Adhesive sheet, double-sided adhesive sheet, fuel cell, and water electrolysis device

The adhesive resin composition with a specific formulation of acid-modified styrene block copolymer, crosslinking agent, and tackifier addresses the adhesion issues in fuel cells and water electrolysis devices, providing durable sealing in harsh conditions.

WO2026235006A1PCT designated stage Publication Date: 2026-11-12ARISAWA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016261
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-04-23
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing adhesive sheets used in fuel cells and water electrolysis devices exhibit weak adhesion to resin sub-gaskets and metal separators, particularly in high-temperature and acidic or alkaline environments, leading to poor long-term adhesion.

Method used

An adhesive resin composition comprising an acid-modified styrene block copolymer, a crosslinking agent with epoxy groups, and a hydrophobic tackifier with a melting point of 80°C or higher, with specific ratios and types of components to enhance adhesion and resistance to heat and chemicals.

Benefits of technology

The adhesive sheet maintains excellent adhesion to resin and metal materials even in high-temperature and acidic or alkaline environments for extended periods, ensuring effective sealing in fuel cells and water electrolysis devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026016261_12112026_PF_FP_ABST
    Figure JP2026016261_12112026_PF_FP_ABST
Patent Text Reader

Abstract

This adhesive sheet is composed of an adhesive resin composition that contains: an acid-modified styrene block copolymer having an acid-modified functional group; a crosslinking agent having an epoxy group that is reactive with the acid-modified functional group; and a tackifier having hydrophobicity and a melting point of 80°C or higher. The amount of the tackifier contained in the adhesive resin composition is 65 parts by mass to 180 parts by mass inclusive with respect to 100 parts by mass of the acid-modified styrene block copolymer. The equivalent of the epoxy group of the crosslinking agent contained in the adhesive resin composition is 0.7 equivalent to 2.3 equivalents inclusive with respect to 1 equivalent of the acid-modified functional group of the acid-modified styrene block copolymer.
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive sheets, double-sided adhesive sheets, fuel cells, and water electrolysis devices

[0001] The present invention relates to an adhesive sheet, a double-sided adhesive sheet, a fuel cell, and a water electrolysis device.

[0002] Fuel cells, such as polymer electrolyte fuel cells, have a configuration in which multiple power generation cells are stacked. Each power generation cell (hereinafter also simply referred to as "cell") has a stacked configuration in the following order: anode gas diffusion layer, anode catalyst layer, electrolyte membrane, cathode catalyst layer, and cathode gas diffusion layer. A pair of metal separators are provided to sandwich the cells for protection. In each cell, a gas containing hydrogen is supplied to the anode gas diffusion layer from outside the cell, and a gas containing oxygen is supplied to the cathode gas diffusion layer from outside the cell. The outer periphery of the cell is sealed with an adhesive sheet or the like to prevent gas leakage. One example of a configuration sealed with an adhesive sheet is one in which an adhesive sheet is used to seal the space between a metal separator and a sheet-like resin sub-gasket located on the outside of the periphery of the electrolyte membrane. Such an adhesive sheet is required to have excellent adhesion to the metal separator and the resin sub-gasket. More specifically, the adhesive sheet must maintain its adhesion to the resin sub-gasket and the metal separator even when exposed to high temperatures and acidic or alkaline environments for extended periods.

[0003] This is because the environment inside the power generation cell of a fuel cell tends to become acidic or alkaline, and depending on the usage conditions of the fuel cell, it can easily become a high-temperature environment.

[0004] As an example of the adhesive sheet described above, Patent Document 1 discloses an adhesive sheet comprising an adhesive composition containing an acid-modified hydrogenated styrene-based block copolymer, a crosslinking agent that can react with an acid, a polyphenylene ether-based resin, and a tackifying resin.

[0005] Japanese Patent Publication No. 2023-175201

[0006] Adhesive sheets made from such adhesive compositions exhibit weak adhesion to resin sub-gaskets and metal separators from the initial stages. Furthermore, these adhesive sheets have difficulty maintaining their adhesive strength over long periods at high temperatures and in acidic or alkaline environments.

[0007] The present invention has been made in view of the above circumstances, and aims to provide an adhesive sheet or double-sided adhesive sheet, a fuel cell and a water electrolysis device sealed with an adhesive sheet or double-sided adhesive sheet, which have excellent adhesion to resin materials and metal materials, and which maintain excellent adhesion even when left in a high-temperature environment and an acidic or alkaline environment for a long period of time.

[0008] The present invention is as follows:

[0009] [1] The adhesive sheet of the present invention is composed of an adhesive resin composition comprising an acid-modified styrene block copolymer having an acid-modified functional group, a crosslinking agent having an epoxy group that reacts with the acid-modified functional group, and a hydrophobic tackifier having a melting point of 80°C or higher, wherein the amount of the tackifier contained in the adhesive resin composition is 65 parts by mass or more and 180 parts by mass or less per 100 parts by mass of the acid-modified styrene block copolymer, and the equivalent amount of the epoxy group of the crosslinking agent contained in the adhesive resin composition is 0.7 equivalents or more and 2.3 equivalents or less per 1 equivalent of the acid-modified functional group of the acid-modified styrene block copolymer.

[0010] [2] The acid-modified styrene-based block copolymer contained in the adhesive resin composition constituting the adhesive sheet of the present invention may have at least one selected from the group consisting of maleic anhydride, acrylic acid, and glycidyl methacrylate as an acid-modified functional group.

[0011] [3] The tackifier contained in the adhesive resin composition constituting the adhesive sheet of the present invention may consist of at least one tackifier selected from the group consisting of a hydroxyl group-containing tackifier having a hydroxyl value of 5 mg KOH / g or more and 25 mg KOH / g or less, and an acidic functional group-containing tackifier having an acid value of 2 mg KOH / g or more and 20 mg KOH / g or less.

[0012] [4] The hydroxyl group-containing tackifier contained in the adhesive resin composition constituting the adhesive sheet of the present invention may be a hydrogenated terpene phenol resin.

[0013] [5] The acidic functional group-containing tackifier contained in the adhesive resin composition constituting the adhesive sheet of the present invention may be a hydrogenated rosin ester resin.

[0014] [6] The thickness of the adhesive sheet of the present invention may be 30 μm or more and 200 μm or less.

[0015] [7] The double-sided adhesive sheet of the present invention comprises a heat-resistant and acid- and / or alkali-resistant heat- and chemical-resistant film, and an adhesive layer formed on both sides of the heat-resistant and chemical-resistant film, wherein the adhesive layer is composed of an adhesive resin composition comprising an acid-modified styrene block copolymer having acid-modified functional groups, a crosslinking agent having epoxy groups that react with the acid-modified functional groups, and a hydrophobic tackifier having a melting point of 80°C or higher, wherein the amount of the tackifier contained in the adhesive resin composition is 65 parts by mass or more and 180 parts by mass or less per 100 parts by mass of the acid-modified styrene block copolymer, and the equivalent amount of the epoxy groups of the crosslinking agent contained in the adhesive resin composition is 0.7 equivalents or more and 2.3 equivalents or less per 1 equivalent of the acid-modified functional groups of the acid-modified styrene block copolymer.

[0016] [8] The acid-modified styrene-based block copolymer contained in the adhesive resin composition constituting the double-sided adhesive sheet of the present invention may have at least one selected from the group consisting of maleic anhydride, acrylic acid, and glycidyl methacrylate as an acid-modified functional group.

[0017] [9] The tackifier contained in the adhesive resin composition constituting the double-sided adhesive sheet of the present invention may consist of at least one tackifier selected from the group consisting of a hydroxyl group-containing tackifier having a hydroxyl value of 5 mg KOH / g or more and 25 mg KOH / g or less, and an acidic functional group-containing tackifier having an acid value of 2 mg KOH / g or more and 20 mg KOH / g or less.

[0018]

[10] The hydroxyl group-containing tackifier contained in the adhesive resin composition constituting the double-sided adhesive sheet of the present invention may be a hydrogenated terpene phenol resin.

[0019]

[11] The acidic functional group-containing tackifier contained in the adhesive resin composition constituting the double-sided adhesive sheet of the present invention may be a hydrogenated rosin ester resin.

[0020]

[12] The heat-resistant and chemical-resistant film constituting the double-sided adhesive sheet of the present invention may be one film selected from the group consisting of polyethylene naphthalate film, polyphenylene sulfide film, polyphenyl sulfone film, polyphenylene ether film, polyvinyl chloride film, polypropylene film, polystyrene film, polyether ether ketone film, and cyclic olefin copolymer film.

[0021]

[13] The fuel cell of the present invention comprises: an electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; a sheet-shaped sub-gasket arranged to surround the outside of the peripheral edge of the electrolyte membrane; an anode-side gas diffusion layer arranged on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator arranged on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer arranged on the side of the cathode catalyst layer opposite to the side in contact with the cathode catalyst layer; and a cathode-side separator arranged on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. The first surface of the subgasket, which is one surface of the subgasket, and the first inner edge surface of the anode-side separator, which is the peripheral edge of one surface of the anode-side separator, face each other, and the space between the first surface of the subgasket and the first inner edge surface of the anode-side separator is sealed with the adhesive sheet described in any one of [1] to [6] above or the double-sided adhesive sheet described in any one of [7] to

[12] above.

[0022]

[14] In the fuel cell of the present invention, the second surface of the subgasket, which is the other surface of the subgasket, and the first inner edge surface of the cathode-side separator, which is the peripheral edge of one surface of the cathode-side separator, face each other, and the space between the second surface of the subgasket and the first inner edge surface of the cathode-side separator may be sealed with the adhesive sheet described in any one of [1] to [6] above or the double-sided adhesive sheet described in any one of [7] to

[12] above.

[0023]

[15] The fuel cell of the present invention comprises: an electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; an anode-side gas diffusion layer disposed on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator disposed on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer disposed on the side of the cathode catalyst layer opposite to the side in contact with the cathode catalyst layer; and a cathode-side separator disposed on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. The first inner edge surface of the anode-side separator, which is the peripheral edge of one face of the anode-side separator, and the first inner edge surface of the cathode-side separator, which is the peripheral edge of one face of the cathode-side separator, face each other, and the space between the first inner edge surface of the anode-side separator and the first inner edge surface of the cathode-side separator is sealed with an adhesive sheet described in any one of [1] to [6] above or a double-sided adhesive sheet described in any one of [7] to

[12] above.

[0024]

[16] The water electrolysis apparatus of the present invention comprises: an electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; a sheet-shaped sub-gasket arranged to surround the outside of the peripheral edge of the electrolyte membrane; an anode-side gas diffusion layer arranged on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator arranged on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer arranged on the side of the cathode catalyst layer opposite to the side in contact with the cathode catalyst layer; and a cathode-side separator arranged on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. The first surface of the subgasket, which is one surface of the subgasket, and the first inner edge surface of the anode-side separator, which is the peripheral edge of one surface of the anode-side separator, face each other, and the space between the first surface of the subgasket and the first inner edge surface of the anode-side separator is sealed with the adhesive sheet described in any one of [1] to [6] above or the double-sided adhesive sheet described in any one of [7] to

[12] above.

[0025]

[17] In the water electrolysis apparatus of the present invention, the second surface of the subgasket, which is the other surface of the subgasket, and the first inner edge surface of the cathode-side separator, which is the peripheral edge of one surface of the cathode-side separator, face each other, and the space between the second surface of the subgasket and the first inner edge surface of the cathode-side separator may be sealed with the adhesive sheet described in any one of [1] to [6] above or the double-sided adhesive sheet described in any one of [7] to

[12] above.

[0026]

[18] The water electrolysis apparatus of the present invention comprises: an electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; an anode-side gas diffusion layer disposed on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator disposed on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer disposed on the side of the cathode catalyst layer opposite to the side in contact with the electrolyte membrane; and a cathode-side separator disposed on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. The first inner edge surface of the anode-side separator, which is the peripheral edge of one face of the anode-side separator, and the first inner edge surface of the cathode-side separator, which is the peripheral edge of one face of the cathode-side separator, face each other, and the space between the first inner edge surface of the anode-side separator and the first inner edge surface of the cathode-side separator is sealed with an adhesive sheet described in any one of [1] to [6] above or a double-sided adhesive sheet described in any one of [7] to

[12] above.

[0027]

[19] The water electrolysis apparatus of the present invention comprises: an electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; an anode-side gas diffusion layer disposed on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator disposed on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer disposed on the side of the cathode catalyst layer opposite to the side in contact with the electrolyte membrane; and a cathode-side separator disposed on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. The electrolyte membrane first peripheral surface, which is the peripheral edge of one surface of the electrolyte membrane, and the anode side separator first inner surface, which is the peripheral edge of one surface of the anode side separator, face each other, and the space between the electrolyte membrane first peripheral surface and the anode side separator first inner surface is sealed with the adhesive sheet described in any one of [1] to [6] above or the double-sided adhesive sheet described in any one of [7] to

[12] above.

[0028]

[20] In the water electrolysis apparatus of the present invention, the second peripheral surface of the electrolyte membrane, which is the peripheral edge of another surface of the electrolyte membrane, and the first inner surface of the cathode-side separator, which is the peripheral edge of one surface of the cathode-side separator, face each other, and the space between the second peripheral surface of the electrolyte membrane and the first inner surface of the cathode-side separator may be sealed with the adhesive sheet described in any one of [1] to [6] above or the double-sided adhesive sheet described in any one of [7] to

[12] above.

[0029] According to the present invention, it is possible to provide an adhesive sheet or double-sided adhesive sheet, a fuel cell, and a water electrolysis device sealed with an adhesive sheet or double-sided adhesive sheet, which have excellent adhesion to resin materials and metal materials, and which maintain excellent adhesion even when left in a high-temperature environment and in an acidic or alkaline environment for a long period of time.

[0030] This is a schematic cross-sectional view of the adhesive sheet of the embodiment. This is a schematic cross-sectional view of the double-sided adhesive sheet of the embodiment. This is a schematic cross-sectional view of a proton exchange type polymer electrolyte fuel cell, which is an example of a fuel cell of the embodiment. This is a schematic top view of the electrolyte membrane and sub-gasket constituting the fuel cell of the embodiment. This is a schematic cross-sectional view of a proton exchange type polymer electrolyte fuel cell, which is an example of a fuel cell of the embodiment. This is a schematic cross-sectional view of a polymer electrolyte water electrolysis device, which is an example of a water electrolysis device of the embodiment. This is a schematic top view of the electrolyte membrane and sub-gasket constituting the water electrolysis device of the embodiment. This is a schematic cross-sectional view of a polymer electrolyte water electrolysis device, which is an example of a single-sided adhesive sheet used in the water electrolysis device of the embodiment.

[0031] The following describes in detail embodiments of the present invention, including an adhesive sheet, a double-sided adhesive sheet, a fuel cell, and a water electrolysis device. The following embodiments are examples for illustrating the present invention and are not intended to limit the present invention to the following content. The present invention can be implemented by modifying it as appropriate within the scope of its gist. Parts by mass refer to, for example, parts by mass of resin only, excluding volatile components such as organic solvents contained in the resin, and parts by mass of non-volatile components.

[0032] [Adhesive Sheet] The adhesive sheet 10 of the embodiment is made of an adhesive resin composition and has a sheet shape. As shown in Figure 1, both sides of the adhesive sheet 10 are covered with separator films 12 and 14. The adhesive sheet 10 is used after peeling off the separator films 12 and 14. The thickness of the adhesive sheet 10 is 1 μm or more and 200 μm or less, preferably 3 μm or more and 200 μm or less, more preferably 3 μm or more and 150 μm or less, and even more preferably 3 μm or more and 100 μm or less. An adhesive sheet 10 having such a thickness will adhere closely to the uneven surface of a resin sub-gasket or metal separator, which have an uneven surface shape and constitute a fuel cell or water electrolysis device, for example. This will allow the resin sub-gasket and the metal separator to be sealed without any gaps.

[0033] (Adhesive Resin Composition) The adhesive resin composition constituting the adhesive sheet 10 includes an acid-modified styrene-based block copolymer having acid-modified functional groups, a crosslinking agent having epoxy groups that react with the acid-modified functional groups, and a hydrophobic tackifier having a melting point of 80°C or higher. The acid-modified styrene-based block copolymer, crosslinking agent, and tackifier contained in the adhesive resin composition will be described below.

[0034] (Acid-modified styrene block copolymer) The acid-modified styrene block copolymer contained in the adhesive resin composition is a copolymer obtained by acid-modifying hydrogenated styrene-butadiene copolymer (HSB), styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), styrene-ethylene / butylene-styrene block copolymer (SEBS), styrene-ethylene / propylene-styrene block copolymer (SEPS), etc. From the viewpoint of improving the water resistance and adhesiveness of the adhesive resin composition after curing, acid-modified styrene-ethylene / butylene-styrene block copolymer (SEBS) is preferred. The acid-modified functional group is at least one selected from the group consisting of maleic anhydride, acrylic acid, and glycidyl methacrylate, and maleic anhydride is preferred due to its ease of introduction into the copolymer. For example, by adding maleic anhydride to the monomer constituting the copolymer and polymerizing it, an acidic functional group derived from maleic anhydride can be introduced into the copolymer. Examples of acid-modified styrene block copolymers in which the acid-modifying functional group is maleic anhydride include maleic anhydride-modified styrene-ethylene / butylene-styrene block copolymer (SEBS) and hydrogenated maleic anhydride-modified styrene-ethylene / butylene-styrene block copolymer (hydrogenated SEBS). From the viewpoint of increasing the hydrophobicity of the adhesive resin composition, hydrogenated maleic anhydride-modified styrene-ethylene / butylene-styrene block copolymer (hydrogenated SEBS) is preferred as the acid-modified styrene block copolymer.

[0035] From the viewpoint of enhancing reactivity with crosslinking agents and maintaining the toughness of the block copolymer, the amount of acid-modified functional groups (graft rate) introduced into the block copolymer has a lower limit of 0.1 wt%, preferably 0.5 wt%, and an upper limit of 5 wt%, preferably 3 wt%, and more preferably 2 wt%. The acid value of the acid-modified styrene-based block copolymer having acid-modified functional groups has a lower limit of 5 mg KOH / g, preferably 7 mg KOH / g, more preferably 9 mg KOH / g, even more preferably 10 mg KOH / g, and an upper limit of 30 mg KOH / g, preferably 20 mg KOH / g. Block copolymers having such an acid value can enhance reactivity with crosslinking agents and tackifiers.

[0036] (Crosslinking agent) The crosslinking agent contained in the adhesive resin composition reacts with the acid-modified functional groups of the acid-modified styrene block copolymer. This reaction forms a three-dimensional network structure composed of the acid-modified styrene block copolymer and the crosslinking agent. The formation of this three-dimensional network structure improves the heat resistance, alkali resistance, and acid resistance of the adhesive resin composition after curing. Furthermore, if the adhesive resin composition contains a tackifier having acidic functional groups, the crosslinking agent, tackifier, and acid-modified styrene block copolymer react in a complex manner to form a three-dimensional network structure composed of the crosslinking agent, tackifier, and acid-modified styrene block copolymer. An adhesive resin composition with such a three-dimensional network structure after curing has excellent heat resistance, alkali resistance, and acid resistance.

[0037] The crosslinking agent is preferably an epoxy resin having epoxy groups, from the viewpoint of improving the heat resistance, alkali resistance, and acid resistance of the cured adhesive resin composition. The epoxy resin used as the crosslinking agent preferably has two or more epoxy groups in one molecule, and more preferably is a polyfunctional epoxy resin having three or more epoxy groups, from the viewpoint of improving heat resistance, alkali resistance, and acid resistance. The epoxy equivalent of the epoxy resin is 90 g / eq or more and 1000 g / eq or less, preferably 150 g / eq or more and 400 g / eq or less. By including such a crosslinking agent in the adhesive resin composition, the reactivity with the acid-modified functional groups of the acid-modified styrene-based block copolymer can be increased, and the heat resistance, alkali resistance, and acid resistance of the cured adhesive resin composition can be improved.

[0038] Epoxy resins that can be used as crosslinking agents include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, novolac type epoxy resin, biphenyl type epoxy resin, cyclopentadiene type epoxy resin, glycidylamine type epoxy resin, condensation-type epoxy resin, and alicyclic epoxy resin. From the viewpoint of improving the heat resistance, alkali resistance, and acid resistance of the cured adhesive resin composition, alicyclic epoxy resins are preferred, and alicyclic epoxy resins having a cyclohexane skeleton are more preferred.

[0039] The equivalent of the crosslinking agent contained in the adhesive resin composition is such that, relative to 1 equivalent of the acid-modified functional group of the acid-modified styrenic block copolymer, the lower limit of the epoxy group is 0.7 equivalents or more, preferably 0.9 equivalents or more, more preferably 1.0 equivalent or more, and the upper limit is 2.3 equivalents or less, preferably 2.1 equivalents or less, more preferably 2.0 equivalents or less, still more preferably 1.7 equivalents or less, and particularly preferably 1.6 equivalents or less. Thereby, the reactivity with the acid-modified functional group of the acid-modified styrenic block copolymer can be enhanced, and the heat resistance, alkali resistance, and acid resistance of the adhesive resin composition after curing can be improved. In addition, by setting the equivalent of the crosslinking agent contained in the adhesive resin composition to 0.7 equivalents or more, even in an adhesive resin composition containing a tackifier having an acidic functional group, the reaction between the crosslinking agent and the acid-modified styrenic block copolymer, and the combined reaction among the crosslinking agent, the tackifier and the acid-modified styrenic block copolymer can proceed synergistically.

[0040] (Tackifier) The tackifier contained in the adhesive resin composition imparts adhesiveness to the resin composition. The tackifier contained in the adhesive resin composition has hydrophobicity and a melting point of 80°C or higher. From the viewpoint of improving the heat resistance of the adhesive resin composition, the melting point of the tackifier is 80°C or higher, preferably 100°C or higher, and more preferably 110°C or higher. An adhesive sheet composed of an adhesive resin composition containing such a tackifier hardly causes the tackifier to elute even when the temperature environment in use exceeds 70°C, and has tack properties under normal temperature environments. In addition, since the tackifier has hydrophobicity, the water resistance of the adhesive resin composition is improved.

[0041] The tackifier contained in the adhesive resin composition is preferably composed of at least one tackifier selected from the group consisting of a hydroxyl group-containing tackifier having a hydroxyl value of 5 mgKOH / g or more and 25 mgKOH / g or less, and an acidic functional group-containing tackifier having an acid value of 2 mgKOH / g or more and 20 mgKOH / g or less.

[0042] The hydroxyl group-containing tackifier has hydrophobicity and a melting point of 100°C or higher. The cured adhesive resin composition containing the hydroxyl group-containing tackifier with a melting point of 100°C or higher has excellent heat resistance, alkali resistance, and acid resistance. The hydroxyl group-containing tackifier is, for example, a hydrogenated terpene phenol resin.

[0043] The acidic functional group-containing tackifier has hydrophobicity and a melting point of 80°C or higher. The cured adhesive resin composition containing this acidic functional group-containing tackifier has excellent heat resistance, alkali resistance, and acid resistance. Furthermore, since the acidic functional group-containing tackifier also reacts with the crosslinking agent, it exhibits more excellent heat resistance, alkali resistance, and acid resistance. The acidic functional group-containing tackifier is, for example, a hydrogenated rosin ester resin.

[0044] The amount of the tackifier contained in the adhesive resin composition is, for example, relative to 100 parts by mass of the acid-modified styrenic block copolymer, a lower limit of 65 parts by mass or more, preferably 70 parts by mass or more, more preferably 75 parts by mass or more, further preferably 95 parts by mass or more, particularly preferably 100 parts by mass or more, and an upper limit of 180 parts by mass or less, preferably 170 parts by mass or less, more preferably 165 parts by mass or less, further preferably 160 parts by mass or less. Thereby, adhesiveness can be imparted to the cured adhesive resin composition.

[0045] The adhesive resin composition constituting the adhesive sheet of the embodiment can be obtained by placing a predetermined amount of the above-mentioned materials in a container and mixing them. From the viewpoint of uniformly mixing the adhesive resin composition, for example, an organic solvent such as methyl ethyl ketone or toluene may be added to the resin composition. In addition, additives may be added to the resin composition within a range that does not impair the properties of the above-mentioned adhesive resin composition. Examples of the additives include dispersants, thermal aging inhibitors, silane coupling agents, and the like.

[0046] The adhesive sheet of this embodiment, composed of an adhesive resin composition containing the aforementioned acid-modified styrene block copolymer, a crosslinking agent, and a tackifier, exhibits excellent adhesion to metallic materials such as titanium, stainless steel, and copper, and to resin materials such as polyethylene naphthalate, polyphenylene sulfide, polyphenyl sulfone, polyphenylene ether, polyvinyl chloride, polypropylene, polystyrene, and polyether ether ketone. Furthermore, the adhesive sheet of this embodiment maintains excellent adhesion even when exposed to high-temperature environments and acidic or alkaline environments for extended periods.

[0047] (Method for manufacturing adhesive sheet 10) The adhesive sheet 10 of the embodiment can be obtained, for example, by the following procedure. The above-mentioned adhesive resin composition is applied to the separator film 12 using, for example, a coating device to form an adhesive layer made of the adhesive resin composition. Next, the formed adhesive layer is heated, for example, at 120°C to 180°C for 2 minutes to 10 minutes. After cooling, the adhesive layer is heated again for a certain period of time. The separator film 12 is peeled off the adhesive layer obtained in this way to obtain the adhesive sheet 10. Examples of heating conditions for the adhesive layer for a certain period of time include heating at 80°C for 4 days or at 120°C for 1 day.

[0048] Alternatively, after forming an adhesive layer on the separator film 12, the separator film 14 may be attached to the surface of the adhesive layer on the side opposite to the surface where the separator film 12 is attached, while heating it. This protects both sides of the adhesive layer and makes the surface of the adhesive layer smooth.

[0049] The coating equipment used to form the adhesive layer is, for example, a die coater or a comma coater. The material of the separator films 12 and 14 is, for example, polyethylene, polypropylene, polyimide, polyamide-imide, polyethylene naphthalate, polyethylene terephthalate, etc. The thickness of the separator films 12 and 14 is preferably, for example, 12 μm to 100 μm, more preferably 25 μm to 100 μm, and even more preferably 50 μm to 100 μm, from the viewpoint of making it easy to peel the separator films off. Furthermore, from the viewpoint of making it easy to peel the separator films 12 and 14 off from the adhesive layer, the surface of the separator films 12 and 14 may be treated with a release agent. The release agent is, for example, a silicone-based agent or a fluorine-based agent.

[0050] [Double-Sided Adhesive Sheet 11] As shown in Figure 2, the double-sided adhesive sheet 11 of this embodiment is composed of a heat-resistant and chemical-resistant film 11c which is a core material, and an adhesive layer 11a formed on both sides of the heat-resistant and chemical-resistant film 11c. Both sides of the double-sided adhesive sheet 11 are covered with separator films 12 and 14. The thickness of the adhesive layer 11a is preferably 1 μm or more and 200 μm or less, more preferably 3 μm or more and 200 μm or less, even more preferably 3 μm or more and 150 μm or less, and even more preferably 3 μm or more and 100 μm or less. The thickness of the heat-resistant and chemical-resistant film 11c is preferably 10 μm or more and 200 μm or less, and more preferably 25 μm or more and 150 μm or less. The thickness of the double-sided adhesive sheet 11 of this embodiment is preferably 12 μm or more and 600 μm or less. The double-sided adhesive sheet 11 is used after peeling off the separator films 12 and 14. A double-sided adhesive sheet 11 having an adhesive layer 11a with a thickness of 1 μm or more can adhere tightly to, for example, the uneven surface of a resin sub-gasket or a metal separator. This allows for a gap-free seal between the resin sub-gasket and the metal separator.

[0051] (Heat-resistant and chemical-resistant film 11c) The heat-resistant and chemical-resistant film 11c of the double-sided adhesive sheet 11 has heat resistance and acid and / or alkali resistance. The heat-resistant and chemical-resistant film 11c is one type of film selected from the group consisting of polyethylene naphthalate film, polyphenylene sulfide film, polyphenyl sulfone film, polyphenylene ether film, polyvinyl chloride film, polypropylene film, polystyrene film, polyether ether ketone film, and cyclic olefin copolymer film. For example, for the heat-resistant and chemical-resistant film 11c of the double-sided adhesive sheet 11 used in an acidic fuel cell where the environment inside the power cell is acidic, a film having heat resistance and acid resistance is preferred, such as polyethylene naphthalate film and polyphenylene sulfide film. For the heat-resistant and chemical-resistant film 11c of the double-sided adhesive sheet 11 used in an alkaline fuel cell where the environment inside the power cell is alkaline, a film having heat resistance and alkali resistance is preferred, such as polyphenylene sulfide film. The surface of the heat-resistant and chemical-resistant film 11c is preferably surface-treated by corona treatment or plasma treatment in order to improve adhesion with the adhesive layer 11a.

[0052] (Adhesive layer 11a) The adhesive resin composition constituting the adhesive layer 11a can be the same resin composition as the adhesive resin composition constituting the adhesive sheet 10 of the embodiment.

[0053] (Method for manufacturing double-sided adhesive sheet 11) The double-sided adhesive sheet 11 of the embodiment can be obtained, for example, by the following procedure. The above-mentioned adhesive resin composition is applied to one side of a heat-resistant and chemical-resistant film 11c using, for example, a coating device to form an adhesive layer 11a made of the adhesive resin composition. Next, the formed adhesive layer 11a is heated, for example, at 120°C to 180°C for 2 to 10 minutes. After cooling, a separator film 12 is attached to the surface of the formed adhesive layer 11a. Next, the adhesive resin composition is applied to the other side of the heat-resistant and chemical-resistant film 11c, which does not have an adhesive layer 11a formed on it, using a coating device to form an adhesive layer 11a. After that, it is heated, for example, at 120°C to 180°C for 2 to 10 minutes. After cooling, a separator film 14 is attached to the surface of the adhesive layer 11a. Furthermore, the adhesive layer is heated for a certain period of time. The separator films 12 and 14 are peeled off from the resulting laminate to obtain a double-sided adhesive sheet 11. The conditions for heating the adhesive layer for a certain period of time are, for example, 80°C for 4 days or 120°C for 1 day.

[0054] The double-sided adhesive sheet 11 of the embodiment may be obtained by a method other than the one described above. Specifically, an adhesive resin composition is applied to a separator film 12 using, for example, a coating device to form an adhesive layer 11a made of the adhesive resin composition. Next, the formed adhesive layer 11a is heated, for example, at 120°C to 180°C for 2 to 10 minutes. After cooling, an adhesive layer 11a formed on one side of the separator film 12 is obtained. Another adhesive layer 11a formed on one side of the separator film 14 is obtained by the same method. Next, the adhesive layer 11a formed on one side of the separator film 12, the heat-resistant and chemical-resistant film 11c, and the adhesive layer 11a formed on one side of the separator film 14 are laminated in that order, so that the side of the adhesive layer 11a with exposed resin is in contact with the heat-resistant and chemical-resistant film 11c. The resulting laminate is heated in a press molding machine, for example, at a temperature of 50°C to 160°C, while being pressurized with a pressure of 0.5 MPa to 3.0 MPa from a direction perpendicular to the main plane of the laminate. The heating and pressurizing time is 0.1 seconds to 10 seconds. After cooling, the adhesive layer 11a is further heated for a certain period of time. The separator films 12 and 14 are then peeled off from the resulting laminate to obtain a double-sided adhesive sheet 11. The conditions for heating the adhesive layer 11a for a certain period of time are, for example, 80°C for 4 days or 120°C for 1 day.

[0055] The coating apparatus and separator film used in the double-sided adhesive sheet 11 of the embodiment can be the same as the coating apparatus and separator film used in the manufacturing method of the adhesive sheet 10 of the embodiment.

[0056] The adhesive sheet 10 and double-sided adhesive sheet 11 of the above-described embodiment can be used, for example, as an adhesive sheet to seal the space between a separator protecting the power generation cell of a fuel cell and a sheet-like sub-gasket located on the outside of the peripheral edge of the electrolyte membrane, or as an adhesive sheet to seal the space between separators protecting the power generation cell. The thickness of the adhesive sheet 10 used in a fuel cell or water electrolysis device, and the thickness of the adhesive layer 11a and the heat-resistant and chemical-resistant film 11c constituting the double-sided adhesive sheet 11 can be appropriately selected according to the configuration of the fuel cell or water electrolysis device.

[0057] [Fuel Cell] As an example of a fuel cell using the double-sided adhesive sheet 11 of the embodiment, a proton exchange type polymer electrolyte fuel cell 100 will be described.

[0058] (Proton Exchange Type Polymer Electrolyte Fuel Cell 100) As shown in Figure 3, the proton exchange type polymer electrolyte fuel cell 100 comprises an electrolyte membrane 50, an anode catalyst layer 51, a cathode catalyst layer 53, a sub-gasket 52, an anode-side gas diffusion layer 61, an anode-side separator 71, a cathode-side gas diffusion layer 63, and a cathode-side separator 73. The sub-gasket 52 is arranged on the outer circumference of the electrolyte membrane 50 as shown in Figure 4. The anode catalyst layer 51 is arranged on one side of the electrolyte membrane 50. The anode-side gas diffusion layer 61 is arranged on the side of the anode catalyst layer 51 opposite to the side in contact with the electrolyte membrane 50. The anode-side separator 71 is arranged on the side of the anode-side gas diffusion layer 61 opposite to the side in contact with the anode catalyst layer 51. The cathode catalyst layer 53 is arranged on the other side of the electrolyte membrane 50. The cathode-side gas diffusion layer 63 is located on the side of the cathode catalyst layer 53 opposite to the side in contact with the electrolyte membrane 50. The cathode-side separator 73 is located on the side of the cathode-side gas diffusion layer 63 opposite to the side in contact with the cathode catalyst layer 53. Figure 3 is a cross-sectional view of the proton exchange type polymer electrolyte fuel cell 100 in the YZ plane. Figure 4 is a plan view of the sub-gasket 52 and electrolyte membrane 50 of the proton exchange type polymer electrolyte fuel cell 100 in Figure 3 in the XY plane.

[0059] In the XY plane of the proton-exchange type polymer electrolyte fuel cell 100 shown in Figure 3, the size of the anode catalyst layer 51, the anode-side gas diffusion layer 61, the cathode catalyst layer 53, and the cathode-side gas diffusion layer 63 is approximately the same as the size of the electrolyte membrane 50, and smaller than the size of the anode-side separator 71 and the cathode-side separator 73. In the YZ plane of the proton-exchange type polymer electrolyte fuel cell 100 shown in Figure 3, the thickness of the sub-gasket 52 is the same as the thickness of the electrolyte membrane 50. The thickness of the sub-gasket 52 may be thicker or thinner than the thickness of the electrolyte membrane 50.

[0060] One surface of the subgasket 52, the first subgasket surface 52a, faces the anode-side separator first inner edge surface 71a, which is the peripheral edge of one surface of the anode-side separator 71. The space between the first subgasket surface 52a and the anode-side separator first inner edge surface 71a is sealed with a double-sided adhesive sheet 11. The other surface of the subgasket 52, the second subgasket surface 52b, faces the cathode-side separator first inner edge surface 73b, which is the peripheral edge of one surface of the cathode-side separator 73. The space between the second subgasket surface 52b and the cathode-side separator first inner edge surface 73b is sealed with a double-sided adhesive sheet 11. Instead of the double-sided adhesive sheet 11 of this embodiment, the seal may be made with the adhesive sheet 10 of this embodiment. Alternatively, the seal may be made with multiple adhesive sheets 10 of different embodiments.

[0061] In the proton exchange type polymer electrolyte fuel cell 100 shown in Figure 3, the space between the first surface 52a of the subgasket and the first inner edge surface 71a of the anode-side separator, and the space between the second surface 52b of the subgasket and the first inner edge surface 73b of the cathode-side separator are sealed with a double-sided adhesive sheet 11. Depending on the operating conditions, the space between the first surface 52a of the subgasket and the first inner edge surface 71a of the anode-side separator may be sealed with a double-sided adhesive sheet 11 or adhesive sheet 10, and the space between the second surface 52b of the subgasket and the first inner edge surface 73b of the cathode-side separator may be sealed with a known adhesive sheet. Alternatively, the space between the second surface 52b of the subgasket and the first inner edge surface 73b of the cathode-side separator may be sealed with a double-sided adhesive sheet 11 or adhesive sheet 10, and the space between the first surface 52a of the subgasket and the first inner edge surface 71a of the anode-side separator may be sealed with a known adhesive sheet.

[0062] The electrolyte membrane 50 is, for example, made of protons (H +) is a polymer electrolyte membrane that can pass through. The sub-gasket 52 is preferably made of a material that has heat resistance and acid resistance. The material of the sub-gasket 52 is, for example, polyethylene naphthalate or polyphenylene sulfide. The anode catalyst layer 51 may be made of a material that has a catalytic function to promote the oxidation reaction of hydrogen. The material of the anode catalyst layer 51 is, for example, a carbon support with a platinum load of 50 wt%. The cathode catalyst layer 53 may be made of a material that has a catalytic function to promote the reduction reaction of oxygen. The material of the cathode catalyst layer 53 is, for example, a carbon support with a platinum load of 50 wt%. The anode-side gas diffusion layer 61 has the function of diffusing hydrogen supplied from the outside throughout the anode catalyst layer 51. The cathode-side gas diffusion layer 63 has the function of diffusing oxygen supplied from the outside throughout the cathode catalyst layer 53. The anode-side gas diffusion layer 61 and the cathode-side gas diffusion layer 63 are made of carbon paper with a water-repellent treatment applied to its surface.

[0063] The materials constituting the anode separator 71 and the cathode separator 73 can be any material that is resistant to corrosion by acid. Examples of materials constituting the anode separator 71 and the cathode separator 73 are titanium and stainless steel. The anode separator 71 and the cathode separator 73 each have a plurality of grooves 71gi and 73gi on one surface. The grooves 71gi and 73gi are formed on one surface, aligned in a direction perpendicular to the longitudinal direction of the grooves 71gi and 73gi. Hydrogen supplied from the outside is supplied to the anode catalyst layer 51 via the grooves 71gi and the anode gas diffusion layer 61. Oxygen supplied from the outside is supplied to the cathode catalyst layer 53 via the grooves 73gi and the cathode gas diffusion layer 63. In the anode catalyst layer 51, an oxidation reaction of hydrogen occurs, producing protons (H + ) is generated. Hydrogen that did not react in the anode catalyst layer 51 is discharged through the groove 71gi. Also, protons (H) that have passed through the electrolyte membrane 50 in the cathode catalyst layer 53 are generated. +The oxygen reacts with the carbon dioxide to produce water. The produced water and unreacted oxygen are discharged through groove 73gi. As shown in Figure 3, grooves 71go and 73go, the same as grooves 71gi and 73gi, may also be formed on the other surface of the anode-side separator 71 and the other surface of the cathode-side separator 73. The power generation cell can be cooled by flowing cooling water (coolant liquid), not shown, through these grooves.

[0064] The region 80 shown in Figure 3 is in an acidic environment due to protons generated by the oxidation reaction of hydrogen. Therefore, the acid-resistant double-sided adhesive sheet 11 can be suitably used as an adhesive sheet to seal the space between the separators 71 and 73 that protect the power generation cells of the fuel cell and the sheet-like sub-gasket 52 located on the outside of the periphery of the electrolyte membrane 50. Furthermore, the double-sided adhesive sheet 11 has excellent adhesion to resin and metal materials and excellent heat resistance. Such a double-sided adhesive sheet 11 can seal the space between the metal separators 71 and 73 and the resin sub-gasket 52. Moreover, even when the proton exchange type polymer electrolyte fuel cell 100 is placed in a high-temperature environment, the space between the metal separators 71 and 73 and the resin sub-gasket 52 can be sealed.

[0065] Furthermore, the double-sided adhesive sheet 11 of the proton exchange type polymer electrolyte fuel cell 100 may be used as a sub-gasket. Specifically, Figure 5 shows a proton exchange type polymer electrolyte fuel cell 110 in which the sub-gasket 52 of the proton exchange type polymer electrolyte fuel cell 100 is replaced with the double-sided adhesive sheet 11. The power generation cell of the proton exchange type polymer electrolyte fuel cell 110 has a structure in which an anode gas diffusion layer 61, an anode catalyst layer 51, an electrolyte membrane 50, a cathode catalyst layer 53, and a cathode gas diffusion layer 63 are stacked in that order. This power generation cell is sandwiched between a pair of metal separators 71 and 73. The space between the anode side separator first inner edge surface 71a of separator 71 and the cathode side separator first inner edge surface 73b of separator 73 is sealed with the double-sided adhesive sheet 11. If a gap occurs between the double-sided adhesive sheet 11 and the metal separators 71 and 73, the gap may be sealed with another adhesive sheet 10 or the double-sided adhesive sheet 11. Alternatively, the gap between separator 71 and separator 73 may be sealed with one or more adhesive sheets 10. In the proton exchange type polymer electrolyte fuel cell 110 shown in Figure 5, the same components used in the proton exchange type polymer electrolyte fuel cell 100 are given the same numbers and their descriptions are omitted.

[0066] Furthermore, the adhesive sheet 10 and the double-sided adhesive sheet 11 also have alkali resistance. Therefore, hydroxide ions (OH - It can also be suitably used in alkaline polymer electrolyte fuel cells equipped with a polymer electrolyte membrane that allows ) to pass through. Specifically, it can be suitably used as an adhesive sheet for sealing between the separator protecting the power generation cell of an alkaline polymer electrolyte fuel cell and a sheet-like sub-gasket located outside the periphery of the electrolyte membrane.

[0067] [Water Electrolysis Apparatus] The adhesive sheet 10 and the double-sided adhesive sheet 11 of the embodiment can be used as adhesive sheets to seal the space between the separator and the sub-gasket of a water electrolysis apparatus that can obtain hydrogen and oxygen by electrolyzing water, or as adhesive sheets to seal the space between separators. The following description will use a solid polymer water electrolysis apparatus 200 using the double-sided adhesive sheet 11 of the embodiment as an example.

[0068] (Solid Polymer Water Electrolyzer 200) As shown in Figure 6, the solid polymer water electrolyzer 200 comprises an electrolyte membrane 250, an anode catalyst layer 251, a cathode catalyst layer 253, a sub-gasket 252, an anode-side gas diffusion layer 261, an anode-side separator 271, a cathode-side gas diffusion layer 263, and a cathode-side separator 273. The sub-gasket 252 is arranged on the outer circumference of the electrolyte membrane 250 as shown in Figure 7. The anode catalyst layer 251 is arranged on one side of the electrolyte membrane 250. The anode-side gas diffusion layer 261 is arranged on the side of the anode catalyst layer 251 opposite to the side in contact with the electrolyte membrane 250. The anode-side separator 271 is arranged on the side of the anode-side gas diffusion layer 261 opposite to the side in contact with the anode catalyst layer 251. The cathode catalyst layer 253 is arranged on the other side of the electrolyte membrane 250. The cathode-side gas diffusion layer 263 is located on the side of the cathode catalyst layer 253 opposite to the side in contact with the electrolyte membrane 250. The cathode-side separator 273 is located on the side of the cathode-side gas diffusion layer 263 opposite to the side in contact with the cathode catalyst layer 253. Figure 6 is a cross-sectional view of the polymer electrolyte water electrolyzer 200 in the YZ plane. Figure 7 is a plan view of the sub-gasket 252 and electrolyte membrane 250 of the polymer electrolyte water electrolyzer 200 in Figure 6 in the XY plane.

[0069] In the XY plane of the polymer electrolyte water electrolyzer 200 in Figure 6, the size of the anode catalyst layer 251, the anode-side gas diffusion layer 261, the cathode catalyst layer 253, and the cathode-side gas diffusion layer 263 is approximately the same as the size of the electrolyte membrane 250, and smaller than the size of the anode-side separator 271 and the cathode-side separator 273. In the YZ plane of the polymer electrolyte water electrolyzer 200 in Figure 6, the thickness of the sub-gasket 252 is the same as the thickness of the electrolyte membrane 250. The thickness of the sub-gasket 252 may be thicker or thinner than the thickness of the electrolyte membrane 250.

[0070] One surface of the subgasket 252, the first subgasket surface 252a, faces the anode-side separator first inner edge surface 271a, which is the peripheral edge of one surface of the anode-side separator 271. The space between the first subgasket surface 252a and the anode-side separator first inner edge surface 271a is sealed with a double-sided adhesive sheet 11. The other surface of the subgasket 252, the second subgasket surface 252b, faces the cathode-side separator first inner edge surface 273b, which is the peripheral edge of one surface of the cathode-side separator 273. The space between the second subgasket surface 252b and the cathode-side separator first inner edge surface 273b is sealed with a double-sided adhesive sheet 11. The adhesive sheet 10 of the embodiment may be used instead of the double-sided adhesive sheet 11 of the embodiment. Alternatively, multiple adhesive sheets 10 of the embodiments may be used for sealing.

[0071] The electrolyte membrane 250 is, for example, made of protons (H + It is a polymer electrolyte membrane that can allow ) to pass through. The sub-gasket 252 is preferably made of a material that has heat resistance and acid resistance. The material of the sub-gasket 252 is, for example, polyethylene naphthalate or polyphenylene sulfide. The anode catalyst layer 251 may be made of a material that has a catalytic function to promote the water decomposition reaction. The material of the anode catalyst layer 251 is, for example, a carbon support containing iridium oxide. The cathode catalyst layer 253 may be made of a material that has a catalytic function to promote the hydrogen reduction reaction. The material of the cathode catalyst layer 253 is, for example, a carbon support with a platinum load of 50 wt%. The anode-side gas diffusion layer 261 and the cathode-side gas diffusion layer 263 have the function of efficiently guiding the water necessary for electrolysis to the anode catalyst layer 251 by passing electricity (electrons) supplied from the outside, and efficiently discharging hydrogen and oxygen generated in the electrolysis process. The anode-side gas diffusion layer 261 and the cathode-side gas diffusion layer 263 are, for example, a titanium porous material or a carbon nonwoven fabric that has excellent corrosion resistance and high strength.

[0072] The materials constituting the anode-side separator 271 and the cathode-side separator 273 may be any materials that are resistant to corrosion by acids. The materials constituting the anode-side separator 271 and the cathode-side separator 273 are, for example, titanium and stainless steel. The anode-side separator 271 and the cathode-side separator 273 each have a plurality of grooves 271gi, 273gi on one surface. The grooves 271gi and 273gi are formed on the one surface side by side in a direction orthogonal to the longitudinal direction of the grooves 271gi and 273gi. Water required for electrolysis is supplied to the anode catalyst layer 251 through the grooves 271gi and the anode-side gas diffusion layer 261. In the anode catalyst layer 251, water is supplied with electricity (electrons (e - )) from the outside to undergo electrolysis. Oxygen generated by water electrolysis is discharged from the anode-side gas diffusion layer 261 through the grooves 271gi and stored in an external container. In addition, protons (H generated by water electrolysis + ) pass through the electrolyte membrane 250 and reach the cathode catalyst layer 253. Protons (H + ) react with electricity (electrons (e supplied from the outside in the cathode catalyst layer 253 - )) to generate hydrogen (H 2 ). Hydrogen (H 2 ) is discharged through the cathode-side gas diffusion layer 263 and the grooves 273gi, and stored in an external container. As shown in FIG. 6, grooves 271go and 273go similar to the grooves 271gi and 273gi may also be formed on the other surface of the anode-side separator 271 and the other surface of the cathode-side separator 273. The water electrolysis device can be cooled by flowing unillustrated cooling water (coolant liquid) through these grooves.

[0073] As described above, the polymer electrolyte water electrolysis device 200 is a device that obtains hydrogen and oxygen by electrolyzing water. In the electrolysis process, the region 280 shown in FIG. 6 is in an acidic environment due to protons generated by water electrolysis.

[0074] Since region 280 of the polymer electrolyte water electrolysis apparatus 200 is in an acidic environment, the acid-resistant double-sided adhesive sheet 11 can be suitably used as an adhesive sheet to seal the space between the separators 271 and 273 of the polymer electrolyte water electrolysis apparatus 200 and the sheet-like sub-gasket 252 located on the outside of the peripheral edge of the electrolyte membrane 250. Furthermore, the double-sided adhesive sheet 11 has excellent adhesion to resin and metal materials and excellent heat resistance. Such a double-sided adhesive sheet 11 can seal the space between the metal separators 271 and 273 and the resin sub-gasket 252. Moreover, even if the polymer electrolyte water electrolysis apparatus 200 is placed in a high-temperature environment, the space between the metal separators 271 and 273 and the resin sub-gasket 252 can still be sealed.

[0075] In the solid polymer water electrolysis apparatus 200 shown in Figure 6, the space between separator 271 and sub-gasket 252, and the space between separator 273 and sub-gasket 252 are sealed with double-sided adhesive sheets 11. Depending on the operating conditions, the space between separator 271 and sub-gasket 252 may be sealed with double-sided adhesive sheets 11 or adhesive sheets 10, and the space between separator 273 and sub-gasket 252 may be sealed with a known adhesive sheet. Alternatively, the space between separator 273 and sub-gasket 252 may be sealed with double-sided adhesive sheets 11 or adhesive sheets 10, and the space between separator 271 and sub-gasket 252 may be sealed with a known adhesive sheet.

[0076] (Modified Example 1 of a Polymer Electrolyte Water Electrolyte) As a modified example of the Polymer Electrolyte Water Electrolyte 200, Figure 8 shows a Polymer Electrolyte Water Electrolyte 220 in which the sub-gasket 252 of the Polymer Electrolyte Water Electrolyte 200 is replaced with a double-sided adhesive sheet 11. The Polymer Electrolyte Water Electrolyte 220 has a structure in which an anode-side gas diffusion layer 261, an anode catalyst layer 251, an electrolyte membrane 250, a cathode catalyst layer 253, and a cathode-side gas diffusion layer 263 are stacked in that order between a metal separator 271 and a metal separator 273. The space between the first inner edge surface 271a of the anode-side separator 271 and the first inner edge surface 273b of the cathode-side separator 273 is sealed with a double-sided adhesive sheet 11. Alternatively, the seal may be made with the adhesive sheet 10 of the embodiment instead of the double-sided adhesive sheet 11. Alternatively, the seal may be made with multiple adhesive sheets 10. If a gap occurs between the double-sided adhesive sheet 11 and the separator 271, or between the double-sided adhesive sheet 11 and the separator 273, that gap may be sealed with another adhesive sheet 10 or the double-sided adhesive sheet 11. Alternatively, the space between the separator 271 and the separator 273 may be sealed with multiple adhesive sheets 10. In the polymer electrolyte water electrolysis apparatus 220 of Figure 8, the same components used in the polymer electrolyte water electrolysis apparatus 200 are given the same numbers and their descriptions are omitted.

[0077] (Modified Example 2 of a Polymer Electrolyte Water Electrolyzer) Figure 9 shows a modified example of a polymer electrolyzer water electrolyzer 200, namely a polymer electrolyzer water electrolyzer 210. The polymer electrolyzer water electrolyzer 210 comprises an electrolyte membrane 250, an anode catalyst layer 251, a cathode catalyst layer 253, an anode-side gas diffusion layer 261, an anode-side separator 271, a cathode-side gas diffusion layer 263, and a cathode-side separator 273. The polymer electrolyzer water electrolyzer 210 differs from the polymer electrolyzer water electrolyzer 200 in that it does not have a sub-gasket 252 located outside the peripheral edge of the electrolyte membrane 250. Here, in the polymer electrolyzer water electrolyzer 210, the same components used in the polymer electrolyzer water electrolyzer 200 are given the same numbers and their descriptions are omitted.

[0078] The anode catalyst layer 251 is located on one side of the electrolyte membrane 250. The anode-side gas diffusion layer 261 is located on the side of the anode catalyst layer 251 opposite to the side in contact with the electrolyte membrane 250. The anode-side separator 271 is located on the side of the anode-side gas diffusion layer 261 opposite to the side in contact with the anode catalyst layer 251. The cathode catalyst layer 253 is located on the other side of the electrolyte membrane 250. The cathode-side gas diffusion layer 263 is located on the side of the cathode catalyst layer 253 opposite to the side in contact with the electrolyte membrane 250. The cathode-side separator 273 is located on the side of the cathode-side gas diffusion layer 263 opposite to the side in contact with the cathode catalyst layer 253.

[0079] In the XY plane of the solid polymer water electrolysis apparatus 210 shown in Figure 9, the sizes of the anode catalyst layer 251, the anode-side gas diffusion layer 261, the cathode catalyst layer 253, and the cathode-side gas diffusion layer 263 are smaller than the sizes of the electrolyte membrane 250, the anode-side separator 271, and the cathode-side separator 273.

[0080] The first peripheral surface 250a of the electrolyte membrane 250, which is the peripheral edge of one face of the electrolyte membrane 250, faces the first inner surface 271a of the anode-side separator 271, which is the peripheral edge of one face of the anode-side separator 271. The space between the first peripheral surface 250a of the electrolyte membrane and the first inner surface 271a of the anode-side separator is sealed with a double-sided adhesive sheet 11. The second peripheral surface 250b of the electrolyte membrane 250, which is the other face of the electrolyte membrane 250, faces the first inner surface 273b of the cathode-side separator 273, which is the peripheral edge of one face of the cathode-side separator 273. The space between the second peripheral surface 250b of the electrolyte membrane and the first inner surface 273b of the cathode-side separator is sealed with a double-sided adhesive sheet 11.

[0081] The double-sided adhesive sheet 11 of the embodiment may be replaced with the adhesive sheet 10 of the embodiment. Alternatively, the double-sided adhesive sheet 11 of the embodiment may be replaced with the single-sided adhesive sheet 13, which is composed of a heat-resistant and chemical-resistant film 13c and an adhesive layer 13a formed on one side of the heat-resistant and chemical-resistant film 13c as shown in Figure 10. In this case, the heat-resistant and chemical-resistant film 13c of the single-sided adhesive sheet 13 is positioned on the anode-side separator's first inner edge surface 271a side, and the adhesive layer 13a is positioned on the electrolyte membrane's first peripheral edge surface 250a side, so that the space between the anode-side separator's first inner edge surface 271a and the electrolyte membrane's first peripheral edge surface 250a is sealed with the single-sided adhesive sheet 13. Similarly, the space between the electrolyte membrane's second peripheral edge surface 250b and the cathode-side separator's first inner edge surface 273b is also sealed with the single-sided adhesive sheet 13. Here, by fixing the anode catalyst layer 251, the anode-side gas diffusion layer 261, the electrolyte membrane 250, the cathode catalyst layer 253, and the anode-side separator 271 and cathode-side separator 273, which sandwich the cathode-side gas diffusion layer 263, under pressure, the interface between the first inner edge surface 271a of the anode-side separator and the heat-resistant and chemical-resistant film 13c of the single-sided adhesive sheet 13, and the interface between the first inner edge surface 273b of the cathode-side separator and the heat-resistant and chemical-resistant film 13c of the single-sided adhesive sheet 13 can be sealed without an adhesive layer in between.

[0082] The adhesive resin composition constituting the adhesive layer 13a is the same resin composition as the adhesive resin composition constituting the adhesive sheet 10 of the embodiment. The thickness of the adhesive layer 13a is preferably 1 μm or more and 200 μm or less, more preferably 3 μm or more and 200 μm or less, even more preferably 3 μm or more and 150 μm or less, and even more preferably 3 μm or more and 100 μm or less. The heat-resistant and chemical-resistant film 13c is the same film as the film constituting the heat-resistant and chemical-resistant film 11c of the double-sided adhesive sheet 11. The thickness of the heat-resistant and chemical-resistant film 13c is preferably 10 μm or more and 200 μm or less, and more preferably 25 μm or more and 150 μm or less. The single-sided adhesive sheet 13 can be obtained, for example, by the following procedure. The adhesive resin composition is applied to one side of the heat-resistant and chemical-resistant film 13c using a coating device to form an adhesive layer 13a composed of the adhesive resin composition. Next, the formed adhesive layer 13a is heated, for example, at 120°C to 180°C for 2 to 10 minutes. After cooling, the adhesive layer is heated again for a certain period of time to obtain a single-sided adhesive sheet 13.

[0083] The single-sided adhesive sheet 13 may be obtained by a method other than the one described above. For example, an adhesive resin composition is applied to the separator film 12 using a coating device to form an adhesive layer made of the adhesive resin composition. Next, the formed adhesive layer is heated, for example, at 120°C to 180°C for 2 minutes to 10 minutes. After cooling, an adhesive layer is obtained formed on one side of the separator film 12. Next, the adhesive layer formed on one side of the separator film 12 and the heat-resistant and chemical-resistant film 13c are laminated in that order, so that the surface of the adhesive layer with exposed resin is in contact with the heat-resistant and chemical-resistant film 13c. The resulting laminate is heated in a press molding machine, for example, at 50°C to 160°C, and pressurized with a pressure of 0.5 MPa to 3.0 MPa from a direction perpendicular to the main plane of the laminate. The heating and pressurizing time is 0.1 seconds to 10 seconds. After cooling, the adhesive layer is further heated for a certain period of time. The separator film 12 is peeled off from the resulting laminate to obtain a single-sided adhesive sheet 13. The conditions for heating the adhesive layer for a certain period of time are, for example, 80°C for 4 days or 120°C for 1 day.

[0084] The present invention will be described in more detail below with reference to examples. The present invention is not limited in any way by the following examples.

[0085] (Example 1) (Preparation of Adhesive Sheet 10) (1) Preparation of Adhesive Resin Composition In a container, 100 parts by mass of 100 wt% ToughTec M1943 (manufactured by Asahi Kasei Corporation) as an acid-modified styrene block copolymer and 354 parts by mass of toluene as an organic solvent were added and stirred until ToughTec M1943 dissolved in toluene. To the obtained solution, 150 parts by mass of YS Polystar UH115 (manufactured by Yasuhara Chemical Co., Ltd.) as a tackifier and 3.2 parts by mass of EHPE3150 (manufactured by Daicel Corporation) as a crosslinking agent were added and stirred until dissolved to obtain an adhesive resin composition. Here, ToughTec M1943 is an acid-modified styrene block copolymer having an acid value of 10 mg KOH / g. YS Polystar UH115 is a hydrogenated terpene phenol resin having a hydroxyl value of 20 mg KOH / g or more and 25 mg KOH / g or less, and a melting point of 115°C. EHPE3150 is a polyfunctional alicyclic epoxy resin having an epoxy equivalent of 177 g / eq. The amount of crosslinking agent (parts by mass) is such that the epoxy groups of the crosslinking agent amount to 1.0 equivalent (curing equivalent) for every 1 equivalent of acid-modified functional groups of the acid-modified styrene-based block copolymer (3.2 parts by mass).

[0086] (2) Preparation of the adhesive sheet 10 The prepared adhesive resin composition was applied to the release-treated surface of the separator film 14 using a bar coater so that the thickness after heating was 30 μm. After application, it was heated at 150°C for 3 minutes to obtain a laminate in which an adhesive layer was formed on one side of the separator film 14. Next, the separator film 12 was bonded to the exposed adhesive layer and stored in an atmosphere of 80°C for 4 days to obtain the adhesive sheet 10. The adhesive sheet 10 was used after peeling off the separator films 12 and 14. The separator films 12 and 14 are PET films (Lintec 3811) with a thickness of 38 μm and a release treatment applied to one side.

[0087] The adhesive sheet 10 obtained was evaluated for its adhesion to resin materials and metal materials, and for its adhesion in high-temperature environments and in acidic or alkaline environments. The adhesion was evaluated by a peel test. <Peel Test> (1) Preparation of Samples for Measurement (1-1) PPS Film / Adhesive Sheet 10 / PPS Film An adhesive sheet 10 was prepared by cutting it into a square with sides of 100 mm. Next, the adhesive sheet 10 from which the separator film 12 had been peeled off was bonded to a polyphenylene sulfide film (PPS film) cut into a square with sides of 100 mm. Next, the separator film 14 was peeled off, and the adhesive sheet 10 was bonded to a polyphenylene sulfide film (PPS film) cut into a rectangle of 200 mm in length and 100 mm in width to obtain a laminate. This laminate was heated and pressurized in a press molding machine. The temperature at which the laminate was heated at this time was 120°C. Furthermore, the pressure applied to the laminate from above and below was 0.5 MPa. The heating and pressurizing time was 30 seconds. The obtained laminate was stored for 12 hours in an atmosphere of 23°C and 50% relative humidity (hereinafter referred to as 50RH%). Next, the obtained laminate was cut into a rectangle with a width of 10 mm and a length of 100 mm to obtain a sample for measurement. The 200 mm long and 100 mm wide PPS film constituting the laminate was cut into a rectangle with a width of 10 mm and a length of 200 mm to make it easier to grasp the film to be peeled off in the peel test. The PPS film used was Toray Industries' Torelina 3030, with a thickness of 25 μm.

[0088] (1-2) PPS film / adhesive sheet 10 / titanium foil An adhesive sheet 10 cut into a square with sides of 100 mm was prepared. Next, the adhesive sheet 10 from which the separator film 12 had been peeled off was bonded to a titanium foil cut into a square with sides of 100 mm. Next, the separator film 14 was peeled off, and a laminate was obtained by bonding the adhesive sheet 10 to a polyphenylene sulfide film (PPS film) cut into a rectangle of 200 mm in length and 100 mm in width. This laminate was heated and pressurized in a press molding machine. The temperature at which the laminate was heated was 120°C. The pressure applied to the laminate from above and below was 0.5 MPa. The heating and pressurizing time was 30 seconds. The obtained laminate was stored for 12 hours in an atmosphere of 23°C and relative humidity of 50% (hereinafter referred to as 50RH%). Next, the obtained laminate was cut into a rectangle with a width of 10 mm and a length of 100 mm to obtain a sample for measurement. The titanium foil has a thickness of 100 μm. The PPS film that makes up the laminate, measuring 200 mm in length and 100 mm in width, is cut into rectangles 10 mm wide and 200 mm long to facilitate gripping the film to be peeled off during the peel test.

[0089] (2) For the peel strength of the sample used for the peel test, the peel strength of the PPS film was measured in accordance with Section 8.1 of JIS Standard C6471. Specifically, the peel strength in the 180° direction was measured using Shimadzu Corporation's EZ-TEST under the following measurement conditions. The measurement conditions were to pull a 200 mm long PPS film in an atmosphere of 23°C, with a test speed of 50 mm / min. Measurements were performed with n=3 samples, and the average value was taken as the peel strength of the adhesive sheet 10 of Example 1. The 180° direction refers to the plane direction parallel to the main surface of the measurement sample. The higher this peel strength, the higher the adhesion between the adhesive sheet 10 and the PPS film. The evaluation criteria were as follows. Excellent: Peel strength of 5 N / cm or more, Good: Peel strength of 3 N / cm or more but less than 5 N / cm, Poor: Peel strength of less than 3 N / cm.

[0090] In Example 1, the peel strength of the adhesive sheet 10 in the PPS film / adhesive sheet 10 / PPS film was 5.7 N / cm, which was excellent. This peel strength was defined as the initial peel strength.

[0091] (2-1) Peel test of measurement samples immersed in 95°C water for 500 hours The measurement samples were immersed in 95°C water for 500 hours. After that, the measurement samples were removed and stored for 24 hours at 23°C in a 50 RH atmosphere. The peel strength of the PPS film of the measurement samples after storage was measured. Deionized water was used. Deionized water was also used in the other tests below. The evaluation criteria for the peel test of the immersed measurement samples were as follows: Excellent: Peel strength of 3 N / cm or more, Good: Peel strength of 1 N / cm or more but less than 3 N / cm, Poor: Peel strength of less than 1 N / cm.

[0092] The peel strength of the adhesive sheet 10 in the PPS film / adhesive sheet 10 of Example 1 was 4.4 N / cm, which was excellent.

[0093] (2-2) Peel test of a sample immersed in 95°C water for 1000 hours The sample was immersed in 95°C water for 1000 hours. After that, the sample was removed and stored for 24 hours in an atmosphere of 23°C and 50 RH. The peel strength of the PPS film of the sample after storage was measured. The evaluation criteria for the peel test were the same as those for the peel test of a sample immersed in 95°C water for 500 hours.

[0094] The peel strength of the adhesive sheet 10 in the PPS film / adhesive sheet 10 / PPS film in Example 1 was 1.3 N / cm, which was good.

[0095] (2-3) Peel test of a sample immersed in an acidic aqueous solution at 95°C for 1000 hours. The sample was immersed in an acidic aqueous solution at 95°C for 1000 hours. After that, the sample was removed, washed with deionized water, and stored for 24 hours in an atmosphere of 23°C and 50 RH. The peel strength of the PPS film of the sample after storage was measured. The evaluation criteria for the peel test were the same as those for the peel test of a sample immersed in water at 95°C for 500 hours. The acidic aqueous solution was a sulfuric acid aqueous solution prepared by adding deionized water to a 0.005 mol / L sulfuric acid aqueous solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) until the pH of the aqueous solution reached 3.

[0096] The peel strength of the adhesive sheet 10 in the PPS film / adhesive sheet 10 / PPS film in Example 1 was 1.5 N / cm, which was good.

[0097] (2-4) Peel test of a sample immersed in 95°C coolant for 1000 hours The sample was immersed in 95°C coolant for 1000 hours. After that, the sample was removed, washed with deionized water, and stored for 24 hours in an atmosphere of 23°C and 50 RH. The peel strength of the PPS film of the sample after storage was measured. The evaluation criteria for the peel test were the same as those for the peel test of a sample immersed in 95°C water for 500 hours. The coolant was long-life coolant (manufactured by Monotaro Co., Ltd.).

[0098] The peel strength of the adhesive sheet 10 in the PPS film / adhesive sheet 10 / PPS film in Example 1 was 2.4 N / cm, which was good.

[0099] (2-5) Peel test of a sample immersed in an alkaline aqueous solution at 60°C for 1000 hours. The sample was immersed in an alkaline aqueous solution at 60°C for 1000 hours. After that, the sample was removed, washed with deionized water, and stored for 24 hours in an atmosphere of 23°C and 50 RH. The peel strength of the PPS film of the sample after storage was measured. The evaluation criteria for the peel test were the same as those for the peel test of a sample immersed in water at 95°C for 500 hours. The alkaline aqueous solution was a 1 mol / L potassium hydroxide aqueous solution with a pH of 14 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).

[0100] The peel strength of the adhesive sheet 10 in the PPS film / adhesive sheet 10 of Example 1 was 5.2 N / cm, which was excellent.

[0101] The initial peel strength of the PPS film / adhesive sheet 10 / titanium foil of Example 1 was measured using the same test method as that used for the PPS film / adhesive sheet 10 / PPS film of Example 1. The initial peel strength was 8.1 N / cm, which was excellent. In addition, the peel tests of the measurement sample immersed in 95°C water for 500 hours, the peel tests of the measurement sample immersed in 95°C water for 1000 hours, the peel tests of the measurement sample immersed in 95°C acidic aqueous solution for 1000 hours, the peel tests of the measurement sample immersed in 95°C coolant for 1000 hours, and the peel tests of the measurement sample immersed in 60°C alkaline aqueous solution for 1000 hours were performed using the same test method as that used for the PPS film / adhesive sheet 10 / PPS film of Example 1. The results are shown in Table 1. Furthermore, no delamination was observed at the interface between the adhesive sheet 10 and the titanium foil in these tests. This indicates that the adhesive strength between the adhesive sheet 10 and the titanium foil is higher than the adhesive strength between the adhesive sheet 10 and the PPS film.

[0102] In summary, the adhesive sheet 10 of Example 1 exhibits excellent adhesion to the resin material constituting the resin film and the metal material constituting the metal foil, and maintains excellent adhesion even when exposed to high-temperature environments and acidic or alkaline environments for extended periods. Furthermore, the adhesive sheet 10 of Example 1 was found to maintain excellent adhesion even when exposed to high-temperature coolant liquid for extended periods. Moreover, such an adhesive sheet 10 can be suitably used as an adhesive sheet in fuel cells and water electrolysis devices.

[0103] (Examples 2-6, Comparative Examples 1-4) Except for changing the type and amount of tackifier and the amount of crosslinking agent constituting the adhesive resin composition, the adhesive sheets 10 of Examples 2-6 and Comparative Examples 1-4 were prepared using the same method as the adhesive sheet 10 of Example 1. The adhesive sheets 10 of Examples 2-6 and Comparative Examples 1-4 were also evaluated using the same evaluation method as the adhesive sheet 10 of Example 1. The results are shown in Tables 1 and 2. The tackifier used in Example 4 was Haritack SE10 manufactured by Harima Chemicals Co., Ltd. Haritack SE10 is a hydrogenated rosin ester resin having an acid value of 2 mg KOH / g or more and 10 mg KOH / g or less, and a melting point of 83°C. The amount of crosslinking agent (parts by mass) was 5.0 parts by mass, such that the epoxy groups of the crosslinking agent amounted to 1.6 equivalents (curing equivalent) per equivalent of the acid-modified functional groups of the acid-modified styrene-based block copolymer.

[0104]

[0105]

[0106] The adhesive sheets 10 of Examples 2 to 6 were found to have excellent adhesion to the resin material constituting the resin film and the metal material constituting the metal foil, and to maintain excellent adhesion even when exposed to high-temperature environments and acidic or alkaline environments for extended periods. Furthermore, the adhesive sheets 10 of Examples 2 to 6 were found to maintain excellent adhesion even when exposed to high-temperature coolant liquid for extended periods. Moreover, these adhesive sheets 10 can also be suitably used as adhesive sheets in fuel cells and water electrolysis devices.

[0107] The adhesive sheet 10 of Comparative Example 1 was found to have poor initial adhesion and poor adhesion after being exposed to high-temperature and acidic or alkaline environments for extended periods. The adhesive sheet 10 of Comparative Example 2 was found to have poor adhesion to resin film after being exposed to high-temperature and alkaline environments for extended periods. The adhesive sheet 10 of Comparative Example 3 was found to have poor adhesion to resin film and metal foil after being exposed to high-temperature and alkaline environments for extended periods. The adhesive sheet 10 of Comparative Example 4 was found to have poor adhesion to resin film after being exposed to high-temperature and alkaline environments for extended periods. Furthermore, the adhesive sheet 10 of Comparative Example 4 was found to have poor adhesion to metal foil, both initially and after being immersed in high-temperature coolant for extended periods.

[0108] Furthermore, for Example 2, a sample of PEN film / adhesive sheet 10 / PEN film was prepared separately from the measurement sample of PPS film / adhesive sheet 10 / PPS film, and a peel test was performed. This peel test was performed using the same test method as in Example 1. Specifically, (1) the initial peel strength was measured. Furthermore, (2) a peel test was performed on the measurement sample immersed in 95°C water for 1000 hours, (3) a peel test was performed on the measurement sample immersed in an acidic aqueous solution at 95°C for 1000 hours, and (4) a peel test was performed on the measurement sample immersed in a coolant solution at 95°C for 1000 hours. The evaluation method was also the same as the evaluation method used in Example 1.

[0109] The evaluation results of the measurement samples of PEN film / adhesive sheet 10 / PEN film were as follows: (1) The initial peel strength was 5.0 N / cm, which was Excellent. (2) The peel strength of the measurement sample immersed in 95°C water for 1000 hours was 4.8 N / cm, which was Excellent. (3) The peel strength of the measurement sample immersed in 95°C acidic aqueous solution for 1000 hours was 3.1 N / cm, which was Excellent. And (4) The peel strength of the measurement sample immersed in 95°C coolant solution for 1000 hours was 3.5 N / cm, which was Excellent. The high peel strength between the PEN film and the adhesive sheet 10 indicates that the adhesive strength between the PEN film and the adhesive sheet 10 is high.

[0110] In preparing the measurement sample for the PEN film / adhesive sheet 10 / PEN film, the PEN film / adhesive sheet 10 / PPS film configuration was prepared using the same method as the measurement sample for the PPS film / adhesive sheet 10 / PPS film configuration, except that the PPS film was replaced with PEN film. The PEN film is a polyethylene naphthalate film, specifically Toyobo's Theonex Q5100 with a thickness of 25 μm.

[0111] (Example 7) A double-sided adhesive sheet 11 was prepared in order to perform an evaluation test similar to that of Example 1. (1) In a container for preparing the adhesive resin composition, 100 parts by mass of ToughTec M1943 (manufactured by Asahi Kasei Corporation) and 354 parts by mass of toluene as an organic solvent were added and stirred until ToughTec M1943 dissolved in toluene. To the obtained solution, 100 parts by mass of YS Polystar UH115 (manufactured by Yasuhara Chemical Co., Ltd.) and 3.2 parts by mass of EHPE3150 (manufactured by Daicel Corporation) were added and stirred until dissolved to obtain an adhesive resin composition. The amount of crosslinking agent (parts by mass) is such that the epoxy group of the crosslinking agent is 1.0 equivalent (curing equivalent) for every 1 equivalent of the acid-modified functional group of the acid-modified styrene-based block copolymer (3.2 parts by mass).

[0112] (2) Preparation of double-sided adhesive sheet 11 The prepared adhesive resin composition was applied to the release-treated surface of the separator film 12 using a bar coater so that the thickness after heating was 30 μm. After application, it was heated at 150°C for 3 minutes to obtain a laminate in which an adhesive layer was formed on one side of the separator film 12. Using the same method, a laminate in which an adhesive layer was formed on one side of the separator film 14 was obtained. Next, the laminates were laminated so that the adhesive layer was in contact with both sides of the heat-resistant and chemical-resistant film 11c. The obtained laminates were heated and pressurized using a press molding machine. The temperature at which the laminates were heated was 80°C. The pressure applied to the laminates from above and below was 0.5 MPa. The heating and pressurizing time was 10 seconds. After storing the obtained laminates in an atmosphere of 80°C for 4 days, a double-sided adhesive sheet 11 was obtained. The double-sided adhesive sheet 11 was used after peeling off the separator films 12 and 14. The separator films 12 and 14 are 38 μm thick PET films (Lintec 3811) with a release treatment applied to one side. The heat- and chemical-resistant film 11c that makes up the measurement sample (double-sided adhesive sheet 11) immersed in an alkaline aqueous solution at 60°C in the evaluation test is a 75 μm thick PPS film. The heat- and chemical-resistant film 11c that makes up the measurement sample (double-sided adhesive sheet 11) used in the other evaluation tests is a 100 μm thick PEN film.

[0113] The obtained double-sided adhesive sheet 11 was evaluated for its adhesion to resin materials and metal materials, and for its adhesion in high-temperature, acidic, or alkaline environments. The adhesion was evaluated by peel test. The evaluation method for the double-sided adhesive sheet 11 in Example 7 was the same as that for the adhesive sheet 10 in Example 1. The results are shown in Table 1.

[0114] The double-sided adhesive sheet 11 of Example 7 also exhibits excellent adhesion to resin films and metal foils, and was found to maintain excellent adhesion even when exposed to high-temperature environments and acidic or alkaline environments for extended periods. Furthermore, the double-sided adhesive sheet 11 of Example 7 was found to maintain excellent adhesion even when exposed to high-temperature coolant liquid for extended periods. This double-sided adhesive sheet 11 can also be suitably used as an adhesive sheet in fuel cells and water electrolysis devices.

[0115] This invention allows for various embodiments and modifications without departing from the broad spirit and scope of the invention. Furthermore, the embodiments described above are for illustrative purposes only and do not limit the scope of the invention. That is, the scope of the invention is indicated by the claims, not by the embodiments. Various modifications made within the scope of the claims and the equivalent scope of the meaning of the invention are considered to be within the scope of this invention.

[0116] This application is based on Japanese Patent Application No. 2025-077871, filed on 8 May 2025. This specification incorporates reference to the specification, claims, and drawings of Japanese Patent Application No. 2025-077871.

[0117] (Note) The various aspects of this disclosure are described below in summary as notes. (Note 1) An adhesive sheet comprising an adhesive resin composition comprising an acid-modified styrene block copolymer having an acid-modified functional group, a crosslinking agent having an epoxy group that reacts with the acid-modified functional group, and a hydrophobic tackifier having a melting point of 80°C or higher, wherein the amount of the tackifier contained in the adhesive resin composition is 65 parts by mass or more and 180 parts by mass or less per 100 parts by mass of the acid-modified styrene block copolymer, and the equivalent amount of the epoxy group of the crosslinking agent contained in the adhesive resin composition is 0.7 equivalents or more and 2.3 equivalents or less per 1 equivalent of the acid-modified functional group of the acid-modified styrene block copolymer.

[0118] (Note 2) The adhesive sheet according to Note 1, wherein the acid-modified styrene-based block copolymer has at least one selected from the group consisting of maleic anhydride, acrylic acid, and glycidyl methacrylate as an acid-modifying functional group.

[0119] (Note 3) The adhesive sheet according to Note 1 or Note 2, wherein the tackifier comprises at least one tackifier selected from the group consisting of a hydroxyl group-containing tackifier having a hydroxyl value of 5 mg KOH / g or more and 25 mg KOH / g or less, and an acidic functional group-containing tackifier having an acid value of 2 mg KOH / g or more and 20 mg KOH / g or less.

[0120] (Note 4) The adhesive sheet described in Note 3, wherein the hydroxyl group-containing tackifier is a hydrogenated terpene phenol resin.

[0121] (Note 5) The adhesive sheet according to Note 3, wherein the acidic functional group-containing tackifier is a hydrogenated rosin ester resin.

[0122] (Note 6) An adhesive sheet as described in any of Notes 1 to 5, having a thickness of 30 μm or more and 200 μm or less.

[0123] (Note 7) A double-sided adhesive sheet comprising: a heat-resistant and acid- and / or alkali-resistant heat- and chemical-resistant film; and an adhesive layer formed on both sides of the heat-resistant and chemical-resistant film, wherein the adhesive layer is composed of an adhesive resin composition comprising an acid-modified styrene block copolymer having acid-modified functional groups; a crosslinking agent having epoxy groups that react with the acid-modified functional groups; and a hydrophobic tackifier having a melting point of 80°C or higher, wherein the amount of the tackifier contained in the adhesive resin composition is 65 parts by mass or more and 180 parts by mass or less per 100 parts by mass of the acid-modified styrene block copolymer; and the equivalent amount of the epoxy groups of the crosslinking agent contained in the adhesive resin composition is 0.7 equivalents or more and 2.3 equivalents or less per 1 equivalent of the acid-modified functional groups of the acid-modified styrene block copolymer.

[0124] (Note 8) The double-sided adhesive sheet according to Note 7, wherein the acid-modified styrene-based block copolymer has at least one selected from the group consisting of maleic anhydride, acrylic acid, and glycidyl methacrylate as an acid-modifying functional group.

[0125] (Note 9) The double-sided adhesive sheet according to Note 7 or Note 8, wherein the tackifier comprises at least one tackifier selected from the group consisting of a hydroxyl group-containing tackifier having a hydroxyl value of 5 mg KOH / g or more and 25 mg KOH / g or less, and an acidic functional group-containing tackifier having an acid value of 2 mg KOH / g or more and 20 mg KOH / g or less.

[0126] (Note 10) The double-sided adhesive sheet according to Note 9, wherein the hydroxyl group-containing tackifier is a hydrogenated terpene phenol resin.

[0127] (Note 11) The double-sided adhesive sheet according to Note 9, wherein the acidic functional group-containing tackifier is a hydrogenated rosin ester resin.

[0128] (Note 12) The heat-resistant and chemical-resistant film is one film selected from the group consisting of polyethylene naphthalate film, polyphenylene sulfide film, polyphenyl sulfone film, polyphenylene ether film, polyvinyl chloride film, polypropylene film, polystyrene film, polyether ether ketone film, and cyclic olefin copolymer film, as described in any of Notes 7 to 11.

[0129] (Note 13) The electrolyte membrane comprises: an electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; a sheet-like sub-gasket arranged to surround the outside of the peripheral edge of the electrolyte membrane; an anode-side gas diffusion layer arranged on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator arranged on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer arranged on the side of the cathode catalyst layer opposite to the side in contact with the cathode catalyst layer; and a cathode-side separator arranged on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. A fuel cell in which the first surface of the subgasket, which is one surface of the subgasket, and the first inner edge surface of the anode-side separator, which is the peripheral edge of one surface of the anode-side separator, face each other, and the space between the first surface of the subgasket and the first inner edge surface of the anode-side separator is sealed with an adhesive sheet described in any of the appendices 1 to 6 or a double-sided adhesive sheet described in any of the appendices 7 to 12.

[0130] (Note 14) The fuel cell according to Note 13, wherein the second surface of the subgasket, which is the other surface of the subgasket, and the first inner edge surface of the cathode-side separator, which is the peripheral edge of one surface of the cathode-side separator, face each other, and the space between the second surface of the subgasket and the first inner edge surface of the cathode-side separator is sealed with an adhesive sheet described in any of Notes 1 to 6 or a double-sided adhesive sheet described in any of Notes 7 to 12.

[0131] (Note 15) The electrolyte membrane comprises an anode catalyst layer on one side and a cathode catalyst layer on the other side; an anode-side gas diffusion layer disposed on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator disposed on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer disposed on the side of the cathode catalyst layer opposite to the side in contact with the electrolyte membrane; and a cathode-side separator disposed on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. A fuel cell in which the first inner edge surface of the anode-side separator, which is the peripheral edge of one face of the anode-side separator, and the first inner edge surface of the cathode-side separator, which is the peripheral edge of one face of the cathode-side separator, face each other, and the space between the first inner edge surface of the anode-side separator and the first inner edge surface of the cathode-side separator is sealed with an adhesive sheet described in any of the appendices 1 to 6 or a double-sided adhesive sheet described in any of the appendices 7 to 12.

[0132] (Note 16) The electrolyte membrane comprises: an electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; a sheet-like sub-gasket arranged to surround the outside of the peripheral edge of the electrolyte membrane; an anode-side gas diffusion layer arranged on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator arranged on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer arranged on the side of the cathode catalyst layer opposite to the side in contact with the cathode catalyst layer; and a cathode-side separator arranged on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. A water electrolysis apparatus in which the first surface of the subgasket, which is one surface of the subgasket, and the first inner edge surface of the anode-side separator, which is the peripheral edge of one surface of the anode-side separator, face each other, and the space between the first surface of the subgasket and the first inner edge surface of the anode-side separator is sealed with an adhesive sheet described in any of the appendices 1 to 6 or a double-sided adhesive sheet described in any of the appendices 7 to 12.

[0133] (Note 17) The water electrolysis apparatus according to Note 16, wherein the second surface of the subgasket, which is the other surface of the subgasket, and the first inner edge surface of the cathode-side separator, which is the peripheral edge of one surface of the cathode-side separator, face each other, and the space between the second surface of the subgasket and the first inner edge surface of the cathode-side separator is sealed with an adhesive sheet described in any of Notes 1 to 6 or a double-sided adhesive sheet described in any of Notes 7 to 12.

[0134] (Note 18) The electrolyte membrane comprises an anode catalyst layer on one side and a cathode catalyst layer on the other side; an anode-side gas diffusion layer disposed on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator disposed on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer disposed on the side of the cathode catalyst layer opposite to the side in contact with the electrolyte membrane; and a cathode-side separator disposed on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. A water electrolysis apparatus in which the first inner edge surface of the anode-side separator, which is the peripheral edge of one face of the anode-side separator, and the first inner edge surface of the cathode-side separator, which is the peripheral edge of one face of the cathode-side separator, face each other, and the space between the first inner edge surface of the anode-side separator and the first inner edge surface of the cathode-side separator is sealed with an adhesive sheet described in any of the appendices 1 to 6 or a double-sided adhesive sheet described in any of the appendices 7 to 12.

[0135] (Note 19) A water electrolysis apparatus comprising: an electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; an anode-side gas diffusion layer disposed on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator disposed on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer disposed on the side of the cathode catalyst layer opposite to the side in contact with the electrolyte membrane; and a cathode-side separator disposed on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer, wherein the first peripheral surface of the electrolyte membrane, which is the peripheral edge of one side of the electrolyte membrane, and the first inner surface of the anode-side separator, which is the peripheral edge of one side of the anode-side separator, face each other, and the space between the first peripheral surface of the electrolyte membrane and the first inner surface of the anode-side separator is sealed with an adhesive sheet described in any of Notes 1 to 6 or a double-sided adhesive sheet described in any of Notes 7 to 12.

[0136] (Note 20) The water electrolysis apparatus according to Note 19, wherein the second peripheral surface of the electrolyte membrane, which is the peripheral edge of another surface of the electrolyte membrane, and the first inner surface of the cathode-side separator, which is the peripheral edge of one surface of the cathode-side separator, face each other, and the space between the second peripheral surface of the electrolyte membrane and the first inner surface of the cathode-side separator is sealed with an adhesive sheet described in any of Notes 1 to 6 or a double-sided adhesive sheet described in any of Notes 7 to 12.

[0137] 10 Adhesive sheet, 11 Double-sided adhesive sheet, 13 Single-sided adhesive sheet, 11c, 13c Heat-resistant and chemical-resistant film, 11a, 13a Adhesive layer, 12, 14 Separating film, 100, 110 Proton exchange type polymer electrolyte fuel cell, 50 Electrolyte membrane, 51 Anode catalyst layer, 52 Sub-gasket, 52a First surface of sub-gasket, 52b Second surface of sub-gasket, 53 Cathode catalyst layer, 61 Anode-side gas diffusion layer, 71 Anode-side separator or separator, 71a First inner edge surface of anode-side separator, 63 Cathode-side gas diffusion layer, 73 Cathode-side separator or separator, 73b First inner edge surface of cathode-side separator, 71gi, 73gi, 71go, 73go Grooves, 80 Regions, 200, 210, 220 Solid polymer water electrolyzer, 250 electrolyte membrane, 250a first peripheral surface of electrolyte membrane, 250b second peripheral surface of electrolyte membrane, 251 anode catalyst layer, 252 sub-gasket, 252a first surface of sub-gasket, 252b second surface of sub-gasket, 253 cathode catalyst layer, 261 anode-side gas diffusion layer, 271 anode-side separator or separator, 271a first inner surface of anode-side separator, 263 cathode-side gas diffusion layer, 273 cathode-side separator or separator, 273b first inner surface of cathode-side separator, 271gi, 273gi, 271go, 273go grooves, 280 region.

Claims

1. An adhesive sheet comprising an adhesive resin composition comprising an acid-modified styrene block copolymer having an acid-modified functional group, a crosslinking agent having an epoxy group that reacts with the acid-modified functional group, and a hydrophobic tackifier having a melting point of 80°C or higher, wherein the amount of the tackifier contained in the adhesive resin composition is 65 parts by mass or more and 180 parts by mass or less per 100 parts by mass of the acid-modified styrene block copolymer, and the equivalent amount of the epoxy group of the crosslinking agent contained in the adhesive resin composition is 0.7 equivalents or more and 2.3 equivalents or less per 1 equivalent of the acid-modified functional group of the acid-modified styrene block copolymer.

2. The adhesive sheet according to claim 1, wherein the acid-modified styrene-based block copolymer has at least one selected from the group consisting of maleic anhydride, acrylic acid, and glycidyl methacrylate as an acid-modifying functional group.

3. The adhesive sheet according to claim 1 or 2, wherein the tackifier comprises at least one tackifier selected from the group consisting of a hydroxyl group-containing tackifier having a hydroxyl value of 5 mg KOH / g or more and 25 mg KOH / g or less, and an acidic functional group-containing tackifier having an acid value of 2 mg KOH / g or more and 20 mg KOH / g or less.

4. The adhesive sheet according to claim 3, wherein the hydroxyl group-containing tackifier is a hydrogenated terpene phenol resin.

5. The adhesive sheet according to claim 3, wherein the acidic functional group-containing tackifier is a hydrogenated rosin ester resin.

6. An adhesive sheet according to any one of claims 1 to 5, wherein the thickness is 30 μm or more and 200 μm or less.

7. A double-sided adhesive sheet comprising: a heat-resistant and acid- and / or alkali-resistant heat- and chemical-resistant film; and an adhesive layer formed on both sides of the heat-resistant and chemical-resistant film, wherein the adhesive layer is composed of an adhesive resin composition comprising an acid-modified styrene block copolymer having acid-modified functional groups; a crosslinking agent having epoxy groups that react with the acid-modified functional groups; and a hydrophobic tackifier having a melting point of 80°C or higher, wherein the amount of the tackifier contained in the adhesive resin composition is 65 parts by mass or more and 180 parts by mass or less per 100 parts by mass of the acid-modified styrene block copolymer; and the equivalent amount of the epoxy groups of the crosslinking agent contained in the adhesive resin composition is 0.7 equivalents or more and 2.3 equivalents or less per 1 equivalent of the acid-modified functional groups of the acid-modified styrene block copolymer.

8. The double-sided adhesive sheet according to claim 7, wherein the acid-modified styrene-based block copolymer has at least one selected from the group consisting of maleic anhydride, acrylic acid, and glycidyl methacrylate as an acid-modifying functional group.

9. The double-sided adhesive sheet according to claim 7 or 8, wherein the tackifier comprises at least one tackifier selected from the group consisting of a hydroxyl group-containing tackifier having a hydroxyl value of 5 mg KOH / g or more and 25 mg KOH / g or less, and an acidic functional group-containing tackifier having an acid value of 2 mg KOH / g or more and 20 mg KOH / g or less.

10. The double-sided adhesive sheet according to claim 9, wherein the hydroxyl group-containing tackifier is a hydrogenated terpene phenol resin.

11. The double-sided adhesive sheet according to claim 9, wherein the acidic functional group-containing tackifier is a hydrogenated rosin ester resin.

12. The double-sided adhesive sheet according to any one of claims 7 to 11, wherein the heat-resistant and chemical-resistant film is one film selected from the group consisting of polyethylene naphthalate film, polyphenylene sulfide film, polyphenyl sulfone film, polyphenylene ether film, polyvinyl chloride film, polypropylene film, polystyrene film, polyether ether ketone film, and cyclic olefin copolymer film.

13. An electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; a sheet-like sub-gasket arranged to surround the outside of the peripheral edge of the electrolyte membrane; an anode-side gas diffusion layer arranged on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator arranged on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer arranged on the side of the cathode catalyst layer opposite to the side in contact with the electrolyte membrane; and a cathode-side separator arranged on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. A fuel cell in which the first surface of the subgasket, which is one surface of the subgasket, and the first inner edge surface of the anode-side separator, which is the peripheral edge of one surface of the anode-side separator, face each other, and the space between the first surface of the subgasket and the first inner edge surface of the anode-side separator is sealed with an adhesive sheet according to any one of claims 1 to 6 or a double-sided adhesive sheet according to any one of claims 7 to 12.

14. The fuel cell according to claim 13, wherein the second surface of the subgasket, which is the other surface of the subgasket, and the first inner edge surface of the cathode-side separator, which is the peripheral edge of one surface of the cathode-side separator, face each other, and the space between the second surface of the subgasket and the first inner edge surface of the cathode-side separator is sealed with the adhesive sheet according to any one of claims 1 to 6 or the double-sided adhesive sheet according to any one of claims 7 to 12.

15. An electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; an anode-side gas diffusion layer disposed on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator disposed on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer disposed on the side of the cathode catalyst layer opposite to the side in contact with the electrolyte membrane; and a cathode-side separator disposed on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. A fuel cell in which the first inner edge surface of the anode-side separator, which is the peripheral edge of one face of the anode-side separator, and the first inner edge surface of the cathode-side separator, which is the peripheral edge of one face of the cathode-side separator, face each other, and the space between the first inner edge surface of the anode-side separator and the first inner edge surface of the cathode-side separator is sealed with an adhesive sheet according to any one of claims 1 to 6 or a double-sided adhesive sheet according to any one of claims 7 to 12.

16. An electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; a sheet-like sub-gasket arranged to surround the outside of the peripheral edge of the electrolyte membrane; an anode-side gas diffusion layer arranged on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator arranged on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer arranged on the side of the cathode catalyst layer opposite to the side in contact with the electrolyte membrane; and a cathode-side separator arranged on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. A water electrolysis apparatus in which the first surface of the subgasket, which is one surface of the subgasket, and the first inner edge surface of the anode-side separator, which is the peripheral edge of one surface of the anode-side separator, face each other, and the space between the first surface of the subgasket and the first inner edge surface of the anode-side separator is sealed with an adhesive sheet according to any one of claims 1 to 6 or a double-sided adhesive sheet according to any one of claims 7 to 12.

17. The water electrolysis apparatus according to claim 16, wherein the second surface of the subgasket, which is the other surface of the subgasket, and the first inner edge surface of the cathode-side separator, which is the peripheral edge of one surface of the cathode-side separator, face each other, and the space between the second surface of the subgasket and the first inner edge surface of the cathode-side separator is sealed with an adhesive sheet according to any one of claims 1 to 6 or a double-sided adhesive sheet according to any one of claims 7 to 12.

18. An electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; an anode-side gas diffusion layer disposed on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator disposed on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer disposed on the side of the cathode catalyst layer opposite to the side in contact with the electrolyte membrane; and a cathode-side separator disposed on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer. A water electrolysis apparatus in which the first inner edge surface of the anode-side separator, which is the peripheral edge of one face of the anode-side separator, and the first inner edge surface of the cathode-side separator, which is the peripheral edge of one face of the cathode-side separator, face each other, and the space between the first inner edge surface of the anode-side separator and the first inner edge surface of the cathode-side separator is sealed with an adhesive sheet according to any one of claims 1 to 6 or a double-sided adhesive sheet according to any one of claims 7 to 12.

19. A water electrolysis apparatus comprising: an electrolyte membrane having an anode catalyst layer on one side and a cathode catalyst layer on the other side; an anode-side gas diffusion layer disposed on the side of the anode catalyst layer opposite to the side in contact with the electrolyte membrane; an anode-side separator disposed on the side of the anode-side gas diffusion layer opposite to the side in contact with the anode catalyst layer; a cathode-side gas diffusion layer disposed on the side of the cathode catalyst layer opposite to the side in contact with the electrolyte membrane; and a cathode-side separator disposed on the side of the cathode-side gas diffusion layer opposite to the side in contact with the cathode catalyst layer, wherein the first peripheral surface of the electrolyte membrane, which is the peripheral edge of one side of the electrolyte membrane, and the first inner surface of the anode-side separator, which is the peripheral edge of one side of the anode-side separator, face each other, and the space between the first peripheral surface of the electrolyte membrane and the first inner surface of the anode-side separator is sealed with an adhesive sheet according to any one of claims 1 to 6 or a double-sided adhesive sheet according to any one of claims 7 to 12.

20. The water electrolysis apparatus according to claim 19, wherein the second peripheral surface of the electrolyte membrane, which is the peripheral edge of another surface of the electrolyte membrane, and the first inner surface of the cathode-side separator, which is the peripheral edge of one surface of the cathode-side separator, face each other, and the space between the second peripheral surface of the electrolyte membrane and the first inner surface of the cathode-side separator is sealed with an adhesive sheet according to any one of claims 1 to 6 or a double-sided adhesive sheet according to any one of claims 7 to 12.