Plasticizing agent, vinyl chloride resin composition, molded body of said composition, and cable
A polyester plasticizer with specific reactive components enhances coolant resistance in vinyl chloride resin compositions, addressing the issue of rapid deterioration when exposed to coolant liquids.
Patent Information
- Application Number
- PCT/JP2026/014946
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-04-13
- Publication Date
- 2026-11-12
AI Technical Summary
Vinyl chloride resin compositions used in cable coverings deteriorate rapidly when exposed to coolant liquids due to lack of coolant resistance, particularly when used in machine tools where coolant is abundant.
A polyester plasticizer is developed using specific amounts of polyols and polycarboxylic acids with multiple hydroxyl or carboxyl groups, along with aliphatic diols and monocarboxylic acids, to enhance coolant resistance in vinyl chloride resin compositions.
The new plasticizer imparts coolant resistance to vinyl chloride resin compositions, preventing rapid deterioration and ensuring durability in environments with coolant exposure.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Plasticizer, vinyl chloride resin composition, molded article of the composition, and cable
[0001] The present invention relates to a plasticizer, a vinyl chloride resin composition, a molded article of the composition, and a cable.
[0002] Vinyl chloride resin (PVC) is one of the representative plastics. For the purpose of imparting properties such as flexibility and low-temperature characteristics and facilitating thermoformability, it is usually used after adding a plasticizer to soften the vinyl chloride resin.
[0003] Plasticizers for use in vinyl chloride resins are required to have various performances such as compatibility, cold resistance, and heat resistance, and higher alkyl esters of polybasic acids such as phthalic acid esters, adipic acid esters, and trimellitic acid esters are known. Above all, phthalic acid esters are generally used as plasticizers for vinyl chloride resins from the viewpoint of balance between cost and performance.
[0004] Vinyl chloride resin compositions containing a plasticizer are also used as covering materials for electric wires and cables, since vinyl chloride resins are nonflammable. For example, since cables used in machine tools require heat resistance, it has been proposed to use a polyester plasticizer in place of the phthalic acid ester plasticizer (for example, Patent Documents 1 to 3).
[0005] JP 2004-193138 A, JP 2006-291145 A, JP 2009-185199 A
[0006] When cutting with a machine tool, a large amount of coolant (cooling liquid) that suppresses heat generated during cutting is used. The coolant is composed of base oils such as mineral oils, synthetic oils and fatty oils, and various additives (antioxidants, rust inhibitors, non-ferrous metal corrosion inhibitors, antifoaming agents, extreme pressure agents, surfactants, etc.). When these are exposed to cables, there has been a problem that the covering material containing the polyester plasticizer undergoes rapid deterioration.
[0007] One problem that the present invention aims to solve is to provide a plasticizer that can impart coolant resistance. Another problem that the present invention aims to solve is to provide a vinyl chloride resin composition and a vinyl chloride resin molded article that can exhibit coolant resistance.
[0008] As a result of diligent research to solve the above problems, the inventors of the present invention have found that a plasticizer which is a polyester using a specific amount of a polyol having three or more hydroxyl groups in one molecule and / or a polycarboxylic acid having three or more carboxyl groups in one molecule can impart coolant resistance to resin molded products, and have completed the present invention.
[0009] In other words, the present invention relates to the following plasticizers, etc. 1. A plasticizer which is a polyester in which the reactive components are an aliphatic diol having 2 to 18 carbon atoms, an aliphatic dicarboxylic acid having 4 to 14 carbon atoms, a polyol having 3 or more hydroxyl groups in one molecule and / or a polycarboxylic acid having 3 or more carboxyl groups in one molecule, and a monoalcohol having 4 to 18 carbon atoms and / or a monocarboxylic acid having 2 to 21 carbon atoms, wherein the total content ratio of the polyol and the polycarboxylic acid in the reactive components is in the range of 0.3 to 5.0 mol%. 2. The plasticizer according to 1, wherein the polyol is one or more selected from glycerin, trimethylolpropane and pentaerythritol, and the polycarboxylic acid is one or more selected from trimellitic acid and pyromellitic acid. 3. 1. The plasticizer according to claim 1 or 2, wherein the aliphatic diol having 2 to 18 carbon atoms is one or more selected from 1,2-propanediol, 1,2-butanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, neopentyl glycol, and 3-methyl-1,5-pentanediol. 4. The plasticizer according to any one of claims 1 to 3, wherein the aliphatic dicarboxylic acid having 4 to 14 carbon atoms is one or more selected from adipic acid and sebacic acid. 5. The plasticizer according to any one of claims 1 to 4, wherein the monoalcohol having 4 to 18 carbon atoms is one or more selected from octanol, 2-ethylhexanol, and isononyl alcohol. 6. The plasticizer according to any one of claims 1 to 5, wherein the monocarboxylic acid having 2 to 21 carbon atoms comprises two or more aliphatic monocarboxylic acids having 8 to 21 carbon atoms. 7. The plasticizer according to any one of claims 1 to 6, wherein the monocarboxylic acid having 2 to 21 carbon atoms is a hydrogenated vegetable oil fatty acid. 8. The plasticizer according to any one of 1 to 7, wherein the polyester is a polyester in which the reaction components are an aliphatic diol having 2 to 18 carbon atoms, an aliphatic dicarboxylic acid having 2 to 12 carbon atoms, a polyol having 3 or more hydroxyl groups in one molecule, and a monocarboxylic acid having 2 to 21 carbon atoms. 9. The plasticizer according to any one of 1 to 8, wherein the hydroxyl value of the polyester is 15 mg KOH / g or less.10. A plasticizer according to any one of 1 to 9, wherein the number average molecular weight of the polyester is in the range of 1,500 to 4,000. 11. A plasticizer according to any one of 1 to 10, which is a plasticizer for vinyl chloride resin. 12. A vinyl chloride resin composition comprising the plasticizer according to any one of 1 to 11 and vinyl chloride resin. 13. A vinyl chloride resin composition according to 12, wherein the content of the plasticizer is in the range of 10 to 150 parts by mass per 100 parts by mass of the vinyl chloride resin. 14. A molded article of the vinyl chloride resin composition according to 12 or 13. 15. A cable comprising a conductor and an insulating coating layer covering the conductor, wherein the insulating coating layer is a molded article of the vinyl chloride resin composition according to any one of 12 to 14.
[0010] The present invention provides a plasticizer that can impart coolant resistance. The present invention also provides a vinyl chloride resin composition and a vinyl chloride resin molded article that can exhibit coolant resistance.
[0011] One embodiment of the present invention will be described below. The present invention is not limited to the following embodiments, and can be implemented with appropriate modifications without impairing the effects of the present invention. The compounds used herein may be derived from fossil resources or from biological resources.
[0012] [Plasticizer] The plasticizer of the present invention is a polyester in which the reactive components are an aliphatic diol having 2 to 18 carbon atoms, an aliphatic dicarboxylic acid having 4 to 14 carbon atoms, a polyol having 3 or more hydroxyl groups in one molecule and / or a polycarboxylic acid having 3 or more carboxyl groups in one molecule, and a monoalcohol having 4 to 18 carbon atoms and / or a monocarboxylic acid having 2 to 21 carbon atoms, wherein the total content of the polyol and the polycarboxylic acid in the reactive components is in the range of 0.3 to 5.0 mol%. Here, "reactive components" means components that constitute the polyester which is the plasticizer of the present invention (hereinafter sometimes simply referred to as "the polyester of the present invention"), and does not include solvents or catalysts that do not constitute the polyester.
[0013] It is presumed that setting the total content of polyols having three or more hydroxyl groups per molecule and / or polycarboxylic acids having three or more carboxyl groups per molecule in the reaction components to a range of 0.3 to 5.0 mol%, and slightly branching the polyester, is important for improving coolant resistance.
[0014] The lower limit of the total content of polyols having three or more hydroxyl groups per molecule and / or polycarboxylic acids having three or more carboxyl groups per molecule in the reaction components is, for example, 0.3 mol% or more, 0.5 mol% or more, or 1.0 mol% or more. The upper limit of the total content of polyols having three or more hydroxyl groups per molecule and / or polycarboxylic acids having three or more carboxyl groups per molecule in the reaction components is, for example, 5.0 mol% or less, 4.0 mol% or less, or 3.5 mol% or less.
[0015] The fatty chain of the aliphatic diol having 2 to 18 carbon atoms may be linear or branched, and may contain an alicyclic structure and / or ether bonds. Furthermore, the fatty chain of the aliphatic diol may be a saturated fatty chain or an unsaturated fatty chain having carbon-carbon unsaturated bonds.
[0016] The aliphatic diol having 2 to 18 carbon atoms is preferably an alkylene glycol having 2 to 18 carbon atoms or an oxyalkylene glycol having 2 to 18 carbon atoms.
[0017] The alkylene glycols having 2 to 18 carbon atoms include ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 2,2-dimethyl-1,3-propanediol (neopentyl glycol), 1,5-pentanediol, 2,2-diethyl-1,3-propanediol (3,3-dimethyl Examples include tyrolpentane), 2-n-butyl-2-ethyl-1,3-propanediol (3,3-dimethylolheptane), 3-methyl-1,5-pentanediol, 1,6-hexanediol, cyclohexanedimethanol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-octadecanediol.
[0018] The oxyalkylene glycol having 2 to 18 carbon atoms is, for example, an alkylene glycol having 2 to 18 carbon atoms and having one or more ether bonds (-O-), and examples include diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, and tripropylene glycol.
[0019] The aliphatic diol having 2 to 18 carbon atoms is preferably an aliphatic diol having 2 to 12 carbon atoms, and more preferably one or more selected from 1,2-propanediol, 1,2-butanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, neopentyl glycol, and 3-methyl-1,5-pentanediol.
[0020] The aliphatic diols having 2 to 18 carbon atoms, which are the reactive components of the polyester of the present invention, may be used individually or in combination of two or more.
[0021] The fatty chain of an aliphatic dicarboxylic acid having 4 to 14 carbon atoms may be linear or branched, and may contain alicyclic structures and / or ether bonds. Furthermore, the fatty chain of an aliphatic dicarboxylic acid having 4 to 14 carbon atoms may be a saturated fatty chain or an unsaturated fatty chain having carbon-carbon unsaturated bonds.
[0022] The aliphatic dicarboxylic acid having 4 to 14 carbon atoms is preferably an alkylenedicarboxylic acid having 4 to 14 carbon atoms, and more preferably an alkylenedicarboxylic acid having 6 to 12 carbon atoms.
[0023] Examples of alkylenedicarboxylic acids having 4 to 14 carbon atoms include succinic acid, glutaric acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid (dodecanediic acid), cyclohexanedicarboxylic acid, and hexahydrophthalic acid. Of these, adipic acid, azelaic acid, sebacic acid, and dodecanediic acid are more preferred, and adipic acid and sebacic acid are even more preferred.
[0024] The aliphatic dicarboxylic acid having 4 to 14 carbon atoms, which is the reactive component of the polyester of the present invention, may be used alone or in combination of two or more types.
[0025] The monoalcohol having 4 to 18 carbon atoms is preferably an aliphatic monoalcohol having 4 to 18 carbon atoms. The fatty chain of the aliphatic monoalcohol having 4 to 18 carbon atoms may be linear or branched, and may contain alicyclic structures and / or ether bonds. Furthermore, the fatty chain of the aliphatic monoalcohol having 4 to 18 carbon atoms may be a saturated fatty chain or an unsaturated fatty chain having carbon-carbon unsaturated bonds.
[0026] The aliphatic monoalcohol having 4 to 18 carbon atoms is preferably an alkyl alcohol having 4 to 18 carbon atoms, and more preferably one or more selected from butanol, heptanol, hexanol, cyclohexanol, heptanol, octanol, 2-ethylhexanol, isononyl alcohol, nonanol, decanol, undecanol, and dodecanol.
[0027] The monoalcohols having 4 to 18 carbon atoms, which are the reactive components of the polyester of the present invention, may be used alone or in combination of two or more.
[0028] The monocarboxylic acid having 2 to 21 carbon atoms is preferably an aliphatic monocarboxylic acid having 2 to 21 carbon atoms. The fatty chain of the aliphatic monocarboxylic acid having 2 to 21 carbon atoms may be linear or branched, and may contain an alicyclic structure and / or ether bonds. Furthermore, the fatty chain of the aliphatic monocarboxylic acid having 2 to 21 carbon atoms may be a saturated fatty chain or an unsaturated fatty chain having carbon-carbon unsaturated bonds.
[0029] Examples of the aliphatic monocarboxylic acids having 2 to 21 carbon atoms include acetic acid, caproic acid, 2-ethylhexanoic acid, caprylic acid, capric acid, lauric acid, myristic acid, pentadecyl acid, palmitic acid, margaric acid, stearic acid, and arachidic acid.
[0030] The monocarboxylic acid having 2 to 21 carbon atoms may be a hydrogenated vegetable oil fatty acid. Examples of such hydrogenated vegetable oil fatty acids include hydrogenated coconut oil fatty acid, hydrogenated palm kernel oil fatty acid, hydrogenated palm oil fatty acid, hydrogenated olive oil fatty acid, hydrogenated castor oil fatty acid, and hydrogenated rapeseed oil fatty acid. These are obtained by decomposing and hydrogenating oils obtained from coconut, palm kernel, palm, olive, castor, and rapeseed, respectively, and are all mixtures of long-chain aliphatic monocarboxylic acids containing two or more aliphatic monocarboxylic acids having 8 to 21 carbon atoms. In addition, the above vegetable oil fatty acids that have not been hydrogenated may be used as long as they do not impair the effects of the present invention. Furthermore, the vegetable oil fatty acids are not limited to those listed above.
[0031] The polyol having three or more hydroxyl groups in one molecule is preferably an aliphatic polyol having 3 to 12 carbon atoms and having three or more hydroxyl groups in one molecule. The fatty chain of the aliphatic polyol having 3 to 12 carbon atoms and having three or more hydroxyl groups in one molecule may be linear or branched, and may contain an alicyclic structure and / or ether bonds. Furthermore, the aliphatic polyol having three or more hydroxyl groups in one molecule may be a saturated fatty chain or an unsaturated fatty chain having carbon-carbon unsaturated bonds.
[0032] Examples of polyols having three or more hydroxyl groups in a single molecule (hereinafter sometimes simply referred to as "polyols") include trihydric alcohols such as glycerin, 1,1,1-trimethylolethane, 1,1,1-trimethylolpropane, trioxyisobutane, 1,2,3-butanetriol, 1,2,3-pentanetriol, 2,3,4-pentanetriol, and 1,2,5-hexanetriol; tetrahydric alcohols such as pentaerythritol; and pentahydric or higher alcohols such as dipentaerythritol, glucose, sucrose, and sorbitol.
[0033] The polyol is preferably one or more selected from glycerin, trimethylolpropane, and pentaerythritol.
[0034] The polyol, which is the reactive component of the polyester in the present invention, may be used alone or in combination of two or more types.
[0035] Examples of polycarboxylic acids having three or more carboxyl groups in a single molecule (hereinafter sometimes simply referred to as "polycarboxylic acid") include aromatic polycarboxylic acids having 9 to 20 carbon atoms (such as trimellitic acid and pyromellitic acid) and aliphatic polycarboxylic acids having 6 to 20 carbon atoms (such as hexanetricarboxylic acid and cyclohexanetetracarboxylic acid).
[0036] The polycarboxylic acid is preferably one or more selected from trimellitic acid and pyromellitic acid.
[0037] The polycarboxylic acid, which is the reactive component of the polyester in the present invention, may be used alone or in combination of two or more types.
[0038] The plasticizer of the present invention is preferably a polyester in which the reaction components are an aliphatic diol having 2 to 18 carbon atoms, an aliphatic dicarboxylic acid having 4 to 14 carbon atoms, a polyol having 3 or more hydroxyl groups in one molecule, and a monocarboxylic acid having 2 to 21 carbon atoms.
[0039] The polyester of the present invention may be reacted with an aliphatic diol having 2 to 18 carbon atoms, an aliphatic dicarboxylic acid having 4 to 14 carbon atoms, a polyol having 3 or more hydroxyl groups in one molecule and / or a polycarboxylic acid having 3 or more carboxyl groups in one molecule, and a monoalcohol having 4 to 18 carbon atoms and / or a monocarboxylic acid having 2 to 21 carbon atoms. Other reactants may be used as long as they do not impair the effects of the present invention.
[0040] The reaction components of the polyester of the present invention preferably consist substantially of an aliphatic diol having 2 to 18 carbon atoms, an aliphatic dicarboxylic acid having 4 to 14 carbon atoms, a polyol having 3 or more hydroxyl groups in one molecule and / or a polycarboxylic acid having 3 or more carboxyl groups in one molecule, and a monoalcohol having 4 to 18 carbon atoms and / or a monocarboxylic acid having 2 to 21 carbon atoms. Here, "substantially" means that the total of the aliphatic diol, aliphatic dicarboxylic acid, polyol, polycarboxylic acid, monoalcohol, and monocarboxylic acid is 90 mol% or more, 95 mol% or more, 98 mol% or more, 99 mol% or more, or 100 mol% of the reaction components of the polyester of the present invention.
[0041] The number-average molecular weight (Mn) of the polyester of the present invention is, for example, in the range of 500 to 6,000, preferably in the range of 500 to 4,000, more preferably in the range of 1,000 to 4,000, and even more preferably in the range of 1,500 to 4,000. The number-average molecular weight (Mn) of the polyester of the present invention is confirmed by the method described in the examples.
[0042] The acid value of the polyester of the present invention is preferably 2.0 mgKOH / g or less, more preferably 1.0 mgKOH / g or less, in terms of the upper limit. The lower limit of the acid value of the polyester of the present invention is preferably 0.01 mgKOH / g or more, more preferably 0.1 mgKOH / g or more. The hydroxyl value of the polyester of the present invention is preferably 20 mgKOH / g or less, more preferably 15 mgKOH / g or less, in terms of the upper limit. The lower limit of the hydroxyl value of the polyester of the present invention is preferably 0.1 mgKOH / g or more, more preferably 1.0 mgKOH / g or more. The viscosity of the polyester of the present invention is preferably 7,000 mPa·s or less, more preferably 5,000 mPa·s or less. The acid value, hydroxyl value and viscosity of the polyester of the present invention are confirmed by the methods described in the Examples.
[0043] [Method for Producing Plasticizer] The plasticizer of the present invention can be produced by reacting an aliphatic diol having 2 to 18 carbon atoms, an aliphatic dicarboxylic acid having 4 to 14 carbon atoms, a polyol having 3 or more hydroxyl groups in one molecule and / or a polycarboxylic acid having 3 or more carboxyl groups in one molecule, and a monoalcohol having 4 to 18 carbon atoms and / or a monocarboxylic acid having 2 to 21 carbon atoms to synthesize a polyester. The total content ratio of the polyol and the polycarboxylic acid in the components to be reacted is in the range of 0.3 to 5.0 mol%, and the charged amount is adjusted to fall within this range.
[0044] For the production of the polyester, for example, the following methods can be adopted. Method 1: A method of collectively charging an aliphatic diol, an aliphatic dicarboxylic acid, a polyol and / or a polycarboxylic acid, a monoalcohol and / or a monocarboxylic acid, and reacting them Method 2: Reacting an aliphatic diol, an aliphatic dicarboxylic acid, a polyol and / or a polycarboxylic acid to produce a terminal unblocked polyester, and reacting the terminals of the terminal unblocked polyester with a monoalcohol and / or a monocarboxylic acid
[0045] In the synthesis of polyester, the aforementioned reaction is preferably carried out as an esterification reaction for 5 to 25 hours within a temperature range of, for example, 180 to 250°C, in the presence of an esterification catalyst as necessary. The conditions such as the temperature and time of the esterification reaction are not particularly limited, and may be set as appropriate.
[0046] Examples of the esterification catalyst include titanium-based catalysts such as tetraisopropyl titanate and tetrabutyl titanate; tin-based catalysts such as dibutyltin oxide; and organic sulfonic acid-based catalysts such as p-toluenesulfonic acid.
[0047] The usage amount of the esterification catalyst may be set as appropriate, but is usually preferably in the range of 0.001 to 0.1 parts by mass relative to 100 parts by mass of the total amount of reaction components.
[0048] [Vinyl Chloride Resin Composition] The plasticizer of the present invention can be suitably used as a plasticizer for vinyl chloride resins. The vinyl chloride resin composition of the present invention contains the plasticizer of the present invention and a vinyl chloride resin.
[0049] The vinyl chloride resin includes homopolymers of vinyl chloride, homopolymers of vinylidene chloride, copolymers containing vinyl chloride as an essential component, copolymers containing vinylidene chloride as an essential component, and the like. When the vinyl chloride resin is a copolymer containing vinyl chloride as an essential component or a copolymer containing vinylidene chloride as an essential component, examples of copolymerizable comonomers include α-olefins such as ethylene, propylene, and 1-butene; conjugated dienes such as butadiene and isoprene; vinyl alcohol, styrene, acrylonitrile, vinyl acetate, vinyl propionate, fumaric acid, fumaric acid esters, maleic acid, maleic acid esters, maleic anhydride, acrylic acid, acrylic acid esters, methacrylic acid, methacrylic acid esters, isoprenol, and the like.
[0050] The degree of polymerization of the vinyl chloride resin is usually in the range of 300 to 5,000, preferably in the range of 400 to 3,500, and more preferably in the range of 700 to 3,000. When the degree of polymerization of the vinyl chloride resin falls within this range, a molded article with high heat resistance can be obtained, and a vinyl chloride resin composition having excellent processability can be achieved.
[0051] Polyvinyl chloride resin can be manufactured by known methods, such as suspension polymerization in the presence of an oil-soluble polymerization catalyst, or emulsion polymerization in an aqueous medium in the presence of a water-soluble polymerization catalyst. Commercially available polyvinyl chloride resin may also be used. Examples of commercially available polyvinyl chloride resins include TH-640, TH-700, TH-800 (all manufactured by Taiyo Vinyl Chloride Co., Ltd.); S-1004, S-1008, PSH-10 (all manufactured by Kaneka Corporation); TK-700, TK-800, TK-1300 (all manufactured by Shin-Etsu Polymer Co., Ltd.); and ZEST800Z, ZEST1000Z, ZEST1300Z (all manufactured by Shin-Daiichi Vinyl Chloride Co., Ltd.).
[0052] The content of the plasticizer of the present invention in the vinyl chloride resin composition of the present invention is preferably in the range of 10 to 150 parts by mass, more preferably in the range of 30 to 120 parts by mass, even more preferably in the range of 50 to 120 parts by mass, and particularly preferably in the range of 70 to 120 parts by mass, per 100 parts by mass of vinyl chloride resin, from the viewpoint of compatibility with vinyl chloride resin and the like.
[0053] The vinyl chloride resin composition of the present invention may contain a vinyl chloride resin and the plasticizer of the present invention, and may also contain plasticizers other than the plasticizer of the present invention (other plasticizers), other additives, etc.
[0054] Examples of the aforementioned other plasticizers include benzoic acid esters such as diethylene glycol dibenzoate; phthalate esters such as dibutyl phthalate (DBP), di-2-ethylhexyl phthalate (DOP), diisononyl phthalate (DINP), diisodecyl phthalate (DIDP), diundecyl phthalate (DUP), and ditridecyl phthalate (DTDP); and bis(2-ethylhexyl) terephthalate (DOTP) Terephthalate esters such as ); isophthalate esters such as bis(2-ethylhexyl) isophthalate (DOIP); pyromellitic acid esters such as tetra-2-ethylhexyl pyromellitic acid (TOPM); di-2-ethylhexyl adipate (DOA), diisononyl adipate (DINA), diisodecyl adipate (DIDA), di-(2-ethylhexyl) azelate, diisooctyl azelate, Examples include aliphatic dibasic acid esters such as azelaic acid derivatives like di-n-hexylazelate; phosphate esters such as tri-2-ethylhexyl phosphate (TOP) and tricresyl phosphate (TCP); alkyl esters of polyhydric alcohols such as pentaerythritol; polyesters with molecular weights of 800 to 4,000 synthesized by polyesterizing dibasic acids such as adipic acid with glycols; epoxidized esters such as epoxidized soybean oil and epoxidized linseed oil; alicyclic dibasic acids such as diisononyl hexahydrophthalate; fatty acid glycol esters such as 1,4-butanediol dicaprate; tributyl acetyl citrate (ATBC); chlorinated paraffins obtained by chlorinating paraffin wax and n-paraffin; chlorinated fatty acid esters such as chlorinated stearate; and higher fatty acid esters such as butyl oleate.
[0055] Among other plasticizers, it is preferable to use one or more selected from trimellitic acid ester plasticizers and sebacitic acid derivative plasticizers.
[0056] The above trimellitic acid ester plasticizers include trimethyl trimellitic acid, triethyl trimellitic acid, tri-n-propyl trimellitic acid, tri-n-butyl trimellitic acid, tri-n-pentyl trimellitic acid, tri-n-hexyl trimellitic acid, tri-n-heptyl trimellitic acid, tri-n-octyl trimellitic acid, tri-n-nonyl trimellitic acid, tri-n-decyl trimellitic acid, tri-n-undecyl trimellitic acid, tri-n-dodecyl trimellitic acid, and trimellitic acid. Linear trimellitic esters in which the alkyl groups constituting the ester are linear, such as tri-n-tridecyl trimellitic acid, tri-n-tetradecyl trimellitic acid, tri-n-pentadecyl trimellitic acid, tri-n-hexadecyl trimellitic acid, tri-n-heptadecyl trimellitic acid, tri-n-stearyl trimellitic acid, and tri-n-alkyl trimellitic acid (where the number of carbon atoms in the alkyl group of the tri-n-alkyl trimellitic acid ester may differ from one another within a single molecule); Examples include branched trimellitic acid esters, such as tri-i-propyl trimellitic acid, tri-i-butyl trimellitic acid, tri-i-pentyl trimellitic acid, tri-i-hexyl trimellitic acid, tri-i-heptyl trimellitic acid, tri-i-octyl trimellitic acid, tri-(2-ethylhexyl) trimellitic acid, tri-i-nonyl trimellitic acid, tri-i-decyl trimellitic acid, tri-i-undecyl trimellitic acid, tri-i-dodecyl trimellitic acid, tri-i-tridecyl trimellitic acid, tri-i-tetradecyl trimellitic acid, tri-i-pentadecyl trimellitic acid, tri-i-hexadecyl trimellitic acid, tri-i-heptadecyl trimellitic acid, tri-i-octadecyl trimellitic acid, and trialkyl trimellitic acid esters (where the number of carbon atoms in the alkyl group of the trialkyl trimellitic acid ester may differ from one another within a single molecule).
[0057] Examples of the above-mentioned sebaciate derivative plasticizers include di-n-butyl sebacate, di-(2-ethylhexyl) sebacate, diisodecyl sebacate, and di-(2-butyloctyl) sebacate.
[0058] The above-mentioned other plasticizers may be used individually or in combination of two or more.
[0059] Among the other plasticizers mentioned above, trimellitic acid esters and sebacinic acid derivatives are preferred from the viewpoint of obtaining good tensile elongation and cold resistance.
[0060] When the above-mentioned other plasticizers are used in the vinyl chloride resin composition of the present invention, the content of the other plasticizers is, for example, in the range of 10 to 300 parts by mass, preferably in the range of 20 to 200 parts by mass, per 100 parts by mass of the vinyl chloride resin plasticizer of the present invention.
[0061] Examples of the aforementioned other additives include flame retardants, stabilizers, stabilizing aids, colorants, processing aids, fillers, antioxidants (anti-aging agents), ultraviolet absorbers, light stabilizers, lubricants, antistatic agents, crosslinking aids, and the like.
[0062] Examples of the aforementioned flame retardants include inorganic compounds such as aluminum hydroxide, antimony trioxide, magnesium hydroxide, and zinc borate; phosphorus compounds such as cresyl diphenyl phosphate, trischloroethyl phosphate, trischloropropyl phosphate, and trisdichloropropyl phosphate; and halogen compounds such as chlorinated paraffin. When a flame retardant is incorporated into a vinyl chloride resin composition, the amount is usually in the range of 0.1 to 20 parts by mass per 100 parts by mass of vinyl chloride resin.
[0063] Examples of the aforementioned stabilizers include metal soap compounds such as lithium stearate, magnesium stearate, magnesium laurate, calcium ricinoleate, calcium stearate, barium laurate, barium ricinoleate, barium stearate, zinc octoate, zinc laurate, zinc ricinoleate, and zinc stearate; organotin compounds such as dimethyltin bis-2-ethylhexylthioglycolate, dibutyltin maleate, dibutyltin bisbutylmaleate, and dibutyltin dilaurate; antimony mercaptide compounds; and lanthanide-containing compounds such as lanthanum oxide and lanthanum hydroxide. When a stabilizer is incorporated into a vinyl chloride resin composition, the amount is usually in the range of 0.1 to 20 parts by mass per 100 parts by mass of vinyl chloride resin.
[0064] Examples of the stabilizing agent include phosphite compounds such as triphenyl phosphite, monooctyldiphenyl phosphite, and tridecyl phosphite; beta-diketone compounds such as acetylacetone and benzoylacetone; polyol compounds such as glycerin, sorbitol, pentaerythritol, and polyethylene glycol; perchlorate compounds such as barium perchlorate and sodium perchlorate; hydrotalcite compounds; and zeolites. When a stabilizing agent is incorporated into a vinyl chloride resin composition, the amount is usually in the range of 0.1 to 20 parts by mass per 100 parts by mass of vinyl chloride resin.
[0065] Examples of the aforementioned colorants include carbon black, lead sulfide, white carbon, titanium white, lithopone, red ochre, antimony sulfide, chromium yellow, chromium green, cobalt blue, and molybdenum orange. When a colorant is incorporated into a vinyl chloride resin composition, the amount is usually in the range of 1 to 100 parts by mass per 100 parts by mass of vinyl chloride resin.
[0066] Examples of the processing aids include liquid paraffin, polyethylene wax, stearic acid, stearate amide, ethylenebisstearate amide, butyl stearate, and calcium stearate. When a processing aid is incorporated into a vinyl chloride resin composition, the amount is usually in the range of 0.1 to 20 parts by mass per 100 parts by mass of vinyl chloride resin.
[0067] Examples of fillers include calcium carbonate, silica, alumina, clay, talc, diatomaceous earth, metal oxides such as ferrite; glass, carbon, metal fibers and powders; glass spheres, graphite, aluminum hydroxide, barium sulfate, magnesium oxide, magnesium carbonate, magnesium silicate, calcium silicate, and the like. When a filler is incorporated into a vinyl chloride resin composition, the amount is usually in the range of 1 to 100 parts by mass per 100 parts by mass of vinyl chloride resin.
[0068] Examples of the antioxidants include phenolic compounds such as 2,6-di-tert-butylphenol, tetrakis[methylene-3-(3,5-tert-butyl-4-hydroxyphenol)propionate]methane, and 2-hydroxy-4-methoxybenzophenone; sulfuric compounds such as alkyl disulfides, thiodipropionates, and benzothiazoles; phosphoric acid compounds such as trisnonylphenyl phosphite, diphenylisodecyl phosphite, triphenyl phosphite, and tris(2,4-di-tert-butylphenyl) phosphite; and organometallic compounds such as zinc dialkyldithiophosphate and zinc diaryldithiophosphate. When an antioxidant is incorporated into a vinyl chloride resin composition, the amount is usually in the range of 0.2 to 20 parts by mass per 100 parts by mass of vinyl chloride resin.
[0069] Examples of the UV absorbers include salicylate compounds such as phenyl salicylate and p-tert-butylphenyl salicylate; benzophenone compounds such as 2-hydroxy-4-n-octoxybenzophenone and 2-hydroxy-4-n-methoxybenzophenone; benzotriazole compounds such as 5-methyl-1H-benzotriazole and 1-dioctylaminomethylbenzotriazole; and cyanoacrylate compounds. When the UV absorber is incorporated into a vinyl chloride resin composition, the amount is usually in the range of 0.1 to 10 parts by mass per 100 parts by mass of vinyl chloride resin.
[0070] Examples of the aforementioned light stabilizers include hindered amine-based light stabilizers. Specifically, for example, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate and methyl 1,2,2,6,6-pentamethyl-4-piperidyl sebacate (mixture), bis(1,2,2,6,6-pentamethyl-4-piperidyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmalonate, bis(2,2,6,6-) decandioate Tetramethyl-1(octyloxy)-4-piperidyl) ester and reaction products of 1,1-dimethylethyl hydroperoxide and octane, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, ester mixture of 2,2,6,6-tetramethyl-4-piperidinol and higher fatty acids, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate, tetrakis(1,2,2,6,6-pentame (Tyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate, polycondensate of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol, poly{(6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl){(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}}, dibutylamine Examples include a polycondensate of 1,3,5-triazine, N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl-1,6-hexamethylenediamine and N-(2,2,6,6-tetramethyl-4-piperidyl)butylamine, and N,N',N'',N'''-tetrakis-(4,6-bis-(butyl-(N-methyl-2,2,6,6-tetramethylpiperidine-4-yl)amino)-triazine-2-yl)-4,7-diazadecane-1,10-diamine. When a light stabilizer is incorporated into a vinyl chloride resin composition, the amount is usually in the range of 0.1 to 10 parts by mass per 100 parts by mass of vinyl chloride resin.
[0071] Examples of the lubricants include silicone, liquid paraffin, paraffin wax, fatty acid metal salts such as metal stearate and metal laurate; fatty acid amides, fatty acid waxes, and higher fatty acid waxes. When a lubricant is incorporated into a vinyl chloride resin composition, the amount is usually in the range of 0.1 to 10 parts by mass per 100 parts by mass of vinyl chloride resin.
[0072] Examples of the antistatic agents include anionic antistatic agents of the alkyl sulfonate, alkyl ether carboxylic acid, or dialkyl sulfosuccinate type; nonionic antistatic agents such as polyethylene glycol derivatives, sorbitan derivatives, and diethanolamine derivatives; cationic antistatic agents such as quaternary ammonium salts of the alkylamidoamine type and alkyldimethylbenzyl type, and organic acid salts or hydrochlorides of the alkylpyridinium type; and amphoteric antistatic agents such as alkyl betaine type and alkylimidazoline type. When an antistatic agent is incorporated into a vinyl chloride resin composition, the amount is usually in the range of 0.1 to 10 parts by mass per 100 parts by mass of vinyl chloride resin.
[0073] Examples of the crosslinking aids include polyfunctional monomers such as tetraethylene glycol dimethacrylate, divinylbenzene diallyl phthalate, triallyl isocyanurate, trimethylolpropane trialylate, tetramethylolmethane tetramethacrylate, and trimethoxyethoxyvinylsilane. When the crosslinking aid is incorporated into a vinyl chloride resin composition, the amount is usually in the range of 0.5 to 30 parts by mass per 100 parts by mass of vinyl chloride resin.
[0074] The vinyl chloride resin composition of the present invention can be produced by known methods. For example, the vinyl chloride resin composition of the present invention can be prepared by mixing vinyl chloride resin, the plasticizer of the present invention, and optional components (the aforementioned other plasticizers and other additives) using a kneader such as a blender, planetary mixer, or Banbury mixer.
[0075] [Molded Article] A molded article obtained by molding the vinyl chloride resin composition of the present invention (hereinafter sometimes referred to as "the molded article of the present invention") can exhibit high coolant resistance in addition to heat resistance, cold resistance, etc. Here, "coolant resistance" means that even if the molded article is exposed to coolant liquid for a long period of time, the plasticizer will not dissolve into the coolant liquid and the molded article will not deteriorate.
[0076] The above-mentioned coolant is a cooling fluid used to suppress heat generation during cutting processes, for example, when using a machine tool. This coolant is based on mineral oil, synthetic oil, fatty oil, etc., and contains various additives (antioxidants, rust inhibitors, non-ferrous metal corrosion inhibitors, defoamers, extreme pressure agents, surfactants, etc.). Some coolants are used diluted with water, and the molded articles of the present invention can exhibit higher resistance to such water-containing coolants.
[0077] The molded articles of the present invention are not particularly limited in their manufacturing method and can be obtained by molding the vinyl chloride resin composition of the present invention using known molding methods such as vacuum molding, compression molding, extrusion molding, calendering, press molding, blow molding, powder molding, and powder slush molding.
[0078] The molded articles of the present invention can be used, for example, in insulating tapes, insulating sheets, wiring connectors, wire coverings, pipes such as water pipes, pipe fittings, gutters such as rain gutters, window frame siding, flat sheets, corrugated sheets, automotive underbody coatings, dashboards, instrument panels, consoles, door sheets, undercarpets, trunk sheets, door trims and other automotive components, various types of leather, decorative sheets, agricultural films, food packaging films, various foam products, hoses, medical tubes, food tubes, refrigerator gaskets, packings, wallpaper, flooring, boots, curtains, shoe soles, gloves, water-stopping plates, toys, decorative panels, blood bags, infusion bags, tarpaulins, mats, waterproofing sheets, civil engineering sheets, roofing, waterproofing sheets, industrial tapes, glass films, erasers, and the like.
[0079] Among the above applications, the molded article obtained from the polyvinyl chloride resin composition of the present invention can be suitably used as an insulating coating layer for a cable comprising a conductor and an insulating coating layer covering the conductor.
[0080] The present invention will be specifically described below with reference to examples and comparative examples. However, the present invention is not limited to the following examples.
[0081] In the embodiments of this application, the values of acid value, hydroxyl value, and viscosity were evaluated by the following methods. [Method for measuring acid value] Measured according to the method in accordance with JIS K0070-1992. [Method for measuring hydroxyl value] Measured according to the method in accordance with JIS K0070-1992. [Method for measuring viscosity] Measured according to the method in accordance with JIS K6901-1986.
[0082] In the present embodiment, the number-average molecular weight of the polyester is a value converted to polystyrene based on GPC measurement, and the measurement conditions are as follows: [GPC Measurement Conditions] Measurement device: Tosoh Corporation high-speed GPC device "HLC-8420GPC" Column: Tosoh Corporation "TSKgel SuperMultiporeHZ-N" x 4 Detector: RI (differential refractometer) Data processing: Tosoh Corporation "EcoSEC Data Analysis Version 1.07" Column temperature: 40°C Developing solvent: Tetrahydrofuran Flow rate: 0.35 mL / min Sample: 20 mg of the sample was dissolved in 10 ml of tetrahydrofuran, and the resulting solution was filtered through a microfilter to be used as the sample. Sample injection volume: 20 μl Standard substance: Tosoh Corporation "PStQuick MP-N"
[0083] (Synthesis Example 1: Synthesis of Polyester Plasticizer A) In a 1-liter four-necked flask equipped with a thermometer, stirrer, and reflux condenser, 292.0 g of adipic acid, 6.86 g of trimellitic anhydride, 295.8 g of 3-methyl-1,5-pentanediol, 146.4 g of hydrogenated coconut oil fatty acid, and 0.037 g of tetraisopropyl titanate as an esterification catalyst were charged. The mixture was heated in stages to 230°C while stirring under a nitrogen atmosphere, and heating was continued at 230°C, with the generated water being continuously removed to obtain polyester plasticizer A (acid value 0.2 mg KOH / g, hydroxyl value 10.6 mg KOH / g, viscosity 1,250 mPa·s (25°C), Mn 2,070).
[0084] (Synthesis Example 2: Synthesis of Polyester Plasticizer B) In a 1-liter four-necked flask equipped with a thermometer, stirrer, and reflux condenser, 321.2 g of adipic acid, 14.5 g of glycerin, 289.3 g of 3-methyl-1,5-pentanediol, 161.1 g of hydrogenated coconut oil fatty acid, and 0.039 g of tetraisopropyl titanate as an esterification catalyst were charged. The mixture was heated in stages to 230°C while stirring under a nitrogen atmosphere, and heating was continued at 230°C, with the generated water being continuously removed to obtain polyester plasticizer B (acid value 1.2 mg KOH / g, hydroxyl value 8.8 mg KOH / g, viscosity 1,820 mPa·s (25°C), Mn 2,350).
[0085] (Synthesis Example 3: Synthesis of Polyester Plasticizer C) In a 1-liter four-necked flask equipped with a thermometer, stirrer, and reflux condenser, 321.2 g of adipic acid, 14.5 g of glycerin, 220.6 g of 2-methyl-1,3-propanediol, 161.1 g of hydrogenated coconut oil fatty acid, and 0.036 g of tetraisopropyl titanate as an esterification catalyst were charged. The mixture was heated in stages to 230°C while stirring under a nitrogen atmosphere, and heating was continued at 230°C, with the generated water being continuously removed to obtain polyester plasticizer C (acid value 0.2 mg KOH / g, hydroxyl value 7.3 mg KOH / g, viscosity 3,750 mPa·s (25°C), Mn 2,350).
[0086] (Synthesis Example 4: Synthesis of Polyester Plasticizer D) In a 1-liter four-necked flask equipped with a thermometer, stirrer, and reflux condenser, 321.2 g of adipic acid, 11.6 g of glycerin, 285.4 g of 3-methyl-1,5-pentanediol, 128.9 g of hydrogenated coconut oil fatty acid, and 0.037 g of tetraisopropyl titanate as an esterification catalyst were charged. The mixture was heated in stages to 230°C while stirring under a nitrogen atmosphere, and heating was continued at 230°C, with the generated water being continuously removed to obtain polyester plasticizer D (acid value 0.3 mg KOH / g, hydroxyl value 13.2 mg KOH / g, viscosity 2,330 mPa·s (25°C), Mn 2,620).
[0087] (Synthesis Example 5: Synthesis of Polyester Plasticizer E) In a 1-liter four-necked flask equipped with a thermometer, stirrer, and reflux condenser, 321.2 g of adipic acid, 12.8 g of pentaerythritol, 285.4 g of 3-methyl-1,5-pentanediol, 128.9 g of hydrogenated coconut oil fatty acid, and 0.037 g of tetraisopropyl titanate as an esterification catalyst were charged. The mixture was heated in stages to 230°C while stirring under a nitrogen atmosphere, and heating was continued at 230°C, with the generated water being continuously removed to obtain polyester plasticizer E (acid value 0.4 mg KOH / g, hydroxyl value 12.1 mg KOH / g, viscosity 3,200 mPa·s (25°C), Mn 2,850). Evaluation of Polyester Plasticizer E: A vinyl chloride resin composition (5) was prepared in the same manner as in Example 1, except that plasticizer E was used instead of plasticizer A, and various evaluations were performed.
[0088] (Synthesis Example 6: Synthesis of Polyester Plasticizer F) In a 1-liter four-necked flask equipped with a thermometer, stirrer, and reflux condenser, 365.0 g of adipic acid, 19.1 g of trimethylolpropane, 324.3 g of 3-methyl-1,5-pentanediol, 146.4 g of hydrogenated coconut oil fatty acid, and 0.043 g of tetraisopropyl titanate as an esterification catalyst were charged. The mixture was heated in stages to 230°C while stirring under a nitrogen atmosphere, and heating was continued at 230°C, with the generated water being continuously removed to obtain polyester plasticizer F (acid value 0.1 mg KOH / g, hydroxyl value 12.4 mg KOH / g, viscosity 2,740 mPa·s (25°C), Mn 2,540).
[0089] (Synthesis Comparative Example 1: Synthesis of Polyester Plasticizer A') In a 3-liter four-necked flask equipped with a thermometer, stirrer, and reflux condenser, 1168.0 g of adipic acid, 655.2 g of 2-methyl-1,3-propanediol, 287.9 g of isononyl alcohol, and 0.106 g of tetraisopropyl titanate as an esterification catalyst were charged. The mixture was heated in stages to 230°C while stirring under a nitrogen atmosphere, and heating was continued at 230°C, with the generated water being continuously removed to obtain polyester plasticizer A' (acid value 0.2 mg KOH / g, hydroxyl value 4.6 mg KOH / g, viscosity 2,710 mPa·s (25°C), Mn 2,290).
[0090] (Synthesis Comparative Example 2: Synthesis of Polyester Plasticizer B') In a 1-liter four-necked flask equipped with a thermometer, stirrer, and reflux condenser, 365.0 g of adipic acid, 48.9 g of glycerin, 241.5 g of 3-methyl-1,5-pentanediol, 109.0 g of hydrogenated coconut oil fatty acid, and 0.039 g of tetraisopropyl titanate as an esterification catalyst were charged. The mixture was heated in stages to 230°C while stirring under a nitrogen atmosphere, and heating was continued at 230°C, with the generated water being continuously removed to obtain polyester plasticizer B' (acid value 0.8 mg KOH / g, hydroxyl value 10.5 mg KOH / g, viscosity 2,110 mPa·s (25°C), Mn 2,680).
[0091] (Preparation of vinyl chloride resin composition (1)) 100 parts by mass of vinyl chloride resin (degree of polymerization 1,000, ZEST1000Z, manufactured by Shin-Daiichi Vinyl Chloride Co., Ltd.), 50 parts by mass of the obtained polyester plasticizer A, and 4 parts by mass of filler (Greg MP-677D (calcium / zinc composite stabilizer), manufactured by Nisshin Trading Co., Ltd.) were mixed to obtain vinyl chloride resin composition (1). The following evaluation was performed using the obtained vinyl chloride resin composition (1). The results are shown in Table 1.
[0092] (Evaluation of the plasticizing performance of the plasticizer) A vinyl chloride resin composition (1) prepared with two rolls heated to 170°C was kneaded for 10 minutes. The kneaded vinyl chloride resin composition (1) was then molded using a mold that can produce a molded product with a thickness of 1.0 mm (1.0 mm thick mold) and a press heated to 170°C to produce a 1.0 mm thick sheet.
[0093] The obtained sheets were evaluated for 100% modulus (tensile stress at 100% elongation) and tensile elongation according to JIS K6251:2010. Specifically, tensile tests were conducted using 1.0 mm thick sheets under the following conditions, and the 100% modulus and tensile elongation were evaluated. The results are shown in Table 1. The tensile elongation is calculated by subtracting the initial chuck distance of 20 mm from the chuck distance at which the 1.0 mm thick sheet fractured under tension, and dividing the result by the chuck distance of 20 mm, then expressing it as a percentage. Measuring instrument: Tensilon universal material testing machine (manufactured by Orientec Co., Ltd.) Sample shape: Dumbbell-shaped No. 3 Chuck distance: 20 mm Tensile speed: 200 mm / min Measurement atmosphere: Temperature 23 degrees Celsius, humidity 50%
[0094] A lower 100% modulus value indicates a higher plasticizing effect on polyvinyl chloride resin. Similarly, a higher tensile elongation indicates a higher plasticizing effect on polyvinyl chloride resin.
[0095] (Evaluation of cold resistance of molded products) A vinyl chloride resin composition (1) prepared with two rolls heated to 170°C was kneaded for 10 minutes. The kneaded vinyl chloride resin composition (1) was then molded using a mold that produces 1.0 mm thick molded products (1.0 mm thick mold) and a press heated to 170°C to produce a 1.0 mm thick sheet. Test specimens were prepared from the obtained sheet in accordance with the test method specified in JIS K6745:2015, and the flexibility temperature (unit: °C) was evaluated using a Crushberg flexibility temperature tester. The results are shown in Table 1. A lower flexibility temperature indicates better cold resistance.
[0096] (Evaluation of heat resistance of molded product) A vinyl chloride resin composition (1) prepared with two rolls heated to 170°C was kneaded for 10 minutes. The kneaded vinyl chloride resin composition (1) was then molded using a mold that produces a 1.0 mm thick mold (1.0 mm thick mold) and a press heated to 170°C to produce a 1.0 mm thick sheet. From the prepared 1.0 mm thick sheet, a dumbbell-shaped No. 3 dumbbell test piece was prepared in accordance with JIS K6251:2010.
[0097] The fabricated dumbbell test specimens were subjected to a heat aging test at 136°C for 168 hours in accordance with JIS K6257:2017. The mass of the dumbbell test specimens was measured before and after the heat aging test, and the weight loss rate ((mass before heat aging test - mass after heat aging test) / mass before heat aging test) was calculated. The results are shown in Table 1. The smaller the weight loss rate, the more polyester plasticizer A remains in the molded product after the heat aging test, and the greater the expected heat resistance effect of polyester plasticizer A.
[0098] (Evaluation of coolant resistance of molded products) A vinyl chloride resin composition (1) prepared with two rolls heated to 170°C was kneaded for 10 minutes. The kneaded vinyl chloride resin composition (1) was then molded using a mold that produces a 1.0 mm thick mold (1.0 mm thick mold) and a press heated to 170°C to produce a 1.0 mm thick sheet. From the prepared 1.0 mm thick sheet, a dumbbell-shaped No. 3 dumbbell test piece was prepared in accordance with JIS K6251:2010.
[0099] The coolant resistance of the fabricated dumbbell test specimens was evaluated. Specifically, the dumbbell test specimens were immersed in a test tube filled with a water-soluble coolant solution (Yushiroken Synthetic #880, manufactured by Yushiro Chemical Co., Ltd.), and the coolant resistance test was conducted by maintaining this condition at 85°C for 136 hours. The mass of the dumbbell specimens was measured before and after the coolant resistance test, and the difference (weight loss) between the mass before and after the coolant resistance test was calculated as a percentage, with the mass before the coolant resistance test as the baseline. A smaller value indicates that polyester plasticizer A remains in the molded product even after the coolant resistance test, suggesting that the coolant resistance effect of polyester plasticizer A can be expected.
[0100] (Evaluation of Plasticizer Compatibility) A vinyl chloride resin composition (1) prepared with two rolls heated to 170°C was kneaded for 10 minutes. The kneaded vinyl chloride resin composition (1) was then molded using a mold that produces a 1.0 mm thick mold (1.0 mm thick mold) and a press heated to 170°C to produce a 1.0 mm thick sheet. Two 1.0 mm thick sheets were cut from this sheet to a size of 5 cm x 5 cm. The two sheets were stacked and left for 30 days under conditions of 70°C and 95% relative humidity. After that, the condition of the sheet surface and the surface where the sheets overlapped was evaluated according to the following evaluation criteria. The results are shown in Table 1. ○: The sheet surface and the surface where the sheets overlapped were visually inspected and no foreign matter (bleed) such as powder or viscosity was detected, and no bleeding was detected when the sheet surface and the surface where the sheets overlapped were touched with a finger. ×: Bleeding can be confirmed by visually inspecting the surface of the sheet and the surfaces where the sheets overlap, or by touching the surface of the sheet and the surfaces where the sheets overlap with a finger.
[0101] A vinyl chloride resin composition was prepared and evaluated in the same manner as in Example 1, except that a plasticizer shown in Table 1 was used instead of plasticizer A. The results are shown in Table 1.
[0102]
[0103] The symbols in Table 1 have the following meanings: AA: Adipic acid TMA: Trimellitic acid Gly: Glycol PE: Pentaerythritol TMP: Trimethylolpropane HCFA: Hydrogenated coconut oil fatty acid INA: Isononyl alcohol
[0104] From the results of Examples 1-6 and Comparative Examples 1-2 in Table 1, it can be seen that plasticizers for polyesters that do not use any polyols having three or more hydroxyl groups per molecule or polycarboxylic acids having three or more carboxyl groups per molecule do not provide coolant resistance (Comparative Example 1-2), while plasticizers for polyesters that use a specific amount of polyols having three or more hydroxyl groups per molecule and / or polycarboxylic acids having three or more carboxyl groups per molecule provide excellent coolant resistance. Furthermore, it can be seen that using too much polyols having three or more hydroxyl groups per molecule and / or polycarboxylic acids having three or more carboxyl groups per molecule does not provide coolant resistance (Comparative Example 3).
Claims
1. A plasticizer which is a polyester in which the reactive components are an aliphatic diol having 2 to 18 carbon atoms, an aliphatic dicarboxylic acid having 4 to 14 carbon atoms, a polyol having 3 or more hydroxyl groups in one molecule and / or a polycarboxylic acid having 3 or more carboxyl groups in one molecule, and a monoalcohol having 4 to 18 carbon atoms and / or a monocarboxylic acid having 2 to 21 carbon atoms, wherein the total content of the polyol and the polycarboxylic acid in the reactive components is in the range of 0.3 to 5.0 mol%.
2. The plasticizer according to claim 1, wherein the polyol is one or more selected from glycerin, trimethylolpropane, and pentaerythritol, and the polycarboxylic acid is one or more selected from trimellitic acid and pyromellitic acid.
3. The plasticizer according to claim 1, wherein the aliphatic diol having 2 to 18 carbon atoms is one or more selected from 1,2-propanediol, 1,2-butanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, neopentyl glycol, and 3-methyl-1,5-pentanediol.
4. The plasticizer according to claim 1, wherein the aliphatic dicarboxylic acid having 4 to 14 carbon atoms is one or more selected from adipic acid and sebacic acid.
5. The plasticizer according to claim 1, wherein the monoalcohol having 4 to 18 carbon atoms is one or more selected from octanol, 2-ethylhexanol, and isononyl alcohol.
6. The plasticizer according to claim 1, wherein the monocarboxylic acid having 2 to 21 carbon atoms comprises two or more aliphatic monocarboxylic acids having 8 to 21 carbon atoms.
7. The plasticizer according to claim 1, wherein the monocarboxylic acid having 2 to 21 carbon atoms is a hydrogenated vegetable oil fatty acid.
8. The plasticizer according to claim 1, wherein the polyester is a polyester in which the reactants are an aliphatic diol having 2 to 18 carbon atoms, an aliphatic dicarboxylic acid having 2 to 12 carbon atoms, a polyol having 3 or more hydroxyl groups in one molecule, and a monocarboxylic acid having 2 to 21 carbon atoms.
9. The plasticizer according to claim 1, wherein the hydroxyl value of the polyester is 15 mg KOH / g or less.
10. The plasticizer according to claim 1, wherein the number-average molecular weight of the polyester is in the range of 1,500 to 4,000.
11. The plasticizer according to claim 1, which is a plasticizer for polyvinyl chloride resin.
12. A vinyl chloride resin composition comprising a plasticizer and a vinyl chloride resin according to any one of claims 1 to 11.
13. The vinyl chloride resin composition according to claim 12, wherein the content of the plasticizer is in the range of 10 to 150 parts by mass per 100 parts by mass of the vinyl chloride resin.
14. A molded article of the polyvinyl chloride resin composition according to claim 12.
15. A cable comprising a conductor and an insulating coating layer covering the conductor, wherein the insulating coating layer is a molded body of the polyvinyl chloride resin composition described in claim 12.