Repairable underfill material, electronic component device, method for opening electronic component device, method for repairing electronic component device, and method for manufacturing electronic component device
A repairable underfill material with a surfactant content allows for easy peeling from the substrate, addressing the challenge of substrate damage during repair, thereby reducing costs by enabling component replacement in semiconductor devices.
Patent Information
- Application Number
- PCT/JP2026/013909
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-04-01
- Publication Date
- 2026-11-12
AI Technical Summary
Existing underfill materials used in semiconductor devices are difficult to remove without damaging the substrate, making it challenging to repair connection defects, leading to increased manufacturing costs due to the need to replace entire modules.
A repairable underfill material containing a thermosetting compound and a surfactant, with the surfactant present in an amount of 5 parts by mass or more per 100 parts by mass, which allows for easy peeling from the substrate by heating above the solder melting point.
The material enables easy removal of the sealing portion from the substrate, facilitating the repair of faulty components without damaging the substrate, thus reducing manufacturing costs.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Repairable underfill material, electronic component device, method for opening an electronic component device, method for repairing an electronic component device, and method for manufacturing an electronic component device.
[0001] This disclosure relates to a repairable underfill material, an electronic component device, a method for opening an electronic component device, a method for repairing an electronic component device, and a method for manufacturing an electronic component device.
[0002] Underfill materials are widely used in semiconductor devices with bare chip mounting, such as COB (Chip on Board), COG (Chip on Glass), and TCP (Tape Carrier Package). Furthermore, in semiconductor devices (also called flip-chip devices) in which semiconductor elements are directly bump-connected to a wiring board made of ceramic, glass epoxy resin, glass imide resin, polyimide film, etc., underfill materials are used to fill the gap between the bump-connected semiconductor elements and the wiring board.
[0003] While sealing the connection area with the cured underfill material improves connection reliability, it becomes difficult to replace (repair) faulty chips or other components if connection defects are discovered during post-sealing inspection. Because the cured underfill material generally has high adhesive strength to the wiring board, it is difficult to remove it without damaging the board. Therefore, if even one connection defect is discovered, the entire module must be replaced or discarded, leading to increased manufacturing costs.
[0004] Against this backdrop, there is a demand for repairable underfill materials. For example, Patent Document 1 discloses an epoxy resin composition containing an epoxy curing agent represented by the following general formula (1) as an underfill material for repair. The explanation of the symbols in general formula (1) is omitted.
[0005]
[0006] Since epoxy curing agents represented by general formula (1) have a diacylhydrazine bond, certain oxidizing agents (e.g., NaOCl, H) are not suitable for use with them. 2 O 2It is said to be oxidatively decomposable by (etc.). Furthermore, the cured product of the epoxy resin composition described in Patent Document 1 has a glass transition temperature below the melting point of solder and is oxidatively decomposable by a specific oxidizing agent, and is therefore said to have excellent repairability.
[0007] Japanese Patent Publication No. 2011-236381
[0008] Patent Document 1 describes a semiconductor device repair method comprising: a removal step of heating the repair target area of the semiconductor device to remove the semiconductor element from the substrate; a decomposition step of decomposing the cured epoxy resin composition adhering to at least one of the substrate side and the semiconductor element side with an oxidizing agent solution; and a removal step of removing the remaining decomposed cured material from at least one of the substrate side and the semiconductor element side with a solvent. Thus, in Patent Document 1, since the cured epoxy resin composition adheres to the substrate after removal, it is necessary to decompose and remove this adhering material with an oxidizing agent solution. Furthermore, because the adhesive force of the cured epoxy resin composition is strong, the substrate is easily damaged when removing the semiconductor element from the substrate.
[0009] In view of these circumstances, the object of this disclosure is to provide a repairable underfill material that exhibits excellent peelability of the formed sealing portion from the substrate, an electronic component device, a method for opening an electronic component device, a method for repairing an electronic component device, and a method for manufacturing an electronic component device.
[0010] The means for solving the above problems include the following embodiments: <1> A repairable underfill material containing a thermosetting compound and a surfactant, wherein the surfactant is contained in an amount of 5 parts by mass or more per 100 parts by mass of the thermosetting compound. <2> The repairable underfill material according to <1>, wherein the surfactant contains silicone oil. <3> The repairable underfill material according to <2>, wherein the silicone oil contains polyether-modified silicone oil. <4> The repairable underfill material according to any one of <1> to <3>, further comprising an inorganic filler. <5> The repairable underfill material according to <4>, wherein the inorganic filler content is 20% by mass or more. <6> The repairable underfill material according to any one of <1> to <5>, wherein the linear thermal expansion coefficient (CTE2) in the range of 180°C to 200°C when cured is 50 ppm / °C to 170 ppm / °C. <7> An electronic component device comprising: an electronic component; a substrate electrically connected to the electronic component via a connection portion; and a sealing portion containing a cured product of the repairable underfill material described in any one of <1> to <6> that seals the connection portion. <8> A method for opening an electronic component device, comprising heating the electronic component device described in <7> to a temperature higher than the melting point of the solder forming the connection portion, and peeling the sealing portion from the substrate to open it. <9> A method for repairing an electronic component device, comprising removing an electronic component with poor conductivity from the opening portion opened by the method for opening an electronic component device described in <8>. <10> A method for repairing an electronic component device, comprising replacing the electronic component with a new one after removing the electronic component with poor conductivity. <11> A method for manufacturing an electronic component device, comprising the step of forming a sealing portion that seals the connection portion between the electronic component and the substrate electrically connected to the electronic component via a connection portion with the repairable underfill material described in any one of <1> to <6>. <12> A method for manufacturing an electronic component device according to <11>, further comprising: heating the solder forming the connection to a temperature higher than the melting point of the solder, peeling the sealing portion from the substrate and opening it; and removing the electronic component with poor conductivity from the opened portion obtained by peeling the sealing portion from the substrate and replacing it with a new electronic component.
[0011] According to this disclosure, a repairable underfill material with excellent peelability of the formed sealing portion from the substrate, an electronic component device, a method for opening an electronic component device, a method for repairing an electronic component device, and a method for manufacturing an electronic component device are provided.
[0012] In this disclosure, the term "process" includes not only processes that are independent of other processes, but also processes that cannot be clearly distinguished from other processes, provided that the purpose of the process is achieved. In this disclosure, numerical ranges indicated using "~" include the numbers before and after "~" as the minimum and maximum values, respectively. In numerical ranges described in stages in this disclosure, the upper or lower limit of one numerical range may be replaced by the upper or lower limit of another numerical range described in stages. Also, in numerical ranges described in this disclosure, the upper or lower limit of that numerical range may be replaced by the values shown in the examples. In this disclosure, each component may contain multiple types of the corresponding substance. If multiple types of the substance corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple types of substances present in the composition, unless otherwise specified. In this disclosure, each component may contain multiple types of particles. If multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified. In this disclosure, "(meth)acrylic" means at least one of acrylic or methacrylic, "(meth)acrylate" means at least one of acrylate or methacrylate, "(meth)acryloyl" means at least one of acryloyl or methacryloyl, and "(meth)acryloxy" means at least one of acryloxy or methacryloxy.
[0013] <Repairable Underfill Material> The repairable underfill material of this disclosure (hereinafter also simply referred to as "underfill material") contains a thermosetting compound and a surfactant, wherein the surfactant is present in an amount of 5 parts by mass or more per 100 parts by mass of the thermosetting compound. The repairable underfill material may further contain other components as needed.
[0014] Furthermore, the underfill material of this disclosure is preferably liquid at room temperature (25°C). Specifically, being liquid at room temperature (25°C) means that the viscosity measured by an E-type viscometer at 25°C is 1000 Pa·s or less.
[0015] The underfill material of this disclosure exhibits excellent peelability of the cured sealing portion from the substrate. The reason for this is not entirely clear, but it is thought to be as follows: The underfill material of this disclosure contains 5 parts by mass or more of a surfactant. When the sealing portion formed by this underfill material is heated during opening, the surfactant is likely to seep into the interface with the substrate, making it easy to peel from the substrate. The surfactant has an excellent balance of being compatible with the cured product of the thermosetting compound and easily moving to the interface with the substrate when heated during peeling.
[0016] The following describes each component contained in the underfill material of this disclosure.
[0017] [Thermosetting Compounds] The underfill material contains thermosetting compounds. Examples of thermosetting compounds include epoxy resins, polyurethane resins, radical polymerizable compounds, and anionic polymerizable compounds. Among these, epoxy resins or radical polymerizable compounds are preferred. Epoxy resins are suitable because they not only offer a good balance of various properties, but also possess excellent electrical properties, moisture resistance, heat resistance, mechanical properties, and adhesion to inserts, which are necessary for manufacturing highly reliable semiconductor devices. Radical polymerizable compounds are also suitable because they exhibit excellent injection properties due to suppressed viscosity increase during heating during injection.
[0018] (Epoxy resin) Any epoxy resin commonly used can be used without particular limitations, and it is preferable that the epoxy resin has two or more epoxy groups in one molecule.
[0019] As long as the underfill material as a whole is liquid at room temperature, the epoxy resin may be solid or liquid at room temperature, or both may be used in combination. From the viewpoint of reducing the viscosity of the underfill material, it is preferable to use an epoxy resin that is liquid at room temperature.
[0020] The underfill material of this disclosure may use a solid epoxy resin, provided that the desired effect is achieved. In this case, from the viewpoint of fluidity during molding, it is preferable that the content of the solid epoxy resin be 20% by mass or less of the total amount of epoxy resin.
[0021] The epoxy resins include novolac-type epoxy resins (phenol novolac-type epoxy resins, orthocresol novolac-type epoxy resins, etc.) obtained by condensing or co-condensing a novolac resin obtained by condensing or co-condensing a phenolic compound selected from the group consisting of phenol compounds such as phenol, cresol, xylenol, resorcinol, catechol, bisphenol A, bisphenol F, and naphthol compounds such as α-naphthol, β-naphthol, and dihydroxynaphthalene, with an aliphatic aldehyde compound such as formaldehyde, acetaldehyde, or propionaldehyde under an acidic catalyst; triphenylmethane-type epoxy resins obtained by condensing or co-condensing a triphenylmethane-type phenolic resin obtained by condensing or co-condensing the above phenolic compound with an aromatic aldehyde compound such as benzaldehyde or salicylaldehyde under an acidic catalyst; and novolac resins obtained by co-condensing the above phenolic compound and naphthol compound with an aldehyde compound under an acidic catalyst. Copolymer epoxy resins that are phenylated; diphenylmethane-type epoxy resins that are diglycidyl ethers of bisphenol A, bisphenol F, etc.; biphenyl-type epoxy resins that are diglycidyl ethers of alkyl-substituted or unsubstituted biphenols; stilbene-type epoxy resins that are diglycidyl ethers of stilbene-based phenol compounds; sulfur atom-containing epoxy resins that are diglycidyl ethers of bisphenol S, etc.; epoxy resins that are glycidyl ethers of alcohols such as butanediol, polyethylene glycol, and polypropylene glycol; glycidyl ester-type epoxy resins that are glycidyl esters of polycarboxylic acid compounds such as phthalic acid, isophthalic acid, and tetrahydrophthalic acid; glycidylamine-type epoxy resins in which the active hydrogen bonded to the nitrogen atom of aniline, diaminodiphenylmethane, isocyanuric acid, etc. is substituted with a glycidyl group; dicyclopentadiene-type epoxy resins that are epoxidized from a co-condensation resin of dicyclopentadiene and a phenol compound;alicyclic epoxy resins such as vinylcyclohexene diepoxide obtained by epoxidizing the intramolecular olefin bond, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, 2-(3,4-epoxy)cyclohexyl-5,5-spiro(3,4-epoxy)cyclohexane-m-dioxane; para-xylylene-modified epoxy resins which are glycidyl ethers of para-xylylene-modified phenol resins; meta-xylylene-modified epoxy resins which are glycidyl ethers of meta-xylylene-modified phenol resins; terpene-modified epoxy resins which are glycidyl ethers of terpene-modified phenol resins; dicyclopentadiene-modified epoxy resins which are glycidyl ethers of dicyclopentadiene-modified phenol resins; cyclopentadiene-modified epoxy resins which are glycidyl ethers of cyclopentadiene-modified phenol resins; polycyclic aromatic ring-modified epoxy resins which are glycidyl ethers of polycyclic aromatic ring-modified phenol resins; naphthalene-type epoxy resins which are glycidyl ethers of naphthalene ring-containing phenol resins; halogenated phenol novolac-type epoxy resins; hydroquinone-type epoxy resins; trimethylolpropane-type epoxy resins; linear aliphatic epoxy resins obtained by oxidizing an olefin bond with a peracid such as peracetic acid; aralkyl-type epoxy resins obtained by epoxidizing aralkyl-type phenol resins such as phenol aralkyl resins and naphthol aralkyl resins; and the like. Further, aminophenol-type epoxy resins which are glycidyl ethers of aminophenols and the like are also mentioned as epoxy resins. The epoxy resins may be used singly or in combination of two or more kinds.;
[0022] The epoxy equivalent (molecular weight / number of epoxy groups) of the epoxy resin is not particularly limited. From the viewpoint of the balance of various properties such as moldability, reflow resistance, and electrical reliability, it is preferably 100 g / eq to 1000 g / eq, and more preferably 150 g / eq to 600 g / eq. In the present disclosure, the epoxy equivalent of the epoxy resin is a value measured by a method in accordance with JIS K 7236:2009.
[0023] The softening point or melting point of the epoxy resin is not particularly limited. From the viewpoints of moldability and reflow resistance, the softening point or melting point of the epoxy resin is preferably 40°C to 180°C, more preferably 50°C to 130°C from the viewpoint of handleability during the preparation of the underfill material, even more preferably liquid at normal temperature, and from this viewpoint, the melting point is particularly preferably 25°C or lower. The melting point or softening point of the epoxy resin is a value measured by the single-cylinder rotational viscometer method described in JIS K 7234:1986 and JIS K 7233:1986.
[0024] The amount of hydrolyzable chlorine, which is one of the indicators of the purity of the epoxy resin, is preferably 500 ppm or less, more preferably 300 ppm or less, from the viewpoint of suppressing corrosion of wiring on semiconductor elements such as ICs and obtaining an underfill material with excellent moisture resistance. The hydrolyzable chlorine amount is a value scaled by the value obtained by potentiometric titration after dissolving 1 g of epoxy resin in 30 ml of dioxane, adding 5 ml of 1N KOH methanol solution and refluxing for 30 minutes.
[0025] Further, it is also preferred that the epoxy resin includes an epoxy resin having an epoxy equivalent of 300 g / eq to 600 g / eq. The epoxy resin having an epoxy equivalent of 300 g / eq to 600 g / eq is preferably an epoxy resin of 350 g / eq to 550 g / eq, more preferably an epoxy resin having an epoxy equivalent of 400 g / eq to 500 g / eq. When the epoxy resin contains an epoxy resin having an epoxy equivalent of 300 g / eq to 600 g / eq, the temperature cycle resistance tends to be further improved. Although the reason for this is not necessarily clear, it is presumed that the use of the epoxy resin having an epoxy equivalent of 300 g / eq to 600 g / eq reduces the density between crosslinking points, thereby lowering the elastic modulus and improving the toughness.
[0026] The epoxy resin with an epoxy equivalent weight of 300 g / eq to 600 g / eq is preferably at least one selected from the group consisting of epoxy resins having a polyether skeleton, epoxy resins having a fluorene structure, epoxy resins having a long-chain alkyl group, epoxy resins having a siloxane skeleton, epoxy resins having a bisphenol A skeleton, and epoxy resins having a bisphenol F skeleton, from the viewpoint of temperature cycling resistance.
[0027] Among these, epoxy resins with an epoxy equivalent of 300 g / eq to 600 g / eq are preferably epoxy resins having a polyether skeleton. When the epoxy resin has an epoxy equivalent of 300 g / eq to 600 g / eq and contains an epoxy resin having a polyether skeleton, the fracture energy tends to improve and the temperature cycling resistance tends to improve further. The reason for this is not entirely clear, but it is presumed that because epoxy resins having a polyether skeleton are flexible, the elastic modulus decreases and the toughness improves. The polyether skeleton is not particularly limited, and examples include polyalkylene oxide structures.
[0028] When the epoxy resin contains epoxy resin with an epoxy equivalent of 300 g / eq to 600 g / eq, the content of epoxy resin with an epoxy equivalent of 300 g / eq to 600 g / eq relative to the total amount of epoxy resin is not particularly limited. From the viewpoint of temperature cycling resistance, the content is preferably 0.1 parts by mass to 40 parts by mass, more preferably 1 part by mass to 30 parts by mass, and even more preferably 5 parts by mass to 20 parts by mass, per 100 parts by mass of the total epoxy resin. When the content of epoxy resin with an epoxy equivalent of 300 g / eq to 600 g / eq is 0.1 parts by mass to 40 parts by mass per 100 parts by mass of the total epoxy resin, it tends to be possible to improve temperature cycling resistance while maintaining the properties of the underfill material, such as fluidity and linear thermal expansion coefficient, within a desirable range.
[0029] The epoxy resin content in the underfill material is not particularly limited. From the viewpoint of viscosity, glass transition temperature, heat resistance, etc., it is preferably 0.5% to 50% by mass, more preferably 2% to 40% by mass, and even more preferably 2% to 30% by mass.
[0030] [Radical Polymerizable Compounds] Radical polymerizable compounds are not particularly limited, but compounds having an unsaturated double bond in the molecule are preferred. Examples of radical polymerizable compounds include redox polymerizable compounds, emulsion polymerizable compounds, and (meth)acrylate compounds. Radical polymerizable compounds may be used individually or in combination of two or more.
[0031] Considering applicability to electronic components and devices, controllability of curing speed, and handling of underfill material, the radical polymerizable compound preferably contains at least one selected from the group consisting of (meth)acrylic compounds and maleimide compounds, and more preferably contains at least a maleimide compound. From the viewpoint of adhesive strength with the package substrate, the combined use of (meth)acrylic compounds and maleimide compounds is also one of the preferred embodiments.
[0032] The radical polymerizable compound may include other radical polymerizable compounds besides (meth)acrylic compounds and maleimide compounds. Examples of other radical polymerizable compounds include vinyl compounds.
[0033] The total content of (meth)acrylic compounds and maleimide compounds in the underfill material is preferably 40% by mass or more, more preferably 60% by mass or more, even more preferably 80% by mass or more, and may be 100% by mass.
[0034] (Maleimide Compounds) Maleimide compounds as radical polymerizable compounds can be any compound having a maleimide group in one molecule, and may be used alone or in combination of two or more.
[0035] Maleimide compounds preferably have a melting point of 150°C or lower. Since maleimide compounds are usually solids, it is preferable to have them in a molten state when using them as underfill materials. One method for moltening maleimide compounds is to heat a mixture of (meth)acrylic compounds and maleimide compounds to near the melting point of the maleimide compound to make it compatible with the (meth)acrylic compound. Since (meth)acrylic compounds and maleimide compounds undergo an ene reaction and thicken at 150°C to 250°C, the temperature at which the maleimide compound is heated to dissolve is preferably 150°C or lower, and therefore, maleimide compounds having a melting point of 150°C or lower are preferred.
[0036] The maleimide compound may be a polyfunctional maleimide compound having at least two maleimide groups in one molecule, or a monofunctional maleimide compound having one maleimide group in one molecule. The polyfunctional maleimide compound and the monofunctional maleimide compound may be used independently or in combination.
[0037] Examples of polyfunctional maleimide compounds include bismaleimide compounds represented by the following general formula (I) and maleimide compounds represented by the following general formula (II).
[0038]
[0039] In general formula (I), R 1 This represents a divalent hydrocarbon group having 1 to 18 carbon atoms, which may have substituents.
[0040] In general formula (I), R 1 The divalent hydrocarbon group having 1 to 18 carbon atoms, which may have substituents represented by , preferably includes a divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms, an alicyclic hydrocarbon group having 3 to 18 carbon atoms, and an aromatic hydrocarbon group having 6 to 18 carbon atoms.
[0041] R 1The divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms represented by is preferably a divalent aliphatic hydrocarbon group having 1 to 14 carbon atoms, and more preferably a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms. Specific examples of the divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms include methylene group, ethylene group, propylene group, isopropylene group, butylene group, pentylene group, hexylene group, octylene group, decylene group, dodecylene group, vinylene group, ethylidene group, vinylidene group, propenylene group, butadienylene group and the like. As the divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms, methylene group, ethylene group, propylene group, isopropylene group, butylene group or hexylene group is preferred, and methylene group, ethylene group, propylene group, isopropylene group or butylene group is more preferred.
[0042] R 1 The divalent alicyclic hydrocarbon group having 3 to 18 carbon atoms represented by is preferably a divalent alicyclic hydrocarbon group having 3 to 14 carbon atoms, and more preferably a divalent alicyclic hydrocarbon group having 5 to 12 carbon atoms. Specific examples of the divalent alicyclic aliphatic hydrocarbon group having 3 to 18 carbon atoms include cyclopentylene group, cyclohexylene group, cycloheptylene group, cyclopentenylene group, cyclohexenylene group, cyclohexylidene group and the like.
[0043] R 1 The divalent aromatic hydrocarbon group having 6 to 18 carbon atoms represented by is preferably a divalent aromatic hydrocarbon group having 6 to 14 carbon atoms, and more preferably a divalent aromatic hydrocarbon group having 6 to 12 carbon atoms. Specific examples of the divalent aromatic hydrocarbon group having 6 to 18 carbon atoms include phenylene group, biphenylylene group, terphenylene group and the like.
[0044] Among them, R in the general formula (I) 1 is more preferably a divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms which may have a substituent or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and even more preferably a divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms which may have a substituent.
[0045] R in the general formula (I) 1The substituents that may be present include alkyl groups, alkoxy groups, aryl groups, aryloxy groups, hydroxyl groups, amino groups, halogen atoms, methacrylate groups, mercapto groups, imino groups, ureido groups, isocyanate groups, and the like. 1 It is preferable that it does not have substituents.
[0046] Examples of bismaleimide compounds represented by general formula (I) include 4,4'-diphenylmethanebismaleimide, m-phenylenebismaleimide, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethanebismaleimide, 4-methyl-1,3-phenylenebismaleimide, and 1,6'-bismaleimide-(2,2,4-trimethyl)hexane.
[0047]
[0048] In general formula (II), n is 0 or an integer greater than or equal to 1.
[0049] Examples of bismaleimide compounds represented by general formula (II) include phenylmethanemaleimide.
[0050] (Meth)acrylic compounds) The (meth)acrylate compounds used as radical polymerizable compounds are not particularly limited, and conventionally known (meth)acrylate compounds can be used. One (meth)acrylate compound may be used alone, or two or more may be used in combination. When two or more (meth)acrylate compounds are used in combination, the combination of (meth)acrylate compounds is not particularly limited. From the viewpoint of dispensability, it is preferable to use at least one polyfunctional (meth)acrylate compound containing at least two (meth)acryloyl groups in one molecule and at least one monofunctional (meth)acrylate compound containing one (meth)acryloyl group in one molecule in combination. Doing so often results in a low viscosity underfill material, which tends to improve injectability.
[0051] Examples of polyfunctional (meth)acrylate compounds include diethylene glycol diacrylate, triethylene glycol diacrylate, tripropylene glycol diacrylate, tetraethylene glycol diacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, polyethylene glycol diacrylate, polypropylene glycol diacrylate, tricyclodecane dimethylol diacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, tris(β-hydroxyethyl) isocyanurate triacrylate, polycarbonate acrylate, urethane acrylate, and diethylene Examples include methyl glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, polyethylene glycol dimethacrylate, polypropylene glycol dimethacrylate, tricyclodecane dimethylol dimethacrylate, ditrimethylolpropane tetramethacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, dipentaerythritol hexamethacrylate, tris(β-hydroxyethyl) isocyanurate trimethacrylate, polycarbonate methacrylate, urethane methacrylate, and difunctional (meth)acrylate compounds represented by the following formula (II).
[0052] Among these, examples include compounds having an aliphatic cyclic skeleton and at least two (meth)acryloyloxy groups (hereinafter sometimes referred to as alicyclic monomers), and compounds having two (meth)acryloyloxy groups in the molecule, with the two (meth)acryloyloxy groups linked by a linear divalent organic group (hereinafter sometimes referred to as linear monomers). These are polyfunctional (meth)acrylate compounds because they contain two (meth)acryloyl groups in one molecule.
[0053] Alicyclic monomers and linear monomers may be used individually or in combination. From the viewpoint of the linear thermal expansion coefficient of the cured product, it is preferable to include at least alicyclic monomers. The ratio of alicyclic monomers to the total amount of alicyclic monomers and linear monomers is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and may be 100% by mass.
[0054] The aliphatic cyclic skeleton contained in the alicyclic monomer is not particularly limited, and examples include the tricyclodecane skeleton, cyclohexane skeleton, cyclopentane skeleton, 1,3-adamantane skeleton, hydrogenated bisphenol A skeleton, hydrogenated bisphenol F skeleton, hydrogenated bisphenol S skeleton, isobornyl skeleton, etc. Among these, the tricyclodecane skeleton is preferred.
[0055] As the alicyclic monomer, compounds represented by the following general formula (1) are preferred.
[0056]
[0057] In general formula (1), R 1 and R 2 Each of these is independently an aliphatic hydrocarbon group having 1 to 4 carbon atoms or a group represented by the following general formula (2). n1 represents 0 or 1, n2 represents an integer from 0 to 2, and n1 + n2 is 2 or 3. n1 R 1 and n2 R 2 At least two of these are groups represented by the following general formula (2).
[0058]
[0059] In general formula (2), R 1A represents a hydrogen atom or a methyl group, and m represents an integer from 1 to 10.
[0060] R 1 and R 2 Specific examples of aliphatic hydrocarbon groups having 1 to 4 carbon atoms, represented by , include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, and the like.
[0061] The compound represented by general formula (1) may also be a compound represented by the following formula (3A) or formula (3B).
[0062]
[0063] Examples of compounds represented by formula (3A) include tricyclodecanedimethanol diacrylate, and examples of compounds represented by formula (3B) include tricyclodecanedimethanol dimethacrylate.
[0064] The linear monomer is preferably a compound represented by the following general formula (4) or the following general formula (5).
[0065]
[0066] In general formula (4) or general formula (5), R 3 Each of these independently represents either a hydrogen atom or a methyl group, R 4 R represents an alkylene group with 1 to 8 carbon atoms. 5 R represents an alkylene group with 1 to 8 carbon atoms, and p represents an integer from 2 to 5. 3 and R 5 They may be the same or they may be different.
[0067] R in general formula (4) or general formula (5) 3 A methyl group is preferred as the component. R in general formula (4) 4 Specific examples of alkylene groups having 1 to 8 carbon atoms represented by include methylene group, ethylene group, trimethylene group, tetramethylene group, hexamethylene group, octamethylene group, etc. R in general formula (5) 5Specific examples of alkylene groups having 1 to 8 carbon atoms represented by the formula include methylene, ethylene, trimethylene, methylethylene, dimethylmethylene, tetramethylene, hexamethylene, and octamethylene groups, with methylethylene and ethylene groups being preferred, and ethylene groups being more preferred. In general formula (5), p is preferably an integer between 3 and 4.
[0068] Examples of linear monomers include diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, tripropylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,4-butanediol dimethacrylate, and 1,6-hexanediol dimethacrylate.
[0069] Examples of monofunctional (meth)acrylate compounds include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, and octyl (meth)acrylate. Acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, hexadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, tricyclo[5.2.1.0 2,6 Decyl (meth)acrylate, 2-(tricyclo) [5.2.1.0 2,6 Deca-3-en-8-yloxyethyl (meth)acrylate, 2-(tricyclo)[5.2.1.0 2,6Deca-3-en-9-yloxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, dimergol mono (meth)acrylate, diethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, 2-phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxy Polyethylene glycol (meth)acrylate, 2-benzoyloxyethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, benzyl (meth)acrylate, 2-cyanoethyl (meth)acrylate, γ-(meth)acryloyloxypropyltrimethoxysilane, glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, tetrahydropyranyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, 1,2,2,6,6-pentamethylpiperidyl (meth)acrylate, 2,2,6,Examples include 6-tetramethylpiperidinyl (meth)acrylate, (meth)acryloxyethyl phosphate, (meth)acryloxyethyl phenyl acid phosphate, β-(meth)acryloyloxyethyl hydrogen phthalate, β-(meth)acryloyloxyethyl hydrogen succinate, and ethylene oxide-modified neopentyl glycol (meth)acrylate, 2-(meth)acryloyloxyethyl succinate, 2-methacryloyloxyethyl hexahydrophthalate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, and neopentyl glycol (meth)acrylic acid benzoate. ,
[0070] (Meth)acrylic compounds may contain other polymerizable functional groups besides the (meth)acrylic group. Examples of other polymerizable functional groups include glycidyl groups, amino groups, and hydroxyl groups. These functional groups work together with the packaging substrate to increase the adhesive strength to the substrate. Examples of such compounds include 4-hydroxybutyl acrylate glycidyl ether (4HBAGE), 4-hydroxybutyl acrylate (4HBA), and 1,4-cyclohexanedimethanol monoacrylate (CHDMMA). It is desirable not to use other polymerizable functional groups in combination that polymerize, from the viewpoint of suppressing viscosity increase during filling. Examples of polymerizable combinations include epoxy groups and amino groups, and epoxy groups and hydroxyl groups.
[0071] When at least one polyfunctional (meth)acrylate compound and at least one monofunctional (meth)acrylate compound are used in combination as radical polymerizable compounds, the content of the monofunctional (meth)acrylate compound relative to the total amount of polyfunctional (meth)acrylate compounds is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, from the viewpoint of achieving a low modulus of elasticity. Furthermore, the content of the monofunctional (meth)acrylate compound relative to the total amount of polyfunctional (meth)acrylate compounds is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, from the viewpoint of lowering the linear thermal expansion coefficient of the cured product.
[0072] When a maleimide compound and a (meth)acrylate compound are used in combination as a radical polymerizable compound, the content of the maleimide compound relative to the total amount of the maleimide compound and the (meth)acrylate compound is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, from the viewpoint of adhesion to the semiconductor package substrate. Furthermore, from the viewpoint of reducing viscosity, the content of the maleimide compound relative to the total amount of the maleimide compound and the (meth)acrylate compound is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less.
[0073] Examples of radical polymerizable compounds include forms in which a polyfunctional maleimide compound is used alone, forms in which a (meth)acrylate compound is used alone, forms in which a polyfunctional maleimide compound and a polyfunctional (meth)acrylate compound are used in combination, and forms in which a polyfunctional maleimide compound, a polyfunctional (meth)acrylate compound, and a monofunctional (meth)acrylate compound are used in combination. Among these, the form in which a polyfunctional maleimide compound, a polyfunctional (meth)acrylate compound, and a monofunctional (meth)acrylate compound are used in combination is preferred from the viewpoint of achieving both low viscosity and adhesion.
[0074] When a polyfunctional maleimide compound and a polyfunctional (meth)acrylate compound are used in combination as radical polymerizable compounds, the content of the polyfunctional maleimide compound relative to the total amount of the polyfunctional maleimide compound and the polyfunctional (meth)acrylate compound is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, from the viewpoint of adhesion to the semiconductor package substrate. Furthermore, the content of the polyfunctional maleimide compound relative to the total amount of the polyfunctional maleimide compound and the polyfunctional (meth)acrylate compound is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less, from the viewpoint of reducing viscosity.
[0075] [Other Polymerizable Compounds] The underfill material may contain other polymerizable compounds besides radical polymerizable compounds. Examples of polymerizable functional groups in other polymerizable compounds include glycidyl groups, amino groups, and hydroxyl groups. Other polymerizable compounds may be monofunctional or polyfunctional. From the viewpoint of suppressing viscosity increase during filling, it is desirable not to use other polymerizable compounds in combination that polymerize. Examples of polymerizable combinations include epoxy groups and amino groups, and epoxy groups and hydroxyl groups. Since other polymerizable compounds do not have radical polymerizable functional groups, they may seep into the interface with the substrate during the curing process. From the viewpoint of preventing seepage, it is preferable that other polymerizable compounds are not included, or if other polymerizable compounds are included, the content of other polymerizable compounds relative to the total amount of other polymerizable compounds and radical polymerizable compounds is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less.
[0076] The content of radical polymerizable compounds in the underfill material is not particularly limited. From the viewpoint of viscosity, glass transition temperature, heat resistance, etc., it is preferably 0.5% to 50% by mass, more preferably 2% to 40% by mass, and even more preferably 2% to 30% by mass.
[0077] [Surfactants] The underfill material contains surfactants. Examples of surfactants include silicone oil, higher fatty acid esters, phosphate esters, and polyacrylates, with silicone oil being preferred from the viewpoint of ease of opening defective chips. The silicone oil is preferably a polyether-modified silicone oil, and more preferably a silicone oil having polyether moieties in its side chains. The polyether moieties preferably include at least one selected from the group consisting of ethylene oxy moieties and propylene oxy moieties. The ethylene oxy moieties and propylene oxy moieties may be connected to silicon atoms via linking groups.
[0078] The silicone oil may further have amine moieties in its side chains.
[0079] The main chain of the silicone oil may be dimethyl silicone, diphenyl silicone, or methylphenyl silicone, but dimethyl silicone is preferred.
[0080] The viscosity of the surfactant at 25°C is 500 mm². 2 / s ~ 5000mm 2 It is preferable that it be / s, and 1000 mm 2 / s ~ 4500mm 2 It is more preferable that it be / s, 1500 mm 2 / s ~ 4200mm 2 It is even more preferable that the viscosity of the surfactant at 25°C is within the above range. When the cured underfill material is heated during rework, the amount of surfactant seeping into the interface with the substrate is appropriate, and the cured underfill material tends to peel off easily from the substrate.
[0081] The weight-average molecular weight (Mw) of the surfactant is preferably 500 or more, more preferably 750 or more, and even more preferably 1000 or more. When the Mw of the surfactant is within the above range, excessive seepage of the surfactant to the interface with the substrate is avoided, and the cured underfill material tends to peel off easily from the substrate. The weight-average molecular weight (Mw) of the surfactant is preferably 50,000 or less, more preferably 40,000 or less, and even more preferably 30,000 or less. When the Mw of the surfactant is within the above range, the surfactant tends to seep more easily to the interface with the substrate, and the cured underfill material tends to peel off easily from the substrate.
[0082] The weight-average molecular weight refers to the weight-average molecular weight measured in polystyrene equivalent using gel permeation chromatography (for example, Shimadzu Corporation, product name "C-R4A").
[0083] The surfactant content is preferably 5 parts by mass or more, and more preferably 10 parts by mass or more, per 100 parts by mass of the thermosetting compound. Furthermore, from the viewpoint of maintaining adhesion with other components of the package, the surfactant content is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and more preferably 20 parts by mass or less, per 100 parts by mass of the thermosetting compound.
[0084] [Inorganic Filler] The underfill material may contain an inorganic filler. Examples of inorganic fillers include silica such as spherical silica, crystalline silica, and fused silica; powders of calcium carbonate, clay, alumina, silicon nitride, silicon carbide, boron nitride, calcium silicate, potassium titanate, aluminum nitride, beryllia, zirconia, zircon, fossterite, steatite, spinel, mullite, titania, etc., or beads or glass fibers made by shaping these into spheres. Furthermore, as an inorganic filler with flame retardant properties, aluminum hydroxide, magnesium hydroxide, zinc borate, zinc molybdate, etc. may be used. The inorganic filler may be used alone or in combination of two or more types. Among these, silica is preferred from the viewpoint of ease of availability, chemical stability, and material cost, and spherical silica is more preferred from the viewpoint of fluidity and permeability into the fine gaps of the underfill material. Examples of spherical silica include silica obtained by deflagration and fused silica. The inorganic filler may be surface-treated beforehand using various surface treatment agents such as silane coupling agents, as described later.
[0085] The volume-average particle size of the inorganic filler is not particularly limited. For example, in the case of spherical silica, the volume-average particle size is preferably 0.1 μm to 10 μm, more preferably 0.2 μm to 7 μm, even more preferably 0.3 μm to 5 μm, and may also be 0.3 μm to 2.0 μm. When the volume-average particle size is 0.1 μm or more, it tends to have excellent dispersibility in the underfill material, is less likely to impart thixotropy to the underfill material, and has excellent flow characteristics. When the volume-average particle size is 10 μm or less, it tends to reduce the sedimentation of the inorganic filler in the underfill material, improve the permeability and fluidity into fine gaps of the underfill material, and prevent voids and unfilled areas. The volume-average particle size of the inorganic filler can be measured as the particle size (D50) when the cumulative amount from the small diameter side reaches 50% in the volume-based particle size distribution measured by a laser diffraction scattering particle size distribution analyzer.
[0086] The inorganic filler content is not particularly limited, but is preferably 20% by mass or more of the total underfill material, more preferably 25% by mass or more, and even more preferably 30% by mass or more. Furthermore, the inorganic filler content is preferably 80% by mass or less of the total underfill material, preferably 75% by mass or less, and even more preferably 70% by mass or less. When the inorganic filler content is 20% by mass or more, the linear thermal expansion coefficient is easily reduced, and when it is 80% by mass or less, the increase in viscosity of the underfill material is easily suppressed, and the fluidity, permeability, and dispensability tend to be good.
[0087] [Curing Agent] When using epoxy resin as the thermosetting compound, a curing agent may be included. The curing agent can be any curing agent commonly used for epoxy resins without particular limitations. Examples include amine curing agents, phenol curing agents, acid anhydride curing agents, polymercaptan curing agents, polyaminoamide curing agents, isocyanate curing agents, blocked isocyanate curing agents, imidazole curing agents, etc. Among these, from the viewpoint of workability and compositional properties, at least one selected from the group consisting of amine curing agents, phenol curing agents, and acid anhydride curing agents is preferred, and amine curing agents are more preferred. The curing agent may be solid or liquid at room temperature, and is preferably liquid. The curing agent may be used alone or in combination of two or more types.
[0088] In particular, from the viewpoint of having excellent temperature cycle resistance, humidity resistance, etc., and improving the reliability of electronic component devices, the curing agent is preferably an aromatic amine, and more preferably an aromatic amine that is liquid at room temperature (also called a liquid aromatic amine). Examples of liquid aromatic amines include ethyltoluenediamine, diethyltoluenediamine (3,5-diethyltoluene-2,4-diamine and 3,5-diethyltoluene-2,6-diamine, etc.), 1-methyl-3,5-diethyl-2,4-diaminobenzene, 1-methyl-3,5-diethyl-2,6-diaminobenzene, 1,3,5-triethyl-2,6-diaminobenzene, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 3,5,3',5'-tetramethyl-4,4'-diaminodiphenylmethane, dimethylthiotoluenediamine, etc. The curing agent may be used alone or in combination of two or more types.
[0089] In particular, from the viewpoint of storage stability, 3,3'-diethyl-4,4'-diaminodiphenylmethane, ethyltoluenediamine, and dimethylthiotoluenediamine are preferred, and the curing agent is preferably composed mainly of one or a mixture of two or more of these.
[0090] Examples of commercially available aromatic amines include the liquid aromatic amines jER Cure W (manufactured by Mitsubishi Chemical Corporation, trade name), Kayahard A-A, Kayahard A-B, and Kayahard A-S (manufactured by Nippon Kayaku Co., Ltd., trade name), Totamine HM-205 (manufactured by Nippon Steel & Sumitomo Metal Corporation, trade name), Adeka Hardener EH-101 (manufactured by Adeka Corporation, trade name), Epomic Q-640 and Epomic Q-643 (manufactured by Mitsui Chemicals, Inc., trade name), and DETDA80 (manufactured by Lonza, trade name).
[0091] When using a liquid aromatic amine as a curing agent, other commonly used curing agents such as phenol curing agents and acid anhydride curing agents may be used in combination with the liquid aromatic amine. Alternatively, a solid curing agent may be used in combination with the liquid aromatic amine.
[0092] The functional group equivalent of the curing agent is not particularly limited. From the viewpoint of reactivity and compositional properties, the functional group equivalent is preferably 30 g / eq to 800 g / eq, and more preferably 35 g / eq to 700 g / eq. The functional group equivalent of the curing agent shall be a value measured by a method in accordance with JIS K 0070:1992.
[0093] When a curing agent is used, the amount of curing agent to be added to the epoxy resin is not particularly limited. In order to minimize the amount of unreacted components, the equivalent ratio of epoxy resin to curing agent, i.e., the ratio of the number of functional groups in the curing agent to the number of epoxy groups in the epoxy resin (number of functional groups in curing agent / number of epoxy groups in epoxy resin), is preferably 0.5 g / eq to 2.0 g / eq, more preferably 0.6 g / eq to 1.8 g / eq, and even more preferably 0.7 g / eq to 1.5 g / eq.
[0094] [Radical Polymerization Initiators] When using a radical polymerizable compound as a thermosetting compound, it is preferable to include a radical polymerization initiator. The radical polymerization initiator is not particularly limited, and conventionally known radical polymerization initiators can be used. Examples of radical polymerization initiators include organic peroxides, which will be described later; azo compounds such as azobisisobutyronitrile, azobis-4-methoxy-2,4-dimethylvaleronitrile, azobiscyclohexanone-1-carbonitride, and azodibenzoyl; potassium persulfate; and redox catalysts such as a combination of a water-soluble catalyst and a peroxide, or a combination of a persulfate and a reducing agent. The radical polymerization initiator may be used alone or in combination of two or more. In particular, from the viewpoint of storage stability, it is preferable to include at least one organic peroxide.
[0095] Examples of organic peroxides include ketone peroxides such as methyl ethyl ketone peroxide and cyclohexanone peroxide; peroxyketals such as 1,1-di(t-butylperoxy)cyclohexane and 2,2-di(4,4-di(t-butylperoxy)cyclohexyl)propane; hydroperoxides such as p-menthane hydroperoxide, diisopropylbenzene hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide; di(2-t-butylperoxyisopropyl)benzene, dicumyl peroxide, and 2,5-dimethyl-2,5-di(t-butylperoxy Examples include dialkyl peroxides such as hexane, t-butylcumyl peroxide, di-t-hexyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, and di-t-butyl peroxide; diacyl peroxides such as dibenzoyl peroxide and di(4-methylbenzoyl) peroxide; peroxydicarbonates such as di-n-propyl peroxydicarbonate and diisopropyl peroxydicarbonate; and peroxyesters such as 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-hexyl peroxybenzoate, t-butyl peroxybenzoate, and t-butyl peroxy 2-ethylhexanonate.
[0096] Among these, dialkyl peroxides having a phenyl group in the organic peroxide are particularly preferred from the viewpoint of temperature stability in the medium temperature range, and dicumyl peroxide and di(2-t-butylperoxyisopropyl)benzene are more preferred.
[0097] The content of the radical polymerization initiator in the underfill material is not particularly limited. For example, the content of the radical polymerization initiator is preferably 0.1 to 10 parts by mass per 100 parts by mass of the total radical polymerizable compound, and more preferably 0.5 to 5 parts by mass from the viewpoint of curability. When the content of the radical polymerization initiator is 10 parts by mass or less per 100 parts by mass of the total radical polymerizable compound, volatile matter is less likely to be generated and the generation of voids in the cured product tends to be suppressed. Furthermore, when the content of the radical polymerization initiator is 0.3 parts by mass or more per 100 parts by mass of the total radical polymerizable compound, the curability tends to improve.
[0098] The 10-hour half-life temperature of the radical polymerization initiator is preferably 90°C to 150°C, and more preferably 100°C to 140°C from the viewpoint of curability. If the 10-hour half-life temperature of the radical polymerization initiator is 90°C or higher, the start of the curing reaction of the underfill material tends to be suppressed even if the substrate with the underfill material supplied is left in a medium temperature range (for example, on a hot plate stage). If the 10-hour half-life temperature of the radical polymerization initiator is 150°C or lower, the curing rate of the underfill material in the high temperature range (the temperature at which electronic components and wiring boards are joined via the joint) tends to be faster. As a result, the generation of voids tends to be suppressed.
[0099] [Coupling Agent] The underfill material may contain a coupling agent as needed. When the underfill material contains a coupling agent, it tends to strengthen the interfacial adhesion between the epoxy resin and the inorganic filler, or between the epoxy resin and the components of the electronic parts. There are no particular restrictions on the type of coupling agent, and conventionally known ones can be used. Examples include silane compounds having primary and / or secondary and / or tertiary amino groups, epoxysilanes, mercaptosilanes, alkylsilanes, ureidosilanes, vinylsilanes, (meth)acrylsilanes, and various other silane compounds, titanium compounds, aluminum chelates, and aluminum / zirconium compounds. The coupling agent may be used alone or in combination of two or more types.
[0100] As coupling agents, for example, monomers or oligomers may be used. Examples of monomer coupling agents include vinyltrichlorosilane, vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, glycidoxyoctyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, vinyltriacetoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-anilinopropyltrimethoxysilane, γ-anilinopropyltriethoxysilane, γ-(N γ-(N,N-dimethyl)aminopropyltrimethoxysilane, γ-(N,N-diethyl)aminopropyltrimethoxysilane, γ-(N,N-dibutyl)aminopropyltrimethoxysilane, γ-(N-methyl)anilinopropyltrimethoxysilane, γ-(N,N-ethyl)anilinopropyltrimethoxysilane, γ-(N,N-dimethyl)aminopropyltriethoxysilane, γ-(N,N-diethyl)aminopropyltriethoxysilane, γ-(N,N-dibutyl)aminopropyltriethoxysilane, γ-(N-methyl)anilinopropyltriethoxysilane, γ-(N-ethyl)anilinopropyltriethoxysilane, γ-(N,N-dimethyl)aminopropylmethyldimethoxysilane, γ-(N,Silane coupling agents such as N-dibutyl)aminopropylmethyldimethoxysilane, γ-(N-methyl)anilinopropylmethyldimethoxysilane, γ-(N-ethyl)anilinopropylmethyldimethoxysilane, N-(trimethoxysilylpropyl)ethylenediamine, N-(dimethoxymethylsilylisopropyl)ethylenediamine, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, γ-chloropropyltrimethoxysilane, hexamethyldisilazane, vinyltrimethoxysilane, hexenyltrimethoxysilane, octenyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, methacryloxyoctyltrimethoxysilane, etc.; isopropyltriisostearoyl titanate, isopropyltris(dioctylpyrophosphate) titanate, isopropyltri(N-aminoethyl-aminoethyl) titanate, tetraoctylbis(ditridecylphosphite) titanate, tetra(2,2-diaryl Examples of titanate coupling agents include bis(ditridecyl phosphite) titanate, bis(dioctyl pyrophosphate) oxyacetate titanate, bis(dioctyl pyrophosphate) ethylene titanate, isopropyl trioctanoyl titanate, isopropyl dimethacrylate isostearoyl titanate, isopropyl tridodecylbenzenesulfonyl titanate, isopropyl isostearoyl diacrylic titanate, isopropyl tri(dioctyl phosphate) titanate, isopropyl tricumylphenyl titanate, and tetraisopropyl bis(dioctyl phosphite) titanate.
[0101] Furthermore, examples of oligomer coupling agents include methyl-based, methyl / phenyl-based, propyl / phenyl-based, epoxy-modified, mercapto-modified, amine-modified, (meth)acrylic-modified, or polyester resin-modified alkoxy oligomers.
[0102] The content of the coupling agent in the underfill material is not particularly limited. From the viewpoint of adhesion, fluidity, etc., the content of the coupling agent is preferably 0.01% to 20% by mass, and more preferably 0.01% to 10% by mass, relative to the total amount of epoxy resin.
[0103] [Curing Accelerator] When the thermosetting compound is an epoxy resin, a curing accelerator may be included as needed. The type of curing accelerator is not particularly limited, and conventionally known ones can be used. Examples of curing accelerators include cycloamidine compounds such as 1,8-diazabicyclo[5.4.0]undecene-7, 1,5-diazabicyclo[4.3.0]nonene, and 5,6-dibutylamino-1,8-diazabicyclo[5.4.0]undecene-7; tertiary amine compounds such as triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; and 2-methylimidazole and 2-ethylimidazole. Imidazoles such as 4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-phenylimidazole, 1-benzyl-2-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,4-diamino-6-(2'-methylimidazolyl-(1'))-ethyl-s-triazine, and 2-heptadecylimidazole. Examples of organic phosphine compounds include trialkylphosphines such as tributylphosphine, dialkylarylphosphines such as dimethylphenylphosphine, alkyldiarylphosphines such as methyldiphenylphosphine, triphenylphosphine, alkyl-substituted triphenylphosphine, and compounds having intramolecular polarization obtained by adding compounds having π bonds such as maleic anhydride, 1,4-benzoquinone, 2,5-tholquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone, 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, phenyl-1,4-benzoquinone, diazophenylmethane, and phenolic resins to these compounds; phenylborone salts such as 2-ethyl-4-methylimidazole tetraphenylborate and N-methylmorpholine tetraphenylborate; and derivatives thereof. In addition, latent curing accelerators may be used.Examples of latent curing accelerators include core-shell particles, which consist of a compound having an amino group that is solid at room temperature as a core, coated with a shell of an epoxy compound that is solid at room temperature. Examples of such core-shell particles include commercially available products such as Amicure (manufactured by Ajinomoto Co., Inc., trade name) and Novacure (manufactured by Asahi Kasei Chemicals Corporation, trade name), in which microencapsulated amines are dispersed in a bisphenol A type epoxy resin or a bisphenol F type epoxy resin. Curing accelerators may be used individually or in combination of two or more types.
[0104] The content of the curing accelerator is not particularly limited as long as the curing acceleration effect is achieved, but it is preferably 0.1% to 40% by mass relative to the epoxy resin, and more preferably 1% to 30% by mass. When the content of the curing accelerator is 0.1% by mass or more relative to the epoxy resin, it tends to have excellent curing properties even in a short time, and when it is 40% by mass or less, it tends to be easier to control the curing speed and storage stability such as pot life and shell life.
[0105] Furthermore, to promote the condensation reaction of the coupling agent and the reaction between the silanol groups in the coupling agent and the silanol groups of the inorganic filler such as silica, thereby improving the dispersibility of the inorganic filler and lowering the viscosity of the underfill material, catalysts such as proton-supplying acids and Lewis acids may be added. Among these, chelating agents containing metal species are preferred as Lewis acids from the viewpoint of storage stability. Examples of chelating agents containing metal species include aluminum, boron, cobalt, and titanium. The Lewis acid content is preferably 0.001 to 1.0 parts by mass, more preferably 0.002 to 0.8 parts by mass, and even more preferably 0.005 to 0.6 parts by mass per 100 parts by mass of the inorganic filler.
[0106] [Other Components] In addition to the components mentioned above, the underfill material may contain various additives such as flexible agents and ion exchangers. The underfill material may also contain various additives known in the art, as needed, in addition to the additives exemplified below.
[0107] (Flexible Agent) The underfill material may contain various flexible agents other than the core-shell type particles of this disclosure, from the viewpoint of improving thermal shock resistance and reducing stress on semiconductor elements. The type of flexible agent is not particularly limited, and those commonly used in the field, such as silicone rubber, acrylic elastomer, and phenoxy resin, may be applied. Among these, rubber particles are preferred as the flexible agent. Examples of rubber particles include styrene-butadiene rubber (SBR), nitrile-butadiene rubber (NBR), butadiene rubber (BR), urethane rubber (UR), and acrylic rubber (AR). One type of flexible agent may be used alone, or two or more types may be used in combination.
[0108] (Ion Exchanger) The underfill material may contain an ion exchanger as needed. When the underfill material contains an ion exchanger, the migration resistance, moisture resistance, and high-temperature storage characteristics of semiconductor devices such as ICs tend to improve. Examples of ion exchangers include compounds represented by the following compositional formulas (I) or (II): Mg 1-X Al X (OH) 2 (CO 3 ) X / 2 mH 2 O ... (I) (0 < X ≤ 0.5, m is a positive number) Bio x (OH) y (NO 3 ) z ...(II) (0.9≦x≦1.1, 0.6≦y≦0.8, 0.2≦z≦0.4)
[0109] The amount of ion exchanger added is preferably 0.1% to 3.0% by mass, and more preferably 0.3% to 1.5% by mass. The volume-average particle size of the ion exchanger is preferably 0.1 μm to 3.0 μm. The volume-average particle size of the ion exchanger can be measured as the particle size (D50) when the cumulative amount from the smallest diameter side reaches 50% in the volume-based particle size distribution measured by a laser diffraction scattering particle size distribution analyzer. The maximum particle size of the ion exchanger is preferably 10 μm.
[0110] An example of the compound represented by formula (I) above is the commercially available DHT-4A (manufactured by Kyowa Chemical Industry Co., Ltd., trade name). An example of the compound represented by formula (II) above is the commercially available IXE500 (manufactured by Toagosei Co., Ltd., trade name). In addition, other anion exchangers may be added as needed. The type of anion exchanger is not particularly limited, and conventionally known ones can be used. For example, hydrated oxides of elements selected from magnesium, aluminum, titanium, zirconium, antimony, etc. Anion exchangers may be used individually or in combination of two or more types.
[0111] (Other additives) The underfill material may contain other additives as needed, such as dyes, colorants such as carbon black, diluents, leveling agents, and defoamers.
[0112] [Method for preparing underfill material] The resin liquid composition may be prepared by any method as long as the various components can be uniformly dispersed and mixed. For example, it can be obtained by weighing the components, mixing and kneading them using a mixer, mixing roll, planetary mixer, etc., and degassing as necessary.
[0113] [Physical Properties of Underfill Material] (Viscosity) The viscosity of the underfill material is not particularly limited. From the viewpoint of fluidity, the viscosity of the underfill material is preferably 0.1 Pa·s to 200 Pa·s at 25°C, more preferably 1 Pa·s to 100 Pa·s, and even more preferably 1 Pa·s to 50 Pa·s. The viscosity of the underfill material at 25°C is measured using an EHD type rotational viscometer. Specifically, it can be measured by the method described in the examples.
[0114] Furthermore, from the viewpoint of filling properties when filling underfill material in narrow gaps at temperatures around 50°C to 120°C for applications such as underfill material, the viscosity at the underfill material filling temperature is preferably, for example, 0.3 Pa·s or less, and more preferably 0.2 Pa·s or less. The viscosity at the underfill material filling temperature is measured using a rheometer. Specifically, it can be measured by the method described in the examples.
[0115] [Physical properties of hardened underfill material]
[0116] (Linear Thermal Expansion Coefficient) The linear thermal expansion coefficient of the underfill material when it is cured is not particularly limited. For example, the linear thermal expansion coefficient (CTE1) obtained by measuring the temperature increase from 0°C to 300°C at 5°C / min using the compression method, and measuring it as the slope of the tangent between 10°C and 30°C, is preferably 60 ppm / °C or less, more preferably 55 ppm / °C or less, and particularly preferably 45 ppm / °C or less. When the CTE1, which is the linear thermal expansion coefficient below the glass transition temperature, is 60 ppm / °C or less, the occurrence of bump cracks during reflow tends to be suppressed and the temperature cycle resistance characteristics tend to improve. The linear thermal expansion coefficient of CTE1 may be 15 ppm / °C or more.
[0117] Furthermore, the linear thermal expansion coefficient (CTE2), determined by measuring the temperature increase from 0°C to 300°C at 5°C / min using the compression method, is preferably 180 ppm / °C or less, more preferably 170 ppm / °C or less, and even more preferably 160 ppm / °C or less. If the CTE2, which is the linear thermal expansion coefficient above the glass transition temperature, is 180 ppm / °C or less, the sealing portion tends to peel off more easily from the substrate. The linear thermal expansion coefficient of CTE2 may be 50 ppm / °C or more, 60 ppm / °C or more, or 70 ppm / °C or more.
[0118] The linear thermal expansion coefficient can be measured by TMA (thermomechanical analysis). Specifically, it can be measured by the method described in the examples.
[0119] [Applications of Underfill Material] In one embodiment, the underfill material of this disclosure is used to seal a connection portion of an electronic component device comprising an electronic component and a substrate electrically connected to the electronic component via a connection portion. Details of the configuration of the electronic component device and the sealing method are described below. The underfill material of this disclosure may also be used in compression molding.
[0120] <Electronic component device> The electronic component device of the present disclosure comprises an electronic component, a substrate electrically connected to the electronic component via a connection portion, and a sealing portion including a cured product of the repairable underfill material of the present disclosure that seals the connection portion.
[0121] Examples of electronic components include active elements such as semiconductor chips, transistors, diodes, and thyristors, and passive elements such as capacitors, resistors, resistor arrays, coils, and switches. The size of the electronic components is not particularly limited; for example, a semiconductor chip measuring 20 mm in length and 20 mm in width can be used. Furthermore, the underfill material of this disclosure exhibits excellent reliability as an underfill material even when the size of the semiconductor chip is larger.
[0122] Examples of substrates include lead frames, pre-wired tape carriers, wiring boards (rigid or flexible), glass, and silicon wafers.
[0123] In the electronic component device of this disclosure, the electronic component and the substrate are electrically connected via a connection part. Examples of connection parts include bumps. For example, the bump may be a bump made of copper pillars.
[0124] Examples of electronic component devices include flip-chip semiconductor devices obtained by flip-chip bonding electronic components onto a substrate using bump connections. Examples of flip-chip semiconductor devices include BGA (Ball Grid Array), LGA (Land Grid Array), and COF (Chip On Film). The electronic component device may also be a high-density or large-scale electronic component device. The package form may be a system-in-package (SiP) that integrates multiple semiconductor chips into a single package.
[0125] In the electronic component device of this disclosure, the connection portion is sealed with a cured underfill material of this disclosure. The sealing method is not particularly limited and includes dispensing, casting, printing, and the like.
[0126] <Method for opening electronic component devices> The method for opening electronic component devices according to the present disclosure involves heating the electronic component device according to the present disclosure to a temperature higher than the melting point of the solder forming the connection portion, and peeling the sealing portion from the substrate to open it. Since the sealing portion of the electronic component device according to the present disclosure is a cured product of the repairable underfill material according to the present disclosure, it is easy to peel the sealing portion from the substrate, making it easy to open with minimal damage to the substrate, etc.
[0127] The heating temperature during opening must be above the melting point of the solder, for example, it may be 260°C or higher, 265°C or higher, or 270°C or higher. If low-melting-point solder is used for connection, the heating temperature can be lowered to below 260°C. Furthermore, from the viewpoint of minimizing damage to the substrate and other components due to heating during opening, the heating temperature during opening is preferably 300°C or lower, more preferably 290°C or lower, and even more preferably 280°C or lower.
[0128] When opening the package, it is preferable that only the defective chip and its connection point are heated. By preventing heat from being transferred to the good parts, the good parts can continue to be used. Although the good parts will also be heated when the defective chip is heated, the heating temperature of the good parts is preferably 200°C or less, more preferably 190°C or less, and even more preferably 180°C or less. Furthermore, from the viewpoint of minimizing damage to the good parts due to heating, the heating time is preferably 10 minutes or less, and more preferably 5 minutes or less. The sealing portion may also be peeled off the substrate by physically applying force to the defective chip while heating it.
[0129] <Method for repairing electronic component devices> In the method for repairing electronic component devices described herein, the electronic component with poor conductivity is removed from the opening made by the method for opening the electronic component device described herein. The electronic component with poor conductivity in the electronic component device can be identified by inspection. After removing the electronic component from the electronic component device, it is replaced with a new electronic component.
[0130] In the repair method for electronic component devices of this disclosure, since the sealing portion is a cured product of the repairable underfill material of this disclosure, it is easy to peel the sealing portion from the substrate, and it is possible to replace a faulty electronic component with a new one while minimizing damage to the substrate, etc.
[0131] <Method for manufacturing an electronic component device> The method for manufacturing an electronic component device according to the present disclosure includes a step of forming a sealing portion in which the connection portion between an electronic component and a substrate electrically connected to the electronic component via a connection portion is sealed with the repairable underfill material according to the present disclosure.
[0132] Furthermore, the manufacturing method of the electronic component device of the present disclosure may further include the steps of: heating to a temperature higher than the melting point of the solder forming the connection portion to peel the sealing portion from the substrate and open it; and removing the electronic component with poor conductivity from the opened portion obtained by peeling the sealing portion from the substrate and replacing it with a new electronic component. In this method, since the repair method of the electronic component device of the present disclosure is used, it is possible to replace the electronic component with poor conductivity with a new electronic component while minimizing damage to the substrate, etc.
[0133] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.
[0134] <Preparation of Underfill Material> The components used in the underfill material of the examples and comparative examples are as follows: • Epoxy resin 1: Epoxy equivalent weight of 160 g / eq, bisphenol F type liquid epoxy resin • Epoxy resin 2: Epoxy equivalent weight of 95 g / eq, aminophenol type epoxy resin • Epoxy resin 3: Epoxy equivalent weight of 315 g / eq, polypropylene glycol diglycidyl ether • Epoxy resin 4: Epoxy equivalent weight of 130 g / eq, trimethylolpropane polyglycidyl ether
[0135] Radical polymerizable compound 1: 1,6'-bismaleimide-(2,2,4-trimethyl)hexane Radical polymerizable compound 2: Tricyclodecanedimethanol diacrylate Radical polymerizable compound 3: 4-hydroxybutyl acrylate
[0136] - Curing agent 1: Amine-modified latent curing agent with an amine value of 145-155 mg KOH / g - Curing agent 2: Modified aliphatic amine curing agent with an active hydrogen equivalent of 45 g / eq - Curing agent 3: Liquid amine resin with an amine equivalent of 63 g / eq (manufactured by Nippon Kayaku Co., Ltd., product name: Kayahard A-A)
[0137] Radical polymerization initiator 1: t-butyl peroxyl laurate
[0138] • Surfactant 1: Dimethyl silicone oil with polyether moieties in its side chain (viscosity 1600 mm at 25°C) 2 / s) • Surfactant 2: Dimethyl silicone oil having polyether and amine moieties in its side chain (viscosity 3300 mm at 25°C) 2 / s)
[0139] - Inorganic filler 1: Silica particles surface-treated with a silane coupling agent (γ-glycidoxypropyltrimethoxysilane) (average particle size: 1.5 μm, top cut 5 μm) - Inorganic filler 2: Untreated silica particles (average particle size: 1.5 μm, top cut 5 μm) The volume-average particle size of the above inorganic fillers is the median diameter (D50). This volume-average particle size was measured using a laser diffraction scattering particle size analyzer.
[0140] Coupling agent 1: γ-methacryloxypropyltrimethoxysilane
[0141] Each component was blended in the compositions (parts by mass) shown in Tables 1 to 3, and after kneading and dispersing using a three-roll mill and a vacuum grinder, the underfill materials for the examples and comparative examples were prepared.
[0142] <Evaluation of Linear Thermal Expansion Coefficients (CTE1 and CTE2)> Test specimens were prepared by heating and curing the underfill material at the temperatures and times shown in Table 1. The cured underfill material was cut to a size of φ8 mm × 20 mm, and the temperature was measured by increasing the temperature from 0°C to 300°C at a rate of 5°C / min using a thermomechanical analyzer (TA Instruments "TMA450") by compression. The slope of the tangent line between 10°C and 30°C was defined as CTE1, and the slope of the tangent line between 180°C and 200°C was defined as CTE2.
[0143] <Evaluation of Peelability> An underfill material was molded to the surface of a substrate coated with Taiyo Ink's solder resist, product name PSR-800 AUS SR-1, to a diameter of 3 mm and a height of 1 mm. The underfill material was heated and cured at the temperatures and times shown in Table 1. A bond tester (Nordson Advanced Technologies, Series 4000) was used to apply a shear force to the resulting molded material at a shear rate of 50 μm / s while maintaining the substrate temperature at room temperature (25°C) or 260°C. The condition of the substrate after the molded material was peeled off by the shear force was visually inspected. This test was performed four times. The evaluation criteria are as follows: A: The molded material is removed, and the solder resist remains on the substrate. B: The solder resist is removed together with the molded material.
[0144]
[0145]
[0146]
[0147] In Comparative Example 7 and Examples 7-12, the curing agent content (equivalent ratio) represents the number of functional groups (eq) in the curing agent when the number of epoxy groups in the epoxy resin is set to 1. The inorganic filler content represents the amount of inorganic filler relative to the total amount of the composition (mass %).
[0148] The evaluation results showed that even when the type of resin was changed, the examples containing 5 parts by mass or more of surfactant exhibited superior peelability at 260°C compared to the comparative examples that contained no surfactant or less than 5 parts by mass of surfactant. In the examples, the molded product was removed together with the solder resist at 25°C, indicating that the solder resist and the molded product were well bonded at 25°C.
[0149] The disclosure of Japanese Patent Application No. 2025-077583 is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually noted to be incorporated by reference.
Claims
1. A repairable underfill material containing a thermosetting compound and a surfactant, wherein the material contains 5 parts by mass or more of the surfactant per 100 parts by mass of the thermosetting compound.
2. The repairable underfill material according to claim 1, wherein the surfactant comprises silicone oil.
3. The repairable underfill material according to claim 2, wherein the silicone oil comprises a polyether-modified silicone oil.
4. The repairable underfill material according to claim 1 or 2, further comprising an inorganic filler.
5. The repairable underfill material according to claim 4, wherein the inorganic filler content is 20% by mass or more.
6. The repairable underfill material according to claim 1 or claim 2, wherein the linear thermal expansion coefficient (CTE2) in the range of 180°C to 200°C when cured is 50 ppm / °C to 170 ppm / °C.
7. An electronic component device comprising: an electronic component; a substrate electrically connected to the electronic component via a connection portion; and a sealing portion containing a cured product of the repairable underfill material according to claim 1 or claim 2, which seals the connection portion.
8. A method for opening an electronic component device, comprising heating the electronic component device according to claim 7 to a temperature higher than the melting point of the solder forming the connection portion, and peeling the sealing portion from the substrate to open it.
9. A method for repairing an electronic component device, comprising removing an electronic component with poor conductivity from an opening opened by the method for opening an electronic component device described in claim 8.
10. A method for repairing an electronic component device according to claim 9, comprising removing the electronic component with poor conductivity and then replacing it with a new electronic component.
11. A method for manufacturing an electronic component device, comprising the step of forming a sealing portion in which the connection portion between the electronic component and a substrate electrically connected to the electronic component via a connection portion is sealed with the repairable underfill material described in claim 1 or claim 2.
12. A method for manufacturing an electronic component device according to claim 11, further comprising the steps of: heating the solder forming the connection to a temperature higher than the melting point of the solder, peeling the sealing portion from the substrate and opening it; and removing the electronic component with poor conductivity from the opened portion obtained by peeling the sealing portion from the substrate and replacing it with a new electronic component.