Cellulose fiber bundle and method for producing same, microfibrillated cellulose and method for producing same, paper, modifier for paper, coating material, building material, and reinforcing fiber material
The production of algal microfibrillated cellulose through alkali and acid treatments followed by mechanical processing addresses the inefficiencies of wood-derived methods, enhancing productivity and reducing costs, and improves paper properties using aquatic resources.
Patent Information
- Application Number
- PCT/JP2026/017708
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-05-08
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for producing cellulose nanofibers and microfibrillated cellulose from wood pulp require high energy, specialized equipment, result in low productivity, and have high transportation and processing costs due to low solid content concentrations, while methods using algal fibers face challenges in aspect ratio and water content, limiting their applications and efficiency.
A method for producing algal microfibrillated cellulose involves preparing cellulose fiber bundles from algae through alkali and acid treatments, followed by simple mechanical processing, which allows for easy refinement to microfibrillated cellulose without specialized equipment, enhancing transportability and productivity.
The method enables the production of algal microfibrillated cellulose as a substitute for wood-derived cellulose nanofibers, reducing environmental impact, lowering processing costs, and improving paper properties such as elastic modulus and interfiber bonds, while utilizing aquatic resources and reducing forest resource depletion.
Smart Images

Figure JP2026017708_12112026_PF_FP_ABST
Abstract
Description
Cellulose fiber bundles and methods for producing the same, microfibrillated cellulose and methods for producing the same, paper, paper modifiers, paints, building materials, and fiber reinforcing materials.
[0001] This disclosure relates to cellulose fiber bundles and methods for producing the same, microfibrillated cellulose and methods for producing the same, paper, paper modifiers, paints, building materials, and fiber reinforcing materials.
[0002] Approximately 180 million tons of paper pulp are produced worldwide annually, and about 90% of this paper pulp is derived from wood. Research into the planned use of forest resources has been ongoing for a long time, and biodegradable paper is expected to be a substitute for plastic. Processing forest resources requires pulping at high temperatures and under strong alkalinity, which has a significant environmental impact. Therefore, new raw materials for paper pulp that do not rely on wood resources are needed. One example of a new raw material for paper pulp is algal material (see, for example, Patent Document 1). Patent Document 1 discloses a method for producing pulp from red algae, a type of seaweed. Patent Document 2 also discloses a method for obtaining elliptical red algal fibers using red algae as a raw material.
[0003] Furthermore, as a new way to utilize pulp, the use of finely processed cellulose, such as cellulose nanofibers (hereinafter referred to as CNF) obtained by defibrating fibers down to the nanoscale, has been proposed. One example is the production of nanofibers using seaweed (for example, Non-Patent Document 1). Non-Patent Document 1 proposes a method for producing CNF from seaweed and its residues by defibration treatment using a disc mill. Patent Document 3 proposes a method for obtaining cellulose fibers at the several-micron level by mechanical treatment using a beater or homomixer after removing impurities from seaweed biomass such as red algae using an alkaline aqueous solution. While finely processed cellulose is expected to have various material applications, high energy is required to finely process general cellulose fibers (such as wood pulp fibers). In addition, it is highly dependent on equipment for fine processing, such as disc mills, beaters, and homomixers, and productivity is low because many processes cannot be carried out at once. Furthermore, since the finely processed cellulose obtained is obtained as an aqueous dispersion with a low solid content concentration, transportation costs are high.
[0004] Japanese Patent Publication No. 2009-270250, Japanese Patent Publication No. 2025-519275, International Publication No. 2018 / 159980
[0005] Yoshinao Asano, Shinichi Kamiyama, and Yukiyasu Sato, Gifu Prefectural Industrial Technology Center Research Report No. 10 (2016)
[0006] Patent Document 1 describes a method for producing fibers from red algae that requires treatment using alcohols or ketones as reaction solvents and curing with aldehyde-based curing agents, which presents problems in terms of processing costs and environmental impact. Patent Document 2 describes a method for obtaining oval-shaped red algae fibers from red algae, but its low aspect ratio makes biomass recovery difficult, and its high water content results in poor transportability. Furthermore, its applications as a fiber are limited to coatings and the like. Patent Document 3 and Non-Patent Document 1 require long processing times using micronization equipment such as disc mills, beaters, or homomixers, resulting in significant electrical costs. Cellulose nanofibers, obtained by defibrating general pulp fibers (20 μm to 50 μm) to nano-size (fiber width of several nanometers), require a great deal of energy for production and processing. Therefore, depending on the application, there is growing interest in selecting microfibrillated cellulose fibers (hereinafter sometimes referred to as MFC fibers) of micro to sub-nano size (fiber width of several μm to tens of nanometers). However, Patent Document 1 cannot obtain micro- to sub-nanometer sized MFC fibers (fiber width of several μm to tens of nm). Furthermore, productivity is low because a large amount of processing cannot be performed at once. In addition, the obtained finely milled cellulose is obtained as a low-concentration aqueous dispersion, resulting in high transportation costs. Finely milled cellulose presents challenges in terms of equipment dependence and milling costs, low productivity, and transportability due to high water content, but the methods described in Patent Documents 1 to 3 and Non-Patent Document 1 have not been able to solve these problems.
[0007] This disclosure has been made in view of the above-mentioned prior circumstances, and the first aspect of this disclosure aims to provide algal microfibrillated cellulose and a method for producing the same as a substitute material for existing wood-derived CNF. The first aspect of this disclosure also aims to provide paper and a paper modifier using the above-mentioned algal microfibrillated cellulose. Furthermore, the second aspect of this disclosure aims to provide algal cellulose fiber bundles that have excellent transportability and allow for easy preparation of microfibrillated cellulose by simple micronization processing, and a method for producing the same, as well as microfibrillated cellulose and a method for producing the same using these cellulose fiber bundles, paper, a paper modifier, a paint, a building material, and a fiber reinforcement material.
[0008] The specific means for achieving the above objectives are as follows: <1> A cellulose fiber bundle derived from algae, wherein the filtration capacity measured according to ISO 5267-2:2001 is 400 mL or more, and the filtration capacity after disintegration treatment with a cumulative number of rotations of 10,000 under the conditions specified in ISO 5263-1:2004 is 200 mL or less. <2> The cellulose fiber bundle according to <1>, wherein the filtration capacity after disintegration treatment with a cumulative number of rotations of 3,000 under the conditions specified in ISO 5263-1:2004 is 200 mL or less. <3> The cellulose fiber bundle according to <1> or <2>, wherein the filtration capacity after disintegration treatment with a cumulative number of rotations of 1,000 under the conditions specified in ISO 5263-1:2004 is 200 mL or less. <4> A cellulose fiber bundle derived from algae, wherein the filtration capacity measured according to ISO 5267-2:2001 is 400 mL or more, and the filtration capacity after beating treatment with a cumulative number of rotations of 1000 times using a PFI mill as defined in ISO 5264-2:2011 is 200 mL or less. <5> A cellulose fiber bundle according to any one of <1> to <4>, wherein the average minor diameter is 50 μm or more. <6> A cellulose fiber bundle according to any one of <1> to <4>, wherein the average minor diameter is 100 μm or more. <7> A cellulose fiber bundle according to any one of <1> to <4>, wherein the average minor diameter is 200 μm or more. <8> A cellulose fiber bundle according to any one of <1> to <7>, wherein the average minor diameter after the disintegration treatment or the beating treatment is 1 / 3 or less of the average minor diameter before the disintegration treatment or the beating treatment. <9> The cellulose fiber bundle according to any one of <1> to <8>, wherein the algae is a red alga. <10> The cellulose fiber bundle according to claim <9>, wherein the red algae comprises at least one selected from the group consisting of the families Apocynaceae, and Apocynaceae. <11> Microfibrillated cellulose derived from algae, wherein the average short diameter of the microfibrillated cellulose is 1 μm to 10 μm, and the aspect ratio of the microfibrillated cellulose is 100 or more.<12> Microfibrillated cellulose derived from algae, wherein the average short diameter of the microfibrillated cellulose is 30 nm to 1000 nm, and the aspect ratio of the microfibrillated cellulose is 100 or more. <13> Microfibrillated cellulose according to <11> or <12>, wherein the filtration capacity measured according to ISO 5267-2:2001 is 200 mL or less. <14> Paper containing microfibrillated cellulose according to any one of <11> to <13>. <15> Basis weight is 30 g / m². 2 ~100g / m 2A paper according to <14> having an opacity of 80% or less under the conditions. <16> A paper according to <14> or <15> having an opacity of 80% or less, impregnated with at least one selected from the group consisting of polysaccharides, oils and fats, waxes, natural resins and synthetic resins. <17> A paper modifier containing microfibrillated cellulose according to any one of <11> to <13>. <18> A paint containing microfibrillated cellulose according to any one of <11> to <13>. <19> A building material containing microfibrillated cellulose according to any one of <11> to <13>. <20> A fiber reinforcement material containing microfibrillated cellulose according to any one of <11> to <13>. <21> A method for producing cellulose fiber bundles derived from algae according to any one of <1> to <10>, comprising, in this order: a preparation step of preparing algal residue obtained by removing at least a portion of solvent-soluble components from algae; an alkali treatment step of immersing the algal residue in an alkaline aqueous solution; a bleaching step of bleaching the algal residue after the alkali treatment step; and an acid treatment step of immersing the algal residue after the bleaching step in an acid aqueous solution. <22> The method for producing cellulose fiber bundles according to <21>, wherein the pH of the alkaline aqueous solution is 9 to 14. <23> The method for producing cellulose fiber bundles according to <21> or <22>, wherein the temperature of the alkaline aqueous solution is 20°C to 100°C. <24> The method for producing cellulose fiber bundles according to any one of <21> to <23>, wherein the pH of the acid aqueous solution is 1 to 4. <25> The method for producing cellulose fiber bundles according to any one of <21> to <24>, wherein the temperature of the acid aqueous solution is 20°C to 60°C. <26> A method for producing a cellulose fiber bundle according to any one of <21> to <25>, wherein the bleaching agent used in the bleaching step comprises at least one selected from the group consisting of hypochlorite, hydrogen peroxide, and chlorine dioxide. <27> A method for producing a cellulose fiber bundle according to any one of <21> to <26>, further comprising a neutralization step of neutralizing the algal residue after the acid treatment step.<28> A method for producing microfibrillated cellulose derived from algae, comprising a refinement step of refining a cellulose fiber bundle obtained through the method for producing a cellulose fiber bundle described in any one of <21> to <27>. <29> The method for producing microfibrillated cellulose according to <28>, wherein the refinement step refines the average short diameter of the cellulose fiber bundle to 1 / 10 or less of the diameter before the refinement step, or to 10 μm or less.
[0009] The algae used in this disclosure either grow naturally in freshwater or saltwater environments or are cultivated, and are processed into agar and other products by extracting water-soluble components. This process generates residues after the extraction of edible or medicinal components, which need to be disposed of. In addition, some algae proliferate excessively, and their eradication and disposal may require considerable effort. If these algae and residues can be used as raw materials for MFCs and paper, it would be advantageous in terms of raw material supply volume and raw material price. Furthermore, since algae do not contain lignin, they can be pulped into paper without undergoing the highly alkaline and high-temperature pulping process required for wood, and the cost of pulping algae into paper is estimated to be less than half that of wood. By using lignin-free algal fibers (fibers whose main component is cellulose obtained from algae), it is possible that algal fibers can be utilized to the same extent as or even more than wood. As a result, by suppressing the consumption of forest resources, the depletion of forest resources can be mitigated, contributing to the solution of environmental problems. In addition, it provides a useful use for the residues after the extraction of edible or medicinal components from seaweed, which are expected to increase in the future. Because algal fibers are produced in aquatic environments, they do not compete with terrestrial crops and lead to new uses for aquatic resources and blue carbon. Furthermore, by utilizing discarded seaweed residue as a fiber resource, a carbon stock effect can be expected. Currently, microfibrillated cellulose and other finely processed celluloses obtained from wood pulp or algal fibers require a micronization process using specialized equipment such as disc mills, beaters, and homomixers. In some cases, a special chemical reaction called TEMPO oxidation is also used. The algal-derived cellulose fiber bundles obtained by this disclosure are in a state where fine cellulose fibers are aggregated and are obtained in a state that is easily processed, making it possible to obtain MFCs with simple processing. For example, fiber micronization can be carried out by mechanical processing with a light beater or by stirring and disintegrating the fibers with a general agitator, resulting in low cost and low equipment dependence. In addition, because it can be processed with simple processes such as stirring, a large amount of fiber can be produced at once, making it highly productive. Furthermore, the algal fibers obtained by this disclosure can be refined through simple processing without relying on equipment, making it possible to adjust the degree of refinement (filtration degree) without being limited by the processing plant.For example, by transporting the algae-derived MFCs in a low-moisture state with high filtration efficiency (high dewatering ability and easy drying) and then performing micronization at the site of use and processing, it is possible to save on drying costs and achieve high transportability. Furthermore, the algae-derived MFCs obtained by this disclosure have a small fiber width and readily form interfiber bonds when papermaking, resulting in a tendency for the resulting paper to have a high elastic modulus. In addition, by blending the algae-derived MFCs obtained by this disclosure with wood pulp, it is possible to improve interfiber bonds and elastic modulus, and it becomes possible to reduce or eliminate the beating process, which was conventionally performed to enhance interfiber bonds. Therefore, the algae-derived MFCs obtained by this disclosure have advantages such as being usable as a paper modifier aimed at reducing or eliminating the beating process.
[0010] According to a first aspect of this disclosure, algal microfibrillated cellulose and a method for producing the same can be provided as a substitute material for existing wood-derived CNF. Also according to a first aspect of this disclosure, paper and a paper modifier using the above algal microfibrillated cellulose can be provided. Furthermore, according to a second aspect of this disclosure, algal cellulose fiber bundles that have excellent transportability and allow for easy preparation of microfibrillated cellulose by a simple micronization process, and a method for producing the same, as well as microfibrillated cellulose and a method for producing the same using these cellulose fiber bundles, paper, a paper modifier, a paint, a building material, and a fiber reinforcement material can be provided.
[0011] This is an optical microscope image of the MFC obtained in Example 1A. This is an electron microscope image of the surface of the paper obtained in Example 2A. This figure shows the measurement results of the interfiber bonding strength factor for the paper obtained in Comparative Example 2A, Example 2A, and Example 4A. This figure shows the measurement results of the interfiber bonding strength factor for the paper obtained in Comparative Example 9A, Example 5A, and Example 6A. This figure shows the Young's modulus measurement results for the paper obtained in Comparative Example 9A, Example 5A, and Example 6A. This figure shows the specific tensile strength measurement results for the paper obtained in Comparative Example 9A, Example 5A, and Example 6A. This figure shows the opacity evaluation results for the paper obtained in Examples 7A-9A and Comparative Examples 10A-12A. This figure shows the change in filtration water content from 0 to 30,000 cumulative rotations of the propeller section of the disintegrator for Example 1B, etc. This figure shows the change in filtration water content from 0 to 500 cumulative rotations of the propeller section of the disintegrator for Example 1B, etc. This figure shows the change in average minor diameter from 0 to 30,000 cumulative rotations of the propeller section of the disintegrator for Example 1B, etc. This figure shows the change in the average minor diameter for the dissociator's propeller section from 0 to 500 cumulative rotations for Example 1B, etc. This is an optical microscope image of the algae-derived cellulose fiber bundle obtained in Example 1B. This is an optical microscope image of the algae-derived cellulose fiber bundle obtained in Example 2B. This is an optical microscope image of the algae-derived cellulose fiber bundle obtained in Example 3B. This is an optical microscope image of the algae-derived cellulose fiber bundle from Example 1B, which has been finely processed to a filtration degree of approximately 250 to 450 mL by stirring with the dissociator up to a cumulative rotation count of 50 for the propeller section. This is an optical microscope image of the algae-derived cellulose fiber bundle from Example 2B, which has been finely processed to a filtration degree of approximately 250 to 450 mL by stirring with the dissociator up to a cumulative rotation count of 50 for the propeller section. This is an optical microscope image of the algae-derived cellulose fiber bundle from Example 3B, which has been finely processed to a filtration degree of approximately 250 to 450 mL by stirring with the dissociator up to a cumulative rotation count of 50 for the propeller section. This is an optical microscope image of the cellulose fibers derived from algae in Example 1B, which were finely processed by stirring with a disintegrator up to a cumulative number of rotations of the propeller section of 5000. This is an optical microscope image of the cellulose fibers derived from algae in Example 2B, which were finely processed by stirring with a disintegrator up to a cumulative number of rotations of the propeller section of 5000.This is an optical microscope image of the cellulose fibers derived from algae in Example 3B, which were finely processed by stirring with a disintegrator up to a cumulative number of rotations of the propeller section of 5000. This figure shows the change in filtration efficiency from 0 to 5000 cumulative rotations of the PFI mill for Example 1B, etc. This figure shows the change in filtration efficiency from 0 to 500 cumulative rotations of the PFI mill for Example 1B, etc. This figure shows the change in average minor diameter from 0 to 5000 cumulative rotations of the PFI mill for Example 1B, etc. This figure shows the change in average minor diameter from 0 to 500 cumulative rotations of the PFI mill for Example 1B, etc.
[0012] The embodiments of this disclosure are described in detail below. However, this disclosure is not limited to the embodiments described below. In the embodiments described below, the components (including elemental steps, etc.) are not essential unless otherwise specified. The same applies to numerical values and their ranges, and do not limit this disclosure.
[0013] In this disclosure, the term "process" includes not only processes that are independent of other processes, but also processes that cannot be clearly distinguished from other processes, provided that the purpose of the process is achieved. In this disclosure, numerical ranges indicated using "~" include the numbers before and after "~" as the minimum and maximum values, respectively. In numerical ranges described in stages in this disclosure, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Also, in numerical ranges described in this disclosure, the upper or lower limit of that numerical range may be replaced with the values shown in the examples. In this disclosure, "disintegration" refers to the operation of dispersing fibers or fiber bundles in water by mechanical treatment using a standard disintegrator and disintegration conditions as defined in ISO 5263-1:2004. The defibration of fibers or fiber bundles progresses with the disintegration treatment. In this disclosure, "defibration" refers to a state in which fibers or fiber bundles are made finer by mechanical treatment, and in particular in this disclosure, includes cases that occur with disintegration treatment, beating treatment, etc. In this disclosure, "miniaturization" means reducing the average short diameter (fiber width) of a fiber or fiber bundle by performing a "disintegration treatment," "defibration treatment," or "beating treatment."
[0014] <Cellulose Fiber Bundles> The first cellulose fiber bundle of this disclosure is a cellulose fiber bundle derived from algae, having a filtration capacity of 400 mL or more as measured according to ISO 5267-2:2001, and a filtration capacity of 200 mL or less after disintegration treatment with a cumulative number of rotations of 10,000 under the conditions specified in ISO 5263-1:2004. The second cellulose fiber bundle of this disclosure is a cellulose fiber bundle derived from algae, having a filtration capacity of 400 mL or more as measured according to ISO 5267-2:2001, and a filtration capacity of 200 mL or less after disintegration treatment with a cumulative number of rotations of 1,000 using a PFI mill as defined in ISO 5264-2:2011. Hereinafter, the first and second cellulose fiber bundles of this disclosure may be collectively referred to as "the cellulose fiber bundles of this disclosure."
[0015] In the cellulose fiber bundles of this disclosure, the filtration capacity measured according to ISO 5267-2:2001 is set to 400 mL or more. When the filtration capacity of the fiber bundle is 400 mL or more, the fiber exhibits excellent filtration, dewatering, and transportability. The filtration capacity of the fiber bundle is preferably 500 mL or more, and more preferably 600 mL or more. The filtration capacity of the fiber bundle may be 800 mL or less from the viewpoint of fiber refinement. The filtration capacity of the fiber bundle may be between 400 mL and 800 mL. The Japanese Industrial Standard (JIS) corresponding to ISO 5267-2:2001 is JIS P8121-2:2012. The filtration capacity of the cellulose fiber bundle before and after disintegration treatment can be determined by the same method as for algae-derived microfibrillated cellulose described later. The method for adjusting the filtration capacity of the cellulose fiber bundle to 400 mL or more is not particularly limited. When producing cellulose fibers using the method for producing cellulose fiber bundles described later in this disclosure, the filtration rate can be adjusted to 400 mL or more by appropriately adjusting the treatment conditions in the preparation step, alkali treatment step, bleaching step, and acid treatment step.
[0016] In the first cellulose fiber bundle of this disclosure, the filtration capacity after disintegration treatment with a cumulative number of rotations of 10,000 under the conditions specified in ISO 5263-1:2004 is 200 mL or less. When the filtration capacity of the cellulose fiber bundle after disintegration treatment is 200 mL or less, microfibrillated cellulose can be easily prepared by a simple micronization treatment. The filtration capacity of the cellulose fiber bundle after disintegration treatment with a cumulative number of rotations is preferably 150 mL or less, and more preferably 100 mL or less. The filtration capacity of the cellulose fiber bundle after disintegration treatment with a cumulative number of rotations may be 20 mL or more from the viewpoint of adjusting the micronization of the fibers and processability. The filtration capacity of the cellulose fiber bundle after disintegration treatment with a cumulative number of rotations may be 20 mL to 200 mL. The method for adjusting the filtration efficiency of the cellulose fiber bundle after disintegration to 200 mL or less is not particularly limited, and the above-described method for adjusting the filtration efficiency of the cellulose fiber bundle to 400 mL or more can be applied. In particular, when producing cellulose fibers by the method for producing cellulose fiber bundles of this disclosure described later, appropriately adjusting the treatment conditions in the acid treatment step or the fiber bundle refinement conditions is effective in adjusting the filtration efficiency of the cellulose fiber bundle after disintegration to 200 mL or less.
[0017] In the first cellulose fiber bundle of this disclosure, the filtration capacity after disintegration treatment with a cumulative number of rotations of 3000 under the conditions specified in ISO 5263-1:2004 may be 200 mL or less. When the filtration capacity of the cellulose fiber bundle after disintegration treatment with a cumulative number of rotations of 3000 is 200 mL, microfibrillated cellulose can be easily prepared by a simpler refinement treatment. The filtration capacity of the cellulose fiber bundle after disintegration treatment with a cumulative number of rotations is preferably 150 mL or less, and more preferably 100 mL or less. The filtration capacity of the cellulose fiber bundle after disintegration treatment with a cumulative number of rotations may be 20 mL or more from the viewpoint of adjusting the refinement of the fibers and processability. The filtration capacity of the cellulose fiber bundle after disintegration treatment with a cumulative number of rotations may be 20 mL to 200 mL. Furthermore, in the first cellulose fiber bundle of this disclosure, the filtration efficiency after disintegration treatment with a cumulative number of rotations of 1000 under the conditions specified in ISO 5263-1:2004 may be 200 mL or less. If the filtration efficiency of the cellulose fiber bundle after disintegration treatment with a cumulative number of rotations of 1000 is 200 mL, microfibrillated cellulose can be easily prepared by an even simpler micronization treatment. The filtration efficiency of the cellulose fiber bundle after disintegration treatment with a cumulative number of rotations is preferably 150 mL or less, and more preferably 100 mL or less. The filtration efficiency of the cellulose fiber bundle after disintegration treatment with a cumulative number of rotations may be 20 mL or more from the viewpoint of adjusting the micronization of the fibers and processability. The filtration efficiency of the cellulose fiber bundle after disintegration treatment with a cumulative number of rotations may be 20 mL to 200 mL. The first cellulose fiber bundle of this disclosure preferably has a cumulative rotation count of 10,000 or less, more preferably 3,000 or less, and even more preferably 1,000 or less, required to achieve a filtration rate of 200 mL after disintegration treatment.
[0018] In the second cellulose fiber bundle of this disclosure, the filtration efficiency after beating treatment with a cumulative number of rotations of 1000 using a PFI mill as defined in ISO 5264-2:2011 is 200 mL or less. When the filtration efficiency of the cellulose fiber bundle after beating treatment with a cumulative number of rotations of 1000 using a PFI mill is 200 mL or less, microfibrillated cellulose can be easily prepared by a simple micronization treatment. The filtration efficiency of the cellulose fiber bundle after beating treatment with a cumulative number of rotations of 1000 using a PFI mill is preferably 150 mL or less, and more preferably 100 mL or less. The filtration efficiency of the cellulose fiber bundle after beating treatment with a cumulative number of rotations of 1000 using a PFI mill may be 20 mL or more from the viewpoint of fiber micronization, adjustment of the degree of beating, and processability. The filtration efficiency of the cellulose fiber bundle after beating treatment with a cumulative number of rotations of 1000 using a PFI mill may be 20 mL to 200 mL. The second cellulose fiber bundle of this disclosure preferably has a cumulative rotation count of 1,000 rotations or less, more preferably 500 rotations or less, and even more preferably 100 rotations or less, required to achieve a filtration rate of 200 mL after beating.
[0019] The cellulose fiber bundles of this disclosure preferably have an average minor diameter of 50 μm or more from the viewpoint of water filtration and dehydration, more preferably 100 μm or more, and even more preferably 200 μm or more. The average minor diameter of the cellulose fiber bundles of this disclosure may be 3000 μm or less from the viewpoint of fiber refinement. The average minor diameter of the cellulose fiber bundles of this disclosure may be between 50 μm and 3000 μm. The minor diameter of the cellulose fiber bundles of this disclosure refers to the minimum length in the direction perpendicular to the length direction of the structure to be measured (i.e., the cellulose fiber bundle). The minimum length in the direction perpendicular to the length direction of the structure to be measured refers to the value measured by optical microscope observation for each structure to be measured. The arithmetic mean of the values obtained for 100 structures to be measured is taken as the average minor diameter.
[0020] In the cellulose fiber bundles of this disclosure, after disintegration treatment with a cumulative rotation count of 10,000 cycles under the conditions specified in ISO 5263-1:2004, or after beating treatment with a cumulative rotation count of 1,000 cycles using a PFI mill as defined in ISO 5264-2:2011, the average minor diameter is preferably 1 / 3 or less of the average minor diameter before disintegration treatment or before beating treatment, from the viewpoint of fiber refinement and beating properties, more preferably 1 / 20 or less, and even more preferably 1 / 50 or less. The average minor diameter after disintegration treatment may be 1 / 50,000 or more of the average minor diameter before disintegration treatment. The average minor diameter after disintegration treatment may be 1 / 50,000 to 1 / 3 of the average minor diameter before disintegration treatment.
[0021] The cellulose fiber bundles of this disclosure are derived from algae. Using algae as a raw material leads to the utilization of blue carbon. Algae have a fibrous structure, and by processing the fibrous structure to make it finer, the microfibrillated cellulose described below can be obtained. The algae used in the preparation of the cellulose fiber bundles are not particularly limited. The algae may be red algae, or red algae having filamentous cells. Red algae are preferred from the viewpoint that they are widely used industrially worldwide and are readily available as algal residue. As for red algae, at least one species selected from the group consisting of the families Sarcodiaceae, Sarcodiaceae, Sarcodiaceae, Sarcodiaceae, Gelidaceae, Gelidaceae, Gracilaceae, and Pteridaceae is preferred. Examples of algae of the Sarcodiaceae family include Sarcodia ceylanica. Examples of algae of the Sarcodiaceae family include Mastocarpus yendoi. Examples of algae in the family Borealiaceae include Pyropia crassa. Examples of algae in the family Cephalicaceae include Chondracantha tenellus. Examples of algae in the family Gelidaceae include Gelidium elegans, Acanthopeltis japonica, and Pterocladiella tenuis. Examples of algae in the family Myrrhaceae include Kappaphycus alvarezii, Kappaphycus cottonii, and Eucheuma denticulatum (formerly known as Eucheuma spinosum). Examples of algae in the family Grateloupia asiatica include Gracilaria vermiculophylla. Among these, Gelidium elegans is preferred from the viewpoint of being able to utilize the residue after extracting edible components such as agar.
[0022] <Algae-derived microfibrillated cellulose> The first algae-derived microfibrillated cellulose of the present disclosure (hereinafter sometimes referred to as "algae-derived MFC") is algae-derived microfibrillated cellulose, wherein the average minor diameter (hereinafter also referred to as fiber width) of the microfibrillated cellulose is 1 μm to 10 μm, and the aspect ratio of the microfibrillated cellulose is 100 or more. The second algae-derived MFC of the present disclosure is algae-derived microfibrillated cellulose, wherein the average minor diameter of the microfibrillated cellulose is 30 nm to 1000 nm, and the aspect ratio of the microfibrillated cellulose is 100 or more. Hereinafter, the first algae-derived MFC and the second algae-derived MFC of the present disclosure may be collectively referred to as "the algae-derived MFC of the present disclosure".
[0023] The algae serving as the raw material for the algae-derived MFC of the present disclosure are not particularly limited. The algae may be red algae, and may be red algae having filamentous cells. Specific examples and preferred examples of the algae serving as the raw material for the algae-derived MFC of the present disclosure are the same as those for the cellulose fiber bundle of the present disclosure.
[0024] The fiber width of the first algae-derived MFC of the present disclosure is 1 μm to 10 μm. When the fiber width of the first algae-derived MFC is 1 μm or more, the handleability is excellent. The fiber width of the first algae-derived MFC is preferably 1.5 μm or more, more preferably 2 μm or more. When the fiber width of the first algae-derived MFC is 10 μm or less, the strength, transparency and the like after molding are improved. The fiber width of the first algae-derived MFC is preferably 8 μm or less, more preferably 6 μm or less. The fiber width of the second algae-derived MFC of the present disclosure is 30 nm to 1000 nm. When the fiber width of the second algae-derived MFC is 30 nm or more, the processability and productivity are excellent. The fiber width of the second algae-derived MFC is preferably 100 nm or more, more preferably 200 nm or more. When the fiber width of the second algae-derived MFC is 1000 nm or less, the fiber surface area and the fiber network forming ability are increased, and the reinforcing effect is improved. The fiber width of the second algae-derived MFC is preferably 800 nm or less, more preferably 500 nm or less.
[0025] The fiber width of algae-derived MFCs is determined by measuring the fiber width of each individual fiber using a fiber tester (manufactured by ABB Corporation) and taking the arithmetic mean of the fiber widths of a total of 10,000 fibers. It is desirable to disperse the fibers in water, as they condense due to hydrogen bonding when dry. For example, the fibers can be dispersed in water by immersing them in water at approximately 20°C for 180 minutes and stirring them with a magnetic stirrer at 120 rpm for about 10 minutes. If the algae-derived MFCs become finer, the fiber width of each target structure can be measured using an optical microscope or electron microscope, and the arithmetic mean of the values obtained for 100 target structures can be used as the fiber width.
[0026] The fiber length of the algae-derived MFCs in this disclosure is not particularly limited, and the aspect ratio of fiber length to fiber width (fiber length / fiber width) is as long as it is the value described below. The fiber length of the first algae-derived MFC may be, for example, 300 μm or more. If the fiber length of the first algae-derived MFC is 300 μm or more, it has excellent handling properties and improved strength after molding. The fiber length of the first algae-derived MFC is preferably 400 μm or more, and more preferably 500 μm or more. The upper limit of the fiber length of the first algae-derived MFC is not particularly limited, and may be, for example, 1000 μm or less. The fiber length of the second algae-derived MFC may be, for example, 5 μm or more. If the fiber length of the second algae-derived MFC is 5 μm or more, it has improved handling properties. The fiber length of the second algae-derived MFC is preferably 8 μm or more, and more preferably 10 μm or more. The upper limit of the fiber length of the second algae-derived MFC is not particularly limited and may be, for example, 20 μm or less. The method for measuring the fiber length is the same as the method for measuring the fiber width.
[0027] The aspect ratio of the algae-derived MFCs in this disclosure is 100 or higher. When the aspect ratio of the algae-derived MFCs is 100 or higher, the strength of the paper containing the algae-derived MFCs tends to improve. The aspect ratio of the algae-derived MFCs is preferably 150 or higher, and more preferably 200 or higher. The upper limit of the aspect ratio of the algae-derived MFCs is not particularly limited and may be, for example, 300 or less. The aspect ratio refers to the value obtained by dividing the fiber length of the algae-derived MFCs by the fiber width (fiber length / fiber width). Specifically, the aspect ratio of the algae-derived MFCs is obtained by measuring the fiber width and fiber length of each individual fiber using a fiber tester (manufactured by ABB Ltd.), calculating the aspect ratio of each fiber from the obtained values, and taking the arithmetic mean of the aspect ratios of a total of 10,000 fibers. Furthermore, if the fibers being measured are in a dry state, they will condense due to hydrogen bonding; therefore, it is desirable to disperse the fibers in water. The method for dispersing the fibers in water is the same as for measuring fiber width.
[0028] In the first embodiment, the filtration capacity of the algae-derived MFC of this disclosure is preferably 400 mL or less, more preferably 300 mL or less, and even more preferably 200 mL or less, from the viewpoint of increasing the strength of the paper. In this case, the filtration capacity may be 50 mL or more. In a certain embodiment, the filtration capacity of the algae-derived MFC is preferably 50 mL to 400 mL, more preferably 50 mL to 300 mL, and even more preferably 50 mL to 200 mL. In the second embodiment, the filtration capacity of the algae-derived MFC of this disclosure is preferably 200 mL or more, more preferably 300 mL or more, even more preferably 400 mL or more, and particularly preferably 500 mL or more, from the viewpoint of handling. In this case, the filtration capacity may be 700 mL or less. In other embodiments, the filtration capacity of the algae-derived MFC is preferably 200 mL to 700 mL, more preferably 300 mL to 700 mL, even more preferably 400 mL to 700 mL, and particularly preferably 500 mL to 700 mL. In a third embodiment of the algae-derived MFC of this disclosure, from the viewpoint of fiber refinement, the filtration capacity is preferably 200 mL or less, more preferably 150 mL or less, even more preferably 130 mL or less, and particularly preferably 80 mL or less. In this case, the filtration capacity (CSF) may be 5 mL or more, 10 mL or more, 20 mL or more, 30 mL, or 50 mL or more. In a third embodiment, the filtration capacity of the algae-derived MFC is preferably 5 mL to 200 mL, more preferably 10 mL to 150 mL, and even more preferably 20 mL to 150 mL. The filtration capacity of the algae-derived MFC refers to the value obtained by the following method. Disperse 3.0 g of algae-derived MFCs (Myoplastic Fruit Cells) with an oven-dry mass thoroughly in water to prepare a 1 L suspension with a concentration of 0.03%. Place 1 L of this suspension into a filter cylinder and measure the amount of filtered water discharged from the side tube. Record the water temperature at that time. Correct the filter yield according to JIS P 8121-2:2012 Pulp - Filter yield test method - Part 2: Canadian standard filter yield method and ISO 5267-2:2001 to obtain the Canadian standard filter yield. Note that the oven-dry mass refers to the value measured when the material is dried at 105°C until there is no change in mass. As a Canadian standard filter yield tester, a Canadian Free Nest Tester manufactured by Kumagai Riki Kogyo Co., Ltd. can be used. In this disclosure, "filter yield" means Canadian standard filter yield.
[0029] <Method for producing cellulose fiber bundle and method for producing algae-derived MFC> The method for producing a cellulose fiber bundle of the present disclosure may be any method. Examples thereof include a method of mechanically refining using algae as a raw material, a method by TEMPO catalytic oxidation, a method using an enzyme such as cellulase, and the like. From the viewpoint of enabling the cellulose fiber bundle to be produced by a simple method, the cellulose fiber bundle of the present disclosure is produced by the method for producing a cellulose fiber bundle of the present disclosure, which includes a preparation step of preparing an algae residue in which at least a part of solvent-soluble components has been removed from algae, an alkali treatment step of immersing the algae residue in an aqueous alkali solution, a bleaching step of bleaching the algae residue that has undergone the alkali treatment step, and an acid treatment step of immersing the algae residue that has undergone the bleaching step in an aqueous acid solution. The cellulose fiber bundle may be one obtained by the method for producing a cellulose fiber bundle of the present disclosure. The method for producing a cellulose fiber bundle of the present disclosure preferably includes the above-described preparation step, alkali treatment step, bleaching step, and acid treatment step in this order. The algae are not particularly limited, and examples thereof include at least one algae selected from the group consisting of the family Bangiaceae, the family Gigartinaceae, the family Phyllophoraceae, the family Ceramiaceae, the family Gelidiaceae, the family Solieriaceae, the family Gracilariaceae, and the family Caulacanthaceae. Specific examples of these algae are as described above. Hereinafter, each step of the method for producing a cellulose fiber bundle of the present disclosure will be described. The method for producing a cellulose fiber bundle of the present disclosure includes a preparation step, an alkali treatment step, a bleaching step, and an acid treatment step, and may further include other steps such as a neutralization step and a drying step as necessary.
[0030] (Preparation Step) In the preparation step, an algae residue in which at least a part of solvent-soluble components has been removed from algae is prepared. The method for preparing the algae residue is not particularly limited, and for example, a residue obtained after extracting edible components, which is generated by extracting water-soluble components and processing them into agar or the like, may be obtained and used as the algae residue. Using the residue after edible component extraction is desirable because it provides an algae residue in which water-soluble components have been removed to some extent, thereby reducing the burden of treatments such as solvent extraction in the preparation step. It also leads to effective utilization of waste.
[0031] Algal residue may be prepared by removing at least some of the solvent-soluble components from algae. In this case, algal residue may be prepared using algae as waste removed from freshwater or saltwater environments. Alternatively, algal residue may be prepared by further removing at least some of the solvent-soluble components from algal residue after extraction of edible components. Examples of solvent-soluble components include sugars such as starch, agarose, alginic acid, and carrageenan, coloring components such as chlorophyll, and proteins. Methods for removing at least some of the solvent-soluble components from algae may include immersing the algae in a solvent and heating it, and, if necessary, immersing the heated algae in an organic solvent. When heating, a low concentration of acid or alkali may be added to the solvent, or mechanical pressure may be applied to improve the effect of removing solvent-soluble components. When a low concentration of acid is added to the solvent, the pH of the solvent may be 4 to 5. When a low concentration of alkali is added to the solvent, the pH of the solvent may be 8 to 9. In this disclosure, the pH of an aqueous solution refers to the value measured using a pH meter in an environment of 25°C.
[0032] Suitable solvents include water, alcohol-based solvents such as methanol and ethanol, and ketone-based solvents such as acetone and methyl ethyl ketone. Among these, water is preferred from the viewpoint of reducing the burden on the environment. As an organic solvent for immersing heated algae, ethanol is preferred from the viewpoint of productivity and reducing the burden on the environment.
[0033] The heating time is not particularly limited, but from the viewpoint of efficiency, 10 to 240 minutes is preferred, and 100 to 180 minutes is more preferred. The temperature of the solution when heated is not particularly limited, but from the viewpoint of efficiency, 75°C to 100°C is preferred, and 85°C to 100°C is more preferred. The operation of immersing the algae in the solvent and heating may be done once or repeatedly. The number of repetitions may be 2 to 5 times. When immersing the heated algae in an organic solvent, the immersion time is not particularly limited, but from the viewpoint of handling, 5 to 1440 minutes is preferred, and 720 to 1440 minutes is more preferred.
[0034] The algae that have undergone the above treatment can be removed to obtain a fibrous residue. If water is used as the solvent, it is preferable not to dry the fibrous residue, but it may be dried to facilitate long-term storage and transportation.
[0035] (Alkali Treatment Process) In the alkali treatment process, the algal residue is immersed in an alkaline aqueous solution. Immersion of the algal residue in an alkaline aqueous solution makes it possible to remove protein components, sugars, coloring components, and other components remaining in the algal residue. The pH of the alkaline aqueous solution is preferably 9 to 14, more preferably 9 to 12, and even more preferably 10 to 12. Examples of alkaline components include sodium hydroxide, sodium carbonate, and calcium hydroxide. Among these, sodium hydroxide is preferred from the viewpoint of convenience as it can raise the pH with a small amount. The concentration of the alkaline component in the alkaline aqueous solution can be adjusted as appropriate so that the pH of the alkaline aqueous solution reaches the desired value. When sodium hydroxide is used as the alkaline component, it may be added at a concentration of 1% to 10% by mass of the oven-dry mass of the algal residue to be treated. The immersion time when immersing the algal residue in the alkaline aqueous solution is not particularly limited, but from the viewpoint of efficiency, it is preferably 30 to 120 minutes, and more preferably 60 to 90 minutes. The temperature of the alkaline aqueous solution is preferably 20°C to 100°C, and more preferably 40°C to 100°C. From the viewpoint of efficiency, the concentration of algal residue immersed in the alkaline aqueous solution (pulp concentration) is preferably 1% by mass or more. The pulp concentration may be 2% to 5% by mass, 5% to 10% by mass, or 10% to 25% by mass. The operation of immersing the algal residue in the alkaline aqueous solution may be performed once or repeated two or more times. The number of repetitions may be two to five times. When the operation of immersing in the alkaline aqueous solution is repeated two or more times, the type and concentration of the alkaline component may be the same or different.
[0036] (Bleaching Process) In the bleaching process, the algal residue that has undergone the alkaline treatment process is bleached. By bleaching the algal residue, it is possible to remove protein components, sugars, coloring components, and other components remaining in the algal residue. It is particularly useful for removing coloring components. One method of bleaching the algal residue is to immerse the algal residue in a bleaching solution. The bleaching agent used for bleaching algal fibers is not particularly limited, and bleaching agents commonly used in the paper industry can be used. Examples of bleaching agents include hypochlorite, hydrogen peroxide, chlorine dioxide, and ozone. Among these, from the viewpoint of availability, it is preferable that the bleaching agent contains at least one selected from the group consisting of hypochlorite, hydrogen peroxide, chlorine dioxide, and ozone, and more preferably at least one selected from the group consisting of hypochlorite, hydrogen peroxide, and chlorine dioxide. The concentration of the bleaching agent in the bleaching solution can be appropriately set in consideration of the type of bleaching agent, the amount of algal residue added to the bleaching solution, the reaction efficiency, etc. When 100% hydrogen peroxide is used as a bleaching agent, it is preferable to use it in an oven-dry mass ratio of 1% to 15% of the algal residue to be bleached. When hypochlorite is used as a bleaching agent, it is preferable to use it in an oven-dry mass ratio of 1% to 15% of the algal residue to be bleached. The immersion time when immersing the algal residue in the bleaching solution is not particularly limited, but from the viewpoint of efficiency, 30 to 120 minutes is preferred, and 60 to 90 minutes is more preferred. The pH of the bleaching solution is preferably 9 to 12, and more preferably 10 to 12. The temperature of the bleaching solution is preferably 20°C to 60°C, and more preferably 30°C to 60°C. The concentration (pulp concentration) of the algal residue immersed in the bleaching solution is preferably 2% or more by mass, may be 5% to 7.5% by mass, 7.5% to 10% by mass, or 10% to 25% by mass. Productivity can be improved by bleaching the algal residue while maintaining an algal residue concentration (pulp concentration) of 5% by mass or more. The process of immersing the algal residue in the bleaching solution may be done once or repeated two or more times. The number of repetitions may range from two to five.When the process of immersing in a bleach solution is repeated two or more times, the type and concentration of the bleach may be the same or different.
[0037] When bleaching wood-derived fibers, the pulp concentration of the wood-derived fibers is generally kept below 10% by mass. In the case of wood-derived fibers, it is necessary to remove protein components and bleach coloring substances such as lignin in a multi-stage process. For example, the bleaching sequence for typical cedar kraft pulp (used for copy paper with a whiteness of 80% to 90%) often goes through the DEHD or DEHED process, where alkaline extraction is (E), hypochlorous acid treatment is (H), and chlorine dioxide treatment is (D). Hydrogen peroxide treatment (P) is often used as a finishing step because its bleaching power is weak. Since algal residue does not contain lignin, which is a coloring substance that needs to be bleached, it is sometimes possible to achieve a whiteness of 85% or more by going through simplified processes such as EH, ED, and EP. Using algal residue offers advantages over using wood-derived fibers, as it is less environmentally invasive, inexpensive, and allows bleaching with hydrogen peroxide alone, which has inferior bleaching power. Overall, it tends to reduce processing time, chemical usage, and environmental impact.
[0038] (Acid Treatment Process) In the acid treatment process, the algal residue that has undergone the bleaching process is immersed in an acidic aqueous solution. Immersion of the algal residue in the acidic aqueous solution makes it easier to break down the algal fibers contained in the algal residue. As a result, it becomes possible to easily obtain MFC fibers by going through the fine-graining process described later. The solvent for the acidic aqueous solution is mainly water. Examples of acidic components include hydrochloric acid, sulfuric acid, and acetic acid. The pH of the acidic aqueous solution is preferably 1 to 4, and more preferably 2 to 3. The concentration of the acidic component in the acidic aqueous solution can be adjusted as appropriate so that the pH of the acidic aqueous solution reaches a desired value. The immersion time when immersing the algal residue in the acidic aqueous solution is not particularly limited, but from the viewpoint of efficiency, it is preferably 30 to 120 minutes, and more preferably 60 to 90 minutes. The temperature of the acidic aqueous solution is preferably 20°C to 60°C, and more preferably 30°C to 60°C. From the viewpoint of efficiency, the concentration of algal fibers (pulp concentration) immersed in the acidic aqueous solution is preferably 1% by mass or more. The pulp concentration may be 2% to 5% by mass, 5% to 10% by mass, or 10% to 25% by mass. The operation of immersing the algal residue in the acidic aqueous solution may be performed once or repeated two or more times. The number of repetitions may be two to five times. When the operation of immersing in the acidic aqueous solution is repeated two or more times, the type and concentration of the acid component may be the same or different.
[0039] (Neutralization step) After the acid treatment step, a neutralization step may be performed to neutralize the acidic aqueous solution containing the algal residue that has undergone the acid treatment step. By neutralizing the acidic aqueous solution containing the algal residue, the hydrolysis of cellulose fibers contained in the algal residue can be suppressed. As a method for neutralizing the acidic aqueous solution containing the algal residue, for example, an alkaline component such as sodium hydroxide or sodium bicarbonate can be added to the acidic aqueous solution. The pH after neutralization is preferably 6 to 7.
[0040] The method for producing algae-derived MFCs according to this disclosure may be any method. For example, methods include using algae (preferably red algae, more preferably red algae having filamentous cells) as a raw material and mechanically micronizing them, a method using TEMPO-catalyzed oxidation, a method using enzymes such as cellulase, etc. From the viewpoint of enabling the production of algae-derived MFCs by a simple method, the algae-derived MFCs according to this disclosure may be obtained by a method for producing algae-derived MFCs that includes a preparation step of preparing an algal residue from which at least a portion of solvent-soluble components have been removed from algae, an alkali treatment step of immersing the algal residue in an alkaline aqueous solution, a bleaching step of bleaching the algal residue after the alkali treatment step, and an acid treatment step of immersing the algal residue after the bleaching step in an acid aqueous solution. The details of each of these steps are the same as in the case of the method for producing cellulose fiber bundles described above. The method for producing algae-derived MFCs according to this disclosure may further include a micronization step of micronizing the cellulose fiber bundle obtained through the method for producing cellulose fiber bundles according to this disclosure described above.
[0041] (Micronization Process) In the method for producing algae-derived MFCs according to the present disclosure, a micronization process may be carried out to micronize the algal residue after the acid treatment process, or after a neutralization process which is carried out as necessary. Micronization of the algal residue is carried out by mechanical treatment. Specifically, the mechanical treatment is carried out by agitators such as pulpers and mixers, beating machines such as refiners, beaters, and PFI mills, kneaders and dispersers which involve the action of metal or blades on the fibers around a rotating shaft, or by friction between fibers, and defibration and micronization proceed. The micronization treatment conditions are not particularly limited and may be adjusted as appropriate depending on the type of mechanical treatment used. The degree to which the algal residue is micronized is not particularly limited. In the micronization process, the average short diameter of the cellulose fiber bundles may be micronized to 1 / 10 or less of the diameter before the micronization process, or to 10 μm or less.
[0042] <Paper> The paper of the present disclosure contains the algae-derived MFC of the present disclosure. Since the paper of the present disclosure contains the algae-derived MFC of the present disclosure, it leads to the utilization of blue carbon. Furthermore, since the paper of the present disclosure contains the algae-derived MFC of the present disclosure, it is characterized by high density and high elasticity. In addition, due to its high density, there are few gaps between fibers in the paper, and it has the feature of high paper transparency.
[0043] The basis weight of the paper of the present disclosure is preferably 5 g / m from the viewpoint of handleability 2 or more, more preferably 10 g / m 2 or more, and even more preferably 15 g / m 2 or more. The basis weight of the paper of the present disclosure may be 100 g / m 2 or less, may be 60 g / m 2 or less, is preferably 30 g / m from the viewpoint of transparency 2 or less, more preferably 25 g / m 2 or less, and even more preferably 20 g / m 2 or less. The basis weight of the paper of the present disclosure is preferably 5 g / m 2 to 100 g / m 2 , more preferably 10 g / m 2 to 60 g / m 2 , and even more preferably 15 g / m 2 to 30 g / m 2 . From the viewpoint of handleability, the basis weight of the paper may be 60 g / m 2 . The basis weight of paper refers to the value obtained by the following method. The basis weight of paper is determined by dividing the mass (g) of the paper measured with a balance by the area (m 2 ) of the paper.
[0044] The density of the paper of the present disclosure is preferably 0.85 g / cm from the viewpoint of transparency 3 or more, more preferably 1.0 g / cm 3 or more, and even more preferably 1.1 g / cm 3 or more. The density of the paper of the present disclosure is preferably 1.4 g / cm from the viewpoint of flexibility 3 or less, more preferably 1.3 g / cm 3 or less, and even more preferably 1.2 g / cm 3 or less. The density of the paper of the present disclosure is 0.85 g / cm 3 to 1.4 g / cm 3Preferably, 1.0 g / cm³ 3 ~1.3 g / cm 3 More preferably, 1.1 g / cm³ 3 ~1.2 g / cm 3 This is even more preferable. The density of paper refers to the value obtained by the following method. The density of paper is calculated by multiplying the mass of the paper (g) measured on a scale by the area of the paper (m²). 2 Divide by ) to get basis weight (g / m²) 2 ) is calculated, and then divided by the thickness of the paper (μm) to find the answer.
[0045] The smoothness of the paper disclosed herein (Wang Ken smoothness) is preferably 25 seconds or more, more preferably 30 seconds or more, and even more preferably 60 seconds or more, from the viewpoint of printability. From the viewpoint of texture, the smoothness of the paper disclosed herein is preferably 60 seconds or less, more preferably 55 seconds or less, and even more preferably 50 seconds or less. The smoothness of the paper disclosed herein is preferably 25 seconds to 60 seconds. The Wang Ken smoothness (seconds) is measured according to JIS P 8155:2010 Paper and cardboard - Smoothness test method - Wang Ken method.
[0046] The specific tensile strength of the paper disclosed herein is preferably 15 N·m / g or more, more preferably 18 N·m / g or more, and even more preferably 20 N·m / g or more, from the viewpoint of durability. The upper limit of the specific tensile strength of the paper disclosed herein is not particularly limited and may be 100 N·m / g or less, 80 N·m / g or less, or 60 N·m / g or less. The specific tensile strength of the paper disclosed herein may be between 15 N·m / g and 100 N·m / g, between 18 N·m / g and 80 N·m / g, or between 20 N·m / g and 60 N·m / g. The specific tensile strength of the paper is determined by dividing the breaking load of the paper by the product of the basis weight of the paper and the width of the test piece (15 mm in the example below). The breaking load of the paper is determined by preparing 30 test pieces with a width of 15 mm and conducting tensile tests in a constant temperature and humidity chamber under environmental conditions of 23°C and 23%RH to 28%RH, using a tensile testing machine with a grip spacing of 100 mm and a tensile speed of 10 mm / min. The arithmetic mean of the values obtained is calculated from these tests. The MCT series benchtop tensile and compression testing machine from A&D Company, Limited can be used as the tensile testing machine.
[0047] The Young's modulus of the paper in this disclosure is preferably 5 GPa or higher, more preferably 6 GPa or higher, and even more preferably 7 GPa or higher, from the viewpoint of stiffness. The upper limit of the Young's modulus of the paper in this disclosure is not particularly limited and may be 10 GPa or less, 9 GPa or less, or 8 GPa or less. The Young's modulus of the paper in this disclosure may be between 5 GPa and 10 GPa, between 6 GPa and 9 GPa, or between 7 GPa and 8 GPa. The Young's modulus of the paper is calculated as the ratio of the tensile load per unit area to the elongation per unit length in the elastic region of the paper.
[0048] The tensile elongation at break of the paper disclosed herein is preferably 0.5% or more, more preferably 1% or more, and even more preferably 1.5% or more, from the viewpoint of durability. The tensile elongation at break of the paper disclosed herein is preferably 3% or less, more preferably 2.5% or less, and even more preferably 2% or less, from the viewpoint of handling. The tensile elongation at break of the paper disclosed herein is preferably 0.5% to 3%, more preferably 1% to 2.5%, and even more preferably 1.5% to 2%. The tensile elongation at break of the paper is calculated from data obtained under the same conditions as the measurement of the paper's breaking load.
[0049] From the viewpoint of handling, the thickness of the paper of this disclosure is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more. The thickness of the paper of this disclosure may be 100 μm or less, 90 μm or less, or 85 μm or less. From the viewpoint of transparency, the thickness of the paper of this disclosure is preferably 60 μm or less, more preferably 50 μm or less, and even more preferably 40 μm or less. In one embodiment, the thickness of the paper of this disclosure is preferably 10 μm to 100 μm, more preferably 20 μm to 90 μm, and even more preferably 30 μm to 85 μm. In another embodiment, the thickness of the paper of this disclosure is preferably 10 μm to 60 μm, more preferably 20 μm to 50 μm, and even more preferably 30 μm to 40 μm. The paper thickness refers to the value obtained by the following method. In accordance with JIS P8118:2014 Paper and cardboard — Test methods for thickness, density and specific volume, the thickness of each test paper is measured at three points using a micrometer, and the arithmetic mean of the obtained values is taken as the thickness of each test paper. The thickness of five test papers is determined, and the arithmetic mean of the thicknesses of the five test papers is taken as the paper thickness.
[0050] From the viewpoint of color reproducibility by printing, the whiteness of the paper disclosed herein is preferably 75% or more, more preferably 80% or more, even more preferably 85% or more, and particularly preferably 100%. From the viewpoint of reducing the load in the bleaching process, the whiteness of the paper disclosed herein is preferably 90% or less, more preferably 87% or less, even more preferably 82% or less, and particularly preferably 77% or less. The whiteness of the paper disclosed herein may be 75% to 87%, 80% to 90%, 85% to 100%, or 75% to 100%. The whiteness of the paper represents the ratio of reflected light when light is shone on the surface of a test piece. The whiteness of the paper refers to ISO whiteness (JIS P 8148:2018 (ISO 2470-1:2016)). The whiteness of paper can be measured using the Spectrophotometer for Paper PF7000 from Nippon Denshoku Industries, Ltd.
[0051] The paper of this disclosure may further contain wood-derived pulp as needed. Examples of wood-derived pulp include mechanical pulp (broken wood pulp, refiner mechanical pulp, or thermomechanical pulp), semi-chemical pulp (semi-chemical pulp, or chemiground pulp), chemical pulp (kraft pulp, or sulfite pulp), and recycled paper pulp (disintegrated pulp, or deinked pulp). More specifically, examples of wood-derived pulp include bleached hardwood kraft pulp (bleached hardwood pulp fibers (LBKP)), bleached softwood kraft pulp (bleached softwood pulp fibers (NBKP)), and recycled paper pulp. Examples of recycled paper used as raw material for recycled paper pulp include newspapers, flyers, textured magazines, coated magazines, pressure-sensitive recording paper, imitation paper, colored fine paper, copy paper, computer output paper, and mixtures thereof.
[0052] If the paper of this disclosure contains wood-derived pulp, the proportion of wood-derived pulp in the total paper may be 20% to 50% by mass, 10% to 20% by mass, or 10% to 15% by mass in one embodiment. In other embodiments, it may be 70% to 99% by mass, 75% to 98% by mass, or 80% to 97% by mass.
[0053] The paper disclosed herein may contain various additives as needed, such as dyes, fluorescent whitening agents, pH adjusters, defoamers, and sizing agents. The amount of additives is not particularly limited, and only the amount necessary for each additive to exhibit its function should be added.
[0054] The strength of paper is determined by two factors: the strength of the individual fibers and the strength of the interfiber bonds. In most wood-derived papers, the interfiber bonds are the bottleneck that causes breakage, while in papers obtained from algae-derived MFCs, the strength of the individual fibers is the bottleneck that causes breakage. Therefore, in papers obtained by using both types of fibers in combination, the bottlenecks of each fiber can be compensated for, and it is possible to change the physical properties compared to papers obtained using each fiber alone.
[0055] In one embodiment, the paper of this disclosure may have an opacity of 20% or less. In another embodiment, the paper of this disclosure may have a basis weight of 30 g / m². 2 ~100g / m 2 Under these conditions, the opacity may be 80% or less, 50% or less, or 20% or less. In order to achieve the opacity within the above range, the paper of this disclosure may be impregnated with starch, polysaccharides such as glucomannan, oils and fats, waxes, natural resins, polycaprolactone, synthetic resins such as polyethylene, etc. In other embodiments, the paper of this disclosure may be impregnated with at least one selected from the group consisting of polysaccharides, oils and fats, waxes, natural resins, and synthetic resins, and have an opacity of 80% or less. In recent years, research has been conducted on giving transparency to paper as an alternative to plastic. Cellulose contained in algae-derived MFCs is inherently nearly transparent, but when made into paper, light is refracted and diffusely reflected by the gaps between the fibers, making it appear white. However, by filling the gaps between the fibers with oils that have a refractive index close to that of cellulose, it is possible to give transparency to the paper. The algae-derived MFCs of this disclosure have a fiber width that is less than half that of wood pulp and are equivalent to general MFCs. As a result, the paper tends to have a higher density, with fewer gaps between fibers, which is advantageous for imparting transparency.
[0056] The papermaking method is not particularly limited and can be carried out using known papermaking equipment. Examples of papermaking equipment include wire screen machines, round screen machines, cylinders, and twin wire machines. To improve the surface smoothness of the paper, surface treatment may be performed by applying heat and pressure during or after the papermaking process. Specific surface treatment methods include calendering, such as machine calendering and supercalendering. If the paper of this disclosure contains wood-derived pulp, the algae-derived MFC and wood-derived pulp may be mixed after the acid treatment process or the finening process, if necessary. Alternatively, the algae-derived MFC and wood-derived pulp may be mixed and both finened together.
[0057] <Paper Modifier> The paper modifier of this disclosure contains algae-derived MFCs as disclosed. The paper modifier of this disclosure exhibits different properties from wood-derived fibers. Therefore, by adding the paper modifier of this disclosure to paper containing wood-derived fibers, it is possible to obtain paper that exhibits different properties compared to paper made solely from wood-derived fibers. For example, it may be possible to strengthen the interfiber bonding force of wood-derived fibers and improve the Young's modulus. The amount of paper modifier to be added is not particularly limited and can be any amount that results in paper exhibiting the desired properties.
[0058] <Paints, Building Materials, and Fiber Reinforcements> The algae-derived MFCs of this disclosure can be used not only as a paper modifier but also as various additives. The algae-derived MFCs are materials that exhibit excellent hygroscopicity, water absorption, processability, and lightweight properties, and can be used as additives. The algae-derived MFCs can be used as additives contained in paints, building materials, and fiber reinforcements. The paints of this disclosure may contain the algae-derived MFCs of this disclosure. The building materials of this disclosure may contain the algae-derived MFCs of this disclosure. The fiber reinforcements of this disclosure may contain the algae-derived MFCs of this disclosure.
[0059] The present disclosure will be further explained with reference to the following examples. The materials, amounts used, proportions, processing procedures, etc., shown in the following examples can be modified as appropriate, as long as they do not deviate from the spirit of the present disclosure. Therefore, the present disclosure should not be interpreted restrictively by the following specific examples. The pH values described in the examples refer to values measured using a pH meter (EX-20, manufactured by Horiba, Ltd.) in an environment of 25°C.
[0060] [Example 1A] The MFC fibers of Example 1A were obtained by following the steps below. - Treatment of algal fibers - Gelidium elegans, a red alga of the family Gelidaceae, was immersed in water and boiled for 120 minutes. After that, the water was changed and the above steps were repeated to remove most of the water-soluble components contained in the algal fibers and obtain algal residue. The residue (agar shell) obtained by general agar production is supplied in a state where the above treatment has progressed. - Alkaline extraction - The algal residue was immersed in water, and sodium hydroxide of about 5% by mass of the oven-dry mass of the algal residue to be treated was added, and the algal residue was treated for 1 hour in an environment with an algal residue concentration of 10% by mass, pH: 10-12, and 60°C. - Bleaching - The algal residue was bleached for 1 hour in an aqueous sodium hypochlorite solution (available chlorine at 10% by mass of the oven-dry mass of the algal residue) at an algal residue concentration of 10% by mass, pH: 10-11, and 60°C. This bleaching treatment was repeated twice. - Acid treatment - The bleached algal residue was acid-treated for 1 hour in an aqueous hydrochloric acid solution prepared to pH 2 at an algal residue concentration of 10% by mass and 60°C. - Neutralization treatment - The acid-treated algal residue was neutralized to a pH of approximately 6 using an aqueous sodium hydroxide solution. The algal residue was also washed with a large amount of water. - Micronization treatment - After the acid treatment, the neutralized algal residue was placed in the mill house of a PFI mill (manufactured by Kumagai Riki Kogyo Co., Ltd., a beating machine) and beaten 100 times to obtain the algal-derived MFC of Example 1A. The filtration capacity of the algal-derived MFC of Example 1A was 120 mL.
[0061] [Example 2A] Papermaking was performed using the algae-derived MFC of Example 1A to obtain the paper of Example 2A. -Papermaking- Basis weight: 60 g / m² 2 The algae-derived MFC suspension of Example 1A (the area of the handmade sheet is 200 cm²) 2(800 mL was collected when the algae-derived MFC concentration was 0.15% by mass.) The algae-derived MFC suspension was placed in the cylinder of a handmade sheet apparatus filled with water to a height of 20 cm to 30 cm, and then water was added to the cylinder again. The perforated plate was moved up and down inside the cylinder to thoroughly mix the algae-derived MFC, then the water was drained and papermaking was performed. Two sheets of filter paper of the same size were placed on top of the wet paper formed on a wire mesh, and a metal plate was placed on top. The paper was moved back and forth with a cutty roll to absorb water, then the filter paper was removed and the test handmade paper was attached to the metal plate. -Press- The metal plate, paper, thin filter paper, and absorbent filter paper were stacked in that order and pressurized at a pressure of 410 kPa for 5 minutes. After pressurizing, the absorbent filter paper was replaced and pressurized again for 2 minutes. -Drying- The absorbent filter paper was removed, and the paper was dried by sandwiching it with tension drying rings. Subsequently, the dried paper was peeled off the metal plate, and then a thin filter paper was peeled off the dried paper. Through these steps, the paper of Example 2A, which contains fibers derived from Maxa, was obtained.
[0062] [Example 3A] - Preparation of MFC derived from Chondracantha - Algae-derived MFC for Example 3A was obtained in the same manner as in Example 1A, except that Chondracantha tenellus was used instead of Gelidium elegans of the family Gelidaceae. The filtration capacity of the algae-derived MFC for Example 3A was 220 mL.
[0063] [Example 4A] - Paper made using MFCs derived from Japanese cedar - Paper of Example 4A containing Japanese cedar fibers was obtained in the same manner as in Example 2A, except that the algae-derived MFCs of Example 3A were used instead of the algae-derived MFCs of Example 1A.
[0064] [Comparative Example 1A] - Preparation of bleached softwood pulp - Pulp for Comparative Example 1A was obtained from commercially available bleached softwood pulp fibers. Dried bleached softwood pulp fibers (NBKP) were soaked in plenty of water for 24 hours to allow the fibers to swell sufficiently with water. The pulp was sieved and the water was squeezed out by hand to a pulp concentration of 10% by mass. Then, the above pulp was placed in the mill house of a beating mill and the pulp was pressed evenly against the inner wall by hand. Then, a roll was lowered into the mill house, the mill house was rotated, and the roll was rotated and beaten 100 times. After that, the pulp was removed and thoroughly disintegrated using a disintegrator to obtain the pulp for Comparative Example 1A. The filtration efficiency of the pulp for Comparative Example 1A was 710 mL.
[0065] [Comparative Example 2A] - Paper production using bleached coniferous pulp - Papermaking was performed using the pulp from Comparative Example 1A to obtain the paper of Comparative Example 2A. - Papermaking - Basis weight 60 g / m² 2 The pulp suspension (the area of the handmade sheet is 200 cm²) 2 (800 mL was taken when the pulp concentration was 0.15% by mass.) The pulp was then disintegrated so that it was sufficiently dispersed. The pulp suspension was put into a cylinder of a handmade sheet apparatus filled with water to a height of 20 cm to 30 cm, and water was poured into the cylinder again. The perforated plate was moved up and down inside the cylinder to thoroughly agitate the pulp, then the water was drained and papermaking was performed. Two sheets of filter paper of the same size were placed on top of the wet paper formed on a wire mesh, and a metal plate was placed on top. The paper was moved back and forth with a cutty roll to absorb water, then the filter paper was removed and the test handmade paper was attached to the metal plate. -Press- The metal plate, paper, thin filter paper, and absorbent filter paper were stacked in that order and pressurized at a pressure of 410 kPa for 5 minutes. After pressurizing, the absorbent filter paper was replaced and pressurized again for 2 minutes. -Drying- The absorbent filter paper was removed, and the paper was dried by sandwiching it between tension drying rings. Subsequently, the dried paper was peeled off the metal plate, and then a thin filter paper was peeled off the dried paper. Through these steps, the paper of Comparative Example 2A, which contains bleached softwood pulp fibers, was obtained.
[0066] [Comparative Example 3A] Cellulose fibers derived from algae were obtained in the same manner as in Example 1A, except that no acid treatment or micronization treatment was performed, and the bleached algal residue was neutralized with hydrochloric acid. The filtration capacity of the cellulose fibers of Comparative Example 3A was 880 mL. [Comparative Example 4A] Paper of Comparative Example 4A was obtained in the same manner as in Example 2A, except that the cellulose fibers derived from the algal fibers of Comparative Example 3A were used. [Comparative Example 5A] Cellulose fibers derived from algal fibers of Comparative Example 5A were obtained in the same manner as in Example 1A, except that no acid treatment was performed on the bleached algal fibers, and neutralization and micronization treatments were performed with hydrochloric acid. The filtration capacity of the cellulose fibers of Comparative Example 5A was 325 mL. [Comparative Example 6A] Paper of Comparative Example 6A was obtained in the same manner as in Example 2A, except that the algal-derived cellulose fibers of Comparative Example 5A were used. [Comparative Example 7A] The bleached coniferous pulp obtained from Comparative Example 1A was subjected to the acid treatment shown in Example 1A to obtain the pulp of Comparative Example 4A. The filtration efficiency of the pulp in Comparative Example 7A was 715 mL. [Comparative Example 8A] Paper for Comparative Example 8A was obtained in the same manner as in Example 2A, except that the bleached coniferous kraft pulp of Comparative Example 7A was used.
[0067] <Evaluation> -Surface Observation- The algae-derived MFCs obtained in Example 1A were photographed with an optical microscope. The results are shown in Figure 1. To observe the surface of the paper obtained in Example 2A, electron microscope images were taken using a field emission scanning electron microscope (FE-SEM) (SU8020, Hitachi, Ltd.). Before observation, the sample was coated with platinum (Pt) by sputtering. The results are shown in Figure 2.
[0068] - Comparison of Fiber Shapes - The fiber width and fiber length of each individual fiber were measured using a fiber tester (manufactured by ABB Corporation), and the fiber width, fiber length, and aspect ratio of the fibers of Example 1A, Example 3A, Comparative Example 1A, Comparative Example 3A, Comparative Example 5A, and Comparative Example 7A were determined by taking the arithmetic mean of the measurement results for the fiber width, fiber length, and aspect ratio of a total of 10,000 fibers. The results obtained are shown in Table 1. The algae-derived MFCs obtained by this disclosure (Example 1A, Example 3A) had a fiber width of about 1 / 10 or less compared to general wood pulp fibers (Comparative Example 1A), and were found to be minute fibers that generally correspond to MFCs. In addition, the algae-derived MFCs tended to have a higher aspect ratio compared to general wood pulp fibers. The fibers of Comparative Example 3A had a larger fiber width compared to the others, and since branched gel fibers were preserved, it was impossible to measure the fiber length and aspect ratio. It was found that mechanical processing, such as beating using a PFI mill, is necessary to obtain non-branched fibers, compared to Example 1A and Comparative Example 5A. Compared to Comparative Example 5A (Maxa-derived fibers without the acid treatment step), the fiber width of the algae-derived fibers obtained without the acid treatment shown in this disclosure was about 25 μm, and minute fibers corresponding to MFCs could not be obtained. Therefore, it was found that the acid treatment step performed in Example 1A is necessary to obtain algae-derived MFCs. Compared to Comparative Example 7A (coniferous bleached kraft pulp with acid treatment), there was almost no difference in fiber shape compared to Comparative Example 1A even after acid treatment, and MFCs could not be obtained even when acid treatment was performed when the relevant algae was not used as the raw material.
[0069]
[0070] The density, specific tensile strength, and Young's modulus of the paper from Example 2A, Example 4A, Comparative Example 2A, Comparative Example 4A, Comparative Example 6A, and Comparative Example 8A were measured using the method described below. The results are shown in Table 2.
[0071]
[0072] In Example 1A, it was possible to obtain MFCs, which are fine cellulose fibers, by acid treatment, and the density, specific tensile strength, and Young's modulus of the paper produced in Example 2A using these MFCs were all the highest compared to the other examples and comparative examples. Furthermore, Comparative Examples 4A (paper using fibers derived from Maxa that were not acid-treated or micronized) and 6A (paper using fibers derived from Maxa that were not acid-treated) had lower density, Young's modulus, and specific tensile strength compared to Example 2A, indicating that the acid treatment and micronization treatment of algae fibers in this disclosure affect the physical properties of algae fibers and paper derived from algae. Comparing Comparative Example 2A and Comparative Example 8A, there was no significant difference in the physical properties of the resulting paper, indicating that the acid treatment did not affect the physical properties of bleached coniferous kraft pulp fibers or paper derived from them.
[0073] - Measurement of Interfiber Bond Strength Factor - Short-span tensile tests were performed on the papers of Example 2A, Example 4A, and Comparative Example 2A using a zero-span tensile testing machine (Pulmac), and the interfiber strength factor, an index indicating the strength of interfiber bonds, was determined. The results are shown in Figure 3. Comparing the interfiber bond strength factors, the papers made from algae-derived MFCs (Example 2A, Example 4A) had a factor approximately 1.75 times larger than the papers made from general wood pulp (Comparative Example 2A). This is thought to be because the algae-derived fibers are smaller, resulting in the formation of more interfiber bonds.
[0074] [Comparative Example 9A] Pulp for Comparative Example 9A was obtained in the same manner as for Comparative Example 1A, except that the pulp was beaten to a filtration capacity of 450 mL. Paper for Comparative Example 9A was obtained in the same manner as for Comparative Example 2A, except that the obtained pulp was used.
[0075] [Example 5A] - Paper production by mixing MFC derived from Maxa as a paper modifier with bleached softwood pulp - The MFC fibers of Example 1A were added to the pulp used in Comparative Example 9A so that the proportion of the MFC fibers of Example 1A in the total paper was 5% by mass (Example 5A-1), 10% by mass (Example 5A-2), 20% by mass (Example 5A-3), or 30% by mass (Example 5A-4) to obtain each mixed pulp. Papers of Examples 5A-1 to 5A-4 were obtained in the same manner as in Comparative Example 2, except that the obtained mixed pulp was used.
[0076] [Example 6A] - Paper production by mixing MFC derived from cedar algae as a paper modifier with bleached coniferous pulp - The pulp used in Comparative Example 9A was mixed with the MFC fibers of Example 3A so that the proportion of the MFC fibers of Example 3A in the total paper was 5% by mass (Example 6A-1), 10% by mass (Example 6A-2), 20% by mass (Example 6A-3), or 30% by mass (Example 6A-4) to obtain each mixed pulp. Papers of Examples 6A-1 to 6A-4 were obtained in the same manner as in Comparative Example 2A, except that the obtained mixed pulp was used.
[0077] - Measurement of Interfiber Bonding Strength Factor - Short-span tensile tests were performed on the paper of Comparative Example 9A, Example 5A (Example 5A-2) which incorporated 10% by mass of MFC fibers from Example 1A, which is derived from Maxa, and Example 6A (Example 6A-2) which incorporated 10% by mass of MFC fibers from Example 3A, which is derived from Suginori, using a zero-span tensile testing machine (manufactured by Pulmac) to determine the interfiber bonding strength factor, which is an index indicating the interfiber bonding strength. The obtained results are shown in Figure 4. Comparing the interfiber bonding strength factors, the paper incorporating algae-derived MFCs (Examples 5A and 6A) had greater interfiber bonding than the paper made only from wood pulp (Comparative Example 9A). Therefore, it is possible to increase the interfiber bonding strength factor by incorporating the algae-derived MFCs of this disclosure into wood pulp. Generally, beating is performed to increase interfiber bonding strength, but by incorporating the algae-derived MFCs of this disclosure into paper, it is possible to reduce or eliminate the beating process.
[0078] -Tensile Test- For the tensile test of the paper, 30 test pieces with a width of 15 mm were prepared and tested in a constant temperature and humidity chamber under environmental conditions of 23°C at a temperature of 23%RH to 28%RH, with a gripping distance of 10 cm on the tensile testing machine and a tensile speed of 10 mm / min. The arithmetic mean of the values obtained was taken. The tensile testing machine used was the MCT series benchtop tensile and compression testing machine from A&D Co., Ltd. Young's modulus and specific tensile strength were determined for the papers of Comparative Example 9A, Example 5A, and Example 6A. The obtained results are shown in Figures 5 and 6. Young's modulus was higher with increasing proportion of algae-derived MFCs. For specific tensile strength, the paper with 5% by mass of MFCs derived from Makusa and 5% by mass of MFCs derived from Suginori obtained the highest value for Example 5A. Furthermore, compared to the paper of Comparative Example 9A, which was made only from wood pulp, improvements were observed in both Young's modulus and specific tensile strength for the paper with algae-derived MFCs. The above has shown that blending the algae-derived MFCs of this disclosure into wood pulp improves the interfiber bonding strength. Therefore, the improvements in Young's modulus and specific tensile strength are thought to be due to the improved interfiber bonding strength resulting from the blending of algae-derived MFCs, making it possible to utilize them as a paper modifier. On the other hand, the strength of paper is thought to be determined by the strength of the fibers themselves and the interfiber bonding strength. Therefore, it is thought that the specific tensile strength will not continue to improve as the amount of algae-derived MFCs that improve interfiber bonding strength is increased.
[0079] <Transparency Evaluation> [Example 7A] Basis weight during papermaking: 30 g / m² 2 The paper of Example 7A was obtained in the same manner as in Example 2A, except that the pulp suspension was collected in such a manner.
[0080] [Example 8A] - Imparting transparency using starch aqueous solution - The paper of Example 7A was treated as follows and coated with starch to obtain the paper of Example 8A. A 10% by mass starch aqueous solution was obtained from starch powder. The paper of Example 7A (paper made of MFC derived from Maxa) was thoroughly immersed in the 10% by mass starch aqueous solution, fixed in place so as not to deform, and dried to obtain the paper of Example 8A.
[0081] [Example 9A] - Imparting transparency using polycaprolactone - Polycaprolactone (PCL) was heated at 80°C to obtain a melted PCL solution. The melted PCL solution was thoroughly applied to the surface of the paper of Example 7A and pressurized at 30 MPa and 75°C for 5 minutes. After pressurization, it was dried at room temperature to obtain the paper of Example 9A.
[0082] [Comparative Example 10A] Basis weight during papermaking: 30 g / m² 2 Paper for Comparative Example 10A was obtained in the same manner as for Comparative Example 2A, except that the pulp suspension was collected in such a manner.
[0083] [Comparative Example 11A] The paper of Comparative Example 10A was treated in the same manner as in Example 8A to coat it with starch to obtain the paper of Comparative Example 11.
[0084] [Comparative Example 12A] Polycaprolactone was applied to the paper of Comparative Example 10A in the same manner as in Example 9A to obtain the paper of Comparative Example 12A.
[0085] - Imparting Transparency and Measuring Opacity - The opacity of the papers in Examples 7A-9A and Comparative Examples 10A-12A was measured using a Spectrophotometer for Paper manufactured by Nippon Denshoku Industries Ltd. For a single sample, the luminous reflectance (%) and the intrinsic luminous reflectance (%) measured when the material was stacked until it was completely opaque were measured. The quotient obtained by multiplying the former by 100 and dividing the latter was defined as the opacity (%). Therefore, the lower the opacity, the more transparent it appears to the naked eye. The results obtained are shown in Figure 7. For Comparative Examples 10A-12A, which used paper derived from wood pulp, paper with approximately 10% lower opacity was obtained by applying starch aqueous solution or PCL. On the other hand, for Example 7A-9A, which used MFC derived from algae, paper with approximately 30% lower opacity was obtained by applying starch aqueous solution or PCL. Therefore, it was found that using the algae-derived MFCs of this disclosure is advantageous for imparting transparency when applying starch aqueous solutions or PCL.
[0086] [Example 1B] (Preparation of Cellulose Fiber Bundles Derived from Gelidium) Cellulose fiber bundles derived from algae in Example 1B were obtained by the following steps. - Treatment of Algal Fibers - Gelidium elegans, a red alga of the family Gelidaceae, was immersed in water and boiled for 60 minutes. After that, the water was changed and the above steps were repeated to remove the approximate water-soluble components contained in the algal fibers and obtain algal residue. - Alkaline Extraction - The algal residue was immersed in water, and sodium hydroxide of about 5% by mass of the oven-dry mass of the algal residue to be treated was added. The algal residue was treated for 1 hour in an environment with an algal residue concentration of 10% by mass, pH: 10-12, and 60°C. - Bleaching - The algal residue was bleached for 1 hour in an aqueous sodium hypochlorite solution (available chlorine of 10% of the oven-dry mass of the algal residue) in an environment with an algal residue concentration of 10% by mass, pH: 10-11, and 60°C. The bleaching treatment was also performed twice. - Acid Treatment - Bleached algal residue was treated with hydrochloric acid aqueous solution prepared to a pH of approximately 2 at a concentration of 10% by mass of algal residue, in an environment of 25°C for 1 hour. - Neutralization Treatment - The acid-treated algal residue was neutralized to a pH of approximately 6 using sodium hydroxide aqueous solution. The algal residue was also washed with a large amount of water.
[0087] [Example 2B] (Preparation of cellulose fiber bundles derived from Gracilaria) Cellulose fiber bundles derived from algae were obtained in the same manner as in Example 1B, except that Gracilaria vermiculophylla of the family Gracilaceae was used instead of Gelidium elegans, a red alga of the family Gelidaceae.
[0088] [Example 3B] (Preparation of cellulose fiber bundles derived from cottonii) Cellulose fiber bundles derived from algae of Example 3B were obtained in the same manner as in Example 1B, except that cottonii (Kappaphycus cottonii) of the genus Kappaphycus in the family Myelinaceae was used instead of Gelidium elegans, a red alga of the genus Gelidium in the family Gelidaceae.
[0089] [Comparative Example 1B] (Preparation of bleached softwood kraft pulp) The pulp of Comparative Example 1B was obtained from commercially available bleached softwood pulp fibers. Dried bleached softwood pulp fibers (NBKP) were soaked in plenty of water for 24 hours to allow the fibers to swell sufficiently with water, thereby obtaining the pulp of Comparative Example 1B.
[0090] [Comparative Example 2B] (Preparation of bleached hardwood kraft pulp) The pulp of Comparative Example 2B was obtained in the same manner as in Comparative Example 1B, except that bleached hardwood pulp fibers (LBKP) were used instead of NBKP.
[0091] [Comparative Example 3B] The bleached coniferous kraft pulp obtained from Comparative Example 1B was subjected to the acid treatment shown in Example 1B to obtain the pulp of Comparative Example 3B.
[0092] [Comparative Example 4B] (Preparation of pulp derived from red algae as shown in Patent Document 2) The pulp of Comparative Example 4B was obtained by following the steps below, with reference to the method of the example shown in Japanese Patent Publication No. 2025-519275, listed in Patent Document 2. -Removal of carrageenan / agar- Gracilaria vermiculophylla was boiled in an aqueous sulfuric acid solution (5.0% by mass) for 360 minutes to remove the agar-like substance. -Bleaching and washing of the residue- 600 parts by mass of water and 5.0 parts by mass of sodium hypochlorite were added to 100 parts by mass of the residue of Gracilaria, and the mixture was reacted for 5 hours while maintaining a temperature that did not fall below 60°C. The pH of the aqueous solution was 5. After the reaction, the residue was washed with a large amount of water to obtain the pulp of Comparative Example 4B.
[0093] [Comparative Example 5B] (Preparation of red algae-derived pulp as shown in Patent Document 3) The pulp of Comparative Example 5B was obtained by following the steps below, with reference to the method of the example shown in International Publication No. 2018 / 159980 cited in Patent Document 3. - Washing of red algae biomass - Gelidium elegans of the family Gelidaceae was thoroughly washed with water, and any impurities were removed to obtain biomass. - Pulping with alkali - Sodium hydroxide was added to the dry weight of the biomass to a concentration of 20% by mass, and heated in a pressure cooker for 2 hours (heated at approximately 120°C for 2 hours). - Fiberization by mechanical processing - After alkali treatment, solid-liquid separation was performed, and the mixture was beaten using a PFI mill until it became porridge-like. After that, it was further refined using a homomixer. The pulp temperature at this time was above 80°C. After refinement, the fibers were selected using a 200-mesh screen. - Bleaching - The pulp concentration was adjusted to 10% by mass. Subsequently, while continuing to heat and maintain the temperature so that it does not fall below 90°C, 20% by mass of hydrogen peroxide, 20% by mass of sodium hydroxide, and 1% by mass of sodium silicate were added in a ratio of oven-dry pulp mass, and the mixture was bleached for 1 hour. After the treatment, the solution was changed to 10% by mass of hydrogen peroxide, 1.5% by mass of sodium hydroxide, and 0.5% by mass of sodium silicate in a ratio of oven-dry pulp mass, and the mixture was bleached again for 1 hour while maintaining a temperature of 90°C or higher. -Selection- Impurities such as sand contained in the obtained pulp were removed, and the mixture was selected using a 200-mesh screen to obtain the pulp of Comparative Example 5B.
[0094] [Comparative Example 6B] A cellulose fiber bundle derived from algae was obtained in the same manner as in Example 1B, except that no acid treatment or micronization treatment was performed, and a neutralization treatment was carried out on the bleached fibers.
[0095] <Evaluation> - Evaluation of changes in fiber filtration efficiency and dewatering properties due to stirring during disintegration treatment - Filtration efficiency is an index that indicates the speed and ease at which water is discharged from pulp fibers sufficiently dispersed in an aqueous solution. Generally, the finer the fibers are, the greater the surface area of the fibers and the improved water retention between fibers, which inhibits water discharge, thus decreasing filtration efficiency. Also, the higher the filtration efficiency, the faster and easier water discharge is, resulting in high dewatering properties and easy drying. The measurement method used was a Canadian standard filtration efficiency tester (Kumagai Riki Kogyo Co., Ltd., Canadian Free Nest Tester).
[0096] As an experiment to evaluate the filtration efficiency, each fiber bundle and pulp obtained in Examples 1B to 3B and Comparative Examples 1B to 5B was stirred using a disintegrator as defined in ISO 5263-1:2004 for a cumulative number of rotations of 0, 50, 100, 250, 500, 1000, 3000, 5000, 10000, and 30000, respectively, and pulp equivalent to 3.0 g of oven-dry fiber mass was used. This pulp was thoroughly dispersed in water to prepare a 1 L suspension with a concentration of 0.03%. Using this suspension, the Canadian standard filtration efficiency was determined in the same manner as in the case of algae-derived MFCs described above, according to JIS P 8121-2:2012 Pulp - Method for testing filtration efficiency - Part 2: Canadian standard filtration efficiency method and ISO 5267-2:2001.
[0097] Table 3, Figure 8 (cumulative rotations 0-30,000 times), and Figure 9 (cumulative rotations 0-500 times) show the changes in filtration efficiency with respect to the cumulative number of rotations obtained in the above experimental procedure. Figures 8 and 9 plot the results for Examples 1B, 3B, Comparative Examples 1B, 4B-6B. The algal-derived cellulose fiber bundles obtained by this disclosure (Examples 1B, 2B, and 3B) had a relatively high filtration efficiency of approximately 800 mL to 500 mL before stirring by the dissociation treatment, and therefore were in a fibrous state with high dewatering properties. Furthermore, the filtration efficiency changed significantly with respect to the cumulative number of rotations of the dissociator's propeller, bottoming out at approximately 50 mL to 40 mL at around 500 cumulative rotations. Since the filtration efficiency decreased significantly, it is considered that the fibers were refined by stirring during the dissociation treatment. Therefore, the algal-derived cellulose fiber bundles obtained by this disclosure are materials in which the filtration efficiency, dewatering properties, and the stage of fiber refinement can be adjusted by the dissociation treatment. This is thought to be because the acid treatment after bleaching of the algal fibers shown in this disclosure improved the defibrillability of the fiber bundles. The reason why acid treatment improves defibrillability is not entirely clear, but it is thought that, for example, a portion of the components present between the fine cellulose fibers is removed, and the fibers are treated in a state that makes them easier to separate. In the bleached softwood kraft pulp and the bleached hardwood kraft pulp (Comparative Examples 1B and 2B), the filtration rate did not change significantly with agitation using a disintegrator. It is thought that the mechanical treatment was not sufficient to cause a decrease in filtration rate and further micronization in general wood-derived fibers. The disintegrator and disintegration treatment used in this disclosure are defined in ISO 5263-1:2004 as a treatment to sufficiently diffuse wood fibers into water, so micronization of wood-derived pulp does not basically occur, and therefore the filtration rate does not change significantly. In the bleached softwood kraft pulp (Comparative Example 3B) that underwent the acid treatment shown in Example 1B, the filtration rate did not change significantly with agitation. Even when acid treatment is performed, the filtration efficiency of the pulp in Comparative Example 1B is almost the same, and this is thought to be because, as described in this disclosure, when algae with a fine fibrous structure are not used as raw materials, acid treatment does not lead to a decrease in filtration efficiency or further micronization.For the pulp of Comparative Example 4B, which reproduced Patent Document 2, the filtration water content was low, about 200 mL, even before stirring, and the filtration water content did not change significantly regardless of the cumulative number of rotations during stirring. As disclosed in Patent Document 2, since fibers are obtained from the beginning as elliptical red algae fibers, it is thought that the filtration water content was low even before stirring and the dewatering ability was poor. Also, since the acid treatment shown in this disclosure is not included, it is thought that the fineness of the fibers did not progress, and therefore no change in filtration water content occurred with the cumulative number of rotations. Therefore, in the method of Patent Document 2, it is not possible to adjust the filtration water content, dewatering ability, and the stage of fiber fineness by stirring during the disintegration process. For the pulp of Comparative Example 5B, which reproduced Patent Document 3, the filtration water content was low, about 50 mL, even before stirring, and the filtration water content did not change significantly regardless of the cumulative number of rotations during stirring. This is thought to be because, as disclosed in Patent Document 3, fineness had already been sufficiently carried out by mechanical processing using a beater or homomixer. Therefore, the fibers have low filtration efficiency from the start and poor dewatering ability, and the method of Patent Document 3 does not allow for adjustment of filtration efficiency, dewatering ability, and the stage of fiber refinement by stirring during the disintegration process. The cellulose fiber bundle of Comparative Example 6B, which was prepared in the same manner as Example 1B except that no acid treatment was performed, had a relatively high filtration efficiency of about 700 mL before stirring, and therefore the fibers were in a state of high dewatering ability. On the other hand, compared to the cellulose fiber bundles of Examples 1B to 3B, the decrease in filtration efficiency and the progress of refinement with increasing cumulative stirring rotations were slow, and refined cellulose could not be obtained. Therefore, compared to the example in which acid treatment was performed, some degree of fiber refinement by stirring was observed under these conditions, but it was significantly inferior, and it is insufficient as a method for obtaining refined cellulose. Furthermore, the method of Comparative Example 6B does not allow for adjustment of filtration efficiency, dewatering ability, and the stage of fiber refinement by stirring during the disintegration process.
[0098]
[0099] - Evaluation of changes in fiber width and refinement caused by stirring due to disintegration - As shown in the above experiment, stirring using a disintegrator as defined in ISO 5263-1:2004 does not seem to cause a decrease in the filtration efficiency of general wood pulp fibers, nor does it seem to refine the fibers. On the other hand, as shown in the results of the cellulose fiber bundles of Examples 1B to 3B, the cellulose fiber bundles derived from algae of this disclosure undergo a significant change in filtration efficiency, and it is thought that the fibers are refined. In this section, the fiber width of 100 fibers that were stirred with the disintegrator obtained in the above experiment for a cumulative number of rotations of 0, 50, 100, 250, 500, 1000, 3000, 5000, 10000, and 30000 times, respectively, was measured by observation with an optical microscope and is shown in Table 4, Figure 10, and Figure 11. Figures 10 and 11 plot the results for Examples 1B, 3B, Comparative Examples 1B, 4B-6B. Furthermore, for the cellulose fiber bundles in Examples 2B and 3B, fibers with a diameter of 1 μm or less were obtained when the propeller section of the dissociator was stirred for a cumulative number of rotations of 1,000, 3,000, 5,000, 10,000, and 30,000 times. Therefore, the fiber width of 100 fibers was measured by observation using an electron microscope.
[0100] The algae-derived cellulose fiber bundles obtained by this disclosure (Examples 1B to 3B) have a very large fiber width of 200 μm or more when no stirring is performed during the disintegration process. In the evaluation of filtration efficiency described above, the cellulose fiber bundles of Examples 1B to 3B had a very high filtration efficiency before stirring, which is thought to be because this large fiber width is preserved. Furthermore, when the cumulative number of rotations of the propeller section due to stirring reached about 50 to 1000 times, the fiber width rapidly decreased. This is thought to be because the fiber bundles were refined by stirring. Therefore, the algae-derived cellulose fiber bundles obtained by this disclosure are materials in which the fiber width and the stage of refinement obtained by stirring during the disintegration process can be adjusted. In bleached softwood kraft pulp and bleached hardwood kraft pulp (Comparative Examples 1B and 2B), the fiber width did not change significantly with stirring during the disintegration process. In general wood-derived fibers, it is thought that the mechanical treatment was not sufficient to cause a large change in fiber width and promote refinement. The disintegrator and stirring used in this disclosure are procedures specified in ISO 5263-1:2004 to sufficiently diffuse wood fibers into water. Therefore, the wood-derived pulp is not significantly refined, and the fiber width does not change significantly under these conditions. In the bleached coniferous kraft pulp (Comparative Example 3B) that underwent acid treatment as shown in Example 1B, no change in fiber width was observed during stirring. Even after acid treatment, the fiber width was almost the same as that of the pulp in Comparative Example 1B. This is thought to be because, as described in this disclosure, if algae with a fine fiber structure are not used as raw materials, acid treatment does not cause changes in fiber width or refinement. In the case of the pulp of Comparative Example 4B, which reproduces Patent Document 2, the fiber width (corresponding to the minor axis, as the obtained fibers are elliptical) was approximately 100 μm even before stirring, and did not change significantly regardless of the cumulative number of rotations of the propeller during stirring. This is thought to be because, as disclosed in Patent Document 2, the fibers are obtained from the beginning as elliptical red algae fibers, so the fiber width remained constant from before stirring to after stirring. Therefore, in the method described in Patent Document 2, it is not possible to adjust the fiber width or the stage of fiber refinement by stirring during the disintegration process.In the case of the pulp of Comparative Example 5B, which reproduced Patent Document 3, the fiber width was relatively small at 5 μm even before stirring, and the fiber width did not change regardless of the cumulative number of rotations during stirring. This is thought to be because, as disclosed in Patent Document 3, sufficient micronization had already been carried out by mechanical processing using a beater or homomixer. Therefore, the fibers were small from the beginning, and in the method of Patent Document 3, it is not possible to adjust the fiber width and the stage of fiber micronization by stirring during the disintegration process. In the case of the cellulose fiber bundle of Comparative Example 6B, which was prepared to be the same as Example 1B except that no acid treatment was performed, the fiber width before stirring was large, about 380 μm, almost the same as the cellulose fiber bundle of Example 1B. Therefore, it was almost in an undisintegrated state. On the other hand, compared to the cellulose fiber bundle of Example 1B, the change in fiber width and the progress of micronization with respect to the cumulative number of rotations during stirring were slow, and plateaued at around 280 μm, so micronized cellulose could not be obtained. Therefore, compared to the cellulose fiber bundle of Example 1B in which acid treatment was performed, while some degree of fiber refinement by stirring is observed under these conditions, it is significantly inferior and insufficient as a method for obtaining refined cellulose. Furthermore, in the method of Comparative Example 6B, it is not possible to adjust the fiber width and the stage of fiber refinement by stirring during the disintegration treatment.
[0101]
[0102] - Observation of Fiber Shape - Cellulose fiber bundles derived from algae obtained in Examples 1B to 3B were observed using an optical microscope. The results are shown in Figures 12 to 14.
[0103] The cellulose fiber bundles obtained in Examples 1B to 3B retain almost the same structure as conventional algae, resulting in a large average fiber width (average short diameter), with fiber bundles of 200 μm or more observed. As shown in the above experiments, the large fiber width and high filtration efficiency suggest excellent dewatering properties. Furthermore, as shown in the above experiments, the acid treatment described in this disclosure facilitates the refinement of the fibers with a simple treatment. The cellulose fiber bundles derived from algae in Examples 1B to 3B, refined to a filtration efficiency of approximately 250 mL to 450 mL by stirring with a dissociator up to a cumulative propeller rotation count of 50, were observed with an optical microscope. The results are shown in Figures 15 to 17. It can be confirmed that finer fiber bundles and fibers are separated from larger fiber bundles by stirring. The cellulose fibers derived from algae in Example 1B, refined by stirring with a dissociator up to a cumulative propeller rotation count of 5000, were observed with an optical microscope. The results are shown in Figure 18. Furthermore, optical microscope images of the micronized algae-derived cellulose fibers from Examples 2B to 3B are shown in Figures 19 to 20.
[0104] Furthermore, the average minor diameter of the algae-derived cellulose fiber bundles (fiber bundles before refinement) obtained in Examples 1B to 3B, the average fiber width (average minor diameter, W), average fiber length (L), and aspect ratio (L / W) of the algae-derived cellulose fiber bundles (fiber bundles after refinement, i.e., algae-derived MFCs) after a cumulative number of rotations of 10,000 were measured using the same method as described above. The results are shown in Table 5. In addition, the average fiber width (average minor diameter, W), average fiber length (L), and aspect ratio (L / W) of the fiber bundles or pulp before refinement of Comparative Examples 1B to 6B were measured using the same method as described above. The results are shown in Table 6. For the cellulose fiber bundles of Examples 2B and 3B after refinement, the average minor diameter and average fiber length of the obtained fibers were determined using an electron microscope. For the cellulose fiber bundle of Example 1B after refinement, refined fibers of 10 μm or less (approximately 3 μm) were observed. In the cellulose fiber bundles of Examples 2B and 3B after refinement, refined fibers of 1 μm or less (approximately 0.05 μm) were observed.
[0105]
[0106]
[0107] - Evaluation of changes in fiber filtration efficiency and dewatering properties due to beating treatment in a PFI mill - For the pulps obtained in Examples 1B to 3B and Comparative Examples 1B, 4B, and 5B, the Canadian standard filtration efficiency was determined in the same manner as for the algae-derived MFCs described above, except that pulps equivalent to 3.0 g of oven-dry fiber mass were used, after beating treatment using a PFI mill as defined in ISO 5264-2:2011, with cumulative rotation counts of 0, 50, 1000, 250, 500, 1000, 3000, and 5000, respectively.
[0108] Table 7, Figure 21 (cumulative rotations 0-5000 times), and Figure 22 (cumulative rotations 0-500 times) show the changes in filtration efficiency with respect to the cumulative number of rotations using the PFI mill obtained in the above experimental procedure. The algal-derived cellulose fiber bundles obtained by this disclosure (Examples 1B, 2B, and 3B) had a relatively high filtration efficiency of approximately 800 mL to 500 mL before the beating treatment, and therefore were in a fibrous state with high dewatering properties. Furthermore, the filtration efficiency changed significantly with beating by the rotation of the PFI mill, bottoming out at approximately 50 mL to 40 mL at approximately 250 cumulative rotations. Since the filtration efficiency decreased significantly, it is considered that the fibers were refined by the beating treatment. Therefore, the algal-derived cellulose fiber bundles obtained by this disclosure are materials in which the filtration efficiency, dewatering properties, and the stage of fiber refinement can be adjusted by the beating treatment. In the bleached coniferous kraft pulp (Comparative Example 1B), the filtration efficiency gradually decreased with increasing cumulative rotations during the beating treatment using a PFI mill. On the other hand, the rapid changes seen in the cellulose fiber bundles of Examples 1B to 3B were not observed. This is thought to be because the fibers of the wood pulp in Comparative Example 1B, etc., have a more rigid structure than the algae-derived fibers in Examples 1B to 3B, etc. For the pulp of Comparative Example 4B, which reproduced Patent Document 2, the filtration efficiency was low, about 200 mL, even before the beating treatment. Although some decrease in filtration efficiency was observed with increasing cumulative rotations during beating, the change in filtration efficiency was not as significant as that seen in the cellulose fiber bundles of Examples 1B to 3B. As disclosed in Patent Document 2, since the fibers are obtained from the beginning as elliptical red algae fibers, the filtration efficiency was low even before beating, and it is thought that the dewatering ability was poor. Furthermore, since the acid treatment shown in this disclosure is not included, the fineness of the fibers did not progress, and therefore, it is thought that no change in filtration efficiency occurred with increasing cumulative rotations. Therefore, the method described in Patent Document 2 does not allow for adjustment of the degree of filtration, dewatering, and the stage of fiber refinement through the beating process. In the case of the pulp of Comparative Example 5B, which reproduced Patent Document 3, the degree of filtration was low, at about 50 mL, even before the beating process, and the degree of filtration did not change significantly regardless of the cumulative number of rotations during the beating process. This is thought to be because, as disclosed in Patent Document 3, sufficient refinement had already been carried out by mechanical processing using a beater or homomixer.Therefore, the fibers have low filtration capacity from the start and poor dewatering properties, and the method described in Patent Document 3 cannot adjust the filtration capacity, dewatering properties, and the stages of fiber refinement through beating.
[0109]
[0110] - Evaluation of changes in fiber width and refinement due to beating treatment - As shown in the above experiment, the beating treatment using a PFI mill as defined in ISO 5264-2:2011 resulted in a significant decrease in filtration efficiency in the cellulose fiber bundles of Examples 1B to 3B, which is not seen in general wood pulp fibers. From these results, it is considered that algae-derived cellulose fiber bundles undergo a significant change in filtration efficiency and also result in refinement of the fibers. In this section, the fiber widths of 100 fibers subjected to beating treatment with a PFI mill obtained in the above experiment, with cumulative rotation counts of 0, 50, 100, 250, 500, 1000, 3000, and 5000 times, were measured by observation with an optical microscope and are shown in Table 8, Figure 23, and Figure 24. Furthermore, in the cellulose fiber bundles of Examples 1B to 3B, fibers subjected to beating with cumulative rotations of 500, 1000, 3000, and 5000 times yielded fibers with a thickness of 1 μm or less. Therefore, the fiber width of 100 fibers was measured by observation using an electron microscope.
[0111] The algae-derived cellulose fiber bundles obtained by this disclosure (Examples 1B to 3B) have a very large fiber width of 200 μm or more before the beating treatment is performed. In the evaluation of filtration efficiency described above, the cellulose fiber bundles of Examples 1B to 3B had a very high filtration efficiency before the beating treatment, which is thought to be because this large fiber width is preserved. Furthermore, when the cumulative number of rotations by beating in the PFI mill reached about 50 to 1000, the fiber width rapidly decreased. This is thought to be because the beating treatment promoted defibration of the fiber bundles, resulting in finer fibers. It is also thought that the acid treatment created a state where defibration was more likely to occur. Therefore, the algae-derived cellulose fiber bundles obtained by this disclosure are materials in which the fiber width and the stage of finer fibers obtained by the beating treatment can be adjusted. In the case of bleached softwood kraft pulp (Comparative Example 1B), the fiber width did not change significantly during the beating treatment in the PFI mill. In general wood-derived fibers, the fiber width changes significantly, and it is thought that the mechanical treatment was not sufficient to promote finer fibers. In the case of the pulp of Comparative Example 4B, which reproduced Patent Document 2, the fiber width (corresponding to the minor axis, since the obtained fibers are elliptical) was approximately 100 μm even before the beating treatment, and it did not change as much as the cellulose fiber bundles of Examples 1B to 3B, regardless of the cumulative number of rotations during the beating treatment. This is thought to be because, as disclosed in Patent Document 2, the fibers were obtained from the beginning as elliptical red algae fibers, so the fiber width remained constant from before the beating treatment to after the beating treatment. Therefore, in the method of Patent Document 2, it is not possible to adjust the fiber width or the stage of fiber refinement by the beating treatment. In the case of the pulp of Comparative Example 5B, which reproduced Patent Document 3, the fiber width was relatively small at 5 μm even before the beating treatment, and the fiber width did not change regardless of the cumulative number of rotations during stirring. This is thought to be because, as disclosed in Patent Document 3, sufficient refinement had already been carried out by mechanical processing using a beater or homomixer. Furthermore, since the acid treatment process carried out in Examples 1B to 3B was not performed in this disclosure, it is thought that no further refinement occurred.Therefore, since the fibers have a small fiber width from the beginning, the method described in Patent Document 3 does not allow for adjustment of the fiber width or the stage of fiber refinement through the beating process.
[0112]
[0113] The disclosure of Japanese Patent Application No. 2025-078283, filed on 8 May 2025, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually noted to be incorporated by reference.
Claims
1. A cellulose fiber bundle derived from algae, wherein the filtration capacity measured according to ISO 5267-2:2001 is 400 mL or more, and the filtration capacity after disintegration treatment with a cumulative number of rotations of 10,000 under the conditions specified in ISO 5263-1:2004 is 200 mL or less.
2. The cellulose fiber bundle according to claim 1, wherein the filtration capacity after disintegration treatment with a cumulative number of rotations of 3,000 under the conditions specified in ISO 5263-1:2004 is 200 mL or less.
3. The cellulose fiber bundle according to claim 1, wherein the filtration capacity after disintegration treatment with a cumulative number of rotations of 1000 under the conditions specified in ISO 5263-1:2004 is 200 mL or less.
4. Cellulose fiber bundles derived from algae, wherein the filtration capacity measured according to ISO 5267-2:2001 is 400 mL or more, and the filtration capacity after beating treatment with a PFI mill specified in ISO 5264-2:2011 for a cumulative number of rotations is 200 mL or less.
5. The cellulose fiber bundle according to claim 1 or claim 4, wherein the average minor diameter is 50 μm or more.
6. The cellulose fiber bundle according to claim 1 or claim 4, wherein the average minor diameter is 100 μm or more.
7. The cellulose fiber bundle according to claim 1 or claim 4, wherein the average minor diameter is 200 μm or more.
8. The cellulose fiber bundle according to claim 1 or claim 4, wherein the average minor diameter after the disintegration treatment or the beating treatment is 1 / 3 or less of the average minor diameter before the disintegration treatment or the beating treatment.
9. The cellulose fiber bundle according to claim 1 or claim 4, wherein the algae are red algae.
10. The cellulose fiber bundle according to claim 9, wherein the red algae comprises at least one species selected from the group consisting of the families Apocynaceae, Apocynaceae, Apocynaceae, Apocynaceae, Apocynaceae, Apocynaceae, Apocynaceae, Apocynaceae, Apocynaceae, Apocynaceae and Apocynaceae.
11. Microfibrillated cellulose derived from algae, wherein the average short diameter of the microfibrillated cellulose is 1 μm to 10 μm, and the aspect ratio of the microfibrillated cellulose is 100 or more.
12. Microfibrillated cellulose derived from algae, wherein the average short diameter of the microfibrillated cellulose is 30 nm to 1000 nm, and the aspect ratio of the microfibrillated cellulose is 100 or more.
13. Microfibrillated cellulose according to claim 11 or claim 12, wherein the filtration capacity measured in accordance with ISO 5267-2:2001 is 200 mL or less.
14. Paper comprising microfibrillated cellulose as described in claim 11 or claim 12.
15. Basis weight 30 g / m² 2 ~100g / m 2 The paper according to claim 14, wherein the opacity is 80% or less under the conditions.
16. The paper according to claim 14, which is impregnated with at least one selected from the group consisting of polysaccharides, oils and fats, waxes, natural resins and synthetic resins, and has an opacity of 80% or less.
17. A paper modifier comprising microfibrillated cellulose as described in claim 11 or claim 12.
18. A paint comprising microfibrillated cellulose as described in claim 11 or claim 12.
19. A building material comprising microfibrillated cellulose according to claim 11 or claim 12.
20. A fiber-reinforced material comprising microfibrillated cellulose according to claim 11 or claim 12.
21. A method for producing a cellulose fiber bundle derived from algae according to claim 1 or claim 4, comprising, in this order: a preparation step of preparing an algal residue obtained by removing at least a portion of solvent-soluble components from algae; an alkali treatment step of immersing the algal residue in an alkaline aqueous solution; a bleaching step of bleaching the algal residue after the alkali treatment step; and an acid treatment step of immersing the algal residue after the bleaching step in an acid aqueous solution.
22. The method for producing a cellulose fiber bundle according to claim 21, wherein the pH of the alkaline aqueous solution is 9 to 14.
23. The method for producing a cellulose fiber bundle according to claim 21, wherein the temperature of the alkaline aqueous solution is 20°C to 100°C.
24. The method for producing a cellulose fiber bundle according to claim 21, wherein the pH of the acidic aqueous solution is 1 to 4.
25. The method for producing a cellulose fiber bundle according to claim 21, wherein the temperature of the acidic aqueous solution is 20°C to 60°C.
26. The method for producing a cellulose fiber bundle according to claim 21, wherein the bleaching agent used in the bleaching step comprises at least one selected from the group consisting of hypochlorite, hydrogen peroxide, and chlorine dioxide.
27. A method for producing a cellulose fiber bundle according to claim 21, further comprising a neutralization step of neutralizing the algal residue after the acid treatment step.
28. A method for producing microfibrillated cellulose derived from algae, comprising a micronization step of micronizing the cellulose fiber bundle obtained via the method for producing cellulose fiber bundles described in claim 21.
29. The method for producing microfibrillated cellulose according to claim 28, wherein the refinement step refines the average short diameter of the cellulose fiber bundle to 1 / 10 or less of the diameter before the refinement step, or to 10 μm or less.