Negative electrode active material, manufacturing method, negative electrode, and secondary battery

The NSIT-type oxide structure in negative electrode materials addresses the need for enhanced electrochemical properties by incorporating specific voids, resulting in improved battery performance.

WO2026234932A1PCT designated stage Publication Date: 2026-11-12THE UNIV OF TOKYO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/014490
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-04-07
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Current negative electrode materials for lithium-ion batteries do not exhibit optimal electrochemical properties, necessitating the development of materials with improved performance.

Method used

A negative electrode active material composed of an oxide with an NSIT-type structure, containing a group 1 element, titanium, and a sub-element, such as sodium or lithium, is synthesized to enhance electrochemical properties through specific voids in its chemical structure.

Benefits of technology

The NSIT-type oxide structure provides suitable electrochemical properties, leading to improved performance in lithium-ion batteries, particularly in rapid charge and discharge cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026014490_12112026_PF_FP_ABST
    Figure JP2026014490_12112026_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide a negative electrode active material and the like for exhibiting excellent electrochemical characteristics. [Solution] According to one aspect of the present invention, a negative electrode active material composed of an oxide having an NSIT-type structure is provided, the negative electrode active material containing a Group 1 element, titanium, oxygen, and an auxiliary element different from the Group 1 element, titanium, and oxygen.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode active material, manufacturing method, negative electrode, and secondary battery

[0001] This invention relates to a negative electrode active material, a method for manufacturing it, a negative electrode, and a secondary battery.

[0002] Currently, technological development is underway for various types of batteries, including lithium-ion batteries. Regarding such batteries, development has also been made regarding negative electrode materials. For example, Patent Document 1 shows a negative electrode using lithium titanium oxide (LTO).

[0003] Special Publication No. 2024-524971

[0004] On the other hand, there is still room for technological development regarding negative electrode active materials that exhibit excellent electrochemical properties.

[0005] In view of the above circumstances, the present invention aims to provide a negative electrode active material and the like that exhibits excellent electrochemical properties.

[0006] According to one aspect of the present invention, a negative electrode active material is provided which is composed of an oxide having an NSIT type structure and comprises a group 1 element, titanium, oxygen, and a sub-element different from the group 1 element, titanium, and oxygen.

[0007] According to the above embodiment, a negative electrode active material and the like that exhibit excellent electrochemical properties are provided.

[0008] This is a conceptual diagram schematically representing the NSIT type structure. This is a diagram schematically representing the cross-sectional structure of the negative electrode in this embodiment. This is a diagram showing the spectrum obtained by analyzing the negative electrode active material obtained in the example. This is a schematic diagram showing the configuration of the two-electrode coin cell fabricated in the example. This is a graph showing the results of the evaluation of the electrochemical properties of the negative electrode active material 8.

[0009] Embodiments of the present invention will be described below. The various features shown in the embodiments below can be combined with each other. Furthermore, unless otherwise specified, "~" in this specification refers to the above.

[0010] In other words, the negative electrode active material of this embodiment is as follows: A negative electrode active material composed of an oxide having an NSIT type structure, comprising a group 1 element, titanium, oxygen, and a sub-element different from the group 1 element, titanium, and oxygen.

[0011] The following describes the overview, manufacturing method, and applications of such negative electrode active materials.

[0012] [Negative Electrode Active Material] As previously stated, the negative electrode active material of this embodiment is composed of an oxide having a predetermined structure (NSIT type structure). According to the inventors, it has been found that by having such a structure, the oxide can form appropriate voids in its chemical structure, and as a result, when used as a negative electrode active material, it can provide suitable electrochemical properties.

[0013] Here, we will explain the "NSIT-type structure." Figure 1 is a conceptual diagram schematically representing the NSIT-type structure. In this specification, the "NSIT-type structure" is a structure reported by Mumme et al. in 1968, and consists of four MOs. 6 It has a structure in which Z-shaped substructures, formed by octahedrons sharing edges, are linked together in a ribbon-like manner along the b-axis (Acta Cryst B 1968, 24, 625). Such NSIT-type structures may also be simply referred to as "NSIT" structures. Figure 1 shows a typical example: Na 0.85 Cr 0.85 Ti 1.15 O 4 This figure shows the crystal structure of the composition. As can be seen from this figure, in the NSIT type structure, the Z-shaped ribbon shares its vertices, which can form ion channels (channels for sodium ions, etc.) that extend in the b-axis direction. From one perspective, such channels may be called "tunnel structures". It is believed that the negative electrode active material of this embodiment has high electrochemical properties due to this unique structure (specific voids, etc.).

[0014] Note that since the oxide of the present embodiment has the specific chemical structure as described above, a specific peak can be observed in its X-ray diffraction pattern. That is, in the oxide of the present embodiment, Bragg reflections attributable to the orthorhombic lattice of the NSIT-type structure may be observed in the X-ray diffraction pattern.

[0015] Note that the composition shown in FIG. 1 (Na 0.85 Cr 0.85 Ti 1.15 O 4 ) is merely an example, and the oxide constituting the negative electrode active material of the present embodiment may be composed of various elements. That is, the oxide constituting the negative electrode active material of the present embodiment contains a titanium element and an oxygen element, and may further contain the following elements in addition to these.

[0016] That is, the oxide constituting the negative electrode active material of the present embodiment contains a Group 1 element. The Group 1 element herein may include one or more of hydrogen, lithium, sodium, potassium, rubidium, cesium and francium. On the other hand, from the viewpoint of easily obtaining the negative electrode active material of the present embodiment advantageously on an industrial scale and realizing well-balanced electrochemical properties, the Group 1 element herein is preferably sodium or lithium.

[0017] In addition, the oxide constituting the negative electrode active material of the present embodiment contains sub-elements different from the aforementioned Group 1 element, titanium and oxygen. The sub-elements herein may be arbitrarily set within the range where the oxide of the present embodiment can adopt the NSIT-type structure. On the other hand, from the viewpoint of facilitating the oxide of the present embodiment to stably adopt the NSIT-type structure, the sub-elements herein are preferably elements belonging to Groups 2 to 11. Further, from the viewpoint of high handleability and industrially advantageous production of the oxide of the present embodiment, the sub-elements may be selected from the group consisting of chromium (Cr), magnesium (Mg), iron (Fe), vanadium (V) and nickel (Ni).

[0018] As a more specific aspect, the oxide constituting the negative electrode active material of the present embodiment may be represented by each of the formulas shown below.

[0019] In other words, in one embodiment, the oxide constituting the negative electrode active material of this embodiment may be represented by the following formula (1). A x M x/2 Ti 2-(x/2) O 4 ... (1) Here, A is one of the Group 1 elements mentioned above. M is one of the sub-elements mentioned above, and in this equation (1), it is a divalent metallic element. x is a value between 0.7 and 0.9.

[0020] The oxide represented by formula (1) uses a divalent metallic element as M (a secondary element). Various divalent metallic elements may be selected, but typically it may be one or more selected from the group consisting of magnesium (Mg), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), and zinc (Zn). In compounds represented by such formulas, the ratio of the divalent metallic element to the titanium element is set within a predetermined range, and the aforementioned NSIT-type structure is likely to be formed.

[0021] In another embodiment, the oxide constituting the negative electrode active material of this embodiment may be represented by the following formula (2). A x M x Ti 2-x O 4 ... (2) Here, A is one of the Group 1 elements mentioned above. M is one of the sub-elements mentioned above, and in this equation (2), it is a trivalent metallic element. x is a value between 0.7 and 0.9.

[0022] The oxide represented by formula (2) uses a trivalent metallic element as M (sub-element). Various trivalent metallic elements may be selected, but typically it may be one or more selected from the group consisting of vanadium (V), chromium (Cr), iron (Fe), aluminum (Al), and gallium (Ga). In compounds represented by such formulas, the ratio of the trivalent metallic element to the titanium element is set within a predetermined range, and the aforementioned NSIT-type structure is likely to be formed.

[0023] Furthermore, the secondary elements are not necessarily limited to the divalent or trivalent metallic elements mentioned above. In other words, depending on the type and valency of the element used as the secondary element, an oxide with an NSIT-type structure that does not satisfy the above formula may be used as the negative electrode active material in this embodiment.

[0024] [Method for Manufacturing the Negative Electrode Active Material] The negative electrode active material of this embodiment is manufactured by synthesizing an oxide having the NSIT-type structure described above. For example, such an oxide may be synthesized by a solid-phase method. For example, the oxide of this embodiment can be obtained by mixing a compound that is a source of Group 1 elements, a compound that is a source of minor elements, and a compound that is a source of titanium in a predetermined stoichiometric ratio, and then firing the mixture. For example, the compound that is a source of Group 1 elements may be an alkali metal salt (carbonate, bicarbonate, etc.) or an alkali metal hydroxide. The compound that is a source of minor elements may be an oxide, hydroxide, or complex of the minor element. Furthermore, the compound that is a source of titanium may be titanium oxide, etc. The firing conditions may be set appropriately depending on the components used, but for example, temperature conditions in the range of 900 to 1800 K or 1000 to 1500 K may be adopted. The calcined material obtained by this calcination process may be used directly as a negative electrode active material, or it may be used as a precursor in the manufacturing method described below.

[0025] In other words, in one embodiment of the manufacturing method, a predetermined oxide can be obtained by combining the following steps. That is, the manufacturing method here may include a preparation step and a conversion step. In the preparation step, a precursor containing a group 1 element, titanium, oxygen, and a minor element is prepared. In the conversion step, a predetermined oxide is obtained by replacing the group 1 element contained in the precursor with another group 1 element.

[0026] The manufacturing method described here is characterized by obtaining a precursor (the calcined product shown earlier) and then replacing the Group 1 elements contained in the precursor with other Group 1 elements. In a typical embodiment, an oxide containing sodium as a Group 1 element is obtained as the precursor, and a step is taken to replace this sodium with another Group 1 element such as lithium. Such replacement of Group 1 elements can be achieved by various methods, but for example, it may be done by preparing a solution containing other Group 1 elements and bringing the solution into contact with the precursor. Regarding the solution containing other Group 1 elements, the source of the other Group 1 elements may be hydroxides of the other Group 1 elements or various salt compounds such as halides. The solvent used to obtain the solution may be water or an organic solvent. From the viewpoint of facilitating the dissolution of Group 1 elements, the organic solvent here may be an alcohol such as methanol or ethanol.

[0027] [Negative Electrode] The negative electrode active material in this embodiment can be used when manufacturing a negative electrode. That is, the negative electrode in this embodiment may have a structure in which a current collector and a negative electrode active material layer are laminated. The negative electrode active material layer here may include the negative electrode active material described above.

[0028] A typical embodiment of such a negative electrode will be explained with reference to the figures. Figure 2 is a schematic diagram showing the cross-sectional structure of the negative electrode of this embodiment. The negative electrode 1 shown in Figure 2 includes a current collector 2 and negative electrode active material layers (negative electrode active material layers 3A, 3B) laminated on the current collector 2. Although Figure 2 shows an embodiment in which negative electrode active material layers are provided on both sides of the current collector 2, the negative electrode active material layer may be provided on only one side. Furthermore, the negative electrode 1 may be provided with various layers not shown, without departing from the spirit of the invention. For example, a layer (e.g., a primer layer) may be interposed between the current collector 2 and the negative electrode active material layer. Also, multiple negative electrode active material layers may be provided on one side of the current collector 2.

[0029] The negative electrode 1 of this embodiment is characterized in that the negative electrode active material layer (negative electrode active material layer 3A and / or negative electrode active material layer 3B) contains the aforementioned negative electrode active material. This makes it possible to improve the electrochemical properties when the negative electrode 1 is applied to a secondary battery.

[0030] Such a negative electrode active material layer may be formed by preparing a paste containing the above-mentioned negative electrode active material and applying the paste to the current collector 2. Such application can be carried out according to known methods, except for using the above-mentioned negative electrode active material. For example, a paste for forming a negative electrode active material layer can be obtained by mixing the above-mentioned negative electrode active material with an optional component (e.g., binder, conductive material, etc.) and further mixing it with a dispersion medium (organic solvent, water, etc.). By applying the paste obtained in this way to the current collector 2, a negative electrode active material layer can be formed.

[0031] The current collector 2 in this embodiment may be made of metal foil. For example, the current collector 2 may be made of copper foil, aluminum foil, or the like.

[0032] Furthermore, any resin component can be used as the binder mentioned above. For example, various binder resins such as fluororesin, acrylic resin, styrene-butadiene resin, and carboxymethylcellulose can be used as the binder in this embodiment. In addition, carbon materials such as carbon black and graphite may be used as conductive materials that can be combined with the negative electrode active material.

[0033] This type of coating can be carried out using various coating devices such as gravure coaters, comma coaters, slit coaters, and die coaters. Alternatively, after applying the paste to the current collector 2, a drying step may be performed as appropriate.

[0034] Furthermore, drying can also be carried out according to known methods. For example, the dispersion medium can be removed by placing the current collector 2 coated with the paste inside a drying apparatus such as a drying oven. The temperature and drying time during drying can be appropriately set according to the components and solid content concentration of the paste. As an example, the drying temperature is, for example, 60°C to 200°C, preferably 70°C to 150°C. The drying time is, for example, 10 seconds to 30 minutes, preferably 30 seconds to 10 minutes.

[0035] Furthermore, in obtaining the negative electrode 1, a combination of processes such as pressing the laminate obtained as described above or cutting it into a predetermined shape may be used.

[0036] [Secondary Battery] The negative electrode 1 obtained as described above can be used in a secondary battery. That is, the secondary battery of this embodiment may have the negative electrode 1 described above. In a typical embodiment, the secondary battery may include a positive electrode and an electrolyte, along with the negative electrode 1 described above. Here, the positive electrode is provided spaced apart from the negative electrode 1 via the electrolyte. The secondary battery may also have a separator provided between the negative electrode 1 and the positive electrode. In a typical embodiment, the negative electrode 1, positive electrode, electrolyte, etc. are sealed in a predetermined outer material to constitute the secondary battery.

[0037] The positive electrode here may be a positive electrode active material layer containing positive electrode active material, which is laminated on a current collector. Known materials can be used as the positive electrode active material, for example, LiCoO 2 LiNiO 2 , Li(NiCoMn)O 2 Lithium-containing transition metal oxides with layered structures such as LiMn 2 O 4 Spinel-type manganese oxides such as; and LiFePO 4Examples include iron-based compounds such as those mentioned above. Furthermore, when obtaining the positive electrode active material layer, the aforementioned binder and conductive material may be combined and incorporated into the positive electrode active material layer. The current collector, binder, and conductive material that can be used as the positive electrode are the same as the various configurations that can be used as the negative electrode. In one embodiment, lithium foil or the like can also be used as the positive electrode.

[0038] The electrolyte in this embodiment can constitute a field for ion movement between the positive and negative electrodes in a secondary battery. Such an electrolyte is, for example, a predetermined electrolyte dissolved in an organic solvent. The electrolyte is LiPF4. 6 LiBF 4 LiClO 4、 Examples include lithium bis(fluorosulfonyl)imide (LiFSI). Examples of organic solvents for dissolving the electrolyte include 1,2-dimethoxyethane, ethylene carbonate, propylene carbonate, fluoroethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. Two or more of these organic solvents may be used in mixture form.

[0039] Furthermore, the secondary battery of this embodiment may be used for various purposes. For example, the secondary battery of this embodiment may be used as a power source for vehicles such as electric vehicles. In addition, the secondary battery of this embodiment may be used as various types of storage batteries.

[0040] Furthermore, they may be provided in the following embodiments.

[0041] (1) A negative electrode active material composed of an oxide having an NSIT type structure, comprising a group 1 element, titanium, oxygen, and a sub-element different from the group 1 element, titanium, and oxygen.

[0042] (2) A negative electrode active material as described in (1) above, wherein the Group 1 element is lithium or sodium.

[0043] (3) A negative electrode active material as described in (1) or (2) above, wherein the sub-element is an element belonging to Group 2 to Group 11.

[0044] (4) The negative electrode active material described in (3) above, wherein the sub-element is selected from the group consisting of chromium, magnesium, iron, vanadium, and nickel.

[0045] (5) In the negative electrode active material described in any one of (1) to (4) above, the sub-element is a divalent metallic element, and the oxide is represented by the following formula (1), A x M x/2 Ti 2-(x/2) O 4 ... (1) Here, A is a Group 1 element, M is a divalent metallic element, and x is a value between 0.7 and 0.9, which is the negative electrode active material.

[0046] (6) In the negative electrode active material described in any one of (1) to (4) above, the sub-element is a trivalent metallic element, and the oxide is represented by the following formula (2), A x M x Ti 2-x O 4 ... (2) Here, A is a Group 1 element, M is a trivalent metallic element, and x is a value between 0.7 and 0.9, which is the negative electrode active material.

[0047] (7) A method for producing a negative electrode active material according to any one of (1) to (6) above, comprising a preparation step and a conversion step, wherein in the preparation step, a precursor comprising a group 1 element, titanium, oxygen, and the aforementioned sub-elements is prepared, and in the conversion step, the oxide is obtained by replacing the group 1 element contained in the precursor with another group 1 element.

[0048] (8) A negative electrode having a structure in which a current collector and a negative electrode active material layer are stacked, wherein the negative electrode active material layer contains the negative electrode active material described in any one of (1) to (6) above.

[0049] (9) A secondary battery having the negative electrode described in (8) above. Of course, this is not limited to this.

[0050] Although embodiments of the present invention have been described above, these are merely examples, and various other configurations can be adopted. Furthermore, the present invention is not limited to the embodiments described above, and modifications, improvements, etc., within the scope that can achieve the objectives of the present invention are included in the present invention.

[0051] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples.

[0052] [Synthesis of NSIT-type compounds (standard conditions)] The titanium oxide with an NSIT-type structure in this example was synthesized by a solid-phase method. Specifically, various transition metal compounds as precursors, NaHCO3 3 and rutile-type TiO 2 The powders were weighed in stoichiometric ratios. However, Na 0.85 Cr 0.85 Ti 1.15 O 4 In the synthesis of NaHCO 3 An excess of 2% by weight was added. In the synthesis conditions of this example, 60 zirconia balls with a diameter of 5 mm and 10 mL of 2-propanol were sealed in a 45 ml zirconia container, and the various raw materials were wet-mixed using a planetary ball mill (Fritsch). The rotation speed during mixing was set to 450 rpm, and mixing for 5 minutes followed by a 2 minute pause was repeated 36 times. After mixing, it was left in a 353 K oven overnight to volatilize the 2-propanol. The resulting residue was separated from the zirconia balls by sieving, crushed in an agate mortar and pestle, and then formed into 25 mm diameter pellets using a single-screw pressurized pelletizer (Riken Seiki). These pellets were placed in an alumina combustion boat and calcined using an electric tubular furnace and temperature control device AGC-1P (manufactured by Asahi Rika Seisakusho Co., Ltd.) or a box-type electric furnace (manufactured by Denken Highdental Co., Ltd.) under an argon gas flow. The calcination temperature and calcination time were determined appropriately for each compound. To lower the oxygen partial pressure inside the tubular furnace, alumina combustion boats loaded with reduced iron (Fe, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were placed on the upstream and downstream sides of the tubular furnace, respectively. The recovered pellets were crushed into a powder using an agate mortar and pestle.

[0053] [Synthesis of negative electrode active material 1] Na is the negative electrode active material 1.7/8 Mg 7/16 Ti 25/16 O 4 It was synthesized by a solid-phase method. NaHCO 3 Mg(OH) 2 , TiO 2 The two components were mixed in chemically ossibly proportionate ratios and calcined in a box-type electric furnace at 1200 K for 12 hours. X-ray diffraction patterns mainly showed Bragg reflections attributed to an NSIT-type rectangular lattice, and no clear impurity phases were observed.

[0054] [Synthesis of negative electrode active material 2] Na is the negative electrode active material 2. 7/8 V 7/8 Ti 9/8 O 4 is NaHCO 3 , V 2 O 3 , TiO 2 The compound was synthesized by mixing the elements and calcining at 1300 K for 12 hours. To suppress oxidation from V(III) to V(IV), the calcination was carried out under an argon atmosphere. From the X-ray diffraction pattern, Bragg reflections originating from the NSIT-type crystalline phase were mainly observed, and no clear Bragg reflections originating from other crystalline phases were observed.

[0055] [Synthesis of negative electrode active material 3] Na is the negative electrode active material 3. 0.85 Cr 0.85 Ti 1.15 O 4 is NaHCO 3 , Cr(OH) 3 , TiO 2 The mixture was mixed with 2-propanol in a ball mill, dried, and then calcined in an electric tubular furnace under an argon stream to avoid the formation of Cr(VI) through oxidation of Cr(III). In this synthesis system, NaHCO3 3 By adding a 2% excess by weight and firing at 1300K for 12 hours, a sample with an NSIT-type structure as the main phase was obtained.

[0056] [Synthesis of negative electrode active material 4] Na is the negative electrode active material 4. 7/8 Fe 7/8 Ti 9/8 O 4 It was calcined in air. The ratio of both NaHCO3 3 FeC 2 H4 ·2H 2 O, TiO 2 were mixed, and the mixture was fired at 1200 K for 12 hours in a box-type electric furnace to oxidize Fe(II) to Fe(III), and an attempt was made to synthesize an NSIT-type compound. Since Bragg reflections attributed to the NSIT-type orthorhombic lattice were mainly observed from the X-ray diffraction pattern, it is considered that the NSIT-type compound was obtained as the main phase.

[0057] [Synthesis of Negative Electrode Active Material 5] The negative electrode active material 5, Na 7/8 Ni 7/16 Ti 25/16 O 4 was obtained by mixing NaHCO 3 , NiCO 3 ·Ni(OH) 2 , TiO 2 at a stoichiometric ratio, and firing the mixture at 1200 K for 12 hours in a box-type electric furnace. From the X-ray diffraction pattern, Bragg reflections considered to originate from the NSIT-type crystal phase were mainly observed, and clear Bragg reflections of impurity phases were not observed. Therefore, it is considered that a sample having the NSIT phase as the main phase was obtained.

[0058] [Synthesis of Negative Electrode Active Materials 6 to 10] For each of the negative electrode active materials 1 to 5 obtained above, an attempt was made to convert the Na portion to Li. Negative electrode active material 1, Na 7/8 Mg 7/16 Ti 25/16 O 4 and negative electrode active material 4, Na 7/8 Fe 7/8 Ti 9/8 O 4 were brought into contact with a 1 mol dm -3 LiCl-LiOH aqueous solution for 24 hours, to convert them into negative electrode active materials in which the Na portion of the corresponding negative electrode active material was converted to Li, as negative electrode active material 6 and negative electrode active material 9, respectively. Negative electrode active material 2, Na 7/8 V 7/8 Ti 9/8 O 4 and negative electrode active material 5, Na 7/8 Ni 7/16 Ti 25/16 O 4 were brought into contact with a 2 mol dm -3The powder sample was dispersed in a solution of LiBr dissolved in ethanol, and the mixture was sealed in a pressure-resistant container and reacted at 393 K for 24 hours to convert them into negative electrode active material 7 and negative electrode active material 10, respectively. Na was the negative electrode active material 3. 0.85 Cr 0.85 Ti 1.15 O 4 Regarding 393K 2moldm -3 By reacting the material in a LiBr / ethanol solution for 24 hours, Na was converted to Li, which was then used as the negative electrode active material 8.

[0059] Figure 3 shows the spectra obtained by analyzing the negative electrode active materials in the examples. Specifically, the X-ray diffraction patterns and fluorescence X-ray spectra of the various negative electrode active materials obtained are summarized and shown in Figure 3. In the X-ray diffraction patterns, negative electrode active materials 6 to 10 are shown in the upper panel, and negative electrode active materials 1 to 5 are shown in the lower panel. The asterisks (*) in the figure represent AlKα peaks originating from the sample holder.

[0060] [Evaluation of Negative Electrode Active Materials 1] Working electrodes and bipolar coin cells were fabricated using the method described below, and various negative electrode active materials were evaluated. First, the working electrodes were fabricated by coating a copper foil current collector (Showa Laminate Industry Co., Ltd., 20 μm thick) with the synthesized negative electrode active material, a conductive additive carbon black (Li-400, manufactured by Denka Co., Ltd.), and a binder carboxymethylcellulose (CMC). Specifically, various negative electrode active materials and carbon black were weighed in a mass ratio of 80:15, and these were sealed in a 45 ml zirconia container with 60 zirconia balls with a diameter of 5 mm and 5 ml of 2-propanol, and wet-mixed using a planetary ball mill (manufactured by Fritsch). The rotation speed during mixing was set to 250 rpm, and mixing for 5 minutes and resting for 2 minutes were repeated 12 times. After mixing, the mixture was left overnight in a 353 K oven to volatilize the 2-propanol. The obtained residue was separated by sieving and ground using an agate mortar and pestle. To this powder, a 2% CMC aqueous solution was added, with the active material, carbon black, and carboxymethylcellulose in a mass ratio of 80:15:5. This mixture was then mixed using a rotation / revolution type mixer (manufactured by Thinky Co., Ltd.), and the resulting slurry was applied to copper foil to a thickness of 100 μm using a doctor blade and dried in a 353 K oven for several hours. The resulting electrode sheet was punched out to a diameter of Φ = 12 mm and vacuum dried overnight at 393 K. Meanwhile, the bipolar coin cell used lithium metal as the counter electrode and 1 mol / m³ of electrolyte. -3 Lithium bis(fluorosulfonyl)imide (LiFSI) was dissolved in a solution of 1,2-dimethoxyethane (DME, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and fabricated in a glove box (manufactured by Miwa Seisakusho) under an argon atmosphere. To fabricate the coin cell, a stainless steel (SUS) positive electrode case, gasket, working electrode (positive electrode), a Φ=16 mm fiberglass separator, 80 μL of electrolyte, a Φ=12 mm punched lithium metal (negative electrode), a spacer, a wave washer, and a SUS negative electrode case were assembled in that order, and then pressed and sealed using a coin cell crimping machine. Figure 4 is a schematic diagram showing the configuration of the two-electrode coin cell fabricated in the example.

[0061] Constant current charge-discharge measurements were performed using the obtained bipolar coin cell. In the constant current charge-discharge measurements in this embodiment, the current density was set to 20 mA. -1 The voltage was kept constant, and the voltage change was measured and evaluated when charging and discharging were repeated within the potential range of 0.5V to 3.0V.

[0062] In this example, the reversible capacitance and operating potential of the negative electrode active materials 1 to 10 were specifically evaluated. The results are shown in Table 1.

[0063]

[0064] [Evaluation of Negative Electrode Active Material 2] Among the compounds having an NSIT-type structure, negative electrode active material 8, which showed particularly outstanding electrochemical properties, was investigated in more detail. First, in order to investigate the suitability of negative electrode active material 8 as a negative electrode material for rapid charge and discharge, charge and discharge measurements were performed on a Li half cell in the potential range of 0.5V to 3.0V while changing the current density conditions every 5 cycles. Figure 5 is a graph showing the results of the evaluation of the electrochemical properties of negative electrode active material 8. Figure 5(a) shows the current densities during discharge at 20, 40, 100, 200, 400, 1000, 2000, and 4000 mA. -1 The current density during charging is changed in the following order: -1 This is the result of keeping it constant, and Figure 5(b) summarizes the discharge capacity of each cycle obtained. As shown in Figure 5, the current density was 4000 mAg. -1 The discharge capacity is 125 mAhg -1 And, 20 mAg -1 Available capacity: 190mAh -1 It was approximately 65% ​​of that. Finally, the current density during discharge was again measured at 20 mA. -1 A decrease in discharge capacity was confirmed when the system was returned to its original state. Considering these results, it is suggested that the negative electrode active material in this embodiment has excellent load characteristics.

[0065] The results of the above examples support the effectiveness of the negative electrode active material according to the present invention.

[0066] 1: negative electrode, 2: current collector, 3A, 3B: negative electrode active material layer​

Claims

1. A negative electrode active material composed of an oxide having an NSIT type structure, comprising a group 1 element, titanium, oxygen, and a sub-element different from the group 1 element, titanium, and oxygen.

2. The negative electrode active material according to claim 1, wherein the group 1 element is lithium or sodium.

3. A negative electrode active material according to claim 1 or claim 2, wherein the sub-element is an element belonging to Group 2 to Group 11.

4. The negative electrode active material according to claim 3, wherein the sub-element is selected from the group consisting of chromium, magnesium, iron, vanadium, and nickel.

5. The negative electrode active material according to any one of claims 1 to 4, wherein the sub-element is a divalent metallic element, and the oxide is represented by the following formula (1): A x M x/2 Ti 2-(x/2) O 4 ... (1) Here, A is a group 1 element, M is a divalent metallic element, and x is a value between 0.7 and 0.9, which is the negative electrode active material.

6. In the negative electrode active material according to any one of claims 1 to 4, the sub-element is a trivalent metallic element, and the oxide is represented by the following formula (2): A x M x Ti 2-x O 4 ... (2) Here, A is a group 1 element, M is a trivalent metallic element, and x is a value between 0.7 and 0.9, which is the negative electrode active material.

7. A method for producing a negative electrode active material according to any one of claims 1 to 6, comprising: a preparation step and a conversion step, wherein in the preparation step, a precursor comprising a group 1 element, titanium, oxygen, and the aforementioned sub-elements is prepared, and in the conversion step, the oxide is obtained by replacing the group 1 element contained in the precursor with another group 1 element.

8. A negative electrode having a structure in which a current collector and a negative electrode active material layer are laminated, wherein the negative electrode active material layer contains the negative electrode active material described in any one of claims 1 to 6.

9. A secondary battery having the negative electrode described in claim 8.