Spunlace nonwoven fabric

The spunlace nonwoven fabric with a synthetic and water-retaining fiber structure addresses clogging issues by enhancing permeability and retention, achieving superior absorption and retention of both liquid and viscous bodily fluids.

WO2026235047A1PCT designated stage Publication Date: 2026-11-12UNI CHARM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016720
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-04-27
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing bodily fluid absorbent sheets, such as those described in Patent Document 1, face issues with clogging when absorbing viscous fluids like stool or menstrual blood due to the presence of solid components, and they do not effectively differentiate between liquid and viscous fluid absorption.

Method used

A spunlace nonwoven fabric with a skin-facing layer of synthetic fibers and a non-skin-facing layer of water-retaining fibers, where the fibers are not heat-fused, allowing for a coarser weave and predetermined entanglement structures that enhance permeability and retention of both liquid and viscous bodily fluids.

Benefits of technology

The spunlace nonwoven fabric exhibits excellent liquid absorption and viscous fluid retention properties, reducing the likelihood of leakage and adhesion of viscous fluids to the skin, while maintaining effective absorption of both liquid and viscous bodily fluids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026016720_12112026_PF_FP_ABST
    Figure JP2026016720_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present disclosure is to provide a spunlace nonwoven fabric which, when used in a top sheet of an absorbent article, has excellent liquid body fluid absorbency and excellent viscosity-adjusted body fluid retainability. This spunlace nonwoven fabric for a top sheet of an absorbent article is characterized in that: the spunlace nonwoven fabric comprises a skin-side layer containing synthetic fibers and constituting a skin-contacting surface, and a non-skin-side layer that contains water-retaining fibers and that is adjacent to the skin-side layer; the synthetic fibers and the water-retaining fibers are not thermally fused; in a tensile test, the spunlace nonwoven fabric has a maximum elongation of 10‒70% in the conveyance direction during production; and in a 45° inclined artificial urine absorption test, the spunlace nonwoven fabric has a surface flow distance of 110 mm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Spunlace nonwoven fabric

[0001] This disclosure relates to spunlace nonwoven fabrics.

[0002] Research is being conducted on liquid permeability sheets for absorbent articles. For example, Patent Document 1 discloses a body fluid absorbent sheet that takes a short time to absorb body fluids discharged onto the surface, allows body fluids to drain quickly from the surface, and makes it difficult for body fluids to return to the surface. In other words, a body fluid absorbent sheet with high absorption performance (sweat absorption, absorption rate), high liquid drainage, and resistance to rewetting. The body fluid absorbent sheet according to Patent Document 1 is a body fluid absorbent sheet having a first surface and a second surface, comprising: a nonwoven fabric layer containing a plurality of heat-fusible fibers heat-fused to each other, with one surface constituting the first surface; and a hydrophilic fiber layer containing a plurality of hydrophilic fibers, with one surface adjacent to the other surface of the nonwoven fabric layer and the other surface constituting the second surface, wherein a portion of the plurality of hydrophilic fibers in the hydrophilic fiber layer penetrates the nonwoven fabric layer and is exposed on the first surface (Claim 1).

[0003] Japanese Patent Publication No. 2022-46325

[0004] The bodily fluid absorbent sheet described in Patent Document 1 contains multiple heat-fusible fibers that are heat-fused to each other, thereby allowing bodily fluids to be quickly removed from the surface. However, stool, for example, soft stool, contains solid components such as undigested dietary fiber, undigested protein, and detached intestinal mucosa, and menstrual blood contains solid components such as endometrium. The bodily fluid absorbent sheet disclosed in Patent Document 1 may become clogged when absorbing stool, menstrual blood, etc., posing a problem in absorbing stool, menstrual blood, etc. Therefore, the present disclosure aims to provide a spunlace nonwoven fabric that is excellent in both liquid bodily fluid absorption and viscous bodily fluid retention when used as a top sheet for absorbent articles.

[0005] The Disclosers have found a spunlace nonwoven fabric for a top sheet of an absorbent article, wherein the spunlace nonwoven fabric comprises a skin-facing layer containing synthetic fibers that constitutes the skin-contacting surface, and a non-skin-facing layer adjacent to the skin-facing layer containing water-retaining fibers, wherein the synthetic fibers and water-retaining fibers are not heat-fused, the spunlace nonwoven fabric has a maximum elongation of 10-70% in the transport direction during manufacturing in a tensile test, and the spunlace nonwoven fabric has a surface flow distance of 110 mm or less in a 45° inclined artificial urine absorption test.

[0006] The spunlace nonwoven fabric relating to this disclosure exhibits excellent liquid absorption and viscous fluid retention properties when used as a top sheet in absorbent articles.

[0007] Figure 1 is a cross-sectional photograph of nonwoven fabric No. 1 in the example.

[0008] Specifically, this disclosure relates to the following embodiments: [Embodiment 1A] A spunlace nonwoven fabric for a top sheet of an absorbent article, wherein the spunlace nonwoven fabric comprises a skin-facing layer containing synthetic fibers that constitutes the skin-contacting surface, and a non-skin-facing layer adjacent to the skin-facing layer containing water-retaining fibers, wherein the synthetic fibers and the water-retaining fibers are not heat-fused, the spunlace nonwoven fabric has a maximum elongation of 10-70% in the transport direction during manufacturing in a tensile test, and the spunlace nonwoven fabric has a surface flow distance of 110 mm or less in a 45° inclined artificial urine absorption test.

[0009] In the spunlace nonwoven fabric described above, the synthetic fibers and water-retaining fibers are not heat-fused. Therefore, although the spunlace nonwoven fabric has entanglement points where the synthetic fibers and water-retaining fibers are intertwined by water flow, it can be said that the synthetic fibers and water-retaining fibers do not have heat-fused points. Consequently, the spunlace nonwoven fabric has a coarser weave (larger openings formed between fibers) compared to the nonwoven fabric having heat-fused points. As a result, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, it is more permeable to bodily fluids with liquid properties (hereinafter referred to as "liquid bodily fluids," e.g., urine) compared to the nonwoven fabric having heat-fused points. Furthermore, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, it is more permeable to some bodily fluids with viscous properties (hereinafter referred to as "viscous bodily fluids," e.g., loose stools, menstrual blood, vaginal discharge, etc.) compared to the nonwoven fabric having heat-fused points.

[0010] The spunlace nonwoven fabric described above has a predetermined maximum elongation. Therefore, it can be said that the spunlace nonwoven fabric has a predetermined degree of entanglement and comprises a skin-side layer in which water-retaining fibers in the non-skin-side layer penetrate to a certain extent into the skin-side layer, and a non-skin-side layer in which synthetic fibers in the skin-side layer penetrate to a certain extent into the non-skin-side layer. As a result, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, for example, when the absorbent article absorbs bodily fluids, it becomes less likely for synthetic fibers, water-retaining fibers, etc., to come out of the spunlace nonwoven fabric. Note that the "skin-side layer in which water-retaining fibers in the non-skin-side layer penetrate to a certain extent into the skin-side layer" may be referred to as the "skin-side layer having a predetermined entanglement structure," and the "non-skin-side layer in which synthetic fibers in the skin-side layer penetrate to a certain extent into the non-skin-side layer" may be referred to as the "non-skin-side layer having a predetermined entanglement structure."

[0011] The spunlace nonwoven fabric described above has a predetermined surface flow distance in a 45° inclined artificial urine absorption test. Therefore, when the bodily fluid is a liquid bodily fluid (e.g., urine), when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, the skin-side layer having a predetermined entanglement structure can draw in the liquid bodily fluid that reaches the skin-contact surface, the non-skin-side layer having a predetermined entanglement structure can draw in the liquid bodily fluid drawn into the skin-side layer to the non-skin-side layer, and then transfer it to the layer adjacent to the non-skin-side layer (e.g., the absorbent core). As a result, the spunlace nonwoven fabric exhibits excellent liquid bodily fluid absorption when used in absorbent articles. Note that 110 mm corresponds to the distance from the urinary opening of a male baby to the ventral end of the product in a size S tape-type disposable diaper for babies. Therefore, because the spunlace nonwoven fabric has the predetermined surface flow distance described above, it can be said that liquid bodily fluids (e.g., urine) are less likely to leak in disposable diapers in general, including baby disposable diapers.

[0012] Furthermore, when the bodily fluid is a viscous fluid (e.g., loose stool, menstrual blood, vaginal discharge, etc.), when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, the skin-side layer having a predetermined entanglement structure can draw in moisture from the viscous fluid that reaches the skin-contact surface, the non-skin-side layer having a predetermined entanglement structure can draw in the moisture from the bodily fluid drawn into the skin-side layer to the non-skin-side layer, and then transfer it to the layer adjacent to the non-skin-side layer (e.g., the absorbent core). As a result, the spunlace nonwoven fabric can increase the solid content concentration of the viscous fluid, making it less likely to adhere to the wearer's skin, and can also exhibit viscous fluid retention properties that allow the viscous fluid to be retained in the spunlace nonwoven fabric.

[0013] Furthermore, when the bodily fluid is a viscous bodily fluid containing solid components (for example, soft stool containing undigested dietary fiber, undigested protein, shed intestinal mucosa, etc., menstrual blood containing endometrium, etc.), when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, the skin-side layer having a predetermined entanglement structure draws in moisture from the viscous bodily fluid that reaches the skin-contact surface. As a result, the top sheet is less likely to clog, and the non-skin-side layer having a predetermined entanglement structure can continue to draw in moisture from the bodily fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the layer adjacent to the non-skin-side layer (for example, the absorbent core). Consequently, the spunlace nonwoven fabric can increase the solid content concentration of the viscous bodily fluid containing solid components, making it less likely for the viscous bodily fluid containing solid components to adhere to the wearer's skin, while also exhibiting viscous bodily fluid retention properties that retain the viscous bodily fluid in the spunlace nonwoven fabric.

[0014] Based on the above, the spunlace nonwoven fabric exhibits excellent liquid absorption and viscous fluid retention properties when used as a top sheet for absorbent articles. In this specification, the use of the spunlace nonwoven fabric as a top sheet for absorbent articles may be simply referred to as "when used in absorbent articles."

[0015] [Aspect 1B] A spunlace nonwoven fabric for a top sheet of an absorbent article, wherein the spunlace nonwoven fabric comprises a skin-facing layer containing synthetic fibers that constitutes the skin-contacting surface, and a non-skin-facing layer adjacent to the skin-facing layer containing water-retaining fibers, and the synthetic fibers and the water-retaining fibers are not heat-fused.

[0016] In the spunlace nonwoven fabric described above, the synthetic fibers and water-retaining fibers are not heat-fused. Therefore, although the spunlace nonwoven fabric has entanglement points where the synthetic fibers and water-retaining fibers are intertwined by water flow, it can be said that the synthetic fibers and water-retaining fibers do not have heat-fused points. Consequently, the spunlace nonwoven fabric has a coarser weave (larger openings formed between fibers) compared to the nonwoven fabric having heat-fused points. As a result, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, the top sheet is more permeable to liquid fluids and a portion of viscous fluids compared to the nonwoven fabric having heat-fused points.

[0017] The above spunlace nonwoven fabric, during the water flow entanglement treatment, has a skin-side layer having a predetermined entanglement structure and a non-skin-side layer having a predetermined entanglement structure, as the water-retaining fibers in the non-skin-side layer penetrate to a certain extent into the skin-side layer and the synthetic fibers in the skin-side layer penetrate to a certain extent into the non-skin-side layer.

[0018] When the bodily fluid is a liquid bodily fluid, such as urine, and the spunlace nonwoven fabric is used as the top sheet of an absorbent article, the skin-side layer having a predetermined entanglement structure can draw in the liquid bodily fluid that reaches the skin-contact surface, and the non-skin-side layer having a predetermined entanglement structure can draw in the liquid bodily fluid drawn into the skin-side layer to the non-skin-side layer, and then transfer it to the layer adjacent to the non-skin-side layer (for example, the absorbent core). As a result, the spunlace nonwoven fabric exhibits excellent liquid bodily fluid absorption when used in an absorbent article.

[0019] Furthermore, when the bodily fluid is a viscous fluid (e.g., loose stool, menstrual blood, vaginal discharge, etc.), when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, the skin-side layer having a predetermined entanglement structure can draw in moisture from the viscous fluid that reaches the skin-contact surface, the non-skin-side layer having a predetermined entanglement structure can draw in the moisture from the bodily fluid drawn into the skin-side layer to the non-skin-side layer, and then transfer it to the layer adjacent to the non-skin-side layer (e.g., the absorbent core). As a result, the spunlace nonwoven fabric can increase the solid content concentration of the viscous fluid, making it less likely to adhere to the wearer's skin, and can also exhibit viscous fluid retention properties that allow the viscous fluid to be retained in the spunlace nonwoven fabric.

[0020] Furthermore, when the bodily fluid is a viscous bodily fluid containing solid components (for example, soft stool containing undigested dietary fiber, undigested protein, shed intestinal mucosa, etc., menstrual blood containing endometrium, etc.), when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, the top sheet is less likely to clog when the skin-side layer having a predetermined entanglement structure draws in moisture from the viscous bodily fluid that has reached the skin-contact surface. As a result, the non-skin-side layer having a predetermined entanglement structure can continue to draw in moisture from the bodily fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the layer adjacent to the non-skin-side layer (for example, the absorbent core). Consequently, the spunlace nonwoven fabric can increase the solid content concentration of the viscous bodily fluid containing solid components, making it less likely for the viscous bodily fluid containing solid components to adhere to the wearer's skin, while also exhibiting viscous bodily fluid retention properties that allow the viscous bodily fluid to be retained in the spunlace nonwoven fabric.

[0021] Based on the above, the spunlace nonwoven fabric exhibits excellent liquid absorption and viscous fluid retention properties when used as a top sheet for absorbent articles.

[0022] [Aspect 2A] The spunlace nonwoven fabric is the spunlace nonwoven fabric according to aspect 1A or 1B, having a Klem water absorption of 30 to 170 mm.

[0023] The spunlace nonwoven fabric described above has a predetermined Klem water absorption rate. Therefore, when used in absorbent articles, the spunlace nonwoven fabric facilitates the diffusion of bodily fluids in both the planar and thickness directions. As a result, when used as a top sheet in absorbent articles, the spunlace nonwoven fabric exhibits excellent liquid bodily fluid absorption and viscous bodily fluid retention properties.

[0024] [Aspect 2B] The spunlace nonwoven fabric according to aspect 1B, wherein in a tensile test, the spunlace nonwoven fabric has a maximum elongation of 10 to 70% in the conveying direction during manufacturing.

[0025] The spunlace nonwoven fabric described above exhibits a predetermined maximum elongation in tensile tests. Therefore, it can be said that the spunlace nonwoven fabric has a predetermined degree of entanglement and comprises a skin-side layer having a predetermined entanglement structure and a non-skin-side layer having a predetermined entanglement structure. As a result, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, for example, when the absorbent article absorbs bodily fluids, it becomes less likely for synthetic fibers, water-retaining fibers, etc., to come loose from the spunlace nonwoven fabric. Furthermore, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, it exhibits excellent liquid bodily fluid absorption and viscous bodily fluid retention.

[0026] [Aspect 2C] The spunlace nonwoven fabric described in Aspect 1B, wherein the spunlace nonwoven fabric has a surface flow distance of 110 mm or less in a 45° inclined artificial urine absorption test.

[0027] The spunlace nonwoven fabric described above has a predetermined surface flow distance in a 45° inclined artificial urine absorption test. Therefore, when the bodily fluid is a liquid bodily fluid (e.g., urine), when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, the skin-side layer having a predetermined entanglement structure can draw in the liquid bodily fluid that reaches the skin-contact surface, the non-skin-side layer having a predetermined entanglement structure can draw in the liquid bodily fluid drawn into the skin-side layer to the non-skin-side layer, and then transfer it to the layer adjacent to the non-skin-side layer (e.g., the absorbent core). As a result, the spunlace nonwoven fabric exhibits excellent liquid bodily fluid absorption when used in absorbent articles. Note that 110 mm corresponds to the distance from the urinary opening of a male baby to the ventral end of the product in a size S tape-type disposable diaper for babies. Therefore, because the spunlace nonwoven fabric has the predetermined surface flow distance described above, it can be said that liquid bodily fluids (e.g., urine) are less likely to leak in disposable diapers in general, including baby disposable diapers.

[0028] [Aspect 3] The spunlace nonwoven fabric described above is the spunlace nonwoven fabric according to any one of aspects 1A, 1B, 2A, 2B, and 2C, wherein the rewetting rate in the rewetting test is 20% by mass or less.

[0029] The spunlace nonwoven fabric described above has a predetermined rewetting rate. Therefore, it can be said that the spunlace nonwoven fabric has a predetermined entanglement structure in its skin-facing layer and contains a predetermined ratio of synthetic fibers and water-retaining fibers. Consequently, when used in absorbent articles, the spunlace nonwoven fabric exhibits excellent rewetting properties.

[0030] [Aspect 4] The spunlace nonwoven fabric described above has a tensile strength of 1.10 to 4.25 N / 25 mm in the transport direction during manufacturing, as determined in the tensile test described above, and is the spunlace nonwoven fabric described in any one of aspects 1A, 1B, 2A, 2B, 2C, and 3.

[0031] The spunlace nonwoven fabric described above has a predetermined strength at 5% elongation. Therefore, when the spunlace nonwoven fabric is used in absorbent articles, for example, when the absorbent article absorbs bodily fluids, it becomes less likely for synthetic fibers, water-retaining fibers, etc., to detach from the spunlace nonwoven fabric.

[0032] [Aspect 5] The spunlace nonwoven fabric according to any one of Aspects 1A, 1B, 2A, 2B, 2C, 3 and 4, wherein the spunlace nonwoven fabric comprises the synthetic fiber and the water-retentive fiber at a mass ratio of 40 to 80:60 to 20, based on 100 parts by mass of the total of the synthetic fiber and the water-retentive fiber.

[0033] The spunlace nonwoven fabric contains the synthetic fiber and the water-retentive fiber at a predetermined mass ratio. Accordingly, the skin-side layer and the non-skin-side layer can easily exhibit their respective functions, and the spunlace nonwoven fabric is excellent in liquid body fluid absorbability and viscous body fluid retention property when used as a top sheet of an absorbent article.

[0034] [Aspect 6] The spunlace nonwoven fabric has a basis weight of 25 to 70 g / m 2 The spunlace nonwoven fabric according to Aspect 5.

[0035] The spunlace nonwoven fabric contains the synthetic fiber and the water-retentive fiber at a predetermined mass ratio, and has a predetermined basis weight. Accordingly, the skin-side layer and the non-skin-side layer can easily exhibit their respective functions, and the spunlace nonwoven fabric is excellent in liquid body fluid absorbability and viscous body fluid retention property when used as a top sheet of an absorbent article.

[0036] [Aspect 7] The spunlace nonwoven fabric according to any one of Aspects 1A, 1B, 2A, 2B, 2C and 3 to 6, wherein the synthetic fiber has an average fiber length of 30 to 60 mm, and the water-retentive fiber has an average fiber length of 30 to 60 mm.

[0037] In the above-described spunlace nonwoven fabric, each of the synthetic fibers and the water-retaining fibers has a predetermined average fiber length. Therefore, the spunlace nonwoven fabric tends to have a predetermined degree of entanglement, and in the skin-side layer having the predetermined degree of entanglement, a certain amount of water-retaining fibers tends to be present within the skin-side layer, but not excessively on the skin-contact surface of the skin-side layer. As a result, after the skin-side layer draws in moisture from bodily fluids that have reached the skin-contact surface (moisture in urine, moisture in loose stool, etc.), it is easier for the moisture to be transferred to the non-skin-side layer without being retained in the skin-side layer, and the non-skin-side layer then easily transfers the moisture from the bodily fluids it has received to the layer adjacent to the non-skin-side layer (for example, the absorbent core). Based on the above, when the above-described spunlace nonwoven fabric is used as the top sheet of an absorbent article, it exhibits excellent adhesion to liquid bodily fluids and retention of viscous bodily fluids.

[0038] [Aspect 8] The non-skin-facing layer is a spunlace nonwoven fabric according to any one of aspects 1A, 1B, 2A, 2B, 2C and 3 to 7, wherein the non-skin-facing layer has a higher fiber density than the skin-facing layer.

[0039] In the above-described spunlace nonwoven fabric, the non-skin-facing layer has a higher fiber density than the skin-facing layer. Therefore, after the skin-facing layer, which has a predetermined entanglement structure, draws in moisture from bodily fluids that have reached the skin-contacting surface (e.g., moisture from liquid bodily fluids, viscous bodily fluids, etc.), the water-retaining fibers with a high fiber density present in the non-skin-facing layer can further draw in the moisture from the bodily fluids that have been drawn into the skin-facing layer. As a result, when the above-described spunlace nonwoven fabric is used as a top sheet for absorbent articles, it exhibits excellent liquid bodily fluid absorption and viscous bodily fluid retention.

[0040] [Aspect 9] The synthetic fiber is a spunlace nonwoven fabric according to any one of aspects 1A, 1B, 2A, 2B, 2C and 3 to 8, comprising a durable hydrophilic oil agent.

[0041] In the spunlace nonwoven fabric described above, the synthetic fibers contain a durable hydrophilic oil agent. Therefore, during the spunlace treatment, the spunlace nonwoven fabric becomes more prone to entanglement between synthetic fibers, between water-retaining fibers, and between synthetic fibers and water-retaining fibers. Furthermore, the spunlace nonwoven fabric is more likely to have a skin-side layer having a predetermined entanglement structure and a non-skin-side layer having a predetermined entanglement structure. As a result, when used as a top sheet for absorbent articles, the spunlace nonwoven fabric exhibits excellent liquid absorption and viscous fluid retention properties.

[0042] [Aspect 10] The spunlace nonwoven fabric according to any one of aspects 1A, 1B, 2A, 2B, 2C and 3 to 9, wherein the synthetic fiber is polyethylene terephthalate fiber and the water-retaining fiber is rayon fiber.

[0043] In the above-mentioned spunlace nonwoven fabric, the synthetic fiber is polyethylene terephthalate fiber, and the water-retaining fiber is rayon fiber. The use of polyethylene terephthalate fiber as the synthetic fiber makes the spunlace nonwoven fabric easy to manufacture. Furthermore, when used in absorbent articles, the spunlace nonwoven fabric excels in top sheet durability, water retention, versatility, and homogeneity.

[0044] [Aspect 11] A spunlace nonwoven fabric according to any one of aspects 1A, 1B, 2A, 2B, 2C and 3 to 10, wherein at least one of the synthetic fibers and the water-retaining fibers is not bonded.

[0045] In the above-described spunlace nonwoven fabric, at least one of the synthetic fibers and the water-retaining fibers is not bonded. Therefore, when the above-described spunlace nonwoven fabric is used in an absorbent article, the top sheet is more permeable to liquid bodily fluids and a portion of viscous bodily fluids compared to a nonwoven fabric in which at least one of the synthetic fibers and the water-retaining fibers is bonded with an adhesive. Furthermore, when the bodily fluid is a viscous bodily fluid containing solid components, when the above-described spunlace nonwoven fabric is used in an absorbent article, the top sheet (especially the skin-side layer) is less likely to clog when the skin-side layer, which has a predetermined entanglement structure, draws in moisture from the viscous bodily fluid that has reached the skin-contact surface. As a result, the non-skin-side layer, which has a predetermined entanglement structure, can continue to draw in moisture from the bodily fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the layer adjacent to the non-skin-side layer (e.g., the absorbent). Consequently, the viscous bodily fluid containing solid components has a higher solid content concentration, making it less likely to adhere to the wearer's skin.

[0046] [Aspect 12] The spunlace nonwoven fabric is the spunlace nonwoven fabric according to any one of aspects 1A, 1B, 2A, 2B, 2C and 3 to 11, wherein the spunlace nonwoven fabric is not heat-sealed or bonded.

[0047] The spunlace nonwoven fabric described above is not heat-sealed. Therefore, when used in absorbent articles, the spunlace nonwoven fabric allows the top sheet to permeate liquid fluids and a portion of viscous fluids more easily than nonwoven fabrics with heat sealing and / or adhesion. Furthermore, when the fluid is a viscous fluid containing solid components, when the spunlace nonwoven fabric is used in absorbent articles, the top sheet (especially the skin-side layer) is less likely to clog when the skin-side layer, which has a predetermined entanglement structure, draws in moisture from the viscous fluid that has reached the skin-contact surface. As a result, the non-skin-side layer, which also has a predetermined entanglement structure, can continue to draw in moisture from the fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the adjacent layer (e.g., the absorbent material). Consequently, the viscous fluid containing solid components has a higher solid content concentration, making it less likely to adhere to the wearer's skin.

[0048] [Aspect 13] The absorbent article is an absorbent article for absorbing loose stool or menstrual blood, and is a spunlace nonwoven fabric as described in any one of aspects 1A, 1B, 2A, 2B, 2C and 3 to 12.

[0049] The spunlace nonwoven fabric described above is for use as a top sheet in absorbent articles for absorbing loose stools or menstrual blood. In other words, the spunlace nonwoven fabric described above is for use as a top sheet in absorbent articles for absorbing viscous bodily fluids containing solid components. Generally, loose stools contain solid components such as undigested dietary fiber, undigested protein, and shed intestinal mucosa, and menstrual blood contains solid components such as the endometrium, so top sheets tend to clog easily. In contrast, the spunlace nonwoven fabric described above has the structure described in Embodiment 1, and when used in absorbent articles, it is less likely to clog even when absorbing viscous bodily fluids containing solid components. As a result, the spunlace nonwoven fabric can increase the solid content concentration of viscous bodily fluids containing solid components, making it less likely for viscous bodily fluids containing solid components to adhere to the wearer's skin, and can also exhibit viscous bodily fluid retention properties that retain the viscous bodily fluids in the spunlace nonwoven fabric.

[0050] The spunlace nonwoven fabric for top sheets of absorbent articles (hereinafter sometimes simply referred to as "spunlace nonwoven fabric") described herein will be explained in detail below. The spunlace nonwoven fabric relating to this disclosure is for use as a top sheet of absorbent articles. The spunlace nonwoven fabric refers to a nonwoven fabric manufactured by the spunlace method.

[0051] The absorbent article described above is not particularly limited as long as it absorbs bodily fluids and has a liquid-permeable top sheet. The bodily fluid is not particularly limited and includes urine, feces (e.g., loose stools), menstrual blood, vaginal discharge, breast milk, blood, exudate, etc. From the viewpoint of the effects of this disclosure, the bodily fluid is preferably a viscous bodily fluid, and more preferably a viscous bodily fluid containing solid components. Examples of the viscous bodily fluid include loose stools, menstrual blood, vaginal discharge, exudate, etc. Examples of viscous bodily fluids containing solid components include loose stools containing undigested dietary fiber, undigested protein, shed intestinal mucosa, etc., and menstrual blood containing endometrium, etc.

[0052] Examples of absorbent articles include diapers (e.g., disposable diapers, e.g., adult disposable diapers, baby disposable diapers), urine pads, incontinence pads, sanitary napkins, panty liners, shorts-type sanitary napkins, absorbent shorts, breast pads, pet sheets, and pressure ulcer pads. Examples of absorbent articles for absorbing the above-mentioned viscous bodily fluids include diapers (e.g., disposable diapers, e.g., adult disposable diapers, baby disposable diapers), sanitary napkins, panty liners, shorts-type sanitary napkins, and pressure ulcer pads. Examples of absorbent articles for absorbing the above-mentioned viscous bodily fluids containing the above-mentioned solid components include diapers (e.g., disposable diapers, e.g., adult disposable diapers, baby disposable diapers), sanitary napkins, shorts-type sanitary napkins, and pressure ulcer pads.

[0053] The absorbent article described above generally comprises a liquid-permeable top sheet, a liquid-impermeable back sheet, and an absorbent core positioned between the top sheet and the back sheet. Furthermore, the absorbent core may be provided in the absorbent article as an absorbent body comprising the absorbent core and a core wrap covering the absorbent core.

[0054] The absorbent article described above may further include, as constituent materials of the absorbent article, a diffusion sheet (second sheet) disposed between the top sheet and the absorbent core (absorbent body), a diffusion sheet (third sheet) disposed between the absorbent core (absorbent body) and the back sheet, etc. The top sheet has a skin-contact surface that comes into contact with the user's skin and a non-skin-contact surface on the opposite side of the skin-contact surface.

[0055] The spunlace nonwoven fabric described above comprises a skin-facing layer containing synthetic fibers that constitutes the skin-contacting surface, and a non-skin-facing layer adjacent to the skin-facing layer containing water-retaining fibers. In the spunlace nonwoven fabric, the synthetic fibers and water-retaining fibers are not heat-fused (hereinafter, the heat-fusion of fibers will be simply referred to as "heat fusion"). That is, although the spunlace nonwoven fabric has entanglement points where the synthetic fibers and water-retaining fibers are entangled by water flow, the synthetic fibers and water-retaining fibers do not have heat-fused points. As a result, the spunlace nonwoven fabric can be said to have a coarser weave compared to a nonwoven fabric having heat-fused points. Consequently, when the spunlace nonwoven fabric is used in an absorbent article, the top sheet is more permeable to liquid fluids and a portion of viscous fluids compared to a nonwoven fabric having heat-fused points. Furthermore, when the bodily fluid is a viscous bodily fluid containing solid components, the spunlace nonwoven fabric, when used in an absorbent article, is less likely to clog the top sheet (especially the skin-side layer) when the skin-side layer, which has a predetermined entanglement structure, draws in moisture from the viscous bodily fluid that has reached the skin-contact surface. As a result, the non-skin-side layer, which also has a predetermined entanglement structure, can continue to draw in moisture from the bodily fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the layer adjacent to the non-skin-side layer (e.g., the absorbent core). Consequently, the viscous bodily fluid containing solid components has a higher solid content concentration, making it less likely to adhere to the wearer's skin. Note that the heat sealing mentioned above refers to the heat sealing during the formation of the spunlace nonwoven fabric, and does not include heat sealing between the spunlace nonwoven fabric and other materials constituting the absorbent article when used in an absorbent article.

[0056] The spunlace nonwoven fabric described above has a maximum elongation of 10-70% in the transport direction during manufacturing, as measured by tensile testing. The maximum elongation is preferably 15% or more, and more preferably 20% or more. Furthermore, the maximum elongation is preferably 60% or less, and more preferably 55% or less. Thus, the spunlace nonwoven fabric has a predetermined degree of entanglement and comprises a skin-side layer having a predetermined entanglement structure and a non-skin-side layer having a predetermined entanglement structure. Therefore, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, for example, when the absorbent article absorbs bodily fluids, it becomes less likely for fibers such as synthetic fibers and water-retaining fibers to detach from the spunlace nonwoven fabric. In this specification, the transport direction during manufacturing is sometimes referred to as the MD direction, and the direction perpendicular to the MD direction during manufacturing is sometimes referred to as the CD direction.

[0057] In this specification, the tensile test described above is carried out as follows: [Tensile Test] (1) Prepare a sample of spunlace nonwoven fabric (length 230 mm x width 25 mm). When measuring the maximum elongation (%) and 5% elongation strength (N / 25 mm) in the MD direction, prepare the sample so that the MD direction is the length direction, and when measuring the maximum elongation (%) and 5% elongation strength (N / 25 mm) in the CD direction, prepare the sample so that the CD direction is the length direction. (2) Mount the sample on a tensile testing machine (Shimadzu Autograph AGS-1kNG) with a gripping distance of 100 mm, and apply a load at a tensile speed of 100 mm / min until the sample is cut, and measure the 5% elongation strength (N / 25 mm) and the maximum elongation (%). The measurement is carried out at 25°C ± 2°C.

[0058] (3) The strength at 5% elongation (N / 25mm) and the maximum elongation (%) shall be measured on 10 different samples, and the average value shall be adopted. For conditions not specified above for the above tensile test, the "6.3 Tensile strength and elongation (ISO method)" of JIS L 1913:2010 shall be followed. Note that the strength at n% elongation (N / 25mm) means the tensile strength (N) per 25 mm width when the sample is elongated by n%. Also, the maximum elongation (%) means the elongation (%) when the tensile strength reaches its maximum value.

[0059] The spunlace nonwoven fabric described above has a surface flow distance of 110 mm or less, preferably 107 mm or less, more preferably 96 mm or less, even more preferably 80 mm or less, and even more preferably 75 mm or less in a 45° inclined artificial urine absorption test. Furthermore, the spunlace nonwoven fabric has a surface flow distance of preferably 34 mm or more, and more preferably 46 mm or more, in a 45° inclined artificial urine absorption test. As a result, when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, it exhibits excellent liquid fluid absorption and viscous fluid retention. In addition, because the surface flow distance is within the preferred range, liquid fluid leakage is less likely to occur in tape-type disposable diapers for babies from size S to younger months. Note that 110 mm corresponds to the distance from the urinary opening of a male baby to the ventral end of the product in a size S tape-type disposable diaper for babies, and 96 mm corresponds to the distance from the urinary opening of a male baby to the ventral end of the product in a size NB disposable diaper for babies.

[0060] In this specification, the 45° inclined artificial urine absorption test described above is carried out as follows: [45° inclined artificial urine absorption test] (1) In a constant temperature and humidity chamber with a temperature of 23°C ± 2°C and a relative humidity of 50 ± 5% RH, a rigid PVC sheet (length: 450 mm × width: 230 mm × thickness: 5 mm) is placed on the table surface of a table having a horizontal table surface, such that the angle formed by the length direction of the rigid PVC sheet and the table surface is 45°. (2) A sample of spunlace nonwoven fabric (length: 250 mm × width: 67 mm) is prepared. The sample is prepared so that the MD direction is the length direction and the CD direction is the width direction.

[0061] (3) Place the sample on the rigid PVC board in the following manner: (i) the longitudinal direction of the sample aligns with the longitudinal direction of the rigid PVC board, (ii) the center of the sample aligns with the center of the rigid PVC board, (iii) the non-skin side layer of the sample faces the rigid PVC board, and (iv) the longitudinal length of the sample is 254-256 mm (extended by approximately 2% from the original length). While maintaining the stretched state of the sample, secure the edges with cellophane tape or the like. (4) Mark the starting point of an X shape 50 mm from the top of the longitudinal end of the sample and at the center in the width direction using a marker (Zebra, Hi-Mackie (blue)).

[0062] (5) Aspirate 1 mL of artificial urine into a pipette (Gilson Microman E M1000E) equipped with a corresponding tip (capillary & piston CP-1000), and drop 1 mL of artificial urine from a height of 20 ± 3 mm above the starting mark over 0.5 seconds. The artificial urine is prepared by dissolving 200 g of urea, 80 g of sodium chloride, 8 g of magnesium sulfate, 3 g of calcium chloride, and approximately 1 g of the dye Blue No. 1 in 10 L of deionized water. (6) 2.0 seconds after dropping, mark the endpoint with an X at the lowest position of the artificial urine. (7) Measure the longitudinal distance from the starting mark to the endpoint mark. (8) Measure the longitudinal distance a total of 10 times using different samples, and adopt the average value as the surface flow distance.

[0063] The synthetic fibers mentioned above can be any synthetic fibers used in the field of absorbent articles without any particular limitations. Examples of such synthetic fibers include those containing a single component, such as single fibers. Examples of such components include polyolefin polymers, such as polyethylene and polypropylene; polyester polymers, such as terephthalate polymers, such as polyethylene terephthalate (PET), polybutylene terephthalate, and polypentylene terephthalate; polyamide polymers, such as nylon 6 and nylon 6,6; acrylic polymers; polyacrylonitrile polymers; and modified versions thereof. The synthetic fibers are preferably polyethylene terephthalate (PET) fibers. This is due to the ease of manufacturing spunlace nonwoven fabrics due to their high heat resistance and the high durability when used in absorbent articles.

[0064] Preferably, the synthetic fiber contains a durable hydrophilic oil agent, which is a hydrophilic oil agent that has sufficient durability to prevent it from flowing off during spunlace treatment. By containing the durable hydrophilic oil agent, the surface of the synthetic fiber becomes hydrophilic and the surface of the synthetic fiber becomes more likely to maintain its hydrophilic state. As a result, during spunlace treatment, the synthetic fibers become more likely to entangle with each other, with each other, and with each other, and the spunlace nonwoven fabric is more likely to have a skin-side layer with a predetermined entanglement structure and a non-skin-side layer with a predetermined entanglement structure. As a result, when the spunlace nonwoven fabric is used as a top sheet for absorbent articles, it exhibits excellent liquid absorption and viscous fluid retention.

[0065] The above-mentioned durable hydrophilic oil agent is not particularly limited, but examples include polyether esters, ether nonions, polyether-modified silicones, sulfosuccinates, polyoxyethylene amide ethers, alkylimidazoline type cations, polyglycerin polyesters, mixtures of alkyl phosphate ester salts having 10 to 30 carbon atoms with betaine compounds having 10 to 30 carbon atoms, sulfate ester salts, sulfonate salts, etc., or mixed oil agents such as mixtures of alkyl phosphate ester salts and polyether-modified silicones.

[0066] Some of the above synthetic fibers may include an initial hydrophilic oil agent, which is a hydrophilic oil agent that has sufficient durability to flow off during spunlace treatment. Examples of the above initial hydrophilic oil agent include alkyl phosphate ester salts and alkyl phosphate metal salts.

[0067] The above-mentioned synthetic fiber may contain the durable hydrophilic oil by treating the surface of the synthetic fiber with the durable hydrophilic oil, or by kneading the durable hydrophilic oil into the components constituting the synthetic fiber, thereby making the surface of the synthetic fiber hydrophilic. Similarly, the above-mentioned synthetic fiber may contain the initial hydrophilic oil by treating the surface of the synthetic fiber with the initial hydrophilic oil, or by kneading the initial hydrophilic oil into the components constituting the synthetic fiber.

[0068] The above synthetic fibers preferably have an average fiber length of 30 mm or more, more preferably 35 mm or more, and even more preferably 40 mm or more. Alternatively, the above synthetic fibers may have an average fiber length of 60 mm or less, more preferably 57 mm or less, and even more preferably 55 mm or less. This makes it easier for the spunlace nonwoven fabric to have a predetermined degree of entanglement, and while a certain amount of water-retaining fibers in the non-skin-side layer are likely to be present in the skin-side layer, they are less likely to be present in excess on the skin-contacting surface of the skin-side layer.

[0069] The synthetic fibers described above preferably have a fineness of 0.6 dtex or more, more preferably 1.0 dtex or more, and even more preferably 1.4 dtex or more. Alternatively, the synthetic fibers may have a fineness of 3.3 dtex or less, more preferably 2.5 dtex or less, and even more preferably 2.0 dtex or less. This makes it easier for the spunlace nonwoven fabric to have a predetermined degree of entanglement, and while a certain amount of water-retaining fibers in the non-skin-side layer are likely to be present in the skin-side layer, they are less likely to be present in excess on the skin-contacting surface of the skin-side layer.

[0070] In this disclosure, the average fiber length of the fibers is measured according to "A7.1 Measurement of fiber length" in Annex A of JIS L 1015:2010, specifically "A7.1.1 Method A (standard method): Method for measuring the length of individual fibers on a graduated glass plate." This method corresponds to the test method specified in ISO 6989, published in 1981.

[0071] The above-mentioned water-retaining fibers are not particularly limited as long as the fiber itself can retain moisture, and examples include cellulose fibers. Examples of cellulose fibers include natural cellulose fibers, regenerated cellulose fibers, refined cellulose fibers, and semi-synthetic cellulose fibers. Examples of natural cellulose fibers include plant fibers, such as seed hair fibers (e.g., cotton fibers), pulp fibers (e.g., hemp), leaf vein fibers (e.g., Manila hemp), and fruit fibers (e.g., coconut).

[0072] Examples of the cotton fibers mentioned above include cotton fibers from the cotton species *Hirstum* (e.g., Upland cotton), cotton fibers from the cotton species *Barbadense*, cotton fibers from the cotton species *Arboreum*, and cotton fibers from the cotton species *Herbacheum*. Furthermore, these cotton fibers may be organic cotton fibers or pre-organic cotton® fibers. Organic cotton fibers refer to cotton certified by GOTS (Global Organic Textile Standard).

[0073] Examples of the regenerated cellulose fibers mentioned above include rayon, such as viscose rayon obtained from viscose, polynosic and modal, and copper ammonia rayon (also called "cupro") obtained from a copper ammonia salt solution of cellulose.

[0074] Examples of the purified cellulose fibers mentioned above include lyocell, specifically, obtained by dissolving pulp in an aqueous solution of N-methylmorpholine N-oxide to make a spinning stock (dope), and then extruding it into a dilute solution of N-methylmorpholine N-oxide to produce fibers. The purified cellulose is commercially available, for example, as Tencel (trademark). Examples of the semi-synthetic fibers mentioned above include semi-synthetic cellulose, such as acetate fibers, such as triacetate and diacetate.

[0075] The above-mentioned water-retaining fibers are preferably regenerated cellulose fibers, more preferably rayon fibers, and even more preferably rayon fibers that have not been modified with hydroxyl groups. This is because they have high water retention, high versatility, and high homogeneity.

[0076] The above-mentioned water-retaining fibers preferably have an average fiber length of 30 mm or more, more preferably 33 mm or more, and even more preferably 35 mm or more. Furthermore, the above-mentioned water-retaining fibers preferably have an average fiber length of 60 mm or less, more preferably 55 mm or less, and even more preferably 50 mm or less. As a result, the spunlace nonwoven fabric is more likely to have a predetermined degree of entanglement, and the water-retaining fibers in the non-skin-side layer are more likely to be present in a certain amount in the skin-side layer, but are less likely to be present in excess on the skin-contacting surface of the skin-side layer.

[0077] The above water-retaining fibers preferably have a fineness of 0.6 dtex or more, more preferably 1.0 dtex or more, and even more preferably 1.4 dtex or more. Alternatively, the above water-retaining fibers may have a fineness of 3.3 dtex or less, more preferably 2.5 dtex or less, and even more preferably 2.0 dtex or less. This makes it easier for the spunlace nonwoven fabric to have a predetermined degree of entanglement, and while a certain amount of water-retaining fibers in the non-skin-side layer are likely to be present in the skin-side layer, they are less likely to be present in excess on the skin-contacting surface of the skin-side layer.

[0078] The spunlace nonwoven fabric described above contains the synthetic fibers and water-retaining fibers in a mass ratio of preferably 40-80:60-20, more preferably 45-75:55-25, and even more preferably 50-70:50-30, in a total of 100 parts by mass of the synthetic fibers and water-retaining fibers. As a result, the skin-side layer and the non-skin-side layer are able to perform their respective functions more easily, and when the spunlace nonwoven fabric is used as a top sheet for absorbent articles, it exhibits excellent liquid fluid absorption and viscous fluid retention.

[0079] In the spunlace nonwoven fabric described above, the skin-facing layer and the non-skin-facing layer can have any fiber density. For example, the non-skin-facing layer can have a higher or lower fiber density than the skin-facing layer. Preferably, the non-skin-facing layer has a higher fiber density than the skin-facing layer. This makes it easier for the water-retaining fibers with a high fiber density in the non-skin-facing layer to further draw in the moisture from the bodily fluids (e.g., liquid bodily fluids, viscous bodily fluids, etc.) that have reached the skin-contacting surface of the skin-facing layer after the skin-facing layer has drawn in moisture from the bodily fluids.

[0080] The density relationship described above can be achieved, for example, by adjusting the fiber density of the skin-side web forming the skin-side layer and the fiber density of the non-skin-side web forming the non-skin-side layer before manufacturing the spunlace nonwoven fabric, by compressing the webs. The fiber density refers to the density of the fibers constituting each layer (skin-side layer, non-skin-side layer, etc.), and the fiber density in each layer can be visually compared after magnifying each layer with a microscope or the like, as necessary.

[0081] The above spunlace nonwoven fabric is preferably 25 g / m² 2 More preferably 30 g / m 2 The above, and more preferably 35 g / m² 2 It has the above basis weight. Furthermore, the spunlace nonwoven fabric preferably has a basis weight of 70 g / m². 2 More preferably, 65 g / m 2 The following, and more preferably 60 g / m² 2It has the following basis weight. Thereby, the skin-side layer and the non-skin-side layer can easily exhibit their respective functions, and the spunlace nonwoven fabric is excellent in liquid body fluid absorbability and viscous body fluid retention property when used as a top sheet of an absorbent article.

[0082] In the present specification, for the basis weight, 10 samples each having a size of 100 mm × 100 mm are collected, the mass of each sample is measured, and then for each sample, mass (g) / area (m 2 ) is calculated as each basis weight (g / m 2 ), and the average value of the respective basis weights of a total of 10 samples is defined as the basis weight. When it is difficult to collect a sample of the above size, a sample can be collected within a possible range.

[0083] In the spunlace nonwoven fabric described above, it is preferable that at least one of the synthetic fibers and the water-retaining fibers, and more preferably both, are not bonded with an adhesive (hereinafter, when the fibers are bonded with an adhesive, this is simply referred to as "bonding"). As a result, when the spunlace nonwoven fabric is used in an absorbent article, the top sheet is more permeable to liquid fluids and a portion of viscous fluids compared to a nonwoven fabric in which at least one of the synthetic fibers and the water-retaining fibers are bonded with an adhesive. Furthermore, when the bodily fluid is a viscous bodily fluid containing solid components, the spunlace nonwoven fabric, when used in an absorbent article, is less likely to clog the top sheet (especially the skin-side layer) when the skin-side layer, which has a predetermined entanglement structure, draws in moisture from the viscous bodily fluid that has reached the skin-contact surface. As a result, the non-skin-side layer, which also has a predetermined entanglement structure, can continue to draw in moisture from the bodily fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the layer adjacent to the non-skin-side layer (e.g., the absorbent layer). Consequently, the viscous bodily fluid containing solid components has a higher solid content concentration, making it less likely to adhere to the wearer's skin. From a similar viewpoint, it is preferable that the fibers constituting the spunlace (including the synthetic fibers and the water-retaining fibers) in the spunlace nonwoven fabric do not have joint points other than entanglement points where they are entangled with other fibers (for example, heat-sealed points where they are heat-sealed with other fibers, adhesive points where they are bonded with other fibers by adhesive, etc.). Furthermore, the above-mentioned bonding refers to bonding at least one of the synthetic fibers and the water-retaining fibers to each other when forming the spunlace nonwoven fabric, and does not include bonding the spunlace nonwoven fabric to other materials constituting the absorbent article when used in such an article.

[0084] Preferably, the spunlace nonwoven fabric described above does not have heat fusion with synthetic fibers or heat fusion with heat-fusible fibers. Furthermore, preferably, the spunlace nonwoven fabric does not have adhesive properties. As a result, when the spunlace nonwoven fabric is used in an absorbent article, the top sheet is more permeable to liquid fluids and a portion of viscous fluids compared to nonwoven fabrics having heat fusion and / or adhesive properties. Also, when the fluid is a viscous fluid containing solid components, when the spunlace nonwoven fabric is used in an absorbent article, the top sheet (especially the skin-side layer) is less likely to clog when the skin-side layer, which has a predetermined entanglement structure, draws in moisture from the viscous fluid that has reached the skin-contact surface. Therefore, the non-skin-side layer, which has a predetermined entanglement structure, can continue to draw in moisture from the fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the layer adjacent to the non-skin-side layer (e.g., the absorbent). As a result, the viscous liquid containing solid components has a higher concentration of solids, making it less likely to adhere to the wearer's skin. From a similar viewpoint, it is preferable that the spunlace nonwoven fabric does not have any bonding points other than entanglement points where certain fibers constituting the spunlace nonwoven fabric are entangled with other fibers (for example, heat-sealed points where fibers are heat-sealed with other fibers, adhesive points where fibers are bonded with other fibers by an adhesive, etc.).

[0085] The spunlace nonwoven fabric described above has a 5% elongation strength in the MD direction of preferably 1.10 N / 25 mm or more, more preferably 2.00 N / 25 mm or more, and even more preferably 2.50 N / 25 mm or more, in the tensile test described above. Furthermore, the spunlace nonwoven fabric has a 5% elongation strength in the MD direction of preferably 4.25 N / 25 mm or less, more preferably 4.00 N / 25 mm or less, and even more preferably 3.50 N / 25 mm or less, in the tensile test described above. As a result, when the spunlace nonwoven fabric is used in an absorbent article, for example, when the absorbent article absorbs bodily fluids, it becomes less likely for fibers such as synthetic fibers and water-retaining fibers to come out of the spunlace nonwoven fabric. Note that the 5% elongation strength has already been explained in the "Tensile Test" section described above.

[0086] The spunlace nonwoven fabric described above preferably has a Klem water absorption of 30 mm or more, more preferably 80 mm or more, and even more preferably 110 mm or more. Furthermore, the spunlace nonwoven fabric preferably has a Klem water absorption of 170 mm or less, and more preferably 150 mm or less. As a result, when the spunlace nonwoven fabric is used in an absorbent article, it facilitates the diffusion of bodily fluids in the planar and thickness directions. Therefore, when the spunlace nonwoven fabric is used as a top sheet in an absorbent article, it exhibits excellent liquid bodily fluid absorption and viscous bodily fluid retention.

[0087] In this specification, the above-mentioned Klem water absorption is measured in accordance with JIS P8141:2004 "Paper and cardboard - Water absorption test method - Klem method," and the differences from JIS P8141:2004 are as follows: - The dimensions of the test specimen are changed from "length 200 mm or more" to "length 230 mm ± 1 mm" and from "width 15 ± 1 mm" to "width 25 ± 1 mm." - The test specimen is oriented with the MD direction as the longitudinal direction. - The time taken to read the height of the water rise is changed from "10 minutes ± 10 seconds" to "5 minutes ± 10 seconds."

[0088] The above spunlace nonwoven fabric has a rewetting rate of preferably 20.0% by mass or less, more preferably 15.0% by mass or less, even more preferably 10.0% by mass or less, even more preferably 8.0% by mass or less, and even more preferably 6.0% by mass or less in a rewetting test. This means that the skin-side layer of the spunlace nonwoven fabric has a predetermined entanglement structure and contains a predetermined ratio of synthetic fibers and water-retaining fibers. As a result, the spunlace nonwoven fabric exhibits excellent rewetting properties when used in absorbent articles. The lower limit of the above rewetting rate is not particularly limited, but for example, 1.0% by mass is one example.

[0089] In this specification, the rewet test is measured as follows: [Rewet Test] (1) Prepare a nonwoven fabric sample (length: 200 mm x width: 110 mm), a cylinder (inner diameter: 60 mm, height: 50 mm), filter paper (ADVANTEC, Item2, Quality 1000, size: 100 x 100 mm), a burette (capable of dropping 80 mL / 10 seconds), and a weight (3.5 kg, size of base (square): 100 mm x 100 mm) in a constant temperature and humidity chamber with a temperature of 23 °C ± 2 °C and a relative humidity of 50 ± 5% RH. The sample is prepared so that the MD direction is the length direction. (2) Place 10 sheets of the above-mentioned filter paper, which mimics an absorbent material, on a plastic tray, and place the above-mentioned sample on top of the 10 sheets of filter paper so that the non-skin side layer is in contact with the filter paper, thereby forming a simulated absorbent article with the above-mentioned sample as the top sheet.

[0090] (3) Place the cylinder on top of the sample of the simulated absorbent material so that the center of the sample and the center of the cylinder coincide. Drop 10 mL of artificial urine onto the center of the cylinder using a burette at a rate of 80 mL / 10 seconds. The composition of the artificial urine is the same as that used in the "45° Inclined Artificial Urine Absorption Test". (4) After dropping the artificial urine, remove the cylinder once the artificial urine has been completely removed. 60 seconds after dropping the artificial urine, place approximately 50 g of the filter paper, whose initial mass: m0 (g) has been measured in advance, onto the spot where the artificial urine was dropped, so that the center of the filter paper coincides with the center of the sample. Place the weight on top of the filter paper so that the center of the weight coincides with the center of the sample.

[0091] (5) 120 seconds after placing the weight, remove the weight and approximately 50 g of the filter paper, measure the post-test mass of the approximately 50 g of filter paper: m1 (g), and calculate the rewetting rate: R (mass%) using the following formula: R (mass%) = 100 × (m1 - m0) / 10. (6) Measure the rewetting rate: R (mass%) a total of five times using different samples and new filter paper, and adopt the average value.

[0092] The spunlace nonwoven fabric described above may consist of two layers, including the skin-side layer and the non-skin-side layer, and may further include an additional layer positioned on the non-skin side of the non-skin-side layer. Examples of the additional layer include those containing cellulose acetate fibers and the water-retaining fibers described above.

[0093] The spunlace nonwoven fabric according to this disclosure can be manufactured by a spunlace method known in the art. The spunlace nonwoven fabric according to this disclosure can be manufactured by a spunlace method including, for example, the following steps: - A skin-side web preparation step (hereinafter referred to as the "skin-side web preparation step") to prepare a skin-side web constituting the skin-side layer, which includes synthetic fibers. - A non-skin-side web preparation step (hereinafter referred to as the "non-skin-side web preparation step") to prepare a non-skin-side web constituting the non-skin-side layer, which includes water-retaining fibers. - A laminated web forming step (hereinafter referred to as the "laminated web forming step") to laminate the skin-side web and the non-skin-side web to form a laminated web. - A water-entanglement treatment step (hereinafter referred to as the "water-entanglement treatment step") to treat the laminated web with water-entanglement to form a water-entangled spunlace nonwoven fabric. - A drying step (hereinafter referred to as the "drying step") to dry the water-entangled spunlace nonwoven fabric.

[0094] In the above skin-side layer web preparation step, a skin-side layer web constituting the skin-side layer, including synthetic fibers, is prepared. In the above skin-side layer web preparation step, for example, a carding machine can be used to mechanically open the synthetic fibers constituting the skin-side layer and prepare the skin-side layer web. In the above skin-side layer web preparation step, it is preferable that the synthetic fibers included in the skin-side layer web include a durable hydrophilic oil agent. The reason for this will be explained later. The carding machine is well known in the art, so its explanation will be omitted. The above skin-side layer web may contain not only the above synthetic fibers but also the above water-retaining fibers in advance. In that case, from the viewpoint of obtaining the effects according to Embodiment 1, the above skin-side layer web preferably contains 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 97% by mass or more, and even more preferably 98% by mass or more of the above synthetic fibers.

[0095] In the above non-skin layer web preparation step, a non-skin layer web constituting the non-skin layer, which includes water-retaining fibers, is prepared. In the above non-skin layer web preparation step, for example, a carding machine can be used to mechanically open the water-retaining fibers constituting the non-skin layer and prepare the non-skin layer web. The above carding machine is known in the art, so its description is omitted. The above skin layer web may contain not only the above water-retaining fibers but also the above synthetic fibers in advance. In that case, the above non-skin layer web preferably contains 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 97% by mass or more, and even more preferably 98% by mass or more of the above water-retaining fibers.

[0096] In the above-described laminated web formation step, the skin-side layer web and the non-skin-side layer web are laminated to form a laminated web.

[0097] In the above water flow entanglement treatment step, the laminated web is subjected to water flow entanglement to form a water flow entangled spunlace nonwoven fabric. The above water flow entanglement treatment can be carried out according to methods known in the art. The above water flow entanglement treatment may be carried out, for example, with a transport speed of 5 to 20 m / min and a water flow rate of 0.05 to 0.2 m per unit time. 3 This can be carried out under conditions such as flow rate / minute, water flow pressure: 5-20 MPa (skin-side web and non-skin-side web), nozzle diameter: 80-120 μm, nozzle pitch: 0.5-2 mm, and nozzle rows: 2-4 rows.

[0098] The above-described water flow entanglement treatment can be performed, for example, by placing the laminated web on a support and, while conveying the laminated web, spraying a water flow from a nozzle onto the laminated web to entangle it. The water flow can be sprayed onto one side (single side) or both sides (double side) of the skin-side layer web and the non-skin-side layer web. That is, in the spunlace nonwoven fabric according to this disclosure, one or both sides of the skin-contacting surface of the skin-side layer and the non-skin-side surface of the non-skin-side layer may be water flow entangled surfaces.

[0099] When a stream of water is sprayed from the nozzle onto only one side of the non-skin layer web of the laminated web, a portion of the water stream passes from the non-skin layer web (non-skin layer) through the skin layer web (skin layer) to the support side, while the remainder of the water stream bounces back towards the nozzle. At that time, a portion of the water stream pushes the water-retaining fibers in the non-skin layer web into the skin layer web, forming a skin layer with a predetermined entanglement structure. Also, when the remainder of the water stream bounces back towards the nozzle, it pushes the synthetic fibers in the skin layer web back to the non-skin layer web, forming a non-skin layer with a predetermined entanglement structure. Furthermore, if the synthetic fibers in the skin layer web contain a durable hydrophilic oil, the water stream easily adheres to the skin layer web, and the water stream that reaches the skin layer web easily escapes to the support side, making it easier for synthetic fibers to entangle with each other, water-retaining fibers to entangle with each other, and synthetic fibers and water-retaining fibers to entangle with each other. As a result, when the above-mentioned spunlace nonwoven fabric is used as a top sheet for absorbent articles, it exhibits excellent liquid absorption and viscous fluid retention properties.

[0100] When a stream of water is sprayed from a nozzle onto only one side of the skin-side layer web of the laminated web, a portion of the water stream passes from the skin-side layer web (skin-side layer) through the non-skin-side layer web (non-skin-side layer) to the support side, while the remainder of the water stream bounces back towards the nozzle. At this time, a portion of the water stream can push the synthetic fibers in the skin-side layer web into the non-skin-side layer web, forming a non-skin-side layer with a predetermined entanglement structure. Also, when the remainder of the water stream bounces back towards the nozzle, it can push the water-retaining fibers in the non-skin-side layer web back to the skin-side layer web, forming a skin-side layer with a predetermined entanglement structure. Furthermore, if the synthetic fibers in the skin-side layer web contain a durable hydrophilic oil, the water stream will easily adhere to the skin-side layer web, and the water stream that reaches the skin-side layer web will easily pass through the non-skin-side layer web to the support side, making it easier for synthetic fibers to entangle with each other, water-retaining fibers to entangle with each other, and synthetic fibers and water-retaining fibers to entangle with each other. As a result, when the above-mentioned spunlace nonwoven fabric is used as a top sheet for absorbent articles, it exhibits excellent liquid absorption and viscous fluid retention properties.

[0101] The same applies when a stream of water is sprayed from the nozzle onto both the skin-side web and the non-skin-side web of the laminated web. In this specification, it is preferable that in the water entanglement treatment step, a stream of water is sprayed from the nozzle onto only one side of the non-skin-side web of the laminated web. This makes it easier to form a spunlace nonwoven fabric in which the water-retaining fibers in the non-skin-side layer are appropriately interwoven with the synthetic fibers in the skin-side layer, and when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, it exhibits excellent liquid absorption and viscous liquid retention.

[0102] In the drying step described above, the spunlace nonwoven fabric that has been entangled with water is dried. The drying step can be carried out at a predetermined temperature for a predetermined time. The predetermined temperature is preferably a temperature that allows the moisture to evaporate but does not cause the synthetic fibers to heat-fuse together, for example, 100 to 150°C. The predetermined time is, for example, 3 to 8 seconds.

[0103] Furthermore, the above-mentioned spunlace nonwoven fabric can also be manufactured by combining a web-like fiber sheet that constitutes the skin-facing layer with a web-like fiber sheet that constitutes the non-skin-facing layer, resulting in a two-layer structure.

[0104] The present disclosure will be explained below with examples, but the present disclosure is not limited to these examples. [Manufacturing Example 1] Laminated web No. 1 with the following composition was prepared. In laminated web No. 1, skin-side layer web No. 1 and non-skin-side layer web No. 1 were laminated in that order. [Skin-side layer web] Using a carding machine, skin-side layer web No. 1 (basis weight: 15 g / m²) containing 100% by mass of polyethylene terephthalate (PET) fiber as a synthetic fiber (single fiber, synthetic fiber surface coated with a durable hydrophilic oil agent, average fiber length: 51 mm, fineness: 1.6 dtex, hereinafter referred to as "durable hydrophilic PET fiber") was prepared. 2 I prepared (this).

[0105] [Non-skin side layer web] Using a carding machine, a non-skin side layer web No. 1 (basis weight: 15 g / m²) containing 100% by mass of rayon fibers (average fiber length: 40 mm, fineness: 1.7 dtex, hereinafter referred to as "rayon fibers") as water-retaining fibers was produced. 2 I prepared (this).

[0106] Nonwoven fabric No. 1 (spunlace nonwoven fabric, SL) was formed by performing a water jet entanglement treatment step and a drying step on laminated web No. 1. In the water jet entanglement step, while conveying laminated web No. 1, water jet treatment was performed from the non-skin side of the laminated web No. 1, and then from the skin side of the laminated web No. 1. Figure 1 shows a cross-sectional photograph (magnification: 40x) of the nonwoven fabric No. 1 in which rayon fibers were colored with Congo Red. In Figure 1, the upper part is the skin side layer and the lower part is the non-skin side layer. From Figure 1, it can be seen that the skin side layer has a predetermined entanglement structure.

[0107] [Manufacturing Example 2] Using a carding machine, a skin-side web No. 2 (basis weight: 15 g / m²) is produced containing 60% by mass of the above-mentioned durable hydrophilic PET fiber and 40% by mass of polyethylene terephthalate (PET) fiber as a synthetic fiber (single fiber, synthetic fiber surface coated with an initial hydrophilic oil agent, average fiber length: 51 mm, hereinafter referred to as "initial hydrophilic PET fiber") 2 A laminated web No. 2 and nonwoven fabric No. 2 (spunlace nonwoven fabric, SL) were formed in the same manner as in Manufacturing Example 1, except that skin-side layer web No. 1 was changed to skin-side layer web No. 2.

[0108] [Manufacturing Example 3] Using a carding machine, a skin-side layer web No. 3 (basis weight: 15 g / m²) containing 100% by mass of the initial hydrophilic PET was produced. 2 A laminated web No. 3 and nonwoven fabric No. 3 (spunlace nonwoven fabric, SL) were formed in the same manner as in Manufacturing Example 1, except that skin-side layer web No. 1 was changed to skin-side layer web No. 3.

[0109] [Manufacturing Example 4] Using a carding machine, a non-skin side layer web No. 4 (basis weight: 30 g / m²) containing 100% by mass of the above rayon fibers is produced. 2 A laminated web No. 4 and nonwoven fabric No. 4 (spunlace nonwoven fabric, SL) were formed in the same manner as in Manufacturing Example 1, except that the skin-side web No. 1 was not used and the non-skin-side web No. 1 was changed to the non-skin-side web No. 4.

[0110] [Manufacturing Example 5] Using a carding machine, a skin-side layer web No. 5 (basis weight: 9 g / m²) containing 100% by mass of the initial hydrophilic PET was produced. 2 A carding machine was used to create a non-skin side layer web No. 5 (basis weight: 21 g / m²) containing 100% by mass of the above rayon fibers. 2 A laminated web No. 5 and nonwoven fabric No. 5 (spunlace nonwoven fabric, SL) were formed in the same manner as in Manufacturing Example 1, except that the skin-side web No. 1 was changed to skin-side web No. 5 and the non-skin-side web No. 1 was changed to non-skin-side web No. 5.

[0111] [Manufacturing Example 6] Using a carding machine, a skin-side layer web No. 6 (basis weight: 21 g / m²) containing 100% by mass of the initial hydrophilic PET was produced.2 A non-skin side layer web No. 6 (basis weight: 9 g / m²) containing 100% by mass of the above rayon fibers was prepared using a carding machine. 2 A laminated web No. 6 and nonwoven fabric No. 6 (spunlace nonwoven fabric, SL) were formed in the same manner as in Manufacturing Example 1, except that the skin-side web No. 1 was changed to skin-side web No. 6 and the non-skin-side web No. 1 was changed to non-skin-side web No. 6.

[0112] [Manufacturing Example 7] Using a carding machine, a skin-side layer web No. 7 (basis weight: 30 g / m²) containing 100% by mass of the initial hydrophilic PET was produced. 2 A laminated web No. 7 and nonwoven fabric No. 7 (spunlace nonwoven fabric, SL) were formed in the same manner as in Manufacturing Example 1, except that the skin-side layer web No. 1 was changed to skin-side layer web No. 7 and the non-skin-side layer web No. 1 was not used.

[0113] [Production Example 8] Air-through nonwoven fabric (AT) (Basic weight: 30 g / m 2 A core-sheath fiber coated with a durable hydrophilic oil agent (core: polyester, sheath: polyethylene) was prepared and designated as nonwoven fabric No. 8.

[0114] [Example 1] The artificial soft stool adhesion test specified below was performed on nonwoven fabrics No. 1 to No. 8. The results are shown in Table 1. In Table 1, "Durability / Initial" represents the mass ratio of durable hydrophilic PET fibers to initial hydrophilic PET fibers. [Artificial Soft Stool Adhesion Test] (1) Prepare artificial leather (manufactured by Ideatex Japan, PBZ13001, size: 100 mm x 100 mm), an acrylic plate (size: 100 mm x 100 mm), and a weight (mass: 2 kg, size of base (square): 100 mm x 100 mm) as a weight. The mass of the artificial leather before the test: m2 (g) was measured.

[0115] (2) Mix 80.0 parts by mass of deionized water, 0.7 parts by mass of sodium chloride, 10.7 parts by mass of glycerin, 1.4 parts by mass of CMC sodium, 0.04 parts by mass of Triton X-100, 0.01 parts by mass of Red No. 102, and 7.1 parts by mass of powdered cellulose to prepare a simulated soft stool. Dilute the prepared simulated soft stool with deionized water to adjust its viscosity to 400 mPa·s. The viscosity is measured using a TVB10 viscometer (manufactured by Toki Sangyo Co., Ltd.). (3) Peel off the top sheet of a commercially available Moony Natural newborn diaper, place a nonwoven fabric as a top sheet on top to create a simple absorbent item, and attach the simple absorbent item in an unfolded state to a hook tape board (a 500 mm x 300 mm cardboard with hook-and-loop fasteners attached to the entire surface, capable of securing the nonwoven fabric).

[0116] (4) Using a Terumo syringe 50 mL (without needle, side opening) manufactured by Terumo Corporation, draw up 5.0 mL of simulated soft stool and drop it onto the top sheet at a dropping point located 20 cm behind the longitudinal center and width center of the simple absorbent material. Three seconds after dropping, place the artificial skin, acrylic plate, and weight on the dropping point in that order. The artificial skin, acrylic plate, and weight should be placed so that their centers coincide with the dropping point. (5) One minute after placing the weight, remove the weight, acrylic plate, and artificial skin from the simple absorbent material, measure the post-test mass of the artificial skin: m3 (g), and calculate the amount of soft stool attached to the artificial skin: A (g) from the following formula: A (g) = m3 - m2. (6) The amount of loose stool attached: A (g) was measured a total of 10 times using different simple absorbent materials and new artificial skin, and the average value was adopted.

[0117]

[0118] Table 1 shows that nonwoven fabrics No. 1 to No. 4, which are spunlace nonwoven fabrics, exhibit less loose stool adhesion and superior resistance to loose stool adhesion compared to nonwoven fabric No. 8, which is an air-through nonwoven fabric. Furthermore, a comparison of nonwoven fabrics No. 1 to No. 3 shows that the superior resistance to loose stool adhesion is maintained even when the ratio of durable water-resistant PET and initial hydrophilic PET changes. Additionally, a comparison of nonwoven fabrics No. 1 and No. 4 to No. 7 shows that resistance to loose stool adhesion deteriorates as the proportion of the non-skin side layer decreases.

[0119] [Manufacturing Example 9] Laminated web No. 9 with the following composition was prepared. In laminated web No. 9, the skin-side layer web No. 9 and the non-skin-side layer web No. 9 were laminated in that order. [Skin-side layer web] Using a carding machine, skin-side layer web No. 9 (basis weight: 15 g / m²) containing 80% by mass of the above durable hydrophilic PET fiber and 20% by mass of the above initial hydrophilic PET fiber was prepared. 2 I prepared (this).

[0120] [Non-skin layer web] Using a carding machine, a non-skin layer web No. 9 containing 100% by mass of the above rayon fibers (basis weight: 15 g / m²) is produced. 2 I prepared (this).

[0121] Laminated web No. 9 and nonwoven fabric No. 9 (SL) were formed by performing a water entanglement treatment step and a drying step on laminated web No. 9 under the same conditions as in manufacturing example 1.

[0122] [Manufacturing Example 10] Using a carding machine, a skin-side layer web No. 10 (basis weight: 15 g / m²) containing 60% by mass of the durable hydrophilic PET fiber and 40% by mass of the initial hydrophilic PET fiber was produced. 2 A laminated web No. 10 and nonwoven fabric No. 10 (SL) were formed in the same manner as in manufacturing example 9, except that skin-side layer web No. 9 was changed to skin-side layer web No. 10.

[0123] [Example 2] Nonwoven fabrics No. 1, No. 3 to No. 7, No. 9 and No. 10 were subjected to a 45° inclined artificial urine absorption test. The results are shown in Table 2. In Table 2, "Durability / Initial" represents the mass ratio of durable hydrophilic PET fibers to initial hydrophilic PET fibers. For nonwoven fabrics No. 1, No. 9 and No. 10, the maximum elongation (%) in the MD direction and the maximum elongation (%) in the CD direction were measured. The results are shown in Table 2. For nonwoven fabrics No. 3 to No. 5, the strength at 5% elongation in the MD direction and the Klem water absorption were measured. The results are shown in Table 2.

[0124]

[0125] Table 2 shows that nonwoven fabric No. 1 containing 100% by mass of durable hydrophilic PET fibers as synthetic fibers, and nonwoven fabric No. 9 containing 80% by mass of durable hydrophilic PET fibers as synthetic fibers, have shorter surface flow distances compared to nonwoven fabric No. 10 containing 60% by mass of durable hydrophilic PET fibers as synthetic fibers, and also compared to nonwoven fabrics No. 3, No. 4, No. 6, and No. 7 containing 100% of initial hydrophilic PET fibers as synthetic fibers. A comparison of nonwoven fabrics No. 1 to No. 3 shows that as the proportion of durable hydrophilic PET fibers as synthetic fibers increases, the maximum elongation of the nonwoven fabric increases, and the strength of the nonwoven fabric increases.

[0126] [Example 3] A rewetting test was performed on nonwoven fabrics No. 1, No. 4 to No. 8. The results are shown in Table 3.

[0127]

[0128] Table 3 shows that the rewetting properties are excellent because the mass ratio of PET fibers as synthetic fibers to rayon fibers as water-retaining fibers is within a specified range. Regarding the rewetting test, it is considered that there is no difference in results between durable hydrophilic PET fibers and initially hydrophilic PET fibers.

Claims

1. A spunlace nonwoven fabric for a top sheet of an absorbent article, wherein the spunlace nonwoven fabric comprises a skin-facing layer containing synthetic fibers that constitutes the skin-contacting surface, and a non-skin-facing layer adjacent to the skin-facing layer containing water-retaining fibers, wherein the synthetic fibers and the water-retaining fibers are not heat-fused, the spunlace nonwoven fabric has a maximum elongation of 10-70% in the transport direction during manufacturing in a tensile test, and the spunlace nonwoven fabric has a surface flow distance of 110 mm or less in a 45° inclined artificial urine absorption test.

2. The spunlace nonwoven fabric according to claim 1, wherein the spunlace nonwoven fabric has a Klem water absorption of 30 to 170 mm.

3. The spunlace nonwoven fabric according to claim 1 or 2, wherein the spunlace nonwoven fabric has a rewetting rate of 20% by mass or less in a rewetting test.

4. The spunlace nonwoven fabric according to any one of claims 1 to 3, wherein the spunlace nonwoven fabric has a tensile strength of 1.10 to 4.25 N / 25 mm in the transport direction during manufacturing, as determined in the tensile test.

5. The spunlace nonwoven fabric according to any one of claims 1 to 4, wherein the spunlace nonwoven fabric contains the synthetic fiber and the water-retaining fiber in a mass ratio of 40 to 80:60 to 20 in a total of 100 parts by mass of the synthetic fiber and the water-retaining fiber.

6. The spunlace nonwoven fabric has a density of 25 to 70 g / m². 2 A spunlace nonwoven fabric according to claim 5, having the basis weight.

7. The spunlace nonwoven fabric according to any one of claims 1 to 6, wherein the synthetic fibers have an average fiber length of 30 to 60 mm, and the water-retaining fibers have an average fiber length of 30 to 60 mm.

8. The spunlace nonwoven fabric according to any one of claims 1 to 7, wherein the non-skin-facing layer has a higher fiber density than the skin-facing layer.

9. The spunlace nonwoven fabric according to any one of claims 1 to 8, wherein the synthetic fiber comprises a durable hydrophilic oil agent.

10. The spunlace nonwoven fabric according to any one of claims 1 to 9, wherein the synthetic fiber is polyethylene terephthalate fiber and the water-retaining fiber is rayon fiber.

11. The spunlace nonwoven fabric according to any one of claims 1 to 10, wherein at least one of the synthetic fibers and the water-retaining fibers is not bonded.

12. The spunlace nonwoven fabric according to any one of claims 1 to 11, wherein the spunlace nonwoven fabric is not heat-sealed or bonded.