Resin composition and method for producing resin composition

A resin composition with specific pulp and powdered cellulose ratios and processing methods enhances mechanical and impact strength while improving fluidity, resolving moldability and workability challenges in fiber-reinforced resins.

WO2026234915A1PCT designated stage Publication Date: 2026-11-12NIPPON PAPER IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/012248
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-03-26
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing resin compositions containing high amounts of plant fibers with a large aspect ratio suffer from deteriorated fluidity due to fiber entanglement, leading to reduced moldability and workability.

Method used

A resin composition comprising pulp fibers with an average aspect ratio of 10 or more and powdered cellulose with an average L/D ratio of less than 10, combined in a specific proportion, along with a method of mixing and heating to achieve a balance of high mechanical strength, impact strength, and fluidity.

Benefits of technology

The composition achieves a good balance of mechanical strength and impact strength while maintaining excellent fluidity, addressing the moldability and workability issues of previous resin compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

A resin composition comprising a plurality of cellulose materials, wherein the cellulose material is characterized by containing at least component A: pulp fibers having an average aspect ratio of 10 or more, and component B: powder cellulose having an average L / D (major axis / minor axis ratio) of less than 10.
Need to check novelty before this filing date? Find Prior Art

Description

Resin Composition and Method for Producing Resin Composition

[0001] The present invention relates to a resin composition and a method for producing the resin composition.

[0002] Biomass resources have been attracting attention from the perspectives of utilizing sustainable forest resources, reducing emissions of global warming substances and environmentally burdensome substances, and achieving weight reduction.

[0003] Studies have been conducted to produce fiber-reinforced resins by combining plant fibers, which are such biomass resources, with thermoplastic resins. For example, Patent Document 1 proposes obtaining a resin composition with excellent properties such as mechanical strength (flexural modulus, flexural strength), impact strength, and linear expansion coefficient by combining such plant fibers and thermoplastic resins, and its deployment in various applications is expected.

[0004] International Publication No. 2023 / 233955

[0005] However, properties such as mechanical strength are also affected by the content of plant fibers, and when a large amount of plant fibers with a large aspect ratio is contained in the resin composition, there is a concern that the fluidity deteriorates due to entanglement of fibrous materials, which lowers the moldability and workability of the resin composition.

[0006] Accordingly, an object of the present invention is to provide a resin composition that has high mechanical strength and impact strength while also having an excellent balance in fluidity.

[0007] The inventors of this application have, through diligent effort, found that the problem can be solved by the following configurations (1) to (6): (1) A resin composition comprising a plurality of cellulose materials, wherein the cellulose material comprises at least: Component A: pulp fibers having an average aspect ratio of 10 or more, and Component B: powdered cellulose having an average L / D (major axis / minor axis ratio) of less than 10. (2) The resin composition according to (1), wherein Component A has an average kink angle of 55 degrees or more. (3) The resin composition according to (1), wherein Component B has a particle size distribution span in the range of 1.5 to 9. (4) The resin composition according to any one of (1) to (3), wherein the total amount of Component A and Component B is 80% by mass or more of the total mass of the cellulose material, and the content satisfies the condition that Component A ≥ Component B. (5) The resin composition according to any one of (1) to (3), wherein the cellulose material is contained in the resin composition in the range of 5 to 35% by mass. (6) A method for producing a resin composition comprising a plurality of cellulose materials and a thermoplastic resin, wherein the cellulose material comprises at least: Component A: pulp fibers having an average aspect ratio of 10 or more, and Component B: powdered cellulose having an average L / D (long axis / short axis ratio) of less than 10, wherein Component A is obtained by crushing pulp, and Component B is obtained by grinding pulp, and the method for producing a resin composition is characterized by mixing Component A, Component B and the thermoplastic resin and then heating and kneading.

[0008] According to the present invention, it is possible to provide a resin composition that has a good balance of high mechanical strength and impact strength while also having excellent fluidity.

[0009] The present invention will be described in detail below with reference to its preferred embodiments. In this specification, the notation "AA to BB" refers to AA to BB.

[0010] In other words, the present invention is a resin composition comprising a plurality of cellulose materials, wherein the cellulose material comprises at least component A: pulp fibers having an average aspect ratio of 10 or more, and component B: powdered cellulose having an average L / D (long axis / short axis ratio) of less than 10.

[0011] <Component A: Pulp Fiber> For component A of the present invention, it is important to use pulp fibers with an average aspect ratio of 10 or more, preferably 10 or more and less than 100, more preferably 20 or more and less than 90, and even more preferably 30 or more and less than 80. When the average aspect ratio satisfies the above range, an excellent effect in expressing the function of a reinforcing material in the resin composition can be obtained.

[0012] The average aspect ratio of pulp fibers can be calculated from the (length-weighted) average fiber length and (length-weighted) average fiber diameter using the following formula: Average aspect ratio = Average fiber length / Average fiber diameter

[0013] Furthermore, the average fiber length and average fiber diameter can be measured using a Lorentzen & Wettre fiber tester after the pulp has been thoroughly disintegrated in water.

[0014] Such pulp fibers are preferably such that the proportion of pulp fibers with a fiber length of 0.2 mm or less in the total pulp fibers is 35% by mass or less, and the average kink angle is 55 degrees or more. In this specification, pulp fibers with a fiber length of 0.2 mm or less may be referred to as "fine fibers".

[0015] In the present invention, the proportion of fine fibers in the total pulp fibers is 45% by mass or less, preferably 40% by mass or less, more preferably 35% by mass or less, more preferably 30% by mass or less, more preferably 27% by mass or less, and even more preferably 24% by mass or less, in order to exhibit the reinforcing effect of the long fibers. If the proportion of fine fibers is too high, the reinforcing effect may be reduced. The lower limit of the proportion of fine fibers is preferably 0.1% by mass or more, and more preferably 1% by mass or more. The proportion of fine fibers can be measured after the pulp has been sufficiently disintegrated in water, for example, using a fiber tester manufactured by Lorentzen & Wettre.

[0016] The pulp fibers used in this invention have an average kink angle of 55 degrees or more, preferably 58 degrees or more and 150 degrees or less, and more preferably 60 degrees or more and 120 degrees or less, in order to serve as the starting point for void formation that absorbs energy when subjected to stress. Although the details are unclear, it is thought that when the resin-pulp fiber interface peels off, the bending of the fibers makes it easier for fine voids to form around them, and these voids contribute to the improvement of impact strength. If the average kink angle is too small, energy absorption may not be effective and the impact strength may decrease. Also, if the average kink angle is too large, it may be considered similar to fibers with a low aspect ratio and may not exhibit the sufficient reinforcing effect expected of long fibers. In this invention, the kink angle refers to the angle of bending from the position where the fiber was straight. The average kink angle is the average value indicating the degree of bending of a straight fiber, and is, for example, the average value of the angles defined in Olson, J et al., "An Analyzer for Fiber Shape and Length" (Journal of Pulp and Paper Science, Vol. 21, No. 11, 1995, pp. J367-J373). The average kink angle of the present invention can be measured after the pulp has been sufficiently disintegrated in water, for example, using a fiber tester manufactured by Lorentzen & Wettre.

[0017] Such pulp fibers can be obtained, for example, by a method that includes a step of crushing pulp. Specifically, they can be obtained by stirring in water, preferably at a low temperature, with a relatively high pulp solids content concentration, preferably 10% by mass or more, more preferably 20% by mass or more. If the beating treatment is performed with a relatively low pulp solids content concentration, or if the nano-processing is performed excessively, the proportion of fines becomes, for example, more than 30%, which is undesirable. In this application, the pulp solids content concentration is calculated from the mass of pulp and water using the following formula: Pulp solids content concentration (%) = Mass of pulp solids / (Mass of water + Mass of pulp solids) × 100

[0018] In the present invention, the proportion of long fibers (hereinafter also referred to as "long fiber portion") in the total pulp fibers is preferably 45% by mass or more, more preferably 50% by mass or more, and even more preferably 55% by mass or more. If the proportion of long fibers is too low, there is a risk that the effect of improving impact strength and the effect of improving maximum stress will be reduced. There is no particular upper limit to the proportion of long fibers, but in reality it is 100% by mass or less. Here, long fibers in this specification refer to pulp fibers with a fiber length of 0.5 mm or more. The proportion of long fibers can be calculated by measuring the fiber length distribution of pulp fibers using, for example, a fiber tester manufactured by Lorentzen & Wettre after the pulp has been sufficiently disintegrated in water.

[0019] (Pulp Raw Materials) Pulp raw materials are broadly classified into wood pulp and non-wood pulp, depending on the raw materials used. Wood pulp can be produced by pulping wood raw materials. Examples of wood raw materials include coniferous trees such as Japanese red pine, Japanese black pine, Sakhalin fir, Yezo spruce, red pine, Japanese larch, fir, hemlock, Japanese cedar, Japanese cypress, Japanese larch, fir, spruce, Japanese cedar, Douglas fir, hemlock, white fir, spruce, balsam fir, cedar, pine, Merkus fir, and radiata pine, as well as mixtures thereof; and broad-leaved trees such as beech, birch, alder, oak, Machilus thunbergii, Castanopsis sieboldii, white birch, poplar, ash, willow, eucalyptus, mangrove, lauan, and acacia, as well as mixtures thereof.

[0020] The method of pulping wood raw materials is not particularly limited, and examples include pulping methods commonly used in the paper industry. Wood pulp can be classified by pulping method, and examples include chemical pulp obtained by pulping using methods such as the kraft process, sulfite process, soda process, and polysulfide process; mechanical pulp obtained by pulping using mechanical force such as a refiner or grinder; semi-chemical pulp obtained by pulping using mechanical force after chemical pretreatment; recycled paper pulp; and deinked pulp. Wood pulp may be in an unbleached (pre-bleached) state or in a bleached (post-bleached) state.

[0021] Examples of non-wood-derived raw materials include cotton, hemp, sisal, Manila hemp, flax, straw, bamboo, bagasse, kenaf, sugarcane, corn, rice straw, paper mulberry, and paperbush.

[0022] In particular, the characteristics of the average aspect ratio and kink angle in this invention suggest the influence of factors such as cell wall thickness and lignin content, as well as the characteristics of fiber length suggest the influence of multiple factors originating from the characteristics of the tree species and individual wood used as raw material, such as the fiber length specific to the tree species and the crystallinity of those fibers. However, from the viewpoint of fiber characteristics after pulping, it is preferable to use wood raw materials as pulp raw materials that are mainly from the Myrtaceae family (Eucalyptus genus), the Pinaceae family (Larch, Pine, Toga, and Spruce genus), the Cupressaceae family (Cryptomeria japonica, Cunninghamia genus, and Chamaecyparis genus), which have a wide distribution of habitats and possess diverse genetic resources, and that have obtained forest certification and are used for papermaking. These forest-certified pulp raw materials for papermaking are preferable because they are based on selected trees bred and selected through the crossbreeding of diverse genetic resources over many years by humankind, resulting in less variability between individuals in the various characteristics of the wood raw material, and because they utilize tree species that stably express the above-mentioned fiber characteristics through breeding, and are produced through renewable and sustainable management. As such wood raw materials, the genus Eucalyptus of the Myrtaceae family includes Eucalyptus calophila, E. citriodora, E. diversi color, E. globulus, E. grandis, E. gummifera, E. marginata, E. nesophylla, E. nitens, E. macarthurii, E. fastigata, E. amygdalina, E. camaldulensis, E. delegatensis, E. gigantea, E. muelleriana, E. obliqua, E. regnans, E. sieberiana, E. viminalis and the like.Examples of species in the genus Larix (hereinafter abbreviated as L.) of the family Pinaceae include Larix leptolepis, L. laricina, L. occidentalis, L. decidua, and L. gmelinii; examples of species in the genus Pinus (hereinafter abbreviated as P.) of the family Pinaceae include Pinus radiata; examples of species in the genus Pseudotsuga (Pseudotsuga menziesii) and Pseudotsuga japonica; and examples of species in the genus Picea (Picea mariana), Picea sitcheensis, and Picea abies. Furthermore, examples of species in the genus Cryptomeria (Cupressaceae) include Cryptomeria japonica, examples of species in the genus Cunninghamia (Cupressaceae) include Cunninghamia lanceolata, and examples of species in the genus Chamaecyparisobuse (Cupressaceae) include Chamaecyparisifera. Examples of species in the genus Acacia (Fabaceae) include Acacia mangium. Among these, E. globalus and E. grandis of the genus Eucalyptus (Myrtaceae), P. radiata of the genus Pinus (Pinaceae), and A. mangium of the genus Acacia (Fabaceae) are preferred because they are tree species that have been bred for many years, are highly diverse, and make it easy to obtain wood pulp raw materials as in the present invention. In this invention, for example, when referring to a pulp raw material mainly composed of eucalyptus, it means that eucalyptus is present in an amount of 51% by mass or more of the pulp raw material.

[0023] Furthermore, the pulp fibers used in the present invention may be subjected to a modification treatment to impart hydrophobicity. Known methods for imparting hydrophobicity include (1) directly hydrophobicizing pulp fibers by introducing various hydrocarbon groups, etc., by etherification, esterification, dithioesterification, etc., of the hydroxyl groups of cellulose, and (2) indirectly hydrophobicizing pulp fibers by introducing ionic functional groups such as carboxyl groups, phosphate groups, phosphite groups, and amino groups to the hydroxyl groups of cellulose through oxidation, etherification, esterification, carbamate, etc., and then introducing various hydrocarbon groups, etc., to these functional groups through direct ionic bonding, ionic bonding via metal ions, etc., or covalent bonding such as amide bonds and ester bonds. While these hydrophobicization treatments improve dispersibility in the resin composition and enhance various physical properties such as mechanical strength, there are concerns such as a decrease in crystallinity, an increase in the number of steps, and the generation of VOCs when compounds used in the modification treatment remain.

[0024] In this invention, the effects can be achieved even without using these modified pulp fibers, but the pulp fibers may be modified before use in order to adjust their physical properties.

[0025] The pulp used to obtain the resin composition of the present invention may be hydrated pulp or dry pulp. From the viewpoint of stable production, it is preferable that the dry pulp is subjected to processing such as crushing or pulverizing before being used in the production of the resin composition. The pulverizing method can be the same as the pulverizing treatment for powdered cellulose described later.

[0026] <Component B: Powdered Cellulose> The powdered cellulose of the present invention preferably has the following physical properties, and usually has at least a predetermined average L / D among the following physical properties. This makes it possible to reduce fiber entanglement in the resin composition and improve fluidity while maintaining the physical properties of the resin composition.

[0027] (Longest diameter / shortest diameter ratio (average L / D)) The longest diameter / shortest diameter ratio (average L / D) of powdered cellulose is important to be less than 10, preferably 2.0 to 7.0, more preferably 3.0 to 7.0, and even more preferably 3.0 to 6.0.

[0028] The average L / D ratio is presumed to influence the shape of the powdered cellulose and can be considered an indicator that comprehensively represents the particle shape (spherical, rod-shaped, bent rod-shaped, etc.) and fiber aggregation state of the powdered cellulose. If the average L / D ratio is within the preferred range described above, it is possible to select appropriate powdered cellulose that has a suitable fiber length and fiber width and exhibits minimal fiber entanglement when incorporated into a resin composition.

[0029] The average L / D is calculated under the following conditions: Using an optical microscope, powdered cellulose is observed at 100x magnification, and the L and D values ​​of 140 randomly selected powdered cellulose samples are measured. The L / D ratio for each sample is then calculated as the average value of 100 powdered cellulose samples, excluding the top and bottom 20 values ​​from the calculated L / D ratios. The major axis (L) refers to the maximum fiber width of the powdered cellulose observed with an optical microscope. The minor axis (D) refers to the minimum value perpendicular to the major axis of the powdered cellulose fiber width observed with an optical microscope. When the powdered cellulose has a bent structure, L is the maximum fiber width in the bent state. L is usually 35 or more, preferably 40 or more, and more preferably 41 or more. The upper limit is usually 60 or less, preferably 55 or less, and more preferably 53 or less. D is usually 6 or more, preferably 7 or more, and more preferably 8 or more. The upper limit is not particularly limited, and may be 15 or less. It is preferable that L is within the above range along with the average L / D, as this further reduces fiber entanglement in the resin composition. The average L / D is measured after confirming that the powder moisture content of the powdered cellulose, measured with an infrared moisture meter (Kett Scientific Instruments, FD-720 model, 1 g, 105°C), is 3.0 to 4.0%.

[0030] (Average fiber length (μm), average fiber width (μm), aspect ratio) The average fiber length of powdered cellulose is preferably 40 to 100 μm, and more preferably 50 to 90 μm. An average fiber length of 40 to 100 μm allows for appropriate fluidity to be maintained when kneaded with resin.

[0031] The average fiber width of powdered cellulose is typically 10 μm or more, preferably 15 μm or more, and more preferably 20 μm or more. The upper limit is typically 50 μm or less, preferably 40 μm or less, and more preferably 35 μm or less. If the average fiber width is too small, at the nano-order level, the manufacturing cost increases, and the size effect in the nano region increases the specific surface area, which may restrict the surrounding resin and adversely affect fluidity.

[0032] The average fiber length / average fiber width (aspect ratio) of powdered cellulose is preferably 1.0 to 7.0.

[0033] The average fiber length and average fiber width of powdered cellulose were measured using the L&W Fiber Tester Plus (manufactured by ABB) according to the following procedure.

[0034] 0.1 g of the sample was placed in a cylinder containing 200 mL of pure water, stirred for about 1 minute, then transferred to a dedicated 300 mL beaker, set in a sample cycler, and measurement was started. Measurement was continued until more than 55,000 fibers with a fiber length of 0.1 mm or longer were counted. The length-weighted fiber length and width-weighted fiber width were determined and used as the average fiber length and average fiber width of the sample. The measurement was performed after setting the Max value of Fines Limit to 0.0 and the Min value of Length class 1 to 0.001 on the Sample type screen where the measurement conditions are defined. The aspect ratio was calculated by dividing the obtained average fiber length by the average fiber width.

[0035] While the aforementioned average L / D and aspect ratio are similar indices derived from the relationship between fiber length and fiber width, the powdered cellulose used in the present invention is a rod-shaped particulate material, and the average L / D excludes values ​​above and below 20, thus representing a more average shape. Therefore, the average L / D is more suitable as an indicator of powdered cellulose that exhibits the effects of the present invention.

[0036] (Particle size distribution, average particle size, span of particle size distribution) The particle size distribution of powdered cellulose can be expressed as the particle size distribution when the cumulative value of the volume accumulation distribution is 10%, 50%, and 90% (10% diameter, 50% diameter, and 90% diameter, respectively, D.10, D.50, and D.90). In this specification, the particle size distribution is a value obtained by wet measurement (with ultrasonic irradiation), wet measurement (without ultrasonic irradiation), or dry measurement using the laser scattering method as the measurement principle.

[0037] The particle size distribution span is a numerical value that indicates the breadth of the particle size distribution. It is presumed to affect the shape of powdered cellulose, and in this invention, it can be said to be an index that comprehensively represents the particle shape (spherical, rod-shaped, bent rod-shaped, etc.) and fiber aggregation state of powdered cellulose. Powdered cellulose with an appropriate particle size distribution span has appropriate fiber length and fiber width, and can suppress entanglement of fibers in the resin composition.

[0038] The span of the particle size distribution is calculated by substituting D. 10, D. 50, and D. 90 obtained by each method into the following formula: Span of particle size distribution = ((D. 90) - (D. 10)) / (D. 50)

[0039] -Conditions for wet measurement (without ultrasonic irradiation)- In this specification, wet conditions (without ultrasonic irradiation) refer to conditions in which the particle size is measured directly after adding water to the sample without ultrasonic irradiation. The preferred ranges for D. 10, D. 50, D. 90, and span under wet conditions (without ultrasonic irradiation) are as follows.

[0040] D. 10 is usually 5 μm or more, 10.0 μm or more, or 14.0 μm or more, preferably 15.0 μm or more, and more preferably 15.5 μm or more. The upper limit is usually 40.0 μm or less, or 25.0 μm or less, preferably 24.0 μm or less, and more preferably 23.0 μm or less.

[0041] D50 (average particle diameter) is usually 5.0 μm or more, 10.0 μm or more, 20.0 μm or more, 30.0 μm or more, 40.0 μm or more, or 45.0 μm or more, preferably 50.0 μm or more or 55.0 μm or more, more preferably 57.0 μm or more, still more preferably 60.0 μm or more (provided that the value is larger than D10). Thereby, an increase in the agglomeration property of powdered cellulose and a decrease in powder flowability caused thereby can be suppressed, and deterioration of workability can be inhibited. The upper limit is usually 150.0 μm or less, 140.0 μm or less, 130.0 μm or less, 120 μm or less, or 110.0 μm or less, preferably 100 μm or less, 95.0 μm or less, or 90.0 μm or less, more preferably 85.0 μm or less, still more preferably 83.0 μm or less. Thereby, unintended deterioration in flowability at the time of blending into a resin composition can be suppressed.

[0042] D90 is usually 100.0 μm or more, 110.0 μm or more, or 115.0 μm or more, preferably 120.0 μm or more, 125.0 μm or more, or 130.0 μm or more, more preferably 135 μm or more, still more preferably 140.0 μm or more (provided that the value is larger than D50). The upper limit is 250.0 μm or less, 240.0 μm or less, or 230 μm or less, preferably 220 μm or less or 210 μm or less, more preferably 200 μm or less, still more preferably 195 μm or less.

[0043] The span of the particle size distribution is usually 1.5 or more, preferably 1.7 or more, more preferably 1.9 or more, still more preferably 2.0 or more. The upper limit is usually 4.0 or less, preferably 3.0 or less, more preferably 2.5 or less, still more preferably 2.3 or less.

[0044] -Wet measurement (with ultrasonic irradiation)- In the present specification, the wet condition (with ultrasonic irradiation) refers to a condition in which a sample is irradiated with ultrasonic waves after adding water, and then the particle diameter is measured. The preferred ranges of D10, D50, D90, and span in the case of wet (with ultrasonic waves) are as follows.

[0045] D10 is usually 1.0 μm or more, 3.0 μm or more, or 5.0 μm or more, preferably 7.0 μm or more or 8.0 μm or more, more preferably 9.0 μm or more, still more preferably 10.5 μm or more. The upper limit is usually 20.0 μm or less or 18.0 μm or less, preferably 15.0 μm or less, more preferably 13.0 μm or less.

[0046] D50 is usually 5 μm or more, 10.0 μm or more, or 15.0 μm or more, preferably 17 μm or more, 18.0 μm or more, or 20.0 μm or more, more preferably 23.0 μm or more or 25.0 μm or more, still more preferably 26.0 μm or more (provided that the value is larger than D10). The upper limit is usually 70.0 μm or less, 60.0 μm or less, or 50.0 μm or less, preferably 45.0 μm or less or 40.0 μm or less, more preferably 35.0 μm or less, still more preferably 31.0 μm or less.

[0047] D90 is usually 50.0 μm or more, 55.0 μm or more, or 60.0 μm or more, preferably 63.0 μm or more, more preferably 65.0 μm or more, still more preferably 68 μm or more (provided that the value is larger than D50). The upper limit is 180.0 μm or less or 160.0 μm or less, preferably 140.0 μm or less or 120.0 μm or less, more preferably 100.0 μm or less, still more preferably 90.0 μm or less.

[0048] The span of the particle size distribution is usually 1.5 or more, preferably 1.7 or more, more preferably 1.9 or more, still more preferably 2.0 or more. The upper limit is usually 4.0 or less, preferably 3.5 or less, more preferably 3.0 or less.

[0049] -Dry Measurement- As used herein, the dry measurement refers to the condition where the particle size is measured as it is without adding water to the sample. The preferred ranges of D10, D50, D90, and span in the case of dry measurement are as follows.

[0050] D. 10 is usually 1.0 μm or more, 3.0 μm or more, or 5.0 μm or more, preferably 7.0 μm or more, or 10.0 μm or more, more preferably 13.0 μm or more, and even more preferably 16.0 μm or more. The upper limit is usually 40.0 μm or less, or 35.0 μm or less, preferably 30 μm or less, more preferably 25.0 μm or less, and even more preferably 23.0 μm or less.

[0051] D. 50 is usually 5.0 μm or more, 10.0 μm or more, or 15.0 μm or more, preferably 20.0 μm or more, 25.0 μm or more, or 30.0 μm or more, more preferably 35.0 μm or more, or 40.0 μm or more, and even more preferably 43.0 μm or more (however, it is a value greater than D. 10). The upper limit is usually 100.0 μm or less, 95.0 μm or less, or 93.0 μm or less, preferably 90.0 μm or less, and more preferably 85.0 μm or less.

[0052] D.90 is typically 70.0 μm or more, 90.0 μm or more, or 100.0 μm or more, preferably 110.0 μm or more, more preferably 120.0 μm or more, and even more preferably 130.0 μm or more (provided it is a value greater than D.50). The upper limit is 260.0 μm or less or 250.0 μm or less, preferably 240.0 μm or less or 230.0 μm or less, and more preferably 220.0 μm or less.

[0053] The particle size distribution span is usually 1.5 or greater, preferably 1.7 or greater, more preferably 1.9 or greater, and even more preferably 2.0 or greater. The upper limit is usually 10.0 or less, preferably 9.0 or less, more preferably 8.0 or less, and even more preferably 7.0 or less.

[0054] By satisfying the above range, when coexisting with pulp fibers in a resin composition, entanglement between pulp fibers can be reduced, and the fluidity of the resin composition can be improved while maintaining its physical properties without lowering the density of the cellulose material.

[0055] [Method for producing powdered cellulose] The method for producing powdered cellulose is not particularly limited as long as it is a method for obtaining powdered cellulose from a cellulose raw material, but for example, a method that includes at least a grinding process is one example, and a method that further includes an acid hydrolysis treatment is preferred because it is easier to obtain powdered cellulose with fewer impurities.

[0056] (Cellulose raw material) The cellulose raw material is usually naturally derived cellulose, with pulp being preferred and wood-derived pulp being more preferred. Examples of wood-derived pulp include pulp derived from hardwoods and pulp derived from softwoods. Methods for preparing wood-derived pulp include, for example, methods involving pulping (digestion). Pulping (digestion) dissolves and removes lignin, a coloring substance, and yields pulp with high whiteness. Examples of pulping (digestion) methods include sulfite digestion, kraft digestion, soda-quinone digestion, and organosolve digestion, with kraft pulp being preferred from an environmental perspective.

[0057] In the pulp preparation method, it is preferable to further bleach the pulp in addition to the pulping method (digestion method). This results in pulp with higher whiteness. Examples of bleaching methods include chlorine treatment (C), chlorine dioxide bleaching (D), alkaline extraction (E), hypochlorite bleaching (H), hydrogen peroxide bleaching (P), alkaline hydrogen peroxide treatment stage (Ep), alkaline hydrogen peroxide / oxygen treatment stage (Eop), ozone treatment (Z), chelation treatment (Q), and combinations of two or more of these treatments applied to pulp that has been deligned by an optional conventional method. Examples of combinations (sequences) of two or more processes include D-E / P-D, C / D-E-H-D, Z-E-D-PZ / D-Ep-D, Z / D-Ep-DP, D-Ep-D, D-Ep-D-D-P, D-Ep-P-D, Z-Eop-D-D, Z / D-Eop-D, and Z / D-Eop-D-E-D (the " / " in the sequence means that the processes before and after the " / " are performed consecutively without washing). The bleaching process is not limited to the above examples and may be a method commonly used. Pulp that has undergone the bleaching process is usually in a fluid state (fluidized pulp). The whiteness of the pulp is preferably 80% or higher, based on ISO 2470.

[0058] (Acid Hydrolysis Treatment) Cellulose raw materials can be subjected to acid hydrolysis treatment to reduce their molecular weight (fine particle size). Examples of acids used in acid hydrolysis treatment include mineral acids such as hydrochloric acid, sulfuric acid, and nitric acid. The acid concentration is not particularly limited, but from the viewpoint of maintaining the degree of polymerization and whiteness, it is preferable that it be lower than the acid concentration used in conventional acid hydrolysis treatment for powdered cellulose production, more preferably 0.4 to 2.0 N, and more preferably 0.5 to 1.5 N. If the acid concentration is less than 0.4 N, the depolymerization of cellulose by the acid is suppressed, and the decrease in the degree of polymerization of cellulose can be reduced, but fine particle size may become difficult. On the other hand, if it exceeds 2.0 N, the depolymerization of cellulose proceeds and fine particle size becomes easier, so the powder flowability improves, but the hardness of the tablets may decrease (they may become more prone to crumbling when molded) due to the decrease in the degree of polymerization. The reaction conditions for acid hydrolysis treatment are not particularly limited, but the reaction temperature is usually 80 to 100°C, and the reaction time is usually 30 minutes to 3 hours.

[0059] Prior to acid hydrolysis, the cellulose raw material may be pretreated. Examples include slurring of the cellulose raw material (preparation of dispersion) and adjustment of the cellulose raw material concentration. The concentration of the cellulose raw material is usually 3 to 10% by mass (on a solid content basis) relative to the dispersion. If the cellulose raw material is a bleached liquid pulp, it is common to increase the pulp concentration before hydrolysis. Dehydrators such as screw presses and belt filters may be used to adjust (concentrate) the cellulose raw material concentration. Acid hydrolysis may be performed on a slurry of the cellulose raw material, or on a sheet of cellulose raw material. If the cellulose raw material is a dry sheet of pulp, the pulp is usually loosened before acid hydrolysis. A crusher such as a roll crusher may be used to loosen the pulp.

[0060] (Neutralization, Washing, Dehydration, and Drying Treatment) After hydrolysis, the resulting product undergoes appropriate pretreatment before grinding. Examples of pretreatment include neutralization, washing, dehydration, and drying, and it is preferable to perform neutralization, washing, dehydration, and drying in this order. Neutralization can be performed by adding an alkaline agent. Dehydration is usually a solid-liquid separation treatment, which allows for the separation of waste acid from the hydrolyzed product. Furthermore, the hydrolyzed product may undergo drying (dehydration) treatment. This allows for adjustment of the solid content concentration, making it easy to control the physical properties of the powdered cellulose. The solid content concentration is usually adjusted to 15% or more, preferably 20% or more. For drying, it is preferable to use an airflow dryer. This allows for the application of high-speed hot air while dispersing the hydrolyzed product in an airflow, regardless of whether it is a cake-like solid, slurry, solution, etc., and also allows for instantaneous drying by utilizing the reduced pressure effect inside the dryer. Furthermore, because the exposure time to hot air is extremely short, the product temperature can be kept low, making it ideal for drying heat-sensitive products or products with low melting points. The drying conditions for airflow dryers are not particularly limited and can be set as appropriate, but an example is as follows: The outlet drying temperature is usually 80 to 180°C, preferably 90 to 160°C. The air supply volume is usually 150 to 350 m³. 3 / h, preferably 160 to 320 m 3 It is / h.

[0061] On the other hand, when using a spray dryer, the material is sprayed and instantly dried with hot air to produce granules. Therefore, it is often unsuitable for drying solid or semi-solid objects with low moisture content, and the particles are more easily exposed to high heat instantaneously than when dried with an airflow dryer, raising concerns about the impact on the product.

[0062] (Crushing Process) The crushing process is a process in which the processed material that has gone through the previous process is mechanically crushed. Classification may be performed simultaneously with or after crushing.

[0063] Examples of crushers include the following:

[0064] Cutting mills include: mesh mills (manufactured by Horai Co., Ltd.), Atoms (manufactured by Yamamoto Hyakuma Seisakusho Co., Ltd.), knife mills (manufactured by Parman Co., Ltd.), cutter mills (manufactured by Tokyo Atomizer Manufacturing Co., Ltd.), CS cutters (manufactured by Mitsui Mining Co., Ltd.), rotary cutter mills (manufactured by Nara Machinery Works Co., Ltd.), turbo cutters (manufactured by Freund Industrial Co., Ltd.), pulp crushers (manufactured by Zuiko Co., Ltd.), and shredders (manufactured by Shinko Pantech Co., Ltd.), etc.

[0065] Hammer mills: Jaw crusher (manufactured by Makino Corporation), hammer crusher (manufactured by Makino Sangyo Co., Ltd.), and micropulperizer (manufactured by Hosokawa Micron Corporation).

[0066] Impact mills: Pulverizer (manufactured by Hosokawa Micron Corporation), Fine Impact Mill (manufactured by Hosokawa Micron Corporation), Super Micron Mill (manufactured by Hosokawa Micron Corporation), Inomizer (manufactured by Hosokawa Micron Corporation), Fine Mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), CUM type centrifugal mill (manufactured by Mitsui Mining Co., Ltd.), Exceed Mill (manufactured by Makino Sangyo Co., Ltd.), Ultraplex (manufactured by Makino Sangyo Co., Ltd.), Contraplex (manufactured by Makino Sangyo Co., Ltd.), Coroplex (manufactured by Makino Sangyo Co., Ltd.), Sample Mill (manufactured by Seishin Co., Ltd.), Bantam Mill (manufactured by Seishin Co., Ltd.), Atomizer (manufactured by Seishin Co., Ltd.), Tornado Mill (manufactured by Nikkiso Co., Ltd.), Nea Mill (manufactured by Dalton Co., Ltd.), HT type fine grinder (manufactured by Horai Co., Ltd.), free grinder (manufactured by Nara Machine Works Co., Ltd.), New Cosmomizer (manufactured by Nara Machine Works Co., Ltd.), Turbo Mill (manufactured by Freund Industrial Co., Ltd.), Gather Mill (manufactured by Nishimura Machine Works Co., Ltd.), Super Powder Mill (manufactured by Nishimura Machine Works Co., Ltd.), Blade Mill (manufactured by Nisshin Engineering Co., Ltd.), Super Rotor (manufactured by Nisshin Engineering Co., Ltd.), Npa Crusher (manufactured by Sansho Industry Co., Ltd.), Wheeley Grinder (manufactured by Sanki Seisakusho Co., Ltd.), Pulp Grinder (manufactured by Zuiko Co., Ltd.), Jacobson Fine Grinder (manufactured by Shinko Pantech Co., Ltd.), and Universal Mill (manufactured by Tokuju Kogyo Co., Ltd.).

[0067] Airflow mills: CGS type jet mill (manufactured by Mitsui Mining Co., Ltd.), Micron Jet (manufactured by Hosokawa Micron Corporation), Counter Jet Mill (manufactured by Hosokawa Micron Corporation), Cross Jet Mill (manufactured by Kurimoto Iron Works Co., Ltd.), Supersonic Jet Mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), Current Jet (manufactured by Nisshin Engineering Co., Ltd.), Jet Mill (manufactured by Sansho Industry Co., Ltd.), Ebara Jet Micronizer (manufactured by Ebara Corporation), Ebara Triad Jet (manufactured by Ebara Corporation), Selenium Mirror (manufactured by Masuko Sangyo Co., Ltd.), New Microsictomat (manufactured by Masuno Seisakusho Co., Ltd.), and Cryptron (manufactured by Kawasaki Heavy Industries, Ltd.).

[0068] Vertical roller mills: Vertical roller mills (manufactured by Shinion Co., Ltd.), vertical roller mills (manufactured by Schaeffler Japan Co., Ltd.), roller mills (manufactured by Kotobuki Giken Kogyo Co., Ltd.), VX mills (Kurimoto Iron Works Co., Ltd.), KVM type vertical mills (Earth Technica Co., Ltd.), and IS mills (IHI Plant Engineering Co., Ltd.).

[0069] Among these, the following are preferred due to their excellent fine grinding capabilities: Jaw Crusher (manufactured by Makino Corporation), Pulverizer (manufactured by Hosokawa Micron Corporation), Super Micron Mill (manufactured by Hosokawa Micron Corporation), Tornado Mill (manufactured by Nikkiso Co., Ltd.), Free Grinding Machine (manufactured by Nara Machine Works Co., Ltd.), Turbo Mill (manufactured by Freund Industrial Co., Ltd.), Super Powder Mill (manufactured by Nishimura Machine Works Co., Ltd.), Blade Mill (manufactured by Nisshin Engineering Co., Ltd.), Supersonic Jet Mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), or Current Jet (manufactured by Nisshin Engineering Co., Ltd.).

[0070] The conditions for grinding, or classification as needed, can be appropriately set to obtain the desired powdered cellulose. For example, the processing conditions can be adjusted by referring to a calibration curve created from the grinding conditions (e.g., processing time, input amount) and the desired physical properties of the powdered cellulose.

[0071] During the grinding process, at least one other component (e.g., an organic component, an inorganic component) may be added to the acid hydrolyzed product along with the grinding process, if necessary. This can impart or improve the functionality of the powdered cellulose. The amount of the other component should be appropriately selected.

[0072] The powdered cellulose may be chemically treated as needed. The chemical treatment should preferably be one that does not significantly impair the degree of polymerization of the cellulose raw material. The chemical treatment may be performed on the cellulose raw material (before acid hydrolysis) or during the grinding process.

[0073] <Other Cellulose Materials> In addition to components A and B described above, other cellulose materials may be included as long as they do not hinder the effects of the present invention. Examples of such cellulose materials include cellulose nanofibers, microfibril cellulose, cellulose nanocrystals, and cellulose derivatives (such as carboxymethyl cellulose).

[0074] In the cellulose material of the present invention, the total amount of component A and component B is preferably 80% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more, or 95% by mass or more, of the total mass of the cellulose material. By having components A and B in the cellulose material within this range, the effects of the present invention can be further improved.

[0075] <Thermoplastic Resin> Any thermoplastic resin (also called the base resin) can be used in the resin composition of the present invention as long as it can be plasticized and molded by heat. However, in this specification, it usually refers to a thermoplastic resin that has not been modified with hydrophilic functional groups (specifically, hydroxyl groups, carboxyl groups, carbonyl groups, amino groups, amide groups, sulfo groups, etc.). Examples include polyethylene, polypropylene, polystyrene, polyamide, and polylactic acid. It is preferable to use a polyolefin resin or a polyester resin as the thermoplastic resin (base resin) according to the present invention. It is also possible to use two or more types of thermoplastic resins simultaneously.

[0076] As polyolefin resins, for example, polyolefins such as homopolypropylene (hPP), high-density polyethylene (HDPE), low-density polyethylene (LDPE), and linear low-density polyethylene (L-LDPE), and block copolymers such as block polypropylene (bPP) can be suitably used, and among these, polypropylene is preferred from the viewpoint of heat resistance in practical use. In one embodiment, the melting point of homopolypropylene may be 165 to 170°C, the melting point of high-density polyethylene may be 130 to 135°C, the melting point of low-density polyethylene may be 95 to 135°C, the melting point of linear low-density polyethylene may be about 124°C, and the melting point of block polypropylene may be 150 to 170°C.

[0077] Examples of polyester resins include aliphatic polyesters, such as polylactic acid, polybutylene succinate, polybutylene adipate terephthalate, and polycaprolactone, which can be suitably used. Among these, polylactic acid is preferred from the viewpoint of affinity with cellulose.

[0078] Furthermore, it is preferable to use a thermoplastic resin with a melt mass flow rate (MFR) of 2 to 110 g / 10 min.

[0079] In this invention, an elastomer may be used in combination with the thermoplastic resin, as long as the effect is not impaired. As the elastomer, a common thermoplastic elastomer can be selected and used depending on the purpose. Examples include polyurethane elastomers, polyester elastomers, polyamide elastomers, olefin elastomers, and styrene elastomers. These elastomers may be used individually or in combination of two or more types.

[0080] The content of thermoplastic resin in 100 parts by mass of the resin composition is preferably 40 to 95 parts by mass, and more preferably 50 to 90 parts by mass, from the viewpoint of moldability. If the content of thermoplastic resin is too high, a good reinforcing effect may not be observed, and conversely, if it is too low, molding may not be possible.

[0081] When an elastomer is used in combination with a thermoplastic resin, the blending ratio of the elastomer is preferably 30 parts by mass or less, and more preferably 20 parts by mass or less, per 100 parts by mass of the total of the base resin and the elastomer. If the amount of elastomer is too high, it may adversely affect the mold release properties.

[0082] (Polymer compound having amino groups in the side chain) The resin composition of the present invention preferably contains a polymer compound having amino groups in the side chain, from the viewpoint of being able to improve tensile strength and flexural modulus while maintaining impact strength above a certain value. Furthermore, it is preferable that the amino group is a primary amino group.

[0083] The weight-average molecular weight of polymer compounds having amino groups in their side chains is typically around 10 million to 1 million, preferably around 12 million to 700,000.

[0084] In this invention, the weight-average molecular weight is a value measured by one of the following methods: gel permeation chromatography (GPC) (PEG equivalent), GPC (pullulan equivalent), or GPC-MALLS, which involves connecting a multi-angle light scattering detector to a GPC column.

[0085] The amino group in a polymer compound having an amino group in its side chain may form a salt with an organic or inorganic acid. Examples of inorganic acids in which the amino group can form a salt include hydrochloric acid, sulfuric acid, phosphoric acid, boric acid, hydrobromic acid, and hydroiodic acid, while examples of organic acids include formic acid, acetic acid, propionic acid, p-toluenesulfonic acid, methanesulfonic acid, citric acid, and tartaric acid. Furthermore, a single polymer compound having an amino group in its side chain may be used, or two or more may be used in combination. Polymer compounds having an amino group in their side chain may be synthesized by conventionally known methods, or commercially available products may be used.

[0086] Examples of polymer compounds having a primary amino group include compounds having allylamine units represented by the following general formula (i) as repeating units, and salts thereof.

[0087]

[0088] A compound having a repeating unit represented by general formula (i) may be a copolymer or graft polymer containing other repeating units in addition to the repeating unit represented by general formula (i).

[0089] Other repeating units that combine with the repeating unit represented by the general formula (i) above to form copolymers and graft polymers include, for example, units containing secondary amines such as polyacrylate units, polymethacrylate units, polyacrylamide units, and polydiallylamine units, units containing tertiary amines such as polymethyldiallylamine units, and units containing quaternary ammonium salts such as polydiallyldimethylammonium salt units. The bonding order of each repeating unit is not limited and may be random or in blocks.

[0090] However, if the amount of repeating units other than the repeating unit represented by general formula (i) becomes too large, the number of primary amino groups per unit weight decreases, which is undesirable. It is more preferable that the compound containing the repeating unit represented by general formula (i) is a homopolymer or salt thereof containing only the repeating unit represented by general formula (i).

[0091] Examples of salts of compounds having repeating units represented by general formula (i) include inorganic acid salts such as hydrochloride, sulfate, phosphate, hydrobromide, and hydroiodide, and organic acid salts such as formate, acetate, propionate, p-toluenesulfonate, methanesulfonate, citrate, and tartrate. Compounds having repeating units represented by general formula (i) can be synthesized using conventionally known polymerization methods with allylamine and the like as raw materials, and commercially available products are readily available.

[0092] Furthermore, examples of polymer compounds having primary amino groups include compounds having vinylamine units represented by the following general formula (ii) as repeating units, and salts thereof.

[0093]

[0094] A compound having a repeating unit represented by general formula (ii) may be a copolymer or graft polymer containing other repeating units in addition to the repeating unit represented by general formula (ii).

[0095] Other repeating units that combine with the repeating unit represented by the general formula (ii) above to form copolymers and graft polymers include polyacrylate units, polymethyl methacrylate units, polyacrylamide units, polyvinylformamide units, polyvinylacetamide units, units containing secondary amines such as polydiallylamine units, units containing tertiary amines such as polymethyldiallylamine units, and units containing quaternary ammonium salts such as polydiallyldimethylammonium salt units. The bonding order of each repeating unit is not limited and may be random or in blocks.

[0096] However, if the amount of repeating units other than the repeating unit represented by general formula (ii) becomes too large, the number of primary amino groups per unit weight decreases, which is undesirable. It is more preferable that the compound containing the repeating unit represented by general formula (ii) is a homopolymer or salt thereof containing only the repeating unit represented by general formula (ii).

[0097] Examples of salts of compounds having repeating units represented by general formula (ii) include inorganic salts such as hydrochloride, sulfate, phosphate, hydrobromide, and hydroiodide, and organic salts such as formate, acetate, propionate, p-toluenesulfonate, methanesulfonate, citrate, and tartrate.

[0098] Compounds having repeating units represented by general formula (ii) can be synthesized by conventionally known polymerization methods, such as hydrolysis of polymers of N-substituted amides like N-vinylformamide and N-vinylacetamide, or by Hoffmann modification of polyacrylamide, and commercially available products are readily available.

[0099] Furthermore, examples of polymer compounds having primary amino groups include compounds having repeating units represented by the following general formula (iii) and their salts.

[0100]

[0101] Compounds having repeating units represented by general formula (iii) may have repeating units represented by general formula (iii) that extend in a linear chain or that have a branched structure. In addition, graft polymers may also contain other repeating units besides general formula (iii).

[0102] If the amount of repeating units other than the repeating unit represented by general formula (iii) becomes too large, the number of primary amino groups per unit weight decreases, which is undesirable. It is more preferable that the compound containing the repeating unit represented by general formula (iii) is a homopolymer or salt thereof containing only the repeating unit represented by general formula (iii). Examples of such preferred homopolymers or salts thereof include polyethyleneimine or a salt thereof.

[0103] Examples of salts of compounds having repeating units represented by general formula (iii) include inorganic salts such as hydrochloride, sulfate, phosphate, hydrobromide, and hydroiodide, and organic salts such as formate, acetate, propionate, p-toluenesulfonate, methanesulfonate, citrate, and tartrate.

[0104] Compounds having repeating units represented by general formula (iii) are known as cationic polymers and can be synthesized using aziridine as a raw material by conventionally known polymerization methods, and commercially available products are readily available.

[0105] The resin composition of the present invention preferably contains at least one selected from the group consisting of compounds having repeating units represented by the above general formulas (i), (ii), and (iii), and salts thereof.

[0106] In the resin composition of the present invention, when a polymer compound having an amino group in its side chain is included, the amount of the polymer compound is preferably 1 to 35 parts by mass, more preferably 3 to 35 parts by mass, and even more preferably 4 to 17 parts by mass, per 100 parts by mass of cellulose material.

[0107] (Compatibilizing Resin) In the present invention, the compatibilizing resin serves to improve the uniform mixing and adhesion between cellulose materials with different hydrophobic properties and the aforementioned thermoplastic resins (base resin, elastomer). From the viewpoint of performing the above function, it is preferable that the compatibilizing resin is modified with hydrophilic functional groups. In the present invention, hydrophilicity means having good affinity with water and the cellulose surface that constitutes the pulp. Examples of hydrophilic functional groups include hydroxyl groups, carboxyl groups, carbonyl groups, amino groups, amide groups, sulfo groups, etc. Examples of such compatibilizing resins include base-modified polyolefins and acid-modified polyolefins, among which maleic anhydride-modified polypropylene (MAPP) and maleic anhydride-modified polyethylene (MAPE) are particularly noteworthy.

[0108] From the viewpoint of easy dispersibility, the melting point of the compatibilizing resin that can be used in the present invention is preferably below the melting point of the thermoplastic resin (base resin) mentioned above. For example, the melting point of maleic anhydride-modified polypropylene (MAPP) is 150°C, and the melting point of maleic anhydride-modified polyethylene (MAPE) is 120°C.

[0109] Factors that determine the characteristics of a compatible resin include, for example, the amount of dicarboxylic acid added and the weight-average molecular weight of the base polyolefin resin in the case of maleic anhydride-modified polyolefins. Polyolefin resins with a large amount of added dicarboxylic acid improve compatibility with hydrophilic polymers such as cellulose, but the molecular weight of the resin decreases during the addition process, reducing the strength of the molded product. The optimal balance for the amount of added dicarboxylic acid is 20 to 100 mg KOH / g, and more preferably 45 to 65 mg KOH / g. If the amount added is small, there are fewer points in the resin that interact with the hydroxyl groups of cellulose and the hydroxyl groups and modified functional groups contained in modified cellulose. If the amount added is large, self-aggregation due to hydrogen bonding between carboxyl groups in the resin and a decrease in the molecular weight of the base olefin resin due to excessive addition reactions result in insufficient strength as a reinforcing resin. The molecular weight of the polyolefin resin is preferably 35,000 to 250,000, and more preferably 50,000 to 100,000. If the molecular weight is smaller than this range, the strength of the resin decreases. If it is larger than this range, the viscosity increases significantly during melting, reducing workability during mixing and causing molding defects.

[0110] The amount of compatibilizing resin added is not particularly limited, but is preferably 1 to 100 parts by mass, and more preferably 10 to 80 parts by mass, per 100 parts by mass of cellulose material. If the amount added exceeds 100 parts by mass, it will exceed the amount necessary for interface formation between cellulose and resin, and it is thought that the strength of the composite will decrease.

[0111] Furthermore, the compatible resin may be used alone or as a mixture of two or more resins. When used as a graft body of one or more polymers and polyolefins, the polyolefin resin constituting the graft body is not particularly limited, but polyethylene, polypropylene, polybutylene, etc. can be used from the viewpoint of ease of manufacturing the graft body.

[0112] Furthermore, the resin composition of the present invention may also contain an antioxidant. Examples of antioxidants that can be used include thioether-based antioxidants and hindered phenol-based antioxidants. An example of a hindered phenol-based antioxidant is Irganox 1010 manufactured by BASF Japan Ltd. In addition, depending on the application, the present invention may be used in combination with mineral-based fillers such as talc, calcium carbonate, titanium dioxide, and glass beads, or fibrous fillers such as whiskers, glass fibers, carbon fibers, aramid fibers, and carbon nanotubes, or other fillers other than cellulose fibers. There are no particular restrictions on the content ratio as long as the effects of the present invention are not impaired, but for example, 0.01 to 10% by mass in the resin composition is preferred.

[0113] The resin composition of the present invention may contain, in addition to the above-mentioned thermoplastic resin, or a blend of thermoplastic resin and elastomer, and cellulose material, any additives as needed. Examples of optional additives include low molecular weight compatibilizers, surfactants, starches, polysaccharides such as alginic acid, natural proteins such as gelatin, glue, and casein, inorganic compounds such as tannins, zeolites, ceramics, and metal powders, viscosity modifiers, colorants, plasticizers, pigments, dyes, antistatic agents, ultraviolet absorbers, antioxidants, light stabilizers, and flame retardants. There are no particular restrictions on the content ratio of any additive as long as the effects of the present invention are not impaired, but for example, 0.01 to 10% by mass in the resin composition is preferred.

[0114] (Preparation of Resin Composition) The resin composition of the present invention is obtained by heating and kneading the above-mentioned thermoplastic resin, cellulose material, and any optional additives used as needed.

[0115] In order to achieve the effects expected in this invention, it is important that the resin composition is densely packed, with an appropriate amount of cellulose material uniformly and evenly filling the resin composition, resulting in a homogeneous structure and reduced structural defects. Therefore, the mixing ratio of the thermoplastic resin to the cellulose material cannot be uniformly determined as it is related to the impact strength and degree of fiber defibration of the thermoplastic resin used. However, for example, by nano-sizing the entire cellulose material, the effect can be achieved with a small amount of addition, while even if not severely defibrated, sufficient addition of cellulose material can improve impact strength. The mixing ratio of thermoplastic resin to cellulose material can be manufactured as a mass ratio of 97:3 to 60:40 in the resin composition, preferably 95:5 to 62:38, and more preferably 90:10 to 65:35, allowing for the production of a resin composition with excellent mechanical strength, impact strength, and coefficient of linear expansion. Furthermore, even if cellulose defibration has not reached the nano level, the effect can be achieved if the cellulose material in the resin composition is 5% by mass or more, and the effect can be achieved more strongly if it is 10% by mass or more. While exceeding 40% by mass of cellulose material is undesirable because it reduces fluidity during molding, impairs moldability, and leads to various molding defects, the higher cellulose content increases convenience and cost-effectiveness during transportation. Therefore, when used as a masterbatch for the cellulose material in this invention, a high-concentration formulation with 50% or more cellulose may be used. Furthermore, it has been found that using a thermoplastic resin with high impact strength improves impact strength even with the same amount of cellulose material added, making it possible to adjust the balance of the ultimately required mechanical properties, impact strength, and coefficient of thermal expansion.

[0116] Furthermore, in the cellulose material, it is preferable that the content of component A ≥ component B. In the resin composition of the present invention, mechanical strength and impact strength are proportional to the amount of component A added, so if the content of component A is lower than that of component B, these strengths may decrease. Therefore, it is necessary to increase the content ratio of component A. However, if the content ratio of component A is too high, there is a concern that the fluidity will decrease due to the entanglement of the fibers that are densely dispersed in the resin composition. Therefore, by coexisting with an appropriate amount of component B, the balance with fluidity can be further adjusted.

[0117] The heating temperature can be adjusted to match the melting point of the thermoplastic resin used. A heating temperature of approximately ±10°C from the minimum processing temperature recommended by the thermoplastic resin supplier is preferable. By setting the heating temperature within this range, the thermoplastic resin, cellulose fibers, and any additional additives can be uniformly mixed.

[0118] The heating and kneading time should be adjusted within the range recommended by the kneader manufacturer, taking into account the production volume, and considering the equipment's performance and operating conditions such as rotation speed. A shorter heating time is preferable because it prevents deterioration due to heat and oxidation during heating and kneading, but if the heating time is too short, dispersion in the resin may be insufficient. Therefore, it is preferable to include components that enhance kneading, such as a rotor or kneader, within the screw piece during heating and kneading.

[0119] Furthermore, in order to prevent deterioration due to heating and oxidation during heating and kneading, it is preferable to add additives such as antioxidants and knead under a nitrogen atmosphere.

[0120] A single-screw or multi-screw mixer can be used as the mixing machine, but a twin-screw mixer is preferred.

[0121] Furthermore, in this invention, the entire amount of thermoplastic resin, cellulose material, and any optional additives may be supplied to the kneader at once, or components A and B and any optional additives may be supplied to the kneader in multiple portions. When supplying in multiple portions, a side feeder or the like may be used.

[0122] There are no particular restrictions on the number of times the resin composition is processed in the kneader, but in the case of multiple processing, the same material may be kneaded multiple times. Also, in the case of multiple processing, the cellulose material may be produced at a high concentration of 30-80% in the first processing, and with each subsequent processing, thermoplastic resin, cellulose material, and any optional additives may be added so that the final resin composition obtained falls within the scope of the present invention.

[0123] <Molded Articles> The resin composition of the present invention can be used as a molded article processed into a desired shape. When manufacturing molded articles, the resin composition of the present invention can be used as a molding material in various shapes, such as pellets, flakes, powder, sheets, plates, and films.

[0124] Molding methods include injection molding, die molding, extrusion molding, blow molding, vacuum pressure molding, and 3D printing. It is also possible to perform molding that involves physical or chemical foaming. The shape of the molded article can be sheet-like, plate-like, film-like, or a three-dimensional structure. Various shapes of molded articles can be manufactured using the above molding methods according to the application. By using the resin composition of the present invention, it is possible to obtain a molded article that maintains moldability (fluidity) while exhibiting excellent mechanical strength (flexural modulus, flexural strength), impact strength, and coefficient of linear expansion.

[0125] Molded articles produced from the resin composition of the present invention can be used in fields requiring mechanical strength, impact strength, and coefficient of thermal expansion. Specifically, they can be used for interior materials, exterior materials, and structural materials of transportation equipment such as automobiles, trains, ships, and airplanes; casings, structural materials, and internal components of electrical appliances such as personal computers, televisions, telephones, and watches; casings, structural materials, and internal components of mobile communication equipment such as mobile phones; casings, structural materials, and internal components of portable music players, video players, printing machines, photocopiers, and sporting goods; building materials; and containers and other office equipment such as stationery.

[0126] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. In the following, "parts" refers to mass unless otherwise specified.

[0127] (Manufacturing Example 1: Pulp Fiber 1) Water was added to a pulp raw material mainly composed of eucalyptus (E. grandis), and the material was crushed using a Henschel mixer while still moist to obtain pulp fiber 1 with a fine content of 14.5% by mass, an average kink angle of 67.2 degrees, an average aspect ratio of 42.1, a long fiber content of 65.3% by mass, and a moisture content of 40%.

[0128] (Manufacturing Example 2: Pulp Fiber 2) Pulp fiber 2 was obtained in the same manner as in Manufacturing Example 1, except that a pulp raw material mainly composed of pine (P. radiata) was used, with a fine fiber content of 21.9% by mass, an average kink angle of 65.2 degrees, an average aspect ratio of 69.8, a long fiber content of 52.0% by mass, and a moisture content of 40%.

[0129] The pulp fibers in Production Examples 1 and 2 were measured using the following method. The average fiber length, average fiber diameter, fineness, average kink angle, and fiber length distribution of the pulp fibers were measured using a Lorentzen & Wettre fiber tester. In this invention, fiber length refers to the length-weighted average fiber length based on ISO 16065. In this invention, fiber diameter refers to the length-weighted average fiber diameter. Specifically, water was added to 0.15 g of oven-dry pulp to a total volume of 300 g, stirred in a homodisper at 3000 rpm for 2 minutes, and then measured with a fiber tester.

[0130] (Manufacturing Example 3: Powdered Cellulose 1) Chlorine-free bleached pulp was subjected to a hydrolysis reaction at 95°C for 2 hours in a pulp concentration of 5.5% and a hydrochloric acid concentration of 0.30 N. After the hydrolysis reaction was completed, it was neutralized with sodium hydroxide, washed with industrial water, and then dehydrated. This was then dehydrated to a solid content of 50% or more. The dehydrated material was kneaded in a planetarium mixer (manufactured by Inoue Seisakusho Co., Ltd.) and air-dried in an explosion-proof forced-air dryer at a temperature of 60°C for about 1 day to obtain acid hydrolysis treated pulp. The obtained acid hydrolysis treated pulp was mechanically crushed and classified as appropriate using a hammer mill (manufactured by Hosokawa Micron Corporation, AP-S type) to obtain powdered cellulose 1 with an average particle size of 31.1 μm and an average L / D of 4.7.

[0131] (Manufacturing Example 4: Powdered Cellulose 2) Chlorine-free bleached pulp was subjected to a hydrolysis reaction at 95°C for 2 hours in a pulp concentration of 5.5% and a hydrochloric acid concentration of 1.2N. After the hydrolysis reaction was completed, it was neutralized with sodium hydroxide, washed with industrial water, and then dehydrated. This was then dehydrated to a solid content of 25% or more, and dried at an outlet drying temperature of 100°C and an air supply of 180 m³. 3 The pulp was air-dried in an airflow dryer at a rate of 1 hour to obtain acid hydrolysis-treated pulp. The obtained acid hydrolysis-treated pulp was mechanically crushed and classified as appropriate using a hammer mill (Hosokawa Micron Corporation, Micropulperizer AP-S type) to obtain powdered cellulose 2 with an average particle size of 61.3 μm and an average L / D ratio of 4.8.

[0132]

[0133] The powdered cellulose in production examples 3 and 4 was measured using the following method.

[0134] <Longest diameter (L), shortest diameter (D), longest diameter / shortest diameter ratio (L / D)> 1 g of powdered cellulose was classified using a JIS test sieve (Tokyo Screen Co., Ltd.: 75 μm) to prepare observation samples. The observation samples were observed at 100x magnification using an optical microscope, and the longest diameter (L) and shortest diameter (D) of 140 randomly selected powdered cellulose samples were measured. The longest diameter / shortest diameter ratio (L / D) for each was calculated. L represents the maximum diameter, and D represents the minimum diameter. The longest diameter / shortest diameter ratio (L / D) was calculated as the average value of 100 powdered cellulose samples, excluding the top and bottom 20 values.

[0135] <Particle Size Distribution, Average Particle Size, and Particle Size Distribution Span> A laser diffraction particle size distribution analyzer (Mastersizer 3000, Malvern Panalytic Division, Spectris) was used. Using the laser scattering method as the measurement principle, particle size distributions were measured using dry measurement, wet measurement (with ultrasonic irradiation), and wet measurement (without ultrasonic irradiation). When the particle size distribution is expressed as a volume accumulation distribution, the values ​​where the cumulative volume accumulation distribution reaches 10%, 50%, and 90% were defined as particle size distributions D. 10, D. 50, and D. 90, respectively. D. 50 for the wet measurement (without ultrasonic irradiation) was defined as the average particle size. Furthermore, the span of the particle size distribution was calculated using the following formula: Particle size distribution span = ((D. 90) - (D. 10)) / (D. 50)

[0136] Dry measurements were performed by adding the sample to the feed port so that the scattering intensity was less than 1%, under the following conditions: • Dispersion unit: Aero 5 • Air pressure: 2 bar • Feed rate: 25

[0137] For wet measurements, the sample was added to the measurement section of water being stirred at 3500 rpm, with the scattering intensity set to approximately 10%. When irradiating with ultrasound, the sample in the water was exposed to ultrasound before the wet measurement was performed under the following conditions: Mode: Continuous, Intensity: 100%, Time: 600 seconds.

[0138] The particle size distribution analysis was performed under the following conditions for all measurement conditions: • Analysis: General purpose • Analysis sensitivity: Enhanced • Light scattering model: Mie theory

[0139] (Example 1) The aforementioned (A) pulp fibers 1 and (B) powdered cellulose 1, (C) thermoplastic resin, (D) compatibilizer resin, (E) elastomer, and (F) antioxidant were mixed so that the solid content ratio of (A) / (B) / (C) / (D) / (E) / (F) was (5 / 5 / 78 / 1.7 / 10 / 0.3). (Note that the mass of (A) in this mass ratio is the mass as an absolute dry product.) The mass of water contained in (A) and (B) was 18.2% by mass relative to the total solid content mass of (A) to (E).

[0140] The obtained mixture was placed in a kneader and kneaded at a set temperature of 160°C to obtain a resin composition. Next, this was pelletized using a pelletizer to obtain pelletized resin composition 1.

[0141] The following raw materials were used for (C) to (F): (C) Thermoplastic resin: Polypropylene (PP) (J707EG, manufactured by Prime Polymer Co., Ltd., melting point: 160-165°C, MFR: 30 g / 10 min) (D) Compatibilizing resin: MAPP (acid-modified polypropylene H1000P, manufactured by Toyobo Co., Ltd., melting point: 150°C) (E) Elastomer: (Toughmer A20090S, manufactured by Mitsui Chemicals, Inc., melting point: 77°C) (F) Antioxidant: (Irganox 1010, manufactured by BASF Japan Ltd.)

[0142] (Example 2) A pelletized resin composition 2 was obtained in the same manner as in Example 1, except that the solid content ratio of (A) / (B) / (C) / (D) / (E) / (F) was changed to (15 / 15 / 54 / 5 / 10 / 1).

[0143] (Example 3) A pelletized resin composition 3 was obtained in the same manner as in Example 1, except that (C) the thermoplastic resin was changed to hPP (high elastic PP) polypropylene J108M manufactured by Prime Polymer Co., Ltd., with a melting point of 165-170°C, and the solid content ratio of (A) / (B) / (C) / (D) / (E) / (F) was changed to (20 / 10 / 64 / 5 / 0 / 1).

[0144] (Example 4) A pelletized resin composition 4 was obtained in the same manner as in Example 1, except that (A) the pulp fibers 1 were crushed using a crushing device (HA-2542, manufactured by Horai Co., Ltd.) with a screen diameter of φ0.5 mm and the average aspect ratio was adjusted to 19.4, and (C) the thermoplastic resin was changed to bPP (high-flow PP), which is polypropylene BC10HRF (melting point 160-168℃) manufactured by Nippon Polypropylene Co., Ltd., and the solid content ratio of (A) / (B) / (C) / (D) / (E) / (F) was changed to (15 / 10 / 58 / 4.2 / 12 / 0.8).

[0145] (Manufacturing Example 5: Pulp Fiber 3) An LBKP (bleached hardwood kraft pulp) sheet (manufactured by Nippon Paper Industries Ltd.) was mixed in a Henschel mixer to obtain a crushed product. Further crushing was performed in a pulverizer to obtain pulp fiber 3. The obtained pulp fiber 3 had a fine content of 21.2% by mass, an average kink angle of 55.4 degrees, an average aspect ratio of 32.7, a long fiber content of 46.0% by mass, and a moisture content of 6.5%. The average fiber length, average fiber diameter, fine content, average kink angle, and fiber length distribution of pulp fiber 3 were determined using the same measurement methods as for pulp fibers 1 and 2 in Manufacturing Examples 1 and 2.

[0146] (Example 5) The above-mentioned (A) pulp fibers 3 and (B) powdered cellulose 1, (C) polylactic acid (PLA) as a thermoplastic resin (manufactured by NatureWorks, Ingeo, melting point 155-170°C), (D) MAPP as a compatibilizer resin (Yumex 100TS, manufactured by Sanyo Chemical Industries, Ltd., molecular weight 11000, melting point 136°C), and (F) antioxidant were mixed so that the solid content ratio of (A) / (B) / (C) / (D) / (F) was (21 / 5 / 11.7 / 4.33 / 0.87). (Note that the mass of (A) in this mass ratio is the mass of the absolute dry product.) The mass of water contained in (A) and (B) was 2% by mass relative to the total solid content mass of (A) to (D). The obtained mixture was placed in a kneader and kneaded at the maximum set temperature of 150°C to obtain a resin composition masterbatch. Furthermore, 42.9 parts of the obtained masterbatch and 57.1 parts of (C) polypropylene (PP) as the thermoplastic resin were mixed and placed in a kneader and kneaded at the set temperature of 160°C to obtain a resin composition. Next, this was pelletized using a pelletizer to obtain pelletized resin composition 5. The same materials as in Example 1 were used for (F) antioxidant and (C) polypropylene (PP) as the thermoplastic resin.

[0147] (Example 6) A resin composition masterbatch was obtained in the same manner as in Example 5, except that the solid content ratio of (A) / (B) / (C) / (D) / (F) was set to (16 / 10 / 11.7 / 4.33 / 0.87).

[0148] (Example 7) A resin composition masterbatch was obtained in the same manner as in Example 5, except that the solid content ratio of (A) / (B) / (C) / (D) / (F) was set to (11 / 15 / 11.7 / 4.33 / 0.87).

[0149] (Comparative Example 1) A pelletized resin composition 8 was obtained in the same manner as in Example 1, except that the solid content ratio of (A) / (B) / (C) / (D) / (E) / (F) was changed to (30 / 0 / 54 / 5 / 10 / 1).

[0150] (Preparation of evaluation specimens) 200 g of the pelletized resin composition obtained in the examples and comparative examples was placed into an injection molding machine (NEX50-IV manufactured by Nissei Plastic Industrial Co., Ltd.), and dumbbell-shaped test specimens (Type A1, JIS K 7139) were molded under the conditions of a heating cylinder temperature of 210°C and a mold temperature of 40°C.

[0151] (Tensile Test) The elastic modulus of the specimens obtained as described above was measured using a precision universal testing machine (Shimadzu Corporation's "Autograph AG-Xplus") at a test speed of 50 mm / min and an initial gauge length of 50 mm, and this was used as the tensile strength. The results are shown in Table 2.

[0152] (Measurement of flexural modulus and maximum stress) The elastic modulus and maximum stress were measured for the test specimens obtained as described above using a precision universal testing machine (Shimadzu Corporation's "Autograph AG-Xplus") at a test speed of 2 mm / min and a support distance of 64 mm. The results are shown in Table 2.

[0153] (Charpy Impact Strength Test) A 2 mm deep notch was inserted into the center of the test specimen obtained as described above. An impact test was performed on the notched test specimen according to JIS K 7111-1, and the Charpy impact strength was determined. A higher value indicates better impact resistance. The results are shown in Table 2.

[0154] (Fluidity Test (MFR)) 5 g of the pelletized resin composition (resin molded body) obtained in the examples and comparative examples was measured for MFR using a melt indexer ("Melt Indexer G-02" manufactured by Toyo Seiki Seisakusho Co., Ltd.) under the conditions of JIS K 6921-1.

[0155] (Test specimen density) The test specimens obtained as described above were measured using a dry automatic density meter, Accupic II 1340-10CC (manufactured by Shimadzu Corporation). The results are shown in Table 2.

[0156]

Claims

1. A resin composition comprising a plurality of cellulose materials, wherein the cellulose materials comprise at least: Component A: Pulp fibers with an average aspect ratio of 10 or more; and Component B: Powdered cellulose with an average L / D (long axis / short axis ratio) of less than 10.

2. The resin composition according to claim 1, characterized in that component A has an average kink angle of 55 degrees or more.

3. The resin composition according to claim 1, characterized in that the particle size distribution span of component B is in the range of 1.5 to 9.

4. The resin composition according to any one of claims 1 to 3, characterized in that the total amount of component A and component B is 80% by mass or more of the total mass of the cellulose material, and the content satisfies the condition that component A ≥ component B.

5. The resin composition according to any one of claims 1 to 3, characterized in that the cellulose material is contained in the resin composition in an amount of 5 to 35% by mass.

6. A method for producing a resin composition comprising a plurality of cellulose materials and a thermoplastic resin, wherein the cellulose material comprises at least: Component A: pulp fibers having an average aspect ratio of 10 or more; and Component B: powdered cellulose having an average L / D (long axis / short axis ratio) of less than 10, wherein Component A is obtained by crushing pulp, and Component B is obtained by grinding pulp, and the method is characterized by mixing Component A, Component B and the thermoplastic resin and then heating and kneading.