Resin composition
A modified EVOH resin composition with Zn(OH)(CH₃CO₂)₂·2H₂O compound addresses the issue of insufficient gas barrier and solution stability in EVOH films under high humidity, providing enhanced performance for packaging materials.
Patent Information
- Application Number
- PCT/JP2026/017497
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
Existing ethylene-vinyl alcohol copolymer (EVOH) films exhibit insufficient gas barrier properties and solution stability under high humidity conditions.
A resin composition combining a modified EVOH resin with a specific structural unit and Zn(OH)(CH₃CO₂)₂·2H₂O compound, with controlled content and proportions, to enhance both solution stability and gas barrier properties.
The resin composition achieves excellent solution stability and superior gas barrier properties under high humidity conditions, suitable for various packaging applications.
Smart Images

Figure JP2026017497_12112026_PF_FP_ABST
Abstract
Description
resin composition
[0001] The present invention relates to a resin composition, and more particularly to a resin composition that exhibits excellent solution stability and excellent gas barrier properties under high humidity conditions when formed into a film.
[0002] Films obtained from ethylene-vinyl alcohol copolymers (sometimes referred to as "EVOH resins") exhibit excellent transparency and gas barrier properties such as oxygen, making them useful as various packaging materials for food, medical products, industrial chemicals, etc., or as composite materials laminated with plastic films, paper, or metal foils.
[0003] Furthermore, while any method can be used to form an EVOH resin coating, solution coating methods, which involve applying a solution of EVOH resin dissolved in a solvent or an aqueous dispersion of EVOH resin dispersed in water to a substrate, are attracting attention because they allow for the formation of relatively thin films, easy coating of substrates with complex shapes such as hollow containers, and relatively simple equipment for the coating operation.
[0004] For example, Patent Document 1 discloses a coating agent containing inorganic fine particles in a modified EVOH resin solution. Patent Document 2 also discloses a resin composition in which a Zn-containing layered compound is added to an EVOH resin.
[0005] Japanese Patent Publication No. 2024-127188, International Publication No. 2021 / 029353
[0006] Although the technology disclosed in Patent Document 1 can provide a multilayer structure including an EVOH resin layer with improved gas barrier properties, it was found that the gas barrier properties under high humidity conditions are insufficient, and the storage stability of the coating solution is also insufficient. Furthermore, although the technology disclosed in Patent Document 2 improves gas barrier properties under high humidity conditions, it was found that the solution stability is insufficient.
[0007] Therefore, against this background, the present invention provides a resin composition that exhibits excellent solution stability while also having excellent gas barrier properties under high humidity conditions when formed into a film.
[0008] In light of these circumstances, the inventors conducted extensive research and found that by combining a specific metal compound with a modified EVOH resin having a specific structural unit, it is possible to achieve excellent solution stability while also exhibiting excellent gas barrier properties under high humidity conditions when made into a film.
[0009] In other words, the present invention has the following aspects: [1] Modified ethylene-vinyl alcohol copolymer and Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 A resin composition containing O, wherein the modified ethylene-vinyl alcohol copolymer has at least one structural unit of the following formulas (1) and (2), and the content of the structural unit is 0.1 mol% or more and less than 3.0 mol%. [2] The resin composition according to [1], wherein the modified ethylene-vinyl alcohol copolymer has the structural unit of formula (1) or (2). [3] The resin composition according to [1] or [2], wherein the content of the structural unit is 1.0 mol% or more and less than 3.0 mol%. [4] The resin composition according to any one of [1] to [3], wherein the zinc content is 0.1 parts by mass per 100 parts by mass of the modified ethylene-vinyl alcohol copolymer. [5] The resin composition according to any one of [1] to [4], wherein the zinc content is less than 5.0 parts by mass per 100 parts by mass of the modified ethylene-vinyl alcohol copolymer. [6] The resin composition according to any one of [1] to [5], wherein the content of the ethylene structural unit in the modified ethylene-vinyl alcohol copolymer is 20 to 60 mol%. [7] The resin composition according to any one of [1] to [6], wherein the content of the modified ethylene-vinyl alcohol copolymer is 0.1% by mass or more and 50% by mass or less of the entire resin composition. [8] The resin composition according to any one of [1] to [7], wherein the content of the modified ethylene-vinyl alcohol copolymer is 1% by mass or more and less than 20% by mass of the entire resin composition. [9] The resin composition according to any one of [1] to [8], wherein the resin composition contains sodium, and the content of the sodium is more than 0 ppm and 600 ppm or less of the entire resin composition.
[10] The resin composition according to any one of [1] to [9], further comprising water.
[11] The resin composition according to any one of [1] to
[10] , further comprising alcohol.
[12] The resin composition according to any one of [1] to
[11] , wherein the form of the resin composition is a solution.
[13] A molding material comprising the resin composition according to any one of [1] to
[12] .
[14] A molded article comprising the resin composition according to any one of [1] to [9].
[15] A multilayer structure comprising the resin composition according to any one of [1] to [9].
[16] A film comprising the resin composition according to any one of [1] to [9].
[17] A food packaging material comprising the resin composition described in any of [1] to [9].
[18] A medical packaging material comprising the resin composition described in any of [1] to [9].
[19] A method for producing a multilayer structure, comprising coating it with the resin composition described in any of [1] to
[12] .
[0010] This invention offers excellent solution stability while also providing superior gas barrier properties under high humidity conditions when formed into a film.
[0011] This is a front view showing a glass bottle with a screw cap.
[0012] The present invention will be described below based on examples of embodiments for carrying out the present invention. However, the present invention is not limited to the embodiments described below.
[0013] In the present specification, the expression "x and / or y (x and y are arbitrary constituents)" means at least one of x and y, and refers to the three cases of x alone, y alone, and x and y. When expressed as "X to Y" (X and Y are arbitrary numbers), unless otherwise specified, it means "not less than X and not more than Y", and also includes the meanings of "preferably more than X" or "preferably less than Y". When expressed as "not less than X" (X is an arbitrary number) or "not more than Y" (Y is an arbitrary number), it also includes the meaning of "preferably more than X" or "preferably less than Y". Regarding the numerical ranges described stepwise in the present specification, the upper limit or lower limit of the numerical range in a certain step can be arbitrarily combined with the upper limit or lower limit of the numerical range in another step. Further, in the numerical ranges described in the present specification, the upper limit value or lower limit value of the numerical range may be replaced with the values shown in the Examples. In the present specification, a combination of preferred embodiments is a more preferred embodiment. In the present specification, normal temperature, room temperature, and various physical property values and characteristic values are those at 23°C unless otherwise specified. When a measurement method or the like based on a standard is described in the present specification, it is based on the relevant standard as of the filing date of the present application (or the priority date if a priority date exists) unless otherwise specified. If the relevant standard has been abolished at that time, it shall be based on the standard at the time of abolition. In the present specification, "solution stability" refers to the property that gelation hardly occurs, viscosity increase and aggregation over time are suppressed, and a uniform solution state is maintained. In the present specification, "film" has the meaning including relatively thin layers such as "tape" and "sheet" in addition to thick layers.
[0014] <<Resin Composition>> A resin composition according to one embodiment of the present invention (hereinafter sometimes referred to as "the present resin composition") comprises a modified EVOH resin and Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ·2H 2A resin composition containing O, wherein the modified EVOH resin has at least one of the structural units of the following formulas (1) and (2), and the content of the structural unit is 0.1 mol% or more and less than 3.0 mol%. The following is a description of each component.
[0015] <Modified EVOH resin> EVOH resin is a thermoplastic resin obtained by saponifying an ethylene-vinyl ester copolymer, which is typically a copolymer of ethylene and vinyl ester monomers. It mainly consists of ethylene structural units and vinyl alcohol structural units, and usually contains a small amount of vinyl ester structural units that remain unsaponified.
[0016] Furthermore, the modified EVOH resin contained in this resin composition is a modified EVOH resin having at least one of the structural units of the following formulas (1) and (2). Among these, a modified EVOH resin having the structural unit of the following formula (1) or (2) is preferred.
[0017]
[0018]
[0019] To obtain a modified EVOH resin containing the structural units of formula (1) and / or (2), for example, one method involves copolymerizing 2-methylene-1,3-propanediol diacetate and / or 3,4-diacetoxy-1-butene with ethylene and vinyl ester monomers, followed by saponification.
[0020] The following describes the method for producing modified EVOH resin. First, ethylene, vinyl ester monomer, and 2-methylene-1,3-propanediol diacetate and / or 3,4-diacetoxy-1-butene are copolymerized.
[0021] Examples of the vinyl ester monomers include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl versatate, and vinyl trifluoroacetate. These may be used individually or in combination of two or more. Among these, vinyl acetate is preferred from an economic standpoint.
[0022] Furthermore, copolymerizable ethylenically unsaturated monomers may be copolymerized as copolymerization components within a range that does not inhibit the effects of the present invention (for example, 10% by mass or less of the copolymerization components). Examples of such ethylenically unsaturated monomers include olefins such as propylene, 1-butene, and isobutene; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, (anhydride) phthalic acid, (anhydride) maleic acid, (anhydride) itaconic acid, or their salts or mono- or dialkyl esters having 1 to 18 carbon atoms; acrylamide, N-alkylmethacrylamide having 1 to 18 carbon atoms, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid, or their salts; acrylamides such as acrylamidopropyldimethylamine, its acid salts, or its quaternary salts; methacrylamide, having 1 to 18 carbon atoms Examples include methacrylamides such as N-alkylmethacrylamide, N,N-dimethylmethacrylamide, 2-methacrylamidepropanesulfonic acid or salts thereof; N-vinylamides such as N-vinylpyrrolidone, N-vinylformamide, and N-vinylacetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl ethers such as alkyl vinyl ethers, hydroxyalkyl vinyl ethers, and alkoxyalkyl vinyl ethers having 1 to 18 carbon atoms; vinyl halogens such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, and vinyl bromide; and vinylsilanes. These may be used individually or in combination of two or more.
[0023] In these copolymerization reactions, known methods such as bulk polymerization, solution polymerization, suspension polymerization, dispersion polymerization, or emulsion polymerization can be employed. Among these, solution polymerization, which allows for easy copolymerization control, is preferably used.
[0024] When such copolymerization is carried out by solution polymerization, suitable solvents include, for example, lower alcohols having 1 to 5 carbon atoms such as methanol, ethanol, 1-propanol, 2-propanol, and butanol, and ketones such as acetone and 2-butanone. These may be used individually or in combination of two or more. Among these, methanol is preferably used due to the ease of controlling the polymerization reaction. Furthermore, 2-propanol is preferably used when synthesizing copolymers with a low degree of polymerization.
[0025] The amount of solvent used can be appropriately selected considering the degree of polymerization of the target modified EVOH resin and the chain transfer constant of the solvent. When the solvent is methanol or 2-propanol, S (solvent) / M (monomer) = 0.01 to 10 (mass ratio) is preferred, and 0.05 to 7 (mass ratio) is more preferred.
[0026] As for the method of preparing copolymer components in solution polymerization, any method can be employed, such as initial batch preparation, divided preparation, or continuous preparation such as the Hanna method that takes into account the reactivity ratio of monomers.
[0027] Polymerization initiators are used in the copolymerization described above. Examples of such polymerization initiators include azo initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and peroxide initiators such as acetyl peroxide, benzoyl peroxide, lauryl peroxide, t-butyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, diisopropyl peroxydicarbonate, and di-2-ethylhexyl peroxydicarbonate. These may be used individually or in combination of two or more.
[0028] The amount of polymerization initiator used cannot be determined in general, as it varies depending on the degree of polymerization of the target modified EVOH resin and the type of polymerization initiator, but it can be arbitrarily selected according to the polymerization rate. For example, when using 2,2'-azobisisobutyronitrile or t-butyl peroxyneodecanoate, the amount is usually 10 to 2000 ppm relative to the vinyl ester monomer, preferably 50 to 1000 ppm.
[0029] The polymerization temperature for copolymerization is preferably selected from a range of 40°C to the boiling point, depending on the solvent and ethylene pressure used.
[0030] Furthermore, copolymerization may be carried out in the presence of a chain transfer agent, to the extent that it does not hinder the effects of the present invention. Examples of chain transfer agents include aldehydes such as acetaldehyde, propionaldehyde, and crotonaldehyde; and mercaptans such as 2-hydroxyethanethiol. These may be used individually or in combination of two or more. The amount of chain transfer agent added during copolymerization is determined according to the chain transfer constant of the chain transfer agent and the degree of polymerization of the target modified EVOH resin, but generally, 0.1 to 10 parts by mass per 100 parts by mass of vinyl ester monomer is preferred.
[0031] The degree of polymerization of ethylene-vinyl ester copolymers can be controlled by the polymerization method during the polymerization process, the monomer concentration in solution polymerization (the S (solvent) / M (monomer) ratio mentioned above), the ratio of vinyl ester monomer to other monomers (especially the ratio of vinyl ester monomer to 2-methylene-1,3-propanediol diacetate and / or 3,4-diacetoxy-1-butene), the amount of polymerization initiator used, the amount of chain transfer agent used, and the polymerization rate. Generally, the degree of polymerization tends to be higher with higher monomer concentrations, lower ratios of other monomers to vinyl ester monomers, lower amounts of polymerization initiators, lower amounts of chain transfer agents, and lower polymerization rates.
[0032] After copolymerizing the copolymer components, it is also preferable to add a conjugated polyene such as sorbic acid as a polymerization inhibitor to ensure that the reaction is stopped. When the modified EVOH resin described later is washed, this conjugated polyene dissolves in the washing solution, and its content decreases with washing. However, the content in the modified EVOH resin can be controlled by controlling the washing method.
[0033] A modified EVOH resin can be obtained by saponifying the ethylene-vinyl ester copolymer thus obtained. Furthermore, before saponification, it is preferable to reduce the content of unreacted vinyl ester monomers remaining in the solution by heating or other means, from the viewpoint of suppressing discoloration of the obtained modified EVOH resin. The saponification method can be a known method, for example, by adding a saponification catalyst to an alcohol or aqueous alcohol in which the ethylene-vinyl ester copolymer obtained above has been dissolved.
[0034] Examples of the alcohol include lower alcohols having 1 to 5 carbon atoms, such as methanol, ethanol, and propanol. These may be used individually or in combination of two or more. Methanol is particularly preferred. The concentration of the ethylene-vinyl ester copolymer in the alcohol is appropriately selected depending on the viscosity, and is usually 5 to 60% by mass.
[0035] Examples of the saponification catalyst include alkali catalysts such as alkali metal hydroxides and alkoxides, such as sodium hydroxide, potassium hydroxide, sodium methylate, sodium ethylate, potassium methylate, and potassium ethylate; and acid catalysts such as sulfuric acid, hydrochloric acid, nitric acid, and metasulfonic acid. Preferably, sodium hydroxides and alkoxides, such as sodium hydroxide and sodium methylate, are used.
[0036] The temperature for saponification is not limited, but a range of 20 to 140°C is preferable. As saponification progresses, particulate matter is formed, indicating that the reaction has proceeded. If a gel-like product precipitates at this point, the product can be pulverized. The resulting particulate matter can be washed and dried to obtain modified EVOH resin.
[0037] To increase the degree of saponification of the modified EVOH resin, it is also preferable to perform secondary saponification by removing by-products (vinyl acetate as the vinyl ester monomer, and methyl acetate when methanol is used as the solvent during saponification) from the initially formed particulate matter by washing, etc., then disperse it again in alcohol or the like, add an alkaline catalyst, and proceed with the reaction further.
[0038] In the modified EVOH resin, complete deprotection may not occur during the saponification reaction, and a small amount of ester groups may remain. Similarly, the protecting groups of the side chains may not be completely deprotected, and a small amount of ester groups may remain.
[0039] After the saponification reaction is complete, the alkaline or acidic catalyst is neutralized as needed, followed by solid-liquid separation, washing, and drying to obtain the modified EVOH resin.
[0040] The content of ethylene structural units in the modified EVOH resin is preferably 20 to 60 mol%, more preferably 22 to 55 mol%, and even more preferably 25 to 50 mol%. When the content of ethylene structural units is above the lower limit, the resin tends to exhibit excellent gas barrier properties under high humidity. When the content of ethylene structural units is below the upper limit, the resin tends to exhibit excellent gas barrier properties under low humidity. The content of ethylene structural units in the modified EVOH resin can be controlled by adjusting the ethylene pressure during copolymerization. The content of ethylene structural units is typically, 1 It is measured by 1H-NMR measurement. For example, 1 1H-NMR measurement was used, with DMSO-d as the measurement solvent. 6 A measurement method is used that employs a device and sets the measurement temperature to 50°C.
[0041] The content (modification amount) of the structural units of formula (1) and / or (2) in the modified EVOH resin is 0.1 mol% or more and less than 3.0 mol%. The content of the structural units is preferably more than 0.5 mol%, more preferably 0.6 mol% or more, even more preferably 0.8 mol% or more, and particularly preferably 1.0 mol% or more. Furthermore, the content of the structural units is preferably 2.5 mol% or less, more preferably 2.2 mol% or less, and even more preferably less than 2.0 mol%. Therefore, for example, the content of the structural units is preferably more than 0.5 mol% and less than 3.0 mol%, more preferably 0.6 mol% or more and 2.5 mol% or less, even more preferably 0.8 mol% or more and 2.2 mol% or less, and particularly preferably 1.0 mol% or more and less than 2.0 mol%. The proportion of structural units of formula (1) and / or (2) can be controlled by the amount of 2-methylene-1,3-propanediol diacetate and / or 3,4-diacetoxy-1-butene used as copolymer monomers.
[0042] When the content of the structural units of formula (1) and / or (2) is above the lower limit, the modified EVOH resin tends to have a lower melting point and is less prone to decomposition during melt molding. Furthermore, when preparing aqueous solutions, the cloud point does not become too low, which tends to improve workability. Additionally, when the content of the structural units of formula (1) and / or (2) is below the upper limit, the resin tends to exhibit excellent gas barrier properties under high humidity conditions.
[0043] The degree of saponification of the modified EVOH resin is greater than 98.5 mol%, preferably between 98.7 mol% and less than 99.9 mol%, and preferably between 99.0 mol% and less than 99.8 mol%. When the degree of saponification is above the lower limit, it tends to exhibit excellent gas barrier properties, fragrance retention, solvent resistance, and oil resistance under high humidity conditions. When the degree of saponification is below the upper limit, the manufacturing conditions can be optimized, and manufacturing costs tend to be reduced. The degree of saponification of such modified EVOH resin is usually, 1 It is measured by 1H-NMR measurement. For example, 1 1H-NMR measurement was used, with DMSO-d as the measurement solvent. 6A measurement method is used that employs a device and sets the measurement temperature to 50°C.
[0044] The content of modified EVOH resin in this resin composition, on a solid content basis, is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more, relative to the total resin composition.
[0045] <Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 O> Zn used in this embodiment 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 O (hereinafter sometimes referred to as "this zinc compound") has a structure in which specific structural units are layered with specific interplanar spacings.
[0046] This zinc compound can be obtained by reacting zinc acetate or its hydrate under specific conditions.
[0047] This zinc compound can be obtained using the aforementioned zinc acetate or its hydrate by, for example, (I) a method of reacting zinc acetate or its hydrate under a base, or (II) a method of reacting zinc acetate or its hydrate by heating. Each method will be described in detail below.
[0048] [Method (I)] Method (I) is a method of reacting zinc acetate or its hydrate under a base.
[0049] Examples of bases used in the method described in (I) above include hydroxides of alkali metals or alkaline earth metals. Among these, alkali metal hydroxides are preferred due to their excellent reactivity with zinc-containing compounds, and sodium hydroxide is particularly preferred.
[0050] In the reaction between zinc acetate or its hydrate and a base, the zinc acetate or its hydrate and the base are usually mixed in a solution and reacted. The method of mixing is not particularly limited, but examples include mixing a solution in which zinc acetate or its hydrate is dissolved with a solution in which the base is dissolved, or mixing a slurry in which zinc acetate or its hydrate is dispersed with a solution in which the base is dissolved. Among these, the method of mixing a solution in which zinc acetate or its hydrate is dissolved with a solution in which the base is dissolved is preferred from the viewpoint of reaction efficiency.
[0051] The solvent used to dissolve the zinc acetate or its hydrate and the base is not particularly limited as long as it can dissolve the zinc acetate or its hydrate and the base. Examples include water, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, and 2-butanol, which are lower alcohols having 1 to 5 carbon atoms. These may be used individually or in combination of two or more. Among these, water is preferred because it facilitates post-treatment.
[0052] The concentration of zinc acetate or its hydrate in the solution obtained by dissolving zinc acetate or its hydrate is usually 0.5 to 3 mol / L, preferably 1 to 2 mol / L. The concentration of the base in the solution obtained by dissolving the base in the solvent is usually 0.01 to 100 mol / L, preferably 0.1 to 30 mol / L, particularly preferably 1 to 10 mol / L. When the concentrations of zinc acetate or its hydrate and the base are above the lower limit, the reaction tends to proceed easily. Furthermore, when the concentrations of zinc acetate or its hydrate and the base are below the upper limit, side reactions tend to be less likely to occur.
[0053] The molar ratio of zinc acetate or its hydrate to the base (zinc acetate or its hydrate:base) is usually 0.5:2 to 2:0.5, preferably 0.8:1.5 to 1.5:0.8, and particularly preferably 0.9:1.2 to 1:1. When the molar ratio is within the above range, the reaction tends to proceed easily.
[0054] Furthermore, the pH when reacting zinc acetate or its hydrate with a base is usually 4 to 9, preferably 5 to 8. When the pH is above the lower limit, the reaction tends to proceed more easily. When the pH is below the upper limit, the resulting zinc compound tends to decompose less easily. The pH can be adjusted by changing the amount of a solution containing dissolved zinc acetate or its hydrate, or a slurry containing dispersed zinc acetate or its hydrate, and a solution containing a dissolved base used.
[0055] The reaction temperature in the above reaction is usually 15 to 60°C, preferably 20 to 40°C. When the reaction temperature is above the lower limit, the reaction tends to proceed easily, and when the reaction temperature is below the upper limit, zinc acetate or its hydrate is less likely to decompose due to heat, and the target zinc compound tends to be obtained more easily. The reaction time is usually 0.5 to 5 hours, preferably 1 to 3 hours, and the reaction can be carried out at atmospheric pressure.
[0056] After the above reaction, the zinc compound is obtained as a precipitate. The obtained zinc compound may be used as is, but it is preferable to purify the zinc compound by washing or grinding before use.
[0057] [Method (II)] Method (II) is a method of heating zinc acetate or its hydrate to cause a reaction.
[0058] The method described in (II) above is usually carried out by heating a solution in which zinc acetate or its hydrate is dissolved while stirring.
[0059] As a solvent for dissolving zinc acetate or its hydrate, the solvents listed in method (I) above can be used. Among these, water and alcohols are preferred, and a mixed solvent of water and 1-propanol is particularly preferred.
[0060] The heating conditions mentioned above are such that the solution is heated to a temperature of 20 to 100°C, preferably 50 to 95°C, and particularly preferably 70 to 90°C. When the reaction temperature is above the lower limit, the reaction tends to proceed easily, and when the reaction temperature is below the upper limit, zinc acetate or its hydrate is less likely to decompose due to heat, and the target zinc compound tends to be obtained more easily. The reaction time is usually 0.1 to 100 hours, preferably 0.5 to 30 hours, and particularly preferably 1 to 10 hours, and the reaction pressure can be normal pressure.
[0061] After the above reaction, the zinc compound is obtained as a precipitate. The obtained zinc compound may be used as is, or it may be purified by washing, grinding, or other operations before use.
[0062] This zinc compound exhibits excellent gas barrier properties, particularly oxygen barrier properties, under high humidity conditions. Therefore, when measured by wide-angle X-ray diffraction using CuKα rays, it is preferable that the main peak of the X-ray diffraction is at 2θ = 2 to 15°, more preferably at 2θ = 2 to 9°, and particularly preferably at 2θ = 3 to 8°. This is because when the main peak of the X-ray diffraction is in the aforementioned range, the zinc compound interacts with the EVOH resin, increasing the polarity of the modified EVOH resin, resulting in excellent oxygen barrier properties under high humidity conditions.
[0063] The interlayer distance (distance between layers) of this zinc compound is preferably 0.01 to 50 nm, and more preferably 0.1 to 30 nm, from the standpoint of interaction with the molecules of the modified EVOH resin and water molecules. The interlayer distance of this zinc compound can be calculated from Bragg's formula based on the diffraction position of the strongest peak in the range of 2θ = 2 to 15° when analyzed by X-ray diffraction.
[0064] The molecular weight of the layered structural units exfoliated from this zinc compound is preferably 100 to 10,000, and particularly preferably 200 to 2,000, in order to enable interaction with the modified EVOH resin at the molecular level.
[0065] Furthermore, it is preferable that the structural units of this zinc compound are hydrophilic in terms of their interaction with the molecules of the EVOH resin. In addition, it is preferable that the structural units of this zinc compound do not decompose even when left standing for 1000 hours in an environment of 20°C and 90% RH.
[0066] The metal equivalent content (zinc content) of this zinc compound is preferably more than 0.1 parts by mass, more preferably 0.2 parts by mass or more, and even more preferably 0.3 parts by mass or more, per 100 parts by mass of the modified EVOH resin. The upper limit is preferably less than 5.0 parts by mass, more preferably 4.5 parts by mass or less, and even more preferably 4.0 parts by mass or less. The range of the metal equivalent content is, for example, more than 0.1 parts by mass and less than 5.0 parts by mass. When the zinc content is above the lower limit, it tends to have excellent gas barrier properties under high humidity, and when the zinc content is below the upper limit, it tends to have excellent transparency when made into a film or the like. The content of this zinc compound can be determined by a standard addition method using ICP-MS.
[0067] <Other Thermoplastic Resins> The resin composition may contain thermoplastic resins other than the modified EVOH resin, in a range that does not impede the effects of the present invention (for example, usually 30% by mass or less, preferably 20% by mass or less, more preferably 10% by mass or less, with a lower limit of usually 0% by mass). Other thermoplastic resins that can be used are known thermoplastic resins, such as polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used individually or in combination of two or more.
[0068] <Other Compounding Agents> The resin composition may also contain compounding agents commonly used in thermoplastic resins (excluding transition metals of groups 7 to 11 of the periodic table) within a range that does not impede the effects of the present invention (for example, usually 30% by mass or less of the resin composition, preferably 20% by mass or less, more preferably 10% by mass or less, with a lower limit of usually 0% by mass). Examples of such compounding agents include inorganic double salts (e.g., hydrotalcite), plasticizers (e.g., ethylene glycol, glycerin, aliphatic polyhydric alcohols such as hexanediol), oxygen absorbers [e.g., inorganic oxygen absorbers such as aluminum powder and potassium sulfite; ascorbic acid, and further its fatty acid esters and metal salts, etc.; gallic acid, polyhydric phenols such as hydroxyl group-containing phenol aldehyde resins, terpene compounds, blends of tertiary hydrogen-containing resins and transition metals (e.g., a combination of polypropylene and cobalt), and carbon-carbon unsaturated bond-containing resins]. Blends with transition metals (e.g., a combination of polybutadiene and cobalt), photo-oxidative degradable resins (e.g., polyketones), anthraquinone polymers (e.g., polyvinylanthraquinone), and polymeric oxygen absorbers such as those obtained by adding photoinitiators (e.g., benzophenone), antioxidants or deodorants other than those mentioned above (e.g., activated carbon), heat stabilizers, light stabilizers, ultraviolet absorbers, colorants, antistatic agents, surfactants (except those used as lubricants), antibacterial agents, antiblocking agents, fillers (e.g., inorganic fillers), etc. may also be incorporated. These compounds can be used individually or in combination of two or more.
[0069] <<Method for producing the resin composition>> This resin composition is made of the modified EVOH resin and Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 O can be produced by mixing it using known methods, such as the dry blending method, melt mixing method, solution mixing method, impregnation method, etc.
[0070] The dry blending method mentioned above includes, for example, (i) pelletized modified EVOH resin and Zn 5 (OH) 8 (CH 3CO 2 ) 2 ・2H 2 One possible method is to dry-blend O and the other using a tumbler or similar device.
[0071] The aforementioned melt-mixing method includes, for example, (ii) pelletized modified EVOH resin and Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 (iii) A method of melting and kneading a dry blend obtained by dry blending O and, 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 One example is a method involving adding oxygen and then melt-kneading the mixture.
[0072] As for the aforementioned solution mixing method, for example, (iv) prepare a solution using a commercially available modified EVOH resin, and add Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 One possible method involves mixing in oxygen (O), solidifying and molding the mixture, and then separating the solid and liquid components by known means and drying it.
[0073] As for the impregnation method, for example, (v) pelletized modified EVOH resin, Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 By contacting the modified EVOH resin with an aqueous solution containing O, Zn is introduced. 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 Methods include drying after incorporating oxygen.
[0074] As described above, in this embodiment, it is possible to combine the different methods mentioned above.
[0075] The resin composition obtained in this manner can be prepared in various forms, such as pellets, powder, or liquid, and provided as a molding material for various molded articles. In particular, in this embodiment, it is preferable that the material be provided as a solution, as this tends to allow the effects of the present invention to be obtained more efficiently.
[0076] The preparation of the solution (coating liquid) of the resin composition can be, for example, by adding all components to a solvent at once and mixing them, or by adding other components to a solution in which some components are dissolved in a solvent and mixing them. In particular, from the viewpoint of workability, it is preferable to prepare the solution by mixing water, alcohol, and the zinc acetate or its hydrate with a solution in which the modified EVOH resin is dissolved in a solvent, thereby generating the zinc compound in the solution.
[0077] As the aforementioned solvent, a water-alcohol mixed solvent, which is a mixed solvent of water and alcohol, can be used.
[0078] The aforementioned alcohol is not particularly limited as long as it can dissolve the modified EVOH resin, but examples include monohydric alcohols such as methyl alcohol, ethyl alcohol, propyl alcohol, and butyl alcohol; dihydric alcohols such as ethylene glycol and propylene glycol; trihydric alcohols such as glycerin; and phenols such as phenol and cresol. These can be used individually or in combination of two or more. Among these, n-propyl alcohol (such as n-propyl alcohol, isopropyl alcohol, and methyl alcohol) is preferred, and n-propyl alcohol is more preferred.
[0079] The alcohol concentration in the water-alcohol mixed solvent is preferably more than 30% by mass and less than 70% by mass, more preferably 35% by mass or more and 67% by mass or less, even more preferably 40% by mass or more and 63% by mass or less, and even more preferably 45% by mass or more and 60% by mass or less. Having the alcohol concentration within this range tends to suppress an increase in the viscosity of the solution (coating liquid) of the resin composition.
[0080] The content of the water-alcohol mixed solvent is preferably 80% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more, relative to the solution (coating liquid) of the resin composition. The upper limit is usually 99% by mass. Such a content within the above range tends to result in excellent coating properties.
[0081] Furthermore, the content of the modified EVOH resin is preferably 0.1% to 50% by mass, more preferably 1% to less than 20% by mass, even more preferably 3% to 18% by mass, and particularly preferably 5% to 16% by mass, relative to the solution (coating liquid) of the resin composition. If the concentration of the modified EVOH resin is too high, the solution stability tends to deteriorate, and the coating properties tend to worsen, such as the occurrence of mark flow during coating. If the concentration of the modified EVOH resin is too low, a uniform film cannot be obtained during coating, the gas barrier properties tend to worsen, and the film surface tends to whiten.
[0082] Furthermore, it is preferable to incorporate a boron compound into the solution (coating liquid) of the resin composition in order to improve stability. Examples of such boron compounds include boric acid or its metal salts, calcium borate, cobalt borate, zinc borate (zinc tetraborate, zinc metaborate, etc.), aluminum potassium borate, ammonium borate (ammonium metaborate, ammonium tetraborate, ammonium pentaborate, ammonium octaborate, etc.), cadmium borate (cadmium orthoborate, cadmium tetraborate, etc.), and potassium borate (potassium metaborate). (e.g., potassium tetraborate, potassium pentaborate, potassium hexaborate, potassium octaborate, etc.), silver borate (silver metaborate, silver tetraborate, etc.), copper borate (copper dicorate, copper metaborate, copper tetraborate, etc.), sodium borate (sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate, sodium octaborate, etc.), lead borate (lead metaborate, lead hexaborate, etc.), nickel borate (ortho) Nickel borate, nickel diborate, nickel tetraborate, nickel octaborate, etc.), barium borate (barium orthoborate, barium metaborate, barium diborate, barium tetraborate, etc.), bismuth borate, magnesium borate (magnesium orthoborate, magnesium diborate, magnesium metaborate, trimagnesium tetraborate, pentamagnesium tetraborate, etc.), manganese borate (manganese borate, magnesium metaborate) Examples of suitable materials include manganese tetraborate, lithium borate (lithium metaborate, lithium tetraborate, lithium pentaborate, etc.), as well as borate minerals such as borax, carnite, inyoite, kotoite, syuanite, and zyberite. Preferably, boric acid and sodium borate (sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate, sodium octaborate, etc.) are used.
[0083] The content of such compounding agents is usually 30% by mass or less, preferably 20% by mass or less, and particularly preferably 10% by mass or less, of the solution (coating liquid) of the resin composition, with the lower limit usually being 0% by mass.
[0084] The zinc content in this resin composition is preferably more than 0.1 parts by mass, more preferably 0.2 parts by mass or more, and even more preferably 0.3 parts by mass or more, per 100 parts by mass of the modified EVOH resin. The upper limit is preferably less than 5.0 parts by mass, more preferably 4.5 parts by mass or less, and even more preferably 4.0 parts by mass or less. The range of the metal equivalent content is, for example, more than 0.1 parts by mass and less than 5.0 parts by mass. When the zinc content is above the lower limit, it tends to have excellent gas barrier properties under high humidity, and when the zinc content is below the upper limit, it tends to have excellent transparency when made into a film or the like. The content of the zinc compound can be determined by a standard addition method using ICP-MS.
[0085] This resin composition may contain sodium during the manufacturing process of the modified EVOH resin. If sodium is present, its content is preferably more than 0 ppm and less than 600 ppm relative to the entire resin composition (or, if the resin composition is a solution, relative to the solution of the resin composition), more preferably more than 0 ppm and 500 ppm or less, and even more preferably more than 0 ppm and 400 ppm or less.
[0086] The solution (coating liquid) of the resin composition obtained in this manner exhibits excellent solution stability, and the gelation time of the coating liquid, measured according to the low-temperature solution stability evaluation described in the examples below, is typically 30 days or more.
[0087] The solution (coating liquid) of the resin composition can be used to coat an object to obtain a multilayer structure with excellent gas barrier properties. In a method for manufacturing a multilayer structure according to one embodiment of the present invention, when a coating method is used, the method includes at least the steps of coating the resin composition onto a substrate and drying the coated resin composition. This makes it possible to obtain a multilayer structure having a coated layer made of the resin composition on a substrate.
[0088] Coating methods include, for example, wet coating methods such as spraying, showering, dipping, flow coating, gravure printing, flexographic printing, roll, knife, bar, spin, dispenser, inkjet printing, and screen printing.
[0089] The coating amount of the aforementioned resin composition solution (coating liquid) is typically 1 to 50 g / m². 2 Preferably 2 to 30 g / m 2 Particularly preferably 3 to 20 g / m 2 Therefore, when the coating amount of the resin composition solution (coating liquid) is within the aforementioned range, the oxygen permeability tends to be within a suitable range.
[0090] The drying conditions are not particularly limited and may be carried out at or near room temperature or by heating, for example, at around 25 to 120°C, preferably 50 to 100°C, and more preferably 60 to 90°C. The drying time is not particularly limited as long as the solvent can be sufficiently evaporated, for example, at around 10 seconds to 30 minutes, preferably 15 seconds to 10 minutes.
[0091] The thickness of the solution (coating liquid) of this resin composition after drying is usually 0.1 to 15 μm, preferably 0.2 to 10 μm, and more preferably 0.5 to 5 μm.
[0092] <<Molded Article>> A molded article according to one embodiment of the present invention (hereinafter sometimes referred to as "the molded article") is a molded article containing the resin composition, and may be formed by molding the resin composition or by molding a composition containing the resin composition. Examples of the shape of the molded article include films, sheets, tapes, cups, trays, tubes, bottles, pipes, filaments, extruded articles with irregular cross-sections, and various irregularly shaped articles. The molded article may also be a molded article having a coating layer containing the resin composition (for example, a multilayer structure formed by coating a substrate with the resin composition).
[0093] There are no particular restrictions on the molding method for this molded article; any molding method applicable to general resin compositions can be used. For example, a method of forming a film using a solution (coating liquid) of a composition containing the resin composition, or a melt molding method can be used. The coating liquid consists of a modified EVOH resin and Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 It is prepared by mixing O with solvents and other compounding agents as needed. Examples of melt molding methods include extrusion molding (T-die extrusion, inflation extrusion, blow molding, melt spinning, mold extrusion, etc.) and injection molding.
[0094] Examples of the molded articles include single-layer films molded from the resin composition, and multilayer structures having layers made of the resin composition. Furthermore, the molded articles include the modified EVOH resin and Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 The molded article may have a coating layer containing the resin composition containing O (for example, a multilayer structure formed by coating a substrate with the resin composition).
[0095] <Film, Multilayer Structure> A film according to one embodiment of the present invention (hereinafter sometimes referred to as "this film") is a film containing this resin composition, and may be obtained by forming a film of this resin composition, or by forming a film of a composition containing this resin composition, but it is preferable that this film be obtained by forming a film of this resin composition.
[0096] Methods for producing this film include, for example, using a solution (coating liquid) of the resin composition, melting the resin composition and extruding it using an extruder, and melt-molding pelletized resin composition using an extruder. Among these, the method using a solution (coating liquid) of the resin composition is preferred.
[0097] Furthermore, the film may be subjected to stretching operations such as uniaxial stretching or biaxial stretching as needed.
[0098] The film may be a single-layer structure or a multilayer structure. Preferably, the multilayer structure has at least one layer made of the film. When a melt extrusion method is used in the manufacturing method of the multilayer structure, it is preferable to melt the resin composition in an extruder and extrude the molten resin composition from a die, thereby laminating it with other base resins. The multilayer structure may be made by laminating the formed film or by laminating it with other base resins.
[0099] The material to be coated is not particularly limited, but can be a wide range of polyolefins, including linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ionomer, ethylene-propylene copolymer, ethylene-acrylic acid ester copolymer, polypropylene, propylene-α-olefin (α-olefin with 4 to 20 carbon atoms) copolymer, polybutene, polypentene, and other olefins, either alone or in copolymer form, or these olefins, either alone or in copolymer form, graft-modified with unsaturated carboxylic acids or their esters. Examples of suitable substrates include stretched or unstretched films, sheets, hollow containers, paper, cellophane, cellulose, cellulose acetate, natural rubber, synthetic rubber, metal foil, woven fabric, nonwoven fabric, metal cotton strips, and wood surfaces, all made from various plastics such as fats, polystyrene resins, polyesters, polyamides, copolymerized polyamides, polyvinyl chloride, polyvinylidene chloride, acrylic resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, and EVOH resins. The appropriate film thickness of such substrates is approximately 10 to 1000 μm.
[0100] The oxygen permeability of the film obtained in this way is typically 25 cc·μm / m 2 - The pressure is less than or equal to 1 day·atm, preferably 20 cc·μm / m 2·day·atm or less. Such oxygen permeability can be measured, for example, according to the gas barrier property evaluation under high humidity described in the Examples below.
[0101] In general, EVOH resins have high crystallinity due to strong hydrogen bonding from intramolecular hydroxyl groups, which is a factor that develops excellent gas barrier properties. However, in modified EVOH modified by introducing at least one of specific structural units (1) and (2), the relevant structural unit moderately inhibits crystallization, so the crystallinity tends to decrease compared to unmodified EVOH, and the packing of molecular chains in the amorphous region tends to become irregular. While such modified EVOH has the advantage of excellent solubility in solvents and solution stability, moisture easily penetrates into the fine voids generated in the amorphous region, and the gas barrier property tends to decrease. In contrast, in the present resin composition, a specific layered compound Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ·2H 2 By containing O, an interaction develops between the zinc compound and the hydroxyl groups of EVOH, the amorphous portion is controlled, and as a result, moisture uptake into the voids is effectively suppressed, which is presumed to provide excellent gas barrier properties under high humidity.
[0102] The present resin composition, and molded articles, films, and multilayer structures containing the present resin composition are useful as packaging materials, and can be suitably used particularly as food packaging materials, medical packaging materials, and the like.
[0103] Hereinafter, the present invention will be described more specifically with reference to Examples, but the present invention is not limited to the following Examples as long as it does not exceed the gist thereof. In the Examples, "parts" and "%" mean mass basis.
[0104] <Example 1> As a modified EVOH resin, modified EVOH resin pellets having an ethylene structural unit content of 33 mol%, a structural unit content (modification amount) represented by the following formula (1) of 1.0 mol%, and a saponification degree of 99.6 mol% were added to a mixed solvent of water and 1-propyl alcohol (water / alcohol = 50 / 50 (mass ratio)), and the mixture was heated and stirred at 87°C for 1 hour to completely dissolve the modified EVOH resin. Thereafter, zinc acetate or a hydrate thereof as Zn(CH 3 CO 2 ) 2 ·H 2 O was added so that the zinc content was 0.3 parts relative to 100 parts of the modified EVOH resin, and the mixture was stirred at 87°C for 2 hours to prepare a coating liquid containing the modified EVOH resin and Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ·2H 2 O (the modification ratio of the modified EVOH resin is 15%).
[0105] [Preparation of measurement sample] The prepared coating liquid was applied to the corona-treated surface of a 12 μm-thick PET base material subjected to corona treatment using wire bar #9, and dried at 100°C for 2 minutes. Thereby, a two-layer film in which a 1 μm-thick film layer was laminated on the PET base material was produced. The obtained EVOH coating film was isolated with cellophane tape, and then the following analysis was performed.
[0106] [Identification of chemical structure] Measurements by solid-state NMR and wide-angle X-ray diffraction were performed, and it was identified that Zn(CH 3 CO 2 ) 2 ·H 2 O was obtained.
[0107] [Solid-state NMR( 13 C-CP / MAS) Measurement] The sample was filled in a 4 mmφ zirconia rotor, and sealed with a polyethylene drive tip to obtain a measurement sample. This measurement sample was subjected to solid-state NMR [AVANCE III 400WB( 1 H: 400 MHz, 13Measurements were performed using a CP / MAS probe with a 100MHz (C) (manufactured by Bruker). The measurement conditions were as follows: rotation at 5000Hz, 90° pulse width of 45μs, contact time of 2ms, number of integrations of 485, acquisition time of 50ms, and delay time of 5 seconds.
[0108] [Wide-angle X-ray diffraction (XRD) measurement] Wide-angle X-ray diffraction (XRD) measurements were performed on the sample under the following conditions. [Measurement conditions] ・Equipment used: D8 DISCOVER (Bruker Japan) ・Voltage: 50kV ・Current: 100mA ・Camera length: 150mm ・Measurement method: Reflection method ・Integration time: 20 minutes ・As a result of the measurement, peaks were mainly detected at 2θ = 6.8°, 13.5°, and 20.2°.
[0109] Based on the measurement results of the solid-state NMR and wide-angle X-ray diffraction, the obtained zinc compound was found to be consistent with the layered zinc compound described in Inorg. Chem. 2013, 52, 95-102, and therefore the obtained zinc compound was named [Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 It was identified as O.
[0110] Also, the above [Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 When [O] was measured by wide-angle X-ray diffraction, the interlayer distance was calculated from Bragg's equation based on the diffraction position at 2θ = 6.8°, where the peak intensity was strongest. 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 [O] was a layered compound with an interlayer distance of 1.3 nm.
[0111] <Examples 2-14, Comparative Examples 1-2> In Example 1, a film was prepared in the same manner as in Example 1, except that the type of modified EVOH resin pellets, the composition ratio of the mixed solvent of water and 1-propyl alcohol, the concentration of modified EVOH resin in the coating solution, and the zinc content were changed to the values shown in Tables 1 and 2 below.
[0112] <Example 15> In Example 1, the modified EVOH resin having the structural unit of formula (1) was replaced with pellets of modified EVOH resin having the structural unit of formula (2) (ethylene structural unit content 29 mol%, structural unit content (modification amount) represented by formula (2) 1.0 mol%, degree of saponification 99.6 mol%), and the concentration of the modified EVOH resin and the zinc content in the coating solution were changed to the values shown in Table 1 below. Otherwise, a film was prepared in the same manner as in Example 1.
[0113] <Example 16> In Example 1, the modified EVOH resin having the structural unit of formula (1) was replaced with pellets of modified EVOH resin having the structural unit of formula (2) (ethylene structural unit content 29 mol%, structural unit content (modification amount) represented by formula (2) 1.0 mol%, degree of saponification 99.6 mol%), and the concentration of the modified EVOH resin and the zinc content in the coating solution were changed to the values shown in Table 1 below. Otherwise, a film was prepared in the same manner as in Example 1.
[0114] <Example 17> In Example 1, the modified EVOH resin having the structural unit of formula (1) was replaced with pellets of modified EVOH resin having the structural unit of formula (2) (ethylene structural unit content 38 mol%, structural unit content (modification amount) represented by formula (2) 1.0 mol%, degree of saponification 99.6 mol%), and the concentration of the modified EVOH resin and the zinc content in the coating solution were changed to the values shown in Table 1 below. Otherwise, a film was prepared in the same manner as in Example 1.
[0115] <Comparative Example 3> A film was prepared in the same manner as in Example 1, except that the modified EVOH resin was changed to unmodified EVOH resin pellets (ethylene structural unit content 33 mol%, degree of saponification 99.7 mol%) and the zinc content was changed to 1.0 part.
[0116] <Comparative Example 4> A film was prepared in the same manner as in Example 1, except that the modified EVOH resin was changed to unmodified EVOH resin pellets (ethylene structural unit content 29 mol%, degree of saponification 99.7 mol%) and the zinc content was changed to 1.0 part.
[0117] <Comparative Example 5> A film was prepared in the same manner as in Example 1, except that the modified EVOH resin was changed to unmodified EVOH resin pellets (ethylene structural unit content 44 mol%, degree of saponification 99.7 mol%) and the zinc content was changed to 1.0 part.
[0118] <Comparative Example 6> In Example 1, Zn(CH 3 CO 2 ) 2 ・H 2 A film was prepared in the same manner as in Example 1, except that O was replaced with zinc oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).
[0119] <Comparative Example 7> A film was prepared in the same manner as in Example 1, except that the content of ethylene structural units was changed to 29 mol% and the content of structural units represented by formula (1) was changed to 3.0 mol%.
[0120] <Comparative Example 8> A film was prepared in the same manner as in Example 15, except that the content of the structural unit represented by formula (2) was changed to 3.0 mol%.
[0121] The films obtained from Examples 1 to 15 and Comparative Examples 1 to 8 were used to evaluate the solution stability of the coating solution at low temperatures and the gas barrier properties under high humidity. The results are shown in Tables 1 and 2 below.
[0122] [Evaluation of Solution Stability of Coating Solution at Low Temperatures] Immediately after preparing 150 mL of each coating solution, as shown in Figure 1, it was sealed in a screw-cap glass bottle with a cylindrical body (body inner diameter 55 mm, mouth inner diameter 35 mm, body length 90 mm, total length 110 mm), and after being kept at 40°C for one day, it was allowed to gel by standing in an incubator at 10°C. The number of days from when the coating solution was placed in the incubator until gelation was completed was defined as the gelation time. Here, if no flow of the coating solution was observed after 1 minute when the glass bottle was turned upside down with the cap closed, gelation was considered complete.
[0123] [Evaluation of gas barrier properties under high humidity] Each film was measured using an oxygen permeability analyzer (OX-TRAN2-21, manufactured by MOCON) under conditions of 20°C and 90% RH.
[0124]
[0125]
[0126] From the results in Tables 1 and 2, the modified EVOH resin having the structural units of formula (1) and / or (2), and Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 The solutions (coating liquids) of the resin composition in Examples 1 to 14, which contain O, exhibited excellent solution stability because they could suppress the progression of gelation even at low temperatures, and further exhibited excellent gas barrier properties under high humidity conditions when made into films. On the other hand, Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2Solutions (coating liquids) of the resin compositions of Comparative Examples 1 and 2 that do not contain O, solutions (coating liquids) of the resin compositions of Comparative Examples 3 to 5 that do not contain modified EVOH resin having the structural units of formula (1) and / or (2), solutions (coating liquids) of the resin composition of Comparative Example 6 that contains metal compounds other than specific metal compounds, and solutions (coating liquids) of the resin compositions of Comparative Examples 7 and 8 in which the content (modification amount) of the structural units of formula (1) and / or (2) is greater than or equal to a specific amount, all exhibited insufficient solution stability or gas barrier properties under high humidity when formed into films.
[0127] While the above embodiments illustrate specific forms of the present invention, these embodiments are merely illustrative and should not be interpreted restrictively. Various modifications that are obvious to those skilled in the art are intended to fall within the scope of the present invention.
[0128] The resin composition of the present invention can suppress the progression of gelation when storing a solution of this resin composition, and furthermore, when made into a film, it exhibits excellent gas barrier properties under high humidity. Therefore, it is useful, for example, as a packaging material for food, medical products, industrial chemicals, etc., or as a composite material laminated with plastic film, paper, or metal foil.
Claims
1. Modified ethylene-vinyl alcohol copolymer and Zn 5 (OH) 8 (CH 3 CO 2 ) 2 ・2H 2 A resin composition containing O, wherein the modified ethylene-vinyl alcohol copolymer has at least one structural unit of the following formulas (1) and (2), and the content of the structural unit is 0.1 mol% or more and less than 3.0 mol%.
2. The resin composition according to claim 1, wherein the modified ethylene-vinyl alcohol copolymer has a structural unit of formula (1) or (2).
3. The resin composition according to claim 1, wherein the content of the structural unit is 1.0 mol% or more and less than 3.0 mol%.
4. The resin composition according to claim 1, wherein the zinc content is 0.1 parts by mass more than 100 parts by mass of the modified ethylene-vinyl alcohol copolymer.
5. The resin composition according to claim 1, wherein the zinc content is less than 5.0 parts by mass per 100 parts by mass of the modified ethylene-vinyl alcohol copolymer.
6. The resin composition according to claim 1, wherein the content of ethylene structural units in the modified ethylene-vinyl alcohol copolymer is 20 to 60 mol%.
7. The resin composition according to claim 1, wherein the content of the modified ethylene-vinyl alcohol copolymer is 0.1% by mass or more and 50% by mass or less of the total resin composition.
8. The resin composition according to claim 1, wherein the content of the modified ethylene-vinyl alcohol copolymer is 1% by mass or more and less than 20% by mass of the entire resin composition.
9. The resin composition according to claim 1, wherein the resin composition contains sodium, and the content of the sodium is greater than 0 ppm and less than or equal to 600 ppm of the entire resin composition.
10. The resin composition according to claim 1, further comprising water.
11. The resin composition according to claim 1, further comprising an alcohol.
12. The resin composition according to claim 1, wherein the form of the resin composition is a solution.
13. A molding material comprising the resin composition according to any one of claims 1 to 12.
14. A molded article comprising the resin composition according to any one of claims 1 to 9.
15. A multilayer structure comprising the resin composition according to any one of claims 1 to 9.
16. A film comprising the resin composition according to any one of claims 1 to 9.
17. A food packaging material comprising the resin composition according to any one of claims 1 to 9.
18. A medical packaging material comprising the resin composition described in any one of claims 1 to 9.
19. A method for producing a multilayer structure, comprising coating it with the resin composition described in any one of claims 1 to 12.