereon. As shown in Figure 2, the cross-sectional shape (outer circumference shape) of the first and second stage protrusions in a plan view is circular. As shown in Figure 3, the protrusion 11 is a multi-stage protrusion having a two-stage structure of a first stage 11f and a second stage 11s. In this embodiment, in order to mitigate the impact of a fall when an object falls and collides with the protrusion 11, the protrusion includes a multi-stage protrusion having a multi-stage structure of two or more stages. The multi-stage protrusion may preferably have three or more stages, and more preferably four or more stages. In this embodiment, from the viewpoint of obtaining cushioning properties, the proportion of multi-stage protrusions among the protrusions may preferably be 50% or more, more preferably 70% or more, and even more preferably 80% or more. Alternatively, all protrusions may be multi-stage protrusions. In a multi-stage protrusion, the cross-sectional area of ​​the upper surface of each stage constituting the multi-stage structure decreases in a plan view of the molded body in the direction in which the protrusion protrudes. For example, in the multi-stage protrusion 11 shown in Figure 3, the cross-sectional area of ​​the upper surface of the second stage 11s is smaller than the cross-sectional area of ​​the upper surface of the first stage 11f. In this embodiment, the cross-sectional shape of the multi-stage structure may be stepped or tapered, and in the case of a tapered shape, the cross-sectional area of ​​the upper surface of each stage constituting the multi-stage structure may gradually decrease in a plan view of the molded body. Also, in this embodiment, the cross-sectional shapes of the upper surfaces of each stage constituting the multi-stage structure may be the same or different from each other in a plan view of the molded body. Furthermore, in a plan view of the molded body, the cross-sectional area of ​​the upper surface of the lowest stage of the multi-stage protrusion may be larger than the cross-sectional area of ​​the upper surface of the stage adjacent to the uppermost stage of the multi-stage protrusion in the stage adjacent to the lowest stage.

[0014] When the packaged object falls and collides with such a multi-stage protrusion, the protrusion that collides with the packaged object is crushed, thereby mitigating the impact of the fall on the packaged object. That is, when a load is applied to the upper surface of the uppermost stage of the multi-stage protrusion that constitutes the protrusion, each stage constituting the multi-stage protrusion may be crushed. From the viewpoint of mitigating the impact on the packaged object when it falls, the height H11 of the protrusion 11 may be a ratio (height H11 of the protrusion 11 / height of the object) of preferably 0.2 or more, more preferably 0.33 or more, and even more preferably 1 or more, to the height of the packaged object. Also, the height H11 of the protrusion 11 may be preferably 0.1 cm to 5 cm, more preferably 0.2 cm to 4 cm, and even more preferably 0.3 cm to 3 cm. Furthermore, the height H11 of the protrusion 11 may be, more preferably, 0.5 or more, and even more preferably, 1 or more, in terms of the ratio of the height H11 of the protrusion 11 to the diameter of the cross-sectional shape of the first stage 11f of the protrusion 11 (height H11 of the protrusion 11 / diameter of the cross-sectional shape of the first stage 11f of the protrusion 11).

[0015] Furthermore, when the packaged object falls and collides with the protrusion 11, the protrusion 11 collapses, thereby mitigating the impact on the packaged object. From this viewpoint, the height H11f of the first stage 11f of the protrusion 11 may be a ratio (height H11f / H11) of 0.066 or more, more preferably 0.2 or more, and even more preferably 0.5 or more. Also, the height H11f of the first stage 11f of the protrusion 11 may be a ratio of 0.1 cm to 1.4 cm, more preferably 0.2 cm to 1.3 cm, and even more preferably 0.3 cm to 1.2 cm. Furthermore, the height H11f of the first stage h11f of the protrusion 11 may be preferably 0.066 or more, more preferably 0.133 or more, and even more preferably 0.5 or more, as a ratio (height H11f of the first stage 11f of the protrusion 11 / diameter of the cross-sectional shape of the first stage 11f of the protrusion 11).

[0016] Furthermore, when the packaged object falls and collides with the protrusion 11, the protrusion 11 collapses, thereby mitigating the impact on the packaged object. From this viewpoint, the height H11s of the second stage 11s of the protrusion 11 may be a ratio (height H11s of the second stage 11s of the protrusion 11 / H11) of 0.066 or more, more preferably 0.2 or more, and even more preferably 0.5 or more. Also, the height H11s of the second stage 11s of the protrusion 11 may be a ratio of 0.1 cm to 1.4 cm, more preferably 0.2 cm to 1.3 cm, and even more preferably 0.3 cm to 1.2 cm. Furthermore, the height H11s of the second stage 11s of the protrusion 11 may be, more preferably, 0.133 or more, and even more preferably 0.5 or more, as a ratio (height H11s of the second stage 11s of the protrusion 11 / diameter of the cross-sectional shape of the first stage 11f of the protrusion 11).

[0017] In this embodiment, when the packaged object falls and collides with the protrusion 11, the protrusion 11 maintains a shape in which the entire protrusion 11 is crushed by the packaged object. Alternatively, when the packaged object falls and collides with the protrusion 11, the protrusion 11 maintains a shape in which a portion of the protrusion 11 is crushed by the packaged object. The molded body of this embodiment does not easily return to its original shape after being crushed, and therefore it is possible to mitigate the impact of a fall on the packaged object.

[0018] Figure 4 is a plan view photograph showing how the protrusion 11 of the molded body is crushed when the packaged object P falls and collides with it. Figure 5 is a perspective view photograph showing how the protrusion 11 is crushed when the packaged object P falls and collides with it. Figure 6 is a perspective view photograph showing the state of the protrusion 11 after the object P has been removed, following the crushing of the protrusion 11 when the packaged object P falls and collides with it. In Figures 4, 5, and 6, the protrusion 11A retains the shape in which the entire protrusion 11 is crushed. The protrusion 11B retains the shape in which a part of the protrusion 11 is crushed. The protrusion 11C retains its original, uncrushed shape.

[0019] In this embodiment, the protrusions 11 of the molded body 10 after the packaged object P has fallen may consist only of the completely flattened protrusions 11A, or they may consist of a partially flattened protrusion 11B and the protrusions 11A. Furthermore, the protrusions 11 may include protrusions 11C that maintain their original shape and are not flattened because they have not collided with the packaged object P.

[0020] The molded body of this embodiment may be a molded body 20 in which protrusions 21 having a three-tiered structure are scattered instead of the two-tiered protrusions 11 in the molded body 10 shown in Figure 1. Figure 7 is a plan view of a molded body 20 with a plurality of protrusions 21 scattered according to this embodiment. Figure 8 is an enlarged perspective view of the protrusions 21. Figure 9 is a cross-sectional view taken along line A-A in Figure 7.

[0021] In this embodiment, the cross-sectional shape of the protrusion in plan view is preferably circular. Furthermore, in the case of a multi-stage protrusion having a multi-stage structure, the cross-sectional shape of the upper surface of each stage constituting the multi-stage structure in plan view may be concentric circles. Also, the cross-sectional shape of the protrusion in plan view in this embodiment may be rectangular, such as a square or rectangle, or polygonal, such as a pentagon or hexagon. Note that in a plan view of the molded body, the cross-sectional shapes of the upper surfaces of each stage constituting the multi-stage structure may be the same or different from each other. As shown in Figure 7, the cross-sectional shape (outer circumference) of the protrusions 21 scattered on the molded body 20 in plan view is circular. As shown in Figures 8 and 9, the protrusion 21 is a multi-stage protrusion having a three-stage structure: first stage 21f, second stage 21s, and third stage 21t. In the multi-stage protrusion 21, in a plan view of the molded body, the cross-sectional area of ​​the upper surface of each stage constituting the multi-stage structure gradually decreases in the direction in which the protrusion protrudes. For example, in the multi-stage protrusion 21 shown in Figures 7, 8, and 9, the cross-sectional area of ​​the upper surface of the second stage 21s is smaller than the cross-sectional area of ​​the upper surface of the first stage 21f, and the cross-sectional area of ​​the upper surface of the third stage 21t is smaller than the cross-sectional area of ​​the upper surface of the second stage 21s. When the object to be packaged is dropped and collides with such a multi-stage protrusion, the protrusion of the stage that comes into contact with the object to be packaged is prone to being crushed. From the viewpoint of mitigating the impact of the fall when the object to be packaged is dropped, the height H21 of the protrusion 21 may be preferably 0.2 or more, more preferably 0.33 or more, and even more preferably 0.5 or more, as a ratio to the height of the object to be packaged (height H21 of the protrusion 21 / height of the object). Also, the height H21 of the protrusion 21 may be preferably 0.1 cm to 5 cm, more preferably 0.2 cm to 0.4 cm, and even more preferably 0.3 cm to 3 cm. Furthermore, the height H21 of the protrusion 21 may be, more preferably, 0.5 or more, and even more preferably 1 or more, in terms of the ratio of the height H21 of the protrusion 21 to the diameter of the cross-sectional shape of the protrusion 21 (height H21 of the protrusion 21 / diameter of the cross-sectional shape of the protrusion 21). In addition, in a plan view of the molded body, the cross-sectional area of ​​the upper surface of the lowest stage of the multi-stage protrusion may be larger than the cross-sectional area of ​​the upper surface of the stage adjacent to the uppermost stage of the multi-stage protrusion of the stage adjacent to the lowest stage.

[0022] Furthermore, the height H21f of the first stage 21f of the protrusion 21 is preferably 0.1 cm to 1.4 cm, more preferably 0.2 cm to 1.3 cm, and even more preferably 0.3 cm to 1.2 cm. Also, the ratio of the height H21f of the first stage 21f of the protrusion 21 to the diameter of the cross-sectional shape of the first stage 21f of the protrusion 21 (height H21f of the first stage of the protrusion 21 / diameter of the cross-sectional shape of the first stage 21f of the protrusion 21) is preferably 0.066 or more, more preferably 0.2 or more, and even more preferably 0.33 or more.

[0023] Furthermore, from the viewpoint of making the protrusion 21 more easily crushed when the packaged object falls and collides with the protrusion 21, the height H21s of the second stage 21s of the protrusion 21 may be a ratio of (height H21s of the second stage 21s of the protrusion 21 / H21) of 0.066 or more, more preferably 0.2 or more, and even more preferably 0.33 or more. Also, the height H21s of the second stage 21s of the protrusion 21 may be a ratio of 0.1 cm to 1.4 cm, more preferably 0.2 cm to 1.3 cm, and even more preferably 0.3 cm to 1.2 cm. Furthermore, the height H21s of the second stage 21s of the protrusion 21 may be, more preferably, 0.2 or more, and even more preferably, 0.33 or more, as a ratio (height H21s of the second stage of the protrusion 21 / diameter of the cross-sectional shape of the first stage 21f of the protrusion 21).

[0024] Furthermore, from the viewpoint of making the protrusion 21 more easily crushed when the packaged object falls and collides with the protrusion 21, the height H21t of the third stage 21t of the protrusion 21 may be a ratio of (height H21t of the third stage 21t of the protrusion 21 / H21) of 0.066 or more, more preferably 0.2 or more, and even more preferably 0.33 or more. Also, the height H21t of the third stage 21t of the protrusion 21 may be a ratio of 0.1 cm to 1.4 cm, more preferably 0.2 cm to 1.3 cm, and even more preferably 0.3 cm to 1.2 cm. Furthermore, the height H21t of the third stage 21t of the protrusion 21 may be preferably 0.066 or more, more preferably 0.2 or more, and even more preferably 0.33 or more, as a ratio to the diameter of the cross-sectional shape of the first stage 21f of the protrusion 21 (height H21t of the third stage 21t of the protrusion 21 / diameter of the cross-sectional shape of the first stage 21f of the protrusion 21).

[0025] In the multi-stage protrusion of the molded body of this embodiment, recesses may be formed along the outer circumference direction of the upper surface of each stage. Figure 10 is an enlarged plan view of a multi-stage protrusion in which recesses are formed along the outer circumference direction of the upper surface of each stage. As shown in Figure 10, a recess 22f is formed along the outer circumference direction of the upper surface of the first stage 21f of the multi-stage protrusion 21, and a recess 22s is formed along the outer circumference direction of the upper surface of the second stage 21s. The recesses may be formed continuously along the outer circumference, as shown in Figure 10, or they may be formed intermittently, resulting in a number of holes in the outer circumference direction.

[0026] By forming recesses along the outer circumference of the upper surface of each tier, when the packaged object falls and collides with the protrusion 21, the tiers with recesses are more likely to collapse, thus reducing the impact of the fall. For example, as shown in Figure 10, if a recess 22f is formed along the outer circumference of the upper surface of the first tier 21f of the multi-tier protrusion 21, and a recess 22s is formed along the outer circumference of the upper surface of the second tier 21s, when the packaged object collides with the uppermost tier of the third tier 21t of the multi-tier protrusion 21, the second tier 21s and the first tier 21f will collapse, making it easier to absorb the impact of the fall. Note that recesses may also be formed on the upper surfaces of tiers other than those including the uppermost tier of the multi-tier protrusion.

[0027] In this embodiment, when a load is applied from above to the upper surface of the uppermost of the multi-stage protrusions, the minimum load at which the multi-stage protrusions collapse is preferably 1000 N or less, more preferably 800 N or less, even more preferably 600 N or less, and even more preferably 400 N or less. If the minimum load at which the multi-stage protrusions collapse exceeds 1000 N, the impact of a fall cannot be mitigated, resulting in poor cushioning performance.

[0028] The molded body of this embodiment has a recovery rate of 40% or more, preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more, calculated based on the displacement of the uppermost surface of the multi-stage protrusion before and after a compression test in which a load is applied from above to the uppermost surface of the multi-stage protrusion. If the recovery rate is less than 40%, it will not be able to mitigate the impact of a fall. The method for measuring the recovery rate will be described below.

[0029] (Measurement of recovery rate)

[0030] The recovery rate is calculated by cutting out a multi-stage protrusion from the molded body, performing a compression test on the multi-stage protrusion under predetermined conditions, and determining the displacement of the uppermost surface of the multi-stage protrusion before and after compression.

[0031] The recovery rate of the molded product is measured using the following procedure.

[0032] (i) First, a 35 mm x 35 mm sample S is cut out so that it includes one multi-stage protrusion of the molded body. (ii) Figure 11 is a photograph showing the sample S placed between the movable plate UP and the fixed plate LP of the compression testing machine (Strograph VE20D, manufactured by Toyo Seiki Co., Ltd.) with an initial distance of 40 mm between the movable plate UP and the fixed plate LP before applying load. The movable plate UP is held in a position that allows it to move forward and backward by an electric motor (not shown).

[0033] (iii) Control the electric motor, operate the movable plate UP relative to the fixed plate LP and the sample S, continuously subject the sample S to pressure treatment under the following conditions, and completely crush the multi-stage convex portions of the molded body. Move the movable plate UP upward to finish the pressure treatment, and let the sample S stand still on the fixed plate LP for 10 minutes. Moving speed of movable plate UP: 20 mm / min Load limit: 100 N to 1000 N (adjust as appropriate according to the composition of the molded body) Number of tests: N=3

[0034] FIG. 12 shows the height H of the top surface of the uppermost stage of the multi-stage convex portions before the compression test b and the height H of the top surface of the uppermost stage of the convex portions after the compression test a . After the compression test is completed, the restoration rate is calculated from the following formula using the height H of the top surface of the uppermost stage of the multi-stage convex portions before the compression test shown in FIG. 12 b and the height H of the top surface of the uppermost stage of the multi-stage convex portions before the compression test a . Restoration rate (%) = (H a / H b ) × 100

[0035] From the viewpoint of mitigating drop impact, when the molded body of the present embodiment is compressed by applying a load from above to the top surface of the uppermost stage of the multi-stage convex portions, the load at a compression displacement of 8 mm may be preferably 60 N or less, more preferably 50 N or less, and still more preferably 40 N or less. FIG. 28 is a graph showing the relationship between the compression displacement and the compression load when a circular three-stage convex portion is compressed. The measurement of the compression displacement and the compression load is the same as the sample, apparatus, and method used in the above-described measurement of the restoration rate of the molded body, and thus the description thereof is omitted.

[0036] Next, the molded body of the present embodiment will be described. The molded body of the present embodiment may be a film or a sheet. When the molded body of the present embodiment is a film, the average thickness may be preferably 10 μm to 100 μm, more preferably 20 μm to 80 μm, and still more preferably 30 μm to 70 μm. When the molded body of the present embodiment is a sheet, the average thickness may be preferably 0.1 mm to 2 mm, 0.3 mm to 1.2 mm, more preferably 0.5 mm to 1.5 mm, and still more preferably 0.7 mm to 1.3 mm.

[0037] Further, when the molded article of the present embodiment is a sheet, it may be a single-layer sheet with one layer, or may be a multilayer sheet in which a plurality of layers such as two layers or three layers are laminated. Hereinafter, the single-layer sheet will be described first, and then the multilayer sheet will be described.

[0038] [Single-Layer Sheet]

[0039] The single-layer sheet according to the present embodiment may be formed from a resin composition. The resin composition may preferably contain a biomass material and a thermoplastic resin. In the present embodiment, by including the biomass material, it is possible to obtain cushioning properties that mitigate drop impact when a packaged object falls.

[0040] The biomass material is preferably a plant-derived biomass material, and more specific examples thereof include starch materials and cellulose materials. The starch material and the cellulose material may be classified as waste-based biomass, unused biomass, or resource grains. In addition, the biomass material may be of animal origin, and examples thereof include biologically derived calcium carbonate such as eggshells and scallop shells.

[0041] As the starch material, raw starch can be used, and examples thereof include underground starch and above-ground starch. The underground starch is starch accumulated underground, for example, starch accumulated in rhizomes or roots. Examples of the underground starch include, but are not limited to, tapioca starch (cassava starch), potato starch, sweet potato starch, kudzu starch, and bracken starch.

[0042] The above-ground starch is starch accumulated above ground, for example, starch accumulated in seeds and the like. Examples of the above-ground starch include, but are not limited to, corn starch, wheat starch, sago starch, acorn starch, and rice starch.

[0043] In the single-layer sheet according to the present embodiment, above-ground starch is preferably used.

[0044] The starch material may be a modified starch (i.e., modified starch), particularly a modified ground-based starch. Examples of such modified starches include chemically modified starches. Examples of chemically modified starches include acetoacetate esterified starch, acetate esterified starch, hydroxymethyl etherified starch, hydroxypropyl etherified starch, carboxymethyl etherified starch, allyl etherified starch, methyl etherified starch, succinate esterified starch, xanthogene acetate esterified starch, nitrate esterified starch, urea phosphate esterified starch, phosphate esterified starch, phosphate cross-linked starch, formaldehyde cross-linked starch, acrolein cross-linked starch, epichlorohydrin cross-linked starch, and the like.

[0045] When the starch material is corn starch, its particle size is preferably 5 μm or larger, more preferably 10 μm or larger, and even more preferably 15 μm or larger. The upper limit of the particle size is not particularly limited, but is preferably 50 μm or smaller, more preferably 40 μm or smaller, and even more preferably 30 μm or smaller.

[0046] Furthermore, when the starch material is tapioca starch, its particle size is preferably 2 μm or larger, more preferably 10 μm or larger, and even more preferably 15 μm or larger. The upper limit of the particle size is not particularly limited, but is preferably 40 μm or smaller, more preferably 30 μm or smaller, and even more preferably 25 μm or smaller.

[0047] When the starch material is potato starch, its particle size is preferably 2 μm or larger, more preferably 20 μm or larger, and even more preferably 30 μm or larger. The upper limit of the particle size is not particularly limited, but is preferably 80 μm or smaller, more preferably 60 μm or smaller, and even more preferably 40 μm or smaller.

[0048] Furthermore, the starch material may preferably contain equilibrium moisture. The amount of equilibrium moisture may be, for example, preferably 10% to 15% by mass, more preferably 10% to 14% by mass, even more preferably 10% to 13% by mass, and even more preferably 11% to 13% by mass, relative to the mass of the starch material. When compounded with a thermoplastic resin, the moisture content of the starch may preferably be 3% or less.

[0049] Examples of cellulose materials used in this embodiment include paper, paper pulp, cotton, or crushed cloth.

[0050] The particle size D50 (median diameter) of the cellulose material is, for example, 15 μm to 150 μm, and particularly preferably 20 μm to 100 μm. The particle size D50 is determined by wet measurement using a laser diffraction particle size distribution analyzer (SALD-3100, Shimadzu Corporation). By having a particle size within the above numerical range, the cellulose material can contribute to improving the dispersibility of the cellulose material contained in the thermoplastic resin.

[0051] Of the cellulose fibers constituting the cellulose material, the number of cellulose fibers having a particle size of 9.8 μm to 110.6 μm accounts for 65% to 100%, preferably 70% to 100%, more preferably 80% to 100%, and even more preferably 85% to 100% of the total number of cellulose fibers constituting the cellulose material. The above proportions regarding the number of cellulose fibers are determined by wet measurement using the laser diffraction particle size distribution analyzer to determine the proportion of cellulose fibers having a particle size of 0 μm to 9.8 μm (hereinafter referred to as the "first proportion") and the proportion of cellulose fibers having a particle size of 0 μm to 110.6 μm (hereinafter referred to as the "second proportion") out of the total number of cellulose fibers in the cellulose material, and then subtracting the first proportion from the second proportion. The numerical ranges "0 μm to 9.8 μm" and "0 μm to 110.6 μm" are both numerical ranges input to the laser diffraction particle size distribution analyzer during the wet measurement.

[0052] In this embodiment, particularly preferably, the number of cellulose fibers having a particle size of 110.6 μm to 998.4 μm among the cellulose fibers constituting the cellulose material accounts for 0% to 30%, preferably 0% to 25%, more preferably 0% to 20%, and even more preferably 0% to 15% of the total number of cellulose fibers constituting the cellulose material. The above proportions regarding the number of cellulose fibers are determined by wet measurement using the laser diffraction particle size distribution analyzer to determine the proportion of cellulose fibers having a particle size of 0 μm to 110.6 μm (the "second proportion" above) and the proportion of cellulose fibers having a particle size of 0 μm to 998.4 μm (hereinafter referred to as the "third proportion") among the total number of cellulose fibers in the cellulose material, and then subtracting the second proportion from the third proportion. The numerical ranges "0 μm to 110.6 μm" and "0 μm to 998.4 μm" are both numerical ranges input to the laser diffraction particle size distribution analyzer in the wet measurement.

[0053] A cellulose material having the above particle size distribution can be produced, for example, by treating pulp with a chemical such as an acid. An example of a cellulose material having the above particle size distribution is KC Floc W400 (Nippon Paper Industries Co., Ltd.). Using cellulose powder having the above particle size distribution provides better moldability when manufacturing sheets.

[0054] In particular, if the number of cellulose fibers having a particle size of 9.8 μm to 110.6 μm among the cellulose fibers constituting the cellulose powder accounts for 80% to 100%, and more preferably 85% to 100%, of the total number of cellulose fibers constituting the cellulose powder, it is possible to prevent tearing or the occurrence of holes in the sheet obtained by molding the thermoplastic resin. In order to prevent tearing or the occurrence of holes in the sheet, it is particularly preferable that the number of cellulose fibers having a particle size of 110.6 μm to 998.4 μm among the cellulose fibers constituting the cellulose powder accounts for 0% to 20%, and more preferably 0% to 15%, of the total number of cellulose fibers constituting the cellulose powder.

[0055] In another embodiment, the cellulose powder may have a particle size such that 90% or more of the particles pass through a 100-mesh grid. In this embodiment, more preferably, the cellulose powder has a particle size such that 90% or more of the particles pass through a 100-mesh grid, and the apparent specific gravity of the cellulose powder may be 0.30 g / ml to 0.40 g / ml.

[0056] The particle size is measured by the standard sieving method, specifically as follows: 10 g of the sample is placed in a 100-mesh standard sieve, a receiving tray and lid are set on the sieve, and the sample is shaken for 40 minutes using a rotary shaker. The particle size is then calculated from the sample mass (10 g) and the mass of the sieved residue using the following formula: Particle size (%) = [(Sample mass (g) - Sieved residue (g)) / Sample mass (g)] × 100

[0057] The apparent specific gravity is measured as follows: 10 g of the sample is accurately weighed on a balance and placed in a 50 ml graduated cylinder. The bottom of the graduated cylinder is tapped on a rubber-covered surface, taking care not to spill the sample. This tapping process is continued until no more sample can clog the cylinder. After tapping, the surface of the sample is flattened, and the scale (volume, ml) is read. The apparent specific gravity is then calculated using the following formula: Apparent specific gravity (g / ml) = Sample (10 g) / Volume (ml)

[0058] Cellulose powder having the above particle size (or the above particle size and apparent specific gravity) can be produced, for example, by mechanically grinding pulp (e.g., by jet mill grinding). An example of cellulose powder having the above particle size (or the above particle size and apparent specific gravity) is KC Floc 100GK.

[0059] In this embodiment, from the viewpoint of obtaining cushioning properties against the impact of dropping the packaged object from the multiple protrusions scattered on the formed sheet, the biomass material content is preferably 4% to 95% by mass, more preferably 6% to 93% by mass, and even more preferably 8% to 90% by mass, relative to the mass of the resin composition.

[0060] The thermoplastic resin used in the single-layer sheet according to this embodiment may be a polyolefin resin, a polyester resin, or a mixture of these resins. Alternatively, the thermoplastic resin may be a polystyrene resin. Furthermore, the thermoplastic resin may contain biodegradable materials to avoid reducing its biodegradability.

[0061] Polyolefin resins are polymers obtained by polymerization using olefins (e.g., α-olefins) as the main monomers. Polyolefin resins may be, for example, polyethylene (PE) resins or polypropylene (PP) resins, or combinations thereof. Furthermore, polyolefin resins may be homopolymers, block copolymers, or random copolymers.

[0062] The polyethylene resin may be, for example, low-density polyethylene resin (LDPE), high-density polyethylene resin (HDPE), very low-density polyethylene resin (VLDPE), linear low-density polyethylene resin (LLDPE), ethylene copolymers such as ethylene-vinyl acetate copolymer (EVA resin), or ultra-high molecular weight polyethylene resin (UHMW-PE), or a combination thereof.

[0063] The polyolefin resin may preferably be a biomass-derived polyolefin resin (for example, a biomass-derived polyethylene resin), and may be, for example, a biomass polyethylene resin. The biomass polyethylene resin may be, for example, LDPE, LLDPE, or HDPE. This can reduce CO2 emissions.

[0064] The polyolefin resin may be a polyolefin resin produced using a metallocene catalyst. That is, the thermoplastic resin may be, for example, a metallocene catalyst-based polyethylene resin or polypropylene resin, or a combination thereof. The polystyrene resin may be a metallocene catalyst-based polystyrene resin.

[0065] Polyester resins are polymers formed by the polymerization of monomers via ester bonds. Examples of polyester resins include polyethylene terephthalate resin (PET), polyethylene naphthalate resin (PEN), polybutylene terephthalate resin (PBT), polylactic acid resin (PLA), or polycarbonate resin (PC), polybutylene adipate terephthalate resin (PBAT), polybutylene succinate resin (PBS), polyhydroxyalkanoate resin (PHA), or combinations of two or more of these.

[0066] Polystyrene resins are polymers formed by the polymerization of styrene monomers. Polystyrene resins may include, for example, polystyrene resin, rubber-reinforced polystyrene resin (high-impact polystyrene resin, HIPS), acrylonitrile-styrene copolymer (AS resin), methacrylic acid ester-styrene copolymer, acrylonitrile-acrylic rubber-styrene copolymer, and acrylonitrile-ethylene propylene-styrene copolymer, or combinations of two or more of these.

[0067] In this embodiment, the type of thermoplastic resin may be appropriately selected by those skilled in the art, for example, depending on the packaging application, and a thermoplastic resin with a low processing temperature is preferred. For example, in the case of a sheet used for food packaging, the thermoplastic resin may be, for example, preferably a polyolefin resin, more preferably a polyethylene resin or a polypropylene resin, and even more preferably a polypropylene resin.

[0068] In this embodiment, the melting point of the thermoplastic resin is preferably 170°C or lower, and more preferably 165°C or lower. By using a thermoplastic resin with a lower melting point, the temperature during sheet molding can be reduced. Furthermore, the melting point of the thermoplastic resin is preferably 90°C or higher, and more preferably 95°C or higher.

[0069] As the thermoplastic resin, pelletized granular material may be used. The content of the thermoplastic resin is preferably 3% to 95% by mass, more preferably 5% to 93% by mass, and even more preferably 8% to 90% by mass, based on the mass of the resin composition.

[0070] Examples of the biodegradable materials include cellulose derivatives such as methylcellulose, hydroxymethylcellulose, hydroxyethylcellulose, hydroxypropylmethylcellulose, hydroxyethylmethylcellulose, and hydroxybutylmethylcellulose; hydrophilic polymer materials such as polyvinyl alcohol, carboxymethylcellulose, polyacrylic acid polymers, and polyacrylamide; emulsions such as various acrylates, ethylene / vinyl acetate copolymers, and polyurethanes; and aliphatic polyester resins such as caprolactone, polylactic acid, polybutylene adipate, polybutylene succinate, and polyhydroxybutyrate / variate copolymers.

[0071] The single-layer sheet according to this embodiment may further contain additives in addition to the biomass material and the thermoplastic resin. As such additives, low-melting-point additives that have a melting point lower than the melting temperature of the thermoplastic resin and melt at a relatively low temperature may be used. Preferably, such low-melting-point additives melt at 100°C or below, and more preferably melt at 60 to 100°C. As such low-melting-point additives, ester compounds that are liquid or solid at room temperature are preferably used. Specifically, examples of low-melting-point additives include monoglycerides, diglycerides, triglycerides, acetylated monoglycerides, organic acid monoglycerides, medium-chain fatty acid monoglycerides, polyglycerin fatty acid esters, sorbitan fatty acid esters, propylene glycol fatty acid esters, special fatty acid esters, and higher alcohol fatty acid esters. Preferably, glycerin-based fatty acid esters are used. Low-melting-point additives melt at a relatively low temperature, have viscosity, and can function to entangle and adhere to the biomass material powder.

[0072] The low-melting-point additive may be blended in a proportion of, for example, preferably 0.1 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, per 100 parts by mass of biomass material.

[0073] Furthermore, the low-melting-point additive may be included in the resin composition in a content ratio of, for example, preferably 0.1% to 5% by mass, and more preferably 0.1% to 3% by mass, relative to the mass of the resin composition.

[0074] Furthermore, the resin composition may contain a high-melting-point additive having a higher melting point than the low-melting-point additive. Such a high-melting-point additive may have a higher melting point than the low-melting-point additive, preferably in the range of 100 to 150°C, solidify before the low-melting-point additive, and have a melting point lower than the melting temperature of the thermoplastic resin. Examples of such high-melting-point additives include fatty acid metal salts, hydrocarbons, higher alcohols, aliphatic amides, and fatty acid esters. Specifically, magnesium stearate, zinc stearate, calcium stearate, aluminum stearate, sodium lauryl sulfate, magnesium lauryl sulfate, potassium benzoate, sodium benzoate, and sodium stearyl fumarate are used.

[0075] The high-melting-point additive may be included in the resin composition in a content ratio of, for example, preferably 0.1% to 10% by mass, more preferably 0.1% to 5% by mass, relative to the mass of the resin composition.

[0076] Other additives that can be used include compatibilizers to improve the affinity between biomass materials and thermoplastic resins. The compatibilizer may be selected depending on the type of thermoplastic resin. Examples of such compatibilizers include acid-modified polyolefins, acid-modified nylons, acid-modified polystyrenes, acid-modified EVA, acid-modified ethylene copolymers, acid-modified acrylates, acrylic acid-modified EVA, and modified ethylene acrylates.

[0077] When the thermoplastic resin is a polyolefin-based resin, the compatibilizer is preferably an acid-modified polyolefin, and in particular may be a carboxylic acid anhydride-modified polyolefin or an olefin-based comonomer.

[0078] The carboxylic anhydride constituting the carboxylic anhydride-modified polyolefin can preferably be maleic anhydride. The compatibilizer is, for example, a maleic anhydride-grafted polyolefin resin, and more particularly may be one or a combination of two or more selected from the group consisting of maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, and maleic anhydride-modified ethylene-propylene copolymer. A rubber component may be dispersed in the compatibilizer.

[0079] The compatibilizer may be contained in the resin composition at a content ratio of, for example, 0.1 mass% to 10 mass%, more preferably 1.0 mass% to 5.0 mass%, relative to the mass of the resin composition.

[0080] A colorant can be used as another additive.

[0081] The colorant can be used to color the resin composition. Examples of the colorant include titanium oxide, carbon black, dyes, and pigments.

[0082] An inorganic filler can be used as another additive. Examples of the inorganic filler include inorganic powder. As the inorganic powder, for example, shell powder, mineral powder and the like are preferably used. The specific gravity of the inorganic powder used is preferably 2.5 g / cm 3 or more, more preferably 2.55 g / cm 3 or more, further preferably 2.6 g / cm 3 or more, still further preferably 2.65 g / cm 3 or more.

[0083] Shell powder refers to a powder made by crushing shells. The shells used are not particularly limited, and can include shells of scallops, oysters, surf clams, abalone, mussels, clams, and cockles. Shell powder may be obtained, for example, by washing and sterilizing shells discarded from food factories and then crushing them, or it may be obtained from shells of shellfish not used for food purposes. The method of crushing the shells is not particularly limited, and any known crushing method may be appropriately selected and adopted, and it may be either wet or dry. Alternatively, the shells may be pre-crushed in a coarse crusher and then powdered in a pulverizer. Specifically, coarse crushers include jaw crushers, cone crushers, cutter mills, and hammer crushers, and pulverizers include roll mills, stamp mills, hammer mills, ball mills, vibrating ball mills, roller mills, and vertical mills. Preferably, the shell powder is scallop shell powder. Examples of scallop shell powder include uncalcined scallop shell powder and calcined scallop shell powder. Uncalcined scallop shell powder is made by grinding natural scallop shells into a powder and keeping them in an uncalcined state. Its main component (approximately 96%) is usually calcium carbonate. Uncalcined scallop shell powder is available commercially.

[0084] Examples of mineral powders include clay mineral powder. Such clay mineral powders can be either natural or synthetic. Examples of clay mineral powders include calcium carbonate, magnesium carbonate, zinc oxide, titanium oxide, silica, alumina, clay, talc, kaolin, aluminum hydroxide, magnesium hydroxide, aluminum silicate, magnesium silicate, calcium silicate, aluminum sulfate, magnesium sulfate, calcium sulfate, magnesium phosphate, barium sulfate, silica sand, carbon black, zeolite, molybdenum, diatomaceous earth, sericite, shirasu, calcium sulfite, sodium sulfate, potassium titanate, bentonite, wollastonite, dolomite, and graphite. Among these, talc powder is particularly preferred. As for inorganic powders, only seashell powder may be used, only mineral powder may be used, or a mixture of seashell powder and mineral powder may be used.

[0085] Furthermore, other components such as antioxidants, crosslinking agents, UV absorbers, foaming agents, and impact absorbing agents may be used. Commercially available additives may be used for these purposes.

[0086] [Multilayer sheet]

[0087] Next, a multilayer sheet according to this embodiment will be described with reference to the drawings. Figure 13 shows a two-layer sheet composed of layer A and layer B according to this embodiment. As shown in Figure 13, in a two-layer multilayer sheet, layer A is formed from a resin composition containing a polyolefin resin. The polyolefin resin has been described in the single-layer sheet above, so its explanation will be omitted. In layer A, the polyolefin resin contained in the resin composition may be preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and may be 100% by mass, based on the mass of the resin composition. Layer B is formed from a resin composition containing a biomass material and a thermoplastic resin, etc., as described in the single-layer sheet above. The resin composition has also been described above, so its explanation will be omitted. In a two-layer multilayer sheet, either layer A or layer B may be on the convex surface side.

[0088] Furthermore, the multilayer sheet according to this embodiment may be a three-layer sheet. Figure 14 shows a three-layer sheet according to this embodiment, consisting of layer A, layer B, and layer A. As shown in Figure 14, it has a structure in which layer B is used as an intermediate layer, and layer A is laminated on both sides of the intermediate layer as an outer layer. Figure 15 shows a three-layer sheet according to this embodiment, consisting of layer A, layer B, and layer C. As shown in Figure 15, it has a structure in which layer B is used as an intermediate layer, and layer A and layer C are laminated on both sides of the intermediate layer as outer layers. Layers A and B are as described in the single-layer sheet above, so their description is omitted. Layer C is a compound layer formed from a polyolefin resin. In the three-layer multilayer sheet, either layer A or layer C may be on the convex surface side.

[0089] (2) Method for manufacturing a molded article

[0090] [Method for manufacturing a single-layer sheet]

[0091] A method for manufacturing a molded article of this embodiment will now be described. When the molded article is a single-layer sheet, the method for manufacturing a single-layer sheet may include: a biomass material drying step in which biomass material is placed in a container equipped with a heating element on the outside, and the biomass material is dried while the inside of the container is heated by the heating element, thereby preventing the biomass material from adhering to the inner surface of the container; a resin composition preparation step in which the biomass material dried in the biomass material drying step is mixed with a thermoplastic resin to prepare a resin composition; and a molding step in which the resin composition prepared in the resin composition preparation step is molded to obtain a sheet with scattered protrusions.

[0092] The method for manufacturing a single-layer sheet according to this embodiment may include a biomass material drying step (S1), a resin composition preparation step (S2), and a molding step (S3). Each step will be described below.

[0093] <Biomass material drying process (S1)>

[0094] In the biomass material drying process (S1), the biomass material is placed inside a container. The container in which the biomass material is placed is equipped with an external heating element that heats the inside of the container. Examples of such containers include a heating agitator having a heating jacket around a cylindrical container made of stainless steel or steel. In such a heating agitator, the outer circumference of the containment section in which the biomass material is placed is covered with a heating jacket. Agitation blades are provided inside the containment section. The heating jacket is filled with a heat transfer medium such as oil, hot water, or heated steam, and the heating jacket can function as a heating element. The heating jacket heats the containment section inside the container by heating the inner surfaces such as the inner walls, lid, and bottom surfaces of the container. The heating jacket heats the inner surfaces inside the container so that there are no areas that are not sufficiently heated. By ensuring that there are no areas that are not sufficiently heated inside the container, condensation of moisture in the biomass material evaporated by heating is suppressed from coming into contact with areas that are not sufficiently heated. By suppressing condensation on the inner surface of the heating agitator, the biomass material contained in the container, which prevents starch and other biomass materials from gelatinizing and adhering to the inner surface of the heating agitator, is dried within the heated container. Furthermore, during the drying of the biomass material, gelatinization of starch and other biomass materials can be prevented and drying efficiency can be improved by continuously moving the biomass material using stirring blades. The shape of the stirring blades 12 can be selected from any shape such as propeller blades, paddle blades, inclined paddle blades, turbine blades, screw blades, anchor blades, ribbon blades, and large grid blades. Such a heating agitator is also called an external heating jacket type mixer.

[0095] In this process, from the viewpoint of efficiently drying the biomass material, the temperature inside the container is preferably 120°C or higher, more preferably 135°C or higher, and even more preferably 150°C or higher. Furthermore, from the viewpoint of suppressing thermal degradation of the biomass material, the temperature inside the container is preferably 200°C or lower, more preferably 190°C or lower, and even more preferably 180°C or lower.

[0096] For stirring, the rotation speed of the stirring blades may be set to preferably 500 to 2000 rpm, more preferably 750 to 1750 rpm, and even more preferably 1000 to 1500 rpm.

[0097] In this process, the drying time for the biomass material is not limited, but can be set appropriately depending on the amount of biomass material from the viewpoint of drying efficiency. For example, it may be preferably 10 to 30 minutes, more preferably 15 to 30 minutes, and even more preferably 15 to 25 minutes.

[0098] In this process, the biomass material is prevented from adhering to the inner surface of the container where it is contained. When the biomass material is heated inside the container, the water contained in the biomass material evaporates. The evaporated water comes into contact with areas on the inner surface of the container, such as the inner wall surface, the inner surface of the lid, and the bottom surface, where the temperature rise due to heating is insufficient, causing condensation. When the biomass material contained inside the container adheres to the inner surface of the container where condensation has occurred, the biomass material is heated in the presence of water. For example, if the biomass material is starch, water enters the molecular chain of the starch under heating, causing the molecular structure to loosen and swell (alpha-gelatinization), resulting in granular material known as "white grains." In the infrared absorption spectrum, "white grains" have an absorption peak derived from starch. Such an absorption peak is a peak derived from OH bonds, and the peak is located in the range of 3000 to 3500 cm⁻¹. Also, "white grains" do not color when stained with iodine. Typically, starch particles have a major axis of 10-20 μm, while granular material referred to as "white grains" has a major axis of 100-200 μm, which is larger than ungelatinized starch particles. Unungelatinized starch refers to starch that has not gelatinized before heating or even after heat drying treatment. Such "white grains" can cause mesh clogging and inclusion of white grains in the sheet during sheet or film extrusion molding, leading to brown discoloration, and can also cause holes in the resulting molded product during molding. In this process, the inside of the container is heated by an externally provided heating element, ensuring that there are no areas on the inner surface of the container where the temperature rise is insufficient. This suppresses condensation and prevents the biomass material inside the container from adhering to the inner surface. By preventing the biomass material from adhering to the inner surface of the container in this way, the generation of white grains can be suppressed, making it possible to efficiently manufacture molded products with superior quality. Furthermore, stirring the biomass material inside the container to prevent it from accumulating in one place is also preferable to suppress the biomass material from adhering to the inner surface of the container.

[0099] The above describes the use of an externally heated jacketed mixer, but in the biomass material drying process (S1) in this embodiment, a heated jacketed vacuum dryer may also be used. This dryer preferably has an external heating jacket and stirring blades inside the container, and the biomass material can be dried by creating a vacuum inside the container.

[0100] When using a heated jacket type vacuum dryer, from the viewpoint of efficiently drying the biomass material, the temperature inside the container is preferably 100°C or higher, more preferably 115°C or higher, and even more preferably 130°C or higher. Furthermore, from the viewpoint of suppressing thermal degradation of the biomass material, the temperature inside the container is preferably 200°C or lower, more preferably 185°C or lower, and even more preferably 170°C or lower.

[0101] The vacuum level inside the container is preferably set to 5 kPa to 30 kPa, more preferably to 5 kPa to 25 kPa, and even more preferably to 5 kPa to 20 kPa.

[0102] In this process, the drying time for the biomass material is not limited, but can be appropriately set depending on the amount of biomass material from the viewpoint of drying efficiency. For example, it is preferably 30 to 90 minutes, more preferably 40 to 80 minutes, and even more preferably 50 to 70 minutes. In this process, the biomass material may be dried to a moisture content of preferably 5% or less, more preferably 2% or less.

[0103] <Resin composition preparation step (S2)>

[0104] In the resin composition preparation step (S2), the biomass material dried in the drying step (S1) and the thermoplastic resin are mixed in an extruder to prepare the resin composition. In this step, when mixing the dried biomass material and the thermoplastic resin, for example, the dried biomass material and the thermoplastic resin may be simply mixed in a dry state to prepare a resin composition which is a mixture of powdered biomass material and pelletized thermoplastic resin. Alternatively, the dried biomass material and thermoplastic resin may be simultaneously fed into the extruder via a feeder, and the biomass material and thermoplastic resin may be uniformly kneaded and mixed by heating and kneading while controlling the rotation speed, stirring time, and temperature, thereby forming a resin composition from the molten and kneaded mixture of biomass material and thermoplastic resin present in the extruder. Furthermore, the molten and kneaded mixture of biomass material and thermoplastic resin may be extruded from the extruder, cooled, and pelletized to form the resin composition. A single-screw extruder or a twin-screw extruder can be used as such an extruder. Furthermore, when feeding biomass material and thermoplastic resin into the extruder, additives may be added at the same time. Examples of such additives include low-melting-point additives and high-melting-point additives. Alternatively, the biomass material, thermoplastic resin, and additives may each be fed individually via a feeder in predetermined proportions.

[0105] When mixing the biomass material and the thermoplastic resin in an extruder, the heating temperature (cylinder temperature) may be set to a temperature below the melting point of the thermoplastic resin, or above the melting point of the high-melting-point additive, from the viewpoint of suppressing material deterioration and discoloration. For example, the heating temperature (cylinder temperature) may be set to 100 to 190°C.

[0106] <Molding process (S3)>

[0107] In this process, the resin composition prepared in the resin composition preparation step (S2) is molded to obtain a sheet. For example, in the resin composition preparation step (S2), biomass material and thermoplastic resin are sufficiently heated and mixed in an extruder to prepare a resin composition. The resin composition is then transferred to a molding machine, and the resin composition is molded using the molding machine to form a sheet. The temperature used for molding the sheet may preferably be set to a temperature above the melting temperature of the thermoplastic resin, for example, 150 to 450°C, and the molding pressure may be set appropriately. The formed sheet is further molded using a vacuum molding machine to obtain a sheet with scattered protrusions. An example of such a vacuum molding machine is the WAKITEC FVS-500P (Wakisaka Engineering Co., Ltd.). The shape of the mold used in the vacuum molding machine can be matched to the shape of the protrusions to be formed on the sheet to create protrusions of the required shape on the sheet surface. Alternatively, the protrusions may be created simultaneously with the sheet molding.

[0108] <Biomass material cooling process (S4)>

[0109] In the method for manufacturing a single-layer sheet according to this embodiment, a biomass material cooling step (S4) may be provided between the biomass material drying step (S1) and the resin composition preparation step (S2). This step can be carried out, for example, using a manufacturing apparatus having a heating agitator, a cooling agitator, and an extruder.

[0110] The biomass material and thermoplastic resin are heated and stirred in a heating agitator. Alternatively, the biomass material, thermoplastic resin, and low-melting-point additive may be heated and stirred in the heating agitator. After that, the mixture of biomass material and thermoplastic resin may be transferred to a cooling agitator and cooled while being stirred in the cooling agitator to a temperature above the melting temperature of the low-melting-point additive, and close to its melting temperature. Alternatively, the mixture of biomass material and thermoplastic resin may be cooled without stirring.

[0111] [Film manufacturing method]

[0112] When the molded body is a film, the method for manufacturing the film may include: a biomass material drying step in which biomass material is placed in a container equipped with an external heating element, and the biomass material is dried while the inside of the container is heated by the heating element, thereby preventing the biomass material from adhering to the inner surface of the container; a resin composition preparation step in which the biomass material dried in the biomass material drying step is mixed with a thermoplastic resin to prepare a resin composition; and a molding step in which the resin composition prepared in the resin composition preparation step is molded to obtain a film with scattered protrusions.

[0113] Note that the biomass material drying process and the resin composition preparation process are the same as the processes in the single-layer sheet manufacturing method, so their explanation will be omitted. The molding process will be described below. An inflation molding machine can be used in the molding process. For example, a ring die may be used as the inflation molding machine. The molded body formed into a film shape by the inflation molding machine may be immediately cooled to a predetermined thickness by setting the temperature of the take-up roll appropriately, taken up as a raw material roll, and wound up.

[0114] [Manufacturing method for multilayer sheets]

[0115] In the case of a multilayer sheet according to this embodiment, the multilayer sheet may include a biomass material drying step in which biomass material is contained in a container equipped with an external heating element, and the biomass material is dried by stirring while the inside of the container is heated by the heating element; a resin composition preparation step in which the biomass material dried in the biomass material drying step is mixed with a thermoplastic resin to prepare a resin composition; and a multilayer extrusion molding step in which the resin composition prepared in the resin composition preparation step and a resin composition of a different type from the resin composition are multilayer extruded to obtain a laminate in which different types of resin layers are laminated together.

[0116] The method for manufacturing a multilayer sheet according to this embodiment may include a biomass material drying step (S1), a resin composition preparation step (S2), and a multilayer extrusion molding step (S6). It may also include a biomass material cooling step (S4). Note that the biomass material drying step (S1), the resin composition preparation step (S2), and the biomass material cooling step (S4) are the same steps as in the method for manufacturing a single-layer sheet, so their explanation will be omitted. The multilayer extrusion molding step (S6) will be described below.

[0117] <Multilayer extrusion molding process (S6)>

[0118] In the multilayer extrusion molding process (S6), a resin composition of a different type from the resin composition is extruded and molded so that different types of resin layers are stacked on top of each other to obtain a laminate. The laminate can be obtained, for example, using a multilayer co-extrusion molding machine. The multilayer co-extrusion molding machine may have an extruder for layer A, an extruder for layer B, an extruder for layer C, a feed block, and dies. Using the multilayer co-extrusion molding machine, a three-layer structure sheet is co-extruded in which layers A, B, and C are stacked, with layer B containing biomass material as the middle layer and layers A and C as the surface layers. The extruder for layer B extrudes the resin composition prepared in the resin composition preparation process (S2), and the extruder for layer A and the extruder for layer C each extrude a thermoplastic resin composition of a different type from the resin composition extruded from the extruder for layer B. When manufacturing a two-layer sheet consisting of layer A and layer B, for example, the sheet is formed using the extruder for layer A and the extruder for layer B. Furthermore, when manufacturing a three-layer sheet in which layer B is the intermediate layer and layer A is the outer layer, for example, an extruder for layer A, an extruder for layer B, and an extruder for layer C are used, and the resin composition used for the extruder for layer B is supplied to the extruder for layer C to form the three-layer sheet. The same method as for a single-layer sheet may be used to scatter protrusions on the sheet, and the protrusions can be formed simultaneously on layers A, B, and C.

[0119] (3) Purpose

[0120] The molded body according to this embodiment can absorb the impact of a fall within the packaging container when the transported object is dropped during transportation of goods or products, thereby mitigating the impact applied to the transported object.

[0121] 2. Second Embodiment (Another Example of a Molded Body)

[0122] (1) Structure of the molded body

[0123] The molded body of this embodiment is molded to match the shape of the object to be packaged. When the object to be packaged is placed in the molded body from the opening toward the bottom, multiple protrusions are formed on the bottom side that comes into contact with the object to be packaged. The multiple protrusions include multi-stage protrusions. Furthermore, the multi-stage protrusions have a multi-stage structure. In a plan view of the molded body, the cross-sectional area of ​​the upper surface of each stage constituting the multi-stage structure decreases in the direction in which the protrusions protrude. In addition, the recovery rate calculated based on the displacement of the upper surface of the uppermost stage of the multi-stage protrusion before and after a compression test in which a load is applied from above to compress the upper surface of the uppermost stage of the multi-stage protrusion is 40% or more.

[0124] The configuration of the molded body of this embodiment will now be described with reference to the drawings. Figure 16 is a plan view of the bottom 30 of the molded body, which has a plurality of protrusions 31 scattered thereon. Figure 17 is an enlarged perspective view of the protrusions 31. Figure 18 is a cross-sectional view taken along line A-A in Figure 16.

[0125] In this embodiment, the cross-sectional shape of the protrusion in plan view is preferably circular. In the case of a multi-stage protrusion having a multi-stage structure, the cross-sectional shape of the upper surface of each stage constituting the multi-stage structure in plan view is concentric. In addition, the cross-sectional shape of the protrusion in plan view in this embodiment is rectangular, such as a square or rectangle, or polygonal, such as a pentagon or hexagon. As shown in Figure 16, the cross-sectional shape (outer circumference) of the protrusions 31 scattered on the bottom 30 of the molded body in plan view is circular. As shown in Figures 17 and 18, the protrusion 31 is a multi-stage protrusion having a three-stage structure: first stage 31f, second stage 31s, and third stage 31t. In the multi-stage protrusion 31, in the direction in which the protrusion protrudes, the cross-sectional area of ​​the upper surface of each stage constituting the multi-stage structure gradually decreases in a plan view of the molded body. For example, in the multi-stage protrusion 31 shown in Figures 16, 17, and 18, the cross-sectional area of ​​the upper surface of the second stage 31s is smaller than the cross-sectional area of ​​the upper surface of the first stage 31f, and the cross-sectional area of ​​the upper surface of the third stage 31t is smaller than the cross-sectional area of ​​the upper surface of the second stage 31s. When an object to be packaged is dropped and collides with such a multi-stage protrusion 31, the protrusions of the stages that come into contact with the object to be packaged are prone to being crushed. From the viewpoint of mitigating the impact of a fall when an object to be packaged is dropped, the height H31 of the protrusion 31 may be preferably 0.2 or more, more preferably 0.33 or more, and even more preferably 0.5 or more, as a ratio to the height of the object to be packaged (height H31 of the protrusion 31 / height of the object). Also, the height H31 of the protrusion 31 may be preferably 0.1 cm to 5 cm, more preferably 0.2 cm to 0.4 cm, and even more preferably 0.3 cm to 3 cm. Furthermore, the height H31 of the protrusion 31 may be, more preferably, 0.5 or more, and even more preferably 1 or more, in terms of the ratio of the height H31 of the protrusion 31 to the diameter of the cross-sectional shape of the protrusion 31 (height H31 of the protrusion 31 / diameter of the cross-sectional shape of the protrusion 31).

[0126] Furthermore, the height H31f of the first stage 31f of the protrusion 31 may preferably be 0.1 cm to 1.4 cm, more preferably 0.2 cm to 1.3 cm, and even more preferably 0.3 cm to 1.2 cm. Also, the ratio of the height H31f of the first stage 31f of the protrusion 31 to the diameter of the cross-sectional shape of the first stage 31f of the protrusion 31 (height H31f of the first stage of the protrusion 31 / diameter of the cross-sectional shape of the first stage 31f of the protrusion 31) may preferably be 0.066 or more, more preferably 0.2 or more, and even more preferably 0.33 or more.

[0127] Furthermore, from the viewpoint of making the protrusion 31 more easily crushed when the packaged object falls and collides with the protrusion 31, the height H31s of the second stage 31s of the protrusion 31 may be a ratio of (height H31s of the second stage 31s of the protrusion 31 / H31) of 0.066 or more, more preferably 0.2 or more, and even more preferably 0.33 or more. Also, the height H31s of the second stage 31s of the protrusion 31 may be a ratio of 0.1 cm to 1.4 cm, more preferably 0.2 cm to 1.3 cm, and even more preferably 0.3 cm to 1.2 cm. Furthermore, the height H31s of the second stage 31s of the protrusion 31 may be, more preferably, 0.2 or more, and even more preferably 0.33 or more, as a ratio (height H31s of the second stage of the protrusion 31 / diameter of the cross-sectional shape of the first stage 31f of the protrusion 31).

[0128] Furthermore, from the viewpoint of making the protrusion 31 more easily crushed when the packaged object falls and collides with the protrusion 31, the height H31t of the third stage 31t of the protrusion 31 may be a ratio of (height H31t of the third stage 31t of the protrusion 31 / H31) of 0.066 or more, more preferably 0.2 or more, and even more preferably 0.33 or more. Also, the height H31t of the third stage 31t of the protrusion 31 may be a ratio of 0.1 cm to 1.4 cm, more preferably 0.2 cm to 1.3 cm, and even more preferably 0.3 cm to 1.2 cm. Furthermore, the height H31t of the third stage 31t of the protrusion 31 may be preferably 0.066 or more, more preferably 0.2 or more, and even more preferably 0.33 or more, as a ratio to the diameter of the cross-sectional shape of the first stage 31f of the protrusion 31 (height H31t of the third stage 31t of the protrusion 31 / diameter of the cross-sectional shape of the first stage 31f of the protrusion 31).

[0129] In the multi-stage protrusion of the molded body of this embodiment, recesses may be formed along the outer circumference direction of the upper surface of each stage. Figure 19 is an enlarged plan view of a multi-stage protrusion in which recesses are formed along the outer circumference direction of the upper surface of each stage. As shown in Figure 19, a recess 32f is formed along the outer circumference direction of the upper surface of the first stage 31f of the multi-stage protrusion 31, and a recess 32s is formed along the outer circumference direction of the upper surface of the second stage 31s. The recesses may be formed continuously along the outer circumference, as shown in Figure 19, or they may be formed intermittently, resulting in a number of holes in the outer circumference direction.

[0130] Because recesses are formed along the outer circumference of the upper surface of each tier, when the packaged object falls and collides with the protrusion 31, the tiers with recesses are more likely to collapse, thus reducing the impact of the fall. For example, as shown in Figure 19, if a recess 32f is formed along the outer circumference of the upper surface of the first tier 31f of the multi-tier protrusion 31, and a recess 32s is formed along the outer circumference of the upper surface of the second tier 31s, when the packaged object collides with the uppermost end surface of the third tier 31t of the multi-tier protrusion 31, the second tier 31s and the first tier 31f will collapse, making it easier to absorb the impact of the fall.

[0131] The molded body of this embodiment has a recovery rate of 40% or more, preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more, calculated based on the displacement of the uppermost surface of the multi-stage protrusion before and after a compression test in which a load is applied from above to the uppermost surface of the multi-stage protrusion. If the recovery rate is less than 40%, it will not be able to mitigate the impact of a fall. The method for measuring the recovery rate is the same as the method for measuring the recovery rate of the molded body of the first embodiment, so a description will be omitted.

[0132] Figures 20(A) and (B) are cross-sectional views showing the relationship between the object to be packaged P, which is contained in the molded body from the opening 43 toward the bottom 40, the bottom 40 of the molded body, the protrusion 41, and the side portion 42 of the molded body. Figure 20(A) shows the state before the object to be packaged P falls and collides with the protrusion 41 formed on the bottom 40. Figure 20(B) shows the state after the object to be packaged P falls and collides with the protrusion 41 formed on the bottom 40. In Figure 20(A), the arrow indicates the direction in which the object to be packaged P falls. As shown in Figure 20(A), the molded body is formed from the bottom 40 and the side portion 42 which is upright from the bottom 40 toward the opening 43 along the outer circumference of the bottom 40, in accordance with the shape of the object to be packaged P.

[0133] As shown in Figure 20(B), when the packaged object P falls and collides with the protrusion 41 formed on the bottom 40, the protrusion 41 is crushed. By crushing the protrusion 41, it becomes possible to mitigate the impact of the fall applied to the packaged object P, similar to the molded body in the first embodiment.

[0134] In this embodiment, the lowest stage of the multi-stage protrusion may be formed at the corner of the bottom of the molded body. Figure 26 is a photograph of a circular four-stage protrusion 45 formed at the corner of the bottom of the molded body. As shown in Figure 26, the cross-sectional shape of the circular four-stage protrusion 45 in plan view is circular. Also, as shown in Figure 26, the circular four-stage protrusion 45 is a multi-stage protrusion having a four-stage structure: first stage 45b, second stage 45s, third stage 45t, and fourth stage 45f. The cross-sectional shapes of the second stage 45s, third stage 45t, and fourth stage 45f in plan view are circular. On the other hand, the cross-sectional shape of the first stage 45b in plan view is triangular. Also, the cross-sectional area of ​​the first stage 45b in plan view is larger than the cross-sectional area of ​​the second stage 45s in plan view. By forming such a first stage 45b, the cushioning effect when the packaged object is dropped is increased by the thickness of the first stage 45b. Figure 27 is a cross-sectional view of a circular four-stage protrusion 45 formed at the corner of the bottom of the molded body. As shown in Figure 27, the circular four-stage protrusion 45 is a multi-stage protrusion having a four-stage structure consisting of a first stage 45b, a second stage 45s, a third stage 45t, and a fourth stage 45f, which protrude upward from the bottom 46 of the molded body. In addition, from the viewpoint of mitigating the impact by making the second stage 45s and the third stage 45t more easily crushed when the packaged object falls and collides with the upper surface of the fourth stage 45f, the upper surface 45sp of the second stage 45s and the upper surface 45tp of the third stage 45t may each be angled upward with respect to the bottom 46 by an upward angle α (°). When the upward angle α° is 0°, these upper surfaces are parallel to the bottom. Such an upward angle α (°) may preferably be 0 to 20°, more preferably 0 to 15°, and even more preferably 0 to 10°.

[0135] The configuration of the molded body in this embodiment is the same as that of the molded body in the first embodiment, so a description will be omitted.

[0136] (2) Method for manufacturing a molded article

[0137] The method for manufacturing the molded article in this embodiment is the same as that for manufacturing the molded article in the first embodiment, so a description will be omitted.

[0138] (3) Purpose

[0139] The application of the molded article in this embodiment is the same as that of the molded article in the first embodiment, so a description will be omitted.

[0140] 3. Examples

[0141] The present invention will be described in more detail below based on the examples. The examples described below are representative examples of the present invention, and the scope of the present invention is not limited to these examples. The evaluation methods and evaluation criteria used in the examples are as follows.

[0142] (Example 1)

[0143] In a heated agitator (external heated jacket type mixer, Kawata Co., Ltd.), 50.4 parts by mass of corn starch (manufactured by Showa Sangyo Co., Ltd.) with an initial moisture content of 14% and 0.9 parts by mass of glycerin fatty acid ester were mixed with a total of 100 parts by mass of each component (ratio of corn starch before drying), and the mixture was dried for 20 minutes at a heated jacket temperature of 150°C. The moisture content of the corn starch after drying was 2%. Corn starch, 37 parts by mass of polypropylene (product name: EA9, Nippon Polypropylene Co., Ltd.), 0.9 parts by mass of zinc stearate, 2.7 parts by mass of magnesium stearate, 2.8 parts by mass of styrene-based thermoplastic elastomer (product name: ToughTec H1041, manufactured by Asahi Kasei Corporation), 2.8 parts by mass of acid-modified polyethylene (product name: Fusabond® N493, manufactured by DuPont), and 2.5 parts by mass of white pigment were compounded using a twin-screw extruder (Ikegai Co., Ltd. PCM30, screw diameter: 30φ) to obtain pellets. The obtained pellets were supplied via a hopper to the B-layer extruder of a multi-layer co-extrusion molding machine (manufactured by LAB TECH Engineering Co., Ltd.).

[0144] Furthermore, a polypropylene resin composition (product name: EG6D, manufactured by Nippon Polypropylene Co., Ltd.) was supplied to the A-layer extruder of a multilayer co-extrusion molding machine (manufactured by LAB TECH Engineering Co., Ltd.) via a hopper, and the same polypropylene resin composition (product name: EG6D, manufactured by Nippon Polypropylene Co., Ltd.) was supplied to the C-layer extruder via a hopper. The resin compositions supplied to the A-layer extruder, B-layer extruder, and C-layer extruder were co-extruded to obtain a multilayer sheet with a three-layer structure, with the B-layer as the middle layer. The thickness of the obtained multilayer sheet was 0.8 mm.

[0145] The cylinder temperature and adapter temperature of the extruder for layer A (model number: LE25-30 / C (manufactured by LAB TECH Engineering Co., Ltd.), L / D: 30, φ: 250 mm), the extruder for layer B (model number: LE25-30 / C (manufactured by LAB TECH Engineering Co., Ltd.), L / D: 30, φ: 250 mm), and the extruder for layer C (model number: LE25-30 / C (manufactured by LAB TECH Engineering Co., Ltd.), L / D: 30, φ: 250 mm) were set to 200°C. In addition, the screw speed of the extruder for layer B was set to 90 RPM, and the screw speeds of the extruders for layer A and layer C were set to 20 RPM.

[0146] The obtained multilayer sheet was used in a vacuum forming machine (WAKITEC FVS-500P (Wakisaka Engineering Co.)) to form a sheet 50 on the A-layer side surface, which had a circular two-stage protrusion with a circular cross-section, a square three-stage protrusion with a square cross-section, a circular three-stage protrusion with a circular cross-section, and a circular three-stage protrusion with a circular cross-section, where recesses were formed along the outer circumference in the first and second stages. Figure 21 is a plan view photograph of the obtained sheet 50. As shown in Figure 21, the sheet 50 had a circular two-stage protrusion 51 with a circular cross-section, a square three-stage protrusion 52 with a square cross-section, a circular three-stage protrusion 53 with a circular cross-section, and a circular three-stage protrusion 54 with a circular cross-section, where recesses were formed along the outer circumference in the first and second stages.

[0147] A sample was obtained by cutting out a 3.5 mm x 3.5 mm section from sheet 50, containing each of the following: a circular two-tiered protrusion 51, a rectangular three-tiered protrusion 52, a circular three-tiered protrusion 53, and a circular three-tiered protrusion 54. Figure 22 is a plan view photograph of the circular two-tiered protrusion 51 contained in the cut-out sample. Figure 23 is a plan view photograph of the rectangular three-tiered protrusion 52 contained in the cut-out sample. Figure 24 is a plan view photograph of the circular three-tiered protrusion 53 contained in the cut-out sample. Figure 25 is a plan view photograph of the circular three-tiered protrusion 54 contained in the cut-out sample.

[0148] [Compression test]

[0149] The initial distance between the movable plate UP and the fixed plate LP of the compression testing machine (Strograph VE20D, manufactured by Toyo Seiki Co., Ltd.) was set to 40 mm, and each of the samples, including the cut-out circular two-stage protrusion 51, the square three-stage protrusion 52, the circular three-stage protrusion 53, and the circular three-stage protrusion 54, was placed between the movable plate UP and the fixed plate LP.

[0150] The electric motor was controlled to operate the movable plate UP on the fixed plate LP and each sample, and each sample was continuously subjected to pressure under the following conditions until the protrusions of each sample were completely crushed. After confirming that the protrusions were completely crushed, the movable plate UP was moved upward, and each sample was left to stand on the fixed plate LP for 10 minutes. Movable plate UP movement speed: 20 mm / min Load limit: 1000 N Number of tests: N3

[0151] After the compression test is complete, the height H of the uppermost surface of the protrusion before the compression test, as shown in Figure 12, is measured for each sample. b and the height H of the uppermost end surface of the protrusion before the compression test a The recovery rate is calculated using the following formula: Recovery rate (%) = (H a / H b ) × 100

[0152] The results are shown in Table 1 below.

[0153]

[0154] All of the protrusions had a recovery rate of 40% or more, demonstrating excellent resilience. In particular, the circular three-tiered protrusion had better resilience than the circular two-tiered protrusion and the square three-tiered protrusion. Furthermore, the circular three-tiered protrusion, which had a circular cross-section and recesses formed along the outer circumference of the first and second tiers, had the best resilience. This suggests that the first and second tiers, where the recesses were formed, were easily crushed by compression, exhibiting a spring-like cushioning effect.

[0155] (Example 2)

[0156] A multilayer sheet was formed in the same manner as in Example 1, except that the thickness of the obtained multilayer sheet was 1.0 mm. From the obtained multilayer sheet, a sheet was formed in the same manner as in Example 1, in which a circular two-stage protrusion with a circular cross-section, a square three-stage protrusion with a square cross-section, a circular three-stage protrusion with a circular cross-section, and a circular three-stage protrusion with a circular cross-section and recesses formed along the outer circumference in the first and second stages were formed on the A-layer side surface.

[0157] Similar to Example 1, samples were cut from the sheet to form circular two-stage protrusions, square three-stage protrusions with a square cross-section, circular three-stage protrusions with a circular cross-section, and circular three-stage protrusions with a circular cross-section and recesses formed along the outer circumference in the first and second stages. Compression tests were performed on the obtained samples using the same method as in Example 1, and the recovery rate of each sample was measured.

[0158] The results are shown in Table 2 below.

[0159]

[0160] All of the protrusions exhibited excellent resilience, with a recovery rate of over 40%. In particular, the circular three-tiered protrusions showed superior resilience compared to the circular two-tiered protrusions and the square three-tiered protrusions. Furthermore, the circular three-tiered protrusions, with a circular cross-section and recesses formed along the outer circumference of the first and second tiers, showed the best resilience. This suggests that the first and second tiers, where the recesses were formed, were easily crushed by compression, exhibiting a spring-like cushioning effect.

[0161] The configurations, methods, processes, shapes, materials, and numerical values ​​mentioned in the above embodiments and examples are merely examples, and different configurations, methods, processes, shapes, materials, and numerical values ​​may be used as needed.

[0162] Furthermore, the configurations, methods, processes, shapes, materials, and numerical values ​​of the above-described embodiments and examples can be combined with each other, as long as they do not depart from the spirit of these embodiments.

[0163] Furthermore, in this specification, numerical ranges indicated using "~" represent a range that includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In numerical ranges described stepwise in this specification, the upper or lower limit of a numerical range in one step may be replaced with the upper or lower limit of a numerical range in another step. Unless otherwise specified, the materials exemplified in this specification can be used individually or in combination of two or more.

[0164] 10 Sheet 11 Protrusion 11f First stage 11s Second stage 20 Sheet 21 Protrusion 21f First stage 21s Second stage 21t Third stage 22f First stage recess 22s Second stage recess UP Movable plate LP Fixed plate S Sample 30 Sheet 31 Protrusion 31f First stage 31s Second stage 31t Third stage 32f First stage recess 32s Second stage recess P Packaging object 40 Bottom 41 Protrusion 42 Side 43 Opening 50 Sheet 51 Circular two-stage protrusion 52 Square three-stage protrusion 53 Circular three-stage protrusion (no recess) 54 Circular three-stage protrusion (with recess)

Claims

1. A molded body formed by a plurality of scattered protrusions, wherein the plurality of protrusions include a multi-stage protrusion, the multi-stage protrusion has a multi-stage structure, the multi-stage protrusion has a decrease in the cross-sectional area of ​​the upper surface of each stage constituting the multi-stage structure in a plan view of the molded body in the direction in which the protrusion protrudes, and the recovery rate calculated based on the amount of displacement of the upper surface of the uppermost stage before and after a compression test in which a load is applied from above to the uppermost stage of the multi-stage protrusion is 40% or more.

2. The molded article according to claim 1, wherein the molded article is formed from a resin composition comprising a biomass material and a thermoplastic resin.

3. The molded body according to claim 1, wherein, in a plan view of the molded body, the cross-sectional shape of the upper surface of each step constituting the multi-stage structure is circular.

4. The molded body according to claim 3, wherein, in a plan view of the molded body, the cross-sectional shape of the upper surface of each step constituting the multi-stage structure is a concentric circle shape.

5. The molded body according to claim 1, wherein, in a plan view of the molded body, the cross-sectional shape of the upper surface of each step constituting the multi-stage structure is polygonal.

6. The molded article according to claim 1, wherein the multi-stage structure is a three-stage structure.

7. The molded body according to claim 1, wherein when a load is applied to the upper surface of the uppermost of the multi-stage protrusions, each of the stages constituting the multi-stage protrusions collapses.

8. The molded body according to claim 1, wherein the average thickness of the molded body is 0.3 mm to 1.2 mm.

9. The molded body according to claim 1, wherein in the multi-stage protrusion, a recess is formed along the outer peripheral direction of the upper surface of each stage.

10. The molded body according to claim 9, wherein the recess is formed on the upper surface of the steps other than the uppermost step of the multi-step protrusion.

11. The molded body according to claim 1, wherein, in a plan view of the molded body, the cross-sectional shapes of the upper surfaces of each stage constituting the multi-stage structure are the same or different from each other.

12. The molded body according to claim 1, wherein, in a plan view of the molded body, the cross-sectional area of ​​the upper surface of the lowest of the multi-stage protrusions is larger than the cross-sectional area of ​​the upper surface of the step adjacent to the uppermost of the multi-stage protrusions of the step adjacent to the lowest of the multi-stage protrusions.

13. A molded body formed to conform to the shape of an object to be packaged, wherein, when the object to be packaged is placed in the molded body from the opening toward the bottom, a plurality of protrusions are formed on the bottom side that comes into contact with the object to be packaged, the plurality of protrusions include a multi-stage protrusion, the multi-stage protrusion has a multi-stage structure, the cross-sectional area of ​​the upper surface of each stage constituting the multi-stage structure decreases in a plan view of the molded body in the direction in which the protrusion protrudes, and the recovery rate calculated based on the amount of displacement of the upper surface of the uppermost stage before and after a compression test in which a load is applied from above to the uppermost stage of the multi-stage protrusion is 40% or more.

14. The molded article according to claim 13, wherein the molded article is formed from a resin composition comprising a biomass material and a thermoplastic resin.

15. The molded body according to claim 13, wherein, in a plan view of the molded body, the cross-sectional shape of the upper surface of each step constituting the multi-stage structure is circular.

16. The molded body according to claim 15, wherein, in a plan view of the molded body, the cross-sectional shape of the upper surface of each step constituting the multi-stage structure is concentric.

17. The molded body according to claim 13, wherein, in a plan view of the molded body, the cross-sectional shape of the upper surface of each step constituting the multi-stage structure is polygonal.

18. The molded article according to claim 13, wherein the multi-stage structure is a three-stage structure.

19. The molded body according to claim 13, wherein when a load is applied to the upper surface of the uppermost stage of the multi-stage protrusion, each stage constituting the multi-stage protrusion collapses.

20. The molded body according to claim 13, wherein the average thickness of the molded body is 0.3 mm to 1.2 mm.

21. The molded body according to claim 13, wherein in the multi-stage protrusion, a recess is formed along the outer peripheral direction of the upper surface of each stage.

22. The molded body according to claim 21, wherein the recess is formed on the upper surface of the steps other than the uppermost step of the multi-step protrusion.

23. The molded body according to claim 13, wherein, in a plan view of the molded body, the cross-sectional shapes of the upper surfaces of each stage constituting the multi-stage structure are the same or different from each other.

24. The molded body according to claim 13, wherein, in a plan view of the molded body, the cross-sectional area of ​​the upper surface of the lowest of the multi-stage protrusions is larger than the cross-sectional area of ​​the upper surface of the step adjacent to the uppermost of the multi-stage protrusions of the step adjacent to the lowest of the protrusions.

25. The molded body according to claim 13, wherein the lowest stage of the multi-stage protrusion is formed at the corner of the bottom of the molded body.