Method for manufacturing electronic component device

By employing a radical polymerizable compound and a radical polymerization initiator with controlled temperature processes, the method addresses the challenge of prolonged filling times in large semiconductor substrates, achieving efficient and rapid underfill material application.

WO2026234891A1PCT designated stage Publication Date: 2026-11-12RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/007204
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-02-26
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The increasing size of substrates in semiconductor devices leads to prolonged filling times for underfill materials due to their viscosity increasing during the filling process, making it difficult to fill gaps efficiently.

Method used

A method involving the use of an underfill material containing a radical polymerizable compound and a radical polymerization initiator, where the filling is done at a temperature at least 10°C lower than the 10-hour half-life temperature of the initiator, followed by curing at a temperature at least 10°C higher, allowing separate processes for filling and curing.

Benefits of technology

This method extends the time for which the underfill material maintains low viscosity, enabling faster filling and effective curing, suitable for large-area substrates and narrow gaps without requiring new equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

This method for manufacturing an electronic component device includes: filling a gap between an electronic component and a substrate electrically connected to the electronic component via a connection part with an underfill material containing a radical polymerizable compound and a radical polymerization initiator at a temperature lower than a 10-hour half-life temperature of the radical polymerization initiator by 10°C or more; and heating the underfill material to a temperature higher than the 10-hour half-life temperature of the radical polymerization initiator by 10°C or more after or simultaneously with completion of filling the gap with the underfill material to cure the underfill material.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method for electronic component devices

[0001] This disclosure relates to a method for manufacturing electronic component devices.

[0002] Underfill materials are widely used in semiconductor devices with bare chip mounting, such as COB (Chip on Board), COG (Chip on Glass), and TCP (Tape Carrier Package). Furthermore, in semiconductor devices (also called flip-chip devices) in which semiconductor elements are directly bump-connected to a wiring board made of ceramic, glass epoxy resin, glass imide resin, polyimide film, etc., underfill materials are used to fill the gap between the bump-connected semiconductor elements and the wiring board.

[0003] In recent years, with the advancement of information technology, electronic devices have become even smaller, more integrated, and more multifunctional, leading to smaller bump diameters, narrower pitches, and narrower gaps due to the increased number of pins. Therefore, the development of underfill materials with excellent gap injection properties is being investigated (see, for example, Patent Document 1).

[0004] Japanese Patent Publication No. 2002-97342

[0005] However, in recent years, the increasing size of substrates has led to a situation where filling with underfill material takes a long time. In light of these circumstances, the object of this disclosure is to provide a method for manufacturing electronic component devices that can extend the time for which the low viscosity of the underfill material can be maintained.

[0006] The means for solving the above problems include the following embodiments: <1> A method for manufacturing an electronic component device, comprising: filling the gap between an electronic component and a substrate electrically connected to the electronic component via a connection portion with an underfill material containing a radical polymerizable compound and a radical polymerization initiator at a temperature at least 10°C lower than the 10-hour half-life temperature of the radical polymerization initiator; and curing the underfill material by heating it to a temperature at least 10°C higher than the 10-hour half-life temperature of the radical polymerization initiator after or immediately after the filling of the underfill material into the gap is completed. <2> The method for manufacturing an electronic component device according to <1>, wherein the radical polymerizable compound includes at least one selected from the group consisting of (meth)acrylic compounds and maleimide compounds. <3> The method for manufacturing an electronic component device according to <1> or <2>, wherein it does not contain any other polymerizable compounds other than the radical polymerizable compound, or the content of other polymerizable compounds relative to the total amount of other polymerizable compounds and the radical polymerizable compound is 20% by mass or less. <4> The method for manufacturing an electronic component device according to any one of <1> to <3>, wherein the radical polymerization initiator comprises a peroxide having a 10-hour half-life temperature of 90°C to 110°C. <5> The method for manufacturing an electronic component device according to any one of <1> to <4>, wherein the underfill material further comprises an inorganic filler. <6> The method for manufacturing an electronic component device according to <5>, wherein the underfill material contains 20% by mass or more of the inorganic filler.

[0007] According to this disclosure, a method for manufacturing an electronic component device is provided that makes it possible to extend the time for which the low viscosity of the underfill material can be maintained.

[0008] In this disclosure, the term "process" includes not only processes that are independent of other processes, but also processes that cannot be clearly distinguished from other processes, provided that the purpose of the process is achieved. In this disclosure, numerical ranges indicated using "~" include the numbers before and after "~" as the minimum and maximum values, respectively. In numerical ranges described in stages in this disclosure, the upper or lower limit of one numerical range may be replaced by the upper or lower limit of another numerical range described in stages. Also, in numerical ranges described in this disclosure, the upper or lower limit of that numerical range may be replaced by the values ​​shown in the examples. In this disclosure, each component may contain multiple types of the corresponding substance. If multiple types of the substance corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple types of substances present in the composition, unless otherwise specified. In this disclosure, each component may contain multiple types of particles. If multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified. In this disclosure, "(meth)acrylic" means at least one of acrylic or methacrylic, "(meth)acrylate" means at least one of acrylate or methacrylate, "(meth)acryloyl" means at least one of acryloyl or methacryloyl, and "(meth)acryloxy" means at least one of acryloxy or methacryloxy.

[0009] In the method for manufacturing an electronic component device according to the present disclosure, an underfill material containing a radical polymerizable compound and a radical polymerization initiator is filled into the gap between an electronic component and a substrate electrically connected to the electronic component via a connection portion at a temperature at least 10°C lower than the 10-hour half-life temperature of the radical polymerization initiator (hereinafter also referred to as the "filling step"). After or immediately after the filling of the underfill material into the gap is completed, the underfill material is heated to a temperature at least 10°C higher than the 10-hour half-life temperature of the radical polymerization initiator to cure it (hereinafter also referred to as the "curing step").

[0010] The method for manufacturing electronic component devices described herein makes it possible to extend the time for which the low viscosity of the underfill material is maintained. The reason for this is thought to be as follows. The underfill material described herein uses a radical polymerizable compound. Even when heat is applied to a radical polymerizable compound, the polymerization reaction is suppressed as long as radicals are not present, and the thickening caused by heating during filling is suppressed. Because the thickening is suppressed, the time required for filling can be shortened, and it is possible to handle even large-area substrates. Therefore, the filling of the underfill material into the gaps is carried out at a temperature at least 10°C lower than the 10-hour half-life temperature of the radical polymerization initiator, so as to be carried out at a temperature in which radical generation is suppressed. As a result, the polymerization reaction of the radical polymerizable compound by radicals is suppressed, and the thickening of the underfill material is suppressed. Since the underfill material can be filled into the gaps while its thickening is suppressed, the filling time for the underfill material can be shortened. After filling is completed, the underfill material is heated to a temperature at least 10°C higher than the 10-hour half-life temperature of the radical polymerization initiator to advance the polymerization reaction of the radical polymerizable compound and harden the underfill material. At this stage, there is no need to consider the thickening due to the polymerization of radical polymerizable compounds, so the temperature can be increased to allow the curing reaction to proceed sufficiently.

[0011] Thus, the method for manufacturing an electronic component device according to this disclosure separates the underfill material filling process and the curing process into separate processes, thereby shortening the underfill material filling time while ensuring sufficient curing progress.

[0012] In contrast, epoxy resins, which are widely used in conventional underfill materials, undergo a gradual polymerization reaction due to heating during filling, causing the underfill material to thicken. As a result, the time required for filling increases. Lowering the heating temperature during filling reduces the initial fluidity of the underfill material, which again increases the time required for filling and prevents sufficient curing. This is due to the fact that the filling process and the curing process cannot be separated, or are difficult to separate, as separate processes. In particular, as the substrate area increases, the time required for injection of underfill materials containing epoxy resin increases even further, or it becomes difficult to inject it over the entire surface.

[0013] Furthermore, in the method for manufacturing electronic component devices described herein, the filling temperature and curing temperature of the underfill material can be appropriately changed by changing the type of radical polymerization initiator depending on the underfill material filling equipment. Therefore, the method for manufacturing electronic component devices described herein can be used with conventionally used equipment as is. Alternatively, in line with the recent trend toward carbon neutrality, it is also possible to lower the filling temperature and curing temperature of the underfill material by changing the type of radical polymerization initiator to accommodate processes at lower temperatures. The following describes each step.

[0014] <Filling Process> In the filling process, an underfill material containing a radical polymerizable compound and a radical polymerization initiator is filled into the gap between the electronic component and the substrate, which is electrically connected to the electronic component via a connector, at a temperature at least 10°C lower than the 10-hour half-life temperature of the radical polymerization initiator.

[0015] Examples of electronic components include active elements such as semiconductor chips, transistors, diodes, and thyristors, and passive elements such as capacitors, resistors, resistor arrays, coils, and switches.

[0016] Examples of substrates include lead frames, pre-wired tape carriers, printed circuit boards (rigid or flexible), glass, and silicon wafers.

[0017] In the electronic component device of this disclosure, the electronic component and the substrate are electrically connected via a connection part. Examples of connection parts include bumps. For example, the bump may be a bump made of copper pillars.

[0018] Examples of electronic component devices include flip-chip semiconductor devices obtained by flip-chip bonding electronic components onto a substrate using bump connections. Examples of flip-chip semiconductor devices include BGA (Ball Grid Array), LGA (Land Grid Array), and COF (Chip On Film).

[0019] Electronic components may be high-density or large in size. Generally, the area of ​​a large substrate is 50 x 50 mm. 2 The size may be greater than or equal to 60 x 60 mm. 2 The size may be greater than or equal to 70 x 70 mm. 2 The above is also acceptable. Even with electronic components having such enlarged substrates, the manufacturing method of the electronic component apparatus of this disclosure is suitably applicable because it is possible to maintain low viscosity for a longer period of time. Furthermore, since the manufacturing method of the electronic component apparatus of this disclosure is possible to shorten the filling time, it is also applicable to electronic components of conventional size. An example of an electronic component of conventional size is a semiconductor chip with a length of 10 mm and a width of 10 mm.

[0020] Furthermore, since the manufacturing method of the electronic component device described herein can shorten the filling time, it can also be applied to electronic components with narrow gaps. The gap spacing may be 30 μm or less, 20 μm or less, or 15 μm or less.

[0021] The method of filling the gaps with underfill material is not particularly limited and can include dispensing, casting, printing, and compression molding methods. An example of a dispensing method is to place the substrate on a hot plate stage and fill it with underfill material while heating it. When a hot plate is used as a heating device, the temperature at which the underfill material is filled into the gaps (filling temperature) may be considered as the temperature of the hot plate.

[0022] The filling temperature is a temperature at which radical generation from the radical polymerization initiator is suppressed. Specifically, it is at least 10°C lower than the 10-hour half-life temperature of the radical polymerization initiator, and preferably at least 15°C lower.

[0023] The specific filling temperature varies depending on the half-life temperature of the radical polymerization initiator. For example, it may be 130°C or lower, 120°C or lower, 110°C or lower, or 100°C or lower. In light of the recent trend towards carbon neutrality and the need to accommodate processes at lower temperatures, the filling temperature can be set to 90°C or lower, 85°C or lower, or 80°C or lower by selecting the type of radical polymerization initiator. From the viewpoint of reducing viscosity, the filling temperature is preferably 60°C or higher, more preferably 70°C or higher, and even more preferably 80°C or higher.

[0024] The underfill material is preferably liquid at room temperature (25°C). Specifically, being liquid at room temperature (25°C) means that the viscosity measured by an E-type viscometer at 25°C is 1000 Pa·s or less. The components contained in the underfill material according to this disclosure will be described below.

[0025] [Radical Polymerizable Compounds] The underfill material contains radical polymerizable compounds. Radical polymerizable compounds are not particularly limited, but compounds having an unsaturated double bond in the molecule are preferred. Examples of radical polymerizable compounds include redox polymerizable compounds, emulsion polymerizable compounds, and (meth)acrylate compounds. One radical polymerizable compound may be used alone, or two or more may be used in combination.

[0026] Considering applicability to electronic components and devices, controllability of curing speed, and handling of underfill material, the radical polymerizable compound preferably contains at least one selected from the group consisting of (meth)acrylic compounds and maleimide compounds, and more preferably contains at least a maleimide compound. From the viewpoint of adhesive strength with the package substrate, the combined use of (meth)acrylic compounds and maleimide compounds is also one of the preferred embodiments.

[0027] The radical polymerizable compound may include other radical polymerizable compounds besides (meth)acrylic compounds and maleimide compounds. Examples of other radical polymerizable compounds include vinyl compounds.

[0028] The total content of (meth)acrylic compounds and maleimide compounds in the underfill material is preferably 40% by mass or more, more preferably 60% by mass or more, even more preferably 80% by mass or more, and may be 100% by mass.

[0029] (Maleimide Compounds) Maleimide compounds as radical polymerizable compounds can be any compound having a maleimide group in one molecule, and may be used alone or in combination of two or more.

[0030] Maleimide compounds preferably have a melting point of 150°C or lower. Since maleimide compounds are usually solids, it is preferable to have them in a molten state when using them as underfill materials. One method for moltening maleimide compounds is to heat a mixture of (meth)acrylic compounds and maleimide compounds to near the melting point of the maleimide compound to make it compatible with the (meth)acrylic compound. Since (meth)acrylic compounds and maleimide compounds undergo an ene reaction and thicken at 150°C to 250°C, the temperature at which the maleimide compound is heated to dissolve is preferably 150°C or lower, and therefore, maleimide compounds having a melting point of 150°C or lower are preferred.

[0031] The maleimide compound may be a polyfunctional maleimide compound having at least two maleimide groups in one molecule, or a monofunctional maleimide compound having one maleimide group in one molecule. The monofunctional maleimide compound and the polyfunctional maleimide compound may be used independently or in combination.

[0032] Examples of polyfunctional maleimide compounds include bismaleimide compounds represented by the following general formula (I); and polymaleimide resins (hereinafter referred to as polymaleimide resin (A1)) having a substructure represented by the following general formula (1), a substructure represented by general formula (T-1) chemically bonded to the substructure represented by general formula (1), and a substructure represented by general formula (T-2) chemically bonded to the substructure represented by general formula (1).

[0033]

[0034] In general formula (I), R 1 This represents a divalent hydrocarbon group having 1 to 18 carbon atoms, which may have substituents.

[0035] In general formula (I), R 1 The divalent hydrocarbon group having 1 to 18 carbon atoms, which may have substituents represented by , preferably includes a divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms, an alicyclic hydrocarbon group having 3 to 18 carbon atoms, and an aromatic hydrocarbon group having 6 to 18 carbon atoms.

[0036] R 1The divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms represented by is preferably a divalent aliphatic hydrocarbon group having 1 to 14 carbon atoms, and more preferably a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms. Specific examples of the divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms include methylene group, ethylene group, propylene group, isopropylene group, butylene group, pentylene group, hexylene group, octylene group, decylene group, dodecylene group, vinylene group, ethylidene group, vinylidene group, propenylene group, butadienylene group and the like. As the divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms, methylene group, ethylene group, propylene group, isopropylene group, butylene group or hexylene group is preferred, and methylene group, ethylene group, propylene group, isopropylene group or butylene group is more preferred.

[0037] R 1 The divalent alicyclic hydrocarbon group having 3 to 18 carbon atoms represented by is preferably a divalent alicyclic hydrocarbon group having 3 to 14 carbon atoms, and more preferably a divalent alicyclic hydrocarbon group having 5 to 12 carbon atoms. Specific examples of the divalent alicyclic aliphatic hydrocarbon group having 3 to 18 carbon atoms include cyclopentylene group, cyclohexylene group, cycloheptylene group, cyclopentenylene group, cyclohexenylene group, cyclohexylidene group and the like.

[0038] R 1 The divalent aromatic hydrocarbon group having 6 to 18 carbon atoms represented by is preferably a divalent aromatic hydrocarbon group having 6 to 14 carbon atoms, and more preferably a divalent aromatic hydrocarbon group having 6 to 12 carbon atoms. Specific examples of the divalent aromatic hydrocarbon group having 6 to 18 carbon atoms include phenylene group, biphenylylene group, terphenylene group and the like.

[0039] Among them, R in the general formula (I) 1 is more preferably a divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms which may have a substituent or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and even more preferably a divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms which may have a substituent.

[0040] R in the general formula (I) 1The substituents that may be present include alkyl groups, alkoxy groups, aryl groups, aryloxy groups, hydroxyl groups, amino groups, halogen atoms, methacrylate groups, mercapto groups, imino groups, ureido groups, isocyanate groups, and the like. 1 It is preferable that it does not have substituents.

[0041] Examples of bismaleimide compounds represented by general formula (I) include 4,4'-diphenylmethanebismaleimide, m-phenylenebismaleimide, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethanebismaleimide, 4-methyl-1,3-phenylenebismaleimide, and 1,6'-bismaleimide-(2,2,4-trimethyl)hexane.

[0042]

[0043] In general formula (1), R 13 Each of these independently represents an alkyl group having 1 to 18 carbon atoms, m 2 represents an integer between 0 and 4, and n 1 represents the average number of repeating units, the two *s each represent a bond, and one of the bond is L in the general formula (T-1) below. 13 or L 14 A chemical bond is formed at the position, and the other bond is L in the general formula (T-2) below. 11 or L 12 This indicates that a chemical bond is formed at that position.

[0044] In general formula (T-1) or (T-2), R 11 and R 15 Each of these independently represents a hydrogen atom or a hydrocarbon group having 1 to 18 carbon atoms, and R 12 and R 14 Each of these independently represents a hydrocarbon group having 1 to 18 carbon atoms, L 11 ~L 14 Each of these independently represents a bonding bond or a hydrogen atom, however, L 11 or L 12 At the position, it is chemically bonded to the substructure represented by general formula (1), and L 13 or L 14At this position, L is chemically bonded to the substructure represented by general formula (1), and L is not chemically bonded to the substructure represented by general formula (1). 11 ~L 14 is a hydrogen atom, m 1 and m 3 Each of these represents 2.

[0045] The molecular structure of polymaleimide resin (A1) has only one bonding site each at the ortho and para positions of the benzene ring to which the maleimide group is attached. As a result, after the reaction, a polymaleimide resin with a linearly elongated chain is obtained, making molecular weight control easy, and tending to improve heat resistance, dielectric properties, and solvent solubility.

[0046] In general formula (1), the two *s each represent a bond. And one of the two bonds is L in general formula (T-1). 13 or L 14 A chemical bond is formed at the position. The other bond is L in general formula (T-2). 11 or L 12 Chemical bonding occurs at the position. Therefore, the polymaleimide resin of this embodiment has a structural unit in which a substructure represented by general formula (T-1) and a substructure represented by general formula (T-2) are linked by a substructure represented by general formula (1), and the substructure represented by general formula (1) is chemically bonded to the maleimide group on the benzene ring in general formula (T-1) and general formula (T-2) at the para position or one ortho position. Note that in general formula (1), n 1 If the number is 2 or more, there are multiple R 13 They may be the same or they may be different. 2 If the number is 2 or more, there are multiple R 13 They may be the same or they may be different.

[0047] In general formula (1), R 13Each of these independently represents a hydrocarbon group having 1 to 18 carbon atoms, preferably a hydrocarbon group having 1 to 12 carbon atoms, more preferably a hydrocarbon group having 1 to 6 carbon atoms, even more preferably a hydrocarbon group having 1 to 3 carbon atoms, and even more preferably a hydrocarbon group having 1 or 2 carbon atoms. 2 If R is an integer greater than or equal to 2, there are multiple R's. 13 These may be the same or different. Preferred R in general formula (1) 13 Preferably, the group is a methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, tert-butyl group, n-pentyl group, isopentyl group, tert-pentyl group, or neopentyl group, and a linear alkyl group is more preferred.

[0048] In general formula (1), m 2 R represents an integer between 0 and 4, preferably an integer less than or equal to 2, and more preferably 2. Note that R in general formula (1) 13 In a benzene ring to which R is bonded, if the 1st and 3rd positions are bonded by a methylene group, then the 4th and 6th positions are R 13 It is preferable that each of them is combined. In general formula (1), n 1 n represents the average number of repeating units. 1 From the viewpoint of the viscosity of the resulting polymaleimide resin, the ratio is preferably 0 to 50, preferably 0 to 30, and preferably 0 to 15. The average number of repeating units can be calculated from the charge ratio or NMR analysis results, etc.

[0049] The polymaleimide resin (A1) preferably contains 1 to 99% by mass of the substructure represented by general formula (1) in 100% by mass of the polymaleimide resin (A1), more preferably 1 to 97% by mass, even more preferably 3 to 97% by mass, and particularly preferably 5 to 95% by mass.

[0050] In general formula (T-1), R 15Each independently represents a hydrogen atom or a hydrocarbon group having 1 to 18 carbon atoms, preferably a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms, more preferably a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. Particularly preferred R 15 These are hydrogen atoms or linear alkyl groups having 1 to 6 carbon atoms. 3 Since is 2, two R 15 They may be the same or different. In general formula (T-1), R 14 Each of these independently represents a hydrocarbon group having 1 to 18 carbon atoms, preferably a hydrocarbon group having 1 to 12 carbon atoms, and more preferably a hydrocarbon group having 1 to 6 carbon atoms. Particularly preferred R 14 As such, it is a linear alkyl group having 1 to 6 carbon atoms. By allowing a bonding site with the substructure represented by general formula (1) at the ortho position (position 6) of the benzene ring of general formula (T-1) or general formula (T-2), it has high solubility in solvents and exhibits superior low dielectric loss tangent and high heat resistance during curing. In general formula (T-1), L 13 or L 14 Each of these independently represents a bond or a hydrogen atom. However, L 13 or L 14 At least one of the positions of the substructure is chemically bonded to the substructure represented by general formula (1) and the substructure represented by general formula (T-1). In addition, L does not chemically bond to the substructure represented by general formula (1). 13 or L 14 L is a hydrogen atom. 13 and L 14 A substructure represented by general formula (1) may be chemically bonded to each of the two locations.

[0051] In general formula (T-2), R 11 Each independently represents a hydrogen atom or a hydrocarbon group having 1 to 18 carbon atoms, preferably a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms, more preferably a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. Preferred R 11 These are hydrogen atoms or linear alkyl groups having 1 to 6 carbon atoms. 1 Since is 2, two R 11They may be the same or different. In the general formula (T-2), R 12 Each of these independently represents a hydrocarbon group having 1 to 18 carbon atoms, preferably a hydrocarbon group having 1 to 12 carbon atoms, and more preferably a hydrocarbon group having 1 to 6 carbon atoms. Preferred R 12 As such, it represents a linear alkyl group having 1 to 6 carbon atoms. In the general formula (T-2), L 11 or L 12 Each of these independently represents a bond or a hydrogen atom. However, L 11 or L 12 At least one of the positions of the substructure is chemically bonded to the substructure represented by general formula (1) and the substructure represented by general formula (T-2). In addition, L does not chemically bond to the substructure represented by general formula (1). 11 or L 12 L is a hydrogen atom. 11 and L 12 A substructure represented by general formula (1) may be chemically bonded to each of the two locations.

[0052] The polymaleimide resin (A1) preferably contains 1 to 99% by mass of the substructure represented by general formula (T-1) per 100% by mass of the polymaleimide resin (A1), more preferably 1 to 97% by mass, even more preferably 3 to 97% by mass, and particularly preferably 5 to 95% by mass. The polymaleimide resin (A1) preferably contains 1 to 99% by mass of the substructure represented by general formula (T-2) per 100% by mass of the polymaleimide resin (A1), more preferably 1 to 97% by mass, even more preferably 3 to 97% by mass, and particularly preferably 5 to 95% by mass.

[0053] There are no particular restrictions on the method for producing the polymaleimide resin (A1), and the method for producing the polymaleimide resin and the examples in Japanese Patent Application Publication No. 2024-4392 can be referred to.

[0054] The polymaleimide resin (A1) may be a maleimide compound represented by the following general formula (II).

[0055]

[0056] In general formula (II), n is 0 or an integer greater than or equal to 1.

[0057] Examples of bismaleimide compounds represented by general formula (II) include phenylmethanemaleimide.

[0058] (Meth)acrylic compounds) The (meth)acrylate compounds used as radical polymerizable compounds are not particularly limited, and conventionally known (meth)acrylate compounds can be used. One (meth)acrylate compound may be used alone, or two or more may be used in combination. When two or more (meth)acrylate compounds are used in combination, the combination of (meth)acrylate compounds is not particularly limited. From the viewpoint of dispensability, it is preferable to use at least one polyfunctional (meth)acrylate compound containing at least two (meth)acryloyl groups in one molecule and at least one monofunctional (meth)acrylate compound containing one (meth)acryloyl group in one molecule in combination. Doing so often results in a low viscosity underfill material, which tends to improve injectability.

[0059] Examples of polyfunctional (meth)acrylate compounds include diethylene glycol diacrylate, triethylene glycol diacrylate, tripropylene glycol diacrylate, tetraethylene glycol diacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, polyethylene glycol diacrylate, polypropylene glycol diacrylate, tricyclodecane dimethylol diacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, tris(β-hydroxyethyl) isocyanurate triacrylate, polycarbonate acrylate, urethane acrylate, and diethylene Examples include methyl glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, polyethylene glycol dimethacrylate, polypropylene glycol dimethacrylate, tricyclodecane dimethylol dimethacrylate, ditrimethylolpropane tetramethacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, dipentaerythritol hexamethacrylate, tris(β-hydroxyethyl) isocyanurate trimethacrylate, polycarbonate methacrylate, urethane methacrylate, and difunctional (meth)acrylate compounds represented by the following formula (II).

[0060] Among these, examples include compounds having an aliphatic cyclic skeleton and at least two (meth)acryloyloxy groups (hereinafter sometimes referred to as alicyclic monomers), and compounds having two (meth)acryloyloxy groups in the molecule, with the two (meth)acryloyloxy groups linked by a linear divalent organic group (hereinafter sometimes referred to as linear monomers). These are polyfunctional (meth)acrylate compounds because they contain two (meth)acryloyl groups in one molecule.

[0061] Alicyclic monomers and linear monomers may be used individually or in combination. From the viewpoint of the linear thermal expansion coefficient of the cured product, it is preferable to include at least alicyclic monomers. The ratio of alicyclic monomers to the total amount of alicyclic monomers and linear monomers is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and may be 100% by mass.

[0062] The aliphatic cyclic skeleton contained in the alicyclic monomer is not particularly limited, and examples include the tricyclodecane skeleton, cyclohexane skeleton, cyclopentane skeleton, 1,3-adamantane skeleton, hydrogenated bisphenol A skeleton, hydrogenated bisphenol F skeleton, hydrogenated bisphenol S skeleton, isobornyl skeleton, etc. Among these, the tricyclodecane skeleton is preferred.

[0063] As the alicyclic monomer, compounds represented by the following general formula (1) are preferred.

[0064]

[0065] In general formula (1), R 1 and R 2 Each of these is independently an aliphatic hydrocarbon group having 1 to 4 carbon atoms or a group represented by the following general formula (2). n1 represents 0 or 1, n2 represents an integer from 0 to 2, and n1 + n2 is 2 or 3. n1 R 1 and n2 R 2 At least two of these are groups represented by the following general formula (2).

[0066]

[0067] In the general formula (2), R 1A represents a hydrogen atom or a methyl group, and m represents an integer of 1 to 10.

[0068] R 1 and R 2 Specific examples of the aliphatic hydrocarbon group having 1 to 4 carbon atoms represented by include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group and the like.

[0069] The compound represented by the general formula (1) may be a compound represented by the following formula (3A) or the following formula (3B).

[0070]

[0071] Examples of the compound represented by formula (3A) include tricyclodecane dimethanol diacrylate, and examples of the compound represented by formula (3B) include tricyclodecane dimethanol dimethacrylate.

[0072] The linear monomer is preferably a compound represented by the following general formula (4) or the following general formula (5).

[0073]

[0074] In general formula (4) or general formula (5), R 3 each independently represents a hydrogen atom or a methyl group, R 4 represents an alkylene group having 1 to 8 carbon atoms, R 5 represents an alkylene group having 1 to 8 carbon atoms, and p represents an integer of 2 to 5. A plurality of R 3 and R 5 may be the same or different.

[0075] As R in general formula (4) or general formula (5) 3 , a methyl group is preferred. As for R in general formula (4) 4 Specific examples of the alkylene group having 1 to 8 carbon atoms represented by include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a hexamethylene group, an octamethylene group and the like. As for R in general formula (5) 5Specific examples of alkylene groups having 1 to 8 carbon atoms represented by the formula include methylene, ethylene, trimethylene, methylethylene, dimethylmethylene, tetramethylene, hexamethylene, and octamethylene groups, with methylethylene and ethylene groups being preferred, and ethylene groups being more preferred. In general formula (5), p is preferably an integer between 3 and 4.

[0076] Examples of linear monomers include diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, tripropylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,4-butanediol dimethacrylate, and 1,6-hexanediol dimethacrylate.

[0077] Examples of monofunctional (meth)acrylate compounds include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, and decyl 2-(tricyclo)[5.2.1.02,6]decyl(meth)acrylate, 2-(tricyclo)[5.2.1.02,6]decyl(meth)acrylate, 2-(tricyclo)[5.2.1.02,6]decal(meth)acrylate, 2-(tricyclo)[5.2.1.02,6]deca-3-en-8-yloxyethyl(meth)acrylate, 2-(tricyclo)[5.2.1.02,6] Deca-3-en-9-yloxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, dimergol mono (meth)acrylate, diethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, 2-phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxy Polyethylene glycol (meth)acrylate, 2-benzoyloxyethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, benzyl (meth)acrylate, 2-cyanoethyl (meth)acrylate, γ-(meth)acryloyloxypropyltrimethoxysilane, glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, tetrahydropyranyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, 1,2,2,6,6-pentamethylpiperidinyl (meth)acrylate, 2,2,6,Examples include 6-tetramethylpiperidinyl (meth)acrylate, (meth)acryloxyethyl phosphate, (meth)acryloxyethyl phenyl acid phosphate, β-(meth)acryloyloxyethyl hydrogen phthalate, β-(meth)acryloyloxyethyl hydrogen succinate, and ethylene oxide-modified neopentyl glycol (meth)acrylate, 2-(meth)acryloyloxyethyl succinate, 2-methacryloyloxyethyl hexahydrophthalate, isobonyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, and neopentyl glycol (meth)acrylic acid benzoate. ,

[0078] (Meth)acrylic compounds may contain other polymerizable functional groups besides the (meth)acrylic group. Examples of other polymerizable functional groups include glycidyl groups, amino groups, and hydroxyl groups. These functional groups interact with the packaging substrate to increase the adhesive strength to the substrate. Examples of such compounds include 4-hydroxybutyl acrylate glycidyl ether (4HBAGE), 4-hydroxybutyl acrylate (4HBA), and 1,4-cyclohexanedimethanol monoacrylate (CHDMMA). However, from the viewpoint of suppressing viscosity increase during filling, it is desirable not to use other polymerizable functional groups in combination. Examples of combinations that polymerize include epoxy groups and amino groups, and epoxy groups and hydroxyl groups.

[0079] When at least one polyfunctional (meth)acrylate compound and at least one monofunctional (meth)acrylate compound are used in combination as radical polymerizable compounds, the content of the monofunctional (meth)acrylate compound relative to the total amount of polyfunctional (meth)acrylate compounds is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, from the viewpoint of achieving a low modulus of elasticity. Furthermore, the content of the monofunctional (meth)acrylate compound relative to the total amount of polyfunctional (meth)acrylate compounds is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, from the viewpoint of lowering the linear thermal expansion coefficient of the cured product.

[0080] When a maleimide compound and a (meth)acrylate compound are used in combination as a radical polymerizable compound, the content of the maleimide compound relative to the total amount of the maleimide compound and the (meth)acrylate compound is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, from the viewpoint of adhesion to the semiconductor package substrate. Furthermore, from the viewpoint of reducing viscosity, the content of the maleimide compound relative to the total amount of the maleimide compound and the (meth)acrylate compound is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less.

[0081] Examples of radical polymerizable compounds include forms in which a polyfunctional maleimide compound is used alone, forms in which a (meth)acrylate compound is used alone, forms in which a polyfunctional maleimide compound and a polyfunctional (meth)acrylate compound are used in combination, and forms in which a polyfunctional maleimide compound, a polyfunctional (meth)acrylate compound, and a monofunctional (meth)acrylate compound are used in combination. Among these, the form in which a polyfunctional maleimide compound, a polyfunctional (meth)acrylate compound, and a monofunctional (meth)acrylate compound are used in combination is preferred from the viewpoint of achieving both low viscosity and adhesion.

[0082] When a polyfunctional maleimide compound and a polyfunctional (meth)acrylate compound are used in combination as radical polymerizable compounds, the content of the polyfunctional maleimide compound relative to the total amount of the polyfunctional maleimide compound and the polyfunctional (meth)acrylate compound is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, from the viewpoint of adhesion to the semiconductor package substrate. Furthermore, the content of the polyfunctional maleimide compound relative to the total amount of the polyfunctional maleimide compound and the polyfunctional (meth)acrylate compound is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less, from the viewpoint of reducing viscosity.

[0083] [Other Polymerizable Compounds] The underfill material may contain other polymerizable compounds besides radical polymerizable compounds. Examples of polymerizable functional groups in other polymerizable compounds include glycidyl groups, amino groups, and hydroxyl groups. Other polymerizable compounds may be monofunctional or polyfunctional. From the viewpoint of suppressing viscosity increase during filling, it is desirable not to use other polymerizable compounds in combination that polymerize. Examples of polymerizable combinations include epoxy groups and amino groups, and epoxy groups and hydroxyl groups. Since other polymerizable compounds do not have radical polymerizable functional groups, they may seep into the interface with the substrate during the curing process. From the viewpoint of preventing seepage, it is preferable that other polymerizable compounds are not included, or if other polymerizable compounds are included, the content of other polymerizable compounds relative to the total amount of other polymerizable compounds and radical polymerizable compounds is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less.

[0084] The content of radical polymerizable compounds in the underfill material is not particularly limited. From the viewpoint of viscosity, glass transition temperature, heat resistance, etc., it is preferably 0.5% to 80% by mass, more preferably 2% to 70% by mass, and even more preferably 2% to 60% by mass.

[0085] [Radical Polymerization Initiators] Radical polymerization initiators are not particularly limited, and conventionally known radical polymerization initiators can be used. Examples of radical polymerization initiators include organic peroxides, which will be described later; azo compounds such as azobisisobutyronitrile, azobis-4-methoxy-2,4-dimethylvaleronitrile, azobiscyclohexanone-1-carbonitride, and azodibenzoyl; potassium persulfate; and redox catalysts consisting of a combination of a water-soluble catalyst such as ammonium persulfate and a peroxide, or a combination of a persulfate and a reducing agent. Radical polymerization initiators may be used alone or in combination of two or more. In particular, from the viewpoint of storage stability, it is preferable to include at least one organic peroxide.

[0086] The organic peroxide is preferably an organic peroxide containing a peroxy group and a hydrocarbon group, and may further contain a ketone group. Examples of organic peroxides include ketone peroxides such as methyl ethyl ketone peroxide and cyclohexanone peroxide; peroxyketals such as 1,1-di(t-butylperoxy)cyclohexane and 2,2-di(4,4-di(t-butylperoxy)cyclohexyl)propane; hydroperoxides such as p-menthane hydroperoxide, diisopropylbenzene hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide; di(2-t-butylperoxyisopropyl)benzene, dicumyl peroxide, and 2,5-dimethyl-2,5-di(t-butylperoxy Examples include dialkyl peroxides such as hexane, t-butylcumyl peroxide, di-t-hexyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, and di-t-butyl peroxide; diacyl peroxides such as dibenzoyl peroxide and di(4-methylbenzoyl) peroxide; peroxydicarbonates such as di-n-propyl peroxydicarbonate and diisopropyl peroxydicarbonate; and peroxyesters such as 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-hexyl peroxybenzoate, t-butyl peroxybenzoate, and t-butyl peroxy 2-ethylhexanonate.

[0087] From the viewpoint of application to low-temperature processes, it is preferable that the radical polymerization initiator does not contain aromatic rings in its hydrocarbon group. The hydrocarbon group is preferably linear or branched.

[0088] Furthermore, the 10-hour half-life temperature of the radical polymerization initiator can be appropriately adjusted depending on the underfill material filling device used, for example, it may be 90°C or higher, 95°C or higher, or 100°C or higher. If the 10-hour half-life temperature of the radical polymerization initiator is 90°C or higher, the start of the curing reaction of the underfill material will be suppressed even if the substrate filled with underfill material is left in a medium temperature range (for example, on a hot plate stage).

[0089] The 10-hour half-life temperature of the radical polymerization initiator may be 110°C or lower, 95°C or lower, or 90°C or lower. If the 10-hour half-life temperature of the radical polymerization initiator is 95°C or lower, it becomes possible to lower the curing temperature of the underfill material compared to the conventional curing temperature (150-175°C). As a result, package warping can be suppressed.

[0090] The half-life temperature of a specific peroxide is calculated using the following formula (in °C). The half-life temperature is listed in the catalog of commercially available products, so you may refer to that.

[0091]

[0092] τ: Half-life, C: Constant, Ea: Activation energy, R: Gas constant, T: Absolute temperature

[0093] The content of the radical polymerization initiator in the underfill material is not particularly limited. For example, the content of the radical polymerization initiator is preferably 0.1 to 20 parts by mass per 100 parts by mass of the total radical polymerizable compound, and more preferably 0.5 to 10 parts by mass from the viewpoint of curability. When the content of the radical polymerization initiator is 20 parts by mass or less per 100 parts by mass of the total radical polymerizable compound, volatile matter is less likely to be generated and the generation of voids in the cured product tends to be suppressed. In addition, since a rapid increase in radical concentration is suppressed, termination reactions of radical polymerization are less likely to occur, and a long-chain crosslinked structure tends to be obtained. As a result, cracks are less likely to occur in the cured product. Furthermore, when the content of the radical polymerization initiator is 0.3 parts by mass or more per 100 parts by mass of the total radical polymerizable compound, the curability tends to improve.

[0094] [Inorganic Fillers] The underfill material may contain inorganic fillers. Examples of inorganic fillers include silica such as spherical silica, crystalline silica, and fused silica; calcium carbonate, clay, alumina, silicon nitride, silicon carbide, boron nitride, calcium silicate, potassium titanate, aluminum nitride, beryllia, zirconia, zircon, fossterite, steatite, spinel, mullite, titania, and other powders, or beads or glass fibers made from these materials. Furthermore, as inorganic fillers with flame-retardant properties, aluminum hydroxide, magnesium hydroxide, zinc borate, zinc molybdate, etc., may be used. Inorganic fillers may be used individually or in combination of two or more types.

[0095] Among these, silica is preferred from the viewpoint of ease of availability, chemical stability, and material cost, and spherical silica is more preferred from the viewpoint of fluidity and permeability into the fine gaps of the underfill material. Examples of spherical silica include silica obtained by deflagration and fused silica. The inorganic filler may be surface-treated in advance using various surface treatment agents such as silane coupling agents described later.

[0096] The inorganic filler may be alumina, boron nitride, aluminum nitride, silica, magnesium oxide, silicon nitride, silicon carbide, or other highly thermally conductive inorganic fillers. Underfill materials containing these highly thermally conductive inorganic fillers tend to have high viscosity and require long filling times. However, according to the manufacturing method of this disclosure, the filling time can be shortened even when the underfill material contains a highly thermally conductive inorganic filler.

[0097] The volume-average particle size of the inorganic filler is not particularly limited. For example, in the case of spherical silica, the volume-average particle size is preferably 0.1 μm to 10 μm, more preferably 0.2 μm to 7 μm, even more preferably 0.3 μm to 5 μm, and may also be 0.3 μm to 2.0 μm. When the volume-average particle size is 0.1 μm or more, it tends to have excellent dispersibility in the underfill material, is less likely to impart thixotropy to the underfill material, and has excellent flow characteristics. When the volume-average particle size is 10 μm or less, it tends to reduce the sedimentation of the inorganic filler in the underfill material, improve the permeability and fluidity into fine gaps of the underfill material, and prevent voids and unfilled areas. The volume-average particle size of the inorganic filler can be measured as the particle size (D50) when the cumulative amount from the small diameter side reaches 50% in the volume-based particle size distribution measured by a laser diffraction scattering particle size distribution analyzer.

[0098] The inorganic filler content is not particularly limited, but is preferably 20% by mass or more of the total underfill material, more preferably 25% by mass or more, and even more preferably 30% by mass or more. Furthermore, the inorganic filler content is preferably 80% by mass or less of the total underfill material, preferably 75% by mass or less, and even more preferably 70% by mass or less. When the inorganic filler content is 20% by mass or more, the linear thermal expansion coefficient is easily reduced, and when it is 80% by mass or less, the increase in viscosity of the underfill material is easily suppressed, and the fluidity, permeability, and filling properties tend to be good.

[0099] [Surfactants] The underfill material contains surfactants. Examples of surfactants include silicone oil, higher fatty acid esters, phosphate esters, and polyacrylates, with silicone oil being preferred. The silicone oil is preferably a polyether-modified silicone oil, and more preferably a silicone oil having polyether moieties in its side chains. The polyether moieties preferably include at least one selected from the group consisting of ethylene oxy moieties and propylene oxy moieties. The ethylene oxy moieties and propylene oxy moieties may be connected to silicon atoms via linking groups.

[0100] The silicone oil may further have an amine moiety in its side chain.

[0101] The main chain of the silicone oil may be any of dimethylsilicone, diphenylsilicone, and methylphenylsilicone, and is preferably dimethylsilicone.

[0102] The viscosity of the surfactant at 25°C is 500 mm 2 / s to 5000 mm 2 / s, preferably 1000 mm 2 / s to 4500 mm 2 / s, more preferably 1500 mm 2 / s to 4200 mm 2 / s, still more preferably. When the viscosity of the surfactant at 25°C falls within the above range, the exudation state of the surfactant to the interface with the substrate becomes appropriate when the cured product of the underfill material is heated during rework, and the cured product of the underfill material tends to be easily peeled off from the substrate.

[0103] When the surfactant is contained, the content of the surfactant is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, relative to 100 parts by mass of the radically polymerizable compound. Further, from the viewpoint of preventing exudation of the surfactant to the interface with the substrate, the content of the surfactant is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, relative to 100 parts by mass of the radically polymerizable compound.

[0104] [Coupling Agent] The underfill material may contain a coupling agent as needed. When the underfill material contains a coupling agent, it tends to strengthen the interfacial adhesion between the radical polymerizable compound and the inorganic filler, or between the radical polymerizable compound and the components of the electronic component. There are no particular restrictions on the type of coupling agent, and conventionally known ones can be used. Examples include silane compounds having primary and / or secondary and / or tertiary amino groups, epoxysilanes, mercaptosilanes, alkylsilanes, ureidosilanes, vinylsilanes, (meth)acrylsilanes, and various other silane compounds, titanium compounds, aluminum chelates, and aluminum / zirconium compounds. The coupling agent may be used alone or in combination of two or more types.

[0105] As coupling agents, for example, monomers or oligomers may be used. Examples of monomer coupling agents include vinyltrichlorosilane, vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, glycidoxyoctyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, vinyltriacetoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-anilinopropyltrimethoxysilane, γ-anilinopropyltriethoxysilane, γ-(N γ-(N,N-dimethyl)aminopropyltrimethoxysilane, γ-(N,N-diethyl)aminopropyltrimethoxysilane, γ-(N,N-dibutyl)aminopropyltrimethoxysilane, γ-(N-methyl)anilinopropyltrimethoxysilane, γ-(N,N-ethyl)anilinopropyltrimethoxysilane, γ-(N,N-dimethyl)aminopropyltriethoxysilane, γ-(N,N-diethyl)aminopropyltriethoxysilane, γ-(N,N-dibutyl)aminopropyltriethoxysilane, γ-(N-methyl)anilinopropyltriethoxysilane, γ-(N-ethyl)anilinopropyltriethoxysilane, γ-(N,N-dimethyl)aminopropylmethyldimethoxysilane, γ-(N,Silane coupling agents such as N-dibutyl)aminopropylmethyldimethoxysilane, γ-(N-methyl)anilinopropylmethyldimethoxysilane, γ-(N-ethyl)anilinopropylmethyldimethoxysilane, N-(trimethoxysilylpropyl)ethylenediamine, N-(dimethoxymethylsilylisopropyl)ethylenediamine, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, γ-chloropropyltrimethoxysilane, hexamethyldisilazane, vinyltrimethoxysilane, hexenyltrimethoxysilane, octenyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, methacryloxyoctyltrimethoxysilane, etc.; isopropyltriisostearoyl titanate, isopropyltris(dioctylpyrophosphate) titanate, etc. Examples of titanate coupling agents include sopropyltri(N-aminoethyl-aminoethyl)titanate, tetraoctylbis(ditridecylphosphite)titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecylphosphite)titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, bis(dioctyl pyrophosphate)ethylene titanate, isopropyltrioctanoyltitanate, isopropyldimethacrylateisostearoyltitanate, isopropyltridodecylbenzenesulfonyltitanate, isopropylisostearoyldiacrylictitanate, isopropyltri(dioctylphosphate)titanate, isopropyltricumylphenyl titanate, and tetraisopropylbis(dioctylphosphite)titanate.

[0106] Furthermore, examples of oligomer coupling agents include methyl-based, methyl / phenyl-based, propyl / phenyl-based, epoxy-modified, mercapto-modified, amine-modified, (meth)acrylic-modified, or polyester resin-modified alkoxy oligomers.

[0107] The content of the coupling agent in the underfill material is not particularly limited. From the viewpoint of adhesion, fluidity, etc., the content of the coupling agent is preferably 0.01% to 20% by mass, and more preferably 0.01% to 10% by mass, relative to the total amount of radical polymerizable compounds.

[0108] [Other Components] In addition to the components mentioned above, the underfill material may contain various additives such as flexible agents, catalysts, and ion exchangers. The underfill material may also contain various additives known in the art, as needed, in addition to the additives exemplified below.

[0109] (Flexible Agent) The underfill material may contain a flexible agent from the viewpoint of improving thermal shock resistance and reducing stress on semiconductor elements. The type of flexible agent is not particularly limited, and those commonly used in this field, such as silicone rubber, acrylic elastomer, and phenoxy resin, may be used. Among these, rubber particles are preferred as the flexible agent. Examples of rubber particles include styrene-butadiene rubber (SBR), nitrile-butadiene rubber (NBR), butadiene rubber (BR), urethane rubber (UR), and acrylic rubber (AR). One type of flexible agent may be used alone, or two or more types may be used in combination.

[0110] (Catalyst) To promote the condensation reaction of the coupling agent and the reaction between the silanol groups in the coupling agent and the silanol groups of the inorganic filler such as silica, thereby improving the dispersibility of the inorganic filler and lowering the viscosity of the underfill material, a catalyst such as a proton-supplying acid or Lewis acid may be added. Among these, a chelating agent containing a metal species is preferred as the Lewis acid from the viewpoint of storage stability. Examples of chelating agents containing a metal species include aluminum, boron, cobalt, and titanium. The Lewis acid content is preferably 0.001 parts by mass to 1.0 part by mass, more preferably 0.002 parts by mass to 0.8 parts by mass, and even more preferably 0.005 parts by mass to 0.6 parts by mass per 100 parts by mass of the inorganic filler.

[0111] (Ion Exchanger) The underfill material may contain an ion exchanger as needed. When the underfill material contains an ion exchanger, the migration resistance, moisture resistance, and high-temperature storage characteristics of semiconductor devices such as ICs tend to improve. Examples of ion exchangers include compounds represented by the following compositional formulas (A) or (B): Mg 1-X Al X (OH) 2 (CO 3 ) X / 2 mH 2 O ... (A) (0 < X ​​≤ 0.5, m is a positive number) Bio x (OH) y (NO 3 ) z  ...(B) (0.9≦x≦1.1, 0.6≦y≦0.8, 0.2≦z≦0.4)

[0112] The amount of ion exchanger added is preferably 0.1% to 3.0% by mass, and more preferably 0.3% to 1.5% by mass. The volume-average particle size of the ion exchanger is preferably 0.1 μm to 3.0 μm. The volume-average particle size of the ion exchanger can be measured as the particle size (D50) when the cumulative amount from the smallest diameter side reaches 50% in the volume-based particle size distribution measured by a laser diffraction scattering particle size distribution analyzer. The maximum particle size of the ion exchanger is preferably 10 μm.

[0113] An example of the compound represented by formula (A) above is the commercially available DHT-4A (manufactured by Kyowa Chemical Industry Co., Ltd., trade name). An example of the compound represented by formula (B) above is the commercially available IXE500 (manufactured by Toagosei Co., Ltd., trade name). In addition, other anion exchangers may be added as needed. The type of anion exchanger is not particularly limited, and conventionally known ones can be used. For example, hydrated oxides of elements selected from magnesium, aluminum, titanium, zirconium, antimony, etc. Anion exchangers may be used individually or in combination of two or more types.

[0114] (Other additives) The underfill material may contain other additives as needed, such as polymerization inhibitors, dyes, colorants such as carbon black, diluents, leveling agents, and defoamers.

[0115] (Polymerization inhibitors) Examples of polymerization inhibitors include phenolic compounds such as hydroquinone, methylhydroquinone, hydroquinone monomethyl ether, catechol, and pyrogallol; and hindered amine compounds.

[0116] [Method for preparing underfill material] The resin liquid composition may be prepared by any method as long as the various components can be uniformly dispersed and mixed. For example, it can be obtained by weighing the components, mixing and kneading them using a mixer, mixing roll, planetary mixer, etc., and degassing as necessary.

[0117] [Physical Properties of Underfill Material] (Viscosity) From the viewpoint of fluidity, the viscosity of the underfill material is preferably 100 Pa·s or less, more preferably 50 Pa·s or less, and even more preferably 30 Pa·s or less at 25°C. The viscosity of the underfill material at 25°C is measured using an EHD type rotational viscometer. Specifically, it can be measured by the method described in the examples.

[0118] Furthermore, from the viewpoint of filling properties when filling narrow gaps with underfill material at temperatures around 50°C to 100°C for applications such as underfill material, the viscosity of the underfill material at 80°C is preferably, for example, 1 Pa·s or less, and more preferably 0.5 Pa·s or less. The viscosity of the underfill material at 80°C is measured using a rheometer. Specifically, it can be measured by the method described in the examples.

[0119] (Heat generation) The heat generation of the underfill material is not particularly limited. From the viewpoint of increasing the crosslinking density and preventing cracks, the heat generation of the underfill material is preferably 60 J / g or more, more preferably 70 J / g or more, and even more preferably 80 J / g or more. The heat generation of the underfill material is measured using a differential scanning calorimeter. Specifically, it can be measured by the method described in the examples.

[0120] (Temperature at the peak of the exothermic reaction) The temperature at the peak of the exothermic reaction of the underfill material (hereinafter also referred to as the "exothermic reaction peak temperature") is not particularly limited. From the viewpoint of enabling processing at low temperatures, the exothermic reaction peak temperature of the underfill material is preferably 160°C or lower, more preferably 150°C or lower, and even more preferably 140°C or lower. Furthermore, from the viewpoint of suppressing viscosity increase during filling, the exothermic reaction peak temperature of the underfill material is preferably 90°C or higher, more preferably 95°C or higher, and even more preferably 100°C or higher. The exothermic reaction peak temperature of the underfill material is measured using a differential scanning calorimeter. Specifically, it can be measured by the method described in the examples.

[0121] (Onset Temperature of Heat Generation Peak) The onset temperature of the heat generation peak of the underfill material (hereinafter also referred to as the "heat generation onset temperature") is not particularly limited. From the viewpoint of enabling processing at low temperatures, the heat generation onset temperature of the underfill material is preferably 150°C or lower, more preferably 140°C or lower, and even more preferably 130°C or lower. Furthermore, from the viewpoint of suppressing viscosity increase during filling, the heat generation onset temperature of the underfill material is preferably 80°C or higher, more preferably 85°C or higher, and even more preferably 90°C or higher. The heat generation onset temperature of the underfill material is measured using a differential scanning calorimeter. Specifically, it can be measured by the method described in the examples.

[0122] [Physical Properties of Cured Underfill Material] In the measurement of the heat generation, linear thermal expansion coefficient, elastic modulus, fracture energy, and glass transition temperature of the cured underfill material described below, the cured material shall be assumed to be obtained by heating the underfill material at 120°C for 2 hours.

[0123] (Heat Generation) The progress of curing of the underfill material can be determined from the amount of heat generated by the underfill material after curing. From the viewpoint of suppressing tack and changes in physical properties after curing of the cured material, the amount of heat generated by the cured material is preferably 10% or less, more preferably 8% or less, and even more preferably 5% or less compared to the amount of heat generated before curing. The amount of heat generated by the cured underfill material is measured using a differential scanning calorimeter. Specifically, it can be measured by the method described in the examples.

[0124] (Linear Thermal Expansion Coefficient) The linear thermal expansion coefficient of the underfill material when it is cured is not particularly limited. For example, the linear thermal expansion coefficient (CTE1) obtained by measuring the temperature increase from 0°C to 300°C at 5°C / min using the compression method, and measuring it as the slope of the tangent between 10°C and 30°C, is preferably 35 ppm / K or less, more preferably 32 ppm / K or less, even more preferably 30 ppm / °C or less, and particularly preferably 28 ppm / K or less. When the CTE1, which is the linear thermal expansion coefficient below the glass transition temperature, is 35 ppm / K or less, the occurrence of bump cracks during reflow tends to be suppressed and the temperature cycle resistance characteristics tend to improve. The linear thermal expansion coefficient of CTE1 may be 15 ppm / K or more.

[0125] Furthermore, the linear thermal expansion coefficient (CTE2), determined by measuring the temperature increase from 0°C to 300°C at 5°C / min using the compression method, is preferably 130 ppm / K or less, more preferably 115 ppm / K or less, and even more preferably 100 ppm / K or less. When the CTE2, which is the linear thermal expansion coefficient above the glass transition temperature, is 115 ppm / K or less, the sealing portion tends to become even less likely to peel off from the substrate.

[0126] (Modulus of Elasticity) The modulus of elasticity of the underfill material when it is cured is not particularly limited. For example, from the viewpoint of reducing warping, the modulus of elasticity of the underfill material when it is cured is preferably 5.0 GPa or higher at room temperature (25°C), more preferably 5.5 GPa or higher, and even more preferably 6.0 GPa or higher. Also, from the same viewpoint, the modulus of elasticity of the underfill material when it is cured is preferably 0.5 GPa or higher at 240°C, more preferably 0.75 GPa or higher, and even more preferably 1.0 GPa or higher.

[0127] Furthermore, from the viewpoint of improving conformability to substrates, etc., by lowering the elastic modulus, for example, the elastic modulus at room temperature (25°C) when the underfill material is cured is preferably 8.0 GPa or less, more preferably 7.5 GPa or less, and even more preferably 7.0 GPa or less. From a similar viewpoint, the elastic modulus at 240°C when the underfill material is cured is preferably 1.25 GPa or less, more preferably 1.00 GPa or less, and even more preferably 0.75 GPa or less.

[0128] The elastic modulus of the underfill material after curing can be measured by DMA (dynamic viscoelasticity measurement). Specifically, it can be measured by the method described in the examples.

[0129] (Glass Transition Temperature) The glass transition temperature (Tg) of the underfill material when it is cured is not particularly limited, but is preferably 60°C or higher, more preferably 70°C or higher, and even more preferably 80°C or higher. When the glass transition temperature is 60°C or higher, the protection of bumps at high temperatures is high and wire breakage tends to occur less easily. The glass transition temperature of the cured underfill material can be measured by DMA (dynamic viscoelasticity measurement). Specifically, it can be measured by the method described in the examples.

[0130] <Curing Process> In the curing process, after or immediately after the filling of the gaps in the underfill material is complete, the underfill material is heated to a temperature higher than the temperature at which radical generation from the radical polymerization initiator is suppressed (curing temperature) to cure it.

[0131] The curing temperature should be higher than the temperature at which radical generation from the radical polymerization initiator is suppressed. Specifically, it is preferably 10°C or more higher than the 10-hour half-life temperature of the radical polymerization initiator, more preferably 15°C or more higher, and even more preferably 20°C or more higher.

[0132] The difference between the filling temperature and the curing temperature is not particularly limited. From the viewpoint of suppressing viscosity increase during filling while ensuring sufficient curing, the difference between the filling temperature and the curing temperature is preferably 20°C or more, more preferably 30°C or more, and even more preferably 40°C or more.

[0133] The specific curing temperature varies depending on the half-life temperature of the radical polymerization initiator. For example, it may be 100°C or higher, 120°C or higher, 140°C or higher, or 160°C or higher. In light of the recent trend towards carbon neutrality and the need to accommodate lower-temperature processes, the curing temperature can be set to 130°C or lower, 125°C or lower, or 120°C or lower by selecting the type of radical polymerization initiator.

[0134] <Application Examples> The manufacturing method of electronic component devices of this disclosure can be applied to semiconductor devices with bare chip mounting, semiconductor devices with flip-chip connections, etc. In particular, since the manufacturing method of electronic component devices of this disclosure can suppress viscosity increase during filling, it can be suitably applied to large-area electronic component devices and electronic component devices with narrow gaps.

[0135] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0136] <Preparation of Underfill Material> The components used in the underfill material of the examples and comparative examples are shown below.

[0137] Radical polymerizable compound 1: 4,4'-diphenylmethanedimaleimide; Radical polymerizable compound 2: 1,6'-bismaleimide-(2,2,4-trimethyl)hexane; Radical polymerizable compound 3: The polymaleimide resin (A1) mentioned above; a polymaleimide resin in which an aromatic ring substituted with one hydrocarbon group having 1 to 18 carbon atoms is bonded to the nitrogen atom of a maleimide group. Radical polymerizable compound 3 was prepared according to Example 1 of Japanese Patent Application Publication No. 2024-4392, and then the solvent was removed in a vacuum dryer heated to 70°C for 6 hours until the solid content concentration was 95% or higher. The solid content concentration was calculated from the weight change rate before and after heating by heating the material after the solvent was removed in an oven at 175°C for 1 hour. Radical polymerizable compound 4: Tripropylene glycol diacrylate Radical polymerizable compound 5: Tricyclodecanedimethanol dimethacrylate Radical polymerizable compound 6: Tricyclodecanedimethanol diacrylate Radical polymerizable compound 7: 4-Hydroxybutyl acrylate

[0138] • Epoxy resin 1: Bisphenol F type epoxy resin (epoxy equivalent 160 g / eq) • Epoxy resin 2: Aminophenol type epoxy resin (epoxy equivalent 98 g / eq) • Curing agent 1: Amine curing agent (active hydrogen equivalent 45 g / eq) • Curing agent 2: Diethyldiaminodiphenylmethane (active hydrogen equivalent: 63 g / eq)

[0139] • Surfactant 1: Dimethyl silicone oil having polyether and amine moieties in its side chain (viscosity 3300 mm at 25°C) 2 / s) • Surfactant 2: Phosphate ester-based wetting and dispersing agent

[0140] • Peroxide 1: t-butyl peroxyl laurate (1-hour half-life temperature 118.2°C, 10-hour half-life temperature 98.3°C) • Peroxide 2: di-t-butyl peroxide (1-hour half-life temperature 144.1°C, 10-hour half-life temperature 123.7°C)

[0141] • Inorganic filler 1: Silica particles (average particle size: 0.5 μm) The volume-average particle size of the above inorganic filler is the median diameter (D50). This volume-average particle size was measured using a laser diffraction scattering particle size analyzer.

[0142] Coupling agent 1: 3-glycidoxypropyltrimethoxysilane; Coupling agent 2: γ-methacryloxypropyltrimethoxysilane

[0143] Each component was blended in the composition (parts by mass) shown in Table 1 or Table 2, and after kneading and dispersing using a three-roll mill and a vacuum grinder, the underfill materials for the examples and comparative examples were prepared.

[0144] <Differential Scanning Calorimetry of Underfill Material> The underfill material was placed in a differential scanning calorimeter (DSC) (TA Instruments "DSC Q200") and heated from 25°C to 500°C at a heating rate of 10°C / min to obtain a DSC curve. The temperature at the rise point of the exothermic peak from the baseline (onset) and the temperature at the top of the exothermic peak (top) were determined. Furthermore, the peak area of ​​the exothermic peak was determined from the DSC curve using a method compliant with JIS K7122:2012, and the amount of heat generated was calculated as the transition heat.

[0145] <Viscosity Measurement of Underfill Material> The viscosity of the underfill material at 25°C and 80°C was measured using a rheometer (TA Instruments "ARES G2").

[0146] <Pot life at 25°C> The viscosity at 25°C after mixing was measured and defined as the initial viscosity. Then, the mixture was stored at 25°C for a predetermined time, and the viscosity at 25°C after storage was measured. The viscosity increase rate was then calculated according to the following formula: Viscosity increase rate = (Viscosity after predetermined storage time - Initial viscosity) / Initial viscosity × 100 If the viscosity increase rate after one week of storage is 50% or less, the pot life is judged to be one week or more and evaluated as A. If the viscosity increase rate after one week of storage is more than 50%, the pot life is judged to be less than one week and evaluated as B.

[0147] <Long-term filling capability> The rheometer measuring jig was heated to the same temperature as the filling temperature shown in Table 2, and the underfill material was dropped onto it. The viscosity was continuously measured while maintaining the filling temperature, and the change in viscosity over time at the filling temperature was measured. The viscosity increase rate was then calculated according to the following formula: Viscosity increase rate = (Viscosity after holding at the filling temperature for 30 minutes - Initial viscosity at the filling temperature) / (Initial viscosity at the filling temperature) × 100 If the viscosity increase rate after holding for 30 minutes is 100% or less, it is judged that filling is possible for 30 minutes and is evaluated as A. If the viscosity increase rate after holding for 30 minutes is more than 100%, it is judged that filling is not possible for 30 minutes and is evaluated as B.

[0148] <Differential Scanning Calorimetry of Cured Materials> Test specimens were prepared by curing underfill material at 120°C for 2 hours. These specimens were placed in a differential scanning calorimeter (DSC) (TA Instruments "DSC Q200") and heated from 25°C to 500°C at a heating rate of 10°C / min to obtain a DSC curve. The peak area of ​​the exothermic peak was determined from the DSC curve according to the method in accordance with JIS K7122:2012, and the amount of heat generated was calculated as the transition heat.

[0149]

[0150]

[0151]

[0152]

[0153] In Comparative Example 1, the curing agent content (equivalent ratio) represents the number of functional groups (eq) in the curing agent when the number of epoxy groups in the epoxy resin is set to 1. The inorganic filler content represents the amount of inorganic filler relative to the total amount of the composition (mass %).

[0154] As shown in Tables 3 and 4, Examples 1 to 7 maintain a low viscosity during filling for a longer period compared to Comparative Example 1. Furthermore, Examples 1 to 7 exhibit superior storage stability at 25°C compared to Comparative Example 1.

[0155] The disclosure of Japanese Patent Application No. 2025-077585 is incorporated in its entirety by reference. All documents, patent applications, and technical standards in this disclosure are incorporated by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually noted to be incorporated by reference.

Claims

1. A method for manufacturing an electronic component device, comprising: filling the gap between an electronic component and a substrate electrically connected to the electronic component via a connector with an underfill material containing a radical polymerizable compound and a radical polymerization initiator at a temperature at least 10°C lower than the 10-hour half-life temperature of the radical polymerization initiator; and curing the underfill material by heating it to a temperature at least 10°C higher than the 10-hour half-life temperature of the radical polymerization initiator after or immediately after the underfill material has been filled into the gap.

2. The method for manufacturing an electronic component device according to claim 1, wherein the radical polymerizable compound comprises at least one selected from the group consisting of (meth)acrylic compounds and maleimide compounds.

3. A method for manufacturing an electronic component device according to claim 1 or 2, wherein the device does not contain any polymerizable compounds other than radical polymerizable compounds, or the content of other polymerizable compounds relative to the total amount of other polymerizable compounds and radical polymerizable compounds is 20% by mass or less.

4. The method for manufacturing an electronic component device according to claim 1 or 2, wherein the radical polymerization initiator comprises a peroxide having a 10-hour half-life temperature of 90°C to 110°C.

5. The method for manufacturing an electronic component device according to claim 1 or 2, wherein the underfill material further comprises an inorganic filler.

6. The method for manufacturing an electronic component device according to claim 5, wherein the underfill material contains 20% by mass or more of the inorganic filler.